Semiconductor device and method for manufacturing semiconductor device

The semiconductor device design with a specific transistor configuration and layer structure addresses the challenges of high-speed operation and integration, achieving efficient data storage and low power consumption while maintaining cost-effectiveness.

WO2024241188A1PCT designated stage expired Publication Date: 2024-11-28SEMICON ENERGY LAB CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2024/054866
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-20
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current semiconductor devices face challenges in achieving high-speed operation, low power consumption, miniaturization, high integration, and reliable electrical characteristics while maintaining low costs and efficient manufacturing processes.

Method used

A semiconductor device design featuring a first and second transistor configuration with specific insulating and conductive layers, including recesses and openings to enhance electrical characteristics and reduce parasitic capacitance, allowing for improved on-state currents and efficient data storage without the need for additional capacitors.

Benefits of technology

The design enables high-speed operation, low power consumption, and high integration while reducing manufacturing complexity and costs, achieving enhanced electrical characteristics and increased storage capacity per unit area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2024054866_28112024_PF_FP_ABST
    Figure IB2024054866_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor device that operates at high speed. This semiconductor device includes a first transistor and a second transistor on the first transistor. The first transistor has first to third conductive layers. The second transistor has third to fifth conductive layers. An insulating layer is provided between the first conductive layer and the second conductive layer and between the third conductive layer and the fourth conductive layer. Each insulating layer has an opening which reaches the first conductive layer, or an opening which reaches the third conductive layer. The first and third conductive layers have a recess which reaches said opening. A semiconductor layer is provided so as to contact said recess. The third conductive layer has a region which faces the semiconductor layer, with the gate insulating layer of the first transistor sandwiched therebetween, inside the opening which reaches the first conductive layer. The fifth conductive layer has a region which faces the semiconductor layer, with the gate insulating layer of the second transistor interposed therebetween, inside the opening which reaches the third conductive layer.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor device and method for manufacturing the same

[0001] 1. Field of the Invention One embodiment of the present invention relates to a semiconductor device, a memory device, and an electronic device. Another embodiment of the present invention relates to a manufacturing method of a semiconductor device.

[0002] One embodiment of the present invention is not limited to the above technical field, and examples of the technical field of one embodiment of the present invention include semiconductor devices, display devices, light-emitting devices, power storage devices, memory devices, electronic devices, lighting devices, input devices (e.g., touch sensors), input / output devices (e.g., touch panels), driving methods thereof, and manufacturing methods thereof.

[0003] In this specification and the like, a semiconductor device is a device that utilizes semiconductor characteristics, and refers to a circuit including a semiconductor element (transistor, diode, photodiode, etc.), a device having such a circuit, etc. Also, it refers to any device that can function by utilizing semiconductor characteristics. For example, an integrated circuit, a chip including an integrated circuit, and an electronic component in which a chip is housed in a package are examples of semiconductor devices. Furthermore, a memory device, a display device, a light-emitting device, a lighting device, and an electronic device may themselves be semiconductor devices and each may have a semiconductor device.

[0004] In recent years, the development of semiconductor devices has progressed, and semiconductor devices mainly use LSIs (Large Scale Integration), CPUs (Central Processing Units), memories, etc. A CPU is an assembly of semiconductor elements that have semiconductor integrated circuits (at least transistors and memories) formed into chips by processing a semiconductor wafer and on which electrodes serving as connection terminals are formed.

[0005] 2. Description of the Related Art Semiconductor circuits (IC chips) such as LSIs, CPUs, and memories are mounted on circuit boards, such as printed wiring boards, and are used as components of various electronic devices.

[0006] Furthermore, a technology for constructing a transistor using a semiconductor thin film formed on a substrate having an insulating surface has attracted attention. Such transistors are widely applied to electronic devices such as integrated circuits (ICs) and display devices. While silicon-based semiconductor materials are widely known as semiconductor thin films applicable to transistors, oxide semiconductors have also attracted attention as other materials.

[0007] Furthermore, it is known that a transistor using an oxide semiconductor has an extremely small leakage current in an off state. For example, Patent Document 1 discloses a CPU with low power consumption that utilizes the property of a transistor using an oxide semiconductor that has a small leakage current. Furthermore, Patent Document 2 discloses a memory device that can retain stored data for a long period of time by utilizing the property of a transistor using an oxide semiconductor that has a small leakage current.

[0008] In addition, with the recent trend toward smaller and lighter electronic devices, there is an increasing demand for higher density integrated circuits. There is also a demand for improved productivity of semiconductor devices including integrated circuits. For example, Patent Document 3 and Non-Patent Document 1 disclose a technique for increasing the density of integrated circuits by stacking a first transistor using an oxide semiconductor film and a second transistor using an oxide semiconductor film to provide multiple memory cells in an overlapping manner. Patent Document 4 discloses a technique for increasing the density of integrated circuits by vertically arranging the channel of a transistor using an oxide semiconductor film.

[0009] JP 2012-257187 A JP 2011-151383 A WO 2021 / 053473 JP 2013-211537 A

[0010] M. Oota et. al, “3D-Stacked CAAC-In-Ga-Zn Oxide FETs with Gate Length of 72nm”, IEDM Tech. Dig. , 2019, pp. 50-53

[0011] An object of one embodiment of the present invention is to provide a semiconductor device with high operating speed. Another object of one embodiment of the present invention is to provide a low-cost semiconductor device. Another object of one embodiment of the present invention is to provide a semiconductor device that can be miniaturized or highly integrated. Another object of one embodiment of the present invention is to provide a semiconductor device including a transistor with favorable electrical characteristics. Another object of one embodiment of the present invention is to provide a semiconductor device including a transistor with high on-state current. Another object of one embodiment of the present invention is to provide a highly reliable semiconductor device. Another object of one embodiment of the present invention is to provide a semiconductor device with low power consumption. Another object of one embodiment of the present invention is to provide a novel semiconductor device. Another object of one embodiment of the present invention is to provide a method for manufacturing the semiconductor device.

[0012] Note that the description of these problems does not preclude the existence of other problems. One embodiment of the present invention does not necessarily have to solve all of these problems. Problems other than these can be extracted from the description in the specification, drawings, and claims.

[0013] One aspect of the present invention provides a transistor including a first transistor, a second transistor, a first insulating layer, a second insulating layer, and a third insulating layer, wherein the first transistor includes a first semiconductor layer, a first conductive layer, a second conductive layer, a third conductive layer, and a fourth insulating layer, and the second transistor includes a second semiconductor layer, a third conductive layer, a fourth conductive layer, a fifth conductive layer, and a fifth insulating layer, wherein the first insulating layer is located on the first conductive layer, and the second conductive layer is located on the first insulating layer. the first conductive layer has a first recess, the first insulating layer and the second conductive layer have a first opening at a position overlapping the first recess, the first semiconductor layer contacts an upper surface of the second conductive layer and the first recess, and contacts a side surface of the second conductive layer and a side surface of the first insulating layer within the first opening, the fourth insulating layer has a region located on the second conductive layer and a region located on the first semiconductor layer within the first opening, and the third conductive layer has a first The opening has a region facing the first semiconductor layer with the fourth insulating layer sandwiched therebetween, the third conductive layer has a region overlapping with the second conductive layer via the fourth insulating layer, the third conductive layer has a second recess, the second insulating layer is located on the third conductive layer, the fourth conductive layer is located on the second insulating layer, the second insulating layer and the fourth conductive layer have a second opening at a position overlapping with the second recess, the second semiconductor layer is in contact with an upper surface of the fourth conductive layer and the second recess, and the fifth insulating layer is in contact with a side surface of the fourth conductive layer and a side surface of the second insulating layer inside the second opening, the fifth insulating layer is located on the second semiconductor layer inside the second opening, the third insulating layer has a region that overlaps with the fourth conductive layer via the second semiconductor layer and has a third opening at a position that overlaps with the second opening, and the fifth conductive layer has a region that faces the second semiconductor layer with the fifth insulating layer sandwiched between them inside the second opening, and a region that is located inside the third opening.

[0014] Alternatively, in the above aspect, the second opening may at least partially overlap the first opening.

[0015] Alternatively, in the above aspect, there may be a sixth insulating layer, on which the first insulating layer and the first conductive layer are located, and the shortest distance from the top surface of the sixth insulating layer to the top surface of the first conductive layer that contacts the first insulating layer is longer than the shortest distance from the top surface of the sixth insulating layer to the bottom surface in a region overlapping with the first recess of the fourth insulating layer, and the shortest distance from the top surface of the sixth insulating layer to the top surface of the third conductive layer that contacts the second insulating layer and overlaps with the second conductive layer may be longer than the shortest distance from the top surface of the sixth insulating layer to the bottom surface in a region overlapping with the second recess of the fifth insulating layer.

[0016] Alternatively, in the above aspect, there may be a sixth insulating layer, on which the first insulating layer and the first conductive layer are located, and the shortest distance from the top surface of the sixth insulating layer to the top surface of the first conductive layer that contacts the first insulating layer is equal to or greater than the shortest distance from the top surface of the sixth insulating layer to the bottom surface of the third conductive layer in a region that overlaps with the first recess, and the shortest distance from the top surface of the sixth insulating layer to the top surface of the third conductive layer that contacts the second insulating layer and overlaps with the second conductive layer may be equal to or greater than the shortest distance from the top surface of the sixth insulating layer to the bottom surface of the fifth conductive layer in a region that overlaps with the second recess.

[0017] Alternatively, in the above aspect, the first conductive layer may have a sixth conductive layer and a seventh conductive layer on the sixth conductive layer, the third conductive layer may have an eighth conductive layer and a ninth conductive layer on the eighth conductive layer, the seventh conductive layer may have a first recess, and the ninth conductive layer may have a second recess.

[0018] Alternatively, in the above aspect, a sixth conductive layer may be provided, and the sixth conductive layer may be provided so as to be in contact with the upper surface of the fifth conductive layer.

[0019] Alternatively, in the above aspect, the film thickness of the third insulating layer in the region overlapping with the fourth conductive layer and the second semiconductor layer may be thicker than the film thickness of the fourth insulating layer.

[0020] Alternatively, in the above aspect, at least a portion of the fifth insulating layer may be located inside the third opening.

[0021] Alternatively, in the above aspect, the first transistor may have a sixth conductive layer, the second transistor may have a seventh conductive layer, the first insulating layer may have a first layer and a second layer on the first layer, the second insulating layer may have a third layer and a fourth layer on the third layer, the sixth conductive layer may be located on the first layer, the seventh conductive layer may be located on the third layer, the second layer may cover an upper surface and a side surface of the sixth conductive layer, and the fourth layer may cover an upper surface and a side surface of the seventh conductive layer, in a cross-sectional view, the first semiconductor layer may have a region that faces the sixth conductive layer across the second layer and that faces the third conductive layer across the fourth insulating layer, and in a cross-sectional view, the second semiconductor layer may have a region that faces the seventh conductive layer across the fourth layer and that faces the fifth conductive layer across the fifth insulating layer.

[0022] Alternatively, in the above aspect, the first semiconductor layer and the second semiconductor layer each include an oxide semiconductor, and the oxide semiconductor includes one or more elements selected from indium, an element M, and zinc, and the element M may be one or more elements selected from aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony.

[0023] Alternatively, in the above aspect, the first insulating layer may have a first region in contact with the first semiconductor layer, the second insulating layer may have a second region in contact with the second semiconductor layer, and the first region and the second region may each contain a halogen element.

[0024] Alternatively, in the above embodiment, the halogen element may be one or more elements selected from chlorine, fluorine, bromine, and iodine.

[0025] Alternatively, in the above aspect, the first semiconductor layer may have a first region in contact with the bottom surface of the first recess and a second region in contact with the top surface of the second conductive layer, and the second semiconductor layer may have a third region in contact with the bottom surface of the second recess and a fourth region in contact with the top surface of the fourth conductive layer, and each of the first to fourth regions may contain boron or phosphorus.

[0026] One embodiment of the present invention provides a method for forming a first conductive layer, forming a first insulating layer on the first conductive layer, forming a second conductive layer on the first insulating layer, forming a first opening in the second conductive layer and the first insulating layer at a position overlapping with the first conductive layer, and forming a first recess in the first conductive layer to overlap with the first opening, forming a first semiconductor layer in contact with an upper surface of the second conductive layer and the first recess, and in contact with a side surface of the second conductive layer and a side surface of the first insulating layer inside the first opening, and and processing the second conductive layer to expose a portion of the upper surface of the first insulating layer; forming a second insulating layer so as to have a region located on the second conductive layer and a region located on the first semiconductor layer inside the first opening; forming a third conductive layer so as to have a region facing the first semiconductor layer with the second insulating layer sandwiched between them inside the first opening and having a region overlapping with the second conductive layer via the second insulating layer; forming a third insulating layer on the third conductive layer; and forming a fourth conductive layer on the third insulating layer. a second opening is formed in the fourth conductive layer and the third insulating layer at a position overlapping the third conductive layer, and a second recess is formed in the third conductive layer so as to overlap the second opening; a second semiconductor layer is formed in contact with an upper surface of the fourth conductive layer and the second recess, and in contact with a side surface of the fourth conductive layer and a side surface of the third insulating layer within the second opening; and the second semiconductor layer and the fourth conductive layer are processed to expose a portion of the upper surface of the third insulating layer, at least a portion of which is located within the second opening. a fourth insulating layer to cover the fourth conductive layer, the second semiconductor layer, and the sacrificial layer; planarizing the fourth insulating layer and the sacrificial layer to planarize an upper surface of the sacrificial layer; removing the sacrificial layer; forming a fifth insulating layer to cover the second opening; forming a fifth conductive layer on the fifth insulating layer; and planarizing the fifth conductive layer to remove a region of the fifth conductive layer and the fifth insulating layer that overlaps with an upper surface of the fourth insulating layer.

[0027] Alternatively, in the above aspect, the second opening may be formed at a position where at least a portion of the second opening overlaps with the first opening.

[0028] Alternatively, in the above embodiment, the sixth conductive layer may be formed so as to be in contact with the upper surface of the fifth conductive layer.

[0029] Alternatively, in the above aspect, the fourth insulating layer may be formed to have a thickness greater than that of the second insulating layer.

[0030] According to one embodiment of the present invention, a semiconductor device with high operating speed can be provided. According to another embodiment of the present invention, a low-cost semiconductor device can be provided. According to another embodiment of the present invention, a semiconductor device that can be miniaturized or highly integrated can be provided. According to another embodiment of the present invention, a semiconductor device including a transistor with favorable electrical characteristics can be provided. According to another embodiment of the present invention, a semiconductor device including a transistor with high on-state current can be provided. According to another embodiment of the present invention, a highly reliable semiconductor device can be provided. According to another embodiment of the present invention, a semiconductor device with low power consumption can be provided. According to another embodiment of the present invention, a novel semiconductor device can be provided. According to another embodiment of the present invention, a method for manufacturing the semiconductor device can be provided.

[0031] Note that the description of these effects does not preclude the existence of other effects. One embodiment of the present invention does not necessarily have all of these effects. Effects other than these can be extracted from the description in the specification, drawings, and claims.

[0032] FIGS. 1A to 1C are circuit diagrams showing an example of a memory cell. FIGS. 1D and 1E are plan views showing an example of a semiconductor device. FIGS. 1F and 1G are cross-sectional views showing an example of a semiconductor device. FIG. 2A is a cross-sectional view showing an example of a semiconductor device. FIG. 2B is a plan view showing an example of a semiconductor device. FIGS. 3A to 3D are diagrams explaining the concept of heat treatment. FIGS. 4A and 4B are cross-sectional views showing an example of a semiconductor device. FIGS. 5A and 5B are plan views showing an example of a semiconductor device. FIGS. 5C and 5D are cross-sectional views showing an example of a semiconductor device. FIGS. 6A and 6B are cross-sectional views showing an example of a semiconductor device. FIGS. 7A and 7B are cross-sectional views showing an example of a semiconductor device. FIGS. 8A and 8B are cross-sectional views showing an example of a semiconductor device. FIGS. 9A and 9B are cross-sectional views showing an example of a semiconductor device. FIGS. 10A and 10B are cross-sectional views showing an example of a semiconductor device. FIGS. 11A and 11B are plan views showing an example of a semiconductor device. FIGS. 11C and 11D are cross-sectional views showing an example of a semiconductor device. 12A to 12F are cross-sectional views illustrating an example of a manufacturing method of a semiconductor device. FIGS. 13A to 13D are cross-sectional views illustrating an example of a manufacturing method of a semiconductor device. FIGS. 14A to 14D are cross-sectional views illustrating an example of a manufacturing method of a semiconductor device. FIGS. 15A to 15E are cross-sectional views illustrating an example of a manufacturing method of a semiconductor device. FIG. 16A is a plan view illustrating an example of a memory device. FIG. 16B is a cross-sectional view illustrating an example of a memory device. FIG. 17 is a cross-sectional view illustrating an example of a memory device. FIG. 18 is a cross-sectional view illustrating an example of a memory device. FIG. 19 is a block diagram illustrating a structural example of a semiconductor device. FIGS. 20A and 20B are perspective views illustrating an example of a semiconductor device. FIG. 21 is a block diagram illustrating a CPU. FIGS. 22A and 22B are perspective views illustrating an example of a semiconductor device. FIGS. 23A and 23B are perspective views illustrating an example of a semiconductor device. FIGS. 24A and 24B are views illustrating various memory devices by layer. FIGS. 25A and 25B are views illustrating an example of an electronic component. 26A to 26C are diagrams showing an example of a mainframe computer, and Fig. 26D is a diagram showing an example of space equipment.FIG. 26E is a diagram illustrating an example of a storage system applicable to a data center.

[0033] The embodiments will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various changes can be made in form and detail without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.

[0034] In the configuration of the invention described below, the same parts or parts having similar functions are denoted by the same reference numerals in different drawings, and repeated explanations thereof will be omitted. Furthermore, when referring to similar functions, the same hatching pattern may be used and no particular reference numeral may be assigned.

[0035] Furthermore, for ease of understanding, the position, size, range, etc. of each component shown in the drawings may not represent the actual position, size, range, etc. Therefore, the disclosed invention is not necessarily limited to the position, size, range, etc. disclosed in the drawings.

[0036] In this specification, the ordinal numbers such as "first" and "second" are used for convenience and do not limit the number of components or the order of the components (for example, the order of processes or the order of stacking). Furthermore, an ordinal number assigned to a component in one part of this specification may not match an ordinal number assigned to the same component in another part of this specification or in the claims.

[0037] A transistor is a type of semiconductor element that can perform functions such as amplifying current or voltage and performing a switching operation to control conduction or non-conduction. The term "transistor" used in this specification includes an insulated gate field effect transistor (IGFET) and a thin film transistor (TFT).

[0038] In this specification and the like, a transistor using an oxide semiconductor or a metal oxide for a semiconductor layer and a transistor having an oxide semiconductor or a metal oxide for a channel formation region may be referred to as an OS transistor. A transistor having silicon for a channel formation region may be referred to as a Si transistor.

[0039] In this specification and the like, a transistor is an element having at least three terminals including a gate, a drain, and a source. A transistor has a region (also referred to as a channel formation region) where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode), and current can flow between the source and the drain through the channel formation region. Note that in this specification and the like, the channel formation region refers to a region through which current mainly flows.

[0040] Furthermore, the functions of "source" and "drain" may be interchanged when transistors of different polarities are used, or when the direction of current flow changes during circuit operation, etc. Therefore, in this specification, the terms "source" and "drain" may be used interchangeably.

[0041] Note that impurities in a semiconductor refer to, for example, elements other than the main components constituting the semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be considered an impurity. The presence of impurities may increase the density of defect states in the semiconductor or reduce the crystallinity, for example. When the semiconductor is an oxide semiconductor, impurities that change the characteristics of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor. Specific examples include hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, and nitrogen. Note that water may also function as an impurity. For example, the inclusion of impurities may cause oxygen deficiency (V) in the oxide semiconductor. O In some cases, a nucleus (also referred to as a nucleus) may be formed.

[0042] In this specification and the like, an oxynitride refers to a material having a composition in which oxygen is contained in a larger amount than nitrogen, and a nitride oxide refers to a material having a composition in which nitrogen is contained in a larger amount than oxygen.

[0043] To analyze the content of elements such as hydrogen, oxygen, carbon, or nitrogen contained in a film, for example, secondary ion mass spectrometry (SIMS) or X-ray photoelectron spectroscopy (XPS) can be used. XPS is suitable when the content of the target element is high (e.g., 0.5 atomic% or more, or 1 atomic% or more). On the other hand, SIMS is suitable when the content of the target element is low (e.g., 0.5 atomic% or less, or 1 atomic% or less). When comparing the content of elements, it is more preferable to perform a combined analysis using both SIMS and XPS analytical techniques.

[0044] It should be noted that the terms "film" and "layer" can be interchangeable depending on the circumstances. For example, the term "conductive layer" can be changed to the term "conductive film." Or, for example, the term "insulating film" can be changed to the term "insulating layer."

[0045] Furthermore, in this specification, "parallel" refers to a state in which two straight lines are arranged at an angle of -10 degrees or more and 10 degrees or less. Therefore, it also includes cases in which the angle is -5 degrees or more and 5 degrees or less. Furthermore, "substantially parallel" refers to a state in which two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. Furthermore, "perpendicular" refers to a state in which two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it also includes cases in which the angle is 85 degrees or more and 95 degrees or less. Furthermore, "substantially perpendicular" refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less.

[0046] In this specification, "electrically connected" includes a connection via "something that has some kind of electrical function." Here, "something that has some kind of electrical function" is not particularly limited as long as it allows electrical signals to be transmitted and received between the connected objects. For example, "something that has some kind of electrical function" includes electrodes or wiring, as well as switching elements such as transistors, resistive elements, coils, and other elements with various functions.

[0047] In this specification and the like, unless otherwise specified, the off-state current refers to the leakage current between the source and drain when the transistor is in an off state (also referred to as a non-conducting state or a cut-off state). Unless otherwise specified, the off-state current refers to the leakage current between the source and the gate when the voltage V gs is the threshold voltage V th (For p-channel transistors, V th This refers to a state of being (higher than)

[0048] In this specification, "normally on" refers to a state in which a channel exists and a current flows through a transistor even when no voltage is applied to the gate, and "normally off" refers to a state in which no current flows through a transistor when no potential is applied to the gate or when a ground potential is applied to the gate.

[0049] In this specification and the like, a tapered shape refers to a shape in which at least a portion of the side surface of a structure is inclined with respect to the substrate surface or the surface to be formed. For example, it is preferable to have a region in which the angle (also called the taper angle) between the inclined side surface and the substrate surface or the surface to be formed is greater than 0 degrees and less than 90 degrees. Note that the side surface of the structure, the substrate surface, and the surface to be formed do not necessarily need to be completely flat, and may be approximately planar with a slight curvature or approximately planar with a slight unevenness.

[0050] In this specification, when it is stated that A is located on B, at least a portion of A is located on B. Therefore, for example, it can be rephrased as "A has a region located on B." Similarly, when it is stated that A contacts B or A overlaps B, at least a portion of A contacts B or overlaps B. Therefore, it can be rephrased as "A has a region contacting B" or "A has a region overlapping B," respectively. Similarly, in this specification, when it is stated that A covers B, at least a portion of A covers B. Therefore, for example, it can be rephrased as "A has a region covering B."

[0051] In addition, for example, in the drawings related to this specification, arrows indicating the X direction, Y direction, and Z direction may be added. In this specification, etc., the "X direction" refers to the direction along the X axis, and there may be no distinction between the forward direction and the reverse direction unless explicitly stated. The same applies to the "Y direction" and the "Z direction." Furthermore, the X direction, Y direction, and Z direction are directions that intersect with each other. For example, the X direction, Y direction, and Z direction are directions that are perpendicular to each other.

[0052] Embodiment 1 In this embodiment, a semiconductor device of one embodiment of the present invention and a manufacturing method thereof will be described with reference to drawings.

[0053] A semiconductor device according to one embodiment of the present invention is a memory device provided with a memory cell including a first transistor and a second transistor over the first transistor. The semiconductor device according to one embodiment of the present invention includes a first insulating layer, a second insulating layer, and a third insulating layer in addition to the first and second transistors.

[0054] The first transistor includes a first semiconductor layer, a first conductive layer, a second conductive layer, a third conductive layer, and a fourth insulating layer, and the second transistor includes a second semiconductor layer, a third conductive layer, a fourth conductive layer, a fifth conductive layer, and a fifth insulating layer.

[0055] The first conductive layer functions as one of the source electrode and drain electrode of the first transistor. The second conductive layer functions as the other of the source electrode and drain electrode of the first transistor. The third conductive layer functions as the gate electrode of the first transistor and one of the source electrode and drain electrode of the second transistor. The fourth conductive layer functions as the other of the source electrode and drain electrode of the second transistor. The fifth conductive layer functions as the gate electrode of the second transistor. The fourth insulating layer functions as the gate insulating layer of the first transistor. The fifth insulating layer functions as the gate insulating layer of the second transistor.

[0056] A first insulating layer is provided between the first conductive layer and the second conductive layer. A first opening is provided in the first insulating layer and the second conductive layer, reaching the first conductive layer. The first semiconductor layer contacts an upper surface of the first conductive layer, a side surface of the second conductive layer, and a side surface of the first insulating layer within the first opening. The first semiconductor layer also contacts an upper surface of the second conductive layer. The fourth insulating layer has a region located on the first semiconductor layer within the first opening. The third conductive layer has a region facing the first semiconductor layer within the first opening, with the fourth insulating layer sandwiched therebetween.

[0057] A second insulating layer is provided between the third conductive layer and the fourth conductive layer. A second opening is provided in the second insulating layer and the fourth conductive layer, reaching the third conductive layer. The second semiconductor layer contacts an upper surface of the third conductive layer, a side surface of the fourth conductive layer, and a side surface of the second insulating layer within the second opening. The second semiconductor layer also contacts an upper surface of the fourth conductive layer. The fifth insulating layer has a region located on the second semiconductor layer within the second opening. The fifth conductive layer has a region facing the second semiconductor layer within the second opening, with the fifth insulating layer sandwiched therebetween.

[0058] In a semiconductor device according to one embodiment of the present invention, a first recess is provided in the first conductive layer and a second recess is provided in the second conductive layer. This allows the height of the lower surface of the fourth insulating layer and the height of the lower surface of the third conductive layer within the first opening to be lower than when the first recess is not provided in the first conductive layer. Furthermore, the height of the lower surface of the fifth insulating layer and the height of the lower surface of the fifth conductive layer within the second opening to be lower than when the third conductive layer is not provided with the second recess.

[0059] As a result, a gate electric field is easily applied to the first semiconductor layer and the second semiconductor layer. Therefore, the electrical characteristics of the first transistor and the second transistor can be improved. For example, the on-state current of the first transistor and the second transistor can be increased. Therefore, the semiconductor device of one embodiment of the present invention can have high operating speed.

[0060] In the semiconductor device of one embodiment of the present invention, a fourth insulating layer functioning as a gate insulating layer of the first transistor is provided to cover the first semiconductor layer and the second conductive layer. Furthermore, a third conductive layer functioning as a gate electrode of the first transistor is provided to have a region overlapping with the second conductive layer with the fourth insulating layer interposed therebetween. As a result, in the semiconductor device of one embodiment of the present invention, a capacitance is formed in which the fourth insulating layer serves as a dielectric layer and the second conductive layer and the third conductive layer serve as a pair of electrodes. Therefore, the semiconductor device of one embodiment of the present invention can retain data without forming a capacitor in the memory cell. Therefore, the semiconductor device of one embodiment of the present invention can be manufactured with fewer manufacturing steps than a semiconductor device in which a capacitor is formed in the memory cell. As described above, the semiconductor device of one embodiment of the present invention can be a low-cost semiconductor device. Furthermore, by not forming a capacitor in the memory cell, the area occupied by the memory cell can be reduced in some cases. In this case, the semiconductor device of one embodiment of the present invention can be a semiconductor device that can be miniaturized or highly integrated.

[0061] Furthermore, in the semiconductor device of one embodiment of the present invention, a third insulating layer is provided over the second semiconductor layer to have a region overlapping with a fourth conductive layer functioning as the other of the source electrode and drain electrode of the second transistor. In other words, the third insulating layer is provided to have a region overlapping with the fourth conductive layer with the second semiconductor layer interposed therebetween. The third insulating layer has a third opening at a position overlapping with the second opening. A fifth conductive layer is provided inside the third opening. Then, a sixth conductive layer is provided to be in contact with a top surface of the third insulating layer and a top surface of the fifth conductive layer functioning as the gate electrode of the second transistor. The sixth conductive layer functions as a gate wiring.

[0062] In the second transistor, a third insulating layer is provided between the fourth conductive layer and the sixth conductive layer. Here, the thickness of the third insulating layer, for example, the thickness of the third insulating layer in the region overlapping with the fourth conductive layer and the second semiconductor layer, is thicker than the thickness of the fourth insulating layer functioning as the gate insulating layer of the first transistor. Therefore, the parasitic capacitance between the fourth conductive layer and the sixth conductive layer can be made smaller than the parasitic capacitance between the second conductive layer and the third conductive layer.

[0063] As a result, the second transistor can have favorable electrical characteristics. For example, the second transistor can operate at high speed. Therefore, a semiconductor device according to one embodiment of the present invention can have a transistor with favorable electrical characteristics.

[0064] Note that in the semiconductor device of one embodiment of the present invention, a groove (slit) may be provided instead of the opening.

[0065] In a transistor according to one embodiment of the present invention, a source electrode and a drain electrode are located at different heights, and a current flows in a semiconductor layer in the height direction. That is, it can be said that the channel length direction has a component in the height direction (vertical direction). Therefore, the transistor according to one embodiment of the present invention can also be called a VFET (Vertical Field Effect Transistor), a vertical transistor, a vertical channel transistor, a vertical channel transistor, or the like.

[0066] In the transistor of one embodiment of the present invention, a source electrode, a semiconductor layer, and a drain electrode can be provided in a stacked manner, and therefore the area occupied can be significantly reduced compared to a so-called planar transistor in which a semiconductor layer is arranged in a planar shape.

[0067] 1A is a circuit diagram illustrating a configuration example of a memory cell 10 included in a semiconductor device of one embodiment of the present invention. The memory cell 10 includes a transistor 100 and a transistor 200.

