Glass-ceramic article with a ceramic decoration, method for producing a glass-ceramic article and ink for use in a method of this type
The glass-ceramic article with a ceramic decoration, produced using inkjet printing and optimized ink composition, addresses thermal and mechanical stress issues by matching thermal expansion coefficients and enhancing surface smoothness, resulting in improved durability and resistance to detachment.
Patent Information
- Application Number
- PCT/EP2024/062841
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-21
AI Technical Summary
Existing glass-ceramic decorations on cooking surfaces face challenges with thermal and mechanical stress due to mismatched thermal expansion coefficients and rough surfaces, leading to potential detachment and reduced durability.
A glass-ceramic article with a ceramic decoration featuring pigment particles embedded in a glass matrix, produced using inkjet printing, which has a controlled thermal expansion coefficient difference of ≤6 ppm/K, a smooth surface with low blurriness and roughness, and improved mechanical resistance through optimized ink composition and printing processes.
The solution enhances the thermal and mechanical resilience of the decoration, reducing the risk of detachment and improving the durability and appearance of the glass-ceramic surface under thermal and mechanical loads.
Smart Images

Figure EP2024062841_21112024_PF_FP_ABST
Abstract
Description
[0001] Glass-ceramic article with a ceramic decoration, method for producing a glass-ceramic article and ink for use in such a method
[0002] Description
[0003] The invention relates to a glass-ceramic article according to the preamble of claim 1, as well as a method for producing such an article and an ink for use in such a method.
[0004] Glass-ceramic articles are known in the prior art in various forms. A "glass-ceramic article" is understood to mean an article whose main component is glass-ceramic. Well-known examples of this are cooking surfaces made of glass-ceramic. Typically, a multitude of markings and other optical elements are applied to the upper surface of such a cooking surface, for example, to indicate the boundaries of cooking zones or to highlight control elements, particularly touch-sensitive sensor surfaces. Furthermore, the type of cooking surface or a manufacturer's logo can also be applied to the upper surface of a cooking surface. Such markings and optical elements are collectively referred to below as "decoration." Therefore, a decoration within the meaning of the present invention does not have a purely artistic content, but rather serves a technical purpose.
[0005] During use on a cooktop, such decors are typically exposed to high thermal and mechanical stress. For example, significant local temperature differences exist in the area of the cooking zones or at their edges, which place stringent demands on the thermal expansion of such decors. At the same time, the decors are subjected to significant mechanical stress, for example, when moving cookware or cleaning the cooktop with an abrasive cleaner. These stresses must not lead to abrasion of the decor and thus a deterioration of the cooktop's visual appearance.
[0006] In the prior art, materials whose physical properties are similar to the substrate to which the decoration is applied, for example a plate made of glass ceramic, are therefore often used to produce such decorations. In particular, a glass frit is often used which is mixed with pigment particles and other substances to produce an ink and then applied to the substrate. During subsequent firing of the ink, the glass frit is melted and thus forms a glass matrix that is firmly bonded to the substrate and in which the pigment particles are embedded. With the appropriate choice of glass frit, a small difference in the thermal expansion coefficients between the substrate and the decoration can be achieved, thus preventing the decoration from detaching due to different thermal expansion between the substrate and decoration.
[0007] In the prior art, such decorations are usually applied using a screen printing process in which the ink is spread through a correspondingly structured screen using a squeegee, so that the ink is only deposited on the areas of the substrate defined by the screen. The decorations on substrates printed in this way often have a comparatively rough surface, which has a negative impact on the mechanical durability of the decoration. Furthermore, when a decoration is applied using screen printing, the specific shape of the decoration is predetermined by the corresponding screen. Changing the decoration is therefore only possible by replacing the screen, which is usually only possible by interrupting the printing process and a time-consuming retooling of the printing device.
[0008] In contrast, the present invention is based on the object of providing a glass-ceramic article with a ceramic decoration, which is characterized by high thermal and mechanical strength and can preferably be produced by alternative printing processes, in particular inkjet printing processes (hereinafter also referred to as "inkjet"). Furthermore, a corresponding process for producing such an article and an ink for use in such a process are specified.
