Gradient-performance spliced neodymium-iron-boron magnet and preparation method therefor

By performing gradient performance splicing on the NdFeB magnet, the grain boundary diffusion and aging treatment of Dy and Tb elements are used to solve the demagnetization problem caused by the eddy current effect of the NdFeB magnet in the motor, reducing costs and improving motor efficiency Magnet performance.

WO2024239516A1PCT designated stage expired Publication Date: 2024-11-28NINGBO SONGKE MAGNETIC MATERIAL
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/124121
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2023-10-12
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

In motors, the temperature rises due to the eddy current effect, which may lead to demagnetization, which will affect the performance of the motor. The existing diffusion process cannot effectively improve local coercive force, and the heavy rare earth elements are used in large quantities and cost high.

Method used

By cutting the neodymium iron boron magnet into thin sheets in the non-oriented direction, covering the surface with Dy and Tb elements, the grain boundary diffusion and aging are performed, and the gradient performance splicing is performed according to the demagnetization characteristics of different positions to form high correction Magnets with stubborn force and high remanent magnets.

Benefits of technology

It reduces the eddy current loss of magnet steel, improves motor efficiency and rotor temperature rise, reduces material costs, simplifies processing technology, reduces bonding workload, and improves the temperature resistance and magnetic energy density of magnets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023124121_28112024_PF_FP_ABST
    Figure CN2023124121_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a gradient-performance spliced neodymium-iron-boron magnet and a preparation method therefor. The preparation method for the gradient-performance spliced neodymium-iron-boron magnet comprises: S100, processing and cutting a neodymium-iron-boron magnet raw material in a non-orientation direction to obtain neodymium-iron-boron magnetic steel sheets; S200, sequentially carrying out surface cleaning, coating, grain boundary diffusion, and aging on the neodymium-iron-boron magnetic steel sheets to obtain neodymium-iron-boron sheets before splicing; and S300, splicing and combining the neodymium-iron-boron sheets to obtain the gradient-performance spliced neodymium-iron-boron magnet. In the preparation method for the gradient-performance spliced neodymium-iron-boron magnet of the present invention, the process is simplified: the bonding workload is reduced by 80% or more compared to that of a conventional process, and the six-surface treatment after bonding is not needed; therefore, the processing work is greatly reduced, and the yield is also improved. Additionally, the method facilitates production and processing, improves motor efficiency, and alleviates the problem of rises in rotor temperature.
Need to check novelty before this filing date? Find Prior Art

Description

A gradient performance spliced ​​NdFeB magnet and its preparation method CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority to Chinese patent application No. 202310591368.9 filed in China on May 24, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0002] The present invention relates to the technical field of NdFeB magnet processing, and in particular to a gradient performance spliced ​​NdFeB magnet and a preparation method thereof. Background Art

[0003] In the field of electric motors, as motor speed or power increases, eddy currents appear within NdFeB magnets, causing the magnet temperature to rise. At a certain temperature, this can cause the NdFeB magnet material to demagnetize, impairing motor performance. When NdFeB magnets are used in motors, the motor's operation causes the temperature to rise. Heat generated by iron loss comes partly from heating of the silicon steel sheets and partly from eddy currents within the NdFeB magnets themselves. In the actual production of NdFeB magnets, to ensure magnetic performance in the highest temperature range, the performance of the entire magnet must meet the magnetic performance attenuation requirements in this highest temperature range. This, to some extent, hinders improving the remanence of NdFeB magnets and reducing their cost. Typically, permanent magnets in motors are made of NdFeB material, which has high coercivity and remanence. Therefore, how to effectively reduce eddy current losses in NdFeB magnets, effectively reduce the amount of heavy rare earth elements used, and lower the cost of the entire magnet without affecting motor performance is a challenge facing those skilled in the art.

