Positive electrode active material particles, positive electrode active material mixture, positive electrode for power storage element, power storage element, and power storage device

Positive electrode active material particles with a high destructive test force, including lithium transition metal compounds and additives like zirconium and niobium, address the adhesion issues in power storage elements, leading to increased initial output and improved performance.

WO2024236910A1PCT designated stage expired Publication Date: 2024-11-21GS YUASA INT LTD
View PDF 5 Cites -1 Cited by

Patent Information

Application Number
PCT/JP2024/012215
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-03-27
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Lithium transition metal compounds with a polyanion structure used in positive electrodes of power storage elements often exhibit low adhesion to the base material, leading to decreased initial output due to low destructive test force, which affects the arrangement and adhesion of active material particles.

Method used

Developing positive electrode active material particles with a lithium transition metal compound having a polyanionic structure and a destructive test force of 3.5 mN or more, potentially incorporating elements like zirconium and niobium, to enhance adhesion and reduce interfacial resistance.

Benefits of technology

The increased destructive test force improves the adhesion between the positive electrode base material and active material particles, resulting in higher initial output and reduced interfacial resistance, thereby enhancing the performance of power storage elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012215_21112024_PF_FP_ABST
    Figure JP2024012215_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Positive electrode active material particles according to one aspect of the present invention contain a lithium transition metal compound having a polyanionic structure, and have a fracture test force of 3.5 mN or more.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material particles, positive electrode active material mixture, positive electrode for energy storage element, energy storage element, and energy storage device

[0001] The present invention relates to positive electrode active material particles, a positive electrode active material mixture, a positive electrode for an electricity storage element, an electricity storage element, and an electricity storage device.

[0002] Due to their high energy density, non-aqueous electrolyte secondary batteries, such as lithium-ion non-aqueous electrolyte secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc. Non-aqueous electrolyte secondary batteries generally include an electrode assembly having a pair of electrodes electrically isolated by a separator, and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring charge-transporting ions between the electrodes. Furthermore, as energy storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium-ion capacitors and electric double layer capacitors, as well as energy storage elements using electrolytes other than non-aqueous electrolytes, are also widely used.

[0003] Lithium transition metal compounds having a polyanion structure, such as lithium iron phosphate, are known as positive electrode active materials used in energy storage devices. Patent Document 1 describes a nonaqueous electrolyte secondary battery including a positive electrode containing lithium iron olivine (lithium iron phosphate) as the positive electrode active material and a negative electrode containing graphite as the negative electrode active material.

[0004] Japanese Patent Application Laid-Open No. 2021-153021

[0005] When positive electrode active material particles containing a lithium transition metal compound having a polyanion structure are used in the positive electrode of a storage element, the initial output of the storage element may be reduced due to poor adhesion between the positive electrode substrate and the positive electrode active material particles.

[0006] The present invention has been made in light of the above circumstances, and has an object to provide positive electrode active material particles that can increase the initial output of an electricity storage element.

[0007] Positive electrode active material particles according to one aspect of the present invention include a lithium transition metal compound having a polyanionic structure and have a breaking test strength of 3.5 mN or more. Positive electrode active material particles according to another aspect of the present invention include a lithium transition metal compound having a polyanionic structure and have a breaking test strength of 4.2 mN or more. Positive electrode active material particles according to another aspect of the present invention include a lithium transition metal compound having a polyanionic structure and at least one of zirconium and niobium, and have a breaking test strength of 3.5 mN or more.

[0008] The positive electrode active material particles according to one aspect of the present invention can increase the initial output of an electricity storage device.

[0009] Fig. 1 is a perspective view showing one embodiment of an electric storage element having positive electrode active material particles according to the present invention, and Fig. 2 is a schematic diagram showing one embodiment of an electric storage device formed by assembling a plurality of electric storage elements having positive electrode active material particles according to the present invention.

[0010] First, an overview of the positive electrode active material particles and other embodiments disclosed in this specification will be described.

[0011] [1] Positive electrode active material particles according to one aspect of the present invention contain a lithium transition metal compound having a polyanion structure and have a breaking test strength of 3.5 mN or more.

[0012] The positive electrode active material particles described in [1] above can increase the initial output of an energy storage device. While the reason for this is unclear, the following is presumed. Conventional positive electrode active material particles, when containing a lithium transition metal compound having a polyanion structure, were prone to deformation and breakage when pressed onto a positive electrode substrate during positive electrode fabrication. This made it difficult to arrange the positive electrode active material particles so that they were embedded into the surface of the positive electrode substrate, which sometimes made it difficult to enhance adhesion between the positive electrode substrate and the positive electrode active material particles. In contrast, the positive electrode active material particles described in [1] above have a fracture test force of 3.5 mN or more and high hardness. Therefore, they are less prone to deformation and breakage when pressed onto a positive electrode substrate, are easily arranged so that they are embedded into the surface of the positive electrode substrate, and facilitate enhanced adhesion between the positive electrode substrate and the positive electrode active material particles. High adhesion between the positive electrode active material particles and the positive electrode substrate can reduce the interfacial resistance between the positive electrode active material particles and the positive electrode substrate. This, in turn, increases the initial output of an energy storage device. In addition, evaluation of particle hardness using destructive test force is considered to be able to appropriately evaluate particle hardness independent of the size of the particles being measured, compared to when using indicators such as the change in particle size when the particles are compressed.

[0013] In the present invention, "having a polyanion structure" means an oxoacid anion (PO 4 3- , SiO 4 4- , B.O. 3 3- etc.)

[0014] In the present invention, the term "breaking test force" refers to the test force at which cracks occur in the positive electrode active material particles when compressed. The breaking test force of the positive electrode active material particles is measured by a microcompression test using a microcompression tester (Shimadzu Corporation's "MCT-511"). A diamond flat indenter with a diameter of 50 μm is used as the probe. The test force is set to 1 mN to 30 mN at a probe speed of 0.134 mN / sec, and pressure is applied to each positive electrode active material particle while changing the test force at a constant rate. The inflection point of the resulting test force-displacement graph is considered to be the point at which cracks occur in the positive electrode active material particles, and the test force at this inflection point is taken as the breaking test force. The breaking test force is measured for five positive electrode active material particles, and the average value is used. The positive electrode active material particles to be measured are selected from particles with a particle size between 1 / 2 and 2 times the average particle size of the positive electrode active material particles. The "particle size" of each particle is taken as the average value of the minor axis and the major axis. The minor axis is the shortest axis passing through the center of the smallest circumscribing circle of a particle, and the major axis is the axis passing through the center and perpendicular to the minor axis. If there are two or more shortest axes, the longest axis perpendicular to the shortest axes is taken as the minor axis. "Average particle size" refers to the value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50%, based on the particle size distribution measured by laser diffraction / scattering in a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).

