Modified inorganic fiber material and preparation method therefor, automobile roof lining composite material, sound insulation composite material, and vehicle
Through the coating and freeze-drying process of modified inorganic fiber materials, the problem of insufficient sound absorption and noise reduction function of existing automobile ceiling materials is solved, significant noise reduction and passenger comfort improvement are achieved, and the preparation process is simple and easy to perform.
Patent Information
- Application Number
- PCT/CN2024/093718
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-21
AI Technical Summary
The existing car ceiling materials have shortcomings in improving sound absorption and noise reduction functions, and have failed to effectively improve the material level, resulting in poor noise control in the car and affecting passenger comfort.
Modified inorganic fiber material is used, which is distributed in the three-dimensional network structure by adhesive bonding and distributing it through a coating and freeze-drying process to improve the sound absorption and noise reduction performance of the material.
It significantly improves the sound absorption coefficient and provides efficient sound absorption and noise reduction function. It can significantly reduce the noise inside the car without changing the preparation process of the car ceiling composite material and improve passenger comfort. The preparation method is simple and easy to operate, and there is no need for special operations. equipment.
Smart Images

Figure CN2024093718_21112024_PF_FP_ABST
Abstract
Description
Modified inorganic fiber material and preparation method thereof, automobile roof composite material, sound insulation composite material and vehicle
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 17, 2023, with application number 202310557936.3 and invention name “A modified inorganic fiber material, its preparation method and automobile roof composite material”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The invention relates to a modified inorganic fiber material and a preparation method thereof, an automobile roof composite material, a sound insulation composite material and a vehicle, and belongs to the field of materials, in particular to the technical field of related materials used in automobiles. Background Art
[0003] With the development and progress of society and the improvement of people's living standards, cars have become a common consumer product and have become increasingly commonplace in thousands of households. At the same time, consumers are increasingly concerned about and demanding higher levels of noise and vibration control within their vehicles. NVH (noise vibration harshness) is a passenger's subjective perception of a vehicle through auditory, tactile, and visual factors. NVH performance is the most perceptible aspect of a vehicle and is a key indicator of vehicle quality.
[0004] The car roof is a key component of the interior, significantly enhancing the aesthetic quality of the vehicle's interior while also providing thermal insulation and noise reduction, thereby enhancing passenger comfort. Due to its large surface area, the roof significantly impacts the absorption of interior noise. Therefore, developing highly effective sound-absorbing and noise-reducing roof materials is crucial for significantly reducing interior noise and improving passenger comfort.
[0005] Some companies have made some attempts and efforts to enhance and improve the sound absorption and noise reduction functions of car roofs, as follows.
[0006] CN103921504A discloses a novel automobile roof and its production process. The novel automobile roof disclosed in the invention is composed of a composite knitted fabric, glass fiber felt, foam board, glass fiber felt and a bottom non-woven fabric from top to bottom, and each layer is compounded by a film. The process for producing the novel automobile roof as described above combines the advantages of the simple process and fast production cycle of the dry molding process, and the advantages of the wet molding process such as better product molding performance than the dry process ceiling and lightweight products. The molding process is also a dry wet molding (cold material hot mold) molding process. This prior art reduces the VOC performance of the product and improves the NVH performance of the product, and has the advantages of good product molding performance, lightweight products, improved product production cycle, and less pollution to the production environment.
[0007] CN211417409U discloses a composite car roof, comprising a carbon fiber composite roof body and a sunroof frame. The left end of the carbon fiber composite roof body is adhesively connected to a front reinforcement, and the right end of the carbon fiber composite roof body is adhesively connected to a rear reinforcement, and the sunroof frame is located inside the left end of the carbon fiber composite roof body. Compared with existing ordinary car roofs, this composite car roof can reduce the weight of the car, making the car lightweight, thereby achieving the effect of energy conservation and emission reduction, improving the environmental friendliness of the car roof, and improving the rigidity and aging resistance of the car roof, thereby improving the dent resistance and service life of the car roof. At the same time, it also increases the specific modulus of the car roof, improves the NVH performance of the car roof, and improves the damping of the car roof and the sound insulation performance of the car roof. At the same time, it adopts a wet molding process.
[0008] However, both of these existing technologies improve the preparation process of the automobile roof, but do not improve the sound absorption and noise reduction functions of the materials used in the automobile roof.
[0009] Therefore, providing a novel modified inorganic fiber material and a preparation method thereof, and an automobile roof composite material, a sound insulation composite material and a vehicle comprising the modified inorganic fiber material has become a technical problem that urgently needs to be solved in the field.
[0010] Summary of the Invention
[0011] In order to solve the above-mentioned shortcomings and deficiencies, an object of the present invention is to provide a modified inorganic fiber material.
[0012] Another object of the present invention is to provide a method for preparing the modified inorganic fiber material.
[0013] Another object of the present invention is to provide a composite material for automobile roof, wherein the inorganic fiber material layer is made of the modified inorganic fiber material described above.
[0014] Another object of the present invention is to provide a sound insulation composite material, wherein the inorganic fiber material layer is made of the modified inorganic fiber material described above.
[0015] The final object of the present invention is to provide a vehicle comprising the above-mentioned sound insulation composite material.
