Thermoplastic liquid-crystal polymer film, and multilayer object and circuit board obtained using same
The thermoplastic liquid crystal polymer film with controlled thermal expansion and molecular orientation addresses the high dielectric loss and interlayer connectivity issues in conventional films, achieving improved reliability and processing stability for circuit boards.
Patent Information
- Application Number
- PCT/JP2024/017576
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional thermoplastic liquid crystal polymer films used in circuit boards face issues with high dielectric loss tangent and interlayer connectivity problems, such as warping and cracking, especially when laminated with metal layers and subjected to thermal environments during circuit processing.
A thermoplastic liquid crystal polymer film with a specific dielectric loss tangent and controlled thermal expansion coefficient is developed, featuring a structural unit composition and heat treatment process that ensures a low dielectric loss tangent and improved interlayer connectivity, achieved through precise control of thermal expansion and molecular orientation.
The solution effectively reduces dielectric loss tangent to 0.0015 or less at 5 GHz and limits thermal expansion change to 40 ppm/°C or less, preventing delamination and deformation during electronic component mounting, thereby enhancing circuit board processing and reliability.
Smart Images

Figure JP2024017576_21112024_PF_FP_ABST
Abstract
Description
Thermoplastic liquid crystal polymer film, and laminate and circuit board using the same Related Applications
[0001] This application claims priority from Japanese Patent Application No. 2023-080081, filed May 15, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a film containing a polymer capable of forming an optically anisotropic melt phase (hereinafter referred to as a thermoplastic liquid crystal polymer), a laminate using this film, and a circuit board using this film.
[0003] Films containing thermoplastic liquid crystal polymers (hereinafter sometimes referred to as "thermoplastic liquid crystal polymer films") have high heat resistance, low moisture absorption, and excellent strength, and are therefore used as insulating materials for flexible circuit boards. Circuit boards are manufactured by laminating a metal layer on an insulating layer, and then undergo various thermal processes in downstream processes such as circuit processing and electronic component mounting. Therefore, thermoplastic liquid crystal polymer films with thermal expansion coefficients adjusted to values close to those of metals have also been developed. In recent years, the use of gigahertz frequencies has become increasingly common in information processing devices, communication devices, and the like. Thermoplastic liquid crystal polymer films, with their low dielectric loss tangent and ability to suppress dielectric loss, have also attracted attention as high-frequency circuit board materials.
[0004] Conventionally, as a thermoplastic liquid crystal polymer film with an adjusted thermal expansion coefficient for use as a circuit board material, a wholly aromatic liquid crystal polyester film mainly composed of structural units (repeating units) derived from hydroxynaphthoic acid and hydroxybenzoic acid has been known, and efforts have been made to improve the dielectric properties of this film for use as a high-frequency circuit board material. For example, Non-Patent Document 1 discloses the dielectric properties, such as the dielectric loss tangent, of Vecstar (registered trademark) CT-Z, a thermoplastic liquid crystal polymer film manufactured by Kuraray Co., Ltd.
[0005] Development of electronic devices compatible with fifth-generation mobile communication systems (5G) is currently underway. Because 5G uses even higher frequency bands than conventional systems, circuit board materials are also required to have even lower dielectric loss tangents. Therefore, research is underway into thermoplastic liquid crystal polymer materials that can reduce dielectric loss tangents even further than the conventional thermoplastic liquid crystal polymer films primarily composed of structural units (repeating units) derived from hydroxynaphthoic acid and hydroxybenzoic acid. For example, Patent Document 1 discloses a thermoplastic liquid crystal polymer containing four types of repeating units: repeating unit (I) provided by a monomer exemplified by 6-hydroxy-2-naphthoic acid and its derivatives, repeating unit (II) provided by a monomer exemplified by 2,6-naphthalenedicarboxylic acid and its derivatives, and repeating units (IV) and (V) derived from different divalent aromatic diols. The publication describes that a thermoplastic liquid crystal polymer film using this polymer exhibits an even smaller dielectric loss tangent than a comparative thermoplastic liquid crystal polymer film composed of repeating units derived from 6-hydroxy-2-naphthoic acid and 4-hydroxybenzoic acid.
[0006] The 26th Japan Institute of Electronics Packaging Spring Conference SA-02
[0007] International Publication No. 2018 / 181222
[0008] Currently, various attempts have been made to reduce the dielectric loss tangent of thermoplastic liquid crystal polymer films by adjusting the composition, including Patent Document 1. However, thermoplastic liquid crystal polymer films with reduced dielectric loss tangent have problems with interlayer connectivity of circuits, such as warping when laminated with a metal layer such as copper foil, and cracking due to the thermal environment during circuit processing.
[0009] In view of the above circumstances, the present invention aims to provide a thermoplastic liquid crystal polymer film having a low dielectric tangent and excellent interlayer connection of a circuit. Another object of the present invention is to provide a laminate and a circuit board including the above thermoplastic liquid crystal polymer film. Another object of the present invention is to provide a method for producing the above thermoplastic liquid crystal polymer film.
[0010] As a result of intensive research to achieve the above-mentioned object, the inventors of the present invention discovered that a thermoplastic liquid crystal polymer film having a specific dielectric tangent and a specific range of change in thermal expansion coefficient before and after heating can solve the above-mentioned problems, and thus completed the present invention.
[0011] That is, the present invention can be configured in the following aspects. [Aspect 1] A film containing a thermoplastic polymer capable of forming an optically anisotropic molten phase (hereinafter referred to as a thermoplastic liquid crystal polymer), wherein the absolute value of the change in thermal expansion coefficient in the film thickness direction before and after heating the film at the melting point (Tm) of the thermoplastic liquid crystal polymer + 20°C for 60 seconds is 40 ppm / °C or less (preferably 20 ppm / °C or less, more preferably 10 ppm / °C or less), and the dielectric dissipation factor at 5 GHz is 0.0015 or less (preferably 0.0010 or less, more preferably 0.0008 or less). [Aspect 2] The thermoplastic liquid crystal polymer film according to Aspect 1, wherein the thermal expansion coefficient in the film thickness direction is 100 ppm / °C or more and 250 ppm / °C or less (preferably 230 ppm / °C or less, more preferably 210 ppm / °C or less).
[0012] [Aspect 3] The thermoplastic liquid crystal polymer film according to Aspect 1 or 2, wherein the amount of orientation component Z in the film thickness direction satisfies the following: 0.001≦Z≦0.250 [Aspect 4] The thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 3, wherein the amount of orientation component X in the MD of the film and the amount of orientation component Y in the TD of the film satisfy the following: 0.400≦X≦0.600 0.300≦Y≦0.500
[0013] [Embodiment 5] The thermoplastic liquid crystal polymer film according to any one of embodiments 1 to 4, wherein the structural unit represented by the following formula (1) is contained in an amount of 30 mol % to 90 mol % of all structural units constituting the thermoplastic liquid crystal polymer. [In the formula, a, b, c, and d are each independently 0 or 1. However, a+b=1 and c+d=1, and b and c cannot simultaneously be 0.] [Embodiment 6] The thermoplastic liquid crystal polymer film according to any one of embodiments 1 to 5, wherein, of all structural units constituting the thermoplastic liquid crystal polymer, the thermoplastic liquid crystal polymer contains 20 mol% to 90 mol% of structural units represented by formula (2), 0 mol% to 80 mol% of structural units represented by formula (3), 0.1 mol% to 40 mol% of structural units represented by formula (4), and 0.1 mol% to 40 mol% of structural units represented by formula (5). -CO-Ar1-O-(2) -CO-Ar2-O-(3) -CO-Ar3-CO-(4) -O-Ar4-O-(5) In formulas (2) to (5), Ar1 represents a naphthylene group, Ar2 represents a phenylene group, a biphenylene group, or a group represented by formula (6), Ar3 represents a phenylene group, a naphthylene group, a biphenylene group, or a group represented by formula (6), Ar4 represents a phenylene group, a naphthylene group, a biphenylene group, or a group represented by formula (6), -Ar5-Z-Ar6-(6) In formula (6), Ar5 and Ar6 each independently represent a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylidene group.
[0014] [Aspect 7] The thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 6, wherein the relative dielectric constant in the thickness direction of the film is 3.0 or less (preferably 2.9 or less, for example 2.4 to 2.9). [Aspect 8] A laminate comprising an insulating layer comprising the thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 7, and a metal layer. [Aspect 9] A circuit board comprising at least one selected from the group consisting of the thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 7 and the laminate according to Aspect 8. Aspect 10 is a method for producing a thermoplastic liquid crystal polymer film according to any one of Aspects 1 to 7, comprising the steps of: preparing a raw film by melt extrusion molding of a thermoplastic liquid crystal polymer; performing a first heat treatment on the raw film at a melting point (Tm) (the melting point of the thermoplastic liquid crystal polymer; the same applies hereinafter) of -20°C to a melting point (Tm) of -5°C (preferably a melting point (Tm) of -15°C to a melting point (Tm) of -7°C) for 10 seconds to 5 minutes (preferably 20 seconds to 3 minutes, more preferably 30 seconds to 2 minutes) while applying a pressure of 0.1 to 50 MPa (preferably 0.3 to 10 MPa, more preferably 0.5 to 5 MPa) to produce a precursor film; and performing a second heat treatment on the precursor film at a melting point (Tm) of -10°C to a melting point (Tm) of +30°C (preferably a melting point (Tm) of -8°C to a melting point (Tm) of +20°C) for 10 seconds to 10 minutes (preferably 20 seconds to 8 minutes, more preferably 30 seconds to 5 minutes). [Embodiment 11] The method for producing a thermoplastic liquid crystal polymer film according to embodiment 10, wherein the second heat treatment is carried out after pressing the precursor film onto a support.
