Preparation method for modified nickel paste for mlcc

By using nano BaTiO3 predispersion and modified nickel powder technology in MLCC, combined with end epoxy-based hyperbranched polyester binder, the problem of uneven dispersion of nano BaTiO3 powder in nickel slurry is solved, and the finished MLCC product has been improved Dispersive performance and voltage and high temperature resistance.

WO2024239611A1PCT designated stage expired Publication Date: 2024-11-28CHANGDI NEW MATERIAL TECHNOLOGY (SHANGHAI) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/138421
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2023-12-13
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The nano BaTiO3 powder in nickel slurry in MLCC is unevenly dispersed, resulting in holes and discontinuities in the finished MLCC products, affecting performance.

Method used

NanobaTiO3 predispersion and modified nickel powder are used, and dispersed by specific proportion mixing and three-roller dispersion, combined with end epoxy-based hyperbranched polyester as a binder bridge to improve the dispersion and adhesion of nickel slurry.

Benefits of technology

It achieves good dispersion and high performance of MLCC finished products, improves the adhesion between nickel slurry and ceramic coating, and improves the voltage and high temperature resistance of MLCC.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023138421_28112024_PF_FP_ABST
    Figure CN2023138421_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the field of multilayer ceramic capacitor (MLCC) electronic materials, in particular to a preparation method for a modified nickel paste for MLCCs. The preparation method for the modified nickel paste for MLCCs comprises the following steps: nano BaTiO3 pre-dispersion: uniformly mixing a nano BaTiO3 powder, a diluent and a dispersing agent according to a specific mass ratio, and dispersing same to obtain a nano BaTiO3 pre-dispersion body; and mixing the BaTiO3 pre-dispersion body, a binder, a dispersing agent, a diluent and nickel powder according to a specific mass ratio, dispersing and filtering same to obtain the modified nickel paste for MLCCs.
Need to check novelty before this filing date? Find Prior Art

Description

A preparation method of modified nickel paste for MLCC Technical Field

[0001] The present application relates to the field of electronic materials for chip-type multilayer ceramic capacitors, and specifically to a method for preparing a modified nickel paste for MLCC. Background Art

[0002] MLCC (Multi-layer Ceramic Capacitors) is the abbreviation for chip-type multilayer ceramic capacitors. They are made by stacking ceramic dielectric diaphragms with printed electrodes (inner electrodes) in an offset manner. They undergo a single high-temperature sintering process to form a ceramic chip. Metal layers (outer electrodes) are then sealed at both ends of the chip, creating a structure similar to a monolithic structure. Hence, they are also called monolithic capacitors.

[0003] Currently, the slurry used in MLCC internal electrodes is typically nickel slurry. In related technologies, nickel powder, nano-BaTiO3, a binder, a dispersant, and an organic solvent are mixed and stirred evenly, and then the raw materials are dispersed using the pressure, gap, and friction shear force of a three-roll mill to produce nickel slurry. However, because the particle size of nano-BaTiO3 powder is smaller than that of nickel powder, the gap of the three-roll mill needs to be reduced when considering the dispersion effect of nano-BaTiO3, which will damage the nickel powder with larger particle size. When considering the dispersion effect of nickel powder, the gap of the three-roll mill needs to be increased, which will cause the nano-BaTiO3 with smaller particle size to agglomerate, preventing a good dispersion effect. For nickel slurry used in MLCC, the dispersibility of nickel powder is extremely important. Therefore, nano-BaTiO3 usually cannot achieve a good dispersion effect, which will cause holes and discontinuities in the MLCC internal electrodes, thereby affecting the performance of the MLCC finished product.

[0004] Therefore, it is urgent to improve the dispersion performance of nano-BaTiO3 powder in nickel paste to improve the performance of MLCC finished products.

[0005] Summary of the Invention

[0006] In order to solve the problem of uneven dispersion of nano-BaTiO3 powder in nickel paste for MLCC, the present application provides a method for preparing a modified nickel paste for MLCC.

[0007] In the first aspect, the present application provides a method for preparing a modified nickel paste for MLCC, using the following technical solution:

[0008] A method for preparing a modified nickel paste for MLCC, comprising the following steps:

[0009] Nano-BaTiO3 pre-dispersion: Nano-BaTiO3 powder, diluent, and dispersant are mixed and dispersed in a mass ratio of (60-90): (20-30): 1 to obtain a nano-BaTiO3 pre-dispersion;

[0010] Preparation of nickel paste: BaTiO3 pre-dispersion, binder, dispersant, diluent and nickel powder are mixed and dispersed in a mass ratio of 10:(10-15):(0.1-1):(10-15):(25-60), and filtered to obtain modified nickel paste for MLCC.

[0011] By adopting the above technical solution, the nano-BaTiO3 powder is first pre-dispersed with a dispersant to obtain a uniformly dispersed nano-BaTiO3 pre-dispersion, and then the nano-BaTiO3 pre-dispersion is mixed with nickel powder and other raw materials in the above proportions, and dispersed using a three-roller mill to obtain a uniformly dispersed nickel slurry, thereby solving the problem of uneven dispersion of nano-BaTiO3 powder in the nickel slurry for MLCC and improving the performance of the MLCC finished product.

[0012] Preferably, the mass ratio of the BaTiO3 pre-dispersion to nickel powder is 10:(50-60).

[0013] Preferably, the particle size of the nano BaTiO3 powder is 10-200 nm.

[0014] By adopting the above technical solution, when the particle size of the nano-BaTiO3 powder is within the above range, the dispersion performance of the nano-BaTiO3 powder in the nickel slurry is better.

[0015] Preferably, the preparation method of the binder comprises the following steps:

[0016] Preparation of epoxy-terminated hyperbranched polyester: reacting hydroxyl-terminated hyperbranched polyester with epichlorohydrin in a mass ratio of (10-20):1 to obtain epoxy-terminated hyperbranched polyester;

[0017] Preparation of modified polyvinyl butyral: reacting epoxy-terminated hyperbranched polyester with polyvinyl butyral in a mass ratio of (10-25):1 to obtain modified polyvinyl butyral;

[0018] Preparation of the binder: Modified polyvinyl butyral ester and ethyl cellulose are reacted in a mass ratio of (2-10):1 to obtain the binder.

