Secondary battery and production method for secondary battery

The described method for manufacturing lithium-ion secondary batteries using sulfur and reduced graphene oxide improves capacity and cycle life, addressing existing challenges in battery technology by enhancing conductivity and adhesion, and eliminating the need for costly cobalt.

WO2024241189A1PCT designated stage expired Publication Date: 2024-11-28SEMICON ENERGY LAB CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2024/054868
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-20
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current lithium-ion secondary batteries face challenges in achieving high capacity, lightweight design, excellent charge/discharge cycle characteristics, and long cycle life while maintaining safety and reliability, particularly with the use of sulfur as a positive electrode active material.

Method used

A manufacturing method involving a positive electrode made from sulfur and graphene oxide, where graphene oxide is reduced using ascorbic acid and lithium hydroxide, and a slurry is formed with a conductive additive and binder to create a sulfur-based active material layer on a carbon current collector, enhancing the electrode's conductivity and adhesion.

Benefits of technology

The method results in a lithium-ion secondary battery with increased discharge capacity, improved electrical resistance, and extended cycle life, making it suitable for high-energy density applications while avoiding the use of rare metals like cobalt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2024054868_28112024_PF_FP_ABST
    Figure IB2024054868_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a lightweight, high-capacity lithium ion secondary battery and a production method therefor. The present invention involves mixing sodium thiosulfate and water in which graphene oxide has been dispersed, adding hydrochloric acid and mixing, drying to form a powder, adding the powder to pure water and stirring before adding a mixed aqueous solution of ascorbic acid and lithium hydroxide, heating to remove the water and produce a powdered positive electrode active material, adding a conductivity aid, a solvent, and a binder to form a slurry, and applying the slurry to a positive electrode collector to form a material that includes elemental sulfur as a positive electrode active material layer and produce a positive electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Secondary battery and method for manufacturing the secondary battery

[0001] One embodiment of the present invention relates to an object, a method, or a manufacturing method. Alternatively, the present invention relates to a process, a machine, a manufacture, or a composition of matter. One embodiment of the present invention relates to a power storage device including a secondary battery, a semiconductor device, a display device, a light-emitting device, a lighting device, an electronic device, or a manufacturing method thereof.

[0002] In this specification, the term "electronic device" refers to any device having a power storage device, and includes electro-optical devices having a power storage device, information terminal devices having a power storage device, and the like.

[0003] In this specification, the term "electricity storage device" refers to elements and devices in general that have an electricity storage function, including, for example, lithium ion secondary battery electricity storage devices (also called secondary batteries), lithium ion capacitors, and electric double layer capacitors.

[0004] In recent years, various types of power storage devices, such as lithium-ion secondary batteries, lithium-ion capacitors, and air batteries, have been actively developed. In particular, lithium-ion secondary batteries, which have high output and high energy density, are applied to mobile information terminals such as mobile phones, smartphones, and notebook computers, portable music players, digital cameras, medical devices, and next-generation clean energy vehicles such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs). Demand for lithium-ion secondary batteries has expanded rapidly along with the development of the semiconductor industry, and they have become indispensable in the modern information society as a rechargeable energy source.

[0005] In addition, lightweight, high-capacity secondary batteries are desired, and secondary batteries using sulfur-containing materials as positive electrode active materials have attracted attention. Sulfur has a high theoretical capacity of approximately 1670 mAh / g and is known to be a promising positive electrode active material in terms of energy density.

[0006] Furthermore, materials containing elemental sulfur are abundant resources, and therefore have the advantage of being cheaper than transition metals such as cobalt.

[0007] For example, research is being conducted on sulfur-based secondary batteries using sulfur and three-dimensional graphene sponge (3DGS) (Non-Patent Document 1).

[0008] Chao Lin et al. , “A facile synthesis of three dimensional graphene sponge composited with sulfur nanoparticles for flexible Li-S cathodes”, Phys. Chem. Chem. Phys. ,2016,18,22146-22153

[0009] In secondary batteries that use a material containing elemental sulfur as a positive electrode active material, lithium metal is used as an example of a negative electrode active material. During discharge, lithium metal dissolves in the electrolyte at the negative electrode to become ions, which react with sulfur at the positive electrode to be oxidized, resulting in the formation of an intermediate reaction product, lithium polysulfide (Li 2 S n (2≦n≦8)) and then lithium sulfide (Li 2 S).