[0068] One of the source and the drain of the transistor 100 is electrically connected to a wiring 13. The other of the source and the drain of the transistor 100 is electrically connected to a wiring 15. The gate of the transistor 100 is electrically connected to one of the source and the drain of the transistor 200. The other of the source and the drain of the transistor 200 is electrically connected to a wiring 23. The gate of the transistor 200 is electrically connected to a wiring 21. Here, a node to which the gate of the transistor 100 and the one of the source and the drain of the transistor 200 are connected is referred to as a node ND1.

[0069] As will be described in detail later, a capacitance Cp is formed between an electrode serving as the other of the source and drain of the transistor 100, the gate of the transistor 100, and an electrode serving as one of the source and drain of the transistor 200.

[0070] The wiring 21 functions as a word line. A signal for controlling the on / off state of the transistor 200 is supplied to the wiring 21.

[0071] The wiring 23 functions as a bit line. A data signal to be supplied to the memory cell 10 is supplied to the wiring 23. When the transistor 200 is on, data corresponding to the potential of the wiring 23 is written to the memory cell 10. When the transistor 200 is turned off, the data written to the memory cell 10 is held. Specifically, the potential of the node ND1 is held.

[0072] The wiring 13 functions as a bit line. The wiring 15 functions as a power supply line and is supplied with a power supply potential. As described above, when data is written to the memory cell 10, the potential of the node ND1 becomes a potential corresponding to the data. A current having a magnitude corresponding to the potential of the node ND1 flows between the wiring 15 and the wiring 13. As a result, the potential of the wiring 13 becomes a potential corresponding to the data stored in the memory cell 10. In this way, the data stored in the memory cell 10 can be read. This reading can be performed non-destructively.

[0073] As described above, data is written to the memory cell 10 via the wiring 23, and the data stored in the memory cell 10 is read via the wiring 13. Therefore, the wiring 23 can be called a write bit line, and the wiring 13 can be called a read bit line.

[0074] 1B and 1C are circuit diagrams showing configuration examples of a memory cell 10, and illustrate examples in which the position of the capacitance Cp is different from that of the memory cell 10 shown in FIG. 1A. Fig. 1B illustrates an example in which the capacitance Cp is formed between an electrode functioning as one of the source and drain of the transistor 100 and an electrode functioning as the gate of the transistor 100 and one of the source and drain of the transistor 200. Fig. 1C illustrates an example in which the capacitance Cp is formed between an electrode functioning as the gate of the transistor 200 and an electrode functioning as the gate of the transistor 100 and one of the source and drain of the transistor 200.

[0075] Fig. 1D is a plan view showing a configuration example of a transistor 100. Fig. 1E is a plan view showing a configuration example of a transistor 200. The plan views shown in Fig. 1D and Fig. 1E can also be said to show configuration examples in the XY plane. Note that in the plan views of Fig. 1D and Fig. 1E, some elements are omitted for clarity. The same applies to the subsequent plan views.

[0076] Fig. 1F is a cross-sectional view taken along dashed lines A1-A2 in Fig. 1D and Fig. 1E. Fig. 1G is a cross-sectional view taken along dashed lines A3-A4 in Fig. 1D and Fig. 1E. Fig. 1F can also be said to show an example of the configuration in the XZ plane. Fig. 1G can also be said to show an example of the configuration in the YZ plane.

[0077] Fig. 2A is a cross-sectional view taken along dashed dotted line A1-A2 in Fig. 1D and Fig. 1E, and is an enlarged view of Fig. 1F. Fig. 2B is a plan view showing a configuration example of the cross section taken along dashed dotted line A5-A6 in Fig. 2A.

[0078] 1D to 1G, 2A, and 2B includes an insulating layer 110 over a substrate (not shown), a transistor 100 and an insulating layer 180 over the insulating layer 110, a transistor 200 and an insulating layer 280 over the transistor 100 and the insulating layer 180, an insulating layer 283 over the transistor 200 and the insulating layer 280, an insulating layer 285 over the insulating layer 283, and a conductive layer 265 over the transistor 200 and the insulating layer 285. The insulating layer 110, the insulating layer 180, the insulating layer 280, the insulating layer 283, and the insulating layer 285 function as interlayer films.

[0079] The transistor 100 includes a conductive layer 120, a conductive layer 140 over an insulating layer 180, a semiconductor layer 130, an insulating layer 150 over the semiconductor layer 130, and a conductive layer 220 over the insulating layer 150. The conductive layer 120 includes a conductive layer 120a and a conductive layer 120b over the conductive layer 120a. The conductive layer 140 includes a conductive layer 140a and a conductive layer 140b over the conductive layer 140a. The conductive layer 220 includes a conductive layer 220a and a conductive layer 220b over the conductive layer 220a.

[0080] The transistor 200 includes a conductive layer 220, a conductive layer 240 over an insulating layer 280, a semiconductor layer 230, an insulating layer 250 over the semiconductor layer 230, and a conductive layer 260 over the insulating layer 250. The conductive layer 240 includes a conductive layer 240a and a conductive layer 240b over the conductive layer 240a. Note that the conductive layer 120, the conductive layer 140, the conductive layer 220, and the conductive layer 240 may each have a single-layer structure or a stacked structure of three or more layers.

[0081] The conductive layer 120 functions as one of a source electrode and a drain electrode of the transistor 100. The conductive layer 140 functions as the other of the source electrode and the drain electrode of the transistor 100. The conductive layer 220 functions as the gate electrode of the transistor 100 and one of the source electrode and the drain electrode of the transistor 200. The conductive layer 240 functions as the other of the source electrode and the drain electrode of the transistor 200. The conductive layer 260 functions as the gate electrode of the transistor 200. The insulating layer 150 functions as a gate insulating layer of the transistor 100. The insulating layer 250 functions as a gate insulating layer of the transistor 200. The conductive layer 265 functions as a gate wiring.

[0082] At least a portion of the conductive layer 120 can function as the wiring 13 shown in FIG. 1A. At least a portion of the conductive layer 140 can function as the wiring 15 shown in FIG. 1A. At least a portion of the conductive layer 240 can function as the wiring 23 shown in FIG. 1A. At least a portion of the conductive layer 265 can function as the wiring 21 shown in FIG. 1A. Note that at least a portion of the conductive layer 120 may function as the wiring 15, and at least a portion of the conductive layer 140 may function as the wiring 13.

[0083] At least a part of a region of the semiconductor layer 130 in contact with the insulating layer 180 functions as a channel formation region of the transistor 100. At least a part of a region of the semiconductor layer 230 in contact with the insulating layer 280 functions as a channel formation region of the transistor 200. One of the region of the semiconductor layer 130 in contact with the conductive layer 120 and the region of the semiconductor layer 130 in contact with the conductive layer 140 functions as a source region, and the other functions as a drain region. One of the region of the semiconductor layer 230 in contact with the conductive layer 220 and the region of the semiconductor layer 230 in contact with the conductive layer 240 functions as a source region, and the other functions as a drain region. As described above, the channel formation region of the transistor 100 and the channel formation region of the transistor 200 are sandwiched between the source region and the drain region.

[0084] 1F and 1G, an opening 190 is provided in the conductive layer 140 and the insulating layer 180, reaching the conductive layer 120. A recess 191 is provided in the conductive layer 120 at a position overlapping the opening 190. Specifically, the recess 191 is provided in the conductive layer 120b. The bottom of the recess 191 corresponds to the upper surface of the conductive layer 120, specifically the upper surface of the conductive layer 120b. The sidewall of the recess 191 corresponds to the side surface of the conductive layer 120, specifically the side surface of the conductive layer 120b.

[0085] Opening 190 includes an opening in insulating layer 180 and an opening in conductive layer 140. In other words, the opening in the region where insulating layer 180 overlaps with conductive layer 120 is a part of opening 190, and the opening in the region where conductive layer 140 overlaps with conductive layer 120 is another part of opening 190. Note that opening 190 may or may not include recess 191.

[0086] An opening 290 reaching the conductive layer 220 is provided in the conductive layer 240 and the insulating layer 280. A recess 291 is provided in the conductive layer 220 at a position overlapping the opening 290. Specifically, the recess 291 is provided in the conductive layer 220b. The bottom of the recess 291 corresponds to the upper surface of the conductive layer 220, specifically the upper surface of the conductive layer 220b. The sidewall of the recess 291 corresponds to the side surface of the conductive layer 220, specifically the side surface of the conductive layer 220b.

[0087] The opening 290 is provided at a position where at least a portion thereof overlaps with the opening 190. As described above, the recess 191 is provided at a position where at least a portion thereof overlaps with the opening 190. As a result, the recess 191, the opening 190, the recess 291, and the opening 290 at least partially overlap with one another. This allows the area occupied by the memory cell 10 to be smaller than when, for example, the opening 190 and the opening 290 do not overlap. Therefore, the semiconductor device of one embodiment of the present invention can be a semiconductor device that can be miniaturized or highly integrated. Furthermore, the storage capacity per unit area can be increased.

[0088] The opening 290 includes an opening in the insulating layer 280 and an opening in the conductive layer 240. In other words, the opening in the region where the insulating layer 280 overlaps with the conductive layer 220 is a part of the opening 290, and the opening in the region where the conductive layer 240 overlaps with the conductive layer 220 is another part of the opening 290. Note that the recess 291 may or may not be included in the opening 290.

[0089] The shapes and sizes of openings 190 and 290 in a plan view may differ depending on the layer. When opening 190 as a whole has a circular shape in a plan view, the openings in each layer may or may not be concentric. Similarly, when opening 290 as a whole has a circular shape in a plan view, the openings in each layer may or may not be concentric.

[0090] At least some of the components of the transistor 100 are disposed inside the opening 190. Specifically, the semiconductor layer 130, the insulating layer 150, and the conductive layer 220 are disposed so that at least a portion thereof is located inside the opening 190. The semiconductor layer 130 contacts the top surface of the conductive layer 140. The semiconductor layer 130 also contacts the bottom and sidewall of the recess 191. Furthermore, the semiconductor layer 130 contacts the side surfaces of the conductive layer 140 and the insulating layer 180 inside the opening 190. The insulating layer 150 has a region located on the conductive layer 140 and a region located on the semiconductor layer 130 inside the opening 190. The insulating layer 150 can be provided so as to cover the semiconductor layer 130 and the conductive layer 140. The conductive layer 220 has a region inside the opening 190 that faces the semiconductor layer 130 with the insulating layer 150 sandwiched therebetween.

[0091] Furthermore, the regions of the semiconductor layer 130 and the insulating layer 150 that are disposed inside the opening 190 are provided to reflect the shapes of the recess 191 and the opening 190. Specifically, the semiconductor layer 130 is provided so as to cover the bottom and sidewalls of the recess 191 and the sidewalls of the opening 190, and the insulating layer 150 is provided so as to cover the semiconductor layer 130. Then, the conductive layer 220 is provided so as to fill at least a portion of the recess of the insulating layer 150.

[0092] At least some of the components of the transistor 200 are disposed inside the opening 290. Specifically, the semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are disposed so that at least a portion thereof is located inside the opening 290. The semiconductor layer 230 contacts the top surface of the conductive layer 240. The semiconductor layer 230 also contacts the bottom and sidewall of the recess 291. Furthermore, the semiconductor layer 230 contacts the side surfaces of the conductive layer 240 and the insulating layer 280 inside the opening 290. The insulating layer 250 is located on the semiconductor layer 230 inside the opening 290. The conductive layer 260 has a region inside the opening 290 that faces the semiconductor layer 230 with the insulating layer 250 sandwiched therebetween.

[0093] Furthermore, the regions of the semiconductor layer 230 and the insulating layer 250 that are disposed inside the opening 290 are provided to reflect the shapes of the recess 291 and the opening 290. Specifically, the semiconductor layer 230 is provided so as to cover the bottom and sidewall of the recess 291 and the sidewall of the opening 290, and the insulating layer 250 is provided so as to cover the semiconductor layer 230. Then, the conductive layer 260 is provided so as to fill at least a portion of the recess of the insulating layer 250.

[0094] By having the recess 191 in the conductive layer 120, the height of the lower surfaces of the insulating layer 150 and the conductive layer 220 inside the opening 190 can be made lower than the height of at least a part of the upper surface of the conductive layer 120 that contacts the insulating layer 180, compared to when the recess 191 is not present. Furthermore, by having the recess 291 in the conductive layer 220, the height of the lower surfaces of the insulating layer 250 and the conductive layer 260 inside the opening 290 can be made lower than the height of at least a part of the upper surface of the conductive layer 220 that contacts the insulating layer 280, compared to when the recess 291 is not present.

[0095] The height of each surface can be determined based on the surface where the transistor is formed. Here, the top surface of the insulating layer 110 can be used as the reference. The surface used as the reference is not limited to the surface where the transistor is formed. For example, the top surface of a substrate on which the transistor or semiconductor device is provided can be used as the reference.

[0096] 2A shows distances Ta1, Tb1, Tc1, Ta2, Tb2, and Tc2. Distance Ta1 is the shortest distance from the upper surface of insulating layer 110 to the lower surface of insulating layer 150 in the region overlapping recess 191. Distance Tb1 is the shortest distance from the upper surface of insulating layer 110 to the lower surface of conductive layer 220 in the region overlapping recess 191. Distance Tc1 is the shortest distance from the upper surface of insulating layer 110 to the upper surface of conductive layer 120 that contacts insulating layer 180. Distance Ta2 is the shortest distance from the upper surface of insulating layer 110 to the lower surface of insulating layer 250 in the region overlapping recess 291. Distance Tb2 is the shortest distance from the upper surface of insulating layer 110 to the lower surface of conductive layer 260 in the region overlapping recess 291. Distance Tc2 is the shortest distance from the top surface of insulating layer 110 to the top surface of conductive layer 220 that contacts insulating layer 280 and overlaps with conductive layer 140 .

[0097] The distance Tc1 is preferably longer than the distance Ta1. This increases the contact area between the side surface of the conductive layer 120 and the semiconductor layer 130, thereby reducing the contact resistance between the conductive layer 120 and the semiconductor layer 130. Therefore, a decrease in the on-current of the transistor 100 due to the contact resistance between the conductive layer 120 and the semiconductor layer 130 can be suppressed.

[0098] Furthermore, it is preferable that the distance Tc2 is longer than the distance Ta2. This increases the contact area between the side surface of the conductive layer 220 and the semiconductor layer 230, thereby reducing the contact resistance between the conductive layer 220 and the semiconductor layer 230. Therefore, a decrease in the on-current of the transistor 200 due to the contact resistance between the conductive layer 220 and the semiconductor layer 230 can be suppressed.

[0099] Furthermore, the distance Tc1 is preferably equal to or greater than the distance Tb1, and is further preferably greater than the distance Tb1. This makes it easier to apply a gate electric field to the channel formation region of the semiconductor layer 130, thereby improving the electrical characteristics of the transistor 100. Furthermore, since a gate electric field is also easier to apply to the region of the semiconductor layer 130 that is in contact with the conductive layer 120, the on-state current of the transistor 100 can be increased. Furthermore, regardless of whether the conductive layer 120 or the conductive layer 140 is used as the drain electrode, the electrical characteristics of the transistor 100 can be improved.

[0100] Furthermore, the distance Tc2 is preferably equal to or greater than the distance Tb2, and more preferably greater than the distance Tb2. This makes it easier to apply a gate electric field to the channel formation region of the semiconductor layer 230, thereby improving the electrical characteristics of the transistor 200. Furthermore, since a gate electric field is also easier to apply to a region of the semiconductor layer 230 in contact with the conductive layer 220, the on-state current of the transistor 200 can be increased. Furthermore, regardless of whether the conductive layer 220 or the conductive layer 240 is used as the drain electrode, the electrical characteristics of the transistor 200 can be improved.

[0101] Furthermore, it is preferable to use a conductive material containing oxygen for the conductive layer 120b. As a result, even when a metal oxide is used for the semiconductor layer 130, it is possible to prevent a region with high electrical resistance from being formed in the region of the conductive layer 120b that is in contact with the semiconductor layer 130 and in a region nearby the region, due to oxygen contained in the metal oxide. This reduces the contact resistance between the semiconductor layer 130 and the conductive layer 120b. Similarly, it is preferable to use a conductive material containing oxygen for the conductive layer 140a. As a result, when a metal oxide is used for the semiconductor layer 130, it is possible to reduce the contact resistance between the semiconductor layer 130 and the conductive layer 140a. Furthermore, it is preferable to use a conductive material containing oxygen for the conductive layer 220b. As a result, when a metal oxide is used for the semiconductor layer 230, it is possible to reduce the contact resistance between the semiconductor layer 230 and the conductive layer 220b. Similarly, it is preferable to use a conductive material containing oxygen for the conductive layer 240a. As a result, when a metal oxide is used for the semiconductor layer 230, it is possible to reduce the contact resistance between the semiconductor layer 230 and the conductive layer 240a.

[0102] When the conductive layer 120, the conductive layer 220, and the conductive layer 240 each have a stacked structure, a conductive material containing oxygen is used for a layer of the stacked structure that is closest to a channel formation region, and the contact resistance with the semiconductor layer 130 or the semiconductor layer 230 is reduced, thereby shortening the current path between the source and the drain. This can increase the on-state current of the transistor. As the conductive material containing oxygen, a conductive metal oxide (also referred to as an oxide conductor) is preferably used.

[0103] When the semiconductor layer 130 contacts the upper surface and side surfaces of the conductive layer 140, the contact area with the conductive layer 140 is larger than when the semiconductor layer 130 contacts only the side surfaces of the conductive layer 140. This allows the contact resistance between the semiconductor layer 130 and the conductive layer 140 to be lowered. Therefore, a decrease in the on-current of the transistor 100 due to contact resistance can be suppressed. Furthermore, when the semiconductor layer 230 contacts the upper surface and side surfaces of the conductive layer 240, the contact area with the conductive layer 240 is larger than when the semiconductor layer 230 contacts only the side surfaces of the conductive layer 240. This allows the contact resistance between the semiconductor layer 230 and the conductive layer 240 to be lowered. Therefore, a decrease in the on-current of the transistor 200 due to contact resistance can be suppressed.

[0104] As shown in FIGS. 1F and 1G, the insulating layer 150 is provided to cover the semiconductor layer 130 and the conductive layer 140. The conductive layer 220 is also provided to have an area that overlaps with the conductive layer 140 via the insulating layer 150. As a result, the memory cell 10 has a capacitance Cp as shown in FIG. 1A or 1B. In the examples shown in FIGS. 1A and 1B, the capacitance Cp can be a capacitance in which the insulating layer 150 serves as a dielectric layer and the conductive layer 140 and the conductive layer 220 serve as a pair of electrodes. Note that the capacitance Cp shown in FIG. 1C has the insulating layer 250 as a dielectric layer and the conductive layer 220 and the conductive layer 260 serve as a pair of electrodes.

[0105] As described above, in the semiconductor device of one embodiment of the present invention, data can be held by the capacitance Cp without forming a capacitor in the memory cell 10. Therefore, the number of manufacturing steps for the semiconductor device of one embodiment of the present invention can be reduced compared to when a capacitor is formed in the memory cell 10. As described above, the semiconductor device of one embodiment of the present invention can be a low-cost semiconductor device. Furthermore, by not forming a capacitor in the memory cell 10, the area occupied by the memory cell 10 can be reduced in some cases. In this case, the semiconductor device of one embodiment of the present invention can be a semiconductor device that can be miniaturized or highly integrated. Furthermore, the storage capacity per unit area can be increased. Note that, for example, the sum of the capacitance value of the capacitance Cp shown in FIG. 1A or 1B and the capacitance value of the capacitance Cp shown in FIG. 1C can be used as the capacitance value of the capacitance for holding data.

[0106] In the semiconductor device of one embodiment of the present invention, a capacitor may be formed in the memory cell 10. Specifically, a capacitor connected to the node ND1 of the memory cell 10 can be provided. This allows data to be held in the memory cell 10 for a long period of time.

[0107] Here, the larger the region where the conductive layer 140 and the conductive layer 220 overlap with each other via the insulating layer 150, the larger the capacitance value of the capacitance Cp can be. This allows data to be retained in the memory cell 10 for a long period of time. On the other hand, if the capacitance value of the capacitance Cp is too large, the operation of the semiconductor device of one embodiment of the present invention, specifically, the operation of the memory cell 10, may be slow. For the above reasons, it is preferable to adjust the area during the manufacture of the semiconductor device of one embodiment of the present invention so that the capacitance Cp has a desired value. Note that FIGS. 1F and 2A show an example in which part of the side surface of the conductive layer 140 is covered with the conductive layer 220 via the insulating layer 150. In this case, the capacitance value of the capacitance Cp can be larger than when the side surface of the conductive layer 140 is not covered with the conductive layer 220.

[0108] 1F and 1G, the insulating layer 285 has an opening 270 that reaches the semiconductor layer 230 and overlaps with the opening 290. At least some of the components of the transistor 200 are disposed inside the opening 270. Specifically, the insulating layer 250 and the conductive layer 260 are disposed so that at least a portion thereof is located inside the opening 270. Furthermore, at least a portion of the insulating layer 283 is located inside the opening 270. The insulating layer 283 covers the top surface and side surfaces of the semiconductor layer 230 and the side surfaces of the conductive layer 240. The insulating layer 250 is in contact with the insulating layer 283 inside the opening 270. Note that the opening 270 may be provided in the insulating layer 283.

[0109] The region of insulating layer 250 that is disposed inside opening 270 is provided to reflect the shape of opening 270. Specifically, insulating layer 283 is provided so as to cover the sidewall of opening 270 (the side surface of insulating layer 285), and insulating layer 250 is provided inside insulating layer 283. Then, conductive layer 260 is provided so as to fill at least a portion of the recess in insulating layer 250 that reflects the shape of opening 270.

[0110] In the transistor 200, the conductive layer 260 does not overlap with the top surface of the conductive layer 240, and therefore, the parasitic capacitance between the conductive layer 240 and the conductive layer 260 can be reduced. As shown in FIG. 2A , in a cross-sectional view, the maximum width of the conductive layer 260 is smaller than the width D of the opening 290. When the maximum width of the conductive layer 260 is smaller than the width D of the opening 290, the parasitic capacitance between the conductive layer 260 and the conductive layer 240 can be reduced, which is preferable. Note that, for example, as shown in FIG. 2A , the magnitude relationship between the two widths in the semiconductor device of one embodiment of the present invention can be confirmed by a cross section parallel to the Z direction.

[0111] In this specification, the term "in a cross-sectional view" is used, but it can be specifically rephrased as "in a cross-sectional view from the same direction." For example, when explaining the relationship between multiple components, the relationship in a cross-sectional view from the same direction is explained. In this case, the relationship between the multiple components can be explained using one cross-sectional view.

[0112] The width D of the opening 290 may vary in the depth direction. Here, the shortest distance between the two side surfaces of the conductive layer 240 on the opening 290 side in a cross-sectional view is used as the width D. In other words, the minimum value of the width of the opening 290 in the conductive layer 240 is used as the width D of the opening 290.

[0113] It is preferable that the height of the top surface of the conductive layer 260 and the height of the top surface of the insulating layer 285 are the same or approximately the same. The conductive layer 265 is provided over the insulating layer 285, the insulating layer 283, the insulating layer 250, and the conductive layer 260, and is in contact with the top surface of the conductive layer 260. The conductive layer 265 can also be in contact with the top surface of the insulating layer 285, the top surface of the insulating layer 283, and the top surface of the insulating layer 250. It can also be said that the conductive layer 260 and the conductive layer 265 are electrically connected to each other. The insulating layer 283 and the insulating layer 285 are located between the conductive layer 265 and the conductive layer 240. Here, the thickness of the insulating layer 283 and the insulating layer 285, for example, the total thickness of the insulating layer 283 and the insulating layer 285 in the regions overlapping with the conductive layer 240 and the semiconductor layer 230, is thicker than the thickness of the insulating layer 150. Therefore, the parasitic capacitance between the conductive layer 240 and the conductive layer 265 can be made smaller than the capacitance Cp between the conductive layer 140 and the conductive layer 220 .

[0114] That is, the transistor 200 has a structure in which the parasitic capacitance between the other of the source electrode and the drain electrode and the gate electrode and the parasitic capacitance between the other of the source electrode and the drain electrode and the gate wiring are reduced. Therefore, the transistor 200 can operate at high speed, and the frequency characteristics of the memory cell 10 can be improved. Furthermore, the transistor 200 can have favorable electrical characteristics. Therefore, the semiconductor device of one embodiment of the present invention can be a semiconductor device including a transistor with favorable electrical characteristics.

[0115] 1F shows an example in which the end of the conductive layer 140a, the end of the conductive layer 140b, and the end of the semiconductor layer 130 are aligned outside the opening 190. Also, FIG. 1F shows an example in which the end of the conductive layer 240a, the end of the conductive layer 240b, and the end of the semiconductor layer 230 are aligned outside the opening 290. As in a manufacturing method example described later, the conductive layer 140a, the conductive layer 140b, and the semiconductor layer 130 can be manufactured by processing using the same mask. Furthermore, the conductive layer 240a, the conductive layer 240b, and the semiconductor layer 230 can be manufactured by processing using the same mask. Therefore, the number of masks required for manufacturing a semiconductor device can be reduced, which is preferable.

[0116] The conductive layer 140 has an opening 190 in a region overlapping with the conductive layer 120. Furthermore, it is preferable that the conductive layer 140 is not provided inside the opening 190 of the insulating layer 180. That is, it is preferable that the conductive layer 140 does not contact the side surface of the insulating layer 180 inside the opening 190. With this configuration, the opening 190 can be formed simultaneously in the conductive layer 140 and the insulating layer 180. Furthermore, if the side surface of the conductive layer 140 inside the opening 190 and the side surface of the insulating layer 180 inside the opening 190 are aligned, the film thickness distribution of the semiconductor layer 130 provided inside the opening 190 can be made uniform. Furthermore, it is possible to prevent the semiconductor layer 130 from being divided by a step between the conductive layer 140 and the insulating layer 180.

[0117] Similarly to the above, the conductive layer 240 has an opening 290 in a region overlapping with the conductive layer 220. Furthermore, it is preferable that the conductive layer 240 is not provided inside the opening 290 of the insulating layer 280. In other words, it is preferable that the conductive layer 240 does not contact the side surface of the insulating layer 280 inside the opening 290.

[0118] 1F and 1G show an example in which the inclination of the side surface of the conductive layer 140 inside the opening 190 is equal to the inclination of the side surface of the insulating layer 180 inside the opening 190, but the inclinations of these side surfaces may be different. In this case, for example, it is preferable that the taper angle of the side surface of the conductive layer 140 inside the opening 190 is smaller than the taper angle of the side surface of the insulating layer 180 inside the opening 190. This configuration improves the coverage of the semiconductor layer 130 on the side surface of the conductive layer 140 inside the opening 190, thereby reducing defects such as voids. Furthermore, when the insulating layer 180 has a stacked structure, the inclination of the side surface of each layer inside the opening 190 may be different. Similarly, when the conductive layer 140 has a stacked structure, the inclination of the side surface of each layer inside the opening 190 may be different.

[0119] As described above, Figures 1F and 1G show an example in which the slope of the side surface of the conductive layer 240 inside the opening 290 is equal to the slope of the side surface of the insulating layer 280 inside the opening 290, but the slopes of these sides may be different.

[0120] The transistor 100 includes a metal oxide (also referred to as an oxide semiconductor) that functions as a semiconductor in the semiconductor layer 130 including a channel formation region. The transistor 200 includes a metal oxide (also referred to as an oxide semiconductor) that functions as a semiconductor in the semiconductor layer 230 including a channel formation region. Thus, the transistor 100 and the transistor 200 can be considered OS transistors.

[0121] An OS transistor has an oxygen vacancy (V O ) and impurities, the electrical characteristics are likely to fluctuate, and reliability may be reduced. In addition, hydrogen in the vicinity of the oxygen vacancy may become a defect in which hydrogen enters the oxygen vacancy (hereinafter referred to as V OH) and generate electrons that serve as carriers. Therefore, if oxygen vacancies are present in the channel formation region of the oxide semiconductor, the OS transistor is likely to be normally on. Therefore, it is preferable that oxygen vacancies and impurities are reduced as much as possible in the channel formation region of the oxide semiconductor. In other words, it is preferable that the carrier concentration of the channel formation region of the oxide semiconductor is reduced and the channel formation region of the oxide semiconductor is made i-type (intrinsic) or substantially i-type.

[0122] On the other hand, the source and drain regions of an OS transistor have more oxygen vacancies than the channel formation region. O The source and drain regions of an OS transistor are preferably n-type regions having a high carrier concentration and low resistance compared to a channel formation region, and the source and drain regions of the OS transistor preferably have a high carrier concentration and low resistance due to a high concentration of H or a high concentration of impurities such as hydrogen, nitrogen, or a metal element.

[0123] An OS transistor has a low off-state current. Therefore, by using an OS transistor, particularly for the transistor 100, data can be retained in the memory cell 10 for a long period of time. Therefore, a refresh operation is not necessary. Alternatively, the frequency of the refresh operation can be significantly reduced. As a result, the semiconductor device of one embodiment of the present invention can be a semiconductor device with low power consumption. Here, the transistor 200 can also be an OS transistor, like the transistor 100.

[0124] As described above, the semiconductor layer 130 is provided inside the opening 190 of the insulating layer 180. The transistor 100 has a structure in which one of the source electrode and the drain electrode (the conductive layer 120 in this case) is located below and the other of the source electrode and the drain electrode (the conductive layer 140 in this case) is located above, and thus current flows vertically. That is, a channel is formed along the side surface of the opening 190 of the insulating layer 180. Similarly, the transistor 200 has a channel formed along the side surface of the opening 290 of the insulating layer 280.

[0125] 2B , the insulating layer 280 is in contact with the entire outer periphery of the semiconductor layer 230. Therefore, the channel formation region of the transistor 200 can be formed over the entire outer periphery of the semiconductor layer 230 inside the opening 290 (the entire region in contact with the insulating layer 280). Similarly, the insulating layer 180 is in contact with the entire outer periphery of the semiconductor layer 130. Therefore, the channel formation region of the transistor 100 can be formed over the entire outer periphery of the semiconductor layer 130 inside the opening 190 (the entire region in contact with the insulating layer 180). Note that FIG. 2B can also be considered a cross-sectional view in the XY plane including the channel formation region of the semiconductor layer 230.

