Hot-rolled h-shaped steel for fabricated building structure and preparation method therefor
By optimizing chemical composition and smelting process, combined with fine rolling and cooling processes, the problem of insufficient low-temperature toughness and welding performance of hot-rolled H-shaped steel for prefabricated building structures in cold areas is solved, and high yield strength and tensile resistance are achieved Strength, suitable for use in cold areas.
Patent Information
- Application Number
- PCT/CN2023/129494
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2023-11-03
- Publication Date
- 2024-11-21
AI Technical Summary
The existing hot-rolled H-shaped steel for prefabricated building structures has insufficient low temperature toughness and welding performance in cold areas, making it difficult to meet the low temperature environment needs of -20℃ or even -40℃. At the same time, the yield ratio is too high, which affects the comprehensive performance of the material. .
By optimizing chemical composition and smelting process, the content of chemical compositions such as C, Si, Mn, P, Cr, Ni, Nb, Ti, Al, Mo and other elements is controlled, Ti and Al are added to refine the grains, and Cu and Ni are used to Improve weather resistance, and control grain size and ferrite structure through fine rolling and cooling processes, reduce the yield strength ratio and enhance low-temperature impact toughness.
It has achieved good impact toughness and welding performance of H-shaped steel at -40℃, with yield strength and tensile strength reaching 355MPa and above, with an elongation of 21% and above. It is suitable for use in cold areas, with good welding properties and meets more than 50 years of use. Life expectancy.
Smart Images

Figure CN2023129494_21112024_PF_FP_ABST
Abstract
Description
Hot-rolled H-shaped steel for assembled building structure and preparation method thereof
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310555052.4 filed on May 17, 2023, which is hereby incorporated by reference in its entirety. Technical Field
[0003] The present invention belongs to the field of steel smelting technology and rolling forming technology, and in particular, the present invention relates to a hot-rolled H-shaped steel for assembled building structures and a preparation method thereof. Background Art
[0004] With the increasing promotion of prefabricated buildings, the proportion of prefabricated buildings in steel structures is gradually increasing. Prefabricated buildings not only conform to the development trend of green, energy-saving and environmentally friendly buildings, but also offer technical advantages such as excellent seismic resistance, light weight, fast construction speed, high degree of industrialization, and a high prefabrication rate. Compared with traditional construction, prefabricated buildings have significant construction time advantages. Therefore, the rapid development momentum requires the vigorous development of prefabricated steel structures. Prefabricated steel structures are primarily composed of steel, a green and environmentally friendly building material with unparalleled environmental advantages over concrete in terms of recycling and reuse. With the promotion of prefabricated buildings, hot-rolled H-beams with excellent comprehensive performance meet the needs of prefabricated buildings, requiring weather resistance, fire resistance, and excellent weldability. This is particularly applicable to tropical, temperate, and cold regions. In addition to meeting these requirements, hot-rolled H-beams used in prefabricated buildings in cold regions must also exhibit good low-temperature toughness and be suitable for welding in low-temperature environments. In some areas, the ductile-brittle transition temperature must be maintained below -20°C or even -40°C, meeting the requirements of excellent comprehensive performance.
[0005] Currently, hot-rolled H-shaped steel used in building structures generally meets only one performance requirement. For prefabricated building structures, hot-rolled H-shaped steel, as it is encased in the building structure, must have a service life of at least 50 years without replacement. Furthermore, for environmental reasons, it must be exposed and unpainted. Therefore, it must not only meet strength requirements of 355MPa or above, but also maintain a moderately high yield-to-strength ratio. It must also possess excellent fire and seismic resistance, weldability, and suitability for welding in low-temperature environments. Furthermore, its weathering properties must be higher than those of standard weathering steel.
[0006] Summary of the Invention
[0007] The present invention aims to overcome the shortcomings of the prior art and, to meet the needs of prefabricated building structures in a wider range of regions, provide a hot-rolled H-beam suitable for use in prefabricated buildings in cold regions, and its preparation method, in response to the high crack sensitivity of steel produced from special-shaped castings. The H-beam achieves excellent overall performance at the flanges and webs, including excellent corrosion resistance, weldability, and a low yield strength ratio, while also achieving good impact toughness at -40°C. This material meets the application needs of hot-rolled H-beam materials in steel construction, including prefabricated building structures in both ordinary and cold regions, and provides support for the widespread promotion of H-beam in prefabricated building structures.
