Surface-treated powder and cosmetic using same

Surface-treating fine particle titanium oxide with a targeted fatty acid to particle diameter ratio addresses photoactivity and stability issues in cosmetics, enhancing UV protection and formulation stability by optimizing fatty acid usage.

WO2024237294A1PCT designated stage expired Publication Date: 2024-11-21TAYCA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018030
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-05-15
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Fine particle titanium oxide used in cosmetics faces challenges with photoactivity and dispersibility, particularly when combined with carbomer in O/W emulsified cosmetics, leading to instability and insufficient UV protection due to excess fatty acid treatment.

Method used

Surface-treating fine particle titanium oxide with a specific range of fatty acid to particle diameter ratio, between 1.5 and 3.7, to suppress photoactivity and improve stability, while minimizing fatty acid elution and enhancing dispersibility.

Benefits of technology

The surface-treated powder effectively reduces photoactivity and improves the stability and UV protection of cosmetic formulations by controlling the amount of fatty acid used, maintaining effective dispersibility and viscosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a surface-treated powder of fine particulate titanium oxide in which it is possible to enhance the suppression of the optical activity of the fine particulate titanium oxide and enhance the stability of a formulation. The surface-treated powder contains fine particulate titanium oxide as a powder to be subjected to a surface treatment and a fatty acid. The product of the average primary particle size (nm) of the fine particulate titanium oxide and the ratio of the mass of the fatty acid to the mass of the fine particulate titanium oxide (in terms of the fatty acid) is 1.5-3.7.
Need to check novelty before this filing date? Find Prior Art

Description

Surface-treated powder and cosmetics using the same

[0001] The present invention generally relates to a surface-treated fine particle titanium dioxide powder, and more particularly to a surface-treated fine particle titanium dioxide powder to be contained in a cosmetic product, and a cosmetic product using the same.

[0002] Fine particle titanium dioxide has a high UV-B protection effect and is incorporated into many cosmetics. Because fine particle titanium dioxide has high photoactivity, it is generally treated with hydrated silica or aluminum hydroxide to suppress photoactivity. Furthermore, to improve dispersibility in oils, it is often surface-treated with fatty acids such as stearic acid. Most fine particle titanium dioxide that has been surface-treated with aluminum hydroxide or fatty acids to improve dispersibility in oils is incorporated into W / O emulsion cosmetics.

[0003] For example, Japanese Patent Application Laid-Open No. 11-171541 (patent document) describes a method of first coating titanium dioxide with a water-soluble aluminum salt, and then coating titanium dioxide with a fatty acid having seven or more carbon atoms or a water-soluble salt thereof, and then blending the resulting titanium dioxide fine particles into a cosmetic product.

[0004] On the other hand, many O / W emulsion cosmetics often contain carbomer (carboxyvinyl polymer) to achieve a fresh feel when used. Carbomer imparts a thickening effect by the repulsion of negative charges between the carboxyl groups in the structure. However, when titanium dioxide fine particles surface-treated with aluminum hydroxide are blended into O / W emulsion cosmetics, when aluminum ions are eluted, the eluted aluminum ions interact electrically with the carbomer, resulting in the problem of not being able to maintain the thickening effect of the carbomer.

[0005] Therefore, when fine particle titanium dioxide and carbomer are used in combination in an O / W emulsion cosmetic, it is preferable to use fine particle titanium dioxide that has not been treated with aluminum hydroxide.

[0006] Japanese Patent Application Publication No. 11-171541

[0007] However, in order to suppress the photoactivity of titanium dioxide microparticles by treatment with fatty acids alone, it is necessary to surface treat the titanium dioxide microparticles with an amount of fatty acid in excess of the amount of fatty acid required to improve dispersibility in oil solutions. In this case, the excess amount of fatty acid will dissolve into polar oils, etc. in the formulation, and the dissolved fatty acid may react with other components to produce by-products, which may affect the viscosity and stability of the formulation. On the other hand, if the amount of fatty acid is limited to the amount required to disperse the titanium dioxide microparticles in oil solutions, the photoactivity of the titanium dioxide microparticles will not be sufficiently suppressed, and sufficient water repellency will not be obtained, resulting in poor dispersibility when incorporated into formulations and poor formulation stability.

