Topological cyclodextrin / chitosan composite membrane, preparation method therefor and use thereof

By using α-cyclodextrin and PEG in chitosan composite membranes, the problem of insufficient mechanical properties of chitosan composite membranes is solved, and a significant improvement in high tensile strength and elongation of break is achieved. And simplified the preparation process.

WO2024240183A1PCT designated stage expired Publication Date: 2024-11-28JIANGNAN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/094688
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-22
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing chitosan composite membrane preparation process is complex, with poor mechanical strength and elongation at break performance, which cannot meet the needs.

Method used

Using α-cyclodextrin and polyethylene glycol (PEG) as raw materials to prepare cyclodextrin-polyethylene glycol nanoparticles with topological structure, filled in chitosan network matrix, and topological rings are prepared by casting method. Dextrin/chitosan composite membrane improves its mechanical properties.

Benefits of technology

The tensile strength and elongation of the chitosan composite film were significantly improved, the breaking strength was increased by more than 160%, the elongation of the breaking was increased by 21.6%, and the flexibility of the film was enhanced, simplified the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024094688-FTAPPB-I100001
    Figure PCTCN2024094688-FTAPPB-I100001
  • Figure PCTCN2024094688-FTAPPB-I100002
    Figure PCTCN2024094688-FTAPPB-I100002
  • Figure PCTCN2024094688-FTAPPB-I100003
    Figure PCTCN2024094688-FTAPPB-I100003
Patent Text Reader

Abstract

The present invention relates to the technical field of bio-based nano materials. Disclosed are a topological cyclodextrin / chitosan composite membrane, a preparation method therefor and a use thereof. In the present invention, α-cyclodextrin and polyethylene glycol (PEG) are taken as raw materials to prepare cyclodextrin-polyethylene glycol "ring-sliding" nano particles (TNPs) having a topological structure; TNPs, as green and degradable nano-particles, fill a chitosan network matrix, and the hydrogen bond interaction between the TNPs and chitosan molecules is enhanced, thereby improving the mechanical properties of a chitosan membrane; the method not only involves simple raw materials and convenient and easily implemented operations, but also can effectively improve the mechanical strength of a chitosan composite membrane, effectively solves the problem in the prior art of poor mechanical strength of the chitosan composite membrane, and provides a simple and effective way for actual production.
Need to check novelty before this filing date? Find Prior Art

Description

A topological cyclodextrin / chitosan composite membrane and its preparation method and application Technical Field

[0001] The present invention relates to the technical field of bio-based nanomaterials, and in particular to a topological cyclodextrin / chitosan composite membrane and a preparation method and application thereof. Background Art

[0002] In recent years, plastic pollution has caused irreversible damage to soil and water sources. Against the backdrop of the "plastic ban", "carbon neutrality" and "carbon peak", the development of new environmentally friendly and degradable packaging is an important development direction for future food packaging.

[0003] Currently, most commonly used food packaging materials are made from polyethylene (PE), a type of plastic. These packaging materials are not only highly susceptible to secondary environmental pollution but also pose a threat to human health. Therefore, developing green, safe, and biodegradable food packaging alternatives to plastic packaging is imperative.

[0004] Chitosan is a natural bioactive polymer widely distributed in nature, exhibiting excellent biocompatibility, biodegradability, and antimicrobial activity. Its excellent film-forming properties make it one of the most popular biodegradable materials. However, pure chitosan films exhibit poor water resistance and mechanical properties degrade upon contact with water, significantly limiting their practical applications. Furthermore, pure chitosan films also suffer from insufficient mechanical properties and limited antimicrobial activity.

[0005] In response to the shortcomings of these chitosan films, current research mainly focuses on developing nanoparticles to enhance the mechanical properties of chitosan films; for example, metal nanoparticles and metal oxide nanoparticles are commonly used additives in bioactive packaging systems, but they have poor biocompatibility, are non-degradable, and have potential biotoxicity.

[0006] Cyclodextrins (CDs) are a class of cyclic oligosaccharides prepared by enzymatic hydrolysis of starch. Their unique hydrophobic inner cavity can act as a host molecule to capture hydrophobic guest molecules, resulting in host-guest interactions, and have attracted widespread attention in the design of supramolecular crosslinkers.