[0008] To achieve the above objectives, the technical solution adopted by the present invention has the following specific requirements:
[0009] The present invention provides a hot-rolled H-shaped steel for prefabricated building structures suitable for use in cold regions. The chemical composition of the H-shaped steel is as follows by weight percentage (wt%): C: 0.03-0.05; Si: <0.15; Mn: 0.6-0.9; P: 0.030-0.045; S≤0.005; Cu: 0.20-0.35; Cr: 0.25-0.50; Ni: 0.20-0.50, Nb: 0.02-0.04, Ti: 0.01-0.025; Al: 0.005-0.015; Mo: 0.10-0.15; Cu / Ni≤1.0, Al+Ti≤0.03, As+Sn+Zn+Ca+Mg+B≤0.030. The remainder is Fe and unavoidable impurities.
[0010] Preferably, the chemical composition of the H-shaped steel is as follows by weight percentage (wt%): Si: 0.05-0.15; 0.001≤S≤0.005, 0.015≤Al+Ti≤0.03.
[0011] Preferably, in the hot-rolled H-beam, As+Sn+Zn+Ca+Mg+B ≤ 0.025. During the smelting process, the gas content of the steel is controlled by weight to be 0.003 ≤ N ≤ 0.007, 3 ≤ Ti / N ≤ 4, and T.[O] ≤ 0.002. To improve low-temperature toughness, the number and size of inclusions are strictly controlled. Al deoxidation is used to control the purity of the molten steel. The residual element content (wt%) in the molten steel is controlled within the range of As+Sn+Zn+Ca+Mg+B ≤ 0.025. To prevent increased nitride precipitation, the N content is strictly controlled, while Al+Ti is limited to ≤ 0.03% and 3 ≤ Ti / N ≤ 4. A control range of Cu / Ni ≤ 1.0 is used to prevent cracking in the ingot while ensuring improved low-temperature toughness. More preferably, 0.7 ≤ Cu / Ni ≤ 1.0.
[0012] The specific purpose of the present invention is to control Ti: 0.01-0.025%; Al: 0.005-0.015%, Al+Ti≤0.03% in the range of: due to the low compression ratio during H-beam rolling, the degree of grain refinement during the rolling process is low, and in order to improve the low-temperature resistance of H-beam, the grain size level of the rolled material needs to be no less than level 8, so the grain size control requirement is achieved by refining the ingot grains; the specific operation is: 0.01-0.025% Ti and 0.005-0.015% Al are added to the molten steel, and the nitrogen element is controlled to be 0.003%≤N≤0.007%, 3≤Ti / N≤4. When Ti and N are within this content range, Ti reacts with the nitrogen element in the molten steel to form fine and dispersed TiN inclusions, and the TiN inclusions can be used as It is the crystallization nucleation point during the solidification process of the ingot grains, and can refine the original grain size of the ingot (after continuous casting and before entering the heating furnace) to above level 5. In addition, the fine and dispersed TiN inclusions can be pinned to the grain boundaries of the ingot, preventing the growth of the ingot grains during the heating process of the ingot, and can control the grain size level of the ingot out of the heating furnace to above level 4.5, which is conducive to achieving the goal of the grain size level of the rolled material being not less than level 8. The purpose of adding 0.005-0.015% Al to the molten steel is to remove dissolved oxygen in the molten steel and improve the recovery rate of the Ti alloy element in the steelmaking process. However, excessive addition of Ti and Al will lead to excessive inclusions of TiO2 and Al2O3, which can easily cause nodules in the continuous casting nozzle and affect the smooth progress of continuous casting. Therefore, it is necessary to control Al+Ti≤0.03%.
