Contact lenses comprising hydrogel coatings and method of forming contact lenses with hydrogel coatings
The method of using PAA or PMAA with metal cations or copolymers to create a stable hydrogel coating on silicone hydrogel contact lenses addresses the hydrophobicity issues, enhancing comfort and durability while being cost-effective and compatible with existing manufacturing processes.
Patent Information
- Application Number
- PCT/US2023/028428
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2023-07-23
- Publication Date
- 2024-11-21
AI Technical Summary
Silicone hydrogel contact lenses face challenges with hydrophobicity leading to poor wettability and user discomfort, and existing surface treatments are unstable, inconsistent, and capital-intensive, making them difficult to manufacture effectively.
A method involving immersion of contact lenses in a first treatment solution containing PAA or PMAA with alcohol and water, followed by a second treatment solution with metal cations or copolymers to create a stable, non-silicone hydrogel coating that improves lubricity and hydrophilicity without requiring additional costly processes.
The method results in a durable, biocompatible, and stable hydrogel coating that enhances user comfort by improving lubricity and water break-up time, maintaining stability for the life of the contact lens without the need for elevated temperature chemical reactions, thus being cost-effective and compatible with conventional manufacturing processes.
Smart Images

Figure US2023028428_21112024_PF_FP_ABST
Abstract
Description
CONTACT LENSES COMPRISING HYDROGEL COATINGS ANDMETHOD OF FORMING CONTACT LENSES WITH HYDROGELCOATINGSFIELD OF THE DISCLOSURE
[0001] This disclosure relates to methods of forming hydrogel coatings on contact lenses, and to the contact lens made thereby.BACKGROUND
[0002] The trend of needing refractive corrections in daily life is increasing. With more and more advanced digital technologies and increasing web-produced knowledge, people’s reliance on ophthalmic devices (such as glasses and contact lenses for near- and far-sightedness) is also increasing. Contact lenses have been one of the major refractive corrective devices and have become increasingly popular due to their effectiveness, convenience, and aesthetics.
[0003] HEMA-based (PolyHydroxylethyl Methacrylate) soft contact lenses have been used for decades because of their good wettability and user’s comfort. However, more and more users experience blurred vision, excessive tearing, a scratchy feeling, and burning due to hypoxia or lack of sufficient oxygen during prolonged wearing. Silicone hydrogel (SiHy) based soft contact lenses have been popular since 1999 because the lens materials provide better oxygen permeation.
[0004] Although silicone hydrogel contact lens formulations provide better oxygen permeation, they render the lenses more hydrophobic or having poor wettability due to the hydrophobicity nature of silicone moi eties, which directly affects the user’s comfort. In order to overcome the hydrophobic nature of the silicone moieties or to render the surface of SiHy contact lens wettable, varies surface treatment technologies have been introduced since the market introduction of the silicone-based contact lenses in 1999. These technologies include plasma coating, mold coating with hydrophilic polymer, and surface coating of SiHy contact lenses. The main challenges of the SiHy surface treatment are their stability, consistency, robustness, and biocompatibility. Thedurability of the coating for the entire life time of the contact lenses is extremely challenging. The coating of the contact lenses loses its properties over the product’s shelf life. Moreover, contact lens manufacturing demands automation for mass production, and any additional manufacturing processes or alterations to accommodate surface treatments of the contact lens become capital intensive.
[0005] An improved contact lens and method of its manufacture is needed to reduce one or more issues associated with existing contact lenses and methods of their manufacture.SUMMARY
[0006] In one embodiment, a method of coating a contact lens is disclosed. In one step, a contact lens is immersed in a first treatment solution comprising: (1) PAA or PMAA; and (2) alcohol, water, or a mixture of the alcohol and the water. In a second step, the contact lens is immersed in a second treatment solution to create the coating on the contact lens. The second treatment solution comprises an aqueous solution of: (1) only metal cations; or (2) metal cations and copolymers.
[0007] In another embodiment, a contact lens comprises a coating. The coating comprises: PAA or PMAA. The coating further comprises: (1) only metal cations; or (2) metal cations and copolymers.
[0008] The scope of the present disclosure is defined solely by the appended claims and is not affected by the statements within this summary.BRIEF DESCRIPTION OF THE DRAWINGS
[0009] The disclosure can be better understood with reference to the following drawings and description. The components in the figures are not necessarily to scale, emphasis instead being placed upon illustrating the principles of the disclosure.
[0010] Figure 1 is a flowchart illustrating one embodiment of a method of forming a contact lens.
[0011] Figure 2 is a flowchart illustrating one embodiment of a method of coating a contact lens.
