System for assessing the toughness of longitudinal high frequency induction or resistance welds in steel tubes and associated method

The system evaluates weld toughness through image analysis and microstructural profiling, addressing the limitations of existing methods by providing a non-destructive, systematic approach for assessing the integrity of high-frequency induction or resistance welds in steel tubes, particularly in hydrogen environments, thereby enhancing pipeline safety.

WO2024236214A1PCT designated stage expired Publication Date: 2024-11-21CONSEJO SUPERIOR DE INVESTIGACIONES CIENTIFICAS (CSIC)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/ES2024/070297
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-05-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current methods for evaluating the toughness of longitudinal high-frequency induction or resistance welds in steel tubes are either destructive, costly, or limited to large diameter tubes, and do not effectively assess toughness in the presence of gases like hydrogen, which embrittles the steel, posing a risk for gas pipeline safety.

Method used

A non-destructive system and method using image acquisition, processing, and analysis to categorize the toughness of welds based on microstructural characteristics around the joint line, providing a gray scale profile and evaluating hardness, allowing for systematic evaluation of weld integrity without mechanical tests.

Benefits of technology

Enables accurate, non-destructive assessment of weld toughness, improving the categorization of steel tubes as PSL1 or PSL2 and enhancing safety by identifying potential weaknesses in gas pipelines, especially in hydrogen environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure ES2024070297_21112024_PF_FP_ABST
    Figure ES2024070297_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention falls within the technical field of systems and methods for the assessment of longitudinal welds in steel tubes, and more specifically of longitudinal welds made by high-frequency induction welding (HFW) or electric resistance welding (ERW), and consists of a system for the assessment of the toughness of longitudinal high-frequency induction or resistance welds in steel tubes, and an associated method.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] SYSTEM FOR EVALUATING THE TENACITY OF LONGITUDINAL WELDMENT BY HIGH FREQUENCY INDUCTION OR RESISTANCE IN STEEL PIPES AND ASSOCIATED METHOD

[0002] DESCRIPTION

[0003] OBJECT OF THE INVENTION

[0004] The present invention falls within the technical field of systems and methods for evaluating longitudinal welds in steel pipes, and more specifically longitudinal welds made by high frequency induction heating (HFW, acronym in English for “High Frequency Welding”) or by resistance (ERW, acronym in English for “Electric Resistance Welding”).

[0005] The object of the invention consists of a system for evaluating the toughness of longitudinal welds by high frequency induction or resistance in steel tubes and an associated method, where the associated method can be carried out in air or in the presence of gases that can embrittle the steel, such as hydrogen or mixtures of hydrogen with other gases.

[0006] BACKGROUND OF THE INVENTION

[0007] Currently, there are a multitude of pipes manufactured worldwide with different diameters and wall thicknesses using resistance or induction welding. These pipes are manufactured in different steel compositions (Grade B, X42, X52, X60, X70, and X80 in the gas transportation industry) and are primarily used for the transportation of low-pressure fluids (typically <200 bar), such as natural gas, oil, or water. Additionally, these pipes are used in other applications such as foundation work, the automotive sector, and for the protection of communication cables.

[0008] High-frequency induction or resistance welding is a complex process that is carried out without filler material or shielding gas, and in which the welding operation is determined by a huge number of parameters, some of them interrelated. These parameters affect the quality of the weld and the microstructure of the different typical regions called: bond line (LU), thermo-mechanically affected (TMAZ) and thermally affected (HAZ), as shown in Figure 1.

[0009] The welding process, and specifically its adjustment, depends on the chemical composition of the material used to manufacture the tube: the frequency of the induced electric field, the position of the inductor, the maximum temperature reached, the speed of the tube's advance as it passes through the inductor or the resistance, the mechanical stresses applied to the material at the welding point and the angle (vee) at the point of contact of the sheets mainly.