[0013] The present invention controls the Cu content to 0.20-0.35%, the Ni content to 0.20-0.50%, and the Cu / Ni ratio to ≤1.0 for the following specific purposes: The addition of Cu and Ni improves the weather resistance of H-beams, and Ni significantly enhances the low-temperature resistance of rolled steel. However, excessive Cu addition can easily cause cracks in the ingot. The addition of Ni effectively prevents the formation of "copper brittleness" defects and the formation of copper-rich phases. Adding nickel to copper-containing steel transforms the surface enriched layer of the steel into a copper-nickel-rich layer with a melting point exceeding 1200°C. Furthermore, the addition of Ni effectively modifies the morphology of sulfide inclusions in the steel, transforming long MnS inclusions into spindles, short strips, and even spheres, thereby improving transverse properties and reducing the hot working sensitivity caused by the addition of Cu. Cu / Ni≤1.0 can ensure that no cracks are generated during the continuous casting process of the ingot. At the same time, since the ability of Cu element to improve the refractory performance of steel is close to that of Ni element, it is further preferred to be 0.7≤Cu / Ni≤1.0. Controlling 0.7≤Cu / Ni can save the amount of expensive Ni element alloy added.
[0014] The specific purpose of controlling the carbon content in the present invention to 0.03-0.05% is that the steel is used in cold regions. Due to the low carbon content of the steel, low-carbon bainite or low-carbon martensite is generated at an ambient cooling rate after welding. Due to the low carbon content in the structure, the supersaturation of carbon causes a small dislocation increment in the bainite or martensite structure, a low expansion rate during the structural phase transformation, and a small hardness increment and residual stress at the weld. Accordingly, the weld has good impact resistance and can improve the low-temperature impact resistance of the weld and the weld heat-affected zone. Therefore, the steel is also suitable for welding operations in cold regions. No preheating or heat preservation is required before and after welding, which can simplify the welding process.
[0015] The specific purpose of controlling P: 0.030-0.045% in the present invention is: since the steel is designed with a low carbon component and has a high nickel content, the low-temperature resistance of the steel can be better guaranteed. When C and Ni are within this range, appropriately increasing the phosphorus content can still meet the low-temperature resistance of the rolled material. In addition, increasing the phosphorus content can improve the weather resistance of the steel and reduce the dephosphorization cost of the converter. Therefore, P: 0.030-0.045% is controlled.
[0016] Preferably, the hot-rolled H-shaped steel for prefabricated buildings with excellent performance provided by the present invention, its preparation method, and specific process control specifically include the following aspects:
[0017] 1Smelting process
[0018] 1) Converter smelting
[0019] Arsenic, tin, and other metals are present in the molten iron fed into the converter, all below 80 ppm. Heavy, low-sulfur, high-quality scrap steel is used for internal processing. Nickel plates and copper plates (granules) are added along with the scrap. The final slag basicity is controlled within the range of 2.8-3.8. Slag is added three minutes before the tapping point, ensuring thorough and complete slag formation. The final gun pressure time is ≥1 minute. Silicon, calcium, and barium are added during tapping at 2.8-3.2 kg / ton for deoxidation. Any deficiencies in deoxidation are supplemented during subsequent refining. Alloys are added evenly when the molten steel is 1 / 4 to 3 / 8 filled, and are completed when the steel is 3 / 4 to 7 / 8 filled. These alloys include one or more of silicon-manganese, ferrosilicon, medium-carbon ferrochromium, and ferroniobium. Synthetic slag is added at 6-10 kg / ton during or after tapping. Slag blocking is performed, and the tapping time is no less than 3 minutes.
[0020] 2) Refining LF+VD control
[0021] LF refining uses bottom-blown argon for stirring throughout the entire process. Calcium carbide, calcium silicon, barium, and aluminum particles are used to condition the slag. The top slag must be white or yellowish-white before leaving the station. Low-pressure soft blowing is used before leaving the station to ensure inclusions float. Soft argon blowing during refining is maintained for at least 15 minutes. 100-150 m / furnace of high-calcium wire is fed before soft argon blowing. [O] content in steel leaving the LF refining station is <10 ppm. At the end of LF refining, the molten steel temperature is controlled between 1590°C and 1610°C.
[0022] Before the molten steel enters the VD furnace, slag is removed. The vacuum level during VD refining is less than 70MPa, and the vacuum is maintained for more than 7 minutes. Bottom-blowing nitrogen stirring is performed throughout the VD refining process according to process requirements. The VD soft blowing time is more than 10 minutes, and the molten steel is strictly prohibited during the soft blowing process. The VD refining cycle is no less than 30 minutes. The [O] content of the steel leaving the VD refining station is less than 10ppm, and 30ppm≤N≤70ppm.