[0012] Figure 3 illustrates one embodiment of the chemical makeup of PAA.
[0013] Figure 4 illustrates one embodiment of the chemical makeup of the copolymers.
[0014] Figure 5 is a side-view of one embodiment of a contact lens made following the methods of Figures 1-2.
[0015] Figure 6 shows the chemistry of one embodiment of a coating of / on a surface of the contact lens of Figure 5.
[0016] Figure 7 illustrates one embodiment of a table showing weight percentages of various monomers in contact lens A.
[0017] Figure 8 illustrates one embodiment of a table showing weight percentages of various monomers in contact lens B.
[0018] Figure 9 illustrates a table showing testing results on contact lens A, made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data A-D) versus control contact lens (data E) with no treatment solution applied. The testing results show lubricity CCOF (critical coefficient of friction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. The PAA has a Mv (viscosity average molecular weight) of 450,000.
[0019] Figure 10 illustrates a table showing testing results on contact lens A, made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data F-J). The testing results show lubricity CCOF (critical coefficient of friction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. The PAA has a Mv (viscosity average molecular weight) of 450,000.
[0020] Figure 11 illustrates a table showing testing results on contact lens A, made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data K-M). The testing results show lubricity CCOF (critical coefficient of friction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. The PAA has a Mv (viscosity average molecular weight) of 450,000.
[0021] Figure 12 illustrates a table showing testing results on contact lens A, made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data N-O). The testing results show lubricity CCOF (critical coefficient offriction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. The PAA has a Mv (viscosity average molecular weight) of 450,000.
[0022] Figure 13 illustrates a table showing testing results on contact lens A, made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data P-Q). The testing results show lubricity CCOF (critical coefficient of friction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. The PAA has a Mv (viscosity average molecular weight) of 450,000.
[0023] Figure 14 illustrates a table showing testing results on contact lens B made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data R-S) versus control contact lens (data T) with no treatment solution applied. The testing results show lubricity CCOF (critical coefficient of friction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. The PAA has a Mv (viscosity average molecular weight) of 450,000.
[0024] Figure 15 illustrates a table showing testing results on contact lens A, made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data U-V). The testing results show lubricity CCOF (critical coefficient of friction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. The PAA has a Mv (viscosity average molecular weight) of 450,000.DETAILED DESCRIPTION
[0025] Figure 1 is a flowchart illustrating one embodiment of a method 10 of forming a contact lens. The contact lens may comprise a soft, silicone contact lens.
[0026] Step 12 may comprise dispensing a monomer mix in between male and female portions of a mold. The monomer mix may comprise varying materials.
[0027] In one embodiment, the monomer mix may comprise TRIS, 3- Methacryloyloxypropyltris-(Trimethylsilyloxy) Silane, CAS# 17096-07-0, purchased from Gelest Inc (CAT# SIM6487.6). In another embodiment, the monomer mix maycomprise mPDMS 700, Mono-Methacryloxypropyl Terminated Polydimethylsiloxane, CAS# 146632-07-7, purchased from Gelest Inc (Cat# MCS-M07). In still another embodiment, the monomer mix may comprise SIGMA, (3 -Methacryloxy -2- hydroxypropoxypropyl) Methyl Bis (Trimethylsiloxy) Silane, CAS# 69861-02-5, purchased from Gelest Inc (Cat# SIM6481.15). In yet another embodiment, the monomer mix may comprise HEMA, Hydroxyethyl Methacrylate, CAS# 868-77-9, purchased from Sigma Aldrich Co. In another embodiment, the monomer mix may comprise IBM, Isobornyl Methacrylate, CAS# 7534-94-3, purchased from Sigma Aldrich Co. In an additional embodiment, the monomer mix may comprise NVP, 1- Vinyl-2-Pyrrolidone, CAS# 88-12-0, purchased from Sigma Aldrich Co. In still another embodiment, the monomer mix may comprise MAA, Methacrylic Acid, CAS# 79-41-4, purchased from Sigma Aldrich Co. In yet another embodiment, the monomer mix may comprise PVP (K90), Polyvinylpyrrolidone K90, CAS# 9003-39-8, purchased from Sigma Aldrich Co. In an additional embodiment, the monomer mix may comprise EGDMA, Ethylene Glycol Dimethacrylate, CAS# 97-90-5, purchased from Sigma Aldrich Co. In an additional embodiment, the monomer mix may comprise TEGDMA, Tri ethylene Glycol Dimethacrylate, CAS# 109-16-0, purchased from Sigma Aldrich Co. In yet another embodiment, the monomer mix may comprise DMA, N,N- Dimethylacrylamide, CAS# 2680-03-7, purchased from Sigma Aldrich Co. In another embodiment, the monomer mix may comprise AIBN (thermal initiator), Azobisisobutyronitrile, CAS# 78-67-1, purchased from Sigma Aldrich Co. In still another embodiment, the monomer mix may comprise nPA (n-propanol or 1 -propanol), CAS# 71-23-8, purchased from Sigma Aldrich Co. In yet another embodiment, the monomer mix may comprise D30 (3,7-dimethyl-3-octanol), CAS# 106-21-8, purchased from Sigma Aldrich Co. In an additional embodiment, the monomer mix may comprise ME, 2-Mercaptoethanol, CAS# 60-24-2, purchased from Sigma Aldrich Co. In yet another embodiment, the monomer mix may comprise PEGMA, Poly(Ethylene Glycol Methacrylate), CAS# 25736-86-1, Mn 360, purchased from Sigma Aldrich Co. In an additional embodiment, the monomer mix may comprise IrgaCure 819, Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, CAS# 162881-26-7, purchased from Sigma Aldrich Co. In other embodiments, the monomer mix may vary.