[0019] By adopting the above technical solution, a hydroxyl-terminated hyperbranched polyester is reacted with epichlorohydrin in the above mass ratio to obtain an epoxy-terminated hyperbranched polyester; an excess of the epoxy-terminated hyperbranched polyester is then reacted with polyvinyl butyral ester, during which the epoxy groups on the epoxy-terminated hyperbranched polyester react with the hydroxy groups on the polyvinyl butyral ester to generate hydroxy groups and ether bonds to obtain modified polyvinyl butyral ester, wherein the modified polyvinyl butyral ester contains unreacted epoxy groups; the modified polyvinyl butyral ester is then reacted with ethyl cellulose, and the epoxy groups on the modified polyvinyl butyral ester react with the hydroxy groups on the ethyl cellulose to generate hydroxy groups and ether bonds;

[0020] In summary, the epoxy-terminated hyperbranched polyester is used as a bridge to graft ethyl cellulose onto the polyvinyl butyral ester molecule to obtain a binder containing multiple active groups. The binder is added to the nickel paste. Some of the active groups on the binder cross-link with each other to firmly bond the components, and the other part of the active groups bond with the hydroxyl groups on the ceramic coating, so that the nickel paste and the ceramic coating have good adhesion, thereby improving the performance of the MLCC finished product.

[0021] Preferably, the mass ratio of the epoxy-terminated hyperbranched polyester to polyvinyl butyral is (10-15):1.

[0022] Preferably, the diluent is one or more of terpineol, isoborneol acetate, isophorone, and butyl acetate.

[0023] Preferably, the diluent is prepared by compounding terpineol, isoborneol acetate and butyl acetate in a mass ratio of (0.2-1):(0.5-1.5):1.

[0024] By adopting the above technical solution, a diluent prepared by compounding terpineol, isoborneol acetate and butyl acetate according to the above specific mass ratio is added to the nickel slurry, which has little impact on the ceramic coating and reduces the possibility of the diluent damaging the ceramic coating.

[0025] Preferably, the nickel powder is synthesized by chemical method, and the raw materials of the nickel powder include nickel sulfate and other metal salts; the other metal salts are one or more of chromium sulfate, copper sulfate and silver sulfate.

[0026] By adopting the above technical solution, other metals and sulfur are doped into nickel powder to give the nickel powder good voltage resistance and high temperature resistance. This nickel powder is used as a raw material to make nickel paste, and then the nickel paste is used in the manufacture of MLCC, so that MLCC finished products with good voltage resistance and high temperature resistance can be produced.

[0027] Preferably, the nickel powder is synthesized by physical vapor deposition, and the raw materials of the nickel powder include nickel target, sulfur powder and other metal targets; the other metal targets are one or more of chromium target, copper target and silver target.

[0028] By adopting the above technical solution, other metals and sulfur are doped into nickel powder to give the nickel powder good voltage resistance and high temperature resistance. This nickel powder is used as a raw material to make nickel paste, and then the nickel paste is used in the manufacture of MLCC, so that MLCC finished products with good voltage resistance and high temperature resistance can be produced.

[0029] In summary, this application has the following beneficial effects:

[0030] 1. In the present application, nano-BaTiO3 powder is pre-dispersed with a dispersant to obtain a uniformly dispersed nano-BaTiO3 pre-dispersion, and then the nano-BaTiO3 pre-dispersion is mixed with nickel powder and other raw materials in a specific proportion and dispersed to obtain a uniformly dispersed nickel slurry, thereby solving the problem of uneven dispersion of nano-BaTiO3 powder in the nickel slurry for MLCC and improving the performance of the MLCC finished product.

[0031] 2. This application uses epoxy-terminated hyperbranched polyester as a bridge to graft ethyl cellulose onto polyvinyl butyral ester molecules to obtain a binder containing multiple active groups. The binder is added to the nickel paste. Some of the active groups on the binder cross-link with each other to firmly bond the components, and the other part of the active groups bond with the hydroxyl groups on the ceramic coating, so that the nickel paste and the ceramic coating have good adhesion, thereby improving the performance of the MLCC finished product.

[0032] 3. This application modifies nickel powder, introduces sulfur and other metals into the nickel powder, uses this modified nickel powder as a raw material to prepare nickel paste, and then uses the nickel paste for the manufacture of MLCC, which can produce MLCC finished products with good voltage resistance and high temperature resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a SEM image of Example 23 of the present application.

[0034] Figure 2 is a SEM image of Example 24 of the present application.

[0035] Figure 3 is a SEM image of Example 25 of the present application.

[0036] FIG4 is a SEM image of Example 26 of the present application.

[0037] FIG5 is a SEM image of Example 27 of the present application.

[0038] FIG6 is a SEM image of Example 28 of the present application. DETAILED DESCRIPTION

[0039] The present application is further described in detail below with reference to the embodiments.

[0040] Unless otherwise specified, the raw material specifications used in the following examples and comparative examples are shown in Table 1.

[0041] Table 1. Raw material specifications

[0042] Preparation example of adhesive

[0043] Preparation Example 1

[0044] The binder is prepared according to the following steps:

[0045] Preparation of epoxy-terminated hyperbranched polyester: 10 kg of hydroxyl-terminated hyperbranched polyester was mixed evenly with 20 kg of DMF, heated to 60°C, purged with nitrogen, and 1 kg of epichlorohydrin was added. The mixture was kept warm for 3 h, cooled to 30°C, 550 g of a saturated sodium hydroxide solution was added, and the temperature was kept constant for 3 h. 500 g of dichloromethane was added, and the mixture was washed with water three times and dried to obtain epoxy-terminated hyperbranched polyester.

[0046] Preparation of modified polyvinyl butyral: 5 kg of the above-mentioned epoxy-terminated hyperbranched polyester was mixed with 10 kg of DMF, heated to 50°C, and 0.5 kg of polyvinyl butyral was added. The mixture was kept warm for 5 hours and dried to obtain modified polyvinyl butyral.

[0047] Preparation of the binder: 2 kg of the modified polyvinyl butyral prepared above was mixed with 5 kg of DMF, the mixture was heated to 65° C., 1 kg of ethyl cellulose was added, the mixture was kept warm for 8 h, and dried to obtain the binder.