[0007] Chinese patent CN107474295A discloses a method for preparing a β-cyclodextrin-chitosan composite material, specifically comprising dissolving β-cyclodextrin, citric acid, and PEG-400 in water to form solution A; adding a catalyst to solution A to form a β-cyclodextrin polymer, which is then added to a chitosan aqueous solution to prepare a β-cyclodextrin-chitosan composite material. Chinese patent CN105384973B discloses a modified β-cyclodextrin / chitosan complex and its preparation and application, specifically comprising preparing an intermediate product using β-cyclodextrin, a modifier, a catalyst, and a cross-linking agent; then adding the intermediate product to a chitosan solution to obtain a modified β-cyclodextrin / chitosan complex under the action of a catalyst. Although both methods employ β-cyclodextrin to enhance the tensile and tear resistance of chitosan, the preparation process requires the use of a cross-linking agent and a catalyst, resulting in a cumbersome process. Furthermore, the improvement in the mechanical properties of the chitosan composite film is limited, which still fails to meet the demand.

[0008] Summary of the Invention [Technical Issues]

[0009] The existing chitosan composite membrane preparation process is complicated, and the chitosan composite membrane has poor tensile strength and elongation at break properties, which cannot meet the needs.

[0010] [Technical solution]

[0011] In response to the defects and shortcomings of the existing technology, the present invention provides a topological cyclodextrin / chitosan composite membrane and its preparation method and application; the preparation of the topological cyclodextrin / chitosan composite membrane of the present invention is to develop elastic cyclodextrin nanoparticles with a topological structure using α-cyclodextrin and polyethylene glycol (molecular weight of 600-8000) as raw materials, and add the cyclodextrin nanoparticles to chitosan to prepare a chitosan composite membrane with high strength; this method not only has simple raw materials and is easy to operate and implement, but also can effectively improve the mechanical strength of the chitosan composite membrane, effectively compensating for the problem of poor mechanical strength of the chitosan composite membrane in the existing technology, and providing a simple and effective way for actual production.

[0012] The first object of the present invention is to provide a method for preparing a topological cyclodextrin / chitosan composite membrane, the method comprising the following steps:

[0013] (1) Dissolving α-cyclodextrin in water by heating, adding polyethylene glycol and stirring, and allowing to stand to form a precipitate, which is then filtered and dried to obtain α-cyclodextrin-polyethylene glycol nanoparticles (TNPs);

[0014] (2) dissolving chitosan, adding glycerol and the α-cyclodextrin-polyethylene glycol nanoparticles prepared in step (1), stirring and dissolving to obtain a mixed membrane solution;

[0015] (3) The mixed membrane solution obtained in step (2) is used to form a membrane by a casting method to obtain a topological cyclodextrin / chitosan composite membrane.

[0016] In one embodiment, the heating temperature in step (1) is 40-70°C.

[0017] In one embodiment, the heating temperature in step (1) is 60-70°C.

[0018] In one embodiment, the dissolving of α-cyclodextrin in step (1) refers to dissolving α-cyclodextrin in water to form an α-cyclodextrin aqueous solution; wherein the solid-liquid ratio of α-cyclodextrin to water is 1-5:10-20, g / ml; preferably 1:10, g / ml.

[0019] In one embodiment, the polyethylene glycol (PEG) in step (1) has a molecular weight of 600 to 8000.

[0020] In one embodiment, the molecular weight of the polyethylene glycol PEG in step (1) is 800 to 6000.

[0021] In one embodiment, the polyethylene glycol (PEG) in step (1) has a molecular weight of 1000 to 2000.

[0022] In one embodiment, the polyethylene glycol PEG in step (1) is PEG1000.

[0023] In one embodiment, the mass ratio of the polyethylene glycol to α-cyclodextrin in step (1) is 1-5:2-3.

[0024] In one embodiment, the mass ratio of the polyethylene glycol to α-cyclodextrin in step (1) is 1:1.

[0025] In one embodiment, the stirring time in step (1) is 2 to 6 hours.

[0026] In one embodiment, the stirring time in step (1) is 2 to 4 hours.

[0027] In one embodiment, the filtration in step (1) is performed using a vacuum pump to obtain a precipitate.

[0028] In one embodiment, the drying conditions in step (1) are: a temperature of 40 to 60° C., and drying to a constant weight.

