Method for preparing long-chain α-olefins from polyethylene
By thermally cracking the polyethylene in a pressurized superheated water vapor environment, it is divided into two steps: low temperature preliminary and high temperature depth, which solves the problems of low yield, safety hazards and environmental pollution in the existing long-chain α-olefin preparation process. , realizes efficient and environmentally friendly long-chain α-olefin preparation and high value-added conversion of waste polyethylene.
Patent Information
- Application Number
- PCT/CN2024/092294
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-05
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-28
AI Technical Summary
The existing long-chain α-olefin preparation process has low yield, complex operation, environmental pollution and safety risks, especially the high energy consumption, expensive catalysts and high temperature and high pressure conditions of wax cracking and ethylene oligomerization, resulting in high costs and safety risks. big.
Polyethylene is used as raw material to carry out thermal cracking reaction in a pressurized superheated water vapor environment. By rapid preheating and thermal cracking, long-chain α-olefins and co-products are obtained, which are divided into low-temperature preliminary thermal cracking and high-temperature deep thermal cracking. Two steps to improve yield and carbon number distribution narrowness.
Achieve high yield, low energy consumption, high safety and environmental protection long-chain α-olefin preparation, provides a new raw material route and converts waste polyethylene into high value-added products, with a yield of more than 70%, and a carbon number distribution Focus on C5-C15.
Smart Images

Figure CN2024092294_28112024_PF_FP_ABST
Abstract
Description
A method for preparing long-chain alpha-olefins from polyethylene Technical Field
[0001] The present invention relates to a method for producing long-chain alpha-olefins, and in particular to a method for efficiently converting polyethylene as a raw material into long-chain alpha-olefins. Background Art
[0002] Long-chain α-olefins have a wide range of applications in chemical synthesis, serving as raw materials for the synthesis of various chemicals. Applications vary depending on the length of the carbon chain. For example, C4-C8 α-olefins are primarily used as comonomers for ethylene and propylene; C12-C18 α-olefins are primarily used in synthetic detergents; C6-C20 α-olefins are used in the synthesis of lubricants; and C6-C10 α-olefins are used as plasticizers.
[0003] At present, the mainstream long-chain α-olefin preparation processes at home and abroad include wax cracking, alkane dehydrogenation and ethylene polymerization.
[0004] Industrial alpha-olefins were first produced through wax cracking. The typical Chevron wax cracking process includes vaporization, cracking, quenching, and separation. Due to the high wax content of crude oil in China, such as crude oil from Daqing and Renqiu, which has a wax content as high as 23%-25%, domestic alpha-olefin production relies primarily on wax cracking. Domestic wax cracking generally uses wax with an oil content greater than 30% as a feedstock. It is carried out under low pressure, vapor phase, high temperature, and short residence time conditions, with appropriate steam (or water) injection to increase linear velocity and prevent coking in the tubular reactor. To maximize olefin yields, the single-pass wax cracking rate is typically controlled at 25%-30%, and the extensive recycling of the material increases energy consumption.
[0005] The n-paraffin dehydrogenation process, pioneered by UOP and used in conjunction with alkylbenzenes and fatty alcohols, involves molecular sieve separation of n-paraffins, n-paraffin dehydrogenation, and distillation of the alkylated products. The C10-C14 linear alkanes are separated from straight-run kerosene / light diesel fractions and then hydrotreated to remove aromatic sulfur and nitrogen impurities. The process's weakest link is the single-pass conversion rate of n-paraffins, which is only 11%-13%, resulting in high product costs.
[0006] Ethylene oligomerization is currently the predominant α-olefin production process internationally. Companies that own this technology, such as Shell, Ineos, UOP, DuPont, Exxon, Linde, and Amoco, have refused to transfer it, and domestic ethylene oligomerization technology is still in the development and improvement stage. Ethylene oligomerization uses ethylene as a raw material, which is then polymerized in the presence of a catalyst to produce long-chain α-olefins. Depending on the catalyst, processes can be categorized as aluminum alkyl, nickel complex, and zirconium alkyl. The aluminum alkyl catalytic process can be further divided into a one-step and a two-step process. In the one-step process, triethylaluminum is used as a catalyst. Ethylene is compressed and preheated to 23 MPa and 180°C before being introduced into a reactor for oligomerization and metathesis reactions with a residence time of approximately 15 minutes. The separated ethylene is recycled, and the liquid product is terminated with aqueous NaOH solution before liquid separation and distillation to produce long-chain α-olefin products with varying carbon numbers. The two-step process also uses triethylaluminum as a catalyst. Ethylene is compressed and preheated before being introduced into two reactors in parallel. The first reactor is controlled at a temperature of 160-275°C and a pressure of 10-25 MPa, primarily synthesizing long-chain α-olefins (C4-C10). In the second reactor, ethylene undergoes chain growth at 60-100°C and 10-20 MPa, followed by a displacement reaction at 245-300°C and 0.7-20.0 MPa, producing long-chain α-olefins (C12-C18). The reaction products are separated, recovered, recycled, and distilled to yield long-chain α-olefins with varying carbon numbers. While the ethylene oligomerization process offers excellent product performance, the catalyst is expensive, exhibits low catalytic activity, and exhibits poor selectivity, requiring large quantities of cocatalysts and supports. Furthermore, the process is demanding, requiring high temperatures and pressures, and presents a risk of explosion.
[0007] Therefore, there is a need in the art for a method for preparing long-chain α-olefins with high yield, simple operation, environmental protection and high safety.
[0008] Summary of the Invention
[0009] The purpose of the present invention is to provide a method for efficiently converting long-chain α-olefins with high yield, simple operation, environmental protection and high safety.
[0010] In a first aspect of the present invention, there is provided a method for preparing long-chain α-olefins, the method comprising the steps of:
[0011] (s1) providing a preheated gas-liquid mixture comprising molten polyethylene and water vapor; and
[0012] (s2) The gas-liquid mixture is subjected to a thermal cracking reaction under a pressurized environment to obtain long-chain α-olefins.
[0013] In another preferred embodiment, the long-chain α-olefin refers to a long-chain α-olefin having 7 to 30 carbon atoms, preferably a C7-C30 long-chain α-olefin.
[0014] In another preferred embodiment, the polyethylene is selected from the group consisting of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, or a combination thereof.
[0015] In another preferred embodiment, the weight average molecular weight of the polyethylene is 2×10 4 g / mol~30×10 4 g / mol, preferably 5×10 4 g / mol~20×10 4 g / mol.
[0016] In another preferred embodiment, the number average molecular weight of the polyethylene is 1×10 4 g / mol~10×10 4 g / mol, preferably 2×10 4 g / mol~8×10 4 g / mol.
[0017] In another preferred embodiment, the melting point of the polyethylene is 100-200°C, preferably 100-180°C.
[0018] In another preferred embodiment, the density of the polyethylene is 0.75-1.0 g / mL.
[0019] In another preferred example, the mass ratio of the polyethylene to the superheated water steam is 10:1 to 1:10, preferably 5:1 to 1:5, such as 5:1, 2:1, 1:1.5, and 1:2.
[0020] In another preferred embodiment, the method further comprises a pre-treatment step of purging with an inert gas, wherein the inert gas is selected from one or more of nitrogen, argon, and helium.
[0021] In another preferred embodiment, the gas-liquid mixture is obtained by preheating (a) polyethylene and (b) water or steam.
[0022] In another preferred embodiment, the preheating refers to preheating to 450-550°C, such as 485°C, 500°C, 515°C, or 545°C.
[0023] In another preferred embodiment, the preheating is rapid preheating, preferably with a temperature increase of 20 to 50° C. / min.
[0024] In another preferred embodiment, the preheating time is between 5-20 min, preferably 10-20 min, such as 12 min, 14 min, 15 min, 16 min, 18 min.
[0025] In another preferred embodiment, the gas-liquid mixture is a high-temperature gas-liquid mixture, and the temperature of the gas-liquid mixture is 450-550°C.
[0026] In another preferred embodiment, the pressurized environment means that the pressure of the reaction system is controlled at 0.2-2.0 MPa (absolute pressure), such as 0.5 MPa, 1 MPa, or 1.5 MPa.
[0027] In another preferred embodiment, the thermal cracking reaction is carried out at 450-550°C, such as 485°C, 515°C, or 545°C.