[0048] Preparation Example 2-3

[0049] The difference between the binder and Preparation Example 1 is that the amounts of some materials used in the preparation process of the binder are different. The specific amounts are shown in Table 2 below:

[0050] Table 2. Quality of some materials in the adhesive preparation process

[0051] Preparation example of nickel powder

[0052] Preparation Example a

[0053] Nickel powder is prepared according to the following steps:

[0054] S1: Prepare a mixed solution: weigh 10 kg nickel nitrate and 2 kg sodium citrate dihydrate, and dissolve them in 40 L deionized water;

[0055] S2: Prepare reducing solution: weigh 6.5 kg of 80% hydrazine hydrate, add 8 kg of sodium hydroxide, 1 kg of triethanolamine and 120 L of deionized water, and stir to dissolve;

[0056] S3: Place the mixed solution in an 80°C water bath, add the reducing solution dropwise to the mixed solution, and after reacting for 10 minutes, the solution begins to turn gray and bubbles gradually appear. Add 1.2 kg of triethanolamine and 0.1 kg of polydimethylsiloxane defoaming agent, continue the reaction for 30 minutes, stop cooling, let it stand overnight, pour out the supernatant, wash, and dry in a vacuum drying oven at 70°C to obtain nickel powder.

[0057] Preparation Example b

[0058] The nickel powder differs from that of Preparation Example a in that 10 kg of nickel nitrate is replaced with 9.5 kg of nickel sulfate hexahydrate + 0.2 kg of copper sulfate + 0.3 kg of silver sulfate.

[0059] Preparation Example c

[0060] Nickel powder is prepared according to the following steps:

[0061] S1, screen 10 kg of nickel target and load it into the reactor;

[0062] S2, nitrogen is filled into the reactor and the pressure in the reactor is controlled to 100 kPa;

[0063] S3, ignite the arc, make the arc burn between the plasma gun and the nickel, control the plasma gun current until the nickel particles are completely melted;

[0064] S4, increasing and controlling the current of the plasma gun until the nickel particles gradually evaporate into nickel particles and enter the condenser, forming nickel powder in a collector connected to the condenser.

[0065] Preparation Example d

[0066] Nickel powder is prepared according to the following steps:

[0067] S1, screen 9.8 kg nickel target, 0.1 kg sulfur powder, and 0.1 kg chromium target, and load them into the reactor;

[0068] S2, nitrogen is filled into the reactor and the pressure in the reactor is controlled to 100 kPa;

[0069] S3, ignite the arc, make the arc burn between the plasma gun and the nickel, control the plasma gun current until the nickel particles are completely melted;

[0070] S4, increasing and controlling the current of the plasma gun until the nickel particles gradually evaporate into nickel particles and enter the condenser, forming nickel powder in a collector connected to the condenser.

[0071] Preparation example of diluent

[0072] Preparation Example A

[0073] The diluent is prepared according to the following steps:

[0074] 2 kg of electronic grade terpineol, 5 kg of electronic grade isoborneol acetate and 10 kg of electronic grade butyl acetate were uniformly mixed to prepare a diluent.

[0075] Preparation Example B

[0076] The diluent is prepared according to the following steps:

[0077] 4.85 kg of electronic grade terpineol, 7.3 kg of electronic grade isoborneol acetate and 4.85 kg of electronic grade butyl acetate were uniformly mixed to prepare a diluent.

[0078] Preparation Example C

[0079] The diluent is prepared according to the following steps:

[0080] 1.1 kg of electronic grade terpineol, 5.3 kg of electronic grade isoborneol acetate and 10.6 kg of electronic grade butyl acetate were uniformly mixed to prepare a diluent.

[0081] Preparation Example D

[0082] The diluent is prepared according to the following steps:

[0083] 2.4 kg of electronic grade terpineol, 2.4 kg of electronic grade isoborneol acetate and 12.2 kg of electronic grade butyl acetate were uniformly mixed to prepare a diluent.

[0084] Preparation Example E

[0085] The diluent is prepared according to the following steps:

[0086] 7.6 kg of electronic grade terpineol, 3.1 kg of electronic grade isoborneol acetate and 6.3 kg of electronic grade butyl acetate were uniformly mixed to prepare a diluent.

[0087] Preparation Example F

[0088] The diluent is prepared according to the following steps:

[0089] 1.1 kg of electronic grade terpineol, 10.6 kg of electronic grade isoborneol acetate and 5.3 kg of electronic grade butyl acetate were uniformly mixed to prepare a diluent.

[0090] Preparation Example G

[0091] The diluent is different from that in Preparation Example A in that the diluent in this Preparation Example is 17 kg of electronic grade terpineol.

[0092] Preparation Example H

[0093] The diluent is different from that in Preparation Example A in that the diluent in this Preparation Example is 17 kg of electronic grade isoborneol acetate.

[0094] Preparation Example 1

[0095] The diluent is different from that in Preparation Example A in that the diluent in this Preparation Example is 17 kg of electronic grade butyl acetate.

[0096] Example

[0097] Example 1

[0098] A modified nickel paste for MLCC is prepared according to the following steps:

[0099] Nano-BaTiO3 pre-dispersion: 6 kg of nano-BaTiO3 powder with a particle size of 10 nm, 2 kg of the diluent prepared in Preparation Example A, and 0.1 kg of a dispersant were mixed and stirred in a mixer for 30 min. After uniform mixing, the mixture was ground and dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion. The process parameters of the three-roll mill were as follows: ① the speed ratio of the three rollers was 1:3:9, and the speeds of the three rollers were 50 r / min, 150 r / min, and 450 r / min, respectively; ② the center-height design of the rollers was: the center-height curvature was 50 μm; ③ the temperature of the three rollers was 25°C; ④ the hydraulic pressure of the three rollers was 3 bar, and the pressure between the scraper and the rollers was 1 bar; ⑤ the number of grindings was 5 times;

[0100] Preparation of nickel slurry: 1 kg of BaTiO3 pre-dispersion, 1 kg of binder prepared in Preparation Example 1, 0.01 kg of dispersant, 1 kg of diluent prepared in Preparation Example A, and 3 kg of nickel powder prepared in Preparation Example a were mixed to obtain a mixture, and the mixture was added to a planetary mixer for pre-mixing. The mixed nickel slurry was then added to a three-roll mill for grinding and dispersion. The dispersed nickel slurry was then pressure-filtered with a filter element having a pore size of 15 μm and a pressure of 10 kPa to obtain a modified nickel slurry for MLCC.