[0028] In one embodiment, the mold may be manufactured using injection molding to form male and female mating portions of the mold. The mold may be made from a variety of materials such as homo-polymers or copolymers including Polypropylene, Ethylene vinyl alcohol, Polybutylene Terephthalate, Polystyrene, and Nylon. The mold may be dimensionally stable within two hours after manufacture for shrinkage consistency. Nucleating agents may be used to speed up the molding process. In other embodiments, the mold may be manufactured using varying materials, systems, and methods.
[0029] Step 14 may comprise closing the male and female portions of the mold with the monomer mix disposed within the mold. Step 16 may comprise curing the monomer mix in the closed male and female portions of the mold. The curing may utilize thermal energy, radiation, or other type of curing process. In step 18, the male and female portions of the mold may be separated (i.e. demolded) to open the mold. In step 20, a contact lens formed within the male and female portions of the mold may be removed from the mold. This may occur by mechanical dry delensing, by using a solution to float the contact lens off the mold, or through another removal process.
[0030] Figure 2 is a flowchart illustrating one embodiment of a method 30 of coating a contact lens. The contact lens may have been formed using the method of Figure 1. In other embodiments, the contact lens may have been formed using varying methods. The contact lens may be a soft, silicone contact lens. In other embodiments, the contact lens may vary. In step 32, the contact lens may be immersed in a first treatment solution. In one embodiment, the contact lens may be immersed in the first treatment solution from 1 minute to 60 minutes. Preferably, the contact lens is immersed in the first treatment solution from 5 minutes to 30 minutes. The immersion temperature, and / or the temperature of the first treatment solution may be from 5°C to 65°C. Preferably the immersion temperature, and / or the temperature of the first treatment solution is from room temperature to 45°C. In other embodiments, the time the contact lens is immersed in the first treatment solution, and the immersion temperature and / or the temperature of the first treatment solution may vary. If the solution float-off was used for the delensing step, the delensing step and the immersion in the first treatment solution may be combined into a single step.
[0031] In one embodiment, the first treatment solution may contain PAA (Poly Acrylic Acid, CAS# 9003-01-4) and alcohol, water, or a mixture of the water and the alcohol. The PAA may be purchased from Sigma Aldrich Co. Figure 3 illustrates one embodiment of the chemical makeup of PAA. In other embodiments, the PAA may vary. In another embodiment, the first treatment solution may contain PMAA (Polymethacrylic Acid, CAS# 25086-62-8) and alcohol, water, or a mixture of the water and the alcohol. The PMAA may be purchased from Sigma Aldrich Co. The first treatment solution may comprise a molecular weight ranging from 100,000 to 4,000,000. Preferably the molecular weight ranges from 400,000 to 1,500,000. The PAA solution was made by dissolving PAA in a water / alcohol mixture having a concentration ranging from .01% to 5%. Preferably, it has a concentration ranging from .05% to 2%. The PAA solution may have a pH ranging from 1 to 6. Preferably, the PAA solution has a pH ranging from 2 to 4. The alcohol may comprise IPA (isopropanol), nPA (n-propanol), ethanol, or other swelling solvents , such as, propylene glycol monomethyl ether that can swell the contact lens. The alcohol concentration may range from 0% to 100%. The alcohol concentration preferably ranges from 20% to 60%. The first treatment solution may achieve the effects of surface modification without heat or autoclave. In other embodiments, the first treatment solution may vary.
