Method for granulating and molding polyhydroxyalkanoate, and molded body thereof
By controlling the temperature and using the shear force of the rotating screw, the problems of PHA degradation and insufficient melt strength during thermal processing are solved, and efficient and stable granulation molding is achieved, maintaining the high purity and production efficiency of the material.
Patent Information
- Application Number
- PCT/CN2024/088841
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-28
AI Technical Summary
In the prior art, polyhydroxy fatty acid ester (PHA) is prone to degradation during hot processing, and the melt strength is not high, resulting in poor granulation and low efficiency, and additives are required to improve the thermal processing performance. The types of additives are limited and require a large amount of use, which affects the high purity of the material.
Using a special granulation molding method, the processing temperature is controlled between 40℃ below the melting point of the raw material and 3℃ above the melting point. The shear force of the rotating screw is realized, and the pelletization is cut at an appropriate temperature to avoid the use of additional additives and reduce the use of Equipment takes up space and cooling time to improve production efficiency.
It realizes efficient, stable and continuous granulation of PHA materials, maintains high purity, shortens the molding cycle, reduces energy consumption and cost, avoids the phenomenon of sticking the knife, and improves the production efficiency and the stability of the molded body.
Smart Images

Figure CN2024088841_28112024_PF_FP_ABST
Abstract
Description
A method for granulating and molding polyhydroxyalkanoate and a molded body thereof Technical Field
[0001] The present invention relates to the technical field of processing and modification of degradable materials, and in particular to a method for granulating and molding polyhydroxyalkanoate (PHA) and a molded body thereof. Background Art
[0002] Polyhydroxyalkanoate (PHA) is a bio-friendly, marine-degradable, and bio-based polymer with adjustable properties, offering broad application prospects. However, PHA obtained through microbial fermentation has a small, powdery particle size and low bulk density, making it difficult to use directly in downstream processing. It must be granulated to obtain a relatively regular granular body before it can be used in downstream product applications.
[0003] However, according to the traditional melt granulation method, pure PHA is easily degraded during the thermal processing process, and the melt strength is low. Even if it is extruded into strips, it is often difficult to cool, so it is very easy to stick to the knife during pelletizing. Otherwise, the strips must be annealed before pelletizing, which greatly prolongs the pelletizing cycle. In short, the pelletizing effect of pure PHA is poor and the efficiency is low.
[0004] To facilitate the pelletization of PHA powder, additives such as nucleating agents, melt strength enhancers, thermal stabilizers, chain extenders, and grafting agents are commonly added to improve the thermal processing properties of PHA. These additives increase melt strength, expand the thermal processing window, and accelerate cooling crystallization. However, in practice, these additives are far from satisfactory. Currently, only a limited number of additives have been found that are suitable for PHA, or significant effects require large addition amounts, hindering the ability to maintain high purity levels in PHA pellets.
[0005] In summary, there is an urgent need for a granulation and molding method for polyhydroxyalkanoates that can maintain high purity of PHA while also being able to granulate and mold smoothly, efficiently, continuously, and stably to ensure that purer pellets can be used downstream.
[0006] Summary of the Invention
[0007] The present invention abandons the conventional process of thermal processing of polymer materials and adopts a special granulation and molding method. Without the need for additional additives, pure PHA resin pellets with rounded and full particles can be obtained, which reduces the equipment space occupied, increases the cooling speed, shortens the molding cycle, and greatly improves production efficiency.
[0008] A first aspect of the present invention provides a granulation molding method, which comprises processing raw materials at a highest temperature of a first temperature, and then extruding at a second temperature and pelletizing to obtain a molded body.
[0009] The raw materials include polyhydroxyalkanoate.
[0010] Preferably, the first temperature is any value from 40°C below the melting point of the raw material to 3°C above the melting point. Further preferably, the first temperature is any value from 40°C below the melting point of the raw material to less than 10°C below the melting point; further preferably, the first temperature is greater than 10°C below the melting point of the raw material to 3°C above the melting point. Preferably, the first temperature is any value from 40°C below the melting point, 35°C below the melting point, 30°C below the melting point, 25°C below the melting point, 20°C below the melting point, 15°C below the melting point, 10°C below the melting point, 9°C below the melting point, 8°C below the melting point, 7°C below the melting point, 6°C below the melting point, 5°C below the melting point, 4°C below the melting point, 3°C below the melting point, 2°C below the melting point, 1°C below the melting point to the melting point or 1°C, 2°C, or 3°C above the melting point.
[0011] Preferably, the processing comprises feeding the raw materials into a barrel equipped with a screw, and melting them by the shear force of the rotating screw at the processing temperature.
[0012] The screw is fixed inside the barrel.
[0013] The interior of the barrel can be any irregular shape such as a hollow cylinder, a hollow cuboid, a hollow cube, a hollow ellipsoid, or a hollow cone.
[0014] If the interior is a hollow cylinder, the two ends of the screw are respectively facing the upper and lower bottom surfaces of the cylinder.
[0015] The screw is provided with a screw groove. After the raw material is fed into the barrel from one end of the screw, the raw material is pushed forward in the screw groove to the other end by the rotating screw.
[0016] Preferably, the screw speed during processing is any value in the range of 100-450 rpm, preferably any value in the range of 150-400 rpm, and more preferably any value in the range of 190-370 rpm, for example, 100, 135, 150, 190, 192, 198, 200, 215, 216, 225, 250, 252, 270, 300, 310, 315, 320, 324, 350, 360, 370, 400, 405 or 450 rpm.
[0017] Preferably, the feeding speed during the process is any value in the range of 3-200 rpm, preferably any value in the range of 5-200 rpm, for example 3, 5, 10, 20, 30, 40, 50, 55, 60, 65, 70, 75, 80, 85, 88, 90, 95, 96, 98, 100, 110, 112, 118, 120, 130, 135, 138, 140, 142, 145, 150, 160, 165, 170, 180, 190 or 200 rpm.
[0018] Preferably, the processing temperature is a non-fixed temperature, including temperature zones. Further preferably, it includes 2-20 temperature zones, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 zones.