[0009] In a first aspect, the invention accordingly relates to a glass-ceramic article with a ceramic decoration, wherein the decoration comprises pigment particles embedded in a glass matrix. The article has a glass-ceramic substrate with a first thermal expansion coefficient e n , wherein the decoration has a second thermal expansion coefficient θ 2 . The difference λa between the expansion coefficients λ and λ t 2 is at most 6 ppm / K, preferably at most 4 ppm / K, particularly preferably at most 3 ppm / K. Furthermore, the decoration has a layer thickness of 0.5 - 5 pm, and a blurriness according to ISO 24790 of less than 100 pm, preferably less than 70 pm, particularly preferably less than 50 pm.
[0010] It is further provided that the smoothness Sdq of the decoration has a value of less than 25 pm / mm, preferably less than 20 pm / mm, particularly preferably less than 15 pm / mm, wherein the smoothness is calculated as follows: where z describes an elevation of the decorative surface above a reference surface, the reference surface being spanned parallel to the surface of the glass-ceramic substrate and A describing a partial area of the surface of the decorative surface.
[0011] Limiting the smoothness of the decoration to values less than 25 pm / mm has the effect of providing a smaller surface area for forces acting essentially parallel to the surface of the substrate, which could lead to the decoration detaching from the substrate. Consequently, the inventive design of the decoration increases its mechanical strength.
[0012] The smoothness Sdq, described as a characteristic feature, describes the gradient of the decorative surface compared to the substrate surface, averaged over a reference surface A. The values x and y describe the width and length of a measuring window in the form of the reference surface A, while the height function z(x,y) describes the local elevation of the decoration above a reference surface, in particular the surface of the decoration. In this case, the reference surface A can be a measuring window with a size of 1.5 x 1.5 mm. 2be provided which lies completely within the decoration, i.e. does not include any unprinted areas of the substrate. The partial derivatives of the height function dz(x,y) / dx and dz(x,y) / dy indicate the gradient of the decoration surface in the x and y directions at each measuring point on the measuring area A. These gradients per measuring point in the x and y directions are added quadratically and summed for each measuring point (x,y) on the measuring area A. The result thus obtained is then divided by the measuring area A and the square root is taken from the result.
[0013] A "ceramic decoration" is generally understood to be a decoration whose main components are inorganic, non-metallic materials. The glass frit used, in which the pigment particles of the decoration are embedded after the glass frit is melted during a firing process, is adapted in its mechanical and thermal properties to the properties of the substrate. In particular, the chemical composition of the glass frit can be designed to closely match the chemical composition of the substrate, so that the substrate and decoration have approximately the same thermal expansion coefficients.
[0014] As already stated above, the decoration further exhibits a blurriness according to ISO 24790 of less than 100 pm, preferably less than 70 pm, and particularly preferably less than 50 pm. Blurriness is a measure of the sharpness of the edges of a decoration and indicates the distance over which the thickness of the decoration at its edge decreases from its nominal thickness to a defined level. The previously described mechanical resistance of the decoration is further improved according to a further embodiment in that the scattering Sq of the decorative layer has a value of less than 250 nm, preferably less than 200 nm, wherein the scattering Sq of the decorative layer is calculated as follows:
[0015] Sq = J A where z describes a distance of the decorative surface from a reference surface, the reference surface being spanned parallel to the surface of the glass-ceramic substrate and A describing a partial area of the surface of the decorative surface.
[0016] The scattering of the decorative layer Sq according to the previously described calculation method provides a measure of the roughness of the surface of the decoration. The parameters used in the calculation method are defined analogously to the previously described calculation of the smoothness of the decoration Sdq. The value Sq represents the root mean square of the ordinate values z(x,y) of the decoration within the reference surface A and corresponds to the standard deviation of the roughness within the reference surface A. Analogous to the previous considerations, a lower roughness of the surface of the decoration also results in the decoration offering only a small area of attack for forces acting on the decoration essentially parallel to the surface of the substrate, which further increases the mechanical resistance of the decoration.
[0017] The roughness of the decorative layer is influenced by a variety of properties of the decor. Among other things, a homogeneous distribution of the decorative components, and in particular a homogeneous distribution of the pigment particles within the decor, contributes to low roughness, as this prevents local accumulations or clusters of pigment particles, which can lead to a local increase in the thickness of the decor and thus to an increase in roughness and a reduction in the smoothness of the decor.
