Power storage element and power storage device

By using lithium transition metal compound particles with a polyanionic structure and high destructive test force, and a low-deformation-rate separator, the power storage element achieves improved initial output and sustained capacity retention through enhanced adhesion and reduced deformation, addressing the issues of low adhesion and capacity loss in existing technologies.

WO2024236911A1PCT designated stage expired Publication Date: 2024-11-21GS YUASA INT LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012216
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-03-27
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Lithium transition metal compound-based positive electrode active materials in power storage elements experience low adhesion with the base material, leading to reduced initial output and capacity retention due to deformation and non-uniform charging/discharging reactions, which decrease the battery's performance over charge/discharge cycles.

Method used

Incorporating positive electrode active material particles with a lithium transition metal compound having a polyanionic structure and a destructive test force of 5.0 mN or more, and a separator with a deformation rate of 10% or less, ensures strong adhesion and reduces capacity retention loss by maintaining close contact between the active material and the base material, even under expansion and contraction.

Benefits of technology

This configuration enhances the initial output and maintains a high capacity retention rate by improving adhesion and reducing interfacial resistance, while minimizing separator deformation and electrolyte extrusion, thus extending the battery's performance over repeated charge/discharge cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012216_21112024_PF_FP_ABST
    Figure JP2024012216_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A power storage element according to one aspect of the present invention comprises an electrode body in which a positive electrode and a negative electrode are laminated with a separator interposed therebetween. The positive electrode has a positive electrode base material and a positive electrode active material layer containing positive electrode active material particles and laminated on the positive electrode base material. The positive electrode active material particles include a lithium transition metal compound having a polyanionic structure. The fracture test force of the positive electrode active material particles is 5.0 mN or more, and the deformation rate of the separator is 10% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Energy storage element and energy storage device

[0001] The present invention relates to an energy storage element and an energy storage device.

[0002] Due to their high energy density, non-aqueous electrolyte secondary batteries, such as lithium-ion non-aqueous electrolyte secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc. Non-aqueous electrolyte secondary batteries generally include an electrode assembly having a pair of electrodes electrically isolated by a separator, and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring charge-transporting ions between the electrodes. Furthermore, as energy storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium-ion capacitors and electric double layer capacitors, as well as energy storage elements using electrolytes other than non-aqueous electrolytes, are also widely used.

[0003] Lithium transition metal compounds having a polyanion structure, such as lithium iron phosphate, are known as positive electrode active materials used in energy storage devices. Patent Document 1 describes a nonaqueous electrolyte secondary battery including a positive electrode containing lithium iron olivine (lithium iron phosphate) as the positive electrode active material and a negative electrode containing graphite as the negative electrode active material.

[0004] Japanese Patent Application Laid-Open No. 2021-153021

[0005] When positive electrode active material particles containing a lithium transition metal compound having a polyanion structure are used in the positive electrode of an energy storage device, the initial output of the energy storage device may be reduced due to poor adhesion between the positive electrode substrate and the positive electrode active material particles. Furthermore, repeated charge-discharge cycles may repeatedly compress the separator due to expansion and contraction of the positive electrode active material particles. As a result, the capacity retention rate of the energy storage device may be reduced due to non-uniform charge-discharge reactions caused by changes in the separator shape or extrusion of electrolytes and other substances from the separator.

[0006] The present invention has been made in light of the above circumstances, and aims to provide an energy storage element and an energy storage device that have a large initial output and can suppress a decrease in capacity retention rate after charge / discharge cycles.

[0007] An energy storage element according to one aspect of the present invention includes an electrode body in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween, the positive electrode having a positive electrode substrate and a positive electrode active material layer stacked on the positive electrode substrate and containing positive electrode active material particles, the positive electrode active material particles contain a lithium transition metal compound having a polyanion structure, the positive electrode active material particles have a breaking test strength of 5.0 mN or more, and the separator has a deformation rate of 10% or less.

[0008] An electricity storage device according to another aspect of the present invention includes two or more electricity storage elements, and includes one or more electricity storage elements according to the aspect of the present invention.

[0009] The energy storage element and energy storage device according to one aspect of the present invention have a large initial output and can suppress a decrease in capacity retention rate after charge / discharge cycles.

[0010] Fig. 1 is a perspective view showing an embodiment of an energy storage element according to the present invention, and Fig. 2 is a schematic view showing an embodiment of an energy storage device formed by assembling a plurality of energy storage elements according to the present invention.

[0011] First, an overview of the energy storage element and the energy storage device disclosed in this specification will be described.

[0012] [1] An energy storage element according to one aspect of the present invention includes an electrode assembly in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween, the positive electrode having a positive electrode substrate and a positive electrode active material layer stacked on the positive electrode substrate and containing positive electrode active material particles, the positive electrode active material particles contain a lithium transition metal compound having a polyanion structure, the positive electrode active material particles have a breaking test strength of 5.0 mN or more, and the separator has a deformation rate of 10% or less.

[0013] The energy storage element described in [1] above has a high initial output and can suppress a decrease in capacity retention rate after charge-discharge cycling. While the reason for this is unclear, the following is presumed. Positive electrode active material particles containing a lithium transition metal compound with a polyanionic structure, as contained in conventional energy storage elements, are prone to deformation and breakage when pressed onto a positive electrode substrate during positive electrode fabrication. This makes it difficult to arrange the positive electrode active material particles so that they sink into the surface of the positive electrode substrate, which can make it difficult to enhance adhesion between the positive electrode substrate and the positive electrode active material particles. In contrast, the energy storage element described in [1] above has positive electrode active material particles with a breaking test force of 5.0 mN or more and high hardness. These positive electrode active material particles are resistant to deformation and breakage when pressed onto the positive electrode substrate, are easy to arrange so that they sink into the surface of the positive electrode substrate, and facilitate enhancing adhesion between the positive electrode substrate and the positive electrode active material particles. High adhesion between the positive electrode active material particles and the positive electrode substrate can reduce interfacial resistance between the positive electrode active material particles and the positive electrode substrate. Therefore, the energy storage device has a high initial output. Furthermore, adhesion between the positive electrode active material particles and the positive electrode substrate is easily maintained even after repeated charge-discharge cycles, thereby suppressing a decrease in the capacity retention rate after charge-discharge cycles. It is believed that evaluating particle hardness using a destructive test force can appropriately evaluate particle hardness without depending on the size of the particles being measured, compared to methods that use, for example, changes in particle diameter when the particles are compressed as an indicator. On the other hand, if the positive electrode active material particles have high hardness, the separator disposed between the positive electrode and the negative electrode is more likely to be compressed by the positive electrode active material particles. Furthermore, repeated charge-discharge cycles may repeatedly compress the separator due to the expansion and contraction of the positive electrode active material particles, making it more likely that electrolytes and other substances will be extruded from the separator. This may result in a decrease in the capacity retention rate of the energy storage device due to non-uniform charge-discharge reactions caused by changes in the separator shape or the extrusion of electrolytes and other substances from the separator. In contrast, in the energy storage device described in [1] above, the separator has a deformation rate of 10% or less, thereby suppressing changes in the separator shape. This further suppresses the decrease in capacity retention rate after charge-discharge cycles.