[0015] When the positive electrode active material particles are incorporated into an energy storage device as a positive electrode active material, the breaking test force is measured on the device in a fully discharged state using the following method. First, the energy storage device is charged at a constant current of 0.05 C until the end-of-charge voltage in normal use is reached, and then fully charged. After a 30-minute rest, the device is discharged at a constant current of 0.05 C until the end-of-charge voltage in normal use (lower limit voltage) is reached. The device is disassembled, the positive electrode is removed, and a test battery is assembled using a metallic lithium electrode as the counter electrode. The positive electrode potential is measured at a current value of 10 mA per 1 g of positive electrode mixture until the positive electrode potential reaches 2.0 V vs. Li / Li. +The positive electrode is adjusted to a fully discharged state by constant current discharge until the positive electrode reaches a fully discharged state. The device is disassembled again and the positive electrode is removed. The electrolyte and other materials adhering to the removed positive electrode are thoroughly washed using dimethyl carbonate, and the device is dried at room temperature for one day and one night, after which the positive electrode active material particles are collected. The collected positive electrode active material particles are subjected to measurement. The operations from disassembling the energy storage device to collecting the positive electrode active material particles are carried out in an argon atmosphere with a dew point of -60°C or below. "During normal use" refers to the case where the energy storage device is used under the charging and discharging conditions recommended or specified for the energy storage device. Regarding charging conditions, for example, if a charger for the energy storage device is provided, this refers to the case where the energy storage device is used using the charger.

[0016] [2] Positive electrode active material particles according to one aspect of the present invention contain a lithium transition metal compound having a polyanion structure and have a breaking strength of 4.2 mN or more.

[0017] The positive electrode active material particles described in the above [2] have a fracture test strength of 4.2 mN or more and high hardness, and therefore, for the same reason as described in the above [1], the interfacial resistance with the positive electrode substrate can be reduced, thereby increasing the initial output of the energy storage device.

[0018] [3] Positive electrode active material particles according to another aspect of the present invention include a lithium transition metal compound having a polyanion structure and at least one of zirconium and niobium, and have a breaking strength of 3.5 mN or more.

[0019] The positive electrode active material particles described in [3] above have a fracture test strength of 3.5 mN or more and high hardness, and therefore can reduce the interfacial resistance with the positive electrode substrate for the same reasons as those described in [1] above. Furthermore, zirconium and niobium act as lithium ion conductors in the form of oxides, etc., and therefore contribute to reducing the interfacial resistance between the positive electrode active material particles and between the positive electrode active material particles and the positive electrode substrate. Therefore, the positive electrode active material particles described in [3] above have a fracture test strength of 3.5 mN or more and contain at least one of zirconium and niobium, thereby synergistically increasing the initial output of the energy storage device.

[0020] [4] A positive electrode active material mixture according to another aspect of the present invention contains the positive electrode active material particles according to any one of [1] to [3] above.

[0021] The positive electrode active material mixture described in [4] above contains the positive electrode active material particles described in any one of [1] to [3] above, and therefore can increase the initial output of the electricity storage device.

[0022] [5] A positive electrode for a storage device according to another aspect of the present invention includes a positive electrode substrate and the positive electrode active material mixture described in [4] above laminated on the positive electrode substrate. The positive electrode active material mixture described in [4] above may be laminated directly on the positive electrode substrate, or may be laminated on the positive electrode substrate via an intermediate layer containing a conductive agent or the like.

[0023] The positive electrode for a storage battery element according to the above [5] contains the positive electrode active material mixture according to the above [4] which contains the positive electrode active material particles, and therefore can increase the initial output of the storage battery element.

[0024] [6] An electric storage device according to another aspect of the present invention includes the electric storage device positive electrode according to [5] above.

[0025] The electric storage device according to the above [6] includes the electric storage device positive electrode according to the above [5] containing the positive electrode active material particles, and therefore has a large initial output.

[0026] [7] A power storage device according to yet another aspect of the present invention includes two or more power storage elements, and includes one or more of the power storage elements described in [6] above.

[0027] The electricity storage device according to the above [7] includes one or more electricity storage elements according to the above [6], and therefore has a large initial output.

[0028] Hereinafter, a cathode active material particle, a cathode active material mixture, a cathode for a storage device, a method for manufacturing a cathode, a storage device, a storage device, a method for manufacturing a storage device, and other embodiments according to one embodiment of the present invention will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.

[0029] [Positive Electrode Active Material Particles] [Configuration of Positive Electrode Active Material Particles A] Positive electrode active material particles A according to one embodiment of the present invention contain a lithium transition metal compound having a polyanion structure. The positive electrode active material particles A have a breaking strength of 3.5 mN or more. The lithium transition metal compound having a polyanion structure is usually used in the form of particles coated with a carbon material from the viewpoint of electronic conductivity, etc. That is, the positive electrode active material particles A according to one embodiment of the present invention may more specifically be particles in which particles containing a lithium transition metal compound having a polyanion structure are coated with a carbon material.

[0030] The lithium transition metal compound having a polyanion structure includes an oxo acid anion (PO 4 3- , S.O. 4 2- , SiO 4 4- , B.O. 3 3- , V.O. 4 3- The oxo acid anion may be a compound containing a condensed anion (P 2 O 7 4- , P 3 O 10 5- The lithium transition metal compound having a polyanion structure may have an olivine-type crystal structure. The lithium transition metal compound having a polyanion structure is typically a polyanion compound containing a lithium element and a transition metal element, and may further contain other elements (for example, halogen elements, etc.). As the transition metal element contained in the lithium transition metal compound having a polyanion structure, iron element, manganese element, nickel element, and cobalt element are preferred, iron element and nickel element are more preferred, and iron element is even more preferred. As the oxo acid anion contained in the lithium transition metal compound having a polyanion structure, phosphate anion (PO 4 3- ) is preferred.

