Method for preparing coatings made of two-dimensional material by means of massive parallel mechanical exfoliation and coating obtained
The massive parallel mechanical exfoliation procedure addresses the limitations of existing methods by producing high-lateral-size two-dimensional material flakes with improved coverage and energy efficiency, achieving superior electronic and optical properties and enabling high-performance semiconductor devices.
Patent Information
- Application Number
- PCT/ES2024/070259
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-28
AI Technical Summary
Current methods for producing two-dimensional materials, such as mechanical exfoliation, chemical vapor deposition, and liquid phase exfoliation, face limitations in scalability, size control, energy consumption, and complexity, while failing to achieve high electronic and optical properties consistently.
A procedure involving massive parallel mechanical exfoliation using rollers with adhesive surfaces and controlled pressure and speed to produce high-lateral-size two-dimensional material flakes with improved coverage and energy efficiency, utilizing a first roller with a diameter D and a second roller with a smaller diameter d, applying forces between 1 N and 50 N, and heating the substrate to transfer flakes efficiently.
This method achieves scalable two-dimensional material coatings with flakes of high lateral size and thin thickness, providing coverage greater than 50% with enhanced electronic and optical properties, comparable to or exceeding state-of-the-art materials, and enabling the production of high-performance semiconductor devices like transistors and photodetectors.
Smart Images

Figure ES2024070259_28112024_PF_FP_ABST
Abstract
Description
[0001] DESCRIPTION
[0002] PROCEDURE FOR PREPARING TWO-DIMENSIONAL MATERIAL COATINGS BY MASSIVE PARALLEL MECHANICAL EXFOLIATION AND OBTAINED COATING
[0003] OBJECT OF THE INVENTION
[0004] The present invention falls within the sector of two-dimensional materials with optical and electronic applications.
[0005] A process is presented for providing films of two-dimensional materials by scalable parallel mechanical exfoliation, with low energy consumption, which comprises pressing rollers and rolling them between them at a range of speeds and pressures that gives coatings of scalable two-dimensional materials, with flakes of two-dimensional material of high lateral size compared to the state of the art, of low complexity compared to existing processes and involving a lower amount of energy than other processes present in the state of the art.
[0006] Thin coatings of a two-dimensional material obtained by the aforementioned process have electronic and optical properties comparable to or better than those of other materials in the state of the art.
[0007] STATE OF THE ART
[0008] Van der Waals materials are those that have a microscopic structure with layers of material a few atoms thick, similar to that of graphite, which are held together by van der Waals forces.
[0009] This characteristic is repeated in a series of van der Waals materials present in the form of minerals or of synthetic origin; in powder form or with a crystalline “bulk” material (“single crystal”, polycrystalline); materials such as Graphite (for C,) Molybdenite (for M0S2), BN, M0O3, WSe2, WS2, InSe, black phosphorus are some of those of interest to this invention, but it is not limited to them. The production of three-dimensional materials, characterized by having a ratio between their typical lateral size and their thickness much greater than 1, from van der Waals materials can be done through a series of techniques: a) the mechanical exfoliation of van der Waals materials invented in 2004 or ME (from its acronym in English “Mechanical Exfoliation”) produces a host of flakes each three-dimensional, on a flat substrate from a crystal of two-dimensional material such as graphite. However:
[0010] - The ME technique presents limitations in terms of size control, as well as the thickness of the material resulting from the exfoliation.
[0011] - Furthermore, it has not been possible to present a scalable technique to date; that is, it does not allow for simple increases in the resulting product volume.
[0012] However:
[0013] - The electronic and optical properties of van der Waals materials produced by mechanical exfoliation can be excellent and are frequently used in the investigation of the properties of these materials by integrating them into experimental devices.
[0014] - The complexity of the production process for van der Waals materials by mechanical exfoliation is low, as is the energy required to carry out the process. b) Chemical vapor deposition (CVD) is a well-known process in the semiconductor industry for producing thin films on a flat substrate. Some advantages of CVD are:
[0015] - It is characterized by providing two-dimensional materials with high control over the coverage of the van der Waals material produced, as well as its thickness.
[0016] - CVD technique is a scalable procedure.
[0017] - The electronic and optical properties of coatings produced by CVD are remarkable, although they do not produce devices that achieve performance as high as those produced by ME.
