Curable silicone composition, cured object formed from same, and method for producing same

The curable silicone composition, featuring thermosetting silicone, functional inorganic filler, and polyolefin wax, addresses the challenges of high fluidity, gap fill, and adhesion in semiconductor encapsulation by providing a homogenous and efficient molding solution with enhanced demoldability and adhesion properties.

WO2024236999A1PCT designated stage expired Publication Date: 2024-11-21DOW TORAY CO LTD
View PDF 39 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015276
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-04-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing hot-melt curable silicone compositions face challenges in achieving high fluidity and gap fill properties at high temperatures, uniformity, and strong adhesion to substrates while maintaining demoldability during molding processes, particularly in semiconductor device encapsulation, due to limitations in wax component optimization and the presence of functional inorganic fillers.

Method used

A curable silicone composition comprising thermosetting silicone, functional inorganic filler, and polyolefin wax with specific melting point and viscosity characteristics, which is homogenized by melt-kneading and formed into granules or tablets, enabling excellent hot-melt properties, gap fill capabilities, and strong adhesion, suitable for transfer, compression, and press molding processes.

Benefits of technology

The composition exhibits high fluidity and uniformity at high temperatures, ensures strong adhesion to substrates, and improves demoldability, enhancing production efficiency and homogeneity in semiconductor device encapsulation and sealing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

[Problem] To provide: a curable silicone composition that can contain a functional inorganic filler in a large amount, has hot-melt properties and gap-filling properties, which are characterized by high flowability at high temperatures, and gives a cured object having excellent homogeneity, the cured object having satisfactory demoldability, and that is suitable for use in molding, e.g., transfer molding, and in sealing processes, is less apt to generate dust, and has excellent handleability; and a method for producing the curable silicone composition with excellent production efficiency and homogeneity. [Solution] The curable silicone composition has hot-melt properties and comprises (A) a heat-curable silicone, (B) a functional inorganic filler, and (C) a polyolefin-based wax having a melting point of 130°C or lower and a viscosity of 100 mPas or higher at 140°C, and preferably may further contain (D) a wax having a melting point of 130°C or lower and a viscosity of less than 100 mPas at 140°C. Also provided is a use of the curable silicone composition.
Need to check novelty before this filing date? Find Prior Art

Description

Curable silicone composition, cured product thereof, and method for producing the same

[0001] The present invention relates to a curable silicone composition that has hot-melt properties, high fluidity and gap-filling properties at high temperatures, excellent demoldability during molding, and provides a cured product that exhibits strong adhesion to substrates. The present invention also relates to a cured product made from the curable silicone composition, a molding method for this cured product, and uses such as semiconductor devices that include this cured product. In this invention, the property of being solid at 25°C but exhibiting viscosity at 180°C is referred to as "hot-melt properties."

[0002] Curable silicone compositions are used in a wide range of industrial fields because they cure to form cured products with excellent heat resistance, cold resistance, electrical insulation, weather resistance, water repellency, and transparency. Cured products of such curable silicone compositions are generally less susceptible to discoloration than other organic materials, and also suffer less deterioration in physical properties, making them suitable as sealants for optical materials and semiconductor devices. Meanwhile, in recent years, from the standpoint of ease of handling and workability, hot-melt curable silicone compositions have been widely used as sealants for optical materials and semiconductor devices.

[0003] In Patent Documents 1 and 2, the applicant has proposed hot-melt granular curable silicone compositions for molding that are primarily composed of resinous silicone and can be used for the applications described above, and that can be applied to transfer molding processes when made into pellet or tablet form. However, when these compositions are used in transfer molding, there is the problem that, depending on the shape of the mold, they can be difficult to remove from the mold after molding.

[0004] A common method for improving demoldability during molding is to add a small amount of wax to a composition. Patent Documents 1 to 4 disclose that adding a common wax is acceptable. However, depending on the type and amount of wax added, these wax components can improve demoldability during molding, but at the same time, they can also result in a loss of adhesive strength in the cured product. Therefore, the type and amount of wax added must be optimized, but the above documents do not disclose this information. Patent Document 5 discloses that moisture-curable hot-melt silicone adhesive compositions may contain "plasticizers, non-reactive waxes, reactive waxes, tackifier resins, and combinations thereof" as optional components (rheological aids for improving melt viscosity, etc.). However, Patent Document 5 does not disclose or suggest the use of a thermosetting silicone in combination with a specific wax, or a composition that can incorporate a large amount of functional inorganic filler. Furthermore, because the composition is moisture-curing, the cure speed and the mechanical strength of the cured product may be insufficient. In addition, Patent Document 5 does not disclose or suggest fast-curing thermosetting silicones that contain a specific branched silicone as the base component and a large amount of a specific wax or combination thereof, or a functional filler.

[0005] International Publication No. 2018 / 030288 Pamphlet International Publication No. 2018 / 235491 Pamphlet International Publication No. 2018 / 235492 Pamphlet Japanese Patent No. 4964928 Publication No. 2016-514172

[0006]

[0003] The object of the present invention is to provide a curable silicone composition that can contain large amounts of functional inorganic filler, that has excellent hot-melt properties (characterized by high fluidity at high temperatures), gap-filling properties, and uniformity, and that gives a cured product that exhibits strong adhesive strength, that is suitable for use in molding or encapsulation processes such as transfer molding, compression molding, and press molding, and that has excellent demoldability during molding, and a method for producing the same that is excellent in production efficiency and uniformity. Furthermore, the present invention also provides a cured product obtained by curing the curable silicone composition, a semiconductor device component made of the cured product, a semiconductor device comprising the cured product, and a method for molding the cured product.

[0007] As a result of extensive research, the present inventors discovered that the above-mentioned problems could be solved by a curable silicone composition comprising (A) a thermosetting silicone, (B) a functional inorganic filler, and (C) a polyolefin wax having a melting point of 130°C or lower and a viscosity at 140°C of 100 mPas or higher, wherein the amount of component (B) is 40 parts by mass or higher per 100 parts by mass of component (A), and the composition as a whole exhibits hot-melt properties, and thus completed the present invention.

[0008] The composition may further contain (D) a wax having a melting point of 130°C or lower and a viscosity at 140°C of less than 100 mPas, and the component (A) may be (A1) RSiO 3/2 The silicone may be a thermosetting silicone comprising at least an organopolysiloxane resin containing siloxane units represented by the formula (wherein R is a monovalent hydrocarbon group) in an amount of at least 20 mol % of all siloxane units, and (A2) a curing agent.

[0009] The composition may be melt-kneaded in a temperature range of 50 to 150° C. to homogenize the composition and then molded into granules. The composition of the present invention may also be compressed (particularly including tableting) into pellets or tablets.

[0010] The above problems are also solved by a cured product of the above curable silicone composition, its use as a semiconductor device component, and a method for molding the cured product.

[0011] The present invention can provide a curable silicone composition that contains a high content of functional inorganic filler and exhibits high fluidity at high temperatures, thereby forming a cured product that exhibits excellent hot-melt properties, gap-filling properties, and uniformity and that firmly adheres to substrates. Because of these properties, the curable silicone composition can be suitably used in molding or encapsulation processes such as transfer molding, compression molding, and press molding. Furthermore, the composition exhibits excellent demoldability during molding, making it possible to provide a method for producing such a cured product with excellent production efficiency and uniformity. The present invention can also provide a cured product obtained by curing the curable silicone composition, a semiconductor device component made of the cured product, a semiconductor device having the cured product, and a method for molding the cured product.

[0012] [Curable Silicone Composition] The curable silicone composition of the present invention has the following compositional features and, as a result, the entire composition has hot-melt properties. The composition is solid at room temperature, but from the standpoint of ease of handling and moldability, it may be a granular composition, and may be, and is preferably, in the form of a pellet or tablet molded product obtained by compression molding this.

[0013] The curable silicone composition of the present invention comprises: (A) a thermosetting silicone; (B) a functional inorganic filler; and (C) a polyolefin wax having a melting point of 130°C or lower and a viscosity at 140°C of 100 mPas or higher, wherein the content of component (B) is 40 parts by mass or higher per 100 parts by mass of component (A), and the composition as a whole is characterized by exhibiting hot-melt properties. However, the composition may also contain component (D) described below and other optional components as necessary.

[0014] [Component (A)] Component (A) is the main component of the composition and is a silicone component that exhibits thermosetting properties. As long as it exhibits thermosetting properties, it may be a single component or a mixture of several components. Furthermore, the thermosetting functional group may be of one type or two or more types.

[0015] Component (A) preferably has a thermosetting reactive functional group, such as a hydrosilylation reactive group or a radical reactive group. Examples of hydrosilylation reactive groups include alkenyl groups having 2 to 20 carbon atoms, such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, and dodecenyl, as well as silicon-bonded hydrogen atoms. The hydrosilylation reactive group is preferably an alkenyl group. This alkenyl group may be linear or branched, and is preferably a vinyl group or a hexenyl group. Component (A) preferably has at least two hydrosilylation reactive groups per molecule.

[0016] Examples of groups bonded to silicon atoms in component (A) other than hydrosilylation reactive groups include alkyl groups having 1 to 20 carbon atoms such as methyl groups, halogen-substituted alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 20 carbon atoms such as phenyl groups, halogen-substituted aryl groups having 6 to 20 carbon atoms, aralkyl groups having 7 to 20 carbon atoms, alkoxy groups, and hydroxyl groups. Methyl groups, phenyl groups, and hydroxyl groups are particularly preferred.

[0017] Examples of radically reactive groups in component (A) include alkyl groups having 1 to 20 carbon atoms, such as methyl groups; alkenyl groups having 2 to 20 carbon atoms, such as vinyl groups and hexenyl groups; acrylic-containing groups, such as 3-acryloxypropyl groups and 4-acryloxybutyl groups; methacrylic-containing groups, such as 3-methacryloxypropyl groups and 4-methacryloxybutyl groups; and silicon-bonded hydrogen atoms. Alkenyl groups are preferred as this radically reactive group. These alkenyl groups may be linear or branched, and are preferably vinyl or hexenyl groups. It is preferred that component (A) have at least two radically reactive groups per molecule.

[0018] Examples of groups bonded to silicon atoms in component (A) other than radical reactive groups include halogen-substituted alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 20 carbon atoms, halogen-substituted aryl groups having 6 to 20 carbon atoms, aralkyl groups having 7 to 20 carbon atoms, alkoxy groups, and hydroxyl groups, including the same groups as those listed above. Phenyl groups and hydroxyl groups are particularly preferred. It is particularly preferred that component (A) have aryl groups, especially phenyl groups, accounting for 10 mol % or more of all organic groups in the molecule.

[0019] From the viewpoint of imparting practical hot-melt properties and thermosetting properties to the present composition, the component (A) is: (A1) RSiO 3/2 The composition preferably comprises at least an organopolysiloxane resin containing siloxane units represented by the formula (wherein R is a monovalent hydrocarbon group) in an amount of at least 20 mol % of all siloxane units, and (A2) a curing agent.

[0020] [Component (A1)] The component (A1) is RSiO 3/2 (wherein R is a monovalent hydrocarbon group), and has the above-mentioned thermosetting functional group within the molecule. From the viewpoint of the curing speed of the resulting composition, it is preferable that the thermosetting functional group in component (A1) undergoes either a hydrosilylation reaction or a radical reaction, or both. Furthermore, it is preferable that component (A1) be an organopolysiloxane resin component that has a softening point of 30°C or higher and that itself has hot-melt properties.

[0021] [Component (A1-1)] Component (A1) is a hot-melt organopolysiloxane resin having a softening point of 30°C or higher and containing carbon-carbon double bond groups (hydrosilylation reactive groups and / or radical reactive groups) in the molecule, and RSiO 3/2(wherein R is a monovalent hydrocarbon group) preferably accounts for at least 20 mol % of all siloxane units. Furthermore, component (A1) is preferably (A1-1-1), a hot-melt organopolysiloxane resin in which at least 10 mol % of the silicon-bonded organic groups are aryl groups.

