Chemically-endcapped melamine polyphosphate having high temperature resistance and leaching resistance, preparation method and apparatus thereof, and use thereof in flame-retardant nylon
High-temperature-resistant and precipitated melamine polyphosphate was prepared by chemical end-capping and thermal polymerization, which solved the problem of insufficient temperature resistance and precipitation performance in the existing technology, and achieved high nitrogen content and excellent flame retardant effect, which is suitable for flame retardant nylon materials.
Patent Information
- Application Number
- PCT/CN2024/105797
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-21
AI Technical Summary
Existing melamine polyphosphate flame retardants have insufficient temperature resistance and exudation properties, which cannot meet the requirements of certain applications.
A chemically capped melamine polyphosphate flame retardant is prepared by combining thermal polymerization and a capping agent to produce a high-temperature resistant and precipitated melamine polyphosphate. The reaction is carried out in an inert gas environment, and a special device is used for stirring and rotation control to improve the uniformity of the reaction.
It improves the temperature resistance and exudation performance of melamine polyphosphate, achieves high nitrogen content, and enhances product whiteness and thermal stability. It is suitable for flame-retardant nylon and has excellent flame retardant effect and exudation resistance.
Smart Images

Figure PCTCN2024105797-APPB-I100001 
Figure PCTCN2024105797-APPB-I100002 
Figure PCTCN2024105797-APPB-I100003
Abstract
Description
A chemically terminated melamine polyphosphate with high temperature resistance and precipitation, a preparation method and device thereof, and application in flame-retardant nylon Technical Field
[0001] The present invention relates to the technical field of flame retardants, and in particular to a highly temperature-resistant and precipitated chemically blocked melamine polyphosphate, a preparation method and a device thereof, and application thereof in flame-retardant nylon. Background Art
[0002] Melamine and its phosphate salts are widely used in polymers or coatings such as plastics and rubbers, and have excellent flame retardant and fireproof properties. It not only has the functions of general intumescent flame retardants, but also has its own advantages: (1) Low water solubility, usually less than 0.5g at room temperature. This advantage is of great benefit to coating systems under humid conditions and to the compatibility of plastics and rubbers; (2) High thermal stability, which is not only beneficial to the processing and molding of flame-retardant plastics and rubbers, but also to flame retardant and fireproof properties; (3) Excellent flame retardant properties, because it dissolves phosphorus and nitrogen into one to form (PON) x , making good use of the synergistic effect of phosphorus and nitrogen. At the same time, with thermal degradation, a series of condensation products are gradually generated, accompanied by the generation of water vapor that absorbs a lot of heat and non-flammable ammonia and other gases, which have a good coordination effect on the expansion and carbonization of the entire expansion system, and also increase the amount of expansion carbon layer formed; (4) It has good compatibility with other flame retardants. For example, using polyphosphate melamine and ammonium polyphosphate in a certain proportion will achieve better flame retardant effect.
[0003] There are two methods for synthesizing melamine polyphosphate: one is to react polyphosphoric acid with melamine under acidic conditions; the other is to use a solid-phase synthesis method, which involves direct dehydration of melamine phosphate at a specific temperature. However, the first method suffers from the same problem as the synthesis of melamine phosphate: the presence of excessive inorganic salts in the product. The second method also suffers from the solid-phase nature of the reaction, making mass and heat transfer difficult and production challenging. For example, Chinese patents CN 102127230 A, CN 105504292 A, and CN 104693483 A primarily involve calcining melamine orthophosphate at temperatures between 120°C and 350°C. Calcination equipment can include hot air drying, kneading machines, rotary kilns, paddle dryers, extruders, and other devices. In recent years, a number of improved melamine polyphosphates have emerged, such as Hostaflam AP-750, Melapur PA-90, and MELAPUR P46. Among them, the more mature ones and those already in industrial production include Melapur 200-70 from BASF of Germany, which can achieve a 1% thermogravimetric loss at 350°C or higher; XPM-1000 developed and sold by MONSANTO of the United States; Melabis designed and synthesized by Borg-Warner Chemical Company of the United States; and Char-Guard CN-329, an intumescent flame retardant produced by Great Lakes Chemical Company of the United States, as shown in formula (1).
[0004] Formula (1)
[0005] Current R&D efforts in melamine polyphosphates focus on improving preparation processes, optimizing synthesis routes, and developing synergistic compounding technologies. While melamine polyphosphates themselves possess a certain degree of water resistance, their heat resistance and precipitation resistance still fall short of meeting all product requirements. There is an urgent need to develop new melamine polyphosphates and preparation methods to meet practical application needs. Summary of the Invention
[0006] The present invention aims to provide a chemically blocked melamine polyphosphate flame retardant with high temperature resistance and precipitation, so as to solve the technical problems of the existing melamine polyphosphate flame retardants in terms of flame retardancy, stability and other unsatisfactory properties.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant, wherein the structural formula of the melamine polyphosphate is shown in the following chemical formula, and the melamine polyphosphate is blocked by a blocking agent;
[0009]
[0010] Wherein, n=1000-3000; the end-capping agent is a nitrogen-containing compound having no hydroxyl group and an NH bond.
[0011] This solution also provides a method for preparing a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant, comprising the following steps in sequence:
[0012] S1: Melamine phosphate is subjected to thermal polymerization and dehydration to obtain melamine polyphosphate;
[0013] S2: After the melamine polyphosphate and the blocking agent are heat-treated, chemically blocked melamine polyphosphate is obtained.