[0032] In step 34, the contact lens may be rinsed with water. In other embodiments, the contact lens may be rinsed with varying solutions.
[0033] In step 36, the contact lens may be immersed in a second treatment solution to create the coating on the contact lens. In one embodiment, the second treatment solution may comprise an aqueous solution comprising only metal cations. In another embodiment, the second treatment solution may comprise an aqueous solution comprising metal cations and copolymers. In yet another embodiment, the second treatment solution may vary. The contact lens may be immersed in the second treatment solution for 1 minute to 60 minutes. Preferably the contact lens is immersed in the second treatment solution from 5 minutes to 15 minutes. The immersion temperature of the second treatment solution may be at a temperature of from 5°C to 65°C. Preferably the immersion temperature of the second treatment solution is at atemperature from room temperature to 45°C. In other embodiments, the contact lens may be immersed in the second treatment solution for varying amounts of time, and the immersion temperature and / or the second treatment solution may be at varying temperatures.
[0034] In one embodiment, the metal cations may comprise Cationic salt such as CaCh. In another embodiment, the metal cations may comprise a metal ionic salt comprising a water-soluble chemical containing any of the following cations: Ca2+, Mg2+, Ba2+, Zn2+, Fe3+, Ag+, or varying cations. The metal cations may comprise a concentration ranging from .01% to 10%. Preferably, the metal cations may comprise a concentration ranging from .01% to 5%. Most preferably, the metal cations may comprise a concentration ranging from .01% to 2%. In other embodiments, the metal cations may vary.
[0035] The copolymers may have a concentration ranging from 0.01% to 10%. Preferably, the copolymers have a concentration ranging from .01% to 5%. Most preferably the copolymers have a concentration ranging from .01% to 2%.
[0036] In one embodiment, the copolymers may comprise an acid comprising copolymers of Acrylamide and Acrylic Acid such as Poly(Acrylamide-co-Acrylic Acid) (80% / 20%) i.e. Poly AAm-co-AA, purchased from Sigma Aldrich, CAS# 62649- 23-4, having a molecular weight of 520,000. Figure 4 illustrates one embodiment of the chemical makeup of the copolymers. In other embodiments, the copolymers may vary. In another embodiment, the copolymers may comprise an acid comprising copolymers of Poly(Acrylamide-co- Acrylic Acid) (95% / 5%) made from a mixture of 9.5 grams of Acrylamide, 0.5 grams of Acrylic Acid, and .5 grams of AIBN in 90 milliliter (ml) of water. The mixture may be cured at 100°C under Nitrogen for 1 hour and the resultant polymer may comprise 10% in water. In still another embodiment, the copolymers may comprise an acid comprising copolymers of Poly(NVP-co-MAA) (90% / l 0%) made from a mixture of 8.9 grams of NVP, 1 gram of MAA, .05 grams of ME, and .05 grams of AIBN in 40 ml of water. The mixture may be cured at 80°C under Nitrogen for 4 hours and the resultant polymer may be 20% in water. In yet another embodiment, the copolymers may comprise an acid comprising copolymers of Poly(PEGMA-co-MAA) (90% / l 0%) made from a mixture of 8.9 grams of PEGMA, 1gram of MAA, .05 grams of ME, and 0.05 grams of AIBN in 40 ml of water. The mixture may be cured at 80°C under Nitrogen for 4 hours and the resultant polymer may be 20% in water. In still other embodiments, the copolymers may vary.
[0037] In step 38, the contact lens may be rinsed with water. In other embodiments, the contact lens may be rinsed with varying solutions.
[0038] In optional step 40, the contact lens may be immersed in a third treatment solution. The third treatment solution may comprise an aqueous solution of only metal cations. In other embodiments, the third treatment solution may vary. The contact lens may be rinsed with water afterwards. In other embodiments, the contact lens may be rinsed with varying solutions afterwards.
[0039] The contact lens may be immersed in the third treatment solution for 1 minute to 60 minutes. Preferably the contact lens is immersed in the third treatment solution from 5 minutes to 15 minutes. The immersion temperature and / or the third treatment solution may be at a temperature of from 5°C to 65°C. Preferably the immersion temperature and / or the third treatment solution is at a temperature from room temperature to 45°C. In other embodiments, the contact lens may be immersed in the third treatment solution for varying amounts of time, and the immersion temperature and / or the third treatment solution may be at varying temperatures.
