Surface coating method and semiconductor device

By using a multi-layer coating method combined with atomic layer deposition and plasma immersion processes on the surface of semiconductor equipment, a ceramic thin film protective layer is formed, which solves the problem of equipment surface corrosion and improves process stability and production efficiency.

WO2024235185A1PCT designated stage expired Publication Date: 2024-11-21JIANGSU LEUVEN INSTR CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/092796
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The prior art cannot form a comprehensive and stable protective layer on the surface of semiconductor equipment, resulting in corrosion of internal components of the reaction chamber and affecting chip processing quality and process stability.

Method used

The surface coating method combined with atomic layer deposition process and plasma immersion process is used to form multiple layers of atomic layer films and ceramic film protective layers in sequence to enhance the corrosion resistance of the equipment surface.

Benefits of technology

It achieves all-round coverage of the surface of semiconductor equipment, significantly reduces particle and trace elements pollution, improves process stability and production efficiency, and extends the service life of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024092796_21112024_PF_FP_ABST
    Figure CN2024092796_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses a surface coating method and a semiconductor device. The surface coating method comprises: providing a device body to be coated; and forming a first protective layer on the surface of the device body, wherein the first protective layer at least comprises a first sub-protective layer formed on the basis of an atomic layer deposition process. According to the technical solution of the present application, the first protective layer is formed on the surface of the device body, the first protective layer at least comprises the first sub-protective layer formed on the basis of the atomic layer deposition process, and all-around film coverage can be achieved on the surface of the device body to improve the corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Surface coating method and semiconductor device

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 18, 2023, with application number 202310566008.3 and invention name “A Surface Coating Method and Semiconductor Device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of surface protection technology for enhancing the functionality of semiconductor devices, and more specifically, to a surface coating method and semiconductor devices. Background Art

[0003] Because semiconductor equipment (such as thin film deposition and plasma etchers) performs chip processing (such as plasma etching and thin film deposition) on large-scale integrated circuits with a scale below 15nm, the reaction gases or plasmas used in most processes (such as plasma containing elements such as O, F, Cl, Br, or H) also corrode the surface of components inside the reaction chamber, changing the size and surface composition of the components, affecting the quality of chip processing and the stability of the process.

[0004] To enable atomic-level precision processing of chips using plasma and other processes, the dimensions and composition of reaction chamber components must be highly consistent during chip fabrication processes such as thin film deposition or plasma etching. To achieve this, a protective layer must be formed on the surface of semiconductor devices. However, existing technologies have been unable to form a comprehensive and stable protective layer on the surface of semiconductor devices.

[0005] Summary of the Invention

[0006] In view of this, the present application provides a semiconductor device and a surface coating method thereof, the scheme is as follows:

[0007] A surface coating method for semiconductor equipment, comprising:

[0008] Provide the equipment body to be coated;

[0009] A first protective layer is formed on the surface of the device body; wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

[0010] Preferably, in the above surface coating method, the method of forming the first sub-protective layer includes:

[0011] An atomic layer deposition process is adopted to sequentially form an atomic layer thin film on the surface of the device body as the first sub-protective layer.

[0012] Preferably, in the above surface coating method, the method of forming the first sub-protective layer includes:

[0013] forming a first atomic layer film based on saturated chemical adsorption and reaction between the first precursor and the surface of the device body;

[0014] forming another atomic layer film based on saturated chemical adsorption and reaction of the second precursor with the surface of the previous atomic layer film;

[0015] Before forming the next atomic layer film, the precursor used to form the previous atomic layer film is purged and discharged.

[0016] Preferably, in the above surface coating method, before forming the first protective layer, the method further comprises:

[0017] The surface of the device body is pretreated to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0018] Preferably, in the above-mentioned surface coating method, the method of pre-treating the surface of the device body includes:

[0019] The surface of the device body is modified by adopting a first plasma immersion process, so that a gentle transition layer with a gradual change of doping components is formed on the surface of the device body.

[0020] Preferably, in the above-mentioned surface coating method, a first plasma immersion process is used to modify the surface of the device body, including:

[0021] Under a first pulse bias voltage, performing ion implantation to a first depth into the surface of the device body;

[0022] Under a second pulse bias voltage, performing ion implantation to a second depth into the surface of the device body, and / or achieving surface alloying of the device body;

[0023] The second depth is smaller than the first depth.

[0024] Preferably, in the above surface coating method, the method of forming the first protective layer further comprises:

[0025] A second plasma immersion process is performed to form a second sub-protective layer on the surface of the first sub-protective layer.

[0026] Preferably, in the above surface coating method, a second plasma immersion process is used to form a second sub-protective layer on the surface of the first sub-protective layer, comprising:

[0027] Under a negative bias voltage less than 15 kV, omnidirectional coating is performed on the surface of the device body formed with the first sub-protective layer to form the second sub-protective layer.

[0028] Preferably, in the above surface coating method, it also includes:

[0029] forming a second protective layer on a surface of the first protective layer;

[0030] Wherein, the thickness of the second protective layer is greater than that of the first protective layer.

[0031] Preferably, in the above-mentioned surface coating method, the method of forming the second protective layer includes:

[0032] The second protective layer is formed by a plasma enhanced physical vapor deposition process.

[0033] The present application also provides a semiconductor device, comprising:

[0034] Equipment body;

[0035] A first protective layer covering the device body, wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

[0036] Preferably, in the above semiconductor device, the first sub-protective layer includes multiple atomic layer films stacked in sequence.

[0037] Preferably, in the above-mentioned semiconductor device, the surface of the device body is modified to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0038] Preferably, in the above semiconductor device, the first protective layer further comprises: a second sub-protective layer located on the surface of the first sub-protective layer;

[0039] Wherein, the second sub-protective layer is a film layer formed by a plasma immersion process.

[0040] Preferably, in the above semiconductor device, the first protective layer includes a ceramic film.

[0041] Preferably, the above semiconductor device further comprises:

[0042] A second protective layer is located on a surface of the first protective layer.

[0043] Preferably, in the above semiconductor device, the second protective layer is a plasma enhanced physical vapor deposition film.

[0044] Preferably, in the above semiconductor device, the thickness of the first protective layer is less than 25 μm, and the thickness of the second protective layer is greater than 10 μm.

[0045] Preferably, in the above semiconductor device, the second protective layer is a ceramic film.

[0046] Preferably, in the above semiconductor device, the thickness of the second protective layer is greater than the thickness of the first protective layer.