[0126] The channel lengths of the transistors 100 and 200 are the distances between the source and drain regions. The channel length of the transistor 100 can correspond to the length of the side surface of the insulating layer 180 on the opening 190 side. The channel length of the transistor 200 can correspond to the length of the side surface of the insulating layer 280 on the opening 290 side. In FIG. 2A , the channel lengths L1 of the transistor 100 and L2 of the transistor 200 are indicated by dashed double-headed arrows. Here, an example is shown in which the channel length L1 corresponds to the length of the side surface of the insulating layer 180 on the opening 190 side. Also, an example is shown in which the channel length L2 corresponds to the length of the side surface of the insulating layer 280 on the opening 290 side.

[0127] In conventional transistors, the channel length is set by the exposure limit of photolithography. However, in one embodiment of the present invention, the channel length can be set by the film thickness of the insulating layer 180 or 280. Therefore, the channel lengths of the transistors 100 and 200 can be made into extremely fine structures that are equal to or less than the exposure limit of photolithography (for example, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less, and 0.1 nm or more, 1 nm or more, or 5 nm or more). As a result, the on-state current of the transistors 100 and 200 can be increased, and the frequency characteristics can be improved.

[0128] Furthermore, as described above, a channel formation region, a source region, and a drain region can be formed inside the opening 190 and the opening 290. As a result, the area occupied by the transistor 100 and the transistor 200 can be reduced compared to a lateral transistor in which the channel formation region, the source region, and the drain region are separately provided on the XY plane. Therefore, the semiconductor device can be highly integrated. Furthermore, when the semiconductor device of one embodiment of the present invention is used for a memory device, the memory capacity per unit area can be increased.

[0129] As shown in FIG. 2B , the semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are arranged concentrically. Therefore, the side surface of the conductive layer 260 located at the center faces the side surface of the semiconductor layer 230 via the insulating layer 250. That is, in a planar view, the entire periphery of the semiconductor layer 230 forms a channel formation region. In this case, for example, the length of the periphery of the semiconductor layer 230 determines the channel width of the transistor 200. That is, the channel width of the transistor 200 can be determined by the width of the opening 290 (or the diameter if the opening 290 is circular in a planar view). In FIGS. 2A and 2B , the width D of the opening 290 is indicated by a double-headed, dashed arrow. In FIG. 2B , the channel width W of the transistor 200 is indicated by a double-headed, dashed arrow. Increasing the width D of the opening 290 increases the channel width per unit area, thereby increasing the on-current. Similarly, in a planar view, the entire periphery of the semiconductor layer 130 forms a channel formation region. In this case, for example, the channel width of the transistor 100 is determined by the periphery length of the semiconductor layer 130. In other words, it can be said that the channel width of the transistor 100 is determined by the width of the opening 190 (or the diameter if the opening 190 is circular in plan view).

[0130] When the opening 290 is formed using photolithography, the width D of the opening 290 is set by the exposure limit of photolithography. The width D of the opening 290 is also set by the film thickness of the semiconductor layer 230, insulating layer 250, and conductive layer 260 provided inside the opening 290. The width D of the opening 290 is, for example, 5 nm or more, 10 nm or more, or 20 nm or more, and is preferably 100 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, or 30 nm or less. When the opening 290 is circular in plan view, the width D of the opening 290 corresponds to the diameter of the opening 290, and the channel width W can be calculated as "D × π." The above can also be applied to the width of the opening 190 by replacing the opening 290, semiconductor layer 230, insulating layer 250, and conductive layer 260 with the opening 190, semiconductor layer 130, insulating layer 150, and conductive layer 220, respectively.

[0131] The channel length L2 of the transistor 200 is preferably at least shorter than the channel width W of the transistor 200. The channel length L2 of the transistor 200 is preferably 0.1 to 0.99 times, and more preferably 0.5 to 0.8 times, the channel width W of the transistor 200. Similarly, the channel length L1 of the transistor 100 is preferably at least shorter than the channel width of the transistor 100. The channel length L1 of the transistor 100 is preferably 0.1 to 0.99 times, and more preferably 0.5 to 0.8 times, the channel width W of the transistor 100. With this structure, the transistors 100 and 200 can have favorable electrical characteristics and high reliability.

[0132] Furthermore, by forming the opening 190 so as to have a circular shape in a plan view, the semiconductor layer 130, the insulating layer 150, and the conductive layer 220 are provided concentrically. This makes the distance between the conductive layer 220 and the semiconductor layer 130 approximately uniform, allowing a gate electric field to be applied approximately uniformly to the semiconductor layer 130. Similarly, by forming the opening 290 so as to have a circular shape in a plan view, it is possible to apply a gate electric field approximately uniformly to the semiconductor layer 230.

[0133] Although the present embodiment illustrates an example in which openings 190, 290, and 270 are circular in plan view, the present invention is not limited thereto. In plan view, openings 190, 290, and 270 can each be, for example, a circle, an approximately circular shape such as an oval, a polygonal shape such as a triangle, a quadrangle (including a rectangle, a diamond, and a square), a pentagon, or a star-shaped polygon, or a polygonal shape with rounded corners. The polygon may be either a concave polygon (a polygon with at least one interior angle exceeding 180 degrees) or a convex polygon (a polygon with all interior angles equal to or less than 180 degrees). As shown in FIGS. 1D and 1E, openings 190, 290, and 270 are preferably circular in plan view. By using a circular shape, the processing accuracy when forming the openings can be improved, allowing for the formation of openings of a finer size. In this specification, a circle is not limited to a perfect circle.

[0134] <Constituent Materials of Semiconductor Device> Materials that can be used in the semiconductor device of this embodiment will be described below. Note that each layer constituting the semiconductor device of this embodiment may have a single-layer structure or a stacked-layer structure. FIGS. 1F and 1G show an example in which the conductive layer 120a, the conductive layer 220a, the semiconductor layer 130, the semiconductor layer 230, and the conductive layer 260 have a single-layer structure. FIG. 2A shows an example in which the conductive layer 120a, the conductive layer 220a, the semiconductor layer 130, the semiconductor layer 230, and the conductive layer 260 have a stacked-layer structure.

[0135] [Semiconductor Layer 130 and Semiconductor Layer 230] As described above, the semiconductor layer 130 and the semiconductor layer 230 have a channel formation region. The channel formation region is i-type (intrinsic) or substantially i-type. The semiconductor layer 130 and the semiconductor layer 230 further have a source region and a drain region. The source region and the drain region are n-type regions (low-resistance regions) with a higher carrier concentration than the channel formation region.

[0136] The crystallinity of the semiconductor material used for the semiconductor layer 130 and the semiconductor layer 230 is not particularly limited, and any of an amorphous semiconductor, a single crystalline semiconductor, and a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part) may be used. Use of a single crystalline semiconductor or a crystalline semiconductor is preferable because it can suppress deterioration of transistor characteristics.

[0137] Furthermore, metal oxide can be used for the semiconductor layer 130 and the semiconductor layer 230. In this case, the semiconductor layer 130 and the semiconductor layer 230 can be called oxide semiconductor layers.

[0138] The band gap of a metal oxide functioning as a semiconductor is preferably 2.0 eV or more, more preferably 2.5 eV or more. By using a metal oxide with a wide band gap, the off-state current of a transistor can be reduced. Because the off-state current of an OS transistor is low, the power consumption of a semiconductor device can be sufficiently reduced. Furthermore, because the frequency characteristics of an OS transistor are high, the semiconductor device can operate at high speed.

[0139] Examples of metal oxides that can be used for the semiconductor layer 130 and the semiconductor layer 230 include indium oxide, gallium oxide, and zinc oxide. The metal oxide preferably contains at least indium (In) or zinc (Zn). The metal oxide preferably contains two or three elements selected from indium, element M, and zinc. The element M is a metal element or a metalloid element having a high bond energy with oxygen, for example, a metal element or a metalloid element having a bond energy with oxygen higher than that of indium. Specific examples of the element M include aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony. The element M contained in the metal oxide is preferably one or more of the above elements, more preferably one or more selected from aluminum, gallium, tin, and yttrium, and even more preferably gallium. In this specification and the like, metal elements and metalloid elements may be collectively referred to as "metal elements," and the "metal elements" described in this specification and the like may include metalloid elements.

[0140] The semiconductor layer 130 and the semiconductor layer 230 may be made of, for example, indium oxide (In oxide), indium zinc oxide (In—Zn oxide, also referred to as IZO (registered trademark)), indium tin oxide (In—Sn oxide), indium titanium oxide (In—Ti oxide), indium gallium oxide (In—Ga oxide), indium gallium aluminum oxide (In—Ga—Al oxide), indium gallium tin oxide (In—Ga—Sn oxide, also referred to as IGTO), gallium zinc oxide (Ga—Zn oxide, also referred to as GZO), aluminum zinc oxide (Al—Zn oxide, also referred to as AZO), or the like. Examples of usable materials include indium aluminum zinc oxide (In-Al-Zn oxide, also referred to as IAZO), indium tin zinc oxide (In-Sn-Zn oxide, also referred to as ITZO (registered trademark)), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium zinc oxide (In-Ga-Zn oxide, also referred to as IGZO), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide, also referred to as IGZTO), and indium gallium aluminum zinc oxide (In-Ga-Al-Zn oxide, also referred to as IGAZO, IGZAO, or IAGZO). Alternatively, examples of usable materials include silicon-containing indium tin oxide, gallium tin oxide (Ga-Sn oxide), and aluminum tin oxide (Al-Sn oxide).

[0141] By increasing the ratio of the number of indium atoms to the total number of atoms of all metal elements contained in the metal oxide, the field-effect mobility of the transistor can be increased, and a transistor with a large on-state current can be realized.

[0142] Note that the metal oxide may contain one or more metal elements having a higher period number in the periodic table instead of or in addition to indium. The greater the overlap of the orbitals of metal elements, the greater the carrier conduction in the metal oxide. Therefore, including a metal element having a higher period number in the periodic table may improve the field-effect mobility of a transistor. Examples of metal elements having a higher period number in the periodic table include metal elements belonging to the fifth period and the sixth period. Specific examples of such metal elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium. Lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium are called light rare earth elements.

[0143] The metal oxide may also contain one or more nonmetallic elements. The presence of a nonmetallic element in the metal oxide may increase the carrier concentration or narrow the band gap, thereby increasing the field-effect mobility of the transistor. Examples of nonmetallic elements include carbon, nitrogen, phosphorus, sulfur, selenium, bromine, and hydrogen.

[0144] Furthermore, by increasing the ratio of the number of zinc atoms to the sum of the numbers of atoms of all metal elements contained in the metal oxide, the metal oxide can be made highly crystalline, and the diffusion of impurities in the metal oxide can be suppressed, thereby suppressing fluctuations in the electrical characteristics of the transistor and improving its reliability.

[0145] Furthermore, by increasing the ratio of the number of atoms of element M to the sum of the number of atoms of all metal elements contained in the metal oxide, a metal oxide with a wide band gap can be obtained. Furthermore, the formation of oxygen vacancies in the metal oxide can be suppressed. Therefore, carrier generation due to oxygen vacancies can be suppressed, resulting in a transistor with a low off-state current. Furthermore, a shift in the threshold voltage of the transistor can be suppressed. Furthermore, fluctuations in the electrical characteristics of the transistor can be suppressed, resulting in improved reliability.

[0146] The electrical characteristics and reliability of a transistor vary depending on the composition of the metal oxide used in the semiconductor layer 130 and the semiconductor layer 230. Therefore, by varying the composition of the metal oxide depending on the electrical characteristics and reliability required of the transistor, a semiconductor device that has both excellent electrical characteristics and high reliability can be obtained.

[0147] When the metal oxide is an In-M-Zn oxide, the atomic ratio of In in the In-M-Zn oxide is preferably equal to or greater than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxides include In:M:Zn=1:1:0.5, In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=1:1:2, In:M:Zn=2:1:3, In:M:Zn=3:1:1, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:3, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, and compositions close to these. Note that the term "nearby composition" includes a range of ±30% of the desired atomic ratio. By increasing the atomic ratio of indium in the metal oxide, the on-state current, field-effect mobility, and the like of the transistor can be increased.

[0148] Furthermore, the atomic ratio of In in the In-M-Zn oxide may be less than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxide include In:M:Zn=1:3:2, In:M:Zn=1:3:3, In:M:Zn=1:3:4, and compositions close to these. By increasing the proportion of M atoms in the metal oxide, the generation of oxygen vacancies can be suppressed.

[0149] When the element M contains a plurality of metal elements, the total proportion of the number of atoms of the metal elements can be used as the proportion of the number of atoms of the element M.

[0150] In this specification and the like, the ratio of the number of indium atoms to the sum of the numbers of atoms of all contained metal elements may be referred to as the indium content. The same applies to other metal elements.

[0151] Furthermore, when the metal oxide is an In-Zn oxide, the atomic ratio of the metal elements in the In-Zn oxide may be, for example, In:Zn = 1:1, In:Zn = 2:1, In:Zn = 4:1, or a composition in the vicinity thereof. The In-Zn oxide may also contain a trace amount of element M. For example, when Sn is contained as element M, the atomic ratio of the metal elements in the metal oxide may be, for example, In:Sn:Zn = 2:0.1:1, In:Sn:Zn = 4:0.1:1, or a composition in the vicinity thereof.

[0152] For example, energy dispersive X-ray spectrometry (EDX), X-ray photoelectron spectrometry (XPS), inductively coupled plasma mass spectrometry (ICP-MS), or inductively coupled plasma atomic emission spectrometry (ICP-AES) can be used to analyze the compositions of the metal oxides used in the semiconductor layer 130 and the semiconductor layer 230. Alternatively, a combination of these techniques may be used for the analysis. In addition, for elements with low content, the actual content and the content obtained by analysis may differ due to the influence of analytical accuracy. For example, when the content of element M is low, the content of element M obtained by analysis may be lower than the actual content. Furthermore, it may be difficult to quantify element M, or element M may not be detected.

[0153] The metal oxide can be preferably formed by sputtering or ALD. When forming a metal oxide by sputtering, the composition of the metal oxide after film formation may differ from the composition of the target. In particular, the zinc content in the metal oxide after film formation may be reduced to about 50% compared to the target. Alternatively, the metal oxide may be formed by chemical vapor deposition (CVD), molecular beam epitaxy (MBE), pulsed laser deposition (PLD), or the like.

[0154] The semiconductor layer 130 and the semiconductor layer 230 may have a stacked structure including two or more metal oxide layers. The two or more metal oxide layers included in the semiconductor layer 130 and the semiconductor layer 230 may have the same or approximately the same composition. By using a stacked structure of metal oxide layers with the same composition, for example, the same sputtering target can be used for formation, thereby reducing manufacturing costs.

[0155] The two or more metal oxide layers included in the semiconductor layer 130 and the semiconductor layer 230 may have different compositions.

[0156] 2A shows an example in which the semiconductor layer 130 has a two-layer structure of an oxide layer 130a and an oxide layer 130b on the oxide layer 130a, and an example in which the semiconductor layer 230 has a two-layer structure of an oxide layer 230a and an oxide layer 230b on the oxide layer 230a.

[0157] For example, the oxide layer 130a and the oxide layer 230a preferably have a higher conductivity than the oxide layer 130b and the oxide layer 230b. By using a highly conductive material for the oxide layer 130a in contact with the source and drain electrodes (conductive layer 120 and conductive layer 140) of the transistor 100, the contact resistance between the semiconductor layer 130 and the conductive layer 120 and the contact resistance between the semiconductor layer 130 and the conductive layer 140 can be reduced. Therefore, the transistor 100 can have a high on-state current. Similarly, by using a highly conductive material for the oxide layer 230a in contact with the source and drain electrodes (conductive layer 220 and conductive layer 240) of the transistor 200, the contact resistance between the semiconductor layer 230 and the conductive layer 220 and the contact resistance between the semiconductor layer 230 and the conductive layer 240 can be reduced. Therefore, the transistor 200 can have a high on-state current.

[0158] Here, if a material with high conductivity is used for the oxide layer 130b provided on the conductive layer 220 side, the threshold voltage of the transistor 100 may shift. As a result, the drain current (hereinafter also referred to as cutoff current) that flows when the gate voltage is 0 V may become large. Specifically, when the transistor 100 is an n-channel transistor, the threshold voltage may be reduced. Similarly, if a material with high conductivity is used for the oxide layer 230b provided on the conductive layer 260 side, the threshold voltage of the transistor 200 may shift. As a result, the cutoff current of the transistor 200 may become large. Specifically, when the transistor 200 is an n-channel transistor, the threshold voltage may be reduced. For the above reasons, it is preferable to use a material with lower conductivity than the oxide layer 130a and the oxide layer 230a for the oxide layer 130b and the oxide layer 230b. As a result, when the transistor 100 and the transistor 200 are n-channel transistors, the threshold voltage can be increased and the cutoff current can be reduced. A small cutoff current may be referred to as normally off.

[0159] As described above, by using a stacked structure of the semiconductor layer 130 and the semiconductor layer 230 and using a material having higher conductivity than the oxide layer 130b and the oxide layer 230b for the oxide layer 130a and the oxide layer 230a, a normally-off transistor with a large on-state current can be obtained. Therefore, a semiconductor device that achieves both low power consumption and high performance can be provided.

[0160] The carrier concentration of the oxide layer 130a and the oxide layer 230a is preferably higher than that of the oxide layer 130b and the oxide layer 230b. Increasing the carrier concentration of the oxide layer 130a and the oxide layer 230a increases the conductivity. Therefore, the contact resistance between the semiconductor layer 130 and the conductive layer 120, the contact resistance between the semiconductor layer 130 and the conductive layer 140, the contact resistance between the semiconductor layer 230 and the conductive layer 220, and the contact resistance between the semiconductor layer 230 and the conductive layer 240 can be reduced. Therefore, the transistor 100 and the transistor 200 can have a large on-state current. Furthermore, decreasing the carrier concentration of the oxide layer 130b and the oxide layer 230b reduces the conductivity, and the transistor 100 and the transistor 200 can be normally-off transistors.

[0161] The semiconductor layer 130 and the semiconductor layer 230 are not limited to the above-described configuration, and the oxide layer 130a and the oxide layer 230a may be made of a material having lower conductivity than the oxide layer 130b and the oxide layer 230b. The carrier concentration of the oxide layer 130a and the oxide layer 230a may be lower than the carrier concentration of the oxide layer 130b and the oxide layer 230b.

[0162] The band gap of the first metal oxide used in the oxide layer 130a and the oxide layer 230a is preferably different from the band gap of the second metal oxide used in the oxide layer 130b and the oxide layer 230b. For example, the difference between the band gap of the first metal oxide and the band gap of the second metal oxide is preferably 0.1 eV or more, more preferably 0.2 eV or more, and even more preferably 0.3 eV or more.

[0163] The band gap of the first metal oxide used for the oxide layer 130a and the oxide layer 230a is preferably smaller than the band gap of the second metal oxide used for the oxide layer 130b and the oxide layer 230b. This can reduce the contact resistance between the semiconductor layer 130 and the conductive layer 120, the contact resistance between the semiconductor layer 130 and the conductive layer 140, the contact resistance between the semiconductor layer 230 and the conductive layer 220, and the contact resistance between the semiconductor layer 230 and the conductive layer 240. Therefore, the transistor 100 and the transistor 200 can have a large on-state current. Furthermore, when the transistor 100 and the transistor 200 are n-channel transistors, the threshold voltage can be increased, and the transistors can be normally-off transistors. Furthermore, the large band gap of the second metal oxide can suppress generation and induction of carriers in the oxide layer 130b and the oxide layer 230b, at the interface between the oxide layer 130b and the insulating layer 150, and at the interface between the oxide layer 230b and the insulating layer 250. This can improve the reliability of the transistor.

[0164] For example, the content of element M in the first metal oxide is preferably lower than the content of element M in the second metal oxide. More specifically, for example, it is preferable to use a metal oxide having a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition thereabout for the oxide layers 130a and 230a, and to use a metal oxide having a composition of In:M:Zn=1:3:2 [atomic ratio] or a composition thereabout for the oxide layers 130b and 230b. In this case, it is particularly preferable to use one or more of gallium, aluminum, and tin as the element M.

[0165] The semiconductor layer 130 and the semiconductor layer 230 are not limited to the above-described configuration, and the band gap of the first metal oxide may be larger than the band gap of the second metal oxide.

[0166] Furthermore, the content of element M in the first metal oxide is preferably lower than the content of element M in the second metal oxide. The first metal oxide may contain a trace amount of element M or may not contain element M. For example, it is preferable that the first metal oxide used in the oxide layer 130a and the oxide layer 230a be an In—Zn oxide, and the second metal oxide used in the oxide layer 130b and the oxide layer 230b be an In-M-Zn oxide. Specifically, the first metal oxide can be an In—Zn oxide, and the second metal oxide can be an In—Ga—Zn oxide.

[0167] For example, for the oxide layer 130a and the oxide layer 230a, it is preferable to use a metal oxide having a composition of In:Zn=1:1 (atomic ratio) or approximately thereto, a metal oxide having a composition of In:Zn=2:1 (atomic ratio) or approximately thereto, a metal oxide having a composition of In:Sn:Zn=2:0.1:1 (atomic ratio) or approximately thereto, a metal oxide having a composition of In:Zn=4:1 (atomic ratio) or approximately thereto, a metal oxide having a composition of In:Sn:Zn=4:0.1:1 (atomic ratio) or approximately thereto, or indium oxide. Furthermore, for the oxide layer 130b and the oxide layer 230b, a metal oxide having an atomic ratio of In:Ga:Zn=1:1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Ga:Zn=1:3:2 or a composition thereof, or a metal oxide having an atomic ratio of In:Ga:Zn=1:3:4 or a composition thereof is preferably used. This enables the on-state current of the transistor 200 to be increased and the transistor structure to have high reliability and little variation.

[0168] For example, when a metal oxide is used for the conductive layer 120 or the conductive layer 140 (in the case of a stacked structure, the layer closest to the channel formation region of the semiconductor layer 130), it is preferable to use In—Zn oxide or In—Sn—Zn oxide for the semiconductor layer 130 (or the oxide layer 130a) because the contact resistance can be reduced compared to when In—Ga—Zn oxide is used for the semiconductor layer 130 (or the oxide layer 130a). Specifically, it is preferable to use indium tin oxide (also referred to as ITO) or indium tin oxide with silicon added (also referred to as ITSO) for the conductive layer 120b and the conductive layer 140a in FIG. 2A , use In—Zn oxide or In—Sn—Zn oxide for the oxide layer 130a, and use In—Ga—Zn oxide for the oxide layer 130b.

[0169] Similarly, when a metal oxide is used for the conductive layer 220 or the conductive layer 240 (in the case of a stacked structure, the layer closest to the channel formation region of the semiconductor layer 230), it is preferable to use In—Zn oxide or In—Sn—Zn oxide for the semiconductor layer 230 (or the oxide layer 230a), because this can reduce the contact resistance compared to when In—Ga—Zn oxide is used for the semiconductor layer 230 (or the oxide layer 230a). Specifically, it is preferable to use ITO or ITSO for the conductive layer 220b and the conductive layer 240a in FIG. 2A , use In—Zn oxide or In—Sn—Zn oxide for the oxide layer 230a, and use In—Ga—Zn oxide for the oxide layer 230b.

[0170] The semiconductor layer 130 and the semiconductor layer 230 are not limited to the above-described configuration, and the content of the element M in the first metal oxide may be higher than the content of the element M in the second metal oxide.

[0171] The crystallinity of the semiconductor material used for the semiconductor layer 130 and the semiconductor layer 230 is not particularly limited, and any of an amorphous semiconductor (a semiconductor having an amorphous structure), a single crystal semiconductor (a semiconductor having a single crystal structure), and a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part) may be used. Use of a single crystal semiconductor or a crystalline semiconductor is preferable because it can suppress deterioration of transistor characteristics.

[0172] The semiconductor layer 130 and the semiconductor layer 230 each preferably include a crystalline metal oxide layer. Examples of crystalline metal oxide structures include a c-axis aligned crystal (CAAC) structure, a polycrystalline (poly-crystal) structure, and a nanocrystalline (nc: nano-crystal) structure. By using a crystalline metal oxide layer for the semiconductor layer 130 and the semiconductor layer 230, the density of defect states in the semiconductor layer 130 and the semiconductor layer 230 can be reduced, thereby achieving a highly reliable semiconductor device. Note that the CAAC structure is a crystal structure in which multiple microcrystals (typically, multiple IGZO microcrystals) have c-axis orientation and are connected without being oriented in the a-b plane. Furthermore, when a cross section of an OS film having a CAAC structure is observed using a high-resolution TEM image, it can be confirmed that metal atoms are arranged in a layered manner in the crystalline portion. Therefore, an OS film having a CAAC structure can also be said to have a structure having layered crystal parts.

[0173] A polycrystalline structure has crystal grain boundaries. Furthermore, when a heat treatment is performed after forming an oxide semiconductor layer with a polycrystalline structure, tiny gaps (also referred to as nanocracks or microcracks) or tiny spaces (also referred to as nanospaces or microspaces) can be formed between crystal portions. When tiny gaps or tiny spaces are formed in the oxide semiconductor layer, the electrical resistance of the oxide semiconductor layer increases. This is because the electrical resistance of the tiny gaps or tiny spaces is very high, for example, infinite. When an oxide semiconductor layer having tiny gaps or tiny spaces is used in a channel formation region of a transistor, the contact resistance between the oxide semiconductor layer and one or both of a source electrode and a drain electrode increases. This adversely affects the initial characteristics or reliability of the transistor. The CAAC structure has fewer crystal grain boundaries in the a-b plane than a polycrystalline structure, and therefore can realize a highly reliable semiconductor device.

[0174] The higher the crystallinity of the metal oxide layers used for the semiconductor layer 130 and the semiconductor layer 230, the more the density of defect states in the semiconductor layer 130 and the semiconductor layer 230 can be reduced. On the other hand, by using a metal oxide layer with low crystallinity, a transistor capable of passing a large current can be realized.

[0175] The higher the substrate temperature (stage temperature) during the formation of the metal oxide layer, the higher the crystallinity of the formed metal oxide layer.Furthermore, the higher the ratio of the flow rate of oxygen gas to the total film formation gas used during the formation (hereinafter also referred to as oxygen flow rate ratio), the higher the crystallinity of the formed metal oxide layer.

[0176] The crystallinity of the semiconductor layer 130 and the semiconductor layer 230 can be analyzed by, for example, X-ray diffraction (XRD), a transmission electron microscope (TEM), or electron diffraction (ED). Alternatively, the analysis may be performed by combining a plurality of these techniques.

[0177] The semiconductor layer 130 and the semiconductor layer 230 can each have a stacked structure of two or more metal oxide layers with different crystallinity. In this case, the two or more metal oxide layers may have different compositions or may have the same or approximately the same composition. For example, a stacked structure of a first metal oxide layer and a second metal oxide layer provided on the first metal oxide layer can be used, and the second metal oxide layer can have a region with higher crystallinity than the first metal oxide layer. Alternatively, the second metal oxide layer can have a region with lower crystallinity than the first metal oxide layer. Note that when the second metal oxide layer has a region with lower crystallinity than the first metal oxide layer, the crystallinity of the second metal oxide layer can be increased by performing heat treatment (also referred to as crystallization treatment) after forming the second metal oxide layer.

[0178] For example, it is preferable to use a metal oxide having an In:M:Zn = 1:3:2 (atomic ratio) or a similar composition for the oxide layer 130a, or a metal oxide having an In:M:Zn = 1:3:4 (atomic ratio) or a similar composition for the oxide layer 130b, and a metal oxide having an In:M:Zn = 1:1:1 (atomic ratio) or a similar composition for the oxide layer 130a. Using a metal oxide with a high ratio of Zn to In for the oxide layer 130a can improve the crystallinity of the oxide layer 130a. Furthermore, forming the oxide layer 130b on the highly crystalline oxide layer 130a also facilitates improving the crystallinity of the oxide layer 130b. The same applies to the oxide layers 230a and 230b. This preferably improves the crystallinity of the entire semiconductor layer 130 and the entire semiconductor layer 230. In this case, it is particularly preferable to use gallium, aluminum, or tin as the element M. For example, two layers of IGZO having different compositions may be stacked. Alternatively, for example, a stacked structure of any one selected from indium oxide, indium gallium oxide, and IGZO and any one selected from IAZO, IAGZO, and ITZO (registered trademark) may be used.

[0179] Furthermore, the semiconductor layer 130 and the semiconductor layer 230 may each have a stacked structure of three or more layers. The semiconductor layer 130 may have a three-layer structure including, for example, an oxide layer, an oxide layer 130a on the oxide layer, and an oxide layer 130b on the oxide layer 130a. The following description will be given taking as an example a case where the semiconductor layer 130 has a three-layer structure, but a similar structure can also be applied to the semiconductor layer 230.

[0180] The oxide layer 130a and the oxide layer 130b can have the same structure as that applicable to the oxide layer 130b. The oxide layer located under the oxide layer 130a can have the same structure as that applicable to the oxide layer 130b. In the following, the oxide layers will be collectively described as a pair of oxide layers sandwiching the oxide layer 130a.

[0181] For example, the oxide layer 130a may preferably be made of a metal oxide having an atomic ratio of In:Zn=1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Zn=2:1 or a composition thereof, a metal oxide having an atomic ratio of In:Sn:Zn=2:0.1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Zn=4:1 or a composition thereof, a metal oxide having an atomic ratio of In:Sn:Zn=4:0.1:1 or a composition thereof, or an indium oxide. Furthermore, the pair of oxide layers sandwiching the oxide layer 130a may preferably be made of a metal oxide having an atomic ratio of In:Ga:Zn=1:1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Ga:Zn=1:3:2 or a composition thereof, or a metal oxide having an atomic ratio of In:Ga:Zn=1:3:4 or a composition thereof.

[0182] Preferably, the pair of oxide layers sandwiching the oxide layer 130a each have a band gap larger than that of the oxide layer 130a. As a result, the oxide layer 130a is sandwiched between the pair of oxide layers with a larger band gap, and the oxide layer 130a functions primarily as a current path (channel). By sandwiching the oxide layer 130a between the pair of oxide layers, trap levels at the interface of the oxide layer 130a and its vicinity can be reduced. This allows for a buried channel transistor in which the channel is spaced away from the insulating layer interface, thereby increasing field-effect mobility. Furthermore, the influence of interface states that may form on the back channel side can be reduced, suppressing photodegradation (e.g., photodegradation due to negative bias current) of the transistor and improving the reliability of the transistor.