[0101] The speed of the disperser disk in the planetary mixer is 100 r / min, the speed of the central axis disk is 200 r / min, the vacuum pressure is 10 kPa, and the mixing time is 60 min.

[0102] Among them, the process parameters of the three-roller machine when dispersing nickel slurry are as follows: ① The speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min respectively; ② The middle and high design of the rollers is: the middle and high arc is 100μm; ③ The temperature of the three rollers is 25℃; ④ The hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the roller is 2bar; ⑤ The number of grinding times is 5 times.

[0103] Example 2

[0104] A modified nickel paste for MLCC is different from Example 1 in the choice of binder. This example uses the binder prepared in Preparation Example 2.

[0105] Example 3

[0106] A modified nickel paste for MLCC is different from Example 1 in the choice of binder. This example uses the binder prepared in Preparation Example 3.

[0107] Example 4

[0108] A modified nickel paste for MLCC is different from Example 1 in the choice of binder. In this example, the binder prepared in Preparation Example 1 is replaced with polyvinyl butyral.

[0109] Example 5

[0110] A modified nickel paste for MLCC is different from Example 1 in the choice of binder. In this example, the binder prepared in Preparation Example 1 is replaced with ethyl cellulose.

[0111] Example 6

[0112] A modified nickel paste for MLCC is prepared according to the following steps:

[0113] Nano-BaTiO3 pre-dispersion: 6.02 kg of nano-BaTiO3 powder with a particle size of 10 nm, 2.01 kg of the diluent prepared in Preparation Example A, and 0.07 kg of the dispersant were mixed, and after uniform mixing, the mixture was dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion; wherein the process parameters of the three-roll mill were the same as those in Example 1;

[0114] Preparation of nickel slurry: 0.85 kg of BaTiO3 pre-dispersion, 1.27 kg of the binder prepared in Preparation Example 1, 0.08 kg of dispersant, 1.27 kg of the diluent prepared in Preparation Example A, and 2.54 kg of the nickel powder prepared in Preparation Example a were mixed to obtain a mixture, and the mixture was added to a planetary mixer for premixing. The mixed nickel slurry was then added to a three-roll mill for dispersion, and the dispersed nickel slurry was pressure filtered to obtain a modified nickel slurry for MLCC; wherein the filter element specifications, planetary mixer process parameters, and three-roll mill process parameters were the same as in Example 1.

[0115] Example 7

[0116] A modified nickel paste for MLCC is prepared according to the following steps:

[0117] Nano-BaTiO3 pre-dispersion: 6.08 kg of nano-BaTiO3 powder with a particle size of 10 nm, 1.94 kg of the diluent prepared in Preparation Example A, and 0.08 kg of a dispersant were mixed and uniformly dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion; wherein the process parameters of the three-roll mill were the same as those in Example 1;

[0118] Preparation of nickel slurry: 0.94 kg of BaTiO3 pre-dispersion, 1.25 kg of the binder prepared in Preparation Example 1, 0.06 kg of dispersant, 1.25 kg of the diluent prepared in Preparation Example A, and 2.51 kg of the nickel powder prepared in Preparation Example a were mixed to obtain a mixture, and the mixture was added to a planetary mixer for premixing. The mixed nickel slurry was then added to a three-roll mill for dispersion, and the dispersed nickel slurry was pressure filtered to obtain a modified nickel slurry for MLCC; wherein the filter element specifications, planetary mixer process parameters, and three-roll mill process parameters were the same as in Example 1.

[0119] Example 8

[0120] A modified nickel paste for MLCC differs from Example 1 in that, in the preparation steps of the nickel paste, the masses of the BaTiO3 pre-dispersion, binder, dispersant, diluent and nickel powder are different. In this embodiment, the masses of the above materials are 0.75 kg, 0.75 kg, 0.01 kg, 0.75 kg and 3.75 kg, respectively.

[0121] Example 9

[0122] A modified nickel paste for MLCC differs from Example 1 in that, in the preparation steps of the nickel paste, the masses of the BaTiO3 predispersion, binder, dispersant, diluent, and nickel powder are different. In this embodiment, the masses of the above materials are 0.667 kg, 0.667 kg, 0.007 kg, 0.667 kg, and 4.002 kg, respectively.

[0123] Example 10

[0124] A modified nickel paste for MLCC is different from Example 1 in that the particle size of the nano-BaTiO3 powder is different. In this embodiment, the particle size of the nano-BaTiO3 powder is 200 nm.

[0125] Examples 11-18

[0126] A modified nickel paste for MLCC differs from Example 1 in that the source of the diluent is different. The specific sources are shown in Table 3 below:

[0127] Table 3. Sources of diluents

[0128] Example 19

[0129] A modified nickel paste for MLCC is different from Example 1 in that the source of nickel powder is different. In this example, the nickel powder prepared in Preparation Example a is replaced with the nickel powder prepared in Preparation Example b.

[0130] Example 20

[0131] A modified nickel paste for MLCC is different from Example 1 in that the source of nickel powder is different. In this example, the nickel powder prepared in Preparation Example a is replaced with the nickel powder prepared in Preparation Example c.

[0132] Example 21

[0133] A modified nickel paste for MLCC is different from Example 1 in that the source of nickel powder is different. In this example, the nickel powder prepared in Preparation Example a is replaced with the nickel powder prepared in Preparation Example d.

[0134] Example 22

[0135] A modified nickel paste for MLCC is different from Example 1 in the choice of binder. The binder of this embodiment is prepared by compounding 0.5 kg of polyvinyl butyral and 0.5 kg of ethyl cellulose.