[0019] Preferably, the temperature of each zone may be the same or different.
[0020] Preferably, the temperature of each zone can be set to gradually rise to the first temperature, or, can be set to gradually rise to the first temperature and then maintain it, or can be set to gradually rise to the first temperature and then gradually decrease (preferably, the temperature of each zone can be set so that after rising to the first temperature, the next zone starts to decrease; or, after rising to the first temperature, it is maintained for several zones and then gradually decreases).
[0021] Preferably, the gradually rising to the first temperature means that the temperature of each zone is raised by 2-20°C (for example, by 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20°C) until the first temperature is reached.
[0022] Further preferably, the temperature rise between each zone may be the same or different.
[0023] Preferably, the gradual decrease means that the temperature of each zone decreases by 3-15°C (e.g., 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15°C) from the first temperature zone by zone.
[0024] Further preferably, the temperature drop between each zone may be the same or different.
[0025] Preferably, in the temperature zone, the lowest temperature is set to 90°C below the melting point to 20°C below the melting point, preferably 87°C below the melting point to 25°C below the melting point, for example, 20°C below the melting point, 25°C below the melting point, 33°C below the melting point, 38°C below the melting point, 42°C below the melting point, 45°C below the melting point, 50°C below the melting point, 58.5°C below the melting point, 60°C below the melting point, 62°C below the melting point, 68.5°C below the melting point, 70°C below the melting point, 78.5°C below the melting point, 80°C below the melting point, 82°C below the melting point, 85°C below the melting point, 87°C below the melting point or 90°C below the melting point.
[0026] Preferably, in the temperature zones, the temperature of each zone gradually rises from the lowest temperature to the first temperature.
[0027] Preferably, in the temperature zones, the temperature of each zone gradually rises from the lowest temperature to the first temperature and then gradually decreases.
[0028] Preferably, in the temperature zones, the temperature of the last zone is close to the die temperature or even lower than the die temperature. Further preferably, the temperature of the last zone is 40°C below the die temperature to 10°C above the die temperature, more preferably 35°C below the die temperature to 5°C above the die temperature, for example, 40°C below the die temperature, 35°C below the die temperature, 15°C below the die temperature, 12°C below the die temperature, 10°C below the die temperature, 8.5°C below the die temperature, 7°C below the die temperature, 5°C below the die temperature, 4°C below the die temperature, 3°C below the die temperature, 2°C below the die temperature, 1°C below the die temperature, equal to the die temperature, 1°C above the die temperature, 2°C above the die temperature, 3°C above the die temperature, 4°C above the die temperature, 5°C above the die temperature, 6°C above the die temperature, 7°C above the die temperature, 8°C above the die temperature, 9°C above the die temperature or 10°C above the die temperature.
[0029] The die is a whole assembly installed at the end of the barrel.
[0030] Preferably, the number of screws in the barrel equipped with screws is at least 1, at least 2, at least 3, at least 4, at least 5, at least 6, at least 7, at least 8, at least 9, at least 10, at least 11 or at least 12, etc.
[0031] Preferably, the barrel includes a feeding device, wherein when the raw material is added to the barrel, the feeding speed is any value in the range of 3-200 rpm, preferably any value in the range of 5-200 rpm, for example, 3, 5, 10, 20, 30, 40, 50, 55, 60, 65, 70, 75, 80, 85, 88, 90, 95, 96, 98, 100, 110, 112, 118, 120, 130, 135, 138, 140, 142, 145, 150, 160, 165, 170, 180, 190 or 200 rpm.
[0032] Preferably, the aspect ratio of the screw includes but is not limited to (36-64):1, preferably (36-52):1, more preferably (36-48):1, and even more preferably (36-44):1, such as 36:1, 40:1, 44:1, 45:1, 48:1, 50:1, 52:1, 55:1, 56:1, 60:1, or 64:1. One end and the other end of the screw are relative to the length direction of the screw.
[0033] In practical applications, the larger the aspect ratio, the longer the material stays in the heat treatment and the stronger the shearing effect it is subjected to. Therefore, it is necessary to maintain a lower screw speed. Correspondingly, the feeding speed also needs to be slowed down proportionally, and the final output will also decrease year-on-year.
[0034] Preferably, the barrel equipped with a screw includes but is not limited to a screw extruder, and the screw extruder includes a transmission device, a feeding device, a barrel, a screw, and a die (die).
[0035] More preferably, the barrel equipped with a screw is one of a single-screw extruder, a twin-screw extruder or a multi-screw extruder.
[0036] The method described in this application can adapt PHA materials to continuous processing in various types of twin-screw extruders.
[0037] Preferably, the screw type of the twin-screw extruder includes but is not limited to parallel twin screws, conical twin screws, fully meshing (including same-direction meshing, opposite-direction meshing), partially meshing, same-direction rotation, opposite-direction rotation (inward, outward), equal distance and depth, equal distance and depth, variable pitch and equal depth, and variable pitch and depth.
[0038] Preferably, the second temperature is the die temperature or the die head temperature.
[0039] The die or die head is a porous component installed at the end of the barrel.
[0040] Preferably, the second temperature is any value from 50°C below the melting point of the raw material to less than the melting point of the raw material, further preferably, the second temperature is 50°C below the melting point of the raw material to 20°C below the melting point of the raw material, more preferably, the second temperature is 50°C below the melting point of the raw material to less than 15°C below the melting point of the raw material, further preferably, the second temperature is 40°C below the melting point of the raw material to less than 15°C below the melting point of the raw material, further preferably, the second temperature is greater than 15°C below the melting point of the raw material to 10°C below the melting point of the raw material. Preferably, the second temperature is any value from 50°C, 45°C, 40°C, 35°C, 30°C, 25°C, 20°C, 15°C, 10°C, 8°C, 7°C, 5°C, 3°C, 1°C below the melting point of the raw material to less than the melting point of the raw material.
[0041] Preferably, the pelletizing includes but is not limited to underwater die surface pelletizing, water ring die surface pelletizing or air-cooled die surface pelletizing.