[0010] The high-frequency induction welding process generates a microstructure around the bond line (BL) with very low toughness, i.e., low resistance to crack propagation. This low toughness is microstructurally explained by the clustering of grains with the same crystallographic orientation around the bond line (BL), and also by the presence of low-toughness, high-hardness phases such as retained austenite or martensite. Each color in Figure 2 represents a crystallographic orientation. Furthermore, this zone of inherent low toughness is particularly damaging because it is perfectly aligned along the longitudinal direction of the tube. To prevent the low toughness of the tubes after the welding process, the welded tubes undergo a high-temperature heat treatment called normalizing (or double normalizing), or quenching and annealing.These treatments are usually effective in modifying, preferably to the point of virtually eliminating, the detrimental microstructure around the bond line (BL) generated during high-frequency induction or resistance welding. If this heat treatment is performed properly, brittle phases (e.g., martensite) and the grouping of grains with the same crystallographic orientation should disappear, but this is not always the case. Despite single or even double normalization, the low bond line (BL) toughness sometimes persists. The integrity of high-frequency induction or resistance welding on tubes is assessed differently at the factory than it is when the tube is in service.During the manufacturing process, quality control of the tube is carried out through the inspection of the process parameters used during welding (temperature, travel speed of the tube as it passes through the inductor or resistance, stresses generated on the material at the welding point, vee angle, electrical characteristics of the induction process, etc. (Experimental Investigation of Temperature and Contact Pressure Influence on HFI Welded Joint Properties, Christian Egger, Martin Kroll, Kerstin Kern, Yannik Steimer, Michael Schreiner and Wolfgang Tillmann). Additionally, a visual inspection of the weld is carried out and, in the highest quality standard, PSL2, a series of destructive mechanical tests are performed, including the resilience test (Charpy test) to evaluate the toughness of the weld.Pipelines in service undergo periodic inspections to assess their integrity and detect the presence of cracks, corrosion attacks, and other defects that could jeopardize the installation. This inspection and study of the integrity of gas pipelines is typically performed using systems called PIGS (Pipeline Integrity Gauges). These systems travel inside the pipe using the pressure of the fluid transported in the installation and detect defects using technologies such as magnetic flux leakage or ultrasound. However, the use of these systems is limited to large-diameter pipes and installations designed to allow the PIG to move around the installation, for example, avoiding sharp bends. In any case, these systems cannot determine the toughness value of the pipe in service.Toughness is the key aspect that differentiates the two quality levels of HFI / ERW pipes, described as PSL1 and PSL2 according to the API 5L standard. Pipes designated PSL1 must meet several requirements, such as the chemical composition of the steel, type of pipe end finish (plain, threaded or flared), etc. PSL2 pipes, of higher quality than PSL1, are subject to mechanical requirements in terms of yield strength, ultimate stress, and bond line toughness (BLT). Categorizing a pipe as PSL1 or PSL2 without performing mechanical testing remains a challenge for the low-pressure fluid transportation industry, such as gas pipelines. Furthermore, despite the numerous quality controls applied to HFW and ERW pipes, both in the factory and in service, hundreds of accidents occur annually due to lower bond line toughness compared to the base material of the pipe.One of the reasons for this high number of accidents is that the bond line (BL) toughness assessment of new pipes in the factory was not properly performed until the latest amendment to the European standard ISO 3183, Petroleum and natural gas industries - Steel pipes for pipeline transport systems (ISO 3183:2019). Bond line toughness (BL) toughness (resilience) determination according to these standards is performed using low-temperature Charpy tests (maximum 0. eC). Performing these tests has several negative aspects, such as the fact that they are destructive tests, their cost, and the time required to correctly machine the specimens and the test time. Specifically, the evaluation of bond line toughness (BLT) requires machining the specimens with extremely high precision with respect to the bond line (BLT), + / - 250pm around the bond line (BLT) at most. This procedure has been included in the latest version of the ISO 3183:2019 standard, but despite the fact that it allows the evaluation of bond line toughness (BLT) of HFW and ERW pipes, it is also a destructive evaluation system.

[0011] In recent years, promising new systems have been developed to non-destructively evaluate the toughness of in-service pipes through surface mechanical testing by performing controlled scratching or peeling processes on the pipe surface, as in “Nondestructive Evaluation for Yield Strength and Toughness of Steel Pipelines” SD Palkovic, K. Taniguchi, SC Bellemare: Massachusetts Materials Technologies, LLC, Cambridge, MA 2: Massachusetts Institute of Technology, Cambridge, MA. Conference: NACE 2018. At: Phoenix, AZ. These methods perform a friction sliding procedure and characterize the generated grooves or ligaments to evaluate the hardness and toughness around the bond line (BL), respectively. However, this method is not purely experimental and is based on the use of data from finite element simulations.Furthermore, the previous document acknowledges that further testing and calibration are still needed to validate the method in real-life cases.

[0012] Additionally, the current global decarbonization trend has led to the repurposing of gas transportation infrastructure for the transport of hydrogen or mixtures of hydrogen and other gases (mainly natural gas). The presence of hydrogen in gas pipelines will reduce the toughness of components, primarily welds, including HFI / ERW welds. This reduction in toughness is directly related to the presence of high-hardness zones, strong microstructural gradients, and compositional segregations (e.g., MnS). Currently, there is no system that allows the non-destructive evaluation of the toughness of HFI / ERW welds in air, hydrogen, or hydrogen / natural gas mixtures with other gases.

[0013] The system for evaluating the toughness of longitudinal welds by high-frequency induction or resistance welding in steel tubes and the associated method solve all of the above drawbacks.

[0014] DESCRIPTION OF THE INVENTION

[0015] The present invention relates to a system for evaluating the toughness of longitudinal welds by high frequency induction (HFW, acronym in English for “High Frequency Welding”) or by resistance (ERW, acronym in English for “Electric Resistance Welding”), in steel tubes that provides a systematic and non-destructive evaluation of the toughness of the joint line from the characteristics of the microstructure around the joint line in the outer area of ​​the tube in the area of ​​the longitudinal weld carried out by means of high frequency induction heating or by resistance without performing mechanical tests.