[0136] Example 23

[0137] A modified nickel paste for MLCC is prepared according to the following steps:

[0138] Nano-BaTiO3 pre-dispersion: 750g of nano-BaTiO3 powder with a particle size of 150nm, 240g of the diluent obtained in Preparation Example A, and 10g of a dispersant were mixed, stirred in a mixer for 30min, and after uniform mixing, ground and dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion; wherein the process parameters of the three-roll mill are as follows: ① the speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min, respectively; ② the middle and high design of the rollers is: the middle and high curvature is 50μm; ③ the temperature of the three rollers is 25°C; ④ the hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the rollers is 1bar; ⑤ the number of grindings is 5 times;

[0139] Preparation of nickel slurry: The above-mentioned BaTiO3 pre-dispersion, the binder prepared in Preparation Example 1, the dispersant DISPERBYK-108, the diluent prepared in Preparation Example A, and the nickel powder with a particle size of 600nm prepared in Preparation Example b were mixed in a mass ratio of 20:20:1:20:50 (the mass of the BaTiO3 pre-dispersion was 600g) to obtain a mixture, and the mixture was added to a planetary mixer for pre-mixing. The mixed nickel slurry was then added to a three-roll mill for grinding and dispersion, and the dispersed nickel slurry was pressure-filtered with a filter element having a pore size of 15μm and a pressure of 10kPa to obtain a modified nickel slurry for MLCC.

[0140] The speed of the disperser disk in the planetary mixer is 100 r / min, the speed of the central axis disk is 200 r / min, the vacuum pressure is 10 kPa, and the mixing time is 60 min.

[0141] Among them, the process parameters of the three-roller machine when dispersing nickel slurry are as follows: ① The speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min respectively; ② The middle and high design of the rollers is: the middle and high arc is 100μm; ③ The temperature of the three rollers is 25℃; ④ The hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the roller is 2bar; ⑤ The number of grinding times is 5 times.

[0142] Example 24

[0143] A modified nickel paste for MLCC is prepared according to the following steps:

[0144] Nano-BaTiO3 pre-dispersion: 750g of nano-BaTiO3 powder with a particle size of 100nm, 240g of the diluent obtained in Preparation Example A, and 10g of a dispersant were mixed, stirred in a mixer for 30min, and after uniform mixing, ground and dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion; wherein the process parameters of the three-roll mill are as follows: ① the speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min, respectively; ② the middle and high design of the rollers is: the middle and high curvature is 50μm; ③ the temperature of the three rollers is 25°C; ④ the hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the rollers is 1bar; ⑤ the number of grindings is 5 times;

[0145] Preparation of nickel slurry: The above-mentioned BaTiO3 pre-dispersion, the binder prepared in Preparation Example 1, the dispersant DISPERBYK-108, the diluent prepared in Preparation Example A, and the nickel powder with a particle size of 400nm prepared in Preparation Example b are mixed in a mass ratio of 20:20:1:20:50 (the mass of the BaTiO3 pre-dispersion is 600g) to obtain a mixture, and the mixture is added to a planetary mixer for pre-mixing. The mixed nickel slurry is then added to a three-roll mill for grinding and dispersion, and the dispersed nickel slurry is pressure-filtered. The pore size of the filter element is 15μm and the pressure is 10kPa. Finally, a modified nickel slurry for MLCC is obtained;

[0146] The speed of the disperser disk in the planetary mixer is 100 r / min, the speed of the central axis disk is 200 r / min, the vacuum pressure is 10 kPa, and the mixing time is 60 min.

[0147] Among them, the process parameters of the three-roller machine when dispersing nickel slurry are as follows: ① The speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min respectively; ② The middle and high design of the rollers is: the middle and high arc is 100μm; ③ The temperature of the three rollers is 25℃; ④ The hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the roller is 2bar; ⑤ The number of grinding times is 5 times.

[0148] Example 25

[0149] A modified nickel paste for MLCC is prepared according to the following steps:

[0150] Nano-BaTiO3 pre-dispersion: 750g of nano-BaTiO3 powder with a particle size of 80nm, 240g of the diluent obtained in Preparation Example A, and 10g of a dispersant were mixed and stirred in a mixer for 30min. After uniform mixing, the mixture was ground and dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion; wherein the process parameters of the three-roll mill are as follows: ① the speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min, respectively; ② the middle and high design of the rollers is: the middle and high curvature is 50μm; ③ the temperature of the three rollers is 25°C; ④ the hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the rollers is 1bar; ⑤ the number of grindings is 5 times;

[0151] Preparation of nickel slurry: The above-mentioned BaTiO3 pre-dispersion, the binder prepared in Preparation Example 1, the dispersant DISPERBYK-108, the diluent prepared in Preparation Example A, and the nickel powder with a particle size of 400nm prepared in Preparation Example b are mixed in a mass ratio of 20:20:1:20:50 (the mass of the BaTiO3 pre-dispersion is 600g) to obtain a mixture, and the mixture is added to a planetary mixer for pre-mixing. The mixed nickel slurry is then added to a three-roll mill for grinding and dispersion, and the dispersed nickel slurry is pressure-filtered. The pore size of the filter element is 15μm and the pressure is 10kPa. Finally, a modified nickel slurry for MLCC is obtained;

[0152] The speed of the disperser disk in the planetary mixer is 100 r / min, the speed of the central axis disk is 200 r / min, the vacuum pressure is 10 kPa, and the mixing time is 60 min.

[0153] Among them, the process parameters of the three-roller machine when dispersing nickel slurry are as follows: ① The speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min respectively; ② The middle and high design of the rollers is: the middle and high arc is 100μm; ③ The temperature of the three rollers is 25℃; ④ The hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the roller is 2bar; ⑤ The number of grinding times is 5 times.

