Recycling treatment method for waste wind turbine blade

Through the cutting, acid-decomposition reaction, soaking and calcining of waste wind power blades, the problems of low strength and morphology of recycling glass fibers are solved, and the recycling of high-purity and long-beam glass fibers is achieved, meeting its wide application needs , and reduces chemical reagent use and contamination.

WO2024234592A1PCT designated stage expired Publication Date: 2024-11-21CHINA ENERGY LONGYUAN ENVIRONMENTAL PROTECTION CO LTD

Patent Information

Application Number
PCT/CN2023/131350
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2023-11-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recycle glass fibers in waste wind power blades, resulting in low strength and damaged morphology of the recycled glass fibers, which cannot meet the needs of their wide application.

Method used

By cutting waste wind blades into blocks and mixing them with inorganic acid solution or metal salts, then soaking and calcining in organic solvents, the resin is gradually removed, the strength and form of glass fibers are retained, and finally soaked in fatty alcohols Improve dispersion and achieve high purity and bundled recycling of glass fibers.

Benefits of technology

Successfully recovered glass fiber bundle-like products with excellent strength and long length, with small loss of tensile strength, suitable for a wider range of industrial applications, and reduce the use of chemical reagents, avoiding high energy consumption and high pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023131350_21112024_PF_FP_ABST
    Figure CN2023131350_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the field of solid waste treatment. Disclosed is a recycling treatment method for a waste wind turbine blade. The method comprises the following steps: (1) cutting a waste wind turbine blade into blocks; (2) mixing the blocks with an inorganic acid solution for reaction, or mixing the blocks with a material A and a metal salt for reaction, and then filtering same; (3) soaking filter residue obtained in step (2) in an organic solvent, then filtering same, and collecting materials having a particle size ≥ 1.5 mm for calcination; and (4) soaking a calcined product obtained in step (3) in an aliphatic alcohol B and then filtering same. According to the described method, recycling treatment of waste wind turbine blades can be implemented. Moreover, a glass fiber product having excellent strength performance can be recovered. In addition, the appearance of recovered glass fiber can be better maintained, so that a glass fiber beam product having a wide range of subsequent applications is recovered.
Need to check novelty before this filing date? Find Prior Art

Description

Method for resource processing of discarded wind turbine blades

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Chinese patent application No. 202310556533.7 filed on May 17, 2023, the contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to the field of solid waste treatment, and in particular to a method for resource treatment of discarded wind turbine blades. Background Art

[0004] Glass fiber composites, commonly known as fiberglass reinforced plastics (GFRP), refer to materials made by reinforcing unsaturated polyester, epoxy resin, and phenolic resin with glass fiber. Glass fiber composites are widely used in various industries due to their low density and high strength. Wind turbine blades in wind turbines are their most important application area, and most wind turbine blades are currently made of glass fiber composites. However, wind turbine blades have a limited service life. As they age, replaced wind turbine blades and accidentally damaged blades accumulate in large quantities, posing a significant threat to the environment. At the same time, because discarded wind turbine blades contain certain environmentally harmful chemicals, traditional landfilling is not an option. Therefore, a large number of discarded wind turbine blades face the problem of recycling and disposal.

[0005] Currently, common recycling methods for discarded wind turbine blades fail to prioritize the strength of the recycled glass fiber, resulting in significant strength loss and a significant reduction in commercial value. Furthermore, because glass fiber and resin are interlaced and difficult to separate in discarded wind turbine blades, most current recycling methods rely on pulverizing the discarded blades to recover glass fiber powder, without prioritizing the morphology of the recovered glass fiber. However, glass fiber bundles generally have a wider range of applications than glass fiber powder.

[0006] In addition, bundled glass fibers have a wider range of industrial applications. However, during the recycling process of discarded wind turbine blades, the original bundled glass fibers are extremely easy to break, so what is usually recycled is glass fiber powder or smaller lengths.

[0007] Summary of the Invention

[0008] The purpose of the present invention is to overcome the problems existing in the prior art, such as the difficulty in recycling glass fibers from discarded wind turbine blades, the low strength of the recycled glass fibers, and the difficulty in recycling bundled glass fibers of longer lengths. A method for resource processing of discarded wind turbine blades is provided. This method can realize the resource processing of discarded wind turbine blades, and can also recycle glass fiber products with excellent strength performance, and can also better maintain the morphology of the recycled glass fibers, and recycle glass fiber bundle products with a wider range of subsequent applications.

