Method for obtaining lignin dispersion, lignin dispersion, use of the lignin dispersion, phenolic resin composition with lignin, and use of the phenolic resin composition with lignin
The alkaline catalysis process for lignin dispersion addresses the reactivity and compatibility issues of lignin in phenolic resin replacement, enabling its use as a sustainable adhesive with improved mechanical and processing properties, effectively replacing phenolic resins in adhesive applications for wooden substrates.
Patent Information
- Application Number
- PCT/BR2024/050205
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-20
- Publication Date
- 2024-11-28
AI Technical Summary
Current methods face challenges in replacing phenolic resins with lignin due to lignin's lower reactivity towards formaldehyde, leading to inefficiencies and compatibility issues, particularly in adhesive applications for wooden substrates, where lignin's limited cross-linking positions and higher viscosity upon solubilization hinder its full utilization.
A process involving alkaline catalysis to produce lignin dispersion, which replaces phenolic resins up to 50% with lignin, utilizing a combination of temperature and vacuum distillation to control viscosity and maintain suitable properties for adhesive applications, ensuring the lignin dispersion can be used as a sustainable substitute with improved processing ease and mechanical properties.
The process enables the production of lignin-based adhesives with properties comparable to traditional phenolic resins, reducing free formaldehyde and phenol content, while maintaining adhesive performance and applicability, thus providing a sustainable and efficient solution for bonding wooden substrates.
Smart Images

Figure BR2024050205_28112024_PF_FP_ABST
Abstract
Description
PROCESS FOR OBTAINING LIGNIN DISPERSION, LIGNIN DISPERSION, USE OF LIGNIN DISPERSION, PHENOLIC RESIN COMPOSITION WITH LIGNIN AND USE OF PHENOLIC RESIN COMPOSITION WITH LIGNIN TECHNICAL FIELD
[0001] The present invention belongs to the field of renewable materials and relates to a process for obtaining lignin dispersion, to said lignin dispersion and its respective use, to a phenolic resin composition with lignin and its respective use.
[0002] Specifically, the process of the present invention relates to the preparation of lignin dispersion, which directly replaces phenolic resins (resol) with lignin in up to 50% of the resin, while obtaining phenolic resin compositions with lignin possessing suitable physicochemical properties for application in bonding different wood substrates (e.g., plywood, MDF (medium density fiberboard), MDP (medium density particleboard), and OSB (oriented strand board)). FUNDAMENTALS OF THE INVENTION
[0003] In the current context where sustainability has gained increasing relevance, the search for high-quality materials from renewable sources has intensified, making the replacement of fossil components with natural components particularly advantageous.
[0004] In the search for renewable materials, biomass from lignocellulosic sources has always offered different alternatives, given its wide availability and variety, with its primary constituents being cellulose, hemicellulose, and lignin.
[0005] Special mention should be made of lignin, as it can be considered the most abundant aromatic macromolecule of renewable origin in nature, formed from phenylpropane units (basically by random linkages of three monolignol precursors: coniferyl alcohol (guaiacyl), p-coumaryl alcohol (hydroxyphenyl) and sinapil alcohol (syringyl)).
[0006] Lignin is generally present in the residual fractions generated as secondary flows in carbohydrate-based conversion processes, such as the pulp and paper and bioethanol industries, and is usually burned to obtain energy. Instead, lignin can be used to manufacture new high value-added products, improving the sustainability and competitiveness of these lignocellulosic transformation processes (BORRERO-LÓPEZ, 2020).
[0007] One of the most discussed applications for the use of lignin refers to its use in phenolic synthesis (KALAMI, 2018; CETIN, 2002). Specifically, its nature The phenolic nature of this material makes it a potential substitute for phenolic products, with particular emphasis in the literature on its potential for partial replacement of phenol in the synthesis of phenol-formaldehyde resins.
[0008] However, the lower reactivity of lignin towards formaldehyde has been extensively reported, caused by the greater steric hindrance of macromolecules, lower accessibility of free positions in the reactive ring compared to formaldehyde, and lower availability of reactive aromatic sites. These are some factors that must be considered in the development and limit the complete replacement of phenol by lignin. Many researchers have used different modification techniques to improve the low reactivity of lignin towards formaldehyde, such as demethylation, phenolation, and methylation (GORBHANI, 2018).
[0009] It is worth highlighting that there are other technological routes for incorporating lignin into phenolic resins. Since lignin is basically formed by aromatic macromolecules, instead of using it as a derivative of phenol synthesis, it can also be employed as a substitute for phenol-formaldehyde resins in various applications.
[0010] Phenolic resins are considered prepolymers that need to be cured during the application process to transform into thermosets with adhesive properties. This process for conversion into highly cross-linked products can be promoted without the addition of a curing agent. This is possible due to the presence of hydroxymethyl groups attached to the ring. Thus, solely through thermal action, the phenolic system initiates the characteristic curing reactions, with the temperature used varying according to the process in which the resin is being used, as well as the composition of the resol (BORGES, 2004).
[0011] In macromolecular chemistry, crosslinking refers to reactions in which a large number of individual molecules are linked to form a three-dimensional network. The linking can be achieved by direct configuration of macromolecules or by reaction to existing polymers. This can be easily measured using differential scanning calorimetry (DSC).
[0012] It is important to highlight that the chemical structure of phenolic resin varies according to the different synthesis conditions and the proportions of the reagents, and this diversity in its chemical structure determines the complexity of the phenolic resin curing process. At the same time, the diversity of phenolic resin species also leads to completely different curing reaction mechanisms (PILATO, 2010).