[0014] In the present invention, "having a polyanion structure" means an oxoacid anion (PO 4 3- , SiO4 4- , B.O. 3 3- etc.)

[0015] In the present invention, the term "breaking test force" refers to the test force at which cracks occur in the positive electrode active material particles when compressed. The breaking test force of the positive electrode active material particles is measured by a microcompression test using a microcompression tester (Shimadzu Corporation, "MCT-511"). A diamond flat indenter with a diameter of 50 μm is used as the probe. The test force is set to 1 mN to 30 mN at a probe speed of 0.134 mN / sec, and pressure is applied to each positive electrode active material particle while changing the test force at a constant rate. The inflection point of the resulting test force-displacement graph is considered to be the point at which cracks occur in the positive electrode active material particles, and the test force at this inflection point is taken as the breaking test force. The breaking test force is measured for five positive electrode active material particles, and the average value is used. The positive electrode active material particles to be measured are selected from particles with a particle size between 1 / 2 and 2 times the average particle size of the positive electrode active material particles. The "particle size" of each particle is taken as the average value of the minor axis and the major axis. The minor axis is the shortest axis passing through the center of the smallest circumscribing circle of a particle, and the major axis is the axis passing through the center and perpendicular to the minor axis. If there are two or more shortest axes, the longest axis perpendicular to the shortest axes is taken as the minor axis. "Average particle size" refers to the value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50%, based on the particle size distribution measured by laser diffraction / scattering in a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).

[0016] When the positive electrode active material particles are incorporated into an energy storage device as a positive electrode active material, the breaking test force is measured on the device in a fully discharged state using the following method. First, the energy storage device is charged at a constant current of 0.05 C until the end-of-charge voltage in normal use is reached, and then fully charged. After a 30-minute rest, the device is discharged at a constant current of 0.05 C until the end-of-charge voltage in normal use (lower limit voltage) is reached. The device is disassembled, the positive electrode is removed, and a test battery is assembled using a metallic lithium electrode as the counter electrode. The positive electrode potential is measured at a current value of 10 mA per 1 g of positive electrode mixture until the positive electrode potential reaches 2.0 V vs. Li / Li. +The positive electrode is adjusted to a fully discharged state by constant current discharge until the positive electrode reaches a fully discharged state. The device is disassembled again and the positive electrode is removed. The electrolyte and other materials adhering to the removed positive electrode are thoroughly washed using dimethyl carbonate, and the device is dried at room temperature for one day and one night, after which the positive electrode active material particles are collected. The collected positive electrode active material particles are subjected to measurement. The operations from disassembling the energy storage device to collecting the positive electrode active material particles are carried out in an argon atmosphere with a dew point of -60°C or below. "During normal use" refers to the case where the energy storage device is used under the charging and discharging conditions recommended or specified for the energy storage device. Regarding charging conditions, for example, if a charger for the energy storage device is provided, this refers to the case where the energy storage device is used using the charger.

[0017] In the present invention, the deformation rate of a separator refers to a value calculated as the bending creep strain measured by a creep test in accordance with JIS-K-7116 (1999) for a test piece of the separator. The creep test is performed under the following test conditions: temperature: 65°C, load: 2 MPa, and test time: 24 hours. In measuring the deformation rate of the separator, if the separator is incorporated into an electric storage element, a portion of the separator where the positive electrode, negative electrode, etc. are not laminated is removed from the electric storage element, or the separator is separated from the positive electrode, negative electrode, etc., and then the electrolyte, etc. is thoroughly washed off using dimethyl carbonate, and the separator is used for measurement.

[0018] [2] In the energy storage element described in [1] above, the electrode body may be a flat, wound electrode body.

[0019] In the energy storage element described in [2] above, since the electrode body is a flat wound electrode body, the charge / discharge reaction is likely to be uneven between the curved surface portion of the electrode body and the other portion, and therefore the effect of the present invention, which can suppress a decrease in the capacity retention rate after charge / discharge cycles of the energy storage element, is significantly achieved.

[0020] [3] A power storage device according to another aspect of the present invention includes two or more power storage elements, and includes one or more of the power storage elements described in [1] or [2] above.

[0021] The energy storage device according to the above [3] includes one or more energy storage elements according to the above [1] or [2], and therefore has a large initial output and can suppress a decrease in capacity retention rate after charge / discharge cycles.

[0022] Hereinafter, an energy storage element, an energy storage device, a method for manufacturing an energy storage element according to an embodiment of the present invention, and other embodiments will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.

[0023] [Electricity storage element] An electric storage element according to one embodiment of the present invention includes an electrode assembly in which positive electrodes and negative electrodes are stacked with a separator interposed therebetween, a non-aqueous electrolyte, and a container for accommodating the electrode assembly and the non-aqueous electrolyte. The electrode assembly is typically a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked with a separator interposed therebetween, or a wound type in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound. The non-aqueous electrolyte is present in a state contained in the positive electrode, the negative electrode, and the separator. As an example of an electric storage element, a non-aqueous electrolyte secondary battery (hereinafter also simply referred to as a "secondary battery") will be described.

[0024] [Positive Electrode] The positive electrode has a positive electrode substrate and a positive electrode active material layer laminated on the positive electrode substrate directly or via an intermediate layer.

