Cerium-doped bismuth germanate single crystal scintillator, preparation method therefor, and use thereof

By doping cerium elements into bismuth germanate to form Bi4Ge3O12:Ce single crystal scintillator, the problems of light output saturation, radiation damage and long attenuation time of bismuth germanate are solved, and higher radiation resistance and Time response rate, suitable for applications in fields such as high energy physics.

WO2024239393A1PCT designated stage expired Publication Date: 2024-11-28SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/100382
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2023-06-15
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Bismuth germanate scintillator has problems with light output saturation, radiation damage and long attenuation time in high-energy physics and large scientific devices, limiting its ability to detect and perform stability in high-counting rate radiation.

Method used

By doping cerium element (Ce) into bismuth germanate, Bi4Ge3O12:Ce single crystal scintillator is formed, which reduces light output, improves radiation resistance, and shortens attenuation time. The crucible drop method, lifting method, and bubble generation method are used to use the crucible drop method, lifting method, and bubble generation method Preparation by single crystal growth method.

Benefits of technology

It significantly reduces the light output of bismuth germanate scintillator, improves its radiation resistance and time response rate, and meets the higher requirements for material light output, radiation resistance and time response characteristics in the fields of high-energy physics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023100382_28112024_PF_FP_ABST
    Figure CN2023100382_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A cerium-doped bismuth germanate single crystal scintillator, a preparation method therefor, and a use thereof. The chemical formula of the cerium-doped bismuth germanate single crystal scintillator is Bi4Ge3O12:Ce, wherein the doping amount of the Ce element does not exceed 0.7 wt%.
Need to check novelty before this filing date? Find Prior Art

Description

A cerium-doped bismuth germanate single crystal scintillator and its preparation method and application Technical Field

[0001] The invention relates to a cerium-doped bismuth germanate single crystal scintillator for improving the scintillation performance of bismuth germanate, a preparation method and an application thereof, and belongs to the field of scintillators for radiation detection. Background Art

[0002] Scintillators are a class of functional materials that can convert the energy of absorbed high-energy particles or radiation into ultraviolet-visible or near-infrared photons. These signals are then converted into electrical signals by photodetectors such as photomultiplier tubes (PMTs) and silicon photomultipliers (SiPMs), enabling precise detection and discrimination of the type, quantity, energy, direction, and position of incident high-energy particles or radiation. Scintillator-based scintillation detectors have been widely used in high-energy physics, medical imaging, security inspections, resource exploration, environmental monitoring, and industrial testing.

[0003] Doping is a reliable means to improve and overcome the deficiencies of existing scintillating materials. With the differentiated demand for radiation detection, while researching and developing new scintillators with better performance, people have been trying to improve the scintillation properties of existing materials with large-scale manufacturing capabilities through doping, such as calcium-cerium co-doping to shorten the decay time of lutetium silicate crystals and enhance their light output (M.A.Spurrier et al., Effects of Ca on Lutetium Silicate Crystals). 2+ Co-Doping on the Scintillation Properties of LSO: Ce, IEEE Trans. Nucl. Sci., 55(2008): 1178-1182), yttrium doping suppresses the slow scintillation component in barium fluoride scintillating crystals, which has a light output 4-5 times that of the fast scintillation component (J. Chen et al., Slow Scintillation Suppression in Yttrium Doped BaF2Crystals, IEEE Trans. Nucl. Sci. 65(2018): 2147-2151), fluorine doping improves the light output of lead tungstate scintillating crystals, and yttrium doping improves their transmittance and photoresponse uniformity (Wang Shaohua, Macroscopic defects in lead tungstate crystals and their doping effects, doctoral dissertation of Shanghai Institute of Ceramics, Chinese Academy of Sciences, 1999).

[0004] Bismuth germanate (Bi4Ge3O 12 , BGO) crystal is an inorganic scintillator with excellent comprehensive performance and high density (7.13g / cm 3 ), large effective atomic number (Z eff, 74), with outstanding advantages such as strong radiation blocking ability, high detection efficiency, moderate energy resolution, large intrinsic peak / comparison ratio, good uniformity, no luminescence self-absorption, no afterglow, stable physical and chemical properties and good machinability, it has extensive and important applications in high energy physics, astrophysics, nuclear physics, nuclear medicine imaging, geological exploration, oil well logging and industrial detection. Since the 1980s, this crystal has been mass-produced, and with the deepening of research and development, there have been continuous breakthroughs in size and performance. It is still one of the most important and largest-scale inorganic scintillators. The Circular Electron Positron Collider (CEPC) and the Future Circular Collider (FCC) are large-scale scientific facilities at the forefront of intensity. The beam intensity is significantly higher than that of existing devices such as the Large Hadron Collider (LHC), which puts higher requirements on the hardness and time response characteristics of the scintillating crystals.