[0013] Thus, when lignin is mixed with a phenolic resin for substrate bonding, the curing and adhesion mechanisms of the mixture system are expected to be different from those of the resin alone.
[0014] When lignin is used as a substitute for phenolic resins, for example, as an adhesive for wood panels, the efficiency may not be the same, since lignin is a polymer with few positions to promote cross-linking, thus limiting the percentage of substitution.
[0015] In fact, the lower reactivity of lignin towards formaldehyde, as mentioned above, prevents and discourages its use as a substitute for the fossil component of phenolic resin.
[0016] Furthermore, the use of a powdered material, such as Kraft lignin, as a substitute for liquid phenolic resin, becomes a hindrance, as it causes inconvenience or impacts for the end user who is accustomed to and has infrastructure designed for liquid dispensing.
[0017] Furthermore, the known technique of solubilizing lignin in caustic soda (NaOH) as a way to make its use viable in liquid form results in a mixture with high viscosity and a lower content of active solids, so that it becomes a solid paste and not a liquid that can be added to or transported in the product.
[0018] For example, the paper by Yang, M. et al, “Preparation and properties of adhesives based on phenolic resin containing lignin micro and nanoparticles: A comparative study”, Materials and Design, 161, 55-63, 2019, reveals a complex physicochemical modification process of lignin for its use in a resin and lignin mixture in an ice bath.
[0019] The document by Wang, G. et al, “Carbohydrate elimination of alkaline-extracted lignin liquor by steam explosion and its methylolation for substitution of phenolic adhesive”, Industrial Crops and Products, 53, 93-101, 2014, describes a process for activating lignin so that it can participate in the curing process of resol, in which activation is achieved through a hydroxymethylation treatment of the lignin with formaldehyde, a toxic reagent.
[0020] However, none of the prior art documents have been able to provide a lignin solubilization process that would enable its use in phenolic resin compositions, that is, where the resulting lignin dispersion exhibits good viscosity, solids content, and residual enthalpy characteristics. These characteristics would ensure that lignin could replace resol in a phenolic resin mixture, allowing the mixture to cure and obtain a thermosetting polymer with adhesive properties.
[0021] Thus, considering that there are a number of challenges related to replacing phenolic resins with renewable materials, mainly with regard to compatibility with other components and the workability of the final product, obtaining an environmentally friendly product with suitable physical-chemical and mechanical properties to be applied as an adhesive in bonding different wood substrates or as a binder is still a challenge and a necessity in the field.
[0022] Therefore, the present invention provides a technical solution to this need through a process for obtaining lignin dispersion and its use in a phenolic resin composition with lignin for application as an adhesive on wood substrates, for example, plywood, MDF, MDP and OSB, wherein the phenolic resin compositions with lignin exhibit physicochemical and mechanical properties similar to phenolic resins without lignin.
[0023] Specifically, the present invention relates to the replacement of a petrochemical adhesive (fossil component) with a renewable and environmentally friendly material as obtained by the process of the present invention. This replacement will consequently provide the technical advantage of reducing the free formaldehyde and phenol content in the final composition of the phenolic resin material, while maintaining the applicability characteristics of phenolic resins without said replacement. SUMMARY OF THE INVENTION
[0024] The present invention discloses a process for obtaining a lignin dispersion, in which said dispersion is produced under alkaline catalysis for application in a phenolic resin composition that will be used as an adhesive on wood substrates or as a binder.
[0025] Specifically, lignin dispersion directly replaces phenolic resins with lignin.
[0026] Furthermore, the present invention also offers the advantage that the lignin dispersion already has a solids content close to that of phenolic resin, thus providing greater ease of product processing, as well as the possibility of a higher degree of lignin incorporation into the resin.
[0027] One embodiment of the invention relates to a process for obtaining a lignin dispersion comprising the following steps: a) charging the reactor with water at ambient temperature; b) adding lignin under agitation; c) adding an alkalizing agent and checking the resulting pH; d) adjusting the pH; e) Heat the mixture and allow it to react; f) Perform distillation under vacuum and temperature; g) Monitor the viscosity of the mixture.
[0028] Another embodiment of the invention describes a lignin dispersion.
[0029] In another embodiment of the invention, the use of lignin dispersion to partially replace phenolic resin (resol) with lignin in a mixture of phenolic resin with lignin is described.
[0030] In yet another embodiment of the invention, a phenolic resin composition with lignin is described, possessing suitable viscosity, solids content, and residual enthalpy characteristics for application in bonding different wood substrates (e.g., plywood, MDF, MDP, and OSB).
[0031] In another embodiment of the invention, the use of a phenolic resin composition with lignin as an adhesive or binder is described. BRIEF DESCRIPTION OF THE FIGURES
[0032] To aid in identifying the main features of the present invention, some figures are presented, to which reference is made, as follows:
[0033] FIG. 1 illustrates a graph tracking the viscosity of the acid lignin dispersion after its production over a period of 30 days.
[0034] Figures 2 and 3 illustrate graphs monitoring the viscosity of phenolic resin mixtures with lignin dispersions produced in different ways, as a function of shelf life under ambient conditions.
[0035] FIG. 4 is a differential scanning calorimetry (DSC) analysis of samples with different levels of lignin substitution of phenolic resin compared to the reference phenolic resin, i.e., without lignin.
