Method for forging and rolling austenitic stainless steel tube

By combining forging and hot rolling with water-cooling shaping, the problem of uneven size and grain size in the production of austenitic stainless steel pipes has been solved, achieving efficient production of large-size pipes and high material utilization.

WO2024234896A1PCT designated stage expired Publication Date: 2024-11-21SHANGHAI ELECTRIC SHMP CASTING & FORGING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/087951
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-04-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve uniformity in both size and grain size during the production of austenitic stainless steel pipes, especially for large-sized pipes where the required grain size is difficult to meet, and the processing efficiency and material utilization are low.

Method used

The method combines forging and hot rolling, using forging initial forming and hot rolling forming processes, combined with water cooling and shaping treatment, to refine the grains and control the pipe dimensions. This includes forging initial forming, hot rolling forming, and cooling and shaping steps, ensuring the uniformity of grain size and dimensions.

Benefits of technology

This technology achieves uniform grain size and meets dimensional requirements for large-size austenitic stainless steel pipes, improves material utilization, and enhances production efficiency and economy, solving the problems of large processing allowance and low efficiency in existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024087951_21112024_PF_FP_ABST
    Figure CN2024087951_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A method for forging and rolling an austenitic stainless steel tube, comprising the following steps: primary forming in forging: forging an electroslag ingot to form a primarily formed billet, wherein the diameter of the primarily formed billet is determined according to the total elongation ratio requirement of a hot-rolled tube and a target tube size, and the grain size of the primarily formed billet is determined according to a target grain size and the rolling deformation amount of a tube; hot rolling forming: sequentially performing positioning hole drilling treatment, cross-roll piercing and finish rolling on the primarily formed billet to form a formed tube, wherein each elongation ratio is determined according to the total elongation ratio of the tube and the number of processes; and cooling and shaping: cooling the formed tube to form a target tube. Also disclosed is an austenitic stainless steel tube produced by using the method. Austenitic stainless steel tubes taking into account both the size and the grain size can be produced by using the method.
Need to check novelty before this filing date? Find Prior Art

Description

Austenitic stainless steel pipe forging method Technical Field

[0001] The invention relates to the field of austenitic stainless steel pipe manufacturing, and in particular to an austenitic stainless steel pipe forging method. Background Art

[0002] For the manufacture of stainless steel pipes, there are currently three main production methods: rolling, free forging and direct cutting.

[0003] Due to the material properties of austenitic stainless steel pipes, it is difficult to effectively improve the product grain size through heat treatment processes such as solid solution treatment. Therefore, for pipes with high grain size requirements, the grain size must be effectively controlled during the forging or rolling process.

[0004] The direct cutting method of bar or tubular material not only has low material utilization, but also has large machining allowance and low economic efficiency.

[0005] The sizes and specifications that can be produced by forging pipes are limited, the machining allowance in the diameter direction is large, the material utilization rate is not high, the processing cost is high, and the length of forged pipes is short. Generally, only pipes with a length of less than 5m can be produced. In addition, the forging operation has low production efficiency and high requirements for forging process control. Uneven deformation, local coarse grains, mixed crystals and other problems are prone to occur during the forging process, resulting in products that cannot meet the requirements.

[0006] Hot-rolled pipes are typically rolled from continuously cast billets, offering high production efficiency, precise stock control, and minimal processing effort. However, due to the inherent limitations of rolling production, hot-rolled pipes exhibit uneven grain size along the rolling direction. This is particularly true for large-sized stainless steel pipes with high grain size requirements, making it difficult to achieve the required grain size.

[0007] Summary of the Invention

[0008] In order to solve the problem of difficulty in balancing size and grain size in the production of related austenitic stainless steel pipes, the present invention provides a forging method for austenitic stainless steel pipes. The technical solution is:

[0009] A forging method for an austenitic stainless steel pipe, comprising:

[0010] Forging primary forming: Forging the electroslag ingot to form a primary forming blank, wherein the diameter of the primary forming blank is determined according to the total extension ratio requirement of the hot-rolled pipe and the target size of the pipe, and the grain size of the primary forming blank is determined according to the target grain size of the pipe and the rolling deformation;

[0011] Hot rolling forming: the preformed blank is subjected to positioning hole punching, oblique rolling and piercing and finish rolling in sequence to form a formed pipe, and the extension ratio of each time is determined according to the total extension ratio of the pipe and the number of steps;

[0012] Cooling and shaping: the formed pipe is water-cooled within 5 minutes to form the target pipe.

