Chemical solution and chemical-solution-accommodating body

A chemical solution combining 2-heptanone, water, and specific carbonyl compounds addresses the challenges of cleanliness and defect suppression in semiconductor manufacturing, enhancing in-plane uniformity and wafer bevel cleaning, and effectively reducing substrate defects.

WO2024237109A1PCT designated stage expired Publication Date: 2024-11-21FUJIFILM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016806
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-05-01
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In semiconductor manufacturing, particularly in lithography processes, there is a need for chemical solutions that provide excellent in-plane cleanliness uniformity, wafer bevel cleaning performance, and defect suppression on substrates, which existing solutions fail to adequately address, especially with the increasing complexity of submicron and quarter-micron pattern formation and the use of shorter exposure wavelengths.

Method used

A chemical solution comprising 2-heptanone, water, and a carbonyl compound with 6 to 8 carbon atoms, where 2-heptanone constitutes 60% of the solution by mass, water is present in 1 to 1000 ppm, and the carbonyl compound is in the range of 0.1 to 1000 ppm, along with optional cycloalkane compounds and metal atoms like Mn and Fe, to enhance cleaning and defect suppression.

Benefits of technology

The solution achieves superior in-plane cleanliness uniformity, improved wafer bevel cleaning, and reduced defect occurrence on substrates, while maintaining the electrical conductivity and preventing moisture-induced defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a chemical solution that realizes excellent cleanness in-plane uniformity with respect to a substrate, that demonstrates excellent cleaning performance for wafer bevels, and that, when brought into contact with a substrate, exceptionally suppresses the occurrence of defects on the substrate. The present invention also addresses the problem of providing a chemical solution accommodating body that accommodates the chemical solution. The chemical solution according to the present invention contains 2-heptanone, water, and a C6-8 carbonyl compound other than 2-heptanone. The 2-heptanone content is 60 mass% or more with respect to the total mass of the chemical solution, the water content is 1-1000 mass ppm with respect to the total mass of the chemical solution, and the P value obtained by formula (1) is 3-10. Formula (1): P = -log10 (X × Y), where X represents a numerical value X when the concentration of water in the chemical solution is defined as X mol / L, and Y represents a numerical value Y when the concentration of the carbonyl compound in the chemical solution is defined as Y mol / L.
Need to check novelty before this filing date? Find Prior Art

Description

Chemical solution, chemical solution container

[0001] The present invention relates to a drug solution and a drug solution container.

[0002] Conventionally, in the manufacturing process of semiconductor devices such as ICs (Integrated Circuits) and LSIs (Large Scale Integrated Circuits), microfabrication has been performed by lithography using a photoresist composition. In recent years, with the increasing integration density of integrated circuits, there has been a demand for the formation of ultrafine patterns in the submicron and quarter-micron ranges. Accordingly, there has been a trend toward shorter exposure wavelengths, from g-line to i-line and then to KrF excimer laser light. Furthermore, in addition to excimer laser light, lithography using electron beams, X-rays, or EUV (Extreme Ultra Violet) light is also currently being developed. In such lithography, a film (resist film) is formed using an actinic ray- or radiation-sensitive composition (also referred to as a "resist composition"), followed by exposure to light, development using a developer, and subsequent rinsing of the developed film with a rinse solution.

[0003] As a developer used in the above-mentioned lithography, for example, Patent Document 1 discloses a developer having a Hansen solubility parameter δH+δP of about 16 (J / cm 3 ) 1/2 and the value of the Hansen solubility parameter δH + δP is about 16 (J / cm 3 ) 1/2 Developer compositions for use in developing organometallic patterned layers are disclosed, which contain at least 0.25 to 45 volume percent of a solvent represented by the formula:

[0004] Special Publication No. 2022-526031

[0005] The present inventors, with reference to Patent Document 1, have studied chemical solutions used in semiconductor substrate manufacturing processes, particularly chemical solutions used as cleaning solutions, developing solutions, rinse solutions, and pre-wet solutions in semiconductor substrate manufacturing processes that include a step of forming a metal resist film using a metal resist composition, and have found that there is room for further improvement in the cleanliness of each region of the substrate surface after application of the chemical solutions, the ability to suppress defects, and the like.

[0006] In view of the above circumstances, an object of the present invention is to provide a chemical solution that is excellent in in-plane cleanliness uniformity and wafer bevel cleaning performance on a substrate, and that is excellent in the ability to suppress the occurrence of defects on the substrate when brought into contact with the substrate. Another object of the present invention is to provide a chemical solution container that contains the chemical solution.

[0007] As a result of extensive research into solving the above problems, the present inventors have found that the problems can be solved by the following configuration.

[0008] [1] A chemical solution containing 2-heptanone, water, and a carbonyl compound having 6 to 8 carbon atoms other than 2-heptanone, wherein the content of the 2-heptanone is 60 mass% or more relative to the total mass of the chemical solution, the content of the water is 1 to 1000 mass ppm relative to the total mass of the chemical solution, and the P value calculated by the formula (1) described below is 3 to 10. [2] The chemical solution according to [1], wherein the content of water is 1 to 100 mass ppm relative to the total mass of the chemical solution. [3] The chemical solution according to [1] or [2], wherein the content of the carbonyl compound is 0.1 to 1000 mass ppm relative to the total mass of the chemical solution. [4] The chemical solution according to any of [1] to [3], wherein the carbonyl compound includes a ketone having 6 to 8 carbon atoms other than 2-heptanone. [5] The chemical solution according to any one of [1] to [4], wherein the carbonyl compound contains two or more ketones having 6 to 8 carbon atoms other than 2-heptanone. [6] The chemical solution according to any one of [1] to [5], wherein the carbonyl compound contains at least one selected from the group consisting of 5-methyl-2-hexanone and 4-heptanone. [7] The chemical solution according to any one of [1] to [5], wherein the carbonyl compound is a compound represented by the chemical formula C 7 H 14[8] The chemical solution according to any one of [1] to [6], which contains a carbonyl compound represented by the formula: O. [8] The carbonyl compound contains a ketone having 6 to 8 carbon atoms other than 2-heptanone and an aldehyde having 6 to 8 carbon atoms, and the ratio of the content of the aldehyde to the content of the ketone is 1.0 × 10 -5 ~1.0 x 10 2 [9] The chemical solution according to any one of [1] to [8], further comprising a cycloalkane compound having a boiling point of 160°C or higher and 8 to 12 carbon atoms, wherein the content of the cycloalkane compound is 0.1 to 1000 ppm by mass relative to the total mass of the chemical solution.

[10] The chemical solution according to [9], wherein the cycloalkane compound comprises at least one selected from the group consisting of 1-methyl-2-isopropylcyclohexane, 1-methyl-3-isopropylcyclohexane, and 1-methyl-4-isopropylcyclohexane.

[11] The chemical solution according to [9] or

[10] , wherein the cycloalkane compound comprises 1-methyl-4-isopropylcyclohexane.

[12] The chemical solution according to any one of [1] to

[11] , further comprising Mn atoms, wherein the content of the Mn atoms is 0.001 to 10 ppt by mass relative to the total mass of the chemical solution.

[13] Further, the composition contains Mn atoms and Fe atoms, and the ratio of the content of the Mn atoms to the content of the Fe atoms is 1.0 × 10 -3

[14] The chemical solution according to any one of [1] to

[13] , which is used as at least one selected from the group consisting of a cleaning solution, a developer, a pre-wet solution, and a rinse solution.

[15] The chemical solution according to any one of [1] to

[14] , which is used as at least one selected from the group consisting of a pre-wet solution, a rinse solution, a cleaning solution, and a developer, in a semiconductor substrate manufacturing process having a step of forming a metal resist film.

[16] A chemical solution container comprising a container and the chemical solution according to any one of [1] to

[15] contained in the container.

[17] The chemical solution container according to

[16] , wherein a liquid-contacting portion of the container that comes into contact with the chemical solution is formed of a non-metallic material or stainless steel.

[18] The drug solution container according to

[16] or

[17] , wherein the non-metallic material is at least one selected from the group consisting of polyethylene resin, polypropylene resin, polyethylene-polypropylene resin, tetrafluoroethylene resin, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-hexafluoropropylene copolymer resin, tetrafluoroethylene-ethylene copolymer resin, trifluorochloroethylene-ethylene copolymer resin, vinylidene fluoride resin, trifluorochloroethylene copolymer resin, and vinyl fluoride resin.

[0009] According to the present invention, it is possible to provide a chemical solution that is excellent in in-plane cleanliness uniformity on a substrate, excellent in wafer bevel cleaning performance, and excellent in performance in suppressing the occurrence of defects on a substrate when brought into contact with the substrate. The present invention also provides a chemical solution container that contains the above chemical solution.

[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0011] In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0012] As used herein, "actinic rays" or "radiation" refers to, for example, the bright line spectrum of a mercury lamp, far ultraviolet rays typified by excimer lasers, extreme ultraviolet rays (EUV light: Extreme Ultraviolet), X-rays, and electron beams (EB: Electron Beam). As used herein, "light" refers to actinic rays or radiation. Unless otherwise specified, "exposure" as used herein includes not only exposure using the bright line spectrum of a mercury lamp, far ultraviolet rays typified by excimer lasers, extreme ultraviolet rays, X-rays, and EUV light, but also drawing using particle beams such as electron beams and ion beams.

[0013] Unless otherwise specified, the substituent is preferably a monovalent substituent. The bonding direction of a divalent group described in this specification is not limited unless otherwise specified. For example, when Y is -COO- in a compound represented by the formula "X-Y-Z", Y may be -CO-O- or -O-CO-. Furthermore, the compound may be "X-CO-O-Z" or "X-O-CO-Z". In this specification, examples of halogen atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0014] In this specification, the term "solid content" refers to components that form a metal resist film, and does not include solvents (e.g., organic solvents, water, etc.). In addition, any component that forms a metal resist film is considered to be a solid content even if it is in a liquid state. In this specification, when two or more types of a component are present, the "content" of that component refers to the total content of those two or more components. In this specification, "ppm" means "parts-per-million (10 -6 ) and "ppb" stands for "parts-per-billion (10 -9 ) and "ppt" stands for "parts-per-trillion (10 -12 )"

[0015] The chemical solution, the chemical solution container, the preparation of the chemical solution, and the method for manufacturing the electronic device according to the present invention will be described below in order.

[0016] [Chemical Solution] The chemical solution of the present invention will be described in detail below. The chemical solution of the present invention is a chemical solution containing 2-heptanone, water, and a carbonyl compound having 6 to 8 carbon atoms other than 2-heptanone (hereinafter also referred to as a "specific carbonyl compound"), wherein the content of 2-heptanone is 60 mass% or more relative to the total mass of the chemical solution, the content of water is 1 to 1000 mass ppm relative to the total mass of the chemical solution, and P (hereinafter also simply referred to as the "P value") calculated by the formula (1) described below is 3 to 10. Hereinafter, the term "excellent effects of the present invention" refers to an excellent chemical solution in at least one of the following: in-plane uniformity of cleanliness on a substrate, wafer bevel cleanability, and ability to suppress the occurrence of defects on a substrate when brought into contact with the substrate.

[0017] [2-Heptanone] The chemical solution of the present invention contains 2-heptanone. The content of 2-heptanone is 60% by mass or more relative to the total mass of the chemical solution. When the content of 2-heptanone in the chemical solution is within the above range, a chemical solution having excellent dissolving ability for metal resist films can be obtained. The content of 2-heptanone is preferably 65% ​​by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, in terms of even better dissolving ability for metal resist films. The upper limit is not particularly limited, and may be the remainder other than water, the specific carbonyl compound, and the optional components described below. The content of 2-heptanone is, for example, 99.999% by mass or less relative to the total mass of the chemical solution, and preferably 99.99% by mass or less.

[0018] [Water] The chemical solution of the present invention contains water. The content of water contained in the chemical solution of the present invention is 1 to 1,000 ppm by mass relative to the total mass of the chemical solution. In a chemical solution containing 2-heptanone, water, and a specific carbonyl compound, the water content within the above range improves the ability to suppress the occurrence of defects on a substrate when the chemical solution is brought into contact with the substrate (hereinafter, also referred to as "moisture-induced defect suppression"). The reason why the water content within the above range improves the suppression of moisture-induced defects is unclear; however, it is thought that, for example, a water content equal to or greater than the above lower limit increases the electrical conductivity of the chemical solution and suppresses surface charging of components (e.g., piping, filters, etc.) that come into contact during the chemical solution preparation process. This suppresses the generation of sparks that cause dielectric breakdown of the contact components, thereby suppressing the introduction of foreign matter due to dielectric breakdown and the occurrence of defects on the substrate surface caused by foreign matter. Furthermore, it is thought that a water content equal to or less than the above upper limit can suppress the occurrence of stain-like defects due to moisture remaining on the substrate surface.

[0019] From the above viewpoints, the lower limit of the water content is preferably 5 ppm by mass or more, and more preferably 10 ppm by mass or more, relative to the total mass of the chemical solution. From the above viewpoints, the upper limit of the water content is preferably 500 ppm by mass or less, and more preferably 100 ppm by mass or less, relative to the total mass of the chemical solution. The water content can be measured using an apparatus that employs the Karl Fischer moisture determination method as its measurement principle. For example, a Karl Fischer moisture meter (product name "MKC-710M", manufactured by Kyoto Electronics Manufacturing Co., Ltd., Karl Fischer coulometric titration type) can be used as the apparatus.