[0016] To achieve the above objectives, the present invention provides a modified inorganic fiber material, wherein the modified inorganic fiber material comprises a porous inorganic fiber material and a porous powder material, wherein the porous powder material is distributed in a three-dimensional network structure on the surface of the porous inorganic fiber material and in the interior space thereof by bonding with an adhesive;
[0017] The content of the porous powder material and adhesive is 10-200 g / m 2 , the content = (CB) / A, where A and B are the surface area and mass of the porous inorganic fiber material, respectively, in units of m 2 and g, C is the total weight of the modified inorganic fiber material, in g.
[0018] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the modified inorganic fiber material is prepared by first uniformly mixing a porous powder material, an adhesive, an additive and water to obtain a mixed slurry, then uniformly coating the mixed slurry on the surface of the porous inorganic fiber material, and then freeze-molding and vacuum freeze-drying.
[0019] As a specific embodiment of the modified inorganic fiber material of the present invention, the porous inorganic fiber material has a loose porous three-dimensional network structure, a thickness of 80-600 μm, and a gram weight of 20-200 g / m 2 .
[0020] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the porous inorganic fiber material includes glass fiber, ceramic fiber, basalt fiber, carbon fiber, quartz fiber, asbestos fiber, volcanic rock fiber, metal fiber or alumina fiber.
[0021] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the porous powder material is a porous powder material with sound absorption and noise reduction functions, including one or a combination of zeolite molecular sieve, activated silica, activated carbon, surface porous calcium carbonate and surface porous calcium silicate.
[0022] In order to enhance the sound absorption and noise reduction effect of the modified inorganic fiber material to a greater extent, as a specific embodiment of the modified inorganic fiber material described above in the present invention, the zeolite molecular sieve includes one or a combination of MFI structure molecular sieve, FER structure molecular sieve, CHA structure molecular sieve, MEL structure molecular sieve, TON structure molecular sieve and MTT structure molecular sieve.
[0023] As a specific embodiment of the modified inorganic fiber material of the present invention, the particle size of the zeolite molecular sieve is 0.5-10 μm.
[0024] As a specific embodiment of the modified inorganic fiber material described above, the zeolite molecular sieve includes micropores with a pore size of 0.3-0.7 nm and mesopores with a pore size of 10-30 nm.
[0025] As a specific embodiment of the modified inorganic fiber material of the present invention, the zeolite molecular sieve is ZSM-5 molecular sieve.
[0026] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the adhesive includes an organic adhesive and / or an inorganic adhesive; the organic adhesive includes one or a combination of polyacrylate, acrylic copolymer, polyurethane, polystyrene butadiene emulsion, polystyrene acrylate, polystyrene acetate emulsion, polyvinyl acetate emulsion, silicone resin and polybutadiene rubber emulsion; the inorganic adhesive includes one or a combination of silica sol, aluminum sol, pseudo-boehmite, etc.
[0027] As a specific embodiment of the modified inorganic fiber material of the present invention, the thickness of the modified inorganic fiber material is determined by the porous inorganic fiber material, and therefore the thickness range is also 80-600 μm.
[0028] On the other hand, the present invention also provides a method for preparing the modified inorganic fiber material described above, wherein the preparation method comprises:
[0029] (1) uniformly mixing the porous powder material, adhesive, additive and water to obtain a mixed slurry;
[0030] (2) uniformly coating the mixed slurry on the surface of a porous inorganic fiber material;
[0031] (3) Drying the product obtained in step (2) to obtain the modified inorganic fiber material.
[0032] In step (2) of the preparation method of the modified inorganic fiber material described above, the mixed slurry can be evenly coated on one side surface of the porous inorganic fiber material. After coating, the mixed slurry will enter the interior of the porous inorganic fiber material and then diffuse to the other side surface of the porous inorganic fiber material. Alternatively, the mixed slurry can be evenly coated on both sides of the porous inorganic fiber material at the same time. After coating, the mixed slurry will enter the interior of the porous inorganic fiber material. Under the premise that the coating amount, that is, the mass of the absolute dry coating (porous powder material and adhesive in the present invention) per unit area is the same, the effects of these two coating methods are the same. It can be seen that no matter which coating method is adopted, both sides of the inorganic fiber material are modified.
[0033] As a specific embodiment of the preparation method described above in the present invention, the mass ratio of the porous powder material, adhesive, water and additive is 100:4-10:1-159:1-159, preferably 100:5-8.5:5-95:5-95, and the amount of the porous powder material, adhesive and additive is calculated based on the absolute dry mass of the active ingredient.
[0034] As a specific embodiment of the above-mentioned preparation method of the present invention, the auxiliary agent is a liquid auxiliary agent that can be frozen at -30°C to -50°C and can sublime at a temperature of 60-80°C and a vacuum degree of less than 15Pa.
[0035] As a specific embodiment of the above preparation method of the present invention, wherein, under the condition of a temperature of 20° C., the viscosity of the liquid additive is not less than 500 cp.
[0036] As a specific embodiment of the preparation method described above of the present invention, the auxiliary agent includes one or a combination of ethylene glycol (melting point of -13°C, boiling point of 194°C / 760 mmHg), 2,3-butanediol (melting point of 18°C, boiling point of 179°C / 760 mmHg), 1,4-butanediol, 1,3-butanediol and 1,5-pentanediol.