[0154] Example 26

[0155] A modified nickel paste for MLCC is prepared according to the following steps:

[0156] Nano-BaTiO3 pre-dispersion: 750g of nano-BaTiO3 powder with a particle size of 60nm, 240g of the diluent obtained in Preparation Example A, and 10g of a dispersant were mixed and stirred in a mixer for 30min. After uniform mixing, the mixture was ground and dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion. The process parameters of the three-roll mill were as follows: ① the speed ratio of the three rollers was 1:3:9, and the speeds of the three rollers were 50r / min, 150r / min, and 450r / min, respectively; ② the center-height design of the rollers was: the center-height curvature was 50μm; ③ the temperature of the three rollers was 25°C; ④ the hydraulic pressure of the three rollers was 3bar, and the pressure between the scraper and the rollers was 1bar; ⑤ the number of grindings was 5 times;

[0157] Preparation of nickel slurry: The above-mentioned BaTiO3 pre-dispersion, the binder prepared in Preparation Example 1, the dispersant DISPERBYK-108, the diluent prepared in Preparation Example A, and the nickel powder prepared in Preparation Example b with a particle size of 300nm are mixed in a mass ratio of 20:20:1:20:50 (the mass of the BaTiO3 pre-dispersion is 600g) to obtain a mixture, and the mixture is added to a planetary mixer for pre-mixing. The mixed nickel slurry is then added to a three-roll mill for grinding and dispersion, and the dispersed nickel slurry is pressure-filtered. The pore size of the filter element is 15μm and the pressure is 10kPa. Finally, a modified nickel slurry for MLCC is obtained;

[0158] The speed of the disperser disk in the planetary mixer is 100 r / min, the speed of the central axis disk is 200 r / min, the vacuum pressure is 10 kPa, and the mixing time is 60 min.

[0159] Among them, the process parameters of the three-roller machine when dispersing nickel slurry are as follows: ① The speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min respectively; ② The middle and high design of the rollers is: the middle and high arc is 100μm; ③ The temperature of the three rollers is 25℃; ④ The hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the roller is 2bar; ⑤ The number of grinding times is 5 times.

[0160] Example 27

[0161] A modified nickel paste for MLCC is prepared according to the following steps:

[0162] Nano-BaTiO3 pre-dispersion: 750g of nano-BaTiO3 powder with a particle size of 50nm, 240g of the diluent obtained in Preparation Example A, and 10g of a dispersant were mixed and stirred in a mixer for 30min. After uniform mixing, the mixture was ground and dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion. The process parameters of the three-roll mill were as follows: ① the speed ratio of the three rollers was 1:3:9, and the speeds of the three rollers were 50r / min, 150r / min, and 450r / min, respectively; ② the center-height design of the rollers was: the center-height curvature was 50μm; ③ the temperature of the three rollers was 25°C; ④ the hydraulic pressure of the three rollers was 6bar, and the pressure between the scraper and the rollers was 5bar; ⑤ the number of grindings was 5 times;

[0163] Preparation of nickel slurry: The above-mentioned BaTiO3 pre-dispersion, the binder prepared in Preparation Example 1, the dispersant DISPERBYK-108, the diluent prepared in Preparation Example A, and the nickel powder prepared in Preparation Example b with a particle size of 300nm are mixed in a mass ratio of 20:20:1:20:50 (the mass of the BaTiO3 pre-dispersion is 600g) to obtain a mixture, and the mixture is added to a planetary mixer for pre-mixing. The mixed nickel slurry is then added to a three-roll mill for grinding and dispersion, and the dispersed nickel slurry is pressure-filtered. The pore size of the filter element is 15μm and the pressure is 10kPa. Finally, a modified nickel slurry for MLCC is obtained;

[0164] The speed of the disperser disk in the planetary mixer is 100 r / min, the speed of the central axis disk is 200 r / min, the vacuum pressure is 10 kPa, and the mixing time is 60 min.

[0165] Among them, the process parameters of the three-roller machine when dispersing nickel slurry are as follows: ① The speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min respectively; ② The middle and high design of the rollers is: the middle and high arc is 100μm; ③ The temperature of the three rollers is 25℃; ④ The hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the roller is 2bar; ⑤ The number of grinding times is 5 times.

[0166] Example 28

[0167] A modified nickel paste for MLCC is prepared according to the following steps:

[0168] Nano-BaTiO3 pre-dispersion: 750g of nano-BaTiO3 powder with a particle size of 40nm, 240g of the diluent obtained in Preparation Example A, and 10g of a dispersant were mixed and stirred in a mixer for 30min. After uniform mixing, the mixture was ground and dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion. The process parameters of the three-roll mill were as follows: ① the speed ratio of the three rollers was 1:3:9, and the speeds of the three rollers were 50r / min, 150r / min, and 450r / min, respectively; ② the center-height design of the rollers was: the center-height curvature was 50μm; ③ the temperature of the three rollers was 25°C; ④ the hydraulic pressure of the three rollers was 3bar, and the pressure between the scraper and the rollers was 1bar; ⑤ the number of grindings was 5 times;

[0169] Preparation of nickel slurry: The above-mentioned BaTiO3 pre-dispersion, the binder prepared in Preparation Example 1, the dispersant DISPERBYK-108, the diluent prepared in Preparation Example A, and the nickel powder with a particle size of 200nm prepared in Preparation Example b are mixed in a mass ratio of 20:20:1:20:50 (the mass of the BaTiO3 pre-dispersion is 600g) to obtain a mixture, and the mixture is added to a planetary mixer for pre-mixing. The mixed nickel slurry is then added to a three-roll mill for grinding and dispersion, and the dispersed nickel slurry is pressure-filtered. The pore size of the filter element is 15μm and the pressure is 10kPa. Finally, a modified nickel slurry for MLCC is obtained;

[0170] The speed of the disperser disk in the planetary mixer is 100 r / min, the speed of the central axis disk is 200 r / min, the vacuum pressure is 10 kPa, and the mixing time is 60 min.

[0171] Among them, the process parameters of the three-roller machine when dispersing nickel slurry are as follows: ① The speed ratio of the three rollers is 1:3:9, and the speeds of the three rollers are 50r / min, 150r / min, and 450r / min respectively; ② The middle and high design of the rollers is: the middle and high arc is 100μm; ③ The temperature of the three rollers is 25℃; ④ The hydraulic pressure of the three rollers is 3bar, and the pressure between the scraper and the roller is 2bar; ⑤ The number of grinding times is 5 times.