[0183] The thickness of the semiconductor layer 130 and the semiconductor layer 230 is preferably 3 nm or more and 200 nm or less, more preferably 3 nm or more and 100 nm or less, further preferably 5 nm or more and 100 nm or less, further preferably 10 nm or more and 100 nm or less, further preferably 10 nm or more and 70 nm or less, further preferably 15 nm or more and 70 nm or less, further preferably 15 nm or more and 50 nm or less, further preferably 20 nm or more and 50 nm or less. In transistors used in smaller semiconductor devices, the thickness of the semiconductor layer 130 and the semiconductor layer 230 is preferably 1 nm or more, 3 nm or more, or 5 nm or more, and 20 nm or less, 15 nm or less, 12 nm or less, or 10 nm or less.

[0184] In addition, it is preferable to use two types of film formation methods, namely, a sputtering method and an ALD method, when forming an oxide semiconductor layer. For example, if a first oxide semiconductor layer having a CAAC structure is formed by a sputtering method and then a second oxide semiconductor layer having lower crystallinity than the CAAC structure is formed by an ALD method, it is expected that the atomic layer of the second oxide semiconductor layer fills or repairs gaps in the atomic-level crystalline portions of the CAAC structure of the first oxide semiconductor layer. In addition, it is preferable to perform heat treatment (for example, at 100° C. or higher and 500° C. or lower, preferably 200° C. or higher and 450° C. or lower, more preferably 300° C. or higher and 400° C. or lower) after forming the second oxide semiconductor layer by the ALD method. It is expected that the heat treatment repairs gaps in the atomic-level crystalline portions of the CAAC structure of the first oxide semiconductor layer with the second oxide semiconductor layer (in other words, each crystalline molecule formed by the ALD method). An oxide semiconductor layer formed using the above two types of film formation methods may be referred to as a hybrid OS.

[0185] Here, the concept of heat treatment for improving the crystallinity of an oxide semiconductor layer will be described with reference to Figures 3A, 3B, 3C, and 3D. Figures 3A, 3B, 3C, and 3D are conceptual diagrams illustrating cross sections of an oxide semiconductor layer having a CAAC structure. In each of the figures, the c-axis is indicated by an arrow.

[0186] The oxide semiconductor layer 370a shown in FIG. 3A includes a region 372a and a region 372b located between the regions 372a. The region 372a corresponds to a region with a CAAC structure (i.e., a structure having layered crystal portions), and the region 372b corresponds to a region between the CAAC structures. The CAAC structure has fewer crystal grain boundaries in the a-b plane than the polycrystalline structure. Thus, even in the oxide semiconductor layer 370a having the CAAC structure, minute gaps or spaces (regions 372b in FIG. 3A ) may exist between the crystal portions.

[0187] Therefore, in order to improve the crystallinity of the oxide semiconductor layer, in other words, to reduce the region 372b shown in FIG. 3A , an oxide semiconductor layer having a CAAC structure is formed as a first oxide semiconductor layer by a sputtering method, and then an oxide semiconductor layer having a microcrystalline structure or an amorphous structure, which has lower crystallinity than the CAAC structure, is formed as a second oxide semiconductor layer by an ALD method.

[0188] 3B , an oxide semiconductor layer having a region 372 a is formed by sputtering as a first oxide semiconductor layer, and then an oxide semiconductor layer having a region 372 c with lower crystallinity than the CAAC structure is formed by ALD as a second oxide semiconductor layer. In FIG. 3B , the oxide semiconductor layer 370 b has the region 372 a and the region 372 c. Since the ALD method can deposit atoms layer by layer, the second oxide semiconductor layer can be formed to fill the region 372 b.

[0189] Then, heat treatment is performed to enhance the crystallinity of the region 372c of the second oxide semiconductor layer using the region 372a of the first oxide semiconductor layer as a seed. In other words, the region 372c of the second oxide semiconductor layer can be crystal-grown using the region 372a of the first oxide semiconductor layer as a seed. Alternatively, the region 372a of the first oxide semiconductor layer having a CAAC structure can be used as a nucleus to crystal-grow the region 372c of the second oxide semiconductor layer having an amorphous structure. This crystal growth model can be considered as a concept equivalent to heteroepitaxy. Note that in FIG. 3C , the oxide semiconductor layer 370c includes a region 372a and a region 372c. The region 372a shown in FIG. 3C has higher crystallinity or a higher density of crystalline portions than the region 372a shown in FIG. 3B. By performing heat treatment, the crystallinity of one or both of the regions 372a and 372c can be increased. Furthermore, the region 372c has, for example, a crystalline portion with the same crystal structure as the crystalline portion of the region 372a. Alternatively, the region 372c has, for example, a crystalline portion connected to the crystalline portion of the region 372a.

[0190] 3D , the oxide semiconductor layer 370d includes a region 372a. The region 372a has improved crystallinity compared to the region 372a shown in FIGS. 3B and 3C , and the boundary between the region 372a and the region 372c disappears, or the boundary between the region 372a and the region 372c is no longer visible. Therefore, the entire oxide semiconductor layer 370d has a CAAC structure. When the entire oxide semiconductor layer 370d has a CAAC structure as shown in FIG. 3D , a highly reliable semiconductor device can be realized. The presence or absence of the boundary between the region 372a and the region 372c can be confirmed using, for example, cross-sectional TEM or cross-sectional STEM.

[0191] Even when the first oxide semiconductor layer has minute gaps or spaces, the minute gaps or spaces in the first oxide semiconductor layer can be filled by forming a second oxide semiconductor layer over the first oxide semiconductor layer or by forming the second oxide semiconductor layer and then performing heat treatment. In this manner, by using an oxide semiconductor layer with a CAAC structure for the first oxide semiconductor layer and an oxide semiconductor layer with a microcrystalline structure or an amorphous structure for the second oxide semiconductor layer, a dense oxide semiconductor layer with increased crystallinity can be obtained. When the dense oxide semiconductor layer with increased crystallinity is used for a channel formation region of a transistor, it is expected that an increase in the electrical resistance of the oxide semiconductor layer can be suppressed or initial characteristics (particularly, on-state current) of the transistor can be improved, thereby making the transistor suitable for high-speed operation.

[0192] When an oxide semiconductor layer is formed by both a sputtering method and an ALD method, if the thickness of the oxide semiconductor layer formed by the ALD method is small, the oxide semiconductor layer can be regarded as a single-layer structure, not a stacked structure of the oxide semiconductor layer formed by the sputtering method and the oxide semiconductor layer formed by the ALD method. For example, when the thickness of the oxide semiconductor layer formed by the ALD method is more than 0 nm and less than or equal to 3 nm, preferably more than 0 nm and less than or equal to 2 nm, and more preferably more than 0 nm and less than or equal to 1 nm, the oxide semiconductor layer formed by the two film formation methods, i.e., the sputtering method and the ALD method, can be regarded as a single-layer structure. In such a case, for example, in a cross-sectional TEM image or a cross-sectional STEM image, the boundary between the oxide semiconductor layer formed by the sputtering method and the oxide semiconductor layer formed by the ALD method is not observed. On the other hand, when the thickness of the oxide semiconductor layer formed by the ALD method exceeds 3 nm, the oxide semiconductor layer may be considered to have a stacked structure, a multilayer structure, or a multiple structure including an oxide semiconductor layer formed by the sputtering method and an oxide semiconductor layer formed by the ALD method.

[0193] Furthermore, when an oxide semiconductor layer is formed by both a sputtering method and an ALD method, it is preferable that the compositions of the metal oxide layers be different from each other. Typically, a metal oxide having an atomic ratio of In:Ga:Zn=1:1:1 or a composition thereabout can be formed by a sputtering method, and then a metal oxide having an atomic ratio of In:Ga:Zn=4:0.1:1 or a composition thereabout can be formed by an ALD method. By using an oxide semiconductor layer having the above composition, a structure can be obtained in which the metal oxide layer having an atomic ratio of In:Ga:Zn=1:1:1 has high reliability, and the metal oxide having an atomic ratio of In:Ga:Zn=4:0.1:1 or a composition thereabout can have high on-state current or high field-effect mobility. Instead of a metal oxide having a composition of In:Ga:Zn=4:0.1:1 (atomic ratio) or a composition close to that, a metal oxide having an atomic ratio of In:Ga:Zn=1:0:0 (atomic ratio), i.e., indium oxide or a metal oxide having a high proportion of In, can be used.

[0194] The oxide semiconductor layer formed by the above two types of film formation methods can be regarded as a structure in which gaps between crystal parts of a CAAC structure are filled with atomic layers formed by an ALD method. Note that the structure can be analyzed by analytical techniques such as cross-sectional SEM, cross-sectional STEM, cross-sectional TEM, SIMS, and EDX.

[0195] Furthermore, an oxide semiconductor layer having a CAAC structure formed by the above-described two kinds of film formation methods may have higher dielectric constant, film density, and film hardness than an oxide semiconductor layer having a CAAC structure formed by one kind of film formation method. Thus, by using an oxide semiconductor layer having a CAAC structure formed by two kinds of film formation methods in a channel formation region of a transistor, a transistor with excellent characteristics (e.g., a transistor with high on-state current, a transistor with high field-effect mobility, a transistor with a small S value, a transistor with high frequency characteristics (also referred to as f characteristics), a highly reliable transistor, etc.) can be realized.

[0196] Hydrogen contained in the oxide semiconductor reacts with oxygen that bonds to metal atoms to form water, and oxygen vacancies (VO In addition, defects in which hydrogen enters oxygen vacancies (hereinafter referred to as V O Hydrogen atoms (H) may function as donors and generate electrons as carriers. Furthermore, some of the hydrogen atoms may bond with oxygen atoms that are bonded to metal atoms to generate electrons as carriers. Therefore, a transistor using an oxide semiconductor containing a large amount of hydrogen tends to be normally on (i.e., has a negative threshold voltage). Furthermore, hydrogen atoms in an oxide semiconductor tend to move due to stresses such as heat or an electric field. Therefore, if an oxide semiconductor contains a large amount of hydrogen, the reliability of the transistor may be reduced.

[0197] V in the semiconductor layer 130 and the semiconductor layer 230 O It is preferable to reduce H as much as possible to make the semiconductor layer 130 and the semiconductor layer 230 highly intrinsic or substantially highly intrinsic. O To obtain an oxide semiconductor in which H is sufficiently reduced, it is important to remove impurities such as water and hydrogen from the oxide semiconductor (sometimes referred to as dehydration or dehydrogenation treatment) and to supply oxygen to the oxide semiconductor to repair oxygen vacancies. O Stable electrical characteristics can be obtained by using an oxide semiconductor in which impurities such as H are sufficiently reduced for a channel formation region of a transistor. Note that supplying oxygen to an oxide semiconductor to repair oxygen vacancies is sometimes referred to as oxygen-adding treatment.

[0198] The carrier concentration of the oxide semiconductor in the region functioning as a channel formation region is 1×10 18 cm −3 Preferably, it is 1×10 or less. 17 cm −3 More preferably, it is less than 1×10 16 cm −3 More preferably, it is less than 1×10 13 cm −3 More preferably, it is less than 1×10 12 cm −3The lower limit of the carrier concentration of the oxide semiconductor in the region functioning as a channel formation region is not particularly limited, but is preferably, for example, 1×10 −9 cm −3 It can be said that:

[0199] Here, the influence of each impurity in a metal oxide (oxide semiconductor) will be described.

[0200] When an oxide semiconductor contains silicon or carbon, which is one of the Group 14 elements, defect levels are formed in the oxide semiconductor. Therefore, the carbon concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3 Less than or equal to 3×10 18 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 The silicon concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3 Less than or equal to 3×10 18 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 The following applies.

[0201] Furthermore, when nitrogen is contained in an oxide semiconductor, electrons serving as carriers are generated, the carrier concentration increases, and the semiconductor is likely to become n-type. As a result, a transistor using an oxide semiconductor containing nitrogen as a semiconductor is likely to be normally on. Alternatively, when nitrogen is contained in an oxide semiconductor, trap states may be formed. As a result, the electrical characteristics of the transistor may become unstable. Therefore, the nitrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than 1×10, more preferably 1×10 19 atoms / cm 3 Less than or equal to 5×10, more preferably 18 atoms / cm 3 Less than 1×10, more preferably 1×10 18 atoms / cm 3 or less, more preferably 5 × 10 17 atoms / cm 3 The following applies.

[0202] Furthermore, hydrogen contained in an oxide semiconductor reacts with oxygen bonded to a metal atom to form water, which may form an oxygen vacancy. Hydrogen entering the oxygen vacancy may generate electrons as carriers. Furthermore, some of the hydrogen may bond with oxygen bonded to a metal atom to generate electrons as carriers. Therefore, a transistor using an oxide semiconductor containing hydrogen is likely to be normally on. Therefore, it is preferable to reduce hydrogen as much as possible in the channel formation region of the oxide semiconductor. Specifically, the hydrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Less than 5×10 19 atoms / cm 3 less than 1×10 19 atoms / cm 3 less than 5×10 18 atoms / cm 3 less than 1×1018 atoms / cm 3 Less than.

[0203] Furthermore, when an oxide semiconductor contains an alkali metal or an alkaline earth metal, defect levels are formed and carriers are generated in some cases. Therefore, a transistor using an oxide semiconductor containing an alkali metal or an alkaline earth metal is likely to be normally on. Therefore, when the concentration of the alkali metal or the alkaline earth metal in the channel formation region of the oxide semiconductor obtained by SIMS is set to 1×10 18 atoms / cm 3 Below 2 × 10, preferably 16 atoms / cm 3 Do the following:

[0204] When an oxide semiconductor with sufficiently reduced impurities is used for a channel formation region of a transistor, stable electrical characteristics can be obtained.

[0205] Note that the semiconductor device of this embodiment may also be applied to a transistor using another semiconductor material in the channel formation region. Examples of such another semiconductor material include semiconductors made of simple elements or compound semiconductors. Examples of semiconductors made of simple elements include silicon and germanium. Examples of compound semiconductors include gallium arsenide and silicon germanium. Other examples of compound semiconductors include organic semiconductors and nitride semiconductors. Note that the aforementioned oxide semiconductor is also a type of compound semiconductor. Note that these semiconductor materials may contain impurities as dopants.

[0206] Silicon that can be used as a semiconductor material for a transistor includes single crystal silicon, polycrystalline silicon, microcrystalline silicon, and amorphous silicon. An example of polycrystalline silicon is low temperature polysilicon (LTPS).

[0207] The semiconductor layer of the transistor may include a layered material that functions as a semiconductor. A layered material is a general term for a group of materials having a layered crystal structure. A layered crystal structure is a structure in which layers formed by covalent or ionic bonds are stacked via bonds weaker than covalent or ionic bonds, such as van der Waals bonds. A layered material has high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, a transistor with a large on-state current can be provided.

[0208] Examples of the layered material include graphene, silicene, and chalcogenides. Chalcogenides are compounds containing chalcogen (an element belonging to Group 16). Examples of chalcogenides include transition metal chalcogenides and Group 13 chalcogenides. Specific examples of transition metal chalcogenides that can be used as semiconductor layers of transistors include molybdenum sulfide (typically MoS 2 ), molybdenum selenide (typically MoSe 2 ), molybdenum telluride (typically MoTe 2 ), tungsten sulfide (typically WS 2 ), tungsten selenide (typically WSe 2 ), tungsten tellurium (typically WTe 2 ), hafnium sulfide (typically HfS 2 ), hafnium selenide (typically HfSe 2 ), zirconium sulfide (typically ZrS 2 ), and zirconium selenide (typically ZrSe 2 ) etc.

[0209] [Insulating Layer] It is preferable to use an inorganic insulating film for each of the insulating layers (insulating layer 110, insulating layer 150, insulating layer 180, insulating layer 250, insulating layer 280, insulating layer 283, insulating layer 285, etc.) included in the semiconductor device. Examples of inorganic insulating films include an oxide insulating film, a nitride insulating film, an oxynitride insulating film, and a nitride oxide insulating film. Examples of oxide insulating films include a silicon oxide film, an aluminum oxide film, a magnesium oxide film, a gallium oxide film, a germanium oxide film, a yttrium oxide film, a zirconium oxide film, a lanthanum oxide film, a neodymium oxide film, a hafnium oxide film, a tantalum oxide film, a cerium oxide film, a gallium zinc oxide film, and a hafnium aluminate film. Examples of nitride insulating films include a silicon nitride film and an aluminum nitride film. Examples of oxynitride insulating films include a silicon oxynitride film, an aluminum oxynitride film, a gallium oxynitride film, an yttrium oxynitride film, and a hafnium oxynitride film. Examples of the nitride oxide insulating film include a silicon nitride oxide film and an aluminum nitride oxide film. An organic insulating film may also be used for an insulating layer included in a semiconductor device.

[0210] For example, as transistors become more miniaturized and highly integrated, problems such as leakage current may occur due to thinner gate insulating layers. Using high-k materials for the gate insulating layer allows for lower voltages during transistor operation while maintaining the physical film thickness. It also allows for thinner equivalent oxide thickness (EOT) of the gate insulating layer. Meanwhile, using a material with a low dielectric constant for the insulating layer that functions as an interlayer film can reduce the parasitic capacitance that occurs between wiring. Therefore, it is advisable to select materials according to the function of the insulating layer. Materials with a low dielectric constant also have high dielectric strength.

[0211] Examples of materials with a high relative dielectric constant (high-k) include aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, and nitrides containing silicon and hafnium.

[0212] Examples of materials with a low relative dielectric constant include inorganic insulating materials such as silicon oxide, silicon oxynitride, and silicon nitride oxide, and resins such as polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate, and acrylic resin. Other examples of inorganic insulating materials with a low relative dielectric constant include silicon oxide doped with fluorine, silicon oxide doped with carbon, and silicon oxide doped with carbon and nitrogen. Another example is silicon oxide having vacancies. These silicon oxides may contain nitrogen.

[0213] Furthermore, a material capable of exhibiting ferroelectricity may be used for the insulating layer of the semiconductor device. Examples of the material capable of exhibiting ferroelectricity include hafnium oxide, zirconium oxide, and HfZrO. X(X is a real number greater than 0). Ferroelectric materials include hafnium oxide to which element J1 (here, element J1 is one or more selected from zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) is added. The ratio of the number of hafnium atoms to the number of element J1 can be set as appropriate; for example, the ratio of the number of hafnium atoms to the number of element J1 can be set to 1:1 or close thereto. Ferroelectric materials include zirconium oxide to which element J2 (here, element J2 is one or more selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) is added. The ratio of the number of zirconium atoms to the number of element J2 can be set as appropriate; for example, the ratio of the number of zirconium atoms to the number of element J2 can be set to 1:1 or close thereto. Furthermore, lead titanate (PbTiO X Piezoelectric ceramics having a perovskite structure, such as barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), or barium titanate, may also be used.

[0214] Furthermore, examples of materials that may exhibit ferroelectricity include metal nitrides containing element M1, element M2, and nitrogen. Here, element M1 is one or more elements selected from aluminum, gallium, indium, etc. Furthermore, element M2 is one or more elements selected from boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, etc. The ratio of the number of atoms of element M1 to the number of atoms of element M2 can be appropriately set. Furthermore, metal oxides containing element M1 and nitrogen may exhibit ferroelectricity even without containing element M2. Furthermore, examples of materials that may exhibit ferroelectricity include materials in which element M3 is added to the above metal nitrides. Furthermore, element M3 is one or more elements selected from magnesium, calcium, strontium, zinc, cadmium, etc. Here, the ratio of the number of atoms of the element M1, the number of atoms of the element M2, and the number of atoms of the element M3 can be set appropriately.

[0215] Furthermore, materials that can have ferroelectricity include SrTaO 2 N or BaTaO 2 Perovskite-type oxynitrides such as GaFeO and GaFeO with κ-alumina structure 3 etc.

[0216] In the above description, metal oxides and metal nitrides are used as examples, but the present invention is not limited thereto. For example, metal oxynitrides in which nitrogen is added to the above metal oxides, or metal oxynitrides in which oxygen is added to the above metal nitrides, etc. may also be used.

[0217] Furthermore, as a material capable of exhibiting ferroelectricity, for example, a mixture or compound made of multiple materials selected from the materials listed above can be used. Alternatively, the insulating layer of a semiconductor device can have a laminated structure made of multiple materials selected from the materials listed above. However, since the crystal structure (characteristics) of the materials listed above may change not only depending on the film formation conditions but also on various processes, in this specification and the like, not only materials that exhibit ferroelectricity are referred to as ferroelectrics, but also as materials capable of exhibiting ferroelectricity.

[0218] Metal oxides containing either or both of hafnium and zirconium can exhibit ferroelectricity even when processed into thin films of a few nanometers. Furthermore, metal oxides containing either or both of hafnium and zirconium can exhibit ferroelectricity even in very small areas. Therefore, the use of metal oxides containing either or both of hafnium and zirconium allows for miniaturization of semiconductor devices.

[0219] In this specification, a layer of a material that can have ferroelectricity may be referred to as a ferroelectric layer, a metal oxide film, or a metal nitride film. Also, in this specification, a device having such a ferroelectric layer, a metal oxide film, or a metal nitride film may be referred to as a ferroelectric device.

[0220] Ferroelectricity is believed to be exhibited by the displacement of oxygen or nitrogen in crystals contained in the ferroelectric layer due to an external electric field. Furthermore, it is believed that the exhibiting of ferroelectricity depends on the crystal structure of the crystals contained in the ferroelectric layer. Therefore, for an insulating layer to exhibit ferroelectricity, the insulating layer must contain crystals. In particular, an insulating layer containing crystals having an orthorhombic crystal structure is preferred because it exhibits ferroelectricity. The crystal structure of the crystals contained in the insulating layer may be one or more selected from cubic, tetragonal, orthorhombic, monoclinic, and hexagonal crystals. The insulating layer may also have an amorphous structure. In this case, the insulating layer may have a composite structure having an amorphous structure and a crystalline structure.

[0221] Furthermore, adding a Group 3 element (also referred to as a IIIa element) in the periodic table to an oxide containing one or both of hafnium and zirconium increases the oxygen vacancy concentration in the oxide, making it easier to form crystals with an orthorhombic crystal structure. This is preferable because it increases the proportion of crystals with an orthorhombic crystal structure and increases the remanent polarization. On the other hand, adding too much of the Group 3 element may reduce the crystallinity of the oxide and make it difficult to exhibit ferroelectricity. Therefore, the content of the Group 3 element in the oxide containing one or both of hafnium and zirconium is preferably 0.1 atomic% to 10 atomic%, more preferably 0.1 atomic% to 5 atomic%, and even more preferably 0.1 atomic% to 3 atomic%. Here, the content of the Group 3 element refers to the ratio of the number of atoms of the Group 3 element to the sum of the number of atoms of all metal elements contained in the layer. The Group 3 element is preferably one or more selected from scandium, lanthanum, and yttrium, and more preferably one or both of lanthanum and yttrium.

[0222] Furthermore, a transistor using a metal oxide can have stable electrical characteristics by being surrounded by an insulating layer that has a function of suppressing the permeation of impurities and oxygen. The insulating layer that has a function of suppressing the permeation of impurities and oxygen can be, for example, a single-layer or stacked insulating layer containing one or more elements selected from boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum. Specifically, the insulating layer that has a function of suppressing the permeation of impurities and oxygen can be made of a metal oxide such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, or tantalum oxide, or a metal nitride such as aluminum nitride, silicon nitride oxide, or silicon nitride.

[0223] Specifically, examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide. Examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include oxides containing aluminum and hafnium (hafnium aluminate). Examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include metal nitrides such as aluminum nitride, aluminum titanium nitride, titanium nitride, silicon nitride oxide, and silicon nitride.

[0224] An insulating layer such as a gate insulating layer that is in contact with an oxide semiconductor layer or that is provided near the oxide semiconductor layer is preferably an insulating layer having a region containing oxygen that is released by heating (hereinafter, sometimes referred to as excess oxygen). For example, when an insulating layer having a region containing excess oxygen is in contact with an oxide semiconductor layer or is located near the oxide semiconductor layer, oxygen vacancies in the oxide semiconductor layer can be reduced. Examples of insulating layers that are likely to have a region containing excess oxygen include silicon oxide, silicon oxynitride, and silicon oxide having vacancies.

[0225] Since the insulating layer 110 functions as an interlayer film, it is preferable that the insulating layer 110 has a low dielectric constant. By using a material with a low dielectric constant for the interlayer film, the parasitic capacitance generated between wirings can be reduced. Silicon oxide and silicon oxynitride are both thermally stable, and therefore are suitable for the insulating layer 110.

[0226] The concentration of impurities such as water and hydrogen in the insulating layer 110 is preferably reduced. This can prevent impurities such as water and hydrogen from entering the channel formation region of the semiconductor layer 130, for example.

[0227] Furthermore, a barrier insulating layer against hydrogen is preferably used as the insulating layer 110. When the insulating layer 110 provided on the outside of the semiconductor layer 130 has a barrier property against hydrogen, diffusion of hydrogen into the semiconductor layer 130 can be suppressed, for example.

[0228] Examples of materials for the barrier insulating layer against hydrogen include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide.

[0229] In this specification and the like, a barrier insulating layer refers to an insulating layer having barrier properties. The barrier properties refer to a property that makes it difficult for a corresponding substance to diffuse (also referred to as a property that makes it difficult for a corresponding substance to permeate, a property that the permeability of a corresponding substance is low, or a function that suppresses the diffusion of a corresponding substance). Note that hydrogen when described as a corresponding substance includes, for example, a hydrogen atom, a hydrogen molecule, a water molecule, and OH. − Furthermore, unless otherwise specified, impurities when described as corresponding substances refer to impurities in the channel formation region or semiconductor layer, and include, for example, hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, and nitrogen oxide molecules (N 2 O, NO, NO 2 The term "oxygen" refers to at least one of an oxygen atom, an oxygen molecule, etc., when described as a corresponding substance.

[0230] For example, it is preferable to use a silicon nitride film as the insulating layer 110 .

[0231] The insulating layer 180 and the insulating layer 280 preferably have the aforementioned barrier insulating layer against hydrogen. The insulating layer 180 is provided so as to surround the semiconductor layer 130. The insulating layer 280 is provided so as to surround the semiconductor layer 230. When the insulating layer 180 provided on the outside of the semiconductor layer 130 has a barrier property against hydrogen, the diffusion of hydrogen into the semiconductor layer 130 can be suppressed. Similarly, when the insulating layer 280 provided on the outside of the semiconductor layer 230 has a barrier property against hydrogen, the diffusion of hydrogen into the semiconductor layer 230 can be suppressed. For example, the insulating layer 180 and the insulating layer 280 preferably have one or both of an aluminum oxide film and a silicon nitride film.

[0232] Silicon nitride also has a barrier property against oxygen. Therefore, by using silicon nitride for the insulating layer 180, it is possible to suppress the extraction of oxygen from the semiconductor layer 130. This makes it possible to suppress the formation of an excessive amount of oxygen vacancies in the semiconductor layer 130. Similarly, by using silicon nitride for the insulating layer 280, it is possible to suppress the extraction of oxygen from the semiconductor layer 230. This makes it possible to suppress the formation of an excessive amount of oxygen vacancies in the semiconductor layer 230.

[0233] Furthermore, using silicon nitride for the insulating layer 180 can prevent excess oxygen from being supplied to the semiconductor layer 130. Therefore, excess oxygen can be prevented from being contained in the channel formation region of the semiconductor layer 130, thereby improving the reliability of the transistor 100. Similarly, using silicon nitride for the insulating layer 280 can improve the reliability of the transistor 200.

[0234] The insulating layer 180 and the insulating layer 280 each preferably include the above-described insulating oxide insulating film, the oxynitride insulating film, or the insulating layer having a region containing excess oxygen.

[0235] For example, an insulating layer having a region containing excess oxygen can be formed by sputtering in an oxygen-containing atmosphere. Here, the sputtering method does not require the use of hydrogen-containing molecules in the deposition gas. Therefore, by using sputtering to deposit the insulating layer 180 and the insulating layer 280, the hydrogen concentrations in the insulating layer 180 and the insulating layer 280 can be reduced. By depositing at least a portion of the insulating layer 180 by sputtering, oxygen can be supplied from the insulating layer 180 to the channel formation region of the semiconductor layer 130, thereby reducing oxygen vacancies and VoH. Furthermore, by depositing at least a portion of the insulating layer 280 by sputtering, oxygen can be supplied from the insulating layer 280 to the channel formation region of the semiconductor layer 230, thereby reducing oxygen vacancies and VoH.

[0236] The concentrations of impurities such as water and hydrogen are preferably reduced in the insulating layer 180 and the insulating layer 280. This can prevent impurities such as water and hydrogen from entering the channel formation regions of the semiconductor layer 130 and the semiconductor layer 230.

[0237] The thickness of the insulating layer 180 on the conductive layer 120 corresponds to the channel length of the transistor 100. Therefore, the thickness of the insulating layer 180 is set appropriately in accordance with the design value of the channel length of the transistor 100. Similarly, the thickness of the insulating layer 280 on the conductive layer 220 corresponds to the channel length of the transistor 200. Therefore, the thickness of the insulating layer 280 is set appropriately in accordance with the design value of the channel length of the transistor 200.

[0238] It is preferable to use a single-layer structure of, for example, a silicon nitride film, a silicon nitride oxide film, or an aluminum oxide film as the insulating layer 180 and the insulating layer 280. Alternatively, it is preferable to use a three-layer structure in which, for example, a silicon nitride film, a silicon oxide film, and a silicon nitride film are stacked in this order as the insulating layer 180 and the insulating layer 280. It is preferable to use a three-layer structure in which, for example, an aluminum oxide film, a silicon oxide film, and an aluminum oxide film are stacked in this order as the insulating layer 180 and the insulating layer 280.

[0239] The insulating layer 150 and the insulating layer 250 preferably have a function of capturing and fixing hydrogen. This can reduce the hydrogen concentration in the semiconductor layer 130 and the semiconductor layer 230 (particularly, the hydrogen concentration in the channel formation region of the transistor). Therefore, the V O By reducing H, the channel forming region can be made i-type or substantially i-type.

[0240] Examples of materials for insulating layers capable of capturing or fixing hydrogen include metal oxides such as oxides containing hafnium, oxides containing magnesium, oxides containing aluminum, and oxides containing aluminum and hafnium (hafnium aluminate). These metal oxides may further contain zirconium, such as oxides containing hafnium and zirconium. Metal oxides with amorphous structures have dangling bonds in some oxygen atoms, which enhance their ability to capture or fix hydrogen. Therefore, these metal oxides preferably have an amorphous structure. For example, an amorphous structure may be achieved by including silicon in these oxides. For example, it is preferable to use an oxide containing hafnium and silicon (hafnium silicate). Metal oxides may have crystalline regions and / or grain boundaries in some regions.