[0008] Therefore, the object of the present invention is to provide a surface-treated powder of fine titanium dioxide particles that can suppress the photoactivity of fine titanium dioxide particles while suppressing the amount of fatty acid processed, thereby improving the photoactivity suppression effect of fine titanium dioxide particles and improving the stability of the formulation.

[0009] As a result of extensive research, the present inventors have discovered the following: Because titanium dioxide microparticles have a small particle size, the amount of surface hydroxyl groups is large, and therefore, in order to suppress photoactivity and obtain dispersibility in oil solutions, more fatty acid is required than in the case of titanium dioxide with a large particle size. The present inventors have found that by setting the product of the particle size of titanium dioxide microparticles and the amount of fatty acid treated within a predetermined range, it is possible to both suppress photoactivity and reduce the amount of fatty acid treated. By reducing the amount of fatty acid treated, the amount of fatty acid eluted is reduced, thereby improving the stability of the formulation.

[0010] Based on the above findings, the surface-treated powder of the present invention contains fine titanium dioxide particles and a fatty acid as the powder to be surface-treated, and the product of the average primary particle diameter (nm) of the fine titanium dioxide particles and the ratio of the mass of the fatty acid to the mass of the fine titanium dioxide particles is 1.5 or more and 3.7 or less.

[0011] In this way, it is possible to provide a surface-treated powder of titanium dioxide fine particles that can suppress the photoactivity of titanium dioxide fine particles and improve the stability of the formulation.

[0012] The surface-treated powder of the present invention and a cosmetic containing the same will be described in detail below, with specific examples. Note that the present invention is not limited to the following embodiments, and various modifications are possible within the scope of the technical concept of the present invention.

[0013] 1. Production of Surface-Treated Powder In one embodiment, the surface-treated powder according to the present invention is produced by mixing finely divided titanium dioxide with a fatty acid or a fatty acid salt, followed by drying.

[0014] 2. Surface-treated Powder Titanium dioxide fine particles as the surface-treated powder are produced by known methods. The crystalline form of the surface-treated powder is selected depending on the intended use. For example, when titanium dioxide fine particles are to be incorporated into an emulsified cosmetic, they preferably contain rutile-type crystals. The particle size is selected depending on the intended use, etc. For example, when incorporated into an emulsified cosmetic, the average primary particle size is preferably 5 nm or more and 50 nm or less, more preferably 8 nm or more and 40 nm or less, and even more preferably 12 nm or more and 35 nm.

[0015] 3. Fatty Acids Fatty acids are contained in the surface-treated powder as a hydrophobic treatment agent for the surface-treated powder. As fatty acids, stearic acid or its salt, lauric acid or its salt, myristic acid or its salt, palmitic acid or its salt, or isostearic acid or its salt are preferably used, with stearic acid or its salt and isostearic acid or its salt being more preferred. Mixed fatty acids may also be used for treatment. The salt of the fatty acid is preferably an alkali metal, more preferably sodium or potassium. The product of the average primary particle diameter (nm) of the titanium dioxide fine particle serving as the surface-treated powder and the ratio of the mass of the fatty acid to the mass of the titanium dioxide fine particle is 1.5 to 3.7, more preferably 2.0 to 3.0. The content of the fatty acid in the surface-treated powder, calculated as fatty acid equivalent, is preferably 7% to 16% of the weight of the surface-treated powder, more preferably 9% to 11%. The fatty acid equivalent is a value calculated excluding the countercation contained in the fatty acid or its salt.

[0016] 4. Other Treatments The powder to be surface-treated can be treated with a metal hydrate oxide or metal oxide, but from the viewpoint of the charge interaction with carbomer, the amount of metal hydroxide or metal oxide treated should be small. In particular, it is preferable not to treat alkaline earth metals, aluminum, or zinc, which are likely to interact with carbomer in a charge interaction. When used for surface treatment, the amount of other metal hydrate oxide or metal oxide treated is preferably 3% or less of the mass of the powder to be surface-treated (fine particle titanium oxide), more preferably 1% or less, and even more preferably not to treat it substantially. Furthermore, silane, silane coupling agent, and silicone may be used for surface treatment.

[0017] 5. Cosmetics The surface-treated powder of the present invention can be blended into cosmetics. There are no limitations on the type of cosmetics to be blended, and the cosmetics may be any of O / W emulsion cosmetics, W / O emulsion cosmetics, and oil-type cosmetics.