[0005] Silicon photomultipliers (SiPMs) are a new type of highly sensitive semiconductor photodetector device. They consist of an array of multiple pixels connected in parallel and operating in Geiger mode. Each pixel consists of an avalanche photodiode and a quenching resistor in series. SiPMs offer high quantum efficiency, high gain, good signal-to-noise ratio, fast time response, low operating voltage, magnetic field insensitivity, and a compact structure. They have become the preferred scintillation photodetector for devices such as CEPCs and FCCs, and are also the preferred choice for optical readout of various scintillation detectors. Due to the high number of scintillation photons generated by GeV-TeV high-energy particles, the SiPM's output signal saturates when all pixels detect a photon simultaneously, meaning there are no more pixels left to detect additional incident photons, directly impacting the dynamic range and accuracy of the electrochemical device. Although the crystal's light output can be reduced using attenuators, their stability and reliability in strong radiation environments cannot be guaranteed. Therefore, it is imperative to reduce the light output of BGO crystals to better meet the urgent application needs of large scientific facilities such as CEPCs and FCCs.

[0006] In addition, after being exposed to a certain dose of high-energy particles, rays or ultraviolet radiation, the BGO crystal will scintillate and its optical performance will decay due to coloring, which will affect the crystal's light output and light response uniformity. This is called "irradiation damage." How to reduce the radiation damage effect has always been one of the important research and development directions of BGO crystals. In addition, BGO crystals have a long decay time of ~0.3μs, which limits their application in high-count rate radiation detection such as high-energy physics and resource exploration. How to shorten their decay time has also received continuous attention.

[0007] Summary of the Invention

[0008] To this end, the object of the present invention is to provide a cerium-doped bismuth germanate single crystal scintillator, which reduces the light output of the BGO scintillator, improves its radiation resistance and shortens its decay time, and its preparation method and application.

[0009] In one aspect, the present invention provides a cerium-doped bismuth germanate single crystal scintillator, wherein the cerium-doped bismuth germanate single crystal scintillator has a chemical formula of Bi4Ge3O 12 :Ce, wherein the doping amount of Ce element does not exceed 0.7wt%. Preferably, wherein Ce element is Ce 3+ and Ce 4+ Two ionic forms exist.

[0010] In this disclosure, after cerium doping BGO, Ce 3+ and Ce 4+ Two ion forms exist in BGO scintillator, due to Ce 3+ and Ce 4+ The ionic radius is much larger than that of Ge 3+ Ionic radius, and Bi 3+ The ionic radius is slightly larger than that of Ce 3+ and Ce 4+ According to the general principle that the doped ions must meet the ionic radius similar to that of the substituted ions in the matrix lattice, after Ce ion doping, it will occupy the Bi 3+ Moreover, the irradiation change of Ce ions can inhibit the radiation in Bi4Ge3O 12 The formation of color centers caused by the 12 Furthermore, the present disclosure reduces BGO light output through Ce doping, suppressing radiation damage while also shortening its decay time, which has important research significance and practical value. The emission peak of the cerium-doped bismuth germanium oxide single crystal scintillator in this patent does not shift, thus avoiding the impact on detection efficiency caused by emission peak shift.

[0011] Preferably, the doping amount of Ce element is 0.005 wt% to 0.5 wt%, more preferably the doping amount of Ce element is 0.01 to 0.4 wt%, and more preferably the doping amount of Ce element is 0.04 wt% to 0.2 wt%.

[0012] Preferably, the size of the cerium-doped bismuth germanium oxide single crystal scintillator reaches the centimeter level in at least one of the length, width and height. Preferably, the length×width×height is at least 1 cm×1 cm×1 cm.