[0036] FIG. 5 is a comparative graph of the residual enthalpy of samples with different levels of lignin replacement of phenolic resin compared to the reference phenolic resin, in cold tests or under lignin cooking conditions.
[0037] FIG. 6 is a Fourier Transform Infrared Spectroscopy (FTIR) image of samples with different levels of Kraft lignin incorporation with commercial phenolic resin without a curing process.
[0038] FIG. 7 is a Fourier Transform Infrared Spectroscopy (FTIR) image of samples with different levels of Kraft lignin incorporation with commercial phenolic resin after a curing process at 154°C. DETAILED DESCRIPTION OF THE INVENTION
[0039] The invention relates to a process for obtaining a lignin-based adhesive dispersion for application in phenolic resin compositions, wherein the reference phenolic resin is partially replaced in said composition by lignin in a proportion of up to 50%.
[0040] The term "dispersion" should be understood as a mixture of substances, of a solid finely distributed in a liquid.
[0041] The terms “phenolic resin composition with lignin”, “phenolic resin composition with lignin dispersion”, “phenol-formaldehyde resin mixture with lignin dispersion”, “phenolic resin mixture” and “phenolic resin mixture with lignin” are interchangeable and should be understood as the product resulting from the partial replacement of phenolic resin with a lignin dispersion.
[0042] Specifically, the phenolic resin composition with lignin dispersion of the present invention is used for application as an adhesive on wood substrates or as a binder. 1 '), in which an activated lignin dispersion directly replaces phenolic resins (resol), while maintaining suitable viscosity, solids content and residual enthalpy characteristics for application in bonding different wood substrates (e.g., plywood, MDF, MDP and OSB).
[0043] Lignin is inherently less crosslinkable than resol, primarily due to the limited number of positions where molecules can link to form a three-dimensional network, thus limiting the percentage of substitution. Therefore, the Kraft pulping process yields a more reactive lignin (Kraft lignin) to be added to the lignin dispersion production process of the present invention.
[0044] Despite the known difficulty related to increasing viscosity in the process of solubilizing lignin in sodium hydroxide (NaOH), the inventors of the present invention were unexpectedly able to obtain a method that combines the application of vacuum (pressure) and temperature during the preparation of a lignin dispersion for application in a phenolic resin mixture with lignin, in which the properties of the final product are positively impacted, allowing greater flexibility in application due to viscosity control and a high solids content.
[0045] When the technical solution described in this application is used, involving a whole sequence of steps and the use of vacuum temperature, this lignin dispersion can be mixed with phenolic resin without presenting problems of increased viscosity, which would make its application unfeasible, since the increase in viscosity would transform the product into a solid paste and not a liquid that can be transported or added to the phenolic resin mixture.
[0046] In other words, the technical solution described in the present invention relates to the use of a combined strategy of temperature and distillation under reduced pressure to obtain a lignin dispersion that, by replacing the resol, allows the phenolic resin composition with lignin to be applicable as an adhesive with mechanical and physicochemical properties similar to phenolic resins without said lignin, but with the advantage of comprising a sustainable component partially replacing a fossil component.
[0047] Surprisingly, the inventors of the present invention have demonstrated that by distilling and heating the lignin dispersion, the residual enthalpy of cure decreases, which provides the technical advantage of applying the phenolic resin and lignin composition as an adhesive in bonding wood substrates.
[0048] In fact, the reduction of residual enthalpy as a consequence of the process of the present invention complements the crosslinking process (curing process) for transforming the phenolic resin mixture with lignin described herein into a thermosetting material for application as an adhesive.
[0049] In a first embodiment, a process for obtaining lignin dispersion in an aqueous and basic medium is revealed, comprising the following steps: a) charging the reactor with water at room temperature; b) adding lignin under agitation; c) adding an alkalizing agent and checking the resulting pH; d) adjusting the pH; e) heating the mixture and allowing it to react; f) performing distillation under vacuum and temperature; g) monitoring the viscosity of the mixture.
[0050] Optionally, the process for obtaining lignin dispersion also includes the following steps: h) cooling the reaction; and i) unload and sift the resulting material.
[0051] In some embodiments, the amount of water carried in step a) is in the range of 800 to 2,000 g, preferably in the range of 1,000 to 1,900 g, more preferably in the range of 1,100 to 1,800 g.
[0052] In some embodiments, the lignin from step b) is selected from the group consisting of powdered lignin, acid lignin cake, and unwashed lignin cake (alkaline lignin).
[0053] When lignin is in powder form, step b) of adding said lignin is carried out under vigorous stirring and homogenization is maintained at room temperature. Furthermore, heating is maintained in step e) to ensure complete dissolution of the lignin.
[0054] In some embodiments, the amount of lignin powder added in step b) is in the range of 800 to 1,100 g, preferably in the range of 900 to 1,000 g, more preferably 966 g.
[0055] When lignin is in the form of acid lignin cake or unwashed cake, step b) of adding said lignin is through dispersion under stirring until a homogeneous paste (“slun”) is obtained.
[0056] In some embodiments, the acid lignin cake is dispersed in step b), in an amount in the range of 1,300 to 1,700 g, preferably in the range of 1,500 to 1,600 g, more preferably 1,548 g.
[0057] In some embodiments, the acid lignin cake has a solids content in the range of 50% to 80%, preferably in the range of 55% to 65%, more preferably 59%.
