Porous glass material with uniform pore channels, and atomizing core and electronic atomizer

By optimizing the pore channel structure and process in porous glass materials, the problems of uneven liquid conduction velocity and local overheating caused by uneven pore channels of existing pore glass materials are solved, and more uniform liquid conduction and temperature distribution is achieved, improving electronics Performance and service life of the atomizer.

WO2024239803A1PCT designated stage expired Publication Date: 2024-11-28SMOORE INTERNATIONAL HOLDINGS LIMITED +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/085494
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-04-02
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The pore channels of existing pores and glass materials are uneven, resulting in large differences in the transmission speed of the atomized liquid matrix, which is prone to insufficient oil supply and local overheating, resulting in coking and carbon deposits, affecting the suction experience and life of the electronic atomizer.

Method used

Using porous glass material with uniform pore channels, by adjusting the average diameter and distribution range of pore throat, combining the glass-covered fiber tread structure and optimized sintering process, a multi-directional communication hole structure is prepared to improve the fluid conduction speed and temperature field uniformity. sex.

Benefits of technology

The liquid conduction speed is improved, local overheating and carbon deposits are avoided, the suction experience and atomization effect are improved, and the overall uniformity and temperature field uniformity of porous glass materials are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024085494_28112024_PF_FP_ABST
    Figure CN2024085494_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of porous materials, and particularly relates to a porous glass material with uniform pore channels, and an atomizing core and an electronic atomizer. The porous glass material with uniform pore channels comprises a framework, and multi-directional communicating pores, which are in communication with each other by means of pore throats, wherein the average diameter of the pore throats is 25-45 microns, the pore throats are distributed within a range of 5-60 microns, and not less than 50% of the pore throats are distributed within a range of 20-45 microns. In the present application, the sizes of the pore throats are defined to make the sizes of communicating channels among the pores uniform, such that local overheating due to a non-uniform liquid guide speed during use of the atomizing core is prevented, and thus local burning and carbon deposition are prevented, and almost no reduction of the amount of vapor is realized in a vaping process. Compared with commercially available ceramic heating elements, under the same conditions, a porous glass matrix is not prone to carbon deposition after e-cigarette vaping. In addition, the liquid guide speed is obviously increased, and compared with commercially available porous ceramic heating elements, the liquid guide speed can be at most increased by not less than 33%.
Need to check novelty before this filing date? Find Prior Art

Description

A porous glass material with uniform pore channels, an atomizing core, and an electronic atomizer

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on May 19, 2023, with application number 202310574687.9 and invention name “A porous glass material with uniform pore channels, atomizing core and electronic atomizer”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application belongs to the technical field of porous materials, and specifically relates to a porous glass material with uniform pore channels, an atomizing core, and an electronic atomizer. Background Art

[0004] An electronic vaporizer is a product that transforms a vaporized medium into vapor through atomization and other means for the user to inhale. The atomizer core is the core component of the electronic vaporizer and plays a crucial role in its performance, including taste and aerosol volume.

[0005] Most closed electronic atomizers use porous ceramics as the atomization core. Most of them use diatomaceous earth, silicon oxide, aluminum oxide, etc. as raw materials, add glass powder, pore-forming agents, etc., and produce porous ceramics by sintering the prepared particles. The use of porous ceramics as the atomization core has the characteristics of good uniformity, long life, delicate taste, and high degree of mechanization. However, the porous ceramic heating element has a certain proportion of semi-closed pores and fine pores, which easily cause the adsorption of low-viscosity components in the atomization medium, thereby affecting the suction taste and aroma restoration. At the same time, the microscopic surface of the porous ceramic heating element is rough and has low continuity, and it cannot be used with a thin film heating film.

[0006] Compared to porous ceramics, porous glass has a smooth, continuous microstructure and a low proportion of micro- and nanopores, making it less susceptible to adsorption of the atomized medium. This, to a certain extent, improves the taste and aroma reproduction of electronic atomizers. However, the porous glass used in existing technologies has an uneven pore structure and large variations in the size of the pore channels, resulting in large variations in the transmission speed of the atomized liquid matrix. In areas where the atomized liquid matrix transmission speed is slow, insufficient oil supply can easily occur, leading to local overheating, localized coking, and carbon deposits. This, in turn, seriously affects the customer's puffing experience as the puff progresses, accelerating the failure of the e-cigarette. Furthermore, the liquid transmission speed needs to be further improved.

