Cement composition and production method therefor

The cement composition, featuring a specific blend of cement clinker, inorganic minerals, and gypsum, addresses the challenge of reducing carbon emissions and maintaining strength by promoting hydration reactions, effectively replacing traditional cement clinker with mixed materials to enhance strength and reduce emissions.

WO2024236981A1PCT designated stage expired Publication Date: 2024-11-21MITSUBISHI UBE CEMENT CORP

Patent Information

Application Number
PCT/JP2024/015029
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-04-15
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current cement compositions face challenges in reducing carbon emissions while maintaining strength, as increasing the replacement ratio of cement clinker with mixed materials beyond the standard 5% by mass leads to decreased strength, and the availability of suitable replacement materials like kaolin is limited.

Method used

A cement composition comprising cement clinker, an inorganic mineral with a reduced BET specific surface area post-pulverization, carbonate, and gypsum, where the inorganic mineral content is between 0.5% to 14.0% by mass, and the total carbonate content is more than 5% to 15% by mass, along with cement clinker and gypsum making up 85% to 95% by mass, promoting easier hydration reactions for enhanced strength development.

Benefits of technology

The proposed cement composition achieves excellent strength development while reducing carbon emissions by facilitating hydration reactions and controlling heat generation, thus addressing the limitations of traditional cement compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This cement composition contains a cement clinker, an inorganic mineral, a carbonate, and gypsum. The inorganic mineral has a BET specific surface area reduced by pulverization. The content of the inorganic mineral in the cement composition is 0.5-14.0 mass%, the total content of the inorganic mineral and the carbonate is more than 5 mass% and at most 15 mass%, and the total content of the cement clinker and the gypsum is at least 85 mass% and less than 95 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Cement composition and method for producing the same

[0001] The present disclosure relates to cement compositions and methods for making same.

[0002] As part of our efforts to promote low carbonization, we are reducing CO2 emissions during manufacturing. 2 Cement compositions in which part of the cement clinker, which has a large amount of emissions, is replaced with admixtures are being used. Limestone is widely used as an admixture added to cement because it is easily available and inexpensive.

[0003] Currently, the amount of admixtures added to ordinary Portland cement is set at 5% by mass or less according to JIS R 5210:2009. However, from the perspective of preventing global warming and achieving low carbon, it is desirable to further increase the proportion of cement clinker replaced by admixtures to produce an even lower-carbon cement in order to reduce the amount of cement clinker used. However, it is known that simply adding limestone in excess of the current 5% by mass results in a decrease in strength compared to ordinary Portland cement (see, for example, Non-Patent Document 1).

[0004] Regarding the types of admixtures, the JIS standard allows for the use of fly ash, blast furnace slag, and silica fume in addition to limestone as minor admixture components, but other promising admixtures are being explored. For example, it is known that adding metakaolin, a calcined natural material made from kaolin, to cement can improve strength development (Non-Patent Document 2).

[0005] Ayuka Nakaguchi et al., "Quality Evaluation of Cement with Increased Amounts of Minor Mixture Components," Abstracts of the Cement Technology Conference, 2018, pp. 270-271; Karen Scrivener et al.: Calcinated Clay Limestone Cements (LC3), Cement and Concrete Research, Vol. 114, pp. 49-56 (2018)

[0006] However, the kaolin used as the raw material for metakaolin in Non-Patent Document 2 is produced in limited regions and countries. Therefore, if there is a material other than kaolin that can be used as an admixture, it would be extremely useful for developing low-carbon cement.

[0007] The present disclosure has been made in view of the above circumstances, and aims to provide a low-carbon cement composition having excellent strength development properties and a method for producing the same.

[0008] One aspect of the present disclosure provides a cement composition comprising cement clinker, an inorganic mineral, a carbonate, and gypsum, wherein the inorganic mineral has a BET specific surface area that is reduced by grinding, the content of the inorganic mineral being 0.5 to 14.0 mass%, the total content of the inorganic mineral and the carbonate being more than 5 mass% and 15 mass% or less, and the total content of the cement clinker and the gypsum being 85 mass% or more and less than 95 mass%.

[0009] The cement composition contains inorganic minerals whose BET specific surface area decreases upon pulverization. Such inorganic minerals have minute pores before pulverization and adsorb nitrogen into the pores, resulting in a large BET specific surface area. When such inorganic minerals are pulverized, the microstructure that forms the pores is destroyed, resulting in a smaller BET specific surface area. When such microstructures are destroyed, the hydration reaction of cement is facilitated, contributing to the strength development of the cement composition. The cement composition contains predetermined amounts of such inorganic minerals and carbonates along with cement clinker and gypsum. Therefore, it has excellent strength development despite being low carbon. In this specification, a low carbon cement composition refers to a cement composition that is produced by replacing cement clinker with an admixture, thereby reducing the CO2 emissions during the production of the cement composition. 2 It means a cement composition that can reduce emissions.

[0010] One aspect of the present disclosure includes a mixing step of mixing an inorganic mineral, cement clinker, carbonate, and gypsum, the BET specific surface area of ​​which is reduced by pulverization, to obtain a cement composition having a content of the inorganic mineral of 0.5 to 14.0 mass%, a total content of the inorganic mineral and the carbonate of more than 5 mass% and not more than 15 mass%, and a total content of the cement clinker and the gypsum of 85 mass% or more and less than 95 mass%, wherein in the mixing step, the Blaine specific surface area of ​​the cement composition is 3000 cm 2 The present invention provides a method for producing a cement composition, in which the cement composition is mixed while being pulverized so that the total weight of the cement is 100g or more.

[0011] The method for producing the cement composition includes a mixing step of mixing inorganic minerals, carbonates, cement clinker, and gypsum, the BET specific surface area of ​​which is reduced by pulverization, to obtain a cement composition containing these minerals in a predetermined ratio. When the inorganic minerals are pulverized, the microstructure that forms the pores is destroyed, thereby reducing the BET specific surface area. When such a microstructure is destroyed, the hydration reaction of the cement is facilitated, contributing to the development of strength in the cement composition. The method for producing the cement composition includes a mixing step of mixing the cement composition so that the Blaine specific surface area of ​​the cement composition is reduced to 3000 cm. 2 The inorganic minerals are crushed and mixed to a carbon content of at least 1 / g, which allows the inorganic minerals to be crushed appropriately and promotes the hydration reaction of the cement. This allows for the production of a low-carbon cement composition that has excellent strength development.

