Flame-retardant resin composition, preparation method therefor, and fiber-reinforced composite material
By controlling the ratio of polyisocyanate to epoxy resin and the curing accelerator content, a specific heterocyclic structure is formed, which solves the problems of flammability and poor processability of thermosetting resins, and achieves the low viscosity, rapid curing and high mechanical properties of flame retardant resins. Suitable for liquid forming processes of composite materials and meet high-level flame retardant grade requirements.
Patent Information
- Application Number
- PCT/CN2023/134827
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2023-11-28
- Publication Date
- 2024-11-21
AI Technical Summary
The existing thermosetting resin matrix is flammable, the traditional flame retardant is low in efficiency, high viscosity and poor processability, and cannot be suitable for liquid forming processes of composite materials, and the mechanical properties and heat resistance are insufficient.
The polyisocyanate and epoxy resin composition is used to control the ratio of isocyanate to epoxy groups and the content of curing accelerator to form a six-membered heterocyclic ring and an oxazolidinone five-membered heterocyclic structure, which improves flame retardant performance and Heat resistance, and at the same time adapt to the liquid forming process of composite materials.
The flame retardant resin composition is achieved with low viscosity, long operating cycle, fast curing and high mechanical properties, and the fiber reinforced composite material has excellent flame retardant properties and heat resistance, meeting the requirements of rail transit grades.
Smart Images

Figure PCTCN2023134827-FTAPPB-I100001 
Figure PCTCN2023134827-FTAPPB-I100002 
Figure PCTCN2023134827-FTAPPB-I100003
Abstract
Description
Flame retardant resin composition, preparation method thereof, and fiber-reinforced composite material
[0001] Cross-references
[0002] This application claims priority to Chinese application No. 202310550825X, filed on May 16, 2023. The contents of the above application are incorporated herein by reference. Technical Field
[0003] The present invention relates to the technical field of thermosetting resins, and in particular to a flame retardant resin composition, a preparation method thereof, and a fiber-reinforced composite material. Background Art
[0004] Since most thermosetting resin matrices are flammable and extremely prone to fire, their development has been limited. Traditional flame-retardant resin-based composites often utilize halogen-containing flame retardants, such as bromine-containing flame retardants. These solutions suffer from low flame retardant efficiency, high smoke density, and high smoke toxicity during combustion. While the addition of common powdered flame retardants, such as red phosphorus, metal hydrides, and ammonium polyphosphate, can achieve halogen-free and environmentally friendly flame retardancy, the high dosage increases the viscosity of the resin matrix, resulting in poor processability and unsuitability for wet-molding composite materials processes such as infusion, RTM, and pultrusion. Mechanical properties are also reduced, preventing the full utilization of the low-density, high-strength, and lightweight advantages of fiber-reinforced composites. While the use of liquid flame retardants, such as phosphonates and polyphosphonates, can achieve low-viscosity flame-retardant resin liquid molding composites, they suffer from low flame retardant efficiency and the significant plasticizing effect of large amounts of liquid flame retardants, resulting in reduced heat resistance and poor water resistance.
[0005] Chinese patent publication number CN104394985A discloses a polyisocyanate compound and an epoxy resin that are heated and cured under the action of lithium chloride (LiCl) catalyst to form a polymerized isocyanurate polymer. The polyisocyanate and resin composition has low viscosity, a long operating cycle, and high-temperature resistance of the cured product. However, the polyisocyanate trimerization is sensitive to moisture and easily foams. The cured product has a high degree of polymerization, poor toughness, and poor mechanical properties.
[0006] Chinese patent publication number CN104603173A discloses a polyisocyanate compound, an epoxy resin, and a polyol resin, which are heated and cured under the action of a boron trichloride n-octylamine (DY9577) catalyst to form a polymerized isocyanurate polymer, as well as a fiber-reinforced composite material prepared by an RTM process. The polyisocyanate, epoxy resin, and polyol resin composition has low viscosity, a long operating cycle, and high-temperature resistance of the cured product. The flame retardant properties of the glass fiber composite material can reach EN45545-2 R1 HL2 grade; however, the polyisocyanate trimerization cure is also sensitive to moisture and prone to foaming. The cured product has a high degree of polymerization, poor toughness, and poor mechanical properties.
[0007] Therefore, it is necessary to provide a new flame retardant resin composition and a preparation method thereof and a fiber reinforced composite material to solve the above-mentioned problems existing in the prior art.
[0008] Summary of the Invention
[0009] In order to comprehensively improve the flame retardant efficiency, process characteristics and mechanical properties of the resin composition and the molded composite material, the present application provides a flame retardant resin composition and a preparation method thereof and a fiber reinforced composite material.
[0010] The present invention provides a flame retardant resin composition, which adopts the following technical solution:
[0011] A flame retardant resin composition comprises a component A and a component B, wherein the component A comprises a polyisocyanate component and a curing accelerator component, wherein the polyisocyanate component comprises one or more polyisocyanates, each of which comprises at least two isocyanate groups; the component B comprises an epoxy resin component, wherein the ratio of the isocyanate groups in the polyisocyanate component to the epoxy groups in the epoxy resin component is (10-3):1; and the curing accelerator component accounts for 0.1-5.0% of the total amount of the polyisocyanate component and the epoxy resin component.
[0012] By adopting the above technical solution, the ratio of isocyanate groups to epoxy groups is controlled to be (10-3):1, and the curing accelerator component accounts for 0.1-5.0% of the total amount of the polyisocyanate component and the epoxy resin component, so that the flame retardant resin composition has a low initial viscosity of the mixture, a long viscosity doubling time, and a long operating pot life, thereby adapting to the composite material liquid molding process, having a long operating cycle at room temperature and being able to quickly cure and mold at medium and high temperatures (quickly gel at 140°C, with a gel time of 80-160 seconds); the excess isocyanate groups form an isocyanurate six-membered heterocyclic structure under the joint catalytic action of the curing accelerator component and the epoxy resin component, so that the flame retardant resin composition has good flame retardant properties; the epoxy groups react with the isocyanate groups to form an oxazolidinone five-membered heterocyclic structure, so that the flame retardant resin composition has good heat resistance (glass transition temperature Tg is 150-210°C) and mechanical properties, ultimately achieving a balanced improvement in the flame retardant properties, process characteristics, and mechanical properties of the flame retardant resin composition and its molded composite.