[0023] 3) Continuous casting
[0024] The continuous casting adopts a sleeve-type protective pouring process, using a large ladle nozzle with a sealing ring. The tundish uses a low-carbon alkaline covering agent + rice husk. The mold protection slag uses a special protective slag for peritectic steel. The thickness of the liquid slag layer is measured during the casting process to ensure that the liquid slag layer thickness is greater than the crystallizer amplitude. The secondary cooling adopts weak cooling, and the continuous casting speed is 0.8-0.9m / min. The superheat is controlled below 20℃; the smelted molten steel is cast into special-shaped billets. To avoid the occurrence of surface cracks in the billets, the special-shaped billets are hot-transferred and hot-loaded into the heating furnace after casting. The hot transfer temperature of the billets is controlled above 500℃ to avoid residual stress during the cooling process that may cause surface cracks.
[0025] 2 Rolling process
[0026] 1) Heating control
[0027] The shaped blanks are uniformly heated in the heating furnace. A high amount of alloying elements is added to the steel, and a low-temperature, long-term heating process is used to ensure uniform heating, prevent excessive and abnormal growth of austenite, and ensure sufficient solid solution diffusion of the alloying elements. The soaking stage temperature is controlled at 1230-1260°C for 130-180 minutes, after which the blanks are removed from the furnace for rolling.
[0028] 2) Controlled rolling and controlled cooling
[0029] The section steel production line utilizes a controlled rolling / controlled cooling process. The BD rough rolling process achieves shape-focused pass rolling with nine or fewer passes. The TM finishing process utilizes performance-controlled rolling with seven or fewer passes. The finishing temperature is controlled between 780°C and 830°C. Once the product temperature drops below 80°C, it enters the straightening mill for straightening, ensuring that the primary surface oxide scale is retained.
[0030] The finishing process utilizes both pre- and post-finishing mill cooling. A specially designed cooling device provides interpass cooling during the finishing rolling process (see Figure 1). Cooling water pipe A is installed before the finishing mill and cooling water pipe B is installed after the mill for control. During the finishing rolling process, section B is used for odd-numbered passes, and section A is used for even-numbered passes. The cooling device comprises: a front roller table 1, skirts 2, cooling water pipelines 3, upper nozzles 4, middle nozzles 5, and lower nozzles 6. Skirts 2 on both sides of the mill are mounted above the front roller table 1 and move according to the height of the workpiece as it passes through. The upper nozzles 4, middle nozzles 5, and lower nozzles 6 are connected to the cooling water pipeline 3, and cooling water is supplied through the pipeline. The middle nozzle 5 on the skirt 2 cools the outer flange, the upper nozzle 4 cools the upper web and upper rounded corners, and the lower nozzle 6 cools the lower web and lower rounded corners. The water volume in the nozzles is precisely controlled by valves based on temperature fluctuations. The cooling control method and working principle of the post-mill cooling section B rolling process are consistent with those of section A, and they can work together. At the same time, the cooling can be reduced according to the size of the steel rolled piece to meet the temperature control range requirements. The last pass is used to accurately control the temperature of the bar to meet the temperature difference changes in different parts during the rolling process, and to ensure that the temperature is uniform along the entire longitudinal direction of the rolled piece. Through the above device, the temperature difference between the upper and lower leg flanges is within 10°C, and the temperature difference between the web is within 5°C. The above equipment, combined with the micro-alloying design, can achieve the performance requirements of the final hot-rolled H-shaped steel; at the same time, it ensures that it has -40°C low-temperature resistance and fire resistance, and excellent weather resistance, and avoids the formation of a large amount of bainite and martensite due to the addition of Mo, which causes abnormal fluctuations in the mechanical properties of the flange and web.
[0031] 3) Cooling bed cooling control
[0032] After the product comes off the line, it is slowly cooled on the cooling bed. The cooling rate is strictly controlled according to the adjustment of the cooling bed fan and the movement rhythm of the rolled piece. Specifically, during the final rolling to 700℃ section, the cooling rate of the rolled material is 2-5℃ / s; during the period below 700℃, the cooling rate of the rolled material is below 2℃ / s to avoid the formation of coarse and abnormal tissues.