[0013] In another aspect, the present invention provides a method for preparing a cerium-doped bismuth germanate single crystal scintillator, comprising:

[0014] (1) According to the chemical composition Bi4Ge3O 12 :xCe weigh Bi2O3 powder, GeO2 powder and Ce source and mix them to obtain a mixed powder;

[0015] (2) The obtained mixed powder is directly loaded into a crucible or loaded into a crucible after a melting reaction, and grown by a crucible lowering method, a pulling method, a kyberyzing method, a heat exchange method or a micro-pull-down method to obtain the cerium-doped bismuth germanate single crystal scintillator.

[0016] Preferably, the purity of the Bi2O3 powder is ≥99.9%;

[0017] The purity of the GeO2 powder is ≥99.9%;

[0018] The Ce source is selected from at least one of CeO2, Ce2O3 and Ce salt.

[0019] Furthermore, preferably, the Ce salt is selected from at least one of CeF3 and Ce(NO3)3.

[0020] Preferably, the temperature of the melting reaction is 900-1200° C., and the holding time is 2-10 hours.

[0021] Preferably, the parameters of the crucible descent method include: a growth temperature of 900 to 1300° C.; and a descent rate of 0.2 to 1 mm / h.

[0022] Preferably, the parameters of the pulling method include: a growth temperature of 900 to 1300° C.; a rotation speed of 3 to 20 r / min; and a pulling rate of 0.2 to 3 mm / h.

[0023] Preferably, the parameters of the kygroma method include: a growth temperature of 900 to 1300° C.; and a growth rate of 0.1 to 3 mm / h.

[0024] Preferably, the parameters of the heat exchange method include: a growth temperature of 900 to 1300° C., a constant temperature time of 1 to 24 hours, and a cooling rate of 1 to 10° C. / h.

[0025] Preferably, the parameters of the micro-pull-down method include: a growth temperature of 1000-1300° C., and a crucible descending speed of 1-10 mm / h.

[0026] In another aspect, the present invention provides an application of a cerium-doped bismuth germanate single crystal scintillator in radiation detection applications, including high-energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection, and industrial testing. In practical applications, the cerium-doped bismuth germanate single crystal scintillator can be coupled with a SiPM, PMT, CCD, or CMOS detector to form a small detection module. These modules can then be assembled into a two-dimensional or three-dimensional detection array, depending on the application requirements. High-energy radiation or particles interact with the detection array module and are recorded.

[0027] Beneficial effects of the present invention:

[0028] The present invention reduces the light output of BGO scintillators by doping them with cerium, improves their radiation resistance, and shortens their decay time, significantly improving the scintillation properties of BGO. The resulting cerium-doped bismuth germanium oxide (BGO:Ce) single crystal scintillators can be applied in radiation detection fields such as high-energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspections, and industrial testing. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a physical picture of pure BGO single crystal and BGO:Ce single crystal grown by the crucible drop method;

[0030] Figure 2 shows the UV-visible optical transmittance of pure BGO single crystal and BGO:Ce single crystal;

[0031] FIG3 is a gamma-ray pulse height spectrum of pure BGO single crystal and BGO:Ce single crystal;

[0032] Figure 4 shows the normalized light output of pure BGO single crystal and BGO:Ce single crystal as a function of irradiation time;

[0033] FIG5 is a gamma-ray pulse time spectrum of pure BGO single crystal and BGO:Ce single crystal;

[0034] Table 1 in FIG6 shows the Bi4Ge3O 12 : Preparation parameters of Ce single crystal;

[0035] Table 2 in FIG7 shows some Bi4Ge3O prepared by the present invention. 12 :Ce single crystal performance parameters. DETAILED DESCRIPTION

[0036] The present invention is further described below through the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, rather than to limit the present invention.

[0037] In the present disclosure, the chemical formula of the cerium-doped bismuth germanate single crystal scintillator is Bi4Ge3O 12 :Ce, wherein the doping amount of Ce element does not exceed 0.7wt% (for example, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, etc.). Preferably, the doping amount of Ce element is 0.005wt% to 0.5wt%, and more preferably the doping amount of Ce element is 0.04 to 0.2wt%. If the doping amount of Ce element is too high, the grown Bi4Ge3O 12 :Ce single crystal will produce more defects.

[0038] The following is an exemplary description of a method for preparing a cerium-doped bismuth germanate single crystal scintillator.