[0020] Examples of water include distilled water, ion-exchanged water, pure water, and ultrapure water, with ultrapure water being preferred. Water may be intentionally added, water inevitably contained in the raw materials of the chemical solution, or water inevitably contained during the production, storage, and / or transportation of the chemical solution.

[0021] The method for adjusting the water content is not particularly limited, and examples include methods for removing water from the chemical solution and / or raw materials used in preparing the chemical solution, methods for adding water, and combinations thereof. Water removal methods can be performed using known dehydration methods, such as dehydration using a water adsorbent, distillation, and dehydration using a dehydration membrane. Examples of water adsorbents include zeolite (e.g., molecular sieves), sodium sulfate, magnesium sulfate, silica gel, calcium chloride, anhydrous zinc chloride, fuming sulfuric acid, and soda lime. Examples of dehydration methods using a dehydration membrane include membrane dehydration by pervaporation (PV) or vapor permeation (VP). Examples of the dehydration membrane include membranes made of polymeric materials such as polyimide, cellulose, and polyvinyl alcohol, as well as inorganic materials such as zeolite.

[0022] [Specific Carbonyl Compound] The chemical solution of the present invention contains a specific carbonyl compound, which is a carbonyl compound having 6 to 8 carbon atoms other than 2-heptanone.

[0023] The specific carbonyl compound is not particularly limited as long as it is a compound other than 2-heptanone, has a carbonyl group, and has 6 to 8 carbon atoms, and examples thereof include ketones having 6 to 8 carbon atoms other than 2-heptanone (hereinafter also referred to as "specific ketones"), and aldehydes having 6 to 8 carbon atoms (hereinafter also referred to as "specific aldehydes"). The number of carbonyl groups that the specific carbonyl compound has is not particularly limited, but is preferably 1 or 2, and more preferably 1. The specific carbonyl compound is a C 6 H 12 O.C. 7 H 14 O and C 8 H 16 Preferably, the carbonyl compound is a carbonyl compound represented by any one of the chemical formulas of C 7 H 14 It is more preferable that the carbonyl compound is a carbonyl compound represented by O.

[0024] Among the specific carbonyl compounds, examples of the specific ketones include ketones having 6 carbon atoms such as 2-hexanone, 3-hexanone, 4-methyl-2-pentanone, and 3-methyl-2-pentanone; ketones having 7 carbon atoms (excluding 2-heptanone) such as 3-heptanone, 4-heptanone, 5-methyl-2-hexanone, 5-methyl-3-hexanone, and 4-methyl-3-hexanone; and ketones having 8 carbon atoms such as 2-octanone, 3-octanone, 4-octanone, 5-methyl-2-heptanone, 5-methyl-3-heptanone, and 4-methyl-3-heptanone. Among these, 5-methyl-2-hexanone, 4-heptanone, 3-heptanone, or 5-methyl-3-hexanone is preferred, and 5-methyl-2-hexanone or 4-heptanone is more preferred, as they provide better effects for the present invention.

[0025] Among the specific carbonyl compounds, examples of the specific aldehyde include aldehydes having 6 carbon atoms such as 2-methylpentanal, 2-ethylbutanal, and 3-methylpentanal; aldehydes having 7 carbon atoms such as 2-methylhexanal, 2-ethyl-3-methylbutanal, 2-ethylpentanal, and 3-methylhexanal; and aldehydes having 8 carbon atoms such as 2-methylheptanal, 2-ethyl-3-methylpentanal, 2-ethylhexanal, and 6-methylheptanal. Among these, 2-methylhexanal, 2-ethyl-3-methylbutanal, and 2-ethylhexanal are preferred in terms of the superior effects of the present invention.

[0026] As the specific carbonyl compound, 5-methyl-2-hexanone, 4-heptanone, 3-heptanone, 5-methyl-3-hexanone, 2-methylhexanal, 2-ethyl-3-methylbutanal, or 2-ethylhexanal is preferred, and 5-methyl-2-hexanone or 4-heptanone is more preferred, in terms of better effects of the present invention.

[0027] The specific carbonyl compound may be used alone or in combination of two or more. When the chemical solution contains two or more specific carbonyl compounds, it may contain two or more specific ketones, may contain two or more specific aldehydes, or may contain a combination of one or more specific ketones and one or more specific aldehydes.

[0028] <Ratio of Content of Specific Ketone to Content of Specific Aldehyde> When the chemical solution contains a combination of a specific ketone and a specific aldehyde, the contents of both are not particularly limited. However, in order to obtain the effects of the present invention and to achieve a more excellent performance in suppressing adhesion of organic substances to the substrate after cleaning, it is preferable that the ratio of the content of the specific aldehyde to the content of the specific ketone in the chemical solution is 1.0 × 10 -6 ~1.0 x 10 3 It is preferable that the -5 ~1.0 x 10 2 More preferably, it is 1.0 × 10 -4 ~5.0 x 10 1 More preferably, it is 1.0 × 10 -3 ~1.0 x 10 1 The specific ketone and the specific aldehyde have different polarities and reactivities, and it is presumed that by mixing substances with such different properties within the above ratio range, the removal performance and rinsing performance of the metal resist on the surface to be removed are improved.

[0029] The content of the specific carbonyl compound is preferably 0.1 ppm by mass or more, more preferably 0.5 ppm by mass or more, and even more preferably 1.0 ppm by mass or more, relative to the total mass of the chemical solution, and preferably 1,000 ppm by mass or less, more preferably 500 ppm by mass or less, and even more preferably 100 ppm by mass or less, relative to the total mass of the chemical solution.

[0030] The contents of specific carbonyl compounds and organic compounds such as specific cycloalkane compounds, which will be described later, contained in the chemical solution can be measured using a GC-MS (gas chromatography mass spectrometry). As the GC-MS, a known GC-MS device can be used, such as a device that combines a gas chromatograph "7890B" (manufactured by Agilent) with a mass spectrometer "JMS-Q1500" (manufactured by JEOL Ltd.).

[0031] The method for adjusting the content of the specific carbonyl compound is not particularly limited, but examples include a method in which a liquid to be purified containing 2-heptanone as a main component and containing very little organic impurities such as the specific carbonyl compound is prepared by the method described below, and then a purification treatment is carried out as necessary, and then the specific carbonyl compound is further added as necessary.

[0032] [P Value] The chemical solution of the present invention is characterized by containing water and a specific carbonyl compound in amounts such that the P value calculated by the following formula (1) satisfies 3 to 10: P=-log 10 (X×Y) Formula (1) X represents the value X when the concentration of water in the chemical solution is X mol / L, and Y represents the value Y when the concentration of the carbonyl compound in the chemical solution is Y mol / L.

[0033] In a chemical solution containing 2-heptanone, water, and a specific carbonyl compound, the P value within the above range improves the in-plane uniformity of cleanliness on a substrate contacted with the chemical solution (hereinafter also referred to as "in-plane uniformity of cleanliness") and the cleaning performance on the bevel portion of the substrate contacted with the chemical solution (hereinafter also referred to as "wafer bevel cleanability"). While the reason why a P value within the above range improves the suppression of moisture-induced defects is unclear, the following reason is presumed. It is believed that the specific carbonyl compound adsorbs to the surface of a substrate formed from silicon or a silicon derivative material (such as TEOS, low-k material, or SiN), causing defects or affecting the action of the chemical solution on the target object. In particular, with cutting-edge semiconductor devices, even trace amounts of organic impurities other than the main solvent in the chemical solution used in the manufacturing process are thought to affect yield. On the other hand, when the chemical solution contains the specific carbonyl compound and water in amounts such that the P value is equal to or less than the above-mentioned upper limit, the carbonyl group of the specific carbonyl compound is hydrated to form a hydrate that has a smaller dipole moment than the specific carbonyl compound and is therefore less likely to adhere to the substrate surface, thereby reducing the area on the substrate surface that has been affected by the specific carbonyl compound different from 2-heptanone, and as a result, it is presumed that the in-plane uniformity of cleanliness on the substrate surface is improved. Also, when the chemical solution contains the specific carbonyl compound and water in amounts such that the P value is equal to or greater than the above-mentioned lower limit, the amount of the hydrate, which has significantly different wettability from the main component, 2-heptanone, is suppressed to a predetermined amount or less, thereby maintaining the fluidity of the chemical solution in the bevel portion having an edge bead and improving the cleaning performance of the bevel portion.

[0034] The P value in the chemical solution is preferably 3.5 or more, more preferably 4 or more, and even more preferably 5 or more, in terms of providing better effects of the present invention. The P value in the chemical solution is preferably 9 or less, more preferably 8.5 or less, and even more preferably 8 or less, in terms of providing better effects of the present invention.

[0035] [Optional Components] The chemical solution may contain optional components other than those described above, such as a specific cycloalkane compound, metal atoms such as Mn atoms and Fe atoms, and a surfactant, as described below.

[0036] <Specific cycloalkane compound> The chemical solution may further contain a cycloalkane compound having a boiling point of 160°C or higher and having 8 to 12 carbon atoms (hereinafter also referred to as "specific cycloalkane compound"), and preferably contains the specific cycloalkane compound.

[0037] The specific cycloalkane compound is not particularly limited as long as it has a boiling point of 160°C or higher, has a cycloalkane ring, and has 8 to 12 carbon atoms. The cycloalkane ring of the specific cycloalkane compound may be monocyclic or polycyclic, but is preferably monocyclic. Examples of the cycloalkane ring include cycloalkane rings having 5 to 10 carbon atoms, and a cyclopentane ring, a cyclohexane ring, or a cycloheptane ring is preferred, with a cyclohexane ring being more preferred.

[0038] The cycloalkane ring may have a substituent. The specific cycloalkane compound is preferably a compound in which the cycloalkane ring has a substituent. As the substituent, for example, a hydrocarbon group is preferred, and an alkyl group is more preferred. That is, the specific cycloalkane compound is preferably a hydrocarbon. The number of carbon atoms in the hydrocarbon group and the alkyl group is appropriately selected so that the total number of carbon atoms together with the number of carbon atoms in the cycloalkane ring is 8 to 12, for example, 1 to 3. The cycloalkane ring may have only one type of substituent, or may have two or more types of substituents. Furthermore, the specific cycloalkane compound is preferably a compound having a boiling point of 150 to 190°C, more preferably a compound having a boiling point of 160 to 180°C.

[0039] Specific examples of the specific cycloalkane compound include 1-methyl-2-isopropylcyclohexane (boiling point: 170.85°C), 1-methyl-3-isopropylcyclohexane (boiling point: 161°C), 1-methyl-4-isopropylcyclohexane (boiling point: 171°C), 1-methyl-2-propylcyclohexane (boiling point: 176.15°C), 1-methyl-3-propylcyclohexane (boiling point: 172.55°C), and 1-methyl-4-propylcyclohexane (boiling point: 170.08°C). Among these, 1-methyl-2-isopropylcyclohexane, 1-methyl-3-isopropylcyclohexane, or 1-methyl-4-isopropylcyclohexane is preferred, and 1-methyl-4-isopropylcyclohexane is more preferred.

[0040] The specific cycloalkane compound may be used alone or in combination of two or more. The content of the specific cycloalkane compound may be, for example, 0.1 to 1000 ppm by mass, relative to the total mass of the chemical solution. The content of the specific cycloalkane compound is preferably 0.3 ppm by mass or more, more preferably 0.5 ppm by mass or more, and even more preferably 1.0 ppm by mass or more, relative to the total mass of the chemical solution. When the chemical solution contains the specific cycloalkane compound within the above content range, treating a substrate with the chemical solution can improve the performance of dissolving and removing organic matter with low polarity attached to the surface of the substrate. Furthermore, the content of the specific cycloalkane compound is preferably 1000 ppm by mass or less, more preferably 700 ppm by mass or less, even more preferably 500 ppm by mass or less, and particularly preferably 100 ppm by mass or less, relative to the total mass of the chemical solution, in order to prevent the specific cycloalkane compound from remaining as organic matter on the substrate after contact with the chemical solution and drying and / or baking.

[0041] <Metal Atoms> The chemical solution may contain Mn atoms (manganese atoms). The chemical solution preferably contains Mn atoms, since this suppresses the occurrence of defects resulting from the chemical solution when the chemical solution is brought into contact with a substrate. The form of the Mn atoms in the chemical solution is not particularly limited, and the Mn atoms may be contained as Mn particles or Mn ions. The Mn particles may be in the form of a simple substance consisting of Mn atoms, an alloy of Mn atoms with other metal atoms, or Mn atoms associated with an organic substance. The Mn ions may form a salt and / or a complex.

[0042] The content of Mn atoms in the chemical solution is preferably 20 mass ppt or less, more preferably 10 mass ppt or less, even more preferably 7.5 mass ppt or less, particularly preferably 5 mass ppt or less, and most preferably 1.0 mass ppt or less, relative to the total mass of the chemical solution. By keeping the Mn atom content within the above range, the occurrence of nanoparticle defects derived from Mn atoms can be suppressed. The lower limit of the Mn atom content is preferably 0.001 mass ppt or more, more preferably 0.005 mass ppt or more, and even more preferably 0.01 mass ppt or more, relative to the total mass of the chemical solution.