[0016] The system for evaluating the toughness of longitudinal welds by high frequency induction or by resistance in steel tubes comprises: image acquisition means configured to acquire, in use, at least one two-dimensional image of an outer surface of the tube in an analysis region around a joint line (LU) of the longitudinal weld, where the two-dimensional image comprises a first dimension essentially perpendicular to the joint line of the weld and a second dimension essentially parallel to the joint line, and where the three-dimensional image comprises data associated with the microstructure of the tube in the analysis region; processing means configured to provide, from the data associated with the microstructure of the tube in the analysis region, a grayscale profile with respect to the first dimension;and analysis means configured to analyze the grayscale profile and categorize the toughness of the tube in the analysis region around the longitudinal weld joint line.

[0017] In this way, using at least one two-dimensional image, it is possible to obtain the grayscale profile of the different areas of the tube's microstructure around the joint line in the analysis region, where the analysis region preferably corresponds to a thermomechanically affected region (TMAZ). More preferably, the analysis region is a 25x25 mm region.

[0018] Thus, bond line (BL) toughness can be categorized from an image of the tube's outer surface, preferably considering microstructural gradients in the region and, optionally, the hardness of the study area or compositional segregations. The toughness requirement for categorizing a tube as PSL2 is based on the material having a homogeneous microstructure (including crystallographic orientation) around the bond line, and, optionally, on the absence of high-hardness zones or significant compositional segregations (e.g., MnS). Microstructural gradients are generated during the tube manufacturing process, including heat treatments, in this analysis region.

[0019] The microstructure of the material around the joint line for steels that make up tubes that are welded by high-frequency induction or resistance welding is mainly composed of ferrite and pearlite or bainite, although in some grades from X60 onwards it is also possible to find retained austenite and / or martensite. If the welding process or the subsequent heat treatments of quenching, tempering or normalizing have not been carried out correctly, the toughness of the weld is not adequate and this low toughness is reflected in some aspects of the microstructure. The system of the present invention provides a systematic and non-destructive evaluation of the toughness of the joint line from the characteristics of the microstructure around the joint line in the outer area of ​​the tube in the longitudinal weld zone.

[0020] Optionally, the system further comprises means for coupling the image acquisition means to the tube. Preferably, the coupling means comprise a support comprising a lower edge with a curvature essentially equal to the curvature of the tube.

[0021] Optionally, the coupling means comprise anchoring means configured to secure the image acquisition means to the surface of the tube. Preferably, the anchoring means comprise magnetic or electromagnetic anchors.

[0022] Optionally, the system also includes automatic roughing means configured, in use, to remove the outer or inner layers of the tube, preferably paint and rust, down to the metallic material.

[0023] Optionally, the system further comprises sanding means configured, in use, to sand the metallic material of the tube.

[0024] Optionally, the system further comprises polishing means configured, in use, to obtain a mirror-like gloss finish on the tube.

[0025] Optionally, the system also comprises chemical means configured, in use, to chemically attack the tube.

[0026] Optionally, the system further comprises cleaning means configured, in use, to remove the film left on the tube by the chemical means and not leave marks in the analysis region. Optionally, the image acquisition means are digital image acquisition means.

[0027] Optionally, the system further comprises a robotic module configured to move the surface cleaning means and / or the image acquisition means along the tube.

[0028] The invention also relates to a method for evaluating the toughness of longitudinal welds by high frequency induction or by resistance in steel tubes comprising: an image acquisition step where at least one two-dimensional image of an outer surface of the tube is acquired in an analysis region around a joint line (LU) of the longitudinal weld, where the acquisition step is carried out such that the two-dimensional image comprises a first dimension essentially perpendicular to the joint line of the weld and a second dimension essentially parallel to the joint line, and where in the acquisition step data associated with the microstructure of the tube in the analysis region are obtained from the two-dimensional image;a processing step in which a grayscale profile with respect to the first dimension is provided based on data associated with the tube's microstructure in the analysis region; and an analysis step in which the grayscale profile is analyzed and the toughness of the tube in the analysis region around the longitudinal weld seam is categorized.

[0029] Optionally, the method further comprises a step of evaluating the hardness of the area around the joint line (LU) from the grayscale profile obtained.

[0030] Optionally, the method further comprises a tube coupling step prior to the image acquisition step. Optionally, the method further comprises an automatic roughing step where the outer or inner layers of the tube are removed until the metallic material is reached.

[0031] Optionally, the method also comprises a sanding stage where the metal material of the tube is sanded.

[0032] Optionally, the method further comprises a step of polishing the tube to obtain a mirror-like glossy finish of the tube.

[0033] Optionally, the method further comprises a step of chemically etching the tube.

[0034] Optionally, the method also includes a cleaning step where the film left on the tube after the chemical attack step is removed.

[0035] DESCRIPTION OF THE DRAWINGS

[0036] To complement the description being made and in order to help better understand the characteristics of the invention, in accordance with a preferred example of practical implementation thereof, a set of drawings is attached as an integral part of said description, in which the following has been represented for illustrative and non-limiting purposes:

[0037] Figure 1 .- Shows a view of the different regions of the tube around the joint line.