[0037] The auxiliary agent used in the present invention is a high-viscosity liquid auxiliary agent. By adjusting its added amount, the purpose of adjusting the viscosity of the mixed slurry can be achieved, so that the viscosity of the mixed slurry meets the needs of the coating operation; at the same time, during the molding and drying process of the modified inorganic fiber material, it is easy to separate from the porous inorganic fiber material, porous powder material and adhesive, and does not affect the acoustic properties of the modified inorganic fiber material; and for the auxiliary agents commonly used in this field, such as starch, polyvinyl alcohol, carboxymethyl cellulose, and synthetic coating thickeners, although the purpose of adjusting the viscosity of the mixed slurry can also be achieved by adjusting its added amount, these substances do not volatilize during the molding and drying process of the modified inorganic fiber material, and they will be adsorbed by the porous powder material, thereby having a serious negative impact on the acoustic properties and sound absorption and noise reduction performance of the modified inorganic fiber material.
[0038] As a specific embodiment of the above-mentioned preparation method of the present invention, the viscosity of the mixed slurry is 30-800cp.
[0039] As a specific embodiment of the above-mentioned preparation method of the present invention, the water includes one or a combination of deionized water, distilled water, reverse osmosis water, etc.
[0040] As a specific embodiment of the preparation method described above of the present invention, wherein, in step (3), the drying comprises first freeze-forming the product obtained in step (2), and then performing a vacuum freeze-drying treatment on the product obtained after freeze-forming;
[0041] Alternatively, the drying includes directly drying the product obtained in step (2) at high temperature.
[0042] As a specific embodiment of the preparation method described above, the freezing molding temperature is not higher than -20°C, preferably -30°C to -50°C, and the freezing molding time is within 60 seconds;
[0043] The vacuum freeze drying process comprises: after freeze molding, raising the temperature from no higher than -20°C to 60-80°C through programmed temperature increase, and maintaining the vacuum degree less than 15Pa for vacuum freeze drying process.
[0044] As a specific embodiment of the preparation method described above, the high-temperature drying is performed at 85-150° C. for 60-300 min.
[0045] Preferably, the high-temperature drying is performed under reduced pressure or vacuum. Under such high-temperature drying conditions, water and additives in the mixed slurry are also removed, while the porous powder material and adhesive continue to be distributed on the surface and throughout the internal structure (the three-dimensional network structure of the internal space) of the porous inorganic fiber material, thereby obtaining a modified inorganic fiber material.
[0046] As a specific embodiment of the preparation method described above, step (1) specifically comprises:
[0047] Accurately weigh the required porous powder material, adhesive, and additives and add them to the required amount of water. Then, through conventional stirring, shearing, ultrasonic and other dispersion methods, the porous powder material, adhesive, and additives are uniformly dispersed and mixed to obtain a uniformly dispersed mixed slurry. It can be seen that the purpose of step (1) is to prepare a uniformly dispersed mixed slurry and to make the mixed slurry have a certain viscosity so as to meet the requirements of the coating operation in step (2).
[0048] As a specific embodiment of the preparation method described above, step (2) specifically comprises:
[0049] The mixed slurry is evenly coated on the surface of the porous inorganic fiber material using a conventional rod coater, blade coater, film transfer coater (also known as a roller transfer coater), rod + blade coater, etc. During the coating process, the coating amount can be adjusted by adjusting the settings of the coater, adjusting the concentration of the porous powder material in the mixed slurry and the viscosity of the mixed slurry, and selecting porous inorganic fiber materials of different thicknesses to obtain a coating amount of 10-200 g / m 2 The modified inorganic fiber material.
[0050] Because the porous inorganic fiber material used in the present invention has a loose, porous, three-dimensional network structure, after coating, the mixed slurry will be evenly absorbed by the surface and internal three-dimensional network structure of the porous inorganic fiber material, thereby being evenly distributed throughout the surface and internal structure (the three-dimensional network structure of the internal space) of the porous inorganic fiber material. This is different from the coating of currently used coated paper, which requires that the coating be as close to the surface of the base paper as possible after coating.
[0051] As a specific embodiment of the preparation method described above, the freeze molding in step (3) specifically includes: after the coating operation is completed, the product obtained in step (2) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding.
[0052] As a specific embodiment of the preparation method described above in the present invention, the vacuum freeze-drying treatment in step (3) specifically includes: after the mixed slurry is completely frozen and formed on the surface and the entire internal structure (the three-dimensional network structure of the internal space) of the porous planar carrier material, turning on the vacuum pump and setting the heating program of the vacuum freeze dryer so that the temperature is raised from no higher than -20°C, preferably from -30°C to -50°C to 60-80°C through the programmed temperature increase, and maintaining the vacuum degree less than 15Pa for vacuum freeze-drying treatment.
[0053] During the operation of the vacuum freeze dryer, due to the extremely low ultimate vacuum of the equipment, usually less than 15Pa, the frozen water and additives in the mixed slurry will gradually begin to sublime, while the porous powder material and adhesive continue to be distributed on the surface and throughout the internal structure of the porous inorganic fiber material (the three-dimensional network structure of the internal space), thereby obtaining a modified inorganic fiber material. At the same time, the sublimation of water and additives causes a large number of evenly distributed pores to form on the surface and inside the modified inorganic fiber material, which facilitates air circulation and helps to fully utilize the acoustic properties and sound absorption and noise reduction properties of the porous powder material.