[0172] Comparative Example

[0173] Comparative Example 1

[0174] A modified nickel paste for MLCC is prepared according to the following steps:

[0175] 0.74 kg of nano-BaTiO3 powder with a particle size of 10 nm, 1 kg of the binder prepared in Preparation Example 1, 0.02 kg of dispersant, 1.25 kg of the diluent prepared in Preparation Example A, and 3 kg of the nickel powder prepared in Preparation Example a were mixed to obtain a mixture, and the mixture was added to a planetary mixer for premixing. The mixed nickel slurry was then added to a three-roll mill for dispersion, and the dispersed nickel slurry was pressure filtered to obtain a modified nickel slurry for MLCC; wherein the filter element specifications, planetary mixer process parameters, and three-roll mill process parameters are the same as in Example 1.

[0176] Comparative Example 2

[0177] A modified nickel paste for MLCC is prepared according to the following steps:

[0178] Nano-BaTiO3 pre-dispersion: 6 kg of nano-BaTiO3 powder with a particle size of 10 nm, 2 kg of the diluent prepared in Preparation Example A, and 0.1 kg of a dispersant were mixed, and after uniform mixing, the mixture was dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion; wherein the process parameters of the three-roll mill were the same as those in Example 1;

[0179] Preparation of nickel slurry: 0.55 kg of BaTiO3 pre-dispersion, 1.09 kg of the binder prepared in Preparation Example 1, 0.01 kg of dispersant, 1.09 kg of the diluent prepared in Preparation Example A, and 3.27 kg of the nickel powder prepared in Preparation Example a were mixed to obtain a mixture, and the mixture was added to a planetary mixer for premixing. The mixed nickel slurry was then added to a three-roll mill for dispersion, and the dispersed nickel slurry was pressure filtered to obtain a modified nickel slurry for MLCC; wherein the filter element specifications, planetary mixer process parameters, and three-roll mill process parameters were the same as in Example 1.

[0180] Comparative Example 3

[0181] A modified nickel paste for MLCC is prepared according to the following steps:

[0182] Nano-BaTiO3 pre-dispersion: 6 kg of nano-BaTiO3 powder with a particle size of 10 nm, 2 kg of the diluent prepared in Preparation Example A, and 0.1 kg of a dispersant were mixed, and after uniform mixing, the mixture was dispersed on a three-roll mill to obtain a nano-BaTiO3 pre-dispersion; wherein the process parameters of the three-roll mill were the same as those in Example 1;

[0183] Preparation of nickel slurry: 2 kg of BaTiO3 pre-dispersion, 0.8 kg of binder prepared in Preparation Example 1, 0.01 kg of dispersant, 0.8 kg of diluent prepared in Preparation Example A and 2.4 kg of nickel powder prepared in Preparation Example a were mixed to obtain a mixture, and the mixture was added to a planetary mixer for premixing. The mixed nickel slurry was then added to a three-roll mill for dispersion, and the dispersed nickel slurry was pressure filtered to obtain a modified nickel slurry for MLCC; wherein the filter element specifications, planetary mixer process parameters, and three-roll mill process parameters were the same as in Example 1.

[0184] Detection method

[0185] Dispersion test: Using a surface roughness tester, the modified nickel paste for MLCC prepared in Examples 1-28 and Comparative Examples 1-3 was screen-printed onto a glass substrate with a regular pattern of length × width = 10 mm × 10 mm. After drying in a bag drying oven, the surface roughness Ra and Rt were measured to characterize the dispersion performance of the modified nickel paste. The lower the roughness, the better the dispersion performance.

[0186] Electrical performance test: Take the modified nickel paste for MLCC prepared in Examples 1-28 and Comparative Examples 1-3, and prepare MLCC according to the following process: first, design the thickness of the porcelain powder casting film according to the size specifications of the MLCC and the K value of the selected porcelain powder, and then go through the porcelain powder casting film (porcelain paste preparation and porcelain film casting) - internal electrode production (nickel paste screen printing and bottom layer) - capacitor chip production (lamination and cutting separation) - sintering into porcelain (binding removal, sintering and chamfering) - external electrode production (capping, sintering and electroplating);

[0187] A four-parameter testing machine was used to perform performance tests on the MLCCs prepared above (each embodiment / comparative example was a group, and 50 MLCCs were made in each group). The capacitance, loss, withstand voltage and TCC at 200°C of the MLCC were tested. TCC = (C(200°C) - C(25°C)) / C(25°C) × 100%. The smaller the absolute value of TCC, the better the high temperature resistance of the MLCC (C(200°C) and C(25°C) represent the capacitance of the MLCC at different temperatures). The test voltage was 1V and the frequency was 1kHz. The specific test results are shown in Table 4 below.

[0188] The capacitance, loss, and TCC at 200°C are the average values ​​of 50 MLCCs, and the withstand voltage is a range value.

[0189] Accelerated aging test: The MLCC prepared above was placed in an aging box (each embodiment / comparative example was a group, and each group corresponded to 100 MLCCs). Under the conditions of 8Ur, 150°C, and 8h, the capacity (C), loss (DF), and insulation resistance (IR) of the MLCC before and after entering the box were tested. The products that met |ΔC / C|≤20%, DF≤2 times the initial value, and IR≥2000mΩ were qualified products. The pass rate of each group was tested to characterize the adhesion performance of the modified nickel paste and the ceramic coating and the effect of the diluent on the ceramic coating (pass rate = number of qualified products / 100).

[0190] Table 4. Performance test

[0191] It can be seen from Table 4 that the nickel paste prepared in the embodiment of the present application has Ra≤0.083μm and Rt≤0.692μm, indicating that the nickel paste prepared in the embodiment of the present application has better dispersion performance and the nano-BaTiO3 powder is well dispersed in the nickel paste; the MLCC made using the nickel paste prepared in the embodiment of the present application has a capacitance ≥0.95uF, a loss ≤2.9%, a withstand voltage ≥345V, an absolute value of TCC at 200°C ≤13.1, and a qualified rate under the accelerated aging test ≥85%, which indicates that the MLCC finished product has better performance.