[0038] Figure 2a.- Shows a scanning electron microscopy image of the backscattered electron diffraction type applied to an analysis region around a longitudinal weld joint line (LU) for a low tenacity X60 tube without normalizing treatment.

[0039] Figure 2b.- Shows a scanning electron microscopy image of the backscattered electron diffraction type applied to an analysis region around a longitudinal weld joint line (LU) for an X60 PSL2 pipe in accordance with the API 5L standard.

[0040] Figure 3a.- Shows a perspective view of the image acquisition means arranged in the coupling means of the system for evaluating the toughness of longitudinal welds by high frequency induction or resistance in steel tubes of the present invention.

[0041] Figure 3b.- Shows a perspective view of the image acquisition means arranged in the coupling means of the system located inside the tube for the evaluation of the toughness of longitudinal welds by high frequency induction or by resistance in steel tubes of the present invention.

[0042] Figure 4.- Shows a schematic view of the system for evaluating the toughness of longitudinal welds by high frequency induction or resistance in steel tubes of the present invention.

[0043] Figure 5a.- Shows the microstructural area around the joint line for a first Pattern sample (Pattern 1) without normalizing treatment, with low toughness for the X60 steel tube in Figure 2a.

[0044] Figure 5a.- Shows the microstructural zone around the joint line for a sample with normalized treatment, high toughness AT for the X60 steel tube in Figure 2b.

[0045] Figure 6.- Shows the toughness value (CVN) at the joint line of tubes with different normalized microstructural gradients in the analysis region obtained according to the method of the present invention.

[0046] Figure 7.- Shows the Vickers hardness values, HV10, around the joint line for several high frequency induction heating HFI welds.

[0047] PREFERRED EMBODIMENT OF THE INVENTION The system for evaluating the toughness of longitudinal welds by high frequency induction or by resistance in steel tubes of the present invention will now be described in detail, where the system comprises: image acquisition means (1) configured to acquire, in use, at least one two-dimensional image (2) of an outer surface of the tube (10) in an analysis region (RA) around a joint line (LU) of the longitudinal weld, where the two-dimensional image (2) comprises a first dimension (2x) essentially perpendicular to the joint line of the weld and a second dimension (2y) essentially parallel to the joint line (LU), and where the two-dimensional image (2) comprises data associated with the microstructure of the tube (10) in the analysis region (RA);processing means (3) configured to provide, from the data associated with the microstructure of the tube (10) in the analysis region (RA), a grayscale profile (4) with respect to the first dimension (2x); and analysis means (5) configured to analyze the grayscale profile (4) and categorize the toughness of the tube (10) in the analysis region (RA) around the joint line (LU) of the longitudinal weld.

[0048] Preferably, the system further comprises coupling means (6) of the image acquisition means (5) to the tube (10), where the coupling means (6) comprise a support which in turn comprises a lower edge with a curvature essentially equal to the curvature of the tube.

[0049] EXAMPLE 1

[0050] The method of the present invention comprises, in a first step, preparing the outer surface of the tube. The tubes must be surface prepared according to the protocol described below:

[0051] 1.- Automatic grinding using an abrasive disc to remove the outer layers of paint and rust from the pipe down to the metal. An area of ​​at least 2000 mm must be roughened. 2 The width and height of said area being similar. 2.- Automatic sanding sequence with a sanding disc from coarse to finer grit: 80 - 240 - 320, removing the marks from the previous sanding with each step; and / or

[0052] 3.- Manual sanding sequence with 400, 600, 1200, and 2000 grit sanding discs, alternating the sanding direction between the discs. This sequence eliminates scuff marks and scratches from the previous sequence.

[0053] 4.- Manual polishing with 3 pm diamond paste applied with a polishing cloth, which leaves a shiny mirror-like finish.

[0054] 5.- Etching with an alcoholic nitric acid solution for a period of 15 to 60 seconds, depending on the chemical composition of the tube under study, where the nitric acid concentration is less than or equal to 5%. The process is performed manually using a cotton ball soaked in the acid. During this step, it is essential to avoid contact of the acid with the paint on the tube, so as not to dirty the area under study.

[0055] 6.- Cleaning with ethanol and drying the surface preferably with forced air (dryer) to remove the ethanol film and not leave marks in the area under study.

[0056] Once the surface has been properly prepared according to steps 1 to 6, the image acquisition stage begins using a device developed to be coupled to the outer surface of the tube, shown in Figure 3.

[0057] The images to evaluate the tenacity of the bond line (LU) of HFI / ERW pipes are obtained by means of image acquisition means, preferably a digital camera, coupled to coupling means or a box that is coupled to the outer surface of the pipe, made of mechanically resistant material that is opaque to the bond line (LU) with an opening that allows the camera to be coupled to take the images.