[0043] The chemical solution may contain Fe (iron) atoms in addition to Mn atoms. The form of the Fe atoms in the chemical solution is not particularly limited, and they may be contained as Fe particles or Fe ions. The Fe particles may be in the form of a simple substance consisting of Fe atoms, an alloy of Fe atoms and metal atoms other than Mn, or an Fe atom associated with an organic substance. The Fe ions may form a salt and / or a complex.

[0044] When the chemical solution contains Mn atoms and Fe atoms, the effect of the present invention and the suppression of defects derived from the chemical solution are more excellent, and the ratio of the content of Mn atoms to the content of Fe atoms in the chemical solution (hereinafter also referred to as the "Mn / Fe ratio") is 1.0 × 10 -3 Preferably, up to 1.0, and 1.0 x 10 -2 ~7.0 x 10 -1 More preferably, 1.0 × 10 -2 ~5.0 x 10 -1 is more preferably 5.0 × 10 -2~2.5 x 10 -1 is particularly preferred. Although the reason why a Mn / Fe ratio within the above range provides excellent suppression of chemical-induced defects is unclear, it is presumed that a Mn / Fe ratio equal to or less than the above upper limit reduces the relative content of Mn, which has a lower oxidation-reduction potential than Fe and is likely to exist as an ion, thereby suppressing the proportion of particulate Fe among Fe atoms and making it possible to suppress the occurrence of chemical-induced defects caused by particulate Fe. Furthermore, it is presumed that a Mn / Fe ratio equal to or greater than the above lower limit makes it possible to suppress the occurrence of nanoparticle defects caused by Fe atoms.

[0045] The content of Fe atoms in the chemical solution is preferably 0.01 to 200 mass ppt, more preferably 0.05 to 100 mass ppt, still more preferably 0.1 to 50 mass ppt, and particularly preferably 0.1 to 1 mass ppt, relative to the total mass of the chemical solution.

[0046] Mn atoms and Fe atoms (hereinafter collectively referred to as "specific metal atoms") may be intentionally added, unavoidably contained in the raw materials of the chemical solution, or unavoidably contained during the production, storage, and / or transportation of the chemical solution. The method for adjusting the content of the specific metal atoms is not particularly limited, and examples include a method for removing the specific metal atoms from the chemical solution and / or the raw materials used to prepare the chemical solution, a method for adding a component containing the specific metal atoms (a specific metal atom source), and a combination thereof. Removing the specific metal atoms from the chemical solution and / or the raw materials used to prepare the chemical solution includes, for example, removing metal particles and metal ions from the raw materials. Among these, a method for adding a specific metal atom source to a mixture of raw materials from which the specific metal atoms have been removed is preferred because it simplifies composition control. The method for removing the specific metal atoms may be appropriately selected from known methods depending on the form of the specific metal atoms in the chemical solution and / or the raw materials used to prepare the chemical solution. Examples include purification processes such as ion removal and filtration, which will be described later. When the specific metal atoms are in the form of metal particles, filtration is preferred, and when the specific metal atoms are in the form of metal ions, ion removal is preferred. The specific metal atom source is not particularly limited, and examples thereof include metal particles such as metal nanoparticles, metal oxide particles, and compounds containing metal ions such as metal salts (e.g., metal halides) and organometallic complexes, with metal nanoparticles being preferred.

[0047] The chemical solution preferably contains metal atoms other than Mn atoms and Fe atoms (e.g., Pb, Cr, Ni, Sn, Co, Na, Cu, Mg, Li, Al, and Ag) at a content of 1000 mass ppt or less, and more preferably 500 mass ppt or less. Since it is expected that chemical solutions of even higher purity will be required in the manufacture of cutting-edge semiconductor devices, the content of the above-mentioned other metal atoms is more preferably less than 500 mass ppt, particularly preferably less than 150 mass ppt, and most preferably less than 100 mass ppt. The lower limit is preferably 0.

[0048] Examples of the method for reducing the other metal atoms include purification processes such as filtration, ion removal, and distillation, which will be described later. Other examples include a method of using a container that is less likely to leach out metal components as a container for containing raw materials or the produced chemical solution, and a method of lining the inner wall of a pipe or the like with a fluororesin to prevent metal components from leaching out from the pipe during the production of the chemical solution.

[0049] The types and contents of Mn atoms, Fe atoms, and the other metal atoms can be measured by ICP-MS (inductively coupled plasma mass spectrometry). Examples of instruments that can be used to perform ICP-MS include Agilent 8900 triple quadrupole ICP-MS (inductively coupled plasma mass spectrometry, for semiconductor analysis, option #200) manufactured by Agilent Technologies, NexION350S manufactured by PerkinElmer, and Agilent 8800 manufactured by Agilent Technologies.

[0050] When measuring the content of the metal atoms in the chemical solution, the chemical solution may be concentrated before measurement. The chemical solution is concentrated according to the following procedure. A polytetrafluoroethylene container is used as the container for concentration. The chemical solution is then heated to 160 to 180°C while refluxing, and at least a portion of the organic solvent and water contained in the chemical solution is removed, thereby concentrating the chemical solution. Note that, in the concentration step, the content of metal atoms in the chemical solution is calculated for chemical solutions whose concentration ratio is changed from 10 to 1000 times. If a positive correlation (positive linear correlation) is observed between the concentration ratio and the value of the content of metal atoms, it can be confirmed that the content of metal atoms contained in the chemical solution can be quantified using the above method.

[0051] <Surfactant> As the surfactant, known surfactants can be used, for example, nonionic surfactants and fluorine-based surfactants can be used. As the surfactant, for example, the compounds exemplified in paragraph

[0126] of WO 2022 / 044893 can be used.

[0052] <Coarse particles> The chemical solution may contain coarse particles, but the content thereof is preferably low. Coarse particles refer to particles having a diameter (particle size) of 1 μm or more when the particle shape is considered to be a sphere. The coarse particles contained in the chemical solution include particles such as dust, dirt, organic solids, and inorganic solids contained as impurities in the raw material, as well as particles such as dust, dirt, organic solids, and inorganic solids brought in as contaminants during the preparation of the chemical solution, and which ultimately exist as particles without dissolving in the chemical solution.

[0053] The content of coarse particles in the chemical solution is preferably 100 or less, more preferably 50 or less, particles with a particle size of 1 μm or more per mL of the chemical solution. The lower limit is preferably 0. The content of coarse particles present in the chemical solution can be measured in the liquid phase using a commercially available measuring device that uses a laser as a light source for light scattering liquid particle measurement. Methods for removing coarse particles include, for example, purification processes such as filtration, which will be described later.

[0054] [Uses] The chemical solution of the present invention can be used in the manufacturing process of semiconductor substrates, and is particularly suitable as a processing solution for semiconductor substrates. Examples of such processing solutions include cleaning solutions (etching solutions) for removing target materials from semiconductor substrates, developers for removing resist films formed on semiconductor substrates, rinse solutions for rinsing away substances adhering to semiconductor substrates, and pre-wet solutions applied to semiconductor substrates to improve the coatability of resist compositions. In particular, the chemical solution is preferably used as a cleaning solution (more preferably, a metal resist cleaning solution such as an edge bead remover), developer, rinse, or pre-wet solution in a semiconductor substrate manufacturing process that includes a step of forming a metal resist film using a metal resist composition. The chemical solution of the present invention can also be used for other purposes, such as a filter cleaning solution, a pipe cleaning solution, and a tank cleaning solution.

[0055] In order to avoid dissolution of the pattern formed using the metal resist composition, it is preferable to use a chemical solution that has a lower solubility for the metal resist film than the developer solution as the rinse solution. Here, the "solubility of the metal resist film" possessed by the developer solution or rinse solution is an index indicating the ease with which the metal resist film dissolves in the developer solution or rinse solution. For example, when two types of chemical solutions are supplied to the metal resist film in equal amounts, the chemical solution that dissolves the metal resist film less per unit time (volume reduction) is the chemical solution with a relatively low solubility for the metal resist film. Generally, the developer solution has a solubility that does not dissolve the metal resist film in the exposed area. However, if a rinse solution with a higher solubility than the developer solution is used, the metal resist film in the exposed area will dissolve, causing concern about the collapse of the pattern shape. Furthermore, in some areas where the metal resist film is present in the exposed area, the polymerization reaction may proceed more slowly than in other areas of the resist film in the exposed area, and this area may become more soluble in organic solvents. In the above case, if the solubility of the metal resist film is the same in the rinse solution and the developer, there is a concern that the area will dissolve slightly, leading to the collapse of the pattern shape. Therefore, it is presumed that the collapse of the pattern can be suppressed by using a chemical solution as the rinse solution that has a lower solubility of the metal resist film than the developer.

[0056] When the chemical solution of the present invention is used as a developer and then a rinse solution is used for cleaning, the rinse solution is not particularly limited as long as it is a chemical solution or rinse solution that dissolves the metal resist film less than the developer. The rinse solution may be a mixture of two or more organic solvents. When the developer is the chemical solution of the present invention, examples of the rinse solution include methyl isobutyl carbinol (MIBC), PGMEA (propylene glycol monomethyl ether acetate), PGME (propylene glycol monomethyl ether), a mixture of PGMEA and PGME, and n-butyl acetate (nBA). The rinse solution may be purified by a purification method for various components contained in the chemical solution, which will be described later.

[0057] [Method for Preparing Chemical Solution] The chemical solution can be prepared by a known method. For example, it can be prepared by mixing the above-mentioned components to a predetermined concentration. The order in which the components are mixed is not particularly limited. In order to remove excess components and / or impurities, the raw materials for the chemical solution and / or a mixture thereof may be subjected to a purification treatment. In particular, for 2-heptanone, water, the specific carbonyl compound, and the specific cycloalkane compound, it is preferable to prepare the chemical solution using products obtained by subjecting a purification treatment to a material to be purified containing each component. Furthermore, when preparing a chemical solution containing a predetermined amount of the above-mentioned specific metal atoms, it is preferable to subject a material to be purified containing each component (2-heptanone, water, the specific carbonyl compound, and the specific cycloalkane compound) to a purification treatment as described above to reduce impurities such as the specific metal atoms, and then to supply a predetermined amount of the specific metal atoms to a mixture obtained by mixing the obtained raw materials, thereby preparing a chemical solution containing the predetermined component. By subjecting the material to be purified containing the components used (2-heptanone, water, the specific carbonyl compound, and the specific cycloalkane compound) to a purification treatment as described above, impurities other than the specific metal atoms can also be reduced.

[0058] The above-mentioned purification target material may be procured by purchase or may be synthesized from raw materials. It is preferable that the purification target material has a low impurity content. Examples of commercially available products of such purification target material include those called "semiconductor grade products" or "high purity grade products."

[0059] The above-mentioned 2-heptanone-containing purification product contains very little of the above-mentioned components other than 2-heptanone, and adding the above-mentioned components other than 2-heptanone makes it much easier to adjust the content of each component within the above-mentioned range. Therefore, it is preferable to prepare the product by a method of synthesizing 2-heptanone by the hydration reaction of an alkyne. Specifically, 1-heptyne is reacted with water in the presence of an acid catalyst and mercury ions, and water is added to the triple bond of 1-heptyne to produce 1-hepten-2-ol, which is then subjected to keto-enol tautomerization, thereby preparing a purification product containing 2-heptanone. Note that, for the above-mentioned method of synthesizing 2-heptanone by the hydration reaction of an alkyne, reference can be made to the synthesis method described on page 283 of "Organic Chemistry, 4th Edition" (by William H. Brown, Christopher S. Foote, and Brent L. Iverson, Brooks / Cole Publishing Company, 2004).

[0060] Known methods can be used to purify the product to be purified, including, for example, filtration, ion removal, and distillation. The purification method for the product to be purified may involve a combination of multiple processes selected from the group consisting of filtration, ion removal, and distillation. For example, a primary purification process may be performed by distilling the product to be purified, followed by a secondary purification process in which the resulting product is passed through an ion exchange resin and / or a filter. Alternatively, a primary purification process may be performed by passing the product to be purified through an ion exchange resin and / or a filter, followed by a secondary purification process in which the resulting product is distilled. Each purification process may be performed multiple times.

[0061] <Filtration Treatment> The filtration treatment method is not particularly limited, and known methods can be used. Among them, filtering in which the material to be purified is filtered using a filter is preferred. Components removed by filtration treatment are not particularly limited, but examples thereof include metal particles and coarse particles.

[0062] The filter used for filtering is not particularly limited, and known filters can be used. Examples of materials for the filter include fluororesins such as PTFE (polytetrafluoroethylene) and PFA (perfluoroalkoxyalkane), polyamide resins such as 6-nylon and 6,6-nylon, polyolefin resins (including high density and ultra-high molecular weight) such as polyethylene and polypropylene, diatomaceous earth, and glass. Among these, PTFE, polyamide resins, UPE (ultra-high density polyethylene), HDPE (high density polyethylene), and HDPP (ultra-high density polypropylene) are preferred. Using a filter made of these materials can more effectively remove highly polar foreign matter and metal impurities that are likely to cause particle defects.