[0022] Suitable examples of such component (A1-1) include MT resins, MDT resins, MTQ resins, MDTQ resins, TD resins, TQ resins, and TDQ resins, which are composed of any combination of triorganosiloxy units (M units) (the organo groups are methyl groups only, methyl groups and the above-mentioned curable functional groups, or phenyl groups), diorganosiloxy units (D units) (the organo groups are methyl groups only, methyl groups and the above-mentioned curable functional groups, or phenyl groups), monoorganosiloxy units (T units) (the organo groups are methyl groups, the above-mentioned curable functional groups, or phenyl groups), and siloxy units (Q units), in which the content of T units is at least 20 mol% of the total siloxane units. It is preferable that component (A1) contains curing-reactive functional groups (hydrosilylation-reactive groups and / or radical-reactive groups) containing at least two carbon-carbon double bonds in the molecule, and that 10 mol % or more of all silicon-bonded organic groups in the molecule be aryl groups, particularly phenyl groups.

[0023] Preferably, the component (A1-1) is one of the following (R 1 3 SiO 1/2 ) a (R 2 2 SiO 2/2 ) b (R 3 SiO 3/2 ) c (SiO 4/2 ) d (R 4 O 1/2)e It is an organopolysiloxane that is solid at room temperature but softens as the temperature rises, exhibiting hot-melt properties.

[0024] In the formula, each R 1 , R 2 , R 3are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that at least two of all R in one molecule must be the above-mentioned curing reactive functional groups, and 70 mol % or more of all curing reactive functional groups must be R 1 It is preferable that R 4 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; and a, b, c, d, and e are numbers that satisfy the following: (0.10≦a≦0.40, 0≦b≦0.50, 0.20≦c≦0.90, 0≦d≦0.20, 0≦e≦0.05, with the proviso that a+b+c+d=1).

[0025] The preferred content of the curing reactive functional group is 10 to 20 mol% of the total R component. Below this range, a cured product exhibiting sufficient strength cannot be obtained, while above this range, the cured product tends to be hard and brittle. The curing reactive functional group is preferably an alkenyl group, and examples thereof include a vinyl group, an allyl group, a butenyl group, a pentenyl group, and a hexenyl group. From the viewpoint of imparting suitable hot melt properties to this component, it is preferred to use an alkenyl group containing 10 to 20 mol% of the curing reactive functional group. 1 , R 2 , R 3 At least a part of the groups is preferably an aryl group, more preferably a phenyl group. Examples of other monovalent hydrocarbon groups include a methyl group.

[0026] Furthermore, in the formula, a represents a group represented by the general formula: R 1 3 SiO 1 / 2 is a number that indicates the proportion of siloxane units represented by the formula: R 2 2 SiO 2 / 2 and is a number that satisfies the relationship 0≦b≦0.5. This is because good hot melt properties can be obtained when b is equal to or less than the upper limit of the above range. Furthermore, c is a number that indicates the proportion of siloxane units represented by the general formula: R 3 SiO 3 / 2is a number that indicates the proportion of siloxane units represented by the general formula: SiO 4 / 2 is a number that indicates the proportion of siloxane units represented by the formula: R, and is a number that satisfies 0≦d≦0.20, preferably 0≦d≦0.10. This is because when d is equal to or less than the upper limit of the above range, the mechanical strength of the resulting cured product is good. 2 O 1 / 2 is a number indicating the proportion of units represented by the formula a, b, c, and d, and satisfies the condition 0≦e≦0.05. This is because when e is equal to or less than the upper limit of the above range, the hardness of the resulting cured product at room temperature is good. In the formula, the sum of a, b, c, and d is 1.

[0027] Component (A1) exhibits hot-melt properties; specifically, it is non-flowable at 25°C, and has a melt viscosity at 150°C of 8000 Pa s or less, preferably 5000 Pa s or less, and more preferably in the range of 10 to 3000 Pa s. "Non-flowable" means that it does not flow under no load, and refers to a state below the softening point measured by the ring and ball softening point test method for hot-melt adhesives specified in JIS K 6863-1994 "Softening Point Test Method for Hot-Melt Adhesives." In other words, in order to be non-flowable at 25°C, the softening point must be higher than 25°C.

[0028] Component (A), preferably component (A1), and more preferably component (A1-1), may be an organosiloxane resin of any molecular weight as long as it exhibits the structure and melting properties described above. For example, an organopolysiloxane having the structure described above may be used in which some of the curing-reactive functional groups (e.g., alkenyl groups) are crosslinked with component (A2) described below to increase the molecular weight, but from the perspective of the melting properties of the resulting composition, the molecular weight (Mw) is preferably 20,000 g / mol or less.

[0029] As described above, the component (A1), preferably the component (A1-1), is a solid at room temperature. Therefore, from the viewpoint of ease of handling when mixed with other components, it is preferable to use the component (A1) as a fine particle resin or to dissolve the component (A1-1) in other components required for the present composition and use the resulting liquid mixture.

[0030] When component (A1), preferably component (A1-1), is used in the form of fine particles, the particle size is not limited, but the average primary particle size is preferably within the range of 1 to 5,000 μm, 1 to 500 μm, 1 to 100 μm, 1 to 20 μm, or 1 to 10 μm. This average primary particle size can be determined, for example, by observation with an optical microscope or SEM. The shape of the fine particle (A1) component is not limited, and examples include spherical, spindle-shaped, plate-shaped, needle-shaped, and irregular shapes. Spherical or true spherical shapes are preferred because they melt uniformly. In particular, by forming component (A1) into true spherical fine particles, the process of producing the present composition by powder mixing or melt-kneading, as described below, can be carried out efficiently.

[0031] When component (A1) is microparticulated, the production method is not limited, and known methods can be used. When obtaining microparticulate component (A1), a hydrosilylation reaction catalyst, which is component (A2) described below, may also be microparticulated together with component (A1), and this is preferred.

[0032] Specific methods for microparticulating component (A1) include pulverizing component (A1), which is solid at room temperature, using a pulverizer, and directly microparticulating component (A1) in the presence of a solvent. The pulverizer is not limited, and examples include a roll mill, a ball mill, a jet mill, a turbo mill, and a planetary mill. Alternatively, component (A1) may be directly microparticulated in the presence of a solvent, for example, by spraying with a spray dryer, or by microparticulation with a twin-screw kneader or belt dryer. When microparticulating component (A1), it is preferable to obtain spherical hot-melt organopolysiloxane resin microparticles by spraying with a spray dryer.

[0033] By using a spray dryer or the like, it is possible to produce component (A1) that is spherical and has an average primary particle size of 1 to 500 μm. The heating and drying temperature of the spray dryer must be appropriately set based on the heat resistance of the organopolysiloxane resin microparticles. In order to prevent secondary aggregation of the organopolysiloxane resin microparticles, it is preferable to control the temperature of the organopolysiloxane resin microparticles below their glass transition temperature. The organopolysiloxane resin microparticles obtained in this manner can be recovered using a cyclone, bag filter, or the like.

[0034] To obtain a uniform component (A1), a solvent may be used in the above step as long as it does not inhibit the curing reaction. The solvent is not limited, but examples include aliphatic hydrocarbons such as n-hexane, cyclohexane, and n-heptane; aromatic hydrocarbons such as toluene, xylene, and mesitylene; ethers such as tetrahydrofuran and dipropyl ether; silicones such as hexamethyldisiloxane, octamethyltrisiloxane, and decamethyltetrasiloxane; esters such as ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate; and ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone.

[0035] Furthermore, when a silicone compound that is liquid at room temperature is used as all or part of the component (A2) described below, the component (A1) may be dissolved in part of the component (A2). Liquid silicone compounds exhibit a certain degree of mutual solubility with the component (A1), and the component (A1) can be dissolved by adding, for example, 10 to 50 parts by mass of a part of the component (A2) per 100 parts by mass of the component (A1). By liquefying the component (A1), it is possible to efficiently produce the present composition described below by powder mixing or melt kneading.

[0036] [Component (A2)] Component (A2) is a curing agent for curing component (A1), and is not limited as long as it can cure component (A1). When component (A1) contains a curable functional group containing a carbon-carbon double bond, such as an alkenyl group, component (A2) is an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule and a hydrosilylation catalyst. When component (A1) contains an alkenyl group and a hydrosilylation catalyst, component (A2) may be an organopolysiloxane having at least two silicon-bonded hydrogen atoms per molecule alone, or may be used in combination with a hydrosilylation catalyst. Furthermore, when component (A1) contains an alkenyl group, component (A2) may be an organic peroxide, or may be used in combination with an organopolysiloxane having at least two silicon-bonded hydrogen atoms per molecule. On the other hand, when component (A1) contains silicon-bonded hydrogen atoms, component (A2) is an organopolysiloxane having a curable functional group containing at least two carbon-carbon double bonds, such as alkenyl groups, per molecule, and a hydrosilylation catalyst. When component (A1) contains silicon-bonded hydrogen atoms and contains a hydrosilylation catalyst, component (A2) may consist solely of an organopolysiloxane having a curable functional group containing at least two carbon-carbon double bonds, such as alkenyl groups, per molecule, although a hydrosilylation catalyst may also be used in combination. Furthermore, when component (A1) contains reactive silanol groups, a condensation catalyst may also be used. Note that when a condensation reaction is used as the curing reaction, a known thermal base generator or the like may be used as part of component (A2).

[0037] As mentioned above, component (A2) contains a curing catalyst suited to the selected reaction system, and for the purpose of achieving compositional uniformity, the composition of the present invention is preferably homogenized by melt kneading or the like in a temperature range of 50 to 150°C, and preferably in a temperature range of 50 to 120°C. Therefore, from the standpoint of suppressing unintended curing reactions and maintaining the curing reactivity of the curable silicone composition of the present invention, component (A2) preferably contains a curing catalyst that is not active unless it is stimulated by a certain amount of thermal energy; specifically, a curing agent containing a curing reaction catalyst that becomes active in the composition when stimulated by thermal energy at 80°C or higher, preferably 100°C or higher, and more preferably 120°C or higher, and a curing catalyst that does not initiate a curing reaction below these temperatures is particularly preferred.

[0038] More specifically, component (A2) preferably contains one or more curing catalysts selected from (A2-1) organic peroxides having a 10-hour half-life at a temperature of 80° C. or higher, and (A2-2) hydrosilylation reaction catalyst-containing thermoplastic resin microparticles containing a thermoplastic resin having a softening point or glass transition point of 80° C. or higher, or a combination thereof. This is because, by using component (A2-1) or (A2-2) as part of the curing agent, unintended curing reactions can be effectively suppressed, even when the composition is homogenized and granulated by a process involving heating, such as melt-kneading, and the resulting granular composition can exhibit both good hot-melt properties and high-temperature curing properties.

[0039] Component (A2-1) is a curing agent that is preferably used when a radical reaction is used as the curing reaction for the present composition, and is preferably an organic peroxide that has a 10-hour half-life at a temperature of 90° C. or higher, or 95° C. or higher. Examples of such organic peroxides include dicumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, t-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,3-bis(tert-butylperoxyisopropyl)benzene, di-(2-t-butylperoxyisopropyl)benzene, and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane.

[0040] There are no restrictions on the amount of organic peroxide contained, but it is preferable that the amount be within a range of 0.05 to 10 parts by weight, or within a range of 0.10 to 5.0 parts by weight, per 100 parts by weight of component (A1).

[0041] Component (A2-2) is a part of a curing agent suitable for use when a hydrosilylation reaction is used as the curing reaction for the present composition. It may be either fine particles in which a platinum-based catalyst is dissolved or dispersed in a thermoplastic resin, or microcapsule fine particles in which a platinum-based catalyst is contained as a core within a thermoplastic resin shell. Examples of platinum-based catalysts include platinum black, platinum-supported carbon fine powder, platinum-supported silica fine powder, chloroplatinic acid, alcohol-modified chloroplatinic acid, platinum olefin complexes, and platinum alkenylsiloxane complexes. The thermoplastic resin used in component (A2-2) is not particularly limited as long as it is substantially impermeable to the platinum-based catalyst at least during production and storage of the present composition and is substantially soluble in the organopolysiloxane, the main component of the present composition. However, the softening point or glass transition point of this thermoplastic resin is preferably 80°C or higher, and more preferably 120°C or higher. Specifically, silicone resins, polysilane resins, epoxy resins, acrylic resins, methylcellulose resins, and polycarbonate resins are suitable, but they must have low solubility in the present composition. The softening point is the temperature at which the resin begins to flow under its own weight or surface tension, and can be measured by observing pulverized particles under a microscope while increasing the temperature at a constant rate. The glass transition point can also be measured using a differential scanning calorimeter (DSC). In the present invention, it is preferable that either the softening point or the glass transition point is 120°C or higher. This is because if the softening point or glass transition point of the thermoplastic resin is below 120°C, there is a risk that the platinum component will begin to leach out during the process of homogenizing the present composition, as described below. The average particle size of the platinum-based catalyst-containing thermoplastic microparticles is not limited, but is preferably within the range of 0.1 to 500 μm, and more preferably within the range of 0.3 to 100 μm. This is because it is difficult to prepare platinum-based catalyst-containing thermoplastic resin microparticles with an average particle size below the lower limit of the above range, while if the average particle size exceeds the upper limit of the above range, dispersibility in the curable silicone resin composition decreases.