[0028] In another preferred embodiment, the thermal cracking reaction is carried out at a preheating temperature.
[0029] In another preferred embodiment, the method comprises the steps of:
[0030] Under pressure, (a) polyethylene and (b) water or steam are mixed and quickly preheated to a set pyrolysis temperature, and the reaction is continued to perform thermal cracking to obtain long-chain α-olefins.
[0031] In another preferred embodiment, the reaction is carried out batchwise or continuously.
[0032] In another preferred embodiment, when the reaction is carried out in an intermittent manner, the reaction time of the thermal cracking reaction is 0.5 to 10 min, for example, 0.5 min, 1 min, 3 min, 5 min, or 10 min.
[0033] In another preferred embodiment, when the reaction is carried out continuously, the reaction time of the thermal cracking reaction is 0.5 to 10 min, for example, 0.5 min, 1 min, 3 min, 5 min, or 10 min.
[0034] In another preferred embodiment, the reaction space time is defined as reaction space time = reactor volume / (feed mass flow rate / polyethylene density).
[0035] In another preferred embodiment, the reaction further comprises a step of rapidly cooling to quench the reaction.
[0036] In another preferred embodiment, when the reaction is carried out in an intermittent manner, the reaction includes: adding polyethylene and water, purging with nitrogen for pretreatment, preheating the materials in the kettle to a preheating temperature (preferably 450-550°C), controlling the system pressure at 0.2-2.0 MPa (absolute pressure), continuing the reaction for a period of time (preferably 0.5-10 min) after reaching the preset thermal cracking temperature, and rapidly cooling to quench the thermal cracking.
[0037] In another preferred embodiment, when the reaction is carried out in a continuous manner, the reaction includes: molten polyethylene is mixed with superheated water steam and enters the reaction tube, which is rapidly preheated to reach the thermal cracking temperature, and the pressure in the reaction system is controlled at 0.2 to 2.0 MPa (absolute pressure), and then the product flows out of the reactor.
[0038] In another preferred embodiment, when the reaction is carried out in a continuous manner, the reaction includes: molten polyethylene is mixed with superheated water steam and enters the reaction tube, first rapidly preheated in the preheating section to reach the thermal cracking temperature, then enters the thermal cracking section and maintains the temperature, controls the reaction time (preferably 0.5 to 10 minutes), and the obtained product flows out of the reactor, wherein the pressure in the reaction system is controlled at 0.2 to 2.0 MPa (absolute pressure).
[0039] In another preferred embodiment, the thermal cracking reaction is carried out in one reactor.
[0040] In another preferred embodiment, the thermal cracking reaction is carried out at the same temperature, wherein the "same temperature" means that the temperature difference does not exceed 5°C.
[0041] In another preferred embodiment, the yield of the long-chain α-olefin obtained in the reaction is greater than 15 wt%, preferably greater than 20 wt%, and more preferably greater than 25 wt%.
[0042] In another preferred embodiment, the olefin content in the liquid product obtained by the reaction is greater than 30 wt%, preferably greater than 35 wt%, and more preferably greater than 40 wt%.
[0043] In another preferred embodiment, the step (s2) can also be performed under a non-pressurized environment.
[0044] In another preferred embodiment, the thermal cracking reaction is carried out at 0.1 to 2.0 MPa (absolute pressure), for example, 0.1 MPa, 0.2 MPa, 0.5 MPa, 1 MPa, or 1.5 MPa.
[0045] In another preferred embodiment, the thermal cracking reaction includes a low-temperature preliminary thermal cracking reaction and a high-temperature deep thermal cracking reaction.
[0046] In another preferred embodiment, the thermal cracking reaction includes a low-temperature preliminary thermal cracking reaction carried out in a first reactor, and a high-temperature deep thermal cracking reaction carried out in a second reactor.
[0047] In another preferred embodiment, the thermal cracking reaction is carried out at different temperatures, wherein the "same temperature" means that the temperature difference exceeds 20°C.
[0048] In another preferred embodiment, the step (s2) comprises the following steps:
[0049] (s3) in the first reactor, at a second temperature, performing a low-temperature preliminary thermal cracking reaction on the polyethylene and the superheated gas;
[0050] (s4) the intermediate product obtained in step (s3) is entrained by superheated gas into the second reactor in series;
[0051] (s5) At a third temperature, the mixture in step (s4) enters a second reactor to undergo a high-temperature deep thermal cracking reaction to obtain the long-chain α-olefin.
[0052] In another preferred embodiment, the step (s3), step (s4), step (s5), the first reactor, the second reactor, the second temperature, and the third temperature are each independently as described in the third aspect of the present invention.
[0053] In a second aspect of the present invention, a device is provided, comprising a tubular reaction device, a pressurizing device, and a thermocouple, wherein the tubular reaction device comprises a first temperature control zone and a second temperature control zone, wherein the first temperature control zone is used for preheating, and the second temperature control zone is used for performing a thermal cracking reaction.
[0054] The device is configured to perform the method according to the first aspect of the present invention.
[0055] In another preferred example, the inner diameter of the reaction tube of the tubular reactor is 2 cm and the length is 400 cm.
[0056] In another preferred example, the device further comprises a heating device, and the heating device optionally comprises a first heating device and a second heating device.
[0057] In another preferred embodiment, the first heating device is used to heat the first temperature-controlled zone, and the second heating device is used to heat the second temperature-controlled zone.
[0058] In another preferred embodiment, the thermocouple is a retractable thermocouple to determine the axial temperature distribution.
[0059] In another preferred embodiment, the pressurizing device is configured to control the pressure within a range of 0.2 to 2.0 MPa (absolute pressure).
[0060] In another preferred example, the heating device is configured to control the temperature at a preheating temperature.
[0061] In a third aspect of the present invention, a method for preparing long-chain α-olefins by thermal cracking of polyethylene is provided, the method comprising the steps of:
[0062] (s1) providing polyethylene in a first reactor;
[0063] (s2) continuously introducing a superheated gas at a first temperature into the first reactor, wherein the volume of the superheated gas vapor accounts for more than 50% of the total volume of the superheated gas;
[0064] (s3) in the first reactor, at a second temperature, performing a low-temperature preliminary thermal cracking reaction on the polyethylene and the superheated gas;
[0065] (s4) the intermediate product obtained in step (s3) is entrained by superheated gas into the second reactor in series;
[0066] (s5) At a third temperature, the mixture in step (s4) enters a second reactor to undergo a high-temperature deep thermal cracking reaction to obtain the long-chain α-olefin.
[0067] In another preferred embodiment, the first temperature is between 500°C and 650°C, preferably between 550°C and 600°C, such as 550°C or 580°C.
[0068] In another preferred embodiment, the second temperature is between 400°C and 550°C, preferably between 450°C and 500°C, such as 450°C or 480°C.
[0069] In another preferred embodiment, the third temperature is between 500°C and 650°C, preferably between 550°C and 600°C, such as 550°C or 580°C.
[0070] In another preferred embodiment, the temperature difference between the first temperature and the third temperature is ≤10°C, preferably ≤5°C, more preferably ≤2°C, for example, the first temperature is the same as the third temperature.
[0071] In another preferred embodiment, the third temperature is higher than the second temperature by at least 30°C, preferably at least 50°C, more preferably at least 70°C, more preferably 100°C.
[0072] In another preferred embodiment, the first temperature is higher than the second temperature by at least 30°C, preferably at least 50°C, more preferably at least 70°C, more preferably 100°C.
[0073] In another preferred embodiment, the first reactor is a tank reactor, preferably a tank reactor with a mixing device, and more preferably a tank reactor with a stirring paddle.
[0074] In another preferred embodiment, the second reactor is a tubular reactor.
[0075] In another preferred embodiment, the preliminary thermal cracking reaction and the deep thermal cracking reaction are each independently carried out under a low-pressure environment.
[0076] In another preferred embodiment, the operating pressures of the preliminary thermal cracking reaction and the deep thermal cracking reaction are independently 0.1 to 0.5 MPa (absolute), for example, 0.1 MPa (absolute) and 0.2 MPa (absolute).
[0077] In another preferred embodiment, the long-chain α-olefins are long-chain α-olefins with 5 to 20 (preferably 5 to 18) carbon atoms, i.e. C5 to C 20 (Preferably C5~C 18 ) has a content of long-chain α-olefins exceeding 99 wt%, preferably exceeding 99.5%, and more preferably exceeding 99.9%.