[0015] It should be noted that any combination of at least two elements disclosed in the claims and / or the specification and / or the drawings is included in the present invention, and in particular any combination of two or more of the claims set forth in the claims is included in the present invention.
[0016] The thermoplastic liquid crystal polymer film of the present invention has a low dielectric loss tangent, and in laminates and circuit boards containing this thermoplastic liquid crystal polymer film, by appropriately controlling the thermal expansion coefficient in the thickness direction of the film, it is possible to suppress delamination and deformation even when heated during the circuit processing process or the mounting process of electronic components.
[0017] Fig. 1 is a schematic perspective view showing the relationship between the X-ray irradiation direction and the measurement target surface of an object according to one embodiment of the present invention. Fig. 2 is a schematic perspective view showing the relationship between MD and TD in an example of a thermoplastic liquid crystal polymer film and the X-ray irradiation direction and azimuthal angle direction. Fig. 3 is a schematic perspective view showing the relationship between MD and TD in an example of a thermoplastic liquid crystal polymer film and the X-ray irradiation direction and azimuthal angle direction. Fig. 4 is a schematic perspective view showing the relationship between MD and TD in an example of a thermoplastic liquid crystal polymer film and the X-ray irradiation direction and azimuthal angle direction. Fig. 5 is a schematic view for explaining a method of calculating each component of a reference vector.
[0018] The thermoplastic liquid crystal polymer film of the present invention is a thermoplastic liquid crystal polymer film in which the absolute value of the change in thermal expansion coefficient in the film thickness direction before and after heating the film at the melting point (Tm) of the thermoplastic liquid crystal polymer + 20°C for 60 seconds is 40 ppm / °C or less, and the dielectric loss tangent at 5 GHz is 0.0015 or less. Note that the thermal expansion coefficient will hereinafter also be referred to as "CTE".
[0019] Conventional thermoplastic liquid crystal polymer films have a dielectric loss tangent of about 0.002 and are commercially available. Thermoplastic liquid crystal polymer films with a dielectric loss tangent of less than 0.002, for example, thermoplastic liquid crystal polymer films having three or more different structural units (repeating units), are known. However, such conventional films have problems with circuit processability, such as warping when laminated with a metal layer such as copper foil, and cracking due to thermal load during circuit processing. In the present invention, by controlling the change in the thermal expansion coefficient in the thickness direction (hereinafter also referred to as the "Z direction") before and after the heat treatment under the above conditions, a thermoplastic liquid crystal polymer film that can be used in circuit processing and electronic component mounting processes can be obtained.
[0020] In the present invention, the thermoplastic liquid crystal polymer is melt-extruded, stretched and processed into a film, and then subjected to a distortion control treatment at a predetermined temperature lower than the melting point Tm of the raw film. Then, heat treatment is performed again at a predetermined temperature close to the melting point Tm, thereby suppressing the change in the thermal expansion coefficient in the thickness direction during subsequent heat treatments.
[0021] [Thermoplastic liquid crystal polymer] The thermoplastic liquid crystal polymer film contains a thermoplastic liquid crystal polymer. The thermoplastic liquid crystal polymer is composed of a melt-moldable liquid crystal polymer (or a polymer that can form an optically anisotropic melt phase), and its chemical structure is not particularly limited as long as it is a melt-moldable liquid crystal polymer, but examples thereof include thermoplastic liquid crystal polyesters and thermoplastic liquid crystal polyester amides in which amide bonds are introduced therein.
[0022] The thermoplastic liquid crystal polymer may also be a polymer in which an isocyanate-derived bond such as an imide bond, a carbonate bond, a carbodiimide bond or an isocyanurate bond is further introduced into an aromatic polyester or an aromatic polyester amide.
[0023] Specific examples of the thermoplastic liquid crystal polymer used in the present invention include known thermoplastic liquid crystal polyesters and thermoplastic liquid crystal polyester amides derived from the compounds classified as (1) to (4) shown below and their derivatives. However, it goes without saying that there is an appropriate range for the combination of various raw material compounds in order to form a polymer that can form an optically anisotropic molten phase.
[0024] (1) Aromatic or aliphatic diol (see Table 1 for representative examples)
[0025] (2) Aromatic or aliphatic dicarboxylic acids (see Table 2 for representative examples)
[0026] (3) Aromatic hydroxycarboxylic acids (see Table 3 for representative examples)
[0027] (4) Aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids (see Table 4 for representative examples)
[0028] Representative examples of thermoplastic liquid crystal polymers obtained from these raw material compounds include copolymers having the repeating units shown in Tables 5 and 6.
[0029]
[0030] In the present invention, the thermoplastic liquid crystal polymer preferably contains at least a structural unit represented by the following formula (1) in a predetermined range.
[0031]
[0032] (In the formula, a, b, c, and d are each independently 0 or 1, provided that a+b=1 and c+d=1, and b and c cannot be 0 at the same time.)
[0033] Specific examples of the structural unit represented by formula (1) include a structural unit derived from 6-hydroxy-2-naphthoic acid (including 2-hydroxy-6-naphthoic acid) and a structural unit derived from 2,6-naphthalenedicarboxylic acid. These structural units may be used alone or in combination of two or more.
[0034] The structural unit represented by formula (1) is preferably contained in an amount of 30 to 90 mol% of all structural units constituting the thermoplastic liquid crystal polymer, from the viewpoint of suppressing the rotational motion of the carbonyl group in the polymer. By containing the structural unit represented by formula (1) in this range, it is possible to control the proportion of permanent dipoles in the liquid crystal polymer in which carbonyl groups are bonded to the naphthalene skeleton, and it is possible to suppress an increase in the dielectric loss tangent due to vibration of the permanent dipole. The structural unit represented by formula (1) may be contained in an amount of preferably about 40 to 90 mol%, more preferably about 45 to 85 mol%, of all structural units constituting the thermoplastic liquid crystal polymer.
[0035] Furthermore, the thermoplastic liquid crystal polymer may preferably contain, for example, 30 to 100 mol %, more preferably 40 to 100 mol %, and even more preferably 50 to 100 mol % of structural units derived from 6-hydroxy-2-naphthoic acid in the structural units of formula (1).
[0036] A preferred thermoplastic liquid crystal polymer may contain, in addition to the structural unit represented by formula (1), a structural unit represented by the following formula (7) within a predetermined range.
[0037]
[0038] (In the formula, e, f, g, and h are each independently 0 or 1, provided that e+f=1 and g+h=1, and that f and g cannot be 0 at the same time.)
[0039] Specific examples of the structural unit represented by formula (7) include a structural unit derived from p-hydroxybenzoic acid, a structural unit derived from terephthalic acid, and a structural unit derived from isophthalic acid. These structural units may be used alone or in combination of two or more. Of these, the structural unit derived from p-hydroxybenzoic acid and the structural unit derived from terephthalic acid are preferred.
[0040] The structural unit represented by formula (7) may be contained in a molar ratio of, for example, the structural unit of formula (1) / the structural unit of formula (7)=99 / 1 to 30 / 70, preferably 99 / 1 to 50 / 50, from the viewpoint of suppressing an increase in the dielectric loss tangent due to a carbonyl group bonded to a benzene ring.
[0041] In the present invention, the above-mentioned thermoplastic liquid crystal polymer film may be a liquid crystal polymer film containing two different structural units (repeating units), as long as it can obtain a low dielectric tangent and suppress the temperature change of the thermal expansion coefficient, but it may also be a thermoplastic liquid crystal polymer film containing three or more different structural units (repeating units).
[0042] For example, a liquid crystal polymer that can be suitably used in the present invention may contain, among all structural units (repeating units), 20 mol % to 90 mol % of structural units represented by the following formula (2), 0 mol % to 80 mol % of structural units represented by formula (3), 0.1 mol % to 40 mol % of structural units represented by formula (4), and 0.1 mol % to 40 mol % of structural units represented by formula (5). -CO-Ar1-O-(2) -CO-Ar2-O-(3) -CO-Ar3-CO-(4) -O-Ar4-O-(5) In formulas (2) to (5), Ar1 represents a naphthylene group, Ar2 represents a phenylene group, a biphenylene group, or a group represented by formula (6), Ar3 represents a phenylene group, a naphthylene group, a biphenylene group, or a group represented by formula (6), Ar4 represents a phenylene group, a naphthylene group, a biphenylene group, or a group represented by formula (6), -Ar5-Z-Ar6-(6) In formula (6), Ar5 and Ar6 each independently represent a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylidene group.
[0043] The thermoplastic liquid crystal polymer can be synthesized by a known polycondensation method. As the monomer to be subjected to polycondensation, various aromatic diols, aromatic dicarboxylic acids, aromatic hydroxycarboxylic acids, or carboxylic acid derivatives such as acylated products of the hydroxyl groups obtained by activating the terminals of these monomers, esterified products of the carboxyl groups, acid halides, and acid anhydrides can also be used.
[0044] The ability to form an optically anisotropic molten phase in the present invention can be confirmed, for example, by placing a sample on a hot stage, heating it in a nitrogen atmosphere, and observing the light transmitted through the sample.