[0025] The positive electrode substrate has electrical conductivity. Whether or not it has electrical conductivity is determined by whether or not the volume resistivity measured in accordance with JIS-H-0505 (1975) is 10 -2 The resistance is determined using Ω cm as a threshold value. Metals such as aluminum, titanium, tantalum, and stainless steel, or alloys thereof, are used as the material for the positive electrode substrate. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high conductivity, and cost. Examples of the positive electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, and A1N30, as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).

[0026] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate and increase the energy density per volume of the energy storage element.

[0027] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.

[0028] The positive electrode active material layer contains positive electrode active material particles. The positive electrode active material layer may further contain optional components such as a positive electrode active material other than the positive electrode active material particles, a conductive agent, a binder, a thickener, and a filler, as needed.

[0029] (Configuration of Positive Electrode Active Material Particles) In one embodiment of the present invention, the positive electrode active material particles contain a lithium transition metal compound having a polyanion structure. The lithium transition metal compound having a polyanion structure is usually used in the form of particles coated with a carbon material from the viewpoint of electronic conductivity, etc. That is, in one embodiment of the present invention, the positive electrode active material particles may be particles in which particles containing a lithium transition metal compound having a polyanion structure are coated with a carbon material.

[0030] The lithium transition metal compound having a polyanion structure includes an oxo acid anion (PO 4 3- , S.O. 4 2- , SiO 4 4- , B.O. 3 3- , V.O. 4 3- The oxo acid anion may be a compound containing a condensed anion (P 2 O 7 4- , P 3 O 10 5-The lithium transition metal compound having a polyanion structure may have an olivine-type crystal structure. The lithium transition metal compound having a polyanion structure is typically a polyanion compound containing a lithium element and a transition metal element, and may further contain other elements (for example, halogen elements, etc.). As the transition metal element contained in the lithium transition metal compound having a polyanion structure, iron element, manganese element, nickel element, and cobalt element are preferred, iron element and nickel element are more preferred, and iron element is even more preferred. As the oxo acid anion contained in the lithium transition metal compound having a polyanion structure, phosphate anion (PO 4 3- ) is preferred.

[0031] The lithium transition metal compound having a polyanion structure is preferably a compound represented by the following formula (1): Li a M b (A.O. c ) d X e ... (1) In formula (1), M is at least one transition metal element. A is at least one selected from B, Al, Si, P, S, Cl, Ti, V, Cr, Mo, and W. X is at least one halogen element. a, b, c, d, and e are numbers satisfying 0<a≦3, 0<b≦2, 2≦c≦4, 1≦d≦3, and 0≦e≦1. a, b, c, d, and e may all be integers or decimals.

[0032] As M in formula (1), any one of Fe, Mn, Ni, and Co, or a combination of any two of them, is preferable. As M, Fe, Mn, or a combination thereof is more preferable, and Fe is more preferable. Furthermore, the content of Fe in M ​​is preferably 50 mol% or more, more preferably 70 mol% or more, 90 mol% or more, or 99 mol% or more. As A, P is preferable. As X, F is preferable. In one embodiment, a = 1, b = 1, c = 4, d = 1, and e = 0 may be preferable.

[0033] Specific examples of lithium transition metal compounds having a polyanion structure include LiFePO 4 , LiCoPO 4 , LiFe 0.5 Co 0.5 P.O. 4 , LiMnPO 4 , LiNiPO 4 , LiMn 0.5 Fe 0.5 P.O. 4 , LiCrPO 4 , LiFeVO 4 , Li 2 FeSiO 4 , Li 2 Fe 2 (SO 4 ) 3 , LiFeBO 3 , LiFePO 3.9 F 0.2 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 F. Atoms or polyanions in these lithium transition metal compounds having a polyanion structure may be partially substituted with other atoms or anion species. The lithium transition metal compounds having a polyanion structure may be used alone or in combination of two or more.

[0034] The content of the lithium transition metal compound having a polyanion structure in the particles containing the lithium transition metal compound having a polyanion structure may be 60% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, or 99% by mass or more.

[0035] The particles containing the lithium transition metal compound having a polyanion structure may be single particles in which a plurality of primary particles are present independently without aggregation, but are preferably secondary particles formed by aggregation of a plurality of primary particles, such as secondary particles of the lithium transition metal compound having a polyanion structure.

[0036] In one embodiment of the present invention, particles containing a lithium transition metal compound having a polyanionic structure are coated with a carbon material to form positive electrode active material particles. A portion of the carbon material may be present inside the particles containing the lithium transition metal compound having a polyanionic structure. The positive electrode active material particles may have portions that are not coated with the carbon material (e.g., portions where the lithium transition metal compound having a polyanionic structure is exposed).

[0037] The carbon material coats particles containing a lithium transition metal compound having a polyanion structure, allowing the positive electrode active material particles to exhibit sufficient electron conductivity between particles. The carbon material is, for example, an inorganic material having a carbon element content of 80% by mass or more and 100% by mass or less. The carbon element content in the carbon material may be 90% by mass or more, or may be 95% by mass or more. Elements other than carbon that may be contained in the carbon material include oxygen, hydrogen, and nitrogen. Examples of the carbon material include graphite and non-graphitic carbon.

[0038] The content of the carbon material in the positive electrode active material particles is preferably 0.1% by mass or more and 20% by mass or less, more preferably 0.2% by mass or more and 10% by mass or less, even more preferably 0.3% by mass or more and 5% by mass or less, and even more preferably 0.5% by mass or more and 2% by mass or less. When the content of the carbon material in the positive electrode active material particles is equal to or greater than the lower limit, it is possible to improve electronic conductivity, etc. When the content of the carbon material in the positive electrode active material particles is equal to or less than the upper limit, it is possible to increase the content of the lithium transition metal compound having a polyanion structure, and it is possible to increase the discharge capacity per volume of the energy storage device, etc.

[0039] The total content of the lithium transition metal compound having a polyanion structure and the carbon material in the positive electrode active material particles is preferably 90% by mass or more and 100% by mass or less, and may be 95% by mass or more, 98% by mass or more, 99% by mass or more, or 99.9% by mass or more.