[0047] From the above description, it can be seen that in the surface coating method and semiconductor device provided by the technical solution of the present application, a first protective layer is formed on the surface of the device body, and the first protective layer includes at least a first sub-protective layer formed based on the atomic layer deposition process, which can achieve all-round thin film coverage of the surface of the device body to improve corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the technical solutions in the embodiments of the present application or related technologies, the following briefly introduces the drawings required for use in the embodiments or descriptions of the prior art. Obviously, the drawings described below are merely embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without any creative work.

[0049] The structures, proportions, sizes, etc. depicted in the drawings of this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with this technology. They are not intended to limit the conditions under which this application can be implemented, and therefore have no substantive technical significance. Any structural modifications, changes in proportional relationships, or adjustments in size, without affecting the efficacy and objectives that can be achieved by this application, should still fall within the scope of the technical contents disclosed in this application.

[0050] FIG1 is a schematic flow chart of a method for coating a surface of a semiconductor device according to an embodiment of the present application;

[0051] FIG2 is a flow chart of an ALD (atomic layer deposition) method for forming a first sub-protective layer provided in an embodiment of the present application;

[0052] 3 to 6 are schematic diagrams showing the principles of a method for manufacturing a first sub-protective layer in different process steps provided by an embodiment of the present application;

[0053] FIG7 is a schematic flow chart of another method for coating a surface of a semiconductor device according to an embodiment of the present application;

[0054] FIG8 is a schematic diagram of the principle of a plasma immersion ion processing (PIIP) provided in an embodiment of the present application;

[0055] FIG9 is a schematic diagram showing a principle of modifying the surface of a device body according to an embodiment of the present application;

[0056] FIG10 is a flow chart of a method for modifying the surface of a device body provided in an embodiment of the present application;

[0057] Figure 11 is a top view of the device body;

[0058] FIG12 is a cross-sectional view of the device body shown in FIG11;

[0059] FIG13 is a partial enlarged view of the device body shown in FIG11;

[0060] FIG14 is a partial enlarged view of a device body having a corrosion-resistant protective layer formed thereon according to a coating method according to an embodiment of the present application;

[0061] FIG15 is a partial enlarged view of another device body having a corrosion-resistant protective layer formed thereon based on the coating method according to an embodiment of the present application;

[0062] FIG16 is a partial enlarged view of another device body having a corrosion-resistant protective layer formed thereon according to the coating method of an embodiment of the present application;

[0063] FIG17 is another partially enlarged view of a device body having a corrosion-resistant protective layer formed thereon based on the coating method according to an embodiment of the present application. DETAILED DESCRIPTION

[0064] The following will be combined with the accompanying drawings in the embodiments of this application to clearly and completely describe the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0065] Currently, in a large number of semiconductor thin film deposition equipment, such as physical vapor deposition (PVD) and chemical vapor deposition (CVD) systems, flat-plate gas distribution plates based on 6061T aluminum alloy, such as aluminum alloy shower heads (SH), are still widely used within the reaction chamber. Aluminum alloy components without surface protection are not suitable for direct contact with reactive gases and plasma to prevent corrosion and metal and particle contamination. The unstable surface structure and composition of these aluminum alloy components interact with chemical reactant gases (such as O2, SiH4, TMA, TEOS, NH3, SiCl4, N2O, C2F6, SF6, SiC4, HBr, NF3, CF4, CHF3, CH2F2, Cl2, CCl4, BCl3, SiF4, etc.) and the resulting plasma during semiconductor thin film deposition processes such as CVD and PVD. This results in unnecessary chemical reactions and consumption of the chemical components that form the film deposit on the chamber surface, leading to uneven and unstable film deposition rates, as well as particle and trace element contamination, which seriously affects the process stability of the film deposition. Therefore, improving the component structure and surface material stability of the semiconductor equipment reaction chamber through all-round material surface modification, such as all-round coating protection, and reducing particle contamination (particle size and number) during thin film deposition and etching processes is an important way to ensure the stability of high-quality chip processing and reduce production costs.

[0066] In semiconductor chip thin film deposition and plasma etching systems, anodic oxidation and plasma spraying (PS) of yttrium oxide are commonly used to protect the inner walls of the reaction chamber and key components to enhance the surface resistance of the chamber components to chemical corrosion and plasma etching. Although anodic oxidation can achieve comprehensive oxidation protection for aluminum alloy workpiece surfaces, the stability of the anodic oxidation structure is very poor and it cannot operate stably in environments above 100°C, making it unsuitable for higher-temperature thin film deposition processes (such as PVD and PECVD). In addition, even components with anodic protection layers are not recommended for direct contact with the reaction gas or plasma. This is because the anodic oxidation structure contains cracks, which can generate contamination from particles and trace elements (such as Al) in the plasma environment. PS coatings (such as PS Y2O3) have loose structures and rough surfaces, which easily generate contaminant particles during the plasma etching process, making high-precision chip etching processes (such as below 15nm) difficult to perform stably.

[0067] In recent years, the use of plasma enhanced physical vapor deposition (PEPVD) to deposit dense thick coatings has been gradually expanded to effectively improve the surface structure stability and service life of key components such as gas shower heads and ceramic windows. However, the linear thin film deposition characteristics of PEPVD make it impossible for this process to effectively coat and protect certain key components such as the pores of the gas shower head and the inside of the gas pipeline. It is also impossible to deposit a plasma-etching-resistant protective film on the inner surface of the pores. This cannot prevent the inner surface of the pores from being corroded by the reaction gas or contaminated by metal and particles generated by plasma etching during the plasma etching process.

[0068] Cylindrical workpieces and gas pipes used in semiconductor equipment are mostly made of aluminum alloy or stainless steel, which present the same problems mentioned above. Because these workpieces are often used to transport plasma or various reactive gases, their inner surfaces are inevitably corroded by the plasma and reactive gases. Conventional coating processes (such as PS, PECVD, and PVD) cannot effectively protect the inner surfaces of these workpieces with thin films, requiring only anodizing. As mentioned above, this leads to metal and particle contamination in many processes. Furthermore, for stainless steel gas pipes with smaller diameters (e.g., less than 1 cm), when corroded by reactive gases (such as Cl2, NF3, and HBr), especially at temperatures of 150°C and above, the inner surface cannot be effectively protected by the surface coating, resulting in the formation of particles and trace elements on the surface structure. This, in turn, introduces contamination from these particles and trace elements during chip processing. To address this issue, expensive hafnium alloys or heat-resistant alloys with high Cr or Ni content are generally used.