[0063] The critical surface tension of the filter is preferably 70 to 95 mN / m, and more preferably 75 to 85 mN / m. The manufacturer's nominal value can be used as the critical surface tension value. By using a filter with a critical surface tension within the above range, highly polar foreign matter that is likely to cause particle defects and metal impurities can be more effectively removed.

[0064] The pore size of the filter is preferably 0.1 nm to 1.0 μm, more preferably 0.5 nm to 0.1 μm, and even more preferably 1.0 to 50.0 nm. By setting the pore size of the filter within this range, fine foreign matter contained in the product to be purified can be effectively removed while preventing clogging of the filter.

[0065] The filter may be surface-treated. The surface treatment method is not particularly limited, and known methods can be used. Examples of surface treatments include chemical modification treatment, plasma treatment, hydrophobic treatment, coating, gas treatment, and sintering, with chemical modification treatment or plasma treatment being preferred. The chemical modification treatment is preferably a treatment to introduce ion exchange groups. That is, the filter may be an ion exchange filter. Examples of the ion exchange groups include cation exchange groups such as sulfonic acid groups, carboxy groups, and phosphate groups, and anion exchange groups such as quaternary ammonium groups. The method for introducing ion exchange groups into the filter is not particularly limited, and examples include a method in which a compound containing an ion exchange group and a polymerizable group is reacted with a polymer contained in the filter to perform grafting.

[0066] The filtering may be a multistage filtration process in which the purified product is passed through two or more filters, each differing in at least one property selected from the group consisting of filter material, pore size, and pore structure. The purified product may be passed through the same filter multiple times, or through multiple filters of the same type. Among these, a circulating filtration process is preferred, in which the purified product is passed through multiple filters using a filtration device combining multiple filters and return paths. The number of cycles in the circulating filtration process is not particularly limited and may be selected appropriately depending on the desired purity and impurities. However, 2 to 100 cycles are preferred, 20 to 80 cycles are more preferred, and 30 to 70 cycles are even more preferred. The number of filters to be combined is not particularly limited, but 1 to 10 are preferred, and 2 to 5 are more preferred. When filtering using a combination of different filters, it is preferable that the pore size of the filter that comes into contact with the liquid first is the same as or larger than the pore size of the filter that comes into contact with the liquid second. The nominal pore size can be determined by referring to the filter manufacturer's nominal value.

[0067] Commercially available filters can be selected from various filters provided by, for example, Nippon Pall Co., Ltd., Advantec Toyo Co., Ltd., Nippon Entegris Co., Ltd., Kitz Microfilter Co., Ltd., and the like.

[0068] The temperature during filtering is preferably 25° C. or lower, more preferably 23° C. or lower, and even more preferably 20° C. or lower. The lower limit is preferably 0° C. or higher, more preferably 5° C. or higher, and even more preferably 10° C. or higher. When the temperature during filtering is within the above range, particulate foreign matter and impurities dissolved in the chemical solution are precipitated and can be efficiently removed.

[0069] <Ion Removal Treatment> The ion removal treatment is a treatment in which the product to be purified is subjected to ion exchange or ion adsorption by a chelating group. The components removed by the ion removal treatment are not particularly limited, but examples thereof include acids and metal ions.

[0070] The method of ion exchange treatment is not particularly limited, and known methods can be used. For example, a method of contacting the material to be purified with an ion exchange resin can be mentioned, and a method of passing the material to be purified through a packing section filled with ion exchange resin is preferred. In the ion exchange treatment, the material to be purified may be passed through the same ion exchange resin multiple times, or may be passed through different ion exchange resins.

[0071] Examples of ion exchange resins include anion exchange resins and cation exchange resins. When both cation exchange resins and anion exchange resins are used, the ion exchange resin may be passed through a packed section filled with a mixed resin containing both resins, or may be passed through multiple packed sections filled with each resin.

[0072] As the anion exchange resin, known anion exchange resins can be used, and it is preferable to use a gel-type anion exchange resin, such as a strongly basic anion exchange resin having a quaternary ammonium group and a weakly basic anion exchange resin having an amino group. As the anion exchange resin, commercially available products can be used, and examples thereof include Amberlite IRA-400J, Amberlite IRA-410J, Amberlite IRA-900J, Amberlite IRA67, ORLITE DS-2, ORLITE DS-5, and ORLITE DS-6 (manufactured by Organo Corporation), Duolite A113LF, Duolite A116, and Duolite A-375LF (manufactured by Sumika Chemtex Co., Ltd.), and DIAION SA12A, DIAION SA10A, DIAION SA10AOH, DIAION SA20A, and DIAION WA10 (manufactured by Mitsubishi Chemical Corporation). As the anion exchange resin, the anion exchange resin described in JP-A-2009-155208 can also be used.

[0073] As the cation exchange resin, known cation exchange resins can be used, and gel-type cation exchange resins are preferred. Specific examples of the cation exchange resin include sulfonic acid-type cation exchange resins and carboxylic acid-type cation exchange resins. As the cation exchange resin, commercially available products can be used, and examples thereof include Amberlite IR-124, Amberlite IR-120B, Amberlite IR-200CT, ORLITE DS-1, ORLITE DS-4 (all manufactured by Organo Corporation), Duolite C20J, Duolite C20LF, Duolite C255LFH, Duolite C-433LF (all manufactured by Sumika Chemtex Co., Ltd.), DIAION SK-110, DIAION SK1B, and DIAION SK1BH (all manufactured by Mitsubishi Chemical Corporation), Purolite S957, and Purolite S985 (all manufactured by Purolite Co., Ltd.), and the like.

[0074] The ion adsorption treatment using chelating groups is not particularly limited, and known methods can be used. For example, a method in which the material to be purified is passed through a packed section filled with a chelating resin having chelating groups can be used. In the ion removal treatment, the material to be purified may be passed through the same chelating resin multiple times, or may be passed through different chelating resins.

[0075] Examples of the chelating resin include a chelating group or a resin having chelating ability, such as an amidoxime group, a thiourea group, a thiouronium group, iminodiacetic acid, amidophosphoric acid, phosphonic acid, aminophosphoric acid, aminocarboxylic acid, N-methylglucamine, an alkylamino group, a pyridine ring, a cyclic cyanine, a phthalocyanine ring, and a cyclic ether.

[0076] The ion removal treatment may be combined with the above-mentioned filtration treatment. For example, a method may be used in which a column packed with an ion exchange resin is incorporated into the above-mentioned circulation filtration device, and the water is passed continuously through the ion exchange resin packed section and the filter.

[0077] <Distillation Treatment> The distillation treatment method is not particularly limited, and known methods can be used. For example, a method using a distillation column can be used. Components removed by the distillation step are not particularly limited, and examples thereof include acids, organic compounds, and water.

[0078] Although there are no particular limitations on the liquid-contacting parts of the distillation column, they are preferably made of a corrosion-resistant material, such as the materials used for the chemical containers described below.

[0079] In the distillation process, the material to be purified may be passed through the same distillation column multiple times, or through different distillation columns. When the material to be purified is passed through different distillation columns, for example, a crude distillation process is performed by passing the material through a distillation column to remove low-boiling point acids, and then a rectification process is performed by passing the material through a distillation column different from the crude distillation process to remove acid components and other organic compounds. In this case, the distillation column used in the crude distillation process may be a tray distillation column, and the distillation column used in the rectification process may be at least one of a tray distillation column and a vacuum tray distillation column. When a tray distillation column is used, the number of theoretical plates is preferably 50 or more, more preferably 100 or more. There is no particular upper limit, but it is often 200 or less. Furthermore, vacuum distillation may be used to achieve both thermal stability during distillation and purification accuracy.

[0080] The distillation treatment may be used in combination with at least one selected from the above-mentioned filtration treatment and ion removal treatment. For example, a distillation column may be disposed on the upstream side of the purification apparatus subjected to the above-mentioned filtration treatment, and the distilled product to be purified may be introduced into the purification apparatus.

[0081] <Other Purification Treatments> As a purification treatment other than the above, for example, a dehydration treatment may be carried out. As the dehydration treatment, for example, the above-mentioned water removal methods can be used.

[0082] A preferred method for preparing the chemical solution involves preparing a purification target containing 2-heptanone, water, and an organic acid, subjecting each target to a purification treatment, and mixing the resulting purified targets to prepare the chemical solution. The purification treatment preferably includes at least the distillation and filtration treatments described above. In this case, the order of the distillation and filtration treatments is not particularly limited; the filtration treatment may be performed after the distillation treatment, or after the filtration treatment. The filtration treatment preferably uses at least one first filter selected from the group consisting of ion exchange filters and filters containing polyamide resins (e.g., nylon filters) and at least one second filter selected from the group consisting of PTFE filters and UPE filters. The first filter primarily removes ionic impurities, and the second filter primarily removes particles (metal particles, organic fine particles, etc.). Multiple first and second filters may be used. It is particularly preferable to use three or more second filters. As described above, the filtration treatment may also involve a circulating filtration process. The number of times of the circulating filtration treatment is as described above, but is preferably 30 or more. As the distillation treatment, it is preferable to pass the product to be purified through different distillation columns. By carrying out the above-mentioned procedure, it is possible to reduce impurities contained in the raw material of the chemical solution, and as a result, it is possible to prepare a chemical solution with a low impurity content.

[0083] <Handling> Handling of chemicals, preparation, purification treatment, opening of containers, cleaning of containers and equipment, storage of chemicals, analysis, etc. are preferably all performed in a clean room. The clean room is preferably a clean room with a cleanliness of class 4 or higher as defined by the international standard ISO 14644-1:2015 established by the International Organization for Standardization. Specifically, it is preferable that the clean room meets any of ISO class 1, ISO class 2, ISO class 3, and ISO class 4, more preferably ISO class 1 or ISO class 2, and particularly preferably ISO class 1.

[0084] In order to maintain stable performance for a long period of time, it is preferable that the handling, preparation, purification, containing, and storage of the chemical solution be carried out at 30° C. or lower. The lower limit is preferably 5° C. or higher, and more preferably 10° C. or higher.

[0085] [Medicine Solution Container] The medicine solution may be stored in a container. The container and the medicine solution contained in the container are collectively referred to as a medicine solution container. The medicine solution container of the present invention includes the container and the medicine solution of the present invention contained in the container.

[0086] To prevent changes in the components of the solution during storage, the container may be filled with an inert gas (such as nitrogen or argon) with a purity of 99.99995% by volume or higher. A gas with a low moisture content is preferred as the inert gas. During transportation and / or storage, the solution may be stored at room temperature, but the temperature may be controlled to a range of -20°C to 20°C to prevent deterioration.

[0087] [Container] Known containers can be used as containers for containing chemical solutions, and those with a high level of cleanliness within the container for semiconductor applications and low elution of impurities are preferred. Examples of containers include the "Clean Bottle" series (manufactured by Aicello Chemical Co., Ltd.) and the "Pure Bottle" (manufactured by Kodama Resin Industry Co., Ltd.). Furthermore, in order to prevent impurities from being mixed into the raw materials and chemical solutions (contamination), it is also preferable to use a multilayer container whose inner wall has a six-layer structure made of six types of resin, or a multilayer container whose inner wall has a seven-layer structure made of seven types of resin. Examples of multilayer containers include those described in JP 2015-123351 A, the contents of which are incorporated herein by reference.

[0088] The liquid-contacting parts of the container that come into contact with the chemical solution (e.g., the container inner wall, the chemical solution inlet, and the chemical solution outlet) may be formed from either a non-metallic material or a metallic material, and from the viewpoint described below, it is preferable that they be formed from a non-metallic material or stainless steel.

[0089] The liquid-contacting portion of the container is preferably formed from a non-metallic material in terms of preventing contamination. The non-metallic material is not particularly limited, and known materials can be used. Examples include polyethylene resin, polypropylene resin, polyethylene-polypropylene resin, tetrafluoroethylene resin, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-hexafluoropropylene copolymer resin, tetrafluoroethylene-ethylene copolymer resin, trifluorochloroethylene-ethylene copolymer resin, vinylidene fluoride resin, trifluorochloroethylene copolymer resin, and vinyl fluoride resin. Among these, fluororesins are preferably used in terms of preventing contamination.

[0090] A specific example of a container whose liquid-contacting portion is made of a fluorine-based resin is a FluoroPure PFA composite drum manufactured by Entegris. Containers described on page 4 or the like of JP-A-3-502677, page 3 or the like of WO 2004 / 016526, and pages 9 and 16 or the like of WO 99 / 046309 can also be used. When a container whose liquid-contacting portion is made of a non-metallic material is used, it is preferable that the elution of organic components in the non-metallic material into the chemical solution is suppressed.

[0091] The liquid-contacting portion may be made of a metal material. The metal material is not particularly limited, but is preferably a metal material containing more than 25 mass% of chromium relative to the total mass of the metal material. Examples of such metal materials include stainless steel and nickel-chromium alloys, with stainless steel being preferred.

[0092] The stainless steel is not particularly limited, and known stainless steels can be used. Among them, an alloy containing 8% by mass or more of nickel is preferred, and an austenitic stainless steel containing 8% by mass or more of nickel is more preferred. Examples of austenitic stainless steel include SUS (Steel Use Stainless Steel) 304 (Ni content 8% by mass, Cr content 18% by mass), SUS304L (Ni content 9% by mass, Cr content 18% by mass), SUS316 (Ni content 10% by mass, Cr content 16% by mass), and SUS316L (Ni content 12% by mass, Cr content 16% by mass).