[0013] Optionally, the polyisocyanate includes at least one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, triphenylmethane triisocyanate and polymethylene polyphenyl isocyanate.
[0014] Optionally, the epoxy resin component includes at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, aliphatic epoxy resin, alicyclic epoxy resin, phenolic epoxy resin, toughened modified epoxy resin and phosphorus-containing modified epoxy resin.
[0015] Optionally, the curing accelerator component includes at least one of a boron amine complex, a boron alkyl tertiary amine, DBU and its salts, a quaternary ammonium salt, a quaternary phosphonium salt and an imidazole accelerator.
[0016] Optionally, the curing accelerator component includes at least one of trichloro(N,N-dimethyloctylamine)boron, curing agent 594, 1,8-diazabicyclo[5.4.0]undec-7-ene, DBU phenolate, DBU isooctanoate, tetrabutylammonium bromide, benzyltriphenylphosphonium chloride, 2-methylimidazole, 2-ethyl-4-methylimidazole and 2-phenyl-1-benzylimidazole.
[0017] Optionally, the flame retardant resin composition further comprises a flame retardant, and the flame retardant comprises a halogen-free flame retardant.
[0018] Optionally, the halogen-free flame retardant includes at least one of phosphate ester, polyphosphate ester, ammonium polyphosphate, diethyl aluminum hypophosphite, piperazine pyrophosphate, aluminum hydroxide, magnesium hydroxide and hydrated zinc borate.
[0019] Optionally, the flame retardant resin composition further comprises a toughening agent, and the toughening agent comprises at least one of a CTBN rubber toughening agent, a core-shell particle toughening agent, and a nanoparticle toughening agent.
[0020] Optionally, the flame retardant resin composition further comprises an auxiliary agent, wherein the auxiliary agent comprises at least one of a wetting agent, a defoaming agent and an internal release agent.
[0021] Another object of the present invention is to provide a method for preparing a flame retardant resin composition, comprising the following steps:
[0022] Preparation of component A: uniformly mixing the polyisocyanate component and the curing accelerator component to obtain component A;
[0023] Preparation of component B: Mix the epoxy resin components uniformly to obtain component B;
[0024] The component A and the component B are uniformly mixed to obtain the flame retardant resin composition, wherein the weight ratio of the component A to the component B is 100:(18-68).
[0025] Another object of the present invention is to provide a fiber-reinforced composite material comprising the flame retardant resin composition and reinforcing fibers, wherein the reinforcing fibers comprise at least one of carbon fibers, glass fibers, basalt fibers and aramid fibers.
[0026] Optionally, the flame retardant resin composition and the reinforcing fiber are subjected to a composite material molding process to prepare the fiber-reinforced composite material, and the composite material molding process includes any one of vacuum infusion, RTM, wet molding, HP-RTM and pultrusion.
[0027] In summary, this application includes at least one of the following beneficial technical effects:
[0028] 1. The flame retardant resin composition provided in the present application controls the ratio of isocyanate groups to epoxy groups and the proportion of the curing accelerator component to the total amount of the polyisocyanate component and the epoxy resin component, so that the flame retardant resin composition has a low initial viscosity, a long viscosity doubling time, and a long operating period, thereby adapting to the liquid molding process of the composite material, having a long operating cycle at room temperature and rapid curing molding at medium and high temperatures; the excess isocyanate groups form an isocyanurate six-membered heterocyclic structure under the joint catalytic action of the curing accelerator component and the epoxy resin component, so that the flame retardant resin composition has good flame retardant properties; the epoxy group reacts with the isocyanate group to form an oxazolidinone five-membered heterocyclic structure, so that the flame retardant resin composition has good heat resistance (glass transition temperature Tg is 150~210℃) and mechanical properties, ultimately achieving a balanced improvement in the flame retardant properties, process characteristics and mechanical properties of the flame retardant resin composition.
[0029] 2. The flame retardant resin composition provided in the present application can flexibly adjust the operation time and curing efficiency of the flame retardant resin composition by compounding the curing accelerator and adjusting the proportion of the curing accelerator, and control the proportion of the generated isocyanurate six-membered heterocyclic structure (polyisocyanate trimer, sensitive to moisture) and oxazolidone five-membered heterocyclic structure. No special process is required to pre-dehydrate the reinforcing fiber. The flame retardant resin composition and the reinforcing fiber are vacuum infused to obtain a fiber-reinforced composite material. The fiber-reinforced composite material is not easy to foam, and will not have defects such as lack of glue and delamination, which can effectively improve the molding quality and efficiency of the fiber-reinforced composite material.
[0030] 3. This application further introduces halogen-free flame retardants to achieve high-efficiency flame retardant performance of the flame retardant resin composition, and the flame retardant performance of the fiber-reinforced composite material can reach EN45545-2 R1 HL3 level, meeting the highest FST flame retardant grade requirements for rail transit composite materials.
[0031] 4. The flame retardant resin composition provided in this application has the advantages of low viscosity and excellent processability. It is suitable for the preparation of fiber-reinforced composite materials by a variety of composite material liquid molding processes, and the obtained fiber-reinforced composite materials have excellent mechanical properties. The composite material liquid molding process includes any one of vacuum infusion, RTM, wet molding, HP-RTM, and pultrusion processes. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with ordinary skills in the field to which the invention belongs. The words "including" and similar words used in this article mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0033] An embodiment of the present invention provides a flame retardant resin composition, comprising a component A and a component B, wherein the component A comprises a polyisocyanate component and a curing accelerator component, the polyisocyanate component comprises one or more polyisocyanates, and the polyisocyanate comprises at least two isocyanate groups; the component B comprises an epoxy resin component, and the ratio of the isocyanate groups in the polyisocyanate component to the epoxy groups in the epoxy resin component is (10-3):1; the curing accelerator component accounts for 0.1-5.0% of the total amount of the polyisocyanate component and the epoxy resin component.