[0042] The method for preparing such platinum-based catalyst-containing thermoplastic resin microparticles is not limited, and examples include conventionally known chemical methods such as interfacial polymerization and in-situ polymerization, as well as physical and mechanical methods such as coacervation and submerged drying. Submerged drying and vapor-phase drying are particularly desirable because they allow for the relatively easy production of microcapsule microparticles with a narrow particle size distribution. While the microparticles obtained by these methods can be used as is, it is desirable to wash them with an appropriate cleaning solvent to remove the platinum-based catalyst adhering to their surface in order to obtain a curable silicone resin composition with excellent storage stability. A suitable cleaning solvent is one that does not dissolve the thermoplastic resin but dissolves the platinum-based catalyst. Examples of such cleaning solvents include alcohols such as methyl alcohol and ethyl alcohol, and low-molecular-weight organopolysiloxanes such as hexamethyldisiloxane. The ratio of the hydrosilylation catalyst to the thermoplastic resin varies significantly depending on the method for producing the granules, so no particular limitation can be placed on it. However, it is preferable for the platinum-based catalyst content to be 0.01% by mass or greater relative to the thermoplastic resin. This is because if the platinum catalyst content is less than 0.01% by mass, the physical properties of the cured product will be impaired unless the composition contains a large amount of platinum catalyst-containing thermoplastic resin particles.

[0043] The amount of the hydrosilylation catalyst added is preferably an amount that provides a metal atom concentration, by mass, of 0.01 to 500 ppm, 0.01 to 100 ppm, or 0.01 to 50 ppm, relative to the entire composition.

[0044] When a hydrosilylation reaction is used as the curing reaction for the present composition, component (A2) may contain, in addition to a hydrosilylation reaction catalyst (preferably the aforementioned component (A2-2)), an organosiloxane component other than component (A1) as a hydrosilylation crosslinking component, and preferably contains (A2-3) an organohydrogenpolysiloxane. The structure is not particularly limited and may be linear, branched, cyclic, or resinous, but from the viewpoint of excellent curing properties of the resulting composition, it is preferable to use an organohydrogenpolysiloxane having an HR group at the terminal. 2 SiO 1/2Hydrogen diorganosiloxy units (M H Preferably, the organohydrogenpolysiloxane has a unit (R) independently representing a monovalent organic group.

[0045] More specifically, the organohydrogenpolysiloxane (A2-3) serving as the hydrosilylation crosslinking component is preferably an organopolysiloxane in which 20 to 70 mol % of all silicon-bonded organic groups are phenyl groups. This is because when the phenyl group content is at least the lower limit of the above range, the resulting cured product has good mechanical strength at high temperatures, while when it is at most the upper limit of the above range, the resulting cured product has good mechanical strength.

[0046] Component (A2-3) contains two or more silicon-bonded hydrogen atoms per molecule, which provides sufficient crosslinking reactivity for curing and results in good hardness of the resulting cured product. Examples of silicon-bonded organic groups in component (A2-3) include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, and xylyl; and aralkyl groups such as benzyl and phenethyl. Of these, phenyl and alkyl groups having 1 to 6 carbon atoms are preferred.

[0047] Examples of such component (A2-3) include: (A2-3-1) a compound represented by the general formula: HR 4 2 SiO(R 4 2 SiO) n SI 4 2 and (A2-3-2) a linear organopolysiloxane represented by the average unit formula: (R 4 SiO 3/2 ) p (R 4 2 SiO 2/2 ) q (HR 4 2 SiO 1/2 ) r (SiO 4/2 ) s(XO 1/2 ) t It is preferable to use a combination of these two types of component (A2-3) as the hydrosilylation crosslinking component.

[0048] In the formula, R 4 are the same or different and are phenyl groups or alkyl groups having 1 to 6 carbon atoms. 4 Examples of the alkyl group of R include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a cyclopentyl group, and a cyclohexyl group. 4 The content of phenyl groups is in the range of 30 to 70 mol %.

[0049] In the formula, n is an integer in the range of 5 to 1,000. In the formula, p is a positive number, q is 0 or a positive number, r is a positive number, s is 0 or a positive number, t is 0 or a positive number, q / p is a number in the range of 0 to 10, r / p is a number in the range of 0.1 to 5, s / (p+q+r+s) is a number in the range of 0 to 0.3, and t / (p+q+r+s) is a number in the range of 0 to 0.4.

[0050] In the case of such component (A2-3), it is preferable to use a combination of components (A2-3-1) and (A2-3-2) from the viewpoint of easy control of the curing rate of the composition and the crosslink density of the resulting cured product. The ratio of the two components, per alkenyl group in the entire composition, is preferably (A2-3-1):(A2-3-2)=0.05-0.6:0.4-0.95, more preferably 0.05-0.5:0.5-0.95, and even more preferably 0.05-0.4:0.5-0.95.

[0051] When the above-mentioned organohydrogenpolysiloxane is used as part of component (A2), there are no restrictions on its content, but in order to cure the composition, it is preferable that the amount be in the range of 0.5 to 20 moles, or 1.0 to 10 moles, of silicon-bonded hydrogen atoms per mole of alkenyl groups in the composition. The amount of hydrosilylation reaction catalyst used is as described above.

[0052] In the composition of the present invention, a particularly suitable component (A2) is one that contains the above-mentioned components (A2-2), (A2-3-1), and (A2-3-2). This composition as a whole effectively suppresses side reactions and unintended curing reactions, and has the advantages of excellent hot-melt properties and heat-curing properties at high temperatures.

[0053] [Component (B)] The component (B) of the present invention is a functional inorganic filler that can impart functionality to the cured product depending on the type of inorganic filler. In particular, it can provide a curable silicone composition that cures to give a cured product with excellent hardness and toughness at room temperature to high temperatures. In the present invention, the above-mentioned properties can be achieved by adding 40 parts by mass or more of component (B) per 100 parts by mass of component (A). If a harder and tougher cured product is desired, the component (B) can be blended in a range of 100 to 3,000 parts by mass, 500 to 3,000 parts by mass, or 800 to 3,000 parts by mass. By selecting component (A), it is possible to achieve a low melt viscosity suitable for encapsulation, transfer molding, compression molding, and press molding, even when component (B) is highly loaded.

[0054] From the standpoint of achieving a low average linear expansion coefficient for the cured product of the curable silicone composition of the present invention, the content of component (B) is preferably at least 50% by volume of the entire composition, more preferably at least 60% by volume, even more preferably at least 70% by volume, and especially preferably in the range of 80 to 95% by volume.

[0055] To achieve the above blending amounts and a low average linear expansion coefficient for the resulting cured product, it is preferable that the (B) component be treated with a specific surface treatment agent (B' component), particularly 0.1 to 2.0 mass%, 0.1 to 1.0 mass%, or 0.2 to 0.8 mass% of the (B' component) based on the total mass of the (B) component. Treating the (B) component with the above treatment amount of the (B' component) has the advantage of allowing a high volume percentage of the (B) component to be stably blended into the composition. Furthermore, any surface treatment method can be used, and any desired method can be used, such as a homogeneous mixing method using mechanical force (dry method) or a wet mixing method using a solvent.

[0056] Examples of these (B') components include fluorine compounds such as methylhydrogenpolysiloxane, silicone resin, metal soap, silane coupling agent, perfluoroalkylsilane, and perfluoroalkyl phosphate ester salt, among others. Silicone-based surface treatment agents are particularly preferred, as described below. Selecting a silane-based surface treatment agent such as methyltrimethoxysilane or phenyltrimethoxysilane as the (B') component may impair the hot-melt properties of the entire composition, and may also prevent the (B) component from being stably blended up to the volume percent content described above. Selecting an alkyltrialkoxysilane having a long-chain alkyl group such as an octyl group as the surface treatment agent tends to maintain the hot-melt properties of the composition and the blending stability of the (B) component, but may result in a deterioration in the strength of the cured product obtained by curing the composition of the present invention, which may lead to cracking or molding defects.

[0057] Here, examples of the organosilicon compound of component (B') include low molecular weight organosilicon compounds such as silane, silazane, siloxane or the like, and organosilicon polymers or oligomers such as polysiloxane, polycarbosiloxane or the like.Preferred examples of silanes are so-called silane coupling agents.Representative examples of such silane coupling agents include alkyltrialkoxysilanes (methyltrimethoxysilane, vinyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane or the like), organic functional group-containing trialkoxysilanes (glycidoxypropyltrimethoxysilane, epoxycyclohexylethyltrimethoxysilane, methacryloxypropyltrimethoxysilane, aminopropyltrimethoxysilane or the like). Preferred siloxanes and polysiloxanes include hexamethyldisiloxane, 1,3-dihexyl-tetramethyldisiloxane, trialkoxysilyl single-terminated polydimethylsiloxane, trialkoxysilyl single-terminated dimethylvinyl single-terminated polydimethylsiloxane, trialkoxysilyl single-terminated organofunctional group single-terminated polydimethylsiloxane, trialkoxysilyl doubly-terminated polydimethylsiloxane, organofunctional group doubly-terminated polydimethylsiloxane, or the like. When siloxanes are used, the number n of siloxane bonds preferably ranges from 2 to 150. Examples of preferred silazanes include hexamethyldisilazane, 1,3-dihexyl-tetramethyldisilazane, or the like. Examples of preferred polycarbosiloxanes are polymers having Si-C-C-Si bonds within the polymer backbone.

[0058] Particularly preferred examples of the component (B') include silicone-based surface treatment agents having at least one polysiloxane structure and a hydrolyzable silyl group in the molecule. Most preferred is the use of a silicone-based surface treatment agent having at least one polysiloxane structure and a hydrolyzable silyl group in the molecule, represented by the structural formula (1): R' n (RO) 3-n SiO—(R′ 2 SiO)m -SiR' n (RO) 3-n or structural formula (2): R' 3 SiO—(R′ 2 SiO) m -SiR' n (RO) 3-n Examples include organopolysiloxanes having a linear alkoxysilyl end group represented by the formula: In this formula, R is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms (= methyl, ethyl, or propyl), and each R' is independently an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, examples of which are the same as those described above. n is a number ranging from 0 to 2, and m is a number ranging from 2 to 200, and may also be a number ranging from 2 to 150.

[0059] Component (B) is preferably at least one filler that has no softening point or that does not soften below the softening point of component (A1). It may also be a component that improves the handling and workability of the composition and imparts mechanical and other properties to the cured product of the composition. Examples of component (B) include reinforcing fillers, pigments (especially black or white pigments), thermally conductive fillers, electrically conductive fillers, phosphors, and mixtures of at least two of these. To achieve a high volumetric loading, it is preferable that 40% or more of the total component (B) contains reinforcing fillers with an average particle size of 10.0 μm or more. Examples of organic fillers include silicone resin-based fillers, fluororesin-based fillers, and polybutadiene resin-based fillers. The shape of these fillers is not particularly limited and may be spherical, spindle-shaped, flat, acicular, plate-like, or amorphous.