[0004] In addition, in many application fields, the demagnetization field of NdFeB magnets mainly acts on the edge area of ​​the magnet. Improving the coercive force of this area can significantly improve the overall anti-demagnetization of NdFeB magnets in actual use. At present, the diffusion process is widely used to increase the coercive force of NdFeB magnets. The conventional diffusion process is to place NdFeB magnets in an environment containing heavy rare earth elements such as Dy and Tb, and undergo high-temperature diffusion and aging treatment to allow Dy and Tb elements to diffuse along the grain boundaries to the Nd2Fe 14 B phase boundary, increasing Nd2Fe 14 B's magnetic anisotropy, thereby effectively improving the coercive force of NdFeB magnets.

[0005] However, this type of method generally coats both surfaces of the magnet in the perpendicular magnetization direction with heavy rare earth materials or coats all surfaces of the magnet with heavy rare earth elements (including burying the entire magnet in heavy rare earth elements) and then performs diffusion treatment. This type of diffusion does not perform local diffusion treatment on the easily demagnetized areas in actual applications of the magnet to increase the coercive force of the local areas, but rather increases the overall coercive force of the magnet through overall diffusion to improve the resistance to demagnetization in actual applications. Therefore, the overall coating area of ​​the heavy rare earth elements is large, and the overall usage of heavy rare earth elements is relatively large. Summary of the Invention

[0006] Therefore, the present invention provides a gradient performance spliced ​​NdFeB magnet and its preparation method, selects a reasonable processing path, can obtain good magnetic properties, meet the requirements of motor design, and is easy to produce and process. When the motor runs at high speed, the magnet can reduce the eddy current loss of the magnet, improve the motor efficiency, and improve the rotor temperature rise.

[0007] To solve the above problems, the present invention provides a method for preparing a gradient performance spliced ​​NdFeB magnet, comprising the following steps:

[0008] S100, processing and cutting the first NdFeB magnet raw material in a non-oriented direction to obtain a NdFeB magnetic steel sheet F1; processing and cutting the second NdFeB magnet raw material in a non-oriented direction to obtain a NdFeB magnetic steel sheet M1;

[0009] S200, performing surface cleaning treatment, coating treatment, grain boundary diffusion treatment, and aging treatment on the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1, respectively, to obtain NdFeB magnetic steel sheet F11 and NdFeB magnetic steel sheet M11, respectively; wherein the intrinsic coercivity of the NdFeB magnetic steel sheet F11 is greater than the intrinsic coercivity of the NdFeB magnetic steel sheet M11 by more than 3kOe;

[0010] S300, splicing and combining the NdFeB magnetic steel sheets F11 and the NdFeB magnetic steel sheets M11 in the order of at least one NdFeB magnetic steel sheet M11 being provided between two NdFeB magnetic steel sheets F11, to obtain a gradient performance spliced ​​NdFeB magnet.

[0011] Compared with the existing technology, the technical effect achieved by adopting this technical solution is as follows: this technical solution processes and cuts the raw materials of NdFeB magnets, covers the two surfaces in the non-magnetized direction with a thin film of Dy, Tb or alloy or compound powder containing Dy and Tb elements, and performs grain boundary diffusion treatment and aging treatment on the NdFeB magnet slices covered with the heavy rare earth film layer, and then splices and combines them into large blocks of gradient performance magnets; thereby simplifying the processing technology, reducing the bonding workload by more than 80% compared with the conventional process, and eliminating the need for six-sided trimming after bonding, which greatly reduces the processing volume and improves the yield. The product obtained by this technical solution is very helpful in reducing losses, reducing eddy current losses of magnetic steel, improving motor efficiency, and improving rotor temperature rise. In addition, according to the different demagnetization characteristics of different positions of the magnet, the edge area that is prone to demagnetization is set to have a higher intrinsic coercive force to improve the temperature resistance of the magnetic steel. It is also possible to set a higher remanence at the center of the magnet to obtain a greater magnetic energy density, thereby obtaining a gradient performance NdFeB magnet with high magnetic energy density and high temperature resistance, and the material cost of the central part of the magnet is lower.

[0012] In one technical solution of the present invention, in S100: the thickness of the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1 is less than or equal to 12 mm; and / or the thickness direction of the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1 is the direction of the non-oriented plane.