[0034] Specifically, by adopting the above technical solution, the ratio of isocyanate groups to epoxy groups is controlled to be (10-3):1, and the curing accelerator component accounts for 0.1-5.0% of the total amount of the polyisocyanate component and the epoxy resin component, so that the flame retardant resin composition has a low initial viscosity of the mixture, a long viscosity doubling time, and a long working life, thereby being suitable for the liquid molding process of the composite material, having a long operating cycle at room temperature and being able to quickly cure and mold at medium and high temperatures (quickly gel at 140°C, with a gel time of 80-160 seconds); the excess isocyanate groups form an isocyanurate six-membered heterocyclic structure under the joint catalytic action of the curing accelerator component and the epoxy resin component, so that the flame retardant resin composition has good flame retardant properties; the epoxy groups react with the isocyanate groups to form an oxazolidinone five-membered heterocyclic structure, so that the flame retardant resin composition has good heat resistance (glass transition temperature Tg is 150-210°C) and mechanical properties, ultimately achieving a balanced improvement in the flame retardant properties of the flame retardant resin composition, process characteristics, and mechanical properties of the molded composite material.
[0035] In some embodiments of the present invention, the polyisocyanate includes at least one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, triphenylmethane triisocyanate and polymethylene polyphenyl isocyanate. In some specific embodiments, the CAS number of the toluene diisocyanate is 26471-62-5; the CAS number of the isophorone diisocyanate is 4098-71-9; the CAS number of the diphenylmethane diisocyanate is 101-68-8; the CAS number of the dicyclohexylmethane diisocyanate is 5124-30-1; the CAS number of the hexamethylene diisocyanate is 822-06-0; the CAS number of the lysine diisocyanate is 45172-15-4; the CAS number of the triphenylmethane triisocyanate is 2422-91-5; and the CAS number of the polymethylene polyphenyl isocyanate is 9016-87-9.
[0036] In some specific embodiments of the present invention, the epoxy resin component includes at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, aliphatic epoxy resin, alicyclic epoxy resin, phenolic epoxy resin, toughened modified epoxy resin and phosphorus-containing modified epoxy resin.
[0037] In some embodiments of the present invention, the curing accelerator component includes at least one of a boron amine complex, a boron alkyl tertiary amine, DBU and its salts, a quaternary ammonium salt, a quaternary phosphonium salt, and an imidazole accelerator.
[0038] In some embodiments of the present invention, the curing accelerator component includes at least one of trichloro(N,N-dimethyloctylamine)boron, curing agent 594, 1,8-diazabicyclo[5.4.0]undec-7-ene, DBU phenolate, DBU isooctanoate, tetrabutylammonium bromide, benzyltriphenylphosphonium chloride, 2-methylimidazole, 2-ethyl-4-methylimidazole, and 2-phenyl-1-benzylimidazole.
[0039] In some embodiments of the present invention, the flame retardant resin composition further comprises a flame retardant, and the flame retardant comprises a halogen-free flame retardant.
[0040] In some embodiments of the present invention, the halogen-free flame retardant includes at least one of phosphate ester, polyphosphate ester, ammonium polyphosphate, diethyl aluminum hypophosphite, piperazine pyrophosphate, aluminum hydroxide, magnesium hydroxide and hydrated zinc borate.
[0041] In some embodiments of the present invention, the flame retardant resin composition further comprises a toughening agent, and the toughening agent comprises at least one of a CTBN rubber toughening agent, a core-shell particle toughening agent, and a nanoparticle toughening agent.
[0042] By adding toughening agent, the brittleness of flame retardant resin composition is improved and the tensile strength, flexural strength and impact strength are improved. The impact strength of flame retardant resin composition reaches 20KJ / m 2 above.
[0043] In some embodiments of the present invention, the flame retardant resin composition further comprises an auxiliary agent, wherein the auxiliary agent comprises at least one of a wetting agent, a defoaming agent, and an internal release agent.
[0044] An embodiment of the present invention provides a method for preparing a flame retardant resin composition, comprising the following steps:
[0045] Preparation of component A: uniformly mixing the polyisocyanate component and the curing accelerator component to obtain component A;
[0046] Preparation of component B: Mix the epoxy resin components uniformly to obtain component B;
[0047] The component A and the component B are uniformly mixed to obtain the flame retardant resin composition, wherein the weight ratio of the component A to the component B is 100:(18-68).
[0048] An embodiment of the present invention provides a fiber-reinforced composite material, comprising the flame-retardant resin composition and reinforcing fibers, wherein the reinforcing fibers comprise at least one of carbon fibers, glass fibers, basalt fibers, and aramid fibers.
[0049] In some embodiments of the present invention, the flame retardant resin composition and the reinforcing fiber are subjected to a composite material molding process to produce the fiber-reinforced composite material, and the composite material molding process includes any one of vacuum infusion, RTM, wet molding, HP-RTM and pultrusion.
[0050] The fiber-reinforced composite material prepared using the flame-retardant resin composition has good mechanical properties and excellent flame retardant properties, and can meet the flame retardant grade requirements of EN45545-2 R1 HL2 and above for rail transit.
[0051] The technical solutions of the embodiments of the present invention are described in detail below through specific examples.
[0052] Example
[0053] The raw materials used in the examples include polyisocyanate, epoxy resin, curing accelerator, halogen-free flame retardant, toughening agent and auxiliary agent.
[0054] Polyisocyanates: Wanhua's liquefied MDI-100L, carbodiimide-uretonimine modified 4,4'-diphenylmethane diisocyanate; BASF's MM 103C, a modified isocyanate based on diphenylmethane diisocyanate; Desmodur 44V20L, polymethylene polyphenylene isocyanate.