[0031] The lithium transition metal compound having a polyanion structure is preferably a compound represented by the following formula (1): Li a M b (A.O. c ) d X e ... (1) In formula (1), M is at least one transition metal element. A is at least one selected from B, Al, Si, P, S, Cl, Ti, V, Cr, Mo, and W. X is at least one halogen element. a, b, c, d, and e are numbers satisfying 0<a≦3, 0<b≦2, 2≦c≦4, 1≦d≦3, and 0≦e≦1. a, b, c, d, and e may all be integers or decimals.

[0032] As M in formula (1), any one of Fe, Mn, Ni, and Co, or a combination of any two of them, is preferable. As M, Fe, Mn, or a combination thereof is more preferable, and Fe is more preferable. Furthermore, the content of Fe in M ​​is preferably 50 mol% or more, more preferably 70 mol% or more, 90 mol% or more, or 99 mol% or more. As A, P is preferable. As X, F is preferable. In one embodiment, a = 1, b = 1, c = 4, d = 1, and e = 0 may be preferable.

[0033] Specific examples of lithium transition metal compounds having a polyanion structure include LiFePO 4 , LiCoPO 4 , LiFe 0.5 Co 0.5 P.O. 4 , LiMnPO 4 , LiNiPO 4 , LiMn 0.5 Fe 0.5 P.O. 4 , LiCrPO 4 , LiFeVO 4 , Li 2 FeSiO 4 , Li 2 Fe 2 (SO 4 ) 3 , LiFeBO 3 , LiFePO 3.9 F0.2 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 F. Atoms or polyanions in these lithium transition metal compounds having a polyanion structure may be partially substituted with other atoms or anion species. The lithium transition metal compounds having a polyanion structure may be used alone or in combination of two or more.

[0034] The content of the lithium transition metal compound having a polyanion structure in the particles containing the lithium transition metal compound having a polyanion structure may be 60% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, or 99% by mass or more.

[0035] The particles containing the lithium transition metal compound having a polyanion structure may be single particles in which a plurality of primary particles are present independently without aggregation, but are preferably secondary particles formed by aggregation of a plurality of primary particles, such as secondary particles of the lithium transition metal compound having a polyanion structure.

[0036] In one embodiment of the present invention, particles containing a lithium transition metal compound having a polyanion structure are coated with a carbon material to form positive electrode active material particles A. A portion of the carbon material may be present inside the particles containing the lithium transition metal compound having a polyanion structure. The positive electrode active material particles A may have portions that are not coated with the carbon material (for example, portions where the lithium transition metal compound having a polyanion structure is exposed).

[0037] The carbon material coats the particles containing a lithium transition metal compound having a polyanion structure, allowing the positive electrode active material particles A to exhibit sufficient electron conductivity between particles. The carbon material is, for example, an inorganic material with a carbon element content of 80% by mass or more and 100% by mass or less. The carbon element content in the carbon material may be 90% by mass or more, or may be 95% by mass or more. Elements other than carbon that may be contained in the carbon material include oxygen, hydrogen, and nitrogen. Examples of the carbon material include graphite and non-graphitic carbon.

[0038] The content of the carbon material in the positive electrode active material particles A is preferably 0.1% by mass or more and 20% by mass or less, more preferably 0.2% by mass or more and 10% by mass or less, even more preferably 0.3% by mass or more and 5% by mass or less, and even more preferably 0.5% by mass or more and 2% by mass or less. When the content of the carbon material in the positive electrode active material particles A is equal to or greater than the above lower limit, it is possible to increase electronic conductivity, etc. When the content of the carbon material in the positive electrode active material particles A is equal to or less than the above upper limit, it is possible to increase the content of the lithium transition metal compound having a polyanion structure, and it is possible to increase the discharge capacity per volume of a positive electrode using the positive electrode active material particles A, etc.

[0039] The total content of the lithium transition metal compound having a polyanion structure and the carbon material in the positive electrode active material particles A is preferably 90% by mass or more and 100% by mass or less, and may be 95% by mass or more, 98% by mass or more, 99% by mass or more, or 99.9% by mass or more.

[0040] As described above, the lower limit of the breaking test force of the positive electrode active material particles A is 3.5 mN, preferably 4.2 mN, more preferably 6.0 mN, even more preferably 8.0 mN, and even more preferably 8.5 mN. When the breaking test force is equal to or greater than the lower limit, the adhesion of the positive electrode active material particles A to the positive electrode substrate can be improved when pressed onto the positive electrode substrate. This also increases the initial output of the energy storage device. On the other hand, from the viewpoint of manufacturability, the upper limit of the breaking test force of the positive electrode active material particles A is preferably 30 mN, more preferably 25 mN, and even more preferably 20 mN. The breaking test force of the positive electrode active material particles A may be equal to or greater than any of the lower limits and equal to or less than any of the upper limits. In addition, when an intermediate layer containing a conductive agent or the like is formed on the positive electrode substrate of the energy storage device, the positive electrode active material particles A may be pressed onto the positive electrode substrate via the intermediate layer. In this case, the adhesion of the positive electrode active material particles A to the intermediate layer or the positive electrode substrate can be improved when pressed onto the positive electrode substrate via the intermediate layer.

[0041] The average particle size of the positive electrode active material particles A is preferably 0.5 μm or more and 30 μm or less, more preferably 1 μm or more and 25 μm or less, even more preferably 2 μm or more and 20 μm or less, even more preferably 4 μm or more and 15 μm or less, and even more preferably 6 μm or more and 12 μm or less. When the average particle size of the positive electrode active material particles A is within the above range, the contact area with the positive electrode substrate or the intermediate layer described above can be increased, thereby increasing the initial output of the energy storage device. Furthermore, when the average particle size of the positive electrode active material particles A is within the above range, the electrode density and output density of the positive electrode using the positive electrode active material particles A can be increased. To obtain the positive electrode active material particles A with a predetermined average particle size, a pulverizer, a classifier, or the like is used. Examples of pulverization methods include methods using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow jet mill, or a sieve. Wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, or the like may be used as needed for both dry and wet classification.

[0042] From the viewpoint of increasing the contact area with the positive electrode substrate or the intermediate layer, the positive electrode active material particles A are preferably spherical. From the same viewpoint, the average aspect ratio of the positive electrode active material particles A is preferably 1.0 to 1.5, more preferably 1.0 to 1.4, and even more preferably 1.0 to 1.2. The "average aspect ratio" is determined as the arithmetic mean value of the T / Y value, which is the ratio of the longest major axis T of the positive electrode active material particles A to the longest minor axis Y in the direction perpendicular to the longest axis T, averaged over 10 positive electrode active material particles A in a cross-sectional SEM image of the positive electrode containing the positive electrode active material particles A. A JSM-7001F (manufactured by JEOL Ltd.) scanning electron microscope was used to obtain the cross-sectional SEM image of the positive electrode. The cross-sectional SEM image was obtained by observing a secondary electron image. The acceleration voltage was 5 kV. The observation magnification was set so that 3 to 15 positive electrode active material particles A appeared in one field of view. The cross-sectional SEM image obtained is saved as an image file. Other conditions such as spot diameter, working distance, irradiation current, brightness, and focus are appropriately set so that the contours of the positive electrode active material particles A are clearly visible.