[0029] In one embodiment, the chitosan dissolving in step (2) refers to dissolving chitosan in acetic acid solution to form a chitosan solution; wherein the mass concentration of chitosan in the chitosan solution is 1 wt% to 3 wt%.

[0030] In one embodiment, the acetic acid solution is an acetic acid aqueous solution with a mass concentration of 1 to 5%.

[0031] In one embodiment, the chitosan is dissolved in the acetic acid solution at 40-60° C. and stirred at a stirring speed of 400-800 r / min for 4-8 hours.

[0032] In one embodiment, the chitosan is dissolved in the acetic acid solution at 40° C. and stirred at a stirring speed of 600 r / min for 4 hours.

[0033] In one embodiment, the mass of the glycerol in step (2) is 3% to 5% of the mass of the chitosan solution.

[0034] In one embodiment, the mass of the glycerol in step (2) is 3% of the mass of the chitosan solution.

[0035] In one embodiment, the mass of the α-cyclodextrin-polyethylene glycol nanoparticles TNPs in step (2) is 0.2%-0.8% of the mass of the chitosan solution.

[0036] In one embodiment, the mass of the α-cyclodextrin-polyethylene glycol nanoparticles TNPs in step (2) is 0.6% of the mass of the chitosan solution.

[0037] In one embodiment, the mass ratio of chitosan to α-cyclodextrin-polyethylene glycol nanoparticles in step (2) is 1:0.2-0.8.

[0038] In one embodiment, the mass ratio of chitosan to α-cyclodextrin-polyethylene glycol nanoparticles in step (2) is 1:0.2 to 0.6, preferably 1:0.6.

[0039] In one embodiment, the stirring speed in step (2) is 200 to 600 r / min, and the stirring time is 2 to 4 hours.

[0040] In one embodiment, the casting method in step (3) is to remove bubbles from the mixed membrane liquid obtained in step (2), and then evenly pour it onto a flat plate, dry it, and balance it.

[0041] In one embodiment, the air bubbles are removed by vacuum.

[0042] In one embodiment, the amount of the mixed membrane solution is 1 to 3 mL / cm 2 .

[0043] In one embodiment, the plate is a polystyrene culture dish.

[0044] In one embodiment, the drying temperature is 40° C. to 50° C., and the drying time is 2 to 3 hours.

[0045] In one embodiment, the equilibrium condition is a humidity of 50% to 60% and the time is 2 to 3 days.

[0046] The second object of the present invention is to provide a topological cyclodextrin / chitosan composite membrane prepared by the above method.

[0047] The third object of the present invention is to provide an application of the topological cyclodextrin / chitosan composite film described above in the fields of preparing packaging materials, fruit and vegetable preservation, and medical materials.

[0048] The fourth object of the present invention is to provide a packaging material, which is prepared using the topological cyclodextrin / chitosan composite film described above.

[0049] The fifth object of the present invention is to provide a medical composite membrane material, which is prepared using the topological cyclodextrin / chitosan composite membrane described above.

[0050] A sixth object of the present invention is to provide a method for enhancing the mechanical properties of chitosan membranes based on topological cyclodextrin nanoparticles, the method comprising the following steps:

[0051] (1) Dissolving α-cyclodextrin in water by heating, adding polyethylene glycol and stirring, and allowing to stand to form a precipitate, which is then filtered and dried to obtain α-cyclodextrin-polyethylene glycol nanoparticles (TNPs);

[0052] (2) dissolving chitosan, adding glycerol and the α-cyclodextrin-polyethylene glycol nanoparticles prepared in step (1), stirring and dissolving to obtain a mixed membrane solution;

[0053] (3) The mixed membrane solution obtained in step (2) is subjected to a casting method to obtain a topological cyclodextrin / chitosan composite membrane.

[0054] In one embodiment, the heating temperature in step (1) is 40-70°C.

[0055] In one embodiment, the heating temperature in step (1) is 60-70°C.

[0056] In one embodiment, the dissolving of α-cyclodextrin in step (1) refers to dissolving α-cyclodextrin in water to form an α-cyclodextrin aqueous solution; wherein the solid-liquid ratio of α-cyclodextrin to water is 1-5:10-20, g / ml; preferably 1:10, g / ml.