[0054] In another aspect, the present invention provides a composite material for an automobile roof, comprising a polyurethane layer, an inorganic fiber material layer disposed on either side of the polyurethane layer, and a decorative layer, wherein the inorganic fiber material layer is made of the modified inorganic fiber material described above. The composite material for an automobile roof provided by the present invention is highly effective in sound absorption and noise reduction.
[0055] The present invention does not impose any specific requirements on the preparation method of the automobile roof composite material. The existing conventional method can be used for preparation, and the preparation method can also be reasonably adjusted and improved according to actual on-site operation needs, as long as the automobile roof composite material can be obtained.
[0056] On the other hand, the present invention also provides a sound insulation composite material, comprising an inorganic fiber material layer and a protective layer arranged on at least one side of the inorganic fiber material layer, wherein the material of the inorganic fiber material layer is the modified inorganic fiber material described above.
[0057] The present invention does not impose specific requirements on the material of the protective layer in the sound insulation composite material, and the material can be reasonably selected and adjusted according to actual needs. For example, the material of the protective layer includes a material that prevents powder from falling and / or a waterproof material. The material that prevents powder from falling can be a mesh, and the waterproof material can be a waterproof membrane.
[0058] Finally, the present invention provides a vehicle comprising the aforementioned sound insulation composite material, wherein the sound insulation composite material is affixed to the vehicle body structure and / or the interior of the vehicle. Affixing the sound insulation composite material to the vehicle body structure and / or the interior of the vehicle can reduce noise generated by vehicle operation and / or noise transmitted from outside the vehicle.
[0059] Compared with the prior art, the beneficial technical effects achieved by the present invention include:
[0060] 1. The modified inorganic fiber material provided by the present invention has a significantly improved sound absorption coefficient and has a highly efficient sound absorption and noise reduction function;
[0061] 2. The modified inorganic fiber material provided by the present invention is used as the material of the inorganic fiber material layer in the automobile roof composite material. Without changing the original automobile roof composite material preparation process, the sound absorption and noise reduction function of the automobile roof composite material can be significantly improved, thereby reducing the noise inside the car and improving the comfort of the passengers inside the car.
[0062] 3. The preparation method of the modified inorganic fiber material provided by the present invention is simple and easy, does not require special equipment, and is simple to operate. In addition, since a coating operation is adopted when preparing the modified inorganic fiber material, the present invention can efficiently prepare the modified inorganic fiber material. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0064] Figure 1 is a graph obtained using a high-definition digital microscope using a gram weight of 25g / m 2 Schematic diagram of the surface of glass fiber.
[0065] FIG2 is a schematic diagram of the surface of the modified glass fiber obtained in Example 1 of the present invention obtained using a high-definition digital microscope.
[0066] FIG3 is a schematic cross-sectional view of the modified glass fiber obtained in Example 1 of the present invention, obtained using a high-definition digital microscope.
[0067] FIG4 is a schematic cross-sectional view of the modified glass fiber obtained in Example 3 of the present invention, obtained using a high-definition digital microscope.
[0068] FIG5 is a schematic structural diagram of the automobile roof composite material provided in Example 4 of the present invention.
[0069] Explanation of the main figures: 1. Polyurethane layer; 2. Inorganic fiber material layer; 3. Decorative layer. DETAILED DESCRIPTION
[0070] It should be noted that the term "comprise" and any variations thereof in the description and claims of the present invention are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or are inherent to these processes, methods, products or apparatus.
[0071] The "range" disclosed in the present invention is given in the form of a lower limit and an upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges defined in this way are combinable, i.e., any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values listed are 1 and 2, and the maximum range values listed are 3, 4, and 5, then the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5.
[0072] In the present invention, unless otherwise specified, the numerical range "ab" is an abbreviation for any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" are listed in this invention, and "0-5" is merely an abbreviation for these numerical combinations.
[0073] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned in the present invention can be combined with each other to form a new technical solution.
[0074] In the present invention, unless otherwise specified, all technical features and preferred features mentioned in the present invention can be combined with each other to form a new technical solution.
[0075] In the present invention, unless otherwise specified, the term "two" used in this specification means "at least two".
[0076] In the present invention, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method comprising steps (a) and (b) indicates that the method may comprise steps (a) and (b) performed sequentially, or may comprise steps (b) and (a) performed sequentially. For example, the method further comprising step (c) indicates that step (c) may be added to the method in any order, for example, the method may comprise steps (a), (b) and (c), or may comprise steps (a), (c) and (b), or may comprise steps (c), (a) and (b), etc.
[0077] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the attached table, drawings and examples. The following embodiments are some embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0078] Example 1
[0079] This embodiment provides a modified glass fiber material, which is prepared by a preparation method comprising the following specific steps:
[0080] (a) Accurately weigh 100 parts by weight of ZSM-5 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, 85 parts by weight of deionized water, and 5 parts by weight of ethylene glycol, wherein the amounts of ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol are calculated based on the absolute dry weight of the active ingredients. Add the ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol to the deionized water and mix and stir to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 52.5 cP;
[0081] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm.