[0018] A homogeneous distribution of the decoration and the pigment particles is also reflected, among other parameters, which particularly describe the print quality of the decoration. According to another embodiment, the decoration has a raggedness according to ISO 24790 of no more than 20 μm, preferably no more than 10 μm. Raggedness refers to the fraying of edges or margins of the decoration, for example, the local deviation of the edge of the decoration from the actually achievable, ideal geometry of the intended decoration. Even minimal fraying of the contours of the decoration contributes to the decoration offering the smallest possible surface area for acting forces, so that even minimal raggedness contributes to the mechanical resistance of the decoration.According to a further embodiment, a particularly homogeneous decorative layer is further achieved in that the particle size distribution of the pigment particles is D100 less than 5 pm, D90 less than 5 pm, preferably less than 2.5 pm, particularly preferably less than 1 pm, and D50 less than 1 pm. As already described, this contributes to the high smoothness, low roughness, and clean edge quality of the decoration, resulting in a high mechanical resistance of the decoration. The small size and uniform size distribution of the pigment particles also contribute to the achievement of low layer thicknesses of the decoration, whereby the layers are very homogeneous and thus particularly stable.
[0019] The high mechanical resistance of the decoration is also demonstrated in a further embodiment in that the decoration, after carrying out an abrasion test using an abrasive medium with abrasive particles, preferably consisting of AI2O3 with a d50 of 5-20 pm and a solid content of 30-35%, at a contact pressure on the decoration of 1 N / cm 2after 500 strokes over a distance of 15 cm, has an abrasion of less than 0.5 pm, preferably less than 0.3 pm. “Abrasion” is understood to mean the reduction in the thickness of the decoration as a result of the abrasion test. To carry out such an abrasion test, a cloth can be used, for example, as the carrier material for the abrasive medium, whereby a commercially available cleaning agent with the properties mentioned above can be used as the abrasive medium. When carrying out the abrasion test, the test is preferably carried out on a track with a width of approximately 2 cm. To pre-treat the area to be tested, it is preferred that the area to be tested is cleaned of dirt using another cleaner before carrying out the abrasion test and then dried so that reproducible test conditions are established.
[0020] Such tests can also be automated, for example, with the aid of a suitable testing device such as the Elcometer 1720 Washability Tester. In particular, a test speed can be set that specifies the speed at which the abrasive medium is moved over the decoration to be tested. A test speed of approximately 35 to 40, particularly 37, test cycles or strokes per minute is preferred.
[0021] The degree of abrasion is influenced, among other things, by the specific nature of the solids acting as abrasive particles in the abrasive medium. It is preferred that the abrasive particles essentially have a size of 1 pm to 50 pm. In particular, the grain size distribution of the abrasive particles can be such that D10 is approximately 1 pm, D50 approximately 9 pm, and D90 approximately 30 pm. The abrasive particles can consist of aluminum oxide, for example, and can be emulsified in a suitable carrier medium.
[0022] According to a further embodiment, it is further provided that the weight ratio of glass to pigment of the decoration is 1:0.15 or greater. A high proportion of glass compared to pigment in the decoration can positively influence the surface quality of the decoration, since the glass portion essentially melts smoothly when the decoration is fired, thus promoting a smooth surface of the decoration. With a higher pigment proportion, on the other hand, the surface would possibly be roughened by protruding pigment particles. As already described above, a high level of smoothness of the decorative surface has a very positive effect on the mechanical resistance of the decoration to mechanical stress.
[0023] According to a further embodiment, the high quality of a decoration according to the invention is particularly evident in that the decoration has a partial geometry, wherein the partial geometry has a line width of at most 0.5 mm, preferably at most 3 mm, particularly preferably at most 1 mm.
[0024] In a further aspect, the invention relates to a method for producing a glass-ceramic article according to one of the preceding claims, comprising the steps:
[0025] • Providing the glass-ceramic substrate,
[0026] • Determining a target decoration to be applied to the substrate, wherein the target decoration is divided into a grid of regularly arranged pixels,
[0027] • pixel-by-pixel application of an ink to positions on the substrate corresponding to the pixels of the desired decoration by means of a printing device, in particular an inkjet printer, and
[0028] • Burning the ink onto the substrate.