[0057] In one embodiment, the polyethylene glycol (PEG) in step (1) has a molecular weight of 600 to 8000.

[0058] In one embodiment, the molecular weight of the polyethylene glycol PEG in step (1) is 800 to 6000.

[0059] In one embodiment, the polyethylene glycol (PEG) in step (1) has a molecular weight of 1000 to 2000.

[0060] In one embodiment, the polyethylene glycol PEG in step (1) is PEG1000.

[0061] In one embodiment, the mass ratio of the polyethylene glycol to α-cyclodextrin in step (1) is 1-5:2-3.

[0062] In one embodiment, the mass ratio of the polyethylene glycol to α-cyclodextrin in step (1) is 1:1.

[0063] In one embodiment, the stirring time in step (1) is 2 to 6 hours.

[0064] In one embodiment, the stirring time in step (1) is 2 to 4 hours.

[0065] In one embodiment, the filtration in step (1) is performed using a vacuum pump to obtain a precipitate.

[0066] In one embodiment, the drying conditions in step (1) are: a temperature of 40 to 60° C., and drying to a constant weight.

[0067] In one embodiment, the chitosan dissolving in step (2) refers to dissolving chitosan in acetic acid solution to form a chitosan solution; wherein the mass concentration of chitosan in the chitosan solution is 1 wt% to 3 wt%.

[0068] In one embodiment, the acetic acid solution is an acetic acid aqueous solution with a mass concentration of 1 to 5%.

[0069] In one embodiment, the chitosan is dissolved in the acetic acid solution at 40-60° C. and stirred at a stirring speed of 400-800 r / min for 4-8 hours.

[0070] In one embodiment, the chitosan is dissolved in the acetic acid solution at 40° C. and stirred at a stirring speed of 600 r / min for 4 hours.

[0071] In one embodiment, the mass of the glycerol in step (2) is 3% to 5% of the mass of the chitosan solution.

[0072] In one embodiment, the mass of the glycerol in step (2) is 3% of the mass of the chitosan solution.

[0073] In one embodiment, the mass of the α-cyclodextrin-polyethylene glycol nanoparticles TNPs in step (2) is 0.2%-0.8% of the mass of the chitosan solution.

[0074] In one embodiment, the mass of the α-cyclodextrin-polyethylene glycol nanoparticles TNPs in step (2) is 0.6% of the mass of the chitosan solution.

[0075] In one embodiment, the mass ratio of chitosan to α-cyclodextrin-polyethylene glycol nanoparticles in step (2) is 1:0.2-0.8.

[0076] In one embodiment, the mass ratio of chitosan to α-cyclodextrin-polyethylene glycol nanoparticles in step (2) is 1:0.2 to 0.6, preferably 1:0.6.

[0077] In one embodiment, the stirring speed in step (2) is 200 to 600 r / min, and the stirring time is 2 to 4 hours.

[0078] In one embodiment, the casting method in step (3) is to remove bubbles from the mixed membrane liquid obtained in step (2), and then evenly pour it onto a flat plate, dry it, and balance it.

[0079] In one embodiment, the air bubbles are removed by vacuum.

[0080] In one embodiment, the amount of the mixed membrane solution is 1 to 3 mL / cm 2 .

[0081] In one embodiment, the plate is a polystyrene culture dish.

[0082] In one embodiment, the drying temperature is 40° C. to 50° C., and the drying time is 2 to 3 hours.

[0083] In one embodiment, the equilibrium condition is a humidity of 50% to 60% and the time is 2 to 3 days.

[0084] Beneficial effects of the present invention:

[0085] (1) The present invention uses α-cyclodextrin and polyethylene glycol (PEG) as raw materials to prepare cyclodextrin-polyethylene glycol "ring-slip" nanoparticles (TNPs) with a topological structure; TNPs, as a green and degradable nanoparticle, are filled in the chitosan network matrix to enhance the hydrogen bond interaction between the TNPs and the chitosan molecules, thereby improving the mechanical properties of the chitosan membrane; compared with ordinary chitosan membranes, the composite membrane has stronger tensile strength and elongation at break; and compared with the chitosan composite membrane formed with β-cyclodextrin as raw material, the mechanical properties are also significantly improved, such as the fracture strength is increased by more than 160%, and the elongation at break is increased by 21.6%; This shows that α-cyclodextrin and PEG can assemble to form "ring-slip" nanoparticles with a topological structure, which is more conducive to enhancing the mechanical properties of the chitosan composite membrane;