[0040] The lower limit of the breaking test force of the positive electrode active material particles is 5.0 mN, preferably 6.0 mN, more preferably 8.0 mN, and even more preferably 8.5 mN. When the breaking test force is equal to or greater than the lower limit, the adhesion of the positive electrode active material particles to the positive electrode substrate can be improved when the positive electrode active material particles are pressed onto the positive electrode substrate. This also increases the initial output of the energy storage device. On the other hand, from the viewpoint of manufacturability, the upper limit of the breaking test force of the positive electrode active material particles is preferably 30 mN, more preferably 25 mN, and even more preferably 20 mN. The breaking test force of the positive electrode active material particles may be equal to or greater than any of the lower limits and equal to or less than any of the upper limits. In addition, when an intermediate layer containing a conductive agent or the like is formed on the positive electrode substrate of the energy storage device, the positive electrode active material particles can be pressed onto the positive electrode substrate via the intermediate layer. In this case, the adhesion of the positive electrode active material particles to the intermediate layer or the positive electrode substrate can be improved when the positive electrode active material particles are pressed onto the positive electrode substrate via the intermediate layer.

[0041] The average particle size of the positive electrode active material particles is preferably 0.5 μm or more and 30 μm or less, more preferably 1 μm or more and 25 μm or less, even more preferably 2 μm or more and 20 μm or less, even more preferably 4 μm or more and 15 μm or less, and even more preferably 6 μm or more and 12 μm or less. By having the average particle size of the positive electrode active material particles within the above range, the contact area with the positive electrode substrate or the intermediate layer described above can be increased, thereby increasing the initial output of the energy storage device. Furthermore, by having the average particle size of the positive electrode active material particles within the above range, the density of the positive electrode active material layer can be increased, thereby increasing the discharge capacity per volume of the energy storage device. To obtain positive electrode active material particles with a predetermined average particle size, a pulverizer or a classifier can be used. Examples of pulverization methods include methods using a mortar, ball mill, sand mill, vibration ball mill, planetary ball mill, jet mill, counter jet mill, swirling airflow jet mill, or sieve. Wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, or the like may be used as needed for both dry and wet classification.

[0042] From the viewpoint of increasing the contact area with the positive electrode substrate or the intermediate layer, the positive electrode active material particles are preferably spherical. From the same viewpoint, the average aspect ratio of the positive electrode active material particles is preferably 1.0 to 1.5, more preferably 1.0 to 1.4, and even more preferably 1.0 to 1.2. The "average aspect ratio" is determined as the arithmetic mean value of the T / Y value, which is the ratio of the longest major axis T of the positive electrode active material particle to the longest minor axis Y in the direction perpendicular to the longest axis T, averaged over 10 positive electrode active material particles in a cross-sectional SEM image of the positive electrode containing the positive electrode active material particles. A JSM-7001F (manufactured by JEOL Ltd.) scanning electron microscope was used to obtain the cross-sectional SEM image of the positive electrode. The cross-sectional SEM image was obtained by observing a secondary electron image. The acceleration voltage was 5 kV. The observation magnification was set to a magnification such that 3 to 15 positive electrode active material particles appeared in one field of view. The cross-sectional SEM image obtained is saved as an image file. Other conditions such as spot diameter, working distance, irradiation current, brightness, and focus are appropriately set so that the contours of the positive electrode active material particles are clearly visible.

[0043] The content of the positive electrode active material particles in the positive electrode active material layer is preferably 50% by mass to 99% by mass, more preferably 70% by mass to 98% by mass, and even more preferably 80% by mass to 95% by mass. By setting the content of the positive electrode active material particles within the above range, it is possible to achieve both an increase in the discharge capacity per volume of the energy storage element and manufacturability.

[0044] (Method for producing positive electrode active material particles) Positive electrode active material particles according to one embodiment of the present invention can be efficiently obtained by adjusting the pH of the reaction solution using aqueous ammonia or the like when producing the hydroxide precursor in a method using a hydroxide precursor, a lithium source, and a carbon source. By using such a production method, spherical positive electrode active material particles with high hardness can be obtained. The production method will be described in detail below. However, the positive electrode active material particles according to the present invention are not limited to those produced by the following production method.

[0045] First, a hydroxide precursor is obtained by a precipitation reaction between transition metal ions and hydroxide ions in water. Specifically, for example, a transition metal salt aqueous solution and a sodium hydroxide aqueous solution are dropped into water to obtain a hydroxide precursor (a transition metal hydroxide). The transition metal salt may be any water-soluble salt containing the transition metal element that constitutes the desired lithium transition metal compound, such as iron sulfate, iron chloride, cobalt sulfate, manganese sulfate, or nickel sulfate. Alternatively, a potassium hydroxide aqueous solution may be used instead of the sodium hydroxide aqueous solution. When the transition metal salt aqueous solution and the sodium hydroxide aqueous solution are dropped into water, an ammonia aqueous solution or the like is further dropped into the reaction solution to maintain the pH of the water (reaction solution) into which these aqueous solutions are dropped within a predetermined range. The pH of the reaction solution is preferably in the range of 8.5 to 10.6. If the pH of the reaction solution is outside the above range, or if an aqueous ammonia solution or the like is not added dropwise to the reaction solution even if the pH of the reaction solution is within the above range, the amount of change in particle size when pressurized of the finally obtained positive electrode active material particles tends to be large, that is, the breaking strength of the positive electrode active material particles tends to be small. 3 1mol / dm or more 3 The pH of the reaction solution can be adjusted to about 100% or less. The pH of the reaction solution can be adjusted by adjusting the concentrations, amounts, etc. of the aqueous ammonia solution and the aqueous sodium hydroxide solution to be added dropwise. Another alkaline aqueous solution such as an aqueous hydrazine solution may be added dropwise together with the aqueous ammonia solution. The pH of the reaction solution can also be adjusted by the amount, etc., of the other alkaline aqueous solution added.