[0093] The nickel-chromium alloy is not particularly limited, and known nickel-chromium alloys can be used. Examples of nickel-chromium alloys include Hastelloy (trade name, the same applies hereinafter), Monel (trade name, the same applies hereinafter), and Inconel (trade name, the same applies hereinafter). More specific examples include Hastelloy C-276 (Ni content 63 mass%, Cr content 16 mass%), Hastelloy-C (Ni content 60 mass%, Cr content 17 mass%), and Hastelloy C-22 (Ni content 61 mass%, Cr content 22 mass%). Furthermore, the nickel-chromium alloy may further contain silicon, tungsten, molybdenum, copper, cobalt, etc., in addition to the above-mentioned alloys, as necessary.

[0094] The metal material is preferably electropolished, and more preferably electropolished stainless steel. As the electropolishing method, a known method can be used, for example, the methods described in

[0011] to

[0014] of JP 2015-227501 A and

[0036] to

[0042] of JP 2008-264929 A can be used.

[0095] The metal material may be buffed to prevent contamination. The buffing method is not particularly limited, and known methods can be used. The size of the abrasive grains used for buffing is not particularly limited, but #400 or smaller is preferred, as this tends to reduce the surface irregularities of the metal material. Buffing is preferably performed before electrolytic polishing. The metal material may also be processed by one or a combination of two or more of multiple buffing steps using different grit sizes of abrasive grains, acid cleaning, and magnetic fluid polishing.

[0096] The inside of the container is preferably washed before filling it with the chemical solution. The liquid used for washing is preferably the above-mentioned chemical solution or a diluted version of the above-mentioned chemical solution.

[0097] [Pattern Forming Method] The chemical solution of the present invention can be used, for example, in the following pattern forming method. The pattern forming method includes: Step 1 of forming a metal resist film on a substrate using an actinic ray- or radiation-sensitive composition (hereinafter also referred to as a "metal resist composition") containing a metal compound having at least one bond selected from the group consisting of a metal-carbon bond and a metal-oxygen bond (hereinafter also referred to as a "specific metal compound"); Step 2 of exposing the metal resist film to light; and Step 3 of developing the exposed metal resist film using a developer to remove unexposed areas, thereby obtaining a pattern. The pattern forming method may further include Step 4 of cleaning the pattern using a rinse solution after Step 3. Each step will be described in detail below.

[0098] [Step 1] Step 1 is a step of forming a metal resist film using a metal resist composition. Methods of forming a metal resist film using a metal resist composition include, for example, a method of applying the metal resist composition onto a substrate, and a method of vapor-depositing a metal resist component onto a substrate. The metal resist composition will be described later. Methods of applying the metal resist composition onto a substrate include, for example, a method of applying the metal resist composition onto a substrate (e.g., silicon) used in the manufacture of semiconductor devices such as integrated circuits, using an apparatus such as a spinner or coater. Spin coating using a spinner is preferred as the coating method. The rotation speed during spin coating is preferably 1000 to 3000 rpm.

[0099] A metal resist film may be formed by drying the substrate coated with the metal resist composition. Examples of drying methods include heating (prebaking). The heating may be performed using a means provided in a known exposure machine and / or a known developing machine, and a hot plate may also be used. The heating temperature is preferably 80 to 150°C, more preferably 80 to 140°C, and even more preferably 80 to 130°C. The heating time is preferably 30 to 1,000 seconds, more preferably 30 to 800 seconds, and even more preferably 40 to 600 seconds. Heating may be performed two or more times.

[0100] The thickness of the metal resist film is preferably 10 to 90 nm, more preferably 10 to 65 nm, and even more preferably 15 to 50 nm, in order to form a finer pattern with higher precision.

[0101] Furthermore, an undercoat film (e.g., an inorganic film, an organic film, an anti-reflective film, etc.) may be formed between the substrate and the metal resist film. The undercoat film can be formed using a known organic or inorganic material. Examples of compositions for forming undercoats include AL412 (manufactured by Brewer Science) and the SHB series (e.g., SHB-A940, etc., manufactured by Shin-Etsu Chemical Co., Ltd.). The thickness of the undercoat film is preferably 10 to 90 nm, more preferably 10 to 50 nm, and even more preferably 10 to 30 nm.

[0102] A top coat may be formed on the surface of the metal resist film opposite the substrate using a top coat composition. It is preferable that the top coat composition does not mix with the metal resist film and can be uniformly applied to the surface of the metal resist film opposite the substrate. The top coat composition preferably contains a resin, an additive, and a solvent. Examples of methods for forming the top coat include known top coat formation methods, and specific examples include the top coat formation methods described in

[0072] to

[0082] of JP 2014-059543 A.

[0103] <Metal Resist Composition> The metal resist composition contains a specific metal compound. The specific metal compound is a metal compound having at least one bond selected from the group consisting of a metal-carbon bond (MC) and a metal-oxygen bond (MO). M represents a metal atom. The metal-carbon bond refers to a state in which a metal atom and at least one carbon atom are bonded via a covalent bond, a coordinate bond, an ionic bond, a van der Waals bond, or the like. The covalent bond may be a single bond, a double bond, or a triple bond. The metal-oxygen bond refers to a state in which at least one metal atom and at least one oxygen atom in the specific metal compound are bonded via a covalent bond, a coordinate bond, an ionic bond, a van der Waals bond, or the like. The covalent bond may be a single bond or a double bond. When the specific metal compound has a metal-carbon bond, the specific metal compound is a so-called organometallic compound. The number of bonds selected from the group above that the specific metal compound has is preferably two or more, and more preferably three or more. The upper limit is preferably 10 or less, and more preferably 5 or less.

[0104] Examples of metal atoms constituting the specific metal compound include metal atoms of Groups 3 to 16 in the periodic table, and tin, antimony, tellurium, indium, hafnium, tartan, tungsten, bismuth, titanium, cobalt, nickel, zirconium, or palladium is preferred, with tin being more preferred. Note that in this specification, silicon atoms are included in the metal atoms.

[0105] The specific metal compound includes a compound represented by formula (1).

[0106]

[0107] In formula (1), M represents a metal atom. Examples of M include metal atoms constituting the specific metal compound, and are preferably tin, antimony, tellurium, indium, hafnium, tartan, tungsten, bismuth, titanium, cobalt, nickel, zirconium, or palladium, and more preferably tin.

[0108] In formula (1), R 1 represents an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. The alkyl group may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group is preferably 1 to 30, more preferably 1 to 16, and even more preferably 1 to 5. R 1 When the alkyl group represented by the formula (I) is an alkyl group having a substituent, the number of carbon atoms includes the number of carbon atoms of the substituent. Examples of the substituent that the alkyl group may have include a halogen atom, a hydroxyl group, a cyano group, a nitro group, an amino group, and an aromatic ring group. The aromatic ring group is preferably a phenyl group. The alkyl group having a phenyl group is preferably a benzyl group. The aliphatic unsaturated hydrocarbon group is an aliphatic hydrocarbon group having an unsaturated group therein. Examples of the unsaturated group include a double bond or a triple bond. The aliphatic unsaturated hydrocarbon group may be linear, branched, or cyclic. The number of carbon atoms of the aliphatic unsaturated hydrocarbon group is preferably 2 to 30, more preferably 2 to 16, and even more preferably 2 to 5. R 1When the aliphatic unsaturated hydrocarbon group represented by the formula (I) is a substituted aliphatic unsaturated hydrocarbon group, the number of carbon atoms included in the substituent is also included. The aliphatic unsaturated hydrocarbon group is preferably a vinyl group or an allyl group. Examples of the substituent that the aliphatic unsaturated hydrocarbon group may have include a halogen atom, a hydroxyl group, a cyano group, a nitro group, an amino group, and an aromatic ring group. The aryl group may be either a monocyclic or polycyclic ring. The number of carbon atoms in the aryl group is preferably 6 to 30, more preferably 6 to 12, and even more preferably 6 to 8. R 1 When the aryl group represented by the formula (I) is an aryl group having a substituent, the number of carbon atoms mentioned above includes the number of carbon atoms of the substituent. The aryl group is preferably a phenyl group or a naphthyl group. Examples of the substituent that the aryl group may have include an alkyl group, a halogen atom, a hydroxyl group, a cyano group, a nitro group, an amino group, and an aromatic ring group.

[0109] In formula (1), R 2 Is -OCOR r1 Or -OR r2 Represents R r1 represents a hydrogen atom, an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. r2 represents an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. 2 As an example, -OCOR r1 is preferred. r1 or R r2 The alkyl group which may have a substituent, the aliphatic unsaturated hydrocarbon group which may have a substituent, and the aryl group which may have a substituent, which are represented by the above R 1 Examples of the groups include those represented by the following formula:

[0110] In formula (1), n1+m1 represents the valence of the metal atom represented by M. n1+m1 is appropriately selected according to the possible valence of the metal atom represented by M. n1 is preferably an integer of 0 to 2, more preferably 1. m1 is preferably an integer of 0 to 4, more preferably 3. R 1 If there are multiple 1 R may be the same or different. 2 If there are multiple 2 They may be the same or different.

[0111] The specific metal compound also includes a compound represented by formula (2) and a condensate thereof.

[0112]

[0113] In formula (2), R 3 represents a hydrocarbon group which may have a substituent. Examples of the hydrocarbon group include an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, and an aryl group which may have a substituent. Preferred embodiments of the alkyl group, the aliphatic unsaturated hydrocarbon group, and the aryl group are those represented by R 1 The preferred embodiments are the same as those of each group represented by R 3 If there are multiple 3 They may be the same or different.

[0114] z and x represent numbers that satisfy the relationship of formula (2-1) and the relationship of formula (2-2).

[0115] The specific metal compound also includes a compound represented by formula (3).

[0116]

[0117] In formula (3), M represents a metal atom. Examples of M include the metal atoms represented by M in formula (1). R 4 and R 6 R each independently represents an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. 4and R 6 Examples of the R 1 Examples of the group include a group represented by R 5 and R 7 are each independently -OCOR r3 Or -OR r4 Represents R r3 represents a hydrogen atom, an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. r4 represents an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. r3 and R r4 For example, the above R r1 and the above R r2 Examples of the group include a group represented by R 5 and R 7 Examples of the R 2 Examples of the group include a group represented by R 4 If there are multiple 4 R may be the same or different. 5 If there are multiple 5 R may be the same or different. 6 If there are multiple 6 R may be the same or different. 7 If there are multiple 7 may be the same or different. L represents a single bond or a divalent linking group. Examples of the divalent linking group include an alkylene group and an arylene group. n2+m2 and n3+m3 each independently represent the valence of the metal atom represented by M minus 1.

[0118] The specific metal compound also includes a compound represented by formula (4), a hydrolyzate thereof, and a condensate of the hydrolyzate.

[0119]

[0120] In formula (4), R 8 represents a hydrocarbon group which may have a substituent. Examples of the hydrocarbon group include the above R1 X represents a hydrolyzable group. nz represents 1 or 2. Examples of X include groups represented by -NHR x1 , -NR x1 R x2 , -OSiR x1 R x2 R x3 , -N(SiR x1 3 ) (R x2 ), —N(SiR x1 3 ) (SiR x2 3 ), an azido group, —C≡CR x1 , -NH(COR x1 ), -NR x1 (COR x2 ), -NR x1 C (NR x2 ) R x3 (amidinate group) and imide group, and —NHR x1 or -NR x1 R x2 is preferred. x1 ~R x3 R each independently represents a hydrocarbon group having 1 to 10 carbon atoms. x1 ~R x3 As R, an alkyl group having 1 to 10 carbon atoms is preferred. 8 If there are multiple 8 When a plurality of X's are present, the X's may be the same or different.

[0121] The specific metal compound is preferably a compound represented by formula (5).

[0122]

[0123] In formula (5), R 9 represents an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. 10 Is -OCOR r5 Or -OR r6 Represents R r5represents a hydrogen atom, an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. r6 represents an alkyl group which may have a substituent, an aliphatic unsaturated hydrocarbon group which may have a substituent, or an aryl group which may have a substituent. 9 , R 10 , R r5 and R r6 are respectively represented by R in formula (1). 1 , R 2 , R r1 and R r2 The same definition and preferred embodiments are also applicable. 10 They may be the same or different.

[0124] The specific metal compound preferably includes at least one selected from the group consisting of a compound represented by formula (1), a compound represented by formula (2), and a condensate thereof, more preferably includes at least one selected from the group consisting of a compound represented by formula (5), a compound represented by formula (2), and a condensate thereof, and even more preferably includes at least one selected from the group consisting of a compound represented by formula (2) and a condensate thereof.

[0125] Examples of the specific metal compound include the specific metal compounds described in JP 2021-047426 A, JP 2021-179606 A, Japanese Patent No. 6805244, and WO 2019 / 111727.

[0126] The specific metal compound may be used alone or in combination of two or more. The content of the specific metal compound is preferably 50 to 100 mass %, more preferably 80 to 100 mass %, based on the total solid content of the metal resist composition.