[0029] The glass-ceramic substrate is preferably a glass-ceramic plate, particularly intended for use as a cooktop. Both colored and uncolored, transparent substrates can be used.
[0030] The target decor can be determined in particular by automated reading of a storage medium. The target decor can have different types of decor. For example, a target decor can be composed of line patterns and flat printed areas. Furthermore, the target decor can also include areas that have certain geometric patterns. The target decor is specified in the form of a regular grid, in particular, with a color value, in particular a gray value, being specified for each individual pixel of the grid. The target decor can also be derived from a precursor graphic, which does not necessarily have to be in raster form. For example, in a preceding step, it can also be provided that a graphic initially available in a different format, e.g. a vector graphic, is converted into a raster graphic and then interpreted as the target decor.
[0031] The subsequent pixel-by-pixel application of the ink to the substrate is preferably carried out by moving a corresponding print head of the printing device, which is particularly designed as an inkjet printer, to a point on the substrate corresponding to the raster point of the desired decoration. At the corresponding position, a defined amount of ink is then applied to the substrate according to the specified operating parameters of the printing device. The resulting print image can be adapted to individual requirements by varying the operating parameters of the printing device accordingly.
[0032] Once all of the pixels of the desired decoration have been transferred to the substrate, the ink is then fired onto the substrate. Firing here means that the ink is exposed to a temperature that causes the glass portion of the ink to melt. This can also cause volatile components of the ink to evaporate. By melting the glass, the pigment particles are firmly embedded in the resulting glass matrix. Firing can take place at a firing temperature of preferably < 1200 °C, more preferably < 900 °C, even more preferably < 850 °C, even more preferably < 800 °C, in particular < 750 °C and preferably a firing time in the range of 2 minutes to 5 hours, more preferably 5 minutes to 1 hour, in particular 10 to 15 minutes.
[0033] According to one embodiment, the quality of the decoration or the achieved print image and the homogeneity of the layer produced thereby are improved in that the method further comprises modifying the target decoration, wherein the modification of the target decoration includes selectively deleting pixels from the target decoration. "Deleting pixels" is to be understood as meaning that at an inked raster point, i.e., a raster point at whose corresponding position on the substrate ink is to be applied, the corresponding information is changed such that no ink is applied to the substrate. In effect, therefore, the pixel itself is not deleted, but rather the color information is changed to "not printed."
[0034] For example, such deletion of pixels can be provided for an area that is to be printed over the entire surface, i.e., for all pixels in a larger area, ink is to be applied to the corresponding position on the substrate. In this case, for example, the homogeneity of the resulting layer and thus the mechanical durability of the decoration can be increased if a certain percentage of the corresponding pixels are deleted. Furthermore, the overall print image can also be improved in this way.
[0035] When using an inkjet printer, printing is usually done line by line. This means that the inkjet printer's print head moves over all positions on the substrate that are adjacent to one another in a line of the target decoration, with a corresponding amount of ink being applied to corresponding positions on the substrate where a color value is specified according to the target decoration. Once the print head has moved over all points in a line, the procedure is repeated for an adjacent line. According to one embodiment, the printing process itself can be accelerated by applying the ink to a plurality of pixels arranged next to one another in a row simultaneously. In this way, several lines of the target decoration can effectively be transferred to the substrate simultaneously with a single pass of the print head, which can significantly shorten the overall duration of the printing process.Particularly preferably, it can be provided that the transfer of the desired decoration is carried out by means of a single pass of the print head onto the substrate, i.e. all lines of the desired decoration are printed simultaneously.
[0036] In a further aspect, the invention relates to an ink for use in a method according to any one of claims 8 to 10, wherein the ink comprises pigment particles, glass particles (also referred to as "glass frit"), a solvent, a dispersant, and a wetting additive, characterized in that the ink is free of binders. A binder is typically used to maintain the structural fidelity and layer morphology of the ink applied to the substrate until the glass particles melt. However, it has been shown that omitting a binder in the ink has a positive effect on the resulting printed image and, in particular, on the durability of a corresponding decoration.