[0007] Summary of the Invention

[0008] Therefore, the technical problem to be solved by the present application is to overcome the above-mentioned defects of the porous glass materials in the prior art, especially the series of problems caused by large differences in pore channels and the need to improve the liquid conduction speed, so as to provide a porous glass material with uniform pore channels, an atomizing core and an electronic atomizer.

[0009] To this end, this application provides the following technical solutions:

[0010] The present application provides a porous glass material with uniform pore channels, comprising a skeleton and multi-directional connected pores, wherein the multi-directional connected pores are interconnected by pore throats, wherein:

[0011] The average diameter of the pore throats is 25-45 microns, and the pore throats are distributed in the range of 5-60 microns, wherein more than 50% of the pore throats are distributed in the range of 20-45 microns.

[0012] Optionally, the average diameter of the pore throats is 28-36 microns, the pore throats are distributed in the 10-55 micron region, and more than 90% of the pore throats are distributed in the 20-45 micron region.

[0013] Optionally, the average diameter of the pore throats is about 29-35 microns, the pore throats are distributed in the range of 12-50 microns, and the proportion of pore throats distributed in the range of 20-45 microns is greater than 95%;

[0014] Optionally, the pore throats are distributed between 20 and 45 microns.

[0015] Optionally, the skeleton is a glass-coated fiber scaffolding structure, including a scaffolding body and a connector connecting the scaffolding bodies: the average diameter of the scaffolding body is 20 to 45 microns, and the average length is 60 to 100 microns.

[0016] Optionally, the multi-directional connecting holes have a diameter of 70-100 microns.

[0017] Optionally, the porosity of the porous glass material is 65-80%, optionally 70-74%.

[0018] Optionally, the porous glass material has a liquid conduction rate of 0.09 mm / s or more at room temperature for an atomized matrix with a viscosity of 230 cP; optionally, the liquid conduction rate at room temperature is 0.10 mm / s or more; further optionally, the liquid conduction rate at room temperature is 0.12 mm / s or more.

[0019] The present application also provides an atomizing core, which uses the above-mentioned porous glass material as a substrate, and a heating unit is provided on the substrate.

[0020] Optionally, during the atomization process, the temperature field deviation of the atomizer core is less than 10°C.

[0021] The present application also provides an electronic atomizer, comprising the above-mentioned atomization core.

[0022] The porous glass substrate can be in the shape of a flat rectangular parallelepiped, a cylinder, or a special-shaped structure. The thickness of the atomized surface is 0.5-4 mm, and optionally 1.5-2.5 mm. Typically, but not limited to, the outer dimensions of the porous glass substrate are 9.0 mm in length, 4.0 mm in width, and 1.6±0.1 (mm), 2.0±0.2 (mm), or 2.4±0.1 (mm) thick. Alternatively, the outer dimensions of the porous glass substrate are 7.4 mm in length, 4.0 mm in width, and 1.6±0.1 (mm), 2.0±0.2 (mm), or 2.4±0.1 (mm) thick.

[0023] The preparation method of the porous glass material generally includes the following steps: mixing glass powder, fiber components, and pore-forming agents to prepare a green body, performing debinding, and sintering.

[0024] Optionally, the fiber component has a diameter of 3-30 μm and a length of 20-500 μm;

[0025] Optionally, the fiber component has a diameter of 10-25 μm and a length of 20-150 μm.

[0026] Optionally, the aspect ratio of the fiber component is 1-10, and optionally, the aspect ratio of the fiber with a length of 50-150 μm is 2-5;

[0027] And / or, in the fiber component, fibers with a fiber length of more than 50 μm account for 25%, optionally, account for more than 40%; further optionally, account for 40-100%.