[0069] In view of this, the embodiment of the present application provides a semiconductor device and a surface coating method thereof, which can be used for thin film deposition (such as PVD, CVD, etc.) equipment and important components of plasma etcher (Plasma Etcher), such as flat-plate key workpieces (such as SH, etc.) and hollow cylindrical workpieces (such as cylinders and air pipes, etc.). The surface coating method is a comprehensive surface coating protection method for the surface of a material that can effectively enhance working stability. Even when the diameter and depth of the circular hole reach 1:200, an effective protective layer can be prepared on the inner surface of the cylindrical workpiece to extend the service life of the workpiece. The technical solution of the present application can effectively enhance the process stability of semiconductor equipment (such as thin film deposition and plasma etching equipment), significantly reduce the risk of particle contamination and trace element contamination in the process of different semiconductor equipment, thereby improving the process stability of integrated circuit chip production, improving production efficiency, and reducing the production cost of semiconductor equipment.

[0070] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below with reference to the accompanying drawings and specific implementation methods.

[0071] Referring to FIG. 1 , FIG. 1 is a schematic flow chart of a method for coating a surface of a semiconductor device according to an embodiment of the present application. The method comprises:

[0072] Step S11: providing a device body to be coated;

[0073] In the embodiments of this application, semiconductor equipment includes thin film deposition equipment and plasma etchers. The equipment body includes any workpiece in the semiconductor equipment that needs to come into contact with reactive gases or plasma, such as showerheads, gas lines, and reaction chambers. The embodiments of this application do not limit the specific nature of the semiconductor equipment and the equipment body.

[0074] Step S12: forming a first protective layer on the surface of the device body; wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

[0075] The atomic layer deposition process is a special chemical vapor deposition process that grows a single layer of atoms. The film growth process can be carried out in a low-temperature, low-pressure environment of 450°C. Unlike ordinary CVD, the chemical reaction precursors in the atomic layer deposition process do not decompose before contacting the surface of the device to be coated. Instead, after being adsorbed onto the surface of the device body, chemical decomposition reactions occur on the surface of the device body, and the decomposed chemical components evenly cover the entire surface of the device body to form an atomic layer film. Therefore, as long as the distribution of the reaction gas is controlled during the atomic layer deposition process so that the chemical reaction precursors can fully diffuse and contact the component surface, and sufficient time is provided to purge the remaining precursors, the atomic layer deposition process can form a uniform multi-atomic layer stacked film on the device body with complex surfaces (such as surfaces with complex geometric shapes, the inner and outer walls of cylindrical tubes, and the inner surfaces of small pores). Because the atomic layer growth is carried out by precursor decomposition, the film formed by the atomic layer deposition process is very dense, can form full-surface coverage of the device body, and has good interfacial bonding and structural thermal stability.

[0076] Optionally, in an embodiment of the present application, the method for forming the first sub-protective layer includes: sequentially forming multiple layers of atomic layer thin films on the surface of the device body using an atomic layer deposition process to serve as the first sub-protective layer. The thickness of the first sub-protective layer can be precisely controlled by controlling the number of atomic layer thin film deposition cycles.

[0077] Referring to FIG. 2 , FIG. 2 is a flow chart of a method for forming a first sub-protective layer provided in an embodiment of the present application. The first sub-protective layer includes multiple atomic layer films. The method for forming the first sub-protective layer includes:

[0078] Step S21: forming a first atomic layer film based on saturated chemical adsorption and reaction between the first precursor and the surface of the device body;

[0079] Step S22: forming another atomic layer film based on saturated chemical adsorption and reaction between the second precursor and the surface of the previous atomic layer film.

[0080] Before forming the next atomic layer film, the precursor used to form the previous atomic layer film is purged and discharged.

[0081] The number of cycles for depositing the atomic layer film is set based on demand, so that the thickness of the first sub-protective layer can be accurately controlled.

[0082] 3 to 6 , which are schematic diagrams of the principles of a method for manufacturing a first sub-protective layer in different process steps provided by an embodiment of the present application, the manufacturing method includes:

[0083] First, as shown in FIG3 , a first precursor 11 is introduced, and a first atomic layer film 12 is formed based on the saturated chemical adsorption and reaction between the first precursor 11 and the surface of the device body 13.

[0084] Then, as shown in FIG. 4 , the first precursor 11 is exhausted by purging.

[0085] As shown in FIG. 5 , a second precursor 14 is introduced, and a second atomic layer film 15 is formed based on saturated chemical adsorption and reaction between the second precursor 14 and the surface of the first atomic layer film 12 .

[0086] As shown in FIG6 , the second precursor 14 is discharged by purging.

[0087] In the methods shown in Figures 3-6, the formation of the first sub-protective layer is illustrated using the formation of two atomic layer thin films as an example. As mentioned above, in the embodiments of the present application, the number of cycles for depositing the atomic layer thin film can be set based on demand, enabling accurate control of the thickness of the first sub-protective layer. The precursors used for different atomic layer thin films can be the same or different, and the precursor composition is set based on the reaction requirements, which is not limited in the embodiments of the present application.

[0088] In an embodiment of the present application, the first protective layer includes at least a first sub-protective layer formed based on an atomic layer deposition process, which is used to protect the surface of the device body and prevent the surface of the device body from being corroded by reactive gases and plasma. Compared with conventional limited coating methods such as CVD and PVD, the first sub-protective layer formed by the atomic layer deposition process has the following advantages: the first sub-protective layer is a pinhole-free dense film formed by low-temperature deposition, which can effectively avoid erosion by reactive gases and plasma; it can form a large film on the surface of various device bodies with complex shapes in all directions; it can precisely control the composition and thickness of the film, and the thickness can be increased from 1nm to more than 10μm; the film has excellent penetration, and the width-to-depth ratio of the film can reach more than 1:200, which is convenient for film formation on the inner surface of deep holes and pipes; the film has good bonding strength with the device body and good high temperature resistance.

[0089] In order to improve the interfacial bonding strength of the first sub-protective layer on the device body, before forming the first protective layer, the surface of the device body is pretreated so that the surface of the device body is modified to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0090] In order to improve the interfacial bonding strength of the first sub-protective layer on the surface of the equipment body, before forming the first sub-protective layer, the surface of the equipment body is also pretreated so that the thickness of the side of the equipment body to be coated is converted into a gentle transition layer. The first sub-protective layer has good adhesion stability in the gentle transition layer, so as to improve the adhesion stability of the first sub-protective layer on the surface of the equipment body.