[0013] Compared with the existing technology, the technical effect achieved by adopting this technical solution is as follows: gradient performance setting is made for the easily demagnetized area of ​​the magnet, and the area is configured with a higher intrinsic coercive force; and the magnetic energy density of the relatively difficult to demagnetize area is improved to form a combined magnet with different performances, thereby obtaining a magnet with high magnetic energy density and locally enhanced demagnetization effect, and greatly reducing material costs.

[0014] In one technical solution of the present invention, in S200: the process parameter temperature of the grain boundary diffusion treatment is 800°C to 1000°C, and the time is 8h to 50h; and / or the process parameter temperature of the aging treatment is 400°C to 600°C, and the time is 2h to 6h.

[0015] Compared with the existing technology, the technical effect achieved by adopting this technical solution is: when the process parameter temperature of the grain boundary diffusion treatment is 800℃ to 1000℃ and the time is 8h to 50h; the process parameter temperature of the aging treatment is 400℃ to 600℃ and the time is 2h to 6h, a neodymium iron boron magnet with high magnetic energy density and high temperature resistance can be obtained, which has a higher intrinsic coercive force and improves the temperature resistance of the magnetic steel.

[0016] In one technical solution of the present invention, in S200: the surface cleaning treatment includes shot blasting, pickling, and ultrasonic cleaning.

[0017] Compared with the existing technology, the technical effect achieved by adopting this technical solution is: surface cleaning treatment affects the diffusion effect, thereby further improving the gradient performance of NdFeB magnets.

[0018] In one technical solution of the present invention, in S200: the coating treatment uses a diffusion source including one or more of Dy powder, DyF3 powder, Tb powder, TbF3 powder, and heavy rare earth alloy powder;

[0019] The general formula of heavy rare earth alloy powder is HRE-X;

[0020] HRE includes Dy and / or Tb;

[0021] X includes one or more of Pr, Nd, Al, Cu, Ga, Ni, Co, Fe, Zr, Nb, Ti, Hf, W, and V.

[0022] In one technical solution of the present invention, in S300: the NdFeB magnetic steel sheet F11 and the NdFeB magnetic steel sheet M11 are diffused in non-oriented surfaces; and / or the splicing agent for gradient performance splicing of NdFeB magnets selects high-temperature resistant non-conductive glue; and / or when there are multiple NdFeB magnetic steel sheets M11, the sheet thickness spacing between the bonding seams includes equal spacing and / or unequal spacing.

[0023] Compared with the existing technology, the technical effects achieved by adopting this technical solution are as follows: the product bonding uses high-temperature resistant insulating glue, which can greatly reduce the eddy current loss of the magnetic steel, improve the motor efficiency, and improve the rotor temperature rise; in addition, when there are multiple gradient performance spliced ​​NdFeB magnets, according to the different demagnetization characteristics of different positions of the magnets, the thickness spacing between the bonding seams includes equal spacing and / or unequal spacing, and the processing cost is relatively low, which ensures that the initial magnetic properties are not deteriorated and is very helpful in reducing losses, reducing the eddy current loss of the magnet, and improving the motor efficiency. Compared with conventional square magnets, this spliced ​​gradient performance magnet can reduce the eddy current effect of the magnet by more than 25% during the operation of the motor, and the motor temperature rise caused by the eddy current effect is reduced by more than 25°C; in addition, the local performance of the magnet is set according to the difference in demand so that the edge area has a higher intrinsic coercive force than the central area, and the central area has a comparable or higher remanence than the edge area, which maximizes the magnet performance and greatly reduces the material cost.

[0024] In a technical solution of the present invention, the method for preparing a gradient performance spliced ​​NdFeB magnet further includes the following steps after S300:

[0025] S400, anti-corrosion treatment is performed on the surface of gradient performance spliced ​​NdFeB magnets.

[0026] Compared with the existing technology, the technical effect achieved by adopting this technical solution is that the gradient performance spliced ​​NdFeB magnet has increased corrosion resistance through anti-corrosion treatment, thereby improving the service life of the gradient performance spliced ​​NdFeB magnet.