[0039] Bi2O3 and GeO2 are used as raw materials, and one or more Ce oxides or Ce salts such as CeO2, Ce2O3, CeF3, Ce(NO3)3, etc. containing cerium are used as dopants. The raw materials are weighed according to the weight determined by the doping amount of Ce element and then mixed to obtain a mixed powder.

[0040] The mixed powder is directly loaded into a single crystal growth crucible or loaded after a melting reaction, and grown using methods including but not limited to a crucible descent method, a Czochralski method, a Kyropoulos method, a heat exchange method or a micro-pull-down method to obtain the cerium-doped bismuth germanate single crystal scintillator.

[0041] The present invention reduces the light output of the crystal within an appropriate range by adjusting the doping amount of the cerium element, thereby improving the radiation resistance service capability of the crystal and increasing the time response rate of the crystal.

[0042] The following examples are further given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all fall within the scope of protection of the present invention. The specific process parameters and the like in the following examples are only examples within a suitable range, that is, those skilled in the art can make selections within a suitable range through the description herein, and are not limited to the specific numerical values ​​exemplified below.

[0043] Example 1

[0044] Bi2O3 and GeO2 are used as raw materials, and CeO2 is used as a dopant. The materials are weighed and mixed according to a weight ratio of 0.01 wt% (Bi2O3: 373.98 g, GeO2: 125.97 g, CeO2: 0.05 g, i.e., mCeO2 / (mBi2O3+mGeO2+mCeO2)=0.01 wt%) to obtain a mixed powder.

[0045] The resulting mixed powder is placed in a platinum crucible used for single crystal growth and grown using the crucible-descent method to produce a single crystal scintillator made of cerium-doped bismuth germanium oxide. The crucible-descent method parameters are as follows: the mixed powder is first placed in a crystal growth furnace and heated at a constant temperature of 1300°C for 10 hours until the raw materials are completely melted. The crucible is lowered at a rate of 0.6 mm / h, allowing the melt to slowly crystallize from bottom to top. After crystallization is complete, the temperature is cooled to room temperature at a rate of 20°C / h, resulting in a centimeter-scale single crystal scintillator made of cerium-doped bismuth germanium oxide.

[0046] Example 2

[0047] In this embodiment 2, Bi4Ge3O 12The preparation process of Ce single crystal is similar to that of Example 1, except that the amount of CeO2 added is 0.02 wt%, the growth temperature is 1200°C, and the growth rate is 0.5 mm / h.

[0048] Example 3

[0049] In this embodiment 3, Bi4Ge3O 12 The preparation process of Ce single crystal is similar to that of Example 1, except that the amount of CeO2 added is 0.05 wt%, the growth temperature is 1100°C, and the growth rate is 0.4 mm / h.

[0050] Example 4

[0051] In this embodiment 4, Bi4Ge3O 12 The preparation process of Ce single crystal is similar to that of Example 1, except that the amount of CeO2 added is 0.1 wt%, the growth temperature is 1100°C, and the growth rate is 0.4 mm / h.

[0052] Example 5

[0053] In this embodiment 5, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the dopant is CeF3, the addition amount is 0.2wt%, the growth method is the pulling method, the rotation speed is 10r / min, and the pulling rate is 1.0mm / h.

[0054] Example 6

[0055] In this embodiment 6, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 5, except that: the amount of CeO2 added is 0.5wt%, the growth method is the Kyropoulos method, the growth temperature is 1000℃, and the growth rate is 1mm / h.

[0056] Example 7

[0057] In this embodiment 7, Bi4Ge3O 12 : The preparation process of Ce single crystal refers to Example 1, with the following differences: the dopant is Ce(NO3)3, the addition amount is 0.1wt%, the growth method is heat exchange method, the growth temperature is 1100℃, the constant temperature time is 20 hours, and the cooling rate is 5℃ / h.

[0058] Example 8

[0059] In this embodiment 8, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the dopant is CeO2, the addition amount is 0.5wt%, and the growth rate is 0.4mm / h.

[0060] Example 9

[0061] In this embodiment 9, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 1, except that the dopants are Ce(NO3)3 (50%) and CeO2 (50%), the addition amount is 0.1wt%; the growth rate is 0.4mm / h.