[0082] (b) Use a blade coater to evenly coat the mixed slurry on a sheet with a gram weight of 25 g / m 2 on the glass fiber (the surface schematic diagram is shown in Figure 1).
[0083] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding. The freeze molding temperature is -40°C and the time is 5 seconds.
[0084] (d) After the mixed slurry is completely frozen and formed on the surface and the entire internal structure of the glass fiber material (the three-dimensional network structure of the internal space), the vacuum pump is turned on, and the heating program of the vacuum freeze dryer is set so that the temperature is raised from -40°C to 75°C, and the vacuum degree is maintained at less than 15 Pa for vacuum freeze drying. After the treatment, the modified glass fiber material is obtained and marked as test sample 1#.
[0085] The surface schematic diagram and cross-sectional schematic diagram of the test sample 1# prepared in this embodiment are shown in Figures 2 and 3, respectively. Comparing Figures 1 and 2, it can be seen that the porous powder material continues to be distributed on the surface and in the entire internal structure (the three-dimensional network structure of the internal space) of the porous glass fiber material through the bonding effect of the adhesive, and the sublimation of water and the additive causes a large number of evenly distributed pores to be generated on the surface and inside of the modified glass fiber.
[0086] As can be seen from FIG3 , the average thickness of test sample 1# is 134 μm.
[0087] Example 2
[0088] This embodiment provides a modified glass fiber material, which is prepared by a preparation method comprising the following specific steps:
[0089] (a) Accurately weigh 100 parts by weight of ZSM-5 molecular sieve, 7 parts by weight of polystyrene butadiene adhesive, 95 parts by weight of deionized water, and 20 parts by weight of ethylene glycol, wherein the amounts of ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol are calculated based on the absolute dry weight of the active ingredients. Add the ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol to the deionized water and mix and stir to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 60.0 cP;
[0090] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm.
[0091] (b) Use a blade coater to evenly coat the mixed slurry on a sheet with a gram weight of 25 g / m 2 on fiberglass material.
[0092] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding. The freeze molding temperature is -40°C and the time is 8 seconds.
[0093] (d) After the mixed slurry is completely frozen and formed on the surface and the entire internal structure of the glass fiber material (the three-dimensional network structure of the internal space), the vacuum pump is turned on, and the temperature rising program of the vacuum freeze dryer is set so that the temperature is raised from -40°C to 75°C, and the vacuum degree is maintained at less than 15 Pa for vacuum freeze drying. After the treatment, the modified glass fiber material is obtained and marked as test sample 2#.
[0094] It can be reasonably expected from the characterization results in Example 1 that in the test sample 2# prepared in this example, the porous powder material continues to be distributed on the surface and in the entire internal structure (the three-dimensional network structure of the internal space) of the porous glass fiber material through the bonding effect of the adhesive, and the sublimation of water and additives also causes a large number of evenly distributed pores to be generated on the surface and inside of the modified glass fiber.
[0095] Example 3
[0096] This embodiment provides a modified glass fiber material, which is prepared by a preparation method comprising the following specific steps:
[0097] (a) Accurately weigh 50 parts by weight of ZSM-5 molecular sieve, 50 parts by weight of Silicalite-1 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, 3.5 parts by weight of polyacrylate adhesive, 20 parts by weight of deionized water, and 90 parts by weight of ethylene glycol, wherein the ZSM-5 molecular sieve, MFI structure molecular sieve, polystyrene butadiene adhesive, polyacrylate adhesive, and ethylene glycol are all calculated based on the absolute dry mass of the active ingredients. Add the ZSM-5 molecular sieve, MFI structure molecular sieve, polystyrene butadiene adhesive, polyacrylate adhesive, and ethylene glycol to deionized water and mix and stir evenly to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 119 cP;
[0098] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm. The average particle size of the Silicalite-1 molecular sieve porous powder material with sound absorption and noise reduction function is 1.4μm, including micropores with a pore size of 0.60nm and mesopores with a pore size of 11nm.
[0099] (b) Use a scraper coater to evenly coat the mixed slurry on a sheet with a gram weight of 50 g / m 2 on fiberglass material.
[0100] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding. The freeze molding temperature is -40°C and the time is 20 seconds.
[0101] (d) After the mixed slurry is completely frozen and formed on the surface and the entire internal structure of the glass fiber material (the three-dimensional network structure of the internal space), the vacuum pump is turned on, and the heating program of the vacuum freeze dryer is set so that the temperature is raised from -40°C to 75°C, and the vacuum degree is maintained at less than 15 Pa for vacuum freeze drying. After the treatment, the modified glass fiber material is obtained and marked as test sample 3#.
[0102] It can be reasonably expected from the characterization results in Example 1 that in the test sample 3# prepared in this example, the porous powder material continues to be distributed on the surface and in the entire internal structure (the three-dimensional network structure of the internal space) of the porous glass fiber material through the bonding effect of the adhesive, and the sublimation of water and additives also causes a large number of evenly distributed pores to be generated on the surface and inside of the modified glass fiber.
[0103] The cross-sectional schematic diagram of the test sample 3# prepared in this embodiment is shown in FIG4 . As can be seen from FIG4 , the average thickness of the test sample 3# is 352 μm.