[0010] An object of one embodiment of the present invention is to provide a high-capacity lithium-ion secondary battery and a manufacturing method thereof.Another object of one embodiment of the present invention is to provide a lightweight and high-capacity lithium-ion secondary battery and a manufacturing method thereof.

[0011] Another object of one embodiment of the present invention is to provide a lithium-ion secondary battery with excellent charge-discharge cycle characteristics and a manufacturing method thereof.Another object of one embodiment of the present invention is to provide a secondary battery with long cycle life and high safety or reliability and a manufacturing method thereof.

[0012] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description in the specification, drawings, and claims.

[0013] The present specification discloses a method for producing a secondary battery, which includes a positive electrode, a separator, an electrolyte, and a negative electrode. The method includes mixing water in which graphene oxide is dispersed with thiosulfate, adding hydrochloric acid and mixing, filtering, and drying to obtain a powder containing elemental sulfur. The powder is added to pure water and stirred, and then an aqueous mixture of ascorbic acid and lithium hydroxide is added. The mixture is heated to reduce the graphene oxide, and the water is removed to obtain a powdered positive electrode active material. A conductive additive, a solvent, and a binder are added to form a slurry. The slurry is applied to a positive electrode current collector, dried, and heated under reduced pressure to form a positive electrode active material layer made of a material containing elemental sulfur, thereby forming a positive electrode.

[0014] The positive electrode is a current collector coated with a carbon material coated with sulfur or a sulfur compound. Because elemental sulfur is an insulator, it is preferable to attach sulfur to the carbon material or to partially coat it with a thin film. Examples of sulfur compounds (also called sulfides) include metal sulfides and sulfates. Examples of metal sulfides include lithium sulfide and polysulfides (also called polysulfides).

[0015] The carbon material used for the positive electrode is graphene, graphene oxide, or reduced graphene oxide. A chemical or physical bond may exist between the carbon material and the active material (sulfur), or the carbon material and the active material may be in an aggregated state. To obtain a high-capacity positive electrode, a carbon material with a large surface area on which a sulfur or sulfur compound coating is formed is preferred. Therefore, flake-shaped graphene, flake-shaped graphene oxide, or reduced flake-shaped graphene oxide is used. In practice, flake-shaped carbon materials include monoatomic layers or multilayer laminates, and are not flat but rather have a shape resembling a rolled sheet with an irregular surface, which is sometimes referred to as a particle. When using graphene oxide for ease of handling and storage, it is preferable to perform a reduction treatment in a later process. Note that pre-reduced graphene (abbreviated as RGO for reduced graphene oxide) tends to aggregate when dissolved in a solvent, making it difficult to handle.

[0016] In addition, an electrolytic solution or solid electrolyte is provided between the positive electrode and the negative electrode. When a solid electrolyte is used, an all-solid-state battery can be formed. Since an all-solid-state battery does not require the use of an organic electrolyte, problems such as leakage and battery expansion due to evaporation of the organic electrolyte can be solved. In addition, an ionic liquid can be used instead of the electrolytic solution. When an electrolytic solution or an ionic liquid is used, a separator is provided to prevent short circuits.

[0017] In the above-described manufacturing method, ascorbic acid is added as a reducing solution and heated to chemically reduce graphene oxide. The reducing solution is prepared using a reducing agent and a solvent that dissolves the reducing agent. In addition to ascorbic acid, other reducing agents include hydrazine, dimethylhydrazine, hydroquinone, and sodium borohydride (NaBH 4 ), lithium aluminum hydride (LiAlH 4 ), N,N-diethylhydroxylamine, or derivatives thereof can be used. Ascorbic acid and hydroquinone are particularly preferred because they have weaker reducing power than hydrazine or sodium borohydride, are highly safe, and are easily industrially applicable. The solvent used is one or a mixture of two or more of water, methanol, ethanol, acetone, tetrahydrofuran (THF), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), and dimethyl sulfoxide (DMSO). In the above preparation method, lithium hydroxide functions as a pH adjuster for neutralization. The pH of the reducing solution is set to 4 or more and 11 or less.