[0060] When the present composition is used as a sealant, protective agent, adhesive, light reflector, or the like, it is preferable to incorporate a reinforcing filler as component (B) to impart mechanical strength to the cured product and improve protective or adhesive properties. Examples of reinforcing fillers include fumed silica, precipitated silica, fused silica, calcined silica, fumed titanium dioxide, quartz, calcium carbonate, diatomaceous earth, aluminum oxide, aluminum hydroxide, zinc oxide, zinc carbonate, glass beads, glass powder, talc, clay, mica, kaolin, silicon carbide, silicon nitride, aluminum nitride, carbon black, graphite, titanium dioxide, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, barium sulfate, cellulose, and aramid. Furthermore, these reinforcing fillers may be surface-treated with an organoalkoxysilane such as methyltrimethoxysilane; an organohalosilane such as trimethylchlorosilane; an organosilazane such as hexamethyldisilazane; or a siloxane oligomer such as an α,ω-silanol group-blocked dimethylsiloxane oligomer, an α,ω-silanol group-blocked methylphenylsiloxane oligomer, or an α,ω-silanol group-blocked methylvinylsiloxane oligomer. Furthermore, as the reinforcing filler, fibrous inorganic fillers such as calcium metasilicate, potassium titanate, magnesium sulfate, sepiolite, zonolite, aluminum borate, rock wool, glass fiber, carbon fiber, asbestos fiber, metal fiber, wollastonite, attapulgite, sepiolite, aluminum borate whiskers, potassium titanate fiber, calcium carbonate whiskers, titanium oxide whiskers, and ceramic fiber; and fibrous fillers such as aramid fiber, polyimide fiber, and polyparaphenylene benzobisoxazole fiber may be used.Furthermore, plate-like fillers or granular fillers such as talc, kaolin clay, calcium carbonate, zinc oxide, calcium silicate hydrate, mica, glass flakes, glass powder, magnesium carbonate, silica, titanium oxide, alumina, aluminum hydroxide, magnesium hydroxide, barium sulfate, calcium sulfate, calcium sulfite, zinc borate, barium metaborate, aluminum borate, calcium borate, sodium borate, aluminum nitride, boron nitride, silicon nitride, and pulverized products of the above-mentioned fibrous fillers may also be used.

[0061] In particular, from the standpoint of imparting hardness to the present composition at room temperature to high temperatures in the cured product, it is preferred that component (B) be spherical silica or aluminum oxide (alumina) having an average particle size of 10.0 μm or more.

[0062] Component (B) may contain silicone microparticles that do not have hot-melt properties, which can improve or, if desired, adjust stress relaxation properties, etc. Examples of silicone microparticles include non-reactive silicone resin microparticles and silicone elastomer microparticles, with silicone elastomer microparticles being a preferred example from the standpoint of improving flexibility or stress relaxation properties.

[0063] Silicone elastomer microparticles are crosslinked products of linear diorganopolysiloxanes mainly composed of diorganosiloxy units (D units). Silicone elastomer microparticles can be prepared by crosslinking diorganopolysiloxanes through hydrosilylation reactions or silanol group condensation reactions. Among these, they can be suitably obtained by crosslinking an organohydrogenpolysiloxane having silicon-bonded hydrogen atoms in the side chain or at the end with a diorganopolysiloxane having unsaturated hydrocarbon groups such as alkenyl groups in the side chain or at the end in the presence of a hydrosilylation catalyst. Silicone elastomer microparticles can take various shapes, such as spherical, flat, and irregular, but from the viewpoint of dispersibility, spherical is preferred, and true spheres are even more preferred. Examples of commercially available silicone elastomer microparticles (B) include the "Trefil E Series" and "EP Powder Series" manufactured by Toray Dow Corning Co., Ltd., and the "KMP Series" manufactured by Shin-Etsu Chemical Co., Ltd. The silicone elastomer particles may be surface-treated. The elastomer particles may be made of acrylonitrile butadiene rubber, isoprene, styrene butadiene rubber, ethylene propylene rubber, or the like.

[0064] Furthermore, when the present composition is used as a wavelength conversion material for LEDs, a phosphor may be blended as component (B) to convert the wavelength of light emitted from an optical semiconductor element. The phosphor is not particularly limited, and examples thereof include yellow-, red-, green-, and blue-emitting phosphors composed of oxide-based phosphors, oxynitride-based phosphors, nitride-based phosphors, sulfide-based phosphors, oxysulfide-based phosphors, and the like, which are widely used in light-emitting diodes (LEDs). Examples of oxide-based phosphors include yttrium-, aluminum-, and garnet-based YAG-based green- to yellow-emitting phosphors containing cerium ions; terbium-, aluminum-, and garnet-based TAG-based yellow-emitting phosphors containing cerium ions; and silicate-based green- to yellow-emitting phosphors containing cerium and / or europium ions. Examples of oxynitride-based phosphors include silicon-, aluminum-, oxygen-, and nitrogen-based sialon-based red- to green-emitting phosphors containing europium ions. Examples of nitride-based phosphors include calcium, strontium, aluminum, silicon, and nitrogen-based red-emitting phosphors containing europium ions. Examples of sulfide-based phosphors include ZnS-based green-emitting phosphors containing copper ions or aluminum ions. Examples of oxysulfide-based phosphors include YS-based phosphors containing europium ions. 2 O 2 S-based red-emitting phosphors are exemplified. In the present composition, two or more of these phosphors may be used in combination.

[0065] Furthermore, the present composition may contain a thermally conductive filler or an electrically conductive filler to impart thermal conductivity or electrical conductivity to the cured product. Examples of such thermally conductive fillers or electrically conductive fillers include fine metal powders such as gold, silver, nickel, copper, aluminum, tin, lead, zinc, bismuth, and antimony; fine powders obtained by vapor-depositing or plating metals such as gold, silver, nickel, and copper on the surface of fine powders such as ceramic, glass, quartz, and organic resin; metal compounds such as aluminum oxide, magnesium oxide, aluminum nitride, boron nitride, and zinc oxide; graphite, and mixtures of two or more of these. When electrical insulation is required for the present composition, metal oxide powders or metal nitride powders are preferred, and aluminum oxide powder, zinc oxide powder, and aluminum nitride powder are particularly preferred.

[0066] Furthermore, the composition may contain a pigment to impart color to the cured product, such as a white pigment, a black pigment, or other coloring agents.

[0067] The white pigment is a component that imparts whiteness to the cured product and improves light reflectivity. By incorporating this component, the cured product obtained by curing the composition can be used as a light-reflecting material for light-emitting / optical devices. Examples of white pigments include metal oxides such as titanium oxide, aluminum oxide, zinc oxide, zirconium oxide, and magnesium oxide; hollow fillers such as glass balloons and glass beads; and other white pigments such as barium sulfate, zinc sulfate, barium titanate, aluminum nitride, boron nitride, and antimony oxide. Titanium oxide is preferred due to its high light reflectance and hiding power. Aluminum oxide, zinc oxide, and barium titanate are also preferred due to their high light reflectance in the UV region. The average particle size and shape of the white pigment are not limited, but the average particle size is preferably within the range of 0.05 to 10.0 μm or 0.1 to 5.0 μm. The white pigment may also be surface-treated with a silane coupling agent, silica, aluminum oxide, or the like.

[0068] Examples of black pigments or other colorants include black titanium oxide, pitch (a residue obtained by distilling tar obtained by dry distillation of organic substances such as petroleum, coal, and wood), carbon black, acetylene black, and red iron oxide. Acetylene black is preferably used when it is desired to reduce the content of metal impurities. Black dyes such as anthraquinone dyes (sometimes written as "anthraquinone"), azine dyes, azo dyes, disazo dyes, and chromium complex dyes may also be contained, and when used in combination with yellow dyes such as methine dyes, disazo dyes, azocobalt complex dyes, and azochromium complex dyes, a color similar to that obtained using a black pigment can be achieved.

[0069] Furthermore, when it is desired to improve the laser marking properties of the resulting cured product, black titanium oxide and pitch can be suitably used. By using these, excessive absorption of laser energy by the pigment during laser marking can be suppressed. Therefore, excessively deep portions in the print due to loss of the pigment by the laser can be suppressed. Carbonization can also be easily suppressed. In other words, it is possible to suppress the variation in the maximum depth relative to the average depth and reduce the variation in the print depth profile.

[0070] Black titanium oxide is Ti n O (2n-1) (n is a positive integer). The black titanium oxide Ti used in this embodiment n O (2n-1) It is preferable to use a pigment having n of 4 or more and 6 or less. By making n 4 or more, the dispersibility of the pigment in the resin composition can be improved. On the other hand, by making n 6 or less, the laser marking property can be improved. Here, the pigment is black titanium oxide, and Ti 4 O 7 , Ti 5 O 9 , and Ti 6 O 11 It is preferable that the pigment contains at least one of the following. Pitch is a residue obtained by distilling tar obtained by dry distillation of organic substances such as petroleum, coal, and wood. The pitch used as a pigment is not particularly limited, but may be, for example, petroleum pitch or coal pitch. As the pitch, isotropic pitch, mesophase pitch, or mesophase microspheres produced by cooling mesophase pitch and separated as an insoluble component of quinoline can be used. Among these, mesophase microspheres are more preferably used from the viewpoint of improving laser marking properties and dispersibility in the encapsulating resin composition.

[0071] Furthermore, the composition may optionally contain a thermally expandable filler. The incorporation of a thermally expandable filler can improve the volumetric expansion coefficient of the composition of the present invention and may reduce uneven dispersion of the composition. Preferably, the thermally expandable filler has a core-shell structure, containing a volatile expanding agent within the shell of the core-shell structure. Here, a volatile expanding agent refers to a substance that generates gas at temperatures below the softening point of the shell. The thermally expandable filler has a structure in which a volatile expanding agent is encapsulated as a core agent within a shell with gas barrier properties. Therefore, the volatile expanding agent becomes gaseous upon exposure to heat, and the shell softens and expands. Examples of such components are exemplified in, for example, JP 2020-084094 A, and are available from Matsumoto Yushi Seiyaku Co., Ltd., such as FN-100SSD and FN-80GSD.

[0072] When the cured product obtained by curing the composition is used in magnetic components such as dust magnetic needles, coils, and electromagnetic shielding materials, magnetic particles may be included as component (B). Such magnetic particles contain one or more elements selected from the group consisting of Fe, Cr, Co, Ni, Ag, and Mn. In particular, soft magnetic particles may include magnetic particles made of iron (Fe), Fe—Si alloys, Fe—Al alloys, Fe—Ni alloys, Fe—Co alloys, Fe—Si—Al alloys, Fe—Si—Cr alloys, Fe—Cr alloys, carbonyl iron, stainless steel, etc. From the standpoint of availability, magnetic particles made of carbonyl iron may also be used. These magnetic particles may be surface-treated with a silane compound, titanate compound, aluminate compound, or a partial hydrolyzate thereof, as with the inorganic fillers described above, which may prevent deactivation of the curing catalyst or crosslinking agent and improve storage stability. In addition, these magnetic particles may have a surface coating layer containing a siloxane polymer, for example, by the method described in JP-A-2021-036013.

[0073] [Component (C)] Component (C) is one of the characteristic components of the curable silicone composition of the present invention. When the content of component (B) in the composition is 40 parts by mass or more per 100 parts by mass of component (A), component (C) is a component that improves demoldability during molding of the cured product obtained by curing the composition while achieving a high content of functional inorganic filler.

[0074] Specifically, component (C) is a polyolefin wax having a melting point of 130°C or lower and a melt viscosity at 140°C of 100 mPas or higher. Specific examples include polyethylene wax, oxidized polyethylene wax, polypropylene wax, oxidized polypropylene wax, and mixtures thereof, but any polyolefin wax may be used as long as it satisfies the above-mentioned melting point and melt viscosity characteristics. Polyolefin waxes satisfying the above-mentioned characteristics are widely available commercially from Sanyo Chemical Industries, Ltd., Clariant Chemicals K.K., and other companies.

[0075] The preferred amount of component (C) to be added is discussed below. To ensure sufficient demoldability, component (C) is preferably kneaded with the composition at a temperature equal to or higher than its melting point and uniformly dispersed. In consideration of the melt-kneading conditions for the composition, described below, component (C) must have a melting point of 130°C or lower, or 120°C or lower. The melting point may be in the range of 60 to 130°C, 60 to 125°C, 60 to 120°C, or 60 to 120°C. On the other hand, if the melting point of component (C) exceeds the upper limit, demoldability during molding of the cured product may not be improved. Similarly, in order to ensure the adhesive strength of a cured product made from the curable silicone composition of the present invention to a substrate, the melt viscosity of component (C) at 140°C must be 100 mPas or higher, and may be in the range of 100 to 10,000 mPas, 100 to 7,500 mPas, or 500 to 5,500 mPas. On the other hand, if the melt viscosity of component (C) at 140°C is below the above lower limit, the releasability of the cured product will be excessive, and it may be impossible to adhere to the substrate or board. Furthermore, when component (A) is a thermosetting silicone that undergoes an addition curing reaction, particularly a hydrosilylation reaction, it is preferable that component (C) have an acid value of 50 mgKOH / g or less, from the standpoint of being less likely to cause curing inhibition.