[0055] Epoxy resins: Nanya Electronic Materials (Kunshan) Co., Ltd. NPEL-127: low viscosity liquid bisphenol A epoxy resin, epoxy equivalent weight: EEW = 175 ~ 185g / eq., 25 ° C viscosity: 8000 ~ 12000mPa.s; Nanya Electronic Materials (Kunshan) Co., Ltd. NPEL-128: low viscosity liquid bisphenol A epoxy resin, epoxy equivalent weight: EEW = 184 ~ 190g / eq., 25 ° C viscosity: 12000 ~ 15000mPa.s; Nanya Plastics Industry Co., Ltd. NPEF-170: low viscosity liquid bisphenol F epoxy resin, epoxy equivalent weight: EEW = 184 ~ 190g / eq., 25 ° C viscosity: 12000 ~ 15000mPa.s Oxygen equivalent: EEW = 160 ~ 180 g / eq., viscosity at 25 ° C: 2000 ~ 5000 mPa.s; XY622: 4-butanediol diglycidyl ether, a long-chain difunctional epoxy reactive diluent; homemade DPO-170 resin: phosphorus-containing reactive flame retardant diphenylphosphine oxide (DPO) reacts with bisphenol F epoxy resin NPEF-170 to prepare phosphorus-modified epoxy resin, phosphorus content 4.60%, epoxy equivalent: EEW = 330 g / eq., viscosity at 40 ° C: 30000 mPa.s; polyurethane-modified epoxy resin EPU-253: complex high-tech material.
[0056] Curing accelerator: trichloro(N,N-dimethyloctylamine)boron, purchased from Huntsman DY9577; tertiary boroalkylamine, curing agent 594; 1,8-diazabicyclo[5.4.0]undec-7-ene, abbreviated as DBU in English; DBU phenolate; tetrabutylammonium bromide, abbreviated as TBAB in English; 2-ethyl-4-methylimidazole, abbreviated as 2E4MZ in English, purchased from Shikoku Chemicals Co., Ltd. of Japan.
[0057] Halogen-free flame retardants: FR-1035: phosphate flame retardant; F-229: phenyl polyphosphate; WSFR-RDP: diphenyl phosphate flame retardant; ATH-105EP: aluminum hydroxide flame retardant; OP 935: diethyl aluminum hypophosphite, white powder, particle size D50: ≤5μm.
[0058] Toughening agent: Japan Zhongyuan Chemical core-shell toughening agent MZ-100.
[0059] Additives: silane coupling agent, fiber sizing agent, defoaming agent, internal release agent are all commonly used functional additives, and commercially available conventional products can be selected.
[0060] The flame retardant resin composition and the fiber reinforced composite semi-cured material of the present invention were tested for performance, and the test method was as follows:
[0061] The viscosity of the flame retardant resin composition at 25° C. was measured using a TA DHR20 rheometer.
[0062] The gelation time of 1.0 g of the flame retardant resin composition at 140±1° C. was tested using a gelation time tester.
[0063] The thermal gravimetric loss curve of the cured product of the flame retardant resin composition in air atmosphere was measured using a TGA thermal gravimetric loss tester.
[0064] The glass transition temperature Tg of the cured product of the flame retardant resin composition was measured using a DSC (TA DSC X3) method according to GB / T 19466-2004.
[0065] The tensile strength, tensile modulus and elongation at break of the cured flame retardant resin composition were determined using an electronic universal tensile testing machine based on ISO 527-2.
[0066] The Charpy impact strength of the cured product of the flame retardant resin composition was measured using a Charpy impact testing machine based on ISO 179-1 standard.
[0067] The tensile strength and modulus of flame retardant resin composition fiber reinforced composite materials are tested using the test method of an electronic universal tensile testing machine based on ISO 527-4 standard.
[0068] The interlaminar shear strength of fiber-reinforced composite materials of flame-retardant resin compositions was tested using an electronic universal tensile testing machine based on ISO 14130 standard.
[0069] The heat release rate of the flame retardant resin composition fiber reinforced composite material was tested using a cone calorimeter test method based on ISO 5660-1 standard.
[0070] The smoke density of fiber-reinforced composite materials made of flame-retardant resin compositions is tested using the smoke density chamber test method based on EN ISO 5659-2 standard.
[0071] Example 1
[0072] Preparation of component A:
[0073] Preheat a mixing device to 50° C., add 98 parts of polyisocyanate MDI-100L and 2 parts of curing accelerator DY9577 into the mixing device and mix well to obtain component A.
[0074] Preparation of component B:
[0075] 80 parts of bisphenol A epoxy resin NPEL-127 and 20 parts of bisphenol F epoxy resin NPEF-170 were added to a mixing device and mixed uniformly to obtain component B.
[0076] Preparation of flame retardant resin composition:
[0077] Component A and component B were added into a mixing device in a weight ratio of 100:18 and mixed evenly to obtain a flame retardant resin composition.
[0078] Component A was tested using a TA DHR20 rheometer, and the viscosity of component A at 25°C was 28.7 mPa.s.
[0079] 300 g of component A was placed in a sealed PET transparent plastic cup and placed in a 50°C oven. Component A was taken out every two days and the viscosity of component A at 25°C was tested using a TA DHR20 rheometer. The time it took for the viscosity to reach twice the initial viscosity was defined as the viscosity doubling time, which was used to confirm the storage stability of component A. The viscosity doubling time for component A was tested to be 6 days.
[0080] Component B was tested using a TA DHR20 rheometer, and the viscosity of component B at 25°C was 7210 mPa.s.
[0081] The flame retardant resin composition was tested using a TA DHR20 rheometer. The viscosity of the flame retardant resin composition at 25° C. was 155.7 mPa·s.
[0082] 300 g of the evenly mixed flame retardant resin composition was placed in a sealed PET transparent plastic cup and placed in a 25°C oven. The flame retardant resin composition was taken out every hour and the viscosity of the flame retardant resin composition at 25°C was tested using a TA DHR20 rheometer. The time it took for the viscosity to reach twice the initial viscosity was the viscosity doubling time, which was used to confirm the operational applicability of the flame retardant resin composition. The viscosity doubling time of the tested flame retardant resin composition was 8 hours.
[0083] The gel time of the flame retardant resin composition tested by a gel time tester at 140° C. was 80 seconds.