[0058] The images of the joint line (LU) obtained are subsequently evaluated by means of processing means configured to provide, based on the data associated with the microstructure of the tube in the analysis region, a grayscale profile with respect to the first dimension, describing the different microstructural zones around the joint line (LU), including the analysis region (RA) corresponding to the TMAZ. The digital camera allows the adjustment of the different parameters such as joint line (Brightness, focus and ISO) and is configured to acquire a representative image of the area around the joint line (LU) of the weld.

[0059] The image acquisition stage is performed as follows:

[0060] 1.- Delimit the analysis area, preferably 25 x 25 mm, around the joint line (LU) by applying a black mask that adapts to the tube surface and eliminates parasitic reflections. A standard sample or scale must be incorporated to convert the image pixel value to mm, Figure 4.

[0061] 2.- Positioning the image acquisition device. The image acquisition device, with the appropriate coupling to the tube curvature, will be attached to the area of ​​interest.

[0062] 3.- Placement of the standard sample in the tube next to the area of ​​interest. Specifically, a first standard sample (Standard 1) (A) and a second standard sample (Standard 2) (B) will be used as standard samples due to their proven low tenacity at the bond line (LU).

[0063] The use of standard sample(s) is advisable for several reasons: a.- to establish an objective comparison of the slightly different lighting conditions that are sometimes necessary to obtain a good image of the sample under study. b.- to establish a reliable reference for the toughness value of a normalized grayscale profile in image analysis. c.- the influence of the lighting conditions / sample preparation can be normalized by modifying the grayscale of the image using image analysis software and normalized by the average grayscale of the profile.

[0064] 4.- Sample illumination. Adequate illumination of the sample is achieved using a dual longitudinal LED light source at least 10 cm long. This requirement has been proven necessary to adequately contrast the joining line (LU) with the surrounding area. The LED power does not necessarily have to be a fixed value because it must be considered in combination with the camera's exposure time (S), aperture, and ISO parameters when taking the image. That is, using a high lighting power with low S, aperture, and ISO parameters is equivalent to using a low lighting power and high S, aperture, and ISO values.

[0065] A fundamental aspect of the present invention is to acquire a homogeneous image with respect to its lighting; that is:

[0066] - that does not include artifacts or reflections.

[0067] - that it is independent of natural lighting.

[0068] 5. Image acquisition of the area of ​​interest (including the standard). It is advisable to acquire at least three images at different positions along the junction line (LL) to analyze the reproducibility of the result. Image acquisition conditions. Focus and exposure time. Once the sample has been illuminated, the image for analysis must be focused on the junction line (LL). Image analysis must be performed on the images taken of the tubes using the device without modifying the brightness or contrast, and without applying any type of filter or modification to the images.

[0069] 6.- Analysis of the obtained images. A rectangular area centered on the seam line (SL) up to the edge of the TMAZ is taken to perform image analysis, as shown in Figure 4. The rectangular area must be centered on the seam line (SL) and be wide enough to fully encompass the analysis region (AR) on both sides of the seam line (SL). The height of the rectangular area should ideally be 10 mm. This smooths out the grayscale noise and minimizes the effect of seam line misalignment on the results.

[0070] If the height of the selected area were too small, for example, 3 mm, the result would be very noisy. If, on the other hand, it were too large, for example, 20 mm, there would be a high probability that the misalignment around the joint line (LU) would be distorted.

[0071] If the joint line (LL) is not a straight line, the rectangular area should be located so that the upper half of the joint line (LL) is on one side of the rectangular area's axis and the lower half of the joint line (LL) is on the other side. Taking into account all the aspects described above, the analysis region (AR) is usually in the 100-200 grayscale range. Shade 0 corresponds to black, and shade 255 to white.

[0072] The analysis area has been correctly selected if the obtained grayscale profile reveals the peak corresponding to the union line (LU) and the change in hue between the analysis region (RA) and the adjacent material.

[0073] Figures 5a and 5b show the microstructural zones around the bond line (BL) for a sample without normalizing treatment, with low toughness, Pattern 1 (Figure 5a), and another with normalizing treatment, high toughness, BL (Figure 5b). It can be seen how the different heat treatments generate different shades of gray around the bond line (BL).

[0074] The weld joint line (LU) toughness categorization is performed using the microstructural gradients described in gray scale around the joint line (LU), Figures 5a and 5b, with respect to the gray level (GSU, acronym in English for “gray scale units”) corresponding to the joint line (LU) baseline. The basis of the present invention is based on the idea that when the microstructural gradient is greater than a given value, the weld has not been performed correctly and the joint line (LU) behaves as a metallurgical notch that greatly decreases the joint line (LU) toughness. To characterize the metallurgical notch effect, Charpy tests were performed on samples with different processing processes and the CVN values ​​were correlated with the microstructural gradient in the analysis region (AR) area.This microstructural gradient value, which is identified with the presence of metallurgical notch, has been set at 0.05 based on the results obtained and described in Figure 6. Figure 6 shows the toughness value (CVN) at the joint line (LU) of tubes with different microstructural gradients in the analysis region (RA).