[0012] One aspect of the present disclosure provides a method for producing a powdered material having a BET specific surface area lower than that of the inorganic mineral, the method comprising: a first crushing step of crushing an inorganic mineral to obtain a crushed material having a BET specific surface area lower than that of the inorganic mineral; a second crushing step of crushing at least one of cement clinker, gypsum, and carbonate; and a mixing step of mixing at least the crushed materials obtained in the first crushing step and the second crushing step together, wherein the content of the inorganic mineral is 0.5 to 14.0 mass%, the total content of the inorganic mineral and the carbonate is more than 5 mass% and less than 15 mass%, and the total content of the cement clinker and the gypsum is 85 mass% or more and less than 95 mass%, and the Blaine specific surface area is 3000 cm 2The present invention provides a method for producing a cement composition, which can obtain a cement composition having a viscosity of 1000 kJ / g or more.

[0013] The method for producing the cement composition involves pulverizing inorganic minerals in a first pulverization step to obtain a pulverized product having a lower BET specific surface area than the inorganic minerals before pulverization. Because such a pulverized product is obtained by destroying the microstructure that forms the pores of the inorganic minerals, the hydration reaction of cement is facilitated, contributing to the strength development of the cement composition. By mixing at least the pulverized products obtained in the first pulverization step and the second pulverization step, a cement composition is obtained in which the inorganic mineral content, the total content of the inorganic mineral and carbonate, and the total content of the cement clinker and gypsum are in predetermined ratios. In this way, a low-carbon cement composition with excellent strength development can be obtained.

[0014] The present disclosure can provide a low-carbon cement composition having excellent strength development and a method for producing the same.

[0015] Embodiments of the present disclosure are described below. However, the following embodiments are merely examples for explaining the present disclosure and are not intended to limit the present disclosure to the following content. In the following description, when "X to Y" (X and Y are any numerical values ​​satisfying X<Y) is used, it means "X or more and Y or less" unless otherwise specified. When multiple numerical ranges are exemplified in stages, the present disclosure also includes a numerical range in which the upper or lower limit of a first numerical range is replaced with the upper or lower limit of a second numerical range that is narrower than the first numerical range. The present disclosure also includes a numerical range obtained by replacing the upper or lower limit of a numerical range with a numerical value in an example. Unless otherwise specified, the exemplified materials can be used alone or in combination of two or more. When multiple substances corresponding to each component are present in the composition, the content of each component in the composition refers to the total amount of the multiple substances present in the composition, unless otherwise specified.

[0016] <Cement composition> A cement composition according to one embodiment includes inorganic minerals, carbonates, cement clinker, and gypsum. By including inorganic minerals in this cement composition, the content of cement clinker can be reduced. This reduces CO 2 It is possible to create a low-carbon cement composition that can reduce emissions.

[0017] The Blaine specific surface area of ​​the cement composition is 3000 cm 2 / g or more, preferably 3150 cm 2 / g or more, and more preferably 3300 cm 2 / g or more, and more preferably 3500 cm 2 / g or more, and particularly preferably 3700 cm 2 The Blaine specific surface area of ​​the cement composition is preferably 6000 cm 2 / g or less, and more preferably 5000 cm 2 / g or less, and more preferably 4600 cm 2 When the Blaine specific surface area of ​​the cement composition is in the above range, it is possible to achieve both strength development and heat generation suppression at a sufficiently high level, while reducing the crushing cost and CO 2 The Blaine specific surface area of ​​the cement composition can be measured in accordance with the description of JIS R 5201:2015 "Physical measurement methods for cement."

[0018] (Cement clinker) The cement clinker can be Portland cement clinker used to prepare various Portland cements specified in JIS R 5210:2009 "Portland cement." Examples of Portland cement clinker include ordinary Portland cement clinker, high-early-strength Portland cement clinker, moderate-heat Portland cement clinker, low-heat Portland cement clinker, and oil-well Portland cement clinker. The Portland cement clinker may include at least one selected from the group consisting of ordinary Portland cement clinker and high-early-strength Portland cement clinker, and preferably includes ordinary Portland cement clinker.

[0019] Cement clinker has the following mineral composition: 3 S.C. 2 S.C. 3 A and C 4 Includes AF. 3 S.C. 2 S.C. 3 A and C 4 The content of each AF can be calculated using the Bogue formula. The Bogue formula is a widely used formula for calculating the content of major minerals in cement clinker from the content ratio of their chemical compositions. By using the Bogue formula shown below, the content of tricalcium silicate (3CaO.SiO 2 , C 3 S), dicalcium silicate (2CaO.SiO 2 , C 2 S), tricalcium aluminate (3CaO·Al 2 O 3 , C 3 A), and tetracalcium aluminate (4CaO·Al 2 O 3 Fe 2 O 3 , C 4Each chemical formula in the Bogue formula below represents the content (mass%) of each compound indicated by chemical analysis values ​​according to JIS R 5204:2019 "Method for X-ray fluorescence analysis of cement."

[0020] <Bogue style> C 3 S [mass %] = (4.07 x CaO [mass %]) - (7.60 x SiO 2 [mass%]) - (6.72×Al 2 O 3 [mass%]) - (1.43 x Fe 2 O 3 [mass%]) - (2.85 x SO 3 [mass%]) C 2 S [mass%] = (2.87 x SiO 2 [mass%]) - (0.754×C 3 S [mass%]) C 3 A [mass%] = (2.65 x Al 2 O 3 [mass%]) - (1.69×Fe 2 O 3 [mass%]) C 4 AF [mass%] = 3.04 x Fe 2 O 3 [mass%]

[0021] C in cement clinker 3 The amount of S is preferably 30.0 to 70.0 mass%, more preferably 40.0 to 66.0 mass%, and even more preferably 50.0 to 65.0 mass%. 3 By setting the lower limit of the amount of S within the above range, the early strength of the cement composition when hardened can be further improved. 3 By setting the upper limit of the amount of S within the above range, heat generation during hardening of the cement composition can be suppressed.

[0022] C in cement clinker 2 The amount of S is preferably 5.0 to 65.0 mass%, more preferably 8.0 to 50.0 mass%, even more preferably 10.0 to 40.0 mass%, still more preferably 12.0 to 30.0 mass%, and particularly preferably 12.0 to 25.0 mass%.2 By setting the lower limit of the amount of S within the above range, it is possible to further improve the long-term strength of the cement composition when it is hardened. 2 By setting the upper limit of the amount of S within the above range, the early strength of the cement composition upon hardening can be further improved.