[0040] In one embodiment, the metal cations may contain Cationic salt such as CaCh. In another embodiment, the metal cations may comprise a metal ionic salt comprising a water-soluble chemical containing any of the following cations: Ca2+, Mg2+, Ba2+, Zn2+, Fe3+, Ag+, or varying cations. The metal cations may comprise a concentration ranging from .01% to 10%. Preferably, the metal cations may comprise a concentration ranging from .01% to 5%. Most preferably, the metal cations may comprise a concentration ranging from .01% to 2%. In other embodiments, the metal cations may vary.
[0041] In optional step 42, the contact lens may be rinsed with water. In other embodiments, the contact lens may be rinsed with varying solutions.
[0042] In step 44, the contact lens may be placed in a container with a buffer solution and the container may then be sealed. In one embodiment, the container may comprise a glass vial. In another embodiment, the container may comprise a plastic blister. Inother embodiments, the container may vary.
[0043] In one embodiment, the buffer solution may comprise PBS (Phosphate Buffer Saline). The PBS may comprise PBS Tablets purchased from RPI Research Products International. One tablet may be dissolved in 100 ml water resulting in 11.9 mM Sodium Phosphate with pH 7.4. In another embodiment, the buffer solution may comprise TBS (Tris Buffer Saline). The TBS may comprise Trizma Base (Tris(hydroxymethyl)aminomethane), CAS #77-86-1, purchased from Sigma Aldrich. The buffer saline may be prepared by mixing 6.05 grams of Trizma Base and 8.76 grams sodium chloride in 1 liter of water, followed with pH adjustment to 7.4 with IM Hydrochloric Acid (HC1). The resultant buffer solution may comprise 50 mM of Tris(hydroxymethyl)Aminomethane. In still another embodiment, the TBS may comprise TBS-NaAc (Tris Buffer-sodium acetate without Chlorine ions for Silver Nitrate treatment only). The TBS may comprise Trizma Base (Tris(hydroxymethyl)aminomethane), CAS #77-86-1, purchased from Sigma Aldrich. The buffer saline may be prepared by mixing 6.05 grams of Trizma Base and 8.76 grams sodium acetate in 1 liter of water, followed with pH adjustment to 7.4 with 1 M Acetic Acid (HAc). The resultant buffer solution may comprise 50 mM of Tris(hydroxymethyl)Aminomethane. In other embodiments, the buffer solution may vary.
[0044] In step 46, the sealed contact lens may be autoclaved. The contact lens may be autoclaved at 121°C for 40 minutes. In other embodiments, the contact lens may be autoclaved at varying temperatures for varying amounts of time. In still other embodiments, varying processes may be used on the sealed contact lens.
[0045] Figure 5 is a side-view of one embodiment of a contact lens 50 made following the methods of Figures 1-2. Figure 6 shows the coating chemistry of the ionic hydrogel formed by Ca2+crosslinking PAA and Poly (AAm-co-AA) one embodiment of a coating 52 of / on a surface 54 of the contact lens 50 of Figure 5. The coating 52 may comprise a non-silicone, stable, ionic, hydrogel coating formed on the surface 54 of the contact lens 50 as a result of following the methods of Figures 1-2. Alternatively, the non-silicone, stable, ionic, hydrogel coating 52 may comprise any of Polymethacrylic Acid (PMAA), Poly(NVP-co-MAA), Poly(PEGMA-co-MAA), 2+cationic salt such asCaCh or ZnCh, and 1+cationic salt such as AgNOs. In other embodiments, the chemistry of the non-silicone, stable, ionic, hydrogel coating 52 may vary.
[0046] The coating 52 on the contact lens 50, which may comprise a soft, silicone contact lens, may provide improved lubricity, improved hydrophilic properties, and improved water break-up time (WBUT) for the user’s comfort. The coating 52 may comprise a CCOF (Critical Coefficient of Friction) lubricity in a range of 0.02 to 0.06, may have a rubbing lubricity in a range of 3 to 5, and may have a water break-up time (WBUT) longer than 10 seconds. Because of the robust and stable metal ionic gels formed from the methods of Figures 1 and 2 on the contact lens 50, the coating 52 may form metallic ionic gels and behave as a polyelectrolytic gel. The coating 52 may comprise a non-silicone, stable, ionic, hydrogel coating formed with PAA or PMAA and multi-valent cations, such as Ca2+, Mg2+, Ba2+, Zn2+, Fe3+, and Fe2+, which may form crosslinked hydrogel networks prior to additional heating or autoclaving. A single valent cation, such as Ag+, may form an insoluble hydrogel with PAA or PMAA, and may provide anti -microbial applications for the contact lens 50. In other embodiments, various metal cations may form the insoluble hydrogel with PAA, PMAA, or other compounds. The contact lens 50, once placed in the buffer solution, may age for years without the coating 52 changing its composition.