[0045] The melting point Tm (melting point as a resin) of the thermoplastic liquid crystal polymer constituting the thermoplastic liquid crystal polymer film of the present invention is, for example, preferably in the range of 260 to 360 ° C., more preferably in the range of 270 to 350 ° C. As described below, the melting point Tm of the thermoplastic liquid crystal polymer can be obtained by observing the thermal behavior of a thermoplastic liquid crystal polymer sample using a differential scanning calorimeter. That is, after the thermoplastic liquid crystal polymer sample is heated at a rate of 20 ° C. / min to completely melt it, the melt is cooled to 25 ° C. at a rate of 20 ° C. / min, and the position of the endothermic peak that appears after heating again at a rate of 20 ° C. / min is recorded as the melting point Tm of the thermoplastic liquid crystal polymer.
[0046] Further, from the viewpoint of melt moldability, the thermoplastic liquid crystal polymer may have a melt viscosity of, for example, 20 to 200 Pa s at a shear rate of 1000 / s at (Tm + 20) ° C., preferably 30 to 150 Pa s, and more preferably 50 to 100 Pa s.
[0047] (Thermoplastic liquid crystal polymer film) The thermoplastic liquid crystal polymer film is preferably an extrusion-molded film obtained by extruding a thermoplastic liquid crystal polymer. In this case, any extrusion molding method can be used, but well-known T-die film-forming stretching method, laminate stretching method, inflation method, etc. are industrially advantageous. In particular, in the inflation method, stress is applied not only in the machine axis direction (abbreviated as "MD") of the thermoplastic liquid crystal polymer film, but also in the direction perpendicular thereto (transverse direction (abbreviated as "TD", hereinafter also referred to as "width direction"). Since it can be uniformly stretched in MD and TD, a thermoplastic liquid crystal polymer film with controlled molecular orientation, dielectric properties, etc. in MD and TD can be obtained. In this specification, MD may be referred to as the "X direction", TD as the "Y direction", and the thickness direction of the film as the "Z direction".
[0048] In addition, the thermoplastic liquid crystal polymer film may be stretched as needed after extrusion molding.The stretching method itself is known, and either biaxial stretching or uniaxial stretching may be adopted, but biaxial stretching is preferred because it is easier to control the molecular orientation degree.In addition, for stretching, known uniaxial stretching machines, simultaneous biaxial stretching machines, sequential biaxial stretching machines, etc. can be used.
[0049] In extrusion molding, a stretching process may be performed to control the orientation. For example, in extrusion molding using a T-die method, the molten sheet extruded from the T-die may be stretched not only in the MD of the thermoplastic liquid crystal polymer film but also in both the TD and the MD simultaneously to form a film, or the molten sheet extruded from the T-die may be stretched first in the MD and then in the TD to form a film.
[0050] In addition, in extrusion molding by the inflation method, a cylindrical sheet melt-extruded from a ring die may be stretched at a predetermined draw ratio (corresponding to the stretch ratio in MD) and blow ratio (corresponding to the stretch ratio in TD) to form a film.
[0051] In the present invention, the thermoplastic liquid crystal polymer film formed by melt extrusion after film formation is subjected to a strain-controlling heat treatment (first heat treatment) at a predetermined temperature based on the melting point Tm of the thermoplastic liquid crystal polymer constituting the film, followed by a heat treatment (second heat treatment) to adjust the thermal expansion coefficient. Furthermore, the thermoplastic liquid crystal polymer film of the present invention has an absolute value of the change in the thermal expansion coefficient in the film thickness direction before and after heating at the melting point Tm + 20 ° C for 60 seconds (third heat treatment) of 40 ppm / ° C or less. In these heat treatments, the melting point Tm of the thermoplastic liquid crystal polymer, which serves as the reference temperature condition, is measured using a differential scanning calorimeter. The sample is heated to a temperature above the melting point of the thermoplastic liquid crystal polymer, cooled to room temperature, and then reheated. The temperature at which an endothermic peak appears when the sample is recorded as the melting point. In this case, the melting points of the thermoplastic liquid crystal polymer resin before film formation (which may be in pellet or powder form), the film after film formation, the film after the first heat treatment, and the film after the second heat treatment can be measured, but the measured melting points do not substantially change. That is, the melting points observed in the thermoplastic liquid crystal polymer before film formation and the thermoplastic liquid crystal polymer film after film formation are substantially the same, and the melting points observed in the thermoplastic liquid crystal polymer film before and after each heat treatment are also substantially the same. Therefore, in the present invention, the melting point of the thermoplastic liquid crystal polymer constituting the thermoplastic liquid crystal polymer film is described by a single symbol "Tm", regardless of whether the polymer is formed into a film form or whether it has been adjusted by heat treatment, and is described, for example, as "the melting point Tm of the thermoplastic liquid crystal polymer (constituting the film)" or "the melting point Tm of the thermoplastic liquid crystal polymer film". The specific measurement conditions for the melting point Tm are as follows: In accordance with the conditions of the example, a sample of the thermoplastic liquid crystal polymer is heated from room temperature to 350 ° C. at a rate of 20 ° C. per minute, held at the temperature after heating for 2 minutes, cooled to 25 ° C. at a rate of 20 ° C. per minute, held at 25 ° C. for 2 minutes, and then heated again at a rate of 20 ° C. per minute. The endothermic peak temperature derived from the thermoplastic liquid crystal polymer is the melting point Tm. Here, the sample of the thermoplastic liquid crystal polymer may be, for example, pellets of the thermoplastic liquid crystal polymer, or a film containing the thermoplastic liquid crystal polymer.In addition, when a plurality of endothermic peaks derived from the thermoplastic liquid crystal polymer are observed in a sample, the endothermic peak derived from the thermoplastic liquid crystal polymer with the largest weight ratio in the sample is taken as the melting point Tm. In addition, when a plurality of endothermic peaks derived from the thermoplastic liquid crystal polymer are observed in a sample and the weight ratios of the thermoplastic liquid crystal polymers assigned to each endothermic peak are equal, the endothermic peak with the lowest temperature is taken as the melting point Tm.
[0052] In the present invention, a first heat treatment (strain-controlled heat treatment) is performed on an extruded thermoplastic liquid crystal polymer film (raw film). The purpose of the first heat treatment (strain-controlled heat treatment) is to moderately alleviate distortion during film formation while suppressing deformation. The first heat treatment involves, for example, applying a pressure of 0.1 to 50 MPa, preferably 0.3 to 10 MPa, and more preferably 0.5 to 5 MPa in the thickness direction of the film, relative to the melting point (Tm) of the film, to suppress deformation, and performing heat treatment at a temperature of approximately Tm-20°C to Tm-5°C, preferably Tm-15°C to Tm-7°C, for 10 seconds to 5 minutes, preferably 20 seconds to 3 minutes, and more preferably 30 seconds to 2 minutes. In this specification, the film before this first heat treatment is referred to as the raw film, and the film after the first heat treatment is referred to as the precursor film. Pressurization may be performed using a sheet-type heating and pressing device such as a vacuum heat press.
[0053] Next, the precursor film is further heat-treated (second heat treatment) for 10 seconds to 10 minutes, preferably 15 seconds to 8 minutes, more preferably 20 seconds to 5 minutes, at a temperature of Tm-10°C to Tm+30°C, preferably Tm-8°C to Tm+20°C, relative to the melting point Tm of the film, to adjust the thermal expansion coefficient. The second heat treatment may be performed at normal pressure (unpressurized) after the precursor film is pressed onto a support such as aluminum foil.
[0054] The melting point (Tm) of the thermoplastic liquid crystal polymer film may be, for example, 250°C or higher, preferably 260 to 360°C, and more preferably 270 to 350°C.
[0055] The thermoplastic liquid crystal polymer film thus obtained has an absolute change in the thermal expansion coefficient in the film thickness direction before and after heating at the melting point (Tm) of the thermoplastic liquid crystal polymer + 20°C for 60 seconds of 40 ppm / °C or less, and a dielectric loss tangent at 5 GHz of 0.0015 or less. The absolute change in the thermal expansion coefficient is more preferably 20 ppm / °C or less, and even more preferably 10 ppm / °C or less. The dielectric loss tangent at 5 GHz is preferably 0.0010 or less, and may be 0.0008 or less.