[0037] An example composition of the ink is as follows:
[0038] Pigment particles 0.1 - 5 Vol-%
[0039] Glass particles 10 - 20 Vol-%
[0040] Solvent 70 - 85 vol-%
[0041] Dispersant 0.5 - 5 Vol-%
[0042] Wetting additive 0.1 - 5 vol-%
[0043] The pigment particles preferably have a grain size of 0.2 - 2.5 pm, with D10 preferably being 0.2 - 0.3 pm, D50 0.6 - 0.9 pm and D90 1.3 - 1.7 pm. A suitable solvent can be selected from water, alcohols, ethers such as glycol ethers, lactates, acetates, aldehydes, ketones, aromatic hydrocarbons, oils and fatty acid derivatives. Commercially available products can also be used, such as solvents from Johnson Matthey (e.g. high-boiling paste oils such as JM 850-63 or JM 650-63); Dowanol DB (diethylene glycol n-butyl ether from Dow Chemical) or the like. Mixtures of two or more of these compounds are also possible. Preferred examples include, but are not limited to, polyethylene glycol, ethylene glycol monobutyl ether, dipropylene monoglycol ether, 1-methoxy-2-propanol, and diethylene glycol n-butyl ether, as well as commercially available solvents.
[0044] A wide range of dispersants can be used according to the invention. These are, for example, selected from the group consisting of lecithin, phosphoric acid esters, amine salts, polyesterstyrene resins, xylene, castor oil, 3-acryloxypropyltrimethoxysilane, polycarboxylic acids, polycarboxylic acid polyesters, polyacrylates, polyamides, polyamine amides, esters, micronized polyethylene wax, polyethylene glycol, silicones, alkoxysilanes, hybrid polymers, organically modified metal alkoxides, high-molecular-weight copolymers with pigment-affinity groups, block copolymers, graft copolymers, and mixtures thereof. Commercially available dispersants, for example from TEGO or Byk, such as TEGO® Dispers, TEGO® VariPlus, TEGO® ViscoPlus, Bykumen®, Disperbyk®, BYK®, Anti-Terra® U, K-Sperse XD, Efka, Texaphor® or the like, are also used.Particularly preferred are organically modified metal alkoxides, such as 3-methacryloxypropyltriethoxysilane (MPTES), 3-methacryloxypropyltrimethoxysilane (MPTMS), 3-glycidoxypropyltriethoxysilane (GPTES), 3-glycidoxypropyltrimethoxysilane (GPTMS), Dynasylan VTMO, isooctyltriethoxysilane, or 7-octenyltrimethoxysilane, as well as commercial dispersing additives from Byk and TEGO. Mixtures can also be used. In the present invention, the dispersant is also referred to as a dispersing additive, which assists in the distribution of the glass frit and / or the additives in the solvent.
[0045] Commercially available products such as TEGO® Dispers, TEGO® Wet, TEGO® TWIN, BYK® can be used as wetting additives.
[0046] The glass particles preferably have the following composition:
[0047] 45 - 85 wt.% SiO2, 2 - 20 wt.% Al2O3, 0 - 23 wt.%, preferably 0 - 18 wt.% B2O3, 0 wt.% Bi2O3, 0 - 15 wt.%, more preferably 1 - 15 wt.%, even more preferably 1 - 9 wt.% alkali oxides, 0 - 18 wt.% alkaline earth oxides,
[0048] 0 - 7 wt% ZnO,
[0049] 0 - 3 wt.% TiO2,
[0050] 0 - 5 wt% ZrO2, and 0 - 2 wt% halides.
[0051] Preferred embodiments of the invention are explained in more detail below with reference to the figures. In the figures:
[0052] Figure 1 is a schematic representation of an exemplary glass-ceramic article in the form of a hob,
[0053] Figure 2 shows a representation of the surface profile of an exemplary decoration of the hob of Figure 1,
[0054] Figure 3 is a greatly enlarged view of the decoration,
[0055] Figure 4 shows a detailed view of another exemplary decoration,
[0056] Figure 5 is a flowchart of an exemplary method, and
[0057] Figure 6 shows an example representation for modifying a target geometry.