[0018] In this specification, powder refers to solid particles smaller than 1 mm, and an aggregate of powders is called a powder. Powder or granules refer to a loose aggregate or agglomerate of solid particles smaller than 1 mm. In this specification, flake graphene or flake graphene oxide is also called a powder, and an aggregate is called a powder.

[0019] A material containing elemental sulfur is used as the positive electrode active material, and the positive electrode active material is in the form of a powder. When the positive electrode active material is in the form of a powder, maintaining airtightness facilitates storage, and heating under reduced pressure removes moisture from the material containing elemental sulfur, preventing deterioration. Furthermore, because graphene may become graphene oxide when exposed to air, it is preferable to prepare the positive electrode active material and the slurry in an environment filled with an inert gas such as nitrogen or argon and with a low oxygen partial pressure, for example, in a dry room.

[0020] In the above-described production method, when the slurry is applied to the positive electrode current collector, it is necessary to adjust the viscosity so that the slurry is liquid and the neutralization operation is easy. In consideration of the dispersibility of the active material contained in the slurry and the coatability of the slurry, it is preferable that the positive electrode active material be in a powder form before being mixed with the solvent.

[0021] In the above-described production method, the slurry can be prepared by mixing the powder with pure water and then deagglomerating the mixture by ultrasonic irradiation in water to prepare a dispersion. In this specification, pure water refers to pure water having a resistivity of 10 MΩcm or more at room temperature.

[0022] A secondary battery obtained by the above-described manufacturing method is also one of the configurations of the present invention. The secondary battery includes a positive electrode current collector, a separator, and a negative electrode. The positive electrode active material layer includes a plurality of sheet-shaped graphenes, at least some of which are formed by reducing graphene oxide, and the graphene has sulfur element on the surface thereof. The positive electrode active material layer includes at least a crystallized binder. Crystallizing the binder can improve adhesion between the positive electrode active material layer and the positive electrode current collector and reduce the electrical resistance of the positive electrode. Therefore, the discharge capacity or charge capacity of the secondary battery can be increased.

[0023] The heat treatment conditions under reduced pressure for crystallizing the binder are 100° C. or higher and 130° C. or lower, and 30 minutes or longer but less than 2 hours.

[0024] In the above configuration, the negative electrode is lithium metal.

[0025] Secondary batteries that use a material containing elemental sulfur as a positive electrode active material are also called lithium-sulfur batteries, and are not limited to secondary batteries that use lithium metal for the negative electrode, but also include secondary batteries that use silicon or carbon materials for the negative electrode. Typical carbon materials used for the negative electrode include graphite, graphene, graphene oxide, reduced graphene oxide, and carbon nanotubes.

[0026] Furthermore, secondary batteries that use a material containing elemental sulfur as a positive electrode active material are not limited to lithium ions, but also include secondary batteries that use sodium ions or potassium ions instead of lithium ions.

[0027] In a method for producing a positive electrode active material, a powder material such as graphene oxide, which is easy to handle, is used and subjected to a reduction treatment to obtain a powder positive electrode active material. The positive electrode active material has sulfur on the surface of reduced graphene oxide. Since the secondary battery uses reduced graphene oxide and sulfur for the positive electrode and lithium metal for the negative electrode, it can realize a lightweight and high-capacity secondary battery.

[0028] Furthermore, since rare metals such as nickel or cobalt are not used, a low-cost secondary battery can be realized.

[0029] FIG. 1 illustrates an example of a manufacturing flow illustrating one embodiment of the present invention. FIG. 2 illustrates an example of a manufacturing method of a positive electrode. FIG. 3A is an exploded perspective view of a coin-type secondary battery, FIG. 3B is a perspective view of the coin-type secondary battery, and FIG. 3C is a cross-sectional perspective view thereof. FIG. 4A illustrates an example of a cylindrical secondary battery. FIG. 4B is a view of an example of a cylindrical secondary battery. FIG. 4C is a view of an example of a plurality of cylindrical secondary batteries. FIG. 4D is a view of an example of a power storage system including a plurality of cylindrical secondary batteries. FIGS. 5A and 5B are views of the external appearance of a secondary battery. FIGS. 6A to 6C are views illustrating a method for manufacturing a secondary battery. FIGS. 7A to 7D are views illustrating an example of an electronic device. FIGS. 8A to 8C are views illustrating an example of an electronic device. FIGS. 9A to 9C are views illustrating an example of a vehicle. FIGS. 10A and 10B are views illustrating an example of a vehicle. FIG. 11 is a cross-sectional schematic view of a battery cell according to an example. FIG. 12 illustrates charge and discharge characteristics of the battery cell. FIG. 13 illustrates cycle characteristics according to an example.