[0241] The ability to capture or fix a corresponding substance can also be said to have the property of making it difficult for the corresponding substance to diffuse. Therefore, the ability to capture or fix a corresponding substance can be rephrased as barrier properties.

[0242] When the gate insulating layer has a stacked structure, the layer in contact with the semiconductor layer 130 and the layer in contact with the semiconductor layer 230 preferably have a function of capturing and fixing hydrogen. This allows hydrogen contained in the semiconductor layer 130 and the semiconductor layer 230 to be more effectively captured or fixed. Therefore, the hydrogen concentrations in the semiconductor layer 130 and the semiconductor layer 230 can be reduced. For example, hafnium silicate or the like may be used as the layer of the insulating layer 150 in contact with the semiconductor layer 130 and the layer of the insulating layer 250 in contact with the semiconductor layer 230. In addition, the layers preferably have an amorphous structure.

[0243] By making the layer amorphous, it is possible to suppress the formation of crystal grain boundaries. By suppressing the formation of crystal grain boundaries, it is possible to improve the flatness of the layer. This makes the film thickness distribution of the insulating layer 150 and the insulating layer 250 uniform, and it is possible to reduce the area where the film thickness is extremely thin. Therefore, it is possible to improve the breakdown voltage of the insulating layer 150 and the insulating layer 250. It is also possible to make the film thickness distribution of the film provided on the insulating layer 150 and the insulating layer 250 uniform.

[0244] Furthermore, by suppressing the formation of grain boundaries in the layers, leakage current due to defect levels at the grain boundaries can be reduced, allowing the insulating layer 150 and the insulating layer 250 to function as insulating films with low leakage current.

[0245] Furthermore, since hafnium oxide is a high dielectric constant (high-k) material, hafnium silicate can also be a high dielectric constant (high-k) material depending on the silicon content. Therefore, when hafnium oxide or hafnium silicate is used for the gate insulating layer, it is possible to reduce the gate potential applied during transistor operation while maintaining the physical film thickness of the gate insulating layer. Furthermore, it is possible to reduce the equivalent oxide thickness (EOT) of the gate insulating layer.

[0246] From the above, it is preferable to use an oxide containing one or both of aluminum and hafnium for the insulating layer 150 and the insulating layer 250, it is more preferable to use an oxide having an amorphous structure and containing one or both of aluminum and hafnium, and it is even more preferable to use aluminum oxide having an amorphous structure.

[0247] Furthermore, it is preferable to use the above-mentioned barrier insulating layer against hydrogen as the insulating layer 150 and the insulating layer 250. By using a barrier insulating layer against hydrogen for the insulating layer 150, it is possible to suppress the diffusion of impurities contained in the conductive layer 220 into the semiconductor layer 130. Similarly, by using a barrier insulating layer against hydrogen for the insulating layer 250, it is possible to suppress the diffusion of impurities contained in the conductive layer 220 into the semiconductor layer 230. For example, silicon nitride has a high barrier property against hydrogen and is therefore suitable for the insulating layer 150 and the insulating layer 250.

[0248] With such a structure, a semiconductor device having good electrical characteristics, high reliability, little variation in the electrical characteristics of the transistors, and a large on-state current can be provided.

[0249] Furthermore, the insulating layer 150 and the insulating layer 250 may have an insulating layer with a thermally stable structure, such as silicon oxide or silicon oxynitride.

[0250] Furthermore, the insulating layer 150 and the insulating layer 250 may have an insulating layer having a heat-stable structure between a pair of insulating layers having the function of capturing and fixing hydrogen.

[0251] The insulating layer 150 and the insulating layer 250 preferably have a barrier insulating layer against oxygen. This can suppress oxidation of the conductive layer 140, the conductive layer 220, the conductive layer 240, the conductive layer 260, and the like. When the insulating layer 150 and the insulating layer 250 have a stacked structure, a layer in contact with the conductive layer 140 or the conductive layer 240 is preferably a barrier insulating layer against oxygen. In particular, among the layers constituting the insulating layer 150 and the insulating layer 250, a layer in contact with the conductive layer 140, a layer in contact with the conductive layer 220, a layer in contact with the conductive layer 240, and a layer in contact with the conductive layer 260 are preferably barrier insulating layers against oxygen.

[0252] By using a barrier insulating layer against hydrogen and oxygen for the layer of the insulating layer 150 that is in contact with the conductive layer 220, oxidation of the conductive layer 220 can be suppressed. Furthermore, it is possible to suppress the oxygen contained in the semiconductor layer 130 from diffusing into the conductive layer 220 and forming oxygen vacancies in the semiconductor layer 130. Similarly, by using a barrier insulating layer against hydrogen and oxygen for the layer of the insulating layer 250 that is in contact with the conductive layer 260, it is possible to suppress the oxidation of the conductive layer 260. Furthermore, it is possible to suppress the oxygen contained in the semiconductor layer 230 from diffusing into the conductive layer 260 and forming oxygen vacancies in the semiconductor layer 230.

[0253] Examples of the barrier insulating layer against oxygen include oxides containing one or both of aluminum and hafnium, magnesium oxide, gallium oxide, gallium zinc oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide. Examples of oxides containing one or both of aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate).

[0254] The layer of the insulating layer 150 in contact with the conductive layer 140 is preferably less permeable to oxygen than at least the insulating layer 180. When the layer has a barrier property against oxygen, the side surfaces of the conductive layer 140 can be prevented from being oxidized and an oxide film can be prevented from being formed on the side surfaces. This can prevent a decrease in the on-state current or the field-effect mobility of the transistor 100.

[0255] Similarly, the layer in the insulating layer 250 that is in contact with the conductive layer 240 is preferably less permeable to oxygen than at least the insulating layer 280. The layer has a barrier property against oxygen, which can prevent the side surfaces of the conductive layer 240 from being oxidized and an oxide film from being formed on the side surfaces. This can prevent a decrease in the on-state current or the field-effect mobility of the transistor 200.

[0256] Each of the layers constituting the insulating layer 150 and the insulating layer 250 is preferably a thin film. For example, the insulating layer 150 and the insulating layer 250 each have a thickness of 1 nm to 20 nm, preferably 3 nm to 10 nm, to reduce the subthreshold swing (also referred to as the S value), which is one of the transistor characteristics. The S value refers to the amount of change in gate voltage when the drain current is changed by one order of magnitude while the drain voltage is constant in the subthreshold region.

[0257] Furthermore, the film thickness of each layer constituting insulating layer 150 and insulating layer 250 is preferably 0.1 nm or more and 10 nm or less, more preferably 0.1 nm or more and 5 nm or less, more preferably 0.5 nm or more and 5 nm or less, more preferably 1 nm or more and 5 nm or less, and even more preferably 1 nm or more and 3 nm or less.

[0258] Furthermore, the insulating layers 150 and 250 preferably have a three-layer structure in which a first insulating layer having a material with a low dielectric constant, a second insulating layer having a function of capturing or fixing hydrogen, and a third insulating layer having barrier properties against hydrogen and oxygen are stacked in this order from the semiconductor layer 130 side and the semiconductor layer 230 side, respectively. Silicon oxide or silicon oxynitride is preferably used as the material with a low dielectric constant for the first insulating layer. The first insulating layer is a layer in contact with the semiconductor layer 130 or the semiconductor layer 230. Using an oxide for the first insulating layer can supply oxygen to the semiconductor layer 130 or the semiconductor layer 230. Furthermore, providing the third insulating layer can suppress diffusion of oxygen contained in the first insulating layer to the conductive layer 220 or the conductive layer 260, thereby suppressing oxidation of the conductive layer 220 or the conductive layer 260. Furthermore, a decrease in the amount of oxygen supplied from the first insulating layer to the semiconductor layer 130 or the semiconductor layer 230 can be suppressed.

[0259] The insulating layer 150 and the insulating layer 250 preferably have a four-layer structure in which a fourth insulating layer having a barrier property against oxygen, a first insulating layer made of a material with a low dielectric constant, a second insulating layer having a function of capturing or fixing hydrogen, and a third insulating layer having a barrier property against hydrogen and oxygen are stacked in this order from the semiconductor layer 130 side and the semiconductor layer 230 side, respectively. The first to third insulating layers can have a structure similar to that of the layers used in the three-layer structure described above. The fourth insulating layer is a layer in contact with the semiconductor layer 130 or the semiconductor layer 230. The fourth insulating layer has a barrier property against oxygen, which can prevent oxygen from being released from the semiconductor layer 130 or the semiconductor layer 230. For example, aluminum oxide may be used as the fourth insulating layer. Aluminum oxide has a function of capturing or fixing hydrogen, and is therefore suitable as the fourth insulating layer in contact with the semiconductor layer 130 or the semiconductor layer 230.

[0260] Typically, the thicknesses of the fourth insulating layer, the first insulating layer, the second insulating layer, and the third insulating layer are 1 nm, 2 nm, 2 nm, and 1 nm, respectively. With such a structure, the transistor can have good electrical characteristics even when miniaturized or highly integrated.

[0261] It is preferable to use a barrier insulating layer against hydrogen for the insulating layer 283. This can suppress diffusion of hydrogen from above the insulating layer 283 into, for example, the semiconductor layer 230. A silicon nitride film and a silicon nitride oxide film each have the characteristics of releasing little impurities (for example, water and hydrogen) from themselves and being less permeable to oxygen and hydrogen, and therefore can be suitably used for the insulating layer 283.

[0262] It is particularly preferable to use silicon nitride formed by a sputtering method as the insulating layer 283. The sputtering method does not require the use of molecules containing hydrogen in the deposition gas, and therefore can reduce the hydrogen concentration in the insulating layer 283. Furthermore, by forming the insulating layer 283 by a sputtering method, silicon nitride with high density can be formed.

[0263] Alternatively, an insulating layer having a function of capturing or fixing hydrogen may be used as the insulating layer 283. With such a structure, it is possible to suppress diffusion of hydrogen from above the insulating layer 283 to, for example, the semiconductor layer 230, and further to capture or fix hydrogen contained in the semiconductor layer 230. Therefore, for example, the hydrogen concentration in the semiconductor layer 230 can be reduced. As the insulating layer 283, aluminum oxide, hafnium oxide, hafnium silicate, or the like can be used.

[0264] Alternatively, the insulating layer 283 may have a stacked structure of an insulating layer having a function of capturing or fixing hydrogen and a barrier insulating layer against hydrogen. For example, the insulating layer 283 may be a stacked film of aluminum oxide and silicon nitride over the aluminum oxide.

[0265] The insulating layer 285 functions as an interlayer film, and therefore is preferably made of the above-mentioned material having a low relative dielectric constant. For example, the insulating layer 285 preferably includes a silicon oxide film.

[0266] [Conductive Layer] For the conductive layers (conductive layer 120, conductive layer 140, conductive layer 220, conductive layer 240, conductive layer 260, conductive layer 265, etc.) included in the semiconductor device, it is preferable to use a metal element selected from aluminum, chromium, copper, silver, gold, platinum, zinc, tantalum, nickel, titanium, iron, cobalt, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing any of the above metal elements as a component, or an alloy combining any of the above metal elements. As the alloy containing any of the above metal elements as a component, a nitride of the alloy or an oxide of the alloy may be used. For example, it is preferable to use tantalum nitride, titanium nitride, tungsten, a nitride containing titanium and aluminum, a nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel. Alternatively, a semiconductor with high electrical conductivity, typified by polycrystalline silicon containing an impurity element such as phosphorus, or a silicide such as nickel silicide may be used.

[0267] Nitrogen-containing conductive materials, such as nitrides containing tantalum, nitrides containing titanium, nitrides containing molybdenum, nitrides containing tungsten, nitrides containing ruthenium, nitrides containing tantalum and aluminum, or nitrides containing titanium and aluminum; oxygen-containing conductive materials, such as ruthenium oxide, oxides containing strontium and ruthenium, or oxides containing lanthanum and nickel; and materials containing metal elements, such as titanium, tantalum, or ruthenium, are preferred because they are conductive materials that are resistant to oxidation, have a function of suppressing oxygen diffusion, or maintain conductivity even after absorbing oxygen. Examples of oxygen-containing conductive materials include indium oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide, indium tin oxide containing titanium oxide, indium tin oxide with added silicon, indium zinc oxide (also referred to as IZO (registered trademark)), and indium zinc oxide containing tungsten oxide. In this specification and the like, a conductive film formed using a conductive material containing oxygen may be referred to as an oxide conductive film.

[0268] Conductive materials containing tungsten, copper, or aluminum as a main component are preferred because they have high conductivity.

[0269] Furthermore, a plurality of conductive layers formed from the above materials may be stacked. For example, a stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing oxygen. A stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing nitrogen. A stacked structure may be formed by combining the above-described material containing a metal element, a conductive material containing oxygen, and a conductive material containing nitrogen.

[0270] When a metal oxide is used for the channel formation region of a transistor, the conductive layer that functions as a gate electrode preferably has a stacked structure that combines a material containing the metal element and a conductive material containing oxygen. In this case, the conductive material containing oxygen is preferably provided on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen desorbed from the conductive material is easily supplied to the channel formation region.

[0271] The conductive layer 120, the conductive layer 140, the conductive layer 220, and the conductive layer 240 are conductive layers in contact with the semiconductor layer 130 or the semiconductor layer 230, respectively. Therefore, for these conductive layers, it is preferable to use a conductive material that is resistant to oxidation, a conductive material that maintains low electrical resistance even when oxidized, a metal oxide having conductivity (also referred to as an oxide conductor), or a conductive material that has a function of suppressing oxygen diffusion. Examples of such conductive materials include a conductive material containing nitrogen and a conductive material containing oxygen. This can suppress a decrease in the conductivity of the conductive layer 120, the conductive layer 140, the conductive layer 220, and the conductive layer 240.

[0272] By using a conductive material containing oxygen for the conductive layer 120, the conductive layer 140, the conductive layer 220, or the conductive layer 240, the conductivity can be maintained even if the conductive layer 120, the conductive layer 140, the conductive layer 220, or the conductive layer 240 absorbs oxygen. In addition, even when an insulating layer containing oxygen such as hafnium oxide is used as the insulating layer 110, the conductive layer 120 is preferable because it can maintain its conductivity. For each of the conductive layer 120, the conductive layer 140, the conductive layer 220, and the conductive layer 240, it is preferable to use, for example, ITO, ITSO, IZO (registered trademark), or the like.

[0273] 2A shows an example in which conductive layer 120 has a three-layer structure including conductive layer 120a1, conductive layer 120a2 on conductive layer 120a1, and conductive layer 120b on conductive layer 120a2. Also, FIG. 2A shows an example in which conductive layer 220 has a three-layer structure including conductive layer 220a1, conductive layer 220a2 on conductive layer 220a1, and conductive layer 220b on conductive layer 220a2.

[0274] For example, it is preferable to use a conductive material that is resistant to oxidation or a conductive material that has the function of suppressing oxygen diffusion for the conductive layers 120a1 and 220a1, a highly conductive material for the conductive layers 120a2 and 220a2, and a conductive material containing oxygen (more preferably, an oxide conductor) for the conductive layers 120b and 220b. For example, it is preferable to use titanium nitride for the conductive layers 120a1 and 220a1, tungsten for the conductive layers 120a2 and 220a2, and an oxide conductor (e.g., ITO, ITSO, or IZO (registered trademark)) for the conductive layers 120b and 220b. In this case, in the conductive layer 120, titanium nitride is in contact with the insulating layer 110, and the oxide conductor is in contact with the semiconductor layer 130. In the conductive layer 220, the oxide conductor is in contact with the semiconductor layer 230. Furthermore, an oxide conductor is used for the layer closest to the channel formation region of the semiconductor layer 130 and the semiconductor layer 230. Compared to tungsten, the oxide conductor has lower contact resistance with the semiconductor layer 130 and the semiconductor layer 230. Therefore, the current path between the source and drain can be shortened in the transistors 100 and 200. Therefore, the on-state current of the transistors 100 and 200 can be increased. With such a structure, the conductive layer 120 can maintain its conductivity even when in contact with the semiconductor layer 130. Furthermore, the conductive layer 220 can maintain its conductivity even when in contact with the semiconductor layer 230. Furthermore, when an oxide insulating layer is used for the insulating layer 110, excessive oxidation of the conductive layer 120 can be suppressed by the insulating layer 110. Furthermore, by using a metal material (here, tungsten) having higher conductivity than an oxide conductor and titanium nitride for the conductive layer 120a2 and the conductive layer 220a2, the conductivity of the conductive layer 120 and the conductive layer 220 can be increased.

[0275] FIG. 2A shows an example in which the conductive layer 140 has a two-layer structure including a conductive layer 140a and a conductive layer 140b on the conductive layer 140a. FIG. 2A also shows an example in which the conductive layer 240 has a two-layer structure including a conductive layer 240a and a conductive layer 240b on the conductive layer 240a. In this case, the conductive layer 140a and the conductive layer 240a are preferably made of a conductive material containing oxygen, for example. The conductive layer 140b and the conductive layer 240b are preferably made of a material having higher conductivity than the conductive layer 140a and the conductive layer 240a, for example. The conductive layer 140a and the conductive layer 240a are preferably made of an oxide conductor (e.g., ITO, ITSO, or IZO (registered trademark)). The conductive layer 140b and the conductive layer 240b are preferably made of ruthenium, tungsten, titanium nitride, or tantalum nitride, for example.

[0276] It is preferable to use a highly conductive material such as tungsten for the conductive layer 260. It is also preferable to use a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion for the conductive layer 260. As described above, examples of such conductive materials include conductive materials containing nitrogen (e.g., titanium nitride or tantalum nitride) and conductive materials containing oxygen (e.g., ruthenium oxide). This can suppress a decrease in the conductivity of the conductive layer 260.

[0277] The conductive layer 260 is preferably made of a conductive material containing oxygen and a metal element contained in the metal oxide in which the channel is formed. Alternatively, the conductive material containing the above-mentioned metal element and nitrogen (e.g., titanium nitride, tantalum nitride, etc.) may be used. Alternatively, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide doped with silicon may be used. Alternatively, indium gallium zinc oxide containing nitrogen may be used. Using such a material may allow hydrogen contained in the metal oxide in which the channel is formed to be captured. Alternatively, hydrogen introduced from an outer insulating layer or the like may be captured.

[0278] 2A shows an example in which the conductive layer 260 has a two-layer structure including a conductive layer 260a and a conductive layer 260b on the conductive layer 260a. In this case, it is preferable to use titanium nitride for the conductive layer 260a and tungsten for the conductive layer 260b. Alternatively, it is preferable to use tantalum nitride for the conductive layer 260a and copper for the conductive layer 260b. With this structure, the conductivity of the conductive layer 260 can be increased.

[0279] The conductive layer 260 may also have a stacked structure of three or more layers, such as a three-layer structure of tantalum nitride, titanium nitride on the tantalum nitride, and tungsten on the titanium nitride.

[0280] The conductive layer 265 preferably has high conductivity because it functions as a gate wiring. Tungsten is preferably used for the conductive layer 265. The conductive layer 265 may have a structure similar to that of the conductive layer 260. For example, a two-layer structure of titanium nitride and tungsten may be used.

[0281] [Substrate] Substrates on which transistors are formed can include, for example, insulating substrates, semiconductor substrates, or conductive substrates. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconia substrates (e.g., yttria-stabilized zirconia substrates), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon or germanium, or compound semiconductor substrates made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, and gallium oxide. Examples of semiconductor substrates include those having an insulating region within the semiconductor substrate, such as an SOI (Silicon-On-Insulator) substrate. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Examples of substrates include substrates having a metal nitride, substrates having a metal oxide, and the like. Examples of substrates include a substrate having a conductor or semiconductor provided on an insulating substrate, a substrate having a conductor or insulator provided on a semiconductor substrate, and a substrate having a semiconductor or insulator provided on a conductive substrate. Alternatively, a substrate provided with elements may be used, such as a capacitor element, a resistor element, a switch element, a light-emitting element, and a memory element.

[0282] <Structure Example 2 of Semiconductor Device> The structure of a semiconductor device according to another embodiment of the present invention will be described below. Specifically, modified examples of the transistor 100 and the transistor 200 will be described. Note that unless otherwise specified, FIG. 1D can be referred to for the planar structure of the transistor 100, and FIG. 1E can be referred to for the planar structure of the transistor 200.

[0283] [Transistor 100A and Transistor 200A] Fig. 4A is a cross-sectional view taken along dashed dotted lines A1-A2 in Fig. 1D and Fig. 1E. Fig. 4B is a cross-sectional view taken along dashed dotted lines A3-A4 in Fig. 1D and Fig. 1E. Fig. 4A shows a transistor 100A as a modification of the transistor 100. Fig. 4B shows a transistor 200A as a modification of the transistor 200.

[0284] The side surface of the conductive layer 140b in the transistor 100A at the opening 190 is positioned outside the side surface of the conductive layer 140a at the opening 190. The side surface of the conductive layer 240b in the transistor 200A at the opening 290 is positioned outside the side surface of the conductive layer 240a at the opening 290. The conductive layers 140 and 240 shown in FIGS. 4A and 4B may be formed as a result of the steps of forming the openings 190 and 290. For example, the conductive layer 140 in the transistor 100A may be formed by forming the opening 190 by etching and then removing part of the conductive layer 140b. Similarly, the conductive layer 240 in the transistor 200A may be formed by forming the opening 290 by etching and then removing part of the conductive layer 240b.

[0285] In the transistor 100A, the semiconductor layer 130 is in contact with the side surface of the conductive layer 140a as well as the top surface of the conductive layer 140a. Therefore, in the transistor 100A, the contact area between the semiconductor layer 130 and the conductive layer 140a can be larger than that of the transistor 100 shown in FIGS. 1F, 1G, and the like. As described above, the conductive layer 140a can be formed using a conductive material containing oxygen. Therefore, when a metal oxide is used for the semiconductor layer 130, the contact resistance per unit area between the semiconductor layer 130 and the conductive layer 140a can be lower than that per unit area between the semiconductor layer 130 and the conductive layer 140b. Therefore, in the transistor 100A, the contact resistance between the semiconductor layer 130 and the conductive layer 140 can be lower than that of the transistor 100 shown in FIGS. 1F, 1G, and the like. Similarly, in the transistor 200A, the contact resistance between the semiconductor layer 230 and the conductive layer 240 can be lower than that of the transistor 200 shown in FIGS. 1F, 1G, and the like. On the other hand, the transistors 100 and 200 shown in FIGS. 1F and 1G can be manufactured through a process that is simpler than that of the transistors 100A and 200A.

[0286] [Transistor 100B and Transistor 200B] Fig. 5A is a plan view showing a configuration example of a transistor 100B, which is a modification of the transistor 100. Fig. 5B is a plan view showing a configuration example of a transistor 200B, which is a modification of the transistor 200. Fig. 5C is a cross-sectional view taken along dashed lines A1-A2 in Figs. 5A and 5B. Fig. 5D is a cross-sectional view taken along dashed lines A3-A4 in Figs. 5A and 5B.

[0287] The side surfaces of the conductive layers 140a and 140b in the transistor 100B in the opening 190 are positioned outside the side surfaces of the insulating layer 180 in the opening 190. The side surfaces of the conductive layers 240a and 240b in the transistor 200B in the opening 290 are positioned outside the side surfaces of the insulating layer 280 in the opening 290. In Figures 5A to 5D, the opening 190 provided in the insulating layer 180 is referred to as opening 190a, and the openings 190 provided in the conductive layers 140a and 140b are referred to as opening 190b. The opening 290 provided in the insulating layer 280 is referred to as opening 290a, and the openings 290 provided in the conductive layers 240a and 240b are referred to as opening 290b. The steps of forming the openings 190 and 290 may result in the formation of the conductive layers 140 and 240 shown in FIGS. 5A to 5D, respectively.

[0288] [Transistor 100C and Transistor 200C] Fig. 6A is a cross-sectional view taken along dashed dotted lines A1-A2 in Fig. 1D and Fig. 1E. Fig. 6B is a cross-sectional view taken along dashed dotted lines A3-A4 in Fig. 1D and Fig. 1E. Fig. 6A shows a transistor 100C as a modification of the transistor 100. Fig. 6B shows a transistor 200C as a modification of the transistor 200.

[0289] In the semiconductor device including the transistor 100C and the transistor 200C, the opening 190 reaches the conductive layer 120a. The semiconductor layer 130 contacts the top surface of the conductive layer 120a inside the opening 190. The opening 290 reaches the conductive layer 220a. The semiconductor layer 230 contacts the top surface of the conductive layer 220a inside the opening 290. Note that although an example in which recesses are not provided in the conductive layer 120a and the conductive layer 220a is shown in FIGS. 6A and 6B, recesses may be provided in the conductive layer 120a and the conductive layer 220a.

[0290] In the transistor 100C, the conductive layer 120b has an opening 190. Therefore, the difference between the distance Tc1 and the distance Tb1 is larger in the transistor 100C than in the transistor 100 shown in FIG. 2A, for example. The larger the difference between the distance Tc1 and the distance Tb1, the larger the area of ​​the region where the side surface of the conductive layer 220 and the conductive layer 120 face each other in the opening 190 or the recess 191 of the conductive layer 120b. Therefore, a gate electric field is more likely to be applied to the channel formation region of the semiconductor layer 130. Similarly, in the transistor 200C, a gate electric field is more likely to be applied to the channel formation region of the semiconductor layer 230 than in the transistor 200 shown in FIG. 2A, for example.

[0291] On the other hand, for example, in the transistor 100 shown in FIG. 2A , the area overlapping with the opening 190 is in contact with the top surface of the conductive layer 120b. Therefore, for example, in the transistor 100 shown in FIG. 2A , the contact area between the semiconductor layer 130 and the conductive layer 120b is larger than that of the transistor 100C. As described above, a conductive material containing oxygen can be used for the conductive layer 120b. Therefore, when a metal oxide is used for the semiconductor layer 130, the contact resistance per unit area between the semiconductor layer 130 and the conductive layer 120b can be lower than the contact resistance per unit area between the semiconductor layer 130 and the conductive layer 120a. As described above, the transistor 100C can have a lower contact resistance between the semiconductor layer 130 and the conductive layer 120 than, for example, the transistor 100 shown in FIG. 2A . Similarly, the transistor 200C can have a lower contact resistance between the semiconductor layer 230 and the conductive layer 220 than, for example, the transistor 200 shown in FIG. 2A .

[0292] [Transistor 100D and Transistor 200D] Fig. 7A is a cross-sectional view taken along dashed dotted lines A1-A2 in Fig. 1D and Fig. 1E. Fig. 7B is a cross-sectional view taken along dashed dotted lines A3-A4 in Fig. 1D and Fig. 1E. Fig. 7A shows a transistor 100D as a modification of the transistor 100. Fig. 7B shows a transistor 200D as a modification of the transistor 200.

[0293] 7A and 7B, insulating layer 180 has a three-layer structure including insulating layer 180a, insulating layer 180b on insulating layer 180a, and insulating layer 180c on insulating layer 180b. Also, in the semiconductor device shown in Figures 7A and 7B, insulating layer 280 has a three-layer structure including insulating layer 280a, insulating layer 280b on insulating layer 280a, and insulating layer 280c on insulating layer 280b. Note that insulating layer 180 and insulating layer 280 may have a single-layer structure, a two-layer structure, or a four- or more-layer structure.

[0294] The insulating layer 180a has a region in contact with the upper surface of the insulating layer 110, a region in contact with the side surface of the conductive layer 120, and a region in contact with the upper surface of the conductive layer 120. The insulating layer 180c has a region in contact with the lower surface of the conductive layer 140a.

[0295] The insulating layer 280a has a region in contact with the insulating layer 150, a region in contact with the side surface of the conductive layer 220, and a region in contact with the upper surface of the conductive layer 220. The insulating layer 280c has a region in contact with the lower surface of the conductive layer 240a.

[0296] The insulating layer 180b is a layer in contact with a channel formation region of the semiconductor layer 130. By using an insulating layer containing oxygen for the insulating layer 180b, oxygen can be supplied to the semiconductor layer 130. Similarly, the insulating layer 280b is a layer in contact with a channel formation region of the semiconductor layer 230. By using an insulating layer containing oxygen for the insulating layer 280b, oxygen can be supplied to the semiconductor layer 230.

[0297] The insulating layer 180b preferably has a region with a higher oxygen content than either or both of the insulating layer 180a and the insulating layer 180c. In particular, the insulating layer 180b preferably has a region with a higher oxygen content than either of the insulating layer 180a and the insulating layer 180c. Increasing the oxygen content of the insulating layer 180b makes it easier to form an i-type region in the semiconductor layer 130 near the insulating layer 180b.

[0298] Similarly, the insulating layer 280b preferably has a region with a higher oxygen content than either or both of the insulating layer 280a and the insulating layer 280c. In particular, the insulating layer 280b preferably has a region with a higher oxygen content than either of the insulating layer 280a and the insulating layer 280c. Increasing the oxygen content of the insulating layer 280b makes it easier to form an i-type region in the semiconductor layer 230 near the insulating layer 280b.

[0299] It is more preferable to use a film that releases oxygen by heating for the insulating layer 180b and the insulating layer 280b. For example, the insulating layer 180b releases oxygen due to heat applied during the manufacturing process of the transistor 100D, and oxygen can be supplied to the semiconductor layer 130. By supplying oxygen from the insulating layer 180b to the semiconductor layer 130, particularly to the channel formation region of the semiconductor layer 130, oxygen vacancies and V O Therefore, the transistor 100D can be a highly reliable transistor having favorable electrical characteristics. Similarly, the transistor 200D can be a highly reliable transistor having favorable electrical characteristics.

[0300] To improve the electrical characteristics and reliability of an OS transistor, it is important to sufficiently reduce the hydrogen concentration in the oxide semiconductor and then optimize the amount of oxygen supplied to the oxide semiconductor.

[0301] In particular, when the channel length of the transistor 100D and the transistor 200D is short, oxygen vacancies in the channel formation region and V OThe influence of H on the electrical characteristics and reliability is particularly large. Therefore, it is preferable to optimize the amount of oxygen supplied to the semiconductor layer 130 and the semiconductor layer 230 after sufficiently reducing the hydrogen concentration in the semiconductor layer 130 and the hydrogen concentration in the semiconductor layer 230. This makes it possible to realize a transistor with a short channel length that has good electrical characteristics and high reliability.