[0058] In some embodiments, the agitation to obtain the homogeneous paste (“slurr”) in step b) is carried out in the range of 1 to 3 hours, preferably 2 hours.
[0059] In some embodiments, the agitation of stage b) is in the range of 250 to 450 rpm, preferably in the range of 300 to 400 rpm, more preferably 350 rpm.
[0060] In some embodiments, homogenization is carried out in the range of 20 to 60 minutes, preferably in the range of 25 to 45 minutes, and more preferably 30 minutes.
[0061] In some embodiments, the alkalizing agent added in step c) is a strong base to adjust the pH to a range of 12.5 to 13.5. Preferably, the strong base is caustic soda (NaOH). In embodiments where the addition of NaOH is not sufficient to leave the pH in the range of 13.0 + / - 0.5, the pH is adjusted to 13.5 by adding an additional amount of NaOH.
[0062] Optionally, caustic soda can also be added along with the initial water of the process.
[0063] In some embodiments, caustic soda (NaOH) is used in concentrations of 50% (50% NaOH) or 33% (33% NaOH), or in pellet form. Preferably, 50% NaOH is used.
[0064] In some embodiments, the heating of the mixture in step e) is carried out at a temperature in the range of 40 to 95 S C, preferably from 50 to 85 S C, more preferably from 55 to 80 s C. The reaction time of the mixture after heating is 1 to 3 hours, preferably 2 hours.
[0065] In some embodiments, the vacuum distillation step is carried out at a pressure in the range of 150 to 500 mmHg (2.00 x 10 4 a 6.66 x 10 4 Pa), preferably 200 mmHg (2.67 x 10 4 Pa). In turn, the temperature used in the distillation step is in the range of 60 to 95 S C, preferably in the 65 to 85 age range. S C, more preferably in the 70 to 75 range. S W.
[0066] In some embodiments, the vacuum and temperature distillation step is carried out until the viscosity of the system is in the range of 100 to 2,500 cP (0.1 to 2.5 Pa.s), preferably in the range of 400 to 1,600 cP (0.4 to 1.6 Pa.s), more preferably in the range of 700 to 1,000 cP (0.7 to 1.0 Pa.s), even more preferably 915 cP (0.915 Pa.s).
[0067] In some embodiments, the cooling stage is carried out until a temperature between 50 and 60 is reached. s W.
[0068] In some embodiments, the screening stage is carried out with a sieve with a mesh size in the range of 60 to 120 mesh. Preferably, a 66, 80 or 100 mesh sieve is used. Most preferably, a 66 mesh sieve is used.
[0069] After the process is completed, the final dispersion has a solids content in the range of 40% to 55%, preferably 45% to 48%.
[0070] A second embodiment of the invention describes a lignin dispersion obtained by the process according to the first embodiment of the invention. In a particularly preferred embodiment, the lignin dispersion comprises a solids content in the range of 45 to 50%, a pH in the range of 13.0 to 14.0, and a viscosity in the range of 900 to 1600 cP (0.9 to 1.6 Pa.s).
[0071] In a third embodiment of the invention, the use of lignin dispersion to partially replace phenolic resin (resol) with lignin in a mixture of phenolic resin with lignin is described.
[0072] A fourth embodiment of the present invention relates to a phenolic resin composition with lignin produced under alkaline catalysis according to the process of the present invention for application as an adhesive on wood substrates, wherein said lignin directly replaces phenolic resins (resol) with lignin, in up to 50% of the resin.
[0073] Optionally, the replacement of phenolic resins with lignin is in the range of up to 30% of the resin, or in the range of up to 20% of the resin.
[0074] In some embodiments, the lignin is Kraft lignin, preferably from short-fiber hardwood.
[0075] A fifth embodiment of the present invention relates to the use of the phenolic resin composition with lignin as an adhesive or binder. EXAMPLES
[0076] The following examples, described in detail, serve to illustrate embodiments of the present invention without, however, limiting the scope of protection thereof. Example 1 - Process for preparing a hot dispersion of lignin in an aqueous and basic medium.
[0077] The process consists of preparing a lignin dispersion in an aqueous and basic medium, comprising the following steps: a) loading 1.142 g of water at room temperature into the reactor; b) gradually dispersing 1.548 g of acidic lignin cake with a solids content of 59% under stirring for 2 hours, until a homogeneous slurry is obtained, which was homogenized for 30 minutes; c) adding 368 g of 50% sodium hydroxide (NaOH) and checking the resulting pH; d) adjusting the pH to 13.5 with the addition of 100 g of 50% sodium hydroxide (NaOH); e) heating the mixture to a temperature between 50 and 60 s C and allow to react for 2 hours; f) perform vacuum distillation at a pressure of 200 mmHg (2.67 x 10 4 Pa) and a temperature of 70 s C; g) monitor the process until the viscosity of the system is between 700 and 1,600 cP (0.7 to 1.6 Pa.s). Example 2 - Process for preparing a dispersion of lignin powder activated by reaction in an aqueous and alkaline medium at temperature
[0078] The process consists of preparing an alkaline dispersion of acidic lignin, comprising the following steps: a) adding 1.725 g of water at room temperature to the reactor; b) adding 966 g of lignin within two hours, with vigorous stirring at 350 rpm; c) maintaining homogenization for 30 minutes at room temperature; d) adding 367 g of 50% caustic soda (NaOH); e) measuring the pH of the solution and adjusting it with further addition of caustic soda so that the pH is between 13.0 and 13.5; f) heating the reaction to a temperature between 55 and 80°C; g) maintaining heating for complete dissolution of the lignin for 2 hours; h) applying a vacuum at 200 mmHg (2.67 x 10 4Pa) and distill the solution at a temperature between 70 and 85°C until it reaches a viscosity between 100 and 2,500 cP (0.1 to 2.5 Pa.s); i) cool the reaction to a temperature between 50 and 60°C; j) discharge and sieve the resulting material with a 66 mesh sieve; ek) perform analyses of the material.