[0023] C in cement clinker 3 The amount of A is preferably 7.0% by mass or more, more preferably 8.0% by mass or more, even more preferably 8.5% by mass or more, still more preferably 9.0% by mass or more, and particularly preferably 9.5% by mass or more. 3 By setting the amount of A within the above range, it is possible to increase the amount of waste and by-products such as coal ash that are used as raw materials for cement clinker. 3 The amount of A is preferably 13.0% by mass or less, more preferably 12.0% by mass or less, even more preferably 11.0% by mass or less, and even more preferably 10.5% by mass or less. 3 By setting the amount of A within the above range, ettringite (3CaO.Al 2 O 3 3CaSO 4 ・32H 2 O) can be suppressed, and an increase in adiabatic temperature rise during hardening of the cement composition can be suppressed.

[0024] C in cement clinker 4 The AF amount is preferably 7.0% by mass or more, more preferably 8.0% by mass or more, even more preferably 9.0% by mass or more, still more preferably 9.5% by mass or more, and particularly preferably 9.8% by mass or more. 4 By adjusting the AF content within the above range, it is possible to produce a cement composition that utilizes an increased amount of waste and by-products such as coal ash, which are raw materials for cement clinker. 4The AF amount is preferably 14.0% by mass or less, more preferably 13.0% by mass or less, even more preferably 12.0% by mass or less, still more preferably 11.0% by mass or less, and particularly preferably 10.4% by mass or less. 4 By setting the AF amount within the above range, it is possible to suppress an increase in adiabatic temperature rise during hardening of the cement composition.

[0025] The content of cement clinker based on the total amount of the cement composition may be, for example, 80 to 93 mass%, 83 to 92 mass%, or 85 to 91 mass%. When the content of Portland cement clinker in the cement composition is 80 mass% or more, 83 mass% or more, or 85 mass% or more, better compressive strength can be obtained. When the content of Portland cement clinker in the cement composition is 93 mass% or less, 92 mass% or less, or 91 mass% or less, CO 2 Emissions can be further reduced.

[0026] (Inorganic Minerals) The inorganic minerals may be minerals produced by the weathering of volcanic ejecta, i.e., minerals derived from volcanic ejecta. Examples of volcanic ejecta include volcanic ash, lapilli, pumice, and pyroclastic flow deposits. The inorganic minerals may be minerals produced by the weathering of igneous rock. Examples of igneous rock include granite. Allophane is produced by the weathering of volcanic ejecta or igneous rock, and halloysite is produced by further weathering of allophane, and kaolin is produced by further weathering of halloysite. Kaolin, allophane, and halloysite are all clay minerals.

[0027] Examples of inorganic minerals include allophane, halloysite, imogolite, illite, montmorillonite, and pyrophyllite. 2 / Al 2 O 3The mass ratio of these may be 0.5 to 3.0. From the viewpoint of increasing the reactivity with cement clinker, the inorganic mineral preferably contains allophane or halloysite, and more preferably contains allophane. Allophane is an amorphous inorganic mineral. Examples of inorganic minerals containing allophane include Kanuma clay and SEKADO P1 (trade name, manufactured by Shinagawa General Co., Ltd.).

[0028] In this specification, the term "inorganic mineral" includes various forms such as lumps and particles, pulverized materials obtained by pulverizing lumps or particles, aggregates of particles, and granulated materials. The BET specific surface area of ​​such inorganic minerals is preferably 30 to 350 m from the viewpoint of improving kneadability. 2 From the viewpoint of improving the strength development of the cement composition, the BET specific surface area of ​​the inorganic mineral is preferably 350 m 2 / g or less, and more preferably 300m 2 / g or less, and more preferably 270m 2 / g or less, and even more preferably 200m 2 / g or less, and particularly preferably 180m 2 From the viewpoint of reducing the time required for pulverizing the inorganic mineral or cement composition, the BET specific surface area of ​​the inorganic mineral is preferably 50 m 2 / g or more, more preferably 70m 2 / g or more, and more preferably 100m 2 / g or more, and even more preferably 150m 2 The BET specific surface area in this specification is a value obtained from a BET plot in the relative pressure range of 0.05 to 0.35 by a BET multipoint method using nitrogen gas.

[0029] The Blaine specific surface area of ​​an inorganic mineral can be measured in accordance with the description of JIS R 5201:2015 "Physical measurement method for cement". The Blaine specific surface area of ​​an inorganic mineral is, for example, 8000 cm 2 / g or more, preferably 10,000 cm 2 / g or more, and more preferably 12000 cm 2 / g or more, and more preferably 14000 cm 2 / g or more, and even more preferably 18000 cm 2 / g or more. This allows the strength development of the cement composition to be further improved. The Blaine specific surface area of ​​the inorganic mineral is, for example, 30,000 cm 2 / g or less, and preferably 28000 cm 2 / g or less, and more preferably 26000 cm 2 / g or less, which can reduce the cost of pulverization.

[0030] The inorganic mineral is one whose BET specific surface area is reduced by pulverization. The inorganic mineral may also be one whose Blaine specific surface area is increased by pulverization. In the case of allophane, the SiO 2 and Al 2 O 3 The microstructure, such as the layer structure of the aluminum, is destroyed by the crushing. In addition, the coordination number of the aluminum atoms changes from six to four, and the atomic bonding state also changes. It is believed that these changes in the microstructure and molecular structure facilitate the progress of the cement hydration reaction, improving the strength development of the cement composition.

[0031] The pulverized inorganic mineral may be a pulverized product obtained by pulverizing particles or granulated material using a pulverizer such as a mill, or may be a pulverized product obtained by pulverizing the inorganic mineral when preparing the cement composition. For example, by blending a pulverized inorganic mineral in advance when preparing the cement composition, or by selecting conditions for pulverizing the inorganic mineral when preparing the cement composition, a cement composition with excellent strength development can be obtained.

[0032] The BET specific surface area of ​​the pulverized inorganic mineral is preferably 180 m 2 From the viewpoint of improving the strength development of the cement composition, the BET specific surface area of ​​the pulverized material is more preferably 160 m 2 / g or less, and more preferably 100m 2 / g or less, and even more preferably 80m 2From the viewpoint of reducing the time required for pulverization, the BET specific surface area of ​​the pulverized inorganic mineral is preferably 3 m 2 / g or more, more preferably 30m 2 / g or more, and more preferably 50m 2 / g or more, and even more preferably 70m 2 / g or more.