[0084] Preparation of flame retardant resin composition cured product: The flame retardant resin composition is vacuum degassing and cast into resin tensile and impact test strips based on the requirements of GB / T2567-2008 standard, and then cured at 100°C for 2 hours, at 140°C for 2 hours, and at 180°C for 3 hours to obtain a flame retardant resin composition cured product.
[0085] Based on the determination method using DSC (TA DSC Q2000) in GB / T 19466-2004, the glass transition temperature Tg of the cured product of the flame retardant resin composition was measured to be 190.2°C.
[0086] Based on the ISO 527-2 standard, the tensile strength of the flame retardant resin composition cured product was measured using an electronic universal tensile testing machine, and the tensile modulus was 53.0 MPa, the tensile modulus was 3.97 GPa, and the elongation at break was 1.45%. Based on the GBT 1043.1 standard, the simple supported beam impact tester was used to measure the simple supported beam unnotched impact strength of the flame retardant resin composition cured product, and the unnotched impact strength was 5.89 kJ / m 2 .
[0087] Examples 2 to 8
[0088] The preparation method of the flame retardant resin composition and the preparation method of the flame retardant resin composition cured product are the same as in Example 1. The weight parts of the raw materials of each component of the flame retardant resin composition are detailed in Table 1; the viscosity test and gel time test of the flame retardant resin composition, the glass transition temperature Tg test of the flame retardant resin composition cured product, the tensile property test and impact strength test method of the flame retardant resin composition cured product are the same as in Example 1, and the test results are detailed in Table 1.
[0089] Table 1
[0090] Example 7
[0091] Preparation of component A:
[0092] Preheat a mixing device to 50° C., add 99 parts of polyisocyanate 44V20L and 1 part of curing accelerator DY9577 into the mixing device and mix well to obtain component A.
[0093] Preparation of component B:
[0094] 99.5 parts of bisphenol F epoxy resin NPEF-170 and 0.5 parts of boron alkyl tertiary amine curing agent 594 were added to a mixing device and mixed uniformly to obtain component B.
[0095] Preparation of flame retardant resin composition:
[0096] Component A and component B were added into a mixing device in a weight ratio of 100:20 and mixed evenly to obtain a flame retardant resin composition.
[0097] Component A was tested using a TA DHR20 rheometer, and the viscosity of component A at 25°C was 254 mPa.s.
[0098] Component B was tested using a TA DHR20 rheometer, and the viscosity of component B at 25°C was 3990 mPa.s.
[0099] 300 g of component B was placed in a sealed PET transparent plastic cup and placed in a 50°C oven. Component B was taken out every two days and the viscosity of component B at 25°C was tested using a TA DHR20 rheometer. The time it took for the viscosity to reach twice the initial viscosity was defined as the viscosity doubling time, which was used to confirm the storage stability of component B. The viscosity doubling time for component B was tested for 30 days.
[0100] The flame retardant resin composition was tested using a TA DHR20 rheometer. The viscosity of the flame retardant resin composition at 25° C. was 365 mPa·s.
[0101] The gel time of the flame retardant resin composition tested by a gel time tester at 140° C. was 115 seconds.
[0102] Preparation of flame retardant resin composition cured product: The flame retardant resin composition is vacuum degassing and cast into resin tensile and impact test strips based on the requirements of GB / T2567-2008 standard, and then cured at 100°C for 2 hours, at 140°C for 2 hours, and at 180°C for 3 hours to obtain a flame retardant resin composition cured product.
[0103] Based on the determination method using DSC (TA DSC Q2000) in GB / T 19466-2004, the glass transition temperature Tg of the cured product of the flame retardant resin composition was measured to be 186.3°C.
[0104] Examples 8 to 12
[0105] The preparation method of the flame retardant resin composition and the preparation method of the flame retardant resin composition cured product are the same as in Example 7. The weight parts of the raw materials of each component of the flame retardant resin composition are detailed in Table 2; the viscosity test, gel time test and glass transition temperature Tg test method of the flame retardant resin composition cured product are the same as in Example 7. The test results are detailed in Table 2.
[0106] Table 2
[0107] Note: DL-400 is a polyether polyol with CAS number 25322-69-4, purchased from Guangzhou Yinhuan Chemical Co., Ltd.
[0108] Example 13
[0109] Preparation of component A:
[0110] Preheat a mixing device to 50° C., add 99 parts of polyisocyanate 44V20L and 1 part of curing accelerator DY9577 into the mixing device and mix well to obtain component A.
[0111] Preparation of component B:
[0112] 50 parts of bisphenol A bisphenol F epoxy resin NPEF-170 and 50 parts of diphenyl phosphate flame retardant (also known as resorcinol flame retardant) WSFR-RDP were added to a mixing device and mixed evenly to obtain component B.
[0113] Preparation of flame retardant resin composition:
[0114] Component A and component B were added into a mixing device in a weight ratio of 100:40 and mixed evenly to obtain a flame retardant resin composition.
[0115] Component A was tested using a TA DHR20 rheometer, and the viscosity of component A at 25°C was 252 mPa.s.
[0116] Component B was tested using a TA DHR20 rheometer. The viscosity of component B at 25° C. was 1301 mPa.s.
[0117] The flame retardant resin composition was tested using a TA DHR20 rheometer. The viscosity of the flame retardant resin composition at 25° C. was 328 mPa.s.
[0118] The gel time of the flame retardant resin composition tested by a gel time tester at 140° C. was 175 seconds.
[0119] Preparation of flame retardant resin composition cured product: The flame retardant resin composition was vacuum degassing and cast into resin tensile and impact test strips based on the requirements of GB / T2567-2008 standard, and then cured at 70°C for 2 hours, at 110°C for 2 hours, and at 150°C for 3 hours to obtain a resin composition cured product.
[0120] Based on the determination method using DSC (TA DSC Q2000) in GB / T 19466-2004, the Tg of the cured product of the flame retardant resin composition was measured to be 187°C.
[0121] The thermal gravimetric loss curve of the flame retardant resin composition cured product in air atmosphere was measured using a TGA thermal gravimetric tester. The test conditions were: 40-800°C, a temperature rise rate of 10°C / min, and the residual weight at 650°C was measured to be 18.6%, that is, the residual carbon rate at 650°C was 18.6%.