[0127] <Organic Acid> The metal resist composition may contain an organic acid. Examples of the organic acid include carboxylic acids, sulfonic acids, sulfinic acids, organic phosphinic acids, organic phosphonic acids, phenols, enols, thiols, imidic acids, oximes, and sulfonamides, with carboxylic acids being preferred. Examples of carboxylic acids include monocarboxylic acids such as formic acid, propionic acid, butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, 2-ethylhexanoic acid, oleic acid, acrylic acid, methacrylic acid, trans-2,3-dimethylacrylic acid, stearic acid, linoleic acid, linolenic acid, arachidonic acid, salicylic acid, benzoic acid, p-aminobenzoic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, trifluoroacetic acid, pentafluoropropionic acid, gallic acid, and shikimic acid; dicarboxylic acids such as oxalic acid, malonic acid, maleic acid, methylmalonic acid, fumaric acid, adipic acid, sebacic acid, phthalic acid, and tartaric acid; and carboxylic acids having three or more carboxy groups such as citric acid. Examples of organic acids that may be contained in the metal resist composition also include organic acids that may be contained in the composition.

[0128] The organic acid may be used alone or in combination of two or more. The content of the organic acid is preferably 0 to 10 mass %, more preferably 1 to 5 mass %, based on the total solid content of the metal resist composition.

[0129] <Organic Solvent> The metal resist composition may contain an organic solvent. Examples of the organic solvent include ketone solvents, ester solvents, alcohol solvents, amide solvents, ether solvents, and hydrocarbon solvents.

[0130] Examples of ketone solvents include 1-octanone, 2-octanone, 1-nonanone, 2-nonanone, acetone, 2-heptanone, 4-heptanone, 1-hexanone, 2-hexanone, diisobutyl ketone, cyclohexanone, methylcyclohexanone, phenylacetone, methyl ethyl ketone, methyl isobutyl ketone, acetylacetone, acetonylacetone, ionone, diacetonyl alcohol, acetylcarbinol, acetophenone, methyl naphthyl ketone, isophorone, and propylene carbonate, with cyclohexanone, 2-heptanone, or diisobutyl ketone being preferred.

[0131] Examples of ester solvents include methyl acetate, butyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, pentyl acetate, isopentyl acetate, hexyl acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl-3-ethoxypropionate, 3-methoxybutyl acetate, 1-methoxy-2-propyl acetate, 3-methyl-3-methoxybutyl acetate, methyl formate, ethyl formate, butyl formate, propyl formate, ethyl lactate, butyl lactate, propyl lactate, butyl butanoate, 2-hydroxyisobutyrate methyl, isoamyl butyrate, isobutyl isobutyrate, ethyl propionate, propyl propionate, butyl propionate, and isobutyl propionate, and propyl acetate, butyl acetate, hexyl acetate, ethyl lactate, isoamyl butyrate, ethyl propionate, propyl propionate, butyl propionate, or isobutyl propionate is preferred.

[0132] Examples of alcohol-based solvents include methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, sec-butyl alcohol, tert-butyl alcohol, isobutyl alcohol, n-hexyl alcohol, 4-methyl-2-pentanol, n-heptyl alcohol, n-octyl alcohol, n-decanol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monoethyl ether, diethylene glycol monomethyl ether, triethylene glycol monoethyl ether, and methoxymethylbutanol.

[0133] Examples of amide solvents include N,N-dimethylformamide, 1-methyl-2-pyrrolidone, 2-pyrrolidinone, 1,3-dimethyl-2-imidazolidinone, 2-pyrrolidinone, ε-caprolactam, formamide, N-methylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropanamide, and hexamethylphosphoric triamide.

[0134] Examples of ether solvents include dioxane, tetrahydrofuran, anisole, and diisobutyl ether, with diisobutyl ether being preferred.

[0135] Examples of hydrocarbon solvents include saturated aliphatic hydrocarbon solvents such as pentane, hexane, octane, nonane, decane, undecane, dodecane, hexadecane, 2,2,4-trimethylpentane, and 2,2,3-trimethylhexane, and aromatic hydrocarbon solvents such as mesitylene, cumene, pseudocumene, 1,2,4,5-tetramethylbenzene, p-cymene, toluene, xylene, ethylbenzene, propylbenzene, 1-methylpropylbenzene, 2-methylpropylbenzene, dimethylbenzene, diethylbenzene, ethylmethylbenzene, trimethylbenzene, ethyldimethylbenzene, and dipropylbenzene. Saturated aliphatic hydrocarbon solvents are preferred, and octane, nonane, decane, undecane, or dodecane is more preferred.

[0136] <Other Additives> The metal resist composition may contain other additives such as surfactants, water, dissolution-inhibiting compounds, dyes, plasticizers, photosensitizers, light absorbers, and compounds that promote solubility in a developer (for example, phenolic compounds having a molecular weight of 1,000 or less, and alicyclic or aliphatic compounds containing a carboxylic acid group).

[0137] The surfactant is preferably a fluorine-based surfactant or a silicon-based surfactant, and for example, the surfactants described in paragraphs

[0218] and

[0219] of WO 2018 / 193954 can be used.

[0138] [Step 2] Step 2 is a step of exposing the metal resist film. The exposure may be performed as a full-surface exposure or a patterned exposure. Step 2 is preferably a step of performing patterned exposure through a photomask. Examples of the photomask include known photomasks. The photomask may be in contact with the metal resist film. Examples of exposure light for exposing the metal resist film include infrared light, visible light, ultraviolet light, far ultraviolet light, extreme ultraviolet light (EUV), X-rays, and electron beams. The wavelength of the exposure light is preferably 250 nm or less, more preferably 220 nm or less, and even more preferably 1 to 200 nm. Specifically, KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), F2 An excimer laser (wavelength 157 nm), X-rays, EUV (wavelength 13 nm), or an electron beam is preferred, a KrF excimer laser, an ArF excimer laser, EUV, or an electron beam is more preferred, and EUV or an electron beam is even more preferred. The exposure dose is not particularly limited as long as it is an amount that reduces the solubility of the exposed metal resist film in a developer containing an organic solvent. The exposure method may be immersion exposure. Step 2 may be performed once or twice or more times.

[0139] [Step 3] Step 3 is a step of developing the exposed metal resist film using a developer, which removes the unexposed portions of the exposed metal resist film to form a pattern.

[0140] As the development method, known development methods can be used. Specific examples include a method in which the exposed metal resist film is immersed in a tank filled with a developer for a certain period of time (dip method), a method in which the developer is piled up on the surface of the exposed metal resist film by surface tension and left stationary for a certain period of time (puddle method), a method in which the developer is sprayed onto the surface of the exposed metal resist film (spray method), and a method in which the developer is continuously dispensed onto a substrate having an exposed metal resist film rotating at a constant speed while scanning a nozzle that dispenses the developer at a constant speed (dynamic dispense method). After the development step, a step of stopping the development using a solvent other than the developer may be carried out. The development time is preferably 10 to 300 seconds, more preferably 20 to 120 seconds. The temperature of the developer during development is preferably 0 to 50°C, more preferably 15 to 35°C.

[0141] <Developer> The chemical solution of the present invention can be used as the developer in step 3. When the pattern formation method does not include step 4 described below, or when it includes step 4 described below and the rinse liquid in step 4 is a chemical solution other than the chemical solution, the developer in step 3 is preferably the chemical solution of the present invention described above. When the pattern formation method includes step 4 described below and the rinse liquid in step 4 is the chemical solution of the present invention described above, the developer in step 3 may be either the chemical solution of the present invention described above or a chemical solution other than the chemical solution of the present invention.

[0142] The other chemical liquid is a chemical liquid different from the chemical liquid of the present invention described above, and known developers and rinses can be used. The other chemical liquid contains an organic solvent. Examples of organic solvents contained in the other chemical liquid include ketone-based solvents, ester-based solvents, alcohol-based solvents, amide-based solvents, ether-based solvents, and hydrocarbon-based solvents. Specific examples include organic solvents that may be contained in metal resists. The other chemical liquid may contain one organic solvent alone or two or more organic solvents in combination. The other chemical liquid may contain organic solvents other than those described above, water, surfactants, etc.

[0143] [Step 4] Step 4 is a step of cleaning the pattern obtained in step 3 (development step) with a rinse liquid.

[0144] Examples of the rinsing method include the same methods as the developing method in step 3 (e.g., dipping, puddling, spraying, and dynamic dispensing). The processing time is preferably 10 to 300 seconds, more preferably 10 to 120 seconds. The temperature of the rinsing liquid is preferably 0 to 50°C, more preferably 15 to 35°C.

[0145] <Rinse liquid> When the developer in step 3 is the other chemical liquid, the rinse liquid in step 4 is preferably the chemical liquid of the present invention described above. When the developer in step 3 is the chemical liquid of the present invention described above, the rinse liquid in step 4 may be either the chemical liquid of the present invention described above or the other chemical liquid. The other chemical liquid that may be used as the rinse liquid has the same meaning as the other chemical liquid that may be used in the developer described above, and preferred embodiments are also the same.

[0146] [Other Steps] The pattern formation method may further include other steps in addition to the above steps 1 to 4. Examples of the other steps include a post-exposure bake step, a post-bake step, an etching step, and a purification step.

[0147] <Post-Exposure Bake Step> The pattern formation method preferably includes a post-exposure bake (PEB) step after performing step 2 (exposure step) and before performing step 3 (development step). The heating temperature for the post-exposure bake is preferably 80 to 200°C, more preferably 80 to 180°C, and even more preferably 80 to 150°C. The heating time is preferably 10 to 1,000 seconds, more preferably 10 to 180 seconds, and even more preferably 30 to 120 seconds. The post-exposure bake may be performed using a means provided in a known exposure machine and / or developer, or a hot plate. The post-exposure bake may be performed once or twice or more times.

[0148] <Post-baking step> The pattern formation method preferably includes a step of heating the pattern (post-baking step) after step 4 (rinsing step). The post-baking (PB) step can remove the developer and rinse solution remaining between and inside the pattern, and can also improve the surface roughness of the pattern. The heating temperature in the post-baking step is preferably 40 to 250°C, more preferably 80 to 200°C. The heating time in the post-baking step is preferably 10 to 180 seconds, more preferably 30 to 120 seconds.

[0149] <Etching Step> The pattern formation method may include an etching step of etching a substrate using the formed pattern as a mask. Examples of the etching method include known etching methods. Specific examples include the methods described in "Chapter 4: Etching" of "Semiconductor Processing Textbook, 4th Edition, Published in 2007, Publisher: SEMI Japan" in Proceedings of the International Society of Optical Engineering (Proc. of SPIE) Vol. 6924, 692420 (2008) and JP 2009-267112 A.

[0150] <Purification Step> The pattern formation method may include a purification step of purifying the metal resist composition, developer, rinse, and / or other various components (e.g., a composition for forming an undercoat film, a composition for forming a top coat, etc.) used in the pattern formation method. Examples of the purification method include known purification methods, and filtering or a method using an adsorbent is preferred.

[0151] [Method for manufacturing an electronic device] A method for manufacturing an electronic device includes a step of using the chemical solution of the present invention described above. A preferred embodiment of the method for manufacturing an electronic device includes a step of forming a pattern using the chemical solution of the present invention according to the pattern formation method described above. The electronic device is suitably mounted in electrical and electronic equipment (e.g., home appliances, OA (Office Automation), media-related equipment, optical equipment, and communication equipment).

[0152] The present invention will be described in more detail below with reference to the following examples. The materials, amounts used, ratios, treatment details, and treatment procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the following examples.

[0153] [Preparation of Raw Materials] 2-heptanone, carbonyl compounds, and cycloalkane compounds were synthesized and / or purified according to the following procedures.

[0154] [Synthesis and Purification of 2-Heptanone] 2-Heptanone was synthesized by applying a known hydration reaction of alkyne. Specifically, the following amounts of 1-heptyne, water, sulfuric acid, and mercury sulfate were mixed, and the resulting mixture was stirred to carry out the hydration reaction of 1-heptyne (addition of water). 1-Hepten-2-ol produced by this hydration reaction underwent keto-enol tautomerization, yielding a purified product containing 2-heptanone. 1-Heptyne (manufactured by Tokyo Chemical Industry Co., Ltd.): 100 parts by mass (g) Water (ultrapure water): 30 parts by mass (g) Sulfuric acid (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.): 10 parts by mass (g) Mercury sulfate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.): 10 parts by mass (g)

[0155] The obtained purified product was dehydrated by a column method using molecular sieve 3A (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). Next, the dehydrated purified product was distilled using a distillation column consisting of a first tray distillation column (theoretical plate number: 150 plates) without a pressure reduction mechanism and a second tray distillation column (theoretical plate number: 150 plates) equipped with a pressure reduction mechanism, connected in series, starting from the first tray distillation column. Furthermore, the distillation-purified purified product was subjected to circulation filtration purification using a filtration device equipped with a flow path in which the following ion exchange resins and filters were connected in series from upstream to downstream, and a return path for returning the purified product from the most downstream to the most upstream of the flow path. The circulation number was 50. Below, the details of each component of the filtration device are shown in order from the upstream side. Anion exchange resin (anion exchange resin described in Production Example 1 in paragraph 0028 of JP-A No. 2009-155208) Ion exchange filter (IonKleen SL, manufactured by Pall Corporation) Nylon filter (Asymmetric, manufactured by Pall Corporation, pore size 5 nm) UPE filter (Purasol SP / SN solvent purifier, manufactured by Entegris) PTFE filter (XpressKLEEN, manufactured by Pall Corporation, pore size 3 nm) UPE filter (Microgard, manufactured by Entegris, pore size 3 nm) In this type of circulation filtration purification, the operation of passing the product to be purified from the most upstream purification element to the most downstream purification element is counted as one circulation cycle.