[0014] This solution also provides an application of a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant in flame-retardant nylon.
[0015] Furthermore, the end-capping agent includes at least one of R-NH2, R=NH, melamine, urea, biguanidine and iminodiacetonitrile; and R is an alkyl group with 1 to 4 carbon atoms.
[0016] Furthermore, the reaction processes of S1 and S2 are both carried out in an inert gas environment; the reaction temperature, pressure and time of S1 are 220-360°C, 0.05-0.3MPa, and 60-300min, respectively; the reaction temperature, pressure and time of S2 are 180-360°C, 0.1-1.5MPa, and 30-240min, respectively.
[0017] Furthermore, the reaction processes of S1 and S2 are both carried out in a thermal polymerization reaction device; the polymerization reaction device includes a rotary furnace and a temperature control unit; a reaction chamber is provided in the rotary furnace, and a stirring screw is coaxially provided in the reaction chamber; the temperature control unit is used to control the temperature in the reaction chamber; during the reaction process, the stirring screw and the reaction chamber maintain different rotation directions.
[0018] Furthermore, the rotation speed of the stirring screw is 30-300 rpm, and the rotation speed of the reaction chamber is 3-120 rpm.
[0019] Furthermore, the flame retardant nylon, in parts by weight, comprises the following raw materials: 30-80 parts of nylon, 5-60 parts of long glass fiber, 5-20 parts of chemically terminated melamine polyphosphate, 5-20 parts of organic aluminum hypophosphite, 0.5-4 parts of flame retardant synergist, 0.3-2 parts of nucleating agent, 0.5-2 parts of coupling agent, 0.3-3 parts of lubricant, and 0.2-1 parts of antioxidant.
[0020] Furthermore, the nylon includes at least one of nylon 6, nylon 66, nylon 46, nylon 610, nylon 612, nylon 9, nylon 11, nylon 12, nylon 1010, nylon 1012, and nylon 1212; the long glass fiber is a rolled alkali-free glass fiber; the organic aluminum hypophosphite is aluminum diethylphosphinate; the flame retardant synergist includes at least one of anhydrous zinc borate, 3.5-hydrated zinc borate, zinc oxide, and zirconium phosphate; the nucleating agent is BRUGGOLEN P22; the coupling agent is a silane coupling agent; the lubricant includes at least one of ethylene bisstearamide, pentaerythritol stearate, silicone, and amide wax; and the antioxidant includes at least one of antioxidant 168, antioxidant 1010, and antioxidant 1098.
[0021] Furthermore, the flame retardant nylon is prepared by the following method:
[0022] S1: Add nylon, chemically terminated melamine polyphosphate, organic aluminum hypophosphite and flame retardant synergist into a mixer and stir at room temperature for 5-30 minutes;
[0023] S2: Increase the mixer temperature to 80-180°C, add the coupling agent and continue stirring for 10-30 minutes;
[0024] S3: After cooling to room temperature, add lubricant, nucleating agent and antioxidant, and stir for 5-30 minutes to obtain a premix;
[0025] S4: The premix is extruded through a twin-screw extruder, and long glass fibers are fed from the glass fiber port. The temperature during extrusion is 200-300°C. The premix is then drawn and pelletized, and then sieved and dehydrated to obtain flame-retardant reinforced nylon pellets.
[0026] In summary, the beneficial effects of this technical solution are:
[0027] Compared with traditional technologies, the present invention has a good polymerization reaction effect on melamine polyphosphate, uniform heating, uniform and complete polymerization, does not stick to the reaction kettle, and solves the problem of unstable thermal decomposition temperature of solid-phase synthesis products; after chemical end-capping, water resistance, heat resistance and flame retardancy are improved.
[0028] (1) Improve the heat resistance of melamine polyphosphate, improve the precipitation resistance through chemical blocking, and increase the nitrogen content to achieve a nitrogen content greater than 42%;
[0029] (2) Design a production device for chemically capping and thermally polymerizing melamine polyphosphate, which can be continuously scaled up and ensure product whiteness (whiteness greater than 98%) and thermal stability (1% thermogravimetric loss greater than 370°C);
[0030] (3) The application of melamine polyphosphate (chemically terminated) in flame retardant nylon. By compounding the flame retardant formula, adding 10%, the flame retardant effect reaches 0.8mmV-0, and the product passes the UL 746C water immersion test and the GB / T 2423.50 "double 85" test for 1000h without precipitation. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] FIG1 is a front view of a polymerization reaction apparatus for continuous production according to Example 1.
[0032] FIG2 is a cross-sectional view taken along line AA of FIG1 .
[0033] FIG3 is a front view (cross-sectional view) of the stirring screw of Example 1. FIG.
[0034] FIG4 is a TG chart of commercially available melamine polyphosphate of Experimental Example 1. DETAILED DESCRIPTION
[0035] The present invention will be further described in detail below with reference to the examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used are all commercially available.
[0036] The specific reference numerals are: cylinder 1, hot oil tank 2, cold oil tank 3, driven gear 4, drive gear 5, oil chamber 6, stirring screw 7, first motor 8, feed port 9, nitrogen outlet 10, discharge port 11, nitrogen inlet 12, load-bearing wheel 13, second motor 14, support column 15, first conduit 16, first oil pump 17, second conduit 18, second oil pump 19, first rotary joint 20, first rotating conduit 21, second rotary joint 22, second rotating conduit 23, third conduit 24, frame 25, insulation layer 26.