[0030] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various modifications can be made to the embodiments and details. Furthermore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.

[0031] Embodiment 1 In this embodiment, an example of a manufacturing method for using a powdered positive electrode active material 200A as a positive electrode of a secondary battery is shown in FIGS.

[0032] First, a carbon material 890 is prepared. In this embodiment, graphene oxide is used as the carbon material 890.

[0033] In this specification and the like, graphene oxide refers to a material that contains carbon and oxygen, has a flake shape, and has functional groups, particularly epoxy groups, carboxy groups, or hydroxy groups. Graphene oxide can be produced by various synthesis methods, such as the Hummers method, the modified Hummers method, or oxidation of graphite.

[0034] The length of one side of graphene oxide (also referred to as flake size) is 50 nm or more and 100 μm or less, preferably 800 nm or more and 20 μm or less.

[0035] In this specification and the like, reduced graphene oxide refers to a material containing carbon and oxygen, having a sheet-like shape, and having a two-dimensional structure formed by six-membered carbon rings. A single sheet of reduced graphene oxide can function, but multiple sheets may be stacked. Reduced graphene oxide preferably has a portion where the carbon concentration is greater than 80 atomic % and the oxygen concentration is 2 atomic % or more and 15 atomic % or less. By achieving such carbon and oxygen concentrations, reduced graphene oxide can function as a highly conductive material even in small amounts. Furthermore, reduced graphene oxide preferably has an intensity ratio G / D of the G band to the D band in a Raman spectrum of 1 or more. Reduced graphene oxide with such an intensity ratio can function as a highly conductive material even in small amounts.

[0036] In this specification, graphene includes multi-layer graphene and multi-graphene. In other words, graphene refers to a substance that contains carbon, has a shape such as a plate or sheet, and has a two-dimensional structure formed by six-membered carbon rings. The two-dimensional structure formed by six-membered carbon rings is sometimes called a carbon sheet. Furthermore, graphene compounds include graphene oxide, multi-layer graphene oxide, multi-graphene oxide, reduced graphene oxide, reduced multi-layer graphene oxide, reduced multi-graphene oxide, graphene quantum dots, and the like. In other words, graphene compounds may have functional groups. Furthermore, graphene or graphene compounds preferably have a curved shape. Furthermore, graphene or graphene compounds may be rolled, and rolled graphene is sometimes called a carbon nanofiber.

[0037] Then, the carbon material 890 and the pure water 893 are mixed to prepare a dispersion liquid 901 .

[0038] In addition, a material 902 containing sulfur is prepared. In this embodiment, anhydrous sodium thiosulfate (Na thiosulfate) is used as the material 902 containing sulfur. 2 S 2 O3 The sulfur-containing material 902 is not particularly limited as long as it is water-soluble and is a powder containing thiosulfate, and for example, calcium thiosulfate, magnesium thiosulfate, or potassium thiosulfate can be used.

[0039] Then, the dispersion liquid 901 and the sulfur-containing material 902 are mixed to obtain a first mixture liquid 903. Since heat is generated by the reaction during mixing, the mixture is thoroughly stirred while being cooled. In this embodiment, the temperature of the dispersion liquid is maintained at 0° C. and the mixture is mixed for 10 minutes.

[0040] Then, hydrochloric acid 894 is added to obtain a second mixed solution 904. Then, stirring is carried out for 10 hours or more using a stirrer.

[0041] The second mixture 904 is then filtered using a suction filter, and the remaining residue is washed with pure water, filtered again, and dried. The drying of the second mixture 904 can be performed by a method such as ventilation drying or reduced pressure (vacuum) drying.