[0018] When the surface-treated powder of the present invention is blended into an O / W emulsion cosmetic, the blending method can be, for example, to add the surface-treated powder of the present invention to a mixture of raw materials for the oil phase, and then add a mixture of raw materials for the aqueous phase while stirring.

[0019] The surface-treated powder according to the present invention and the cosmetic composition using the same will be described in more detail below, showing specific production examples and test results.

[0020] <Production of Surface-Treated Powder> Example 1

[0021] Step 1) An aqueous solution of titanyl sulfate crystals (TM crystals manufactured by Teika Corporation) is heated to produce a hydrolyzate, which is then filtered and washed to obtain 35 kg of hydrous titanium dioxide cake (titanium dioxide content: TiO 2 To the suspension (equivalent to 10 kg in terms of volumetric sugar), 100 kg of a 48% aqueous solution of sodium hydroxide was added with stirring, and the suspension was heated to a temperature range of 95 to 105°C and stirred for 2 hours. The suspension of titanium dioxide hydrate was then filtered, and the cake was thoroughly washed with water. Approximately 25 kg of water was added to the washed cake to form a slurry, and TiO 2 The converted concentration was adjusted to 220 g / L. Then, 1.7 kg of 35% hydrochloric acid was added while stirring, and water was added to the mixture. 2The concentration was adjusted to 160 g / L in terms of the total concentration. 250 g of anhydrous sodium sulfate was added, followed by 14.0 kg of 35% hydrochloric acid. The mixture was heated and aged at 95°C to 100°C for 2 hours. X-ray diffraction showed that the solid particles in this slurry had a rutile-type titanium dioxide crystal structure.

[0022] Step 2) The concentration of the obtained titanium dioxide aqueous suspension was adjusted to 70 g / L. 2 To a suspension of titanium dioxide (equivalent to 1.4 kg), aqueous ammonia was added to adjust the pH to 6.0, the aqueous suspension was heated to 60°C and aged, and then the pH was adjusted to 6.0 again with aqueous ammonia, and the slurry was filtered and washed to obtain a washed cake. The cake was dispersed in water again and heated to 60°C, and then aqueous ammonia was added to adjust the pH to 7.5 and aged. After aging, the pH was adjusted to 7.5 again with aqueous ammonia, and the slurry was filtered and washed to obtain a washed cake. The washed cake was placed in a dryer (150°C) to remove moisture, and a titanium dioxide powder (dried product) was obtained.

[0023] Step 3) The dried titanium dioxide powder was calcined at 400°C for 120 minutes and then pulverized to obtain fine titanium dioxide particles (calcined product). The average primary particle diameter of the pulverized fine titanium dioxide particles (calcined product) was 24.6 nm.

[0024] Step 4) Water was added to the fine particle titanium oxide (calcined product) to adjust the concentration to 100 g / L. 10 L of the obtained fine particle titanium oxide (calcined product) slurry (TiO 2 (equivalent to 1.0 kg) was heated to 85°C.

[0025] Step 5) After heating, 118 g of sodium stearate (11% by weight in terms of fatty acid relative to the mass of titanium dioxide fine particle) was added to the slurry. The pH gradually increased and reached pH 7.0 after 10 minutes, and the slurry was aged for 1 hour. The pH after aging for 1 hour was between 8.0 and 10.0.

[0026] Step 6) After further aging, the pH value of the slurry was adjusted to 6.7 by adding an aqueous sodium hydroxide solution or an aqueous sulfuric acid solution, and then aging was continued for 30 minutes. The slurry was filtered, washed, and dried at 105°C for 15 hours. The dried product was pulverized using an Eck atomizer to obtain the surface-treated powder of Example 1.

[0027] Example 2 A surface-treated powder was produced in the same manner as in Example 1, except that sodium stearate in step 5 was changed to sodium laurate.

[0028] Example 3 A surface-treated powder was produced in the same manner as in Example 1, except that sodium stearate in step 5 was changed to sodium myristate.

[0029] Example 4 A surface-treated powder was produced in the same manner as in Example 1, except that sodium stearate in step 5 was changed to sodium palmitate.

[0030] Example 5 A surface-treated powder was produced in the same manner as in Example 1, except that sodium stearate in step 5 was changed to isostearic acid.

[0031] Example 6 A surface-treated powder was produced in the same manner as in Example 1, except that the amount of sodium stearate added in step 5 was changed to 75 g (7% by weight in terms of fatty acid relative to the mass of titanium dioxide fine particles).