[0042] Preferably, the temperature of the water environment for underwater die surface pelletizing or water ring die surface pelletizing is any value between -20°C and 70°C, for example, -20°C, -12°C, -15°C, -10°C, -5°C, 0°C, 5°C, 10°C, 15°C, 18°C, 20°C, 22°C, 25°C, 30°C, 32°C, 35°C, 37°C, 40°C, 45°C, 48°C, 50°C, 55°C, 60°C, 65°C, 67°C, and 70°C.
[0043] In a specific embodiment of the present invention, the temperature of the water environment for underwater die surface pelletizing is any value between -12°C and 67°C, or any value between 5°C and 45°C, or any value between 22°C and 67°C, or any value between 25°C and 30°C.
[0044] In a specific embodiment of the present invention, the temperature of the water environment for the water ring die surface pelletizing is any value between 0°C and 70°C, or any value between 15°C and 45°C, or any value between 18°C and 30°C.
[0045] Preferably, the water environment is pure water, or the water environment includes water and antifreeze substances.
[0046] Preferably, the mass proportion of the antifreeze substance in the water environment is any value between 0-50%, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50%.
[0047] Preferably, the antifreeze substance includes but is not limited to one or two of alcohol substances and / or salt substances, and the antifreeze substance only needs to be able to reduce the freezing point to below 0 degrees.
[0048] Further preferably, the antifreeze substance includes but is not limited to one or more of ethanol, ethylene glycol, glycerol, 1,4-butanediol, sodium chloride, calcium chloride, potassium chloride, magnesium sulfate, magnesium chloride, sodium nitrate, polyethylene glycol, sucrose, acetic acid, sodium acetate, potassium acetate, zinc acetate, and magnesium acetate.
[0049] Preferably, the air temperature of the air-cooled die surface pelletizing is any value between -15°C and 75°C, for example, -15°C, -10°C, -8°C, -5°C, 0°C, 3°C, 5°C, 10°C, 15°C, 18°C, 20°C, 25°C, 30°C, 32°C, 35°C, 40°C, 42°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 72°C, and 75°C.
[0050] In a specific embodiment of the present invention, the air temperature of the air-cooled die surface pelletizing is any value between -8°C and 72°C, or any value between 15°C and 40°C, or any value between 20°C and 35°C, or any value between 32°C and 72°C.
[0051] Preferably, the polyhydroxyalkanoate includes but is not limited to a homopolymer, a random copolymer or a block copolymer of monomers constituting the polyhydroxyalkanoate.
[0052] Preferably, the monomers constituting PHA include one or more of 2-hydroxypropionic acid, 3-hydroxypropionic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 5-hydroxyvaleric acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 3-hydroxydecanoic acid, 3-hydroxyundecanoic acid or 3-hydroxydodecanoic acid;
[0053] More preferably, the PHA comprises one or more of P(HB-LA), P3HP, PHB, P4HB, PHV, PHO, PHN, PHD, PHBV, P34HB, PHBHHp, PHBHHx, P3HB4HB3HV or P3HB4HB5HV.
[0054] The melting point of the raw material varies according to the content of the monomer in the polyhydroxyalkanoate. For example, when the polyhydroxyalkanoate is P34HB and the molar ratio of 4HB in P34HB is 10%, the melting point is 172°C, while when the molar ratio of 4HB in P34HB is 30%, the melting point is 83°C.
[0055] In a specific embodiment of the present invention, the polyhydroxyalkanoate is PHB, and the melting point of PHB is 165°C.
[0056] The method uses underwater die surface pelletizing, the first temperature is 80°C to 160°C, the second temperature is 155°C, and the temperature of the water environment for underwater die surface pelletizing is 30°C; or
[0057] The method uses a water ring die surface for pelletizing, the first temperature is 105°C to 150°C, the second temperature is 125°C, and the temperature of the water environment for the underwater die surface pelletizing is 0°C; or
[0058] The method uses air-cooled die face pelletizing, the first temperature is 85°C to 168°C, the second temperature is 150°C, and the air temperature of the air-cooled die face pelletizing is 40°C.
[0059] In a specific embodiment of the present invention, the polyhydroxyalkanoate is P34HB (4HB ratio is 10 mol%), and the melting point of P34HB is 172°C.
[0060] The method uses underwater die surface pelletizing, the first temperature is 85°C to 172°C, the second temperature is 152°C, and the temperature of the water environment for underwater die surface pelletizing is 45°C; or
[0061] The method uses a water ring die surface for pelletizing, the first temperature is 110°C to 155°C, the second temperature is 160°C, and the temperature of the water environment for the underwater die surface pelletizing is 70°C; or
[0062] The method uses air-cooled die face pelletizing, the first temperature is 122°C to 132°C, the second temperature is 132°C, and the air temperature of the air-cooled die face pelletizing is 15°C.
[0063] In a specific embodiment of the present invention, the polyhydroxyalkanoate is P34HB (4HB ratio is 30 mol%), and the melting point of P34HB is 83°C.
[0064] The method uses underwater die surface pelletizing, the first temperature is 45°C to 85°C, the second temperature is 60°C, and the temperature of the water environment for underwater die surface pelletizing is minus 12°C; or
[0065] The method uses a water ring die surface for pelletizing, the first temperature is 58°C to 70°C, the second temperature is 45°C, and the temperature of the water environment for the underwater die surface pelletizing is minus 20°C; or
[0066] The method uses air-cooled die face pelletizing, the first temperature is 50°C to 75°C, the second temperature is 80°C, and the air temperature of the air-cooled die face pelletizing is 20°C.
[0067] In a specific embodiment of the present invention, the polyhydroxyalkanoate is PHBV (3HV ratio is 6 mol%), and the melting point of PHBV is 162°C.
[0068] The method uses underwater die surface pelletizing, the first temperature is 120°C to 138°C, the second temperature is 123°C, and the temperature of the water environment for underwater die surface pelletizing is minus 5°C; or
[0069] The method uses a water ring die surface for pelletizing, the first temperature is 75°C to 162°C, the second temperature is 155°C, and the temperature of the water environment for the underwater die surface pelletizing is minus 48°C; or
[0070] The method uses air-cooled die face pelletizing, the first temperature is 80°C to 160°C, the second temperature is 152°C, and the air temperature of the air-cooled die face pelletizing is 35°C.