[0028] Based on the total mass of the glass powder and the fiber component, the glass powder accounts for 40-62%, and the fiber component accounts for 38-60%;

[0029] And / or, the amount of the pore former is 0.3-2.5 times the total mass of the glass powder and fiber components.

[0030] Select any one of the following processes: tape casting, injection molding, dry pressing, and gel casting to prepare the green body;

[0031] The above-mentioned processes for preparing green compacts are all known in the art, and appropriate processing aids may be added depending on the process selected. Typically, and not limitingly, the gel casting process generally involves the following steps: first, the materials are mixed uniformly, then the mixed materials are added to a sol solution, and stirred at a certain temperature until a paste forms. This paste is then injected into a mold of a corresponding shape and cooled to form a green compact.

[0032] And / or, the debinding temperature is 200-800°C, and the debinding time is 5-50h; optionally, the debinding temperature is 200-350°C.

[0033] And / or, the sintering temperature is 900-1250° C. or 1180-1320° C., and the sintering time is 10-180 min.

[0034] Optionally, the method for preparing the porous glass satisfies at least one of the following (1)-(5):

[0035] (1) The softening temperature of the glass powder is 600-1200°C; the softening point of the selected fiber raw material is above the sintering temperature in the preparation method and can play a skeleton role;

[0036] (2) The particle size of the glass powder is less than 10 μm, and optionally, the particle size is less than 3000 mesh;

[0037] (3) The fiber component is at least one of silicon carbide fiber, silicon nitride fiber, aluminum silicate fiber, quartz fiber, mullite fiber, alumina fiber, hydroxyapatite fiber, and zirconium oxide fiber;

[0038] (4) The pore-forming agent material is one or a mixture of materials such as carbon powder, polystyrene, polymethyl methacrylate, polylactic acid, polyvinyl alcohol, polyethylene terephthalate, engineering plastics, starch, cellulose, sawdust, and graphite powder that can be decomposed, volatilized, or burned at high temperatures;

[0039] (5) The particle size of the pore former is 10-300 μm, and optionally, the average particle size of the pore former is 80 μm. A porous glass material with better connectivity can be obtained by adjusting the addition ratio of pore formers of different diameters.

[0040] In order to obtain the porous glass material with this special pore structure, the glass raw materials and fiber materials are pretreated as follows:

[0041] 1. The raw glass powder particle size should be less than 10 microns, and glass powder with a mesh size of 3000 or less can be used. To obtain glass powder with uniform particle size, commercially available glass powder can be milled in a high-energy planetary ball mill at a speed of 200-500 rpm using ethanol as a solvent for 3-5 hours. The powder can then be dried and sieved before use.

[0042] 2. The fiber can be high-temperature resistant fibers such as mullite fiber, zirconia fiber or alumina. In this case, mullite fiber can be selected, with a fiber diameter of 10-25 microns, a length of less than 150 microns, and a fiber aspect ratio of 1-10. Generally, commercially available 2-5mm chopped fibers are first crushed to less than 0.5mm by a crusher, and then high-energy planetary ball milling is performed for 2-8 hours using ethanol as a solvent and stearic acid as a grinding aid. The ball milling speed is 100-400r / min. Optionally, the ball milling is performed at 300r / min. The ball-milled fiber is washed with ethanol and dried through a 100-mesh sieve to obtain the target fiber. Optionally, the ball milling time is 6 hours to obtain the target fiber. More preferably, the target fiber is a fiber between 300 mesh and 100 mesh sieved after ball milling for 6 hours.

[0043] In order to obtain a porous glass matrix with more uniform pore size, a spherical pore former is selected. The pore former has a particle size of 50 microns, 80 microns, or a mixture of multiple types mixed in a certain proportion.