[0078] In another preferred embodiment, the long-chain α-olefins of 20 to 30 carbon atoms, namely C 20 ~C 30 (Preferred C 18 ~C 30 ) has a content of long-chain α-olefins of less than 1 wt%, preferably less than 0.5 wt%, more preferably less than 0.1 wt%.
[0079] In another preferred embodiment, the long-chain α-olefins include C5 to C 15 The long-chain α-olefin accounts for more than 75 wt% of the total mass of the long-chain α-olefin, preferably more than 80 wt%, for example more than 85 wt%, more than 90 wt%.
[0080] In another preferred embodiment, the polyethylene is selected from the group consisting of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, or a combination thereof.
[0081] In another preferred embodiment, the polyethylene is pure polyethylene resin, or plastic whose main component is polyethylene, or waste plastic whose main component is polyethylene.
[0082] In another preferred embodiment, the weight average molecular weight of the polyethylene is 2×10 4 g / mol~30×10 4 g / mol, preferably 5×10 4 g / mol~20×10 4 g / mol.
[0083] In another preferred embodiment, the number average molecular weight of the polyethylene is 0.5×10 4 g / mol~5×10 4 g / mol, preferably 1×10 4 g / mol~3×10 4 g / mol.
[0084] In another preferred embodiment, the melting point of the polyethylene is 100-200°C, preferably 100-180°C, and more preferably 100-150°C.
[0085] In another preferred embodiment, the density of the polyethylene is 0.75-1.0 g / mL.
[0086] In another preferred embodiment, in step (s1), the polyethylene is added to the first reactor at a temperature lower than the second temperature, preferably at a temperature of 10 to 400°C, and more preferably at room temperature of 10 to 40°C.
[0087] In another preferred embodiment, the step (s2) further comprises a pre-treatment step of purging with an inert gas, wherein the inert gas is selected from one or more of nitrogen, argon, and helium.
[0088] In another preferred embodiment, in step (s2), the volume of the superheated water vapor in the superheated gas accounts for more than 70% of the total volume of the superheated gas, preferably more than 80%, and more preferably more than 90%.
[0089] In another preferred embodiment, in step (s2), the superheated gas is superheated water vapor.
[0090] In another preferred embodiment, in step (s2), the flow rate of the superheated gas is 100-500 mL / min, preferably 100-300 mL / min.
[0091] In another preferred embodiment, in step (s2), the pressure of the superheated gas is 0.1-0.5 MPa (absolute), for example, 0.1 MPa (absolute) or 0.2 MPa (absolute).
[0092] In another preferred embodiment, in step (s2), the superheated gas is continuously introduced into the reaction system until the reaction is completed.
[0093] In another preferred embodiment, the step (s3) further includes the following pre-treatment temperature raising step: heating the first reactor, and when the polyethylene is melted and the viscosity is reduced, starting stirring, and continuing to heat the first reactor to the second temperature.
[0094] In another preferred embodiment, in step (s3), when heated to 200-300°C, the polyethylene melts and the viscosity decreases.
[0095] In another preferred embodiment, the thermal cracking is carried out in a semi-batch manner or a continuous manner, wherein the thermal cracking includes low-temperature preliminary thermal cracking and high-temperature deep thermal cracking.
[0096] In another preferred embodiment, when the thermal cracking is carried out in a semi-batch manner, the step (s3) comprises: in a first reactor at a second temperature, the polyethylene in step (s1) undergoes a low-temperature preliminary thermal cracking reaction with the superheated gas at a first temperature that is continuously introduced into the first reactor.
[0097] In another preferred embodiment, when the thermal cracking is carried out in a continuous manner, the step (s3) includes: continuously introducing superheated gas at the first temperature into the first reactor at the second temperature and continuously adding polyethylene at the second temperature, so that the polyethylene in the first reactor undergoes a low-temperature preliminary thermal cracking reaction with the superheated gas.
[0098] In another preferred embodiment, the polyethylene in the first reactor includes the polyethylene in step (s1) and additionally added polyethylene at the second temperature.
[0099] In another preferred embodiment, in step (s3), the ratio between the polyethylene in step (s1) and the superheated gas introduced is 0.1-10 g:1 mL / min, preferably 0.1-5 g:1 mL / min.
[0100] In another preferred embodiment, in step (s3), the flow rate ratio of the additionally added polyethylene at the second temperature to the flow rate of the superheated gas is 0.01-1 g / min:1 mL / min, preferably 0.01-0.5 g / min:1 mL / min.
[0101] In another preferred embodiment, in step (s5), the time of the deep thermal cracking reaction is 5 to 30 seconds, preferably 10 to 20 seconds.
[0102] In another preferred embodiment, the step (s5) further includes a post-processing step: condensing the reaction mixture through a condenser and entering a collection tank, collecting the liquid phase product (i.e., long-chain α-olefin product) below the collection tank, collecting the gas phase product (i.e., short-chain hydrocarbons of C1 to C4) below the collection tank, and performing necessary oil-water separation on the liquid phase product.
[0103] In another preferred embodiment, the reaction time of the thermal cracking reaction is 20-40 minutes, for example, 30 minutes. The reaction time refers to the time from when the temperature of the first reactor is raised to the second temperature until the reaction is completed and the heating is turned off and the introduction of the superheated gas is stopped.
[0104] In another preferred embodiment, when the method is carried out in a semi-batch manner, the method comprises the following steps:
[0105] (a1) providing polyethylene in a first reactor;
[0106] (b1) continuously introducing a superheated gas at a first temperature into the first reactor, wherein the volume of the superheated gas vapor accounts for more than 50% of the total volume of the superheated gas;
[0107] (c1) starting preheating of the first reactor and the second reactor, wherein the target temperature of the first reactor is the second temperature and the target temperature of the second reactor is the third temperature;
[0108] (d1) when the polyethylene melts and the viscosity decreases, stirring is started and the first reactor is continued to be heated to the second temperature;
[0109] (e1) When the first reactor reaches the second temperature, the timing is started, and the polyethylene and the superheated gas undergo a low-temperature preliminary thermal cracking reaction;
[0110] (f1) the intermediate product obtained in step (e1) is entrained by superheated gas into the second reactor in series;
[0111] (g1) At a third temperature, the intermediate product obtained in step (e1) enters a second reactor for a high-temperature deep thermal cracking reaction to obtain the long-chain α-olefin.
[0112] In another preferred embodiment, when the method is carried out in a continuous manner, the method comprises the following steps:
[0113] (a2) providing polyethylene in a first reactor;
[0114] (b2) continuously introducing a superheated gas at a first temperature into the first reactor, wherein the volume of the superheated gas vapor accounts for more than 50% of the total volume of the superheated gas;
[0115] (c2) starting preheating of the first reactor and the second reactor, wherein the target temperature of the first reactor is the second temperature and the target temperature of the second reactor is the third temperature;
[0116] (d2) when the polyethylene melts and the viscosity decreases, stirring is started and the first reactor is continued to be heated to the second temperature;
[0117] (e2) when the first reactor reaches the second temperature, continuing to introduce the superheated gas at the first temperature and continuously adding polyethylene at the second temperature, so that the polyethylene in the first reactor and the superheated gas undergo a low-temperature preliminary thermal cracking reaction;
[0118] (f2) the intermediate product obtained in step (e2) is entrained by superheated gas into the second reactor in series;
[0119] (g2) At a third temperature, the intermediate product obtained in step (e2) enters a second reactor for a high-temperature deep thermal cracking reaction to obtain the long-chain α-olefin.
[0120] In another preferred embodiment, the yield of long-chain α-olefins obtained by the method is more than 50%, preferably more than 60%, preferably more than 65%.
[0121] In another preferred embodiment, the yield of long-chain α-olefins with a carbon number less than 15 obtained by the method is more than 40%, preferably more than 50%, preferably more than 55%.
[0122] In another preferred embodiment, the co-products obtained by the method include paraffins and a small amount of diolefins.
[0123] In another preferred embodiment, the co-product obtained by the method does not include internal olefins.