[0192] Combining Example 1 and Comparative Example 1 and Table 4, it can be seen that the roughness of the nickel paste in Example 1 is much smaller than that in Comparative Example 1, and the various performances of the MLCC finished product made from the nickel paste in Example 1 are also better than those in Comparative Example 1, which shows that: in Example 1, the nano-BaTiO3 powder is first pre-dispersed with a dispersant to obtain a uniformly dispersed nano-BaTiO3 pre-dispersion, and then the nano-BaTiO3 pre-dispersion is mixed with nickel powder and other raw materials in a specific proportion and dispersed to obtain a uniformly dispersed nickel paste, thereby solving the problem of uneven dispersion of nano-BaTiO3 powder in the nickel paste for MLCC and improving the performance of the MLCC finished product.

[0193] Combining Example 1 and Comparative Examples 2-3 and Table 4, it can be seen that the roughness of the nickel paste in Example 1 is much smaller than that of Comparative Examples 2-3, and the various performances of the MLCC finished product made from the nickel paste of Example 1 are also better than those of Comparative Examples 2-3. This may be because: the mass ratio of BaTiO3 predispersion, binder, dispersant, diluent, and nickel powder in Comparative Examples 2-3 exceeds the scope of this application. After many experiments, the inventors controlled the mass ratio of the above raw materials so that the above raw materials were evenly dispersed in the nickel paste, thereby improving the performance of the MLCC finished product.

[0194] Combining Example 1 and Examples 11-18 and Table 4, it can be seen that the qualified rate of the MLCC finished products prepared by Example 1 and Example 11 is much higher than that of Examples 12-18. This may be because: the diluent selected in Example 1 and Example 11 is compounded by terpineol, isoborneol acetate and butyl acetate in a specific mass ratio. After many experiments, the inventors found that the use of the above diluent can reduce the damage to the ceramic coating, thereby improving the aging resistance of the MLCC finished product.

[0195] Combining Examples 1-5 and 22 with Table 4, it can be seen that the qualified rate of the MLCC products prepared by Example 1-3 is much higher than that of Examples 4-5 and 22. This may be because the binder selected in Example 1-3 is different from that in Examples 4-5 and 22. In Example 1-3, ethyl cellulose is grafted onto polyvinyl butyral molecules using an epoxy-terminated hyperbranched polyester as a bridge, resulting in a binder containing multiple active groups. When the binder is added to the nickel paste, some of the active groups on the binder cross-link with each other to firmly bond the components, while other active groups bond with the hydroxyl groups on the ceramic coating, resulting in good adhesion between the nickel paste and the ceramic coating, thereby improving the performance of the MLCC products.

[0196] The binder of Example 4 is pure polyvinyl butyral, the binder of Example 5 is pure ethyl cellulose, and the binder of Example 22 is a simple compound of polyvinyl butyral and ethyl cellulose. The adhesion of these three binders to the ceramic coating is weaker than the binders selected in Examples 1-3.

[0197] Combining Example 1 and Examples 19-21 and Table 4, it can be seen that the withstand voltage values ​​of the MLCC finished products prepared by Example 19 and Example 21 are much higher than those of Example 1 and Example 20, and the absolute values ​​of TCC at 200°C of the MLCC finished products prepared by Example 19 and Example 21 are lower than those of Example 1 and Example 20. This may be because: the nickel powder selected in Example 19 and Example 21 is doped with sulfur and other metals, and has good voltage resistance and high temperature resistance compared with the nickel powder selected in Example 1 and Example 20. Using this nickel powder for the preparation of MLCC can fundamentally improve the withstand voltage and high temperature resistance of MLCC.

[0198] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed, but as long as they are within the scope of the claims of the present application, they are protected by the patent law.

Claims

1. A method for preparing a modified nickel paste for MLCC, characterized in that: The steps include: Nano-BaTiO3 pre-dispersion: Nano-BaTiO3 powder, diluent, and dispersant are mixed and dispersed in a mass ratio of (60-90):(20-30):1 to obtain a nano-BaTiO3 pre-dispersion; Preparation of nickel paste: BaTiO3 pre-dispersion, binder, dispersant, diluent and nickel powder are mixed and dispersed in a mass ratio of 10:(10-15):(0.1-1):(10-15):(25-60), and filtered to obtain a modified nickel paste for MLCC; The preparation method of the binder comprises the following steps: Preparation of epoxy-terminated hyperbranched polyester: reacting hydroxy-terminated hyperbranched polyester with epichlorohydrin in a mass ratio of (10-20):1 to obtain epoxy-terminated hyperbranched polyester; Preparation of modified polyvinyl butyral ester: reacting terminal epoxy hyperbranched polyester with polyvinyl butyral ester at a mass ratio of (10-25):1 to obtain modified polyvinyl butyral ester; Preparation of the binder: Modified polyvinyl butyral ester and ethyl cellulose are reacted in a mass ratio of (2-10):1 to obtain a binder.

2. The method for preparing a modified nickel paste for MLCC according to claim 1, characterized in that: The mass ratio of the BaTiO3 pre-dispersion to the nickel powder is 10:(50-60).

3. The method for preparing a modified nickel paste for MLCC according to claim 1, characterized in that: The particle size of the nano BaTiO3 powder is 10-200nm.

4. The method for preparing a modified nickel paste for MLCC according to claim 1, characterized in that: The diluent is one or more of terpineol, isoborneol acetate, isophorone and butyl acetate.

5. The method for preparing a modified nickel paste for MLCC according to claim 4, characterized in that: The diluent is prepared by compounding pinene alcohol, isoborneol acetate and butyl acetate in a mass ratio of (0.2-1):(0.5-1.5):

1.

6. The method for preparing a modified nickel paste for MLCC according to claim 1, characterized in that: The nickel powder is synthesized by chemical method, and the raw materials of the nickel powder include nickel sulfate and other metal salts; the other metal salts are one or more of chromium sulfate, copper sulfate and silver sulfate.

7. The method for preparing a modified nickel paste for MLCC according to claim 1, characterized in that: The nickel powder is synthesized by physical vapor deposition, and the raw materials of the nickel powder include nickel target, sulfur powder and other metal target; the other metal target is one or more of chromium target, copper target and silver target.

Citation Information

Patent Citations

  • Nickel electrode slurry, preparation method and application thereof

    CN112768234A

  • Preparation method of modified nickel paste for MLCC

    CN116313512A

  • A Method for Preparing Metal Inner Electrode PasteHaving High Dispersibility for Having Super HighCapacity Multi Layer Ceramic Capacitor