[0079] In this example, the distillate volume from step h) was measured at a value of 600 ml.
[0080] Table 1 illustrates the components of the lignin dispersion from example 2: Table 1 - Components of lignin dispersion
[0081] Table 2 illustrates the lignin dispersion properties of example 2: Table 2 - properties of lignin dispersion
[0082] Figure 1 illustrates the monitoring of the product's viscosity after its production over a period of 30 days.
[0083] The graph in Figure 1 shows that the product of the present invention is stable over time, that is, it does not have a very short shelf life. Specifically, the graph indicates that the product can be stored and used after some time.
[0084] Furthermore, the product's viscosity does not increase exponentially, which would make the product unusable, and no precipitate formation was observed. Example 3 - Process for preparing a lignin dispersion in an aqueous and alkaline medium at a temperature
[0085] The process consists of preparing an alkaline dispersion of acidic lignin, comprising the following steps: a) adding 1.725 g of water at room temperature to the reactor; b) adding 966 g of lignin within two hours, with vigorous stirring at 350 rpm; c) maintaining homogenization for 30 minutes at room temperature; d) adding 367 g of 50% caustic soda (NaOH); e) measuring the pH of the solution and adjusting it with further addition of caustic soda so that the pH is between 13.0 and 13.5; f) heating the reaction to a temperature between 55 and 80°C; g) maintaining heating for complete dissolution of the lignin for 2 hours; h) applying a vacuum at 200 mmHg (2.67 x 10 4 Pa) and distill the solution at a temperature between 70 and 85°C until it reaches a viscosity between 50 and 1,000 cP (0.05 to 1.0 Pa.s); i) cool the reaction to a temperature between 50 and 60°C; j) discharge and sieve the resulting material with a 66 mesh sieve; ek) perform analyses of the material.
[0086] In this example, the distillate volume from step h) was measured at a value of 300 ml.
[0087] Table 3 illustrates the components of the lignin dispersion from example 3: Table 3 - Components of lignin dispersion
[0088] Table 4 illustrates the lignin dispersion properties of example 3: Table 4 - Properties of lignin dispersion
[0089] In other words, from the same quantity of raw materials, two distinct specifications of modified lignin dispersion were produced by the process described. Example 4 - Process for preparing a lignin dispersion using lignin cake activated by reaction in an alkaline medium at temperature
[0090] The process consists of preparing an alkaline dispersion of acidic lignin, comprising the following steps: a) adding 1.725 g of water at room temperature to the reactor; b) adding 966 g of acidic lignin cake within two hours, with vigorous stirring at 350 rpm; c) maintaining homogenization for 30 minutes at room temperature; d) adding 367 g of 50% caustic soda (NaOH); e) measuring the pH of the solution and adjusting it with further addition of caustic soda so that the pH is between 13.0 and 13.5; f) heating the reaction to a temperature between 55 and 80°C; g) maintaining heating for complete dissolution of the lignin for 2 hours; h) applying a vacuum at 200 mmHg (2.67 x 10 4 Pa) and distill the solution at a temperature between 70 and 85°C until it reaches a viscosity between 400 and 1,600 cP (0.4 to 1.6 Pa.s); i) cool the reaction to a temperature between 50 and 60°C; j) discharge and sieve the resulting material with a 66 mesh sieve; ek) perform analyses of the material.
[0091] Table 5 indicates the properties of the acid lignin cake from example 4: Table 5 - Properties of acid lignin cake
[0092] Table 6 illustrates the components of the acid lignin cake dispersion from example 4: Table 6 - Components of acid lignin cake dispersion
[0093] Table 7 illustrates the properties of the acid lignin cake dispersion from example 4: Table 7 - Properties of the acid lignin cake dispersion Example 5 - Partial replacement of the reference phenolic resin with lignin dispersion according to Example 2
[0094] For the partial replacement of the reference phenolic resin with lignin dispersion, a phenol-formaldehyde resin (reference resin) with the following properties indicated in Table 8 was used. Table 8 - Properties of phenol-formaldehyde resin
[0095] Specifically, the following lignin replacement levels were used for the resin: 7.5%, 10%, and 20% as a replacement for active solids.
[0096] The results for the properties of the reference resin and the resins taking into account the solids replacement levels are shown in Table 9 below. Table 9 - Properties of the reference resin and resins with lignin substitution.
[0097] With the increasing replacement of lignin adhesive with phenolic resin, it is possible to observe some differences compared to the reference resin, such as an increase in pH, a decrease in solids content, and an increase in gel time. Example 6 - Phenol-formaldehyde resin mixture with lignin dispersion
[0098] In order to prove that two materials can replace phenol-formaldehyde resins, of the Resol type, mixtures were prepared by replacing phenolic resin with lignin in the following proportions: 10, 20, 30, 40 and 50% (mass of active solid, i.e., dry base resin by lignin dispersion, also in dry mass).