[0033] Further preferably, the above-mentioned method for preparing hot-rolled H-shaped steel suitable for architectural structure applications in different regions mainly includes the following steps: molten iron pretreatment - converter smelting - LF refining - VD refining - continuous casting billet casting and molding - hot delivery and hot charging furnace - heating furnace billet reheating - high-pressure water descaling - rough rolling - high-pressure water secondary descaling - finishing rolling, cooling and temperature-controlled rolling - controlled cooling after rolling - low-temperature straightening - fixed-length sawing - collection and stacking.
[0034] In order to improve the uniformity of the structure and prevent cracks during the smelting process, special process control is carried out: low superheat control is adopted to reduce segregation and control the superheat of the steel to less than 20°C; adding too much P element is likely to cause cracks in the ingot, and low pulling speed control is adopted in the ingot casting process to avoid transverse cracks and steel leakage.
[0035] The main rolling and cooling processes are as follows: the reheating temperature in a walking-beam furnace is controlled between 1220°C and 1245°C. The entire rolling process utilizes the XH rolling method. The roughing process achieves a cumulative deformation rate exceeding 40%, primarily to maintain the H-beam shape while also achieving austenite refinement. The finishing rolling process achieves a deformation rate exceeding 60%, refining the ferrite and pearlite matrix structures, ultimately achieving optimal strength and toughness. Water cooling is used in the finishing process to achieve uniform cooling. The finishing temperature of the upper and lower legs is precisely controlled between 780°C and 830°C, ensuring fine proeutectoid ferrite throughout the flange, excluding the rounded corners. Depending on the specification, the upper and lower flanges can experience a temperature difference of 30°C to 50°C. Precisely controlled cooling is achieved by spraying water on the outer edges of the upper and lower flanges using cooling facilities before and after the finishing mill. Cooling intensity is consistent with the specification. After cooling, the temperature difference within the same area of the upper and lower flanges is reduced to within 5°C, ensuring consistent performance across the entire H-beam. After exiting the finishing mill, the rolled product passes through a conveyor roller table. A heat shield is used to control the cooling rate based on ambient temperature fluctuations, preventing large temperature fluctuations from affecting the overall properties of the steel. After exiting the finishing mill, the product is naturally cooled on a cooling bed. After the product temperature drops below 80°C, it enters a straightening machine for straightening. The finished product flange thickness ranges from 16 to 45 mm. Mechanical properties testing is performed on samples taken from the 1 / 3 of the H-beam flange.
[0036] Due to the complex cross-sectional shape of H-shaped steel, water can easily accumulate in the H-shaped cavity, leading to uneven cooling overall. Water spraying is generally not used to cool H-shaped steel. The present invention provides a water spray cooling method for uniformly cooling H-shaped steel. After cooling, the temperature difference between the upper and lower flanges of the H-shaped steel is reduced to less than 5°C. The specific method is as follows: After rough rolling, a cooling device specially designed for this process is used for inter-pass cooling during the finishing rolling process (see Figure 1). Cooling water pipe A is installed before the finishing mill and cooling water pipe B is installed after the mill for control. During the finishing rolling process, section B is used for odd-numbered passes, and section A is used for even-numbered passes. Upper, middle, and lower water nozzles are installed on the skirt panels 2 on both sides of the rolling mill to control rolling temperature changes. The middle water nozzle 5 on the skirt panel 2 cools the outer side of the flange to achieve water spray cooling, ultimately reducing the temperature difference between the upper and lower flange legs. The above cooling process can minimize the temperature difference between the flange and the temperature difference between the flange and the web to less than 5°C.