[0009] In order to achieve the above-mentioned object, the present invention provides a method for recycling waste wind turbine blades, the method comprising the following steps:

[0010] (1) Cutting discarded wind turbine blades into blocks;

[0011] (2) mixing the block with an inorganic acid solution for reaction, or mixing the block with material A and a metal salt for reaction, followed by filtering;

[0012] (3) soaking the filter residue obtained in step (2) in an organic solvent, followed by filtering, collecting the material with a particle size of ≥1.5 mm and calcining;

[0013] (4) soaking the calcined product obtained in step (3) in fatty alcohol B, and then filtering;

[0014] The material A is selected from water, fatty alcohol A or organic acid.

[0015] Preferably, the conditions for reacting the block with the inorganic acid solution include: a temperature of 60-120° C. and a reaction time of 2-8 h;

[0016] Preferably, the inorganic acid solution is a sulfuric acid solution or a nitric acid solution;

[0017] Preferably, the liquid-to-solid ratio of the block when mixed with the inorganic acid solution for reaction is 3-8 mL:1 g;

[0018] Preferably, H + The concentration is ≥4mol / L.

[0019] Preferably, the conditions for reacting the block with material A and the metal salt include: a temperature of 120-250° C. and a time of 10-120 min;

[0020] Preferably, the liquid-to-solid ratio of the block when mixed with material A and metal salt for reaction is 1-40 mL:1 g;

[0021] Preferably, the metal salt is selected from one or more of zinc chloride, magnesium chloride, aluminum chloride and copper chloride;

[0022] Preferably, the organic acid is selected from acetic acid, propionic acid or butyric acid;

[0023] Preferably, the weight ratio of the metal salt to the discarded wind turbine blades is 0.05-0.3:1.

[0024] Preferably, the block is a cuboid, the length of the cuboid is 3-5 cm, the width of the cuboid is 3-5 cm, and the height of the cuboid is 0.1-0.6 cm.

[0025] Preferably, the fatty alcohol A and the fatty alcohol B are each independently selected from C1-C3 fatty alcohols;

[0026] Preferably, the C1-C3 fatty alcohol is selected from methanol, ethanol or propanol.

[0027] Preferably, in step (3), the soaking conditions include: temperature of 60-90° C. and time of 6-24 h.

[0028] Preferably, in step (3), the solid-liquid ratio during the soaking is 1 g:20-40 mL.

[0029] Preferably, the calcination conditions include: temperature of 200-400° C. and time of 20-60 min.

[0030] Preferably, the atmosphere during calcination is a mixture of oxygen and protective gas;

[0031] Preferably, the volume fraction of oxygen in the mixed gas is ≥40 vol%.

[0032] Preferably, in step (3), the organic solvent is selected from methanol, ethanol or diethyl ether.

[0033] Preferably, in step (4), the soaking conditions include: a temperature of 60-90° C. and a time of 10 min-120 min;

[0034] Preferably, the solid-liquid ratio during the soaking is 1g:10-40mL.

[0035] Preferably, the discarded wind turbine blades contain 65-85 wt% of glass fiber and 15-35 wt% of resin.

[0036] The method of the present invention involves cutting discarded wind turbine blades, subjecting them to acid hydrolysis or catalytic degradation to partially remove resin from the blades, then soaking the resulting product in an organic solvent. The resulting product is then subjected to oxygen-enriched calcination to further remove the resin from the discarded blades and improve the purity of the glass fiber in the recovered product. Finally, the calcined product is again soaked in a fatty alcohol to ensure the dispersibility of the recovered glass fiber. The method of the present invention removes the resin from the discarded wind turbine blades in multiple stages, without significantly compromising the morphology and strength of the glass fiber during the recycling process. The recovered glass fiber is in bundle form and is relatively long, reaching up to 12 mm in length, making it more commercially valuable than powdered glass fiber. Furthermore, the recovered glass fiber has a tensile strength of approximately 96% of that of the raw glass fiber. Furthermore, the recovered glass fiber product is highly pure and in the form of individually dispersed bundles, offering broader industrial application prospects.

[0037] In addition, the method described in the present invention can also avoid the complete use of chemical degradation to recycle the glass fibers in discarded wind turbine blades, reduce the use of chemical reagents, and avoid the resulting disadvantages such as high energy consumption and high pollution. The method described in the present invention is more green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] FIG1 is a photograph of the morphology of the glass fiber product recovered in Example 1 of the present invention. DETAILED DESCRIPTION

[0039] The following describes the specific embodiments of the present invention in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.