[0104] Example 4
[0105] This embodiment provides a modified glass fiber material, which differs from Example 1 only in freeze molding and vacuum freeze drying. The modified glass fiber material is prepared by a preparation method comprising the following specific steps:
[0106] (a) Accurately weigh 100 parts by weight of ZSM-5 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, 85 parts by weight of deionized water, and 5 parts by weight of ethylene glycol, wherein the amounts of ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol are calculated based on the absolute dry weight of the active ingredients. Add the ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol to the deionized water and mix and stir to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 52.5 cP;
[0107] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm.
[0108] (b) Use a scraper coater to evenly coat the mixed slurry on a sheet with a gram weight of 25 g / m 2 on fiberglass material.
[0109] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a 90° C. forced air drying oven for drying. After drying for 60 minutes, the modified glass fiber material is obtained, which is marked as test sample 4#.
[0110] Example 5
[0111] This embodiment provides a series of automobile roof composite materials, a schematic structural diagram of which is shown in Figure 5, including a polyurethane layer 1, an inorganic fiber material layer 2 respectively arranged on both sides of the polyurethane layer 1, and a decorative layer 3 arranged on the inorganic fiber material layer 2 and facing the interior of the automobile, wherein the material of the inorganic fiber material layer 2 is the modified glass fiber material provided in Examples 1 to 4, namely, test samples 1# to 4#.
[0112] The series of automobile roof composite materials provided in this embodiment are all automobile roof composite materials with high-efficiency sound absorption and noise reduction functions.
[0113] Comparative Example 1
[0114] This comparative example provides a modified glass fiber material, which differs from Example 1 only in that no ethylene glycol additive is added. The modified glass fiber material is prepared by a preparation method comprising the following specific steps:
[0115] (a) Accurately weigh 100 parts by weight of ZSM-5 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, and 85 parts by weight of deionized water, where the amounts of ZSM-5 molecular sieve and polystyrene butadiene adhesive are calculated based on the absolute dry weight of the active ingredients. Add the ZSM-5 molecular sieve and polystyrene butadiene adhesive to the deionized water and mix thoroughly to obtain a mixed slurry. The viscosity of the mixed slurry, measured by a digital rotational viscometer, is 6.25 cP.
[0116] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm.
[0117] (b) Use a scraper coater to evenly coat the mixed slurry on a sheet with a gram weight of 25 g / m 2 on fiberglass material.
[0118] Coating results: Since the viscosity of the mixed slurry is particularly low, when it is coated on the glass fiber material, the mixed slurry has too good fluidity, and the glass fiber material absorbs the mixed slurry very quickly, resulting in a particularly high coating amount on the modified glass fiber material, which cannot be precisely controlled, and the uniformity of the obtained material is also very poor.
[0119] Comparison of Example 1 and Comparative Example 1 shows that the viscosity of the mixed slurry is very important for the coating operation. The present invention uses a liquid additive to control the viscosity of the mixed slurry within 30-800 cp to successfully achieve the purpose of preparing a modified glass fiber material with excellent performance.
[0120] Comparative Example 2
[0121] This comparative example provides a modified glass fiber material, which is prepared by a preparation method comprising the following specific steps:
[0122] (a) Accurately weigh 50 parts by weight of ZSM-5 molecular sieve, 50 parts by weight of Silicalite-1 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, 3.5 parts by weight of polyacrylate adhesive, 20 parts by weight of deionized water, and 90 parts by weight of ethylene glycol, wherein the ZSM-5 molecular sieve, MFI structure molecular sieve, polystyrene butadiene adhesive, polyacrylate adhesive, and ethylene glycol are all calculated based on the absolute dry mass of the active ingredients. Add the ZSM-5 molecular sieve, MFI structure molecular sieve, polystyrene butadiene adhesive, polyacrylate adhesive, and ethylene glycol to deionized water and mix and stir evenly to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 119 cP;
[0123] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm. The average particle size of the Silicalite-1 molecular sieve porous powder material with sound absorption and noise reduction function is 1.4μm, including micropores with a pore size of 0.60nm and mesopores with a pore size of 11nm.
[0124] (b) Use a scraper coater to evenly coat the mixed slurry on a sheet with a gram weight of 50 g / m 2 on fiberglass material.
[0125] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding. The freeze molding temperature is -40°C and the time is 20 seconds.
[0126] (d) After the mixed slurry is completely frozen and formed on the surface and the entire internal structure of the glass fiber material (the three-dimensional network structure of the internal space), the vacuum pump is turned on, and the heating program of the vacuum freeze dryer is set so that the temperature is raised from -40°C to 75°C, and the vacuum degree is maintained at less than 15 Pa for vacuum freeze drying treatment. After the treatment, the modified glass fiber material is obtained, which is marked as reference sample 2#.
[0127] Test Example 1
[0128] In this test example, test samples 1# to 4# and reference sample 2# were first cut into 10×10 mm squares, and the contents of molecular sieve and adhesive therein were calculated according to the following formula 1) based on the parameters in Table 1. The specific results of the contents are shown in Table 1.
[0129] Content of molecular sieve and adhesive = (CB) / A, unit: g / m 2 , formula 1);
[0130] In formula 1), A and B are the surface area and mass of the porous glass fiber material, respectively, and the units are m2 and g, C is the total weight of the modified glass fiber material, in g.