[0013] With the above technical solution, forging is used in the initial forming stage to refine the grains and obtain a uniform forged structure, thereby ensuring the grain size for subsequent pipe forming; hot rolling is used in the forming stage to ensure the pipe size, especially the length; and rapid cooling and shaping by water cooling is performed to avoid coarsening or mixed crystals of the pipe grains due to high residual heat, so that the final formed pipe meets both size and grain size requirements.

[0014] In a preferred embodiment of the present invention, the forging primary forming comprises:

[0015] Before forging, the electroslag ingot is kept at a temperature of 1150° C. to 1220° C. for 60 hours to 120 hours.

[0016] By adopting the above technical solution, high-temperature diffusion of the steel ingot is achieved, macro-segregation of the steel ingot is improved, and the heterogeneity of the recrystallization structure is reduced, thereby ensuring the grain size of the final formed pipe.

[0017] In a preferred embodiment of the present invention, the forging initial forming comprises:

[0018] The electroslag ingot is subjected to two upsetting and two drawing processes to form a steel billet, wherein the upsetting ratio is ≥2 and the drawing ratio is ≥2;

[0019] After the steel billet is returned to the furnace and heated at 1150℃~1180℃, the steel billet is stretched into the preformed billet with a cross-sectional diameter of D0 by 35%~55% using an upper flat anvil and a lower V-shaped anvil. The preformed billet satisfies the following requirements: (D0 2 -d0 2 )×L0×0.99=(D 2 -d 2 )×L,

[0020] The total extension ratio of the pipe = L / L0,

[0021] Wherein, D0 is the diameter of the preformed blank, d0 is the diameter of the positioning hole, L0 is the length of the preformed blank, D is the outer diameter of the target pipe, d is the inner diameter of the target pipe, and L is the length of the target pipe.

[0022] By adopting the above technical solution, the steel billet is fully and effectively compacted and crushed into cast dendrites through two upsetting and two drawing operations; by drawing with an upper flat anvil and a lower V-shaped anvil, the grains inside the steel billet are refined as a whole for the first time, and the grain size of the initially formed billet can reach level 2-3.

[0023] In a preferred embodiment of the present invention, the diameter of the positioning hole is 80 mm-120 mm.

[0024] In a preferred embodiment of the present invention, the hot rolling forming comprises:

[0025] The initially formed billet is sequentially subjected to two cross-rolling and piercing passes and one finishing rolling pass, and the total elongation ratio of the pipe is 2.4 to 3.2, the elongation ratio of the first cross-rolling and piercing pass is 1.1 to 1.3, the elongation ratio of the second cross-rolling and piercing pass is 2.0 to 2.2, and the elongation ratio of the finishing rolling pass is 1.07 to 1.1.

[0026] In a preferred embodiment of the present invention, the hot rolling forming comprises:

[0027] The preformed blank after the positioning hole treatment and before the oblique rolling piercing is first heated to 1100±10°C and kept warm for 2 hours, and then quickly heated to 1240±10°C, for example within 1 hour, and kept warm for 4 to 6 hours.

[0028] In a preferred embodiment of the present invention, the preformed blank after the first cross-rolling and piercing is heated to 1100° C. to 1150° C. and kept warm, then heated to 1200° C. to 1240° C. and kept warm, and then subjected to a second cross-rolling and piercing.

[0029] In a preferred embodiment of the present invention, the diameter reduction rate of the finishing rolling pass is 2.6% to 3.0%.

[0030] In a preferred embodiment of the present invention, after the forging initial forming and before the hot rolling forming, the process includes:

[0031] Surface treatment: The preformed blank is subjected to surface peeling treatment, and surface cracks are subjected to carbon arc gouging and grinding and polishing treatment, and the pits formed after grinding and polishing have a length: width: depth ratio of 10:6:1.

[0032] Another technical solution is:

[0033] An austenitic stainless steel pipe is produced by any of the forging and rolling methods described above, and the pipe has a diameter D of Φ500-Φ900 mm, a wall thickness T of 30 mm-70 mm, a length L ≥ 4000 mm, and a full-section grain size ≥ grade 4.