[0044] Specifically, the porous glass in this application is prepared by gel casting, and the preparation method is as follows:

[0045] Glass powder, fiber, and pore-forming agent are mixed in a certain proportion and mixed in a three-dimensional mixer for 2 hours until uniform. The mixed materials are then added to an 80°C agar polysaccharide sol solution and slowly stirred until a uniform paste is formed. The mixture is then injected into the corresponding mold and cooled to obtain a green body. The green body is first cured at 60°C for 1-5 hours, then heated to 200°C over 200 minutes, and then heated to 500°C at 0.5°C per minute. A 2-hour holding time is set at 240°C, 300°C, and 350°C respectively. The temperature is then raised at 5°C per minute to 1150°C-1320°C, held for 15-30 minutes, and naturally cooled to room temperature to obtain a porous glass material. Generally, the optimal debinding process can be obtained based on the thermogravimetric curve of the pore-forming agent.

[0046] Alternatively, the strength and sintering properties of porous glass materials can be improved by adding glass powder binders and / or ceramic fiber materials. Generally, the addition or increase of ceramic powder and non-effective ceramic fibers will reduce the porosity of the porous glass matrix. Generally, hollow glass microspheres, glass powder, and / or ceramic fibers are mixed uniformly in a three-dimensional mixer. The mixed material is then added to an 80°C agar polysaccharide sol solution and slowly stirred until a uniform paste forms. The mixture is then poured into a mold and cooled to produce a green body. The green body is first cured at 60°C for 1-5 hours, then heated to 200°C over 200 minutes, then increased at 0.5°C / minute to 500°C, with a 1-hour hold at 240°C and 350°C, respectively. The temperature is then increased at 5°C / minute to 1000-1150°C, held for 30 minutes, and naturally cooled to room temperature to produce the porous glass material.

[0047] Typically, but not limiting, the atomizer core provided in this application is based on a porous glass material, on which a heating unit is provided, wherein the heating unit is a heating wire, a heating net or a heating film. The heating wire or heating net needs to be embedded in the green body forming process, and then sintered together with the formed green body to obtain a porous glass atomizer core; when a heating film is used, a thick film resistive heating film can be printed on the porous glass substrate by screen printing or a thin film resistive heating film can be sprayed or magnetron sputtered, and the pattern of the heating film can be designed, and then the porous glass atomizer core can be obtained through a sintering step.

[0048] Typically, non-limitingly, a thick film resistive heating film is prepared by screen printing process. The main components of the thick film are nickel-based alloy, iron-based alloy, silver alloy, titanium alloy, aluminum alloy, stainless steel, etc., containing elements such as Fe, Cr, Ni, Ti, Pa, Pt, Al, Mo, Si, Ag, etc. The protruding thickness of the thick film is 11-100μm, the penetration thickness is 10-100μm, the line width is 250-450μm, the line spacing is 300μm-900μm, and the patterns used are S, M, Ω, etc. The sintering temperature of the heating film is 700-1200℃, and the sintering time is 0.5-3h.

[0049] Typically, but not limiting, thin film resistive heating films are prepared by spraying or magnetron sputtering. The main components of the film are nickel-based alloys, silver alloys, titanium alloys, aluminum alloys, stainless steel, etc., containing elements such as Fe, Cr, Ni, Ti, Pa, Pt, Al, Mo, Si, and Ag. The protruding thickness of the film is 0.5-5μm.

[0050] For example, an atomizing core is prepared by sintering a printed film based on a porous glass material, and its heating unit is a porous heating membrane, wherein: the porous heating membrane includes a portion higher than the surface of the porous glass substrate and a portion infiltrated into the porous glass substrate, wherein the portion higher than the surface of the porous glass substrate is a porous structure with a pore size of 5-30 microns, the pores are interconnected and connected to the substrate pores, and its height is 30-100 microns, and the optional height is about 80 microns; the heating membrane infiltrating into the porous glass substrate has a maximum penetration thickness of about 70 microns, and is embedded in the pores of the porous substrate, so that the entire porous heating membrane is firmly bonded to the porous glass substrate; the resistance of the heating membrane is 0.8-1.2 ohms.