[0086] (2) The polyethylene glycol (PEG) in the present invention acts as a plasticizer, which can enhance the flexibility of the chitosan composite film. In addition, PEG can penetrate the cavity of α-cyclodextrin and form a stable inclusion complex, namely TNPs, with α-cyclodextrin molecules. TNPs and chitosan molecules produce stronger hydrogen bond interactions, thereby improving the mechanical properties of the chitosan composite film. In particular, when the molecular weight of PEG is in the range of 600 to 8000, the improvement in the mechanical properties of the chitosan composite film is more prominent.

[0087] (3) The preparation method of the topological cyclodextrin / chitosan composite membrane of the present invention not only has simple raw materials and is easy to operate, but also can effectively improve the mechanical strength of the chitosan composite membrane, effectively compensating for the problem of poor mechanical strength of the chitosan composite membrane in the prior art, and providing a simple and effective way for actual production. DETAILED DESCRIPTION

[0088] The present invention will be described in detail below with reference to the accompanying drawings and examples, but the embodiments of the present invention are not limited thereto.

[0089] 1. Determination of mechanical properties of chitosan composite membrane

[0090] Mechanical strength tests in this experiment included tensile strength and elongation at break. Chitosan composite film samples were prepared into 20 mm x 60 mm strips and mechanical properties were measured using a texture analyzer. The pre-test speed was 1.0 mm / s, the test speed was 1.0 mm / s, the post-test speed was 1.0 mm / s, and the initial distance was 30 mm. The tensile strength and elongation at break of the film were calculated as follows:

[0091] Tensile Strength:

[0092] Elongation at break:

[0093] Where F is the maximum tensile force of the membrane (N), d is the membrane thickness (mm), h is the membrane width (mm), L is the displacement when the membrane breaks (mm), and L0 is the initial length of the membrane (mm).

[0094] Example 1

[0095] A method for preparing a topological cyclodextrin / chitosan composite membrane, comprising the following steps:

[0096] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 1000), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-1000;

[0097] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0098] (3) 0.3 g of glycerol and 0.2 g of α-TNPs-1000 prepared in step (1) (mass concentration of 0.2%) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at 53% humidity for 2 d. After peeling off the film, a topological cyclodextrin / chitosan composite membrane was obtained.

[0099] Example 2

[0100] A method for preparing a topological cyclodextrin / chitosan composite membrane, comprising the following steps:

[0101] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 1000), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-1000;

[0102] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0103] (3) 0.3 g of glycerol and 0.4 g of α-TNPs-1000 prepared in step (1) (mass concentration of 0.4%) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The dish was flattened to ensure that the solution thickness in the dish was uniform, and the dish was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the dish was taken out and placed in a balancer at 53% humidity for 2 d. After peeling off the film, a topological cyclodextrin / chitosan composite membrane was obtained.

[0104] Example 3

[0105] A method for preparing a topological cyclodextrin / chitosan composite membrane, comprising the following steps:

[0106] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 1000), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-1000;

[0107] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0108] (3) 0.3 g of glycerol and 0.6 g of α-TNPs-1000 prepared in step (1) (mass concentration of 0.6%) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a topological cyclodextrin / chitosan composite membrane was obtained.

[0109] Example 4

[0110] A method for preparing a topological cyclodextrin / chitosan composite membrane, comprising the following steps:

[0111] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 1000), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-1000;

[0112] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0113] (3) 0.3 g of glycerol and 0.8 g of α-TNPs-1000 prepared in step (1) (mass concentration of 0.8%) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a topological cyclodextrin / chitosan composite membrane was obtained.

[0114] Example 5

[0115] A method for preparing a topological cyclodextrin / chitosan composite membrane, comprising the following steps:

[0116] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 600), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-600;

[0117] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0118] (3) 0.3 g of glycerol and 0.6 g of α-TNPs-600 (mass concentration of 0.6%) prepared in step (1) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a topological cyclodextrin / chitosan composite membrane was obtained.