[0027] In one technical solution of the present invention, the anti-corrosion treatment includes at least one of electroplating, chemical plating, organic coating and physical vapor deposition.

[0028] The present invention also provides a gradient performance spliced ​​NdFeB magnet, which is obtained by adopting the preparation method of any of the above technical solutions.

[0029] Compared with the existing technology, the technical effects achieved by adopting this technical solution are: the processing path is optimized, the bonding workload is reduced by more than 80% compared with the conventional process, and there is no need for 6-side trimming after bonding, which greatly reduces the processing volume and improves the yield; it can obtain good magnetic properties, meet the design requirements of the motor, and is easy to produce and process. The magnet can reduce the eddy current loss of the magnetic steel when the motor runs at high speed, improve the motor efficiency, and improve the rotor temperature rise.

[0030] After adopting the technical solution of the present invention, the following technical effects can be achieved:

[0031] (1) The processing path is optimized, which greatly reduces the processing volume and improves the yield;

[0032] (2) Reduce eddy current loss of magnetic steel, improve motor efficiency, and improve rotor temperature rise;

[0033] (3) According to the different demagnetization characteristics of different positions of the magnet, the edge area that is prone to demagnetization is set to have a higher intrinsic coercive force to improve the temperature resistance of the magnet; the center of the magnet is set to have a higher remanence to obtain a larger magnetic energy density, thereby obtaining a gradient performance magnet with high magnetic energy density and high temperature resistance, and the material cost of the central part of the magnet is lower. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings to be used in describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. Those skilled in the art can also derive other drawings based on these drawings without inventive effort.

[0035] FIG1 is a substrate blank provided by an embodiment of the present invention;

[0036] FIG2 shows a NdFeB magnetic steel sheet F11 and a NdFeB magnetic steel sheet M11 provided in an embodiment of the present invention;

[0037] FIG3 shows the magnetic energy density of a gradient performance spliced ​​NdFeB magnet provided by an embodiment of the present invention;

[0038] FIG4 shows the intrinsic coercive force of a gradient performance spliced ​​NdFeB magnet provided by an embodiment of the present invention;

[0039] Description of reference numerals:

[0040] 100: NdFeB magnet sheet F11, 200: NdFeB magnet sheet M11. Implementation Method

[0041] To make the above-mentioned objectives, features, and advantages of the present invention more clearly understood, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. All other embodiments obtained by persons of ordinary skill in the art based on the embodiments of the present invention without creative effort shall fall within the scope of protection of the present invention.

[0042] This embodiment provides a method for preparing a gradient performance spliced ​​NdFeB magnet, comprising the following steps:

[0043] S100, processing and cutting the first NdFeB magnet raw material in a non-oriented direction to obtain a NdFeB magnetic steel sheet F1; processing and cutting the second NdFeB magnet raw material in a non-oriented direction to obtain a NdFeB magnetic steel sheet M1;

[0044] S200, performing surface cleaning treatment, coating treatment, grain boundary diffusion treatment, and aging treatment on the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1, respectively, to obtain NdFeB magnetic steel sheet F11 and NdFeB magnetic steel sheet M11, respectively; wherein the intrinsic coercivity of the NdFeB magnetic steel sheet F11 is greater than the intrinsic coercivity of the NdFeB magnetic steel sheet M11 by more than 3kOe;

[0045] S300, splicing and combining the NdFeB magnetic steel sheets F11 and the NdFeB magnetic steel sheets M11 in the order of at least one NdFeB magnetic steel sheet M11 being provided between two NdFeB magnetic steel sheets F11, to obtain a gradient performance spliced ​​NdFeB magnet.