[0091] Referring to FIG. 7 , FIG. 7 is a schematic flow chart of another method for coating a surface of a semiconductor device provided in an embodiment of the present application. The method comprises:

[0092] Step S31: providing a device body to be coated.

[0093] Step S32: pre-treating the surface of the device body to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0094] Step S33: forming a first protective layer on the surface of the device body; wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process (ALD).

[0095] Based on the method shown in FIG1 , in the method shown in FIG7 , pre-treating the surface of the device body before forming the first protective layer can improve the adhesion stability of the first sub-protective layer on the surface of the device body.

[0096] Optionally, the method for pre-treating the surface of the device body includes: performing a first plasma immersion process to modify the surface of the device body, so that a gentle transition layer with a gradual change in doping components is formed on the surface of the device body.

[0097] The first plasma immersion process is used to place the device body in a plasma immersion environment, and the surface of the device body is modified, which can achieve all-round surface modification. It can be applicable to the surface modification of device bodies with complex geometric surfaces, inner and outer walls of cylindrical tubes, and inner surfaces of fine pores, so as to improve the surface bonding strength of the first protective layer.

[0098] Compared with the method of directly forming a protective layer on the surface of the device body based on the atomic layer deposition process, the method shown in Figure 7 combines the plasma immersion process and the atomic layer deposition process, and can perform high-quality all-round coating on the surface of the device body. The first protective layer formed on the surface of the device body has better interface bonding strength and controllable density with the surface of the device body within a certain thickness.

[0099] The process principle of plasma immersion process is shown in Figure 8.

[0100] Referring to FIG8 , which is a schematic diagram of the principle of a plasma immersion process provided in an embodiment of the present application, the device body 13 to be processed is placed in the reaction chamber 21 of the plasma immersion equipment. After evacuation through the vacuum port 211, the reaction gas is input into the reaction chamber 21 through the reaction gas supply device 23. The reaction chamber 21 is connected to one or more external plasma generating power supplies 22, which excite or ignite the reaction gas in the reaction chamber 21 to form a plasma. The device body 13 will be immersed and surrounded by the formed plasma. The device body 13 is placed on a tray. Based on the external signal source 24 connected to the tray, the device body 13 is given a pulse bias. As the density and bias of the plasma change, the charged ions and active chemical components in the plasma surrounding the device body 13 interact with the surface of the device body in all directions.

[0101] The inventors discovered that by adjusting the pulse bias voltage in the plasma immersion process, different process effects can be achieved. At ultra-high pulse bias voltages (>30kV), omnidirectional ion implantation (PIII) can be performed on the workpiece surface. Within an appropriate bias voltage range (5kV-35kV), surface alloying (PIIA) or surface doping (PIID) can be achieved. At relatively low negative bias voltages (<15kV), omnidirectional coating (PIID) can be achieved on the workpiece surface. At even lower bias voltages (<1kV), energetic ion bombardment cleaning (PIIC) can be performed on the workpiece surface. In addition, because PIID uses energetic ions to perform all-around coating on the workpiece surface at a relatively low bias voltage, it also has the function of ion beam assisted deposition (IBAD) and can form a dense thin film structure. Moreover, it can form films on workpiece surfaces at low temperatures (<300°C).

[0102] Because PIIP has these numerous functions, it can perform a full range of surface treatments on a wide range of materials (such as metals, plastics, and ceramics). Furthermore, the thin film formed on the surface of the equipment itself exhibits excellent interfacial bonding strength. This is because PIIP forms a chemically mild interfacial transition layer on the workpiece surface.

[0103] Although PIIP is not easy to form a uniform modified layer on the inner surface of some small-diameter (<1mm) non-penetrating blind holes due to the limitations of gas diffusion and the distribution of the plasma electric field, the technical solution of this application combines it with the atomic layer deposition process. The first sub-protective layer prepared by the atomic layer process can achieve all-round thin film protection. The surface pretreatment based on PIIP can further improve the interfacial bonding strength of the first sub-protective layer on the surface of the device body to a certain extent. Moreover, in semiconductor equipment, the device body used to accommodate reactive gases and plasma generally does not have blind holes with smaller diameters.

[0104] Referring to Figure 9, Figure 9 is a schematic diagram of the principle of modifying the surface of the device body provided by an embodiment of the present application, in which the plasma 10 is controlled by a pulse bias to modify the device body 13. Based on the above description, different modification treatments can be achieved on the surface of the device body by adjusting the pulse bias during the PIIP process. In the direction from the inside of the device body 13 to the surface to be coated (i.e., the direction from right to left in Figure 9), the device body 13 includes: a first injection zone, a second injection zone, and a surface film. The doping components in the first injection zone, the second injection zone, and the surface film increase in sequence. Among them, the first injection zone is the above-mentioned PIII doping process, the second injection zone is the above-mentioned PIIA doping process or surface alloying process, and the surface film is the above-mentioned PIID coating process. Among them, the doping depths of the first injection zone and the second injection zone in this direction are successively reduced, and the concentration of the doping component is successively increased, so that the surface of the device body 13 has a gentle transition layer with increasing doping components, which can improve the interface bonding force of the subsequently formed first sub-protective layer on the surface of the device body.

[0105] Based on the above description, in the surface coating method provided in the embodiment of the present application, a first plasma immersion process is used to modify the surface of the device body as shown in FIG10 .

[0106] Referring to FIG. 10 , FIG. 10 is a flow chart of a method for modifying the surface of a device body provided in an embodiment of the present application, the method comprising:

[0107] Step S41: performing ion implantation to a first depth into the surface of the device body under a first pulse bias voltage;

[0108] Step S42: performing ion implantation to a second depth into the surface of the device body under a second pulse bias voltage, and / or achieving surface alloying of the device body;

[0109] The second depth is smaller than the first depth.

[0110] The first pulse bias voltage forms a first implantation region on the surface of the device body, while the second pulse bias voltage forms a second implantation region or surface metallization on the surface of the device body. This creates a gradual transition layer with increasing dopant composition on the surface of the device body, enhancing the interfacial bonding strength of the subsequently formed first sub-protective layer on the device body surface. Furthermore, the gradual transition layer not only improves the interfacial bonding strength of the first sub-protective layer on the device body but also further enhances the corrosion and high-temperature resistance of the device body surface.