[0033] The ratio α of the BET specific surface area of ​​the pulverized inorganic mineral to the BET specific surface area of ​​the inorganic mineral before pulverization is preferably 0.10 to 0.80. The ratio α is preferably 0.20 or more, more preferably 0.30 or more. This makes it possible to reduce the pulverization cost and the time required for pulverization. The ratio α is preferably 0.70 or less, more preferably 0.60 or less. This makes it possible to further increase the strength development of the cement composition.

[0034] The ratio β of the Blaine specific surface area of ​​the pulverized material to the Blaine specific surface area of ​​the inorganic mineral before pulverization is preferably 1.10 to 1.50. The ratio β is preferably 1.15 or more, more preferably 1.20 or more. This can further increase the strength development of the cement composition. The ratio β is preferably 1.40 or less, more preferably 1.30 or less. This can reduce the pulverization cost and the time required for pulverization.

[0035] The Blaine specific surface area of ​​the pulverized inorganic mineral is preferably 10,000 cm 2 / g or more, and more preferably 12000 cm 2 / g or more, and more preferably 14000 cm 2 / g or more, and particularly preferably 18000 cm 2 / g or more. The inorganic mineral is crushed to a Blaine specific surface area of ​​3000 cm 2 By including such a pulverized material, the compressive strength of the cured product can be increased sufficiently.

[0036] The insoluble residue of the inorganic mineral, as measured by the method for quantifying insoluble residue using the hydrochloric acid-sodium carbonate method of JIS R 5202:2010, is preferably 1 to 50 mass% or less, more preferably 5 to 40 mass% or less, and particularly preferably 10 to 33 mass% or less. Having an insoluble residue of 50 mass% or less enhances the reactivity of the inorganic mineral and makes it possible to further improve the strength development of the cement composition. Furthermore, from the viewpoint of reducing the effort and cost required to remove impurities that become insoluble residue, the inorganic mineral may contain an insoluble residue of 1 mass% or more.

[0037] Inorganic mineral SiO 2 The amount of Al of the inorganic mineral is preferably 15 to 55 mass %, more preferably 20 to 45 mass %, and even more preferably 25 to 35 mass %, from the viewpoint of reactivity with Portland cement clinker. 2 O 3 From the viewpoint of reactivity with Portland cement clinker, the amount is preferably 15 to 55 mass %, more preferably 20 to 45 mass %, and even more preferably 30 to 40 mass %.

[0038] The content of inorganic minerals based on the total amount of the cement composition may be, for example, 0.5 to 14 mass%. The content of inorganic minerals is preferably 1.0 mass% or more, more preferably 1.5 mass% or more, and even more preferably 2.0 mass% or more. This reduces the content of cement clinker in the cement composition and improves CO 2 The inorganic mineral content is preferably 10.0% by mass or less, more preferably 8.0% by mass or less, even more preferably 5.0% by mass or less, and particularly preferably 4.0% by mass or less. This allows the compressive strength of the hardened body at an age of 28 days to be sufficiently high, and also allows for good kneadability.

[0039] (Carbonate) Carbonates can promote the hydration reaction between Portland cement clinker and inorganic minerals. Examples of carbonates include alkali metal carbonates, alkaline earth metal carbonates, and hydrates thereof, such as sodium carbonate and sodium carbonate decahydrate (Na2 CO 3 ・10H 2 O), potassium carbonate (K 2 CO 3 ), calcium carbonate (limestone), magnesium carbonate, etc. Examples of carbonates include sodium sesquicarbonate dihydrate (Na 3 H(CO 3 ) 2 NaHCO 3 ・2H 2 O) can also be used.

[0040] As the limestone, for example, powders containing calcium carbonate as a main component, such as commonly available limestone powder, kansui stone powder, etc. Limestone preferably includes limestone that conforms to the minor mixing components described in JIS R 5210:2009 "Portland cement."

[0041] The carbonate content, based on the total amount of the cement composition, is preferably 1.0 mass% or more, more preferably 2.0 mass% or more, even more preferably 4.0 mass% or more, and even more preferably 5.0 mass% or more, from the viewpoint of improving fluidity. The carbonate content in the cement composition is preferably 14.5 mass% or less, more preferably 14.0 mass% or less, even more preferably 13.0 mass% or less, particularly preferably 11.5 mass% or less, and even more preferably 9.5 mass% or less, from the viewpoint of sufficiently increasing the compressive strength of the hardened body.

[0042] The total content of carbonates and inorganic minerals based on the total amount of the cement composition is CO 2 From the viewpoint of reducing the amount of CO emissions and enhancing the strength development, the CO content is more than 5 mass % and 15 mass % or less. 2 From the viewpoint of further reducing the amount of discharge, the total content of carbonate and inorganic mineral is preferably 6 mass% or more, more preferably 7 mass% or more, and even more preferably 8 mass% or more. From the viewpoint of further increasing the strength development of the cement composition, the total content of carbonate and inorganic mineral is preferably 13 mass% or less, more preferably 12 mass% or less, and even more preferably 10 mass% or less.

[0043] (Gypsum) Examples of gypsum include gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum. The gypsum may contain one of gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum alone, or may contain a combination of two or more of them. By including gypsum in the cement composition, the hydration reaction rate can be adjusted.

[0044] The gypsum content based on the total amount of the cement composition is 3 In terms of conversion, the total amount of the cement composition is taken as 100% by mass, and the content is preferably 0.5 to 3.5% by mass, more preferably 0.7 to 3.0% by mass, and even more preferably 0.8 to 2.5% by mass.

[0045] The total content of gypsum and cement clinker based on the total amount of the cement composition is 2 From the viewpoint of reducing emissions and increasing strength development, the total content of gypsum and cement clinker is preferably 85% by mass or more and less than 95% by mass. From the viewpoint of sufficiently increasing the content of inorganic minerals, the total content of gypsum and cement clinker is preferably 94% by mass or less, more preferably 93% by mass or less, and even more preferably 92% by mass or less. From the viewpoint of further increasing the strength development of the cement composition, the total content of gypsum and cement clinker is preferably 86% by mass or more, more preferably 87% by mass or more, and even more preferably 88% by mass or more.