[0099] The shelf life of the resin and lignin mixture was monitored over time with periodic viscosity measurements.
[0100] Figure 2 illustrates the evolution of the viscosity of the phenolic resin mixture with lignin dispersion produced in example 2 as a function of shelf life under ambient conditions.
[0101] The results for the properties of the phenolic resin mixture with lignin dispersion produced in example 2 are shown in Table 10 below: Table 10 - Properties of the phenol-formaldehyde resin mixture with lignin produced according to example 2.
[0102] Figure 3 illustrates the evolution of the viscosity of the phenolic resin mixture with lignin dispersion produced in example 3 as a function of shelf life under ambient conditions.
[0103] The results of the properties of the phenolic resin mixture with lignin dispersion produced in example 3 are shown in Table 11 below: Table 11 - Properties of the phenol-formaldehyde resin mixture with lignin produced according to example 3
[0104] The most important parameters for applying a resin are viscosity and gel time. In order to verify the stability of the resulting product, the material produced in examples 2 and 3 was subjected to aging under ambient conditions, and these parameters were analyzed 40 and 70 days after its production, as shown in Table 12: Table 12 - Gel time measured in minutes of phenol-formaldehyde resin mixtures with lignin according to examples 2 and 3 as a function of aging time under ambient conditions.
[0105] According to the National Wood Quality Program (PNQM), established by the Brazilian Association of Mechanically Processed Wood Industry, the curing time of a phenolic adhesive should be between 6 and 12 minutes using the methodology employed in this document. Therefore, even after 70 days, despite the reduction in gel time, the material is still within the specification for phenolic resin application.
[0106] This change in gel time is expected and results from condensation reactions of the phenol-formaldehyde resin with lignin that occur as a function of production time.
[0107] Phenolic resins of the resol type applied to wood panels can have a gel time of 6 to 11 minutes. Therefore, the results obtained by replacing resin with lignin are within the desired application range for this material. Table 13 - Brookfield viscosity measured in centipoise (cP) of phenol-formaldehyde resin mixtures with lignin dispersion according to examples 2 and 3 as a function of aging time under ambient conditions.
[0108] The viscosity of the mixtures shows a tendency to increase, which also occurs with phenol-formaldehyde resin as the aging time increases.
[0109] Based on the data reported in Table 13, the mixtures are still suitable for application up to 40 days, as they have a plausible viscosity.
[0110] It has been observed that phenol-formaldehyde resin formulations with partial substitution by a lignin-containing dispersion meet the gel time and viscosity requirements adopted by most users of phenolic resin for the manufacture of plywood. [01 1 1] The process allows the generation of distinct products with different behaviors regarding the viscosity of the mixture, since the product generated in example 3 forms mixtures with lower viscosities than the product generated in example 2, even at the highest lignin substitution levels. In turn, the solids contents of the mixture in example 2 and the mixture in example 3 are similar.
[0112] Specifically, the resins were applied in the production of phenolic plywood panels composed of 5 industrial veneers of Pinus spp., with dimensions of 500 mm x 500 mm x 3.0 mm (length, width, and thickness, respectively), generating a panel with a nominal thickness of 15 mm. In the formulation, in addition to the resin, an extender (common wheat flour) and water were used, generating a glue mix with a solids content of around 30%.
[0113] According to the National Wood Quality Program (PNQM), a newly produced resin should have a viscosity of approximately 400 to 800 cP (0.4 to 0.8 Pa.s).
[0114] This adjustment ensures that the amount of resin applied is the same, since the samples have different solids contents. The parameters used for panel production are listed in Table 14 below. Table 14 - Parameters used for the production of phenolic plywood panels
[0115] To evaluate the mechanical properties, 12.5% resin by mass was applied, relative to the mass of the pine veneer.
[0116] After pressing, the panels were stored until stabilization. Following conditioning, test specimens were prepared to evaluate the bonding quality by measuring the shear strength of the glue line, according to European standards (CEN - European Committee for Standardization). - EN 314-1 (2004) - Plywood- Bonding quality- Test methods - EN 314-2 (2002) - Plywood- Bonding quality- Requirements
[0117] The pre-treatments performed on the test specimens for the different treatments were: Dry (air-conditioned); - Immersion in cold water for 24 hours (20±3°C); - Boiling for 6 hours (Boil for 6 hours and cool for 1 hour in water at 20±3°C); and - Boiling cycle (4 hours of boiling; 16-20 hours of drying at 60±3°C; 4 hours of boiling; cooling for 1 hour in water at 20±3°C).
[0118] After the pretreatments, the shear strength of the glue line was determined as requested by the methodology for each of the samples (reference resin and resins with lignin at 7.5%, 10% and 20%). The average results are detailed in Table 15 below. Table 15 - Shear stress results in wood panels under different test conditions (dry, cold water and boiling cycle)
[0119] The results obtained were subjected to statistical analysis, using tests for: outliers, homogeneity of variances, analysis of variance, and Tukey's comparison of means, at a 95% confidence level.
[0120] Based on the results, it can be seen that the levels of substitution of phenolic resin by alkaline lignin dispersion show the same bonding quality as the reference resin in the different treatments to which they were subjected.
[0121] In the boiling cycle test, it is important to note that, when compared to the reference resin, the average values of the resins with lignin are equal to and greater than 1 MPa. Therefore, the wood panel with different levels of lignin-based adhesive is approved according to the EN 314-2 standard assessments. Example 7 - Evaluation of the residual cure of a mixture of phenolic resin with lignin dispersions
[0122] Starting from lignin powder, two alkaline mixtures were prepared, one made solely from dissolving lignin in 50% water / soda (solids content = 43.5%) and the other following the procedure described in the present invention (solids content = 47%).