[0071] In a specific embodiment of the present invention, the polyhydroxyalkanoate is PHBHHx (3HHx ratio is 5 mol%), and the melting point of PHBHHx is 140°C.
[0072] The method uses underwater die surface pelletizing, the first temperature is 90°C to 120°C, the second temperature is 135°C, and the temperature of the water environment for underwater die surface pelletizing is 37°C; or
[0073] The method uses a water ring die surface for pelletizing, the first temperature is 95°C to 110°C, the second temperature is 117°C, and the temperature of the water environment for the underwater die surface pelletizing is 0°C; or
[0074] The method uses air-cooled die face pelletizing, the first temperature is 80°C to 130°C, the second temperature is 132°C, and the air temperature of the air-cooled die face pelletizing is 42°C.
[0075] In a specific embodiment of the present invention, the polyhydroxyalkanoate is PHBHHx (3HHx ratio is 10 mol%), and the melting point of PHBHHx is 135°C.
[0076] The method uses underwater die surface pelletizing, the first temperature is 85°C to 123°C, the second temperature is 125°C, and the temperature of the water environment for underwater die surface pelletizing is 10°C; or
[0077] The method uses a water ring die surface for pelletizing, the first temperature is 90°C to 101°C, the second temperature is 100°C, and the temperature of the water environment for the underwater die surface pelletizing is minus 20°C; or
[0078] The method uses air-cooled die face pelletizing, the first temperature is 65°C to 136°C, the second temperature is 115°C, and the air temperature of the air-cooled die face pelletizing is 3°C.
[0079] In a specific embodiment of the present invention, the polyhydroxyalkanoate is P3HB4HB3HV (the ratios of 3HB, 4HB, and 3HV are 92.5 mol%, 5 mol%, and 2.5 mol%, respectively), and the melting point of P3HB4HB3HV is 168.5° C.
[0080] The method uses underwater die surface pelletizing, the first temperature is 90°C to 160°C, the second temperature is 158.5°C, and the temperature of the water environment for underwater die surface pelletizing is minus 32°C; or
[0081] The method uses a water ring die surface for pelletizing, the first temperature is 100°C to 150°C, the second temperature is 152°C, and the temperature of the water environment for the underwater die surface pelletizing is 25°C; or,
[0082] The method uses air-cooled die face pelletizing, the first temperature is 110°C to 140°C, the second temperature is 143°C, and the air temperature of the air-cooled die face pelletizing is 18°C.
[0083] Preferably, the pelletizing step further includes a cooling and shaping step.
[0084] Preferably, the cooling and setting time is 1-20 seconds, preferably any value in the range of 1-10 seconds, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 seconds.
[0085] The cooling time reflects the stability and continuity of the process. If the cooling time is too long, the process cannot be continuous. The conveying process must wait until the pellets in front cool and crystallize before continuing. Otherwise, the pellets will accumulate and stick together at a certain stage. Moreover, if the cooling time is too long, it is easy for the scraper to squeeze. After a long time, the uncrystallized material will accumulate on the scraper, even causing the machine to jam, which will greatly reduce the stability of the process.
[0086] Preferably, the method does not require drafting.
[0087] In a specific embodiment of the present invention, the method comprises:
[0088] 1) processing the raw material, wherein the highest processing temperature is a first temperature (40° C. below the melting point of the raw material to 3° C. above the melting point);
[0089] 2) pelletizing after extrusion at a second temperature (50° C. below the melting point of the raw material to the melting point, but less than the melting point); the pelletizing comprising:
[0090] Using underwater die face pelletizing, the temperature of the water environment for underwater die face pelletizing is -20°C to 70°C; or,
[0091] The water ring die surface is used for pelletizing, and the temperature of the water environment for pelletizing is -20℃ to 70℃, or
[0092] The air-cooled die face pelletizing is used, and the air temperature of the air-cooled die face pelletizing is -15°C to 75°C;
[0093] 3) Cooling and shaping.
[0094] The method described uses a twin-screw extruder, preferably,
[0095] The feeding speed of the twin-screw extruder is any value in the range of 3-200 rpm, preferably any value in the range of 5-200 rpm, for example, 3, 5, 10, 20, 30, 40, 50, 55, 60, 65, 70, 75, 80, 85, 88, 90, 95, 96, 98, 100, 110, 112, 118, 120, 130, 135, 138, 140, 142, 145, 150, 160, 165, 170, 180, 190 or 200 rpm.
[0096] During the processing, the screw speed is 100-450 rpm, preferably 150-400 rpm, and more preferably 190-370 rpm, for example, 100, 135, 150, 190, 192, 198, 200, 215, 216, 225, 250, 252, 270, 300, 310, 315, 320, 324, 350, 360, 370, 400, 405 or 450 rpm.
[0097] The aspect ratio of the screw includes but is not limited to (36-64:1), preferably (36-52:1), more preferably (36-48):1, and even more preferably (36-44):1, for example 36:1, 40:1, 44:1, 45:1, 48:1, 50:1, 52:1, 55:1, 56:1, 60:1 or 64:1.
[0098] Preferably, the method of the present invention may further include the addition of an auxiliary agent.
[0099] Preferably, the auxiliary agent comprises one or more of a nucleating agent, an initiator, a cross-linking agent, a chain extender, an anti-hydrolysis agent, an antioxidant or a thermal stabilizer.
[0100] The second aspect of the present invention provides a molded body produced by the method described in the first aspect.
[0101] The molded body prepared by the method described in the first aspect of the present invention has a diameter of 2-3 mm and a nearly spherical shape.
[0102] The third aspect of the present invention provides a use of the molded body described in the second aspect in preparing a biodegradable material.
[0103] Preferably, the biodegradable materials include but are not limited to biomedical materials, biodegradable packaging materials, drug controlled-release materials, degradable medical and cosmetic materials, degradable injection molding materials, degradable straw materials, degradable coating materials, ground film materials and / or fiber textiles, non-woven materials, etc.