[0122] Based on the ISO 527-2 standard, the tensile strength of the flame retardant resin composition cured product was measured using an electronic universal tensile testing machine, and the tensile modulus was 57.3 MPa, the tensile modulus was 3.47 GPa, and the elongation at break was 2.05%. Based on the GBT 1043.1 standard, the simple supported beam impact tester was used to measure the simple supported beam unnotched impact strength of the flame retardant resin composition cured product, and the impact strength was 6.5 kJ / m 2.
[0123] Examples 14 to 17
[0124] The preparation method of the flame retardant resin composition and the preparation method of the flame retardant resin composition cured product are the same as those in Example 13. The weight parts of the raw materials of each component of the flame retardant resin composition are detailed in Table 4; the viscosity test and gel time test of the flame retardant resin composition, the glass transition temperature Tg test of the flame retardant resin composition cured product, the 650°C residual carbon rate test, the tensile property test and impact strength test method of the flame retardant resin composition cured product are the same as those in Example 13. The test results are detailed in Table 4.
[0125] Table 4
[0126] In Examples 1 to 17, polyisocyanate and epoxy resin undergo hybridization reaction under the promotion of a curing accelerator to obtain a flame retardant resin composition, and both component A and component B are storage-stable. The flame retardant resin composition has a low initial viscosity of the mixture, a long viscosity doubling time, and a long operating applicable period, and is suitable for a composite material liquid molding process. The composite material liquid molding process includes any one of vacuum infusion, RTM, wet molding, HP-RTM, and pultrusion processes; and the flame retardant resin composition can quickly gel at 140°C, with a gel time of 80 to 160 seconds. The flame retardant resin composition has the advantage of rapid curing and molding. By compounding the curing accelerator and adjusting the proportion of the curing accelerator, the operating time and curing efficiency of the flame retardant resin composition can be flexibly adjusted, which can effectively improve the molding efficiency of fiber-reinforced composite materials. Polyisocyanate and epoxy resin are co-cured. The isocyanate groups in the excess polyisocyanate, under the action of a curing accelerator and epoxy catalysis, form a six-membered isocyanurate heterocyclic structure, which exhibits excellent flame retardancy. The epoxy groups react with the isocyanate groups to form a five-membered oxazolidone heterocyclic structure, which exhibits excellent heat resistance and mechanical properties. The flame-retardant resin composition has excellent processing characteristics, rapid curing and molding, and high-temperature resistance. The glass transition temperature (Tg) of the flame-retardant resin composition is 150-210°C. The fiber-reinforced composite material prepared using the flame-retardant resin composition has good mechanical properties and excellent flame retardancy, meeting the flame retardancy grade requirements of EN45545-2 R1 HL2 and above for rail transit.
[0127] In Comparative Examples 1 to 5, the curing accelerator component used is not latent. Although the curing accelerator component can promote the hybridization reaction between the polyisocyanate component and the epoxy resin component, it is impossible to prepare a storage-stable component A or component B. At the same time, after mixing component A and component B, a flame retardant resin composition is obtained. The viscosity of the flame retardant resin composition doubles in a short time, the operating applicable period is short, and it is not suitable for the liquid molding process of the composite material; in Comparative Example 4, the weight ratio of component A to component B is 100:135, indicating that when the isocyanate group is not excessive, the viscosity of the flame retardant resin composition will increase, the gel time at 140°C will be shortened, and the glass transition temperature Tg of the flame retardant resin composition will be reduced; when polyether polyol DL-400 is added to Comparative Example 5, polyurethane will be generated inside the flame retardant resin composition, thereby reducing the heat resistance of the flame retardant resin composition.
[0128] The flame-retardant resin composition of the present invention features storage stability, flexible and adjustable operating cycles, and rapid high-temperature curing and molding. It also exhibits excellent flame retardancy, a high carbonization rate, a low heat release rate, low smoke emissions, and low smoke toxicity. When applied to fiber-reinforced composite materials, the resulting composites possess excellent mechanical properties and heat resistance, while also meeting the flame retardancy requirements of materials used in the rail transit and aviation sectors.
[0129] Application Example 1
[0130] Preparation of flame retardant pultruded fiberglass sheets
[0131] Component A and component B were prepared according to the proportions of the flame retardant resin composition in Example 7.
[0132] Preheat the mixing device to 50°C, weigh 29.7 kg of polyisocyanate 44V20L and 0.3 kg of curing accelerator DY9577, add the polyisocyanate 44V20L and curing accelerator DY9577 to the mixing device and mix evenly to obtain component A; weigh 19.9 kg of bisphenol F epoxy resin NPEF-170 and 0.1 kg of borax tertiary amine curing agent 594, add the bisphenol F epoxy resin NPEF-170 and borax tertiary amine curing agent 594 to the mixing device and mix evenly to obtain component B; before use, add 1.0 kg of INT1948 internal release agent to component B and mix evenly to obtain component B1.
[0133] Component A and component B1 were added to storage tanks A and B of a two-component automatic glue mixer, respectively. The mixed weight ratio of tanks A and B in the mixer was set to 100:21, the glue injection flow rate was 90 g / min, and the mixed resin was connected to the glue injection port of a 150 mm × 5 mm glue injection box pultrusion mold; the heating temperatures of the three zones of the mold were set to 130°C, 160°C, and 180°C, 530 2400 tex glass fiber yarns were inserted into the mold, and the pultrusion speed was set to 20 cm / min; the pultrusion production line and the automatic glue mixer were started to carry out the pultrusion process to prepare the flame-retardant sheet, and a flame-retardant pultruded glass fiber sheet with a smooth and flat appearance and light yellow color was obtained.
[0134] Based on the ISO 5660-1 standard and the cone calorimeter test method, six heat release rate test pieces with a length of 100 mm, a width of 100 mm, and a thickness of 5 mm were prepared to test the heat release rate of the flame retardant pultruded glass fiber sheet. The maximum average heat release rate (MARHE) was measured to be 65.0 KW / m 2 .