[0034] By adopting the above technical solution, the obtained pipe takes into account both size and grain size, meeting the demand for large-sized austenitic stainless steel pipes with uniform grains and high grain size grade. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is a schematic diagram of the dimensions of a 5.6-ton electroslag ingot;

[0036] FIG2 is a schematic diagram showing the dimensions of the preformed blank;

[0037] FIG3 is a schematic diagram of the primary formed blank after the positioning hole is punched;

[0038] FIG4 is a heating curve diagram during hot rolling;

[0039] Figure 5 is a schematic diagram of the first oblique rolling piercing;

[0040] Figure 6 is a schematic diagram of the second oblique rolling piercing;

[0041] Figure 7 is a schematic diagram of the finishing rolling process;

[0042] FIG8 is a metallographic diagram of the grain size of the target tube formed. DETAILED DESCRIPTION

[0043] The content of the present invention can be more easily understood by referring to the detailed description of the preferred embodiment of the present invention below and the examples included. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as those of ordinary skill in the art to which the present invention belongs. When there is a contradiction, the definition in this specification shall prevail. As used herein, the term "prepared by..." is synonymous with "comprising". The terms "comprising," "including," "having," "containing," or any other variation thereof used herein are intended to cover non-exclusive inclusions. For example, a composition, step, method, product, or device comprising the listed elements is not necessarily limited to those elements, but may include other elements not explicitly listed or elements inherent to such a composition, step, method, product, or device.

[0044] The conjunction "consisting of" excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed, excluding materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim, rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0045] When amount, concentration or other value or parameter is represented with range, preferred range or the range that a series of upper preferred value and lower preferred value limit are expressed, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, no matter whether this range is disclosed separately.For example, when disclosing scope "1 to 5", described scope should be interpreted as including scope "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc.When numerical range is described in this article, unless otherwise stated, otherwise this scope is intended to include its end value and all integers and fractions within this range.

[0046] The singular includes plural references unless the context clearly dictates otherwise. "Optional" or "either" means that the subsequently described event or incident can or cannot occur, and that the description includes instances where the event occurs and instances where it does not.

[0047] Approximating terms in the specification and claims are used to modify a quantity to indicate that the invention is not limited to that specific quantity and includes acceptable modifications close to that quantity that do not result in a change in the relevant basic function. Accordingly, the use of "about," "approximately," or the like to modify a numerical value indicates that the invention is not limited to that exact numerical value. In some instances, approximating terms may correspond to the precision of the instrument used to measure the value. In the specification and claims of this application, range definitions may be combined and / or interchanged, and unless otherwise indicated, such ranges include all subranges contained therein.

[0048] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention do not limit the quantity requirement (i.e., the number of times the elements or components appear). Therefore, "a" or "an" should be interpreted as including one or at least one, and elements or components in the singular also include plural forms, unless the number is obviously intended to be singular.

[0049] A forging method for austenitic stainless steel pipes. This method, through a "forging + rolling" forming process, can take into account both pipe size and grain size requirements. The method is particularly suitable for producing pipes with large diameters, wall thicknesses, and lengths, and high grain size requirements. For example, thick-walled pipes with a diameter D of 500 to 900 mm, a wall thickness T of 30 mm to 70 mm, and a length of 4000 mm or greater can be produced using this method to achieve uniform grains, a high overall grain size, and a grain size of 4 or greater across the entire cross-section of the pipe.

[0050] The following will be based on the size Taking the target pipe with grain size ≥ 4 and grain size difference not greater than 2 as an example, the method is described in detail. It can be understood that the method can not only produce pipes of this size, but also etc.

[0051] This method includes:

[0052] S1 Forging: The electroslag ingot shown in Figure 1 is forged to form a preformed billet as shown in Figure 2. The diameter of the preformed billet is determined based on the total elongation ratio requirements and target pipe dimensions for hot-rolled pipes. The grain size of the preformed billet is determined based on the target pipe grain size and rolling deformation. Specifically, the grain size of the preformed billet is grade 2-3, which ensures uniform grains and microstructure for the subsequent hot-rolled pipes, as well as grain size differences that meet mining specifications.

[0053] To meet the grain size requirements, the specific steps of forging the initial shape may include:

[0054] Before forging, S11 cuts off the bottom 60mm of the Φ800×1200mm electroslag ingot and heats it in the furnace, keeping it at 1150℃~1220℃ for 60h~120h, thereby achieving high-temperature diffusion of the ingot, improving the macro-segregation of the ingot, reducing the unevenness of the recrystallization structure, and thus ensuring the grain size of the final tube.