[0076] [Component (D)] Component (D) is an optional constituent component of the curable silicone composition of the present invention, provided that component (C) is used. Specifically, component (D) is a wax with a melting point of 130°C or lower and a viscosity at 140°C of less than 100 mPas, characterized by low melting point and a lower melt viscosity at 140°C than component (C). Waxes satisfying the above properties are widely available commercially from companies such as Sasol, Riken Vitamin, and Toa Kasei.

[0077] The use of component (D) in combination with component (C) makes it possible to achieve a balance between the flowability and demoldability of the composition when molded, as well as the adhesive strength of the resulting cured product to the substrate. Specifically, component (C) has such a high melt viscosity that it alone cannot impart low melt viscosity and excellent flowability to the composition when melted. However, by adding a second wax component having a melting point of 130°C or lower and a melt viscosity of less than 100 mPas at 140°C, the above three properties can be simultaneously achieved. On the other hand, if component (C) is absent from the composition, even if only component (D) is used, the adhesive strength and demoldability may be insufficient. In other words, in the present invention, the use of component (D) is premised on the use of component (C).

[0078] Component (D) may be any wax that satisfies the melting point and melt viscosity requirements, including, for example, petroleum waxes such as paraffin, natural waxes such as carnauba wax, Montan acid ester wax, fatty acid esters of erythritol derivatives, and synthetic waxes such as Fischer-Tropsch wax. Addition of even a small amount of component (D) reduces the melt viscosity of the composition and improves flowability, and its preferred content will be described later. The melting point of component (D) must be 130°C or lower, or 100°C or lower, and may be in the range of 60 to 120°C, 60 to 100°C, 60 to 100°C, or 60 to 90°C. Furthermore, the melt viscosity of component (D) at 140°C must be less than 100 mPas, and may be in the range of 1 to 99 mPas, 5 to 95 mPas, or 5 to 50 mPas. When component (A) is an addition-cure thermosetting silicone, the acid value of component (D) is preferably 50 mgKOH / g or less, from the standpoint of being less likely to cause curing inhibition.

[0079] [Amounts of Components (C) and (D)] The composition of the present invention is primarily used as a sealant for sealing substrates. In this application, it is preferable that the sealant adhere firmly to the substrate. Therefore, if the amount of component (C) or component (D) added is too large, the adhesive properties of the resulting cured product may be lost. In particular, from the standpoint of achieving good adhesive properties, demoldability, and flowability of the composition upon heat melting of the cured product, the amount of component (C) added may be in the range of 0.01 to 0.50 parts by mass, 0.01 to 0.40 parts by mass, or 0.02 to 0.30 parts by mass, based on 100 parts by mass of the total composition. Similarly, the amount of component (D) added may be in the range of 0.01 to 0.50 parts by mass, 0.01 to 0.40 parts by mass, or 0.02 to 0.30 parts by mass. If the amount of component (D) used is excessive relative to the amount of component (C), the technical effects of the present invention may not be fully achieved, so in practice, the mass ratio of component (C) to component (D) is preferably in the range of 1:4 to 4:1, 1:3 to 3:1, or 1:2 to 2:1. Furthermore, when the total composition is taken as 100 parts by mass, if the total amount of component (C) and component (D) is too large, adhesive strength may be impaired, so it is preferably 0.50 parts by mass or less, 0.40 parts by mass or less, or 0.30 parts by mass or less.

[0080] [Use as a Release Coating Agent for Mold Surfaces] The composition of the present invention can also be used as a mold surface treatment composition to apply a release coating to the mold surface of a molding machine before molding the sealant composition. In this application, the composition does not need to exhibit adhesion to the substrate, but it does need to form a sufficient release coating on the mold surface during the molding process. In this case, the preferred amount of component (C) added is 0.1 to 5.0 parts by mass, 0.3 to 4.0 parts by mass, or 0.5 to 3.5 parts by mass, based on 100 parts by mass of the entire composition. Depending on the shape of the mold, component (D) may also be used in combination, and the preferred amount is 0.1 to 5.0 parts by mass, 0.3 to 4.0 parts by mass, or 0.5 to 3.5 parts by mass, based on 100 parts by mass of the entire composition. When the amounts of component (C) and component (D) added are within the above ranges, a release coating can be effectively applied to the mold surface of the molding machine. Depending on the composition of the sealant composition to be actually molded and the shape of the mold, wax components other than component (C) and component (D) may also be used. Furthermore, by first using a composition containing a high amount of component (C) or component (D) to effectively apply a release coating to the surface of a mold, and then molding a composition containing a low total amount of component (C) and component (D) as a sealant composition for sealing a substrate or the like, the moldability and releasability may be further improved.

[0081] The composition of the present invention may contain (E) a cure retarder and (F) an adhesion promoter, provided that the object of the present invention is not impaired.

[0082] Component (E) is a cure retarder that effectively suppresses side reactions, particularly when the present composition is thermally cured by a hydrosilylation reaction, and may further improve the storage stability and usable life of the composition when heated and melted.

[0083] Usable cure retarders are not particularly limited in structure or type, and can be selected from known hydrosilylation reaction inhibitors. Examples include alkyne alcohols such as 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 2-phenyl-3-butyn-2-ol, and 1-ethynyl-1-cyclohexanol; eneyne compounds such as 3-methyl-3-penten-1-yne and 3,5-dimethyl-3-hexen-1-yne; alkenyl group-containing low molecular weight siloxanes such as tetramethyltetravinylcyclotetrasiloxane and tetramethyltetrahexenylcyclotetrasiloxane; alkynyloxysilanes such as methyl-tris(1,1-dimethyl-2-propynyloxy)silane and vinyl-tris(1,1-dimethylpropynyloxy)silane; and bis(alkynyloxysilyl)alkanes represented by the following formula: (In the formula, R 1 are independently alkynyl groups having 5 to 12 carbon atoms, and R 2 are independently an alkyl group having 1 to 3 carbon atoms or a hydrogen atom, and R 3 are independently an alkyl group having 1 to 3 carbon atoms, a is independently 1, 2, or 3, b is independently 0, 1, or 2, and a+b is 2 or 3, with the proviso that at least one b is 1 or 2, and n is an integer of 2 to 20.

[0084] In the above formula, R 1 is the formula: an alkynyl group represented by the formula: or an alkynyl group represented by the formula: It is preferable that the alkynyl group is an alkynyl group represented by the following formula:

[0085] It is particularly preferable to use a compound with a boiling point of 200°C or higher at atmospheric pressure as component (E). From the standpoint of compositional homogenization, the granular composition of the present invention can be granulated through a process that involves heating, such as melt-kneading the composition. However, if a compound with a low boiling point is used as a retarder-curing agent, some or all of the cure retarder may volatilize during the melt-kneading or other process required for granulation, and the desired cure retardation effect may not be achieved in the final granular curable silicone composition. Note that methyl-tris(1,1-dimethyl-2-propynyloxy)silane and bis(alkynyloxysilyl)alkanes have boiling points of 245°C or higher and 300°C or higher, respectively, at atmospheric pressure, and are cited as suitable examples of component (E).

[0086] The amount of component (E) used is not limited, but is preferably within the range of 1 to 10,000 ppm by mass relative to the total composition.

[0087] Component (F) is an adhesion promoter, and is exemplified by organosilicon compounds containing at least one alkoxy group bonded to a silicon atom per molecule. Examples of this alkoxy group include methoxy, ethoxy, propoxy, butoxy, and methoxyethoxy groups, with methoxy being particularly preferred. Examples of groups bonded to silicon atoms in organosilicon compounds other than the alkoxy group include halogen-substituted or unsubstituted monovalent hydrocarbon groups such as alkyl, alkenyl, aryl, aralkyl, and halogenated alkyl groups; glycidoxyalkyl groups such as 3-glycidoxypropyl and 4-glycidoxybutyl; epoxycyclohexylalkyl groups such as 2-(3,4-epoxycyclohexyl)ethyl and 3-(3,4-epoxycyclohexyl)propyl; epoxyalkyl groups such as 3,4-epoxybutyl and 7,8-epoxyoctyl; acrylic-containing monovalent organic groups such as 3-methacryloxypropyl; and hydrogen atoms. The organosilicon compound preferably has a group capable of reacting with an alkenyl group or a silicon-bonded hydrogen atom in the composition, and more specifically, a silicon-bonded hydrogen atom or an alkenyl group. Furthermore, since this provides good adhesion to various substrates, the organosilicon compound preferably has at least one epoxy-containing monovalent organic group per molecule. Examples of such organosilicon compounds include organosilane compounds, organosiloxane oligomers, and alkyl silicates. Examples of the molecular structure of the organosiloxane oligomer or alkyl silicate include linear, partially branched linear, branched, cyclic, and network structures, with linear, branched, and network structures being particularly preferred.Examples of organosilicon compounds include silane compounds such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-methacryloxypropyltrimethoxysilane; siloxane compounds having in one molecule at least one silicon-bonded alkenyl group or one silicon-bonded hydrogen atom, and one silicon-bonded alkoxy group; a mixture of a silane compound or siloxane compound having in one molecule at least one silicon-bonded alkoxy group and a siloxane compound having in one molecule at least one silicon-bonded hydroxy group and one silicon-bonded alkenyl group; a reaction mixture of an amino-containing organoalkoxysilane and an epoxy-containing organoalkoxysilane; an organic compound having in one molecule at least two alkoxysilyl groups and containing a bond other than a silicon-oxygen bond between the silyl groups; and compounds represented by the general formula: R. a n Si(OR b ) 4-n (In the formula, R a is a monovalent epoxy group-containing organic group, and R b is an alkyl group having 1 to 6 carbon atoms or a hydrogen atom. n is a number ranging from 1 to 3), or a partial hydrolysis condensate thereof; a reaction mixture of a vinyl group-containing siloxane oligomer (including those with a linear or cyclic structure) with an epoxy group-containing trialkoxysilane; methyl polysilicate, ethyl polysilicate, and epoxy group-containing ethyl polysilicate. This adhesion promoter is preferably a low-viscosity liquid, and although there are no limitations on its viscosity, it is preferably in the range of 1 to 500 mPa·s at 25°C. Furthermore, there are no limitations on the content of this adhesion promoter, but it is preferably in the range of 0.01 to 10 parts by mass per 100 parts by mass of the total composition.

[0088] In the present invention, a particularly suitable adhesion promoter is a reaction mixture of an amino-containing organoalkoxysilane and an epoxy-containing organoalkoxysilane. This component improves the initial adhesion of the curable silicone composition to various substrates that it comes into contact with during curing, and in particular the low-temperature adhesion of the composition to unwashed substrates. Such reaction mixtures are disclosed in Japanese Patent Publication No. 52-8854 and Japanese Patent Laid-Open Publication No. 10-195085.

[0089] Examples of alkoxysilanes having an amino group-containing organic group that constitute such a component include aminomethyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)aminomethyltributoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and 3-anilinopropyltriethoxysilane.

[0090] Examples of epoxy group-containing organoalkoxysilanes include 3-glycidoxyprolyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane.

[0091] The molar ratio of these alkoxysilanes having an amino group-containing organic group to those having an epoxy group-containing organic group is preferably within the range of (1:1.5) to (1:5), and particularly preferably within the range of (1:2) to (1:4). This component can be easily synthesized by mixing the above-mentioned alkoxysilanes having an amino group-containing organic group and alkoxysilanes having an epoxy group-containing organic group and reacting them at room temperature or under heat.

[0092] In particular, in the curable hot-melt silicone composition of the present invention, when an alkoxysilane having an amino group-containing organic group is reacted with an alkoxysilane having an epoxy group-containing organic group by the method described in JP-A-10-195085, a compound having the general formula: {In the formula, R 1 is an alkyl group, an alkenyl group, or an alkoxy group, and R 2 are the same or different general formula: (In the formula, R 4 is an alkylene group or an alkyleneoxyalkylene group, and R 5 is a monovalent hydrocarbon group, and R 6 is an alkyl group, and R 7 is an alkylene group, and R 8 is an alkyl group, an alkenyl group, or an acyl group, and a is 0, 1, or 2; 3 are the same or different hydrogen atoms or alkyl groups.} Examples of such carbasilatrane derivatives include carbasilatrane derivatives having a silicon-bonded alkoxy group or a silicon-bonded alkenyl group in one molecule, as shown in the following structure: (wherein Rc is a group selected from a methoxy group, an ethoxy group, a vinyl group, an allyl group, and a hexenyl group.)