[0051] The technical solution of this application has the following advantages:

[0052] The porous glass material with uniform pore channels provided by the present application includes a skeleton and multi-directional connecting pores, and the multi-directional connecting pores are interconnected by pore throats, wherein: the average diameter of the pore throats is 25-45 microns, and the pore throats are distributed in the 5-60 micron area, wherein more than 50% of the pore throats are distributed in the 20-45 micron range. The present application limits the pore throat size to make the connecting channel size between the pores uniform, thereby avoiding uneven liquid conduction speed and local overheating during the use of the atomizer core, avoiding the generation of local coking and carbon deposits, and the amount of smoke is basically not attenuated during the suction process. Specifically, the prepared atomizer core is tested for its atomization temperature condition using an infrared thermal imager. During the atomization process of the atomizer core, the temperature field is uniformly distributed, there is no local high temperature point, and the atomization temperature is stably distributed between 235-245°C. Compared with commercially available ceramic heating elements, under the same conditions, the porous glass matrix is ​​not prone to carbon deposition after smoking an electronic cigarette. At the same time, the liquid conduction speed is significantly improved. Compared with commercially available porous ceramic heating elements, the liquid conduction speed can be increased by more than 33%.

[0053] The porous glass material with uniform pore channels provided in the present application further improves the overall uniformity of the porous glass material by optimizing the design of parameters such as pore throats, skeletons, multi-directional connected pores, porosity and liquid conduction rate. The oil conduction rate at each location is significantly improved and highly consistent. At the same time, the uniformity of the temperature field during the atomization process is improved, which can further reduce the occurrence of local coking and carbon deposition and improve its atomization effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the following will briefly introduce the drawings required for use in the specific implementation methods or the description of the prior art. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0055] FIG1 is a pore throat size distribution diagram of the porous glass materials provided in Examples 1-3 and Comparative Example 1 of the present application;

[0056] FIG2 is a topographical image (left) and a microscopic image (right) of the atomizer core provided by this application;

[0057] FIG3 is a temperature field distribution and a temperature distribution diagram of Example 1 during the atomization process in the test example;

[0058] FIG4 is a temperature field distribution and a temperature distribution diagram of Comparative Example 1 during the atomization process in the test example;

[0059] FIG5 is a comparison diagram of carbon deposition between Example 1 of the present application and a commercially available ceramic heating element;

[0060] FIG6 is a microscopic morphology diagram of the porous material provided in Example 1 of the present application. DETAILED DESCRIPTION

[0061] The following examples are provided to further better understand the present application, but are not limited to the best implementation mode described herein, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the scope of protection of the present application.

[0062] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in this field can be used. If the manufacturer of the reagents or instruments is not specified, they are all commercially available conventional reagents.

[0063] Example 1

[0064] This embodiment provides a porous glass material with uniform pore channels, and a specific preparation method thereof comprises the following steps:

[0065] Glass powder was ball-milled in a planetary ball mill at 300 rpm for 3 hours using ethanol as a solvent, dried, and sieved to obtain glass powder with a particle size of 3-5 microns. The crushed mullite chopped fibers were ball-milled in ethanol at 300 rpm for 6 hours using stearic acid as a grinding aid. After washing with ethanol, the fibers were dried and sieved through a 100-mesh sieve to obtain fiber raw material. 48 parts of glass powder, 52 parts of mullite fibers, and 100 parts of PMMA (80 micron) as a pore-forming agent were three-dimensionally mixed for 2 hours. The mixed materials were then added to 140 parts of a 3.5% aqueous agar polysaccharide sol solution at 80°C (the same below). The mixture was slowly stirred at 80°C to form a uniform paste. The paste was then poured into a mold of the corresponding shape, cooled, and removed to obtain a green body. The green body was first cured in a 60°C oven for 4 hours, then heated to 200°C over 200 minutes, and then to 500°C at a rate of 0.5°C / min. Hold times of 2 hours were set at 240°C and 350°C, respectively. The body was then heated to 1180°C at a rate of 5°C / min, held for 30 minutes, and naturally cooled to room temperature. This yielded a porous glass material with a porosity of 71.6%, an average pore throat of 34 microns, and a distribution of pore throats between 16 and 55 microns. The pore throats resembled a normal distribution, with more than 50% of the pore throats centered between 25 and 42 microns. The pore throat size distribution is shown in Figure 1a. The average diameter of the skeleton was 25 microns, the average length was 100 microns, and the diameter of the multidirectionally interconnected pores was 75 microns. Figure 6 shows the microscopic morphology of the porous glass material.