[0037] Compared with the prior art, the advantages of the present invention are:
[0038] 1) The H-shaped steel product of the present invention has excellent comprehensive mechanical properties, with a yield strength of 355 MPa or greater, a tensile strength of 470 MPa or greater, and an elongation of 21% or greater; a longitudinal impact energy of 120 J at -40°C, making it suitable for use in prefabricated building structures in cold climates; and a weathering index I value range of 6.0 to 8.5; good weldability, a carbon equivalent Ceq of 0.35 or less, no preheating or insulation is required before and after welding, and a longitudinal impact energy of 90 J at -40°C in the weld and heat-affected zone after welding; a cold crack index Pcm of 0.15 or less; and Z-direction performance reaches the Z35 level, with comprehensive performance meeting the index requirements for H-shaped steel for prefabricated building structures.
[0039] 2) In order to obtain a good yield strength ratio, the present invention adopts a composite microalloying design in conjunction with a cooling device to precisely control the phase transformation, thereby obtaining a good grain size and a reasonable ratio of ferrite + pearlite matrix structure. Ultimately, the yield strength ratio of the H-beam is ≤0.8.
[0040] . BRIEF DESCRIPTION OF THE DRAWINGS
[0041] FIG1 is a structural diagram of a cooling arrangement for H-beam production according to the present invention;
[0042] [Corrected 18.12.2023 according to Rule 91] Figure 2a is a metallographic microstructure of the upper leg of the H-beam obtained in Example 1 of the present invention, Figure 2b is a metallographic microstructure of the lower leg of the H-beam obtained in Example 1 of the present invention, and Figure 2c is a metallographic microstructure of the web of the H-beam obtained in Example 1 of the present invention;
[0043] [Corrected 18.12.2023 according to Rule 91] FIG3a is a scanning electron micrograph of an impact fracture of the upper leg of the H-beam obtained in Example 6 of the present invention; FIG3b is a scanning electron micrograph of an impact fracture of the lower leg of the H-beam obtained in Example 6 of the present invention; and FIG3c is a scanning electron micrograph of an impact fracture of the web of the H-beam obtained in Example 6 of the present invention;
[0044] Reference numerals:
[0045] 1. Front roller table of rolling mill, 2. Skirt plate, 3. Cooling water pipeline, 4. Upper nozzle, 5. Middle nozzle, 6. Lower nozzle. DETAILED DESCRIPTION
[0046] The technical solution of the present invention is described in detail below with reference to the accompanying drawings and embodiments.
[0047] Each embodiment of the present invention is produced according to the following steps:
[0048] 1) After molten iron is smelted in a converter, it enters the LF+VD dual-process for chemical composition, alloying, and inclusion control. At the end of LF refining, the molten steel temperature is controlled at 1590-1610°C. The continuous casting process produces near-net-shape beams. Residual elements in the molten steel are strictly controlled to ≤ 0.030% for As+Sn+Zn+Ca+Mg+B. During the casting process, the casting superheat is controlled to less than 20°C, the casting speed is set between 0.8 and 0.9 m / min, and the straightening temperature is controlled above 840°C.
[0049] 2) During the rolling process, the billet is preferably heated in the soaking section of the heating furnace and kept within the range of 1240-1260°C for 130-180 minutes before being removed from the furnace for rolling. The rough rolling process (BD) consists of 7 or 9 passes, while the finishing (TM) process consists of 5 or 7 passes. The final finishing temperature is controlled between 780°C and 830°C. The cooling equipment before and after the TM mill measures the temperature distribution of the rolled piece and uses a cooling device to cool the piece between passes, ultimately ensuring that the final rolling temperature is within the appropriate temperature range and that surface defects are avoided. Due to the low-carbon design, the rolling force of the mill is low and easy to control. The cooling device includes: a front roller table 1 of the rolling mill, a skirt plate 2, a cooling water pipeline 3, an upper nozzle 4, a middle water nozzle 5, and a lower water nozzle 6; the skirt plates 2 on both sides of the rolling mill are arranged on the front roller table 1 of the rolling mill; the upper nozzle 4, the middle water nozzle 5, and the lower water nozzle 6 are respectively connected to the cooling water pipeline 3, the middle water nozzle 5 on the skirt plate 2 is used to cool the outside of the flange, the upper nozzle 4 is used to cool the upper surface of the web and the upper side R corner, and the lower water nozzle 6 is used to cool the lower web and the lower R corner.