[0043] [Configuration of Positive Electrode Active Material Particles B] Positive electrode active material particles B according to one embodiment of the present invention contain a lithium transition metal compound having a polyanion structure and at least one of zirconium and niobium. The breaking strength of the positive electrode active material particles B is 3.5 mN or more. Like the positive electrode active material particles A, the positive electrode active material particles B according to one embodiment of the present invention are granular materials in which particles containing a lithium transition metal compound having a polyanion structure are coated with a carbon material.

[0044] The lithium transition metal compound having a polyanion structure, the carbon material, and the contents thereof in the positive electrode active material particles B can be the same as those described above for the positive electrode active material particles A. The average particle size and average aspect ratio of the positive electrode active material particles B can also be the same as those of the positive electrode active material particles A.

[0045] The lower limit of the breaking test force of the positive electrode active material particles B is 3.5 mN as described above, preferably 4.0 mN, more preferably 6.0 mN, and even more preferably 8.0 mN. When the breaking test force is equal to or greater than the lower limit, the adhesion of the positive electrode active material particles B to the positive electrode substrate or the intermediate layer described above can be improved when the positive electrode active material particles B are pressed onto the positive electrode substrate. This also increases the initial output of the energy storage device. On the other hand, from the viewpoint of manufacturability, the upper limit of the breaking test force of the positive electrode active material particles B is preferably 30 mN, more preferably 25 mN, and even more preferably 20 mN. The breaking test force of the positive electrode active material particles B may be equal to or greater than any of the lower limits described above and equal to or less than any of the upper limits described above.

[0046] In one embodiment of the present invention, the positive electrode active material particles B contain at least one of zirconium and niobium. Furthermore, the positive electrode active material particles B preferably contain at least zirconium. At least one of zirconium and niobium contributes to reducing the interfacial resistance between the positive electrode active material particles B and between the positive electrode active material particles B and the positive electrode substrate. That is, the positive electrode active material particles B have a fracture strength of 3.5 mN or more, and the positive electrode active material particles B contain at least one of zirconium and niobium, thereby synergistically increasing the initial output of the energy storage device. Examples of the form of the zirconium and niobium elements in the positive electrode active material particles B include zirconium oxide and niobium oxide, and may be, for example, zirconium oxide and niobium oxide.

[0047] The zirconium element and the niobium element are preferably present on the outermost surface of the positive electrode active material particles B, and in this embodiment, are preferably present on the surface of the carbon material. However, a portion of the zirconium element and the niobium element may be present inside the carbon material, at the boundary between the carbon material and the particles containing the lithium transition metal compound having a polyanion structure, or inside the particles containing the lithium transition metal compound having a polyanion structure.

[0048] The total content of zirconium and niobium in the positive electrode active material particles B is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.2% by mass or more and 3% by mass or less, even more preferably 0.3% by mass or more and 1% by mass or less, and even more preferably 0.5% by mass or more and 1% by mass or less. When the total content of zirconium and niobium in the positive electrode active material particles B is equal to or greater than the above lower limit, the interfacial resistance between the positive electrode active material particles B and the positive electrode substrate can be reduced. Furthermore, when the total content of zirconium and niobium in the positive electrode active material particles B is equal to or less than the above upper limit, the content of the lithium transition metal compound having a polyanion structure can be increased, and the discharge capacity per volume of the energy storage device can be increased, for example.

[0049] [Method for producing positive electrode active material particles A and B] The positive electrode active material particles A and B according to one embodiment of the present invention can be efficiently obtained by adjusting the pH of the reaction solution using aqueous ammonia or the like when producing the hydroxide precursor in a method using a hydroxide precursor, a lithium source, and a carbon source. By using such a production method, spherical positive electrode active material particles A and B with high hardness can be obtained. The production method will be described in detail below. However, the positive electrode active material particles A and B according to the present invention are not limited to those produced by the following production method.

[0050] First, a hydroxide precursor is obtained by a precipitation reaction between transition metal ions and hydroxide ions in water. Specifically, for example, a transition metal salt aqueous solution and a sodium hydroxide aqueous solution are dropped into water to obtain a hydroxide precursor (a transition metal hydroxide). The transition metal salt may be any water-soluble salt containing the transition metal element that constitutes the desired lithium transition metal compound, such as iron sulfate, iron chloride, cobalt sulfate, manganese sulfate, or nickel sulfate. Alternatively, a potassium hydroxide aqueous solution may be used instead of the sodium hydroxide aqueous solution. When the transition metal salt aqueous solution and the sodium hydroxide aqueous solution are dropped into water, an ammonia aqueous solution or the like is further dropped into the reaction solution to maintain the pH of the water (reaction solution) into which these aqueous solutions are dropped within a predetermined range. The pH of the reaction solution is preferably in the range of 8.5 to 11.6. If the pH of the reaction solution is outside the above range, or if an aqueous ammonia solution or the like is not added dropwise to the reaction solution even if the pH of the reaction solution is within the above range, the amount of change in particle size when pressurized of the finally obtained positive electrode active material particles tends to be large, that is, the breaking strength of the positive electrode active material particles tends to be small. 3 1mol / dm or more 3 The pH of the reaction solution can be adjusted to about 100% or less. The pH of the reaction solution can be adjusted by adjusting the concentrations, amounts, etc. of the aqueous ammonia solution and the aqueous sodium hydroxide solution to be added dropwise. Another alkaline aqueous solution such as an aqueous hydrazine solution may be added dropwise together with the aqueous ammonia solution. The pH of the reaction solution can also be adjusted by the amount, etc., of the other alkaline aqueous solution added.