[0055] The S12 electroslag ingot is evenly heated and quickly taken out of the furnace. It is quickly and continuously upset twice and drawn twice by a hydraulic press to form a billet, and the upsetting ratio is ≥2 and the drawing ratio is ≥2, so that the billet can be fully and effectively compacted and the cast dendrites can be broken.

[0056] After the billet is returned to the furnace and heated to 1150°C to 1180°C, it is then stretched to a preformed billet with a cross-sectional diameter of D0 by 35% to 55% using a flat upper anvil and a V-shaped lower anvil. This results in an initial overall refinement of the billet's internal grains, resulting in a uniform forged microstructure. The preformed billet's grain size can reach levels 2-3, providing a good foundation for the final pipe's grain size. The V-shaped anvil can be angled between 100° and 120°, with 100° being more preferred. This angle is well-matched to a billet diameter of 650mm, and achieves the best core stress and strain effects during forging, which is conducive to obtaining uniform grains.

[0057] The initial forming blank meets the following requirements: (D0 2 -d0 2 )×L0×0.99=(D 2 -d 2 )×L,

[0058] Total extension ratio of pipe = L / L0,

[0059] Wherein, D0 is the diameter of the preformed blank, d0 is the diameter of the positioning hole, L0 is the length of the preformed blank, D is the outer diameter of the target pipe, d is the inner diameter of the target pipe, and L is the length of the target pipe.

[0060] S2 Hot Rolling: The preformed billet undergoes positioning hole punching (forming the billet shown in Figure 3), cross-rolling piercing (forming the billet shown in Figures 5 and 6), and finish rolling to form the formed tube shown in Figure 7. The elongation ratio for each roll is determined by the total elongation ratio of the tube and the number of roll steps. Hot rolling allows for precise control of tube dimensions.

[0061] The diameter of the positioning hole can be 80mm-120mm, for example, 80mm, 100mm or 120mm. A 100mm through hole can be used, which can reduce the deformation resistance of the stainless steel material.

[0062] For pipes with grain size requirements of ≥4 and unidirectional rolling, the total extension ratio is set at 2.4-3.2, the extension ratio of the first cross-rolling piercing is 1.1-1.3, the extension ratio of the second cross-rolling piercing is 2.0-2.2, and the extension ratio of the finishing pass is 1.07-1.1. Too small an extension ratio will result in substandard dimensions, while too large an extension ratio will increase deformation resistance and damage the equipment. Specifically, the size of the target pipe is The extension ratio of the first cross-rolling piercing pass can be 1.3, the extension ratio of the second cross-rolling piercing pass can be 2.0, the extension ratio of the finishing pass can be 1.1, and the total extension ratio can be 2.7. Therefore, according to the above formula and the extension ratio requirements, the size design of the initial formed billet can be The difference part takes into account the former is the processing For the later rolled tube billet, the heating and holding time before the first piercing is also considered to be long, resulting in fire consumption and burn loss. Here, the fire consumption and burn loss is set to 1%.

[0063] Hot rolling forming can specifically include:

[0064] As shown in FIG4 , S21 is to heat the preformed blank after the positioning hole treatment and before the oblique rolling piercing to 1100±10° C. for 2 hours, and then rapidly heat it to 1240±10° C., for example, within 1 hour, and keep it at this temperature for 4 to 6 hours.

[0065] Since the billet will subsequently undergo high-ratio rolling, its deformation resistance is high. Heating and holding the billet improves its plasticity and reduces the load requirements on the rolling equipment. The billet is initially heated internally at a lower temperature to increase its overall temperature and plasticity. At this temperature, grain growth is very slow, and no significant grain growth occurs. Prolonged heating at the high temperature stage can further rapidly increase the billet's plasticity. Since subsequent rolling will further improve the bar's grain size, the impact is manageable.

[0066] The S22 initially formed billet is quickly taken out of the furnace, and is subjected to two cross-rolling and one finishing rolling in sequence. The cross-rolling and piercing are performed by a cross-rolling unit, and the finishing rolling is performed by a finishing unit. The finishing unit includes multiple groups of forming rollers that alternate vertically and horizontally.