[0032] Example 7 A surface-treated powder was produced in the same manner as in Example 1, except that the amount of sodium stearate added in step 5 was changed to 162 g (15% by weight in terms of fatty acid relative to the mass of titanium dioxide fine particles).

[0033] Example 8 A surface-treated powder was produced in the same manner as in Example 1, except that in step 3, roasting was carried out at a roasting temperature of 500°C, so that the average primary particle diameter of the resulting titanium dioxide fine particles was 30.8 nm, and the amount of sodium stearate added was changed to 97 g (9 wt % in terms of fatty acid relative to the mass of the titanium dioxide fine particles).

[0034] Example 9 A surface-treated powder was produced in the same manner as in Example 1, except that in step 3, the titanium dioxide particles were roasted at a roasting temperature of 350°C for 120 minutes to give an average primary particle size of 23.6 nm, and the amount of sodium stearate added in step 5 was changed to 153 g (14.2 wt % in terms of fatty acid relative to the mass of the titanium dioxide particles).

[0035] Comparative Example 1 A surface-treated powder was produced in the same manner as in Example 1, except that in step 3, roasting was carried out at a roasting temperature of 350°C for 120 minutes to set the average primary particle size of the resulting fine titanium dioxide particles to 23.6 nm, and the amount of sodium stearate added in step 5 was changed to 180 g (16.7% by weight, calculated as fatty acid, relative to the mass of the fine titanium dioxide particles).

[0036] Comparative Example 2 A surface-treated powder was produced in the same manner as in Example 1, except that the amount of sodium stearate added in step 5 was changed to 32 g (3% by weight in terms of fatty acid relative to the mass of fine titanium dioxide particles).

[0037] Comparative Example 3 A surface-treated powder was produced in the same manner as in Example 1, except that the amount of sodium stearate added in step 5 was changed to 215 g (20% by weight in terms of fatty acid relative to the mass of the fine particle titanium dioxide).

[0038] <Method of calculating particle size> The particle size of the titanium dioxide fine particle was measured as the average primary particle size of the titanium dioxide fine particle after pulverization in step 3. The titanium dioxide fine particle was photographed with a transmission electron microscope (TEM), and the particle size was calculated (number of particles: 100) using image analysis particle size distribution measurement software (Mac-View: manufactured by Mountech Co., Ltd.). The Heywood diameter (diameter equivalent to a circle with a projected area) was used to calculate the particle size.

[0039] <Lightfastness Test> The lightfastness of the surface-treated powders of each Example and Comparative Example was evaluated as follows. 3.0 g of fine titanium dioxide particles was weighed into a 100 mL polypropylene cup. Then, 4.0 g of 1,3-butylene glycol was weighed. Using a Teflon rod, the fine titanium dioxide particles and 1,3-butylene glycol were thoroughly mixed until they were well blended to prepare a paste. The paste was placed on a film, and a cover glass was placed on top to prevent oxygen from being supplied. The color tone L of each sample was measured.0 , a 0 , b 0 These samples were exposed to (Q-SUN:Xe-1) at 60 W / m 2 After the specified amount of irradiation, the color tone L of each sample was measured again. 1 , a 1 , b 1 The discoloration (ΔE) of each sample was calculated using the following formula. The lower the ΔE value, the better the lightfastness. The results are shown in Table 1. ΔE=[(L 1 -L 0 ) 2 + (a 1 -a 0 ) 2 +(b 1 -b 0 ) 2 ] 1/2

[0040] <Elution Test> The amount of eluted fatty acids from the surface-treated powders of each Example and Comparative Example was evaluated as follows. 10 g of each surface-treated powder from each Example and Comparative Example was weighed into a 300 mL glass Erlenmeyer flask. Next, 50 g of acetone was weighed, and a condenser was connected to reflux in a 75°C water bath for 10 minutes. After refluxing, filtration was repeated using a Kiriyama funnel and filter paper (5C) until the filtrate became transparent. To the now transparent filtrate, 10 g of ion-exchanged water and 3 drops of 1% phenolphthalein solution were added. Next, titration was performed using 0.1 M aqueous sodium hydroxide solution. The amount of eluted fatty acids (mmol) from each sample was calculated using the following formula. The results are shown in Table 1. Amount of eluted fatty acids (mmol) = Amount of 0.1 M aqueous sodium hydroxide solution used in titration (ml) / 10

[0041]

[0042] In Table 1, the cases where ΔE was 30 or less and the amount of eluted fatty acid was 1 mmol or less were judged as "◯", and the cases where ΔE was more than 30 or the amount of eluted was more than 1 mmol were judged as "X". As shown in Table 1, all of Examples 1 to 9 were judged as "◯", and both the suppression of photoactivity and the suppression of elution of fatty acid were achieved.