[0046] (Other Components) The cement composition may contain other components such as inorganic fine powder, calcium hydroxide, calcium-containing powder other than calcium hydroxide, concrete water-reducing agent, accelerator, retarder, etc. (However, gypsum, carbonate, and inorganic minerals are excluded. When the cement composition contains inorganic fine powder, the compressive strength is further improved. The content of other components can be 10% by mass or less, 8% by mass or less, or 6% by mass or less, based on the total amount of the cement composition. Examples of inorganic fine powder include powdery materials such as silica stone and crushed stone. The content of inorganic fine powder in the cement composition may be more than 0% by mass or 5% by mass or more, based on the total amount of the cement composition, from the viewpoint of fluidity, and may be 10% by mass or less, 8% by mass or less, or 6% by mass or less, based on the total amount of the cement composition, from the viewpoint of compressive strength.

[0047] <Hardened product> The hardened product may be a product obtained by hardening a paste containing the above-mentioned cement composition and water, or may be a mortar or concrete obtained by mixing water and aggregate and hardening it. The hardening conditions are not particularly limited. The hardened product can be prepared in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement."

[0048] The amount of water in the paste is preferably 15 parts by mass or more per 100 parts by mass of the total cement composition from the viewpoint of fluidity, and is preferably 80 parts by mass or less from the viewpoint of facilitating a dense pore structure of the hardened body. From these viewpoints, the amount of water is preferably 25 to 80 parts by mass, more preferably 35 to 60 parts by mass.

[0049] <Method for producing cement composition (1)> A method for producing a cement composition according to one embodiment is a method for producing a cement composition having a BET specific surface area of ​​30 to 350 m, for example. 2The method comprises a first grinding step of grinding an inorganic mineral having a BET specific surface area of ​​0.5 to 14.0% by mass, a total content of the inorganic mineral and the carbonate being more than 5% by mass and 15% by mass or less, and a total content of the cement clinker and the gypsum being 85% by mass or more and less than 95% by mass.

[0050] In the first crushing step, the inorganic mineral is crushed. The BET specific surface area of ​​the inorganic mineral before crushing is preferably 160 m 2 / g or more, more preferably 170m 2 / g or more, and more preferably 180m 2 By carrying out such grinding, it is possible to sufficiently increase the strength development of the cement composition. The BET specific surface area of ​​the inorganic mineral before grinding is 350 m 2 / g or less, and more preferably 300m 2 / g or less, and more preferably 270m 2 This makes it possible to reduce the time and cost required for pulverization.

[0051] In the first grinding step, grinding is performed so that the ratio α of the BET specific surface area of ​​the ground product to the BET specific surface area of ​​the inorganic mineral before grinding is 0.10 to 0.80. The ratio α is preferably 0.20 or more, and more preferably 0.30 or more. This makes it possible to reduce the grinding cost and the time required for grinding. The ratio α is preferably 0.70 or less, and more preferably 0.60 or less. This makes it possible to further increase the strength development of the cement composition.

[0052] In the first crushing step, crushing is performed so that the ratio β of the Blaine specific surface area of ​​the crushed material to the Blaine specific surface area of ​​the inorganic mineral before crushing is preferably 1.10 to 1.50. The ratio β is preferably 1.15 or more, more preferably 1.20 or more. This can further increase the strength development of the cement composition. The ratio β is preferably 1.40 or less, more preferably 1.30 or less. This can reduce the time required for crushing and the crushing costs.

[0053] The pulverization may be carried out using a pulverizer, such as a standard mill, a ball mill, a vertical roller mill, or a roller press. By adjusting the pulverization time, the BET specific surface area, the ratio α, and the ratio β of the pulverized product can be adjusted.

[0054] In the second grinding step, raw materials other than inorganic minerals, i.e., at least one of carbonate, cement clinker, and gypsum, may be ground using the grinder. The carbonate, cement clinker, and gypsum may be ground individually, or at least two of them may be ground together. All of the carbonate, cement clinker, and gypsum may be ground together, or at least one of the carbonate, cement clinker, and gypsum may not be ground. In this way, in the second grinding step, a ground product containing at least one of carbonate, cement clinker, and gypsum is obtained.

[0055] In the mixing step, at least the pulverized products obtained in the first pulverization step and the second pulverization step are mixed together to form a mixture having a Blaine specific surface area of ​​3000 cm 2 A cement composition having a pulverization rate of 1 / g or more is obtained. Of the cement clinker and gypsum, those that were not pulverized in the second pulverization step may be mixed directly with the pulverized material in the mixing step. The mixing step may be performed using a mixer such as a pan mixer, a tilting mixer, or a ribbon mixer, as well as a pulverizer such as a ball mill, a vertical roller mill, or a roller press. One of these may be used alone to perform pulverization or mixing, or a combination of these may be used to pulverize and mix.

[0056] The Blaine specific surface area of ​​the cement composition is preferably 5000 cm 2 / g or less, and more preferably 4500 cm 2 / g or less, and more preferably 4000 cm 2 When the Blaine specific surface area of ​​the cement composition is in the above range, it is possible to achieve both strength development and heat generation suppression at a sufficiently high level, while reducing the crushing cost and CO 2 Emissions can be reduced significantly.

[0057] The method for producing a cement composition may include any optional steps in addition to the first crushing step, the second crushing step, and the mixing step. For example, a sorting step may be included before or after the crushing step. In the sorting step, in order to select inorganic minerals with high strength development, impurities such as sand and iron scraps, which have a large insoluble residue and low reactivity, are removed by sieving, gravity separation, air classification, magnetic separation, or other methods to adjust the particle size and composition of the inorganic minerals. In this case, it is desirable to select the inorganic minerals so that the insoluble residue of the inorganic minerals, as measured by the method for quantifying the insoluble residue using the hydrochloric acid-sodium carbonate method of JIS R 5202:2010, is 50% by mass or less.

[0058] The above description of the embodiment of the <cement composition> also applies to the manufacturing method of this embodiment, so redundant description will be omitted.

[0059] <Method for producing cement composition (2)> In another embodiment, a method for producing a cement composition is carried out using a cement having a BET specific surface area of ​​30 to 350 m, for example. 2 / g, and an inorganic mineral whose BET specific surface area is reduced by grinding, cement clinker, carbonate, and gypsum are mixed to obtain a cement composition having an inorganic mineral content of 0.5 to 14.0 mass%, a total content of the inorganic mineral and the carbonate of more than 5 mass% and 15 mass% or less, and a total content of the cement clinker and gypsum of 85 mass% or more and less than 95 mass%, and in the mixing step, a Blaine specific surface area of ​​the cement composition is reduced to 3000 cm 2 / g or more, more preferably 4000 cm 2 The mixture is mixed while being pulverized so that the solubility becomes 1 / g or more.