[0093] In the present invention, a silatrane derivative represented by the following structural formula may also be used as an adhesion promoter. R in the formula 1 are the same or different hydrogen atoms or alkyl groups, in particular R 1 is preferably a hydrogen atom or a methyl group. 2 represents a hydrogen atom, an alkyl group, or a group represented by the general formula: -R 4 -Si(OR 5 ) x R 6 (3-x) are the same or different groups selected from the group consisting of alkoxysilyl group-containing organic groups represented by the formula:2 At least one of R is an alkoxysilyl group-containing organic group. 2 Examples of the alkyl group of R include a methyl group. 2 In the alkoxysilyl group-containing organic group, R 4 is a divalent organic group, and examples thereof include an alkylene group or an alkyleneoxyalkylene group, and particularly preferably an ethylene group, a propylene group, a butylene group, a methyleneoxypropylene group, or a methyleneoxypentylene group. 5 is an alkyl group having 1 to 10 carbon atoms, and is preferably a methyl group or an ethyl group. 6 is a substituted or unsubstituted monovalent hydrocarbon group, preferably a methyl group, and x in the formula is 1, 2, or 3, preferably 3.

[0094] Such an R 2 Examples of the alkoxysilyl group-containing organic group include the following groups: -(CH 2 ) 2 Si(OCH 3 ) 2 (CH 2 ) 2 Si(OCH 3 ) 2 CH 3 -(CH 2 ) 3 Si(OC 2 H 5 ) 2 (CH 2 ) 3 Si(OC 2 H 5 )(CH 3 ) 2 -CH 2 O(CH 2 ) 3 Si(OCH 3 ) 3 -CH 2 O(CH 2 ) 3 Si(OC 2 H 5 ) 3 -CH 2 O(CH 2 ) 3 Si(OCH3 ) 2 CH 3 -CH 2 O(CH 2 ) 3 Si(OC 2 H 5 ) 2 CH 3 -CH 2 OCH 2 Si(OCH 3 ) 2 CH 2 OCH 2 Si(OCH 3 )(CH 3 ) 2

[0095] R in the above formula 3 is at least one group selected from the group consisting of substituted or unsubstituted monovalent hydrocarbon groups, alkoxy groups having 1 to 10 carbon atoms, glycidoxyalkyl groups, oxiranylalkyl groups, and acyloxyalkyl groups, and R 3 Examples of the monovalent hydrocarbon group of R include alkyl groups such as methyl groups. 3 Examples of the alkoxy group of R include a methoxy group, an ethoxy group, and a propoxy group. 3 An example of the glycidoxyalkyl group of R is a 3-glycidoxypropyl group. 3 Examples of the oxiranylalkyl group of R include a 4-oxiranylbutyl group and an 8-oxiranyloctyl group. 3 Examples of the acyloxyalkyl group include an acetoxypropyl group and a 3-methacryloxypropyl group. 3 is preferably an alkyl group, an alkenyl group, or an alkoxy group, more preferably an alkyl group or an alkenyl group, and particularly preferably a group selected from a methyl group, a vinyl group, an allyl group, and a hexenyl group.

[0096] The amount of component (F) used is not particularly limited, but from the viewpoint of improving adhesion to poorly adhesive substrates, it is preferably in the range of 0.1 to 1.0 mass % of the total composition, and more preferably in the range of 0.2 to 1.0 mass %. The amount of component (F) blended may be in the range of 5 to 50 mass parts, or may be in the range of 5 to 40 mass parts, per 100 mass parts of component (A).

[0097] Furthermore, the present composition may contain other optional components, as long as they do not impair the object of the present invention, such as heat resistance agents such as iron oxide (red iron oxide), cerium oxide, cerium dimethylsilanolate, fatty acid cerium salts, cerium hydroxide, and zirconium compounds; dyes, pigments other than white, flame retardants, heat retardants such as aluminum hydroxide, magnesium hydroxide, zinc borate, zinc molybdate, and phosphazene; ion scavengers and pH adjusters such as hydrotalcite, bismuth oxide, and yttrium oxide; flame retardants such as magnesium chloride, zinc borate, zinc molybdate, phosphazene, etc.; antioxidants such as hindered phenol compounds, hindered amine compounds, thioether compounds, etc.; soft magnetic particles such as pure iron, silicon steel, iron-cobalt alloys, iron-nickel alloys, iron-chromium alloys, iron-aluminum alloys, carbonyl iron, stainless steel, or composite materials containing one or more of these; inorganic flame retardants (for example, hydrated metal compounds such as aluminum hydroxide), halogen-based flame retardants, phosphorus-based flame retardants, organic metal salt-based flame retardants, Silicone oil, silicone rubber, polyisoprene, polybutadienes such as 1,2-polybutadiene and 1,4-polybutadiene, styrene-butadiene rubber, acrylonitrile-butadiene rubber, carboxyl group-terminated butadiene acrylonitrile rubber, thermoplastic elastomers such as polychloroprene, poly(oxypropylene), poly(oxytetramethylene) glycol, polyolefin glycol and poly-ε-caprolactone, stress reducing agents such as polysulfide rubber and fluororubber, barium titanate (BaTiO 3 ), strontium titanate (SrTiO 3 ), lead zirconate titanate (Pb(Zr,Ti)O 3 , also known as PZT), alumina (Al 2 O 3, also known as aluminum oxide), zirconia (ZrO 2 , also known as zirconium dioxide), magnesia (MgO, also known as magnesium oxide), silica (SiO 2 , also known as silicon dioxide), titania (TiO 2 , also known as titanium dioxide), aluminum nitride (AlN), silicon nitride (Si 3 N 4 ), silicon carbide (SiC), barium calcium zirconate titanate (also known as BCTZ), polyvinylidene fluoride or other dielectric ceramics; metal salt stabilizers such as copper chloride, cupric iodide, copper acetate, and cerium stearate; antioxidants and heat stabilizers such as hindered amines, hindered phenols, sulfur-containing compounds, acrylates, and phosphorus-based organic compounds; ultraviolet absorbers, weathering agents, and light stabilizers such as benzophenones, salicylates, and benzotriazoles.

[0098] [Granular Curable Silicone Composition] The curable silicone composition of the present invention is not particularly limited in terms of its form, so long as it has the above-described composition, and as described below, it may be tableted into pellets or tablets. However, because the composition has excellent melting and curing properties, characterized by high fluidity at high temperatures, and is less likely to generate dust, even when it contains a large amount of functional inorganic filler, it is preferable that the composition be formed into granules after the components of the composition have been melt-kneaded to achieve a uniform composition at a temperature in the range of 50 to 150°C. In other words, the curable silicone composition of the present invention is preferably a granular curable silicone composition. The granular curable silicone composition (granular composition) may then be tableted into pellets or tablets.

[0099] The granular composition generates little dust, is easy to handle, and has excellent uniformity of each component, so that the cured product has high hardness, a low coefficient of linear expansion, and good adhesion to substrates, making it particularly suitable for use as sealing, molding, and protective materials for semiconductor devices.Furthermore, the granular composition (granular molded product) of the present invention has the advantage of being efficiently produced by a simple mixing process alone.

[0100] [Composition of the Present Invention and Tablet-Molded Product Thereof] As described above, the curable silicone composition of the present invention is solid at room temperature. However, in order to fully exert the effects of small amounts of component (C) and optional component (D), it is preferable for the composition to be uniform in composition. As described above, the curable silicone composition is preferably molded into granules. Furthermore, by forming the composition into granules with a constant average particle size, the granular composition can be tableted by known methods and used in the form of pellets or tablets. Unlike tableting of granular compositions (powder mixtures) that have not been melt-kneaded, as in Patent Document 1, the granular curable silicone composition of the present invention is uniform in composition. Therefore, using this granular composition not only provides excellent production efficiency for the tablet-molded product, but also has the advantage that the hot-melt properties, melt viscosity, and physical properties of the cured product of the resulting tablet-molded product are even better. Furthermore, granular compositions have the advantage of being less likely to generate dust.

[0101] Here, "pellets" and "tablets" are general names or common names for granular tablet-molded products made from a resin composition. The shape of the pellets / tablets is not limited, but is usually spherical, oval-spherical, or cylindrical. The size of the pellets is also not limited, but may have, for example, an average particle diameter or equivalent circle diameter of 500 μm or more, and may have an average particle diameter or equivalent circle diameter of 1 mm or more.

[0102] [Method for producing a granular curable silicone composition] The present composition is in the form of granules in which the entire composition, including at least the above-mentioned components (A) to (C) and other optional components, has been homogenized in composition beyond the extent of simple mechanical mixing. Such a granular composition is preferably obtained by melt-kneading the entire composition accompanied by heating. More specifically, it is preferable to melt-knead components (A) to (C) and any other optional components at a temperature in the range of 50 to 150°C using a single-screw or twin-screw continuous mixer, a twin-roll mill, a Ross mixer, a kneader mixer, or the like, and then mold the mixture into granules for use. Specific examples of production methods are given below.

[0103] The method for producing a granular curable silicone composition of the present invention comprises the steps of melt-kneading a curable silicone composition comprising the above-mentioned components (A) to (C) and any other optional components, with the content of component (B) being 40 parts by mass or more per 100 parts by mass of component (A), at a temperature range of 50 to 150°C, and then molding the composition into granules. The average particle size of the granular composition is preferably in the range of 0.05 to 10.0 mm.

[0104] The manufacturing method is not particularly limited as long as it includes a step of melt-kneading the composition and then molding it into granules, but it may include, for example, the following steps 1 to 3: Step 1: Kneading the components of the curable silicone composition while heating and melting them at a temperature range of 50 to 150°C; Step 2: Cooling the heated and melted mixture obtained in step 1 while discharging it; Step 3: Cutting or breaking the mixture obtained in step 2 to mold the granular curable silicone composition.

[0105] [Step 1] Step 1 described above involves kneading the components of the curable silicone composition of the present invention while heating and melting them in the temperature range of 50 to 150° C. By heating and kneading the heat-meltable mixture at a temperature above its softening point, preferably in the temperature range of 50 to 120° C., the entire composition melts or softens, allowing components (A) to (C) and any optional components to be uniformly dispersed throughout. In particular, by melt-kneading at a temperature higher than or close to the melting points of component (C) and optional component (D), these components can be uniformly dispersed within the system, allowing their effects to be fully exerted.

[0106] The mixing device used in step 1 is not particularly limited, and may be a batch type heat-kneading device equipped with heating and cooling functions, such as a kneader, Banbury mixer, Henschel mixer, planetary mixer, two-roll mill, three-roll mill, Ross mixer, or Laboplastomill, or a continuous type heat-kneading device equipped with heating and cooling functions, such as a single-screw extruder or twin-screw extruder, and is selected based on the efficiency of processing time and the ability to control shear heat generation. From the perspective of processing time, the device may be a continuous type heat-kneading device such as a single-screw extruder or twin-screw extruder, or a batch type mixer such as a Laboplastomill. However, from the standpoint of production efficiency of the granular curable silicone composition, continuous type heat-kneading devices such as a single-screw extruder or twin-screw extruder are preferably used.

[0107] This mixture is then granulated in step 3 after passing through step 2. If the temperature is below the lower limit, softening will be insufficient, making it difficult to obtain a molten or softened mixture in which the components are uniformly dispersed throughout, even when mechanical force is used. Such a mixture may not have excellent uniformity among the components, and when the resulting granular curable silicone composition is used in a molding process, a uniform cured product may not be obtained. Conversely, if the temperature exceeds the upper limit, the curing agent may react during mixing, causing the entire mixture to significantly thicken or harden, losing its hot-melt properties and forming a cured product, which is undesirable. For this reason, when a hydrosilylation reaction component is used as component (A), it is preferable to use a particulate hydrosilylation reaction catalyst (such as the above-mentioned component (A2-2)) dispersed or encapsulated in a thermoplastic resin whose softening point is at or above the kneading temperature.