[0156] [Purification of carbonyl compounds and cycloalkane compounds] The following compounds were prepared as carbonyl compounds and cycloalkane compounds. All of the following compounds were classified as semiconductor grade or equivalent high purity grade. (Carbonyl compounds (ketones)) 4-heptanone (C 7 H 14 O) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 5-methyl-2-hexanone (C 7 H 14 O) (Tokyo Chemical Industry Co., Ltd.) 5-methyl-3-hexanone (C 7 H 14 O) (Tokyo Chemical Industry Co., Ltd.) 3-heptanone (C 7 H 14 O) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Cyclopentanone (C 5 H 8 O) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 2-pentanone (C 5 H 10 O) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 3-pentanone (C 5 H 10 O) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (carbonyl compound (aldehyde)) 2-methylhexanal (C 7 H 14 O) (manufactured by BOC Science) 2-ethyl-3-methylbutanal (C 7 H 14 O) (Sigma-Aldrich) 2-ethylhexanal (C 8 H 16 O) (Tokyo Chemical Industry Co., Ltd.) 1-pentanal (C 5 H 10 O) (manufactured by Tokyo Chemical Industry Co., Ltd.) (Cycloalkane compounds) 1-methyl-4-isopropylcyclohexane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 1-methyl-2-isopropylcyclohexane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 1-methyl-3-isopropylcyclohexane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0157] Each of the above compounds was subjected to circulating filtration and purification using a filtration device equipped with a flow path formed by connecting the following filters in series in order from upstream to downstream, and a return path for returning the purified product from the most downstream to the most upstream of the flow path. The number of circulations was 50. Details of each component of the filtration device are shown below, starting from the upstream side: - Ion exchange filter (IonKleen SL, manufactured by Pall Corporation) - Nylon filter (Asymmetric, manufactured by Pall Corporation, pore size 5 nm) - UPE filter (Purasol SP / SN solvent purifier, manufactured by Entegris Corporation) - PTFE filter (XpressKLEEN, manufactured by Pall Corporation, pore size 3 nm) - UPE filter (Microgard, manufactured by Entegris Corporation, pore size 3 nm) Each of the compounds subjected to the above circulating filtration and purification was further purified by distillation using the same method as the distillation purification of 2-heptanone.

[0158] As a result, 2-heptanone, a carbonyl compound, and a cycloalkane compound were obtained in which the water content was reduced to below the detection limit and the Mn atom and Fe atom contents were each 0.0001 ppt by mass or less. Furthermore, the total content of the specific carbonyl compounds and the total content of the specific cycloalkane compounds in the obtained 2-heptanone were all below the detection limit. Furthermore, in the obtained 2-heptanone, carbonyl compound, and cycloalkane compound, the contents of organic compounds other than 2-heptanone, the specific carbonyl compound, and the cycloalkane compound, and the contents of inorganic acids such as sulfuric acid were all below the detection limit.

[0159] The water content was measured using the above-mentioned Karl Fischer moisture meter (product name "MKC-710M", manufactured by Kyoto Electronics Manufacturing Co., Ltd., Karl Fischer coulometric titration type). The water detection limit of the above-mentioned device was 1 ppm by mass. The Mn atom and Fe atom contents were measured using the above-mentioned ICP-MS (device used: Agilent 8900 triple quadrupole ICP-MS). With the above-mentioned device, the detection limit for the Mn atom content was 0.02 ppt by mass (unconcentrated), and the detection limit for the Fe atom content was 0.24 ppt by mass (unconcentrated). The carbonyl compound content and the cycloalkane compound content were measured using an apparatus formed by combining the above-mentioned gas chromatograph device "7890B" (manufactured by Agilent) and a mass spectrometer "JMS-Q1500" (manufactured by JEOL Ltd.). The detection limit for the content of carbonyl compounds using the above device was 0.1 ppm by mass, the detection limit for the content of cycloalkane compounds was 1 ppb by mass, and the detection limit for the content of other organic compounds was 0.1 ppm by mass. The content of inorganic acids such as sulfuric acid was measured using a gas chromatograph device (product name "GCMS-2020", manufactured by Shimadzu Corporation). The detection limit for inorganic acids using the above device was 0.001 ppm by mass.

[0160] The Mn atom content and the Fe atom content in 2-heptanone, the carbonyl compound, and the cycloalkane compound were measured using the above-mentioned device after concentration in the same manner as the measurement method for the chemical solution described below, and it was confirmed that the Mn atom content was 0.0001 ppt by mass or less, and the Fe atom content was 0.0001 ppt by mass or less. Furthermore, the 2-heptanone, the carbonyl compound, and the cycloalkane compound obtained above were concentrated in the same manner as the measurement method for the chemical solution described below, and the contents of transition elements measurable by ICP-MS other than Mn atoms and Fe atoms, measured using the above-mentioned device, were all less than 0.0001 ppt by mass.

[0161] [Preparation of Chemical Solutions] The carbonyl compound obtained by the above-mentioned method, ultrapure water, a Mn atom source, an Fe atom source, and a cycloalkane compound obtained by the above-mentioned method, which was added according to the composition, were added all at once or in portions to 2-heptanone obtained by the above-mentioned method so as to obtain the compositions shown in the tables below, to prepare chemical solutions for each Example and Comparative Example. Note that it was confirmed that the content of Mn atoms, the content of Fe atoms, and the total content of transition metal atoms other than Mn atoms and Fe in the ultrapure water used to prepare the chemical solutions were the same as those in the above-mentioned 2-heptanone, etc.

[0162] The Mn atom source was added by adding powdered Mn nanoparticles (S series, manufactured by Forward Science Laboratories) adjusted to a predetermined concentration to the chemical solution, while the Fe atom source was added by adding an aqueous solution of Fe nanoparticles (Sigma-Aldrich, particle size 10 nm) adjusted to a predetermined concentration to the chemical solution.

[0163] The content of Mn atoms in the chemical solution was quantified according to the following procedure. First, the chemical solution for which the content of Mn atoms was to be quantified was heated under reflux conditions at 160 to 180°C, and the organic solvent and water contained in the chemical solution were removed, thereby concentrating the non-volatile components contained in the chemical solution. The content of Mn atoms contained in the resulting concentrated solution was quantified using the above-mentioned device. When the Mn atom content in the chemical solution was calculated for chemical solutions in which the concentration ratio was changed from 10 to 1000 times in the above concentration, a positive correlation was found between the concentration ratio and the value of the Mn atom content, and a coefficient of determination (R 2 ) was more than 0.98. That is, by concentrating the chemical solution using the above method, it was possible to quantify the content of Mn atoms contained in the chemical solution. The content of Fe atoms in the chemical solution and the content of transition elements other than Mn atoms and Fe atoms that can be measured by ICP-MS were also quantified using the above procedure.

[0164] [Preparation of Metal Resist Composition] Monobutyltin oxide hydrate (BuSnOOH) powder (0.209 g, TCI America) was added to 4-methyl-2-pentanol (10 mL) to prepare a metal resist precursor solution. The solution was placed in a closed vial and stirred for 24 hours. The resulting mixture was centrifuged at 4000 rpm for 15 minutes and filtered using a 0.45 μm PTFE syringe filter to remove insoluble materials, yielding a metal resist composition. Note that the organic solvent in the metal resist composition was removed, and the SnO 2 The Sn content determined from the residual mass was 0.093 M. Dynamic light scattering (DLS) analysis of the metal resist precursor solution using a Moebius instrument (Wyatt Technology) revealed a unimodal distribution of particles with an average particle size of 2 nm, consistent with the diameter reported for the dodecamer butyltin hydroxide oxide polyatomic cation (Eychenne-Baron et al., Organometallics, 19, 1940-1949 (2000)).

[0165] [Evaluation] [Suppression of moisture-induced defects] The chemical solutions of each Example and Comparative Example were used as metal resist cleaning solutions (resist removers). The metal resist composition (2.5 mL) prepared above was applied to a 12-inch diameter silicon wafer, and a Sn resist film was formed by spin coating. Next, the chemical solution (10 mL) of each Example and Comparative Example was applied to the Sn resist film, and the silicon wafer was spun at 1500 rpm for 45 seconds until dry. This cleaning operation was repeated 10 times, and then a surface defect inspection device (KLA, SurfScan SP7) was used to irradiate the surface of the silicon wafer with laser light and measure the scattered light to obtain coordinate information of the defect positions on the silicon wafer. The shape of each measured defect was then evaluated using a defect review device (Applied Materials, SEM Vision G7E). From the defect images obtained by the defect review device, stain-like defects and foreign matter-like defects were each distinguished based on the mode of the device. Defects in a form in which the wafer surface was flat and free of irregularities and foreign matter, and only the contrast differed, were distinguished as stain (stain)-like defects, and defects in the form of foreign matter adhering to the wafer were distinguished as foreign matter-like defects. The number of stain-like defects and foreign matter-like defects on the silicon wafer was counted, and the suppression of stain-like defects and foreign matter-like defects was evaluated from the obtained number of defects according to the following evaluation criteria. The fewer the number of each defect, the better.

[0166] <Stain defect evaluation criteria> A: The number of stain defects is 5 or less. B: The number of stain defects is more than 5 and 10 or less. C: The number of stain defects is more than 10 and 50 or less. D: The number of stain defects is more than 50.

[0167] <Foreign matter defect evaluation criteria> A: The number of foreign matter defects is 5 or less. B: The number of foreign matter defects is more than 5 and 10 or less. C: The number of foreign matter defects is more than 10 and 50 or less. D: The number of foreign matter defects is more than 50.

[0168] [Intra-surface cleanliness uniformity] As in the above-mentioned [Suppression of moisture-induced defects], a metal resist composition (2.5 mL) was applied to a silicon wafer having a diameter of 12 inches, and a Sn resist film was formed by spin coating. Next, a chemical solution (10 mL) of each example and comparative example was applied to the Sn resist film, and the silicon wafer was rotated at 1500 rpm for 45 seconds until it dried. This cleaning operation was repeated 10 times. Next, the amount of residual Sn (atoms / cm) at 20 randomly selected points on the silicon wafer surface was measured using a vapor phase decomposition-inductively coupled plasma-mass spectrometer (VPD-ICP-MS, manufactured by Chem Trace). 2 ) was measured. The standard deviation σ of the amount of remaining Sn was calculated from the measured values ​​of the amount of remaining Sn at the above 20 locations. The calculated standard deviation σ was tripled to obtain a 3σ value, from which the in-plane uniformity of cleanliness after cleaning the metal resist with the chemical solution was evaluated according to the following evaluation criteria. The smaller the respective 3σ values, the smaller the variation in cleanliness of the silicon wafer surface after cleaning (removing) the metal resist, and therefore, the more preferable.

[0169] <Cleaning degree in-plane uniformity evaluation criteria> A: 3σ is 1×10 9 atom / cm 2 B: 3σ is less than 1 × 10 9 atom / cm 2 That's it, 2.5 x 10 9 atom / cm 2 C: 3σ is less than 2.5 × 10 9 atom / cm 2 That's it, 5 x 10 9 atom / cm 2 D: 3σ is less than 5 × 10 9 atom / cm 2 That's all.

[0170] [Wafer Bevel Cleaning] As in the above-mentioned [Suppression of Moisture-Induced Defects], a metal resist composition (2.5 mL) was applied to a silicon wafer having a diameter of 12 inches, and a Sn resist film was formed by spin coating. Next, a chemical solution (10 mL) of each Example and Comparative Example was applied to the Sn resist film, and the silicon wafer was rotated at 1500 rpm for 45 seconds until it dried. This cleaning operation was repeated 10 times. Next, the amount of residual Sn (atoms / cm) on the surface of the bevel of the silicon wafer was measured using a vapor phase decomposition-inductively coupled plasma-mass spectrometer (VPD-ICP-MS, manufactured by Chem Trace). 2 ) was measured. The amount of residual Sn was determined by measuring the amount of Sn at 20 points randomly selected from the surface of the bevel portion and calculating the arithmetic mean value of the obtained measurements. From the measured amount of residual Sn on the bevel portion, the cleanability of the wafer bevel with the chemical solution was evaluated according to the following evaluation criteria. The smaller the amount of residual Sn, the better the cleanability (removability) of the metal resist on the bevel portion of the silicon wafer, and therefore, is preferable.

[0171] <Evaluation Criteria for Wafer Bevel Cleanability> S: Remaining Sn amount is 1×10 10 atom / cm 2 A: The remaining Sn content is 1×10 or less. 10 atom / cm 2 Super, 5×10 10 atom / cm 2 B: The remaining Sn content is 5 × 10 or less. 10 atom / cm 2 Super, 1×10 11 atom / cm 2 C: The remaining Sn content is 1×10 or less. 11 atom / cm 2 Super, 5×10 11 atom / cm 2 D: The remaining Sn amount is 5 × 10 or less. 11 atom / cm 2 Super.

