Cutting tool

The cutting tool with a specific coating structure and deposition method addresses the challenge of maintaining tool life during high-temperature machining by providing enhanced wear and oxidation resistance, improving machining efficiency and sustainability.

WO2024236769A1PCT designated stage expired Publication Date: 2024-11-21SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/018430
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional cutting tools face challenges in maintaining tool life during high-speed, high-efficiency machining of difficult-to-cut materials like heat-resistant alloys and titanium, where cutting edge temperatures rise, leading to reduced tool longevity and increased environmental impact due to the need for cooling fluids.

Method used

A cutting tool with a coating comprising alternating layers of W(C1−αNα)x and AlcCr1−cN, where 0.3 ≤ a ≤ 0.8 and 0.40 ≤ c ≤ 0.80, and optionally additional layers, providing improved heat resistance, wear resistance, and oxidation resistance, which are deposited using physical vapor deposition methods to enhance adhesion and durability.

Benefits of technology

The cutting tool exhibits extended tool life and improved wear resistance, oxidation resistance, and thermal insulation properties, even under high cutting edge temperatures, while reducing the need for cooling fluids, thus enhancing machining efficiency and sustainability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023018430_21112024_PF_FP_ABST
    Figure JP2023018430_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A cutting tool comprising a substrate and a coating that is disposed upon the substrate, wherein: the coating includes a first layer; the first layer is formed from alternating layers consisting of first unit layers and second unit layers stacked in an alternating manner; each first unit layer has a hexagonal crystal structure; each first unit layer is composed of W(C1-aNa)x; a is 0.3 to 0.8 inclusive; x is 0.8 to 1.2 inclusive; each second unit layer is composed of AlcCr1-cN; and c is 0.40 to 0.80 inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

cutting tools

[0001] The present disclosure relates to cutting tools.

[0002] Conventionally, cutting tools including a substrate and a coating disposed on the substrate have been used in cutting processes (Patent Documents 1 and 2).

[0003] JP 2022-143690 A International Publication No. 2022 / 176230

[0004] A cutting tool according to one aspect of the present disclosure is a cutting tool including a substrate and a coating disposed on the substrate, wherein the coating includes a first layer, the first layer being composed of alternating layers in which first unit layers and second unit layers are alternately stacked, the first unit layer having a hexagonal crystal structure, and the first unit layer being composed of W(C 1-a N a ) x wherein a is 0.3 or more and 0.8 or less, x is 0.8 or more and 1.2 or less, and the second unit layer is Al c Cr 1-c N, and the c is 0.40 or more and 0.80 or less.

[0005] FIG. 1 is a schematic enlarged cross-sectional view of an example of a cutting tool according to the first embodiment. FIG. 2 is a schematic enlarged cross-sectional view of another example of the cutting tool according to the first embodiment. FIG. 3 is a schematic enlarged cross-sectional view of another example of the cutting tool according to the first embodiment. FIG. 4 is a schematic enlarged cross-sectional view of another example of the cutting tool according to the first embodiment. FIG. 5 is a diagram for explaining an example of a thickness ratio between a first unit layer and a second unit layer. FIG. 6 is a schematic enlarged cross-sectional view of an example of a cutting tool according to the second embodiment. FIG. 7 is a schematic enlarged cross-sectional view of another example of the cutting tool according to the second embodiment. FIG. 8 is a schematic enlarged cross-sectional view of another example of the cutting tool according to the second embodiment. FIG. 9 is a schematic enlarged cross-sectional view of another example of the cutting tool according to the second embodiment. FIG. 10 is a diagram for explaining an example of a thickness ratio between a first unit layer and a third unit layer. FIG. 11 is a schematic cross-sectional view of a cathodic arc ion plating apparatus used in the examples. FIG. 12 is a schematic top view of the cathodic arc ion plating apparatus shown in FIG. 11.

[0006] [Problem to be Solved by the Present Disclosure] Cutting plays a central role in manufacturing technology, and technological evolution and further advancement are constantly being demanded. Cutting technology fundamentally requires high speed, high efficiency, high precision, and ultrafine machining. Recent trends include increasingly difficult-to-cut workpiece materials, and efforts to address this need are also needed. In addition, in cutting fields, attention has been increasingly focused on the Sustainable Development Goals (SDGs) in recent years to realize a sustainable and better world by 2030. Sustainable development means building a social infrastructure that can withstand natural threats without compromising the resources needed by future generations. Improvements in cutting technology are expected to reduce the environmental impact by reducing the number of processes, thereby saving energy during product manufacturing and reducing waste associated with cutting processes. Against this background, the development of coated tool materials that combine high high-temperature hardness and toughness has been pursued to extend the tool life of cutting tools.

[0007] Conventionally, coating tool materials have been coated on substrate surfaces with nitride or boronitride coatings primarily composed of aluminum and chromium (see Patent Documents 1 and 2). However, due to factors such as the need for dry machining without cutting fluids in light of the SDGs and global environmental conservation, increased cutting speeds to improve machining efficiency, and the diversification of workpiece materials, particularly in the aircraft and medical fields, where cutting of heat-resistant alloys and titanium alloys, which are considered difficult to cut, is becoming increasingly common, the cutting edge temperature of cutting tools tends to become high during cutting. High cutting edge temperatures significantly shorten the life of cutting tools. Therefore, there is a need for cutting tools that can maintain excellent tool life even under such harsh cutting conditions.

[0008] Effect of the Present Disclosure According to the present disclosure, it is possible to provide a cutting tool that has a long tool life, especially in cutting operations that are performed under conditions where the cutting edge temperature is high.

[0009] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described. (1) A cutting tool according to one aspect of the present disclosure is a cutting tool including a substrate and a coating disposed on the substrate, wherein the coating includes a first layer, the first layer being composed of alternating layers in which first unit layers and second unit layers are alternately stacked, the first unit layer having a hexagonal crystal structure, and the first unit layer being composed of W(C 1-a N a ) x wherein a is 0.3 or more and 0.8 or less, x is 0.8 or more and 1.2 or less, and the second unit layer is Al c Cr 1-c N, and the c is 0.40 or more and 0.80 or less.

[0010] According to the present disclosure, it is possible to provide a cutting tool that has a long tool life, especially in cutting operations that are performed under conditions where the cutting edge temperature is high.

[0011] (2) In the above (1), the ratio λ2 / λ1 of the thickness λ2 μm of the second unit layer to the thickness λ1 μm of the first unit layer may be 1.0 or more and 5.0 or less, between the first unit layer and the second unit layer adjacent to the first unit layer. This allows the cutting tool to have a longer tool life.

[0012] (3) In the above (1) or (2), the average thickness of the first unit layer may be 0.002 μm or more and 0.2 μm or less, and the average thickness of the second unit layer may be 0.002 μm or more and 0.2 μm or less. This allows the cutting tool to have a longer tool life.

[0013] (4) In any one of the above (1) to (3), the coating may further include a second layer disposed between the substrate and the first layer, and the composition of the second layer may be the same as the composition of the first unit layer or the composition of the second unit layer. This allows the cutting tool to have a longer tool life.

[0014] (5) In the above (4), the second layer may have the same composition as the first unit layer, and the second layer may have a thickness greater than that of the first unit layer. This allows the cutting tool to have a longer tool life.

[0015] (6) In the above (4), the second layer may have the same composition as the second unit layer, and the second layer may have a thickness greater than the thickness of the second unit layer. This allows the cutting tool to have a longer tool life.

[0016] (7) In the above (1) to (6), the coating may further include a third layer provided on the opposite side of the first layer from the substrate, and the third layer may be made of AlCrCN. This allows the cutting tool to have a longer tool life.

[0017] (8) A cutting tool according to another aspect of the present disclosure is a cutting tool including a substrate and a coating disposed on the substrate, wherein the coating includes a first A layer, the first A layer being composed of alternating layers in which first unit layers and third unit layers are alternately stacked, the first unit layer having a hexagonal crystal structure, and the first unit layer being composed of W(C 1-a N a ) x wherein a is 0.3 or more and 0.8 or less, x is 0.8 or more and 1.2 or less, and the third unit layer is Al d Cr 1-d-e M e N, wherein M is silicon, boron, yttrium, cerium, or lanthanum, d is 0.40 or more and 0.80 or less, and e is more than 0 and 0.05 or less.

[0018] According to the present disclosure, it is possible to provide a cutting tool that has a long tool life, especially in cutting operations that are performed under conditions where the cutting edge temperature is high.

[0019] (9) In the above (8), the ratio λ3 / λ1 of the thickness λ3 μm of the third unit layer to the thickness λ1 μm of the first unit layer may be 1.0 or more and 5.0 or less, between the first unit layer and the third unit layer adjacent to the first unit layer. This allows the cutting tool to have a longer tool life.

[0020] (10) In the above (8) or (9), the M may be silicon, which allows the cutting tool to have a longer tool life.

[0021] (11) In the above (8) or (9), the M may be boron. This allows the cutting tool to have a longer tool life.

[0022] (12) In any one of the above (8) to (11), the average thickness of the first unit layer may be 0.002 μm or more and 0.2 μm or less, and the average thickness of the third unit layer may be 0.002 μm or more and 0.2 μm or less. This allows the cutting tool to have a longer tool life.

[0023] (13) In any one of the above (8) to (12), the coating may further include a second A layer disposed between the substrate and the first A layer, and the composition of the second A layer may be the same as the composition of the first unit layer or the composition of the third unit layer. This allows the cutting tool to have a longer tool life.

[0024] (14) In the above (13), the second A layer may have the same composition as the first unit layer, and the second A layer may have a thickness greater than that of the first unit layer. This allows the cutting tool to have a longer tool life.

[0025] (15) In the above (13), the second A layer may have the same composition as the third unit layer, and the second A layer may have a thickness greater than that of the third unit layer. This allows the cutting tool to have a longer tool life.

[0026] (16) In any one of the above (8) to (15), the coating further includes a third A layer provided on the side of the first A layer opposite to the substrate, the third A layer being made of AlCrMeCN, and the Me may be silicon, boron, yttrium, cerium, or lanthanum. This allows the cutting tool to have a longer tool life.

[0027] [Details of the Embodiments of the Present Disclosure] Specific examples of cutting tools according to the present disclosure will be described below with reference to the drawings. In the drawings of the present disclosure, the same reference numerals represent the same or corresponding parts. Furthermore, dimensional relationships such as length, width, thickness, and depth have been appropriately changed for clarity and simplification of the drawings, and do not necessarily represent actual dimensional relationships.