[0037] Example 1: Chemically blocked melamine polyphosphate
[0038] (1) Synthesis process
[0039] The synthesis process of chemically blocked melamine polyphosphate is roughly as follows:
[0040] Using deionized water as a solvent, melamine (ME) and H3PO4 reacted through acid-base neutralization to prepare melamine phosphate (MP) with high purity, high whiteness, and high thermal stability. MP was then subjected to high-temperature thermal polymerization to obtain melamine polyphosphate (MPP). The above synthesis process can be found in the inventor's previously published paper "Zhong Zhiqiang, Synthesis of Melamine Polyphosphate and Its Flame-Retardant Properties of Polypropylene, Engineering Plastics Applications, 2018". Specifically, in this embodiment, the method for preparing melamine phosphate is as follows: the molar ratio of ME to H3PO4 is 1:1.05, the reaction time is 2.0 h, the reaction temperature is 95°C, and the molar ratio of ME to deionized water is 3:97. Under the above conditions, melamine phosphate (Formula (2)) was synthesized. Melamine polyphosphate (MPP) was then synthesized using melamine phosphate, and the synthesis reaction was carried out in a polymerization reaction equipment specifically used for continuous production in this scheme. Melamine phosphate is heat-treated at 220-360°C for 60-300 minutes, and then subjected to thermal polymerization, dehydration, and condensation in an inert gas environment (e.g., nitrogen) at a pressure of 0.05-0.3 MPa to produce melamine polyphosphate (MPP, Formula (2)) of a certain molecular weight. The reaction formula is shown in Formula (4). A capping agent (the mass ratio of the capping agent to the melamine polyphosphate is 3-100:10000) is then added to the reaction system (also using the polymerization reaction equipment specifically designed for continuous production in this scheme). The system is then heat-treated at 180-360°C for 30-240 minutes in an inert gas environment (e.g., nitrogen) at a pressure of 0.1-1.5 MPa. After cooling, the system is ground into powder to produce chemically capped melamine polyphosphate (e.g., Formula (5), using R-NH2 and R=NH as capping agents as an example). The reaction process is shown in Formula (6). During the two-step reaction process, the material stirring screw and the rotating furnace body rotate in different directions. For example, the material stirring screw rotates counterclockwise at a speed of 30-300 rpm and the rotating furnace body rotates clockwise at a speed of 3-120 rpm (preferably 3-60 rpm).
[0041] The end-capping agent is a nitrogen-containing compound containing no hydroxyl group and having an NH bond, which may be: R-NH2 or R=NH, where R is an alkyl group with 1 to 4 carbon atoms; or melamine and its compounds containing no hydroxyl group composed of R-NH2 and R=NH; or amino compounds containing no hydroxyl group composed of R-NH2 and R=NH (for example, urea); or imino compounds containing no hydroxyl group composed of R-NH2 and R=NH (for example, compounds containing a guanidine group (NH2)2-C=NH, biguanidine (1-(diaminomethylene)guanidine), and iminodiacetonitrile C4H5N3). In addition, in formulas (3), (4), (5), and (6), n = 1000-3000.
[0042]
[0043] (2) Synthesis equipment
[0044] The dedicated equipment used in this technical solution is shown in Figure 1. The polymerization reaction equipment for continuous production includes a rotary furnace and a temperature control unit. The rotary furnace includes an inclined cylinder 1, and the temperature control unit includes a hot oil tank 2 and a cold oil tank 3.
[0045] Referring to Figures 1 and 2, a driven gear 4 is sleeved and fixed on the outside of the cylinder 1. The cylinder 1 and the driven gear 4 are concentrically arranged. There are two left and right drive gears 5 meshing with the driven gear 4, and the drive gear 5 drives the cylinder 1 to rotate. The cylinder 1 is a double-layer structure, including a coaxially arranged cylindrical inner wall and outer wall, an oil chamber 6 is formed between the inner wall and the outer wall, and the outer side of the outer wall is covered with an insulation layer 26. The cavity formed by the inner wall is a reaction chamber, and a stirring screw 7 is arranged in the reaction chamber. The upper and lower ends of the stirring screw 7 are rotatably connected to the top and bottom of the cylinder 1. The upper end of the stirring screw 7 is fixed to the output shaft of the first motor 8, and the first motor 8 is fixed on the frame 25. A feed port 9 and a nitrogen outlet 10 are provided at the top of the cylinder 1, and a discharge port 11 and a nitrogen inlet 12 are provided at the bottom of the cylinder 1. The outer wall of the cylinder 1 contacts two sets of upper and lower load-bearing wheels 13 (each set includes two load-bearing wheels 13). The load-bearing wheels 13 are fixed in position and rotatably connected to the frame 25, supporting the cylinder 1 and coordinating its rotation. The drive gear 5 is rotatably connected to the frame 25, and the second motor 14 is fixed to the frame 25. The drive gear 5 is driven by the second motor 14 through a conventional transmission structure in the prior art. The drive gear 5 drives the cylinder 1 to rotate via the driven gear 4. Several support columns 15 are provided in the oil chamber 6, parallel to the central axis of the cylinder 1. The upper and lower ends of the support columns 15 are fixed to the top and bottom of the cylinder 1.