[0104] The term "include" or "comprising" in the present invention is an open description containing the specified components or steps described, as well as other specified components or steps that do not substantially affect them.
[0105] The term "and / or" as used herein includes all combinations of the items connected by the term, and each combination should be deemed to have been listed separately herein. For example, "A and / or B" includes "A," "A and B," and "B." For another example, "A, B, and / or C" includes "A," "B," "C," "A and B," "A and C," "B and C," and "A and B and C."
[0106] Beneficial effects of the present invention:
[0107] 1. The present invention relates to a PHA pelletizing method that abandons conventional processes for thermal processing of polymer materials and instead employs a unique pelletizing method. Specifically, the pelletizing temperature (processing temperature) is controlled to be near or even below the melting point. Specifically, the maximum temperature in each zone within the thermal processing equipment is limited to between 40°C below and 3°C above the melting point of the raw material, rather than 20-60°C above the melting point. This, combined with an appropriate screw speed, reduces energy consumption and minimizes thermal degradation of the PHA material, resulting in efficient and cost-effective pelletizing. Nucleating agents and other additives are not required, and the material's color and purity are not affected, thus reducing costs. Furthermore, the die opening temperature is also below the melting point. Experiments have confirmed that this does not prevent the PHA material from melting, resulting in excessive screw pressure and thus excessive current, nor does it damage the thermal processing equipment or clog the die opening. Instead, it facilitates faster cooling and crystallization, reducing die sticking during pelletizing. This further reduces energy consumption and costs, shortens the pelletizing cycle, and improves production efficiency.
[0108] 2. The present invention relates to a granulation and molding method for PHA. Unlike conventional cooling processes, which control the cooling medium temperature as low as possible, the cooling medium temperature is adjusted within an appropriate range based on the type and proportion of the PHA being processed, the die temperature, and other factors. This greatly accelerates the molding speed and improves production efficiency. It overcomes the limitations of biodegradable materials such as PHA when granulated and molded according to conventional processes, such as their inability to adapt to high aspect ratios, high screw shear forces, and long residence times. Equipment does not need to be modified for PHA, and the granulation efficiency of the extruder is further maximized.
[0109] 3. Compared with the commonly used process of strand granulation after melting, the present invention's PHA granulation and molding method has a smaller equipment footprint and can achieve a closed granulation process, thereby reducing the interaction between the PHA material at high temperatures and the environment, and avoiding the negative effects of external factors on the PHA material.
[0110] 4. The present invention relates to a method for granulating and molding PHAs. During the granulation and molding process, there is essentially no drafting effect, meaning that the PHA material does not need to be oriented, allowing for rapid cooling and crystallization. The resulting molded particles do not stick to the cutter or to each other. Therefore, the overall process is simple and controllable, with high production efficiency. It can adapt to conditions with high aspect ratios, high screw shear forces, and long residence times, which can result in strong thermal and mechanical effects. Furthermore, the process has low equipment requirements, is low-carbon and environmentally friendly, and the resulting particles are stable, uniform, and highly pure. Furthermore, the process can be directly applied to or guide the industrial production of PHA molded bodies.
[0111] The English and Chinese abbreviations and the full Chinese name of this application are compared in Table 1.
[0112] Table 1: Abbreviation and full name comparison table BRIEF DESCRIPTION OF THE DRAWINGS
[0113] Figure 1: PHB particles prepared by the method described in Example 1;
[0114] Figure 2: PHB particles prepared by the method described in Control Example 1;
[0115] Figure 3: PHB particles prepared by the method described in Control Example 4;
[0116] Figure 4: PHB particles prepared by the method described in Control Example 6;
[0117] Figure 5: Comparison of yields of Group A, Group B, and Group C in Control Example 11. DETAILED DESCRIPTION
[0118] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts are within the scope of protection of the present invention.
[0119] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0120] Some of the equipment involved in the present invention comes from the following sources:
[0121] Twin-screw extruder: purchased from Nanjing Juli Chemical Machinery Co., Ltd., 35mm twin-screw extruder.
[0122] Example 1 (PHB, underwater)
[0123] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0124] The processing temperature of the twin-screw extruder is set in the range of 80-160°C, and the die temperature is set at 155°C.
[0125] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0126] The particles are cooled for 5 seconds to set, and the particles are round and full, which can complete the granulation work well and achieve continuous and stable production. The prepared PHB particles are shown in Figure 1.
[0127] Example 2 (PHB, water ring)
[0128] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0129] The processing temperature of the twin-screw extruder is set in the range of 105-150°C, and the die temperature is set at 125°C.
[0130] The pelletizing process was carried out by water ring die surface, and the water environment temperature was set to 0℃.
[0131] The pellets are cooled for 6 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0132] Example 3 (PHB, air-cooled)
[0133] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0134] The processing temperature of the twin-screw extruder is set in the range of 85-168°C, and the die temperature is set at 150°C.
[0135] The pelletizing process was carried out by air-cooling die surface, and the air-cooling temperature was set at 40℃.
[0136] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0137] Example 4 (P34HB, 10 mol%, underwater)
[0138] P34HB (4HB ratio is 10 mol%) powder raw material is melt extruded and granulated. The melting point of P34HB is 172°C after testing.
[0139] The processing temperature of the twin-screw extruder was set in the range of 85-172°C, and the die temperature was set at 152°C.
[0140] Underwater die surface pelletizing was used, and the water environment temperature was set at 45°C.
[0141] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0142] Example 5 (P34HB, 10 mol%, water ring)
[0143] P34HB (4HB ratio is 10 mol%) powder raw material is melt extruded and granulated. The melting point of P34HB is 172°C after testing.
[0144] The processing temperature of the twin-screw extruder is set in the range of 110-155°C, and the die temperature is set at 160°C.
[0145] The pelletizing process was carried out using a water ring die, and the water environment temperature was set at 70°C.