[0062] Example 10

[0063] In this embodiment 10, Bi4Ge3O 12 :The preparation process of Ce single crystal refers to Example 1, with the following differences: the dopants are Ce(NO3)3 (50%), CeO2 (25%) and CeF3 (25%), the added amount is 0.1wt%, the growth method is micro-pull-down method, the growth temperature is 1100℃, and the crucible descent speed is 5mm / h.

[0064] Example 11

[0065] In this embodiment 11, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.01wt% and the growth rate is 0.4mm / h.

[0066] Example 12

[0067] In this embodiment 12, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.02wt% and the growth rate is 0.4mm / h.

[0068] Example 13

[0069] In this embodiment 13, Bi4Ge3O 12 The preparation process of Ce single crystal is similar to that of Example 3, except that the amount of CeO2 added is 0.2 wt % and the growth rate is 0.4 mm / h.

[0070] Example 14

[0071] In this embodiment 14, Bi4Ge3O 12 The preparation process of Ce single crystal is similar to that of Example 3, except that the amount of CeO2 added is 0.3 wt % and the growth rate is 0.4 mm / h.

[0072] Example 15

[0073] In this embodiment 15, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.4wt% and the growth rate is 0.4mm / h.

[0074] Example 16

[0075] In this embodiment 16, Bi4Ge3O 12 The preparation process of Ce single crystal refers to Example 3, except that the amount of CeO2 added is 0.5wt% and the growth rate is 0.4mm / h.

[0076] Comparative Example 1

[0077] In this comparative example 1, Bi4Ge3O 12 The preparation process of the single crystal is similar to that of Example 1, except that the amount of CeO2 added is 0 wt%.

[0078] Table 1 in FIG6 shows the Bi4Ge3O 12 : Preparation parameters of Ce single crystal.

[0079] Table 2 in FIG7 shows some Bi4Ge3O prepared by the present invention. 12 :Ce single crystal performance parameters.

[0080] Figure 1 shows photos of pure BGO (left) and BGO:Ce (middle, Ce doping amount is 0.04wt%; right, Ce doping amount is 0.08wt%) single crystals grown by the crucible drop method. Figure 2 shows the UV-visible optical transmittance of pure BGO and BGO:Ce single crystals. It can be seen from Figures 1 and 2 that after doping with Ce element, high optical quality single crystals can be grown. The crystals change from colorless and transparent to light yellow, and the absorption edge shows a significant red shift.

[0081] Figure 3 shows the gamma-ray pulse height spectra of pure BGO and BGO:Ce single crystals. It can be seen from Figure 3 that the channel number characterizing the crystal light output after the crystal is doped with Ce element is reduced from 703 of the pure crystal to 201 (Ce element doping amount is 0.04wt%), 160 (Ce element doping amount is 0.08wt%) and 204 (Ce element doping amount is 0.16wt%) of the Ce-doped crystal.

[0082] To investigate the radiation resistance of the crystals, pure BGO and BGO:Ce single crystals were irradiated with UVB light. Figure 4 shows the normalized light output curves of pure BGO and BGO:Ce single crystals as a function of UV irradiation time. As can be seen from the figure, Ce doping significantly improves the crystal's radiation resistance, reducing the saturation light output from 25% of pure BGO crystals to 5%. After saturation irradiation, the crystal's light output remains around 95% of its pre-irradiation level. In other words, with increasing Ce doping concentration, the crystal's radiation resistance first significantly improves, then decreases slightly, but still remains above 95%. This is primarily because Ce doping significantly improves the crystal's radiation resistance. However, further increasing the doping concentration leads to an increase in macrodefects in the crystal, making further improvement in radiation resistance difficult. Therefore, the optimal Ce doping level is 0.04wt% to 0.2wt%.

[0083] In order to determine the changing trend of the time response characteristics of the BGO crystal after irradiation, the present invention uses an oscilloscope method to obtain the anode signal pulse of pure BGO and BGO:Ce single crystal under gamma ray excitation, thereby roughly obtaining the gamma ray pulse time spectrum of pure BGO and BGO:Ce crystal. As can be seen from Figure 5, the decay time of the BGO crystal after doping with Ce element is significantly shortened from 381ns (pure BGO crystal) to 253ns (Ce element doping amount is 0.08%), and the decay constant is shortened by 33.6%, which significantly improves the time response characteristics of the BGO crystal. This is mainly because the doping of Ce element changes the crystal field strength of the activator Bi ion in the crystal, changes the probability of radiative or non-radiative transition of Bi ions, thereby shortening the decay time and making it have better time response performance.