[0046] The hot oil tank 2 is connected to a first conduit 16, which is equipped with a first oil pump 17. The cold oil tank 3 is connected to a second conduit 18, which is equipped with a second oil pump 19. The first conduit 16 is connected to a first rotating conduit 21 via a first rotary joint 20; the second conduit 18 is connected to a second rotating conduit 23 via a second rotary joint 22. One end of the first rotating conduit 21 is connected to the oil chamber 6 and is fixed to the bottom of the cylinder 1; one end of the second rotating conduit 23 is connected to the oil chamber 6 and is fixed to the top of the cylinder 1.
[0047] The temperature control unit also includes a third conduit 24. The lower end of the third conduit 24 is connected to two branches (branch A and branch B). Branch B connects to the first conduit 16, and branch A connects to the hot oil tank 2. Both branches A and B are equipped with corresponding control valves. The upper end of the third conduit 24 is connected to two branches (branch C and branch D). Branch D connects to the second conduit 18, and branch C connects to the cold oil tank 3. Both branches C and D are equipped with corresponding control valves. When the hot oil circulates, branch B and branch C are closed, the second oil pump 19 is turned off, the first oil pump 17 is turned on, and branch A and branch D are turned on. This creates a closed-loop circuit between the hot oil tank 2, the first conduit 16, the first rotating conduit 21, the oil chamber 6, the second rotating conduit 23, the second conduit 18, and the third conduit 24. Under the action of the first oil pump 17, the hot oil circulates throughout, maintaining the temperature within the reaction chamber. After the heating reaction is completed, the branch pipe A is closed, and the hot oil in the pipeline returns to the hot oil tank 2 under the action of the first oil pump 17 and the gravity of the hot oil. After the reaction is completed, the cold oil in the cold oil tank 3 is used to cool the reacted material.
[0048] When the cold oil is circulating, branch A and branch D are closed, the first oil pump 17 is turned off, branch B is turned on, branch C is turned on, and the second oil pump 19 is turned on. This forms a closed loop between the cold oil tank 3, the second conduit 18, the second rotating conduit 23, the oil chamber 6, the first rotating conduit 21, the first conduit 16, and the third conduit 24. Under the action of the second oil pump 18, the cold oil circulates through the reaction chamber, cooling it. After the cooling is complete, branch C is closed, and the cold oil in the pipeline is pumped back to the cold oil tank 3 under the action of the second oil pump 18. Following this process, hot oil circulation and cold oil circulation can be alternated according to actual needs, achieving continuous production.
[0049] The specific process of using the device is as follows:
[0050] A. At the beginning of the thermal polymerization reaction, the hot oil tank 2 begins operation, heating the oil to the processing temperature. Materials and inert protective gas are added to the reaction chamber, and the first oil pump 17 is started to press the hot oil in the hot oil tank 2 into the oil cavity 6 on the outer wall of the thermal polymerization rotary furnace barrel 1. The oil circulates between the hot oil tank 2 and the oil cavity 6 on the outer wall of the barrel 1, and the oil is quickly heated to the specified temperature and maintained at a constant temperature.
[0051] B. During the reaction, a circulation system is maintained between the hot oil tank 2 and the oil chamber 6 on the outer wall of the barrel 1 to maintain a constant temperature during the reaction time. The reaction pressure is adjusted by pumping or adding inert gas. Throughout the thermal polymerization process, the rotation direction of the stirring screw 7 remains opposite to that of the reaction chamber.
[0052] C. After the reaction is completed, the first oil pump 17 is started to pump the hot oil in the thermal polymerization reaction rotary furnace into the hot oil tank 2. Then, the second oil pump 19 is started to press the cold oil in the cold oil tank 3 into the oil cavity 6 on the outer wall of the thermal polymerization reaction cylinder 1. This allows the oil to circulate between the cold oil tank 3 and the oil cavity 6 on the outer wall of the rotary furnace, achieving rapid cooling.
[0053] D. After the temperature in the feed pipe drops to the specified temperature and the material is discharged, the second oil pump 19 is started to press the oil in the oil cavity 6 on the outer wall of the rotary furnace into the cold oil tank 3. The material and inert protective gas are then added. After the air in the feed pipe is exhausted, the hot oil in the hot oil tank 2 is pressed into the oil cavity 6 on the outer wall of the rotary furnace shell 1. Steps A to D are repeated to achieve continuous production.
[0054] In the synthesis process of this technical solution, the material (melamine phosphate) and an inert protective gas (nitrogen, 0.05-0.3 MPa) are added to the reaction chamber. Hot oil circulation is used to raise the reaction chamber temperature to 220-360°C and maintain this constant temperature. The reaction proceeds for 60-300 minutes, completing the first step. Nitrogen is then introduced to adjust the reaction pressure to 0.1-1.5 MPa, and the hot oil temperature is adjusted to 180-360°C. The material (capping agent) reacts in the reaction chamber for 30-240 minutes to produce chemically capped melamine polyphosphate. After the reaction is complete, the material is directly discharged to a storage silo outside the system for cooling. This solution primarily synthesizes the target substance, utilizing the aforementioned equipment's constant temperature heating, inert protective gas flow to maintain reaction pressure, and the ability to maintain the rotational directions of the agitator screw 7 and the reaction chamber. Cold oil cooling and continuous production are not required. The process involves adding materials to the reaction chamber, then adjusting the pressure of nitrogen to the desired level. Hot oil circulation is then activated to control the temperature of the reaction chamber. During the reaction, the stirring screw 7 and the reaction chamber rotate in opposite directions. The nitrogen pressure in the reaction chamber and the temperature of the hot oil tank 2 are adjusted according to the requirements of the reaction stage. After the reaction is complete, the materials are directly removed to a storage bin for cooling without cooling the oil.