[0111] In other methods, the surface of the device body is modified, and a doping layer can also be formed on the surface of the device body based on the plasma immersion process. The doping layer can be a doping region with uniform doping components formed based on a constant pulse bias, such as a doping region formed based on a PIII process, or a doping region formed based on a PIIA process, or it can include both the above-mentioned first doping region and the second doping region, and the doping components of the two doping regions are gradually changed. Among them, the gradual change of the doping component refers to the gradual change of the concentration of the doping element. In this way, the interfacial bonding strength of the first sub-protective layer can also be improved to a certain extent.

[0112] In the embodiments of the present application, compared to a solution based on a single atomic layer deposition process to form a first protective layer on the surface of the device body, a solution combining a plasma immersion process and an atomic layer deposition process to form a first protective layer on the surface of the device body can improve the interfacial bonding strength between the first protective layer and the device body based on the gentle transition layer formed on the surface of the device body by the plasma immersion process. Moreover, compared to the plasma immersion process, the atomic layer deposition process has a higher film coverage width-to-depth ratio, making it easier to form a uniform film coverage on the surface of a device body with complex structures and internal pores, and the film thickness control accuracy is very high (the thickness variation is generally less than 5%).

[0113] Optionally, based on any of the above methods, in the surface coating method provided in the embodiment of the present application, the method for forming the first protective layer also includes: forming a second sub-protective layer on the surface of the first sub-protective layer using a second plasma immersion process. The protective layer is provided to include a first sub-protective layer and a second sub-protective layer, and the equipment body can be protected against corrosion by the protective layer when a first sub-protective layer of smaller thickness is used. The thickness of the second sub-protective layer can be 50nm-15μm. Furthermore, when the thickness of the second sub-protective layer can be set to 500nm-1μm, the first protective layer can achieve better corrosion protection.

[0114] Since the atomic layer deposition process forms thin films slowly, and the cost rises rapidly as the thickness of the film increases, the thickness of the first sub-protective layer formed based on the atomic layer deposition process is generally thin, and the thickness of the first sub-protective layer is less than 2000nm. In some cases, the thickness of the first sub-protective layer is less than or equal to 500nm. If the thickness of the first sub-protective layer is too large, it will not only lead to a significant increase in production costs, but also cause the film grains to become coarse and the surface structure to coarsen. In order to improve the quality of the all-round protective layer on the surface of the equipment body and expand the application range of the all-round protective layer, the embodiment of the present application provides a second sub-protective layer prepared based on a plasma immersion process on the first sub-protective layer to increase the thickness of the first protective layer. In this way, a thinner first sub-protective layer can be formed based on the atomic layer deposition process to achieve better corrosion protection effect.

[0115] Optionally, a second plasma immersion process is used to form a second sub-protective layer on the surface of the first sub-protective layer, including: performing a full-scale coating on the surface of the device body having the first sub-protective layer formed thereon under a negative bias voltage of less than 15 kV to form the second sub-protective layer. In this case, a surface film layer can be formed on the surface of the device body based on the aforementioned PIID process.

[0116] In order to further improve the corrosion resistance of the device body, the surface coating method also includes: forming a second protective layer on the surface of the first protective layer; wherein the thickness of the second protective layer can be greater than the thickness of the first protective layer.

[0117] Optionally, the method for forming the second protective layer includes forming the second protective layer using a plasma-enhanced physical vapor deposition process. For a device body having a relatively small-diameter pore, the thinner first protective layer covers the entire surface of the device body, including the inner wall of the pore, while the thicker second protective layer covers the outer surface of the pore and the inner wall near the pore opening.

[0118] Plasma-enhanced physical vapor deposition (PEPD) is essentially a surface thin-film deposition process that combines physical vapor deposition (PVD) with plasma-enhanced processes. PVD can be performed through vacuum evaporation, ion-bombarded sputtering, magnetron sputtering, and other methods, while plasma-enhanced deposition is achieved through ion bombardment in the plasma and ion beam bombardment. The ion bombardment breaks weak atomic bonds during film growth, promoting surface diffusion of atoms and forming a dense, uniformly oriented crystalline or amorphous structure. Therefore, compared to films produced by other thin-film deposition processes such as evaporation and plasma spraying, films produced by PEPD have a denser structure and significantly enhanced resistance to plasma etching. Furthermore, due to its integration of PVD and plasma processes, PEPD can be performed on device surfaces at relatively low temperatures (<200°C) and can achieve film thicknesses exceeding 150μm. This makes it ideal for depositing sufficiently thick (>20μm) ceramic films such as Y2O3 on aluminum alloy surfaces.

[0119] The surface coating method described in the embodiment of the present application is further explained below by taking the device body being a shower head as an example.

[0120] Referring to Figures 11-13, Figure 11 is a top view of the device body, Figure 12 is a cross-sectional view of the device body shown in Figure 11, and Figure 13 is a partially enlarged view of the device body shown in Figure 11. In the methods shown in Figures 11-13, the device body 13 is a spray head having air holes 131. No protective layer is provided on the surface of the device body 13, which makes the surface of the device body 13 susceptible to corrosion by reaction gases and plasma.

[0121] The thickness of the shower head is generally 3 mm to 100 mm, and the diameter of the air holes 131 can range from 0.04 mm to 100 mm. In some shower heads, the diameter of the air holes 131 can be greater than 100 mm. In the embodiment of the present application, the air holes 131 are uniform in diameter for illustration. In other embodiments, the air holes 131 can also be connected by pipes of different diameters.

[0122] Refer to Figure 14, which is a partially enlarged view of a device body formed with a corrosion-resistant protective layer based on the coating method of an embodiment of the present application. Based on the methods shown in Figures 11 to 13, in the method shown in Figure 14, a first protective layer 31 is formed on the surface of the device body 13, and the first protective layer 31 includes a first sub-protective layer 311. The first sub-protective layer 311 formed based on the atomic layer deposition process has excellent film penetration, and the width-to-depth ratio of the thin film can reach more than 1:200, so it can form a full-range thin film coverage on the surface of the device body 13 to form a good corrosion-resistant protective layer.

[0123] Refer to Figure 15, which is another partially enlarged view of a device body formed with a corrosion-resistant protective layer based on the coating method of an embodiment of the present application. Based on the method shown in Figure 14, in the method shown in Figure 15, before forming the first protective layer 31, the surface of the device body 13 is pretreated to form a modified layer 32 to improve the interface bonding strength of the first protective layer 31 on the device body 13.