[0058] In the following, similar or identical features are marked with the same reference symbols.
[0059] Figure 1 shows a schematic representation of an exemplary glass-ceramic article in the form of a hob 100. Accordingly, the hob 100 consists of a plate made of a glass ceramic, which has, for example, dimensions HBT of 4x740x560mm 3 In particular, this can be a colored glass ceramic.
[0060] Different types of decorations are typically applied to the top of such a cooktop, serving different purposes. Figure 1 shows, as an example, a first variant of a top-side decoration in the form of a circular cooking zone boundary 102. Such a cooking zone boundary 102 can, for example, indicate the area of the cooking surface 100 in which cookware can be heated by inductive or radiation-based heating elements arranged beneath the cooktop. Such cooking zone boundaries 102 are typically represented by comparatively thick contours and are subject to strong mechanical stress, for example, when cookware is moved beyond the cooking zone boundary 102.
[0061] At the bottom center of the hob, a control panel 104 is indicated for controlling the hob 100 or the heating elements arranged beneath the hob 100. Such a control panel 104 can have a wide variety of decorative elements. In addition to surface-applied decorative elements, for example, to represent adjustment ranges for a temperature control of the cooking surface 100, very fine decorative elements can also be provided in such an area, by means of which control symbols, in particular numbers and characters, are displayed.
[0062] A third variant of a decoration shown in Figure 1 is a pattern 106 that is applied largely over the entire surface and only has recesses in the area of the cooking zone boundaries 102 and the control panel 104. Such patterns 106 can be applied, for example, for purely aesthetic reasons and can contain colored elements in addition to different patterns. In particular, such a pattern 106 can also contain very finely printed elements that have a line width of 0.1 mm. Not shown in Figure 1 are further markings on the upper side of the cooktop 100 that indicate, for example, the manufacturer of the cooktop, the type of cooktop, or other product-specific information. Such markings are usually arranged in the area of the corners of the cooktop 100.
[0063] The previously described types of decorations are exposed to different types of stress during operation of such a cooking surface 100. A first type of stress is thermal stress, which results from the heating of the cooking surface 100 in certain areas. This creates locally different temperature gradients, which can lead to different thermal expansions depending on the nature of the substrate and the decoration. In extreme cases, this can cause the decoration to detach from the substrate. However, this effect can be compensated for by adapting the thermal expansion coefficient of the decoration to the thermal expansion coefficient of the substrate.
[0064] A second type of stress is mechanical stress on the decoration. Such a stress can occur during operation of the cooking surface 100 due to cookware being moved beyond the cooking zone boundaries 102. In this case, forces can act on the decoration that act essentially parallel to the surface of the substrate and can thus also lead to the decoration detaching from the substrate. The same effect can also occur when the cooking surface is cleaned with abrasive cleaning agents, since in this case a force also acts parallel to the substrate surface. As already described above, the resistance of the decoration to mechanical stress is increased according to the invention in particular by the smoothness Sdq of the surface of the decoration having a value of less than 25 pm / mm, preferably less than 20 pm / mm, particularly preferably less than 15 pm / mm.The smoothness of the decorative surface describes the average gradient of the decorative surface, as described above. For this purpose, Figure 2 a) shows an illustration of the surface profile of an exemplary decoration of the hob in Figure 1, wherein the surface profile was recorded using white light interferometry. The decoration shown in Figure 2 a) was produced using an inkjet printing process, which is described in more detail below. In comparison, Figure 2 b) shows a surface profile of a decoration that was produced using a screen printing process. The local deviation of the height z of the decoration from a reference surface is shown.
[0065] As can be clearly seen in Figure 2 a), particularly in comparison to Figure 2 b), the surface of the decoration according to the invention does indeed have elevations comparable in amplitude to those of the decoration in Figure 2 b). However, the respective elevations are significantly wider and less sharply defined from their surroundings. Accordingly, the number of such elevations within the reference surface under consideration is also significantly lower, resulting in an overall reduced mean gradient of the surface of Figure 2 a) compared to Figure 2 b).