[0046] Next, the obtained hydroxide precursor, a lithium source, and a carbon source are mixed and fired in an inert atmosphere (for example, a nitrogen atmosphere), thereby obtaining positive electrode active material particles according to one embodiment of the present invention. 2 P.O. 4 , Li 3 P.O. 4 , LiHSO 4Compounds having a polyanion structure such as those described above and containing lithium element can be suitably used. Other lithium sources that can be used include LiOH, lithium halide, etc. When the lithium source used is not a compound having a polyanion structure, a compound having a polyanion structure is further mixed and then calcined. Examples of compounds having a polyanion structure include NH 4 H 2 P.O. 4 , (NH 4 ) 3 P.O. 4 , (NH 4 ) 2 HPO 4 , (NH 4 ) 2 SO 4 , N.H. 4 VO 3 Suitable examples of the carbon source include organic substances such as sucrose, lactose, maltose, sucrose, polyvinyl alcohol, and ascorbic acid. The baking temperature can be, for example, 500°C or higher and 800°C or lower.

[0047] (Configuration other than the positive electrode active material particles) The positive electrode active material layer may further contain a positive electrode active material other than the above-described positive electrode active material particles. As the other positive electrode active material, various conventionally known positive electrode active materials can be used. However, the content of the positive electrode active material particles relative to all the positive electrode active materials contained in the positive electrode active material layer (the total of the positive electrode active material particles and other positive electrode active materials) is preferably 90% by mass or more, more preferably 99% by mass or more, and even more preferably 100% by mass. By thus configuring the positive electrode active material substantially only from the positive electrode active material particles, it is possible to further increase the initial output of the energy storage element, for example.

[0048] The conductive agent is not particularly limited as long as it is a material having electrical conductivity. Examples of such conductive agents include carbon materials, metals, conductive ceramics, etc. Examples of carbon materials include graphite, non-graphitic carbon, graphene-based carbon, etc. Examples of non-graphitic carbon include carbon nanofiber, pitch-based carbon fiber, carbon black, etc. Examples of carbon black include furnace black, acetylene black, ketjen black, etc. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, etc. The conductive agent may be in the form of powder, fiber, etc. As the conductive agent, one of these materials may be used alone, or two or more may be mixed and used. These materials may also be used in combination. For example, a composite material of carbon black and CNT may be used. Among these, carbon black is preferred from the viewpoints of electronic conductivity and coatability, and acetylene black is particularly preferred.

[0049] The content of the conductive agent in the positive electrode active material layer is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By setting the content of the conductive agent within the above range, the energy density of the energy storage element can be increased. Note that the content of the conductive agent does not include the carbon material contained in the positive electrode active material particles (the carbon material coating the particles containing the lithium transition metal compound having a polyanion structure).

[0050] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.

[0051] The content of the binder in the positive electrode active material layer is preferably 1% by mass to 10% by mass, more preferably 3% by mass to 9% by mass, by which the positive electrode active material can be stably maintained.

[0052] Examples of thickeners include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose. When the thickener has a functional group that reacts with lithium or the like, the functional group may be deactivated in advance by methylation or the like. When a thickener is used, the content of the thickener in the positive electrode active material layer can be, for example, 0.1% by mass or more and 8% by mass or less, and can also be 5% by mass or less, or 1% by mass or less.

[0053] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, sparingly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof. When a filler is used, the content of the filler in the positive electrode active material layer can be, for example, 0.1% by mass or more and 8% by mass or less, and can also be 5% by mass or less or 1% by mass or less.

[0054] The positive electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material particles, other positive electrode active materials, conductive agents, binders, thickeners, and fillers.

[0055] A method for producing a positive electrode includes, for example, preparing a positive electrode mixture paste containing the positive electrode active material particles, other optional components such as a conductive agent, a binder, a thickener, and a filler, and a dispersion medium; applying the positive electrode mixture paste directly or via an intermediate layer to at least one surface of a positive electrode substrate; drying the positive electrode mixture paste; and pressing the positive electrode active material layer. An organic solvent is preferably used as the dispersion medium used in preparing the positive electrode mixture paste, and examples of the organic solvent include N-methylpyrrolidone (NMP) and toluene. Furthermore, by pressing, it is preferable that at least a portion of the positive electrode active material particles in the positive electrode active material layer are disposed so as to be embedded in the positive electrode substrate or the intermediate layer.

[0056] [Negative electrode] The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode above, for example.

[0057] The negative electrode substrate is conductive. Metals such as copper, nickel, stainless steel, nickel-plated steel, and aluminum, or alloys thereof, carbon materials, and the like are used as the material for the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.

[0058] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, even more preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and also increase the energy density per volume of the energy storage element.

[0059] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, and a filler, as needed. The optional components such as the conductive agent, the binder, the thickener, and the filler can be selected from the materials exemplified for the positive electrode above.

[0060] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0061] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for a lithium ion secondary battery. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li 4 Ti 5 O 12 , LiTiO 2、 TiNb 2 O 7 Examples of the material include titanium-containing oxides such as titanium dioxide, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitizable carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more may be used in combination.

[0062] "Graphite" refers to a graphite material that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of being able to obtain a material with stable physical properties.

[0063] "Non-graphitic carbon" refers to a carbon having an average lattice spacing (d 002) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.

[0064] Here, the "discharged state" refers to a state in which the battery is discharged so that lithium ions capable of being absorbed and desorbed during charging and discharging are sufficiently released from the carbon material serving as the negative electrode active material. For example, this refers to a state in which the open circuit voltage of a half cell using a negative electrode containing a carbon material as the negative electrode active material as the working electrode and metallic Li as the counter electrode is 0.7 V or higher.

[0065] "Non-graphitizable carbon" refers to the above-mentioned d 002 The term "carbon material" refers to a carbon material having a particle size of 0.36 nm or more and 0.42 nm or less.

[0066] "Graphitizable carbon" refers to the above-mentioned d 002 The term "carbon material" refers to a carbon material having a particle size of 0.34 nm or more and less than 0.36 nm.

[0067] The negative electrode active material is usually in the form of particles (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is a carbon material, a titanium-containing oxide, or a polyphosphate compound, the average particle size may be 1 μm or more and 100 μm or less. When the negative electrode active material is Si, Sn, Si oxide, Sn oxide, or the like, the average particle size may be 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to be equal to or greater than the above lower limit, the production or handling of the negative electrode active material becomes easy. By setting the average particle size of the negative electrode active material to be equal to or less than the above upper limit, the electronic conductivity of the negative electrode active material layer is improved. A pulverizer, a classifier, or the like is used to obtain powder with a predetermined particle size. When the negative electrode active material is a metal such as metallic Li, the negative electrode active material layer may be in the form of a foil.