[0060] In this manufacturing method, the Blaine specific surface area of ​​the cement composition is increased to 3000 cm in the mixing step. 2 / g or more, preferably 4000 cm 2 / g or more, a cement composition having excellent strength development can be obtained without using crushed inorganic minerals. The Blaine specific surface area of ​​the cement composition is preferably 6000 cm 2 / g or less, and more preferably 5000 cm 2 / g or less, and more preferably 4600 cm 2 When the Blaine specific surface area of ​​the cement composition is in the above range, the crushing cost and CO 2 can be reduced while achieving both strength development and heat generation suppression at a sufficiently high level. 2 Emissions can be reduced significantly.

[0061] In the mixing step, the order of mixing and pulverization is not particularly limited. That is, the raw materials may be mixed and then pulverized, or the raw materials may be pulverized individually and then mixed, or the raw materials may be mixed and pulverized simultaneously. Some of the raw materials may be mixed while being pulverized, and then the other raw materials may be pulverized and / or mixed separately. The mixing step may be performed using, for example, a mixer such as a pan mixer, a tilting mixer, or a ribbon mixer, or a pulverizer such as a ball mill, a vertical roller mill, or a roller press. One of these may be used alone, or a combination of two or more may be mixed while being pulverized.

[0062] The manufacturing method of this embodiment may or may not include a pulverization step of pulverizing the inorganic mineral. If the pulverization step is not performed, the time and cost required for the pulverization step can be reduced. From this viewpoint, the BET specific surface area of ​​the inorganic mineral used in the mixing step is preferably 160 m 2 / g or more, more preferably 180m 2 / g or more, and more preferably 190m 2 From the viewpoint of further increasing the strength development of the cement composition, the BET specific surface area of ​​the inorganic mineral used is preferably 350 m 2 / g or less, and more preferably 300m 2 / g or less, and more preferably 280m 2 / g or less, and even more preferably 200m 2 / g or less. Furthermore, when a pulverization step is carried out, it is preferable to pulverize the inorganic mineral so that the ratio α of the BET specific surface area of ​​the pulverized inorganic mineral (pulverized product) to the BET specific surface area of ​​the inorganic mineral before pulverization is 0.10 to 0.80. The ratio α is preferably 0.20 or more, more preferably 0.30 or more. This makes it possible to reduce the pulverization cost and the time required for pulverization. The ratio α is preferably 0.70 or less, more preferably 0.60 or less. This makes it possible to further increase the strength development of the cement composition.

[0063] When the raw materials are mixed and pulverized simultaneously in the mixing step, the inorganic mineral is pulverized simultaneously with the other raw materials. In this case, it is preferable to pulverize the raw materials so that the ratio α of the BET specific surface area of ​​the pulverized inorganic mineral to the BET specific surface area of ​​the inorganic mineral before pulverization is 0.10 to 0.80. The preferred range of this ratio α is as described above.

[0064] The BET specific surface area of ​​the inorganic mineral after crushing contained in the cement composition can be determined from the BET specific surface area of ​​the cement composition after crushing. That is, the BET specific surface area of ​​the inorganic mineral after crushing is usually 3,000 to 5,000 cm 2 / g of the cement composition has a BET specific surface area of ​​1 m 2 / g, the BET specific surface area of ​​the cement composition can be sufficiently increased by including an inorganic mineral with a large BET specific surface area. 2 When the cement composition contains 2 mass % of inorganic minerals having a specific surface area of ​​3 m / g, the BET specific surface area of ​​the cement composition is 3 m / g. 2 / g.) Furthermore, when the above inorganic minerals are contained, the BET specific surface area of ​​the entire cement composition decreases due to grinding, so the cement composition is further ground, the BET specific surface area is measured, and the ratio of the BET specific surface areas of the inorganic minerals before and after grinding can be obtained by extrapolation. Furthermore, the addition rate of the above inorganic minerals such as allophane can be determined by an appropriate combination of XRD Rietveld analysis, chemical analysis using fluorescent X-rays, wet analysis, gravity separation, SEM-EDS, TEM-EDS, and the like.

[0065] The above description of the embodiment of the <cement composition> also applies to the manufacturing method of this embodiment. Therefore, redundant description will be omitted. In addition, as in the manufacturing method (1) of the cement composition, a sorting step may be included before the mixing step.

[0066] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above embodiments. The present disclosure includes the following embodiments.

[0067] [1] A cement composition comprising cement clinker, an inorganic mineral, a carbonate, and gypsum, wherein the inorganic mineral has a BET specific surface area that is reduced by grinding, the content of the inorganic mineral is 0.5 to 14.0 mass%, the total content of the inorganic mineral and the carbonate is more than 5 mass% and not more than 15 mass%, and the total content of the cement clinker and the gypsum is 85 mass% or more and less than 95 mass%. [2] The inorganic mineral has a BET specific surface area of ​​180 m 2 / g or less, the ratio of the BET specific surface area of ​​the pulverized material to the BET specific surface area of ​​the inorganic mineral before pulverization is 0.10 to 0.80, and the Blaine specific surface area of ​​the cement composition is 3000 cm 2 [3] The cement composition according to [1], wherein the inorganic mineral has a BET specific surface area of ​​30 to 350 m 2 / g, and the Blaine specific surface area of ​​the cement composition is 4000 cm 2 / g or more. [4] The cement composition according to any one of [1] to [3], wherein the inorganic mineral contains allophane. [5] The cement composition according to any one of [1] to [4], wherein the insoluble residue of the inorganic mineral is 50 mass% or less as measured by the method for quantifying insoluble residue using the hydrochloric acid-sodium carbonate method of JIS R 5202:2010. [6] The cement composition according to any one of [1] to [4], wherein the content of the carbonate is 1.0 to 14.5 mass%. [7] A mixing step of mixing an inorganic mineral whose BET specific surface area is reduced by pulverization, cement clinker, carbonate, and gypsum to obtain a cement composition having a content of the inorganic mineral of 0.5 to 14.0 mass%, a total content of the inorganic mineral and the carbonate of more than 5 mass% and 15 mass% or less, and a total content of the cement clinker and the gypsum of 85 mass% or more and less than 95 mass%, wherein in the mixing step, the Blaine specific surface area of ​​the cement composition is 3000 cm 2 [8] The method for producing a cement composition according to [7], wherein in the mixing step, the inorganic mineral is pulverized so that the ratio of the BET specific surface area after pulverization to the BET specific surface area of ​​the inorganic mixture before pulverization is 0.10 to 0.80. [9] The method for producing a cement composition according to [7], wherein the inorganic mineral is pulverized to a BET specific surface area of ​​180 m lower than that of the inorganic mineral. 2