[0028] In the present disclosure, the notation in the form of "A to B" means the upper and lower limits of a range (i.e., A or more and B or less), and when no unit is specified for A and a unit is specified only for B, the units of A and B are the same.

[0029] In the present disclosure, when a compound or the like is represented by a chemical formula, unless the atomic ratio is particularly limited, it is intended to include any conventionally known atomic ratio, and should not necessarily be limited to only those within the stoichiometric range.

[0030] In the present disclosure, when one or more numerical values ​​are recited as the lower limit and the upper limit of a numerical range, a combination of any one numerical value recited as the lower limit and any one numerical value recited as the upper limit is also considered to be disclosed. For example, when a1 or more, b1 or more, and c1 or more are recited as the lower limit and a2 or less, b2 or less, and c2 or less are recited as the upper limit, a1 or more and a2 or less, a1 or more and b2 or less, a1 or more and c2 or less, b1 or more and a2 or less, b1 or more and b2 or less, b1 or more and c2 or less, c1 or more and a2 or less, c1 or more and b2 or less, and c1 or more and c2 or less are considered to be disclosed.

[0031] [Embodiment 1: Cutting Tool (1)] A cutting tool according to one embodiment of the present disclosure will be described with reference to Figures 1 to 5. A cutting tool 1 according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 1") is a cutting tool including a substrate 2 and a coating 3 disposed on the substrate 2, wherein the coating 3 includes a first layer 13, the first layer 13 being composed of alternating layers in which first unit layers 12 and second unit layers 15 are alternately stacked, the first unit layer 12 having a hexagonal crystal structure, and the first unit layer 12 being composed of W(C 1-a N a ) x a is 0.3 or more and 0.8 or less, x is 0.8 or more and 1.2 or less, and the second unit layer 15 is Al c Cr 1-c N, and c is 0.40 or more and 0.80 or less.

[0032] The cutting tool 1 of the first embodiment can have a long tool life, especially in cutting operations performed under conditions where the cutting edge temperature is high. The reason for this is presumed to be as follows.

[0033] The first unit layer 12 is W(C 1-a N a ) x Since the first unit layer 12 contains C (carbon), the coefficient of friction at the contact interface with the workpiece material is reduced, and cutting resistance can be reduced. 1-a N a ) x Since it contains N (nitrogen), its heat resistance is improved by about 150°C compared to WC. As a result, the first layer including the first unit layer can improve adhesion resistance, sliding properties, and wear resistance in processes where the cutting edge becomes hot, such as dry cutting processes. Therefore, the tool life of a cutting tool including the first layer is improved.

[0034] The second unit layer 15 is made of Al c Cr 1-c The second unit layer 15 contains Al. Since Al is easily oxidized, the coating containing the second unit layer 12 has Al on the surface side of the first layer 13. 2 O 3As a result, the heat insulating property and oxidation resistance of the first layer 13 can be improved. Therefore, the tool life of a cutting tool including the first layer 13 is improved.

[0035] The first layer 13 is composed of alternating layers in which first unit layers 12 and second unit layers 15 are alternately stacked. The composition and crystal lattice are discontinuous at the interface between the first unit layers 12 and the second unit layers 15. Therefore, if a crack occurs from the surface of the coating 3 during cutting, the propagation of the crack can be suppressed at the interface. A coating including the first layer suppresses chipping and fracture. Therefore, a cutting tool including the first layer 13 has an improved tool life.

[0036] 1 and 2, a cutting tool 1 according to one embodiment of the present invention includes a substrate 2 and a coating 3 disposed on the substrate 2. The coating 3 can cover at least a portion of the substrate 2 that is involved in cutting. The coating 3 may also cover the entire surface of the substrate 2. Partially different configurations of the coating 3 do not depart from the scope of this embodiment. In this specification, the portion of the substrate 2 that is involved in cutting refers to a region on the surface of the substrate 2 that is at least 50 μm, 100 μm, or 300 μm away from the cutting edge.

[0037] The cutting tool 1 of this embodiment can be suitably used as cutting tools 1 such as drills, end mills, indexable cutting tips for drills, indexable cutting tips for end mills, indexable cutting tips for milling, indexable cutting tips for turning, metal saws, gear cutting tools, reamers, and taps.

[0038] <Substrate> Any conventionally known material can be used as the substrate 2. For example, the substrate 2 may be made of any one of cemented carbide (WC-based cemented carbide, cemented carbide containing WC and Co, cemented carbide formed by adding carbonitrides of Ti, Ta, Nb, etc. to WC and Co), cermet (mainly composed of TiC, TiN, TiCN, etc.), high-speed steel, ceramics (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide, etc.), cubic boron nitride sintered body, and diamond sintered body.

[0039] The substrate 2 may be, in particular, a WC-based cemented carbide or a cermet (particularly, a TiCN-based cermet). The WC-based cemented carbide or cermet has an excellent balance between hardness and strength, particularly at high temperatures, and therefore, when used as the substrate 2 of the cutting tool 1, it can contribute to extending the life of the cutting tool 1.

[0040] <Coating> The coating 3 of the first embodiment includes a first layer 13. By covering the substrate 2, the coating 3 has the effect of improving various properties of the cutting tool 1, such as wear resistance and chipping resistance, and thereby extending the life of the cutting tool 1.

[0041] The coating 3 may include other layers in addition to the first layer 13. As shown in Figures 3 and 4, the other layers include a second layer 16 disposed between the substrate 2 and the first layer 13, and a third layer 14 provided on the side of the first layer 13 opposite the substrate 2.

[0042] The coating 3 may have an overall thickness of 0.4 μm or more and 15 μm or less. When the overall thickness of the coating 3 is 0.4 μm or more, the effect of providing the coating 3 to extend the life of the cutting tool 1 is easily achieved. On the other hand, when the overall thickness of the coating 3 is 15 μm or less, chipping of the coating 3 is less likely to occur in the early stages of cutting, and the life of the cutting tool 1 can be extended.

[0043] The total thickness of the coating 3 can be measured by observing the cross section of the coating 3 using a scanning electron microscope (SEM). The specific measurement method is as follows: The cutting tool 1 is cut in a direction along the normal to the surface of the coating 3 to prepare a cross section sample. The cross section sample is observed with the SEM. The observation magnification is 5000 to 10000 times, and the measurement field of view is 100 to 500 μm. 2 The thickness width of the coating 3 is measured at three points in one field of view, and the average value of the thickness widths at the three points is calculated. This average value corresponds to the thickness of the coating 3. The thickness of each layer described below is also measured in the same manner unless otherwise specified.

[0044] The compressive residual stress of the coating 3 may have an absolute value of 6 GPa or less. The compressive residual stress of the coating 3 is a type of internal stress (intrinsic strain) present throughout the coating 3, and is a stress expressed as a negative (-) numerical value (unit: GPa is used in this embodiment). Therefore, the concept of a large compressive residual stress refers to a large absolute value of the numerical value, and the concept of a small compressive residual stress refers to a small absolute value of the numerical value. In other words, an absolute value of the compressive residual stress of 6 GPa or less means that the compressive residual stress of the coating 3 is between -6 GPa and 0 GPa.

[0045] When the compressive residual stress of the coating 3 is 0 GPa or less, it is easy to suppress the propagation of cracks that initiate from the outermost surface of the coating 3. On the other hand, when the absolute value of the compressive residual stress is 6 GPa or less, the magnitude of the stress is appropriate, and it is easy to suppress peeling of the coating 3 from the edge portion of the cutting tool 1 before cutting begins.

[0046] The compressive residual stress of the coating 3 was measured using an X-ray residual stress analyzer. 2 It is measured by the ψ method (see pages 54-66 of "X-Ray Stress Measurement Method" (Japan Society of Materials Science, published by Yokendo Co., Ltd. in 1981)).

[0047] The first unit layer 12 can have a hexagonal crystal structure. When the first unit layer 12 has a hexagonal crystal structure, the abrasion resistance of the coating 3 is improved. The second unit layer 15 can include a cubic crystal structure. When the second unit layer 15 has a cubic crystal structure, the hardness of the coating 3 is improved. The crystal structure of each layer in the coating 3 can be analyzed using an X-ray diffraction device known in the art.

[0048] The hardness of the coating 3 is highly effective when it is 30 GPa or more and 55 GPa or less, and may be 35 GPa or more and 50 GPa or less. According to this, the coating 3 has sufficient hardness. The hardness of the entire coating 3 is measured by a nanoindenter method (Nano Indenter XP manufactured by MTS). Specifically, this is performed using a method in accordance with ISO 14577, with a measurement load of 10 mN (1 gf), and the hardness is measured at three locations on the surface of the coating 3, and the average value of the hardness values ​​at the three locations is calculated. This average value corresponds to the hardness of the coating 3.

[0049] <First Layer> The first layer 13 of this embodiment is composed of alternating layers in which first unit layers 12 and second unit layers 15 are alternately stacked. The fact that the first layer 13 is composed of alternating layers in which the first unit layers 12 and the second unit layers 15 are alternately stacked can be confirmed by observing a thin section sample including a cross section of the coating 3 with a TEM (transmission electron microscope) and observing the difference in contrast.

[0050] Either the first unit layer 12 or the second unit layer 15 may be disposed closest to the substrate 2. In FIG. 1 , the first unit layer 12 is disposed directly on the substrate 2. In FIG. 2 , the second unit layer 15 is disposed directly on the substrate 2. Either the first unit layer 12 or the second unit layer 15 may be disposed on the surface side of the coating 3. In FIG. 1 , the second unit layer 15 is disposed on the surface side of the coating 3. In FIG. 2 , the first unit layer 12 is disposed on the surface side of the coating 3.

[0051] The thickness of the first layer 13 may be 0.5 μm or more and 15 μm or less. When the thickness of the first layer 13 is 0.5 μm or more, excellent wear resistance can be exhibited in continuous cutting. When the thickness of the first layer 13 is 15 μm or less, excellent chipping resistance can be exhibited in interrupted cutting.