[0302] The insulating layer 180b and the insulating layer 280b are preferably formed by a deposition method such as a sputtering method or a plasma-enhanced CVD (PECVD) method. In particular, when a sputtering method is used, hydrogen is not used as a deposition gas, and therefore a film with an extremely low hydrogen content can be obtained. Therefore, supply of hydrogen to the semiconductor layer 130 and the semiconductor layer 230 can be suppressed, and the electrical characteristics of the transistor 100D and the transistor 200D can be stabilized.

[0303] To increase the amount of oxygen supplied to the semiconductor layer 130, for example, heat treatment in an oxygen-containing atmosphere or plasma treatment in an oxygen-containing atmosphere may be performed after the insulating layer 180b is formed. Alternatively, oxygen may be supplied by forming an oxide film on the top surface of the insulating layer 180b by a sputtering method in an oxygen atmosphere. The oxide film may then be removed. By performing such treatment, oxygen can be supplied to the insulating layer 180b, thereby increasing the amount of oxygen supplied to the semiconductor layer 130. Alternatively, by performing a similar treatment after the insulating layer 280b is formed, oxygen can be supplied to the insulating layer 280b, thereby increasing the amount of oxygen supplied to the semiconductor layer 230.

[0304] Furthermore, the amount of oxygen supplied to the region of the semiconductor layer 130 that is in contact with the insulating layer 180a and the region of the semiconductor layer 130 that is in contact with the insulating layer 180c is smaller than that to the region of the semiconductor layer 130 that is in contact with the insulating layer 180b. Therefore, the resistance of the region of the semiconductor layer 130 that is in contact with the insulating layer 180a and the region of the semiconductor layer 130 that is in contact with the insulating layer 180c may be reduced. In other words, by adjusting the film thicknesses of the insulating layer 180a and the insulating layer 180c, the range of the region that functions as one of the source region and the drain region of the transistor 100D can be controlled.

[0305] Similarly, the region of the semiconductor layer 230 that contacts the insulating layer 280a and the region that contacts the insulating layer 280c receives less oxygen than the region that contacts the insulating layer 280b. Therefore, by adjusting the film thicknesses of the insulating layer 280a and the insulating layer 280c, the range of the region that functions as one of the source region and the drain region of the transistor 200D can be controlled. As described above, the film thicknesses of the insulating layer 180a, the insulating layer 180c, the insulating layer 280a, and the insulating layer 280c can be set appropriately according to the characteristics desired for the transistor.

[0306] The insulating layer 180b and the insulating layer 280b are preferably made of a material with a low dielectric constant, which can reduce parasitic capacitance between wirings. For example, silicon oxide or silicon oxynitride can be used for the insulating layer 180b and the insulating layer 280b.

[0307] The insulating layer 180a, the insulating layer 180c, the insulating layer 280a, and the insulating layer 280c each preferably use a barrier insulating layer against oxygen. By providing the insulating layer 180a between the insulating layer 180b and the conductive layer 120, it is possible to prevent the conductive layer 120 from being oxidized and the electrical resistance of the conductive layer 120 from increasing. Furthermore, by providing the insulating layer 180c between the insulating layer 180b and the conductive layer 140, it is possible to prevent the conductive layer 140 from being oxidized and the electrical resistance of the conductive layer 140 from increasing. Furthermore, by providing the insulating layer 280a between the insulating layer 280b and the conductive layer 220, it is possible to prevent the conductive layer 220 from being oxidized and the electrical resistance of the conductive layer 220 from increasing. Furthermore, by providing the insulating layer 280c between the insulating layer 280b and the conductive layer 240, it is possible to prevent the conductive layer 240 from being oxidized and the electrical resistance of the conductive layer 240 from increasing.

[0308] Alternatively, an insulating layer having a function of capturing or fixing hydrogen may be used as the insulating layer 180a. This structure can suppress diffusion of hydrogen from below the insulating layer 180a into the semiconductor layer 130 and further allow the hydrogen contained in the semiconductor layer 130 to be captured or fixed. This reduces the hydrogen concentration in the semiconductor layer 130. The insulating layer 180a can be made of magnesium oxide, aluminum oxide, hafnium oxide, or an oxide containing hafnium and silicon. Alternatively, the insulating layer 180a can be made of, for example, a stacked film of aluminum oxide and silicon nitride on the aluminum oxide. Similarly, the insulating layer 180c, the insulating layer 280a, and the insulating layer 280c can be made of insulating layers having a function of capturing or fixing hydrogen.

[0309] For example, the insulating layers 180a, 180c, 280a, and 280c can be formed using silicon nitride, and the insulating layers 180b and 280b can be formed using silicon oxide.

[0310] [Transistor 100E and Transistor 200E] Fig. 8A is a cross-sectional view taken along dashed dotted lines A1-A2 in Fig. 1D and Fig. 1E. Fig. 8B is a cross-sectional view taken along dashed dotted lines A3-A4 in Fig. 1D and Fig. 1E. Fig. 8A shows a transistor 100E as a modification of the transistor 100. Fig. 8B shows a transistor 200E as a modification of the transistor 200.

[0311] The semiconductor device shown in FIGS. 8A and 8B differs from the semiconductor device shown in FIGS. 1F and 1G in that it has an insulating layer 122 .

[0312] In the semiconductor device shown in FIGS. 8A and 8B, an insulating layer 122 is provided over an insulating layer 110, and a conductive layer 120a and an insulating layer 180 are provided over the insulating layer 122.

[0313] An insulating layer having a function of capturing or fixing hydrogen is preferably used as the insulating layer 122. This allows hydrogen in the semiconductor layer 130 to diffuse into the insulating layer 122 through the conductive layers 120a and 120b and the hydrogen can be captured or fixed. Therefore, the hydrogen concentration in the semiconductor layer 130 can be reduced.

[0314] For example, it is preferable to use a silicon nitride film as the insulating layer 110 and an oxide film containing hafnium and silicon (hafnium silicate film) as the insulating layer 122 .

[0315] [Transistor 200F and Transistor 200F] Fig. 9A is a cross-sectional view taken along dashed dotted lines A1-A2 in Fig. 1D and Fig. 1E. Fig. 9B is a cross-sectional view taken along dashed dotted lines A3-A4 in Fig. 1D and Fig. 1E. Fig. 9A shows a transistor 100F as a modification of the transistor 100. Fig. 9B shows a transistor 200F as a modification of the transistor 200.

[0316] 9A and 9B, the insulating layer 180 has a two-layer structure including an insulating layer 180d and an insulating layer 180e over the insulating layer 180d. Furthermore, the semiconductor device shown in FIGS. 9A and 9B has the insulating layer 280 has a two-layer structure including an insulating layer 280d and an insulating layer 280e over the insulating layer 280d.

[0317] In the transistor 100F, the conductive layer 155 is located on the insulating layer 180d, and the insulating layer 180e covers the top surface and side surfaces of the conductive layer 155. In addition, in a cross-sectional view, the semiconductor layer 130 has a region that faces the conductive layer 155 with the insulating layer 180e interposed therebetween and also faces the conductive layer 220 with the insulating layer 150 interposed therebetween.

[0318] In the transistor 200F, the conductive layer 255 is located over the insulating layer 280d, and the insulating layer 280e covers the top surface and side surfaces of the conductive layer 255. In addition, in a cross-sectional view, the semiconductor layer 230 has a region that faces the conductive layer 255 with the insulating layer 280e interposed therebetween and also faces the conductive layer 260 with the insulating layer 250 interposed therebetween.

[0319] The conductive layer 155 functions as a backgate electrode of the transistor 100F. The conductive layer 255 functions as a backgate electrode of the transistor 200F. The backgate electrodes of the transistors 100F and 200F facilitate control of the threshold voltage and suppress fluctuations in the threshold voltage. Therefore, the transistors 100F and 200F can have high electrical characteristics and high reliability.

[0320] For the conductive layer 155 and the conductive layer 255, for example, the same material as that used for the conductive layer 260 can be used.

[0321] [Transistor 100G and Transistor 200G] Fig. 10A is a cross-sectional view taken along dashed dotted lines A1-A2 in Fig. 1D and Fig. 1E. Fig. 10B is a cross-sectional view taken along dashed dotted lines A3-A4 in Fig. 1D and Fig. 1E. Fig. 10A shows a transistor 100G as a modification of the transistor 100. Fig. 10B shows a transistor 200G as a modification of the transistor 200.

[0322] 10A and 10B , the insulating layer 180 has a region 180i, and the insulating layer 280 has a region 280i. The region 180i and the region 280i each contain a halogen element. At least a portion of the region 180i is in contact with the semiconductor layer 130, and at least a portion of the region 280i is in contact with the semiconductor layer 230.

[0323] The halogen element is preferably one or more selected from chlorine, fluorine, bromine, and iodine, and more preferably chlorine or fluorine. From the viewpoint of substituting oxygen, it is preferable to use fluorine, which has a higher electronegativity than oxygen.

[0324] When the region 180i contains a halogen element, the halogen element can be supplied from the region 180i into the semiconductor layer 130. Furthermore, when the region 280i contains a halogen element, the halogen element can be supplied from the region 280i into the semiconductor layer 230. The halogen element (X) forms a defect (VoX) in the semiconductor layer 130 and the semiconductor layer 230, in which the halogen element enters an oxygen vacancy (Vo), and has the function of generating electrons that serve as carriers. For example, when chlorine (Cl) is used as the halogen element, chlorine exists stably in the state of VoCl in the semiconductor layer 130 (particularly at and near the interface between the insulating layer 180 and the semiconductor layer 130) and in the semiconductor layer 230 (particularly at and near the interface between the insulating layer 280 and the semiconductor layer 230). In this case, Cl can enter the state of VoCl not only by entering existing Vo but also by substituting oxygen.

[0325] On the other hand, oxygen substituted with Cl (also referred to as excess oxygen) has the function of trapping electrons. Furthermore, carrier trapping by oxygen occurs preferentially over carrier generation by VoCl. Therefore, negative charges (also referred to as negative fixed charges) are formed at and near the interface between the insulating layer 180 and the semiconductor layer 130. The region 180i is in contact with the channel formation region in the semiconductor layer 130. The presence of negative charges in the channel formation region can positively shift the threshold voltage of the transistor 100G. Therefore, even if the transistor 100G has a fine structure or an extremely short channel length, the transistor 100G can be normally off. Similarly, for example, by including the region 280i in the insulating layer 280, the transistor 200G can be normally off even if the transistor 200G has a fine structure or an extremely short channel length.

[0326] For example, it is preferable to use an aluminum oxide layer for the insulating layer 180 and the insulating layer 280 and to use fluorine as the halogen element. The insulating layer 180 and the insulating layer 280 may have a single-layer structure or a stacked-layer structure. When the insulating layer 180 and the insulating layer 280 have a stacked-layer structure, for example, they preferably include one or both of a silicon oxide layer and a silicon nitride layer in addition to an aluminum oxide layer. At this time, it is considered that oxygen bonded to aluminum is replaced with fluorine, and the desorbed oxygen bonds with hydrogen to form an OH group (Al-O + F → Al-F + O + H → AlF + OH). The presence of AlF on the back channel side not only generates negative charge in the channel formation region and positively shifts the threshold voltages of the transistors 100G and 200G, but also provides a function of capturing or fixing hydrogen (also known as gettering). This can reduce the hydrogen concentration in the semiconductor layer 130 and the semiconductor layer 230. In particular, the hydrogen concentration in the channel formation region of the transistor 100G and the hydrogen concentration in the channel formation region of the transistor 200G can be reduced. Therefore, VoH in the channel formation region can be reduced, and the channel formation region can be made i-type or substantially i-type.

[0327] Note that the conductive layer 120, the conductive layer 140, the conductive layer 220, and the conductive layer 240 may also contain a halogen element. Furthermore, a halogen element may be supplied from the conductive layer 120 or the conductive layer 140 into the semiconductor layer 130. Furthermore, a halogen element may be supplied from the conductive layer 220 or the conductive layer 240 into the semiconductor layer 230. In FIGS. 10A and 10B, the side surfaces of the conductive layer 120 and the conductive layer 140 facing the opening 190 are also hatched with the same hatching pattern as the region 180i. Furthermore, in FIGS. 10A and 10B, the side surfaces of the conductive layer 220 and the conductive layer 240 facing the opening 290 are also hatched with the same hatching pattern as the region 280i.

[0328] Furthermore, the semiconductor layer 130 may be in contact with the insulating layer 180 and may have a region containing a halogen element. Furthermore, the semiconductor layer 230 may be in contact with the insulating layer 280 and may have a region containing a halogen element.

[0329] The source and drain regions of the semiconductor layer 130 and the source and drain regions of the semiconductor layer 230 preferably contain an impurity element. The impurity element is preferably a first element. Alternatively, the impurity elements are preferably both the first element and hydrogen.

[0330] 10A and 10B , a region of the semiconductor layer 130 that contacts the upper surface of the conductive layer 120 in the recess 191 is referred to as region 130n1. A region of the semiconductor layer 130 that contacts the upper surface of the conductive layer 140 is referred to as region 130n2. A region of the semiconductor layer 230 that contacts the upper surface of the conductive layer 220 in the recess 291 is referred to as region 230n1. A region of the semiconductor layer 230 that contacts the upper surface of the conductive layer 240 is referred to as region 230n2. Here, regions 130n1 and 130n2 are collectively referred to as region 130n, and regions 230n1 and 230n2 are collectively referred to as region 230n. Regions 130n and 230n preferably contain an impurity element.

[0331] 10A and 10B, regions of the conductive layer 120 and the conductive layer 140 that are in contact with the semiconductor layer 130 are also hatched with the same hatching pattern as the region 130n. Furthermore, regions of the conductive layer 220 and the conductive layer 240 that are in contact with the semiconductor layer 230 are also hatched with the same hatching pattern as the region 230n.

[0332] As the first element, it is preferable to use one or more of boron, aluminum, indium, carbon, silicon, germanium, tin, phosphorus, arsenic, antimony, magnesium, calcium, titanium, copper, zinc, tungsten, molybdenum, tantalum, hafnium, cerium, and noble gases (helium, neon, argon, krypton, xenon, etc.).

[0333] The first element is not limited to the above elements, and one or more of first transition elements (3d transition elements, 3d transition metals), second transition elements (4d transition elements, 4d transition metals), third transition elements (5d transition elements, 5d transition metals), alkaline earth metal elements, and elements included in rare earth elements can be used.

[0334] By supplying the first element to the source region and the drain region, the first element removes oxygen from these regions, causing oxygen vacancies in these regions. These oxygen vacancies then bond with hydrogen in the film, generating carriers, thereby lowering the resistance of the source region and the drain region. This reduces the sheet resistance of the semiconductor layer 130, the sheet resistance of the semiconductor layer 230, the contact resistance between the semiconductor layer 130 and the conductive layer 120, the contact resistance between the semiconductor layer 130 and the conductive layer 140, the contact resistance between the semiconductor layer 230 and the conductive layer 220, and the contact resistance between the semiconductor layer 230 and the conductive layer 240. Therefore, the transistors 100G and 200G can be transistors with large on-state currents. Increasing the on-state currents can lower the operating voltage of the transistors. This reduces the power consumption of the semiconductor device.

[0335] When an element that easily bonds with oxygen is used as the first element, the first element exists in a state bonded to oxygen in the semiconductor layer. Furthermore, when an element that bonds with oxygen to stabilize the semiconductor layer is used as the first element, the first element in the semiconductor layer exists stably in an oxidized state, and is therefore less likely to be desorbed by heat applied during the fabrication process of the semiconductor device, for example, and a stable low-resistance region with low electrical resistance can be realized. For this reason, it is preferable to use an element whose oxide can exist as a solid at 25°C and 1 atmosphere as the first element. Specifically, preferred first elements include typical nonmetallic elements other than hydrogen, typical metallic elements, and transition elements (transition metals), and particularly preferred first elements include boron, phosphorus, magnesium, aluminum, and silicon.

[0336] For these reasons, it is preferable to use boron, phosphorus, magnesium, aluminum, or silicon as one of the first elements, and it is particularly preferable to use boron or phosphorus as one of the first elements.

[0337] Furthermore, hydrogen is suitable as an impurity element because it has the function of bonding with oxygen vacancies in addition to the function of causing the oxygen vacancies.

[0338] By using both the first element and hydrogen as impurity elements, the electrical resistance of the source region and the drain region in the semiconductor layer 130 and the semiconductor layer 230 can be easily reduced, and the low electrical resistance can be stably maintained.

[0339] Furthermore, when both the first element and hydrogen are supplied, ions generated from the source gas can be added without mass separation, which is preferable because it is possible to increase productivity. 2 H 6 By using the gas, boron and hydrogen can be supplied as impurity elements. 3 By using the gas, phosphorus and hydrogen can be supplied as impurity elements. However, the method of supplying the impurity elements is not limited to this. For example, a specific element may be added by ionizing the source gas and mass-separating the ions. For example, B 2 H 6 After mass separation using a gas, boron may be added to the region 130n and the region 230n.

[0340] The region 130n and the region 230n have an impurity element concentration of 1×10 19 atoms / cm 3 1x10 or more 23 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 5x10 or more 22 atoms / cm 3 or less, more preferably 1 × 10 20 atoms / cm 3 1x10 or more 22 atoms / cm 3It is preferable that the concentration of each impurity element is in the above range.

[0341] Note that the impurity element may also be supplied to the channel formation region in the semiconductor layer 130 and the channel formation region in the semiconductor layer 230. Alternatively, due to the influence of heat or the like during the manufacturing process, part of the impurity element contained in the region 130 n and part of the impurity element contained in the region 230 n may diffuse into the channel formation region. The concentration of the impurity element in the channel formation region is preferably 1 / 10 or less, more preferably 1 / 100 or less, of the concentration of the impurity element in the region 130 n and the region 230 n.

[0342] The concentrations of impurity elements contained in the semiconductor layer 130 (including the region 130 n) and the semiconductor layer 230 (including the region 230 n) can be analyzed by, for example, an analytical method such as SIMS or XPS. When XPS analysis is used, the concentration distribution in the depth direction can be determined by combining ion sputtering from the front side or the back side with XPS analysis.

[0343] In manufacturing a semiconductor device according to one embodiment of the present invention, the source and drain regions of the semiconductor layer 130 and the source and drain regions of the semiconductor layer 230 are preferably doped with an impurity element more easily than the channel formation region. Therefore, the impurity element is preferably doped from a direction perpendicular or substantially perpendicular to the top surface of the substrate. In this case, the amount of the impurity element added to the surfaces of the semiconductor layer 130 and the semiconductor layer 230 that are inclined with respect to the top surface of the substrate is smaller than that to the surfaces that are parallel or substantially parallel to the top surface of the substrate. That is, the amount of the impurity element added to the source and drain regions of the semiconductor layer 130 and the source and drain regions of the semiconductor layer 230 is larger than that to the channel formation region. Therefore, the resistance of the source and drain regions can be preferentially reduced.

[0344] [Transistor 100H and Transistor 200H] Fig. 11A is a plan view showing a configuration example of a transistor 100H, which is a modification of the transistor 100. Fig. 11B is a plan view showing a configuration example of a transistor 200H, which is a modification of the transistor 200. Fig. 11C is a cross-sectional view taken along dashed dotted lines A1-A2 in Figs. 11A and 11B. Fig. 11D is a cross-sectional view taken along dashed dotted lines A3-A4 in Figs. 11A and 11B.

[0345] 1D to 1G does not include a conductive layer 265. As shown in FIGS. 11C and 11D , the semiconductor device has an insulating layer 250 in a region located inside the opening 270, a region located on the insulating layer 283, and a region located on the insulating layer 285. The conductive layer 260 has a region located inside the opening 270, a region located on the insulating layer 283, and a region located on the insulating layer 285. In the semiconductor device shown in FIGS. 11A to 11D , the conductive layer 260 functions as a gate wiring.

[0346] The conductive layer 260 has a region overlapping with the upper surface of the conductive layer 240, and the insulating layer 250, the insulating layer 283, and the insulating layer 285 are located between the region of the conductive layer 260 and the conductive layer 240. This allows the parasitic capacitance between the conductive layer 240 and the conductive layer 260 to be smaller than the capacitance Cp between the conductive layer 140 and the conductive layer 220.

[0347] <Example of Manufacturing Method of Semiconductor Device> Next, a manufacturing method of a semiconductor device according to one embodiment of the present invention will be described with reference to the drawings. Note that, with regard to materials and forming methods of elements, descriptions of parts similar to those described above may be omitted.

[0348] Thin films (insulating films, semiconductor films, conductive films, etc.) constituting a semiconductor device can be formed by a sputtering method, a CVD method, a vacuum evaporation method, a PLD method, an ALD method, or the like.

[0349] Sputtering methods include RF sputtering, which uses a high-frequency power supply as the sputtering power source, DC sputtering, which uses a direct current power supply, and pulsed DC sputtering, which changes the voltage applied to the electrode in a pulsed manner. RF sputtering is mainly used to form insulating films, while DC sputtering is mainly used to form metal conductive films. Pulsed DC sputtering is mainly used to form films of compounds such as oxides, nitrides, or carbides using reactive sputtering.

[0350] CVD methods can be further classified into plasma-enhanced CVD (PECVD) methods that utilize plasma, thermal CVD (TCVD) methods that utilize heat, and photo-CVD (photo-CVD) methods that utilize light. CVD methods can also be further classified into metal CVD (MCVD) methods and metal organic CVD (MOCVD) methods depending on the source gas used.

[0351] The plasma CVD method can produce high-quality films at relatively low temperatures. Furthermore, the thermal CVD method is a film formation method that can reduce plasma damage to the workpiece because it does not use plasma. For example, wiring, electrodes, and elements (transistors, capacitors, etc.) included in a semiconductor device may become charged up by receiving electric charge from the plasma. At this time, the accumulated electric charge may destroy the wiring, electrodes, or elements included in the semiconductor device. On the other hand, the thermal CVD method, which does not use plasma, does not cause such plasma damage, and therefore can increase the yield of semiconductor devices. Furthermore, the thermal CVD method does not cause plasma damage during film formation, so films with fewer defects can be obtained.

[0352] As the ALD method, a thermal ALD method in which a reaction between a precursor and a reactant is carried out using only thermal energy, a PEALD method in which a plasma-excited reactant is used, or the like can be used.

[0353] The CVD and ALD methods differ from sputtering methods in that particles emitted from a target or the like are deposited. Therefore, they are film formation methods that are less affected by the shape of the workpiece and have good step coverage. In particular, the ALD method has excellent step coverage and excellent film thickness uniformity, making it suitable for coating the surface of an opening with a high aspect ratio, for example. However, because the ALD method has a relatively slow film formation rate, it may be preferable to use it in combination with other film formation methods, such as the CVD method, which has a faster film formation rate.

[0354] Furthermore, the CVD method allows deposition of a film of any composition by adjusting the flow rate ratio of the source gases. For example, the CVD method allows deposition of a film with a continuously changing composition by changing the flow rate ratio of the source gases during deposition. When deposition is performed while changing the flow rate ratio of the source gases, the time required for deposition can be shortened compared to deposition using multiple deposition chambers because no time is required for transport or pressure adjustment. Therefore, the productivity of semiconductor devices can be improved in some cases.

[0355] In addition, in the ALD method, a film of any composition can be formed by simultaneously introducing multiple different precursors, or by controlling the number of cycles of each precursor when multiple different precursors are introduced.

[0356] Furthermore, thin films (insulating films, semiconductor films, conductive films, etc.) constituting the semiconductor device can be formed by a wet film formation method such as spin coating, dip coating, spray coating, inkjet printing, dispensing, screen printing, offset printing, doctor knife method, slit coating, roll coating, curtain coating, or knife coating.

[0357] Furthermore, when processing a thin film that constitutes a semiconductor device, for example, a photolithography method can be used. Alternatively, the thin film may be processed by a nanoimprint method, a sandblasting method, a lift-off method, or the like. Furthermore, an island-shaped thin film may be directly formed by a film formation method using a shielding mask such as a metal mask.

[0358] In this specification and the like, the term "island-like" refers to a state in which two or more layers made of the same material and formed in the same process are physically separated.

[0359] There are two typical photolithography methods: one is to form a resist mask on the thin film to be processed, process the thin film by, for example, etching, and then remove the resist mask; the other is to form a photosensitive thin film, and then process the thin film into the desired shape by exposure and development.

[0360] In photolithography, the light used for exposure may be, for example, i-line (wavelength 365 nm), g-line (wavelength 436 nm), h-line (wavelength 405 nm), or a mixture of these. Other light sources that can be used include ultraviolet light, KrF laser light, ArF laser light, etc. Exposure may also be performed by immersion exposure technology. Extreme ultraviolet (EUV) light or X-rays may also be used as the light used for exposure. An electron beam may also be used instead of the light used for exposure. Extreme ultraviolet light, X-rays, or an electron beam are preferred because they enable extremely fine processing. When exposure is performed by scanning a beam such as an electron beam, a photomask is not required.

[0361] The thin film can be etched by dry etching, wet etching, sandblasting, or the like.

[0362] An example of a method for manufacturing the semiconductor device shown in FIG. 1F will be described below.

[0363] First, as shown in FIG. 12A, an insulating layer 110 is formed on a substrate (not shown), a conductive layer 120a is formed on the insulating layer 110, a conductive layer 120b is formed on the conductive layer 120a, an insulating layer 180 is formed on the conductive layer 120b, a conductive layer 140a is formed on the insulating layer 180, and a conductive layer 140b is formed on the conductive layer 140a.

[0364] Note that after the insulating layer 180 is formed, planarization treatment is preferably performed to planarize the top surface of the insulating layer 180. As the planarization treatment, planarization treatment (also referred to as CMP treatment) using a chemical mechanical polishing (CMP) method is preferable. Alternatively, planarization treatment using etching (also referred to as etch-back treatment) may be performed. By performing the planarization treatment on the insulating layer 180, the surfaces on which the conductive layers 140a and 240b are to be formed can be flattened, and discontinuities in the conductive layers 140a and 140b can be suppressed. Note that the planarization treatment is not necessarily performed, and in that case, manufacturing costs can be reduced.

[0365] In this specification and the like, a step disconnection refers to a phenomenon in which a layer, a film, or an electrode is separated due to the shape of the surface on which it is formed (for example, a step).

[0366] 12B , openings 190 are formed in the conductive layer 140b, the conductive layer 140a, and the insulating layer 180 at positions that overlap the conductive layer 120b. At this time, recesses 191 are formed in the conductive layer 120b so as to overlap the openings 190. By forming the recesses 191 in the conductive layer 120b, the contact area with the semiconductor layer 130, which will be formed later, can be increased. Therefore, a decrease in the on-state current of the transistor 100 due to contact resistance between the conductive layer 120b and the semiconductor layer 130 can be suppressed. Furthermore, a gate electric field can be more easily applied to the channel formation region of the semiconductor layer 130, improving the electrical characteristics of the transistor 100.

[0367] To facilitate microfabrication and reduce the size of the transistor, it is preferable to use anisotropic etching to process a portion of the conductive layer 120b, a portion of the conductive layer 140a, a portion of the conductive layer 140b, and a portion of the insulating layer 180 when forming the opening 190. Dry etching is particularly preferable because it is suitable for microfabrication. The opening 190 may be formed under different processing conditions depending on the layer. Note that the slope of the side surface of the conductive layer 120b in the recess 191 and the slope of the side surfaces of the insulating layer 180, the conductive layer 140a, and the conductive layer 140b inside the opening 190 may differ depending on the materials and processing conditions of the conductive layer 120b, the conductive layer 140a, the conductive layer 140b, and the insulating layer 180.

[0368] Furthermore, for example, by the process of forming the opening 190, a region containing a halogen element may be provided on at least one of the top surface and side surface of the conductive layer 120b in the recess 191, the side surface of the insulating layer 180, the conductive layer 140a, and the conductive layer 140b in the opening 190, and the top surface of the conductive layer 140b. Examples of such a region include a region containing fluorine, a region containing chlorine, and a region containing fluorine and chlorine. For example, a halogen element derived from the etching gas used in the dry etching may remain in such a region.

[0369] Subsequently, heat treatment may be performed at a temperature of, for example, 250° C. to 650° C., preferably 300° C. to 500° C., and more preferably 320° C. to 450° C.

[0370] The heat treatment is performed in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more. For example, when the heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas concentration is preferably about 20%. The heat treatment may be performed under reduced pressure. Alternatively, after the heat treatment in the nitrogen gas or inert gas atmosphere, the heat treatment may be performed in an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more to compensate for the desorbed oxygen. By performing the above-described heat treatment, impurities such as water contained in the insulating layer 180 can be reduced before the semiconductor layer 130 is formed.

[0371] The gas used in the heat treatment is preferably highly purified. For example, the amount of moisture contained in the gas used in the heat treatment is preferably 1 ppb or less, more preferably 0.1 ppb or less, and even more preferably 0.05 ppb or less. By performing the heat treatment using a highly purified gas, for example, moisture can be prevented from being absorbed into the insulating layer 180 as much as possible.

[0372] 12C , the semiconductor layer 130 is formed to cover the opening 190. The semiconductor layer 130 is formed to be in contact with the upper surface of the conductive layer 140b. The semiconductor layer 130 is also formed to be in contact with the bottom and sidewall of the recess 191. Furthermore, the semiconductor layer 130 is formed inside the opening 190 to be in contact with the side surfaces of the insulating layer 180, the side surfaces of the conductive layer 140a, and the side surfaces of the conductive layer 140b.

[0373] The semiconductor layer 130 can be formed by, for example, sputtering, CVD, MBE, PLD, or ALD.

[0374] The semiconductor layer 130 is preferably formed as a film with as uniform a thickness as possible along the upper surface and side surfaces of the conductive layer 120b in the recess 191, the side surfaces of the insulating layer 180, the conductive layer 140a, and the conductive layer 140b in the opening 190, and the upper surface of the conductive layer 140b. Here, by forming the film using the ALD method, a thin film can be formed with good controllability. Therefore, it is preferable to form the semiconductor layer 130 using the ALD method.

[0375] Furthermore, when the semiconductor layer 130 has high crystallinity, diffusion of impurities in the semiconductor layer 130 is suppressed, so that the electrical characteristics of the transistor are less likely to fluctuate and reliability can be improved. Forming the semiconductor layer 130 by a sputtering method is preferable because it is easier to form a layer with high crystallinity than when an ALD method is used.