[10] The method for producing a cement composition according to [7], further comprising a grinding step of obtaining a ground product having a BET specific surface area of ​​3000 cm / g or less, wherein in the grinding step, grinding is carried out so that the ratio of the BET specific surface area of ​​the ground product to the BET specific surface area of ​​the inorganic mineral before grinding is 0.10 to 0.80. 2

[11] A method for producing a cement composition according to [9], comprising: a first grinding step of grinding an inorganic mineral to obtain a ground product having a lower BET specific surface area than the inorganic mineral; a second grinding step of grinding at least one of cement clinker, gypsum, and carbonate; and a mixing step of mixing at least the ground products obtained in the first grinding step and the second grinding step, wherein the content of the inorganic mineral is 0.5 to 14.0 mass%, the total content of the inorganic mineral and the carbonate is more than 5 mass% and less than 15 mass%, and the total content of the cement clinker and the gypsum is 85 mass% or more and less than 95 mass%, and the Blaine specific surface area is 3000 cm 2

[12] The method for producing a cement composition according to

[11] , wherein in the first crushing step, crushing is performed so that the ratio of the BET specific surface area of ​​the crushed inorganic mineral to the BET specific surface area of ​​the inorganic mineral before crushing is 0.10 to 0.80.

[0068] The present disclosure will be described in more detail below with reference to examples, comparative examples, and reference examples, although the present disclosure is not limited to the following examples.

[0069] [Raw materials for cement composition] (Cement clinker) As the cement clinker, two types of Portland cement clinker were used, whose mineral compositions calculated by the Bogue formula were as shown in Table 1 below. The chemical composition of the cement used in the Bogue formula calculation was measured in accordance with the method described in JIS R 5204:2019 "Method for X-ray fluorescence analysis of cement."

[0070]

[0071] (Gypsum) As the gypsum, gypsum satisfying the requirements described in JIS R 9151:2009 "Natural gypsum for cement" was used.

[0072] (Admixture) Limestone and inorganic minerals were prepared as admixtures. The limestone was prepared as limestone fine powder (Blaine specific surface area: 7470 cm) by pulverizing limestone that had a calcium carbonate content of 90% by mass or more and an aluminum oxide content of 1.0% by mass or less and that satisfied the requirements for minor admixture components as defined in JIS R 5210:2019 "Portland cement." 2 / g). The inorganic mineral used was one containing allophane. As the inorganic mineral containing allophane, SEKADO P1 (trade name, manufactured by Shinagawa General Co., Ltd.) or Kanuma soil (manufactured by Akagi Engei Co., Ltd.) was used.

[0073] The measurement results of the insoluble residue, ignition loss (Ig. loss), and chemical components of each inorganic mineral are shown in Table 2. Ig. loss was measured in accordance with the method of JIS R 5202:2010, and the insoluble residue was measured by the hydrochloric acid-sodium carbonate method. The chemical components were determined by chemical analysis using the fundamental parameter method of fluorescent X-rays in accordance with JIS R 5202:2010 (instrument used: ZSX-100e manufactured by Rigaku Corporation). 2 O is the alkali content, Na 2 O content +0.658K 2 It was calculated based on the O content.

[0074] Each of the inorganic minerals described above was ground in a standard mill for 60 minutes to prepare a ground inorganic mineral. The measurement results for the density, Blaine specific surface area, and BET specific surface area of ​​the inorganic mineral before and after grinding (ground product) are shown in Table 3. The Blaine specific surface area was measured in accordance with JIS R 5201:2015 "Physical Measurement Methods for Cement." The density value was measured using an automatic density meter (MAT-7000, Seishin Enterprise Co., Ltd.). The BET specific surface area was calculated from the measurement results of the amount of nitrogen gas adsorption in the relative pressure range of 0.05 to 0.35 using a BELSORP MINI (trade name) manufactured by Microtrac-Bell, Inc., using nitrogen gas by the BET multipoint method.

[0075]

[0076]

[0077] The ratio of the BET specific surface area after grinding to the BET specific surface area before grinding, and the ratio of the Blaine specific surface area after grinding to the Blaine specific surface area before grinding are shown in Table 3. As shown in Table 3, the BET specific surface area of ​​both SEKADO P1 and Kanuma soil decreased and the Blaine specific surface area increased after grinding.

[0078] [Preparation of cement composition (1)] For cement clinker A having the chemical composition shown in Table 1, gypsum was added to SO 3 The base cement was prepared by adding 1.0% by mass of limestone fine powder and mixing while grinding. Then, limestone fine powder and the inorganic minerals (before or after grinding) shown in Table 3 were added to the base cement according to the formulation shown in Table 4, and mixed to prepare the cement compositions of Examples 1 to 5 and Comparative Example 1. In Comparative Example 1, the inorganic minerals shown in Table 3 were not blended. Reference Example 1 contains 4% by mass of limestone fine powder and is a cement composition equivalent to ordinary Portland cement specified in JIS R 5210:2009 "Portland cement."

[0079] [Measurement of Blaine Specific Surface Area] The Blaine specific surface area of ​​each component of each cement composition was measured in accordance with JIS R 5201:2015 "Physical measurement methods for cement." The results are shown in Table 4.

[0080] [Preparation of hardened body] The prepared cement composition was mixed with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water, and a hardened body was prepared in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement." The prepared hardened body was cured underwater in a thermostatic chamber at 20°C until it reached an age of 7 days or 28 days.

[0081] [Measurement of Compressive Strength Ratio] The compressive strength of the above-mentioned hardened body was measured at ages of 7 days and 28 days in accordance with JIS R 5201:2015 "Physical Testing Methods for Cement." The results are shown in Table 4. The compressive strength ratio is the ratio (percentage) of the compressive strength of the hardened body to the compressive strength of a reference hardened body. The reference hardened body was prepared by blending ordinary Portland cement with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water in accordance with the method described in JIS R 5201:2015 "Physical Testing Methods for Cement."