[0052] The thickness of the first layer 13 is measured by observing and measuring the cross section of the coating 3 using a transmission electron microscope (TEM). The specific measurement method is as follows: The cutting tool 1 is cut in a direction along the normal to the surface of the coating 3 to prepare a thin section sample including the cross section of the coating 3. The thin section sample is observed with the TEM. The observation magnification is set to 20,000 to 5,000,000 times, and the measurement field of view is set to 0.0016 to 80 μm. 2 The thickness width of the first layer 13 is measured at three locations in one field of view, and the average value of the thickness widths at the three locations is calculated. The average value corresponds to the thickness of the first layer 13.

[0053] The first unit layer 12 may have a hexagonal crystal structure. The hexagonal crystal structure is formed by the W(C 1-a N a ) x The fact that the first unit layer 12 has a hexagonal crystal structure can be confirmed by analyzing it with an XRD measurement. In the obtained XRD spectrum, the ε-W 2 C (01-076-7103) and W 4.6 N 4 When a peak attributed to the hexagonal crystal structure defined in (01-077-2001) is observed, it is confirmed that the first unit layer 12 has a hexagonal crystal structure.

[0054] Even when the coating includes, in addition to the first unit layer, other layers such as the second unit layer 15, the second layer 16, the third layer 14, and an intermediate layer, and peaks originating from layers other than the first unit layer 12 or from the substrate (hereinafter also referred to as "other peaks") are detected in the XRD spectrum from the surface of the coating 3, it is possible to identify that the first unit layer 12 has a hexagonal crystal structure.

[0055] An example of an apparatus used for X-ray diffraction measurement is the "SmartLab" (trade name) manufactured by Rigaku Corporation. The conditions for XRD measurement are as follows: (XRD measurement conditions) Scanning axis: 2θ-θ X-ray source: Cu-Kα ray (1.541862 Å) Detector: 0-dimensional detector (scintillation counter) Tube voltage: 45 kV Tube current: 40 mA Incident optical system: Use of a mirror Receiving optical system: Use of an analyzer crystal (PW3098 / 27) Step: 0.03° Integration time: 2 seconds Scan range (2θ): 10° to 120°

[0056] <Composition of First Unit Layer and Composition of Second Unit Layer> The first unit layer 12 is made of W(C 1-a N a ) x where a is 0.3 or more and 0.8 or less, and x is 0.8 or more and 1.2 or less. This makes the crystal structure of the first unit layer 12 a hexagonal system, and the heat resistance, oxidation resistance, and wear resistance of the first unit layer 12 can be improved.

[0057] The lower limit of a is 0.3 or more, and may be 0.35 or more, 0.40 or more, or 0.45 or more. The upper limit of a is 0.8 or less, and may be 0.75 or less, 0.70 or less, or 0.65 or less. a may be 0.35 or more and 0.75 or less, 0.40 or more and 0.70 or less, or 0.45 or more and 0.65 or less.

[0058] The lower limit of x is 0.8 or more, and may be 0.85 or more, or 0.90 or more. The upper limit of x is 1.2 or less, and may be 1.15 or less, or 1.10 or less. x may be 0.85 or more and 1.15 or less, or 0.90 or more and 1.10 or less, or 1.00.

[0059] In the present disclosure, "the first unit layer is W(C 1-a N a ) x The phrase "consisting of" means that the first unit layer 12 is made of W(C 1-a N a ) xThis means that the first unit layer 12 may contain inevitable impurities in addition to the above. Examples of inevitable impurities include oxygen and carbon. The total content of inevitable impurities in the first unit layer 12 may be greater than 0 atomic % and less than 1 atomic %. In this disclosure, "atomic %" refers to the ratio (%) of the number of atoms to the total number of atoms constituting the layer.

[0060] The second unit layer 15 is made of Al c Cr 1-c N, and c is 0.40 or more and 0.80 or less. The second unit layer 15 can improve the heat resistance, oxidation resistance, and toughness of the coating 3. The lower limit of c is 0.40 or more, and may be 0.45 or more, 0.50 or more, or 0.55 or more. The upper limit of c is 0.80 or less, 0.75 or less, 0.70 or less, or 0.65 or less. c may be 0.45 or more and 0.75 or less, 0.50 or more and 0.70 or less, or 0.55 or more and 0.65 or less.

[0061] In the present disclosure, "the second unit layer is Al c Cr 1-c The phrase "made of AlN" means that the second unit layer 15 is made of AlN as long as it does not impair the effect of the present disclosure. c Cr 1-c This means that the second unit layer 15 may contain unavoidable impurities in addition to N. Examples of the unavoidable impurities include oxygen and carbon. The total content of the unavoidable impurities in the second unit layer 15 may be greater than 0 atomic % and less than 1 atomic %.

[0062] The above a, x, c, and the content of inevitable impurities in the first unit layer 12 and the content of inevitable impurities in the second unit layer 15 are measured by elemental analysis of a cross section of the coating 3 using a transmission electron microscope (TEM). The specific measurement method is as follows: The cutting tool 1 is cut in a direction normal to the surface of the coating 3 to prepare a thin section sample including a cross section of the coating 3. Using an EDS (Energy Dispersive X-ray Spectroscopy) attached to the TEM, the thin section sample is irradiated with an electron beam, and the energy and number of characteristic X-rays generated are measured to perform elemental analysis of the first unit layer 12 and the second unit layer 15. Five layers of each of the first unit layer 12 and the second unit layer 15 are arbitrarily selected and subjected to elemental analysis. The average composition of the five first unit layers 12 is determined. This average composition corresponds to the composition of the first unit layer 12. The average composition of the five second unit layers 15 is determined. This average composition corresponds to the composition of the second unit layers 15. If the number of layers of each of the first unit layers 12 and the second unit layers 15 is four or less, elemental analysis is performed on all layers to determine the average compositions of the first unit layers 12 and the second unit layers 15. It has been confirmed that, as long as measurements are made using the same cutting tool 1, there is no variation in the measurement results even if the measurement location is selected arbitrarily.

[0063] In the present disclosure, the composition W(C 1-a N a ) x In this case, the number of atoms of W is A M1 The total number of C and N atoms A N1 Ratio A N1 / A M1 In the present disclosure, the composition of the second unit layer is Al c Cr 1-c In N, the total number of Al and Cr atoms, A M2 Number of N atoms A N2 Ratio A N2 / A M2 The ratio A is necessarily 0.8 or more and 1.2 or less in terms of manufacturing. N1 / A M1 and ratio A N2 / A M2 can be measured by Rutherford backscattering (RBS) method. N1 / AM1 and ratio A N2 / A M2 It has been confirmed that the effects of the present disclosure are not impaired if the value is within the above range.

[0064] <Average Thickness of First Unit Layer and Average Thickness of Second Unit Layer> The average thickness of the first unit layer 12 may be 0.002 μm or more and 0.2 μm or less, and the average thickness of the second unit layer 15 may be 0.002 μm or more and 0.2 μm or less. This can further suppress the progression of cracks that occur on the surface of the coating 3. The lower limit of the average thickness of the first unit layer 12 may be 0.002 μm or more, 0.005 μm or more, or 0.01 μm or more. The upper limit of the average thickness of the first unit layer 12 may be 0.20 μm or less, 0.15 μm or less, or 0.10 μm or less. The average thickness of the first unit layer 12 may be 0.005 μm or more and 0.15 μm or less, or 0.01 μm or more and 0.1 μm or less. The lower limit of the average thickness of the second unit layer 15 may be 0.002 μm or more, 0.005 μm or more, or 0.01 μm or more. The upper limit of the average thickness of the second unit layer 15 may be 0.20 μm or less, 0.15 μm or less, or 0.10 μm or less. The average thickness of the second unit layer 15 may be 0.005 μm or more and 0.15 μm or less, or 0.01 μm or more and 0.10 μm or less.

[0065] The average thickness of the first unit layer 12 and the average thickness of the second unit layer 15 can be measured by the same method as the method for measuring the thickness of the first layer 13 described above.

[0066] As shown in FIG. 5 , the ratio λ2 / λ1 of the thickness λ2 μm of the second unit layer 15 to the thickness λ1 μm of the first unit layer 12 between the first unit layer 12 and the second unit layer 15 adjacent to the first unit layer 12 may be 1.0 or greater and 5.0 or less. The second unit layer 15 has high oxidation resistance and low thermal conductivity, making it difficult for heat generated during cutting to be transmitted to the substrate 2. When the ratio λ2 / λ1 is 1.0 or greater, the proportion of the second unit layer 15 in the coating 3 increases relatively, and the Al content in the coating 3 increases, improving the heat barrier properties of the cutting tool 1 as a whole. The cutting tool 1 having the coating 3 has improved wear resistance, particularly during continuous cutting. When λ2 / λ1 is 1.0 or greater, the toughness of the coating 3 tends to be improved. On the other hand, when λ2 / λ1 is 5.0 or less, the stacking of the first unit layer 12 and the second unit layer 15 tends to more easily suppress crack propagation.

[0067] λ2 / λ1 may be 1.0 or more, 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, 2.0 or more, or 2.5 or more. λ2 / λ1 may be 5.0 or less, 4.0 or less, or 3.0 or less. λ2 / λ1 may be 1.2 or more and 4.0 or less, or 1.5 or more and 2.5 or less. For the sake of explanation, FIG. 5 shows the thicknesses of all three first unit layers 12 as λ1 and the thicknesses of all three second unit layers 15 as λ2. However, as long as the above λ2 / λ1 relationship is satisfied between adjacent first unit layers and second unit layers, the thicknesses λ1 of the three first unit layers 12 and the thicknesses λ2 of the three second unit layers 15 do not need to be the same.

[0068] In the first layer 13, the number of stacked first unit layers 12 and second unit layers 15 may be 5 or more and 500 or less, or 10 or more and 500 or less. By stacking the first unit layers 12 and the second unit layers 15, it is possible to sufficiently obtain the effect of improving hardness and compressive residual stress in a well-balanced manner. In the first layer 13, the number of stacked first unit layers 12 and second unit layers 15 may be 100 or more and 400 or less, or 200 or more and 350 or less.

[0069] In the first layer 13, the number of layers of each of the first unit layers 12 and the second unit layers 15 can be determined by observing a thin section sample of the cross section of the coating 3 using a TEM (transmission electron microscope) at a magnification of 20,000 to 5,000,000 times.

[0070] 3 and 4, the coating 3 further includes a second layer 16 disposed between the substrate 2 and the first layer 13, and the composition of the second layer 16 may be the same as the composition of the first unit layer 12 or the composition of the second unit layer 15. This can improve the adhesion between the substrate 2 and the coating 3.