[0056] The absolute value of the change in the thermal expansion coefficient in the thickness direction of the film is calculated from the difference between the numerical value of the thermal expansion coefficient after the film is placed on a hot plate heated to the melting point Tm of the thermoplastic liquid crystal polymer + 20 ° C. for 60 seconds (third heat treatment) and the numerical value of the thermal expansion coefficient of the film before heating. In the third heat treatment, in order to avoid difficulty in measuring the thermal expansion coefficient due to thermal deformation of the film, etc., the film is heated with aluminum foil laminated on it as a support. Specifically, the absolute value of the change in the thermal expansion coefficient can be calculated by the following method. A thermoplastic liquid crystal polymer film is sandwiched between two 50 μm thick aluminum foils to form an aluminum foil / thermoplastic liquid crystal polymer film / aluminum foil configuration, and heated and laminated for 1 minute at a temperature of the melting point Tm-10 ° C. of the thermoplastic liquid crystal polymer film using a vacuum heat press device at a pressure of 1 MPa, and then one side of the aluminum foil is peeled off to obtain a laminate having an aluminum foil / thermoplastic liquid crystal polymer film configuration. Subsequently, the obtained laminate was cut to 30 mm x 45 mm so that the MD (X direction) of the film was the long side, and attached to a 50 mm wide x 100 mm long x 1 mm thick SUS plate with heat-resistant polyimide tape, leaving 1 mm of the edge of the laminate around the edge, to produce a SUS plate / aluminum foil / thermoplastic liquid crystal polymer film structure laminate. This SUS plate laminate was heated for 60 seconds on a hot plate heated to the melting point Tm + 20 ° C of the thermoplastic liquid crystal polymer, with the SUS plate side as the contact surface with the hot plate (third heat treatment). The SUS plate, aluminum foil, and heat-resistant polyimide tape were peeled off from the heated SUS plate laminate to obtain a thermoplastic liquid crystal polymer film after the third heat treatment. The coefficient of thermal expansion (CTE) in the thickness direction of the thermoplastic liquid crystal polymer film after the third heat treatment was measured, and the absolute value of the change in CTE was calculated from the CTE values in the thickness direction before and after the heat treatment using the following formula. (Absolute value of CTE change in the thickness direction)=|(CTE in the thickness direction of the thermoplastic liquid crystal polymer film after the third heat treatment)−(CTE in the thickness direction of the thermoplastic liquid crystal polymer film before the third heat treatment)|
[0057] The thickness of the thermoplastic liquid crystal polymer film can be appropriately set depending on the application. For example, when considering use as a material for the insulating layer of a circuit board, it may be 10 to 500 μm, preferably 15 to 250 μm, more preferably 20 to 200 μm, and even more preferably 25 to 150 μm.
[0058] In the thermoplastic liquid crystal polymer film, the relative dielectric constant in the thickness direction of the film is preferably 3.0 or less, more preferably 2.9 or less. For example, the relative dielectric constant in the thickness direction of the film may be 2.4 to 2.9.
[0059] In the above-mentioned thermoplastic liquid crystal polymer film, the lower limit of the thermal expansion coefficient in the film thickness direction is preferably 100 ppm / °C, more preferably 150 ppm / °C. The upper limit of the thermal expansion coefficient in the film thickness direction is preferably 250 ppm / °C, more preferably 230 ppm / °C, even more preferably 210 ppm / °C, and even more preferably 200 ppm / °C. For example, the thermal expansion coefficient in the film thickness direction is preferably 100 ppm / °C or more and 250 ppm / °C or less.
[0060] In the thermoplastic liquid crystal polymer film, the amount of orientation component Z in the film thickness direction preferably satisfies the following condition. The amount of orientation component is a parameter that serves as an index of the orientation of the crystals constituting the film. It is a parameter that represents the molecular orientation in the film in the form of a three-dimensional vector (X, Y, Z) based on the integrated intensity value obtained by X-ray diffraction measurement of the target film from three mutually perpendicular directions (X direction, Y direction, Z direction). It is a parameter that is normalized so that the sum of the components of the three-dimensional vector is 1, and the higher the numerical value of the component, the greater the orientation in that direction. The amount of orientation component is measured by the method described in the Examples below. 0.001≦Z≦0.250 The amount of orientation component Z in the film thickness direction is preferably 0.20 or less, and may be 0.15 or less.
[0061] In the thermoplastic liquid crystal polymer film, the orientation component amount X in the MD of the film and the orientation component amount Y in the TD of the film preferably satisfy the following: 0.400≦X≦0.600 0.300≦Y≦0.500 The orientation component amount X in the MD of the film is preferably 0.550 or less, more preferably 0.500 or less. The orientation component amount Y in the TD of the film is preferably 0.450 or less, more preferably 0.400 or less.
[0062] The thermoplastic liquid crystal polymer film may contain at least one additive selected from the group consisting of thermoplastic resins other than the thermoplastic liquid crystal polymer, inorganic compounds, organic particles, and liquid crystal oligomers. The liquid crystal oligomer refers to an oligomer of 10 or less consisting of repeating units selected from the various repeating units exemplified for the thermoplastic liquid crystal polymer, and is produced by a known polymerization method such as polycondensation of the raw material compounds (monomers) described above. A 10 or less oligomer means that the total number of repeating units in one molecule is 10 or less.
[0063] For example, the thermoplastic liquid crystal polymer film may contain a thermoplastic polymer such as polyethylene terephthalate, modified polyethylene terephthalate, polycarbonate, polyarylate, polyamide, polyphenylene sulfide, polyether ether ketone, polyetherimide, polyphenylene ether, or fluororesin, within a range that does not impair the effects of the present invention.
[0064] The thermoplastic liquid crystal polymer film may contain 50% by weight or more of thermoplastic liquid crystal polymer, preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and even more preferably 98% by weight or more.
[0065] The standard deviation (μm) in the TD within the film plane when measured with a continuous film thickness meter is preferably 10.0 μm or less, more preferably 5.0 μm or less, and more preferably 3.0 μm or less.
[0066] When a thermoplastic liquid crystal polymer film is used as a circuit board material, heating is performed in multiple steps, such as laminating it with metal to form a laminate, processing the laminate into a circuit board, and mounting electronic components on the circuit board. The thermoplastic liquid crystal polymer film of the present invention has a reduced dielectric loss tangent and suppresses the change in the thermal expansion coefficient in the thickness direction before and after heating, so when used in high-frequency circuit boards, especially laminated circuit boards, it is advantageous in stably manufacturing products according to the intended design.
[0067] (Laminate) The laminate of the present invention is a laminate containing at least one layer of the thermoplastic liquid crystal polymer film of the present invention. The laminate may be a single-sided metal-clad laminate in which a metal layer is laminated on one side of a thermoplastic liquid crystal polymer film, or a double-sided metal-clad laminate in which a metal layer is laminated on both sides of a thermoplastic liquid crystal polymer film. The process of laminating a metal layer on a thermoplastic liquid crystal polymer film is not particularly limited, and may include a process of adhering a metal foil via an adhesive layer, a process of directly press-bonding a metal foil to the surface of the thermoplastic liquid crystal polymer film by thermocompression bonding, or a process of forming a metal layer on the surface of the thermoplastic liquid crystal polymer film by dry plating and / or dry plating. When using metal foil as the metal layer, it is preferable to directly laminate it by thermocompression bonding.
[0068] The metal foil used in the laminate is not particularly limited and may be, for example, gold, silver, copper, iron, nickel, aluminum, or an alloy metal thereof, etc. Copper foil or stainless steel foil is preferred from the viewpoints of conductivity, handleability, cost, etc. As the copper foil, rolled copper foil produced by a rolling method or electrolytic copper foil produced by an electrolytic method can be used.
[0069] The thickness of the metal foil can be appropriately set as needed, and may be, for example, 1 to 100 μm, preferably 5 to 50 μm, and more preferably 8 to 35 μm.
[0070] The metal foil may be subjected to a surface treatment such as a conventional roughening treatment. The roughened surface (such as a matte surface) of the metal foil may have an arithmetic mean roughness Ra of 0.10 to 0.70 μm, preferably 0.13 to 0.60 μm, and more preferably 0.15 to 0.50 μm, from the viewpoint of improving adhesion to the thermoplastic liquid crystal polymer film and high-frequency characteristics. The arithmetic mean roughness Ra is an index of roughness in the height direction measured in accordance with JIS B 0601:2001, and is the average value of the absolute deviations from the mean line to the roughness curve for a reference length.
[0071] The roughened surface of the metal foil may have a maximum height roughness Rz of 0.5 to 5.0 μm, preferably 0.8 to 4.5 μm, and more preferably 1.0 to 4.0 μm. The maximum height roughness Rz is an index of roughness in the height direction measured in accordance with JIS B 0601:2001, and represents the sum of the maximum peak height and the maximum valley depth in a roughness curve of a reference length.
[0072] In the thermocompression bonding process, the above-mentioned thermoplastic liquid crystal polymer film and metal foil are superimposed on the first surface of the thermoplastic liquid crystal polymer film so that the metal foil is in contact with the first surface of the thermoplastic liquid crystal polymer film, and then thermocompression bonded to obtain a single-sided metal-clad laminate. The thermocompression bonding process may be carried out using a sheet-type heating and pressing device such as a vacuum hot press, or may be carried out using a hot roll press device, in which the thermoplastic liquid crystal polymer film is superimposed on the surface of the metal foil so that the metal foil is in contact with the surface of the thermoplastic liquid crystal polymer film, and then introduced into a pair of pressure rolls. In addition, from the viewpoint of adhesion, the surface of the thermoplastic liquid crystal polymer film and the roughened surface of the metal foil may be superimposed on each other so that the surface of the thermoplastic liquid crystal polymer film is in contact with the roughened surface of the metal foil.
[0073] The heating temperature during thermocompression bonding may be, for example, in the range of (Tm-20) ° C. to (Tm+40) ° C., preferably about (Tm-10) ° C. to (Tm+30) ° C., for example, (Tm-5) ° C. to (Tm+10) ° C., where Tm is the melting point of the thermoplastic liquid crystal polymer film.
[0074] The pressure applied during thermocompression bonding may be about 0.5 to 6 MPa, preferably 1 to 5 MPa, for example 2 to 3 MPa.
[0075] The time required for thermocompression bonding is not particularly limited as long as the circuit board is well bonded, but may be, for example, about 10 to 40 minutes, or about 12 to 30 minutes.
[0076] The metal layer can also be formed by dry plating such as sputtering or vapor deposition, or wet plating such as electroless plating or electrolytic plating. For example, a metal layer may be formed on the surface of the thermoplastic liquid crystal polymer film by dry plating, and then the thickness of the metal layer may be increased by wet plating.