[0047] In other embodiments, one or more steps of the method 10 may be varied in substance or order, one or more steps of the method 10 may not be followed, or one or more additional steps may be added to the method 10 in any order.
[0048] Figure 7 illustrates one embodiment of a table showing weight percentages of various monomers in contact lens A. Figure 8 illustrates one embodiment of a table showing weight percentages of various monomers in contact lens B. The contact lenses A and B comprise soft, silicone contact lenses. For contact lens A, Dk is 60 - 70 barr and the water content is 55%. The monomer mix was dispensed in the cavity of male and female contact lens molds and cured in nitrogen at 60 °C for 30 min, 80°C for 30 min, and then 100°C for 3 hours. The dry contact lenses were easily removed from the male and female molds. For contact lens B, Dk is 133 - 140 barr and the water content is 35%. The monomer mix was dispensed in the cavity of male and female contact lens molds and cured in nitrogen with radiation, such as UV light (3 mW / cm2) for 90 min.The preferred method of delensing was by the solution float-off The solution was made from 50% water and 50% Isopropyl alcohol.
[0049] Figures 9-13 and 15 illustrates tables showing testing results on contact lens A, as detailed above, made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data A-D, F-Q, and U-V) versus control contact lens (data E) with no treatment solution applied. The testing results show lubricity CCOF (critical coefficient of friction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. Figure 15 additionally illustrates results showing two years of aging of contact lens A in different buffer solutions at room temperature (about 22°C). The PAA used in Figures 9-13 and 15 has a Mv (viscosity average molecular weight) of 450,000.
[0050] Figure 14 illustrates a table showing testing results on contact lens B, as detailed above, made following the methods of Figures 1-2 using varying first, second, and third treatment solutions (data R-S) versus control contact lens (data T) with no treatment solution applied. The testing results show lubricity CCOF (critical coefficient of friction) data, lubricity (rubbing) data, WBUT wettability data, stability data, and contact lens distortion data. The PAA used in Figure 14 has a Mv (viscosity average molecular weight) of 450,000.
[0051] For Figures 9-15, CCOF lubricity data comprises the critical coefficient of friction (CCOF) based on an inclined plane method (Slide Angle, reference to ASTM D4918-97). For this lubricity data, the setup comprised a PBS buffer trough, a borosilicate glass plate situated inside the trough, and a 0.79 grams stainless steel weight. To take the measurements, the contact lenses were placed underneath a stainless-steel weight on the glass surface. The entire trough was filled with PBS buffer. The angle of the inclined glass plane was adjusted and measured with a digital inclinometer. When the slope of the glass plane exceeded a certain angle (critical angle), the stainless-steel weight together with the contact lens began to move and slide to one side of the trough. The tangent of the critical angles is the CCOF (critical coefficient of friction).
[0052] For Figures 9-15, rubbing lubricity data was taken by disposing various contacts lens on a tester’s palm and rubbing the contacts lens with the tester’s finger-tip. Theresults were measured by 0 representing very resistance, 1 representing a feel of resistance, 2 representing a slight feel of resistance, 3 representing a slight feel of slippery, 4 representing more slippery, and 5 representing very slippery.
[0053] For Figures 9-15, WBUT wettability data was taken by removing the contact lenses out of PBS solution and shaking the contact lenses of excess water. The time in seconds was observed for how long it took for the dry area to be larger than half of the lens total area. The longer the WBUT measurement the better wettability of the contact lenses. Contact lenses with very good wettability normally have WBUT measurements in excess of 15 seconds.
[0054] For Figures 9-15, the stability data was taken by triple autoclaving (3x) the contact lenses followed by examining the changes of the rubbing lubricity and diameter.
[0055] For Figures 9-15, the distortion data was taken by making observations as to whether the coatings caused the contact lenses to deform.
[0056] Referring to Figure 9, it is noted that in contact lens A it was observed that the IP A concentration in the 1sttreatment affected the lens lubricity after autoclave. The concentrations of IPA were 10% to 60%, with 30% to 50%, preferably. Other alternatives for IPA, such as nPA, propylene glycol monomethyl ether, may also be used.
[0057] Referring to Figure 10, it is noted that in contact lens A, PMAA worked equally well as PAA in the 1sttreatment. In the 2ndtreatment, the copolymers of Poly AAm- co-AA (5% AA), Poly NVP-co-MAA, and Poly PEGMA-co-MAA provided the same benefits of lubricity as Poly AAm-co-AA (20%AA) used in Figure 9. The co-polymers may have Acrylic Acid functional groups.