[0135] Based on the EN ISO 5659-2 standard and the smoke density chamber test method, six heat release rate test pieces with a length of 75 mm, a width of 75 mm, and a thickness of 5 mm were prepared to test the smoke density of the flame retardant pultruded glass fiber board. The smoke density DS4 in the fourth minute was 41.3, and the cumulative total of the smoke density in the first four minutes, VOF4, was 255.3.
[0136] The heat release rate and smoke density of the flame-retardant pultruded fiberglass sheet meet the flame-retardant grade requirements of EN45545-2R1HL2 for rail transit.
[0137] Application Example 2
[0138] Preparation of vacuum infusion flame retardant carbon fiber sheets
[0139] Component A and component B were prepared according to the proportions of the flame retardant resin composition in Example 13.
[0140] Preheat the mixing device to 50°C, weigh 980g of polyisocyanate 44V20L and 20g of curing accelerator DY9577, add the polyisocyanate 44V20L and curing accelerator DY9577 to the mixing device and mix evenly to obtain component A; weigh 495g of bisphenol F epoxy resin NPEF-170, 5g of tetrabutylammonium bromide TBAB and 500g of F-229 flame retardant, add the bisphenol F epoxy resin NPEF-170, tetrabutylammonium bromide TBAB and F-229 flame retardant to the mixing device and mix evenly to obtain component B.
[0141] Component A and component B are evenly mixed in a weight ratio of 100:40 to obtain a flame retardant resin composition, and the flame retardant resin composition is degassed under a vacuum condition of 5 mbar for 10 minutes; then a carbon fiber sheet is prepared by a vacuum infusion process, and the flame retardant resin composition is vacuum impregnated into 5 layers of 400g T300-12K plain carbon cloth, and the vacuum is maintained and heated to 120°C for pre-curing for 2 hours. Then, the vacuum auxiliary material is removed and the infused carbon fiber sheet is placed in an oven at 150°C and post-cured for 2 hours to obtain a 2.0mm vacuum infused flame retardant carbon fiber sheet. The obtained vacuum infused flame retardant carbon fiber sheet has good effect, no foaming, no dry fiber, and no delamination.
[0142] Based on the UL94-2013 vertical combustion standard, the horizontal vertical combustion instrument test method was used to prepare five vertical combustion test pieces with a length of 130 mm, a width of 13 mm, and a thickness of 2.0 mm. The vertical combustion performance of the vacuum infused flame-retardant carbon fiber sheet was tested. The five vertical combustion test pieces were ignited twice, and the total afterflame time was measured to be 12 seconds. The flame retardant grade of the vacuum infused flame-retardant carbon fiber sheet reached V0.
[0143] Application Example 3
[0144] Preparation of wet-molded flame-retardant glass cloth sheets
[0145] Component A and component B were prepared according to the proportions of the flame retardant resin composition in Example 17.
[0146] Preheat the mixing device to 50°C, weigh 198g of polyisocyanate 44V20L and 2g of curing accelerator DY9577, add the polyisocyanate 44V20L and curing accelerator DY9577 to the mixing device and mix evenly to obtain component A; weigh 63.5g of bisphenol A epoxy resin NPEL-127, 20g of epoxy diluent XY622, 16g of core-shell toughening agent MZ-100 and 0.5g of TBAB, add the bisphenol A epoxy resin NPEL-127, epoxy diluent XY622, core-shell toughening agent MZ-100 and tetrabutylammonium bromide to the mixing device and mix evenly to obtain component B.
[0147] Component A and component B were uniformly mixed in a weight ratio of 100:25 to obtain a flame-retardant resin composition. A flat-plate molding die with a mold cavity thickness of 3.2 mm was preheated to 150° C., and then a release agent was evenly sprayed on the die. Twelve pieces of 400 g EWR400 plain woven glass cloth were cut, and each piece of glass cloth was hand-coated with 26% of the flame-retardant resin composition. The 12 pieces of glass cloth were stacked and placed in a preheated flat-plate molding die, and pressurized to a maximum pressure of 2.0 MPa according to a procedure. The pressure was maintained and hot-pressed for 10 minutes. After the hot-pressing was completed, the mold was removed and the flame-retardant sheet was placed in an oven at 150° C. and cured for 2 hours to obtain a wet-molded flame-retardant glass cloth sheet with a thickness of 3.2 mm.
[0148] Based on the UL94-2013 vertical combustion standard, a horizontal vertical combustion apparatus was used to test the vertical combustion performance of the wet-molded flame-retardant glass cloth sheet. Five vertical combustion test pieces with a length of 130 mm, a width of 13 mm, and a thickness of 3.2 mm were prepared. The five vertical combustion test pieces were ignited twice, and the total afterflame time was measured to be 23 seconds. The flame retardancy grade of the wet-molded flame-retardant glass cloth sheet reached V0.
[0149] Application Example 4
[0150] Preparation of wet-molded flame-retardant glass cloth sheets
[0151] Component A and component B were prepared according to the proportions of the flame retardant resin composition in Example 17.
[0152] Preheat the mixing device to 50°C, weigh 198g of polyisocyanate 44V20L and 2g of curing accelerator DY9577, add the polyisocyanate 44V20L and curing accelerator DY9577 to the mixing device and mix evenly to obtain component A; weigh 63.5g of bisphenol A epoxy resin NPEL-127, 20g of epoxy diluent XY622, 16g of core-shell toughening agent MZ-100 and 0.5g of tetrabutylammonium bromide, add the bisphenol A epoxy resin NPEL-127, epoxy diluent XY622, core-shell toughening agent MZ-100 and tetrabutylammonium bromide to the mixing device and mix evenly to obtain component B.