[0124] Referring to FIG16 , FIG16 is another partially enlarged view of a device body having a corrosion-resistant protective layer formed thereon according to the coating method of an embodiment of the present application. In addition to the method shown in FIG15 , FIG16 further includes a second sub-protective layer 312 formed on the surface of the first sub-protective layer 311. As described above, the first sub-protective layer 311 is limited by the atomic layer deposition process, resulting in a slow film formation speed and the inability to form a film of greater thickness. This method further includes forming a second sub-protective layer 312 on the surface of the first sub-protective layer 311, thereby achieving better corrosion resistance based on the thinner first sub-protective layer 311.

[0125] Refer to Figure 17, which is another partially enlarged view of a device body having a corrosion-resistant protective layer formed based on the coating method of an embodiment of the present application. Based on the method shown in Figure 16, in the method shown in Figure 17, a second protective layer 33 prepared based on the PEPVD process is also formed on the surface of the first protective layer 31.

[0126] As can be seen from the above description, the surface coating method described in the technical solution of the present application is based on the modified layer 32 formed on the surface of the device body 13 by the plasma immersion process. The modified layer 32 is a gentle transition layer with a gradual change in doping components, which is used to enhance the interfacial bonding strength of the first sub-protective layer 311 formed subsequently. The modified layer 32 formed by the plasma immersion process facilitates the formation of a dense first sub-protective layer 311. Compared with the plasma immersion process, the first sub-protective layer 311 formed by the atomic layer deposition process has a very high film coverage width-to-depth ratio. Therefore, the surface coating method provided by the technical solution of the present application uses the atomic layer deposition process to form a first sub-protective layer 311 with uniform thickness and composition on the modified layer 32 formed by the plasma immersion process, which can cover the entire outer surface of the device body 13 and the inner surface of the pores 131. In order to ensure that the final all-round surface protective layer has a fine and dense microstructure, a second sub-protective layer 312 is prepared on the first sub-protective layer 311 based on the plasma immersion process to further increase the thickness of the first protective layer 31. The surface protection layer prepared in this way is very suitable for the surface protection of flat workpieces used in semiconductor coating equipment such as PVD and CVD, such as shower heads made of aluminum alloy.

[0127] In the embodiment of the present application, the first protective layer 31 comprises a ceramic film, forming a fully covered ceramic protective film on the surface of the device body 13. The first sub-protective layer 311 is a ceramic film. When the first protective layer 31 also includes a second sub-protective layer 312, the second sub-protective layer 312 is also a ceramic film.

[0128] To enhance the structural stability of the fully covered first protective layer 31 formed on the surface of the device body 13 and to meet the operating requirements of the operating environment, a plasma-resistant film with a chemical composition and structural structure similar to that of the material of the device body 13 is preferably deposited on the surface of the device body 13 as the first sub-protective layer 311 bonded to the device body 13. When the first sub-protective layer 311 is a ceramic film, the alloying elements in the ceramic film are the same as those of the material of the device body 13. When the ceramic film is deposited on the surface of the device body 13, it exhibits reduced interfacial deformation stress, which helps improve the structural stability of the formed ceramic film. For example, when the device body 13 is made of an aluminum alloy, an Al2O3 film is deposited on its surface as the first sub-protective layer 311; when the device body 13 is made of a silicon substrate, a SiC film is deposited on its surface as the first sub-protective layer 311; and when the device body 13 is made of an yttrium alloy, a Y2O3, YF3, or YOF film is deposited on its surface as the first sub-protective layer 311.

[0129] When the first sub-protective layer 311 is a ceramic film, the alloying elements in the ceramic film are the same as the material of the device body 13, which can also enhance the interfacial bonding between the ceramic film and the device body 13. The amorphous structure of the ceramic film can effectively prevent trace elements in the device body 13 from diffusing to the surface of the ceramic film, thereby reducing trace element contamination caused by the device body 13 during use of the semiconductor device. For aluminum alloy showerheads commonly used in high-temperature conditions, such as those used in PVD and CVD equipment, which may have operating temperatures exceeding 150°C or even 300°C, the amorphous, all-around ceramic film used as the first sub-protective layer 311 can effectively reduce trace element contamination.

[0130] In the semiconductor device improved by the embodiment of the present application, the first sub-protective layer 311 is a multi-layer thin film structure. By setting the thin film properties and the formation order, the required protection device body 13 has a very excellent performance combination in different usage environments.

[0131] Taking the aluminum alloy device body 13 as an example, the first sub-protective layer 311 comprises an alumina ceramic film. Oxygen ion implantation can be performed on the surface of the device body 13 to form a doped layer, which serves as a modified layer 32 to enhance the interfacial bonding strength of the subsequently formed alumina film. After the modified layer 32 is formed on the surface of the device body 13, an amorphous alumina ceramic film is formed on the surface of the modified layer 32. This not only enhances the surface corrosion resistance of the aluminum alloy device body 13, but also prevents alloying elements in the aluminum alloy from diffusing to the surface, thereby enhancing the surface structural stability of the device body 13 and reducing trace element contamination.

[0132] The first sub-protective layer 311 at least includes a first ALD film located on the surface of the device body 13 and a second ALD film located on the surface of the first ALD film. The first ALD film is in contact with the surface of the device body.

[0133] The second ALD film has stronger corrosion resistance than the first ALD film, and the two films have similar thermal expansion coefficients. Thus, the second ALD film can further enhance the corrosion resistance of the first sub-protective layer 311. For example, the first ALD film is made of aluminum oxide, and the second ALD film is made of yttrium oxide. The material properties of the two films are shown in Table 1.

[0134] Table 1

[0135] Table 1 lists the thermal expansion coefficients of the materials at 200-1000°C and the thermal conductivity coefficients at 20°C. As shown in Table 1, the thermal expansion coefficients of aluminum oxide and yttrium oxide are very similar, while yttrium oxide exhibits significantly higher plasma corrosion resistance than aluminum oxide in various plasma environments (such as those containing O₂, F, Cl, and HBr). Therefore, depositing an yttrium oxide film on the surface of the aluminum oxide film can further enhance the corrosion resistance of the first protective layer 31, improving the process stability of the device body 13 (e.g., showerhead) and its application range in various semiconductor devices.

[0136] To further enhance the bonding strength between the second ALD film and the first ALD film, a transition layer can be formed between them. For example, if the first ALD film is amorphous aluminum oxide and the second ALD film is crystalline yttrium oxide, the transition layer can be a crystalline aluminum oxide film. In this case, the multilayer film structure of the first subprotective layer 311 includes amorphous aluminum oxide / crystalline aluminum oxide / crystalline yttrium oxide.