[0071] When the composition of the second layer 16 is the same as the composition of the first unit layer 12, even if the second layer 16 is exposed at the beginning of cutting, the second layer 16 has good sliding properties, and therefore wear resistance can be improved.

[0072] When the composition of the second layer 16 is the same as that of the first unit layer 12, the thickness of the second layer 16 may be thicker than that of the first unit layer 12. This can further improve adhesion between the substrate 2 and the coating 3. Furthermore, even when the second layer 16 is exposed at the beginning of cutting, the second layer 16 has good sliding properties, thereby improving wear resistance. The phrase "the thickness of the second layer is thicker than that of the first unit layer" can be rephrased as "the thickness of the second layer is more than 1.0 times the thickness of the first unit layer." The thickness of the second layer 16 may be 2.0 times or more, 4.0 times or more, or 10.0 times or more the thickness of the first unit layer 12. The thickness of the second layer 16 may be 500 times or less, 120 times or less, or 50 times or less the thickness of the first unit layer 12. The thickness of the second layer 16 may be 2.0 times or more and 500 times or less, 4.0 times or more and 120 times or less, or 10.0 times or more and 50 times or less, the thickness of the first unit layer 12 .

[0073] When the composition of the second layer 16 is the same as the composition of the first unit layer 12, the thickness of the second layer 16 may be 0.1 μm or more. When the thickness of the second layer 16 is less than 0.1 μm, it tends to be difficult to obtain the improved wear resistance that would be obtained by making the second layer 16 have the same composition as the first unit layer 12. When the composition of the second layer 16 is the same as the composition of the first unit layer 12, the thickness of the second layer 16 may be 0.3 μm or more, or even 0.4 μm or more. There is no particular upper limit for the thickness of the second layer 16, but if it exceeds 2 μm, the crystal grains will thicken and grain boundaries will occur, making it difficult to obtain the improved wear resistance. Therefore, considering costs, the thickness of the second layer 16 can be 2 μm or less.

[0074] When the composition of the second layer 16 is the same as the composition of the first unit layer 12, the first unit layer 12 may be stacked directly on the second layer 16, as shown in Fig. 3. Alternatively, the second unit layer 15 may be stacked directly on the second layer 16, as shown in Fig. 4. When the composition of the second layer 16 is the same as the composition of the first unit layer 12 and the first unit layer 12 is stacked directly on the second layer 16, the second layer 16 and the first unit layer 12 have a continuous crystal structure.

[0075] When the composition of the second layer 16 is the same as that of the second unit layer 15, the thickness of the second layer 16 may be thicker than that of the second unit layer 15. This can further enhance adhesion between the substrate 2 and the coating 3. Furthermore, even if the second layer 16 is exposed at the beginning of cutting, oxidation at the interface between the substrate 2 and the coating 3 can be suppressed and cutting heat can be blocked. The phrase "the thickness of the second layer is thicker than that of the second unit layer" can be rephrased as "the thickness of the second layer is more than 1.0 times the thickness of the second unit layer." The thickness of the second layer 16 may be 2.0 times or more, 4.0 times or more, or 10.0 times or more the thickness of the second unit layer 15. The thickness of the second layer 16 may be 500 times or less, 120 times or less, or 50 times or less the thickness of the second unit layer 15. The thickness of the second layer 16 may be 2.0 times or more and 500 times or less, 4.0 times or more and 120 times or less, or 10.0 times or more and 50 times or less, the thickness of the second unit layer 15 .

[0076] When the composition of the second layer 16 is the same as that of the second unit layer 15, the thickness of the second layer 16 may be 0.1 μm or more. If the thickness of the second layer 16 is less than 0.1 μm, it tends to be difficult to obtain the effects of suppressing oxidation at the interface between the substrate 2 and the coating 3 and the cutting heat insulation effect achieved by making the second layer 16 the same composition as the second unit layer 15. When the composition of the second layer 16 is the same as that of the second unit layer 15, the thickness of the second layer 16 may be 0.3 μm or more, or even 0.4 μm or more. While there is no particular upper limit for the thickness of the second layer 16, if it exceeds 2 μm, the crystal grains will thicken and grain boundaries will occur, making it difficult to further improve the above-mentioned oxidation suppression effect. Therefore, considering cost, the thickness of the second layer 16 can be 2 μm or less.

[0077] When the composition of the second layer 16 is the same as the composition of the second unit layer 15, the first unit layer 12 may be stacked directly on the second layer 16, as shown in Fig. 3. Alternatively, the second unit layer 15 may be stacked directly on the second layer 16, as shown in Fig. 4. When the composition of the second layer 16 is the same as the composition of the second unit layer 15 and the second unit layer 15 is stacked directly on the second layer 16, the second layer 16 and the second unit layer 15 have a continuous crystal structure.

[0078] 1 to 4, the coating 3 further includes a third layer 14 provided on the side of the first layer 13 opposite the substrate 2, and the third layer 14 may be made of AlCrCN. This reduces the coefficient of friction of the coating 3, thereby enabling the cutting tool 1 to have a longer life.

[0079] Generally, carbonitrides tend to have a lower coefficient of friction with respect to the workpiece than nitrides. This decrease in the coefficient of friction is believed to be due to the contribution of carbon atoms. When the coating 3 includes the third layer 14, the coefficient of friction of the coating 3 with respect to the workpiece decreases, thereby extending the life of the cutting tool 1.

[0080] It is possible to impart a predetermined color to the third layer 14 by adjusting the composition ratio of N and C. This allows the cutting tool 1 to have a design and distinctive appearance, making it commercially useful.

[0081] The thickness of the third layer 14 may be 0.1 μm or more. When the thickness of the third layer 14 is 0.1 μm or more, the lubricity-imparting effect of the third layer 14 is easily obtained. On the other hand, although there is no particular upper limit for the thickness of the third layer 14, when the thickness exceeds 2 μm, the lubricity-imparting effect described above tends not to be further improved. Therefore, in consideration of cost, the thickness of the third layer 14 may be 2 μm or less.

[0082] <Intermediate Layer> The coating 3 may include an intermediate layer disposed between the second layer 16 and the first layer 13, or between the first layer 13 and the third layer 14. Examples of intermediate layers include AlCrCeN, AlCrN, AlCrBN, AlCrSiN, AlCrYN, and AlCrLaN. The thickness of the intermediate layer may be 0.1 μm or more and 2 μm or less, 0.3 μm or more and 1.5 μm or less, or 0.4 μm or more and 1.0 μm or less.

[0083] [Embodiment 2: Cutting Tool (2)] A cutting tool according to another embodiment of the present disclosure will be described with reference to Figures 6 to 10. A cutting tool 1 according to another embodiment of the present disclosure (hereinafter also referred to as "Embodiment 2") is a cutting tool 1 including a substrate 2 and a coating 3 disposed on the substrate 2, wherein the coating 3 includes a first A layer 13A, the first A layer 13A being composed of alternating layers in which first unit layers 12 and third unit layers 17 are alternately stacked, the first unit layers having a hexagonal crystal structure, and the first unit layers 12 are composed of W(C 1-a N a ) x a is 0.3 or more and 0.8 or less, x is 0.8 or more and 1.2 or less, and the third unit layer 17 is made of Al d Cr 1-d-e M e N; M is silicon, boron, yttrium, cerium, or lanthanum; d is 0.40 or more and 0.80 or less; and e is more than 0 and 0.05 or less.

[0084] The cutting tool 1 of the first embodiment can have a long tool life, especially in cutting operations performed under conditions where the cutting edge temperature is high. The reason for this is presumed to be as follows.

[0085] The first unit layer 12 is W(C 1-a N a ) x Since the first unit layer 12 contains C (carbon), the coefficient of friction at the contact interface with the workpiece material is reduced, and cutting resistance can be reduced. 1-a N a ) x Since it contains N (nitrogen), its heat resistance is improved by about 150°C compared to WC. As a result, the first layer including the first unit layer can improve the wear resistance in processes where the cutting edge becomes hot, such as dry cutting processes. Therefore, the tool life of a cutting tool including the first layer is improved.

[0086] When a layer made of nitrides of Al and Cr (hereinafter also referred to as "AlCrN layer") is compared with a layer made of nitrides containing Al, Cr, and M (M is silicon, boron, yttrium, cerium, or lanthanum) (hereinafter also referred to as "AlCrMN layer"), the AlCrMN layer is less susceptible to spinodal decomposition of AlCrN at high temperatures. If spinodal decomposition occurs, soft hexagonal AlN precipitates, causing a decrease in hardness. The AlCrMN layer has properties that hardness decrease is suppressed even at high temperatures, has large compressive residual stress, and is excellent in chipping resistance. The AlCrMN layer has properties of high thermal insulation. The first A layer 13A is made of W (C 1-a N a ) x Since the first unit layer 13A is composed of alternating layers in which the first unit layer 12 made of AlCrMN layers and the third unit layer 17 made of AlCrMN layers are alternately stacked, it is possible to have the high hardness and low friction coefficient characteristics of the first unit layer 12 and the high heat insulating property characteristics of the third unit layer 17. The large compressive residual stress characteristic of the third unit layer 17 is complemented by the small compressive residual stress of the first unit layer 12. Therefore, the hardness, heat insulating property, and compressive residual stress of the firstA layer 13A as a whole are improved in a balanced manner, and the life of the cutting tool 1 including the firstA layer 13A is extended.

[0087] The first A layer 13A is composed of alternating layers in which first unit layers 12 and third unit layers 17 are alternately stacked. The composition and crystal lattice are discontinuous at the interface between the first unit layers 12 and the third unit layers 17. Therefore, if a crack occurs on the surface of the coating 3 during cutting, the propagation of the crack can be suppressed at the interface. This suppresses chipping and fracture, and extends the life of the cutting tool 1.

[0088] The cutting tool 1 of the second embodiment can have basically the same configuration as the cutting tool 1 of the first embodiment, except for the configurations of the first A layer 13A, the second A layer 16, and the third A layer 14A. The "first A layer," "second A layer," and "third A layer" will be described below.