[0042] Through the above steps, a precursor (powder) 905 can be obtained. The precursor (powder) 905 contains graphene oxide, and the graphene oxide is not reduced. Because it is a powder, it is easier to handle than a gel and can be weighed accurately.

[0043] Next, to prepare a dispersion, pure water 895 and precursor (powder) 905 are mixed.

[0044] Then, in order to carry out the reduction treatment, a mixed solution 896 of ascorbic acid and lithium hydroxide is added, and then the mixture is deagglomerated by ultrasonic irradiation in water. An aqueous solution of ascorbic acid and lithium hydroxide is mixed in advance to prepare a mixed solution 896 of ascorbic acid and lithium hydroxide. The lithium hydroxide is added to adjust the pH, and sodium hydroxide may be used instead of lithium hydroxide.

[0045] Next, a heat treatment is carried out as a reduction treatment. The heat treatment is carried out at a temperature not exceeding the melting point of sulfur, 110° C., for example, 95° C., and refluxing is carried out for 1 hour to 5 hours.

[0046] Thereafter, the mixture is filtered, and the residue is washed with pure water and dried.

[0047] In the powdered positive electrode active material 200A obtained in this manner, a plurality of flake-like substances each having a size of about 5 μm can be confirmed, and among these, clumps formed by aggregation of a plurality of these can also be confirmed.

[0048] The powdered positive electrode active material 200A is a sulfur-containing active material and can be used for the positive electrode of a secondary battery. The sulfur-containing active material is elemental sulfur, lithium disulfide, or lithium polysulfide. Furthermore, because the powdered positive electrode active material 200A is not a gel, it is easy to handle and can be stored stably. Furthermore, because the weighing amount is easy to adjust, it is suitable for mass production.

[0049] Next, a secondary battery in which a positive electrode, a negative electrode, and an electrolyte are housed in an exterior body will be described as an example.

[0050] [Positive Electrode] The positive electrode active material layer contains a positive electrode active material and a conductive material (also called a conductive additive). The positive electrode active material layer preferably also contains a binder. In particular, a material containing fluorine is used as the binder. In this embodiment, a material containing sulfur element is mixed with a conductive material or a binder to form a slurry, and the slurry is applied to a positive electrode current collector to form a positive electrode active material layer.

[0051] In this embodiment, the positive electrode active material 200A described above is used as the positive electrode active material. The positive electrode active material 200A includes a plurality of graphenes, at least some of which are sheet-shaped, that are obtained by subjecting graphene oxide to reduction treatment, and elemental sulfur is present on the surfaces of the graphene.

[0052] Although graphene or graphene oxide does not function as an active material, it is included as part of the positive electrode active material.

[0053] The conductive material, which does not function as an active material, functions as a structure of the positive electrode active material layer and is used to impart conductivity to the positive electrode active material layer, and also functions to support a current path between sulfur and a current collector or a current path between multiple sulfur atoms.

[0054] The conductive material contained in the positive electrode active material may be flake-shaped, such as multilayer graphene, which may appear thread-like in the cross section of the positive electrode.

[0055] When multilayer graphene is used as the flake-like conductive material and carbon black is used as the particulate conductive material, the weight of the carbon black in a mixed slurry state is preferably 1.5 to 20 times, and more preferably 2 to 9.5 times, the weight of the multilayer graphene.

[0056] When the mixing ratio of multilayer graphene to carbon black is within the above range, the carbon black does not aggregate and is easily dispersed. Furthermore, when the mixing ratio of multilayer graphene to carbon black is within the above range, the electrode density can be made higher than when only carbon black is used as the conductive material. By increasing the electrode density, the capacity per unit weight can be increased.

[0057] Furthermore, by setting the mixing ratio of multilayer graphene and carbon black within the above range, rapid charging can be achieved.

[0058] Graphene compounds may have excellent electrical properties, such as high electrical conductivity, and excellent physical properties, such as high flexibility and high mechanical strength. Graphene compounds may also have a flake-like shape. Graphene compounds may have curved surfaces, enabling surface contact with low contact resistance. Even when thin, graphene compounds may have very high electrical conductivity, allowing a small amount of graphene to efficiently form a conductive path within the positive electrode active material layer.