[0018] - The complexity of the CVD production process for two-dimensional materials is high, and it also consumes a relatively high amount of energy. c) Liquid-phase exfoliation (LPE), invented in 2006, is a process that involves the use of ultrasound to exfoliate crystals of van der Waals material in a suitable liquid. The result is a dispersion of three-dimensional materials in said liquid. Some drawbacks of this technique are:
[0019] - The LPE technique lacks precise control over the thickness of the two-dimensional material produced, as well as its size, with the average flake size generally being smaller than the typical size produced by ME.
[0020] - The electronic and optical properties of coatings on two-dimensional materials produced by LPE are low, far from the high performance of those produced by mechanical exfoliation and CVD.
[0021] - The complexity of the production process of coatings of two-dimensional materials by LPE is medium and, in turn, consumes a relatively high amount of energy.
[0022] However, the LPE technique is a scalable technique.
[0023] An in situ exfoliation procedure is shown in A. Pásztor, A. Scarfato, and Ch. Renner: “Mechanical in situ exfoliation of van der Waals materials”, Review of Scientific Instruments 88, 076104 (2017) that involves the use of a wheel-like workpiece (Figure 1 a). This wheel is covered with adhesive tape, but not with the material to be exfoliated. It is implied, however, that this adhesive tape can be coated with material by repeatedly rolling a roller over a thick single crystal in a controlled atmosphere such as ultrahigh vacuum. This is then rolled over a flat substrate such as a silicon oxide wafer (or part of a wafer) to transfer flakes to it, resulting in a coating with less than 25% coverage (Figure 1 b). It is noted that performing the procedure in vacuum can be critical for preparing single-layer flakes of extremely air-sensitive materials.Another relevant technical teaching gathered by Pástzor et al. relates to rolling the roller over the surface of a substrate at a speed of approximately 2 mm / s once or several times. A single roller is used, and no heating step is performed after exfoliation.
[0024] It is therefore of interest to have a method that achieves scalable coatings of two-dimensional materials, with two-dimensional material flakes of high lateral size compared to the state of the art, of low complexity compared to existing methods, involving a lower amount of energy than them, and therefore, more efficient, and that provides thin coatings of a two-dimensional material with electronic and optical properties comparable to or better than those present in the state of the art. DESCRIPTION OF THE INVENTION
[0025] The technical problem is to provide a process that, using van der Waals materials, achieves thin coatings comprising two-dimensional materials, being scalable, with two-dimensional material flakes of high lateral size compared to the state of the art, of low complexity compared to existing processes, involving a lower amount of energy and, therefore, more efficient and that provides thin coatings of a two-dimensional material with electronic and optical properties comparable to or better than those present in the state of the art, and that have a coverage greater than 50%, composed of two-dimensional material flakes.
[0026] For this purpose, a first object of the present invention is a method for preparing coatings of two-dimensional material by massive parallel mechanical exfoliation, in which a first roller of diameter D is provided carrying a flexible, removable, adhesive contact surface in the form of a band comprising a pressure-sensitive acrylic adhesive, a PVC film and a silicone-based coating, the method being characterized in that: a) a second roller of diameter d, smaller than D, is provided, provided with an adhesive contact surface in the form of a band of the same type as that of the first roller. b) a macroscopic-sized quantity of a van der Waals material is dispensed onto the first roller of diameter D. c) the surface of both rollers is brought into contact and a force between them of between 1 N and 50 N is applied.d) the rollers are rotated until the first roller has completed at least 1000 revolutions. e) the strip-shaped contact surface is separated from the second roller. f) the strip-shaped contact surface of the second roller is adhered to a substrate. g) said substrate is heated for a period of more than 5 minutes from a temperature of 95. e C up to a temperature of 110 e C, preferably between 105 °C and 110 °C e C. h) the band-shaped contact surface of the second roller is removed from the substrate. In a preferred embodiment of the invention, steps f), g) and h) are repeated a plurality of times, in particular between 2 and 100 repetitions, preferably between 2 and 10 repetitions, more preferably between 2 and 5 repetitions.
[0027] In successive preferred embodiments of the process of the invention:
[0028] - the roller has a geometry that can be selected between cylindrical and truncated cone.