[0058] Referring to Figure 11, it is noted that in contact lens A, other cations such as Zinc (Zn2+) and Silver (Ag+) provided lubricity as well. However, the buffer solution used for the AgNOs (Silver Nitrate) was Tris-NaAc Buffer Saline (in the materials session), specially made to avoid silver chloride precipitation in the buffer solution.
[0059] Referring to Figure 12, it is noted that in contact lens A, the sample O had the 3rdtreatment of additional CaCE which was intended to complex any unbounded PAA in the coating.
[0060] Referring to Figure 13, it is noted that in contact lens A, sample Q had nocopolymer and still provided stable coating for the product.
[0061] Referring to Figure 14, it is noted that in contact lens B, we observed similar effects of the surface modification but with less effectiveness compared with those on contact lens A.
[0062] Referring to Figure 15, it is noted that in contact lens A after aging for 2 years at room temperature (about 22 °C), the lubricity stability of the contact lens was better maintained in TBS (Tris Buffer Saline) than PBS (Phosphate Buffer Saline).
[0063] The results of the testing shown in Figures 9-15 illustrate the unexpected, critical results of applying the methods of Figures 1-2 to manufacture contact lenses with superior lubricity, WBUT, stability, and distortion results.
[0064] One or more embodiments of the disclosure may provide an efficient, non- costly method to manufacture an effective and long-lasting, non-silicone, hydrophilic coating on a SiHy contact lens surface, prior to the autoclave step, using a procedure that is compatible with conventional contact lens manufacturing processes. The coating process can be adapted into the extraction / hydration steps of existing contact lens manufacturing processes. The methods of the disclosure may create the coating on the contact lens without the need for further chemical reactions at elevated temperatures or conventional autoclave. This may provide substantial time and cost savings during manufacture of the contact lens. Moreover, the coating on the contact lenses manufactured using these methods may be stable, consistent, robust, biocompatible, and durable for the life of the contact lens without losing its properties.
[0065] The Abstract is provided to allow the reader to quickly ascertain the nature of the technical disclosure. It is submitted with the understanding that it will not be used to interpret or limit the scope or meaning of the claims. In addition, in the foregoing Detailed Description, it can be seen that various features are grouped together in various embodiments for the purpose of streamlining the disclosure. This method of disclosure is not to be interpreted as reflecting an intention that the claimed embodiments require more features than are expressly recited in each claim. Rather, as the following claims reflect, inventive subject matter lies in less than all features of a single disclosed embodiment. Thus, the following claims are hereby incorporated into the Detailed Description, with each claim standing on its own as a separately claimed subject matter.
[0066] While particular aspects of the present subject matter described herein have been shown and described, it will be apparent to those skilled in the art that, based upon the teachings herein, changes and modifications may be made without departing from the subject matter described herein and its broader aspects and, therefore, the appended claims are to encompass within their scope all such changes and modifications as are within the true scope of the subject matter described herein. Furthermore, it is to be understood that the disclosure is defined by the appended claims. Accordingly, the disclosure is not to be restricted except in light of the appended claims and their equivalents.
Claims
CLAIMS1. A method of coating a contact lens comprising: immersing a contact lens in a first treatment solution comprising: (1) Poly Acrylic Acid (PAA) or Polymethacrylic Acid (PMAA); and (2) alcohol, water, or a mixture of the alcohol and the water; and immersing the contact lens in a second treatment solution to create the coating on the contact lens, the second treatment solution comprising an aqueous solution of: (1) only metal cations; or (2) metal cations and copolymers.
2. The method of claim 1 wherein the immersing the contact lens in the first treatment solution comprises immersing the contacts lens in the PolyAcrylic Acid (PAA) and the alcohol, the water, or the mixture of the alcohol and the water.
3. The method of claim 1 wherein the immersing the contact lens in the first treatment solution comprises immersing the contact lens in the Polymethacrylic Acid (PMAA) and the alcohol, the water, or the mixture of the alcohol and the water.
4. The method of claim 1 further comprising rinsing the contact lens in water after immersing the contact lens in the first treatment solution before the immersing the contact lens in the second treatment solution.
5. The method of claim 1 wherein the immersing the contact lens in the second treatment solution comprises immersing the contact lens in the aqueous solution of only the metal cations.
6. The method of claim 5 wherein the only metal cations comprise: Ca2+, Mg2+, Ba2+, Zn2+, Fe3+, or Ag+.
7. The method of claim 1 wherein the immersing the contact lens in the second treatment solution comprises immersing the contact lens in the aqueous solution of the metal cations and the copolymers.