[0040] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0041] The present invention provides a method for recycling waste wind turbine blades, the method comprising the following steps:

[0042] (1) Cutting discarded wind turbine blades into blocks;

[0043] (2) mixing the block with an inorganic acid solution for reaction, or mixing the block with material A and a metal salt for reaction, followed by filtering;

[0044] (3) soaking the filter residue obtained in step (2) in an organic solvent, followed by filtering, collecting the material with a particle size of ≥1.5 mm and calcining;

[0045] (4) Soaking the calcined product obtained in step (3) in fatty alcohol B, and then filtering.

[0046] In the method of the present invention, the material A is selected from water, fatty alcohol A or organic acid.

[0047] In the method described in the present invention, the discarded wind turbine blades are blades that have expired their service life or have malfunctioned and been damaged during service. The discarded wind turbine blades are a composite material of glass fiber and resin. The glass fiber in the discarded wind turbine blades is originally in long bundles and is staggered and overlapped with the resin. The discarded wind turbine blades contain 65-85wt% glass fiber and 15-35wt% resin. The content of other components is extremely small and can be ignored, and the properties are not much different from those of the main components.

[0048] In the method of the present invention, in step (1), cutting the discarded wind turbine blades into blocks can increase the purity of the glass fiber subsequently recovered and avoid serious damage to the glass fiber morphology caused by crushing.

[0049] In a preferred embodiment, in order to further improve the yield of the obtained glass fiber, in step (1), the discarded wind turbine blades are cut into several cuboids, and the length of each of the cuboids is controlled to be 3-5 cm, the width of each of the cuboids is controlled to be 3-5 cm, and the height of each of the cuboids is controlled to be 0.1-0.6 cm.

[0050] In the method described in the present invention, in step (1), the size of the rectangular parallelepiped obtained by cutting the discarded wind turbine blades is not limited to the length of the rectangular parallelepiped being smaller than the width, and the relationship between the length, width and height of the rectangular parallelepiped is not particularly limited.

[0051] In a specific implementation, all blocks obtained by cutting discarded wind turbine blades need to be put into subsequent recycling processing.

[0052] In the method of the present invention, in step (2), all the cut blocks are subjected to an acid hydrolysis reaction in an inorganic acid solution, or the discarded wind turbine blades are reacted with material A and a metal salt to remove the resin in the discarded wind turbine blades. Preferably, the resin in the discarded wind turbine blades is removed by acid hydrolysis. In the present invention, by controlling the reaction conditions in step (2) to control the degree of degradation of the resin in the discarded wind turbine blades, it is possible to further avoid serious damage to the compressive strength of the glass fiber and breakage of the glass fiber due to excessive reaction, and further preserve the strength and length of the recovered glass fiber.

[0053] In the method of the present invention, to further maintain the properties of the recycled glass fiber, the conditions for mixing the block with the inorganic acid solution for reaction include: a temperature of 60-120°C and a reaction time of 2-8 hours, preferably 2-5 hours. Specifically, the temperature for mixing the block with the inorganic acid solution for reaction can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, or 120°C; and the reaction time can be 2 hours, 3 hours, 4 hours, 6 hours, or 8 hours.

[0054] In a preferred embodiment, the liquid-to-solid ratio of the block and the inorganic acid solution when mixed for reaction is 3-8 mL:1 g. Specifically, the liquid-to-solid ratio of the block and the inorganic acid solution when mixed for reaction can be 3 mL:1 g, 4 mL:1 g, 5 mL:1 g, 6 mL:1 g, 7 mL:1 g, or 8 mL:1 g.

[0055] In a specific embodiment, the inorganic acid solution is a sulfuric acid solution or a nitric acid solution.

[0056] In a preferred embodiment, the concentration of H+ in the inorganic acid solution is ≥4 mol / L, such as 4-9 mol / L.

[0057] In a further preferred embodiment, in step (2), when the block is mixed with the inorganic acid solution for reaction, when H + When the concentration of the inorganic acid solution is ≥8 mol / L, the block is mixed with the inorganic acid solution for a reaction time of 2-6 hours.