[0137] In order to improve other properties of the first sub-protective layer 311, such as thermal conductivity and electrical conductivity, a thermally conductive / electrically conductive film can be added to the first sub-protective layer 311 so that the first sub-protective layer 311 has good thermal conductivity / electrical conductivity while achieving corrosion resistance, thereby forming a multifunctional first sub-protective layer 311. Ions can also be implanted into the single-element film in the first sub-protective layer 311 to change the film properties. The thickness of the first sub-protective layer 311 and the combination of the thicknesses of different films can be set according to different process conditions and the properties of the film materials, and the embodiments of the present application are not limited to this.

[0138] From the above description, it can be seen that the surface coating method provided by the technical solution of the present application can be used to perform surface coating on workpieces with complex structural surfaces in semiconductor equipment, such as for surface coating of shower heads, cylindrical workpieces and gas pipe-type workpieces. Combining the atomic layer deposition process and the plasma immersion process can achieve all-round coating of the surface of the equipment body, effectively solving the surface protection problem of workpieces with complex structural surfaces in semiconductor equipment.

[0139] This surface coating method exploits the versatility of the plasma immersion process and improves the bonding strength and surface density of all-around thin films based on PIII and PIID. It can effectively improve the quality of thin films formed by single ALD, enhance the structural stability of all-around thin films, reduce the particle and trace element contamination generated by the corrosion of reactive gases or plasma on the surface of workpieces such as protected cavity workpieces, and improve the process stability of semiconductor equipment.

[0140] Moreover, this surface coating method can prepare multi-layer atomic layer films on the surface of the device body according to the working environment requirements of the semiconductor device and the mutual matching compatibility of the organizational structure and performance of different thin film materials, using the stability and process controllability of the ALD process to prepare thin films; through the design of thin film materials, an interface layer with strong bonding force, a ceramic film with surface resistance to plasma corrosion, and a multi-layer structure with special functions (heat resistance / thermal conductivity / electrical conductivity, etc.) are formed on the surface of the device body to meet the working requirements of different semiconductor devices.

[0141] Furthermore, based on the plasma etching characteristics of the semiconductor device, combined with the PEPVD process, a second protective layer with a larger thickness can be deposited on the surface of the prepared all-round covering first protective layer to further improve the plasma corrosion resistance, improve the critical service life and process stability of plasma etching.

[0142] Based on the above-mentioned surface coating method embodiment, another embodiment of the present application further provides a semiconductor device, such as the aforementioned semiconductor device, including but not limited to thin film deposition equipment and plasma etcher. The semiconductor device includes: a device body, which can be a flat workpiece in the semiconductor device, such as a showerhead, or other transmission pipelines, or a reaction chamber.

[0143] 14 , the semiconductor device includes: a device body 13 , a first protective layer 31 covering the device body 13 , and the first protective layer 31 includes at least a first sub-protective layer 311 formed based on an atomic layer deposition process.

[0144] Optionally, in the embodiment of the present application, the first protective sub-layer 311 includes multiple atomic layer films stacked in sequence. Based on the number of atomic layer depositions, the thickness of the first protective sub-layer 311 can be precisely controlled.

[0145] 15 , the surface of the device body is modified so that a certain thickness portion of the surface of the device body serves as a modified layer 32 to improve the adhesion stability of the first sub-protective layer 311 on the surface of the device body 13 .

[0146] In combination with the embodiment shown in FIG. 16 , the first protective layer 31 further includes: a second sub-protective layer 312 located on the surface of the first sub-protective layer 311 ; wherein the second sub-protective layer 312 is a film layer formed by a plasma immersion process.

[0147] In the embodiment of the present application, the first protective layer 31 comprises a ceramic film, thereby forming a fully covered ceramic protective film on the surface of the device body 13. The first sub-protective layer 311 can be a ceramic film. When the first protective layer 31 also includes a second sub-protective layer 312, the second sub-protective layer 312 is a ceramic film.

[0148] Among them, the materials of ceramic films include: Al2O3, Y2O3, YF3, YOF (such as Y5O4F7), ZrO2, Er2O3, SiC, SiO2, HfO2, Si3N4, AlN, B2O3, Nd2O3, Nb2O5, CeO2, Sm2O3, Yb2O3, Y3Al5O 12 (YAG), Er3Al5O 12 One or more of (EAG), Y4Al2O9(YAM), YAlO3(YAP), Er4Al2O9(EAM) and ErAlO3(EAP), or composite ceramic films based on these ceramic materials, have the common characteristics of being resistant to plasma corrosion, having stable performance, and having corrosion resistance and stability far superior to aluminum alloy workpiece materials.

[0149] In combination with the embodiment shown in FIG17 , the semiconductor device further includes: a second protective layer 33 located on the surface of the first protective layer 31 ; optionally, the second protective layer 33 is a plasma enhanced physical vapor deposition film.

[0150] The thickness of the second protective layer 33 may be greater than that of the first protective layer 31. Alternatively, the thickness of the second protective layer 33 may be less than that of the first protective layer 31 by setting the coating time of the coating process.

[0151] The thickness of the first protective layer 31 is less than 25 μm, and the thickness of the second protective layer 33 is greater than 10 μm.

[0152] Optionally, the second protective layer 33 is a ceramic film. The material of the ceramic film can be as described above and will not be repeated here.

[0153] The thickness of the first protective layer 31 produced using atomic layer deposition and plasma immersion processes is generally thin, often less than 10 μm or even less than 2 μm. Therefore, during plasma etching, the first protective layer 31 may be corroded by the plasma due to its thinness. This problem can be resolved by adding a thicker second protective layer 33 on the surface of the first protective layer 31.

[0154] The second protective layer 33 is a dense plasma corrosion-resistant film prepared by PEPVD process, with a thickness greater than 10 μm, such as 20 μm-150 μm. The second protective layer 33 prepared by PEPVD process has good density, no defects, and is resistant to plasma corrosion.

[0155] FIG17 illustrates the device body 13 as a showerhead. The showerhead is made of aluminum alloy. After forming a first protective layer 31 on its surface, a thicker second protective layer 33 is deposited using a PEPVD process. The second protective layer 33 may be made of materials such as Y2O3 or YF3. The showerhead surface coating structure may include a modified layer 32 prepared using a PIIP process, amorphous aluminum oxide (amorphous Al2O3, or α-Al2O3) and crystalline yttrium oxide (Y2O3) prepared using an ALD process, and a thick Y2O3 film prepared using a PEPVD process. This provides the showerhead surface in contact with the plasma with a thick, dense, plasma-resistant protective layer, ensuring the showerhead's service life. The thin first protective layer 31, which covers the entire surface of the showerhead's pores, protects against corrosion from the reactive gases, thereby preventing metal and particle contamination during showerhead operation. Therefore, when the technical solution of the present application is used in a shower head, it can significantly improve the long-term process stability of semiconductor equipment using the shower head, thereby achieving the purpose of improving production efficiency.