[0066] The described smoothness of the decoration is achieved, among other things, by the use of an inkjet printing process to produce the decoration. The composition of the ink used, in particular the pigment particles used, also influences the surface quality of the decoration. As already explained above, it is particularly advantageous if the pigment particles have a particle size distribution with a D50 of less than 1 pm and a D90 of less than 5 pm, preferably less than 2.5 pm, particularly preferably less than 1 pm. For this purpose, Figure 3 a) shows an example of an image of a decorative surface according to the invention taken by means of scanning electron microscopy, while Figure 3 b) shows an image of a decoration applied by means of screen printing for comparison.As can be clearly seen in Figure 3, the pigment particles used in the exemplary decoration of Figure 3 a) are significantly smaller and distributed much more homogeneously than the particles shown in Figure 3 b).
[0067] In addition to the described surface quality, a decoration according to the invention is also characterized by the quality of its edges and contours. For this purpose, Figure 4 shows, by way of example, a detailed view of another exemplary decoration or of a portion of an exemplary decoration with a line geometry. Figure 4 a) again shows an exemplary decoration which was produced using an inkjet printing process, while Figure 4 b) shows, for comparison, a decoration produced using screen printing. As can be seen from a comparison of the figures, the decoration in Figure 4 a) has less fluctuation in the edge profile and less fraying and therefore less raggedness than the decoration in Figure 4 b).The contour sharpness of the decoration in Figure 4 a), expressed by the degree of blurriness, is also greater than the contour sharpness of the decoration in Figure 4 b), which, as previously explained, has a positive effect on the mechanical resistance of the decoration.
[0068] Figure 5 shows a flow diagram of an exemplary method for producing a decoration as described above. In a first method step 200, a glass-ceramic substrate is provided. The substrate can, in principle, be either a volume-colored substrate or a transparent substrate. Providing the substrate can, in particular, include a preparation of the surface of the substrate that is to be subsequently printed. Such preparation can, in particular, include a pretreatment to remove contaminants and deposits, such as production residues from previous processing steps.Furthermore, the provision may also include clamping the substrate in a corresponding carrier device so that the position of the substrate relative to a printing device is firmly defined and no unintentional displacement of the substrate occurs even during the printing process.
[0069] In a second method step 202, which can in principle also be performed in parallel with the first method step, a target decoration to be applied to the substrate is determined. Such "determination" can in particular involve retrieving corresponding information from a storage medium. The target decoration is divided into a grid of regularly arranged pixels and is therefore preferably processed as a raster graphic. Determining the target decoration can also involve converting a precursor graphic, for example, a vector graphic, into such a raster graphic.
[0070] Before the actual printing process, such a target decoration can be subjected to further preprocessing steps. For this purpose, for example, in step 204, the target decoration can be modified, wherein the modification of the target decoration includes a selective deletion of pixels from the target decoration. In this regard, it has been shown that the print image can be significantly improved by a clever selection of the pixels of the target decoration to be deleted. Such selective deletion of pixels is illustrated as an example in Figure 6. Figure 6 a) shows a raster graphic of the letter "R" as the initial target decoration. In Figure 6 b), in contrast, individual pixels have been deleted from the raster graphic, where "deleted" in this case means that the color information at the corresponding positions in the raster graphic is changed to the value "not printed".
[0071] Referring again to Figure 5, after determining and, if necessary, modifying the target decoration in step 206, the target decoration is transferred to the substrate. For this purpose, ink is applied pixel by pixel to positions on the substrate corresponding to the pixels of the target decoration using a printing device, in particular an inkjet printer. For this purpose, a corresponding print head of the inkjet printer is preferably moved to the corresponding position, and a defined amount of ink is deposited onto the substrate depending on the color information of the pixel corresponding to the position. The print head can, in particular, be moved line by line across the substrate.During such a pass over the substrate, according to one embodiment, the ink can also be applied simultaneously to a plurality of pixels arranged next to one another in a row, with such a "row" extending perpendicular to the direction of movement of the print head. Particularly preferably, a print head can also be designed such that the entire decoration is applied to the substrate with a single pass of the print head over the substrate.
[0072] Depending on the design of the inkjet printer, the print image can be adapted to the respective requirements by varying a variety of operating parameters. In particular, parameters such as the speed of the print head during a single pass, the distance of the print head from the substrate surface, or the amount of ink dispensed per pixel can be varied.