[0058] In the method described in the present invention, in step (2), after the block is mixed with an inorganic acid solution for reaction or the block is mixed with material A and a metal salt for reaction, flocculent material will appear in the reaction system, which is then filtered, and the obtained filter residue is then washed with water and soaked in an organic solvent.

[0059] In a specific embodiment, in step (2), the waste wind turbine blades are mixed with material A and metal salt to react so as to partially degrade the resin in the waste wind turbine blades, wherein the metal salt may act as a catalyst to promote the reaction between the waste wind turbine blades and material A in step (2).

[0060] In the method of the present invention, the metal salt is selected from one or more of zinc chloride, magnesium chloride, aluminum chloride and copper chloride, preferably selected from zinc chloride, aluminum chloride or copper chloride, and more preferably zinc chloride.

[0061] In a preferred embodiment, the organic acid is selected from acetic acid, propionic acid or butyric acid.

[0062] In a preferred embodiment, in order to further maintain the length and strength of the recycled glass fiber, the conditions for the reaction of the block with material A and the metal salt include: a temperature of 120-250°C and a reaction time of 10-120 minutes, preferably 30-90 minutes. Specifically, the temperature for the reaction of the block with material A and the metal salt can be 120°C, 150°C, 180°C, 200°C, 220°C or 250°C; and the reaction time of the block with material A and the metal salt can be 10 minutes, 30 minutes, 60 minutes, 90 minutes or 120 minutes.

[0063] In a preferred embodiment, the liquid-to-solid ratio of the block when mixed with material A and the metal salt for reaction is 1-40 mL:1 g, more preferably 5-20 mL:1 g. Specifically, the liquid-to-solid ratio of the block when mixed with material A and the metal salt for reaction can be 1 mL:1 g, 5 mL:1 g, 10 mL:1 g, 15 mL:1 g, 20 mL:1 g, 25 mL:1 g, 30 mL:1 g, 35 mL:1 g, or 40 mL:1 g.

[0064] In a preferred embodiment, in step (2), the weight ratio of the metal salt to the waste wind turbine blades is 0.05-0.3:1, more preferably 0.08-0.2:1. Specifically, the weight ratio of the metal salt to the waste wind turbine blades can be 0.05:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, 0.2:1, or 0.3:1.

[0065] In the method of the present invention, in step (3), the soaking conditions include: a temperature of 60-90°C and a soaking time of 6-24 hours, preferably 10-15 hours. Specifically, the soaking temperature can be 60°C, 70°C, 80°C or 90°C, and the soaking time can be 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 20 hours or 24 hours.

[0066] In a preferred embodiment, in order to further retain the strength and length of the recovered glass fiber, in step (3), the solid-liquid ratio during the soaking is 1 g:20-40 mL, preferably 1 g:25-35 mL. Specifically, the solid-liquid ratio during the soaking can be 1 g:20 mL, 1 g:25 mL, 1 g:30 mL, 1 g:35 mL or 1 g:40 mL.

[0067] In a specific embodiment, in step (3), the organic solvent is selected from methanol, ethanol or diethyl ether, preferably ethanol.

[0068] In a specific embodiment, in step (3), the specific operation of collecting materials with a particle size of ≥1.5 mm is: washing the filtered residue with water and drying it to a constant weight, then passing it through a special sieve with a pore size of 1.5 mm, and taking the material on the sieve.

[0069] In the method of the present invention, to further remove resin from discarded wind turbine blades, the filter residue obtained after soaking is subjected to oxygen-enriched calcination. Preferably, the present invention utilizes low-temperature calcination to maintain the morphology and strength of the resulting glass fiber as much as possible, thereby preventing damage to the morphology and strength of the glass fiber during the calcination process.

[0070] In a specific embodiment, in step (3), the calcination is performed in a flat-laying manner.

[0071] In a preferred embodiment, in step (3), the calcination conditions include: a temperature of 200-400°C, preferably 250-350°C; and a time of 20-60 minutes, preferably 25-40 minutes. Specifically, the calcination temperature can be 200°C, 250°C, 300°C, 350°C, or 400°C; and the calcination time can be 20 minutes, 30 minutes, 40 minutes, 50 minutes, or 60 minutes.

[0072] In the method of the present invention, in order to further increase the glass fiber content in the obtained glass fiber product, the atmosphere during the calcination is a mixture of oxygen and protective gas.

[0073] In a preferred embodiment, the volume fraction of oxygen in the mixed gas is ≥40 vol%, preferably 40-55 vol%.