[0066] A porous glass material with a length of 9mm, a width of 4mm, and a height of 2.5mm was prepared, and its oil conduction speed was tested at room temperature. The e-liquid with a viscosity of 230cP was selected, and the substrate was placed vertically (height 9mm). It took about 75s for the e-liquid to rise 9mm, and the oil conduction speed was 0.12mm / s. Under the same conditions, the commercially available porous ceramic substrate took 100s to raise the e-liquid by 9mm, and the oil conduction speed was 0.09mm / s. Compared with the commercially available ceramic heating element substrate, the oil conduction speed of the porous glass material was increased by more than 33%.

[0067] Example 2

[0068] This embodiment provides a porous glass material with uniform pore channels, and a specific preparation method thereof comprises the following steps:

[0069] Glass powder was ball-milled in a planetary ball mill at 300 rpm for 3 hours using ethanol as a solvent, dried, and sieved to obtain glass powder with a particle size of 3-5 microns. The crushed alumina chopped fibers were ball-milled in ethanol at 300 rpm using stearic acid as a grinding aid for 6 hours. After washing with ethanol, the fibers were dried and sieved through a 100-mesh sieve to obtain the fiber raw material. 40 parts of glass powder, 60 parts of fibers, and 200 parts of PMMA (80 micron) pore-forming agent were mixed in a three-dimensional manner for 2 hours. The mixed materials were then added to 130 parts of 80°C agar polysaccharide sol and slowly stirred at 80°C to form a uniform paste. The paste was then poured into a mold of the corresponding shape and removed after cooling to obtain a green body. The green body was first cured in a 60°C oven for 2 hours, then heated to 200°C over 200 minutes, and then to 500°C at a rate of 0.5°C / minute. The temperature was then held at 240°C and 350°C for 2 hours, respectively. The glass was then heated at a rate of 5°C / minute to 1250°C, held for 30 minutes, and naturally cooled to room temperature to produce a porous glass material. The porous glass material had a porosity of 74.2%, an average pore throat of 40 microns, and a pore throat distribution between 7 and 56 microns, with more than 50% of the pore throats ranging from 38 to 45 microns. The pore throat distribution is shown in Figure 1b. The average diameter of the skeleton was 20 microns, the average length was 100 microns, and the diameter of the multidirectional interconnected pores was 80 microns.

[0070] A porous glass substrate with a length of 9 mm, a width of 4 mm, and a height of 2.5 mm was prepared and its oil conduction speed was tested at room temperature. A smoke oil with a viscosity of 230 cP was selected and the substrate was placed vertically (9 mm in height). It took about 85 seconds for the smoke oil to rise 9 mm, and the oil conduction speed was 0.11 mm / s.

[0071] Example 3

[0072] This embodiment provides a porous glass material with uniform pore channels, and a specific preparation method thereof comprises the following steps:

[0073] Glass powder was ball-milled in a planetary ball mill at 300 rpm for 3 hours using ethanol as a solvent, dried, and sieved to obtain glass powder with a particle size of 3-5 microns. The crushed mullite chopped fibers were ball-milled in ethanol at 300 rpm for 6 hours using stearic acid as a grinding aid. After washing with ethanol, the fibers were dried and sieved through a 100-mesh sieve to obtain the fiber raw material. 62 parts of glass powder, 38 parts of fiber, 50 parts of PMMA (50 micron) pore former, and 190 parts of PMMA (80 micron) pore former were mixed three-dimensionally for 2 hours. The mixed materials were then added to 120 parts of 80°C agar polysaccharide sol and slowly stirred at 80°C to form a uniform paste. The paste was then poured into a mold of the corresponding shape, cooled, and removed to obtain a green body. The green body was first cured in a 60°C oven for 1 hour, then heated to 200°C over 200 minutes, and then to 500°C at a rate of 0.5°C / min. Hold times of 2 hours were set at 240°C and 350°C, respectively. The material was then heated to 1220°C at a rate of 5°C / min, held for 30 minutes, and naturally cooled to room temperature to obtain a porous glass material. The porous glass material had a porosity of 67.7%, an average pore throat of 23 microns, and a distribution of pore throats between 12 and 39 microns. The pore throats exhibited a normal distribution, with more than 50% of the pore throats centered between 22 and 28 microns. The pore throat size distribution is shown in Figure 1c. The average diameter of the skeleton was 25 microns, the average length was 95 microns, and the diameter of the multidirectionally interconnected pores was 60 microns.