[0046] Preferably, two surfaces of the NdFeB magnet raw material in the non-magnetized direction are covered with a thin film of Dy, Tb, or an alloy or compound powder containing Dy and Tb elements, and the NdFeB magnet slices covered with the heavy rare earth film are subjected to grain boundary diffusion treatment and aging treatment, and then spliced ​​and assembled into a large block of gradient performance magnet; thereby simplifying the processing process, reducing the bonding workload by more than 80% compared with conventional processes, and eliminating the need for six-side trimming after bonding, greatly reducing the processing workload and improving the yield;

[0047] The product is very helpful in reducing losses, lowering eddy current losses of magnets, improving motor efficiency, and improving rotor temperature rise. In addition, according to the different demagnetization characteristics of different positions of the magnet, the edge area that is prone to demagnetization is set to have a higher intrinsic coercive force to improve the temperature resistance of the magnet. The center of the magnet can also be set to have a higher remanence to obtain a greater magnetic energy density, thereby obtaining a gradient performance magnet with high magnetic energy density and high temperature resistance, and the material cost of the central part of the magnet is lower.

[0048] In step S300, "the NdFeB magnetic steel sheets F11 and the NdFeB magnetic steel sheets M11 are spliced ​​and combined in the order that at least one NdFeB magnetic steel sheet M11 is provided between the two NdFeB magnetic steel sheets F11" means that at least one NdFeB magnetic steel sheet M11 is provided in the NdFeB magnetic steel sheet F11; therefore, the specific combination of gradient performance spliced ​​NdFeB magnets can be F11-M11-F11, F11-M11-M11-F11, F11-M11-M11-M11-F11 or others, and those skilled in the art can make arrangements according to actual conditions.

[0049] In one embodiment of the present invention, in S100: the thickness of the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1 is less than or equal to 12 mm; and / or the thickness direction of the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1 is the direction of the non-oriented plane.

[0050] Preferably, when the thickness of the NdFeB magnet sheet is less than or equal to 12 mm, a gradient performance setting is performed for the easily demagnetized area of ​​the magnet, and the area is configured with a higher intrinsic coercive force; while the magnetic energy density of the relatively difficult to demagnetize area is increased to form a combined magnet with different performances, thereby obtaining a magnet with high magnetic energy density and locally enhanced demagnetization effect, and greatly reducing material costs.

[0051] In one embodiment of the present invention, in S200: the process parameter temperature of the grain boundary diffusion treatment is 800° C. to 1000° C., and the time is 8 h to 50 h; and / or the process parameter temperature of the aging treatment is 400° C. to 600° C., and the time is 2 h to 6 h.

[0052] Specifically, the grain boundary diffusion treatment allows Dy to exist only at the grain boundaries through diffusion without entering the crystals. This not only improves the performance of the NdFeB material, but also greatly reduces the total amount of Dy elements and reduces the cost of the material. At the same time, Dy vapor is deposited on the surface of the particles during the pulverizing process, and Dy atoms diffuse along the grain boundaries during the subsequent sintering process. The Dy and Fe at the grain boundaries are antiferromagnetically coupled, and the coercive force of the material is significantly increased with almost no reduction in remanence.

[0053] When the process parameters of the grain boundary diffusion treatment are 800°C to 1000°C and the time is 8h to 50h; and the process parameters of the aging treatment are 400°C to 600°C and the time is 2h to 6h, a NdFeB magnet with high magnetic energy density and high temperature resistance can be obtained, which has a higher intrinsic coercive force and improves the temperature resistance of the magnetic steel.

[0054] In one embodiment of the present invention, in S200: the surface cleaning treatment includes shot blasting, pickling, and ultrasonic cleaning.

[0055] Preferably, the surface cleaning treatment affects the diffusion effect, thereby further improving the gradient performance of the NdFeB magnet.

[0056] In one embodiment of the present invention, in S200: the coating process uses a diffusion source including one or more of Dy powder, DyF3 powder, Tb powder, TbF3 powder, and heavy rare earth alloy powder;

[0057] The general formula of heavy rare earth alloy powder is HRE-X;

[0058] HRE includes Dy and / or Tb;

[0059] X includes one or more of Pr, Nd, Al, Cu, Ga, Ni, Co, Fe, Zr, Nb, Ti, Hf, W, and V.

[0060] Specifically, heavy rare earth alloy powder can optimize grain boundaries and increase the intrinsic coercive force of NdFeB magnets.