[0067] The time from the initial forming billet being taken out of the furnace to the start of piercing must be ≤300 seconds. If it exceeds the time limit, it must be returned to the furnace for re-firing. As shown in Figure 5, after the first cross-rolling and piercing, the billet is rolled into a pipe with an outer diameter of D1, an inner diameter of d1, and a length of L1. The first cross-rolling and piercing extension ratio is L1 / L0. In this embodiment, the outer diameter is The pipe with a wall thickness of 165mm and a length of 2100mm has a deformation of 20%.

[0068] After the first oblique rolling and piercing, the initially formed billet is heated to 1050℃~1120℃ and kept warm, for example, 1100℃ for 1h, and then heated to 1200℃~1240℃ and kept warm, for example, 1220℃±10℃ for 2h, and then the second oblique rolling and piercing is performed. Since the temperature of the initially formed billet has been reduced after the first piercing, the deformation resistance has increased; returning to the furnace for heating will improve the plasticity of the billet, and the next large deformation rolling can be achieved. As shown in Figure 6, after the second oblique rolling and piercing, the billet is rolled into a pipe with an outer diameter of D2, an inner diameter of d2, and a length of L2. The extension ratio of the second oblique rolling and piercing is L2 / L1. In this embodiment, the outer diameter is specifically The deformation of the pipe with a wall thickness of 60mm and a length of 4200mm is 53%.

[0069] As shown in Figure 7, after finishing rolling, the billet is rolled into a tube with a diameter of D, an inner diameter of d, and a length of L, and the finishing extension ratio is L / L2. The diameter reduction rate of the finishing pass is 2.6% to 3.0%. The finishing pass is mainly to control the inner and outer diameter dimensions, and the extension ratio should not be too large. It also increases the radial deformation and reduces the anisotropy of the hot-rolled pipe. The finishing rolling can be specifically done by first placing glass powder in the inner hole of the tube billet after oblique rolling and piercing to facilitate the rolling of the finishing mill; then the tube billet that has been obliquely rolled and pierced is quickly sent to the finishing mill group, and the tube billet is rolled into a target size of through multiple groups of longitudinal and transverse alternating forming rollers of the finishing mill group. of pipes.

[0070] Through this hot rolling forming step, it is ensured that the rolling process does not exceed the preset process window, thereby achieving process control, obtaining hot-rolled pipes with stable quality, and ultimately obtaining austenitic stainless steel pipes that meet grain size requirements.

[0071] It is understood that the billet size during hot rolling satisfies: (D1 2 -d1 2 )×L1=(D2 2 -d2 2 )×L2=(D 2 -d 2 )×L×0.99.

[0072] S3 Cooling and Shaping: The formed tube is cooled to prevent coarsening or crystal mixing of the tube grains due to high residual heat. It should be noted that the shorter the cooling time for the formed tube transfer, the better, for example, within 5 minutes, specifically 2 minutes, 3 minutes, 4 minutes, etc., to improve the shaping effect. Furthermore, the faster the cooling rate, the better, such as by using water cooling.

[0073] The grain size of the austenitic stainless steel pipe produced by this method was tested by sampling. The grain size was above level 4, and the grain morphology was generally uniform. The grain size metallographic diagram is shown in Figure 8.

[0074] In a preferred embodiment of the present invention, after S1 forging and before S2 hot rolling, the process includes:

[0075] Surface treatment: The surface of the initially formed blank is peeled, and the surface cracks are carbon arc gouged and polished. The length: width: depth ratio of the pits formed after polishing is 10:6:1, so that folding and cracking will not occur during subsequent rolling. The pits with this length, width and depth ratio are more likely to obtain a surface close to the shape of the pipe after rolling.

[0076] Specifically: 80% of the forging surface area is polished to white by machining, and the remaining black skin part is ground and polished by a pneumatic grinding wheel; for deeper crack defects, the defects are removed by carbon arc air gouging, and then the surface of the carbon gouging is ground and polished. The "length: width: depth" of the pits cleaned by grinding and cleaning meets the "10:6:1" requirement.

[0077] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the invention can be embodied in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as illustrative and non-restrictive, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations that come within the meaning and range of equivalents of the claims be embraced therein.