[0077] The metal for forming the metal layer is not particularly limited, and may be, for example, gold, silver, copper, iron, tin, nickel, aluminum, chromium, or an alloy metal thereof.
[0078] In sputtering or vapor deposition, a metal is sputtered or vapor-deposited to bring the metal parts into contact with each other and bond them together. Sputtering or vapor deposition is a well-known method in the field of electronic substrate manufacturing. Examples of metals for sputtering or vapor deposition include copper, aluminum, gold, tin, and chromium.
[0079] Electroless plating is a process of bonding two materials by depositing a metal from a solution containing metal ions. Electroless plating is a well-known method in the field of manufacturing plated products on non-conductive materials (such as plastics and ceramics). Examples of metals that can be used include copper, nickel, cobalt, gold, tin, and chromium.
[0080] The thickness of the metal layer can be appropriately set depending on the application of the metal-clad laminate, and can be selected from a wide range of, for example, 10 nm to 100 μm. When a metal foil is used as the metal layer, the thickness of the metal layer may be 1 to 100 μm, preferably 5 to 50 μm, and more preferably 8 to 35 μm. When the metal layer is formed by sputtering, vapor deposition, electroless plating, or the like, the thickness of the metal layer may be 10 nm to 35 μm, preferably 50 nm to 12 μm, and more preferably 100 nm to 9 μm.
[0081] The laminate of the present invention can be effectively used as a part used in the fields of electricity and electronics, office equipment and precision equipment, power semiconductors, etc., for example, as a circuit board material.
[0082] The metal layer of the laminate (metal-clad laminate) of the present invention can be processed into a wiring circuit to manufacture a circuit board.As the circuit processing method, a known method can be used, for example, a subtractive method can be used to etch the metal foil on the thermoplastic liquid crystal polymer film to form a circuit, or a semi-additive method can be used to form a circuit.
[0083] Circuit boards using the metal-clad laminate of the present invention are suitable for use as high-frequency circuit boards, in-vehicle sensors, mobile circuit boards, antennas, and the like.
[0084] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, various physical properties were measured by the following methods.
[0085] [Thickness] The thickness of each material was measured using a Digimatic Indicator (manufactured by Mitutoyo Corporation). Measurements were taken across the width of the material at intervals of 1 cm, and the average value of 10 points randomly selected from the center and edge was recorded as the thickness.
[0086] [Melting point Tm] Using a DSCQ2000 (manufactured by TA Instruments Japan Co., Ltd.), a 5 mg sample of a thermoplastic liquid crystal polymer was heated from room temperature to 350 ° C. at a rate of 20 ° C. per minute, held at the temperature for 2 minutes, cooled to 25 ° C. at a rate of 20 ° C. per minute, held at 25 ° C. for 2 minutes, and then heated again at a rate of 20 ° C. per minute. The endothermic peak temperature was taken as the melting point Tm.
[0087] [Method for measuring and deriving coefficient of thermal expansion (CTE)] (X and Y direction coefficient of linear expansion (CTE)) A sample of a thermoplastic liquid crystal polymer film was measured by tensile measurement using a thermomechanical analyzer (TMA450, manufactured by TA Instruments Japan Co., Ltd.) by heating from 25 ° C. to 200 ° C. at a rate of 5 ° C. / min, then cooling to 30 ° C. at a rate of 20 ° C. / min, and again heating at a rate of 5 ° C. / min between 30 ° C. and 150 ° C. Measurements were made in each of the X direction (MD) and Y direction (TD) of the film.
[0088] (Coefficient of linear expansion (CTE) in Z direction (thickness direction)) A sample of a thermoplastic liquid crystal polymer film was measured for expansion using a thermomechanical analyzer (TMA450, manufactured by TA Instruments Japan Co., Ltd.) by heating from 25°C to 200°C at a rate of 5°C / min, then cooling to 30°C at a rate of 20°C / min, and again heating at a rate of 5°C / min between 30°C and 150°C. Measurements were made in the thickness direction of the film.
[0089] (Absolute value of the change in the coefficient of linear expansion (CTE) in the Z direction (thickness direction)) The thermoplastic liquid crystal polymer film was sandwiched between two 50 μm thick aluminum foils to form an aluminum foil / thermoplastic liquid crystal polymer film / aluminum foil configuration, and then heated and laminated for 1 minute at a temperature of the melting point Tm-10 ° C. of the thermoplastic liquid crystal polymer film using a vacuum hot press device at a pressure of 1 MPa, and then peeled off the aluminum foil on one side to obtain a laminate having an aluminum foil / thermoplastic liquid crystal polymer film configuration. Subsequently, the obtained laminate was cut to 30 mm x 45 mm so that the MD (X direction) of the film was the long side, and attached to a 50 mm wide x 100 mm long x 1 mm thick SUS plate with heat-resistant polyimide tape around the edge of the laminate with 1 mm of adhesive margin, and a SUS plate / aluminum foil / thermoplastic liquid crystal polymer film configuration was produced. This SUS plate laminate was heated for 60 seconds on a hot plate heated to the melting point (Tm) of the thermoplastic liquid crystal polymer + 20 ° C., with the SUS plate side in contact with the hot plate (third heat treatment). The SUS plate, aluminum foil, and heat-resistant polyimide tape were peeled off from the heated SUS plate laminate to obtain a thermoplastic liquid crystal polymer film after the third heat treatment. The CTE in the thickness direction of the thermoplastic liquid crystal polymer film after the third heat treatment was measured in the same manner as described above, and the absolute value of the change in CTE was calculated from the values of the CTE in the thickness direction before and after the heat treatment using the following formula: (Absolute value of CTE change in the thickness direction) = | (CTE in the thickness direction of the thermoplastic liquid crystal polymer film after the third heat treatment) - (CTE in the thickness direction of the thermoplastic liquid crystal polymer film before the third heat treatment) |
[0090] (Measurement of dielectric loss tangent) The dielectric properties were measured at a frequency of 5 GHz by a cavity resonator perturbation method. A 5 GHz cavity resonator (Kanto Electronics Application Development Co., Ltd.) was connected to a network analyzer (Agilent Technology Corporation "E8362B"), and a minute material (width: 2 mm x length: 80 mm) was inserted into the cavity resonator, and the dielectric loss tangent of the material was measured under an environment of a temperature of 25°C and a humidity of 65% RH.
[0091] [Circuit Fabrication, Interlayer Connectivity Test] (Sample Fabrication Method) A thermoplastic liquid crystal polymer film with a conductor layer was produced by laminating a 12 μm thick rolled copper foil (manufactured by JX Nippon Mining & Metals Corporation, product name: BHYX-HA-V2) onto a thermoplastic liquid crystal polymer film in a copper foil / film / copper foil configuration at a pressure of 3 MPa for 15 minutes at the melting point (Tm) of the film + 5°C using a vacuum hot press. Through holes with a diameter of 150 μm were formed in the thermoplastic liquid crystal polymer film with the conductor layer using an NC drill, and then copper plating was applied to a thickness of 8 μm.
[0092] (Test Method) A thermal shock reliability test was carried out using a thermal shock device (TSA-43EL, manufactured by Espec Corporation) for 500 cycles, with one cycle consisting of cooling from room temperature to −65° C., heating from −65° C. to room temperature, heating from room temperature to 125° C., and cooling from 125° C. to room temperature.
[0093] (Evaluation method) After the thermal shock reliability test, the through-hole portion of the sample was cut and the cross-sectional state was observed using a scanning electron microscope (FlexSEM1000II, manufactured by Hitachi High-Tech Corporation). When the crack length was less than 2.8 μm in the cross-sectional observation, it was evaluated as good, and when it was 2.8 μm or more, it was evaluated as bad. Furthermore, when producing a thermoplastic liquid crystal polymer film with a conductor layer, warping occurred during copper foil lamination, and circuit production such as NC drilling was difficult. It was evaluated as -.
[0094] [Method for measuring the amount of orientation component] The amount of orientation component is a parameter obtained by a molecular orientation analysis method including the steps of: preparing a sample containing polymer molecules having at least some crystallinity; irradiating the sample with X-rays from the first, second, and third directions, where three different directions are defined as a first direction, a second direction, and a third direction, to obtain first, second, and third X-ray diffraction profiles corresponding to the first, second, and third directions, respectively; selecting predetermined peaks from the X-ray diffraction profiles in the first, second, and third directions, calculating the integrated intensities of the peaks; and calculating the three-dimensional molecular orientation of the sample based on the integrated intensities of the predetermined peaks. In this example, the following method was specifically used.
[0095] (Definition of Surfaces and Directions in Measurement) In the thermoplastic liquid crystal polymer film of the present invention, as shown in FIG. 1, the cut surface of the film is defined as the side surface, and the upper and lower surfaces surrounded by the cut surface are defined as the main surface. When X-rays are irradiated perpendicularly to the main surface of the thermoplastic liquid crystal polymer film, the direction parallel to the main surface where the molecular orientation is strongest is defined as the MD (X direction) of the film, the direction parallel to the main surface and perpendicular to the MD is defined as the TD (Y direction), and the direction perpendicular to the main surface is defined as the thickness direction (Z direction). Regarding the direction of X-ray irradiation, the direction passing through the main surface of the thermoplastic liquid crystal polymer film is referred to as the first direction d1 and Through. The direction in which X-rays are irradiated to the side surface of the film from a direction parallel to TD is referred to as the second direction d2 and Edge, and the direction in which X-rays are irradiated to the side surface of the film from a direction parallel to MD is referred to as the third direction d3 and End.