[0089] <First A Layer> The first A layer 13A of this embodiment is composed of alternating layers in which first unit layers 12 and third unit layers 17 are alternately stacked. The fact that the first A layer 13A is composed of alternating layers in which the first unit layers 12 and the third unit layers 17 are alternately stacked can be confirmed by observing the cross section of the coating 3 with a TEM (transmission electron microscope) and observing the difference in contrast. The thickness of the first A layer 13A can be configured to be the same as the thickness of the first layer 13 described in embodiment 1.

[0090] <Composition of First Unit Layer and Composition of Third Unit Layer> The composition W(C 1-a N a ) x is the composition W(C 1-a N a ) x can be the same as

[0091] The third unit layer 17 is Al d Cr 1-d-e M e The third unit layer 17 is made of N, where M is silicon, boron, yttrium, cerium, or lanthanum, d is 0.40 or more and 0.80 or less, and e is more than 0 and 0.05 or less. The third unit layer 17 can have both excellent hardness and excellent oxidation resistance. The reason for this is presumed to be as follows.

[0092] When M is silicon, the structure of the third unit layer 17 becomes finer, thereby improving the hardness and oxidation resistance of the third unit layer 17 and improving the hardness and oxidation resistance of the entire coating 3 .

[0093] When M is boron, the boron increases the hardness of the third unit layer 17, thereby increasing the hardness of the entire coating 3. In addition, boron oxides formed by oxidation of the surface of the cutting tool 1 during cutting densify the Al oxides in the third unit layer 17, improving the oxidation resistance of the third unit layer 17. Furthermore, boron oxides have a low melting point and therefore act as a lubricant during cutting, thereby suppressing adhesion of the workpiece material.

[0094] When M is yttrium (Y), cerium (Ce), or lanthanum (La), the lattice constant of YN is 4.88 Å, the lattice constant of CeN is 5.01 Å, and the lattice constant of LaN is 5.30 Å. The lattice constants of YN, CeN, and LaN are larger than the lattice constant of TiN, 4.23 Å, and the lattice constant of AlN, 4.12 Å. Therefore, AlN, which is cubic crystallized by adding Y, Ce, or La, has a lattice constant of 4.88 Å, the lattice constant of CeN is 5.01 Å, and the lattice constant of LaN is 5.30 Å. d Cr 1-d-e M e Strain is introduced into the third unit layer 17 made of N, and the structure becomes finer, improving the hardness and wear resistance of the third unit layer 17 and extending the life of the cutting tool 1 including the third unit layer 17.

[0095] The above d is 0.40 or more and 0.80 or less. This makes the crystal structure of the third unit layer 17 a cubic crystal type, increasing the hardness of the third unit layer 17 and improving the wear resistance. The lower limit of d may be 0.45 or more, 0.50 or more, or 0.55 or more. The upper limit of d may be 0.75 or less, 0.70 or less, or 0.65 or less. d may be 0.45 or more and 0.75 or less, 0.50 or more and 0.70 or less, or 0.55 or more and 0.65 or less.

[0096] The above-mentioned e is greater than 0 and less than or equal to 0.05. This can improve the hardness and oxidation resistance of the first A layer 13A. The lower limit of e may be 0.002 or more, 0.005 or more, 0.01 or more, or 0.02 or more. The e may be 0.04 or less, or 0.03 or less. The e may be 0.002 or more and 0.05 or less, 0.01 or more and 0.05 or less, 0.01 or more and 0.03 or less, or 0.02 or more and 0.03 or less.

[0097] In the present disclosure, "the third unit layer is Al d Cr 1-d-e M e The phrase "made of AlN" means that the third unit layer 17 is made of AlN as long as it does not impair the effect of the present disclosure. d Cr 1-d-e M e This means that the third unit layer 17 may contain inevitable impurities in addition to N. Examples of the inevitable impurities include oxygen and carbon. The total content of the inevitable impurities in the third unit layer 17 may be greater than 0 atomic % and less than 1 atomic %.

[0098] The content of inevitable impurities in the above d, e, and the third unit layer 17 can be determined by the same method as the measurement method in the above a. It has been confirmed that there is no variation in the measurement results even if the measurement location is arbitrarily selected, as long as the measurement is performed using the same cutting tool 1.

[0099] In the present disclosure, the composition W(C 1-a N a ) x In this case, the number of atoms of W is A M1 The total number of C and N atoms A N1 Ratio A N1 / A M1 In the present disclosure, the composition of the third unit layer is Al d Cr 1-d-e M e In N, the total number of Al, Cr and M atoms A M3 Number of N atoms A N3 Ratio A N3 / A M3 The ratio A is necessarily 0.8 or more and 1.2 or less in terms of manufacturing. N1 / A M1and ratio A N3 / A M3 can be measured by Rutherford backscattering (RBS) method. N1 / A M1 and ratio A N3 / A M3 It has been confirmed that the effects of the present disclosure are not impaired if the value is within the above range.

[0100] <Average Thickness of First Unit Layer and Average Thickness of Third Unit Layer> The average thickness of the first unit layer 12 may be 0.002 μm or more and 0.2 μm or less, and the average thickness of the third unit layer 17 may be 0.002 μm or more and 0.2 μm or less. This can further suppress the progression of cracks that occur on the surface of the coating 3. The lower limit of the average thickness of the first unit layer 12 may be 0.002 μm or more, 0.005 μm or more, or 0.01 μm or more. The upper limit of the average thickness of the first unit layer 12 may be 0.20 μm or less, 0.15 μm or less, or 0.10 μm or less. The average thickness of the first unit layer 12 may be 0.005 μm or more and 0.15 μm or less, or 0.01 μm or more and 0.1 μm or less. The lower limit of the average thickness of the third unit layer 17 may be 0.002 μm or more, 0.005 μm or more, or 0.01 μm or more. The upper limit of the average thickness of the third unit layer 17 may be 0.20 μm or less, 0.15 μm or less, or 0.10 μm or less. The average thickness of the third unit layer 17 may be 0.005 μm or more and 0.15 μm or less, or 0.01 μm or more and 0.10 μm or less.

[0101] The average thickness of the first unit layer 12 and the average thickness of the third unit layer 17 can be determined by the same method as the method for measuring the thickness of the first layer 13 described above.

[0102] As shown in FIG. 10 , the ratio λ3 / λ1 of the thickness λ3 of the third unit layer 17 to the thickness λ1 of the first unit layer 12 between the first unit layer 12 and the third unit layer 17 adjacent to the first unit layer 12 may be 1.0 or greater and 5.0 or less. The third unit layer 17 has high oxidation resistance and low thermal conductivity, making it difficult for heat generated during cutting to be transmitted to the substrate 2. When the ratio λ3 / λ1 is 1.0 or greater, the proportion of the third unit layer 17 in the coating 3 increases relatively, and the Al content in the coating 3 increases, improving the heat barrier properties of the cutting tool 1 as a whole. The cutting tool 1 having the coating 3 has improved wear resistance, particularly during continuous cutting. When λ3 / λ1 is 1.0 or greater, the toughness of the coating 3 tends to improve. On the other hand, when λ3 / λ1 is 5.0 or less, the stacking of the first unit layer 12 and the third unit layer 17 tends to more easily suppress crack propagation.

[0103] λ3 / λ1 may be 1.0 or more, 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, or 2.0 or more. λ3 / λ1 may be 5.0 or less, 4.0 or less, or 3.0 or less. λ3 / λ1 may be 1.0 or more and 5.0 or less, 1.2 or more and 4.0 or less, 1.5 or more and 4.0 or less, 1.0 or more and 3.0 or less, or 2.0 or more and 3.0 or less. For the sake of explanation, in Figure 10, the thicknesses of all three first unit layers 12 are shown as λ1 and the thicknesses of all three third unit layers 17 are shown as λ3. However, as long as the above-mentioned λ3 / λ1 relationship is satisfied between adjacent first unit layers and third unit layers, the thicknesses λ1 of the three first unit layers 12 do not need to be the same, and the thicknesses λ3 of the three third unit layers 17 do not need to be the same.

[0104] In the first A layer 13A, the number of stacked first unit layers 12 and third unit layers 17 may be 4 or more and 800 or less, or 10 or more and 500 or less. This tends to make it easier to achieve the effect of improving hardness and compressive residual stress in a well-balanced manner by stacking the first unit layers 12 and the third unit layers 17. In the first A layer 13A, the number of stacked first unit layers 12 and third unit layers 17 may be 100 or more and 400 or less, or 200 or more and 350 or less.

[0105] In the first A layer 13A, the number of stacked first unit layers 12 and third unit layers 17 can be determined using a method similar to the method for measuring the number of stacked first unit layers 12 and second unit layers 15 described in embodiment 1.

[0106] 8 and 9, the coating 3 further includes a second A layer 16A disposed between the substrate 2 and the first A layer 13A, and the composition of the second A layer 16A may be the same as the composition of the first unit layer 12 or the composition of the third unit layer 17. This can improve the adhesion between the substrate 2 and the coating 3.

[0107] When the composition of the second A layer 16A is the same as the composition of the first unit layer 12, even if the second A layer 16A is exposed at the beginning of cutting, the second A layer 16A has good sliding properties, so that wear resistance can be improved.

[0108] When the composition of the second A layer 16A is the same as that of the first unit layer 12, the thickness of the second A layer 16A may be thicker than that of the first unit layer 12. This can further improve adhesion between the substrate 2 and the coating 3. Furthermore, even when the second A layer 16A is exposed at the beginning of cutting, the second A layer 16A has good sliding properties, thereby improving wear resistance. The phrase "the thickness of the second A layer is thicker than that of the first unit layer" can be rephrased as "the thickness of the second A layer is more than 1.0 times the thickness of the first unit layer." The thickness of the second A layer 16A may be 2.0 times or more, 4.0 times or more, or 10.0 times or more the thickness of the first unit layer 12. The thickness of the second A layer 16A may be 500 times or less, 120 times or less, or 50 times or less the thickness of the first unit layer 12. The thickness of the second A layer 16A may be 2.0 times or more and 500 times or less, 4.0 times or more and 120 times or less, or 10.0 times or more and 50 times or less, the thickness of the first unit layer 12.