[0074] In a specific embodiment, the protective gas in the mixed gas is selected from nitrogen, argon or helium, preferably nitrogen or argon.

[0075] In the method of the present invention, in step (4), the calcined product obtained in step (3) is placed in fatty alcohol B and soaked again to reduce the adhesion between the recovered glass fibers as much as possible. After the soaking, the product is filtered, and the filter residue is washed with water and dried to a constant weight to obtain a recovered glass fiber product.

[0076] In a specific embodiment, in step (4), the soaking conditions include: a temperature of 60-90°C and a soaking time of 10-120 minutes, preferably 10-60 minutes. Specifically, the soaking temperature can be 60°C, 70°C, 80°C or 90°C; and the soaking time can be 10 minutes, 30 minutes, 60 minutes, 90 minutes or 120 minutes.

[0077] In a preferred embodiment, in step (4), the solid-liquid ratio during the soaking is 1 g:10-40 mL. Specifically, the solid-liquid ratio during the soaking can be 1 g:10 mL, 1 g:20 mL, 1 g:30 mL or 1 g:40 mL.

[0078] In a specific embodiment, in step (4), the drying temperature is 90-105°C.

[0079] In the method of the present invention, the fatty alcohol A and the fatty alcohol B are independently selected from C1-C3 fatty alcohols.

[0080] In a preferred embodiment, the C1-C3 fatty alcohol is selected from methanol, ethanol or propanol, more preferably ethanol.

[0081] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.

[0082] The waste wind turbine blades processed in the following examples and comparative examples were from the Longyuan Electric Power Liaoning Power Plant.

[0083] Example 1

[0084] (1) Cutting discarded wind turbine blades (glass fiber content 65.45 wt%, resin content 34.55 wt%) into 251 cuboids (length 3-5 cm, width 3-5 cm, height 0.1-0.6 cm);

[0085] (2) All the cut cuboids were placed in a nitric acid solution (concentration of 5 mol / L) for acid hydrolysis reaction at 90°C for 3 h with a solid-liquid ratio of 1 g:5 mL. After the reaction was completed, the solid product was filtered and washed with water 3-5 times.

[0086] (3) the product obtained in step (2) was immersed in ethanol for 8 hours at a temperature of 80° C., with a solid-liquid ratio of 1 g:30 mL; after the immersion, the product was filtered, the filter residue was washed with water, and dried at 80° C. to a constant weight; the dried product was then passed through a special sieve with a pore size of 1.5 mm, and the sieve material was calcined at 320° C. for 30 minutes in a calcination atmosphere of a mixture of 50 vol% oxygen and 50 vol% nitrogen;

[0087] (4) Soaking the calcined product obtained in step (3) in ethanol at a soaking temperature of 80° C. for 30 min with a solid-liquid ratio of 1 g:10 mL. After the soaking, the obtained filter residue was washed with water 3-5 times and then dried at 95° C. to constant weight to obtain a glass fiber product.

[0088] Example 2

[0089] (1) Cutting discarded wind turbine blades (glass fiber content 67.82 wt%, resin content 32.18 wt%) into 262 cuboids (length 3-5 cm, width 3-5 cm, height 0.1-0.6 cm);

[0090] (2) In the presence of zinc chloride (the weight ratio of zinc chloride to waste wind turbine blades is 0.1:1), all the cut cuboids are mixed evenly with ethanol and reacted at a reaction temperature of 200°C, a reaction time of 60 min, and a solid-liquid ratio of 1 g:10 mL; after the reaction is completed, the reaction is filtered and the obtained solid product is washed with water 3-5 times;

[0091] (3) the product obtained in step (2) was immersed in ethanol for 9 h at a temperature of 85° C. and a solid-liquid ratio of 1 g:25 mL; after immersion, the product was filtered, the filter residue was washed with water, and dried at 80° C. to a constant weight; the dried product was passed through a special sieve with a pore size of 1.5 mm, and the sieve material was calcined at 300° C. for 30 min in a calcination atmosphere of a mixture of 45 vol% oxygen and 55 vol% nitrogen;

[0092] (4) Soaking the calcined product obtained in step (3) in ethanol at a soaking temperature of 60° C. for 40 min with a solid-liquid ratio of 1 g:15 mL. After the soaking, the obtained filter residue was washed with water 3-5 times and then dried at 95° C. to constant weight to obtain a glass fiber product.