[0096] For example, the measurement procedure for the thermoplastic liquid crystal polymer film obtained in Example 1 will be described below. A D8 DISCOVER IμS instrument manufactured by Bruker was used for wide-angle X-ray diffraction measurement. The thermoplastic liquid crystal polymer film was cut into a 10 mm x 30 mm rectangle for main surface measurement with the MD as the long side, and a 1 mm x 5 mm rectangle for side surface measurement with the MD as the long side, and each was attached to a sample holder. To improve the S / N ratio of the data, multiple thermoplastic liquid crystal polymer films were stacked so that the MD or TD coincided, and the thickness was adjusted to approximately 0.5 mm. CuKα was used as the X-ray source. The filament voltage was 50 kV and the current was 1 mA. A collimator with an aperture diameter of φ0.3 mm was used.
[0097] The MD of the thermoplastic liquid crystal polymer film to be measured was determined in advance by preliminary measurement. Generally, the MD can be determined by performing X-ray diffraction measurement on the main surface of a thermoplastic liquid crystal polymer film whose MD is unknown, thereby confirming the direction in which the molecular orientation is strongest. The MD, which is the direction in which the molecules are most oriented in the film, was determined based on the peak of diffracted X-rays derived from the diffraction plane parallel to the molecular chain. In this case, in the two-dimensional diffraction image obtained by X-ray diffraction measurement on the main surface of the film, the direction shifted by 90 degrees from the azimuth angle with the strongest diffraction intensity is the MD. The size of the thermoplastic liquid crystal polymer film in the preliminary measurement, the settings of the X-ray diffraction measurement device, and the method for obtaining the azimuth angle with the strongest diffraction intensity from the two-dimensional diffraction image are basically the same as the method for measuring the three-dimensional molecular orientation of a thermoplastic liquid crystal polymer film described below.
[0098] The two-dimensional diffraction image was analyzed as follows: The diffraction intensity was the peak appearing at a diffraction angle 2θ of 19 to 21 degrees, which corresponds to the molecular chain direction.
[0099] The sample holder was attached to the apparatus, and the position of the sample was adjusted so that X-rays were irradiated from the main surface or side direction of the thermoplastic liquid crystal polymer film. That is, X-rays were irradiated onto the thermoplastic liquid crystal polymer film from the Through, Edge, and End directions, as shown in Figures 2A to 2C, respectively, and two-dimensional diffraction images corresponding to each direction were obtained (in Figures 2A to 2C, the arrow dI indicates the X-ray irradiation direction, and the arrow dT indicates the film thickness direction of the sample). The distance between the thermoplastic liquid crystal polymer film and the detector (camera distance) was 100 mm. A two-dimensional PSPC detector was used as the detector, and the exposure time was 180 to 600 seconds.
[0100] The obtained two-dimensional diffraction image was converted into a one-dimensional profile corresponding to data in a predetermined azimuth angle range from -5 (355) to 95 degrees by circular averaging. The predetermined azimuth angles φ were selected as 0, 10, 20, 30, 40, 50, 60, 70, 80, and 90 degrees in Figures 2A to 2C. Data in the vicinity of each φ was smoothed within the range of azimuth angles φ ± 5 degrees to obtain a one-dimensional profile at each azimuth angle φ. In the circular averaging, the diffraction angle (2θ) range was set to 5 to 42 degrees, with a 2θ step of 0.05 degrees. The obtained one-dimensional profile is referred to as Data 1. Data 1 includes one-dimensional data Thro-1 to 10, Edge-1 to 10, and End-1 to 10. Thro-1 is a one-dimensional profile corresponding to an azimuth angle of 0 degrees (obtained by smoothing data in the azimuth angle range of -5 to 5 degrees) of a two-dimensional diffraction image measured from the Through direction. Similarly, Thro-2 is 10 degrees (smoothed data in the azimuth angle range of 5 to 15 degrees), Thro-3 is 20 degrees (smoothed data in the azimuth angle range of 15 to 25 degrees), Thro-4 is 30 degrees (smoothed data in the azimuth angle range of 25 to 35 degrees), Thro-5 is 40 degrees (smoothed data in the azimuth angle range of 35 to 45 degrees), Thro-6 is 50 degrees (smoothed data in the azimuth angle range of 45 to 55 degrees), Thro-7 is 60 degrees (smoothed data in the azimuth angle range of 55 to 65 degrees), Thro-8 is 70 degrees (smoothed data in the azimuth angle range of 65 to 75 degrees), Thro-9 is 80 degrees (smoothed data in the azimuth angle range of 75 to 85 degrees), and Thro-10 is 90 degrees (smoothed data in the azimuth angle range of 85 to 95 degrees). These are one-dimensional profiles. Similarly, Edge-1 to 10 and End-1 to 10 are one-dimensional profiles corresponding to azimuth angle ranges of 10 degrees from the low angle side in measurements from the Edge direction and End direction.
[0101] The converted one-dimensional profile (Data 1) was measured under the same conditions to obtain background data (measurement data when no sample was attached), and the effects of parasitic scattering, etc. were removed based on this background data. That is, the obtained background data was converted into a one-dimensional profile, and then the background data was subtracted from the data when a thermoplastic liquid crystal polymer film was attached as a sample. The data obtained by this calculation is Data 2.
[0102] Furthermore, when separating peaks from the spectrum of Data 2 and calculating integrated intensities, a baseline for the spectrum was assumed and subtracted from the spectrum so that the net area of the peaks could be used. The data obtained by this calculation was designated Data 3. Here, the baseline was a linear function connecting the intensity values at 2θ of 5.5 degrees and 40 degrees in Data 2 after background processing.
[0103] In order to perform waveform separation of the peak shapes contained in the spectrum of Data 3, waveform separation analysis was performed on Data 3. In this waveform separation analysis, crystalline and amorphous peaks derived from hexagonal and orthorhombic crystals were also analyzed so that a unique peak set could be determined for the spectrum. For each peak, the peak function type was determined using the peak intensity, peak position, half-width, and the ratio of the Gaussian function of the pseudo-Voigt function to the Lorentzian function (Lor / Gau) as parameters, and the integrated intensity of each peak was calculated. The data obtained by this calculation is Data 4.
[0104] Among the peaks identified in Data 4, a peak having a peak top at a diffraction angle 2θ = 19 to 20 degrees was designated as a predetermined peak, and the amount of orientation component of the thermoplastic liquid crystal polymer was calculated from the integrated intensity of the peak. For the peak, a normalization constant was determined for normalizing the integrated intensity of the peak for each data set: the integrated intensity of Thro-1 to 10 in the measurement in the Through direction, the integrated intensity of Edge-1 to 10 in the measurement in the Edge direction, and the integrated intensity of End-1 to 10 in the measurement in the End direction. The normalization constants for the integrated intensity data sets Thro-1 to 10, Edge-1 to 10, and End-1 to 10 are taken as 1, a1, and a2, respectively, and the values of a1 and a2 were determined to minimize the function determined based on the difference in peak integrated intensity after normalization in each combination of Thro-10 and Edge-1, Thro-1 and End-1, and End-10 and Edge-10. The function is preferably a function represented by the sum of squares of the difference in peak integrated intensity after normalization in each combination of Thro-10 and Edge-1, Thro-1 and End-1, End-10 and Edge-10, and the normalization constants a1 and a2 are determined so that the values of the respective functions obtained by partially differentiating the function with respect to a1 and a2 are both zero. This calculation is based on the assumption that the molecular chains and parallel crystal planes from which the peaks of Thro-10 and Edge-1, Thro-1 and End-1, and End-10 and Edge-10 originate coincide. For example, the peak appearing at an azimuth angle of 90 degrees shown in FIG. 2A (corresponding to Thro-10) is a peak derived from the crystal plane of molecules oriented in the MD of the sample thermoplastic liquid crystal polymer film, while the peak appearing at an azimuth angle of 0 degrees shown in FIG. 2B (corresponding to Edge-1) is also a peak derived from the crystal plane of molecules oriented in the MD of the thermoplastic liquid crystal polymer film. In other words, since Thro-10 and Edge-1 correspond to peaks derived from the crystal plane of the same molecule, by standardizing so that the difference in integrated intensity between Thro-10 and Edge-1 is small, the data obtained by measuring from two different directions, Through and Edge, can be analyzed together.Similarly, the peak appearing at an azimuth angle of 0 degrees shown in FIG. 2A (corresponding to Thro-1) and the peak appearing at an azimuth angle of 0 degrees shown in FIG. 2C (corresponding to End-1) are peaks derived from the crystal plane of molecules oriented in the TD of the sample thermoplastic liquid crystal polymer film, and the peak appearing at an azimuth angle of 90 degrees shown in FIG. 2B (corresponding to Edge-10) and the peak appearing at an azimuth angle of 90 degrees shown in FIG. 2C (corresponding to End-10) are peaks derived from the crystal plane of molecules oriented in the thickness direction of the thermoplastic liquid crystal polymer film. Therefore, by standardizing to minimize the difference in integrated intensity between Thro-10 and Edge-1, Thro-1 and End-1, End-10 and Edge-10, the measurement results from three directions can be evaluated together, enabling three-dimensional analysis of molecular orientation.