[0123] Mixtures of a phenol-formaldehyde resin for wood gluing were prepared, with the resin being replaced by lignin dispersions in increasing percentages (5-20%).
[0124] The resin / lignin mixtures were cured, that is, subjected to heat to transform them into a thermosetting polymer (thermosetting resin) on a sheet at 154 S C, similarly to the ASTM D4040-6 standard, defining the time (expressed in seconds) required for the resin to... When held under a hot surface (at a specific temperature) and moved with a spatula, it polymerizes and adheres to the surface rather than the sheet metal.
[0125] After the curing process, the mixtures were subjected to differential scanning calorimetry (DSC) analysis to check if all the material had cured. This can be seen in the endothermic peak in the thermogram illustrated in Figure 4.
[0126] The results obtained, which are summarized in Figure 4, demonstrate that after the material curing process, the mixtures with varying levels of resin replacement by Kraft lignin adhesive maintain properties similar to the reference resin and, therefore, do not impact the curing process of a resin without lignin.
[0127] Figure 5 illustrates the results for the residual enthalpy analysis in J / g of a lignin-free phenol-formaldehyde resin and of resin mixtures with replacement of said resin with lignin dispersions in increasing amounts (from 5 to 20%) in cold and baked tests.
[0128] Analyzing the residual enthalpy values illustrated in Figure 5, it can be seen that at the temperature used for curing, the reference phenolic resin (i.e., without lignin) did not fully cure, exhibiting a residual enthalpy of 269 J / g.
[0129] However, when the resin is replaced by a cold-dispersed lignin dispersion in an alkaline medium, the residual enthalpy is higher, that is, the mixture cured less than the reference resin during the heating process on the sheet, so the resulting material is more difficult to crosslink.
[0130] In turn, when the process described in this patent application is carried out, that is, replacing resin with a lignin dispersion dispersed under cooking in an alkaline medium, it is found that the residual enthalpy is in the same range of values as the reference resin, even when 20% of the resin has been replaced by the lignin dispersion.
[0131] Thus, the conclusion obtained from this experiment is that the process developed in this patent application is capable of replacing phenol-formaldehyde resin without interfering with the curing process for use as a component of thermosetting resin, which can lead to better adhesion of the material, since this characteristic is also linked to the degree of crosslinking. Example 8 - Evaluation of Fourier Transform Infrared Spectroscopy (FTIR spectra) of the incorporation of lignin adhesive with commercial phenolic resin with different resin substitution levels without a curing process.
[0132] Figure 6 illustrates the FTIR spectra of the reference phenolic resin samples without lignin and of the resin mixtures with lignin at levels of 7.5%, 10%, and 20% resin replacement, but without performing a curing process.
[0133] When comparing the infrared spectra of the reference resin and the resins in which lignin has been incorporated, it is noted that the spectra basically overlap, so that no distinct bands are observed with the incorporation of the new component. This indicates that the product has no structural differences and has similarities to the resins up to a percentage of 20% resin substitution by lignin.
[0134] Specifically, the IR spectrum of the resin in its initial state has the most intense band. The maximum is recorded at a wavelength close to 3400 cm⁻¹. -1 . Example 9 - Evaluation of Fourier Transform Infrared Spectroscopy (FTIR spectra) of the incorporation of lignin adhesive with commercial phenolic resin with different resin substitution levels after a curing process at 154°C. Q W
[0135] Figure 7 illustrates the FTIR spectra of the lignin-free reference phenolic resin samples and of the resin mixtures with lignin at resin replacement levels of 7.5%, 10%, and 20%, but with a curing process performed at 154°C. S W.
[0136] After the material curing process, the infrared spectrum profiles are still very similar, demonstrating, therefore, that replacing the reference resin with lignin does not affect the curing process, the molecular structure, and the adhesive capacity of the thermoset product.
[0137] Thus, it can be observed that the 3400 cm band -1 It is drastically reduced in all cases in Figure 7, showing similar cures.
[0138] It is understood that when a range of parameters is provided, all integers and ranges within that range, and tenths and hundredths, are also provided by the modes. For example, “5-10%” includes 5%, 6%, 7%, 8%, 9%, and 10%; 5.0%, 5.1%, 5.2%, 9.8%, 9.9%, and 10.0%; and 5.00%, 5.01%, 5.02%, 9.98%, 9.99%, and 10.00%, as well as, for example, 6-9%, 5.1%-9.9%, and 5.01%-9.99%. Similarly, when a list is presented, unless otherwise indicated, it should be understood that each individual element of that list and each combination of components of that list is a separate mode. For example, “1, 2, 3, 4 and 5” encompasses, among numerous variations, 1; 2; 3; 1 and 2; 3 and 5; 1, 3 and 5; and 1, 2, 4 and 5.