[0084] In the present invention, the Ce-doped bismuth germanium oxide scintillator has lower light output, stronger radiation resistance and shorter decay time compared to pure bismuth germanium oxide scintillator, and can meet the higher requirements of high-energy physics and other applications on material light output, radiation resistance and time response characteristics.

[0085] Finally, it is necessary to explain here that the above embodiments are only used to further illustrate the technical solution of the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above content of the present invention all fall within the scope of protection of the present invention.

Claims

1. A cerium-doped bismuth germanate single crystal scintillator, It is characterized in that The cerium-doped bismuth germanate single crystal scintillator has a chemical formula of Bi 4 Ge 3 O 12 :Ce, wherein the doping amount of Ce element does not exceed 0.7wt%.

2. The cerium-doped bismuth germanate single crystal scintillator according to claim 1, It is characterized in that The Ce element is Ce 3+ and Ce 4+ Two ionic forms exist.

3. The cerium-doped bismuth germanate single crystal scintillator according to claim 1, It is characterized in that The doping amount of Ce element is 0.005wt% to 0.5wt%.

4. The cerium-doped bismuth germanate single crystal scintillator according to claim 3, It is characterized in that The doping amount of Ce element is 0.04wt% to 0.2wt%.

5. The cerium-doped bismuth germanate single crystal scintillator according to any one of claims 1 to 4, It is characterized in that The size of the cerium-doped bismuth germanate single crystal scintillator reaches the centimeter level in at least one dimension of length, width and height.

6. A method for preparing the cerium-doped bismuth germanate single crystal scintillator according to any one of claims 1 to 5, It is characterized in that include: (1) Weigh Bi according to mass percentage 2 O 3 Powder, GeO 2 powder and a Ce source are mixed to obtain a mixed powder; (2) The obtained mixed powder is directly loaded into a crucible or loaded into a crucible after a melting reaction, and grown by a crucible descent method, a pulling method, a temperature gradient method, a heat exchange method, a kyberyzing method or a micro-pull-down method to obtain the cerium-doped bismuth germanate single crystal scintillator.

7. The preparation method according to claim 6, It is characterized in that The Bi 2 O 3 The purity of powder is ≥99.9%; The GeO 2 The purity of powder is ≥99.9%; The Ce source is selected from CeO 2 、Ce 2 O 3 and at least one of Ce salts; wherein the Ce salt is selected from CeF 3 、Ce(NO 3 ) 3 At least one of .

8. The preparation method according to claim 6, It is characterized in that The temperature of the melting reaction is 900-1200° C., and the insulation time is 2-10 hours.

9. The preparation method according to any one of claims 6 to 8, It is characterized in that The parameters of the crucible descent method include: a growth temperature of 900 to 1300° C.; and a descent rate of 0.2 to 1 mm / h.

10. The preparation method according to any one of claims 6 to 8, It is characterized in that The parameters of the pulling method include: a growth temperature of 900 to 1300° C.; a rotation speed of 3 to 20 r / min; and a pulling rate of 0.2 to 3 mm / h.

11. The preparation method according to any one of claims 6 to 8, It is characterized in that The parameters of the pyrolysis method include: a growth temperature of 900 to 1300° C.; and a growth rate of 0.1 to 3 mm / h.

12. The preparation method according to any one of claims 6 to 8, It is characterized in that The parameters of the heat exchange method include: a growth temperature of 900 to 1300° C., a constant temperature time of 1 to 24 hours, and a cooling rate of 1 to 10° C. / h.

13. The preparation method according to any one of claims 6 to 8, It is characterized in that The growth temperature of the micro-pull-down method is 1000-1300° C., and the crucible descending speed is 1-10 mm / h.

14. Use of the cerium-doped bismuth germanate single crystal scintillator according to any one of claims 1 to 5 in the field of radiation detection, It is characterized in that The radiation detection field includes high energy physics, nuclear physics, space physics, oil well logging, geological exploration, safety inspection and industrial detection.

Citation Information

Patent Citations

  • Production of bismuth germanate single crystal and its apparatus for production

    JP1994293599A