[0061] In one embodiment of the present invention, in S300: the NdFeB magnetic steel sheet F11 and the NdFeB magnetic steel sheet M11 are non-oriented surface diffused; and / or the splicing agent for gradient performance splicing of NdFeB magnets selects high-temperature resistant non-conductive glue; and / or when there are multiple NdFeB magnetic steel sheets M11, the sheet thickness spacing between the bonding seams includes equal spacing and / or unequal spacing.

[0062] Preferably, the product is bonded with high-temperature resistant insulating glue, which can greatly reduce the eddy current loss of the magnet, improve the motor efficiency, and improve the rotor temperature rise; in addition, when there are multiple gradient performance spliced ​​NdFeB magnets, the sheet thickness spacing between the bonding seams includes equal spacing and / or unequal spacing according to the different demagnetization characteristics of different positions of the magnets, and the processing cost is relatively low, which ensures that the initial magnetic properties are not deteriorated and is very helpful in reducing losses, reducing the eddy current loss of the magnet, and improving the motor efficiency. Compared with conventional square magnets, this spliced ​​gradient performance magnet can reduce the eddy current effect of the magnet by more than 25% during the operation of the motor, and the motor temperature rise caused by the eddy current effect is reduced by more than 25°C. In addition, the local performance of the magnet can be set according to different needs so that the edge area has a higher intrinsic coercive force than the central area, and the central area has a comparable or higher remanence than the edge area, so as to maximize the magnet performance and greatly reduce material costs.

[0063] In one embodiment of the present invention, after S300, the method for preparing the gradient performance spliced ​​NdFeB magnet further comprises the following steps:

[0064] S400, anti-corrosion treatment is performed on the surface of gradient performance spliced ​​NdFeB magnets.

[0065] Preferably, the gradient performance spliced ​​NdFeB magnet is subjected to anti-corrosion treatment to increase its corrosion resistance, thereby increasing the service life of the gradient performance spliced ​​NdFeB magnet.

[0066] In one embodiment of the present invention, the anti-corrosion treatment includes at least one of electroplating, chemical plating, organic coating and physical vapor deposition.

[0067] This embodiment also provides a gradient performance spliced ​​NdFeB magnet, which is obtained by using the preparation method of any of the above technical solutions.

[0068] Specifically, the processing path has been optimized, and the bonding workload has been reduced by more than 80% compared with conventional processes. There is no need for 6-side trimming after bonding, which greatly reduces the processing volume and improves the yield. Good magnetic properties can be obtained to meet the design requirements of the motor, and it is easy to produce and process. When the motor runs at high speed, the magnet can reduce the eddy current loss of the magnet, improve the motor efficiency, and improve the rotor temperature rise.

[0069] [First embodiment]

[0070] This embodiment provides a method for preparing a gradient performance spliced ​​NdFeB magnet. The specific steps are as follows:

[0071] S100, a substrate blank 1 with the properties of Br (KGs) 13.75, intrinsic coercivity (KOe) 17.5 Hk / intrinsic coercivity 0.985 was selected, and the blank size was 25 mm × 50.4 mm × 40 mm, of which the orientation direction dimension was 40 mm, as shown in FIG1 ;

[0072] The substrate blank 2 with the properties of Br(KGs) 14.25, intrinsic coercivity (KOe) 16.5 Hk / intrinsic coercivity 0.985 was selected. The blank size was 25mm×43.8mm×40mm, of which the orientation direction dimension was 40mm, as shown in Figure 1;

[0073] S200, processing and cutting the blank 1 in S100 into a size of 23.2 mm × 4.2 mm × 40 mm, wherein the dimension in the orientation direction is 40 mm, to obtain the NdFeB magnetic steel sheet F1;

[0074] The blank 2 in S100 is processed and cut into a size of 23.2 mm × 3.6 mm × 40 mm, wherein the dimension in the orientation direction is 40 mm, to obtain the NdFeB magnetic steel sheet M1;

[0075] S300, pickling the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1;