[0124] In a fourth aspect of the present invention, there is provided an apparatus comprising a first reactor, a second reactor, a ventilation device and an optional feeding device,
[0125] The ventilation device and optionally the feeding device are connected to the first reactor, the second reactor is connected to the first reactor, and the device is configured to carry out the method according to the third aspect of the present invention.
[0126] In another preferred embodiment, the first reactor is a tank reactor, and the second reactor is a tubular reactor.
[0127] In another preferred embodiment, the bottom of the second reactor is connected to the top of the first reactor, so that the intermediate product reacted in the first reactor is entrained by the superheated gas and passed upward into the second reactor.
[0128] In another preferred embodiment, the gas outlet of the ventilation device in the first reactor is located at the bottom end of the first reactor, so that the superheated gas introduced can fully contact with the polyethylene.
[0129] In another preferred embodiment, the outlet of the feeding device in the first reactor is located at the top or bottom of the first reactor.
[0130] In another preferred embodiment, the first reactor further comprises a stirring device for mixing polyethylene.
[0131] In another preferred example, the device further comprises a first heating device and a second heating device, wherein the first heating device is used to heat the first reactor, and the second heating device is used to heat the second reactor.
[0132] In another preferred example, the first heating device is configured to heat to a second temperature.
[0133] In another preferred example, the second heating device is configured to heat to a third temperature.
[0134] In another preferred embodiment, the device further comprises an optional third heating device and an optional fourth heating device, wherein the third heating device is used to heat the superheated gas in the ventilation device, and the fourth heating device is used to heat the polyethylene in the feeding device.
[0135] In another preferred example, the third heating device is configured to heat to a first temperature.
[0136] In another preferred example, the fourth heating device is configured to heat to a fourth temperature.
[0137] In another preferred example, the device further includes a condensing device.
[0138] In another preferred embodiment, the device further comprises a gas-liquid separator for collecting the obtained long-chain α-olefin liquid product.
[0139] It should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features described in detail below (such as in the embodiments) can be combined with each other to form new or preferred technical solutions. Due to space limitations, they will not be listed here one by one. BRIEF DESCRIPTION OF THE DRAWINGS
[0140] Figure 1 shows a schematic diagram of the process of producing long-chain α-olefins by thermal cracking of polyethylene.
[0141] FIG2 shows a schematic diagram of an experimental apparatus for producing long-chain α-olefins by thermal cracking of polyethylene. DETAILED DESCRIPTION
[0142] After extensive and in-depth research, the inventors have discovered for the first time a method for rapidly converting polyethylene into long-chain α-olefins and co-products by subjecting the polyethylene as a raw material to superheated steam, rapid preheating, and thermal cracking of the mixed system for a period of time. This method, which uses polyethylene as a raw material to produce long-chain α-olefins, not only provides an additional raw material route for the production of long-chain α-olefins but also offers a method for converting waste polyethylene into high-value-added long-chain α-olefins. This is the basis for the present invention.
[0143] the term
[0144] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0145] As used herein, the terms "comprise," "include," and "contain" are used interchangeably to include not only closed definitions but also semi-closed and open definitions. In other words, the terms include "consisting of," "consisting essentially of."
[0146] As used herein, when used in reference to a specific recited value, the term "about" means that the value may vary by no more than 1% from the recited value. For example, as used herein, the expression "about 100" includes all values between 99 and 101 (e.g., 99.1, 99.2, 99.3, 99.4, etc.).
[0147] As used herein, the term "internal olefin" refers to an olefin whose carbon-carbon double bond is not at the end of the molecular chain.
[0148] First method of the present invention
[0149] Polyethylene is a thermoplastic resin produced by the polymerization of ethylene. It includes high-density polyethylene (HDPE), low-density polyethylene (LDPE), and linear low-density polyethylene (LLDPE). Polyethylene is primarily used in the manufacture of agricultural films, packaging films, wire and cable, pipes, hollow containers, and coatings. In 2020, global polyethylene production capacity reached 127 million tons. Notably, polyethylene is not only a common plastic but also a significant component of waste plastics. Waste plastics increased from 156 million tons in 2000 to 353 million tons in 2019, with 72% of this waste ending up in landfills, severely damaging the natural environment.
[0150] Based on this, the present invention provides a method for producing long-chain α-olefins using polyethylene as raw material in a pressurized superheated water vapor environment. This method not only provides an additional raw material route for the production of long-chain α-olefins, but also provides a way to convert waste polyethylene into high-value-added long-chain α-olefins.
[0151] Compared with the applicant's previous patent application using polyolefins as raw materials to continuously thermally crack and prepare liquid hydrocarbon products including gasoline and diesel, the present invention uses polyethylene as raw material and can obtain long-chain α-olefins with high efficiency and high yield.
[0152] Furthermore, in the continuous process for producing long-chain α-olefins of the present invention, the tubular reactor includes a preheating section to preheat the reactants before they enter the thermal cracking section for continued heating to maintain the reaction temperature. In contrast, in the prior patent application, the tubular reactor also includes a preheating section to preheat the reactants before they enter the adiabatic section, eliminating the need for external heat supply. Furthermore, parameters such as the preheating temperature and reaction time differ from those in the prior patent application.
[0153] The method of the present invention specifically comprises the following steps: placing polyethylene in a pressurized superheated water steam environment, rapidly preheating the mixed system and thermally cracking it for a certain period of time, thereby completing the efficient conversion of polyethylene into long-chain α-olefins and other co-products (long-chain alkanes and long-chain internal olefins, etc.).
[0154] In the present invention, the yield of long-chain α-olefins = liquid yield × olefin content in the liquid × α-olefin fraction in the olefins.
[0155] Liquid yield, olefin content in liquid, and α-olefin fraction in olefin are complex functions of preheat rate, preheat temperature, and reaction time (space time), and all have a trend of increasing first and then decreasing. Accordingly, it is necessary to preferably combine the operating process to ensure the yield of long-chain α-olefins.
[0156] Therefore, in order to improve the selectivity and yield of long-chain α-olefins in the polyethylene thermal cracking process, the present invention makes optimizations for the type of polyethylene, the ratio of polyethylene to pressurized superheated water vapor, the pressure of the reaction system, the preheating rate of the thermal cracking system, the preheating temperature of the thermal cracking system, the time (space time) of the thermal cracking reaction, the product distribution of the thermal cracking reaction, and the mode of the thermal cracking reaction:
[0157] Preferably, the polyethylene is one or a mixture of high-density polyethylene, low-density polyethylene and linear low-density polyethylene.
[0158] Preferably, the mass ratio of the polyethylene to the pressurized superheated water steam is 10:1 to 1:2.
[0159] Preferably, the pressure of the thermal cracking reaction system is controlled at 0.2-2.0 MPa (absolute pressure).
[0160] Preferably, the mixed system of polyethylene and pressurized superheated water steam is preheated to the preheating temperature at 20-50° C. / min.
[0161] Preferably, the mixed system of polyethylene and pressurized superheated water steam is preheated to 450-550°C.
[0162] Preferably, the mixed system of polyethylene and pressurized superheated water steam is preheated to a set pyrolysis temperature, and the reaction time (space time) is controlled to be 0.5 to 10 minutes.
[0163] Preferably, polyethylene is thermally cracked in the pressurized superheated water steam environment to produce co-products such as C7-C30 long-chain α-olefins, long-chain alkanes and long-chain internal olefins.
[0164] Preferably, the conversion of polyethylene to long-chain α-olefins and other co-products in the pressurized superheated water steam environment is carried out in a batch or continuous manner.
[0165] Preferably, the first method of the present invention is as described in the first aspect of the present invention.
[0166] In the first method of the present invention, the yield of C7-C30 long-chain α-olefins can reach 30%, and they can be converted into C7-C30 long-chain α-olefins with high selectivity, and the percentage of long-chain α-olefins in liquid olefins reaches about 70%.
[0167] However, the yield of long-chain α-olefins in the product of the first method of the present invention is at most 30%. In addition, the carbon number distribution of the product is in a wide range of C7 to C 30 Therefore, the inventors continued to research and developed the second method of the present invention.
[0168] Second method of the present invention
[0169] Based on the first method of the present invention, the inventors unexpectedly found that by dividing the thermal cracking reaction into low-temperature preliminary thermal cracking at different temperatures and high-temperature deep thermal cracking, the yield can be significantly improved (yield reaches 70%), and the carbon number distribution of long-chain α-olefins is unexpectedly significantly narrowed, C5~C 15 The α-olefin content of the long-chain α-olefin is increased to 93.7 wt%.