[0172] [Organic Substance Residue After Baking] The chemical solution (10 mL) of each Example and Comparative Example was applied to a 12-inch diameter silicon wafer, and the silicon wafer was rotated at 1500 rpm for 45 seconds until dry. Next, the amount of organic substance remaining on the silicon wafer surface (unit: ng / wafer) was measured using a silicon wafer analysis-gas chromatography mass spectrometer (SWA-GC / MS "6890N / 5973B", manufactured by Agilent Technologies). In addition, the chemical solution (10 mL) of each Example and Comparative Example was applied to a separately prepared 12-inch diameter silicon wafer, and the silicon wafer was rotated at 1500 rpm for 45 seconds until dry. Next, the obtained silicon wafer was subjected to a bake treatment at 150°C for 1 minute. Thereafter, the amount of organic matter remaining on the baked silicon wafer surface (unit: ng / wafer) was measured using a silicon wafer analysis-gas chromatography mass spectrometer (SWA-GC / MS "6890N / 5973B"). The ratio of the amount of organic matter remaining on the baked silicon wafer surface to the amount of organic matter remaining on the silicon wafer surface that was not baked (organic matter remaining rate) was calculated. From the calculated organic matter remaining rate, the residue of organic matter derived from the chemical solution on the silicon wafer after baking was evaluated according to the following evaluation criteria. The smaller the organic matter remaining rate, the greater the amount of organic matter removed from the silicon wafer surface by the bake treatment, and therefore is preferable.

[0173] <Evaluation criteria for organic residue after baking> S: Organic residue rate is less than 20%. A: Organic residue rate is 20% or more and less than 40%. B: Organic residue rate is 40% or more and less than 60%. C: Organic residue rate is 60% or more.

[0174] [Organic Contamination Suppression After Wafer Cleaning] A 12-inch diameter silicon wafer was left for 1 hour in a clean room meeting U.S. Federal Standard [Fed. Std. 209D] Class 10 (equivalent to the above ISO Class 4), and then the amount of organic matter remaining on the silicon wafer surface (unit: ng / wafer) was measured using an SWA-GC / MS ("6890N / 5973B" manufactured by Agilent Technologies). Furthermore, in the above clean room, a separately prepared 12-inch diameter silicon wafer was coated with the chemical solution (10 mL) of each Example and Comparative Example, and the silicon wafer was spun at 1500 rpm for 45 seconds until dry. This cleaning operation was repeated 10 times, and then the amount of organic matter remaining on the silicon wafer surface (unit: ng / wafer) was measured using the above SWA-GC / MS. The reduction rate of the amount of remaining organic matter due to the cleaning treatment was calculated using the following formula from the amount of remaining organic matter (organic matter remaining amount 1) measured for a silicon wafer that had not been subjected to the cleaning treatment with the above chemical solution and the amount of remaining organic matter (organic matter remaining amount 2) measured for a silicon wafer that had been subjected to the cleaning treatment with the above chemical solution. Reduction rate of remaining organic matter=(organic matter remaining amount 1-organic matter remaining amount 2) / (organic matter remaining amount 1) From the calculated reduction rate of remaining organic matter, the organic contamination suppression ability after wafer cleaning with the chemical solution was evaluated according to the following evaluation criteria. A larger reduction rate is preferable because it means that there is less organic matter adhering to the silicon wafer surface after cleaning with the chemical solution.

[0175] <Evaluation criteria for organic contamination suppression> SS: Reduction rate of remaining organic matter is 20% or more. S: Reduction rate of remaining organic matter is 15% or more and less than 20%. A: Reduction rate of remaining organic matter is 10% or more and less than 15%. B: Reduction rate of remaining organic matter is 5% or more and less than 10%. C: Reduction rate of remaining organic matter is less than 5%.

[0176] [Suppression of defects caused by chemicals] A silicon wafer having a diameter of 12 inches was prepared, and a surface defect inspection device (KLA, SurfScan SP7) was used to irradiate laser light onto the surface of the silicon substrate and measure the scattered light, thereby measuring the position and size of defects on the silicon wafer. A coating and developing device (Tokyo Electron, CLEAN TRACK LITHIUS PRO Z) was used to apply the chemical solution (10 mL) of each example and comparative example to the surface of the silicon wafer. After spin drying at 2000 rpm for 30 seconds, the position and size of defects on the silicon wafer were measured using a surface defect inspection device (KLA, SurfScan SP7) using the method described above. Chemical-induced defects were extracted from the position, number, and size of the defects before and after application of the chemical solution, and the suppression of chemical-induced defects was evaluated according to the following evaluation criteria. The fewer the number of defects caused by the chemical solution, the better.

[0177] <Chemical defect evaluation criteria> S: The number of chemical defects of 20 nm or less is 3 or less. A: The number of chemical defects of 20 nm or less is more than 3 but not more than 10. B: The number of chemical defects of 20 nm or less is more than 10 but not more than 20. C: The number of chemical defects of 20 nm or less is more than 20.

[0178] [Results] The composition of the chemical solution in each example and comparative example, and the evaluation results are shown in Tables 1 to 8. In the tables, the "balance" in the "2-heptanone" column means that 2-heptanone constitutes the remainder other than the specific carbonyl compound, water, cycloalkane compound, Mn atom, and Fe atom described in the table. In each example, the content of 2-heptanone was 60 mass% or more relative to the total mass of the chemical solution. In the tables, "NONE" means that no compound corresponding to the column was detected. In the tables, the "aldehyde / ketone ratio" column indicates the content of the specific aldehyde relative to the content of the specific ketone in a chemical solution containing a specific ketone and a specific aldehyde as specific carbonyl compounds. Note that the "aldehyde / ketone ratio" column lists values ​​without exponential notation, for example, "1.0E-01" is equivalent to "1.0 x 10 -1In the table, "<1" in the "Water content [ppm]" column means that the water content in the chemical solution was below 1 mass ppm, which is the detection limit. In the table, the "P value" column shows the water concentration in each chemical solution as X mol / L, the specific carbonyl compound concentration as Y mol / L, and P = -log 10 The value P calculated from the formula (1) expressed as (X×Y) is shown.

[0179]

[0180]

[0181]

[0182]

[0183]

[0184]

[0185] From the results shown in the above table, it was confirmed that the chemical solutions of the present invention produced in Examples 1 to 112 have superior effects to those of Comparative Examples 1 and 5 in which the water content exceeds 10,000 ppt by mass, Comparative Examples 2, 3, 6, and 7 in which the P value is less than 3 or exceeds 10, Comparative Examples 4 and 8 in which the water content is less than 1 ppt by mass, and Comparative Examples 9 to 12 in which no specific carbonyl compound is contained.

[0186] Comparison of Examples 1 to 4 etc. confirmed that foreign matter defects could be further reduced and wafer bevel cleanability was better when the P value was 9 or less, that foreign matter defects could be further reduced when the P value was 8.5 or less, and that wafer bevel cleanability was even better when the P value was 8 or less. Comparison of Examples 4 to 7 etc. confirmed that stain-like defects could be further reduced when the P value was 3.5 or more, and that stain-like defects could be further reduced and in-plane cleanliness uniformity was better when the P value was 5 or more.

[0187] From the comparison of Examples 38 to 40, it was found that the ratio of the content of the specific aldehyde to the content of the specific ketone in the chemical solution was 1.0 × 102 The effect of the present invention is more excellent when the ratio is 1.0 × 10 1 It has been confirmed that the effects of the present invention are even more excellent when the following conditions are met:

[0188] A comparison of Example 11 with Examples 91 to 93, etc., confirmed that when the content of the specific cycloalkane compound relative to the total mass of the chemical solution is 0.3 ppm by mass or more, the effect of suppressing organic contamination after wafer cleaning is excellent, when it is 0.5 ppm by mass or more, the effect of suppressing organic contamination after wafer cleaning is even better, and when it is 1.0 ppm by mass or more, the effect of suppressing organic contamination after wafer cleaning is even better. Furthermore, a comparison of Example 11, Example 94, Example 95, etc. confirmed that when the content of the specific cycloalkane compound relative to the total mass of the chemical solution is 1000 ppm by mass or less, the effect of suppressing organic matter derived from the chemical solution on silicon wafers after baking is excellent, and when it is 700 ppm by mass or less, the effect of suppressing organic matter derived from the chemical solution on silicon wafers after baking is even better.

[0189] From a comparison of Examples 106 to 109, it was found that the ratio of the Mn atom content to the Fe atom content in the chemical solution (Mn / Fe ratio) was 1.0 × 10 -3 When the ratio is 1.0 × 10 or more, the effect of the present invention and the effect of suppressing defects caused by the chemical solution are more excellent, and -2 When the concentration is 5.0 × 10 or more, the effect of the present invention and the effect of suppressing defects caused by the chemical solution are even more excellent, and -2 Furthermore, from a comparison of Examples 110 to 112, it was confirmed that when the Mn / Fe ratio was 1.0 or less, the effect of the present invention and the effect of suppressing defects caused by the chemical solution were more excellent, and the Mn / Fe ratio was 7.0×10 -1 The effect of the present invention is even better when the ratio is 5.0 × 10 or less. -1 It was confirmed that the effect of suppressing defects caused by chemicals was even more excellent when the content was below the above range.

Claims

1. A chemical solution containing 2-heptanone, water, and a carbonyl compound having 6 to 8 carbon atoms other than 2-heptanone, wherein the content of the 2-heptanone is 60 mass% or more based on the total mass of the chemical solution, the content of the water is 1 to 1000 mass ppm based on the total mass of the chemical solution, and the P value calculated by the following formula (1) is 3 to 10. P=-log 10 (X×Y) Formula (1) X represents a numerical value X when the concentration of the water in the chemical solution is X mol / L, and Y represents a numerical value Y when the concentration of the carbonyl compound in the chemical solution is Y mol / L.

2. The chemical solution according to claim 1, wherein the water content is 1 to 100 ppm by mass based on the total mass of the chemical solution.

3. The chemical solution according to claim 1, wherein the content of the carbonyl compound is 0.1 to 1000 ppm by mass based on the total mass of the chemical solution.

4. The chemical solution according to claim 1, wherein the carbonyl compound comprises a ketone having 6 to 8 carbon atoms other than 2-heptanone.

5. The chemical solution according to claim 1, wherein the carbonyl compound contains two or more ketones having 6 to 8 carbon atoms other than 2-heptanone.

6. The chemical solution according to claim 1, wherein the carbonyl compound comprises at least one selected from the group consisting of 5-methyl-2-hexanone and 4-heptanone.

7. The carbonyl compound is represented by the chemical formula C 7 H 14 The chemical solution according to claim 1 , comprising a carbonyl compound represented by O.

8. The carbonyl compound contains a ketone having 6 to 8 carbon atoms other than 2-heptanone and an aldehyde having 6 to 8 carbon atoms, and the ratio of the content of the aldehyde to the content of the ketone is 1.0 x 10 -5 ~1.0 x 10 2 The drug solution according to claim 1 , 9. The chemical solution according to claim 4, further comprising a cycloalkane compound having a boiling point of 160°C or higher and 8 to 12 carbon atoms, the content of said cycloalkane compound being 0.1 to 1000 ppm by mass relative to the total mass of said chemical solution.

10. The chemical solution according to claim 9, wherein the cycloalkane compound comprises at least one selected from the group consisting of 1-methyl-2-isopropylcyclohexane, 1-methyl-3-isopropylcyclohexane, and 1-methyl-4-isopropylcyclohexane.

11. The chemical solution of claim 9, wherein the cycloalkane compound comprises 1-methyl-4-isopropylcyclohexane.

12. The chemical solution according to claim 1, further comprising Mn atoms, the content of said Mn atoms being 0.001 to 10 ppt by mass relative to the total mass of said chemical solution.

13. The alloy further contains Mn atoms and Fe atoms, and the ratio of the content of the Mn atoms to the content of the Fe atoms is 1.0×10 -3 The drug solution according to claim 1, wherein the pH is 1.0 to 1.

0.

14. The chemical solution according to claim 1, which is used as at least one selected from the group consisting of a cleaning solution, a developing solution, a pre-wetting solution, and a rinsing solution.

15. The chemical solution according to claim 1, which is used as at least one selected from the group consisting of a pre-wet solution, a rinsing solution, a cleaning solution, and a developing solution in a semiconductor substrate manufacturing process having a step of forming a metal resist film.

16. A liquid medicine container comprising a container and the liquid medicine according to any one of claims 1 to 15 contained in the container.

17. The drug solution container according to claim 16, wherein a liquid-contacting portion of the container that comes into contact with the drug solution is made of a nonmetallic material or stainless steel.

18. The drug solution container according to claim 16, wherein the non-metallic material is at least one selected from the group consisting of polyethylene resin, polypropylene resin, polyethylene-polypropylene resin, tetrafluoroethylene resin, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-hexafluoropropylene copolymer resin, tetrafluoroethylene-ethylene copolymer resin, trifluorochloroethylene-ethylene copolymer resin, vinylidene fluoride resin, trifluorochloroethylene copolymer resin, and vinyl fluoride resin.

Citation Information

Patent Citations

  • Method for forming insulating layer

    JP2018031805A