[0109] When the composition of the second A layer 16A is the same as that of the first unit layer 12, the thickness of the second A layer 16A may be 0.1 μm or more. If the thickness of the second A layer 16A is less than 0.1 μm, it tends to be difficult to obtain the improved wear resistance that comes from having the second A layer 16A have the same composition as the first unit layer 12. When the composition of the second A layer 16A is the same as that of the first unit layer 12, the thickness of the second A layer 16A may be 0.3 μm or more, or even 0.4 μm or more. There is no particular upper limit for the thickness of the second A layer 16A, but if it exceeds 2 μm, the crystal grains will thicken and grain boundaries will occur, making it difficult to obtain the improved wear resistance. Therefore, considering costs, the thickness of the second A layer 16A can be 2 μm or less.

[0110] When the composition of the second A layer 16A is the same as the composition of the first unit layer 12, the first unit layer 12 may be stacked directly on the second A layer 16A, as shown in Fig. 8. Furthermore, the second unit layer 15 may be stacked directly on the second A layer 16A, as shown in Fig. 9. When the composition of the second A layer 16A is the same as the composition of the first unit layer 12 and the first unit layer 12 is stacked directly on the second A layer 16A, the second A layer 16A and the first unit layer 12 have a continuous crystal structure.

[0111] When the composition of the second A layer 16A is the same as the composition of the third unit layer 17, the third unit layer 17 tends to have low stress, and therefore the peeling resistance of the coating 3 can be improved, particularly in intermittent machining such as milling and end milling, in which loads are repeatedly applied to the cutting edge.

[0112] When the composition of the second A layer 16A is the same as that of the third unit layer 17, the thickness of the second A layer 16A may be thicker than that of the third unit layer 17. This can further enhance adhesion between the substrate 2 and the coating 3. Furthermore, even if the second A layer 16A is exposed at the beginning of cutting, oxidation at the interface between the substrate 2 and the coating 3 can be suppressed and cutting heat can be blocked. The phrase "the thickness of the second A layer is thicker than that of the third unit layer" can be rephrased as "the thickness of the second A layer is more than 1.0 times the thickness of the third unit layer." The thickness of the second A layer 16A may be 2.0 times or more, 4.0 times or more, or 10.0 times or more the thickness of the third unit layer 17. The thickness of the second A layer 16A may be 500 times or less, 120 times or less, or 50 times or less the thickness of the third unit layer 17. The thickness of the second A layer 16A may be 2.0 times or more and 500 times or less, 4.0 times or more and 120 times or less, or 10.0 times or more and 50 times or less, the thickness of the third unit layer 17.

[0113] When the composition of the second A layer 16A is the same as that of the third unit layer 17, the thickness of the second A layer 16A may be 0.1 μm or more. If the thickness of the second A layer 16A is less than 0.1 μm, it tends to be difficult to obtain the effects of suppressing oxidation at the interface between the substrate 2 and the coating 3 and the cutting heat insulation effect achieved by making the second A layer 16A the same composition as the third unit layer 17. When the composition of the second A layer 16A is the same as that of the third unit layer 17, the thickness of the second A layer 16A may be 0.3 μm or more, or even 0.4 μm or more. There is no particular upper limit for the thickness of the second A layer 16A, but if it exceeds 2 μm, the crystal grains will thicken and grain boundaries will occur, making it difficult to further improve the above-mentioned oxidation suppression effect. Therefore, considering cost, the thickness of the second A layer 16A can be 2 μm or less.

[0114] When the composition of the second A layer 16A is the same as the composition of the third unit layer 17, the first unit layer 12 may be stacked directly on the second A layer 16A, as shown in Fig. 8. Furthermore, the third unit layer 17 may be stacked directly on the second A layer 16A, as shown in Fig. 9. When the composition of the second A layer 16A is the same as the composition of the third unit layer 17 and the third unit layer 17 is stacked directly on the second A layer 16A, the second A layer 16A and the third unit layer 17 have a continuous crystal structure.

[0115] 6 to 9, the coating 3 further includes a third layer 14A provided on the side of the first layer 13 opposite the substrate 2, and the third layer 14A may be made of AlCrMeCN. Here, Me may be silicon, boron, yttrium, cerium, or lanthanum. Me may be the same element as M used in the third unit layer. This reduces the friction coefficient of the coating 3 and extends the life of the cutting tool 1.

[0116] Generally, carbonitrides tend to have a lower coefficient of friction with respect to the workpiece than nitrides. This decrease in the coefficient of friction is believed to be due to the contribution of carbon atoms. When the coating 3 includes the third A layer 14A, the coefficient of friction of the coating 3 with respect to the workpiece decreases, thereby extending the life of the cutting tool 1.

[0117] In the third A layer 14A, it is possible to impart a predetermined color by adjusting the composition ratio of N and C. This allows the cutting tool 1 to have a design and distinctive appearance, making it commercially useful.

[0118] The thickness of the 3A layer 14A may be 0.1 μm or more. When the thickness of the 3A layer 14A is 0.1 μm or more, the lubricity-imparting effect of the 3A layer 14A is easily obtained. On the other hand, although there is no particular upper limit for the thickness of the 3A layer 14A, when it exceeds 2 μm, it tends to be difficult to further improve the above-mentioned lubricity-imparting effect. Therefore, in consideration of cost, the thickness of the 3A layer 14A may be 2 μm or less.

[0119] [Embodiment 3: Method for Manufacturing Cutting Tool] In embodiment 3, a method for manufacturing the cutting tool 1 of embodiment 1 or embodiment 2 will be described. The manufacturing method includes a first step of preparing a substrate 2 and a second step of forming a coating 3 on the substrate 2. The second step includes a step of forming the first layer 13 or the firstA layer 13A. Details of each step will be described below.

[0120] <First Step> In the first step, a substrate 2 is prepared. As the substrate 2, the substrate 2 described in the first embodiment can be used.

[0121] When a cemented carbide is used as the substrate 2, a commercially available substrate may be used, or it may be manufactured by a general powder metallurgy method. When manufactured by a general powder metallurgy method, WC powder and Co powder, etc. are mixed using a ball mill or the like to obtain a mixed powder. The mixed powder is dried and then molded into a predetermined shape to obtain a green body. The green body is then sintered to obtain a WC-Co based cemented carbide (sintered body). Next, the sintered body is subjected to a predetermined cutting edge processing such as honing, thereby producing a substrate made of a WC-Co based cemented carbide. Any substrate other than those described above can also be prepared as long as it is a conventionally known substrate of this type.

[0122] <Second Step> In the second step, the coating 3 is formed on the substrate 2. The second step includes a step of forming the first layer 13 or the first A layer 13A.

[0123] In the "step of forming the first layer," the first layer 13 is formed by alternately stacking first unit layers 12 and second unit layers 15 using a physical vapor deposition (PVD) method. In the "step of forming the firstA layer," the firstA layer 13A is formed by alternately stacking first unit layers 12 and third unit layers 17 using a PVD method. In order to improve the abrasion resistance of the coating 3 including the first layer 13 or the firstA layer 13A, it is effective to form a layer made of a highly crystalline compound. The inventors have investigated various methods for forming the first layer 13 and the firstA layer 13A and have found that by using a physical vapor deposition method, a layer made of a highly crystalline compound can be formed, and the coating 3 has excellent abrasion resistance.

[0124] The PVD method may be at least one selected from the group consisting of cathodic arc ion plating, balanced magnetron sputtering, unbalanced magnetron sputtering, and HiPIMS (High Power Impulse Magnetron Sputtering). In particular, cathodic arc ion plating, which has a high ionization rate of the raw material elements, may be used. When cathodic arc ion plating is used, metal ion bombardment treatment can be performed on the surface of the substrate 2 before forming the first layer 13 or the first A layer 13A. This significantly improves adhesion between the substrate 2 and the coating 3 including the first layer 13 or the first A layer 13A.

[0125] The cathodic arc ion plating method can be carried out, for example, by placing a substrate 2 in an apparatus and a target as a cathode, and then applying a high voltage to the target to generate an arc discharge, thereby ionizing and evaporating the atoms that make up the target, and depositing a substance on the substrate 2.

[0126] The balanced magnetron sputtering method can be carried out, for example, by placing a substrate 2 in an apparatus, placing a target on a magnetron electrode equipped with a magnet that forms a balanced magnetic field, applying high-frequency power between the magnetron electrode and the substrate 2 to generate gas plasma, and causing gas ions generated by the generation of this gas plasma to collide with the target, thereby depositing atoms released from the target on the substrate 2.

[0127] The unbalanced magnetron sputtering method can be performed by unbalancing the magnetic field generated by the magnetron electrodes in the balanced magnetron sputtering method. Furthermore, the HiPIMS method can also be used, which allows the application of a high voltage and produces a dense film.

[0128] <Other Steps> In addition to the step of forming the first layer 13 or the firstA layer 13A, the second step may include a surface treatment step of the coating, such as polishing with a brush or dry or wet shot blasting. The second step may also include the step of forming other layers, such as the second layer 16, the secondA layer 16A, the third layer 14, the thirdA layer 14A, and an intermediate layer. The other layers may be formed by conventionally known chemical vapor deposition or physical vapor deposition. From the viewpoint that the other layers can be formed successively in a single physical vapor deposition apparatus, such as the first unit layer 12 and the second unit layer 15 or the third unit layer 17, it is preferable to form the other layers by physical vapor deposition.

[0129] The present embodiment will be described in more detail with reference to examples, although the present embodiment is not limited to these examples.

[0130] Example 1 Samples 1 to 25, Samples 101 to 106 Fabrication of Cutting Tools FIG. 11 is a schematic cross-sectional view of a cathodic arc ion plating apparatus used in this example, and FIG. 12 is a schematic top view of the apparatus of FIG.

[0131] 11 and 12, a cathode 106 for a first unit layer, a cathode 107 for a second unit layer, and a cathode 120 for a third layer, which are alloy targets serving as the metal raw material for the coating 3, and a rotary substrate holder 104 for placing a substrate are installed in a chamber 101. The composition of the cathode 106 is adjusted to obtain the composition of the first unit layer shown in Table 1. The composition of the cathode 107 is adjusted to obtain the composition of the second unit layer shown in Table 1. The composition of the cathode 120 is adjusted to obtain the composition of the third layer shown in Table 2.

[0132] An arc power supply 108 is attached to cathode 106, an arc power supply 109 is attached to cathode 107, and an arc power supply (not shown) is attached to cathode 120. A bias power supply 110 is attached to substrate holder 104. A gas inlet 105 for introducing gas 102 and a gas outlet 103 for adjusting the pressure inside chamber 101 are provided inside chamber 101, and gas 102 inside chamber 101 can be sucked out from gas outlet 103 by a vacuum pump.