[0170] The purpose of the present invention is to provide a method for efficiently producing long-chain α-olefins with diverse raw material sources, high yield of long-chain α-olefins, narrow carbon number distribution, simple operation, moderate investment and compliance with environmental protection requirements.
[0171] Specifically, polyethylene is first subjected to low-temperature preliminary thermal cracking in a low-pressure steam environment in a first reactor, and the intermediate product is carried by steam into a second reactor in series for high-temperature deep thermal cracking, as shown in Figure 1.
[0172] The main cracking products are C5~C 20 Long-chain α-olefins, with paraffins and a small amount of diolefins as co-products.
[0173] In order to increase the yield of the target product, long-chain α-olefins, and to limit the carbon number distribution, the properties of the raw materials, the thermodynamic state and flow rate of the steam, the type and combination of the reactors, and the operating conditions of the reactors are optimized. Specifically:
[0174] The polyethylene is one of high-density polyethylene, low-density polyethylene and linear low-density polyethylene, or a mixture thereof.
[0175] Polyethylene is either a pure resin, or a plastic whose main component is polyethylene, or a waste plastic whose main component is polyethylene.
[0176] The first reactor can be in the form of a tank reactor or the like.
[0177] Polyethylene is pre-heated and cracked in the first reactor at a low temperature, with the pre-heated cracking temperature being 400-550°C.
[0178] Water vapor is introduced into the first reactor, the pressure of the water vapor is between 0.1 and 0.5 MPa (absolute), and the temperature is between 500 and 650°C.
[0179] The water vapor passes through the first reactor and carries the intermediate products produced by the pre-thermal cracking of polyethylene into the second reactor in series.
[0180] The second reactor can be in the form of a tubular reactor or the like.
[0181] The intermediate product from the first reactor is deeply cracked in the second reactor at a temperature of 550-650°C.
[0182] The residence time of the intermediate product from the first reactor in the second reactor is 5 to 30 seconds.
[0183] The operating pressure of the first reactor and the second reactor is 0.1 to 0.5 MPa (absolute).
[0184] After the polyethylene is thermally cracked in the above manner, the main products are C5~C 20 The co-products are alkanes and a small amount of diolefins.
[0185] The thermal cracking of polyethylene in the above reactor can be operated in a semi-batch mode or in a continuous mode.
[0186] The present invention provides a batch and semi-batch reaction process in which only the reaction temperature is increased. It can be seen that if only the reaction temperature is increased, the yield of α-olefins cannot be significantly improved, and it is impossible to achieve both increased yield and shortened α-olefin carbon number distribution.
[0187] Preferably, the second method of the present invention is as described in the third aspect of the present invention.
[0188] The main advantages of the present invention include:
[0189] (1) The present invention not only provides a new raw material route for the production of long-chain α-olefins, but also provides a way to convert waste polyethylene into high-value-added long-chain α-olefins.
[0190] (2) The method of the present invention has a high yield of long-chain α-olefins, a short reaction time, a high production intensity of the continuous reaction, and a low reaction space time.
[0191] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present invention and are not intended to limit the scope of the invention. The experimental methods in the following examples, for which no specific conditions are specified, are generally based on conventional conditions or the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are by weight.
[0192] Example 1
[0193] Low-density polyethylene was thermally cracked in a batch process, and the differences between pressurized superheated steam and pressurized nitrogen as the reaction medium were compared.
[0194] A low-density polyethylene pellet (manufacturer: Sinopec) is used as a representative of low-density polyethylene, and its basic properties are shown in Table 1.
[0195] Table 1 Basic properties of low-density polyethylene used in the experiment
[0196] Batch thermal cracking
[0197] (1) The reaction medium of the present invention is pressurized superheated steam
[0198] The reactor was initially charged with 10g of low-density polyethylene and 2g of deionized water. The reactor was purged with nitrogen and then sealed. The contents were preheated from room temperature to 485°C for approximately 16 minutes. The system pressure was controlled at 0.5 MPa (absolute) using a back-pressure valve located after the reactor. After reaching the preset pyrolysis temperature, the reaction was continued for 0.5, 3, or 5 minutes, and the reactor was then cooled in a cold water bath to quench the pyrolysis.
[0199] (2) Conventional reaction medium pressurized nitrogen
[0200] The reactor was initially charged with 10g of low-density polyethylene (LDPE). After being purged with nitrogen, the reactor was then filled with nitrogen at 0.5 MPa (absolute pressure). The contents were preheated from room temperature to 485°C for approximately 17 minutes. The system pressure was controlled at 0.5 MPa (absolute pressure) using a back-pressure valve located after the reactor. After reaching the desired thermal cracking temperature, the reaction was continued for 0.5, 3, or 5 minutes, and the reactor was then cooled in a cold water bath to quench the thermal cracking.
[0201] Separation and analysis of products
[0202] The pyrolysis products are separated into wax, liquid products and gas products. Among them, the liquid product is defined as a hydrocarbon substance dissolved in dichloromethane. The yield of wax and liquid products is determined by weighing, and the gas yield is determined by normalization. The olefin content in the liquid product is determined by GC-MS, and the proportion of different types of olefins is determined by 1 The product distributions of LDPE pyrolysis at 0.5, 3 and 5 min are shown in Table 2.
[0203] Distribution of thermal cracking products
[0204] Table 2 Distribution of thermal cracking products of low-density polyethylene in pressurized superheated water steam or nitrogen environment
[0205] It can be seen that when nitrogen is used as the reaction medium, most of the olefins in the liquid are internal olefins and the yield of α-olefins is very low.
[0206] Example 2:
[0207] High density polyethylene is used for thermal cracking in a continuous process.
[0208] A certain high-density polyethylene particle (manufacturer: DuPont, USA) is taken as a representative of high-density polyethylene, and its basic properties are shown in Table 3.
[0209] Table 3 Basic properties of high-density polyethylene used in the experiment
[0210] Continuous thermal cracking
[0211] A tubular reactor with zoned temperature control is used for thermal cracking of high-density polyethylene. The inner diameter of the reaction tube is 2 cm and the length is 400 cm. A retractable thermocouple is installed in the tube to determine the axial temperature distribution. The high-density polyethylene is preheated to melt and mixed with superheated water vapor before entering the reaction tube. The mass ratio of high-density polyethylene to water is controlled at 2:1. The pressure in the reaction system is controlled at 1.0 MPa (absolute pressure) by a rear back-pressure valve. The molten high-density polyethylene and superheated water vapor are first preheated in the preheating section of the tubular reactor. After being preheated to the preheating temperature, they enter the thermal cracking section, where external heat is continuously provided to maintain the temperature. By controlling the feed mass flow rate and heating power, the reaction time of the material in the 500°C isothermal zone (i.e., the thermal cracking section) is controlled to 1, 5, and 10 minutes, respectively.
[0212] Separation and analysis of products
[0213] The pyrolysis products are rapidly cooled to 60°C after flowing out of the reactor. The products are then separated into wax, liquid products and gas products. Among them, liquid products are defined as hydrocarbon substances dissolved in dichloromethane. The yields of wax and liquid products are determined by weighing, and the gas yield is determined by normalization. The olefin content in the liquid product is determined by GC-MS, and the proportion of different types of olefins is determined by 1 The product distributions are shown in Table 4 when the reaction time in the 500°C isothermal zone is 1, 5, and 10 minutes, respectively.
[0214] Distribution of thermal cracking products
[0215] Table 4 Distribution of thermal cracking products of high-density polyethylene in pressurized superheated steam environment
[0216] It can be seen that polyethylene can also be produced in a high yield of α-olefins using a continuous process.
[0217] Example 3:
[0218] A polyolefin mixture was thermally cracked in a batch mode, and the effects of fast preheating (about 35℃ / min) and slow preheating (about 15℃ / min) on the product distribution were compared.
[0219] Linear low-density polyethylene (LLDPE) pellets (manufacturer: Dow Chemical) were used as a representative of LLDPE, and their basic properties are shown in Table 5. The LDPE used in Example 1 was used as a representative of LDPE, and the HDPE used in Example 2 was used as a representative of HDPE. The HDPE, LDPE, and LLDPE pellets were mixed in a mass ratio of 1:1:1 to form a polyethylene mixture.