[0055] Example 2: Application of chemically blocked melamine polyphosphate in flame retardant nylon
[0056] The flame-retardant reinforced nylon composition comprises the following raw materials in parts by weight: 30-80 parts nylon, 5-60 parts long glass fiber, 5-20 parts chemically terminated melamine polyphosphate (or domestically produced common melamine polyphosphate), 5-20 parts organic aluminum hypophosphite, 0.5-4 parts flame retardant synergist, 0.3-2 parts nucleating agent, 0.5-2 parts coupling agent, 0.3-3 parts lubricant, and 0.2-1 parts antioxidant. In addition to excellent flame retardancy, the reinforced nylon composition also possesses exceptional mechanical properties, temperature resistance, and precipitation resistance.
[0057] The nylon is any one of nylon 6, nylon 66, nylon 46, nylon 610, nylon 612, nylon 9, nylon 11, nylon 12, nylon 1010, nylon 1012, and nylon 1212, or a mixture thereof. The long glass fiber is a rolled alkali-free glass fiber with a diameter of 6-10 μm. The organic aluminum hypophosphite is aluminum diethylphosphinate. The flame retardant synergist is any one of anhydrous zinc borate, 3.5-hydrated zinc borate, zinc oxide, and zirconium phosphate, or a mixture thereof. The nucleating agent is BRUGGOLEN P22. The coupling agent is a silane coupling agent, which can be any one of aminosilane coupling agent KH-9120, isocyanate silane coupling agent KT-930, epoxy silane coupling agent KH-1006, and KH-9130, or a mixture thereof. The lubricant is one or more of ethylene bis stearamide, pentaerythritol stearate, silicone powder and amide wax. The antioxidant is antioxidant 168, antioxidant 1010 or antioxidant 1098.
[0058] Flame retardant nylon is prepared by the following process:
[0059] Step 1: Add nylon, chemically blocked melamine polyphosphate (or domestically produced common melamine polyphosphate), organic aluminum hypophosphite and flame retardant synergist into a mixer and stir at room temperature for 5-30 minutes;
[0060] Step 2: In the mixture of step 1, increase the temperature of the mixer to 80-180°C. After ensuring that the temperature of the material in the mixer has reached the set temperature, add the coupling agent and continue stirring for 10-30 minutes;
[0061] Step 3: After cooling the mixture from step 2 to room temperature, add lubricant, nucleating agent and antioxidant and stir for 5-30 minutes;
[0062] Step 4: The mixture of step 3 is extruded by a twin-screw extruder, and long glass fiber is fed from the glass fiber port. The temperature during extrusion is 200-300°C. Then, the mixture is subjected to the process of drawing and pelletizing, and is screened and dehydrated to obtain flame-retardant reinforced nylon granules.
[0063] Experimental Example 1: Synthesis and Performance Testing of Chemically End-Capped Melamine Polyphosphate
[0064] In this experimental example, the specific material synthesis was carried out according to the synthesis route of Example 1. The raw materials and parameter selection are shown in Table 1. In addition, in the synthesis process of melamine polyphosphate and chemically blocked melamine polyphosphate, the special equipment of this scheme was used, and the material stirring screw was kept rotating counterclockwise at a speed of about 200 rpm, and the rotating furnace body was rotated clockwise at a speed of about 50 rpm. The performance of the chemically blocked melamine polyphosphate product obtained by synthesis was tested, including the 1% thermogravimetric loss temperature and whiteness. The 1% thermogravimetric loss temperature was tested according to the standard ASTM E2550-2007, and the whiteness was tested according to the standard GB / T 5950. The test results are detailed in Table 2. Among them, domestic melamine polyphosphate was purchased from the market, and its TG chart is shown in Figure 4.
[0065] Table 1: Synthesis conditions of chemically terminated melamine polyphosphates
[0066]
[0067] Table 2: Performance test results
[0068]
[0069] From the above experimental results, it can be seen that the chemically terminated melamine polyphosphate obtained by the synthesis method of this scheme has a more ideal whiteness (greater than 98%) and 1% thermal weight loss temperature (greater than 370°C) compared with the ordinary melamine polyphosphate in the prior art.
[0070] Experimental Example 2: Specific synthesis and performance testing of flame retardant nylon
[0071] This experimental example carried out specific material synthesis according to the synthesis route of Example 2, and the raw materials and parameter selections are as follows:
[0072] Test 1: 47.9 parts nylon; 30 parts long glass fiber; 10 parts chemically terminated melamine polyphosphate (prepared in Test 1 of Experimental Example 1); 10 parts organic aluminum hypophosphite; 0.5 parts flame retardant synergist; 0.3 parts nucleating agent; 0.5 parts coupling agent; 0.5 parts lubricant; and 0.3 parts antioxidant 1098.
[0073] Test 2: 47.9 parts nylon; 30 parts long glass fiber; 10 parts chemically terminated melamine polyphosphate (prepared in Test 2 of Experimental Example 1); 10 parts organic aluminum hypophosphite; 0.5 parts flame retardant synergist; 0.3 parts nucleating agent; 0.5 parts coupling agent; 0.5 parts lubricant; and 0.3 parts antioxidant 1098.