[0076] S400, performing Tb diffusion source coating on the NdFeB magnetic steel sheet F1 after pickling treatment in the non-oriented direction of 4.2 mm, and performing Dy diffusion source coating on the NdFeB magnetic steel sheet M1 after pickling treatment in the non-oriented direction of 3.6 mm;

[0077] S500, placing the coated NdFeB magnetic steel sheet F1 and the coated NdFeB magnetic steel sheet M1 in a vacuum furnace for heat treatment at a temperature of 900°C for 20 hours; after cooling, performing aging treatment in a vacuum furnace at a temperature of 500°C for 4 hours to obtain NdFeB magnetic steel sheet F11 (100) and NdFeB magnetic steel sheet M11 (200), as shown in FIG2 ;

[0078] The performance test confirmed that the performance of NdFeB magnetic steel sheet F11 (100) is Br (KGs) 13.65 intrinsic coercive force (KOe) 29.2;

[0079] The performance test confirmed that the performance of NdFeB magnetic steel sheet M11 (200) is Br (KGs) 14.05 intrinsic coercive force (KOe) 23.5;

[0080] S600, fine grinding the double end surfaces of the NdFeB magnetic steel sheet F11 (100) to 4.00 mm in the 4.2 mm direction; then pickling;

[0081] The NdFeB magnetic steel sheet M11 (200) is finely ground on both ends in the 3.8mm direction to 3.4mm; and then pickled;

[0082] The pickled NdFeB magnetic steel sheets are stacked and bonded in the thickness direction in the order of F11-M11-M11-M11-F11 to obtain a spliced ​​rough blank 1;

[0083] S700, machining and cutting the obtained spliced ​​rough blank A1 with the specification of 23.2 mm × 18.5 mm (including the bonding seam) * 40 mm to obtain a spliced ​​magnet A11 with good symmetry of 23 mm × 18.5 mm × 3.6 mm;

[0084] The spliced ​​magnet A11 was subjected to surface pickling and surface epoxy treatment to obtain the final spliced ​​gradient performance magnetic steel product. The product performance is shown in Figures 3 and 4;

[0085] In the embodiment of the present invention, the product bonding uses high-temperature resistant insulating glue, which can greatly reduce the eddy current loss of the magnetic steel, improve the motor efficiency, and improve the rotor temperature rise. In addition, the local performance of the magnetic steel is set according to the demand differences, so as to maximize the performance of the magnetic steel and greatly reduce the material cost.

[0086] [Second embodiment]

[0087] This embodiment provides a method for preparing a gradient performance spliced ​​NdFeB magnet. The raw materials are basically the same as those in the first embodiment, except that the temperature of the grain boundary diffusion treatment is 800°C.

[0088] [Third embodiment]

[0089] This embodiment provides a method for preparing a gradient performance spliced ​​NdFeB magnet. The raw materials are basically the same as those in the second embodiment, except that the temperature of the grain boundary diffusion treatment is 1000°C.

[0090] [Fourth embodiment]

[0091] This embodiment provides a method for preparing a gradient performance spliced ​​NdFeB magnet. The raw materials are basically the same as those in the first embodiment, the only difference being that the aging treatment temperature is 400°C.

[0092] [Fifth embodiment]

[0093] This embodiment provides a method for preparing a gradient performance spliced ​​NdFeB magnet. The raw materials are basically the same as those in the fourth embodiment, except that the aging treatment temperature is 600°C.

[0094] The above is a detailed introduction to a low eddy current loss NdFeB magnet provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only for facilitating understanding.