[0146] The pellets are cooled for 4 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0147] Example 6 (P34HB, 10 mol%, air-cooled)
[0148] P34HB (4HB ratio is 10 mol%) powder raw material is melt extruded and granulated. The melting point of P34HB is 172°C after testing.
[0149] The processing temperature setting range of the twin-screw extruder is 122-132°C, and the die temperature is set to 132°C.
[0150] The pelletizing process was carried out by air-cooling die surface, and the air-cooling temperature was set at 15°C.
[0151] The pellets are cooled for 6 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0152] Example 7 (P34HB, 30 mol%, underwater)
[0153] P34HB (4HB ratio is 30 mol%) powder raw material is melt extruded and granulated. The melting point of P34HB is 83°C after testing.
[0154] The processing temperature of the twin-screw extruder is set in the range of 45-85°C, and the die temperature is set at 60°C.
[0155] Underwater die surface pelletizing is used, and the water environment temperature is set to -12℃.
[0156] The pellets are cooled for 6 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0157] Example 8 (P34HB, 30 mol%, water ring)
[0158] P34HB (4HB ratio is 30 mol%) powder raw material is melt extruded and granulated. The melting point of P34HB is 83°C after testing.
[0159] The processing temperature of the twin-screw extruder was set in the range of 58-70°C, and the die temperature was set at 45°C.
[0160] The pelletizing process was carried out using a water ring die, and the water environment temperature was set to -20°C.
[0161] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0162] Example 9 (P34HB, 30 mol%, air-cooled)
[0163] P34HB (4HB ratio is 30 mol%) powder raw material is melt extruded and granulated. The melting point of P34HB is 83°C after testing.
[0164] The processing temperature of the twin-screw extruder is set in the range of 50-75°C, and the die temperature is set at 80°C.
[0165] The pelletizing process was carried out by air-cooling die surface, and the air-cooling temperature was set at 20℃.
[0166] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0167] Example 10 (PHBV, 6 mol%, underwater)
[0168] PHBV (3HV ratio is 6 mol%) powder raw material was melt extruded and granulated. The melting point of PHBV was tested to be 162°C.
[0169] The processing temperature of the twin-screw extruder was set in the range of 120-138°C, and the die temperature was set at 123°C.
[0170] Underwater die surface pelletizing was used, and the water environment temperature was set at 5°C.
[0171] The pellets are cooled for 6 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0172] Example 11 (PHBV, 6 mol%, water ring)
[0173] PHBV (3HV ratio is 6 mol%) powder raw material was melt extruded and granulated. The melting point of PHBV was tested to be 162°C.
[0174] The processing temperature of the twin-screw extruder was set in the range of 75-162°C, and the die temperature was set at 155°C.
[0175] The pelletizing process was carried out using a water ring die, and the water environment temperature was set at 48°C.
[0176] The pellets are cooled for 4 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0177] Example 12 (PHBV, 6 mol%, air-cooled)
[0178] PHBV (3HV ratio is 6 mol%) powder raw material was melt extruded and granulated. The melting point of PHBV was tested to be 162°C.
[0179] The processing temperature of the twin-screw extruder was set in the range of 80-160°C, and the die temperature was set at 152°C.
[0180] The pelletizing process was carried out by air-cooling die surface, and the air-cooling temperature was set at 35°C.
[0181] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0182] Example 13 (PHBHHx, 5 mol%, underwater)
[0183] PHBHHx (3HHx ratio is 5 mol%) powder raw material is melt-extruded and granulated. The melting point of PHBHHx is tested to be 140°C.
[0184] The processing temperature of the twin-screw extruder is set in the range of 90-120°C, and the die temperature is set at 135°C.
[0185] Underwater die surface pelletizing was used, and the water environment temperature was set at 37°C.
[0186] The pellets are cooled for 4 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0187] Example 14 (PHBHHx, 5 mol%, water ring)
[0188] PHBHHx (3HHx ratio is 5 mol%) powder raw material is melt-extruded and granulated. The melting point of PHBHHx is tested to be 140°C.
[0189] The processing temperature of the twin-screw extruder was set in the range of 95-110°C, and the die temperature was set at 117°C.
[0190] The pelletizing process was carried out by water ring die surface, and the water environment temperature was set to 0℃.
[0191] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0192] Example 15 (PHBHHx, 5 mol%, air-cooled)
[0193] PHBHHx (3HHx ratio is 5 mol%) powder raw material is melt-extruded and granulated. The melting point of PHBHHx is tested to be 140°C.
[0194] The processing temperature of the twin-screw extruder was set in the range of 80-130°C, and the die temperature was set at 132°C.
[0195] The pelletizing process was carried out by air-cooled die surface, and the air-cooling temperature was set at 42°C.
[0196] The pellets are cooled for 4 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0197] Example 16 (PHBHHx, 10 mol%, underwater)
[0198] PHBHHx (3HHx ratio is 10 mol%) powder raw material is melt extruded and granulated. The melting point of PHBHHx is tested to be 135°C.
[0199] The processing temperature setting range of the twin-screw extruder is 85-123°C, and the die temperature is set to 125°C.
[0200] Underwater die surface pelletizing was used, and the water environment temperature was set at 10°C.
[0201] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0202] Example 17 (PHBHHx, 10 mol%, air-cooled)
[0203] PHBHHx (3HHx ratio is 10 mol%) powder raw material is melt extruded and granulated. The melting point of PHBHHx is tested to be 135°C.
[0204] The processing temperature of the twin-screw extruder was set in the range of 65-136°C, and the die temperature was set at 115°C.
[0205] The pelletizing process was carried out by air-cooling die surface, and the air-cooling temperature was set at 3°C.
[0206] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0207] Example 18 (PHBHHx, 10 mol%, water ring)
[0208] PHBHHx (3HHx ratio is 10 mol%) powder raw material is melt extruded and granulated. The melting point of PHBHHx is tested to be 135°C.
[0209] The processing temperature of the twin-screw extruder was set in the range of 90-101°C, and the die temperature was set at 100°C.
[0210] The pelletizing process was carried out using a water ring die, and the water environment temperature was set to -20°C.