[0043] <Evaluation of Emulsion Cosmetics> Example 10 Using the surface-treated powder of Example 1, an emulsion cosmetic with a surface-treated powder concentration of 7% by mass was prepared as follows, and the viscosity, SPF, and UVAPF were evaluated. 32.9 g of the mixture of oil phase raw materials shown below was placed in a 100 mL polypropylene cup, and 4.9 g of the surface-treated powder of each Example and Comparative Example was added while stirring at 1400 rpm using a high-speed emulsifier / disperser "T.K. Robomix" manufactured by Primix Corporation. The stirring speed was then increased to 3000 rpm, and the mixture was stirred for 10 minutes. Thereafter, while continuing stirring, 32.2 g of the mixture of aqueous phase raw materials shown below was added, and the mixture was stirred at 3000 rpm for 5 minutes, thereby preparing the emulsion cosmetic of Example 10.

[0044] Comparative Example 4 An emulsified cosmetic of Comparative Example 4 was prepared in the same manner as in Example 10 using the surface-treated powder of Comparative Example 1.

[0045] The oil phase raw materials for the emulsion cosmetic were as follows: Cyclopentasiloxane 25.9 g: "KF-995" manufactured by Shin-Etsu Chemical Co., Ltd. Liquid paraffin 3.5 g: "Moresco White P-70" manufactured by MORESCO Corporation PEG-9-dimethicone 3.5 g: "KF-6019" manufactured by Shin-Etsu Chemical Co., Ltd.

[0046] The aqueous phase ingredients of the emulsion cosmetic were as follows: 22.4 g of ion-exchanged water, 9.8 g of 1,3-butylene glycol

[0047] The viscosity of the emulsion cosmetic was measured using a DV-1+ VISCOMETER (rotor No. S63, rotation speed 12 rpm) manufactured by BROOKFIELD Co., Ltd. The results are shown in Table 2.

[0048] The SPF and UVAPF of the emulsion cosmetics were measured. Each emulsion cosmetic was applied to a PMMA plate at a concentration of 1.3 mg / cm. 2 The amount of the solution was evenly applied and allowed to dry naturally at room temperature for 30 minutes. The SPF and UVAPF were measured using an SPF analyzer (Optometrics, Labsphere UV-2000S). The results are shown in Table 2.

[0049]

[0050] The emulsion cosmetic of Example 10 contains the surface-treated powder of Example 1, which suppresses the elution of fatty acids, and therefore has a relatively low viscosity and improved UVA and UVB blocking ability compared to the emulsion cosmetic of Comparative Example 4, which contains Comparative Example 1, which does not suppress the elution of fatty acids.

[0051] The embodiments and examples disclosed above should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is defined not by the above embodiments and examples but by the claims, and includes all modifications and variations within the meaning and scope equivalent to the claims.

Claims

1. A surface-treated powder comprising fine titanium dioxide particles and a fatty acid as a powder to be surface-treated, wherein the product of the average primary particle diameter (nm) of the fine titanium dioxide particles and the ratio of the mass of the fatty acid (in fatty acid equivalent) to the mass of the fine titanium dioxide particles is 1.5 or more and 3.7 or less.

2. The surface-treated powder according to claim 1, wherein the mass of the fatty acid (calculated as fatty acid) relative to the mass of the fine titanium dioxide particles is 7% or more and 16% or less.

3. A cosmetic comprising the surface-treated powder according to claim 1 or 2.

Citation Information

Patent Citations

  • Production of fine particulate titanium dioxide coating composition

    JP1999171541A

  • Titanium dioxide particles

    JP2021521077A

  • Titanium dioxide particle dispersion and cosmetics containing the same

    JP2022176754A

  • Oily dispersion and cosmetic material incorporating this oily dispersion

    WO2011007668A1

  • Dispersion

    WO2021241444A1