[0093] Example 3

[0094] (1) Cutting discarded wind turbine blades (glass fiber content 71.45 wt %, resin content 28.55 wt %) into 245 cuboids (length 3-5 cm, width 3-5 cm, height 0.1-0.6 cm);

[0095] (2) In the presence of aluminum chloride (the weight ratio of aluminum chloride to waste wind turbine blades is 0.12:1), all the cut cuboids are mixed with acetic acid for reaction at a reaction temperature of 180°C, a reaction time of 80 min, and a solid-liquid ratio of 1 g:20 mL; after the reaction is completed, the reaction is filtered and the obtained solid product is washed with water 3-5 times;

[0096] (3) the product obtained in step (2) was immersed in ethanol for 10 h at a temperature of 70° C. and a solid-liquid ratio of 1 g:33 mL; after the immersion, the product was filtered, the filter residue was washed with water, and dried at 80° C. to a constant weight; the dried product was passed through a special sieve with a pore size of 1.5 mm, and the sieve material was calcined at 340° C. for 40 min in a calcination atmosphere of a mixture of 53 vol% oxygen and 47 vol% nitrogen;

[0097] (4) Soaking the calcined product obtained in step (3) in ethanol at a soaking temperature of 60° C. for 40 min with a solid-liquid ratio of 1 g:20 mL. After soaking, the obtained filter residue was washed with water 3-5 times and then dried at 95° C. to constant weight to obtain a glass fiber product.

[0098] Example 4

[0099] (1) Cutting discarded wind turbine blades (glass fiber content 66.8 wt%, resin content 33.2 wt%) into 232 cuboids (length 3-5 cm, width 3-5 cm, height 0.1-0.6 cm);

[0100] (2) All the cut cuboids were placed in a nitric acid solution (concentration of 5.5 mol / L) for acid hydrolysis reaction at 90°C for 4 h with a solid-liquid ratio of 1 g:8 mL. After the reaction was completed, the solid product was filtered and washed with water 3-5 times.

[0101] (3) soaking the product obtained in step (2) in ethanol for 8 hours at a temperature of 80° C. with a solid-liquid ratio of 1 g:30 mL; filtering the product after soaking, washing the filter residue with water, and drying the filter residue at 80° C. to a constant weight; passing the dried product through a special sieve with a pore size of 1.5 mm, and calcining the product under the sieve at 350° C. for 30 minutes in a calcination atmosphere of a mixture of 55 vol% oxygen and 45 vol% nitrogen;

[0102] (4) Soaking the calcined product obtained in step (3) in ethanol at a soaking temperature of 85° C. for 45 min with a solid-liquid ratio of 1 g:25 mL. After the soaking, the obtained filter residue was washed with water 3-5 times and then dried at 95° C. to constant weight to obtain a glass fiber product.

[0103] Example 5

[0104] The method described in Example 1 is followed, except that the cuboid cut in step (1) has a length of 2-3 cm, a width of 1-2 cm, and a height of 1-2 cm.

[0105] Example 6

[0106] The method described in Example 1 was followed, except that in step (3), the calcination temperature was set to 650°C.

[0107] Example 7

[0108] The method described in Example 1 was followed, except that in step (3), the calcination atmosphere was a mixture of 8 vol% oxygen and 92 vol% nitrogen.

[0109] Comparative Example 1

[0110] (1) Cutting discarded wind turbine blades (glass fiber content 65.45 wt%, resin content 34.55 wt%) into 251 cuboids (length 3-5 cm, width 3-5 cm, height 0.1-0.6 cm);

[0111] (2) All the cut cuboids were placed in a nitric acid solution (concentration of 5 mol / L) for acid hydrolysis reaction at 90°C for 10 h with a solid-liquid ratio of 1 g:12 mL. After the reaction was completed, the solid product was filtered and washed with water 3-5 times.

[0112] (3) Soaking the product obtained in step (2) in ethanol for 8 h at a temperature of 80° C. with a solid-liquid ratio of 1 g:30 mL; filtering the obtained residue after the soaking, washing the residue with water, and drying the residue at 95° C. to a constant weight to obtain a glass fiber product.