[0105] The integrated intensities of Thro-1 to 10, Edge-1 to 10, and End-1 to 10 were normalized using the calculated normalization constant. The normalized integrated intensities and the reference vector were used to calculate the sum vector (X 1 , Y 1 , Z 1 The reference vector and the sum vector are both three-dimensional vectors with three components. The reference vector (X 0 , Y 0 , Z 0 ) are shown in Table 7. Here, the values of each component of the reference vector in Table 7 are values calculated from the azimuth angle of the measured one-dimensional profile based on the relationship shown in Figure 3. Each component of the reference vector is n and φ n,k As a function of (X 0 (n,φ n,k ), Y 0 (n,φ n,k ), Z 0 (n,φ n,k Here, n (n=1, 2, 3) is a variable representing the n-th direction, and φ n,k is the K obtained from the nth X-ray diffraction profile nThe reference vector is the azimuth angle corresponding to the kth one-dimensional profile among the k one-dimensional profiles. A reference vector is defined for each combination of X-ray irradiation direction and azimuth angle φ. The normalized integrated intensity at each direction and azimuth angle contains information about the molecular orientation in a plane defined with the X-ray irradiation direction as the normal. By using the reference vector, each component of a two-dimensional coordinate system within the plane related to the molecular orientation can be obtained from this integrated intensity information. FIG. 3 is a diagram showing the relationship between the direction of molecular orientation of a thermoplastic liquid crystal polymer film and the azimuth angle at which a diffraction X-ray peak resulting from the orientation appears when the X-ray irradiation direction is the Z-axis direction and X-rays are irradiated onto the XY plane of an object in a three-dimensional space of a Cartesian coordinate system. The azimuth angle φ is the angle when the X-axis direction is taken as the reference, i.e., 0°, and the positive direction as shown in FIG. 3 is taken. FIG. 3 is an X-Y plane view, and the vector in the azimuth angle φ direction corresponding to the calculated integrated intensity is indicated by a thick arrow. In this example, the reference vector was normalized to a magnitude of 1. In this case, the magnitude of the vector shown in FIG. 3 is 1. When molecules are oriented in a certain azimuthal angle, the azimuthal angle at which the molecules are oriented and the angle at which the maximum peak originating from the diffraction plane parallel to the molecules appears are different by 90 degrees. Therefore, the integrated intensity at the azimuthal angle φ in Figure 3 is derived from the crystal plane of the molecules oriented in the direction of the vector indicated by the dotted arrow in Figure 3, which is 90 degrees different from the azimuthal angle φ. Therefore, the degree of tilt of the actual molecular orientation in the X and Y directions can be determined from the magnitude of the X and Y components of the vector indicated by the dotted arrow in a direction 90 degrees different from the azimuthal angle φ. The magnitudes of the X and Y components of this vector are sinφ and cosφ, respectively. Furthermore, since the Z component of this vector is zero, the reference vector corresponding to the azimuthal angle φ in X-ray diffraction measurement in the Z direction can be expressed as (sinφ, cosφ, 0). Similarly, each component of the reference vector can be determined, and the reference vector (X 0 (n,φ n,k ), Y 0 (n,φ n,k ), Z 0 (n,φ n,k )) are as shown in Table 7.
[0106]
[0107] When calculating the sum of the normalized peak integrated intensities, the integrated intensities of Thro-10 and Edge-1, Thro-1 and End-1, and End-10 and Edge-10, which are fitted to match, are overlapped and summed. To compensate for this, in Table 7, the component of the reference vector that should be 1.0000 is changed to half that, 0.5000.
[0108] The resulting sum vector (X 1 , Y 1 , Z 1 ) is a three-dimensional vector representing the molecular orientation of the thermoplastic liquid crystal polymer film, and X 1 , Y 1 , Z 1 correspond to the molecular orientation in the MD, TD, and thickness direction dt of the thermoplastic liquid crystal polymer film, respectively. 1 , Y 1 , Z 1 ) vector length and X 1 , Y 1 , Z 1 By normalizing the sum of the vectors (X 1 , Y 1 , Z 1 ) each component X 1 , Y 1 , Z 1 The amount of orientation component of the thermoplastic liquid crystal polymer film was calculated as (X, Y, Z) by normalizing the sum of these to 1. By calculating the amount of orientation component, the contribution of the X, Y, and Z directions in the molecular orientation of the thermoplastic liquid crystal polymer film becomes clearer, making it easier to evaluate the molecular orientation of the object.
[0109] [Preparation of Thermoplastic Liquid Crystal Polymer] (Thermoplastic Liquid Crystal Polymer A) 1034.99 g (55 mol%) of 6-hydroxy-2-naphthoic acid (HNA), 272.52 g (22.5 mol%) of hydroquinone (HQ), 378.33 g (17.5 mol%) of 2,6-naphthalenedicarboxylic acid (NDCA), 83.07 g (5 mol%) of terephthalic acid (TPA), and 1226.87 g of acetic anhydride were added, and acetylation was carried out (145 ° C., reflux for about 1 hour). After that, the temperature was increased at 0.78 ° C. / min, maintained at 310 ° C., and kept at the same temperature for 3 hours to obtain a wholly aromatic liquid crystal polyester. The obtained wholly aromatic liquid crystal polyester was cooled to room temperature and then pulverized to obtain a powder (particle diameter of about 0.1 mm to about 1 mm). This powder was heated to 250 ° C at 3.75 ° C / min, then heated at 0.21 ° C / min until the final temperature reached 315 ° C., which was maintained for 3 hours for solid-state polymerization. The mixture was then granulated at 340 ° C. using a twin-screw extruder to obtain pellets of thermoplastic liquid crystal polymer A. The melting point Tm of the obtained polymer was 320 ° C., and the shear rate at 340 ° C. was 1000 s -1 The melt viscosity of the resin was 75 Pa·s.
[0110] (Thermoplastic liquid crystal polymer B) Thermoplastic liquid crystal polymer B (melting point Tm: 290 ° C., shear rate 1000 s at 310 ° C.) which is a wholly aromatic liquid crystal polyester similar to thermoplastic liquid crystal polymer A, except that the final temperature reached during solid-state polymerization was 285 ° C., using a ratio of 6-hydroxy-2-naphthoic acid (60 mol%), hydroquinone (10 mol%), 2,6-naphthalenedicarboxylic acid (20 mol%), and 4,4-biphenol (BP) (10 mol%). -1 The melt viscosity was 60 Pa·s.
[0111] (Thermoplastic liquid crystal polymer C) A thermoplastic liquid crystal polymer C (melting point Tm: 290 ° C., shear rate 1000 s at 310 ° C.) which is a wholly aromatic liquid crystal polyester similar to the thermoplastic liquid crystal polymer A, in the proportions of 6-hydroxy-2-naphthoic acid (55 mol%), 4,4-biphenol (22.5 mol%), 2,6-naphthalenedicarboxylic acid (5 mol%), and terephthalic acid (17.5 mol%). -1 The melt viscosity was 80 Pa·s.
[0112] (Thermoplastic liquid crystal polymer D) As the thermoplastic liquid crystal polymer, a thermoplastic liquid crystal polymer D (melting point Tm: 280 ° C., shear rate 1000 s at 300 ° C.) which is a wholly aromatic liquid crystal polyester similar to the thermoplastic liquid crystal polymer A, except that the final temperature reached during solid-state polymerization was 275 ° C., using a ratio of p-hydroxybenzoic acid (73 mol%) and 6-hydroxy-2-naphthoic acid (27 mol%). -1 The melt viscosity was 42 Pa·s.
[0113] (Thermoplastic liquid crystal polymer E) Thermoplastic liquid crystal polymer E (melting point Tm: 220 ° C., shear rate 1000 s at 240 ° C.) is a wholly aromatic liquid crystal polyester similar to thermoplastic liquid crystal polymer A, except that the final temperature reached during solid-state polymerization was 215 ° C., using a ratio of 6-hydroxy-2-naphthoic acid (40 mol%), p-hydroxybenzoic acid (40 mol%), hydroquinone (10 mol% as the composition in the polymer), and terephthalic acid (10 mol%). -1 The melt viscosity was 100 Pa·s.
[0114] [Example 1] (1) Preparation of thermoplastic liquid crystal polymer film raw roll (raw roll film) The thermoplastic liquid crystal polymer A obtained above was heated and kneaded in a single-screw extruder, and the film obtained by the T-die molding method was stretched twice in the MD (machine direction) and four times in the TD (transverse direction) to obtain a thermoplastic liquid crystal polymer film raw roll.
[0115] (2) Preparation of strain-controlled thermoplastic liquid crystal polymer film (precursor film) (strain control treatment: first heat treatment) The thermoplastic liquid crystal polymer film raw material obtained in (1) above was cut to a size of 20 cm x 20 cm, and then a 125 μm thick polyimide film (manufactured by DuPont-Toray Co., Ltd., product name: Kapton) was used using a vacuum heat press device. In the configuration of polyimide film / thermoplastic liquid crystal polymer film raw material / polyimide film, the thermoplastic liquid crystal polymer was heated and laminated at a pressure of 1 MPa at the melting point Tm-10 ° C. for 1 minute, and the polyimide film was peeled off from the obtained laminate to prepare a strain-controlled thermoplastic liquid crystal polymer film (precursor film).