[0082]

[0083] As shown in Table 4, the compressive strength of the hardened bodies of Examples 1 to 5 at ages of 7 days and 28 days was at the same level as that of ordinary Portland cement (Reference Example 1). These results demonstrate that the cement compositions of Examples 1 to 5 can reduce the amount of cement clinker, enabling low carbonization, while still providing hardened bodies with compressive strength equivalent to conventional ones.

[0084] [Preparation of cement composition (2)] Gypsum was added to a ground product of cement clinker B having the chemical composition shown in Table 1. 3 The base cement was prepared by adding 2.0 mass% of limestone powder and the inorganic minerals (before crushing) shown in Table 3 to the base cement in the proportions shown in Table 5 and mixing to prepare the cement compositions of Examples 6 and 7 and Comparative Examples 2 and 3. In Comparative Examples 2 and 3, the inorganic minerals shown in Table 3 were not blended.

[0085] The Blaine specific surface area of ​​each cement composition was measured, and the hardened product of each cement composition was prepared and the compressive strength ratio was measured in the same manner as in Example 1. The results are shown in Table 5.

[0086]

[0087] As shown in Table 5, the compressive strength of the hardened bodies of Examples 6 and 7 at ages of 7 days and 28 days was higher than that of Comparative Examples 2 and 3. These results confirmed that the cement compositions of Examples 6 and 7 can reduce the amount of cement clinker, enabling low carbonization, while also providing hardened bodies with compressive strengths equal to or greater than those of conventional products.

Claims

1. A cement composition comprising cement clinker, an inorganic mineral, a carbonate, and gypsum, wherein the inorganic mineral has a BET specific surface area that is reduced by grinding, the content of the inorganic mineral is 0.5 to 14.0 mass%, the total content of the inorganic mineral and the carbonate is more than 5 mass% and 15 mass% or less, and the total content of the cement clinker and the gypsum is 85 mass% or more and less than 95 mass%.

2. The inorganic mineral has a BET specific surface area of ​​180 m 2 / g or less, the ratio of the BET specific surface area of ​​the pulverized material to the BET specific surface area of ​​the inorganic mineral before pulverization is 0.10 to 0.80, and the Blaine specific surface area of ​​the cement composition is 3000 cm 2 The cement composition according to claim 1, wherein the Cementitious Agent is Cr, Mn, MnO, MnO+, MnO2, MnO+ ...

3. The inorganic mineral has a BET specific surface area of ​​30 to 350 m 2 / g, and the Blaine specific surface area of ​​the cement composition is 4000 cm 2 The cement composition according to claim 1, wherein the Cementitious Agent is Cr, Mn, MnO, MnO+, MnO2, MnO+ ...

4. The cement composition according to any one of claims 1 to 3, wherein the inorganic mineral contains allophane.

5. The cement composition according to any one of claims 1 to 3, wherein the insoluble residue of the inorganic mineral is 50 mass% or less as measured by the method for quantifying insoluble residue using a hydrochloric acid-sodium carbonate method of JIS R 5202:2010.

6. A cement composition according to any one of claims 1 to 3, wherein the carbonate content is 1.0 to 14.5 mass%.

7. A mixing step of mixing inorganic minerals whose BET specific surface area is reduced by grinding, cement clinker, carbonates, and gypsum to obtain a cement composition having an inorganic mineral content of 0.5 to 14.0 mass%, an inorganic mineral and a carbonate content of more than 5 mass% and not more than 15 mass%, and a cement clinker and a gypsum content of 85 mass% or more and less than 95 mass%, wherein in the mixing step, the Blaine specific surface area of ​​the cement composition is 3000 cm 2 A method for producing a cement composition, comprising grinding and mixing the resulting mixture so that the total weight of the cement composition is 100g or more.

8. The method for producing a cement composition according to claim 7, wherein in the mixing step, the inorganic mineral is pulverized so that the ratio of the BET specific surface area of ​​the inorganic mineral after pulverization to the BET specific surface area of ​​the inorganic mineral before pulverization is 0.10 to 0.

80.

9. Crush the inorganic mineral to a size less than 180 mm below the inorganic mineral. 2 8. The method for producing a cement composition according to claim 7, further comprising a grinding step of obtaining a ground product having a BET specific surface area of ​​0.1 to 0.80 relative to the BET specific surface area of ​​the inorganic mineral before grinding, wherein the grinding step is performed so that the ratio of the BET specific surface area of ​​the ground product to the BET specific surface area of ​​the inorganic mineral before grinding is 0.10 to 0.

80.

10. In the grinding process, the inorganic mineral is ground to a powder having a Blaine specific surface area of ​​3000 cm 2 The method for producing a cement composition according to claim 9, wherein the cement composition is ground so that the molecular weight of the cement composition increases by at least 1000g.

11. A method for producing a pulverized material having a BET specific surface area lower than that of the inorganic mineral, comprising: a first pulverization step of pulverizing an inorganic mineral to obtain a pulverized material having a lower BET specific surface area than that of the inorganic mineral; a second pulverization step of pulverizing at least one of cement clinker, gypsum, and carbonate; and a mixing step of mixing at least the pulverized materials obtained in the first pulverization step and the second pulverization step together, wherein the content of the inorganic mineral is 0.5 to 14.0 mass%, the total content of the inorganic mineral and the carbonate is more than 5 mass% and less than 15 mass%, and the total content of the cement clinker and the gypsum is 85 mass% or more and less than 95 mass%, and the Blaine specific surface area is 3000 cm 2 A method for producing a cement composition, which obtains a cement composition having a viscosity of 1000:1 or more.

12. A method for producing a cement composition as described in claim 11, wherein in the first crushing step, the inorganic mineral is crushed so that the ratio of the BET specific surface area of ​​the crushed inorganic mineral to the BET specific surface area of ​​the inorganic mineral before crushing is 0.10 to 0.80.

Citation Information

Patent Citations

  • Phosphoaluminate cement-based chloride ion curing agent

    CN108455961A

  • Fire-proof composition

    JP2003128450A

  • Cement composition for spraying

    JP2018172264A

  • Cement composition

    JP2023131119A

  • Fregocement made from a new earth-inspired clinker

    JP2023505199A

Cited By

  • Allophane-containing composition and method for producing the same, and hydraulic composition and method for producing the same

    JP2026161012A

  • Cement composition and method for producing the same, and allophane-containing composition