[0074] Test 3: 47.9 parts nylon; 30 parts long glass fiber; 10 parts chemically terminated melamine polyphosphate (prepared in Test 3 of Experimental Example 1); 10 parts organic aluminum hypophosphite; 0.5 parts flame retardant synergist; 0.3 parts nucleating agent; 0.5 parts coupling agent; 0.5 parts lubricant; 0.3 parts antioxidant 1098.
[0075] Test 4: 47.9 parts nylon; 30 parts long glass fiber; 10 parts chemically terminated melamine polyphosphate (prepared in Test 4 of Experimental Example 1); 10 parts organic aluminum hypophosphite; 0.5 parts flame retardant synergist; 0.3 parts nucleating agent; 0.5 parts coupling agent; 0.5 parts lubricant; 0.3 parts antioxidant 1098.
[0076] Comparative test 1: 47.9 parts of nylon; 30 parts of long glass fiber; 10 parts of domestic melamine polyphosphate; 10 parts of organic aluminum hypophosphite; 0.5 parts of flame retardant synergist; 0.3 parts of nucleating agent; 0.5 parts of coupling agent; 0.5 parts of lubricant; 0.3 parts of antioxidant 1098.
[0077] Among them, the nylon is PA66-EPR27; the long glass fiber diameter is 8 microns; the organic aluminum hypophosphite is diethyl aluminum phosphinate; the flame retardant synergist is anhydrous zinc borate; the nucleating agent is BRUGGOLEN P22; the coupling agent is KH-9130; and the lubricant is silicone powder.
[0078] Comparative Test 2: Referring to Test 1, the difference is that no organic aluminum hypophosphite is added, and 20 parts of chemically blocked melamine polyphosphate (prepared in Test 1 of Experimental Example 1) are added.
[0079] Comparative Test 3: Referring to Test 1, the difference is that no flame retardant synergist is added, and 10.5 parts of chemically blocked melamine polyphosphate (prepared in Test 1 of Experimental Example 1) is added.
[0080] Comparative test 4: Refer to test 1, except that the flame retardant synergist is replaced with zinc oxide in equal amounts.
[0081] Comparative test 5: Refer to test 1, except that the flame retardant synergist is replaced with zirconium phosphate in equal amounts.
[0082] Tests 1-4 and comparative tests 1-5 were conducted according to the following method for preparing the composite material, which is a conventional method in the prior art: nylon, chemically terminated melamine polyphosphate (or domestically produced), organic aluminum hypophosphite and flame retardant synergist were added to a mixer, stirred at room temperature for 10 minutes, and then the temperature of the mixer was increased to 150°C. After ensuring that the temperature of the material in the mixer also reached the set temperature, the coupling agent was added and stirred for 15 minutes; after cooling to room temperature, a lubricant, a nucleating agent and an antioxidant were added and stirred for 10 minutes; the final mixture was extruded using a conventional twin-screw extruder in the prior art and a conventional twin-screw extrusion process was adopted, wherein long glass fibers were fed from the glass fiber port and the temperature during extrusion was 220-260°C. The mixture was then subjected to the processes of drawing and pelletizing, and sieving and dehydration to obtain a flame retardant reinforced nylon composite material.
[0083] Comparative Test 6: Similar to Test 1, except for the preparation process, the following was used: nylon, chemically terminated melamine polyphosphate, organic aluminum hypophosphite, flame retardant synergist, lubricant, nucleating agent, and antioxidant were added to a mixer and stirred at room temperature for 20 minutes. The mixer temperature was then raised to 150°C. After the materials in the mixer reached the set temperature, the coupling agent was added and stirring continued for 15 minutes. The resulting mixture was then used for twin-screw extrusion.
[0084] Comparative Test 7: Similar to Test 1, except for the preparation process, the following steps were used: nylon, chemically terminated melamine polyphosphate, organic aluminum hypophosphite, and flame retardant synergist were added to a mixer and stirred at room temperature for 10 minutes. The mixer temperature was then raised to 200°C. After the materials in the mixer reached the set temperature, the coupling agent was added and stirring continued for 15 minutes. After cooling to room temperature, the lubricant, nucleating agent, and antioxidant were added and stirred for 10 minutes. The resulting mixture was then used for twin-screw extrusion.
[0085] Comparative Test 8: Similar to Test 1, except for the preparation process, the following steps were used: nylon and chemically terminated melamine polyphosphate were added to a mixer and stirred at room temperature for 10 minutes. The mixer temperature was then raised to 150°C. After the materials in the mixer reached the set temperature, the coupling agent was added and stirring continued for 15 minutes. After cooling to room temperature, the lubricant, nucleating agent, antioxidant, organoaluminum hypophosphite, and flame retardant synergist were added and stirred for 10 minutes. The resulting mixture was then used for twin-screw extrusion.
[0086] The synthesized flame-retardant reinforced nylon composites were subjected to performance testing, including flame retardancy testing, the "Double 85" test, and water immersion testing. The flame retardancy test was conducted according to the Test for Flammability of Plastic Materials for Parts in Devices and Appliances (UL 94); the 1000-hour "Double 85" test was conducted according to GB / T 2423.50 Part 2, Test Cy: Steady-State Damp Heat, primarily for accelerated component testing; and the water immersion test was conducted according to Polymeric Materials - Use in Electrical Equipment Evaluations – UL 746C. The test results are detailed in Table 3.