[0068] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% by mass to 99% by mass, more preferably 90% by mass to 98% by mass. By setting the content of the negative electrode active material within this range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.

[0069] [Separator] The separator can be appropriately selected from known separators. Examples of separators that can be used include separators consisting of only a substrate layer and separators in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer. Examples of the shape of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these shapes, porous resin films are preferred from the viewpoint of strength, and nonwoven fabrics are preferred from the viewpoint of non-aqueous electrolyte retention. Materials for the substrate layer of the separator are preferably polyolefins such as polyethylene and polypropylene from the viewpoint of shutdown function, and polyimide and aramid from the viewpoint of oxidative decomposition resistance. A composite material of these resins may also be used for the substrate layer of the separator.

[0070] The heat-resistant particles contained in the heat-resistant layer preferably exhibit a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably exhibit a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials exhibiting a mass loss of a predetermined value or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon and diamond; mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, as well as artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be used in combination. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the energy storage device.

[0071] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.

[0072] The upper limit of the separator deformation rate is 10%, preferably 8%, and more preferably 6%. When the separator deformation rate is equal to or less than the upper limit, it is possible to suppress uneven charge / discharge reactions due to changes in the separator shape and a decrease in the capacity retention rate of the energy storage device after charge / discharge cycling due to extrusion of electrolyte and the like from the separator. The lower limit of the separator deformation rate can be, for example, 0.5%. When the electrode assembly included in the energy storage device is a wound type, the lower limit of the separator deformation rate is preferably 3%, more preferably 5%, from the viewpoint of facilitating winding of the electrode assembly.

[0073] The electrode body of the energy storage device is preferably wound and flat. A flat wound electrode body typically has two curved portions and two flat portions. When the electrode body is a flat wound electrode body, the charge / discharge reaction tends to be uneven between the curved portions of the electrode body and other portions. Therefore, the effect of the present invention, which can suppress a decrease in the capacity retention rate after charge / discharge cycles of the energy storage device, is significantly achieved.

[0074] [Non-aqueous electrolyte] The non-aqueous electrolyte can be appropriately selected from known non-aqueous electrolytes. The non-aqueous electrolyte may be a non-aqueous electrolyte solution. The non-aqueous electrolyte solution contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.

[0075] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of non-aqueous solvents include cyclic carbonates, chain carbonates, carboxylic acid esters, phosphate esters, sulfonic acid esters, ethers, amides, and nitriles. Non-aqueous solvents in which some of the hydrogen atoms contained in these compounds have been substituted with halogens may also be used.

[0076] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Of these, EC is preferred.

[0077] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferred.

[0078] It is preferable to use a cyclic carbonate or a chain carbonate as the non-aqueous solvent, and it is more preferable to use a cyclic carbonate and a chain carbonate in combination. The use of a cyclic carbonate can promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. The use of a chain carbonate can reduce the viscosity of the non-aqueous electrolyte. When a cyclic carbonate and a chain carbonate are used in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is preferably in the range of, for example, 5:95 to 50:50.

[0079] The electrolyte salt can be appropriately selected from known electrolyte salts, such as lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts. Of these, lithium salts are preferred.

[0080] The lithium salt is LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 , LiN(SO 2 F) 2inorganic lithium salts such as lithium oxalate salts, lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); 3 CF 3 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) (SO 2 C 4 F 9 ), LiC(SO 2 CF 3 ) 3 , LiC(SO 2 C 2 F 5 ) 3 Among these, inorganic lithium salts are preferred, and LiPF 6 is more preferred.

[0081] The content of the electrolyte salt in the non-aqueous electrolyte solution is 0.1 mol / dm at 20°C and 1 atmosphere. 3 2.5mol / dm or more 3 It is preferably 0.3 mol / dm or less. 3 2.0mol / dm or more 3 It is more preferable that it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3 It is more preferable that it is 0.7 mol / dm or less. 3 1.5mol / dm or more 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the non-aqueous electrolyte can be increased.

[0082] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of the additives include halogenated carbonates such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC); oxalates such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, and silyl. Aromatic compounds such as cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, and the like. Carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1 ,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, etc. These additives may be used alone or in combination of two or more.

[0083] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass, based on the total mass of the non-aqueous electrolyte. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and further improve safety.

[0084] The non-aqueous electrolyte may be a solid electrolyte, or a non-aqueous electrolytic solution and a solid electrolyte may be used in combination.

[0085] The solid electrolyte can be selected from any material that has ionic conductivity of lithium, sodium, calcium, etc. and is solid at room temperature (e.g., 15° C. to 25° C.) Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.

[0086] As the sulfide solid electrolyte, in the case of a lithium ion secondary battery, for example, Li 2 S-P 2 S 5 , LiI-Li 2 S-P 2 S 5 , Li 10 Ge-P 2 S 12 etc.

[0087] The shape of the energy storage element of this embodiment is not particularly limited, and examples thereof include a cylindrical battery, a prismatic battery, a flat battery, a coin battery, and a button battery.

[0088] FIG. 1 shows an energy storage element 1 as an example of a prismatic battery. Note that this figure is a see-through view of the inside of the container. An electrode assembly 2 having a positive electrode and a negative electrode wound with a separator sandwiched between them is housed in a prismatic container 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51.

[0089] [Electricity Storage Device] The energy storage element of the present embodiment can be mounted as an energy storage unit (battery module) configured by assembling a plurality of energy storage elements in an automobile power source such as an electric vehicle (EV), a hybrid electric vehicle (HEV), or a plug-in hybrid electric vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source, etc. In this case, it is sufficient that the technology of the present invention is applied to at least one energy storage element included in the energy storage unit.

[0090] An energy storage device according to one embodiment of the present invention includes two or more energy storage elements, and includes one or more energy storage elements according to one embodiment of the present invention described above (hereinafter referred to as the "second embodiment"). It is sufficient that the technology according to one embodiment of the present invention is applied to at least one energy storage element included in the energy storage device according to the second embodiment, and the energy storage device may include one energy storage element according to one embodiment of the present invention described above and one or more energy storage elements not according to one embodiment of the present invention described above, or may include two or more energy storage elements according to one embodiment of the present invention described above.