[0029] - the diameters d and D are prime numbers, preferably the size ratio between the rollers d:D is incommensurable, more preferably D is 53 mm and d is 23 mm. Due to this incommensurability ratio of the diameters d:D, the material is exposed to different regions of the roller perimeter during a greater number of cycles, and different contact areas are presented to exfoliate.
[0030] - the rotation speed of the rollers is at least 500 rpm, more preferably between 1000 and 2000 rpm, and they are rolled over each other for a time interval of between 10 s and 60 s, preferably 20 s.
[0031] - the force applied between the rollers during the process is between 20 and 40 N, preferably applied by placing an elastic element as a connection between the rollers, more preferably a stainless steel sheet between 0.1 and 0.5 mm.
[0032] - The van der Waals material is selected from graphite (C), molybdenite (M0S2), BN, M0O3, WSe2, WS2, InSe and black phosphorus.
[0033] - The substrate material is selected from Mylar, polycarbonate (PC) and silicon wafer (YES / YESO2).
[0034] - The material of the adhesive tape on the rollers is selected from Nitto SPV-224PR and “Scotch tape”.
[0035] In the process described in the present invention, the exfoliation of the van der Waals material is caused by the forces on the bulk material due to the relative movement between the two rollers of different radii at a relatively high speed. Thus, starting from a quantity of bulk material, it is possible to arrive at a coating comprising a plurality of flakes of different thicknesses below the micron, preferably below 200 nm, with a significantly high lateral size, preferably above 200 nm and preferably above the micron.
[0036] In the process, the curvature before and after the effective contact zone is different and greater than in the aforementioned prior art document, where there is a single roller. The stresses that lead to the mechanical delamination of the flake contain larger out-of-plane force components. This could explain why the process of the invention produces films with larger lateral flake sizes than other comparable methods. These forces can aid in the delamination of larger areas of the film, so that we can speak of a homogeneous film, as seen in the figures of the present application.
[0037] Furthermore, the film produced has a higher density of flakes of two-dimensional material, as shown in the figures in the application, and therefore differs significantly from standard manual exfoliation and also from the methodology of Pastzor et al. Furthermore, compared to standard manual exfoliation procedures, it is easily scalable.
[0038] The process crucially uses heat to transfer a large amount of film (greater than 80%) to the substrate resulting in a coating comprising flakes of large lateral size (preferably greater than 200 nm) and thin thickness (preferably less than 200 nm) from van der Waals materials.
[0039] This achieves a high coverage coating (>50%) of a substrate such as polycarbonate or a wafer with silicon oxide (either a natural layer or a growth) of flakes from a van der Waals material as shown in the figures of the application.
[0040] The two-dimensional material flakes are arranged one on top of the other, stacked, on their flat faces. This arrangement is different from that produced by other state-of-the-art techniques such as LPE.
[0041] Advantageously, it is possible to treat materials unstable under ambient conditions such as black phosphorus because it can be implemented in an atmosphere suitable for preserving its properties, such as an anaerobic chamber.
[0042] A second subject of this application is a coating of two-dimensional material obtained by a method such as that described above, which covers the substrate by more than 50% of its surface and comprises flakes of the two-dimensional material with an average thickness of less than 1 pm, preferably less than 200 nm, and a lateral size greater than 200 nm, preferably greater than 1 pm. In a particular embodiment, the flakes are made of different three-dimensional materials, forming heterostructures.
[0043] These coatings have been used to produce semiconductor devices such as transistors and photodetectors with performance superior to those manufactured using state-of-the-art methods such as liquid exfoliation and close to the best performance of standard manual exfoliation.
[0044] Compared to other techniques, the vast majority (> 80%) of the devices manufactured using the process of the invention work and, in addition, these devices allow surprisingly high mobility (> 0.5 cm). 2 / Vs, approximately 1 cm 2 / Vs).
[0045] A third object of the present invention is therefore the use of these two-dimensional material coatings as semiconductor devices, particularly as photodetectors or transistors.
[0046] BRIEF DESCRIPTION OF THE FIGURES
[0047] Figure 1. (a) Sketch of the state-of-the-art process and apparatus (b) coating from van der Waals material on silicon oxide.
[0048] Figure 2. Sketch of an embodiment of the present invention.