[0153] Component A and component B are uniformly mixed in a weight ratio of 100:25 to obtain a flame retardant resin composition, a flat-plate compression mold with a mold cavity thickness of 2.0 mm is preheated to 150° C., and then a release agent is evenly sprayed on the mold; 8 pieces of 400 g EWR400 plain woven glass cloth are cut, and each piece of glass cloth is hand-coated with 26% of the flame retardant resin composition. The 8 pieces of glass cloth are stacked and placed in a preheated flat-plate compression mold, and pressurized to a maximum pressure of 2.0 MPa according to a procedure. The pressure is maintained and hot pressed for 10 minutes. After the hot pressing is completed, the mold is removed and the flame retardant sheet is placed in an oven at 150° C. and cured for 2 hours to obtain a wet-molded flame retardant glass cloth sheet with a thickness of 2.1 mm. Based on the GBT1447-2005 standard, 6 Type I dumbbell tensile test pieces with a length of 180 mm were prepared from the obtained wet-molded flame-retardant glass cloth sheet. The tensile strength and tensile modulus of the wet-molded flame-retardant glass cloth sheet were tested. The tensile strength and tensile modulus of the wet-molded flame-retardant glass cloth sheet were measured to be 638.9 MPa and 33.9 GPa.
[0154] Based on the GBT1449-2005 standard, 6 80 mm long and 15 mm wide anti-bending test pieces were prepared from the obtained wet-molded flame-retardant glass cloth sheets. The bending strength and bending modulus of the wet-molded flame-retardant glass cloth sheets were tested. The bending strength and bending modulus of the wet-molded flame-retardant glass cloth sheets were measured to be 950.5 MPa and 30.7 GPa.
[0155] Based on the ISO14130 standard, 10 short beam shear test pieces with a length of 20 mm and a width of 10 mm were prepared from the obtained wet-molded flame-retardant glass cloth sheet to test the short beam shear strength of the wet-molded flame-retardant glass cloth sheet. The short beam shear strength of the wet-molded flame-retardant glass cloth sheet was measured to be 61.4 MPa.
[0156] While the embodiments of the present invention have been described in detail above, it will be apparent to those skilled in the art that various modifications and variations of these embodiments are possible. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as set forth in the claims. Furthermore, the invention described herein is susceptible to other embodiments and may be practiced or implemented in a variety of ways.
Claims
1. A flame retardant resin composition, characterized in that The invention comprises a component A and a component B, wherein the component A comprises a polyisocyanate component and a curing accelerator component, wherein the polyisocyanate component comprises one or more polyisocyanates, wherein the polyisocyanate comprises at least two isocyanate groups, and the component B comprises an epoxy resin component, wherein the ratio of the isocyanate groups in the polyisocyanate component to the epoxy groups in the epoxy resin component is (10-3):1, and the curing accelerator component accounts for 0.1-5.0% of the total amount of the polyisocyanate component and the epoxy resin component.
2. The flame retardant resin composition according to claim 1, characterized in that The polyisocyanate includes at least one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, triphenylmethane triisocyanate and polymethylene polyphenyl isocyanate.
3. The flame retardant resin composition according to claim 1, characterized in that The epoxy resin component includes at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, aliphatic epoxy resin, alicyclic epoxy resin, phenolic epoxy resin, toughened modified epoxy resin and phosphorus-containing modified epoxy resin.
4. The flame retardant resin composition according to claim 1, characterized in that The curing accelerator component includes at least one of boron amine complex, boron alkyl tertiary amine, DBU and its salts, quaternary ammonium salt, quaternary phosphonium salt and imidazole accelerator.
5. The flame retardant resin composition according to claim 1 or 4, characterized in that The curing accelerator component includes at least one of trichloro(N,N-dimethyl-n-octylamine)boron, curing agent 594, 1,8-diazabicyclo[5.4.0]undec-7-ene, DBU phenolate, DBU isooctanoate, tetrabutylammonium bromide, benzyltriphenylphosphonium chloride, 2-methylimidazole, 2-ethyl-4-methylimidazole and 2-phenyl-1-benzylimidazole.
6. The flame retardant resin composition according to claim 1, characterized in that Also included is a flame retardant, which includes a halogen-free flame retardant.
7. The flame retardant resin composition according to claim 6, characterized in that The halogen-free flame retardant includes at least one of phosphate ester, polyphosphate ester, ammonium polyphosphate, diethyl aluminum hypophosphite, piperazine pyrophosphate, aluminum hydroxide, magnesium hydroxide and hydrated zinc borate.
8. The flame retardant resin composition according to claim 1, characterized in that The invention also includes a toughening agent, wherein the toughening agent includes at least one of a CTBN rubber toughening agent, a core-shell particle toughening agent and a nanoparticle toughening agent.
9. The flame retardant resin composition according to claim 1, characterized in that The invention also includes auxiliary agents, which include at least one of a wetting agent, a defoaming agent and an internal release agent.
10. The method for preparing a flame retardant resin composition according to any one of claims 1 to 9, wherein: The following steps are involved: Preparation of component A: uniformly mixing the polyisocyanate component and the curing accelerator component to obtain component A; Preparation of component B: Mix the epoxy resin components uniformly to obtain component B; The component A and the component B are uniformly mixed to obtain the flame retardant resin composition, wherein the weight ratio of the component A to the component B is 100:(18-68).
11. A fiber-reinforced composite material, characterized in that: The invention comprises the flame retardant resin composition according to any one of claims 1 to 9 and reinforcing fibers, wherein the reinforcing fibers comprise at least one of carbon fibers, glass fibers, basalt fibers and aramid fibers.
12. The fiber-reinforced composite material according to claim 11, characterized in that: The flame retardant resin composition and the reinforcing fiber are subjected to a composite material forming process to prepare the fiber reinforced composite material. The composite material forming process includes any one of vacuum infusion, RTM, wet molding, HP-RTM and pultrusion.
Citation Information
Patent Citations
Fibre-reinforced composite components and production thereof
CN104603173A
Cured composition having high impact strength and temperature resistance, based on an epoxy resin and a polyisocyanate
CN109312041A
Method for producing compounds having oxazolidinone groups
CN110431162A
Flame-retardant resin composition, preparation method thereof and fiber-reinforced composite material
CN116574231A
Plural liquid pack type, heat-curable polyisocyanate-polyol-polyepoxy resin composition and process for producing a shaped resin article therefrom
US5223598A