[0091] 2 shows an example of a power storage device 30 according to a second embodiment in which power storage units 20, each of which is a collection of two or more electrically connected power storage elements 1, are further assembled. The power storage device 30 may include a bus bar (not shown) that electrically connects two or more power storage elements 1, a bus bar (not shown) that electrically connects two or more power storage units 20, etc. The power storage unit 20 or the power storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more power storage elements.

[0092] [Method for Manufacturing Energy Storage Element] The method for manufacturing the energy storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode assembly, preparing an electrolyte, and housing the electrode assembly and the electrolyte in a container. Preparing the electrode assembly includes preparing a positive electrode and a negative electrode, and forming the electrode assembly by stacking or winding the positive electrode and the negative electrode with a separator interposed therebetween.

[0093] The method for placing the electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the electrolyte, the non-aqueous electrolyte solution may be poured into the container through an inlet formed in the container, and the inlet may then be sealed.

[0094] [Other Embodiments] The energy storage element and energy storage device of the present invention are not limited to the above-described embodiments, and various modifications may be made without departing from the spirit of the present invention. For example, the configuration of one embodiment can be added to the configuration of another embodiment, and part of the configuration of one embodiment can be replaced with the configuration of another embodiment or well-known technology. Furthermore, part of the configuration of one embodiment can be deleted. Also, well-known technology can be added to the configuration of one embodiment.

[0095] In the above embodiment, the case where the energy storage element is used as a chargeable and dischargeable non-aqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) has been described, but the type, shape, size, capacity, etc. of the energy storage element are arbitrary. The present invention can also be applied to various secondary batteries and capacitors such as electric double layer capacitors and lithium ion capacitors. The energy storage element of the present invention may be an energy storage element other than a non-aqueous electrolyte energy storage element.

[0096] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0097] [Example 1] (Preparation of Positive Electrode Active Material Particles) Positive electrode active material particles in which secondary particles of lithium iron phosphate were coated with a carbon material were obtained by the following procedure. 3 2 dm 3 1 mol / dm 3 FeSO 4 The aqueous solution was added dropwise at a constant rate while adjusting the pH of the reaction solution to 4 mol / dm 3 and 0.75 mol / dm 3 NH 3 aqueous solution and 0.5 mol / dm 3 NH 2 NH 2 The aqueous solution was added dropwise to Fe(OH) 2The temperature of the reaction vessel was set at 50°C ± 2°C. Next, the prepared Fe(OH) 2 The precursor is removed from the reaction vessel and the Fe(OH) 2 LiH per 100 parts by mass of precursor 2 P.O. 4 The resulting mixture was solid-phase mixed with 116 parts by mass of sucrose powder and 10 parts by mass of sucrose powder. The resulting mixture was baked at a baking temperature of 650°C in a nitrogen atmosphere to obtain LiFePO, a lithium transition metal compound having a polyanion structure. 4 The positive electrode active material particles of Example 1 were obtained by coating the particles with a carbon material. The content of the carbon material in the obtained positive electrode active material particles of Example 1 was 1.0 mass%. The average particle size of the positive electrode active material particles of Example 1 measured by the above method was 10 μm. The breaking test force of the positive electrode active material particles of Example 1 measured by the above method was 5.0 mN.

[0098] (Preparation of Positive Electrode) A positive electrode mixture paste was prepared using the obtained positive electrode active material particles, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium. The mass ratio of the positive electrode active material particles, AB, and PVDF was 90:5:5 in terms of solid content. This positive electrode mixture paste was applied to aluminum foil as a positive electrode substrate, dried, and roll-pressed to form a positive electrode active material layer, thereby obtaining the positive electrode of Example 1.

[0099] (Preparation of Negative Electrode) A negative electrode mixture paste was prepared by mixing graphite as a negative electrode active material, styrene-butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a dispersion medium. The mass ratio of graphite to SBR to CMC was 96:3.3:0.7 in terms of solid content. This negative electrode mixture paste was applied to copper foil as a negative electrode substrate, dried, and roll-pressed to form a negative electrode active material layer, thereby obtaining a negative electrode.

[0100] (Non-aqueous electrolyte) A solvent containing ethylene carbonate (EC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC) mixed in a volume ratio of 30:35:35 was added to a 1.1 mol / dm 3 At a concentration of LiPF6 was dissolved to obtain a non-aqueous electrolyte.

[0101] (Separator) A polyethylene microporous film having a deformation rate of 7% measured by the above method was used as the separator.

[0102] The positive electrode, negative electrode, and separator were stacked and wound to prepare an electrode assembly. The obtained electrode assembly was placed in a container, and the non-aqueous electrolyte was then poured into the container, followed by sealing, to obtain the energy storage element of Example 1.

[0103] [Examples 2 to 6, Comparative Examples 1 to 11] In the preparation of positive electrode active material particles, Fe(OH) 2 The positive electrode active material particles of Examples 2 to 6 and Comparative Examples 1 to 11 were obtained in the same manner as in Example 1, except that the reaction solution used to produce the precursor was adjusted to maintain a pH value (±0.1) shown in Table 1. The pH of the reaction solution was adjusted by changing the amount of each aqueous solution added. The carbon material content in each of the obtained positive electrode active material particles was 1.0 mass%. The average particle size of each positive electrode active material particle measured by the above method was 10 μm. The fracture test strength of each positive electrode active material particle measured by the above method is shown in Table 1. Furthermore, the energy storage elements of Examples 2 to 6 and Comparative Examples 1 to 11 were obtained in the same manner as in Example 1, except that the deformation rate of the separator was set as shown in Table 1.

[0104] [Evaluation] (Initial Charge / Discharge) Each of the obtained energy storage elements was initially charged and discharged at 25°C in the following manner. Constant-current, constant-voltage charging was performed with a charging current of 0.2 C and a charge cut-off voltage of 3.5 V. The charge was terminated until the charging current reached 0.01 C. A rest period of 10 minutes was then provided. Subsequently, constant-current discharging was performed with a discharging current of 0.2 C and a discharge cut-off voltage of 2.0 V.