[0119] Example 6

[0120] A method for preparing a topological cyclodextrin / chitosan composite membrane, comprising the following steps:

[0121] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 800), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-800;

[0122] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0123] (3) 0.3 g of glycerol and 0.6 g of α-TNPs-800 (mass concentration of 0.6%) prepared in step (1) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a topological cyclodextrin / chitosan composite membrane was obtained.

[0124] Example 7

[0125] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 2000), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-2000;

[0126] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0127] (3) 0.3 g of glycerol and 0.6 g of α-TNPs-2000 (mass concentration of 0.6%) prepared in step (1) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a chitosan nanocomposite membrane was obtained.

[0128] Example 8

[0129] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 6000), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-6000;

[0130] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0131] (3) 0.3 g of glycerol and 0.6 g of α-TNPs-6000 (mass concentration of 0.6%) prepared in step (1) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a chitosan nanocomposite membrane was obtained.

[0132] Example 9

[0133] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 8000), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-8000;

[0134] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0135] (3) 0.3 g of glycerol and 0.6 g of α-TNPs-8000 (mass concentration of 0.6%) prepared in step (1) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a chitosan nanocomposite membrane was obtained.

[0136] Comparative Example 1

[0137] A method for preparing a chitosan film comprises the following steps:

[0138] Disperse 1 g of chitosan in 100 mL of 1% acetic acid solution, stir at 40°C at a stirring speed of 600 r / min for 4 hours until completely dissolved, add 0.3 g of glycerol, and stir at a stirring speed of 400 r / min for 2 hours to obtain a chitosan membrane solution; degas the chitosan membrane solution in vacuum for 30 minutes, and pour the degassed membrane liquid evenly onto a polystyrene culture dish (10 mm × 10 mm) in a pouring amount of 20 mL; lay the dish flat to ensure that the solution thickness in the dish is uniform, place it in a drying oven at a drying temperature of 40°C and dry it for 24 hours. After drying, take it out and place it in a balancer at 53% humidity for 2 days to balance, and then remove the film to obtain a pure chitosan membrane.

[0139] Comparative Example 2

[0140] (1) Dissolve 10 g of β-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 1000), stir for 2 h, let it stand to precipitate, vacuum filter the precipitate, and then vacuum dry it at 40°C to constant weight to obtain β-TNPs.

[0141] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0142] (3) 0.3 g of glycerol and 0.6 g of β-TNPs (mass concentration of 0.6%) prepared in step (1) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a chitosan nanocomposite membrane was obtained.

[0143] Comparative Example 3

[0144] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 400), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-400;

[0145] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0146] (3) 0.3 g of glycerol and 0.6 g of α-TNPs-400 (mass concentration of 0.6%) prepared in step (1) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a topological cyclodextrin / chitosan composite membrane was obtained.

[0147] Comparative Example 4

[0148] (1) Dissolve 10 g of α-cyclodextrin in 100 mL of water at 65°C, add 10 g of PEG (molecular weight 10,000), stir for 2 h, let stand to precipitate, vacuum filter the precipitate, and then vacuum dry at 40°C to constant weight to obtain α-TNPs-10000.

[0149] (2) Dispersing 1 g of chitosan in 100 mL of 1% acetic acid solution, stirring at 40° C. and 600 rpm for 4 h until completely dissolved, to obtain a chitosan solution;

[0150] (3) 0.3 g of glycerol and 0.6 g of α-TNPs-10000 (mass concentration of 0.6%) prepared in step (1) were added to the chitosan solution prepared in step (2), and stirred at a stirring speed of 400 r / min for 2 h to obtain a chitosan nanoparticle mixed membrane liquid; the mixed membrane liquid was vacuum degassed for 30 min, and the degassed mixed membrane liquid was evenly poured onto a polystyrene culture dish (10 mm×10 mm) with a pouring volume of 20 mL. The culture dish was flattened to ensure that the solution thickness in the culture dish was uniform, and the mixture was placed in a drying oven at a drying temperature of 40°C for 24 h. After drying, the mixture was taken out and placed in a balancer at a humidity of 53% for 2 d. After peeling off the film, a chitosan nanocomposite membrane was obtained.