[0108] The components of the present invention can be fed into the kneading device described above by either feeding each component separately into the kneading device at a constant rate, or by mechanically or other means powder-mixing all of the components to form a granular curable silicone composition, which can then be fed into the kneading device.

[0109] [Step 2] Step 2 is a step in which the mixture melted and kneaded in step 1 is discharged from the kneader. The mixture may be discharged in any shape, but since the mixture is cut and broken into granules in step 3, it is preferable that the mixture be in a shape that allows for easy cutting and breaking. Examples include a rod shape (strand shape) with a diameter of about 0.5 to 5.0 mm or a sheet shape with a thickness of about 0.5 to 5.0 mm. Since the mixture is preferably a non-sticky solid for granulation in step 3, the temperature of the discharged mixture must be lowered to near room temperature by natural cooling or rapid cooling. Examples of rapid cooling methods include a method using a cooler or water cooling.

[0110] [Step 3] Step 3 is a step in which the mixture discharged in Step 2 is cut or broken to form granules. If the mixture is hard enough to be broken by shear stress alone at room temperature, it can be broken and granulated by passing it through a two-roll mill or the like. The size and shape of the granules obtained in Step 3 can be adjusted to some extent by controlling the dimensions of the mixture discharged in Step 2 and the gap between the rolls. In the present invention, there is no limit to the average particle size of the granular product, but from the viewpoint of handleability during tableting, as described below, it is preferably in the range of 0.05 to 10.0 mm. Furthermore, if the mixture cannot be broken down using a roll or the like, it is also possible to obtain granules by discharging the mixture as a rod-shaped mixture in Step 2 and cutting it to a predetermined size using a rotary cutter or the like while cooling.

[0111] The granular curable silicone composition obtained by the production method of the present invention has excellent flowability in hot melt and is highly uniform in composition, so that the composition is less likely to become non-uniform or physically move during molding, such as compression molding, press molding, or lamination. This has the advantage that the entire composition can be easily molded uniformly, making it suitable for use in molding processes that do not generate shear pressure. Additionally, by using the aforementioned component (C), preferably component (D), in combination, the composition exhibits excellent demoldability during the molding process and strong adhesion to the substrate. Furthermore, since the above advantages are not lost even when the granular composition is subjected to secondary molding, the granular curable silicone composition may be compressed or tableted using a tablet press or the like and used as tablets or pellets for transfer molding.

[0112] [Cured Product] The above-mentioned curable silicone composition, particularly the granular (molded) composition or its tablet-molded product, possesses hot-melt properties, exhibiting excellent flowability during melting (hot-melt), ease of handling, and curing properties, and upon curing forms a cured product suitable for semiconductor components, etc. Depending on the type of curing agent (A2), various thermal curing reactions can be selected. However, when component (A2) is selected from a thermal radical polymerization initiator such as an organic peroxide and a hydrosilylation reaction catalyst / its hydrosilylation reaction crosslinking agent, curing is preferably carried out by heat curing in the range of 80°C to 200°C. In the present invention, the physical properties of the cured product, such as the linear expansion coefficient, flexural strength, and hardness, can be easily designed to fall within the following preferred ranges based on the type of component (A) and the quantitative range of component (B). Furthermore, even when a large amount of component (B) is incorporated into the curable silicone composition of the present invention, the combined use of component (C), preferably component (D), improves the mechanical strength of the resulting cured product, and the resulting cured product exhibits excellent demoldability during the molding process and strong adhesion to substrates.

[0113] [Linear Expansion Coefficient of Cured Product] The cured product obtained by curing the composition has an average linear expansion coefficient of 30 ppm / °C or less, preferably 20 ppm / °C or less, in the temperature range of 25°C to 200°C. Within this range, the difference in average linear expansion coefficient from the substrate to be used is small, so that residual stress in the obtained integrally molded product can be reduced, and device reliability can be improved.

[0114] [Flexural Strength of Cured Product] Furthermore, since the cured product is suitable as an encapsulant for semiconductors, which requires high hardness and strength, the flexural strength of the cured product measured by the method specified in JIS K 6911-1995 "General Testing Methods for Thermosetting Plastics" is preferably 15 MPa or more, or 20 MPa or more.

[0115] [Hardness of the Cured Product] Because the composition is suitable for use as a protective material for semiconductors, etc., the cured product obtained by curing the composition preferably has a Type D durometer hardness at 25°C of at least 20. The Type D durometer hardness is determined using a Type D durometer in accordance with JIS K 6253-1997 "Testing method for hardness of vulcanized rubber and thermoplastic rubber."

[0116] [Method of Molding a Cured Product] The present composition (including the granular composition and its tablet-formed pellets or tablets, the same applies hereinafter) can be cured by a method comprising at least the following steps (I) to (III): (I) a step of heating the present composition to 100°C or higher to melt it; (II) a step of injecting the curable silicone composition softened in step (I) into a mold, or a step of dispersing the curable silicone composition obtained in step (I) in the mold by clamping; and (III) a step of curing the curable silicone composition injected in step (II).

[0117] The present composition exhibits a relatively low melt viscosity at temperatures of 100°C or higher, and therefore has excellent hot-melt properties, flowability, and gap-filling properties under pressure, making it suitable for use in molding methods including a coating step in which overmolding and underfilling of semiconductor elements are performed simultaneously (the so-called mold underfill method).

[0118] Furthermore, due to the above-mentioned properties, the present composition can be suitably used in a molding method including a coating step (so-called wafer molding) in which the composition covers the surface of a semiconductor substrate (including a wafer substrate) carrying one or more semiconductor elements and overmoldes the surface so that the gaps between the semiconductor elements are filled with the cured product. In particular, the composition of the present invention has the advantage that the cured molded product has excellent demoldability and adhesion to the substrate.

[0119] In the molding step, a transfer molding machine, a compression molding machine, an injection molding machine, a press molding machine, an auxiliary ram molding machine, a slide molding machine, a double ram molding machine, a low-pressure encapsulation molding machine, or the like can be used.

[0120] In step (III) above, the curable silicone composition injected (applied) in step (II) is cured. The curing method varies depending on the type of component (A2), but when component (A2) is selected from a thermal radical polymerization initiator such as an organic peroxide and a hydrosilylation reaction catalyst / its hydrosilylation reaction crosslinking agent, curing is preferably carried out by heat curing in the range of 80°C to 200°C. In particular, when an organic peroxide is used as component (A2), the heating temperature is preferably 150°C or higher, or 170°C or higher.

[0121] [Uses of the Composition] The curable silicone composition of the present invention (particularly including a granular (molded) composition and its tablet-shaped or pellet-shaped tablet product) has good hot-melt properties, excellent flowability during melting (hot-melt), ease of handling, and curing, and also good demoldability and adhesion to substrates. Therefore, it is suitable as an encapsulant or underfill agent for semiconductors; an encapsulant or underfill agent for power semiconductors such as SiC or GaN; an encapsulant or light-reflecting material for optical semiconductors such as light-emitting diodes, photodiodes, phototransistors, and laser diodes; and an adhesive or protective agent for electrical and electronic devices. Furthermore, because the composition has hot-melt properties, it is also suitable as a material for transfer molding, compression molding, press molding, or injection molding. It is particularly suitable for use as an encapsulant for semiconductors that are molded using mold underfill or wafer molding methods.

[0122] As described above, the present composition is suitable as a sealant for semiconductors, and by using the composition to replace part or all of a conventionally known sealant in the process of sealing semiconductors and the like by molding methods such as an overmolding method using a conventionally known sealant (including non-silicone hot-melt sealants such as epoxy sealants), an underfill method, a mold underfill method in which these are performed at the same time, or a wafer molding method, it is possible to produce semiconductor / optical components such as semiconductor packages, power semiconductor modules, MEMS, small integrated devices such as microsensors (fingerprint sensors), magnetic components such as coils containing magnetic particles, flexible substrates (stretchable wiring boards) used in wearable devices, and optical waveguides connected to electrical wiring boards and connectors. For example, the curable silicone composition according to the present invention is disclosed in Japanese Patent Application Laid-Open No. 2021-097123, Japanese Patent Application Laid-Open No. 2021-024945, Japanese Patent Application Laid-Open No. 2020-132771, Japanese Patent Application Laid-Open No. 2020-132750, Japanese Patent Application Laid-Open No. 2020-125399, Japanese Patent Application Laid-Open No. 2020-123670, Japanese Patent Application Laid-Open No. 2020-084094, Japanese Patent Application Laid-Open No. 2020-088055, Japanese Patent Application Laid-Open No. 2019-006905, Japanese Patent Application Laid-Open No. 2018-188494, Japanese Patent Application Laid-Open No. 2017-179185, Japanese Patent Application Laid-Open No. 2020-023643, Japanese Patent Application Laid-Open No. 2020-063459, Japanese Patent Application Laid-Open No. 2020-090634, Japanese Patent Application Laid-Open No. 2020-088055, It can be used in place of some or all of the sealants (especially silicone elastomer sealants, pastes containing functional fillers, and hot-melt sealants) described in JP 2020-107767, JP 2021-080411, JP 2021-036013, JP 2020-152844, JP 2020-158684, JP 2021-019031, JP 2021-059741, JP 2020-057775, JP 2021-015985, JP 2015-114390, JP 2016-177106, etc. If necessary, the technical elements applied to these sealant compositions may be applied to the present invention, and the composition of the present invention may be adjusted in terms of its composition, physical properties and melting characteristics of the cured product, etc., and is preferred.

[0123] [Uses of the cured product] There are no particular restrictions on the uses of the cured product of the present invention, but the curable silicone composition of the present invention (particularly including granular (molded) compositions and their tablet-shaped or pellet-shaped products) has hot-melt properties and excellent moldability, and the cured product obtained has excellent adhesive properties, a high modulus of elasticity, and a low coefficient of linear expansion. For this reason, the cured product of the present invention can be suitably used as a semiconductor device component, and can be suitably used as an encapsulant for semiconductor elements, IC chips, etc., or as a light-reflecting material for optical semiconductor devices.

[0124] The semiconductor device equipped with a member made of the cured product of the present invention is not particularly limited, but is preferably a semiconductor device mounted on a power semiconductor device, an optical semiconductor device, or a flexible semiconductor device that is stretchable or deformable.

[0125] The hot-melt curable silicone composition of the present invention and its production method are described in detail below using examples and comparative examples. In the formula, Me, Ph, and Vi represent methyl, phenyl, and vinyl groups, respectively. The softening point and melt viscosity of the curable silicone composition of each example and comparative example were measured using the following methods. The curable silicone composition was heated at 180°C for 2 hours to produce a cured product, and the adhesive strength to various substrates was measured using the following method. The results are shown in Table 1.

[0126] [Softening Point of Curable Silicone Composition] The curable silicone composition was molded into a cylindrical pellet measuring φ14 mm x 22 mm. This pellet was placed on a hot plate set to 25°C to 100°C, and a 100 gram load was applied from above for 10 seconds. After the load was removed, the deformation of the pellet was measured. The softening point was determined as the temperature at which the deformation in the height direction reached 1 mm or more.

[0127] [Melt Viscosity] The melt viscosity of the curable silicone composition at 180°C was measured using a Koka-shiki Flow Tester CFT-500EX (manufactured by Shimadzu Corporation) under a pressure of 100 kgf using a nozzle with a diameter of 1.0 mm.

[0128] [Mold Removal Efficiency in the Molding Process] Cylindrical tablets made of the curable silicone composition were thermally cured in a spiral flow mold at 180°C for 3 minutes using a transfer molding machine, and the cured product was then demolded from the mold. The demoldability of each cured product was evaluated according to the following criteria. If the cured product could be demolded simply by opening the upper and lower molds, the demoldability was evaluated as extremely good (◎); if the cured product peeled off smoothly without breaking when demolded with tweezers, the demoldability was evaluated as good (◯); and if the cured product adhered strongly to the mold and was destroyed when demolded with tweezers, the demoldability was evaluated as poor (×).

[0129] [Adhesion strength of cured product] Approximately 500 mg of the curable silicone composition was placed in four locations on various 25 mm x 75 mm substrates. Next, this composition was covered with a 10 mm square glass chip with a thickness of 1 mm, and cured by heating for 2 hours at a temperature of 180°C while thermocompressed with a 1 kg plate. After that, it was cooled to room temperature, and the die shear strength was measured using a shear strength measuring device (Bond Tester SS-100KP manufactured by Seishin Shoji Co., Ltd.).