[0049] Figure 3. Preferred embodiment of the invention (a) diagram, (b) Before and after a number of intermediate steps of the process, (c) films and (d) microscopic enlargement of the film
[0050] Figure 4. Another preferred embodiment of the invention with the intermediate steps schematized (a) View of two coatings on polycarbonate (PC) and a silicon wafer (Si / SiO2) as well as a micrograph of the coating in each case (b) A motif coated with an embodiment of the invention on silicon (Si / SiO2) (c) Micrographs of the result of repeating a set of intermediate steps once and twice according to an advantageous embodiment of the invention (d)
[0051] Figure 5. Topography of a M0S2 coating on silicon (YES / YESO2) made by AFM (a) and histogram of lateral size ("flake length") and thickness ("flake height") for an advantageous embodiment of the invention. Figure 6. An array of electronic devices as shown in the insert manufactured according to an advantageous embodiment of the invention (a), characteristic traces of a field effect transistor (b) and characteristic current voltage versus V gate curve of a device of the array shown in (c).
[0052] Figure 7. Coatings obtained according to embodiments of the invention with BN.
[0053] Figure 8. Coatings obtained according to embodiments of the invention with M0S2.
[0054] Figure 9. AFM images of coatings obtained according to embodiments of the invention with M0S2.
[0055] Figure 10. Characterization of field effect transistors obtained for devices manufactured with coatings according to the present invention (IV).
[0056] Figure 11. Characterization of field effect transistors obtained for devices manufactured with coatings according to the present invention (Ids-Vgate).
[0057] Figure 12. Coatings obtained according to embodiments of the invention with C, M0S2, BN, M0O3, WSe2, WS2.
[0058] Figure 13. Comparison of the various state-of-the-art techniques with the present invention for lateral size (flake length) and thickness.
[0059] Figure 14. Characterization of photodetectors obtained for devices manufactured with coatings according to the present invention.
[0060] MODE OF EMBODIMENT OF THE INVENTION
[0061] In a preferred embodiment of the invention, two adhesive strips are arranged on the circumference of two cylindrical rollers whose diameters are not commensurable numbers (preferably, they are prime numbers). More preferably, a first cylinder with a diameter of 53 mm and a second cylinder with a diameter of 23 mm are provided. This allows 1219 rotations to be made until contact is repeated between the same contact surfaces between the cylinders. The cylinders are made of polyoxymethylene (POM), which is a common choice for greater ease of machining and finishing.
[0062] The adhesive tape comprises a pressure-sensitive acrylic adhesive, a PVC film, and a silicone-based coating and is the standard tape for peeling individual flakes. In this preferred embodiment, it is Nitto SPV-224PR tape, which is adhered to the cylinders using a standard double-sided gel adhesive.
[0063] A quantity of van der Waals material is dispensed onto the adhesive strip of one of them, the one with the largest radius, covering an area of 12 mm x 10 mm of the adhesive tape. The cylinders are brought into contact and a force of 30 N is applied to them thanks to an elastic element, such as a 0.1- to 0.5-mm-thick stainless steel sheet, which provides the necessary flexibility.
[0064] Preferably, one cylinder is rolled over another for between 10 seconds and one minute, and more preferably, 20 seconds. The speed is preferably greater than 500 rpm and more preferably between 1000 rpm and 2000 rpm for molybdenite, and similarly for the rest of van der Waals materials such as Graphite (C), Molybdenite (for M0S2), BN, M0O3, WSe2, WS2, InSe, or black phosphorus. The criterion is that a visual inspection shows a uniform coating, without apparent gaps as shown in Figure 3 (c) for M0S2, where the rotation speed has been 1000 rpm.
[0065] Next:
[0066] - the adhesive strip is removed from the cylinder other than the one used to deposit the two-dimensional material and is glued onto the substrate (Si / SiO2 in one embodiment or Polycarbonate in another embodiment).
[0067] Heat for 5 minutes at 110°C on a “hot plate” under ambient conditions.
[0068] The adhesive strip is removed and the film is transferred to the substrate.
[0069] It is preferable to press the adhesive strip with a soft medium such as a cotton swab to avoid bubbles.
[0070] These steps are repeated (between 2 and 100 times) with another area or another adhesive tape with a film until the desired coverage is achieved through inspection with an optical microscope. A variety of flakes of varying thicknesses can be seen, ranging from atomic thicknesses to tens of nanometers.