[0075] Bond line (BL) toughness is assessed using a scoring system shown in Figure 6 based on the normalized gradient value in the analysis region (AR). A pipe is considered to have low toughness if its T value is greater than 0.05, where: 0.05 where GSUo is the gray tone of the base of the peak corresponding to the union line (LU) and GSU(RA) is the arithmetic difference between the largest and smallest gray tone in the analysis region (RA).

[0076] EXAMPLE 2

[0077] The method of the present invention comprises, in a first step, preparing the inner surface of the tube. The tubes must be surface prepared according to the protocol described below:

[0078] 1. Laser cleaning using a device developed to be coupled to a robotic movement system to remove layers of paint and rust from the pipe down to the metal. An area of ​​at least 2000 mm must be cleaned. 2 the width and height of said area being similar.

[0079] 2.- Attack with an alcoholic nitric acid solution using a device designed to be coupled to a robotic system, for a period of between 15 and 60 seconds, depending on the chemical composition of the tube under study, where the nitric acid concentration is less than or equal to 5%. In this step, it is essential to avoid contact of the acid with the paint on the tube, so as not to contaminate the area under study.

[0080] 3.- Cleaning with ethanol and drying the surface, preferably with forced air (a hairdryer) to remove the ethanol film and avoid leaving marks on the study area. Once the surface has been properly prepared according to steps 1 through 3, the image acquisition stage begins using a device developed to be coupled to the robotic system described above, which moves it inside the tube to analyze its interior surface, as shown in Figure 3b.

[0081] The images for evaluating the toughness of the joint line (LL) of HFI / ERW pipes are obtained using image acquisition means, preferably a digital camera, coupled to coupling means mounted on the robotic system. The obtained images of the joint line (LL) are subsequently evaluated using processing means configured as described in Example 1. The digital camera allows adjustment of the various parameters such as the joint line (brightness, focus, and ISO) and is configured to acquire a representative image of the area around the joint line (LL) of the weld. The image acquisition stage is performed as follows:

[0082] 1 Delimitation of the analysis area, preferably 25 x 25 mm 2 around the joining line (LU) by applying a black mask that adapts to the tube surface and eliminates parasitic reflections.

[0083] 2.- Positioning the image acquisition device by moving the robotic system. The image acquisition device mounted on the robotic system will be docked in the area of ​​interest.

[0084] 3.- Placement of the standard sample in the tube next to the area of ​​interest using the robotic system. Specifically, a first standard sample (Standard 1) (A) and a second standard sample (Standard 2) (B) will be used as standard samples due to their proven low tenacity at the bond line (LU). The use of standard sample(s) is convenient for the reasons described in example 1:

[0085] 4.- Illumination of the sample in an identical manner to that described in example 1.

[0086] 5.- Image acquisition of the area of ​​interest (including the Pattern) in the manner described in example 1.

[0087] 6.- Analysis of the images obtained following the procedure described in example 1.

[0088] The categorization of the weld joint line (LU) toughness is performed in the same manner and with the same equation as described in Example 1.

[0089] EXAMPLE S

[0090] The method of the present invention comprises, in a first step, preparing the inner surface of the tube. The tubes must be surface-prepared according to the protocol described below:

[0091] 1.- Automatic grinding using an abrasive disc to remove the outer layers of paint and rust from the pipe down to the metal. An area of ​​at least 2000 mm must be roughened. 2 the width and height of said area being similar.

[0092] 2.- Automatic sanding sequence with a sanding disc, from coarse to fine grit: 80-240-320, removing the marks from the previous sanding with each step; and / or it is not always necessary to use all the sandpaper.

[0093] 3.- Manual sanding sequence with 400, 600, 1200, and 2000 grit sanding discs, alternating the sanding direction between the discs. This sequence eliminates scuff marks and scratches from the previous sequence.

[0094] 4.- Manual polishing with 3 pm diamond paste applied with a polishing cloth, which leaves a shiny mirror-like finish.

[0095] 5.- Attack with an alcoholic solution of nitric acid with a concentration of less than or equal to 5%, for a period of 30 seconds, followed by cleaning with alcohol and drying.

[0096] 6.- Image acquisition using a device developed to attach to the outer surface of the tube, shown in Figure 3.

[0097] 7.- Attack with an alcoholic solution of nitric acid with a concentration of less than or equal to 5%, for a period of 15 seconds, followed by cleaning with alcohol and drying.

[0098] 8.- Image acquisition using a device developed to be coupled to the outer surface of the tube, shown in Figure 3a.

[0099] 9.- Attack with an alcoholic solution of nitric acid with a concentration of less than or equal to 5%, for a period of 15 seconds, followed by cleaning with alcohol and drying.

[0100] Images for assessing the bond line (BL) toughness of HFI / ERW pipes are obtained using the image acquisition means described in Figure 3a. The image acquisition step is performed as described in Example 2.