[0220] Table 5 Basic properties of linear low density polyethylene used in the experiment
[0221] Rapid preheating intermittent pyrolysis
[0222] The reactor was initially charged with 10g of a polyethylene mixture and 15g of deionized water. The reactor was then sealed after being purged with nitrogen. The contents were preheated from room temperature to 485°C, 515°C, or 545°C for approximately 13, 14, or 16 minutes, respectively. The system pressure was controlled at 1.5 MPa (absolute) using a backpressure valve located after the reactor. After reaching the desired thermal cracking temperature, the reaction was continued for 1 minute, followed by cooling the reactor in a cold water bath to quench the thermal cracking.
[0223] Slow preheating intermittent pyrolysis
[0224] The reactor was initially charged with 10g of a polyethylene mixture and 15g of deionized water. The reactor was then sealed after being purged with nitrogen. The contents were preheated from room temperature to 485°C, 515°C, or 545°C for approximately 31, 33, or 35 minutes, respectively. The system pressure was controlled at 1.5 MPa (absolute) using a backpressure valve located after the reactor. After reaching the desired thermal cracking temperature, the reaction was continued for 1 minute, followed by cooling the reactor in a cold water bath to quench the thermal cracking.
[0225] Separation and analysis of products
[0226] The pyrolysis products are separated into wax, liquid products and gas products. Among them, the liquid product is defined as a hydrocarbon substance dissolved in dichloromethane. The yield of wax and liquid products is determined by weighing, and the gas yield is determined by normalization. The olefin content in the liquid product is determined by GC-MS, and the proportion of different types of olefins is determined by 1 The product distribution under different preset pyrolysis temperature conditions is shown in Table 6.
[0227] Polyethylene blend product distribution
[0228] Table 6 Distribution of thermal cracking products of polyethylene mixture in pressurized superheated water steam environment
[0229] It can be seen that the preheating speed also affects the product distribution. When the preheating speed is slow, the liquid yield is reduced, the olefin content in the liquid is reduced, and a large amount of internal olefins are present in the olefins in the liquid, resulting in a low overall α-olefin yield.
[0230] Embodiment 4:
[0231] Polypropylene was thermally cracked in a batch process.
[0232] A certain polypropylene pellet (manufacturer: Sinopec Maoming Branch) is taken as a representative of polypropylene, and its basic properties are shown in Table 7.
[0233] Table 7 Basic properties of polypropylene used in the experiment
[0234] Batch thermal cracking
[0235] The reactor was initially charged with 10g of polypropylene and 15g of deionized water. The reactor was then sealed after being purged with nitrogen. The contents were preheated from room temperature to 485°C, 515°C, or 545°C for approximately 13, 14, or 16 minutes, respectively. The system pressure was controlled at 1.5 MPa (absolute) using a backpressure valve located after the reactor. After reaching the desired thermal cracking temperature, the reaction was continued for 1 minute, followed by cooling the reactor in a cold water bath to quench the thermal cracking.
[0236] Separation and analysis of products
[0237] The pyrolysis products are separated into wax, liquid products and gas products. Among them, the liquid product is defined as a hydrocarbon substance dissolved in dichloromethane. The yield of wax and liquid products is determined by weighing, and the gas yield is determined by normalization. The olefin content in the liquid product is determined by GC-MS, and the proportion of different types of olefins is determined by 1 Confirmed by H-NMR.
[0238] Distribution of polypropylene thermal cracking products
[0239] For polypropylene feedstock, the yield of liquid products at each preset thermal cracking temperature ranged from 90% to 92%. The highest content of the liquid products was 2,4-dimethyl-1-heptene, with a yield of 7.11%. The remainder consisted of a complex mixture of isomers of various C7-C30 alkanes and alkenes.
[0240] Although polyethylene and polypropylene are both polyolefins, when polypropylene is used as a raw material, only various hydrocarbons with a high degree of branching can be obtained, and long-chain α-olefins cannot be obtained with high selectivity.
[0241] Example 5
[0242] Low-density polyethylene resin is used as raw material. Pre-pyrolysis is carried out in a semi-batch manner in a reactor shown in Figure 2 under a normal pressure steam environment. The steam entrains the pre-pyrolysis intermediates into a series of tubular reactors for deep pyrolysis to obtain products mainly composed of long-chain α-olefins.
[0243] At the same time, referring to the process characteristics described in CN202310571518.X (the first method of the present invention), single lower and higher temperature intermittent or semi-intermittent polyethylene thermal cracking is carried out.
[0244] Raw material: low-density polyethylene resin (manufacturer: Sinopec), the properties of which are shown in Table 8.
[0245] Table 8 Properties of low-density polyethylene resin used in the experiment
[0246] Product analysis method: The possible products of thermal cracking are wax, liquid products and gas products. Among them, liquid products are defined as hydrocarbon substances dissolved in dichloromethane. The yields of wax and liquid products are determined by weighing, and the gas yield is determined by normalization. The olefin content in the liquid product is determined by GC-FID, and the proportion of different types of olefins is determined by 1 Confirmed by H-NMR.
[0247] Reactor: The effective volume of the kettle reactor is 1000 mL, and the heating method is electric heating; the effective volume of the tubular reactor is 50 mL, and the heating method is electric induction heating.
[0248] ●Operation process of the present invention and analysis results of pyrolysis products:
[0249] 1) Place 200 g of polyethylene resin pellets in a tank reactor.
[0250] 2) After nitrogen purging, steam at 0.1 MPa (gauge pressure) and 550°C was introduced into the autoclave reactor at a steam flow rate of 150 mL / min. At this steam flow rate, the residence time of the polyethylene pre-cracking intermediate product entrained in the tubular reactor was approximately 20 seconds.
[0251] 3) Start preheating of the autoclave reactor and the tubular reactor, setting the target temperatures to 450 and 550°C, respectively.
[0252] 4) When the temperature in the autoclave reaches 250°C, start stirring and maintain the stirring speed at 250 RPM.
[0253] 5) Start timing when the temperature in the reactor reaches 450°C.
[0254] 6) After 30 minutes, stop heating the reactor and tubular reactor and stop introducing water vapor.
[0255] 7) After the reaction system is cooled, the product is collected from below the gas-liquid separation tank after the reactor, and various characterizations are performed after necessary oil-water separation.
[0256] The results are shown in Tables 9-10 below. It can be seen that after using staged cracking, the yield of α-olefins increased significantly to more than 70%. In particular, the carbon number distribution of olefins is very narrow, and the vast majority (93.7%) of α-olefins are C5-C 15 Olefins. <C 15 The highest yield of α-olefins reached 65.8 wt%.
[0257] Table 9 Properties and distribution of cracking products
[0258] Table 10 Carbon number distribution of α-olefins in products
[0259] ● Refer to CN202310571518.X, single low temperature intermittent pyrolysis and pyrolysis product analysis results:
[0260] 1) Place 200 g of polyethylene resin pellets in a tank reactor.
[0261] 2) After nitrogen purging, water vapor at 0.1 MPa (gauge pressure) and 450° C. was introduced into the autoclave reactor. The valve above the reactor was then closed, and the introduction of water vapor was stopped.
[0262] 3) Start preheating of the autoclave reactor and set the target temperature to 450°C.
[0263] 4) When the temperature in the autoclave reactor reaches 250°C, start stirring and maintain the stirring speed at 250 RPM.
[0264] 5) Start timing when the temperature in the reactor reaches 450°C.
[0265] 6) Stop heating the reactor after 10, 20 or 30 minutes.
[0266] 7) After the reaction system is cooled, the product is collected from the reactor, and the necessary oil-water separation is performed before various characterizations are performed.
[0267] The results are shown in Tables 11-12 below.
[0268] Table 11 Properties and distribution of cracking products
[0269] Table 12 Carbon number distribution of α-olefins in products (wt%)
[0270] The highest yield of α-olefins obtained by batch thermal cracking of polyethylene at a single low temperature of 450°C was 16.9 wt%. The liquid product had a wide distribution of C7 to C 30 . In the product <C 20 The highest yield of α-olefins is only 13.2 wt%. <C 15 The highest yield of α-olefins was only 8.9 wt%.