[0051] Next, the obtained hydroxide precursor, a lithium source, and a carbon source are mixed and baked in an inert atmosphere (for example, a nitrogen atmosphere), thereby obtaining positive electrode active material particles A according to one embodiment of the present invention. 2 P.O. 4 , Li 3 P.O. 4 , LiHSO 4Compounds having a polyanion structure such as those described above and containing lithium element can be suitably used. Other lithium sources that can be used include LiOH, lithium halide, etc. When the lithium source used is not a compound having a polyanion structure, a compound having a polyanion structure is further mixed and then calcined. Examples of compounds having a polyanion structure include NH 4 H 2 P.O. 4 , (NH 4 ) 3 P.O. 4 , (NH 4 ) 2 HPO 4 , (NH 4 ) 2 SO 4 , N.H. 4 VO 3 Suitable examples of the carbon source include organic substances such as sucrose, lactose, maltose, sucrose, polyvinyl alcohol, and ascorbic acid. The baking temperature can be, for example, 500°C or higher and 800°C or lower.

[0052] In the case of producing the positive electrode active material particles B, a raw material containing at least one of zirconium and niobium is added in addition to the hydroxide precursor, lithium source, and carbon source during the calcination. Examples of the raw material containing at least one of zirconium and niobium include zirconium metal powder and niobium metal powder.

[0053] [Positive Electrode Active Material Mixture] A positive electrode active material mix according to one embodiment of the present invention contains positive electrode active material particles A or positive electrode active material particles B. The positive electrode active material mix may contain optional components such as a positive electrode active material other than the positive electrode active material particles A and the positive electrode active material particles B, a conductive agent, a binder (binding agent), a thickener, a filler, etc., as needed.

[0054] The positive electrode active material particles A or positive electrode active material particles B contained in the positive electrode active material mixture can be the same as those described above as the positive electrode active material particles A or positive electrode active material particles B according to one embodiment of the present invention.

[0055] As the positive electrode active material other than the positive electrode active material particles A and the positive electrode active material particles B, various conventionally known positive electrode active materials can be used. However, the content of the positive electrode active material particles A or the positive electrode active material particles B relative to all the positive electrode active materials contained in the positive electrode active material layer (the total of the positive electrode active material particles A or the positive electrode active material particles B and the other positive electrode active materials) is preferably 90 mass% or more, more preferably 99 mass% or more, and even more preferably 100 mass%. By thus configuring the positive electrode active material substantially only from the positive electrode active material particles A or the positive electrode active material particles B, the initial output of the energy storage element can be further increased.

[0056] The conductive agent is not particularly limited as long as it is a material having electrical conductivity. Examples of such conductive agents include carbon materials, metals, conductive ceramics, etc. Examples of carbon materials include graphite, non-graphitic carbon, graphene-based carbon, etc. Examples of non-graphitic carbon include carbon nanofiber, pitch-based carbon fiber, carbon black, etc. Examples of carbon black include furnace black, acetylene black, ketjen black, etc. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, etc. The conductive agent may be in the form of powder, fiber, etc. As the conductive agent, one of these materials may be used alone, or two or more may be mixed and used. These materials may also be used in combination. For example, a composite material of carbon black and CNT may be used. Among these, carbon black is preferred from the viewpoints of electronic conductivity and coatability, and acetylene black is particularly preferred.

[0057] The content of the conductive agent in the positive electrode active material mixture is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By setting the content of the conductive agent within the above range, the energy density, etc. of the energy storage device can be increased. Note that the content of the conductive agent does not include the carbon material contained in the positive electrode active material particles A or the positive electrode active material particles B (the carbon material coating the particles containing the lithium transition metal compound having a polyanion structure).

[0058] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.

[0059] The content of the binder in the positive electrode active material mixture is preferably 1% by mass to 10% by mass, more preferably 3% by mass to 9% by mass. By setting the binder content within this range, the positive electrode active material can be stably maintained.

[0060] Examples of thickeners include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose. When the thickener has a functional group that reacts with lithium or the like, the functional group may be deactivated in advance by methylation or the like. When a thickener is used, the content of the thickener in the positive electrode active material mixture can be, for example, 0.1% by mass or more and 8% by mass or less, and can also be 5% by mass or less, or 1% by mass or less.

[0061] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof. When a filler is used, the content of the filler in the positive electrode active material mixture can be, for example, 0.1% by mass or more and 8% by mass or less, and can also be 5% by mass or less or 1% by mass or less.

[0062] The positive electrode active material mixture may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material particles A, the positive electrode active material particles B, other positive electrode active materials, the conductive agent, the binder, the thickener, and the filler.

[0063] [Positive electrode for energy storage device] A positive electrode for an energy storage device (hereinafter also referred to as "positive electrode") according to one embodiment of the present invention has a positive electrode substrate and a positive electrode active material mixture laminated on the positive electrode substrate directly or via an intermediate layer. The positive electrode active material mixture laminated on the positive electrode substrate forms a positive electrode active material layer. The positive electrode active material mixture contained in the positive electrode can be the same as that described above as the positive electrode active material mixture according to one embodiment of the present invention.

[0064] The positive electrode substrate has electrical conductivity. Whether or not it has electrical conductivity is determined by whether or not the volume resistivity measured in accordance with JIS-H-0505 (1975) is 10 -2 The resistance is determined using Ω cm as a threshold value. Metals such as aluminum, titanium, tantalum, and stainless steel, or alloys thereof, are used as the material for the positive electrode substrate. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high conductivity, and cost. Examples of the positive electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, and A1N30, as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).

[0065] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate and also increase the energy density per volume of the energy storage element.

[0066] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer (positive electrode active material mixture). The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may include, for example, a binder and a conductive agent.

[0067] [Method for Manufacturing Positive Electrode] A method for manufacturing a positive electrode includes, for example, preparing a positive electrode mixture paste containing a positive electrode active material mixture and a dispersion medium, applying the positive electrode mixture paste directly or via an intermediate layer to at least one surface of a positive electrode substrate, drying the positive electrode mixture paste, and pressing the positive electrode active material mixture. An organic solvent is preferably used as the dispersion medium used in preparing the positive electrode mixture paste, and examples of the organic solvent include N-methylpyrrolidone (NMP) and toluene. Furthermore, by pressing, it is preferable that at least a portion of the positive electrode active material particles A or positive electrode active material particles B in the positive electrode active material mixture be disposed so as to be embedded in the positive electrode substrate or intermediate layer.