[0139] It should be understood that the embodiments described above are merely illustrative and that various modifications may be made to them by a person skilled in the art without departing from the scope of the present invention. Consequently, the present invention should not be considered limited to the exemplary embodiments described in this application. Furthermore, the present disclosure may include matter not claimed at present, but which may be claimed in the future in combination with or separately from the features claimed herein. References: - Antonio M. Borrero-López, Raquel Martín-Sampedro, David Ibarra, Concepcion Valencia, Maria E. Eugenio, José M. Franco, “Evaluation of lignin-enriched side-streams from different biomass conversion processes as thickeners in bio-lubricant formulations”, International Journal of Biological Macromolecules, Volume 162, 2020, páginas 1398-1413, ISSN 0141 -8130, https: / / doi.Org / 10.1016 / j.ijbiomac.2020.07.292. - Kalami, S.; Chen, N.; Borazjani, H.; Nejad, M., “Comparative Analysis of Different Lignins as Phenol Replacement in Phenolic Adhesive Formulations”, Ind. Crop. Prod. 125, 520-528, 2018. - Cetin, N.S.; Ozmen, N., “Use of Organosolv Lignin in Phenol-Formaldehyde Resins for Particleboard Production — I. Organosolv Lignin Modified Resins”, Int. J. Adhes. Adhes. 22, 477- 480, 2002. - Ghorbani, M.; Mahendran, A.; Hendrikus van Herwijnen, W.; Liebner, F., “ Paper-based laminates produced with kraft lignin- rich phenolformaldehyde resoles meet requirements for outdoor usage", European Journal of Wood and Wood Products 76:481-487, 2018. - Borges, SG, “Synthesis and characterization of novolac-type liquid phenolic resins applicable in the pultrusion process”, Master's thesis, Federal University of Rio Grande do Sul - UFRGS. - Pilato L, “Resin chemistr , In: Pilato L (ed) Phenolic Resins: A Century of Progress [M], Berlin, Heidelberg: Springer-Verlag; 2010, pp. 41-91. - Lee, Y., Kim, H., Rafailovich, M., Sokolov, J., “Curing monitoring of phenolic resol resins via atomic force microscope and contact angle”, International Journal of Adhesion and Adhesives, Volume 22, Issue 5, 2002, pages 375-384, ISSN 0143-7496.
Claims
CLAIMS 1. Process for obtaining lignin dispersion characterized by the fact that it comprises the following steps: a) load water at room temperature into the reactor; b) add lignin under stirring; c) add an alkalizing agent and check the resulting pH; d) adjust the pH; e) heat the mixture and let it react; f) perform distillation under vacuum and at temperature; eg) monitor the viscosity of the mixture.
2. Process according to claim 1, characterized in that it further comprises the following steps: h) cooling the reaction; and i) discharging and screening the resulting material.
3. Process according to claim 1 or 2, characterized in that the lignin of step b) is selected from the group consisting of powdered lignin, acidic lignin cake and unwashed lignin cake (alkaline lignin).
4. Process according to claim 3, characterized in that: a) when the lignin is in the form of powdered lignin, step b) of adding said lignin is under vigorous stirring and homogenization is maintained at room temperature; or b) when the lignin is in the form of acid lignin cake or unwashed cake, step b) of adding said lignin is through dispersion under stirring until a homogeneous paste (“slurry”) is obtained.
5. Process according to claim 3, characterized in that: a) when the lignin is in the form of powdered lignin, the heating of step e) is maintained for complete dissolution of the lignin.
6. Process according to any one of claims 1 to 5, characterized in that the lignin is Kraft lignin, preferably from short fiber woods (“hardwood”).
7. Process according to any one of claims 1 to 6, characterized in that the alkalizing agent is a strong base, preferably sodium hydroxide (NaOH).
8. Lignin dispersion characterized by the fact that it is obtained by the process as defined in any one of claims 1 to 7.
9. Lignin dispersion characterized by the fact that it comprises a solids content in the range of 45 to 50%, pH in the range of 13.0 to 14.0 and viscosity in the range of 100 to 2,500 cP (from 0.1 to 2.5 Pa.s).
10. Lignin dispersion according to claim 9, characterized in that the viscosity is in the range of 400 to 2,000 cP (0.4 to 2.0 Pa.s), preferably in the range of 900 to 1,600 cP (0.9 to 1.6 Pa.s).
11. Use of the lignin dispersion as defined in any one of claims 8 to 10 characterized in that it is to partially replace phenolic resin (resole) with lignin in a mixture of phenolic resin with lignin.
12. Composition of phenolic resin with lignin characterized by the fact that said lignin partially replaces phenolic resin (resole) with lignin dispersion.
13. Phenolic resin composition with lignin according to claim 12, characterized in that the lignin replaces phenolic resin in the range of up to 50% of the resin.
14. Phenolic resin composition with lignin according to claim 12 or 13, characterized in that it presents suitable physical-chemical properties to be applied as an adhesive in the bonding of different wooden substrates or as a binder.
15. Phenolic resin composition with lignin according to claim 14, characterized in that the wood substrate is selected from the group consisting of plywood, MDF (medium density fiberboard), MDP (medium density particleboard) and OSB (oriented strand board).
16. Phenolic resin composition with lignin according to claim 14 or 15, characterized in that the physicochemical properties are selected from the group consisting of viscosity, solids content and residual enthalpy.
17. Use of the phenolic resin composition with lignin as defined in any one of claims 12 to 16 characterized in that it is as an adhesive or binder.
Citation Information
Patent Citations
Method for production of lignin
US20150119560A1
High solids, low viscosity lignin solutions
US4306999A
Reactive phenolic resin modifier
US5866642A
A method for increasing the reactivity of lignin
WO2013144454A1
Aqueous lignin dispersions and methods of preparing the same
WO2019081819A1