[0271] ● Refer to CN202310571518.X single high temperature intermittent pyrolysis and pyrolysis product analysis results:
[0272] 1) Place 200 g of polyethylene resin pellets in a tank reactor.
[0273] 2) After nitrogen purging, water vapor at 0.1 MPa (gauge pressure) and 550° C. was introduced into the autoclave reactor. The valve above the reactor was then closed, and the introduction of water vapor was stopped.
[0274] 3) Start preheating of the autoclave reactor and set the target temperature to 550°C.
[0275] 4) When the temperature in the autoclave reactor reaches 250°C, start stirring and maintain the stirring speed at 250 RPM.
[0276] 5) Start timing when the temperature in the reactor reaches 550°C.
[0277] 6) Stop heating the reactor after 10, 20 or 30 minutes.
[0278] 7) After the reaction system is cooled, the product is collected from the reactor, and the necessary oil-water separation is performed before various characterizations are performed.
[0279] The results are shown in Tables 13-14 below.
[0280] Table 13 Properties and distribution of cracking products
[0281] Table 14 Carbon number distribution of α-olefins in products
[0282] The highest yield of α-olefins obtained by batch thermal cracking of polyethylene at a single high temperature of 550°C was 10.3 wt%. The liquid product had a wide distribution of C7 to C 30 . In the product <C 20 The highest yield of α-olefins is only 9.7 wt%. <C 15 The highest yield of α-olefins was only 7.1 wt%.
[0283] Moreover, although the carbon number distribution of α-olefins becomes narrower with the extension of reaction time, the total yield of α-olefins gradually decreases with the extension of reaction time, and the yield of internal olefins in the total olefins increases. After the reaction time is extended from 10 min to 30 min, the yield actually decreases from 10.3 wt% to 4.8 wt%.
[0284] ● Refer to CN202310571518.X, single low temperature semi-batch pyrolysis and pyrolysis product analysis results:
[0285] 1) Place 200 g of polyethylene resin pellets in a tank reactor.
[0286] 2) After nitrogen purging, water vapor at 0.1 MPa (gauge pressure) and 450° C. was introduced into the autoclave reactor at a flow rate of 150 mL / min.
[0287] 3) Start preheating of the autoclave reactor and the tubular reactor, and set the target temperature to 450°C.
[0288] 4) When the temperature in the autoclave reaches 250°C, start stirring and maintain the stirring speed at 250 RPM.
[0289] 5) Start timing when the temperature in the reactor reaches 450°C.
[0290] 6) After 30 minutes, stop heating the reactor and tubular reactor and stop introducing water vapor.
[0291] 7) After the reaction system is cooled, the product is collected from below the gas-liquid separation tank after the reactor, and various characterizations are performed after necessary oil-water separation.
[0292] The results are shown in Tables 15-16 below.
[0293] Table 15 Properties and distribution of cracking products
[0294] Table 16 Carbon number distribution of α-olefins in products
[0295] Semi-batch thermal cracking of polyethylene was carried out at a single lower temperature of 450°C. 24 wt% wax appeared in the product. The highest yield of α-olefins obtained was 17.3 wt%. The liquid product distribution was very broad, ranging from C7 to C 30 , wherein the average content of α-olefins with different carbon numbers is about 20wt% to 30wt%. <C 20 The highest yield of α-olefins is only 11.9wt%. <C 15 The highest yield of α-olefins was only 7.1 wt%.
[0296] ● Refer to CN202310571518.X, single high temperature semi-batch pyrolysis and pyrolysis product analysis results:
[0297] 1) Place 200 g of polyethylene resin pellets in a tank reactor.
[0298] 2) After nitrogen purging, water vapor at 0.1 MPa (gauge pressure) and 550° C. was introduced into the autoclave reactor at a flow rate of 150 mL / min.
[0299] 3) Start preheating of the autoclave reactor and the tubular reactor, and set the target temperature to 550°C.
[0300] 4) When the temperature in the autoclave reaches 250°C, start stirring and maintain the stirring speed at 250 RPM.
[0301] 5) Start timing when the temperature in the reactor reaches 550°C.
[0302] 6) After 30 minutes, stop heating the reactor and tubular reactor and stop introducing water vapor.
[0303] 7) After the reaction system is cooled, the product is collected from below the gas-liquid separation tank after the reactor, and various characterizations are performed after necessary oil-water separation.
[0304] The results are shown in Tables 17-18 below.
[0305] Table 17 Properties and distribution of cracking products
[0306] Table 18 Carbon number distribution of α-olefins in products
[0307] Semi-batch thermal cracking of polyethylene was carried out at a single higher temperature of 550°C. The total olefin content of the liquid was reduced to only 52 wt%, and a large amount of gas was produced. Therefore, the maximum yield of α-olefins obtained was only 29.7 wt%. The liquid product distribution was slightly narrow, with C5 to C 25 . In the product <C 20 The highest yield of α-olefins is only 26.2 wt%. <C 15 The highest yield of α-olefins was only 20.4 wt%.
[0308] Example 6:
[0309] Using waste plastics, primarily high-density polyethylene, as raw material, the process is semi-batch pre-pyrolysis in a normal pressure steam environment in the reactor shown in Figure 2. The steam then carries the pyrolysis intermediates into a series of tubular reactors for deep pyrolysis, yielding products primarily composed of long-chain α-olefins.
[0310] Raw materials: High-density polyethylene (HDPE) waste plastics from shampoo bottles, pre-processed into 2 mm x 2 mm flakes. Basic properties are shown in Table 19.
[0311] Table 19 Properties of high-density polyethylene waste plastics used in the experiment
[0312] Product analysis method: Thermal cracking products may be solids, waxes, liquid products and gaseous products. Among them, solids are defined as substances that remain at the bottom of the reactor after the reaction and have no fluidity at 100°C. Liquid products are defined as hydrocarbon substances dissolved in dichloromethane. The yields of wax and liquid products are determined by weighing, and the gas yield is determined by normalization. The olefin content in the liquid product is determined by GC-FID, and the proportion of different types of olefins is determined by 1 Confirmed by H-NMR.
[0313] Reactor: The effective volume of the kettle reactor is 1000 mL, and the heating method is electric heating; the effective volume of the tubular reactor is 50 mL, and the heating method is electric induction heating.
[0314] Operation process:
[0315] 1) 200 g of polyethylene waste plastic flake particles were placed in a tank reactor.
[0316] 2) After nitrogen purging, water vapor at 0.1 MPa (gauge pressure) and 550° C. is introduced into the autoclave reactor at a water vapor flow rate of 150 mL / min. At this flow rate, the residence time of the water vapor entrained with the polyethylene pre-cracking intermediate in the tubular reactor is about 20 s.
[0317] 3) Start preheating of the autoclave reactor and the tubular reactor, setting the target temperatures to 450 and 550°C, respectively.
[0318] 4) When the temperature in the autoclave reaches 250°C, start stirring and maintain the stirring speed at 250 RPM.
[0319] 5) Start timing when the temperature in the reactor reaches 450°C.
[0320] 6) After 30 minutes, stop heating the reactor and tubular reactor and stop introducing water steam.
[0321] 7) After the reaction system cools down, open the reactor and collect the solid product from the bottom of the reactor; collect the product from the bottom of the gas-liquid separation tank after the reactor, perform necessary oil-water separation, and then perform various characterizations.
[0322] Pyrolysis product analysis results
[0323] The results are shown in Tables 20-21 below. It can be seen that after using the staged temperature cracking, the yield of α-olefins increased significantly to more than 70%. In particular, the carbon number distribution of the olefins was very narrow, and the vast majority (91.2%) of the α-olefins were C5-C 15 Olefins.
[0324] Table 20 Properties and distribution of cracking products
[0325] If the polyethylene content in the waste plastic is 88.2% as a basis, the yield of α-olefin is 71.2%.
[0326] Table 21 Carbon number distribution of α-olefins in products
[0327] Example 7
[0328] A mixture of low-density polyethylene resin, high-density polyethylene resin, and linear low-density polyethylene resin is used as raw material. Pre-pyrolysis is continuously performed in a low-pressure steam environment in the reactor shown in Figure 2. The steam entrains the pyrolysis intermediates into a series of tubular reactors for deep pyrolysis, yielding products primarily composed of long-chain α-olefins.