[0068] [Electricity storage element] An electric storage element according to one embodiment of the present invention includes an electrode assembly having a positive electrode, a negative electrode, and a separator, an electrolyte, and a container that accommodates the electrode assembly and the electrolyte. The electrode assembly is typically a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked with separators interposed therebetween, or a wound type in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound. The electrolyte is present in a state contained in the positive electrode, the negative electrode, and the separator. The electrolyte may be a nonaqueous electrolyte. As an example of an electric storage element, a nonaqueous electrolyte secondary battery (hereinafter also simply referred to as a "secondary battery") in which the electrolyte is a nonaqueous electrolyte will be described.

[0069] [Positive Electrode] The positive electrode included in the electricity storage element can be the same as that described above as the positive electrode according to one embodiment of the present invention.

[0070] [Negative electrode] The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode above, for example.

[0071] The negative electrode substrate is conductive. Metals such as copper, nickel, stainless steel, nickel-plated steel, and aluminum, or alloys thereof, carbon materials, and the like are used as the material for the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.

[0072] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, even more preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and also increase the energy density per volume of the energy storage element.

[0073] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, and a filler, as needed. The optional components such as the conductive agent, the binder, the thickener, and the filler can be selected from the materials exemplified for the positive electrode above.

[0074] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0075] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for a lithium ion secondary battery. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li 4 Ti 5 O 12 , LiTiO 2、 TiNb 2 O 7Examples of the material include titanium-containing oxides such as titanium dioxide, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitizable carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more may be used in combination.

[0076] "Graphite" refers to a graphite material that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of being able to obtain a material with stable physical properties.

[0077] "Non-graphitic carbon" refers to a carbon having an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.

[0078] Here, the "discharged state" refers to a state in which the battery is discharged so that lithium ions capable of being absorbed and desorbed during charging and discharging are sufficiently released from the carbon material serving as the negative electrode active material. For example, this refers to a state in which the open circuit voltage of a half cell using a negative electrode containing a carbon material as the negative electrode active material as the working electrode and metallic Li as the counter electrode is 0.7 V or higher.

[0079] "Non-graphitizable carbon" refers to the above-mentioned d 002 The term "carbon material" refers to a carbon material having a particle size of 0.36 nm or more and 0.42 nm or less.

[0080] "Graphitizable carbon" refers to the above-mentioned d 002 The term "carbon material" refers to a carbon material having a particle size of 0.34 nm or more and less than 0.36 nm.

[0081] The negative electrode active material is usually in the form of particles (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is a carbon material, a titanium-containing oxide, or a polyphosphate compound, the average particle size may be 1 μm or more and 100 μm or less. When the negative electrode active material is Si, Sn, Si oxide, Sn oxide, or the like, the average particle size may be 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to be equal to or greater than the above lower limit, the production or handling of the negative electrode active material becomes easy. By setting the average particle size of the negative electrode active material to be equal to or less than the above upper limit, the electronic conductivity of the negative electrode active material layer is improved. A pulverizer, a classifier, or the like is used to obtain powder with a predetermined particle size. When the negative electrode active material is a metal such as metallic Li, the negative electrode active material layer may be in the form of a foil.

[0082] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% by mass to 99% by mass, more preferably 90% by mass to 98% by mass. By setting the content of the negative electrode active material within this range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.

[0083] [Separator] The separator can be appropriately selected from known separators. Examples of separators that can be used include separators consisting of only a substrate layer and separators in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer. Examples of the shape of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these shapes, porous resin films are preferred from the viewpoint of strength, and nonwoven fabrics are preferred from the viewpoint of non-aqueous electrolyte retention. Materials for the substrate layer of the separator are preferably polyolefins such as polyethylene and polypropylene from the viewpoint of shutdown function, and polyimide and aramid from the viewpoint of oxidative decomposition resistance. A composite material of these resins may also be used for the substrate layer of the separator.

[0084] The heat-resistant particles contained in the heat-resistant layer preferably exhibit a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably exhibit a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials exhibiting a mass loss of a predetermined value or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon and diamond; mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, as well as artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be used in combination. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the energy storage device.

[0085] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.

[0086] The separator may be a polymer gel composed of a polymer and a non-aqueous electrolyte. Examples of polymers include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. The use of a polymer gel has the effect of suppressing leakage. The separator may be a combination of the porous resin film or nonwoven fabric described above and a polymer gel.

[0087] [Non-aqueous electrolyte] The non-aqueous electrolyte can be appropriately selected from known non-aqueous electrolytes. The non-aqueous electrolyte may be a non-aqueous electrolyte solution. The non-aqueous electrolyte solution contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.

[0088] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of non-aqueous solvents include cyclic carbonates, chain carbonates, carboxylic acid esters, phosphate esters, sulfonic acid esters, ethers, amides, and nitriles. Non-aqueous solvents in which some of the hydrogen atoms contained in these compounds have been substituted with halogens may also be used.

[0089] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Of these, EC is preferred.

[0090] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferred.

[0091] It is preferable to use a cyclic carbonate or a chain carbonate as the non-aqueous solvent, and it is more preferable to use a cyclic carbonate and a chain carbonate in combination. The use of a cyclic carbonate can promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. The use of a chain carbonate can reduce the viscosity of the non-aqueous electrolyte. When a cyclic carbonate and a chain carbonate are used in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is preferably in the range of, for example, 5:95 to 50:50.

[0092] The electrolyte salt can be appropriately selected from known electrolyte salts, such as lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts. Of these, lithium salts are preferred.

[0093] The lithium salt is LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 , LiN(SO 2 F) 2 inorganic lithium salts such as lithium oxalate salts, lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); 3 CF 3 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) (SO 2 C 4 F 9 ), LiC(SO 2 CF 3 ) 3 , LiC(SO 2 C 2 F 5 ) 3 Among these, inorganic lithium salts are preferred, and LiPF 6 is more preferred.

[0094] The content of the electrolyte salt in the non-aqueous electrolyte solution is 0.1 mol / dm at 20°C and 1 atmosphere. 3 2.5mol / dm or more 3 It is preferably 0.3 mol / dm or less. 3 2.0mol / dm or more 3 It is more preferable that it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3It is more preferable that it is 0.7 mol / dm or less. 3 1.5mol / dm or more 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the non-aqueous electrolyte can be increased.

[0095] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of the additives include halogenated carbonates such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC); oxalates such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, and silyl. Aromatic compounds such as cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, and the like. Carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1 ,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, etc. These additives may be used alone or in combination of two or more.

[0096] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass, based on the total mass of the non-aqueous electrolyte. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and further improve safety.

[0097] The non-aqueous electrolyte may be a solid electrolyte, or a non-aqueous electrolytic solution and a solid electrolyte may be used in combination.