[0133] The substrate holder 104 was fitted with a substrate made of cemented carbide of grade JIS P30, with a tip of JIS CNMG120408 and a tip of Sumitomo Electric Hardmetal Corp. SEMT13T3AGSN having a shape conforming to JIS CNMG120408.

[0134] Next, the pressure inside the chamber 101 is reduced by a vacuum pump, and the substrate is heated to 500° C. by a heater installed inside the apparatus while being rotated, until the pressure inside the chamber 101 reaches 1.0×10 -4 The chamber was evacuated to a vacuum of 2.0 Pa. Next, argon gas was introduced through the gas inlet to maintain the pressure inside the chamber 101 at 2.0 Pa, and the voltage of the bias power supply 110 was gradually increased to -1000 V, and the surface of the substrate was cleaned for 15 minutes. Thereafter, the argon gas was exhausted from the chamber 101 to clean the substrate (argon bombardment treatment). In this manner, the substrate for each sample cutting tool was prepared.

[0135] Next, while the substrate was rotated at the center, argon and nitrogen were introduced as reactive gases, and an arc current of 100 A was supplied to each of the cathodes 106 and 107 while maintaining the substrate temperature at 400°C, the reactive gas pressure at 3.0 Pa, and the voltage of the bias power supply 110 at a predetermined constant value in the range of -50 V to -200 V. Metal ions were generated from the cathodes 106 and 107, and a second layer having the composition shown in Table 2 and a first layer having the composition shown in Table 1 were formed on the substrate. Here, argon gas was introduced because the first unit layer W(C 1-a N a ) xThe purpose of this method is to clean the surface of a WC cathode used when forming a nitride film. In the manufacturing method disclosed herein, the substrate temperature is 400°C, which is lower than the conventional nitride film formation temperature of 600°C. The reason for this is as follows. The inventors have found that when film formation is performed at a substrate temperature of 600°C, the hardness of the coating tends to decrease. After investigating the reason for this, it was inferred that when film formation is performed at a substrate temperature of 600°C, carbon (C) contained in the cathode for the first unit layer becomes free carbon in the formed coating and precipitates. As a result of extensive research, the inventors have found that by performing film formation at a substrate temperature of 400°C, it is possible to form a coating that maintains excellent hardness even at high temperatures and has excellent wear resistance.

[0136] When a second layer was formed, the first layer was formed by alternately stacking one first unit layer and one second unit layer on the second layer, with the number of layers shown in Table 1. When a second layer was not formed, the first layer was formed by alternately stacking one first unit layer and one second unit layer on the substrate, with the number of layers shown in Table 1. The thickness of the second layer, and the thickness and number of the first unit layer and second unit layer in the first layer were adjusted by the rotation speed of the substrate. The current supplied to the evaporation source was stopped when the thicknesses of the second layer and the first layer reached the thicknesses shown in Tables 2 and 1, respectively.

[0137] Next, while argon, nitrogen, and methane gases were introduced into the chamber 101 as reactive gases, an arc current of 80 A was supplied to the cathode 120 while maintaining the substrate temperature at 400°C, the reactive gas pressure at 2.0 Pa, and the bias power supply 110 at -350 V. This generated metal ions from the cathode 120, forming a third layer on the first layer. The current supplied to the evaporation source was stopped when the thickness of the third layer reached the thickness shown in Table 2. The amounts of nitrogen and methane introduced were adjusted so as to obtain the composition of the third layer shown in Table 2. Thus, each sample cutting tool was fabricated.

[0138]

[0139]

[0140] <Evaluation> For the cutting tools of each sample, the composition of the first unit layer, the composition of the second unit layer, the composition of the second layer, the composition of the third layer, the number of layers of the first unit layer and the second unit layer, the average thickness of the first unit layer, the average thickness of the second unit layer, the thickness of the first layer, the thickness of the second layer, the thickness of the third layer, λ2 / λ1 and the crystal structure of the first unit layer, and the hardness of the coating were measured.

[0141] <Measurement of Composition of First Unit Layer> For each sample cutting tool, the composition of the first unit layer was measured by the method described in embodiment 1, and W(C 1-a N a ) x The values ​​of a and x in the above formula were obtained. The results are shown in the "a" and "x" columns of Table 1. In Table 1, "-" in the "a" and "x" columns means that the first unit layer was not present.

[0142] <Measurement of Composition of Second Unit Layer> The composition of the second unit layer of each cutting tool sample was measured by the method described in embodiment 1. c Cr 1-c The value of c at N was obtained. The results are shown in the "c" column of Table 1. In Table 1, "-" in the "c" column means that the second unit layer was not present.

[0143] <Measurement of Composition of Second Layer and Composition of Third Layer> For each sample cutting tool, the composition of the second layer and the third layer was determined by the method described in embodiment 1. The results are shown in the "Composition" column for "Second Layer" and the "Composition" column for "Third Layer" in Table 2. A "-" in the "Composition" column for "Second Layer" in Table 2 means that the second layer is not present, and a "-" in the "Composition" column for "Third Layer" means that the third layer is not present.

[0144] <Measurement of Number of Layers> For each sample cutting tool, the number of layers of each of the first unit layers and the second unit layers was determined by the method described in embodiment 1. For example, a number of layers of 10 indicates that the alternating layers include 10 first unit layers and 10 second unit layers. The results obtained are shown in the "Number of Layers" column in Table 1.

[0145] <Measurement of Average Thickness of First Unit Layer, Average Thickness of Second Unit Layer, Thickness of First Layer, Thickness of Second Layer, and Thickness of Third Layer> For each sample cutting tool, the average thickness of the first unit layer, the average thickness of the second unit layer, the thickness of the first layer, the thickness of the second layer, and the thickness of the third layer were determined by the method described in embodiment 1. The results obtained are shown in the "Average Thickness [μm]" of "First Unit Layer," "Average Thickness [μm] of "Second Unit Layer," and "Thickness [μm]" of "First Layer" columns in Table 1, and in the "Thickness [μm]" of "Second Layer" and "Thickness [μm]" of "Third Layer" columns in Table 2. A "-" in the "Thickness [μm]" column for "Second Layer" in Table 2 means that the second layer is not present. A "-" in the "Thickness [μm]" column for "Third Layer" in Table 2 means that the third layer is not present.

[0146] <Measurement of λ2 / λ1> For each sample cutting tool, λ2 / λ1 was determined by the method described in embodiment 1. The results obtained are shown in the "λ2 / λ1" column of Table 1. Note that "-" in the "λ2 / λ1" column of Table 1 means that at least one of the first unit layer and the second unit layer is absent.

[0147] <Measurement of Crystal Structure of First Unit Layer> For each sample cutting tool, XRD measurement was performed on the first unit layer to confirm whether the first unit layer had a hexagonal crystal structure. The specific method is as described in embodiment 1. The results are shown in the "Hexagonal Crystal Structure" column of "First Unit Layer" in Table 1. "Present" indicates that the first unit layer has a hexagonal crystal structure, and "Absent" indicates that the first unit layer does not have a hexagonal crystal structure. When the crystal structure of the second unit layer was measured, it was confirmed that the second unit layer in all samples contained a cubic crystal structure.

[0148] <Measurement of Coating Hardness> The coating hardness of Samples 1 to 25 was measured by the method described in Embodiment 1. It was confirmed that the coating hardness of these samples was within the range of 30 GPa or more and 55 GPa or less.

[0149] <Cutting Test 1: Continuous Turning Test> A dry continuous turning test was performed on each sample CNMG120408-shaped cutting tool under the following cutting conditions, and the time until the flank wear of the cutting edge reached 0.2 mm was measured. The results are shown in the "Cutting time [min]" column in Table 2. A longer cutting time indicates a longer tool life. <Cutting Conditions> Workpiece material: SCM440 (HB = 300) Cutting speed: 260 m / min Feed rate: 0.3 mm / rev Depth of cut: 2.0 mm Coolant: Dry The cutting performed under the above cutting conditions is high-speed, high-efficiency cutting of difficult-to-cut materials, and corresponds to cutting performed under conditions of high cutting edge temperatures.

[0150] The cutting tools of Samples 1 to 25 correspond to Examples, and the cutting tools of Samples 101 to 106 correspond to Comparative Examples. It was confirmed that the cutting tools of Samples 1 to 25 have a longer tool life in cutting operations performed under conditions where the cutting edge temperature is high, compared to the cutting tools of Samples 101 to 106.

[0151] <Cutting Test 2: Milling Test> For each sample, a cutting tool with a SEMT13T3AGSN shape was surface milled under the following cutting conditions, aligning the centerline of a 150 mm-wide plate made of a difficult-to-cut material with the center of a wider cutter with a diameter of 160 mm. The cutting length was measured until the flank wear of the cutting edge reached 0.2 mm. The results are shown in the "Cutting Length [km]" column in Table 2. A longer cutting length indicates a longer tool life. <Cutting Conditions> Workpiece: SKD11 (HB = 235); Cutting Speed: 190 m / min; Feed Rate: 0.15 mm / t; Axial Depth of Cut: 1.5 mm; Radial Depth of Cut: 150 mm; Coolant: Dry. The cutting performed under the above cutting conditions was high-speed, high-efficiency milling of a difficult-to-cut material under dry conditions, resulting in high cutting edge temperatures.

[0152] The cutting tools of Samples 1 to 25 correspond to Examples, and the cutting tools of Samples 101 to 106 correspond to Comparative Examples. It was confirmed that the cutting tools of Samples 1 to 25 have a longer tool life in cutting operations performed under conditions where the cutting edge temperature is high, compared to the cutting tools of Samples 101 to 106.