[0211] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0212] Example 19 (P3HB4HB3HV, 92.5 / 5 / 2.5 mol%, underwater)
[0213] P3HB4HB3HV (the ratios of 3HB, 4HB and 3HV are 92.5 mol%, 5 mol% and 2.5 mol% respectively) powder raw material was melt-extruded and granulated. The melting point of P3HB4HB3HV was tested to be 168.5°C.
[0214] The processing temperature of the twin-screw extruder was set in the range of 90-160°C, and the die temperature was set at 158.5°C.
[0215] Underwater die surface pelletizing was used, and the water environment temperature was set at 32°C.
[0216] The pellets are cooled for 4 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0217] Example 20 (P3HB4HB3HV, 92.5 / 5 / 2.5 mol%, water ring)
[0218] P3HB4HB3HV (the ratios of 3HB, 4HB and 3HV are 92.5 mol%, 5 mol% and 2.5 mol% respectively) powder raw material was melt-extruded and granulated. The melting point of P3HB4HB3HV was tested to be 168.5°C.
[0219] The processing temperature of the twin-screw extruder was set in the range of 100-150°C, and the die temperature was set at 152°C.
[0220] The pelletizing process was carried out using a water ring die, and the water environment temperature was set at 25°C.
[0221] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0222] Example 21 (P3HB4HB3HV, 92.5 / 5 / 2.5 mol%, air-cooled)
[0223] P3HB4HB3HV (the ratios of 3HB, 4HB and 3HV are 92.5 mol%, 5 mol% and 2.5 mol% respectively) powder raw material was melt-extruded and granulated. The melting point of P3HB4HB3HV was tested to be 168.5°C.
[0224] The processing temperature of the twin-screw extruder was set in the range of 110-140°C, and the die temperature was set at 143°C.
[0225] The pelletizing process was carried out by air-cooling die surface, and the air-cooling temperature was set at 18°C.
[0226] The pellets are cooled for 5 seconds to set into shape, and the pellets are round and full, which can complete the pelletizing work well and ensure continuous and stable production.
[0227] Comparative Example 1 (Compared with Example 1, the water environment temperature is too low)
[0228] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0229] The processing temperature of the twin-screw extruder is set in the range of 80-160°C, and the die temperature is set at 155°C.
[0230] Underwater die surface pelletizing is used, and the water environment temperature is set to -25℃.
[0231] During the granulation process, the particles adhered severely to each other and were still soft after 60 seconds of cooling, and could not be well shaped. The prepared PHB particles are shown in Figure 2.
[0232] Comparative Example 2 (Compared with Example 1, the water environment temperature is too high)
[0233] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0234] The processing temperature of the twin-screw extruder is set in the range of 80-160°C, and the die temperature is set at 155°C.
[0235] Underwater die surface pelletizing was used, and the water environment temperature was set at 80°C.
[0236] If the water temperature is too high, the PHA material cannot be immediately shaped after leaving the mold hole, and the cooling time must be more than 20 seconds. The material particles are elongated, which is not aesthetically pleasing and can easily cause blockage of the pipelines in subsequent processes, making continuous production impossible.
[0237] Comparative Example 3 (Compared with Example 1, the first temperature is too high)
[0238] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0239] The processing temperature of the twin-screw extruder is set in the range of 80-195°C, and the die temperature is set at 155°C.
[0240] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0241] During the granulation process, the PHA material was severely degraded and could not be granulated. The material was severely adhered at the die mouth. After cooling for 12 hours, the material was still soft and could not be well shaped.
[0242] Comparative Example 4 (Compared with Example 1, the first temperature is higher)
[0243] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0244] The processing temperature setting range of the twin-screw extruder is 80-173°C, and the die temperature is set to 155°C.
[0245] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0246] During the granulation process, the PHA material was degraded, the color of the particles became darker, and there were many "small tails" due to material adhesion. After a cooling time of 5 minutes, the material was still soft and slow to set. The prepared PHB particles are shown in Figure 3.
[0247] Comparative Example 5 (Compared with Example 1, the first temperature is too low)
[0248] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0249] The processing temperature of the twin-screw extruder is set in the range of 80-115°C, and the die temperature is set at 155°C.
[0250] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0251] During the granulation process, the PHA material could not be melted, the extrusion equipment had an overload alarm due to excessive current, and continuous production was impossible.
[0252] Comparative Example 6 (Compared with Example 1, the second temperature is higher)
[0253] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0254] The processing temperature setting range of the twin-screw extruder is 80-160℃, and the die temperature is set to 165℃.
[0255] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0256] During the granulation process, the particles adhered to each other severely. After cooling for 15 minutes, the particles were still soft and could not be well shaped. The prepared PHB particles are shown in Figure 4.
[0257] Comparative Example 7 (Compared with Example 1, the second temperature is too high)
[0258] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0259] The processing temperature of the twin-screw extruder is set in the range of 80-160°C, and the die temperature is set at 180°C.
[0260] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0261] During the granulation process, the particles adhered to each other seriously and were partially degraded. After cooling for 4 hours, the particles were still soft and could not be well shaped.
[0262] Comparative Example 8 (Compared with Example 1, the second temperature is too low)
[0263] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0264] The processing temperature setting range of the twin-screw extruder is 80-160°C, and the die temperature is set to 105°C.
[0265] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0266] The pellets are shaped after cooling for 5 seconds and are round and full. However, the die is blocked every 3 hours or so during the pelletizing process, so stable and continuous production is not possible.
[0267] Comparative Example 9 (compared with Example 1, using traditional thermal processing technology)
[0268] The PHB powder raw material was melt-extruded and granulated, and the melting point of PHB was tested to be 165°C.
[0269] The processing temperature of the twin-screw extruder is set in the range of 80-180°C, and the die temperature is set at 170°C.
[0270] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0271] During the granulation process, the particles adhered to each other very seriously, and after cooling for 8 hours, they were still soft and could not be well shaped.
[0272] Comparative Example 10 (Compared with Example 1, conventional thermal processing technology was used and additives were added)
[0273] PHB powder raw material + 0.5wt% isosorbide + 0.5wt% boron carbide were melt extruded and granulated. The melting point of PHB was tested to be 165°C.