[0131] Table 1
[0132] Test Example 2
[0133] This test example uses a standing wave tube, that is, an impedance tube to measure the modified glass fiber materials provided in Examples 1 to 4 and Comparative Example 2, and the gram weight used in the examples and comparative examples is 25 g / m 2 Glass fiber, weight 50g / m 2 The sound pressure changes of the glass fiber at different frequencies are calculated, and the sound absorption coefficient is calculated based on the sound pressure change data. The experimental results are shown in Table 2 below.
[0134] Table 2
[0135] From the experimental data in Table 2 above, it can be seen that:
[0136] (1) The untreated weight is 25g / m 2 The sound absorption coefficient of the glass fiber material provided in Example 1, Example 2 and Example 4 at different frequencies is significantly lower than the sound absorption coefficient of the modified glass fiber material provided in Example 1, Example 2 and Example 4 at the same frequency, which fully proves that the porous powder material with sound absorption and noise reduction function in the modified glass fiber material provided in the embodiment of the present invention has a very obvious noise absorption effect.
[0137] (2) The untreated weight is 50g / m 2 The sound absorption coefficient of the glass fiber material provided in Example 3 at different frequencies is significantly lower than the sound absorption coefficient of the modified glass fiber material provided in Example 3 at the same frequency, which fully proves that the porous powder material with sound absorption and noise reduction function in the modified glass fiber material provided in the embodiment of the present invention has a very obvious noise absorption effect.
[0138] (3) By comparing the experimental data of Example 4 and Example 1, it can be seen that the sound absorption coefficient of the modified glass fiber material provided by Example 1 at different frequencies is significantly higher than the sound absorption coefficient of the modified glass fiber material provided by Example 4 at the same frequency. This fully demonstrates the importance of the drying method. Freeze drying is better than high-temperature drying. This is because: during the water volatilization process of high-temperature drying, under the action of surface tension, the particles of the porous powder material with sound absorption and noise reduction functions are close to each other, so that no rich pore structure is formed in the glass fiber material; in addition, the film-forming performance of the adhesive in the high-temperature drying process is better than that in the freeze-drying process. After the adhesive film is formed, the glass fiber material is firmly wrapped, so that the pore structure in the glass fiber material is further reduced.
[0139] (4) By comparing the experimental results data of Example 1 or Example 4, Example 2, and Example 3, it can be seen that as the absolute dry adsorption mass of the porous powder material with sound absorption and noise reduction function in the glass fiber material increases (in the modified glass fiber material provided by Example 1 or Example 4, Example 2, and Example 3, the absolute dry adsorption mass of the porous powder material with sound absorption and noise reduction function in the glass fiber material is 9.62 mg, 12.62 mg, and 17.79 mg, respectively), its sound absorption coefficient also increases accordingly.
[0140] In addition, the experimental results of Example 3 and Comparative Example 2 show that when the coating amount exceeds 200 g / m 2 , the sound absorption and noise reduction performance of the modified glass fiber material obtained is reduced. This is because the coating is dense and has high density after drying, and the porosity is reduced, thereby reducing the sound absorption and noise reduction effect of the modified glass fiber material.
[0141] In summary, compared with the prior art, the embodiments of the present invention can achieve the following beneficial technical effects:
[0142] 1. The modified inorganic fiber material provided by the embodiment of the present invention has a significantly improved sound absorption coefficient and has a highly efficient sound absorption and noise reduction function;
[0143] 2. Using the modified inorganic fiber material provided in the embodiments of the present invention as the material for the inorganic fiber material layer in the automobile roof composite material can significantly improve the sound absorption and noise reduction function of the automobile roof composite material without changing the original automobile roof composite material preparation process, thereby reducing the noise inside the vehicle and improving the comfort of the passengers inside the vehicle;
[0144] 3. The preparation method of the modified inorganic fiber material provided in the embodiment of the present invention is simple and easy, does not require special equipment, and is simple to operate. In addition, since a coating operation is adopted when preparing the modified inorganic fiber material, the embodiment of the present invention can efficiently prepare the modified inorganic fiber material.
[0145] The above description is merely a specific embodiment of the present invention and should not be construed as limiting the scope of the invention. Therefore, substitutions of equivalent components, or equivalent changes and modifications made within the scope of patent protection, should still fall within the scope of this patent. Furthermore, the technical features of this invention may be freely combined with one another, with other technical inventions, and with other technical inventions.
Claims
1. A modified inorganic fiber material, characterized in that: The modified inorganic fiber material includes a porous inorganic fiber material and a porous powder material, wherein the porous powder material is distributed on the surface of the porous inorganic fiber material and in a three-dimensional network structure in its internal space through bonding with an adhesive; The content of the porous powder material and the adhesive is 10-200 g / m 2 , the content = (CB) / A, where A and B are the surface area and mass of the porous inorganic fiber material, respectively, in units of m 2 and g, C is the total weight of the modified inorganic fiber material, in g.
2. The modified inorganic fiber material according to claim 1, characterized in that The porous inorganic fiber material has a loose porous three-dimensional network structure, a thickness of 80-600 μm, and a gram weight of 20-200 g / m 2 .
3. The modified inorganic fiber material according to claim 1 or 2, characterized in that: The porous inorganic fiber material includes glass fiber, ceramic fiber, basalt fiber, carbon fiber, quartz fiber, asbestos fiber, volcanic rock fiber, metal fiber or alumina fiber.