[0329] Raw materials: A mixture of low-density polyethylene resin (manufacturer: Sinopec), high-density polyethylene resin (manufacturer: Sinopec), and linear low-density polyethylene resin (manufacturer: Sinopec). The mass ratio of the mixture is 1:1:1. The basic properties of the resin are shown in Table 22.
[0330] Table 22 Properties of the polyethylene resin used in the experiment
[0331] Product analysis method: The possible products of thermal cracking are wax, liquid products and gas products. Liquid products are defined as hydrocarbons dissolved in dichloromethane. The yields of wax and liquid products are determined by weighing, and the gas yield is determined by normalization. The olefin content in the liquid product is determined by GC-FID, and the proportion of different types of olefins is determined by 1 Confirmed by H-NMR.
[0332] Reactor: The effective volume of the kettle reactor is 1000 mL, and the heating method is electric heating; the effective volume of the tubular reactor is 50 mL, and the heating method is electric induction heating.
[0333] Polyethylene feed: screw extrusion is used to feed the kettle reactor.
[0334] Operation process:
[0335] 1) Place 200 g of polyethylene granules in a tank reactor.
[0336] 2) After nitrogen purging, water vapor at 0.2 MPa (gauge pressure) and 580° C. is introduced into the autoclave reactor at a flow rate of 300 mL / min. At this flow rate, the residence time of the water vapor entrained with the polyethylene pre-cracking intermediate in the tubular reactor is about 10 s.
[0337] 3) Start preheating of the autoclave reactor and the tubular reactor, and set the target temperatures to 480 and 580°C, respectively.
[0338] 4) When the temperature in the autoclave reaches 250°C, start stirring and maintain the stirring speed at 250 RPM.
[0339] 5) When the temperature in the reactor reaches 480°C, molten polyethylene at a temperature of 480°C is added into the reactor at a rate of 20 g / min.
[0340] 6) After the system operation is stable, collect the liquid product from the bottom of the gas-liquid separation tank after the reactor, perform necessary oil-water separation and then conduct various characterizations.
[0341] Pyrolysis product analysis results
[0342] The results are shown in Tables 23-24 below. It can be seen that after using the staged temperature cracking, the yield of α-olefins increased significantly to about 70%, especially the carbon number distribution of olefins was very narrow, and all α-olefins were C5~C 18 Olefins, the vast majority (88.4%) of α-olefins are C5-C 15 Olefins.
[0343] Table 23 Properties and distribution of cracking products
[0344] Table 24 Carbon number distribution of α-olefins in products
[0345] All documents mentioned in this application are incorporated herein by reference, just as if each document were incorporated herein by reference individually. It should also be understood that after reading the above teachings of the present invention, those skilled in the art may make various changes or modifications to the present invention, and that such equivalents also fall within the scope of the claims appended hereto.
Claims
1. A method for preparing long-chain α-olefins, characterized in that: The method comprises the steps of: (s1) providing a preheated gas-liquid mixture, wherein the gas-liquid mixture comprises molten polyethylene and water vapor; and (s2) subjecting the gas-liquid mixture to a thermal cracking reaction under a pressurized environment to obtain long-chain α-olefins; The preheating refers to preheating to 450-550°C.
2. The method according to claim 1, characterized in that The polyethylene is selected from the group consisting of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, or a combination thereof.
3. The method according to claim 1, characterized in that The mass ratio of the polyethylene to the water vapor is 10:1 to 1:10, preferably 5:1 to 1:5, for example 5:1, 2:1, 1:1.5, 1:
2.
4. The method according to claim 1, characterized in that The preheating refers to preheating to 450-550° C. at 20-50° C. / min.
5. The method according to claim 1, characterized in that The pressurized environment refers to that the pressure of the reaction system is controlled at 0.2-2.0 MPa (absolute pressure), for example, 0.5 MPa, 1 MPa, 1.5 MPa.
6. The method according to claim 1, characterized in that The thermal cracking reaction is carried out at 450-550°C, for example, 485°C, 515°C, 545°C.
7. The method according to claim 1, characterized in that The reaction is carried out in a batch or continuous manner.
8. The method according to claim 7, characterized in that When the reaction is carried out in an intermittent manner, the reaction time of the thermal cracking reaction is 0.5 to 10 min, for example, 0.5 min, 1 min, 3 min, 5 min, 10 min; When the reaction is carried out in a continuous manner, the reaction time of the thermal cracking reaction is 0.5 to 10 min, for example, 0.5 min, 1 min, 3 min, 5 min, 10 min.
9. The method according to claim 7, characterized in that When the reaction is carried out in an intermittent manner, the reaction includes: adding polyethylene and water, purging with nitrogen for pretreatment, preheating the material in the kettle at 20-50°C / min to a preheating temperature (preferably 450-550°C), controlling the system pressure at 0.2-2.0MPa (absolute pressure), continuing the reaction for a period of time (0.5-10min) after reaching the preset thermal cracking temperature, and rapidly cooling to quench the thermal cracking; When the reaction is carried out in a continuous manner, the reaction includes: molten polyethylene is mixed with superheated water steam and enters the reaction tube, and thermal cracking occurs after being preheated to the preheating temperature. The pressure in the reaction system is controlled at 0.2 to 2.0 MPa (absolute pressure), and then the product flows out of the reactor.
10. A device, characterized in that: The device comprises a tubular reaction device, a pressurizing device and a thermocouple, wherein the tubular reaction device comprises a first temperature control zone and a second temperature control zone, wherein the first temperature control zone is used for preheating, and the second temperature control zone is used for thermal cracking reaction. The apparatus is configured to perform the method as claimed in claim 1.
11. A method for preparing long-chain α-olefins by thermal cracking of polyethylene, the method comprising the steps of: (s1) providing polyethylene in a first reactor; (s2) continuously introducing a superheated gas at a first temperature into the first reactor, wherein the volume of the superheated water vapor in the superheated gas accounts for more than 50% of the total volume of the superheated gas; (s3) in the first reactor, at a second temperature, the polyethylene and the superheated gas undergo a low-temperature preliminary thermal cracking reaction; (s4) the intermediate product obtained in step (s3) enters the second reactor in series under the entrainment of superheated gas; (s5) at a third temperature, the mixture in step (s4) enters a second reactor to undergo a high-temperature deep thermal cracking reaction to obtain the long-chain α-olefin; in, The first temperature is between 500 and 650° C., the second temperature is between 400 and 550° C., and the third temperature is between 500 and 650° C. Furthermore, the first temperature is higher than the second temperature by at least 50° C., and the third temperature is higher than the second temperature by at least 50° C.
12. The method according to claim 11, characterized in that The long-chain α-olefin refers to a long-chain α-olefin having 5 to 20 (preferably 5 to 18) carbon atoms.
13. The method according to claim 11, characterized in that The first reactor is a tank reactor; the second reactor is a tubular reactor.
14. The method according to claim 11, characterized in that The polyethylene is selected from the group consisting of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, or a combination thereof.
15. The method according to claim 11, characterized in that In step (s2), the superheated gas is superheated water vapor.
16. The method according to claim 11, characterized in that In step (s2), the pressure of the superheated gas is 0.1 to 0.5 MPa (absolute).
17. The method according to claim 11, characterized in that The thermal cracking is carried out in a semi-batch mode or a continuous mode.
18. The method according to claim 11, characterized in that In step (s5), the deep thermal cracking reaction time is 5 to 30 seconds, preferably 10 to 20 seconds.
19. A device, characterized in that: The device comprises a first reactor, a second reactor, a ventilation device and an optional feeding device, The aeration device and optionally the feeding device are connected to the first reactor, the second reactor is connected to the first reactor, and the device is configured to carry out the method as claimed in claim 11.
20. The device according to claim 19, characterized in that The bottom of the second reactor is connected to the top of the first reactor; the gas outlet of the ventilation device in the first reactor is located at the bottom end of the first reactor.
Citation Information
Patent Citations
Apparatus and method thereof for directly heating and cracking waste polyolefin by oxy-hydrogen combustion method
CN105524642A
Method for using polyolefin plastic to prepare micromolecule alkene
CN106520176A
Continuous method and system for waste polyolefin thermal cracking resource recovery
CN116063736A
Method for preparing single aromatic ring chemical raw material through thermal cracking of waste polystyrene
CN117185890A
Method for preparing long-chain alpha-olefin from polyethylene
CN117186928A