[0105] (Initial Capacity Confirmation Test) Next, an initial capacity confirmation test was performed on each energy storage element at 25°C in the following manner. Constant current / constant voltage charging was performed with a charging current of 1.0 C and a charge cut-off voltage of 3.5 V. The charge was terminated until the charging current reached 0.01 C. A rest period of 10 minutes was then provided. Subsequently, constant current discharging was performed with a discharging current of 1.0 C and a discharge cut-off voltage of 2.0 V. The discharge capacity at this time was defined as the "initial discharge capacity." The fully charged state based on the initial discharge capacity was defined as 100% SOC (State of Charge).

[0106] (Initial Output Confirmation Test) After the initial capacity confirmation test, each storage element was subjected to constant current charging at a charging current of 0.2 C in a thermostatic chamber at 25°C until the SOC reached 50%. The charge termination condition was set to a total charging time of 2.5 hours. Next, the element was discharged for 60 seconds at discharge currents of 0.2 C, 0.5 C, and 1.0 C. After each discharge, a 10-minute rest period was provided, followed by supplementary charging at a charging current of 0.2 C until the SOC reached 50%. From the current-voltage characteristic graph obtained by plotting the voltage 10 seconds after the start of each discharge on the vertical axis and the discharge current on the horizontal axis, the output [W] at 10 seconds was determined using the IV method with a lower limit voltage of 2.0 V, and this was designated the "initial output at 25°C." The results are shown in Table 1.

[0107] (Charge-Discharge Cycle Test) After the initial output confirmation test, each energy storage element was subjected to a charge-discharge cycle test at 60°C in the following manner. Constant-current charging was performed with a charge current of 8 C and a charge cut-off voltage of 3.9 V. Subsequently, constant-current discharging was performed with a discharge current of 8 C and a discharge cut-off voltage of 3.5 V. No rest period was provided after each charge and discharge. This charge-discharge cycle was repeated 100 times.

[0108] (Capacity Confirmation Test After Charge-Discharge Cycle Test) After the charge-discharge cycle test, a capacity confirmation test after the charge-discharge cycle test was conducted in the same manner as the initial capacity confirmation test. The discharge capacity at this time was designated as the "discharge capacity after charge-discharge cycle test." The percentage of the discharge capacity after the charge-discharge cycle test to the initial discharge capacity for each energy storage element is shown in Table 1 as the "capacity retention rate after cycling."

[0109]

[0110] As shown in Table 1, Comparative Examples 3 to 7, Comparative Examples 10 and 11, and Examples 1 to 6, in which the fracture test force of the positive electrode active material particles was 4.2 mN or more, had an initial output (initial output at 25°C) of 20 W or more, and the initial output was significantly improved compared to Comparative Examples 1, 2, and Comparative Examples 8 and 9, in which the fracture test force of the positive electrode active material particles was less than 4.2 mN. Furthermore, Comparative Examples 4 to 7 and 11, in which the fracture test force of the positive electrode active material particles was 5.0 mN or more, had a capacity retention rate after charge-discharge cycling that was increased by 5% or more compared to Comparative Examples 3 and 10, in which the fracture test force of the positive electrode active material particles was 4.2 mN. This suggests that a fracture test force of 5.0 mN or more improves the adhesion between the positive electrode active material particles and the positive electrode substrate, thereby increasing the initial output and suppressing a decrease in the capacity retention rate after charge-discharge cycling.

[0111] On the other hand, in Examples 1 to 6, in which the breaking test force of the positive electrode active material particles was 5.0 mN or more and the deformation rate of the separator was 10% or less, the capacity retention rate after charge-discharge cycling was increased by an additional 6% or more compared to Comparative Examples 4 to 7 and 11, in which the breaking test force of the positive electrode active material particles was 5.0 mN or more and the deformation rate of the separator was more than 10%. This suggests that a breaking test force of the positive electrode active material particles of 5.0 mN or more and a deformation rate of the separator of 10% or less can increase the initial output and further suppress a decrease in the capacity retention rate after charge-discharge cycling.

[0112] When comparing Comparative Examples 1 to 3, in which the fracture test force of the positive electrode active material particles was less than 5.0 mN and the separator deformation rate exceeded 10%, with Comparative Examples 8 to 10, in which the fracture test force of the positive electrode active material particles was less than 5.0 mN and the separator deformation rate was 10% or less, the capacity retention rates after charge-discharge cycling were comparable. Therefore, the effect of suppressing the decrease in capacity retention rate by setting the separator deformation rate to 10% or less is achieved only when the fracture test force of the positive electrode active material particles is 5.0 mN or more, and is thought to be achieved synergistically with the effect of the positive electrode active material particles having a large fracture test force (hardness).

[0113] The present invention can be applied to electric storage elements used as power sources for electronic devices such as personal computers and communication terminals, and automobiles.

[0114] REFERENCE SIGNS LIST 1 Energy storage element 2 Electrode body 3 Container 4 Positive electrode terminal 41 Positive electrode lead 5 Negative electrode terminal 51 Negative electrode lead 20 Energy storage unit 30 Energy storage device

Claims

1. An energy storage element comprising an electrode assembly in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween, the positive electrode having a positive electrode substrate and a positive electrode active material layer stacked on the positive electrode substrate and containing positive electrode active material particles, the positive electrode active material particles containing a lithium transition metal compound having a polyanion structure, the positive electrode active material particles having a breaking test force of 5.0 mN or more, and the separator having a deformation rate of 10% or less.

2. The energy storage element according to claim 1, wherein the electrode body is a flat, wound electrode body.

3. A power storage device comprising two or more power storage elements, the power storage device comprising one or more of the power storage elements according to claim 1 or 2.

Citation Information

Patent Citations

  • Non-aqueous electrolyte secondary battery

    JP2021153021A

  • Aggregated granular lithium multiple oxide, its production and lithium secondary battery

    JP2001080920A

  • Electrode material, electrode paste for lithium ion battery, electrode for lithium ion battery, and lithium ion battery

    JP2014060142A

  • Positive electrode material for lithium ion secondary battery, method of producing the same, electrode for lithium ion secondary battery, and lithium ion secondary battery

    JP2019160550A

  • Positive electrode for power storage element and power storage element

    JP2022075345A