4. The modified inorganic fiber material according to claim 1, characterized in that The porous powder material includes one or a combination of zeolite molecular sieve, activated silicon dioxide, activated carbon, surface porous calcium carbonate and surface porous calcium silicate.
5. The modified inorganic fiber material according to claim 4, characterized in that The zeolite molecular sieve includes one or a combination of MFI structure molecular sieve, FER structure molecular sieve, CHA structure molecular sieve, MEL structure molecular sieve, TON structure molecular sieve and MTT structure molecular sieve.
6. The modified inorganic fiber material according to claim 4, characterized in that The particle size of the zeolite molecular sieve is 0.5-10 μm.
7. The modified inorganic fiber material according to claim 4, characterized in that The zeolite molecular sieve comprises micropores with a pore size of 0.3-0.7 nm and mesopores with a pore size of 10-30 nm.
8. The modified inorganic fiber material according to any one of claims 4 to 7, characterized in that: The zeolite molecular sieve is ZSM-5 molecular sieve.
9. The modified inorganic fiber material according to claim 1, characterized in that: The adhesive includes an organic adhesive and / or an inorganic adhesive; wherein the organic adhesive includes one or a combination of polyacrylate, acrylic copolymer, polyurethane, polystyrene butadiene emulsion, polystyrene acrylate, polystyrene acetate emulsion, polyvinyl acetate emulsion, silicone resin and polybutadiene rubber emulsion; wherein the inorganic adhesive includes one or a combination of silica sol, alumina sol and pseudo-boehmite.
10. The modified inorganic fiber material according to claim 1 or 2, characterized in that: The thickness of the modified inorganic fiber material is 80-600 μm.
11. The method for preparing the modified inorganic fiber material according to any one of claims 1 to 10, characterized in that: The preparation method comprises: (1) mixing the porous powder material, adhesive, additive and water to obtain a mixed slurry; (2) uniformly coating the mixed slurry on the surface of a porous inorganic fiber material; (3) Drying the product obtained in step (2) to obtain the modified inorganic fiber material.
12. The preparation method according to claim 11, characterized in that: The mass ratio of the porous powder material, adhesive, water and auxiliary agent is 100:4-10:1-159:1-159, and the dosage of the porous powder material, adhesive and auxiliary agent is calculated based on the absolute dry weight of the active ingredient.
13. The preparation method according to claim 11, characterized in that: The auxiliary agent is a liquid auxiliary agent that can be frozen at -30°C to -50°C and can sublime at a temperature of 60-80°C and a vacuum degree of less than 15Pa.
14. The preparation method according to claim 13, characterized in that: At a temperature of 20° C., the viscosity of the liquid additive is not less than 500 cp.
15. The preparation method according to any one of claims 11 to 14, characterized in that: The auxiliary agent includes one or a combination of ethylene glycol, 2,3-butanediol, 1,4-butanediol, 1,3-butanediol and 1,5-pentanediol.
16. The preparation method according to any one of claims 11 to 14, characterized in that: The viscosity of the mixed slurry is 30-800cp.
17. The preparation method according to any one of claims 11 to 14, characterized in that: The water includes deionized water, distilled water, reverse osmosis water or a combination of the two.
18. The preparation method according to any one of claims 11 to 14, characterized in that: In step (3), the drying comprises first freeze-forming the product obtained in step (2), and then performing vacuum freeze-drying treatment on the product obtained after freeze-forming; Alternatively, the drying includes directly subjecting the product obtained in step (2) to high temperature drying.
19. The preparation method according to claim 18, characterized in that: The freezing molding temperature is not higher than -20°C, and the freezing molding time is within 60 seconds; The vacuum freeze drying process comprises: after freeze molding, the temperature is raised from no higher than -20°C to 60-80°C through a program temperature increase, and the vacuum degree is maintained at less than 15Pa for vacuum freeze drying.
20. The preparation method according to claim 19, characterized in that: The freezing molding temperature is -30°C to -50°C.
21. The preparation method according to claim 18, characterized in that: The high temperature drying is drying at 85-150° C. for 60-300 min.
22. The preparation method according to claim 18, characterized in that: The high temperature drying is performed under reduced pressure or vacuum environment.
23. A composite material for automobile ceiling, comprising a polyurethane layer, an inorganic fiber material layer and a decorative layer respectively arranged on both sides of the polyurethane layer, characterized in that: The material of the inorganic fiber material layer is the modified inorganic fiber material according to any one of claims 1-10.
24. A sound insulation composite material, comprising an inorganic fiber material layer and a protective layer arranged on at least one side of the inorganic fiber material layer, characterized in that: The material of the inorganic fiber material layer is the modified inorganic fiber material according to any one of claims 1-10.
25. A vehicle, characterized in that: The vehicle comprises the sound insulation composite material of claim 24, wherein the sound insulation composite material is fixed to a vehicle body structure and / or a vehicle interior.
Citation Information
Patent Citations
Novel vehicle roof and production process thereof
CN103921504A
Composite material automobile top cover
CN211417409U
Sound-absorbing coating material and preparation method thereof
CN102533016A
Sound-absorbing material, sound-generating device, and electronic apparatus
CN115477505A
Porous composite sound absorption material and preparation method thereof
CN115547284A