[0274] The processing temperature of the twin-screw extruder is set in the range of 80-180°C, and the die temperature is set at 170°C.
[0275] Underwater die surface pelletizing was used, and the water environment temperature was set at 30°C.
[0276] During the granulation process, particles occasionally stick together and the cooling time takes about 60 seconds. Due to the added amount of nucleating additives, it is no longer pure PHA.
[0277] Comparative Example 11 (Effect of different screw aspect ratios on output)
[0278] Group A: The same raw materials were processed in the same manner as in Example 1, except that the screw aspect ratios of the twin-screw extruders used were set to 36:1, 40:1, 44:1, 48:1, 52:1, 56:1, 60:1, and 64:1, respectively.
[0279] Group B: The same raw materials were processed in the same way as in Control Example 10. The difference from Control Example 10 was that the screw length-to-diameter ratios of the twin-screw extruders used were set to 36:1, 40:1, 44:1, 48:1, 52:1, 56:1, 60:1, and 64:1, respectively.
[0280] Group C: The same raw materials were processed in the same way as in Control Example 4. The difference from Control Example 4 was that the screw length-to-diameter ratios of the twin-screw extruders used were set to 36:1, 40:1, 44:1, 48:1, 52:1, 56:1, 60:1, and 64:1, respectively.
[0281] Group D: The same settings as Group B were used to process the same raw materials, but the screw speed and feed speed at each screw aspect ratio were set according to those of Group A.
[0282] Group E: The same settings as Group C were used to process the same raw materials, but the screw speed and feed speed at each screw aspect ratio were set according to those of Group A.
[0283] Among them, the aspect ratio, screw speed and feeding speed setting and output of Group A, Group B, Group C, Group D and Group E are shown in Table 2 and Figure 5. It can be found that the output obtained by the method of the present invention is higher than the output obtained by the method described in Control Example 10 (Group B) and Control Example 4 (Group C). However, due to the high first temperature, the die mouth of Group D and Group E will continue to be blocked during the production process, and it is necessary to continuously stop and clean the blockage before restarting, and stable continuous production cannot be achieved. The above conclusions prove that the method described in this application can be applied to various aspect ratios, high screw speeds and feeding speeds, and can achieve high output.
[0284] Table 2 Note: The data for Examples 1-21 and Comparative Examples 1-10 are based on an extruder with a screw diameter of 35 mm. The extruder partitions, temperatures in each zone, process parameters, output, particle size, and shape in each example and comparative example are shown in Tables 3-5 below.
[0285] Table 3
[0286] Table 4
[0287] Table 5
[0288] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A granulation molding method, characterized in that: The method comprises processing the raw material, wherein the highest temperature of the processing is a first temperature, and then extruding at a second temperature and pelletizing to obtain a shaped body; The raw materials include polyhydroxyalkanoates; The first temperature is 40°C below the melting point of the raw material and 3°C above the melting point.
2. The method according to claim 1, characterized in that: The second temperature is 50° C. below the melting point of the raw material to less than the melting point of the raw material.
3. The method according to claim 1, characterized in that The processing includes adding the raw materials into a barrel equipped with a screw, and achieving melting by the shear force of the rotating screw at the processing temperature; Preferably, the screw aspect ratio is (36-64):
1.
4. The method according to claim 3, characterized in that The screw speed during processing is 100-450rpm.
5. The method according to claim 3, characterized in that: The processing temperature is a non-fixed temperature, including temperature zones; Preferably, the temperature of each zone is set to gradually rise to the first temperature, or, is set to gradually rise to the first temperature and then gradually decrease.
6. The method according to claim 5, characterized in that The gradually rising to the first temperature means that the temperature of each zone rises by 2-20°C zone by zone.
7. The method according to claim 5, characterized in that The gradual decrease means that the temperature of each zone decreases by 3-15° C. from the first temperature zone by zone.
8. The method according to claim 5, characterized in that In the temperature zones, the temperature of the last zone is 40°C lower than the die temperature and 10°C higher than the die temperature. Preferably, the temperature of the last zone is 35°C below the die temperature to 5°C above the die temperature.
9. The method according to claim 3, characterized in that: The number of the screws is 1-12; Preferably, the number of the screws is 1-3.
10. The method according to claim 1, characterized in that The pelletizing includes underwater die surface pelletizing, water ring die surface pelletizing or air-cooled die surface pelletizing.
11. The method according to claim 10, characterized in that The temperature of the water environment for underwater die face pelletizing or water ring die face pelletizing is between -20°C and 70°C; the temperature of the air-cooled die face pelletizing is between -15°C and 75°C.
12. The method according to claim 1, characterized in that The step of cooling and shaping is also included after the pelletizing; Preferably, the cooling and setting time is 1-10 seconds.
13. The method according to claim 1, characterized in that The polyhydroxyalkanoate includes a homopolymer, a random copolymer or a block copolymer of the monomers constituting the polyhydroxyalkanoate; Preferably, the monomers constituting the polyhydroxyalkanoic acid ester include one or more of 2-hydroxypropionic acid, 3-hydroxypropionic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 5-hydroxyvaleric acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 3-hydroxydecanoic acid, 3-hydroxyundecanoic acid or 3-hydroxydodecanoic acid; Further preferably, the polyhydroxyalkanoate includes one or more of P3HP, PHB, P(HB-LA), P4HB, PHV, P34HB, PHBV, PHBHHx, PHBHHp, PHO, PHN, PHD, P3HB4HB3HV or P3HB4HB5HV.
14. The method according to claim 1, characterized in that The method described does not require drafting.
15. A shaped body obtained by the method according to any one of claims 1 to 14.
16. Use of the shaped body according to claim 15 in preparing biodegradable materials.
Citation Information
Patent Citations
High-performance polyhydroxyalkanoate as well as preparation method and application thereof
CN114479021A
Granulation processing method of degradable material and formed body prepared by granulation processing method
CN115157478A
Method for granulating and forming polyhydroxyalkanoate and formed body of polyhydroxyalkanoate