[0073] In a final process step 208, the applied ink is then fired onto the substrate. The firing of the decoration preferably takes place at a temperature sufficient to melt the glass particles of the ink used, but does not lead to a change in the substrate, in particular to a ceramization or melting of the substrate surface.
Claims
Patent claims 1. A glass-ceramic article with a ceramic decoration, wherein the decoration comprises pigment particles embedded in a glass matrix, wherein the article has a glass-ceramic substrate with a first thermal expansion coefficient e n , wherein the decoration has a second thermal expansion coefficient Δt2 , wherein the difference Δa between the expansion coefficients Δt and Δt2 is at most 6 ppm / K, preferably at most 4 ppm / K, particularly preferably at most 3 ppm / K, wherein the decoration has a layer thickness of 0.5 - 5 μm, wherein the decoration has a blurriness according to ISO 24790 of less than 100 μm, preferably less than 70 μm, particularly preferably less than 50 μm, and wherein the smoothness Sdq of the decoration has a value of less than 25 μm / mm, preferably less than 20 μm / mm, particularly preferably less than 15 μm / mm, wherein the smoothness is calculated as follows: where z describes an elevation of the decorative surface above a reference surface, the reference surface being spanned parallel to the surface of the glass-ceramic substrate and A describing a partial area of the surface of the decorative surface.
2. Glass-ceramic article according to claim 1, characterized in that the scattering Sq of the decorative layer has a value of less than 250 nm, preferably less than 200 nm, wherein the scattering Sq of the decorative layer is calculated as follows: where z describes a distance of the decorative surface from a reference surface, the reference surface being spanned parallel to the surface of the glass-ceramic substrate and A describing a partial area of the surface of the decorative surface.
3. Glass-ceramic article according to one of the preceding claims, characterized in that the decoration has a raggedness according to ISO 24790 of at most 20 pm, preferably at most 10 pm.
4. Glass-ceramic article according to one of the preceding claims, characterized in that for the particle size distribution of the pigment particles D100 less than 5 pm, D90 less than 5 pm, preferably less than 2.5 pm, particularly preferably less than 1 pm and D50 is less than 1 pm.
5. Glass-ceramic article according to one of the preceding claims, characterized in that the decoration, after carrying out an abrasion test using an abrasive medium with a solid content of 30-35% at a contact pressure on the decoration of 1 N / cm 2 after 500 strokes over a distance of 15 cm, has an abrasion of less than 0.5 pm, preferably less than 0.3 pm.
6. Glass-ceramic article according to one of the preceding claims, characterized in that the weight ratio of glass to pigment of the decoration is 1:0.15 or greater.
7. Glass-ceramic article according to one of the preceding claims, characterized in that the decoration has a partial geometry, wherein the partial geometry has a line width of at most 0.5 mm.
8. A method for producing a glass-ceramic article according to any one of the preceding claims, comprising the steps: • Providing the glass-ceramic substrate, • Determining a target decoration to be applied to the substrate, wherein the target decoration is divided into a grid of regularly arranged pixels, • pixel-by-pixel application of an ink to positions on the substrate corresponding to the pixels of the desired decoration by means of a printing device, in particular an inkjet printer, and • Burning the ink onto the substrate.
9. The method according to claim 8, characterized in that the method further comprises modifying the target decoration, wherein modifying the target decoration includes selectively deleting pixels from the target decoration.
10. Method according to claim 8 or 9, characterized in that the ink is applied simultaneously to a plurality of pixels arranged next to one another in a row.
11. An ink for use in a method according to any one of claims 8 to 10, wherein the ink comprises pigment particles, glass particles, a solvent, a dispersant, and a wetting additive, characterized in that the ink is free of binders.
Citation Information
Patent Citations
ceramic ink jet printing ink for glass and / or glass ceramics, method for their manufacture and use
DE102014010335A1
Plate comprising glass or glass ceramic, method for the production thereof and use thereof
EP4317094A1
Ceramic printing ink, in particular for inkjet printing, for producing a coating on a glass ceramic, and coated glass ceramic panel