[0113] Comparative Example 2

[0114] (1) Cutting discarded wind turbine blades (glass fiber content 67.82 wt%, resin content 32.18 wt%) into 262 cuboids (length 3-5 cm, width 3-5 cm, height 0.1-0.6 cm);

[0115] (2) In the presence of zinc chloride (the weight ratio of zinc chloride to waste wind turbine blades is 0.4:1), all the cut cuboids are mixed evenly with ethanol and reacted at a reaction temperature of 200°C, a reaction time of 6 hours, and a solid-liquid ratio of 1g:10mL; after the reaction is completed, the reaction is filtered and the obtained solid product is washed with water 3-5 times;

[0116] (3) Soaking the product obtained in step (2) in ethanol for 8 h at a temperature of 80° C. with a solid-liquid ratio of 1 g:30 mL; filtering the obtained residue after the soaking, washing the residue with water, and drying the residue at 95° C. to a constant weight to obtain a glass fiber product.

[0117] Comparative Example 3

[0118] (1) Cutting discarded wind turbine blades (glass fiber content 71.45 wt %, resin content 28.55 wt %) into 245 cuboids (length 3-5 cm, width 3-5 cm, height 0.1-0.6 cm);

[0119] (2) In the presence of aluminum chloride (the weight ratio of aluminum chloride to waste wind turbine blades is 0.4:1), all the cut cuboids are mixed with acetic acid for reaction at a reaction temperature of 180°C, a reaction time of 4 hours, and a solid-liquid ratio of 1g:20mL; after the reaction is completed, the reaction is filtered and the obtained solid product is washed with water 3-5 times;

[0120] (3) Soaking the product obtained in step (2) in ethanol for 8 h at a temperature of 80° C. with a solid-liquid ratio of 1 g:30 mL; filtering the obtained residue after the soaking, washing the residue with water, and drying the residue at 95° C. to a constant weight to obtain a glass fiber product.

[0121] Comparative Example 4

[0122] (1) Cutting discarded wind turbine blades (glass fiber content 71.45 wt %, resin content 28.55 wt %) into 245 cuboids (length 3-5 cm, width 3-5 cm, height 0.1-0.6 cm);

[0123] (2) calcining all the obtained cuboids at 550°C for 4 h in a calcination atmosphere of a mixture of 55 vol% oxygen and 45 vol% nitrogen;

[0124] (3) Soaking the calcined product obtained in step (2) in ethanol at a soaking temperature of 60° C. for 30 min with a solid-liquid ratio of 1 g:10 mL. After the soaking, the filter residue was washed with water 3-5 times and then dried at 95° C. to constant weight to obtain a glass fiber product.

[0125] Test Case

[0126] Test Example 1

[0127] The macroscopic morphology of the glass fiber product recovered in Example 1 was observed, and the results are shown in FIG1 .

[0128] As shown in FIG1 , the glass fibers recovered by the method of the present invention are in the form of bundles with individual fibers distributed, indicating that the method of the present invention causes little damage to the morphology of the glass fibers and can successfully recover bundled glass fiber products.

[0129] Test Example 2

[0130] The tensile strength loss rate of the recycled glass fiber was tested.

[0131] Test method: The tensile strength of the glass fibers recovered from the Examples and Comparative Examples, as well as the tensile strength of the glass fiber raw materials, were tested according to ASTM C1557-2003, "Standard Test Method for Tensile Strength and Young's Modulus of Fibers." During the test, the length of the glass fibers to be tested was ensured to be equal to the length of the glass fiber raw materials. The tensile strength loss rate of the recovered glass fibers was calculated according to the following formula. The results are shown in Table 1.

[0132] Glass fiber tensile strength loss rate = (tensile strength of glass fiber raw material - tensile strength of recycled glass fiber) ÷ tensile strength of glass fiber raw material × 100%.

[0133] Test Example 3

[0134] The purity of the glass fibers in the glass fiber products recovered in the test examples and comparative examples, and the degradation rate of the resin in the products obtained after the reaction in step (2) in Examples 1-7 and Comparative Examples 1-3 were tested.

[0135] Glass fiber purity: Weigh the sample to be tested m1g, calcine the sample at 600℃ for 3h, collect the product, and weigh it as m2g. Calculate the purity of the recovered glass fiber product according to the formula: m2 / m1×100%. The results are shown in Table 1.