[0130] A base agent containing component (A) of the present invention was prepared by the method shown in Reference Example 1 below.

[0131] Reference Example 1 In a 1 L flask, there was added component (A1), which is a white solid at 25°C and has a melting point of 100°C and has the average unit formula: (PhSiO 3 / 2 ) 0.80 (Me 2 ViSiO 1 / 2 ) 0.20 100 g of a resinous organopolysiloxane represented by the formula: HMe 2 SiO(Ph 2 SiO)SiMe 2 3.2 g of diphenylsiloxane end-blocked at both molecular chain terminals with dimethylhydrogensiloxy groups (content of silicon-bonded hydrogen atoms = 0.6% by mass) having a viscosity of 5 mPa s, represented by H; component (A3-2) average unit formula: (PhSiO 3 / 2 ) 0.4 (HMe 2 SiO 1 / 2 ) 0.6A viscous silicone mixture (L1) was obtained by mixing 28.0 g of a branched-chain organopolysiloxane having two or more silicon-bonded hydrogen atoms per molecule and a viscosity of 25 mPa s (silicon-bonded hydrogen atom content = 0.65 mass%), represented by the formula:

[0132] The components used in the examples and comparative examples are shown below in detail. The amount of each component used in Table 1 is in parts by mass. (A2-1) 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (the temperature at which the half-life is 10 hours is 118°C) (A2-2) Thermoplastic polycarbonate resin (softening point = 150°C) containing 4000 ppm of a 1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex of Pt (0 valent) as platinum content (softening point = 150°C) (B-1) Fused silica having an average particle size of 14.5 μm (S6105P manufactured by Nippon Steel Materials Micron Co., Ltd.) (B-2) Fused silica having an average particle size of 0.7 μm (SPH507M manufactured by Nippon Steel Materials Micron Co., Ltd.) (B-3) Denka Black Pressed Product (manufactured by Denka Co., Ltd.) (B') A compound having the formula: Me 2 ViSiO(Me 2 SiO) 29 Si(OMe) 3(C-1) A polyethylene wax having a melting point of 100°C and a melt viscosity of 4,300 mPas at 140°C. (C-2) A polyethylene wax having a melting point of 100°C and a melt viscosity of 1,000 mPas at 140°C. (C-3) An oxidized polyethylene wax having a melting point of 120°C and a melt viscosity of 1,800 mPas at 140°C. (C-4c) A polyethylene having a melting point of 135°C and a melt viscosity of 25,000 mPas at 140°C. Polypropylene wax *For comparative experiments (D-1) Fatty acid ester wax having a melting point of 70°C and a melt viscosity of 10 mPas at 140°C (D-2) Carnauba wax having a melting point of 80°C and a melt viscosity of 15 mPas at 140°C (D-3) Fischer-Tropsch wax having a melting point of 80°C and a melt viscosity of 8 mPas at 140°C (D-4c) Calcium stearate having a melting point of 150°C and no melt viscosity at 140°C *For comparative experiments (D-5c) Zinc stearate having a melting point of 120°C and a melt viscosity of 300 mPas at 140°C *For comparative experiments (E-1) Methyltris-1,1-dimethyl-2-propynyloxysilane (boiling point at atmospheric pressure = 245°C) (E-2) 1,6-bis[tris(1,1-dimethyl-2-butynoxy)silyl]hexane (boiling point at atmospheric pressure = 300°C or higher) (F) Bis(trimethoxysilylpropoxymethyl)allylsilatrane

[0133] Production Examples (Examples 1 to 7, Comparative Examples 1 to 6) Components (B), (B'), (C), and (D) were all charged into a small pulverizer and stirred at 100°C for 1 minute, the fused silica was surface-treated, and the temperature of the pulverizer was then returned to 25°C. Next, the liquid silicone mixture (L1) obtained in Reference Example 1, components (E), (F), and (A2) were added to the small pulverizer and stirred at room temperature (25°C) for 1 minute to prepare a uniformly granular curable silicone composition.

[0134] The resulting curable silicone composition was placed in a kneader mixer set to 100°C and melt-kneaded for 1 minute at 100 rpm, resulting in a unified composition that was solid at room temperature. This solid was then pulverized while cooling to 0°C to produce an irregular granular curable silicone composition. The resulting granular composition was tableted to produce a cylindrical tablet-shaped curable silicone composition. The properties, details of each component, and the amounts added are shown in Tables 1 and 2.

[0135] *Improved to ⊚ after three consecutive times (Example 8).

[0136]

[0137] Example 8 The demoldability test for the composition of Example 5 was carried out three times in succession, and the demoldability was improved to ⊚.

[0138] Example 9: Application to mold coating applications and improved demoldability A composition was prepared using the same ingredients and amounts as in Example 1, except that the amount of component (C1) in Example 1 was changed to 30 parts by mass. The resulting cylindrical tablet-shaped curable silicone composition was thermally cured in a spiral flow mold at 180°C for 3 minutes using a transfer molding machine, and the cured product was demolded simply by opening the upper and lower molds. The cylindrical tablet-shaped curable silicone composition obtained in Example 5 was then molded, and its demoldability was improved to extremely good (◎).

[0139] [Summary] In Examples 1 to 3 of the present invention, the inclusion of component (C) confirmed excellent demoldability. On the other hand, component (C) was found to have a low effect of lowering the melt viscosity of the composition, resulting in a high melt viscosity at 180°C. Meanwhile, in Examples 4 to 7, components (C) and (D) were used in combination, and these compositions simultaneously achieved excellent demoldability and a low melt viscosity at 180°C. In particular, the compositions of these Examples were confirmed to have improved wettability to substrates and improved adhesive strength of cured molded products due to their low melt viscosity. Furthermore, the results of Example 8 (repeating Example 5 three times) confirmed that the demoldability of the composition of the present invention is further improved by continuous molding. Furthermore, Example 9 demonstrates the use of the composition of the present invention for mold coating purposes. In this example, molding a composition containing a larger amount of component (C) resulted in the entire mold being coated with the demolding component, and subsequent molding of the composition of Example 5 demonstrated excellent demoldability from the first molding. By combining this with the results of Example 8, long-term continuous molding is possible. In all of the examples, the compositions of the present invention achieved a high content of the functional inorganic filler (specifically, components B-1 to B-3) which is component (B), and it is expected that the cured product will be able to achieve excellent mechanical strength, etc. From the above results, it was confirmed that by using a thermosetting silicone composition of the present invention which has a high content of functional inorganic filler and which also contains the specific polyolefin wax (component (C)) of the present invention, and preferably further contains a wax (component (D)), it is possible to achieve both good demoldability of the cured product during transfer molding and good adhesion to the substrate.

[0140] On the other hand, when a wax component with a melting point of 130°C or higher was used in Comparative Examples 1 and 2, no improvement in demoldability was observed compared to the Examples. Furthermore, Comparative Examples 3 to 6 do not contain the specific polyolefin wax that is component (C), but it was confirmed that even if a similar thermosetting silicone composition uses only component (D), it is difficult to achieve both demoldability and adhesion if component (C) is absent.

Claims

1. A curable silicone composition comprising: (A) a thermosetting silicone; (B) a functional inorganic filler; and (C) a polyolefin wax having a melting point of 130°C or lower and a viscosity at 140°C of 100 mPas or higher, wherein the content of component (B) is 40 parts by mass or more per 100 parts by mass of component (A), and the composition as a whole exhibits hot melt properties.

2. The curable silicone composition according to claim 1, further comprising (D) a wax having a melting point of 130°C or lower and a viscosity at 140°C of less than 100 mPas.

3. Component (A) is (A1) RSiO 3/2 2. The curable silicone composition according to claim 1 , characterized in that it comprises at least an organopolysiloxane resin that contains siloxane units represented by the formula: (wherein R is a monovalent hydrocarbon group) in an amount of at least 20 mol % of all siloxane units; and (A2) a curing agent.

4. The curable silicone composition according to claim 3, wherein component (A2) is a curing agent containing a curing reaction catalyst that becomes active in the composition when stimulated with thermal energy of 80°C or higher.

5. The curable silicone composition according to claim 3, wherein component (A2) contains one or more curing agents selected from the group consisting of: (A2-1) an organic peroxide having a half-life of 10 hours at a temperature of 80°C or higher; and (A2-2) fine particles of thermoplastic resin containing a hydrosilylation reaction catalyst, the fine particles comprising a thermoplastic resin having a softening point or glass transition point of 80°C or higher.

6. At least a part or all of the (A1) component is: (A1-1) a curing reactive functional group having a softening point of 30°C or higher and containing at least one carbon-carbon double bond in the molecule, RSiO 3/2 4. The curable silicone composition according to claim 3, which is a hot-melt organopolysiloxane resin that contains siloxane units represented by the formula: where R is a monovalent hydrocarbon group, in an amount of at least 20 mol % of all siloxane units.

7. At least a part or all of the (A1) component is: (A1-1-1) a curing reactive functional group having a softening point of 30°C or higher and at least one carbon-carbon double bond in the molecule, RSiO 3/2 4. The curable silicone composition according to claim 3, which is a hot-melt organopolysiloxane resin that contains at least 20 mol % of all siloxane units of the formula: (wherein R is a monovalent hydrocarbon group), and in which at least 10 mol % of the silicon-bonded organic groups are aryl groups.

8. The curable silicone composition according to claim 1, wherein component (B) is a reinforcing filler, a pigment, a thermally conductive filler, an electrically conductive filler, a phosphor, a magnetic particle, or a mixture of at least two of these.

9. The curable silicone composition according to any one of claims 1 to 8, which is in the form of granules.

10. A pellet-shaped or tablet-shaped product obtained by compression molding the curable silicone composition according to any one of claims 1 to 9.

11. A cured product obtained by curing the curable silicone composition according to any one of claims 1 to 9, or the pellet-shaped or tablet-shaped product according to claim 10.

12. A member for a semiconductor device comprising the cured product of claim 11.

13. A semiconductor device comprising the cured product of claim 11.

14. A method for producing a granular curable silicone composition as described in claim 9, comprising the steps of melt-kneading a curable silicone composition containing (A) a thermosetting silicone, (B) a functional inorganic filler, and (C) a polyolefin wax having a melting point of 130°C or less and a viscosity at 140°C of 100 mPas or more, in which the content of component (B) is 40 parts by mass or more per 100 parts by mass of component (A), at a temperature range of 50 to 150°C, and then molding the composition into granules.

15. A method for molding a cured product according to claim 11, comprising at least the following steps (I) to (III): (I) a step of heating the curable silicone composition according to any one of claims 1 to 9, or the pellet-like or tablet-like molded product according to claim 10, to 100°C or higher to melt it; (II) a step of injecting the curable silicone composition softened in step (I) into a mold, or a step of spreading the curable silicone composition obtained in step (I) around the mold by clamping the mold; and (III) a step of curing the curable silicone composition injected in step (II).

16. A method for molding the cured product according to claim 15, comprising a coating step in which overmolding and underfilling of a semiconductor element are carried out in one step with a cured product obtained by curing the curable silicone composition according to any one of claims 1 to 10, or the pellet-shaped or tablet-shaped product according to claim 11.

17. A method for molding a cured product according to claim 15, comprising a covering step of covering the surface of a semiconductor substrate carrying one or more semiconductor elements with a cured product obtained by curing the curable silicone composition according to any one of claims 1 to 9, or the pellet-like molded product or tablet-like molded product according to claim 10, and overmolding the cured product so that gaps between the semiconductor elements are filled with the cured product.

Citation Information

Patent Citations

  • Device for detecting oil inside a draining pit

    JP1977008854A

  • Carbasilatrane derivative, its production, adhesion accelerator and hardenable silicone composition

    JP1998195085A

  • Adhesive sheet, optical waveguide with adhesive sheet, photo-electric hybrid board, method for manufacturing photo-electric hybrid board, optical module, and electronic equipment

    JP2015114390A

  • Optical waveguide with connector and method for producing optical waveguide with connector

    JP2016177106A

  • Moisture-curable hot-melt silicone adhesive composition containing an alkoxy-functional siloxane reactive resin