[0050] 3) Cooling bed cooling control
[0051] After the product rolls off the production line, it undergoes a slow cooling process on a cooling bed. The cooling rate is strictly controlled by adjusting the cooling bed fan and the movement of the rolled piece. Specifically, during the final rolling period up to 700°C, the cooling rate is 2-5°C / s; below 700°C, the cooling rate is below 2°C / s to reduce the formation of coarse and abnormal structures. The chemical composition and process parameters of the specific embodiment are shown in the table below.
[0052] Table 1 Chemical composition of various embodiments of the present invention and comparative examples (wt.%)
[0053] According to the formula Ceq = C + Mn / 6 + (Cr + V + Mo) / 5 + (Cu + Ni) / 15 and Pcm = C + Si / 30 + (Mn + Cu + Cr) / 20 + Ni / 60 + Mo / 15 + V / 10 + 5B; the calculated carbon equivalent is less than 0.35; the crack sensitivity index is less than 0.13; the welding performance is excellent, meeting the use requirements of prefabricated building structural steel.
[0054] The main refining process parameters are shown in Table 2
[0055] Table 2 Main refining process parameters
[0056] The specific process parameters of the continuous casting process are shown in Table 3.
[0057] Table 3 Continuous casting process parameters
[0058] Table 3 is a list of main process parameters of various embodiments and comparative examples of the present invention;
[0059] Table 4 Main process parameters
[0060] Table 5 is a table of performance tests of various embodiments and comparative examples of the present invention.
[0061] Table 5: Rolled material mechanical properties record
[0062] Mechanical property tests were performed on samples of the prepared products. Sampling was performed at the 1 / 3 point from the edge to the center of the H-beam flange, and at the center of the web. The test standard was BS EN ISO 377-1997, "Sampling location and preparation of test specimens for mechanical properties tests." Test methods for mechanical properties such as yield strength, tensile strength, and elongation were performed in accordance with ISO 6892-1-2009, "Metallic materials - Room temperature tensile test methods." The impact energy test method was based on ISO 148-1, "Charpy pendulum impact test for metallic materials." The results are shown in Table 5. Comparison revealed that the H-beam flanges and webs produced using the preparation method of the present invention exhibited uniform performance, a low carbon equivalent, ease of welding, and a significantly reduced cracking probability. These H-beams are suitable for use in prefabricated building structures, particularly in cold regions, as an alternative to painted steel products. This allows for green production and industrial upgrading, meets environmental health needs, and does not cause pollution to the residential environment, making them suitable for use in building structures.
[0063] Finally, it should be noted that the above embodiments are intended only to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the embodiments, it should be understood by those skilled in the art that modifications or equivalent substitutions to the technical solutions of the present invention do not depart from the spirit and scope of the technical solutions of the present invention and are intended to be encompassed by the claims of the present invention.
Claims
1. A hot-rolled H-shaped steel for assembled building structure, characterized in that: The chemical composition of the hot-rolled H-beam is as follows by weight percentage: C: 0.03-0.05; Si: <0.15; Mn: 0.6~0.9; P: 0.030~0.045; S≤0.005; Cu: 0.20~0.35; Cr: 0.25~0.50; Ni: 0.20~0.50, Nb: 0.02~0.04, Ti: 0.01~0.025; Al: 0.005~0.015; Mo: 0.10~0.15, Cu / Ni≤1.0, Al+Ti≤0.03, As+Sn+Zn+Ca+Mg+B≤0.030, and the rest are Fe and unavoidable impurities.
2. The hot-rolled H-beam according to claim 1, characterized in that: In the hot-rolled H-shaped steel, As+Sn+Zn+Ca+Mg+B≤0.025, 0.003≤N≤0.007, 3≤Ti / N≤4, 0.7≤Cu / Ni≤1.
0.
3. A method for preparing hot-rolled H-shaped steel for assembled building structures, comprising the following steps: 1) Smelting process: a. Converter smelting; b. Refining; c. Continuous casting; 2) Rolling process: a. Heating control; b. Controlled rolling and controlled cooling: The finishing rolling process uses cooling before the finishing mill and cooling after the finishing mill; the finishing rolling process uses a cooling device for inter-pass cooling, the even-numbered rolling passes are cooled before the finishing mill, and the odd-numbered rolling passes are cooled after the finishing mill; c. Cooling bed cooling control.