[0074] A porous glass substrate with a length of 9 mm, a width of 4 mm, and a height of 2.5 mm was prepared and its oil conduction speed was tested at room temperature. A smoke oil with a viscosity of 230 cP was selected and the substrate was placed vertically (9 mm in height). It took about 80 seconds for the smoke oil to rise 9 mm, and the oil conduction speed was 0.11 mm / s.

[0075] Comparative Example 1

[0076] This comparative example provides a porous glass material, the preparation method of which comprises the following steps:

[0077] Glass powder was ball-milled in a planetary ball mill at 300 rpm for 3 hours using ethanol as a solvent, dried, and sieved to obtain glass powder with a particle size of 3-5 microns. The crushed mullite chopped fibers were ball-milled in ethanol at 300 rpm for 6 hours using stearic acid as a grinding aid. After washing with ethanol, they were dried and sieved through a 100-mesh sieve to obtain the fiber raw material. 70 parts of glass powder, 30 parts of fiber, and 200 parts of PMMA (80 micron) pore-forming agent were mixed in a three-dimensional manner for 2 hours. The mixed materials were then added to 120 parts of 80°C agar polysaccharide sol and slowly stirred at 80°C to form a uniform paste. The paste was then poured into a mold of the corresponding shape, cooled, and removed to obtain a green body. The green body was first cured in a 60°C oven for 1 hour, then heated to 200°C over 200 minutes, and then to 500°C at a rate of 0.5°C / minute. The temperature was then held at 240°C and 350°C for 2 hours, respectively. The glass was then heated at a rate of 5°C / minute to 1180°C, held for 30 minutes, and naturally cooled to room temperature to produce a porous glass material. The porous glass material had a porosity of 47.7%, an average pore throat of 15.2 microns, and a distribution of pore throats between 3 and 30 microns, with more than 50% of the pore throats ranging from 7 to 15 microns. The pore throat distribution is shown in Figure 1d. The average diameter of the skeleton was 35 microns, the average length was 55 microns, and the diameter of the multidirectional interconnected pores was 60 microns.

[0078] A porous glass substrate with a length of 9 mm, a width of 4 mm, and a height of 2.5 mm was prepared and its oil conduction speed was tested at room temperature. A smoke oil with a viscosity of 230 cP was selected and the substrate was placed vertically (9 mm in height). It took about 96 seconds for the smoke oil to rise 9 mm, and the oil conduction speed was 0.094 mm / s.

[0079] Test Case

[0080] The atomizing core is prepared with the porous glass material prepared in the embodiment and the comparative example, and a porous iron-based heating film slurry is used (the specific composition is mainly metal Fe element, including some Ni, Cr, Mn, Mo, and W metal elements). The film is printed and sintered to obtain a porous heating film. The pore size of the porous heating film is 5-30 microns, the pores are interconnected, and the pores are connected to the substrate pores. It is about 80 microns higher than the substrate and has a penetration thickness of about 70 microns. The pattern is shown in Figure 2. The line width is about 330 μm, the line spacing is about 650 μm, the line is about 800 microns away from the edge of the substrate, the sintering temperature is 980°C, and the time is 30 minutes to obtain a porous glass atomizing core. An infrared thermal imager was used to examine the atomization temperature of the porous glass atomizer core. Using a 7.5W power board and a 3s on, 27s off test pattern, fruit-flavored e-liquid was used to evaluate the atomization performance of the porous glass atomizer core. During atomization, the core temperature field was uniform, with no localized high-temperature spots. The atomization temperature of Example 1 was stably distributed between 235-245°C, as shown in Figure 3. The atomization temperature of Comparative Example 1 was unstable, ranging between 240-310°C, as shown in Figure 4. The test results of Examples 2-3 were similar to those of Example 1 and are not presented here separately.