[0071] It is possible to manufacture semiconductor devices with these coated substrates using the procedure described above.
[0072] Surprisingly, devices such as photodetectors and field effect transistors exhibit high figures of merit compared to the described state of the art.
[0073] Table 1
[0074] The table above shows 10 devices from two different batches and their mobility. This table shows the ca nai is the semiconductor channel length in the device, and n is the estimated mobility for the device as manufactured and after annealing. The silicon oxide layer is 440 nm.
[0075] The massively parallel mechanical exfoliation of M0S2 is shown in Figure 3. (a) Schematic of the massively parallel mechanical exfoliation setup. Polyoxymethylene (POM) cylinders with incommensurate diameters (53:23) are covered with double-sided adhesive tape. Nitto SPV 224 tape is fixed to the double-sided tape with the adhesive facing outwards. The two cylinders are then pressed against each other. (b) Image of the assembled setup with an exfoliated macroscopic M0S2 crystal on the surface of one of the tapes before (top) and after (bottom) rolling the cylinders for 20 s. (c) Optical image of the resulting tape after the massively parallel mechanical exfoliation process. (1) to (4) are transmission mode micrographs acquired approximately at the positions highlighted in c) with dashed squares.
[0076] Figure 3 shows the relative simplicity of the process and the high homogeneity of the film produced for coating. As can be seen in Figure 3(c), the film is homogeneous to the naked eye. The micrographs in Figure 3(c) (1 ) to (4) comprise a plurality of flakes of two-dimensional material.
[0077] Figure 4 shows the thermal transfer of a film obtained by massive mechanical exfoliation parallel to a substrate, (a) Scheme of the steps necessary to transfer the exfoliated flakes from the surface of the Nitto SPV 224 tape to the substrate, (a.1) Nitto tape containing massively and mechanically exfoliated flakes in parallel. (a.2) A vinyl mask (designed with a tabletop vinyl cutter) with the desired pattern is adhered to the surface of the tape, leaving some openings where the film is visible, (a.3) In a more preferred embodiment, the tape and the vinyl are adhered to the substrate (e.g., a SIO2 / SIO substrate). Only the flakes of the film in the opening of the vinyl mask will be in contact with the substrate surface, (a.4) The adhesive tape / vinyl mask / acceptor substrate are placed on a hot plate at 110 °C for 5 min.(b, top) Images of two different substrates, polycarbonate and SI2O2 / SI2, after thermal transfer from a 5 x 5 mm film. 2 of few-layered M0S2, (b, bottom) Optical micrographs acquired on the central part of the polycarbonate (transmission mode) and the S02 / S02 (reflection mode), (c) Example of a film of two-dimensional M0S2 material transferred through a vinyl mask to form the lettering 'MoS2' on a S02 / S02 substrate. (d) Transmission mode optical microscopy image illustrating that successive transfers can be performed to create films with higher coverage. In this example, one film of M0S2 was transferred first and then a film of M0S2 was transferred a second time on the right side of the image. Note the sharp interface between the single- and double-transferred regions.
[0078] In Figure 4 it is possible to appreciate that the coating coverage of the same material on two substrates, polycarbonate (PC) and SIO2 / SIO, which is homogeneous and is formed by flakes that cover > 50% of the area. Figure d shows how performing the thermal transfer a plurality of times (2) increases the coating coverage significantly. Figure 5 shows the statistical analysis of the thickness and lateral size of the M0S2 flakes produced by massive parallel mechanical exfoliation, (a) Representative AFM topographic images acquired at two different locations of the M0S2 flake film in Figure 5c. (b) Correlation between flake thickness and flake lateral size dimension obtained from 189 flakes, analyzed from represented AFM images, acquired at 2 different locations of the sample. In the upper right part, the 1 D histogram corresponding to the height and lateral size distributions is shown.
[0079] Figure 5 shows the quality of the coating in terms of lateral size (“flake length”) versus thickness (“flake height”), with typical lateral size values in the range of micrometer units and a typical thickness and height in the range of tens of nanometers.