[0116] (3) Preparation of Thermoplastic Liquid Crystal Polymer Film (Second Heat Treatment) For the 20 cm x 20 cm strain-controlled thermoplastic liquid crystal polymer film (2), a 50 μm thick aluminum foil roll was used as a support, and a heat-resistant rubber roll (hardness 90 degrees) and a heated metal roll were attached to a hot roll press. The strain-controlled thermoplastic liquid crystal polymer film was supplied between the rolls so that the heat-resistant rubber roll surface was in contact with the aluminum foil on the heated metal roll surface, and the film was pressed at a temperature of 260 ° C and a pressure of 1 MPa to produce a thermoplastic liquid crystal polymer film / aluminum laminate. Subsequently, the laminate was heat-treated (second heat treatment) at a speed of 3 m / min in a 1.5 m long hot air circulating heat treatment furnace, the furnace interior of which was controlled to the predetermined temperature listed in Table 8, to obtain a laminate after the second heat treatment. In the obtained laminate, the film was peeled off at an angle of 180 ° relative to the support to obtain a thermoplastic liquid crystal polymer film having a thickness of 50 μm.
[0117] [Example 2] Thermoplastic liquid crystal polymer A was heated and kneaded in a single-screw extruder, and the film obtained by the T-die molding method was stretched twice in MD and five times in TD to produce a raw thermoplastic liquid crystal polymer film. A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained in the same manner as in Example 1, except that the second heat treatment temperature (3) was changed.
[0118] Example 3 A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained in the same manner as in Example 2, except that the thermoplastic liquid crystal polymer B was used.
[0119] Example 4 A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained in the same manner as in Example 2, except that thermoplastic liquid crystal polymer C was used.
[0120] [Example 5] Thermoplastic liquid crystal polymer A was heated and kneaded in a single-screw extruder, and melt-extruded from an annular inflation die (die diameter 46.0 mm, die slit spacing 500 μm) at a draw ratio of 2.5 and a blow ratio of 4.0 to produce a raw film. A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained in the same manner as in Example 1, except that
[0121] [Comparative Example 1] Thermoplastic liquid crystal polymer A was heated and kneaded in a single-screw extruder, and melt-extruded from an annular inflation die (die diameter 46.0 mm, die slit spacing 500 μm) at a draw ratio of 2.5 and a blow ratio of 4.0 to produce a raw film. A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained in the same manner as in Example 2, except that the distortion control treatment (first heat treatment) of (2) was not performed.
[0122] [Comparative Example 2] Thermoplastic liquid crystal polymer A was heated and kneaded in a single-screw extruder, and melt-extruded from an annular inflation die (die diameter 46.0 mm, die slit spacing 500 μm) at a draw ratio of 2.5 and a blow ratio of 4.0 to produce a raw film. A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained in the same manner as in Example 1, except that the heat treatment (second heat treatment) of (3) was not performed.
[0123] [Comparative Example 3] Thermoplastic liquid crystal polymer D was heated and kneaded in a single-screw extruder, and melt-extruded from an annular inflation die (die diameter 46.0 mm, die slit spacing 500 μm) at a draw ratio of 2.5 and a blow ratio of 4.0 to produce a raw film. A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained in the same manner as in Example 1, except that the heat treatment (second heat treatment) of (3) was not performed.
[0124] [Comparative Example 4] Thermoplastic liquid crystal polymer D was used, and the mixture was heated and kneaded in a single-screw extruder, and then melt-extruded from an annular inflation die (die diameter 46.0 mm, die slit spacing 500 μm) at a draw ratio of 2.5 and a blow ratio of 4.0 to produce a raw film. A thermoplastic liquid crystal polymer film having a thickness of 50 μm was obtained in the same manner as in Example 2, except that the raw film was produced.
[0125] Comparative Example 5 A thermoplastic liquid crystal polymer film was obtained in the same manner as in Example 2, except that thermoplastic liquid crystal polymer E was used.
[0126] The orientation component amount, thermal expansion coefficient, dielectric constant in the thickness direction, and dielectric loss tangent (Df) were measured for the films of Examples 1 to 5 and Comparative Examples 1 to 5, and circuit fabrication and interlayer connectivity tests were conducted. A third heat treatment was also performed under the above conditions, and the change in the thermal expansion coefficient in the thickness direction after the third heat treatment was measured. The conditions for Examples 1 to 5 and Comparative Examples 1 to 5 are shown in Table 8, and the analysis results are shown in Table 9.
[0127]
[0128]
[0129] As shown in the table above, the thermoplastic liquid crystal polymer films according to the examples of the present invention also showed good results in circuit formation and interlayer connectivity tests. In contrast, the films of Comparative Examples 1 to 3, in which the change in thermal expansion coefficient in the thickness direction was outside the range of the present invention, exhibited warping, making it impossible to perform circuit formation tests or interlayer connectivity tests. Furthermore, the films of Comparative Examples 4 and 5 had dielectric loss tangents outside the range of the present invention, resulting in poor dielectric properties. Furthermore, the cracks that occurred during circuit formation and interlayer connectivity tests were large, failing to meet the acceptable standards.
[0130] The metal-clad laminate of the present invention can be used for parts used in, for example, the electrical and electronic fields, the office equipment and precision equipment fields, and the power semiconductor field, and can be particularly effectively used as a high-frequency circuit board material.
[0131] While the preferred embodiments of the present invention have been described above, those skilled in the art will readily recognize various changes and modifications within the scope of the present invention, which are obvious from the description of the present invention. Therefore, such changes and modifications are to be interpreted as falling within the scope of the invention as defined by the claims.
[0132] d1, Trough First direction d2, Edge Second direction d3, End Third direction dI X-ray irradiation direction dT Film thickness direction
Claims
1. A film comprising a thermoplastic polymer capable of forming an optically anisotropic molten phase (hereinafter referred to as a thermoplastic liquid crystal polymer), wherein the absolute value of the change in thermal expansion coefficient in the thickness direction of the film before and after heating the film at the melting point (Tm) of the thermoplastic liquid crystal polymer + 20°C for 60 seconds is 40 ppm / °C or less, and the dielectric tangent at 5 GHz is 0.0015 or less.
2. The thermoplastic liquid crystal polymer film according to claim 1, wherein the thermal expansion coefficient in the thickness direction of the film is 100 ppm / °C or more and 250 ppm / °C or less.
3. The thermoplastic liquid crystal polymer film according to claim 1, wherein the amount of orientation component Z in the film thickness direction satisfies the following: 0.001≦Z≦0.
250.
4. The thermoplastic liquid crystal polymer film according to claim 1 or 2, wherein the amount of orientation component X in the MD of the film and the amount of orientation component Y in the TD of the film satisfy the following: 0.400≦X≦0.600 0.300≦Y≦0.500 5. A thermoplastic liquid crystal polymer film according to claim 1 or 2, comprising a structural unit represented by the following formula (1) in an amount of 30 mol % or more and 90 mol % or less of all structural units constituting the thermoplastic liquid crystal polymer: [In the formula, a, b, c, and d are each independently 0 or 1, provided that a+b=1, c+d=1, and b and c cannot be 0 at the same time.] 6. A thermoplastic liquid crystal polymer film according to claim 1 or 2, comprising, among all structural units constituting said thermoplastic liquid crystal polymer, 20 mol % or more and 90 mol % or less of structural units represented by formula (2), 0 mol % or more and 80 mol % or less of structural units represented by formula (3), 0.1 mol % or more and 40 mol % or less of structural units represented by formula (4), and 0.1 mol % or more and 40 mol % or less of structural units represented by formula (5). -CO-Ar1-O-(2) -CO-Ar2-O-(3) -CO-Ar3-CO-(4) -O-Ar4-O-(5) In formulas (2) to (5), Ar1 represents a naphthylene group, Ar2 represents a phenylene group, a biphenylene group, or a group represented by formula (6), Ar3 represents a phenylene group, a naphthylene group, a biphenylene group, or a group represented by formula (6), Ar4 represents a phenylene group, a naphthylene group, a biphenylene group, or a group represented by formula (6), and -Ar5-Z-Ar6-(6) In formula (6), Ar5 and Ar6 each independently represent a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylidene group.
7. A thermoplastic liquid crystal polymer film according to claim 1 or 2, which has a relative dielectric constant in the thickness direction of the film of 3.0 or less.
8. A laminate comprising an insulating layer containing the thermoplastic liquid crystal polymer film according to claim 1 or 2, and a metal layer.
9. A circuit board comprising at least one selected from the group consisting of the thermoplastic liquid crystal polymer film according to claim 1 or 2 and the laminate according to claim 8.
10. A method for producing a thermoplastic liquid crystal polymer film as defined in claim 1 or 2, comprising the steps of: preparing a raw film by melt extrusion molding of a thermoplastic liquid crystal polymer; performing a first heat treatment on the raw film at a melting point (Tm)-20°C to a melting point (Tm)-5°C for 10 seconds to 5 minutes while applying a pressure of 0.1 to 50 MPa to prepare a precursor film; and performing a second heat treatment on the precursor film at a melting point (Tm)-10°C to a melting point (Tm)+30°C for 10 seconds to 10 minutes.
11. The method for producing a thermoplastic liquid crystal polymer film according to claim 10, wherein the second heat treatment is carried out after pressing the precursor film onto a support.
Citation Information
Patent Citations
Method for preparing flexible circuit board based on liquid crystal polymer film
CN112351592A
Thermoplastic liquid crystalline polymer film and circuit board using the same
JP2006137786A
Thermoplastic liquid crystal polymer film and laminate and circuit board using the same
JP2017106020A
Thermoplastic liquid crystal polymer and film of same
WO2018181222A1