[0081] The porous glass atomizer cores prepared in Examples 1-3 and Comparative Example 1 were tested for cigarette loading. Using a 7.5W power battery and fruit-flavored e-liquid, the puffs were simulated using a 3-second draw and 27-second pause. Compared to commercially available ceramic heaters (Feelm heaters from Shenzhen McWel Technology Co., Ltd.), the porous glass atomizer core in Example 1 showed little carbon accumulation after puffing. As shown in Figure 5, after 400 puffs, the porous glass atomizer core (left image) showed a significant advantage over the ceramic heater (right image) in terms of carbon accumulation. However, the commercially available ceramic heaters showed significant carbon accumulation after 400 puffs. The carbon accumulation in Examples 2 and 3 was similar to that in Example 1, and the carbon accumulation in Comparative Example 1 was similar to that of commercially available ceramic heaters. Therefore, images are not shown here.

[0082] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will appreciate that other variations or modifications can be made based on the above description. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications derived therefrom remain within the scope of protection of this application.

Claims

1. A porous glass material with uniform pore channels, characterized in that: It includes a skeleton and multi-directional interconnected holes, and the multi-directional interconnected holes are interconnected by pore throats, among which: The average diameter of the pore throats is 25-45 microns, and the pore throats are distributed in the region of 5-60 microns, wherein more than 50% of the pore throats are distributed in the region of 20-45 microns.

2. The porous glass material with uniform pore channels according to claim 1, characterized in that: The average diameter of the pore throats is 28-36 microns, the pore throats are distributed in the 10-55 micron region, and more than 90% of the pore throats are distributed in the 20-45 micron region.

3. The porous glass material with uniform pore channels according to claim 2, characterized in that: The average diameter of the pore throats is about 29-35 microns, the pore throats are distributed in the 12-50 micron region, and the pore throats distributed in the 20-45 micron region account for more than 95%.

4. The porous glass material with uniform pore channels according to claim 3, characterized in that: The pore throats are distributed in the range of 20-45 microns.

5. The porous glass material with uniform pore channels according to any one of claims 1 to 4, characterized in that: The skeleton is a glass-coated fiber frame structure, including a frame body and a connector connecting the frame body: the average diameter of the frame body is 20-45 microns, and the average length is 60-100 microns.

6. The porous glass material with uniform pore channels according to claim 5, characterized in that: The diameter of the multi-directional interconnected holes is 70-100 microns.

7. The porous glass material with uniform pore channels according to any one of claims 1 to 4, characterized in that: The porosity of the porous glass material is 65-80%.

8. The porous glass material with uniform pore channels according to claim 7 is characterized in that: The porosity of the porous glass material is 70-74%.

9. The porous glass material with uniform pore channels according to claim 7 or 8, characterized in that: The porous glass material has a liquid conduction rate of more than 0.09 mm / s at room temperature for an atomized matrix with a viscosity of 230 cP.

10. The porous glass material with uniform pore channels according to claim 9, characterized in that: The liquid conduction rate at room temperature is above 0.10 mm / s.

11. The porous glass material with uniform pore channels according to claim 9, characterized in that: The liquid conduction rate at room temperature is above 0.12 mm / s.

12. An atomizer core, characterized in that: The porous glass material according to any one of claims 1 to 11 is used as a substrate, and a heating unit is arranged on the substrate.

13. The atomizer core according to claim 12, characterized in that: During the atomization process, the temperature field deviation is less than 10°C.

14. An electronic atomizer, characterized in that: Comprising the atomizer core according to claim 12 or 13.

Citation Information

Patent Citations

  • Atomization core, preparation method, and electronic cigarette

    CN110194662A

  • Porous glass as well as preparation method and application thereof

    CN114804639A

  • Process for producing glass-ceramics

    KR1019920017967A