[0136] Resin degradation rate in step (2): The weight of all the rectangular blocks in step (2) is M g, where the content of the resin is W; the materials obtained in step (2) of Examples 1-7 and Comparative Examples 1-3 are vacuum dried at 80° C. to a constant weight of M1 g, and then calcined at 650° C. for 4 h, and then a calcined product M2 g is collected, where the weight of the resin in the material obtained in step (2) is (M1-M2) g. The degradation rate of the resin in the discarded wind turbine blades in step (2) is calculated according to the following formula, and the results are shown in Table 1;

[0137] In step (2), the resin degradation rate = [(M×W)-(M1-M2)] / (M×W)×100%.

[0138] Table 1

[0139] From the results in Table 1, it can be seen that the method described in the present invention can successfully process waste wind turbine blades for resource recovery, and the morphology of the recycled glass fiber is well maintained. Long bundled glass fiber products can be recycled, and the loss of tensile strength is small, which has a wider range of applications and higher value.

[0140] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.

Claims

1. A method for recycling waste wind turbine blades, characterized in that: The method comprises the following steps: (1) Cutting the discarded wind turbine blades into blocks; (2) mixing the block with an inorganic acid solution for reaction, or mixing the block with material A and a metal salt for reaction, followed by filtering; (3) soaking the filter residue obtained in step (2) in an organic solvent, filtering, collecting materials with a particle size of ≥1.5 mm and calcining; (4) soaking the calcined product obtained in step (3) in fatty alcohol B, and then filtering; The material A is selected from water, fatty alcohol A or organic acid; The conditions for mixing the block with the inorganic acid solution to react include: temperature of 60-120° C., time of 2-8 h; The conditions for reacting the block with material A and metal salt include: temperature of 120-250° C. and time of 10-120 min; The inorganic acid solution is a sulfuric acid solution or a nitric acid solution; The metal salt is selected from one or more of zinc chloride, magnesium chloride, aluminum chloride and copper chloride; The fatty alcohol A and the fatty alcohol B are each independently selected from methanol, ethanol or propanol; The organic acid is selected from acetic acid, propionic acid or butyric acid; The liquid-to-solid ratio of the block when mixed with material A and metal salt for reaction is 1-40 mL:1 g.

2. The method for recycling waste wind turbine blades according to claim 1, characterized in that: The liquid-to-solid ratio when the block is mixed with the inorganic acid solution for reaction is 3-8 mL:1 g; And / or, H + The concentration is ≥4mol / L.

3. The method for recycling waste wind turbine blades according to claim 1, characterized in that: The weight ratio of the metal salt to the waste wind turbine blades is 0.05-0.3:

1.

4. The method for recycling waste wind turbine blades according to claim 1, characterized in that: The block is a cuboid with a length of 3-5 cm, a width of 3-5 cm and a height of 0.1-0.6 cm.

5. The method for recycling waste wind turbine blades according to claim 1, characterized in that: In step (3), the soaking conditions include: temperature of 60-90°C and time of 6-24h.

6. The method for recycling waste wind turbine blades according to claim 1, characterized in that: In step (3), the solid-liquid ratio during the soaking is 1g:20-40mL.

7. The method for recycling waste wind turbine blades according to claim 1, characterized in that: The calcination conditions include: temperature of 200-400° C. and time of 20-60 min.

8. The method for recycling waste wind turbine blades according to claim 1, characterized in that: The calcining atmosphere is a mixture of oxygen and protective gas; And / or, the volume fraction of oxygen in the mixed gas is ≥40 vol%.

9. The method for recycling waste wind turbine blades according to claim 1, characterized in that: In step (3), the organic solvent is selected from methanol, ethanol or diethyl ether.

10. The method for recycling waste wind turbine blades according to claim 1, characterized in that: In step (4), the soaking conditions include: temperature of 60-90°C and time of 10 min-120 min; And / or, the solid-liquid ratio during the soaking is 1g:10-40mL.

Citation Information

Patent Citations

  • Method for recycling epoxy resins and glass fibre from non-metal powder of waste printed circuit board

    CN101407596A

  • Method for recycling wind power blade manufacturing mold through two steps in all-component mode

    CN110802101A

  • Waste wind power blade recovery method

    CN112024583A

  • Method for enriching glass fibers in waste wind turbine blade

    CN115447028A

  • Method for resourceful treatment of waste wind power blades

    CN116274253A

Cited By

  • Waste wind driven generator blade recycling system

    CN120115509A

  • Method for synergistically recovering glass fibers and preparing hard carbon negative electrode material based on retired blades

    CN121317697A

  • Cascade recycling method for all components of waste wind power blade, new material and application