[0080] Field-effect transistors fabricated from massively parallel mechanically exfoliated MOS2 are shown in Figure 6. (a) Image of 20 field-effect transistors fabricated from a large-area film of few-layer MOS2 flakes obtained by massively parallel mechanical exfoliation. (Inset) Magnified image of one of the devices with evaporated T¡(5 nm) / Au(50 nm) electrodes separated by 10 pm. (b) Drain-source current at a fixed bias voltage (Vds = 1 V) while sweeping the gate voltage (Vgate). Both the as-fabricated and post-vacuum annealed data sets are presented in panel b.
[0081] (c) Drain-source current versus bias voltage characteristics acquired for different gate voltage values (data set for after vacuum annealing).
[0082] Figure 6 shows the scalability of the present process, as well as the fabrication of devices such as field-effect transistors from it. For these, a SiO2 / Si substrate is provided with an oxide layer of preferably 200-400 nm, and more preferably 290 nm. Metallic electrodes are preferably defined on the substrate, more preferably made from Au (45 nm thick) on Ti (5 nm thick), but without neglecting other common metallic materials (such as Pt, Ag, Al) depending on whether the work function of the electrode is modulated. Figure 7 shows transfer micrographs of the coating using BN (1 to 5 thermal transfers). It can be seen that the coverage of the coating on the substrate is greater than 50% and is improved with a plurality of thermal transfers.
[0083] Figure 8: Transmission mode optical images taken from the edges of regions consisting of different transfer numbers. The contrast difference indicates that denser coverage on a substrate can be achieved by increasing the number of Nitto transfers to the substrate. It can be seen that the coating coverage on the substrate is greater than 50% and is improved with a plurality of thermal transfers.
[0084] For Figure 9, AFM topography images were taken from 4 different locations to approximate the percentage coverage on a substrate after transfer of exfoliated MoS2 flakes onto a S¡O2 / S¡ substrate (1 transfer). Figure 9 further demonstrates the quality of the coating in terms of lateral size (“flake length”) versus thickness (“flake height”), with typical lateral size values in the micrometer range and typical thickness in the tens of nanometer range. Coverages provided by exemplary embodiments of this coating, greater than 50%, are shown.
[0085] Figure 10 (a) Measured current-voltage (IV) curves for 20 devices (left) and corresponding linear fitted curves determined considering the voltage range (-0.15 to +0.15 V) marked by the dotted rectangle, (b) The histogram plot represents the resistance distribution of the fabricated devices, (c) The 2D heat map demonstrates the variation of resistance values depending on the location of the devices on the substrate. The corresponding devices are as depicted in Fig. 4a.
[0086] Figure 11 shows the current through the source-drain electrodes as a function of gate voltage for the devices as manufactured and after overnight annealing at 150 °C. Each batch differs with respect to the channel length between the source-drain contacts, such that the channel lengths vary in one batch, while in the other they are identical (10 pm). From these measurements it is possible to estimate the surprisingly high mobility of the devices manufactured in this embodiment p = [dld S / dV g ate]x[L / (WC-Vds)], where W is the width of the semiconductor channel, L is the length of the semiconductor channel and C is the capacity of the silicon oxide for a 440 nm layer between the semiconductor channel and the gate electrode per unit area).
[0087] Coatings according to the embodiment of the present invention for various van der Waals materials are shown in Figure 12. It can be seen that the coating coverage on the substrate is greater than 50% based on a plurality of van der Waals materials.
[0088] Figure 13 shows a comparison of the techniques in the state of the art versus the results of the present invention in terms of lateral size and thickness of the two-dimensional material flakes comprising the claimed coating.
[0089] Figure 13 shows that the aspect ratio is much higher for this procedure than for other prior art methods at different flake thicknesses. Panel b also shows that this technique results in a larger lateral length of the flakes included in the coating compared to other techniques over a wide range of thicknesses.
[0090] The optoelectronic properties of the M0S2 photodetector fabricated from polycarbonate are shown in Figure 14. (a) Optical image focused on the channel region between the source-drain contacts connected by multiple M0S2 flakes. (b) Photocurrent and photoresponse values as a function of illumination power for A = 625 nm and Vsd = 1 V. (c) Time-resolved photocurrent cycles measured for different bias voltages with A = 625 nm and P = 3.34 mW, and corresponding photocurrent values. High square wave values correspond to device illumination. (d) Photoswitching behavior of the device with time-varying wavelength (400 to 900 nm). (e) Calculated photocurrent and photoresponse values as a function of wavelength. The illumination powers for each wavelength are represented in the upper left panel.In time-resolved photocurrent measurements, the dark and bright states are switched every 5 s.