[0101] The categorization of the joint line (LU) toughness of welding in a gas atmosphere that embrittles the steel is carried out by combining: i) the calculation of the microstructural gradients described in gray scale around the joint line (LU), figures 5a and 5b, with respect to the gray level (GSU) corresponding to the joint line (LU) baseline. This microstructural gradient value, which is identified with the presence of metallurgical notch, has been set at 0.05 from the results obtained and described in figure 6 and the equation described in example 1 .

[0102] i) Calculation of the bond line hardness (LU). The bond line hardness (LU) is determined from the profiles obtained from the analysis of the images obtained. The bond line hardness (LU) is considered to be proportional to that of the starting material, X42, X52, etc., the grain size and the phases present in the area of ​​interest: polygonal ferrite, acicular ferrite, pearlite, bainite, retained austenite, martensite, etc. The maximum recommended hardness to avoid hydrogen embrittlement in gas pipeline steels is considered to be 275 HV.

[0103] Using imaging techniques, we can determine variations in hardness relative to the corresponding bond line (BL) in the grayscale profiles of the central peak. The harder the grain (finer the grain and finer the pearlite / bainite / martensite), the faster the attack with nital.

[0104] The procedure consists of etching the bond line (BL) with nital for several times, followed by cleaning with alcohol and drying, and then acquiring an image after each etching, cleaning, and drying process. An image of the area of ​​interest is acquired, and a descriptive profile for that area is calculated. The process is repeated with a longer etching time, for example, an additional 30 seconds, followed by cleaning and drying, and images are acquired again to calculate the corresponding profile. The process is repeated a third time (without prejudice to repeating the process as many times as deemed necessary) with a longer etching time, for example, an additional 30 seconds, and an image is acquired again to calculate the corresponding profile. In this case, the total etching time with nital would be 90 seconds. The gray tone difference between the three profiles is then calculated for the etching times of 30, 60, and 90 seconds.GSU gray tone values ​​decrease with etching time depending on the microstructure around the bond line (LU).

[0105] Hardness determination begins by assigning an HV value to the base material, which can be obtained from the yield strength requirement of the base material according to standards. The following hardness values ​​are considered for the base material: 160HV for X42, 170HV for Grade B, and 190HV for X60.

[0106] The hardness value around the LU increases relative to the base material if the microstructure is fine-grained with a pearlitic / bainitic structure. This type of microstructure is evident in a grayscale profile in which the bond line (LU) (central peak of the profile) is quickly revealed (< 30 s), and this profile is maintained for consecutive attacks up to long attack times, for example 90 seconds. However, if the microstructure around the bond line (LU) is coarse-grained pearlitic, a decrease in hardness occurs. In this coarse microstructure, it is typical that there is no decrease in grayscale shades (GSU) until high attack times. There is a relationship between hardness and GSU. In Grade B and X42 materials, the ratio is inversely proportional to 1 HV:3 GSU. In X60 material, the ratio is 1 HV:1 GSU. The decrease in hardness is inversely proportional to the decrease in GSU shade.

[0107] Below are the hardness predictions made according to the method described for the curves summarized in Figure 7.

[0108] T1 : When attacking with nital, there is a progressive drop of 18 GSU until 30s indicating that the microstructure is medium (neither fine nor coarse). There is an equivalence of 1 HV:3 GSU in X42 materials such as T1 , therefore the hardness must increase 6HV around the union line (LU) from 160HV to 166HV. T2: When attacking with nital, there is a progressive drop of 17 GSU until 45s indicating a fine grain and a coarse pearlitic structure. There is an equivalence of 1 HV:3 GSU, therefore the hardness must increase 5HV around the union line (LU) from 160 to 165HV.

[0109] T3: When attacking with nital, there is no decrease in GSU until 45s, when it drops by 13GSU. There is a 1 HV:1 GSU equivalence in X60 materials, therefore, the hardness should decrease by 13HV around the LU from 190 to 177HV.

[0110] T4: Decrease of 20GSU in 15s in the nital attack to maintain the same profile until 45s. There is a 1 HV:1 GSU equivalence in X60 materials, therefore, the hardness must increase by 20HV around the LU from 190 to 210HV.

[0111] T5: The weld is slightly asymmetrical. When etched with nital, there is a 15 GSU drop on the sides of the LU from 220GSU in just 15s, which remains the same for 45s. There is a GSU to HV equivalence of 1 HV:3GSU typical of X42 / Grade B materials such as T5, therefore, the hardness should increase by 5HV around the joint line (LU) from 170 to 175HV.

[0112] T6: The weld is asymmetrical. When etched with nital, a 5 GSU drop occurs on the sides of the joint line (LU) in just 15 s, which remains constant for up to 45 s. There is an equivalence of 1 HV:3 GSU in materials like T6. The hardness must increase by 1-2 HV around the LU from 170 to 172 HV.