[0151] Result determination

[0152] 1. The mechanical properties of the topological cyclodextrin / chitosan composite films prepared in Examples 1 to 4 and the pure chitosan composite film prepared in Comparative Example 1 were measured. The results are shown in Table 1:

[0153] Table 1. Mechanical strength of Examples 1 to 4 and Comparative Example 1

[0154] From the results in Table 1, it can be seen that the tensile properties and elongation at break of the topological cyclodextrin / chitosan composite films prepared in Examples 1-4 are significantly higher than those in Comparative Example 1; the pure chitosan film prepared in Comparative Example 1 has insufficient mechanical properties, with a tensile strength of only 7.33 MPa; among them, the tensile strength of the topological cyclodextrin / chitosan composite film prepared in Example 3 is as high as 32.54 MPa, which is 4.4 times higher than that in Comparative Example 1, indicating that the embedding of α-cyclodextrin nanoparticles can effectively improve the mechanical properties of the chitosan membrane, which is due to the hydrogen bond interaction between chitosan and α-cyclodextrin.

[0155] 2. The mechanical properties of the topological cyclodextrin / chitosan composite films prepared in Example 3, Examples 5 to 9, and Comparative Examples 3 and 4 were measured. The results are shown in Table 2:

[0156] Table 2. Mechanical strength of Examples 3, 5 to 9 and Comparative Examples 3 and 4

[0157] The results in Table 2 show that the molecular weight of PEG significantly affects the elongation at break and tensile strength of chitosan films. As the PEG molecular weight increases, the PEG chain lengthens, and the degree of tortuous crosslinking of the molecular chain increases. Furthermore, the chain growth leads to an increase in the number of molecules penetrating into α-cyclodextrin, thereby increasing the degree of crosslinking between molecular chains, enhancing the membrane's flexibility, and improving the membrane's tensile strength and elongation at break. When the PEG molecular weight reaches 1000-2000, the chitosan composite film can achieve an elongation at break of 68.39% and a tensile strength of 32.54. However, when the PEG molecular weight is too high, the tensile strength and elongation at break of the chitosan film also decrease significantly. This may be because the excessive molecular weight destroys the ordered structure of the membrane, leading to a decrease in the mechanical properties of the chitosan film.

[0158] 3. The mechanical properties of the composite films prepared in Example 3 and Comparative Example 2 were measured. The results are shown in Table 3:

[0159] Table 3. Mechanical strength of Example 3 and Comparative Example 2

[0160] Combined with the data in Table 3, it can be seen that the nanoparticles formed by different cyclodextrin types and PEG-1000 have a great influence on the tensile strength of the chitosan film; the tensile strength of the composite film prepared in Example 3 is significantly higher than that of Comparative Example 2, which is 160.74% higher; this indicates that α-cyclodextrin and PEG can assemble to form "ring-slip" nanoparticles with a topological structure, which is more conducive to enhancing the mechanical properties of the chitosan composite film.

Claims

1. A method for preparing a topological cyclodextrin / chitosan composite membrane, characterized in that: The method comprises the following steps: (1) heating and dissolving α-cyclodextrin in water, adding polyethylene glycol and stirring, standing to form a precipitate, filtering and drying to obtain α-cyclodextrin-polyethylene glycol nanoparticles (TNPs); (2) dissolving chitosan, adding glycerol and α-cyclodextrin-polyethylene glycol nanoparticles TNPs prepared in step (1), stirring and dissolving to obtain a mixed membrane solution; (3) The mixed membrane solution obtained in step (2) is used to form a membrane by a casting method to obtain a topological cyclodextrin / chitosan composite membrane.

2. The method according to claim 1, characterized in that The heating temperature in step (1) is 40-70°C.

3. The method according to claim 1, characterized in that The dissolving of α-cyclodextrin in step (1) refers to dissolving α-cyclodextrin in water to form an α-cyclodextrin aqueous solution; wherein the solid-liquid ratio of α-cyclodextrin to water is 1-5:10-20, g / ml.

4. The method according to claim 1, characterized in that The molecular weight of the polyethylene glycol PEG in step (1) is 600 to 8000.

5. The method according to claim 1, characterized in that The molecular weight of the polyethylene glycol PEG in step (1) is 1000-2000.

6. The method according to claim 1, characterized in that The mass ratio of the polyethylene glycol to α-cyclodextrin in step (1) is 1-5:2-3.

7. The method according to claim 1, characterized in that The mass ratio of polyethylene glycol to α-cyclodextrin in step (1) is 1:

1.