[0098] The solid electrolyte can be selected from any material that has ionic conductivity of lithium, sodium, calcium, etc. and is solid at room temperature (e.g., 15° C. to 25° C.) Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.

[0099] As the sulfide solid electrolyte, in the case of a lithium ion secondary battery, for example, Li 2 S-P 2 S 5 , LiI-Li 2 S-P 2 S 5 , Li 10 Ge-P 2 S 12 etc.

[0100] The shape of the energy storage element of this embodiment is not particularly limited, and examples thereof include a cylindrical battery, a prismatic battery, a flat battery, a coin battery, and a button battery.

[0101] FIG. 1 shows an energy storage element 1 as an example of a prismatic battery. Note that this figure is a see-through view of the inside of the container. An electrode assembly 2 having a positive electrode and a negative electrode wound with a separator sandwiched between them is housed in a prismatic container 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51.

[0102] [Electricity Storage Device] The energy storage element of the present embodiment can be mounted as an energy storage unit (battery module) configured by assembling a plurality of energy storage elements in an automobile power source such as an electric vehicle (EV), a hybrid electric vehicle (HEV), or a plug-in hybrid electric vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source, etc. In this case, it is sufficient that the technology of the present invention is applied to at least one energy storage element included in the energy storage unit.

[0103] An energy storage device according to one embodiment of the present invention includes two or more energy storage elements, and includes one or more energy storage elements according to one embodiment of the present invention described above (hereinafter referred to as the "second embodiment"). It is sufficient that the technology according to one embodiment of the present invention is applied to at least one energy storage element included in the energy storage device according to the second embodiment, and the energy storage device may include one energy storage element according to one embodiment of the present invention described above and one or more energy storage elements not according to one embodiment of the present invention described above, or may include two or more energy storage elements according to one embodiment of the present invention described above.

[0104] 2 shows an example of a power storage device 30 according to a second embodiment in which power storage units 20, each of which is a collection of two or more electrically connected power storage elements 1, are further assembled. The power storage device 30 may include a bus bar (not shown) that electrically connects two or more power storage elements 1, a bus bar (not shown) that electrically connects two or more power storage units 20, etc. The power storage unit 20 or the power storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more power storage elements.

[0105] [Method for Manufacturing Energy Storage Element] The method for manufacturing the energy storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode assembly, preparing an electrolyte, and housing the electrode assembly and the electrolyte in a container. Preparing the electrode assembly includes preparing a positive electrode and a negative electrode, and forming the electrode assembly by stacking or winding the positive electrode and the negative electrode with a separator interposed therebetween.

[0106] The method for placing the electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the electrolyte, the non-aqueous electrolyte solution may be poured into the container through an inlet formed in the container, and the inlet may then be sealed.

[0107] [Other Embodiments] The positive electrode active material particles, positive electrode active material mixture, positive electrode for a storage element, storage element, and storage device of the present invention are not limited to the above-described embodiments, and various modifications may be made without departing from the spirit of the present invention. For example, the configuration of one embodiment can be added to the configuration of another embodiment, and part of the configuration of one embodiment can be replaced with the configuration of another embodiment or well-known technology. Furthermore, part of the configuration of one embodiment can be deleted. Also, well-known technology can be added to the configuration of one embodiment.

[0108] In the above embodiment, the case where the energy storage element is used as a chargeable and dischargeable non-aqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) has been described, but the type, shape, size, capacity, etc. of the energy storage element are arbitrary. The present invention can also be applied to various secondary batteries and capacitors such as electric double layer capacitors and lithium ion capacitors. The energy storage element of the present invention may be an energy storage element other than a non-aqueous electrolyte energy storage element.

[0109] In the above embodiment, the electrode assembly in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode assembly may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode.

[0110] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0111] [Example 1] (Preparation of Positive Electrode Active Material Particles) Positive electrode active material particles in which secondary particles of lithium iron phosphate were coated with a carbon material were obtained by the following procedure. 3 2 dm 3 1 mol / dm 3 FeSO 4The aqueous solution was added dropwise at a constant rate while adjusting the concentration of the solution to 4 mol / dm3 so that the pH of the reaction solution was kept constant at 11.0±0.1. 3 and 0.75 mol / dm 3 NH 3 aqueous solution and 0.5 mol / dm 3 NH 2 NH 2 The aqueous solution was added dropwise to Fe(OH) 2 The temperature of the reaction vessel was set at 50°C ± 2°C. Next, the prepared Fe(OH) 2 The precursor is removed from the reaction vessel and the Fe(OH) 2 LiH per 100 parts by mass of precursor 2 P.O. 4 The resulting mixture was solid-phase mixed with 116 parts by mass of sucrose powder and 10 parts by mass of sucrose powder. The resulting mixture was baked at a baking temperature of 650°C in a nitrogen atmosphere to obtain LiFePO, a lithium transition metal compound having a polyanion structure. 4 The positive electrode active material particles of Example 1 were obtained by coating the particles with a carbon material. The content of the carbon material in the obtained positive electrode active material particles of Example 1 was 1.0 mass%. The average particle size of the positive electrode active material particles of Example 1 measured by the above method was 10 μm. The breaking test force of the positive electrode active material particles of Example 1 measured by the above method was 4.2 mN.

[0112] (Preparation of Positive Electrode) A positive electrode mixture paste was prepared using the obtained positive electrode active material particles, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium. The mass ratio of the positive electrode active material particles, AB, and PVDF was 90:5:5 in terms of solid content. This positive electrode mixture paste was applied to an aluminum foil as a positive electrode substrate, dried, and roll-pressed to form a positive electrode active material layer (positive electrode active material mixture), thereby obtaining the positive electrode of Example 1.

[0113] (Preparation of Negative Electrode) A negative electrode mixture paste was prepared by mixing graphite as a negative electrode active material, styrene-butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a dispersion medium. The mass ratio of graphite to SBR to CMC was 96:3.3:0.7 in terms of solid content. This negative electrode mixture paste was applied to copper foil as a negative electrode substrate, dried, and roll-pressed to form a negative electrode active material layer, thereby obtaining a negative electrode.

[0114] (Non-aqueous electrolyte) A solvent containing ethylene carbonate (EC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC) mixed in a volume ratio of 30:35:35 was added to a 1.1 mol / dm 3 At a concentration of LiPF 6 was dissolved to obtain a non-aqueous electrolyte.

[0115] (Separator) A polyethylene microporous film was used as the separator.