[0087] Table 3: Flame retardant nylon performance test results (NR means non-flame retardant; “—” means that the test is unnecessary because 0.8mm is not flame retardant)
[0088]
[0089] The above data demonstrates that the flame-retardant reinforced nylon composites prepared using the chemically end-capped melamine polyphosphate of this solution as a flame retardant (Tests 1-4) exhibit more ideal flame retardancy and precipitation resistance. Comparative Test 1, using a commercially available melamine polyphosphate flame retardant, yielded flame-retardant nylon with some flame retardancy, but the flame retardancy was inferior to that of Tests 1-4. Furthermore, since Comparative Test 1 lacked chemical end-capping, the mechanical properties and precipitation resistance of the resulting nylon material were negatively impacted.
[0090] Comparative Test 2, in which no organoaluminum hypophosphite was used, and Comparative Test 3, in which no flame retardant synergist was used, resulted in a significant decrease in the flame retardancy of the nylon. This demonstrates that chemically terminated melamine polyphosphate, when used as a flame retardant, requires the use of organoaluminum hypophosphite and a flame retardant synergist in the preparation of flame-retardant nylon to fully achieve its flame retardant effect. Omitting organoaluminum hypophosphite has a slight negative impact on the mechanical properties of the flame-retardant nylon. However, omitting either organoaluminum hypophosphite or a flame retardant synergist does not affect the surface precipitation of the flame-retardant nylon.
[0091] Comparative Tests 4 and 5 investigated the effects of different flame retardant synergists. When zinc oxide was used as a flame retardant synergist, the flame retardancy of the nylon material was worse than when anhydrous zinc borate was used, but no other significant effects were observed. When zirconium phosphate was used as a flame retardant synergist, the flame retardancy of the nylon material decreased somewhat compared to when anhydrous zinc borate was used, and the mechanical properties of the nylon material were also significantly negatively affected.
[0092] Since the chemically terminated melamine polyphosphate prepared in this solution is the first to be added to nylon materials, the inventors also explored the preparation process. If nylon, chemically terminated melamine polyphosphate, organoaluminum hypophosphite, flame retardant synergist, lubricant, nucleating agent, and antioxidant are mixed all at once before adding a coupling agent, the resulting mixture can be pelletized using conventional twin-screw extrusion (Comparative Test 6). While this method reduces process complexity, the coupling agent cannot adequately surface treat the raw materials (especially the flame retardant in this solution) and affects material dispersion, which in turn affects the flame retardant and mechanical properties of the product, and also deteriorates the product's precipitation resistance. If the mixing temperature of nylon, chemically terminated melamine polyphosphate, organoaluminum hypophosphite, and flame retardant synergist is raised to 200°C (Comparative Test 7), the higher temperature hinders the effectiveness of the coupling agent and other additives added later, and may even cause some flame retardant components to slightly decompose (less than 0.5%), affecting the flame retardant effect and mechanical properties, and also deteriorating the product's precipitation resistance.
[0093] If nylon and chemically terminated melamine polyphosphate are first mixed, and then the organoaluminum hypophosphite and flame retardant synergist are added (Comparative Test 8), the flame retardant effect and mechanical properties are affected, and the product's precipitation resistance is also reduced. This further illustrates the important role of organoaluminum hypophosphite and flame retardant synergist in adding chemically terminated melamine polyphosphate, and that a specific mixing process is required to fully realize the synergistic effect of the three substances.
[0094] Comparative Example 1
[0095] This comparative example was essentially the same as Test 1 of Experimental Example 1, except that during the two-step synthesis process, only the material stirring screw was kept rotating (consistent with Test 1 of Experimental Example 1), while the rotary furnace drum (reaction chamber) remained stationary. All other parameters remained unchanged. The resulting chemically terminated melamine polyphosphate was tested for whiteness, nitrogen content, and 1% thermogravimetric loss temperature. The experimental results are shown in Table 4 (Test 1 in Table 4 corresponds to Test 1 in Table 2).
[0096] Comparative Example 2
[0097] This comparative example was essentially the same as Test 1 of Experimental Example 1, except that during the three-step synthesis process, the rotational speed of the material stirring screw remained the same as in Test 1 of Experimental Example 1, but the rotational speed of the rotary furnace drum (reaction chamber) was 150 rpm (a relatively fast rotational speed). All other parameters remained unchanged. The resulting chemically terminated melamine polyphosphate was tested for whiteness, nitrogen content, and 1% thermogravimetric loss temperature. The experimental results are shown in Table 4.
[0098] Comparative Example 3
[0099] This comparative example was essentially the same as Test 1 of Experimental Example 1, except that during the three-step synthesis process, the material stirring screw was maintained at a relatively fast speed of 350 rpm. However, the rotation speed of the rotary furnace drum (reaction chamber) was maintained at the same speed as in Test 1 of Experimental Example 1, with all other parameters remaining unchanged. The resulting chemically terminated melamine polyphosphate was tested for whiteness, nitrogen content, and 1% thermogravimetric loss temperature. The experimental results are shown in Table 4.