8. The method according to claim 1, characterized in that The stirring time in step (1) is 2 to 6 hours.

9. The method according to claim 1, characterized in that: The suction filtration in step (1) is performed using a vacuum pump to obtain a precipitate.

10. The method according to claim 1, characterized in that The drying conditions of step (1) are as follows: the temperature is 40-60° C., and the mixture is dried to a constant weight.

11. The method according to claim 1, characterized in that: The chitosan dissolving in step (2) refers to dissolving chitosan in acetic acid solution to form a chitosan solution; wherein the mass concentration of chitosan in the chitosan solution is 1wt% to 3wt%.

12. The method according to claim 11, characterized in that The acetic acid solution is an acetic acid aqueous solution with a mass concentration of 1 to 5%.

13. The method according to claim 11 or 12, characterized in that: The chitosan is dissolved in the acetic acid solution under the condition of 40-60° C. and stirred at a stirring speed of 400-800 r / min for 4-8 hours.

14. The method according to claim 1, characterized in that The mass of the glycerol in step (2) is 3% to 5% of the mass of the chitosan solution.

15. The method according to claim 1, characterized in that The mass of the α-cyclodextrin-polyethylene glycol nanoparticles TNPs in step (2) is 0.2%-0.8% of the mass of the chitosan solution.

16. The method according to claim 1, characterized in that The mass of the α-cyclodextrin-polyethylene glycol nanoparticles TNPs in step (2) is 0.6% of the mass of the chitosan solution.

17. The method according to claim 1, characterized in that The mass ratio of chitosan to α-cyclodextrin-polyethylene glycol nanoparticles in step (2) is 1:0.2-0.

8.

18. The method according to claim 1, characterized in that The mass ratio of chitosan to α-cyclodextrin-polyethylene glycol nanoparticles in step (2) is 1:0.2-0.

6.

19. The method according to claim 1, characterized in that The casting method in step (3) specifically involves removing bubbles from the mixed film liquid obtained in step (2), then pouring it evenly onto a flat plate, drying it, and balancing it.

20. A topological cyclodextrin / chitosan composite membrane prepared by the method according to any one of claims 1 to 19.

21. Use of the topological cyclodextrin / chitosan composite film according to claim 20 in the fields of preparing packaging materials, fruit and vegetable preservation, and medical materials.

22. A food packaging material, characterized in that: The food packaging material is prepared using the topological cyclodextrin / chitosan composite film described in claim 20.

23. A medical composite membrane material, characterized in that: The medical composite membrane material is prepared by using the topological cyclodextrin / chitosan composite membrane described above.

24. A method for enhancing the mechanical properties of chitosan membranes based on topological cyclodextrin nanoparticles, characterized in that: The method comprises the following steps: 1) heating and dissolving α-cyclodextrin in water, adding polyethylene glycol and stirring, standing to form a precipitate, filtering and drying to obtain α-cyclodextrin-polyethylene glycol nanoparticles TNPs; 2) dissolving chitosan, adding glycerol and α-cyclodextrin-polyethylene glycol nanoparticles TNPs prepared in step 1), stirring and dissolving to obtain a mixed membrane solution; 3) The mixed membrane solution obtained in step 2) is used to form a membrane by a casting method to obtain a topological cyclodextrin / chitosan composite membrane.

25. The method according to claim 24, characterized in that The molecular weight of the polyethylene glycol PEG in step 1) is 600-8000.

26. The method according to claim 24, characterized in that Step 2) The mass ratio of chitosan to α-cyclodextrin-polyethylene glycol nanoparticles is 1:0.2-0.

8.

27. The method according to claim 24, characterized in that Step 2) The mass of the α-cyclodextrin-polyethylene glycol nanoparticles TNPs is 0.2%-0.8% of the mass of the chitosan solution.

Citation Information

Patent Citations

  • Nanoparticles comprising chitosan and cyclodextrin

    CN101217947A

  • Polyethylene glycol modified cyclodextrin, as well as preparation and application thereof

    CN103642190A

  • High-strength super-molecular hydrogel and preparation method thereof

    CN105754316A

  • Citric acid-modified cyclodextrin crosslinking chitosan porous adsorption material, and preparation and application of same

    CN107099049A

  • Topological cyclodextrin / chitosan composite membrane as well as preparation method and application thereof

    CN116515147A