8. The method of claim 7 wherein the metal cations comprise: Ca2+, Mg2+, Ba2+,Zn2+, Fe3+, or Ag+.
9. The method of claim 7 wherein the copolymers comprise an acid containing copolymers comprising: Poly(Acrylamide-co-Acrylic Acid), Poly(NVP-co-MAA), or Poly(PEGMA-co-MAA).
10. The method of claim 1 further comprising rinsing the contact lens with water after immersing the contact lens in the second treatment solution.
11. The method of claim 1 further comprising immersing the contact lens into a third treatment solution containing an aqueous solution of only the metal cations, and then rinsing the contact lens with water.
12. The method of claim 11 wherein the only metal cations comprise: Ca2+, Mg2+, Ba2+, Zn2+, Fe3+, or Ag+.
13. The method of claim 1 further comprising placing the contact lens in a container with a buffer solution, and sealing the contact lens in the container with the buffer solution.
14. The method of claim 13 wherein the buffer solution comprises PBS (Phosphate Buffer Saline) or TBS (Tris Buffer Saline).
15. The method of claim 13 further comprising autoclaving the sealed contact lens in the container with the buffer solution.
16. The method of claim 15 further comprising keeping the contact lens in the container within the buffer solution for years with the coating maintaining its properties and composition.
17. The method of claim 1 further comprising forming crosslinked hydrogel networks on the contact lens prior to autoclaving.
18. The method of claim 1 further comprising the coating comprising metallic ionic gels which behave as polyelectrolytic gels.
19. The method of claim 1 further comprising the coating modifying a surface of the contact lens.
20. The method of claim 1 further comprising the coating comprising a CCOF (critical coefficient of friction) lubricity in a range of 0.02 to 0.06.
21. The method of claim 1 further comprising the coating comprising a water breakup time longer than 10 seconds.
22. The method of claim 1 further comprising the coating comprising anti-microbial properties.
23. The method of claim 22 further comprising the coating comprising Ag+.
24. The method of claim 1 wherein the contact lens comprises a soft contact lens.
25. The method of claim 24 wherein the soft contact lens comprises a silicone contact lens.
26. A contact lens comprising: a coating comprising:(1) Poly Acrylic Acid (PAA) or Polymethacrylic Acid (PMAA); and(1) only metal cations; or (2) metal cations and copolymers.
27. The contact lens of claim 26 wherein the coating comprises the Poly Acrylic Acid (PAA).
28. The contact lens of claim 26 wherein the coating comprises the Polymethacrylic Acid (PMAA).
29. The contact lens of claim 26 wherein the coating comprises only the metal cations.
30. The contact lens of claim 29 wherein the only metal cations comprise Ca2+, Mg2+, Ba2+, Zn2+, Fe3+, or Ag+.
31. The contact lens of claim 26 wherein the coating comprises the metal cations and the copolymers.
32. The contact lens of claim 31 wherein the metal cations comprise: Ca2+, Mg2+, Ba2+, Zn2+, Fe3+, or Ag+.
33. The contact lens of claim 31 wherein the copolymers comprise: Poly(Acrylamide-co- Acrylic Acid), Poly(NVP-co-MAA), or Poly(PEGMA-co-MAA).
34. The contact lens of claim 26 wherein the coating comprises crosslinked hydrogel networks.
35. The contact lens of claim 26 wherein the coating comprises metallic ionic gels which behave as polyelectrolytic gels.
36. The contact lens of claim 26 wherein the coating comprises a CCOF (critical coefficient of friction) lubricity in a range of 0.02 to 0.06.
37. The contact lens of claim 26 wherein the coating comprises a water break-up time longer than 10 seconds.
38. The contact lens of claim 26 wherein the coating comprises anti-microbial properties.
39. The contact lens of claim 38 wherein the coating comprises Ag+.
40. The contact lens of claim 26 wherein the contact lens comprises a soft contact lens.
41. The contact lens of claim 40 wherein the soft contact lens comprises a silicone contact lens.
Citation Information
Patent Citations
Antimicrobial, preserving container for contact lens
JP2001209015A
Method for Making Medical Devices Having Antimicrobial Coatings Thereon
US20130034593A1
Silicone Hydrogel Contact Lenses Having Acceptable Levels Of Energy Loss
US20130261216A1
Contact lens with a hydrophilic layer
US20160223836A1
Silicone hydrogel lenses with water-rich surfaces
US20200017713A1