[0156] The various embodiments in this specification are described in a progressive, parallel, or combined manner. Each embodiment focuses on the differences from other embodiments, and reference can be made to the corresponding similar parts between the various embodiments. With respect to the semiconductor device disclosed in the embodiments, since it corresponds to the surface coating method disclosed in the embodiments, the description is relatively simple. For relevant parts, reference can be made to the relevant description of the surface coating method.

[0157] It should be noted that in the description of this application, it should be understood that the description of the drawings and embodiments is illustrative rather than restrictive. The same figure numbers throughout the embodiments of the specification identify the same structure. In addition, for the purpose of understanding and ease of description, the drawings may exaggerate the thickness of some layers, films, panels, regions, etc. It is also understood that when an element such as a layer, film, region or substrate is referred to as "on" another element, the element may be directly on the other element or there may be an intermediate element. In addition, "on" refers to positioning an element on or below another element, but does not essentially mean positioning on the upper side of another element according to the direction of gravity.

[0158] The terms "upper," "lower," "top," "bottom," "inner," "outer," and the like, indicating positions or locations, are based on the positions or locations shown in the accompanying drawings and are intended solely to facilitate and simplify the description of this application. They are not intended to indicate or imply that the devices or elements referred to must have a specific orientation, be constructed, or operate in a specific orientation. Therefore, they should not be construed as limitations on this application. When a component is considered to be "connected" to another component, it may be directly connected to the other component or there may be a centrally located component.

[0159] It should also be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that an article or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or elements inherent to such article or device. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of additional identical elements in the article or device comprising the aforementioned elements.

[0160] The above description of the disclosed embodiments is intended to enable one skilled in the art to implement or use the present application. Various modifications to these embodiments will be readily apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application is not limited to the embodiments shown herein, but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A surface coating method for semiconductor equipment, It is characterized in that include: Provide the equipment body to be coated; A first protective layer is formed on the surface of the device body; wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

2. The surface coating method according to claim 1, It is characterized in that The method of forming the first sub-protection layer includes: An atomic layer deposition process is adopted to sequentially form multiple layers of atomic layer films on the surface of the device body as the first sub-protective layer.

3. The surface coating method according to claim 2, It is characterized in that The method of forming the first sub-protection layer includes: forming a first atomic layer film based on saturated chemical adsorption and reaction between the first precursor and the surface of the device body; forming another atomic layer film based on saturated chemical adsorption and reaction between the second precursor and the surface of the previous atomic layer film; Before forming a next atomic layer film, the precursor used to form the previous atomic layer film is purged and discharged.

4. The surface coating method according to claim 1, It is characterized in that Before forming the first protective layer, the method further includes: The surface of the device body is pretreated to improve the adhesion stability of the first sub-protection layer on the surface of the device body.

5. The surface coating method according to claim 4, It is characterized in that The method for pre-treating the surface of the device body comprises: The surface of the device body is modified by a first plasma immersion process, so that a gentle transition layer with a gradual change of doping components is formed on the surface of the device body.

6. The surface coating method according to claim 5, It is characterized in that The surface of the device body is modified by a first plasma immersion process, including: Under a first pulse bias, ion implantation to a first depth is performed into the surface of the device body; Under a second pulse bias, ion implantation to a second depth is performed into the surface of the device body, and / or surface alloying of the device body is achieved; Wherein, the second depth is smaller than the first depth.

7. The surface coating method according to claim 2, It is characterized in that The method of forming the first protective layer further includes: A second plasma immersion process is used to form a second sub-protecting layer on the surface of the first sub-protecting layer.

8. The surface coating method according to claim 7, It is characterized in that Using a second plasma immersion process to form a second sub-protective layer on the surface of the first sub-protective layer includes: Under a negative bias voltage less than 15 kV, an all-round coating is performed on the surface of the device body formed with the first sub-protective layer to form the second sub-protective layer.

9. The surface coating method according to any one of claims 1 to 8, It is characterized in that Also includes: forming a second protective layer on a surface of the first protective layer; Wherein, the thickness of the second protective layer is greater than the thickness of the first protective layer.

10. The surface coating method according to claim 9, It is characterized in that The method of forming the second protective layer includes: The second protective layer is formed by a plasma enhanced physical vapor deposition process.

11. A semiconductor device, It is characterized in that include: Equipment body; A first protective layer covers the device body, wherein the first protective layer at least includes a first sub-protective layer formed based on an atomic layer deposition process.

12. The semiconductor device according to claim 11, It is characterized in that The first sub-protection layer includes a plurality of atomic layer films stacked in sequence.

13. The semiconductor device according to claim 11, It is characterized in that The surface of the device body is modified to improve the adhesion stability of the first sub-protective layer on the surface of the device body.

14. The semiconductor device according to claim 11, It is characterized in that The first protective layer further includes: a second sub-protective layer located on the surface of the first sub-protective layer; Wherein, the second sub-protective layer is a film layer formed by a plasma immersion process.

15. The semiconductor device according to claim 11, It is characterized in that The first protection layer includes a ceramic film.

16. The semiconductor device according to claim 11, It is characterized in that Also includes: A second protective layer is located on a surface of the first protective layer.

17. The semiconductor device according to claim 16, It is characterized in that The second protective layer is a plasma enhanced physical vapor deposition film.

18. The semiconductor device according to claim 16, It is characterized in that The thickness of the first protective layer is less than 25 μm, and the thickness of the second protective layer is greater than 10 μm.

19. The semiconductor device according to claim 16, It is characterized in that The second protective layer is a ceramic film.

20. The semiconductor device according to claim 16, It is characterized in that The thickness of the second protective layer is greater than that of the first protective layer.

Citation Information

Patent Citations

  • Treatment method for film deposition reaction cavity and film deposition method

    CN104073775A

  • Gas distributing plate

    CN104701125A

  • Multi-layer plasma resistant coating by atomic layer deposition

    CN108330467A

  • Yttrium oxide based surface coating for semiconductor IC processing vacuum chambers

    US6776873B1