[0091] Figure 14 shows the surprisingly high levels of photoresponse (photoresponsiveness) close to 100 A / W at low power (Power), as well as the variation in the photocurrent itself. The device's behavior under photoswitching is exemplified by the photocurrent, which exhibits behavior close to a square wave in this case, demonstrating the device's rapid response.
[0092] The photocurrent obtained at different wavelengths and the power supplied allow the calculation of the photoresponse at various wavelengths for a device implementation.
Claims
CLAIMS 1.- Method for preparing coatings of two-dimensional material by massive parallel mechanical exfoliation in which a first roller of diameter D is provided that carries a flexible and removable adhesive contact surface in the form of a band comprising a pressure-sensitive acrylic adhesive, a PVC film and a silicone-based coating, the method being characterized in that it comprises the following steps: a) a second roller of diameter d, smaller than D, is provided, provided with an adhesive contact surface in the form of a band of the same type as that of the first roller. b) a macroscopic-sized quantity of a van der Waals material is dispensed onto the first roller of diameter D. c) the surface of both rollers is brought into contact and a force is applied between them of between 1 N and 50 N. d) the rollers are rotated until the first roller has completed at least 1000 revolutions.e) the strip-shaped contact surface is separated from the second roller. f) the strip-shaped contact surface of the second roller is adhered to a substrate. g) said substrate is heated for a period of more than 5 minutes from a temperature of 95. e C up to a temperature of 110 e C. h) the band-shaped contact surface of the second roller is removed from the substrate. 2.- Method according to claim 1, wherein steps f), g) and h) are repeated a plurality of times, particularly between 2 and 100 repetitions. 3.- Method according to one of claims 1 or 2, wherein the rollers have a cylindrical geometry. 4.- Method according to any one of claims 1 to 3, wherein the diameters dy D of the cylindrical rollers are prime numbers. 5.- Method according to claim 4, wherein the size ratio between the rollers d:D is incommensurable. 6.- Method according to claim 5, where D is 53 mm and d is 23 mm. 7.- Method according to any one of claims 1 to 6, wherein the rotation speed of the rollers is at least 500 rpm and they are rolled over each other for a time interval between 10 s and 60 s. 8.- Method according to claim 7, wherein the rotation speed of the rollers is between 1000 and 2000 rpm and they are rotated one over the other for 20 s. 9.- Method according to any one of claims 1 to 8, wherein the force applied between the rollers during the method is between 20 and 40 N, 10.- Method according to claim 9, wherein the force is applied by placing an elastic element such as a stainless steel sheet between 0.1 and 0.5 mm as a connection between rollers. 11.- Method according to any one of claims 1 to 10, wherein the van der Waals material is selected from graphite (C), molybdenite (M0S2), BN, M0O3, WSe2, WS2, InSe and black phosphorus. 12.- Method according to any one of claims 1 to 11, wherein the substrate material is selected from Mylar, polycarbonate (PC) and silicon wafer (SÍ / SÍO2). 13.- Method according to any one of claims 1 to 12, wherein the material of the rollers is polyoxymethylene (POM) or polyoxymethylene (PEEK). 14.- Method according to any one of claims 1 to 13, wherein the material of the adhesive band on the rollers is selected from Nitto SPV-224PR and “Scotch tape”. 15.- Method according to any one of claims 1 to 14, wherein the substrate is heated to a temperature between 105 °C and 1 10 e C. 16.- Coating of two-dimensional material obtained by a process as defined in claims 1 to 15, which has a coverage of the substrate greater than 50% of its surface and which comprises flakes of the two-dimensional material with an average thickness of less than 1 pm and a lateral size greater than 200 nm. 17.- Coating according to claim 16, wherein the average thickness is less than 200 nm and the lateral size is greater than 1 pm. 18.- Coating according to claims 16 or 17, wherein the flakes are made of different two-dimensional materials, forming heterostructures. 19.- Use of a coating as defined in claims 16 to 18 as semiconductor devices, particularly as photodetectors or transistors.
Citation Information
Patent Citations
Roll-to-roll mechanized exfoliator and automatic 2d materials transfer and layering system
WO2023023260A2