[0153] Example 2 Samples 51 to 85, Samples 151 to 176 Fabrication of Cutting Tools Substrates for each sample were prepared in the same manner as in Example 1. While the substrate was rotated at its center, argon and nitrogen were introduced as reactive gases. The substrate temperature was maintained at 450°C, the reactive gas pressure was 2.0 Pa, and the voltage of the bias power supply 110 was maintained at a predetermined constant value in the range of −50 V to −200 V. An arc current of 100 A was supplied to each of cathodes 106 and 107, generating metal ions from cathodes 106 and 107 to form second A layers and first A layers having the compositions shown in Tables 3 to 6 on the substrate. The composition of cathode 106 was adjusted to obtain the composition of the first unit layer shown in Tables 3 to 4. The composition of cathode 107 was adjusted to obtain the composition of the third unit layer shown in Tables 3 to 4. The composition of the cathode 120 was adjusted to obtain the composition of the 3A layer shown in Tables 5 and 6. In the manufacturing method of the present disclosure, the substrate temperature was 450°C, which is lower than the conventional nitride film formation temperature of 600°C. The reason for this is as follows. The inventors have found that when film formation is performed at a substrate temperature of 600°C, the hardness of the coating tends to decrease. After investigating the reason for this, it was inferred that when film formation is performed at a substrate temperature of 600°C, carbon (C) contained in the cathode for the first unit layer becomes free carbon in the formed coating and precipitates. As a result of extensive research, the inventors have found that by performing film formation at a substrate temperature of 450°C, it is possible to form a coating that maintains excellent hardness even at high temperatures and has excellent wear resistance.

[0154] When the 2A layer was formed, the 1A layer was formed by alternately stacking the first unit layer and the third unit layer one by one on the 2A layer, in the number of layers shown in Tables 3 and 4. When the 2A layer was not formed, the 1A layer was formed by alternately stacking the first unit layer and the third unit layer one by one on the substrate, in the number of layers shown in Tables 3 and 4. The thickness of the 2A layer, and the thickness and number of the first unit layer and the third unit layer in the 1A layer were adjusted by the rotation speed of the substrate. Then, the current supplied to the evaporation source was stopped when the thicknesses of the 2A layer and the 1A layer reached the thicknesses shown in Tables 3 to 6, respectively.

[0155] Next, while argon, nitrogen, and methane gas were introduced into the chamber 101 as reactive gases, the substrate temperature was maintained at 350°C, the reactive gas pressure was maintained at 2.0 Pa, and the bias power supply 110 voltage was maintained at -350 V. An arc current of 100 A was supplied to the cathode 120, generating metal ions from the cathode 120 to form a 3A layer on the 1A layer. The current supplied to the evaporation source was stopped when the thickness of the 3A layer reached the thickness shown in Tables 5 and 6. The amounts of nitrogen and methane introduced were adjusted to obtain the compositions of the 3A layer shown in Tables 5 and 6. Thus, cutting tools of each sample were fabricated.

[0156]

[0157]

[0158]

[0159]

[0160] <Evaluation> For the cutting tools of each sample, the composition of the first unit layer, the composition of the third unit layer, the composition of the second A layer, the composition of the third A layer, the number of layers of each of the first unit layer and the third unit layer, the average thickness of the first unit layer, the average thickness of the third unit layer, the thickness of the first A layer, the thickness of the second A layer, the thickness of the third A layer, λ3 / λ1 and the crystal structure of the first unit layer, and the hardness of the coating were measured. The measurement methods for each item were as described in Example 1. The results are shown in Tables 3 to 6.

[0161] <Measurement of Coating Hardness> The coating hardness of Samples 51 to 85 was measured by the method described in Embodiment 1. The coating hardness of these samples was confirmed to be within the range of 30 GPa or more and 55 GPa or less.

[0162] <Cutting Test 3: Continuous Turning Test> A dry continuous turning test was performed on each sample CNMG120408-shaped cutting tool under the following cutting conditions, and the time until the flank wear of the cutting edge reached 0.2 mm was measured. The results are shown in the "Cutting Time [min]" column of Tables 5 and 6. Note that in Tables 5 and 6, a longer cutting time indicates a longer tool life. (Cutting Conditions) Workpiece Material: Inconel 718 (Aged Material: HB = 400) Cutting Speed: 70 m / min Feed Rate: 0.15 mm / rev Depth of Cut: 1.0 mm Coolant: Dry The cutting performed under the above cutting conditions was high-speed, high-efficiency machining of a difficult-to-cut material, and corresponds to cutting performed under conditions of high cutting edge temperatures.

[0163] The cutting tools of Samples 51 to 85 correspond to Examples, and the cutting tools of Samples 151 to 176 correspond to Comparative Examples. It was confirmed that the cutting tools of Samples 51 to 85 have a longer tool life in cutting operations performed under conditions of high cutting edge temperatures than the cutting tools of Samples 151 to 176.

[0164] <Cutting Test 4: Milling Test> For each sample, a cutting tool having a shape of SEMT13T3AGSN was used, with the center line of a 150 mm wide plate made of a difficult-to-cut material aligned with the center of a wider cutter with a diameter of 160 mm. Surface milling was performed under the following cutting conditions, and the cutting length until the flank wear of the cutting edge reached 0.2 mm was measured. The results are shown in the "Cutting Length [km]" column in Tables 5 and 6. In Tables 5 and 6, a longer cutting length indicates a longer tool life. <Cutting conditions> Workpiece material: FCD700 (HB=250) Cutting speed: 260 m / min Feed rate: 0.2 mm / t Axial depth of cut ap: 2.0 mm Radial depth of cut ae: 150 mm Coolant: Dry The cutting performed under the above cutting conditions is high-speed, high-efficiency milling of difficult-to-cut materials under dry conditions, and corresponds to cutting performed under conditions where the cutting edge temperature is high.

[0165] The cutting tools of Samples 51 to 85 correspond to Examples, and the cutting tools of Samples 151 to 176 correspond to Comparative Examples. It was confirmed that the cutting tools of Samples 51 to 85 have a longer tool life in cutting operations performed under conditions of high cutting edge temperatures than the cutting tools of Samples 151 to 176.

[0166] Although the embodiments and examples of the present disclosure have been described above, it is intended from the beginning that the configurations of the above-described embodiments and examples may be appropriately combined or modified in various ways. The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not by the above-described embodiments and examples, and is intended to include meanings equivalent to the claims and all modifications within the scope of the claims.

[0167] 1 Cutting tool, 2 Substrate, 3 Coating, 12 First unit layer, 13 First layer, 13A First A layer, 14 Third layer, 14A Third A layer, 15 Second unit layer, 16 Second layer, 16A Second A layer, 17 Third unit layer, 101 Chamber, 102 Gas, 103 Gas outlet, 104 Substrate holder, 105 Gas inlet, 106, 107, 120 Cathode, 108, 109 Arc power supply, 110 Bias power supply.

Claims

1. A cutting tool comprising a substrate and a coating disposed on the substrate, the coating including a first layer, the first layer being composed of alternating layers in which first unit layers and second unit layers are alternately stacked, the first unit layer having a hexagonal crystal structure, and the first unit layer being composed of W(C 1-a N a ) x The a is 0.3 or more and 0.8 or less, the x is 0.8 or more and 1.2 or less, and the second unit layer is Al c Cr 1-c N, and c is 0.40 or more and 0.80 or less.

2. A cutting tool as described in claim 1, wherein the ratio λ2 / λ1 of the thickness λ2 μm of the second unit layer to the thickness λ1 μm of the first unit layer in the first unit layer and the second unit layer adjacent to the first unit layer is 1.0 or more and 5.0 or less.

3. A cutting tool according to claim 1 or 2, wherein the average thickness of the first unit layer is 0.002 μm or more and 0.2 μm or less, and the average thickness of the second unit layer is 0.002 μm or more and 0.2 μm or less.

4. A cutting tool according to any one of claims 1 to 3, wherein the coating further includes a second layer disposed between the substrate and the first layer, and the composition of the second layer is the same as the composition of the first unit layer or the composition of the second unit layer.

5. The cutting tool according to claim 4, wherein the composition of the second layer is the same as the composition of the first unit layer, and the thickness of the second layer is greater than the thickness of the first unit layer.

6. The cutting tool according to claim 4, wherein the composition of the second layer is the same as the composition of the second unit layer, and the thickness of the second layer is greater than the thickness of the second unit layer.

7. A cutting tool according to any one of claims 1 to 6, wherein the coating further includes a third layer provided on the side opposite the substrate from the first layer, the third layer being made of AlCrCN.

8. A cutting tool comprising a substrate and a coating disposed on the substrate, the coating including a first A layer, the first A layer being composed of alternating layers in which a first unit layer and a third unit layer are alternately laminated, the first unit layer having a hexagonal crystal structure, and the first unit layer being composed of W(C 1-a N a ) x The a is 0.3 or more and 0.8 or less, the x is 0.8 or more and 1.2 or less, and the third unit layer is Al d Cr 1-d-e M e N, M is silicon, boron, yttrium, cerium or lanthanum, d is 0.40 or more and 0.80 or less, and e is more than 0 and 0.05 or less.

9. A cutting tool as described in claim 8, wherein the ratio λ3 / λ1 of the thickness λ3 μm of the third unit layer to the thickness λ1 μm of the first unit layer in the first unit layer and the third unit layer adjacent to the first unit layer is 1.0 or more and 5.0 or less.

10. The cutting tool according to claim 8 or 9, wherein M is silicon.

11. The cutting tool according to claim 8 or 9, wherein M is boron.

12. A cutting tool described in any one of claims 8 to 11, wherein the average thickness of the first unit layer is 0.002 μm or more and 0.2 μm or less, and the average thickness of the third unit layer is 0.002 μm or more and 0.2 μm or less.

13. A cutting tool according to any one of claims 8 to 12, wherein the coating further includes a second A layer disposed between the substrate and the first A layer, and the composition of the second A layer is the same as the composition of the first unit layer or the composition of the third unit layer.

14. The cutting tool according to claim 13, wherein the composition of the second A layer is the same as the composition of the first unit layer, and the thickness of the second A layer is greater than the thickness of the first unit layer.

15. The cutting tool according to claim 13, wherein the composition of the second A layer is the same as the composition of the third unit layer, and the thickness of the second A layer is greater than the thickness of the third unit layer.

16. The cutting tool according to any one of claims 8 to 15, wherein the coating further includes a third A layer provided on the side of the first A layer opposite the substrate, the third A layer being made of AlCrMeCN, and the Me being silicon, boron, yttrium, cerium or lanthanum.

Citation Information

Patent Citations

  • Coated cutting tool

    JP2022143690A

  • Surface coated cutting tool having hard coating layer exerting excellent wear resistance in heavy cutting work

    JP2009125902A

  • Hard film and method for forming the same

    JP2009275293A

  • Hard film and mold

    JP2017206756A

  • Hard lubricating coating film and hard lubricating coating film-covered tool

    WO2015079588A1