Claims

1. System for evaluating the toughness of longitudinal welds by high frequency induction or resistance in steel tubes, comprising: image acquisition means (1 ) configured to acquire, in use, at least one two-dimensional image (2) of an outer surface of the tube (10) in an analysis region (RA) around a joint line (LU) of the longitudinal weld, where the two-dimensional image (2) comprises a first dimension (2x) essentially perpendicular to the joint line of the weld and a second dimension (2y) essentially parallel to the joint line (LU), and where the two-dimensional image (2) comprises data associated with the microstructure of the tube (10) in the analysis region (RA); processing means (3) configured to provide, from the data associated with the microstructure of the tube (10) in the analysis region (RA), a grayscale profile (4) with respect to the first dimension (2x);and analysis means (5) configured to analyze the grayscale profile (4) and categorize the toughness of the tube (10) in the analysis region (RA) around the joint line (LU) of the longitudinal weld.; 2. System according to claim 1, wherein the analysis region preferably corresponds to a thermo-mechanically affected region (TMAZ).

3. System according to any of the preceding claims, further comprising coupling means (6) of the image acquisition means (5) to the tube (10), where the coupling means (6) comprise a support which in turn comprises a lower edge with a curvature essentially equal to the curvature of the tube (10).

4. System according to claim 3, wherein the coupling means (6) comprise anchoring means configured to fix the image acquisition means to the surface of the tube, preferably magnetic or electromagnetic anchors.

5. System according to any of the preceding claims, further comprising automatic roughing means configured, in use, to remove the outer or inner layers of the tube until reaching the metallic material.

6. System according to claim 5, further comprising sanding means configured, in use, to sand the metallic material of the tube.

7. System according to claim 6, further comprising polishing means configured, in use, to obtain a mirror-like gloss finish on the tube.

8. System according to claim 7, further comprising chemical means configured, in use, to chemically attack the tube.

9. System according to claim 7, further comprising cleaning means configured, in use, to remove the film left on the tube by the chemical means and not leave marks in the analysis region.

10. System according to claim 9, the system further comprising a robotic module configured to move the surface cleaning means and / or the image acquisition means (1) along the tube.

11. Method for evaluating the toughness of longitudinal welds by high frequency induction or resistance in steel tubes, comprising: an image acquisition step where at least one two-dimensional image of an outer surface of the tube is acquired in an analysis region around a joint line (LU) of the longitudinal weld, where the acquisition step is carried out such that the two-dimensional image comprises a first dimension essentially perpendicular to the joint line of the weld and a second dimension essentially parallel to the joint line, and where in the acquisition step data associated with the microstructure of the tube in the analysis region are obtained from the two-dimensional image; a processing step where a grayscale profile with respect to the first dimension is provided based on data associated with the tube's microstructure in the analysis region; and an analysis step where the grayscale profile is analyzed and the toughness of the tube in the analysis region around the longitudinal weld seam is categorized.

12. Method according to claim 11, further comprising a stage of coupling to the tube prior to the stage of image acquisition.

13. Method according to any of claims 11 or 12, further comprising an automatic roughing step where the outer or inner layers of the tube are removed until the metallic material is reached.

14. Method according to claim 13, where in the automatic roughing stage an abrasive disc is used to remove the outer layers of the tube until reaching the metallic material, devastating an area of ​​at least 2000 mm.2 .

15. Method according to any of claims 13 or 14, further comprising a sanding step where sanding of the metal material of the tube is carried out.

16. Method according to claim 15, wherein the sanding step comprises a first automatic sanding sequence with a sanding disc from coarse to finer grit: 80 - 240 - 320, eliminating the marks of the previous sanding in each step, and / or a manual sanding sequence with a sanding disc with grit of 400, 600, 1200 and 2000, alternating the sanding direction between sandpapers.

17. Method according to any of claims 15 or 16, further comprising a step of polishing the tube to obtain a mirror-like glossy finish on the tube.

18. Method according to claim 17, wherein the polishing step is a manual polishing step with 3 pm diamond paste applied with a polishing cloth.

19. Method according to any of claims 17 or 18, further comprising a step of chemically etching the tube.

20. Method according to claim 19, where the chemical attack step of the tube is carried out with an alcoholic solution of nitric acid, for a period of time between 15 and 60 seconds, where the nitric acid is at a concentration less than or equal to 5%.

21. Method according to claim 19, wherein the chemical attack step of the tube is carried out with an alcoholic solution of nitric acid, for a period of time of 15 seconds and a first image is acquired, then another period of 30 seconds and a second image is acquired and finally another period of 45 seconds, where the nitric acid is at a concentration less than or equal to 5%.

22. Method according to claim 21, wherein the hardness around the bond line (LU) is determined by the equivalence between GSU and HV from the evolution of the grey profiles for the different attack times.

23. Method according to any of claims 19 or 20, further comprising a cleaning step where the film left on the tube after the chemical attack step is removed.

Citation Information

Patent Citations

  • Welded joint metal streamline angle automatic measurement method of high-frequency welded pipe

    CN110514148A

  • Multi-section pipeline welding seam detection robot

    CN218657472U

  • Method and device for evaluation of jointing regions on workpieces

    US20050041852A1

  • Pipe outer surface inspection apparatus

    US20160320266A1