[0100] Table 4: Performance test results of chemically blocked melamine polyphosphates of Comparative Examples 1-3
[0101]
[0102] The above experimental data demonstrates that during the synthesis process, rotating the material stirring screw and the rotating furnace drum (reaction chamber) at a certain speed and in opposite directions is crucial for improving the flame retardant's whiteness, nitrogen content, and reducing thermal weight loss. If only the material stirring screw rotates, even if its rotation speed is increased (Comparative Example 1 → Comparative Example 3), the resulting product's whiteness and 1% thermal weight loss temperature remain suboptimal. If the rotating furnace drum (reaction chamber) rotates too quickly (Comparative Example 2), this also affects improvements in whiteness and 1% thermal weight loss temperature.
[0103] The above is only an embodiment of the present invention, and the common knowledge such as the specific technical solutions and / or characteristics in the solution are not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several variations and improvements can be made, which should also be regarded as the scope of protection of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the description can be used to interpret the content of the claims.
Claims
1. A highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant, characterized in that: The structural formula of the melamine polyphosphate is shown in the following chemical formula, and the melamine polyphosphate is capped by a capping agent; Wherein, n=1000-3000; the end-capping agent is a nitrogen-containing compound having no hydroxyl group and an NH bond.
2. The highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant according to claim 1, characterized in that: The end-capping agent includes at least one of R-NH2, R=NH, melamine, urea, biguanide and iminodiacetonitrile; R is an alkyl group with 1 to 4 carbon atoms.
3. The method for preparing a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant according to claim 1 or 2, characterized in that: The method includes the following steps in sequence: S1: Melamine phosphate is dehydrated by thermal polymerization to obtain melamine polyphosphate; S2: After the melamine polyphosphate and the blocking agent are heat-treated, chemically blocked melamine polyphosphate is obtained.
4. The method for preparing a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant according to claim 3, characterized in that: The reaction processes of S1 and S2 are both carried out in an inert gas environment; the reaction temperature, pressure and time of S1 are 220-360°C, 0.05-0.3MPa, and 60-300min, respectively; the reaction temperature, pressure and time of S2 are 180-360°C, 0.1-1.5MPa, and 30-240min, respectively.
5. The method for preparing a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant according to claim 3, characterized in that: The reaction processes of S1 and S2 are both carried out in a thermal polymerization reaction device; the polymerization reaction device includes a rotary furnace and a temperature control unit; a reaction chamber is provided in the rotary furnace, and a stirring screw is coaxially provided in the reaction chamber; the temperature control unit is used to control the temperature in the reaction chamber; during the reaction process, the stirring screw and the reaction chamber maintain different rotation directions.
6. The method for preparing a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant according to claim 3, characterized in that: The rotation speed of the stirring screw is 30-300 rpm, and the rotation speed of the reaction chamber is 3-120 rpm.
7. Use of a highly heat-resistant and precipitated chemically terminated melamine polyphosphate flame retardant according to claim 1 or 2 in flame-retardant nylon.
8. The use of a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant in flame-retardant nylon according to claim 7, characterized in that: The raw materials include, by weight: 30-80 parts of nylon, 5-60 parts of long glass fiber, 5-20 parts of chemically terminated melamine polyphosphate, 5-20 parts of organic aluminum hypophosphite, 0.5-4 parts of flame retardant synergist, 0.3-2 parts of nucleating agent, 0.5-2 parts of coupling agent, 0.3-3 parts of lubricant and 0.2-1 parts of antioxidant.
9. The use of a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant in flame-retardant nylon according to claim 8, characterized in that: The nylon comprises at least one of nylon 6, nylon 66, nylon 46, nylon 610, nylon 612, nylon 9, nylon 11, nylon 12, nylon 1010, nylon 1012 and nylon 1212; the long glass fiber is a rolled alkali-free glass fiber; the organic aluminum hypophosphite is diethyl aluminum phosphite; the flame retardant synergist comprises at least one of anhydrous zinc borate, 3.5-water zinc borate, zinc oxide and zirconium phosphate; the nucleating agent is BRUGGOLEN P22; the coupling agent is a silane coupling agent; the lubricant comprises at least one of ethylene bis stearamide, pentaerythritol stearate, silicone and amide wax; the antioxidant comprises at least one of antioxidant 168, antioxidant 1010 and antioxidant 1098.
10. The use of a highly heat-resistant and precipitated chemically blocked melamine polyphosphate flame retardant according to claim 9 in flame-retardant nylon, characterized in that: The flame retardant nylon is prepared by the following method: S1: Add nylon, chemically terminated melamine polyphosphate, organic aluminum hypophosphite and flame retardant synergist into a mixer and stir at room temperature for 5-30 minutes; S2: Raise the mixer temperature to 80-180°C, add the coupling agent and continue stirring for 10-30 minutes; S3: After cooling to room temperature, add lubricant, nucleating agent and antioxidant, and stir for 5-30 minutes to obtain a premix; S4: The premix is extruded by a twin-screw extruder, and long glass fibers are fed from the glass fiber port. The temperature during extrusion is 200-300°C. The premix is then drawn and pelletized, and then sieved and dehydrated to obtain flame-retardant reinforced nylon granules.
Citation Information
Patent Citations
Method for preparing crystallized V-shaped ammonium polyphosphate with stable crystal form
CN101891170A
Organic modified melamine polyphosphate and preparation method thereof
CN107459492A
Organic amine modified melamine polyphosphate and preparation method thereof
CN107556255A
Melamine pyrophosphate with high heat stability and preparation method thereof
CN108129407A
Refrigerating fluid-resistant precipitation-resistant flame-retardant bio-based polyamide composition and preparation method thereof
CN114479442A