[0095] The methods and core concepts of the present invention, including the best mode, also enable any person skilled in the art to practice the present invention, including making and using any device or system, and performing any combined method. It should be noted that those skilled in the art may make various improvements and modifications to the present invention without departing from the principles of the present invention, and such improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a gradient performance spliced ​​NdFeB magnet, characterized in that: The method for preparing the gradient performance spliced ​​NdFeB magnet comprises the following steps: S100, processing and cutting the first NdFeB magnet raw material in a non-oriented direction to obtain a NdFeB magnetic steel sheet F1; processing and cutting the second NdFeB magnet raw material in a non-oriented direction to obtain a NdFeB magnetic steel sheet M1; S200, performing surface cleaning treatment, coating treatment, grain boundary diffusion treatment, and aging treatment on the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1, respectively, to obtain NdFeB magnetic steel sheet F11 and NdFeB magnetic steel sheet M11, respectively; wherein the intrinsic coercive force of the NdFeB magnetic steel sheet F11 is greater than the intrinsic coercive force of the NdFeB magnetic steel sheet M11 by more than 3kOe; S300, splicing and combining the NdFeB magnetic steel sheets F11 and the NdFeB magnetic steel sheets M11 in the order that at least one NdFeB magnetic steel sheet M11 is provided between two NdFeB magnetic steel sheets F11 to obtain the gradient performance spliced ​​NdFeB magnet.

2. The method for preparing a gradient performance spliced ​​NdFeB magnet according to claim 1, characterized in that: In S100: The thickness of the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1 is less than or equal to 12 mm; and / or The thickness direction of the NdFeB magnetic steel sheet F1 and the NdFeB magnetic steel sheet M1 is the direction of the non-oriented surface.

3. The method for preparing a gradient performance spliced ​​NdFeB magnet according to claim 1, characterized in that: In S200: The process parameters of the grain boundary diffusion treatment are a temperature of 800° C. to 1000° C. and a time of 8 h to 50 h; and / or The process parameters of the aging treatment are a temperature of 400° C. to 600° C. and a time of 2 h to 6 h.

4. The method for preparing a gradient performance spliced ​​NdFeB magnet according to claim 1, characterized in that: In S200: the surface cleaning treatment includes shot blasting, pickling, and ultrasonic cleaning.

5. The method for preparing a gradient performance spliced ​​NdFeB magnet according to claim 1, characterized in that: In S200: the diffusion source used in the coating process includes one or more of Dy powder, DyF3 powder, Tb powder, TbF3 powder, and heavy rare earth alloy powder; Wherein, the general formula of the heavy rare earth alloy powder is HRE-X; The HRE comprises Dy and / or Tb; The X includes one or more of Pr, Nd, Al, Cu, Ga, Ni, Co, Fe, Zr, Nb, Ti, Hf, W and V.

6. The method for preparing a gradient performance spliced ​​NdFeB magnet according to claim 1, characterized in that: In S300: The NdFeB magnetic steel sheet F11 and the NdFeB magnetic steel sheet M11 are non-oriented surface diffused; and / or The splicing agent of the gradient performance spliced ​​NdFeB magnets is selected from high temperature resistant non-conductive glue; and / or When there are multiple NdFeB magnetic steel sheets M11, the sheet thickness spacing between the bonding seams includes equal spacing and / or unequal spacing.

7. The method for preparing a gradient performance spliced ​​NdFeB magnet according to claim 1, characterized in that: After S300, the method for preparing the gradient performance spliced ​​NdFeB magnet further comprises the following steps: S400, performing anti-corrosion treatment on the surface of the gradient performance spliced ​​NdFeB magnet.

8. The method for preparing a gradient performance spliced ​​NdFeB magnet according to claim 7, characterized in that: The anti-corrosion treatment includes at least one of electroplating, chemical plating, organic coating and physical vapor deposition.

9. A gradient performance spliced ​​NdFeB magnet, characterized in that: The gradient performance spliced ​​NdFeB magnet is obtained by the preparation method as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Composite magnet manufacturing method using neodymium iron boron magnetic sheets

    CN103839669A

  • Method for accelerating permeation of Dy / Tb adhesive layer on surface of sintered neodymium-iron-boron magnet

    CN104388952A

  • Method for preparing composite NdFeB magnet with coercive gradient distribution characteristic

    CN110136953A

  • Multilayer grain boundary diffusion method of neodymium-iron-boron thick magnet

    CN114334415A

  • Spliced neodymium-iron-boron magnet with gradient performance and preparation method thereof

    CN116564691A