Claims

1. A forging method for an austenitic stainless steel pipe, It is characterized in that include: Forging initial forming: Forging the electroslag ingot to form an initial forming blank, and the diameter of the initial forming blank is determined according to the total extension ratio requirement of the hot-rolled pipe and the target size of the pipe, and the grain size of the initial forming blank is determined according to the target grain size of the pipe and the rolling deformation; Hot rolling forming: the preformed blank is subjected to positioning hole punching, oblique rolling and finish rolling in sequence to form a formed pipe, and the extension ratio of each time is determined according to the total extension ratio of the pipe and the number of processes; Cooling and shaping: the formed pipe is cooled to form a target pipe.

2. The austenitic stainless steel pipe forging method according to claim 1, It is characterized in that The forging initial forming comprises: Before forging, the electroslag ingot is kept at a temperature of 1150° C. to 1220° C. for 60 h to 120 h.

3. The austenitic stainless steel pipe forging method according to claim 1, It is characterized in that The forging initial forming comprises: The electroslag ingot is subjected to two upsetting and two drawing processes to form a steel billet, wherein the upsetting ratio is ≥2 and the drawing ratio is ≥2; After the steel billet is returned to the furnace and heated and kept at 1150° C. to 1180° C., an upper flat anvil and a lower V-shaped anvil are used to stretch the steel billet into the preformed billet with a cross-sectional diameter of D0 by 35% to 55% deformation. The preformed billet meets the following requirements: (D0 2 -d0 2 )×L0×0.99=(D 2 -d 2 )×L, The total extension ratio of the pipe = L / L0, Among them, D0 is the diameter of the initial forming blank, d0 is the diameter of the positioning hole, L0 is the length of the initial forming blank, D is the outer diameter of the target pipe, d is the inner diameter of the target pipe, and L is the length of the target pipe.

4. The austenitic stainless steel pipe forging method according to claim 3, It is characterized in that The diameter of the positioning hole is 80mm-120mm.

5. The austenitic stainless steel pipe forging method according to claim 1, It is characterized in that The hot rolling forming comprises: The initially formed billet is subjected to two oblique rolling and piercing passes and one finishing rolling pass in sequence, and the total elongation ratio of the pipe is 2.4-3.2, the elongation ratio of the first oblique rolling and piercing pass is 1.1-1.3, the elongation ratio of the second oblique rolling and piercing pass is 2.0-2.2, and the elongation ratio of the finishing rolling pass is 1.07-1.

1.

6. The austenitic stainless steel pipe forging method according to claim 5, It is characterized in that The hot rolling forming comprises: The preformed blank after the positioning hole processing and before the oblique rolling piercing is first heated to 1100±10°C, kept warm for 2 hours, and then quickly heated to 1240±10°C, for example within 1 hour, and kept warm for 4 to 6 hours.

7. The austenitic stainless steel pipe forging method according to claim 6, It is characterized in that The initially formed blank after the first oblique rolling and piercing is heated to 1100° C. to 1150° C. and kept warm, then heated to 1200° C. to 1240° C. and kept warm, and then subjected to the second oblique rolling and piercing.

8. The austenitic stainless steel pipe forging method according to claim 5, It is characterized in that The diameter reduction rate of the finishing rolling pass is 2.6% to 3.0%.

9. The austenitic stainless steel pipe forging method according to claim 1, It is characterized in that After the forging initial forming and before the hot rolling forming, the method comprises: Surface treatment: The initially formed blank is subjected to surface peeling treatment, and surface cracks are subjected to carbon arc gouging and grinding and polishing treatment, and the pits formed after grinding and polishing have a length: width: depth of 10:6:

1.

10. An austenitic stainless steel pipe, It is characterized in that The pipe is produced by the forging method as described in any one of claims 1 to 9, and the diameter D of the pipe is Φ500 to Φ900 mm, the wall thickness T is 30 mm to 70 mm, the length L is ≥4000 mm, and the grain size of the entire cross section is ≥4 levels.

Citation Information

Patent Citations

  • Manufacturing process of super austenitic stainless steel pipe

    CN102274854A

  • Production method for high-precision austenite seamless steel pipe

    CN103464507A

  • Manufacturing method of super austenitic stainless steel seamless tube

    CN104826890A

  • X80 steel-grade D1422 mm seamless bent pipe and manufacturing method thereof

    CN110306120A

  • Large-diameter austenitic stainless steel seamless tube and manufacturing method and application thereof

    CN114749508A