[0116] (Assembly of Energy Storage Element) The positive electrode, negative electrode, and separator were stacked to prepare an electrode assembly. The obtained electrode assembly was placed in a container, and the non-aqueous electrolyte was then poured into the container, followed by sealing, to obtain the energy storage element of Example 1.

[0117] [Examples 2 to 5, Comparative Examples 1 and 2] In the preparation of positive electrode active material particles, Fe(OH) 2 The positive electrode active material particles, positive electrodes, and energy storage devices of Examples 2 to 5 and Comparative Examples 1 and 2 were obtained in the same manner as in Example 1, except that the reaction solution used to produce the precursor was adjusted to maintain a pH value (±0.1) shown in Table 1. The pH of the reaction solution was adjusted by changing the amount of each aqueous solution added. The carbon material content of each of the obtained positive electrode active material particles was 1.0 mass%. The average particle size of each positive electrode active material particle measured by the above method was 10 μm. The fracture test strength of each positive electrode active material particle measured by the above method is shown in Table 1.

[0118] [Examples 6 to 11 and Comparative Examples 3 to 5] In the preparation of positive electrode active material particles, Fe(OH) 2The positive electrode active material particles, positive electrodes, and energy storage devices of Examples 6 to 11 and Comparative Examples 3 to 5 were obtained in the same manner as in Example 1, except that the reaction solution used to produce the precursor was adjusted to maintain a pH value (±0.1) shown in Table 1, and raw materials containing the additive elements shown in Table 1 were added to the mixture obtained by solid-state mixing so that the additive elements were contained in an amount of 1 mass %. The raw materials containing the additive elements described above were all oxides, and are shown in parentheses in the "Additive Element" column in Table 1. The carbon material content of the obtained positive electrode active material particles was 1.0 mass %. The average particle size of each positive electrode active material particle measured by the above method was 10 μm. The fracture test strength of each positive electrode active material particle measured by the above method is shown in Table 1.

[0119] [Evaluation] (Initial Charge / Discharge) Each of the obtained energy storage elements was initially charged and discharged at 25°C in the following manner. Constant-current, constant-voltage charging was performed with a charging current of 0.2 C and a charge cut-off voltage of 3.5 V. The charge was terminated until the charging current reached 0.01 C. A rest period of 10 minutes was then provided. Subsequently, constant-current discharging was performed with a discharging current of 0.2 C and a discharge cut-off voltage of 2.0 V.

[0120] (Initial Capacity Confirmation Test) Next, an initial capacity confirmation test was performed on each energy storage element at 25°C in the following manner. Constant current / constant voltage charging was performed with a charging current of 1.0 C and a charge cut-off voltage of 3.5 V. The charge was terminated until the charging current reached 0.01 C. A rest period of 10 minutes was then provided. Subsequently, constant current discharging was performed with a discharging current of 1.0 C and a discharge cut-off voltage of 2.0 V. The discharge capacity at this time was defined as the "initial discharge capacity." The fully charged state based on the initial discharge capacity was defined as 100% SOC (State of Charge).

[0121] (Initial Output Verification Test) After the initial capacity verification test, each storage element was subjected to constant current charging at a charging current of 0.2 C in a thermostatic chamber at 25°C until the SOC reached 50%. The charge termination condition was set to a total charging time of 2.5 hours. Next, the element was discharged for 60 seconds at discharge currents of 0.2 C, 0.5 C, and 1.0 C. After each discharge, a 10-minute rest period was provided, followed by supplemental charging at a charging current of 0.2 C until the SOC reached 50%. From the current-voltage characteristic graph obtained by plotting the voltage 10 seconds after the start of each discharge on the vertical axis and the discharge current on the horizontal axis, the output [W] at 10 seconds was determined using the IV method with a lower limit voltage of 2.0 V, and this was taken as the initial output at 25°C. The results are shown in Table 1.

[0122]

[0123] As shown in Table 1, Examples 1 to 5, which did not contain zirconium element and had a fracture test force of 4.2 mN or more, had higher initial outputs (initial outputs at 25°C) than Comparative Examples 1 and 2, which did not contain zirconium element and had a fracture test force of less than 4.2 mN. Furthermore, Examples 6 to 11, which contained zirconium element and had a fracture test force of 3.5 mN or more, had higher initial outputs than Comparative Example 3, which contained zirconium element and had a fracture test force of less than 3.5 mN. Comparative Examples 4 and 5, which contained aluminum element and boron, respectively, had lower initial outputs than Example 6, which contained zirconium element. These results suggest that the high fracture test force of the positive electrode active material particles reduces the interfacial resistance between the positive electrode substrate and the positive electrode active material particles, and that the addition of zirconium element promotes the reduction in interfacial resistance.

[0124] The present invention can be applied to electric storage elements used as power sources for electronic devices such as personal computers and communication terminals, and automobiles.

[0125] REFERENCE SIGNS LIST 1 Energy storage element 2 Electrode body 3 Container 4 Positive electrode terminal 41 Positive electrode lead 5 Negative electrode terminal 51 Negative electrode lead 20 Energy storage unit 30 Energy storage device

Claims

1. Positive electrode active material particles containing a lithium transition metal compound having a polyanion structure, the particles having a breaking test force of 3.5 mN or more.

2. The positive electrode active material particles according to claim 1, which have a breaking test strength of 4.2 mN or more.

3. The positive electrode active material particles according to claim 1, further comprising at least one of zirconium and niobium.

4. A positive electrode active material mixture containing the positive electrode active material particles according to claim 2 or 3.

5. A positive electrode for a storage battery element, comprising a positive electrode substrate and the positive electrode active material mixture according to claim 4 laminated on the positive electrode substrate.

6. An electric storage element comprising the positive electrode for an electric storage element according to claim 5.

7. A power storage device comprising two or more power storage elements, the power storage device comprising one or more of the power storage elements according to claim 6.

Citation Information

Patent Citations

  • Non-aqueous electrolyte secondary battery

    JP2021153021A

  • Aggregated granular lithium multiple oxide, its production and lithium secondary battery

    JP2001080920A

  • Electrode material, electrode paste for lithium ion battery, electrode for lithium ion battery, and lithium ion battery

    JP2014060142A

  • Positive electrode material for lithium ion secondary battery, method of producing the same, electrode for lithium ion secondary battery, and lithium ion secondary battery

    JP2019160550A

  • Positive electrode for power storage element and power storage element

    JP2022075345A