[0376] When the semiconductor layer 130 is formed by sputtering, oxygen or a mixed gas of oxygen and a noble gas is used as the sputtering gas. By increasing the proportion of oxygen contained in the sputtering gas, the amount of excess oxygen in the oxide film to be formed can be increased. When the oxide film is formed by sputtering, for example, an In-M-Zn oxide target can be used.

[0377] When the semiconductor layer 130 is formed by a sputtering method, an oxygen-excess oxide semiconductor is formed when the percentage of oxygen contained in the sputtering gas is set to more than 30% and less than or equal to 100%, preferably 70% to 100%. A transistor using an oxygen-excess oxide semiconductor for a channel formation region can have relatively high reliability. However, one embodiment of the present invention is not limited thereto. An oxygen-deficient oxide semiconductor is formed when the percentage of oxygen contained in the sputtering gas is set to 1% to 30%, preferably 5% to 20%. A transistor using an oxygen-deficient oxide semiconductor for a channel formation region can have relatively high field-effect mobility. Furthermore, the crystallinity of the oxide semiconductor layer can be improved by performing film formation while heating the substrate.

[0378] The semiconductor layer 130 preferably includes both a layer formed by an ALD method and a layer formed by a sputtering method. This allows the semiconductor layer 130 to be formed with good coverage and improve the crystallinity of the semiconductor layer 130. The semiconductor layer 130 preferably includes, for example, a layer formed by a sputtering method and a layer formed by an ALD method, stacked in this order. An oxide semiconductor layer formed by a sputtering method is likely to have crystallinity. Therefore, by providing a crystalline oxide semiconductor layer as a lower layer of the semiconductor layer 130, the crystallinity of the upper layer of the semiconductor layer 130 can be improved. Even if a pinhole or a discontinuity is formed in the oxide semiconductor layer formed by the sputtering method, the pinhole or the discontinuity can be blocked with the oxide semiconductor layer formed by the ALD method, which has good coverage.

[0379] Specifically, the semiconductor layer 130 can be a two-layer structure in which a layer formed by sputtering and a layer formed by ALD are stacked in this order; a two-layer structure in which a layer formed by ALD and a layer formed by sputtering are stacked in this order; a three-layer structure in which a layer formed by ALD, a layer formed by sputtering, and a layer formed by ALD are stacked in this order; or a three-layer structure in which a layer formed by sputtering, a layer formed by ALD, and a layer formed by sputtering are stacked in this order.

[0380] Next, heat treatment is preferably performed. The heat treatment is preferably performed within a temperature range in which the semiconductor layer 130 does not become polycrystallized. The temperature of the heat treatment is preferably 100° C. or higher and 650° C. or lower, more preferably 250° C. or higher and 600° C. or lower, and further preferably 350° C. or higher and 550° C. or lower. The above description can be referred to for details of the heat treatment.

[0381] In addition, it is preferable that the gas used in the heat treatment be highly purified. By performing the heat treatment using a highly purified gas, for example, moisture can be prevented from being taken into the semiconductor layer 130 as much as possible.

[0382] In this embodiment, the heat treatment is performed at a temperature of 450° C. for one hour with a flow rate ratio of nitrogen gas to oxygen gas of 4:1. This heat treatment using oxygen gas can reduce impurities such as carbon, water, and hydrogen in the semiconductor layer 130. Reducing the impurities in the film in this manner can improve the crystallinity of the semiconductor layer 130, resulting in a denser and more compact structure. This increases the crystalline region in the semiconductor layer 130, reducing in-plane variations in the crystalline region in the semiconductor layer 130. Therefore, in-plane variations in the electrical characteristics of the transistor can be reduced.

[0383] In addition, in the case where the insulating layer 180 contains oxygen, oxygen is preferably supplied from the insulating layer 180 to the channel formation region of the semiconductor layer 130 by heat treatment. This can reduce oxygen vacancies and VoH.

[0384] In this manner, oxygen (also referred to as excess oxygen) released by heating from an insulating layer in contact with the semiconductor layer 130 or an insulating layer located near the semiconductor layer 130 may be supplied to the semiconductor layer 130. The excess oxygen has a function of trapping electrons, which makes it easier for negative charges to be formed. Therefore, the threshold voltage of the transistor is shifted in the positive direction, making it possible to realize a normally-off transistor.

[0385] 12D , the semiconductor layer 130, the conductive layer 140a, and the conductive layer 140b are processed into island shapes to expose a portion of the top surface of the insulating layer 180. The semiconductor layer 130, the conductive layer 140a, and the conductive layer 140b can be processed using the same mask. This is preferable because it allows the number of masks required to manufacture a semiconductor device to be reduced compared to, for example, a case in which the semiconductor layer 130, and the conductive layer 140a and the conductive layer 140b are processed using different masks.

[0386] 12E, the insulating layer 150 is formed to have a region located on the conductive layer 140b and a region located on the semiconductor layer 130 inside the opening 190. Then, a conductive layer 220a is formed on the insulating layer 150, and a conductive layer 220b is formed on the conductive layer 220a. The insulating layer 150 is formed to cover the semiconductor layer 130, the conductive layer 140a, and the conductive layer 140b. Specifically, the insulating layer 150 may be formed in contact with the semiconductor layer 130, the insulating layer 180, the conductive layer 140a, and the conductive layer 140b.

[0387] The insulating layer 150 is formed along the semiconductor layer 130 covering the sidewall of the opening 190, which has a high aspect ratio. Therefore, it is preferable to use a film formation method with good coverage for forming the insulating layer 150. For example, the ALD method is preferably used for forming the insulating layer 150. Furthermore, the conductive layer 220a is formed so as to fill at least a portion of the recess of the insulating layer 150. Therefore, it is preferable to use a film formation method with good embedding properties for forming the conductive layer 220a. For example, it is preferable to use a CVD method for forming the conductive layer 220a. Furthermore, the conductive layer 220a can have a stacked structure of, for example, a layer formed using the ALD method, which has good coverage properties, and a layer formed using the CVD method, which has good embedding properties. The conductive layer 220b can be formed using the same method as the method that can be used for forming the conductive layer 220a. The conductive layer 220b can be formed using, for example, the CVD method.

[0388] The upper surface of the conductive layer 220a may be subjected to planarization treatment. For example, after the conductive layer 220a is formed and subjected to planarization treatment, the conductive layer 220a can be processed by, for example, an etching method. CMP treatment is suitable as the planarization treatment. Note that the upper surface of the conductive layer 220b may also be subjected to planarization treatment.

[0389] The conductive layer 220a is formed to have a region facing the semiconductor layer 130 within the opening 190 with the insulating layer 150 sandwiched therebetween. The conductive layer 220a and the conductive layer 220b are also formed to have regions overlapping with the conductive layer 140a and the conductive layer 140b with the insulating layer 150 interposed therebetween. As described above, the wider the region where the conductive layer 140 and the conductive layer 220 overlap with each other with the insulating layer 150 interposed therebetween, the longer data can be retained in the memory cell 10. Note that FIG. 12E shows an example in which part of the side surface of the conductive layer 140a and part of the side surface of the conductive layer 140b are covered with the conductive layer 220a with the insulating layer 150 interposed therebetween.

[0390] 12F , an insulating layer 280 is formed on the conductive layer 220b and the insulating layer 150, a conductive layer 240a is formed on the insulating layer 280, and a conductive layer 240b is formed on the conductive layer 240a. After that, openings 290 are formed in the conductive layers 240b, 240a, and the insulating layer 280 at positions that overlap with the conductive layer 220b. At this time, recesses 291 are formed in the conductive layer 220b so as to overlap with the openings 290. For the formation of the insulating layer 280, the conductive layers 240a, 240b, the openings 290, and the recesses 291, refer to the descriptions of the formation of the insulating layer 180, the conductive layers 140a, 140b, the openings 190, and the recesses 191, respectively.

[0391] The opening 290 is formed at a position where at least a portion thereof overlaps with the opening 190. As described above, the recess 191 is formed at a position where the recess 191 overlaps with the opening 190. As a result, the recess 191, the opening 190, the recess 291, and the opening 290 at least partially overlap with one another. This allows the area occupied by the memory cell 10 to be smaller than when, for example, the opening 190 and the opening 290 do not overlap. This makes it possible to manufacture a semiconductor device that can be miniaturized or highly integrated. Furthermore, it is possible to manufacture a semiconductor device with a large memory capacity per unit area.

[0392] 13A , a semiconductor layer 230 is formed to cover the opening 290. The semiconductor layer 230 is formed to be in contact with the upper surface of the conductive layer 240b. The semiconductor layer 230 is also formed to be in contact with the bottom and sidewall of the recess 291. Furthermore, the semiconductor layer 230 is formed inside the opening 290 to be in contact with the side surfaces of the insulating layer 280, the side surfaces of the conductive layer 240a, and the side surfaces of the conductive layer 240b. For the formation of the semiconductor layer 230, the above description of the formation of the semiconductor layer 130 can be referred to.

[0393] 13B , a sacrificial layer 262 is formed to cover the conductive layer 240 a, the conductive layer 240 b, and the semiconductor layer 230. The sacrificial layer 262 is formed so that at least a portion thereof is located inside the opening 290. A spin-on-carbon (SOC) film and a spin-on-glass (SOG) film are suitable for the sacrificial layer 262. The sacrificial layer 262 preferably has a two-layer structure, for example, an SOC film and an SOG film on the SOC film.

[0394] Next, as shown in FIG. 13C , a portion of the sacrificial layer 262 is removed. A gate insulating layer and a gate electrode (insulating layer 250 and conductive layer 260) will be provided in the remaining region of the sacrificial layer 262 in a later process. Therefore, it is preferable that the sacrificial layer 262 has a small area that overlaps with the upper surface of the conductive layer 240b, or does not overlap with the upper surface of the conductive layer 240b. This allows fabrication of a semiconductor device with low parasitic capacitance between the conductive layer 240b and the conductive layer 260. In a cross-sectional view, it is preferable that the width of the sacrificial layer 262 does not exceed the sum of the width D of the opening 290 and twice the film thickness of the insulating layer 250 to be formed later. FIG. 13C shows an example in which the width of the sacrificial layer 262 is the width D of the opening 290.

[0395] Subsequently, as shown in FIG. 13D, an insulating layer 283 is formed to cover the insulating layer 280, the conductive layer 240a, the conductive layer 240b, the semiconductor layer 230, and the sacrificial layer 262, and an insulating layer 285 is formed on the insulating layer 283.

[0396] By increasing the thickness of the insulating layer 285, the distance between the conductive layer 240b and the gate wiring (the conductive layer 260 or the conductive layer 265) can be increased, and the parasitic capacitance between the conductive layer 240b and the gate wiring can be reduced. Specifically, by making the thickness of the insulating layer 285 thicker than the thickness of the insulating layer 150, the parasitic capacitance between the conductive layer 240b and the conductive layer 265 formed in a later step can be made smaller than the capacitance Cp between the conductive layer 140b and the conductive layer 220.

[0397] For example, the insulating layer 285 is preferably formed using a silicon oxide film by sputtering.

[0398] If the insulating layer 283 is not provided, the sacrificial layer 262 is exposed to oxygen-containing plasma when a silicon oxide film is formed as the insulating layer 285 by sputtering. Therefore, part or all of the sacrificial layer 262 may be etched. As described above, depending on the method for forming the insulating layer 285, the shape of the sacrificial layer 262 may be reduced or the sacrificial layer 262 may be lost. For this reason, it is preferable that the insulating layer formed on the sacrificial layer 262 has a stacked structure of the insulating layer 283 and the insulating layer 285, rather than a single layer of the insulating layer 285. This provides advantages such as a wider range of materials for the sacrificial layer 262 and the insulating layer 285, and a reduced difficulty in manufacturing a semiconductor device.

[0399] When an oxide film is used for the insulating layer 283, it is preferable to form the insulating layer 283 by a method other than a sputtering method, for example, an ALD method. For example, it is preferable to form an aluminum oxide film, a hafnium oxide film, or a nitride film (such as a silicon nitride film) by an ALD method as the insulating layer 283. This can prevent the sacrificial layer 262 from being unintentionally processed when the insulating layer 283 is formed.

[0400] 14A , a planarization process is performed on the insulating layer 285 and the sacrificial layer 262. This exposes the upper surface of the sacrificial layer 262, and the upper surfaces of the sacrificial layer 262, the insulating layer 283, and the insulating layer 285 are planarized. CMP is a suitable planarization process. In the planarization process, at least a portion of the insulating layer 283 and the insulating layer 285 is removed. Furthermore, a portion of the sacrificial layer 262 may be removed.

[0401] Next, as shown in Fig. 14B , sacrificial layer 262 is removed. There is no particular limit to the method for removing sacrificial layer 262. Here, as shown in Fig. 14B , it can be said that opening 270 having a region overlapping opening 290 is formed in insulating layer 285. It can also be said that opening 270 having a region overlapping opening 290 is formed in insulating layer 283.

[0402] 14C , an insulating layer 250 is formed to cover the openings 270 and 290, and a conductive layer 260 is formed over the insulating layer 250. The insulating layer 250 is provided in contact with the semiconductor layer 230, the insulating layer 283, and the insulating layer 285.

[0403] The insulating layer 250 and the conductive layer 260 are formed inside the openings 290 and 270, respectively, which have a large aspect ratio. Therefore, it is preferable to use a film formation method with good coverage or embedding properties for forming the insulating layer 250 and the conductive layer 260, such as an ALD method or a CVD method. For example, it is preferable to use an ALD method for forming the insulating layer 250. It is also preferable to use a CVD method for forming the conductive layer 260. For example, when the conductive layer 260 has a stacked structure, it is preferable to use a CVD method for forming at least one layer.

[0404] 14D , the conductive layer 260 is subjected to planarization treatment to expose the upper surfaces of the insulating layer 283 and the insulating layer 285, and the upper surfaces of the conductive layer 260, the insulating layer 250, the insulating layer 283, and the insulating layer 285 are planarized. CMP treatment is suitable as the planarization treatment. In the planarization treatment, at least the regions of the conductive layer 260 and the insulating layer 250 that overlap with the upper surface of the insulating layer 285 are removed. This makes it possible to remove the region of the conductive layer 260 that overlaps with the upper surface of the conductive layer 240b. This makes it possible to suppress the occurrence of parasitic capacitance between the conductive layer 260 and the conductive layer 240b.

[0405] By using CMP treatment to remove the region of the conductive layer 260 that overlaps with the top surface of the conductive layer 240b, an increase in the number of masks can be suppressed compared to the case of using dry etching, for example.

[0406] 14D , it is preferable that the height of the upper surface of insulating layer 285 and the height of the upper surface of conductive layer 260 are the same. Alternatively, one of the height of the upper surface of insulating layer 285 and the height of the upper surface of conductive layer 260 may be higher than the other. The height relationship between the upper surfaces of the two layers can be controlled by the difference in polishing rate between the materials of insulating layer 285 and conductive layer 260.

[0407] 1F , a conductive layer 265 is formed on the insulating layer 285, the insulating layer 283, the insulating layer 250, and the conductive layer 260. The conductive layer 265 is formed so as to be in contact with the upper surface of the conductive layer 260. The conductive layer 265 can also be formed so as to be in contact with the upper surfaces of the insulating layer 285, the insulating layer 283, and the insulating layer 250.

[0408] The insulating layer 283 and the insulating layer 285 are located between the conductive layer 265 and the conductive layer 240b. This allows the parasitic capacitance between the conductive layer 240 and the conductive layer 260 to be smaller than the capacitance Cp between the conductive layer 140 and the conductive layer 220.

[0409] Through the above steps, a semiconductor device of one embodiment of the present invention can be manufactured.

[0410] [Addition of Element] As described above, the insulating layer 180 and the insulating layer 280 may each be provided with a region containing a halogen element. The semiconductor layer 130 and the semiconductor layer 230 may each be provided with a region containing a halogen element. The semiconductor layer 130 and the semiconductor layer 230 may each be provided with a region containing the first element. At least one of the conductive layer 120a, the conductive layer 120b, the conductive layer 140a, the conductive layer 140b, the conductive layer 220a, the conductive layer 220b, the conductive layer 240a, and the conductive layer 240b may be provided with a region containing the first element. An example in which a region containing a halogen element is provided in the insulating layer 180 or the semiconductor layer 130, and an example in which a region containing the first element is provided in at least one of the semiconductor layer 130, the conductive layer 120a, the conductive layer 120b, the conductive layer 140a, and the conductive layer 140b will be described below. Note that the following description can be applied even when a halogen element or the first element described above is supplied to these layers by, for example, replacing the insulating layer 180, the semiconductor layer 130, the conductive layer 120a, the conductive layer 120b, the conductive layer 140a, and the conductive layer 140b with the insulating layer 280, the semiconductor layer 230, the conductive layer 220a, the conductive layer 220b, the conductive layer 240a, and the conductive layer 240b, respectively.

[0411] 15A, after the structure shown in FIG. 12B is formed, halogen elements 188 are supplied to the side surfaces of the openings 190 in the insulating layer 180. The region of the insulating layer 180 to which the halogen elements 188 are supplied is shown as region 180i. Region 180i includes at least the side surfaces of the openings 190 in the insulating layer 180. Note that the halogen elements 188 may also be supplied to one or more of the conductive layers 140a, 140b, 120a, and 120b.

[0412] 15A shows an example in which the sidewall of the opening 190 is perpendicular to the top surface of the substrate. In the semiconductor device of one embodiment of the present invention, the sidewall of the opening 190 is perpendicular or approximately perpendicular to the top surface of the substrate, or has a tapered shape. Therefore, when the halogen element 188 is added perpendicular or approximately perpendicular to the top surface of the substrate, it may be difficult to supply the halogen element 188 uniformly to a desired region.

[0413] Therefore, as shown in Figure 15A, it is preferable to add the halogen element 188 from a direction tilted by more than 0 degrees and less than 90 degrees with respect to the upper surface of the substrate. Figure 15A shows an example in which the halogen element 188 is added while tilted at an angle θ188 with respect to the upper surface of the insulating layer 110. The angle θ188 is preferably more than 0 degrees and less than 90 degrees, and is preferably 15 degrees or more and 80 degrees or less. This makes it easy to supply the halogen element to the side surface of the opening 190 of the insulating layer 180. Furthermore, it is not limited to addition from one direction, but it is preferable to supply the halogen element 188 stepwise by changing the angle, which allows the halogen element 188 to be supplied more uniformly to the desired region.

[0414] The elements that can be used for the halogen element 188 are as described above.

[0415] The plasma ion doping method or the ion implantation method can be suitably used to supply the halogen element 188. These methods can control the concentration profile in the depth direction with high precision by adjusting the ion acceleration voltage, dose, etc.

[0416] It should be noted that the angle θ188 can be set within the above range by tilting, for example, one or both of the substrate to be processed and the ion irradiation unit in the apparatus.

[0417] The purity of the supplied halogen element 188 can be increased by using an ion implantation method in which a source gas is ionized and the ions are mass-separated and added. The region 180i is a region in contact with the channel formation region of the semiconductor layer 130. Therefore, if other impurity elements are also supplied to the region 180i when the halogen element 188 is supplied, the impurity elements may diffuse into the channel formation region of the semiconductor layer 130, affecting the characteristics and reliability of the transistor. Therefore, it is preferable to use the ion implantation method to supply the halogen element 188 with high purity to the region 180i.

[0418] Furthermore, by using a plasma ion doping method in which a source gas is ionized and the ions are added without mass separation, productivity can be improved.

[0419] The ion implantation equipment or ion doping equipment used to supply halogen element 188 is also used in the manufacture of Si transistors such as LTPS transistors, so that the equipment in the existing LTPS manufacturing line can be used, which is preferable because no new capital investment is required, thereby reducing the capital investment costs involved in the manufacture of semiconductor devices.

[0420] The source gas of the halogen element 188 can be a gas containing the halogen element described above. As the gas, either a gas of a simple halogen or a halide gas can be used. When fluorine is supplied, typically, F 2 Gas, BF 3 Gas, C 4 F 6 Gas, C 5 F 6 Gas, C 4 F 8 Gas, CF 4 Gas, SF 6 Gas, CHF 3 Gas, CH 2 F 2 Gas or CH 3F gas or the like can be used. When chlorine is supplied, Cl 2 Gas, BCl 3 Gas, SiCl 4 Gas, CCl 4 A gas can be used. A mixed gas obtained by diluting these source gases with hydrogen or a noble gas can also be used. The ion source is not limited to a gas, and a solid or liquid can also be heated and vaporized.

[0421] The supply of the halogen element 188 can be controlled by setting conditions such as acceleration voltage and dose amount, taking into consideration the composition, density, film thickness, etc. of the insulating layer 180 .

[0422] The method for supplying the halogen element 188 is not limited, and may be, for example, plasma treatment or treatment utilizing thermal diffusion by heating. In the case of plasma treatment, the impurity element can be supplied by generating plasma in a gas atmosphere containing the halogen element to be supplied and performing plasma treatment. As an apparatus for generating the plasma, a dry etching apparatus, an ashing apparatus, a plasma CVD apparatus, a high-density plasma CVD apparatus, or the like may be used.

[0423] The supplying step of the halogen element 188 may be performed while heating the substrate. This makes it possible to repair damage to the insulating layer 180 that occurs when the halogen element 188 is added. That is, the addition of the halogen element 188 to the insulating layer 180 and the repair of the damage caused by the addition can be performed in parallel.

[0424] The substrate temperature in the supplying step of halogen element 188 is preferably 150°C or higher and lower than the strain point of the substrate, more preferably 200°C or higher and 500°C or lower, even more preferably 200°C or higher and 450°C or lower, even more preferably 250°C or higher and 400°C or lower, even more preferably 250°C or higher and 350°C or lower, or even more preferably 300°C or higher and 400°C or lower, even more preferably 300°C or higher and 350°C or lower.

[0425] Thereafter, by forming the semiconductor layer 130 while heating the substrate, the halogen element may be supplied from the region 180i to the semiconductor layer 130. Furthermore, during heat treatment performed after the formation of the semiconductor layer 130, the halogen element may be supplied from the region 180i to the semiconductor layer 130.

[0426] As described above, in the semiconductor device of one embodiment of the present invention, the halogen element 188 is added to the insulating layer 180 and then supplied from the insulating layer 180 to the semiconductor layer 130. This makes it possible to prevent damage to the channel formation region of the semiconductor layer 130 due to the addition of the element, to prevent the crystallinity of the channel formation region from being reduced due to the addition of the element, and so on. Therefore, the reliability of the transistor can be improved.

[0427] 15B , after the structure shown in FIG. 12C is formed, the halogen element 188 may be supplied to the side surface of the semiconductor layer 130 located inside the opening 190. The region of the semiconductor layer 130 to which the halogen element 188 is supplied is shown as region 130i. Region 130i includes at least the side surface of the semiconductor layer 130 located inside the opening 190. Note that the halogen element 188 may also be supplied to one or more of the insulating layer 180, the conductive layer 140a, the conductive layer 140b, the conductive layer 120a, and the conductive layer 120b.

[0428] 15C , for example, after the structure shown in FIG. 12B is formed, the impurity element 189 is supplied to the top surface of the conductive layer 120b and the top surface of the conductive layer 140b. A region in the conductive layer 120b to which the impurity element 189 is supplied is denoted by 220n. Similarly, a region in the conductive layer 140b to which the impurity element 189 is supplied is denoted by 140n.

[0429] After that, the semiconductor layer 130 is formed and subjected to, for example, heat treatment, whereby the impurity element 189 can be supplied from the region 120n and the region 140n to the source region and the drain region of the semiconductor layer 130.

[0430] By supplying the impurity element 189 to the semiconductor layer 130 through the conductive layer 120 or the conductive layer 140, a decrease in the crystallinity of the semiconductor layer 130 can be suppressed compared to the case where the impurity element 189 is directly added to the semiconductor layer 130. Therefore, an increase in electrical resistance due to a decrease in crystallinity can be suppressed.

[0431] 15D, after the structure shown in Fig. 12C is formed, the impurity element 189 may be supplied to the semiconductor layer 130. In the semiconductor layer 130, a region to which the impurity element 189 is supplied is shown as a region 130n.

[0432] By adding the impurity element 189 to the semiconductor layer 130, the sheet resistance of the semiconductor layer 130, the contact resistance between the semiconductor layer 130 and the conductive layer 120, and the contact resistance between the semiconductor layer 130 and the conductive layer 140 can be reduced.

[0433] By directly adding the impurity element 189 to the semiconductor layer 130 and then forming the insulating layer 150 over the semiconductor layer 130 , damage to the insulating layer 150 due to the addition of the impurity element 189 can be suppressed.

[0434] The impurity element 189 is preferably added from a direction perpendicular or substantially perpendicular to the top surface of the substrate. In this case, the amount of the impurity element added to a surface of the semiconductor layer 130 that is inclined with respect to the top surface of the substrate or a surface that is perpendicular or substantially perpendicular to the top surface of the substrate is smaller than that to a surface that is parallel or substantially parallel to the top surface of the substrate. That is, the amount of the impurity element added to the source and drain regions of the semiconductor layer 130 is larger than that to the channel formation region. Therefore, the resistance of the source and drain regions can be preferentially reduced.

[0435] FIG. 15D shows an example in which regions 130n are formed at and near the interface between the semiconductor layer 130 and the upper surface of the conductive layer 120b, and at and near the interface between the semiconductor layer 130 and the upper surface of the conductive layer 140b.

[0436] The elements that can be used as the impurity element 189 are as described above.

[0437] The plasma ion doping method or the ion implantation method can be suitably used to supply the impurity element 189. These methods can control the concentration profile in the depth direction with high precision by adjusting the ion acceleration voltage, dose amount, etc.

[0438] The purity of the supplied impurity element can be increased by using an ion implantation method in which a source gas is ionized and the ions are mass-separated and added. When the ion implantation method is used, the first element described above is preferably used as the impurity element 189, and boron or phosphorus is more preferably used. By using an element that bonds with oxygen to stabilize the impurity element 189, a stable region 130n with low electrical resistance can be realized.

[0439] Furthermore, productivity can be improved by using a plasma ion doping method in which a source gas is ionized and the ions are added without mass separation. When using the plasma ion doping method, it is preferable to use both the first element and hydrogen as the impurity element 189, and it is more preferable to use both boron or phosphorus and hydrogen. By using both an element that bonds with oxygen to stabilize the impurity element 189 and hydrogen as the impurity element 189, the electrical resistance of the region 130n can be easily reduced and the low electrical resistance can be stably maintained.

[0440] The ion implantation equipment or ion doping equipment used to supply the impurity element 189 is also used in the manufacture of Si transistors such as LTPS transistors, so that the equipment in the existing LTPS manufacturing line can be used, which is preferable because no new capital investment is required, thereby reducing the capital investment costs involved in the manufacture of semiconductor devices.

[0441] In the supplying treatment of the impurity element 189, the treatment conditions are preferably controlled so that the concentration of the impurity element in a region of the semiconductor layer 130 that overlaps with the top surface of the conductive layer 120b or the top surface of the conductive layer 140b is higher than the concentration of the impurity element in other regions. This allows the impurity element 189 at an optimum concentration to be supplied to the source and drain regions of the semiconductor layer 130.

[0442] As a source gas of the impurity element 189, a gas containing the above-mentioned impurity element can be used. 2 H 6 Gas or BF 3 In addition, when phosphorus is supplied, a typical example is a PH 3 A mixed gas obtained by diluting these source gases with hydrogen or a noble gas may also be used.

[0443] Other raw material gases include CH 4 , N 2 , N.H. 3 , AlH 3 , AlCl 3 , SiH 4 , Si 2 H 6 , F 2 , H.F., H. 2 , (C 5 H 5 ) 2 Mg, noble gases, etc. can be used. The ion source is not limited to gas, and a solid or liquid may be heated and vaporized.

[0444] For example, it is preferable to use a gas containing boron and hydrogen to supply boron and hydrogen as the impurity element 189. In this case, the impurity element 189 can be added without mass separation, and the resistance of the semiconductor layer 130 can be easily reduced, which is preferable because it is possible to improve both the productivity and characteristics of the semiconductor device.

[0445] Furthermore, it is preferable to use the same source gas in the supplying step of the halogen element 188 and the supplying step of the impurity element 189, since this can reduce manufacturing costs. 3 By ionizing the gas and mass-separating the ions, fluorine can be supplied as the halogen element 188, and boron can be supplied as the impurity element 189.

[0446] The supply of the impurity element 189 can be controlled by setting conditions such as acceleration voltage and dose amount in consideration of the composition, density, film thickness, and the like of the semiconductor layer 130 .

[0447] The method for supplying the impurity element 189 is not limited, and may be, for example, plasma treatment or treatment using thermal diffusion by heating. In the case of plasma treatment, the impurity element can be supplied by generating plasma in a gas atmosphere containing the impurity element to be supplied and performing plasma treatment. As an apparatus for generating the plasma, a dry etching apparatus, an ashing apparatus, a plasma CVD apparatus, a high-density plasma CVD apparatus, or the like may be used.

[0448] Furthermore, the step of supplying the impurity element 189 is preferably performed while heating the substrate. This makes it possible to repair damage to the semiconductor layer 130 that occurs when the impurity element 189 is added. That is, the addition of the impurity element 189 to the semiconductor layer 130 and the repair of damage caused by the addition can be performed in parallel.

[0449] The substrate temperature in the supplying step of the impurity element 189 is preferably 150°C or higher and lower than the strain point of the substrate, more preferably 200°C or higher and 500°C or lower, even more preferably 200°C or higher and 450°C or lower, even more preferably 250°C or higher and 400°C or lower, even more preferably 250°C or higher and 350°C or lower, or even more preferably 300°C or higher and 400°C or lower, even more preferably 300°C or higher and 350°C or lower.

[0450] Heat treatment may be performed after supplying the impurity element 189. By performing the heat treatment, damage to the semiconductor layer 130 that occurs in the step of supplying the impurity element 189 can be repaired.

[0451] By using an element that bonds with oxygen to stabilize the impurity element 189, it is possible to prevent the impurity element 189 from being detached due to heat applied during, for example, a manufacturing process of a semiconductor device. Therefore, even if heat treatment is performed or a film formation process is performed while the substrate is heated after the impurity element 189 is added, the region 130 n can maintain a low electrical resistance.

[0452] 15E, the impurity element 189 may be added to the semiconductor layer 130 through the insulating layer 150. At this time, the impurity element 189 may also be supplied to the insulating layer 150. It is preferable that the region 130 n has a region with a higher concentration of the impurity element 189 than the insulating layer 150, because this can further reduce the electrical resistance of the region 130 n.