4. The preparation method according to claim 3, characterized in that: In step 1), the arsenic and tin contents of the molten iron entering the converter are both less than 80ppm, and the final slag basicity is controlled within the range of 2.8-3.8; the slag is added 3 minutes before the end point, and the end point gun pressing time is ≥1 minute; 2.8-3.2kg / ton of silicon, calcium and barium are added during the steel tapping process for deoxidation, and alloys are evenly added when the molten steel is 1 / 4 to 3 / 8, and the addition is completed when the molten steel is 3 / 4 to 7 / 8; 6-10kg / t of synthetic slag is added during or after the steel tapping process; slag blocking operation is performed, and the steel tapping time is not less than 3 minutes.
5. The preparation method according to claim 3, characterized in that: In step 1), the refining is controlled by LF+VD, argon is blown at the bottom during the whole LF refining process, the soft blowing of argon for refining is more than 15 minutes, and 100-150m / furnace of high calcium wire is fed before the soft blowing of argon for refining; [O] in the steel discharged from LF refining is less than 10ppm; the temperature of the molten steel is controlled at 1590-1610°C at the end of LF refining; Slag is removed before the molten steel enters the VD furnace. The vacuum degree of VD refining is less than 70MPa, and the vacuum holding time is greater than 7 minutes. Bottom blowing nitrogen stirring is carried out throughout the VD refining process. The VD soft blowing time is greater than 10 minutes. The VD refining cycle is not less than 30 minutes. [O]<10ppm, 30ppm≤N≤70ppm in the steel leaving the VD refining station.
6. The preparation method according to claim 3, characterized in that: In step 1), continuous casting adopts a sleeve-type protection pouring process, secondary cooling adopts weak cooling, and the continuous casting speed is 0.8-0.9m / min; the superheat is controlled below 20°C; the smelted molten steel is cast into special-shaped billets; after the special-shaped billets are cast and formed, they enter the heating furnace, and the hot delivery temperature of the billets is controlled above 500°C.
7. The preparation method according to claim 3, characterized in that: Step 2) In the heating control, the temperature in the soaking stage is controlled at 1230-1260° C., and the heating time is 130-180 min.
8. The preparation method according to claim 3, characterized in that: Step 2) During controlled rolling and controlled cooling, the rough rolling process is mainly performed with the shape as the main pass, and the number of rolling passes is less than 9; The finishing rolling process is carried out with performance controlled rolling, the number of rolling passes is less than 7, the cumulative deformation rate of the rough rolling process is greater than 40%, and the deformation rate of the finishing rolling process is greater than 60%; the final rolling temperature of the finishing rolling is controlled between 780℃ and 830℃; when the temperature drops below 80℃, it enters the straightening machine for straightening.
9. The preparation method according to claim 3, characterized in that: Step 2) Cooling bed cooling control, During the final rolling to 700℃ section, the cooling rate of the rolled material is 2-5℃ / s; in the period below 700℃, the cooling rate of the rolled material is below 2℃ / s.
10. A cooling device, used in the preparation method according to any one of claims 3 to 9, characterized in that: The cooling device comprises: a front roller table (1) of a rolling mill, a skirt plate (2), a cooling water pipeline (3), an upper nozzle (4), a middle water nozzle (5), and a lower water nozzle (6); the skirt plates (2) on both sides of the rolling mill are arranged on the front roller table (1) of the rolling mill; the upper nozzle (4), the middle water nozzle (5), and the lower water nozzle (6) are respectively connected to the cooling water pipeline (3); the middle water nozzle (5) is used to cool the outer side of the flange, the upper nozzle (4) is used to cool the upper surface of the web and the upper side R angle part, and the lower water nozzle (6) is used to cool the lower web and the lower R angle part.
Citation Information
Patent Citations
High-performance hot-rolled H profile steel resisting atmosphere corrosion and preparation method thereof
CN105734406A
Rolled h-beam steel and production method therefor
CN109642296A
H-steel and method for manufacturing same
CN109715842A
Device and method for reducing web waves of hot-rolled H-shaped steel
CN113546959A
High-toughness hot-rolled H-shaped steel for building and preparation method thereof
CN115418559A