[0453] By supplying the impurity element 189 to the semiconductor layer 130 through the insulating layer 150, a decrease in the crystallinity of the semiconductor layer 130 can be suppressed compared to the case where the impurity element 189 is directly added to the semiconductor layer 130. Therefore, an increase in electrical resistance due to a decrease in crystallinity can be suppressed.

[0454] Furthermore, if the insulating layer 150 is formed after the impurity element 189 is added, the inside of a deposition chamber for the insulating layer 150 may be contaminated. For this reason, it is preferable to add the impurity element 189 after the insulating layer 150 is formed.

[0455] Here, the film thickness of the insulating layer 150 in the direction in which the impurity element 189 is added is thicker in a region provided along the side surface of the insulating layer 180 than in a region provided along the top surface of the conductive layer 120b or the top surface of the conductive layer 140b. As a result, the amount of the impurity element 189 added is larger in a region of the semiconductor layer 130 provided along the top surface of the conductive layer 120b or the top surface of the conductive layer 140b than in a region provided along the side surface of the insulating layer 180. In this way, the impurity element 189 can be prevented from entering the channel formation region of the semiconductor layer 130, and the resistance of the source region and the drain region can be preferentially reduced.

[0456] As described above, the semiconductor device of one embodiment of the present invention has a structure in which a gate electric field is easily applied to the semiconductor layer. Therefore, the electrical characteristics of the transistor can be improved. Furthermore, the semiconductor device of one embodiment of the present invention has a structure in which data can be retained without providing a capacitor. Therefore, a low-cost semiconductor device can be provided.

[0457] This embodiment mode can be combined with other embodiment modes as appropriate. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be combined as appropriate.

[0458] Embodiment 2 In this embodiment, a memory device according to one embodiment of the present invention will be described with reference to drawings. Specifically, the memory device including the memory cell described in the previous embodiment will be described with reference to drawings.

[0459] A memory cell array can be configured by arranging the memory cells 10 in a three-dimensional matrix.

[0460] 16A is a plan view of a memory device, showing an example in which 2×2 memory cells 10 (memory cells 10a to 10d) are arranged in the X and Y directions.

[0461] Fig. 16B is a cross-sectional view taken along dashed line B1-B2 in Fig. 16A. In Fig. 16A and Fig. 16B, two memory cells are connected to a common wiring (conductive layer 145 and conductive layer 245).

[0462] 16A and 16B, conductive layers 140 and 265 are provided in memory cells 10a and 10b, respectively. Also, as shown in FIG. 16A, one conductive layer 140 and one conductive layer 265 are provided in common to memory cells 10a and 10c. That is, conductive layer 140 contacts semiconductor layer 130 of memory cell 10a and semiconductor layer 130 of memory cell 10c. Furthermore, another conductive layer 140 and conductive layer 265 are provided in common to memory cells 10b and 10d.

[0463] One conductive layer 240 is provided in common to the memory cell 10a and the memory cell 10b. That is, the conductive layer 240 contacts the semiconductor layer 230 of the memory cell 10a and the semiconductor layer 230 of the memory cell 10b. Another conductive layer 240 is provided in common to the memory cell 10c and the memory cell 10d.

[0464] 16A and 16B includes an insulating layer 287 located over the conductive layer 265 and the insulating layer 283. The memory device illustrated in FIGS. 16A and 16B also includes a conductive layer 145 and a conductive layer 245 electrically connected to the memory cell 10a and the memory cell 10b and functioning as plugs (which can also be referred to as connection electrodes). The conductive layer 145 is disposed inside openings formed in the insulating layer 110, the insulating layer 180, the insulating layer 150, and the insulating layer 280, and is in contact with the bottom surface of the conductive layer 240a. The conductive layer 245 is disposed inside openings formed in the insulating layer 287, the insulating layer 285, the insulating layer 283, and the semiconductor layer 230, and is in contact with the top surface of the conductive layer 240b. The conductive layer 145 and the conductive layer 245 can be formed using a conductive material or the like that can be used for the conductive layer 140 and the conductive layer 240.

[0465] The conductive layer 245 can be in contact with the top surface of the conductive layer 240a. Alternatively, the conductive layer 245 can be in contact with the top surface of the semiconductor layer 230. That is, the conductive layer 240b may have an opening at a position overlapping with the conductive layer 245. The semiconductor layer 230 does not need to have an opening at a position overlapping with the conductive layer 245. As a connection portion between the memory cell and the plug, it is preferable that a layer having low contact resistance with the conductive layer 245, among the layers constituting the conductive layer 240 and the semiconductor layer 230, be in contact with the conductive layer 245.

[0466] Similarly, the conductive layer 145 can be in contact with a bottom surface of the conductive layer 240b or a bottom surface of the semiconductor layer 230. That is, the conductive layer 240a may have an opening at a position overlapping with the conductive layer 245. Of the layers constituting the conductive layer 240 and the semiconductor layer 230, a layer having low contact resistance with the conductive layer 145 is preferably in contact with the conductive layer 145.

[0467] Furthermore, among the layers constituting the conductive layer 240 and the semiconductor layer 230 , a layer having low wiring resistance is preferably in contact with the conductive layer 145 and the conductive layer 245 .

[0468] The insulating layer 287 preferably has a low relative dielectric constant because it functions as an interlayer film. By using a material with a low relative dielectric constant as the interlayer film, parasitic capacitance occurring between wirings can be reduced.

[0469] The concentration of impurities such as water and hydrogen in the insulating layer 287 is preferably reduced. This can prevent impurities such as water and hydrogen from entering the channel formation region of the semiconductor layer 230.

[0470] The conductive layer 145 and the conductive layer 245 function as plugs or wirings for electrically connecting circuit elements, wirings, electrodes, or terminals, such as switches, transistors, capacitors, inductors, resistors, and diodes, to the memory cells 10a and 10b. For example, the conductive layer 145 can be electrically connected to a sense amplifier (not shown) provided below the memory device shown in FIG. 16B , and the conductive layer 245 can be electrically connected to a similar memory device (not shown) provided above the memory device shown in FIG. 16B . In this case, the conductive layer 145 and the conductive layer 245 function as part of the wiring 23 described in the previous embodiment. In this way, by providing a memory device or the like above or below the memory device shown in FIG. 16B , the memory capacity per unit area can be increased.

[0471] The memory cell 10a and the memory cell 10b are configured in line symmetry with respect to the perpendicular bisector C1-C2 of the dashed-dotted line B1-B2 shown in FIG. 16A . The memory cell 10a and the memory cell 10b are also configured in line symmetry with respect to the perpendicular bisector C3-C4 of the dashed-dotted line B1-B2 shown in FIG. 16B . As described above, the transistors 200a and 200b are also arranged symmetrically with respect to the conductive layers 145 and 245. Here, the conductive layer 240 functions as the other of the source and drain electrodes of the transistor 200a and the other of the source and drain electrodes of the transistor 200b. The transistors 200a and 200b share the conductive layers 145 and 245, which function as plugs. By configuring the connections between the two transistors and the plugs as described above, a memory device capable of miniaturization and high integration can be provided. The transistor 100a and the transistor 100b are also arranged symmetrically with the conductive layer 145 and the conductive layer 245 sandwiched therebetween.

[0472] The conductive layer 120 may be provided in each of the memory cells 10 a and 10 b, or may be provided in common to the memory cells 10 a and 10 b. However, as shown in FIG. 16B , the conductive layer 120 is provided at a distance from the conductive layer 145 to prevent a short circuit between the conductive layer 120 and the conductive layer 145.

[0473] 17 shows an example in which the four memory cells shown in FIG. 16A are stacked in n layers (n is an integer of 3 or more) in the Z direction. FIG. 17 is a cross-sectional view taken along dashed line B1-B2 shown in FIG. 16A.

[0474] The memory device shown in FIG. 17 has n memory layers 60. Specifically, a memory layer 60[2] is provided on memory layer 60[1], and (n-2) memory layers are further provided on memory layer 60[2], with memory layer 60[n] provided at the top. The number of memory cells included in one memory layer 60 is not particularly limited, and two or more memory cells may be included. The memory cells included in the n memory layers 60 are electrically connected to a sense amplifier (not shown) provided below the n memory layers 60 by conductive layers 145, 245, 247, 248, etc.

[0475] 17 shows an example in which the conductive layer 145 is in contact with the bottom surface of the conductive layer 240, and the conductive layer 245 is in contact with the top surface of the semiconductor layer 230. As described above, various modes are possible for the connection points between the plugs such as the conductive layer 145 and the conductive layer 245 and each memory cell, and are not limited to the configuration in FIG.

[0476] 17, by stacking a plurality of memory cells, it is possible to integrate and arrange the cells without increasing the area occupied by the memory cell array, that is, it is possible to configure a 3D memory cell array.

[0477] FIG. 18 shows an example of a cross-sectional configuration of a memory device in which a layer having memory cells is stacked over a layer in which a driver circuit including a sense amplifier is provided.

[0478] In FIG. 18, the memory cell 10 (transistor 100 and transistor 200 ) is provided above the transistor 300 .

[0479] The transistor 300 is one of the transistors included in the sense amplifier.

[0480] 18, the bit line can be shortened by providing a sense amplifier so as to overlap the memory cell 10. This reduces the bit line capacitance and the storage capacitance of the memory cell.

[0481] 18 can correspond to the semiconductor device 900 described in Embodiment 3. Specifically, the transistor 300 corresponds to a transistor included in a sense amplifier 927 in the semiconductor device 900. The memory cell 10 corresponds to a memory cell 950.

[0482] The transistor 300 is provided over a substrate 311 and includes a conductive layer 316 functioning as a gate, an insulating layer 315 functioning as a gate insulating layer, a semiconductor region 313 formed of part of the substrate 311, and a low-resistance region 314 a and a low-resistance region 314 b functioning as a source region or a drain region. The transistor 300 may be either a p-channel type or an n-channel type.

[0483] Here, in the transistor 300 shown in FIG. 18 , a semiconductor region 313 (a part of a substrate 311) where a channel is formed has a convex shape. A conductive layer 316 is provided to cover the side and top surfaces of the semiconductor region 313 with an insulating layer 315 interposed therebetween. Note that the conductive layer 316 may be made of a material that adjusts the work function. Such a transistor 300 is also called a FIN-type transistor because it utilizes the convex portion of the semiconductor substrate. Note that an insulating layer that is in contact with the top of the convex portion and functions as a mask for forming the convex portion may be provided. Here, the case where the convex portion is formed by processing a part of the semiconductor substrate is shown, but a semiconductor film having a convex shape may also be formed by processing an SOI substrate.

[0484] Note that the transistor 300 illustrated in FIG. 18 is just an example, and the structure is not limited thereto. An appropriate transistor can be used depending on the circuit configuration or driving method.

[0485] Between each structure, a wiring layer provided with an interlayer film, wiring, plugs, etc. may be provided. Furthermore, multiple wiring layers may be provided depending on the design. Here, for a conductive layer functioning as a plug or wiring, multiple structures may be collectively assigned the same reference numeral. Furthermore, in this specification and the like, a wiring and a plug electrically connected to the wiring may be integrated. That is, there are cases where a part of the conductive layer functions as a wiring, and cases where a part of the conductive layer functions as a plug.

[0486] For example, an insulating layer 320, an insulating layer 322, an insulating layer 324, and an insulating layer 326 are stacked in this order as an interlayer film over the transistor 300. A conductive layer 328 is embedded in the insulating layer 320 and the insulating layer 322, and a conductive layer 330 is embedded in the insulating layer 324 and the insulating layer 326. The conductive layer 328 and the conductive layer 330 function as plugs or wirings.

[0487] The insulating layer 322 may also function as a planarizing film that covers the underlying unevenness. For example, the top surface of the insulating layer 322 may be planarized by a planarization process using, for example, a CMP method in order to improve the planarity.

[0488] A wiring layer may be provided over the insulating layer 326 and the conductive layer 330. For example, in FIG. 18 , an insulating layer 350, an insulating layer 352, and an insulating layer 354 are stacked in this order. A conductive layer 356 is formed in the insulating layer 350, the insulating layer 352, and the insulating layer 354. The conductive layer 356 functions as a plug or a wiring.

[0489] The insulating layer 352, the insulating layer 354, and the like, which function as interlayer films, can be formed using the above-described insulating layer that can be used in a semiconductor device or a memory device.

[0490] For conductive layers functioning as plugs or wirings, such as the conductive layer 328, the conductive layer 330, and the conductive layer 356, a conductive material applicable to the conductive layer 140 and the conductive layer 240 can be used. A high-melting-point material such as tungsten or molybdenum that has both heat resistance and conductivity is preferably used, and tungsten is particularly preferable. Alternatively, a low-resistance conductive material such as aluminum or copper is preferably used. The use of a low-resistance conductive material can reduce wiring resistance.

[0491] The conductive layer 240 of the transistor 200 is electrically connected to the low-resistance region 314b functioning as a source region or a drain region of the transistor 300 through the conductive layer 643, the conductive layer 642, the conductive layer 644, the conductive layer 645, the conductive layer 646, the conductive layer 356, the conductive layer 330, and the conductive layer 328.

[0492] The conductive layer 643 is buried in the insulating layer 280. The conductive layer 644 is buried in the insulating layer 180 and the insulating layer 150. The conductive layer 646 is buried in the insulating layer 110. The conductive layer 642 is provided between the conductive layer 644 and the insulating layer 150 and between the conductive layer 643 and the insulating layer 280. The conductive layer 645 is provided between the conductive layer 646 and the insulating layer 110 and between the conductive layer 644 and the insulating layer 180. The conductive layer 642 can be manufactured using the same material and in the same process as the conductive layer 220. The conductive layer 645 can be manufactured using the same material and in the same process as the conductive layer 120. The transistor 300 and the conductive layer 120 are electrically insulated by the insulating layer 110.

[0493] This embodiment mode can be combined with other embodiment modes as appropriate. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be combined as appropriate.

[0494] Embodiment 3 In this embodiment, a semiconductor device 900 according to one embodiment of the present invention will be described. The semiconductor device 900 can function as a memory device.

[0495] Fig. 19 is a block diagram showing a configuration example of a semiconductor device 900. The semiconductor device 900 shown in Fig. 19 has a driver circuit 910 and a memory array 920. The memory array 920 has one or more memory cells 950. Fig. 19 shows an example in which the memory array 920 has a plurality of memory cells 950 arranged in a matrix.

[0496] The memory cell 950 can be, for example, the memory device described in the second embodiment (for example, the memory cell 10).

[0497] The drive circuit 910 includes a PSW 931 (power switch), a PSW 932, and a peripheral circuit 915. The peripheral circuit 915 includes a peripheral circuit 911, a control circuit 912, and a voltage generation circuit 928.

[0498] In the semiconductor device 900, each circuit, signal, and voltage can be appropriately selected or omitted as needed. Alternatively, other circuits or signals may be added. The signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are input signals from the outside, and the signal RDA is an output signal to the outside. The signal CLK is a clock signal.

[0499] Furthermore, signals BW, CE, and GW are control signals. Signal CE is a chip enable signal, signal GW is a global write enable signal, and signal BW is a byte write enable signal. Signal ADDR is an address signal. Signal WDA is write data, and signal RDA is read data. Signals PON1 and PON2 are power gating control signals. Note that signals PON1 and PON2 may be generated by the control circuit 912.

[0500] The control circuit 912 is a logic circuit having a function of controlling the overall operation of the semiconductor device 900. For example, the control circuit 912 performs a logical operation on the signals CE, GW, and BW to determine the operation mode (e.g., write operation, read operation) of the semiconductor device 900. Alternatively, the control circuit 912 generates a control signal for the peripheral circuit 911 so that this operation mode is executed.

[0501] The voltage generating circuit 928 has a function of generating a negative voltage. The signal WAKE has a function of controlling the input of the signal CLK to the voltage generating circuit 928. For example, when an H-level signal is given as the signal WAKE, the signal CLK is input to the voltage generating circuit 928, and the voltage generating circuit 928 generates a negative voltage.

[0502] The peripheral circuit 911 is a circuit for writing and reading data to and from the memory cells 950. The peripheral circuit 911 includes a row decoder 941, a column decoder 942, a row driver 923, a column driver 924, an input circuit 925, an output circuit 926, and a sense amplifier 927.

[0503] The row decoder 941 and the column decoder 942 have the function of decoding the signal ADDR. The row decoder 941 is a circuit for specifying a row to be accessed, and the column decoder 942 is a circuit for specifying a column to be accessed. The row driver 923 has the function of selecting the row specified by the row decoder 941. The column driver 924 has the function of writing data to the memory cell 950, the function of reading data from the memory cell 950, and the function of retaining the read data.

[0504] The input circuit 925 has a function of holding a signal WDA. The data held by the input circuit 925 is output to the column driver 924. The output data of the input circuit 925 is data (Din) to be written to the memory cell 950. The data (Dout) read from the memory cell 950 by the column driver 924 is output to the output circuit 926. The output circuit 926 has a function of holding Dout. In addition, the output circuit 926 has a function of outputting Dout to the outside of the semiconductor device 900. The data output from the output circuit 926 is a signal RDA.

[0505] The PSW 931 is a V DD The PSW 932 has the function of controlling the supply of V to the row driver 923. HM Here, the high power supply potential of the semiconductor device 900 is V DD and the low power supply potential is GND (ground potential).HM is the high power supply potential used to drive the word line high, and V DD The signal PON1 controls the on / off state of the PSW 931, and the signal PON2 controls the on / off state of the PSW 932. In FIG. 19, in the peripheral circuit 915, V DD Although the number of power domains to which power is supplied is set to one, it is also possible to set it to a plurality of power domains. In this case, a power switch may be provided for each power domain.

[0506] The driver circuit 910 and memory array 920 of the semiconductor device 900 may be provided on the same plane. Alternatively, as shown in FIG. 20A, the driver circuit 910 and memory array 920 may be provided overlapping each other. By providing the driver circuit 910 and memory array 920 overlapping each other, the signal propagation distance can be shortened. Alternatively, as shown in FIG. 20B, the memory array 920 may be provided in multiple layers on the driver circuit 910.

[0507] Next, an example of a processing unit that can include a semiconductor device such as the memory device will be described.

[0508] 21 shows a block diagram of the arithmetic device 960. The arithmetic device 960 shown in FIG. 21 can be applied to, for example, a CPU. The arithmetic device 960 can also be applied to processors such as a GPU (Graphics Processing Unit), a TPU (Tensor Processing Unit), and an NPU (Neural Processing Unit) that have a larger number (several tens to several hundreds) of processor cores capable of parallel processing than a CPU.

[0509] The arithmetic device 960 shown in FIG. 21 has an ALU 991 (ALU: Arithmetic logic unit, arithmetic circuit), an ALU controller 992, an instruction decoder 993, an interrupt controller 994, a timing controller 995, a register 996, a register controller 997, a bus interface 998, a cache 999, and a cache interface 989 on a substrate 990. The substrate 990 may be a semiconductor substrate, an SOI substrate, a glass substrate, or the like. It may also have a rewritable ROM and a ROM interface. The cache 999 and the cache interface 989 may also be provided on separate chips.

[0510] The cache 999 is connected to a main memory provided on a separate chip via a cache interface 989. The cache interface 989 has a function of supplying part of the data held in the main memory to the cache 999. The cache interface 989 also has a function of outputting part of the data held in the cache 999 to the ALU 991, register 996, etc. via the bus interface 998.

[0511] As will be described later, a memory array 920 can be provided stacked on the arithmetic unit 960. The memory array 920 can be used as a cache. In this case, the cache interface 989 may have a function of supplying data held in the memory array 920 to the cache 999. In this case, it is preferable that a drive circuit 910 be included as part of the cache interface 989.

[0512] It is also possible to use only the memory array 920 as a cache without providing the cache 999 .

[0513] The arithmetic device 960 shown in FIG. 21 is merely an example of a simplified configuration, and actual arithmetic devices 960 have a wide variety of configurations depending on their applications. For example, it is preferable to use a configuration including the arithmetic device 960 shown in FIG. 21 as one core, and to include multiple such cores, each of which operates in parallel, in a so-called multi-core configuration. The greater the number of cores, the higher the computational performance. The greater the number of cores, for example, two, preferably four, more preferably eight, even more preferably twelve, and even more preferably sixteen or more. Furthermore, when extremely high computational performance is required, such as for server applications, a multi-core configuration having 16 or more, preferably 32 or more, and even more preferably 64 or more cores is preferable. Furthermore, the number of bits that the arithmetic device 960 can handle in its internal computation circuit, data bus, etc. can be, for example, 8 bits, 16 bits, 32 bits, or 64 bits.

[0514] An instruction input to the arithmetic unit 960 via the bus interface 998 is input to the instruction decoder 993, decoded, and then input to the ALU controller 992, interrupt controller 994, register controller 997, and timing controller 995.

[0515] The ALU controller 992, interrupt controller 994, register controller 997, and timing controller 995 perform various controls based on the decoded instructions. Specifically, the ALU controller 992 generates signals for controlling the operation of the ALU 991. Furthermore, the interrupt controller 994 determines and processes interrupt requests from external input / output devices or peripheral circuits, etc., based on their priority or mask state, etc., while the arithmetic unit 960 is executing a program. The register controller 997 generates addresses for registers 996 and reads and writes data from and to the registers 996 depending on the state of the arithmetic unit 960.

[0516] Furthermore, the timing controller 995 generates signals that control the timing of the operations of the ALU 991, the ALU controller 992, the instruction decoder 993, the interrupt controller 994, and the register controller 997. For example, the timing controller 995 includes an internal clock generation unit that generates an internal clock signal based on a reference clock signal, and supplies the internal clock signal to the various circuits described above.

[0517] 21 , the register controller 997 selects the holding operation of the register 996 in accordance with an instruction from the ALU 991. That is, it selects whether the memory cells of the register 996 will hold data using flip-flops or using capacitors. If holding data using flip-flops is selected, a power supply potential is supplied to the memory cells in the register 996. If holding data using capacitors is selected, the data is rewritten to the capacitors, and the supply of power supply potential to the memory cells in the register 996 can be stopped.

[0518] The memory array 920 and the arithmetic unit 960 can be provided overlapping each other. Perspective views of a semiconductor device 970A are shown in Figures 22A and 22B. The semiconductor device 970A has a layer 930 on which memory arrays are provided above the arithmetic unit 960. The layer 930 is provided with memory arrays 920L1, 920L2, and 920L3. The arithmetic unit 960 and each memory array have overlapping...

Claims

a first transistor, a second transistor, a first insulating layer, a second insulating layer, and a third insulating layer; the first transistor has a first semiconductor layer, a first conductive layer, a second conductive layer, a third conductive layer, and a fourth insulating layer; the second transistor includes a second semiconductor layer, the third conductive layer, a fourth conductive layer, a fifth conductive layer, and a fifth insulating layer; the first insulating layer overlies the first conductive layer; the second conductive layer is located on the first insulating layer; the first conductive layer has a first recess; the first insulating layer and the second conductive layer have a first opening at a position overlapping the first recess; the first semiconductor layer is in contact with an upper surface of the second conductive layer and the first recess, and is in contact with a side surface of the second conductive layer and a side surface of the first insulating layer inside the first opening; the fourth insulating layer has a region located on the second conductive layer and a region located on the first semiconductor layer within the first opening; the third conductive layer has a region facing the first semiconductor layer with the fourth insulating layer interposed therebetween within the first opening, the third conductive layer has a region overlapping with the second conductive layer via the fourth insulating layer; the third conductive layer has a second recess; the second insulating layer overlies the third conductive layer; the fourth conductive layer is located on the second insulating layer; the second insulating layer and the fourth conductive layer have second openings at positions overlapping with the second recesses; the second semiconductor layer is in contact with an upper surface of the fourth conductive layer and the second recess, and is in contact with a side surface of the fourth conductive layer and a side surface of the second insulating layer inside the second opening; the fifth insulating layer is located on the second semiconductor layer within the second opening; the third insulating layer has a region overlapping with the fourth conductive layer via the second semiconductor layer, and has a third opening at a position overlapping with the second opening; the fifth conductive layer has a region facing the second semiconductor layer with the fifth insulating layer interposed therebetween inside the second opening, and a region located inside the third opening.   In claim 1, The second opening at least partially overlaps with the first opening.   In claim 1, A sixth insulating layer is provided. the first insulating layer and the first conductive layer are located on the sixth insulating layer; a shortest distance from an upper surface of the sixth insulating layer to an upper surface of the first conductive layer that is in contact with the first insulating layer is longer than a shortest distance from the upper surface of the sixth insulating layer to a lower surface of the fourth insulating layer in a region that overlaps with the first recess; a shortest distance from an upper surface of the sixth insulating layer to an upper surface of the third conductive layer that contacts the second insulating layer and overlaps with the second conductive layer is longer than a shortest distance from the upper surface of the sixth insulating layer to a lower surface of the fifth insulating layer in a region that overlaps with the second recess.   In claim 1, A sixth insulating layer is provided. the first insulating layer and the first conductive layer are located on the sixth insulating layer; a shortest distance from an upper surface of the sixth insulating layer to an upper surface of the first conductive layer that is in contact with the first insulating layer is equal to or greater than a shortest distance from the upper surface of the sixth insulating layer to a lower surface of the third conductive layer in a region that overlaps with the first recess, a shortest distance from an upper surface of the sixth insulating layer to an upper surface of the third conductive layer that is in contact with the second insulating layer and overlaps with the second conductive layer is greater than or equal to the shortest distance from the upper surface of the sixth insulating layer to a lower surface of the fifth conductive layer in a region that overlaps with the second recess.   In claim 1, the first conductive layer has a sixth conductive layer and a seventh conductive layer on the sixth conductive layer; the third conductive layer has an eighth conductive layer and a ninth conductive layer on the eighth conductive layer; the seventh conductive layer has the first recess; the ninth conductive layer has the second recess.   In claim 1, A sixth conductive layer is provided; The sixth conductive layer is provided so as to be in contact with an upper surface of the fifth conductive layer.   In claim 6, a thickness of the third insulating layer in a region overlapping the fourth conductive layer and the second semiconductor layer is greater than a thickness of the fourth insulating layer.   In claim 1, At least a portion of the fifth insulating layer is located inside the third opening.   In claim 1, the first transistor has a sixth conductive layer; the second transistor has a seventh conductive layer; the first insulating layer includes a first layer and a second layer on the first layer; the second insulating layer includes a third layer and a fourth layer on the third layer; the sixth conductive layer is located on the first layer; the seventh conductive layer is located on the third layer; the second layer covers an upper surface and a side surface of the sixth conductive layer; the fourth layer covers an upper surface and a side surface of the seventh conductive layer; When viewed in cross section, the first semiconductor layer has a region that faces the sixth conductive layer with the second layer therebetween and that faces the third conductive layer with the fourth insulating layer therebetween; A semiconductor device, wherein, in a cross-sectional view, the second semiconductor layer has a region that faces the seventh conductive layer across the fourth layer and that faces the fifth conductive layer across the fifth insulating layer.   In any one of claims 1 to 9, the first semiconductor layer and the second semiconductor layer each include an oxide semiconductor; the oxide semiconductor contains one or more selected from the group consisting of indium, an element M, and zinc; The element M is one or more selected from aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony.   In claim 10, the first insulating layer has a first region in contact with the first semiconductor layer; the second insulating layer has a second region in contact with the second semiconductor layer; The first region and the second region each contain a halogen element.   In claim 11, The halogen element is one or more elements selected from the group consisting of chlorine, fluorine, bromine, and iodine.   In claim 10, the first semiconductor layer has a first region in contact with a bottom surface of the first recess and a second region in contact with an upper surface of the second conductive layer; the second semiconductor layer has a third region in contact with a bottom surface of the second recess and a fourth region in contact with an upper surface of the fourth conductive layer; The first to fourth regions each contain boron or phosphorus.   forming a first conductive layer; forming a first insulating layer on the first conductive layer; forming a second conductive layer on the first insulating layer; forming a first opening in the second conductive layer and the first insulating layer at a position where the first conductive layer overlaps the first insulating layer, and forming a first recess in the first conductive layer so as to overlap the first opening; forming a first semiconductor layer so as to be in contact with an upper surface of the second conductive layer and the first recess, and to be in contact with a side surface of the second conductive layer and a side surface of the first insulating layer inside the first opening; processing the first semiconductor layer and the second conductive layer to expose a portion of an upper surface of the first insulating layer; forming a second insulating layer having a region located on the second conductive layer and a region located on the first semiconductor layer within the first opening; forming a third conductive layer in the first opening, the third conductive layer having a region facing the first semiconductor layer with the second insulating layer interposed therebetween, and having a region overlapping the second conductive layer with the second insulating layer interposed therebetween; forming a third insulating layer on the third conductive layer; forming a fourth conductive layer on the third insulating layer; forming a second opening in the fourth conductive layer and the third insulating layer at a position overlapping the third conductive layer, and forming a second recess in the third conductive layer so as to overlap the second opening; forming a second semiconductor layer so as to be in contact with an upper surface of the fourth conductive layer and the second recess, and to be in contact with a side surface of the fourth conductive layer and a side surface of the third insulating layer inside the second opening; processing the second semiconductor layer and the fourth conductive layer to expose a portion of an upper surface of the third insulating layer; forming a sacrificial layer such that at least a portion of the sacrificial layer is located within the second opening; forming a fourth insulating layer to cover the fourth conductive layer, the second semiconductor layer, and the sacrificial layer; performing a planarization process on the fourth insulating layer and the sacrificial layer to planarize an upper surface of the sacrificial layer; removing the sacrificial layer; forming a fifth insulating layer to cover the second opening; forming a fifth conductive layer on the fifth insulating layer; A method for manufacturing a semiconductor device, comprising: performing planarization treatment on the fifth conductive layer to remove a region of the fifth conductive layer and the fifth insulating layer that overlaps with a top surface of the fourth insulating layer.   In claim 14, a second opening portion formed at a position at least partially overlapping with the first opening portion;   In claim 14 or 15, forming a sixth conductive layer so as to be in contact with an upper surface of the fifth conductive layer.   In claim 16, The fourth insulating layer is formed to have a thickness larger than that of the second insulating layer.

Citation Information

Patent Citations

  • Thin film transistor, memory, manufacturing method and electronic equipment

    CN114792735A

  • Thin-film semiconductor device

    JP1991291973A

  • Semiconductor device and manufacture thereof

    JP1995099311A

  • Semiconductor device, and manufacturing method for the same

    JP2016149552A

  • Semiconductor device and manufacturing method thereof

    JP2019169490A