[0059] The graphene or graphene compound flakes may be uniformly dispersed in the positive electrode active material layer. The graphene or graphene compound flakes are formed so as to partially cover the active material particles or to be attached to the surfaces of the active material particles, and are in surface contact with each other.

[0060] Here, a plurality of graphenes or graphene compounds are bonded to each other to form a mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or a graphene net).

[0061] Here, it is preferable to use graphene oxide as the graphene or graphene compound, mix it with an active material to form an active material layer, and then reduce it. That is, the completed active material layer preferably contains reduced graphene oxide. By using graphene oxide, which has extremely high dispersibility in polar solvents, to form graphene or graphene compounds, it is possible to achieve a substantially uniform dispersion of the graphene or graphene compound within the active material layer. The solvent is volatilized and removed from the dispersion medium containing the uniformly dispersed graphene oxide, and the graphene oxide is reduced. Therefore, the graphene or graphene compound remaining in the active material layer partially overlaps and is dispersed to the extent that it is in surface contact with each other, thereby forming a three-dimensional conductive path. The reduction of graphene oxide may be performed, for example, by heat treatment or using a reducing agent.

[0062] [Positive Electrode Current Collector] The positive electrode current collector can be made of a highly conductive material, such as a metal such as stainless steel, gold, platinum, aluminum, or titanium, or an alloy thereof. It is preferable that the material used for the positive electrode current collector does not dissolve at the potential of the positive electrode. Aluminum alloys containing elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, or molybdenum, can also be used. The positive electrode current collector may also be made of a metal element that reacts with silicon to form a silicide. Examples of metal elements that react with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, and nickel. The current collector can be in the form of a foil, plate, sheet, mesh, punched metal, expanded metal, or the like. It is preferable to use a current collector with a thickness of 5 μm to 30 μm.

[0063] In order to improve adhesion to the positive electrode active material layer, a positive electrode current collector having a base layer on its surface, which is undercoated with carbon or the like, may be used.

[0064] [Conductive Material] The conductive material functions to assist the current path between the active material and the current collector, or the current path between multiple active materials. To fulfill this function, the conductive material preferably has a lower resistance than the active material. Due to its role, the conductive material is also called a conductive auxiliary or a conductive agent.

[0065] The conductive material is typically a carbon material or a metal material. The conductive material is particulate, and examples of such particulate conductive materials include carbon black (furnace black, acetylene black, graphite, etc.). Many carbon blacks have a smaller particle size than the positive electrode active material. The conductive material is fibrous, and examples of such fibrous conductive materials include carbon nanotubes (CNT) and VGCF (registered trademark).

[0066] Particulate conductive materials can penetrate into gaps in the positive electrode active material and are prone to aggregation. Therefore, particulate conductive materials can assist in the conductive paths between nearby positive electrode active materials. Fibrous conductive materials have bent regions, but are larger than the positive electrode active materials. Therefore, fibrous conductive materials can assist in the conductive paths between distant positive electrode active materials in addition to adjacent positive electrode active materials. In this way, it is recommended to mix two or more shapes of conductive materials.

[0067] Graphene can be used as the conductive material. In this case, first graphene having sulfur on its surface and second graphene not having sulfur on its surface are mixed.

[0068] In addition to graphene and acetylene black, carbon fiber materials (also referred to as carbon nanotubes or CNTs) can be used as conductive materials. Fluorine-containing carbon nanotubes may also be used. The fluorine in the fluorine-containing carbon nanotubes is preferably adsorbed on the surface. Fluorine-containing carbon nanotubes can also be produced by contacting carbon nanotubes with a fluorine compound (called fluorination treatment). The fluorination treatment described for graphene can also be applied to carbon nanotubes.

[0069] [Binder] The binder is necessary to firmly bond the powdered active material without covering the surface of the active material. Furthermore, the binder must be adhesive to the current collector. In other words, the binder should contain a material that exhibits binding properties. Furthermore, in consideration of the expansion of the active material, the binder should be sufficiently flexible and able to adapt to changes in the state of the active material. The binder must also be compatible with the electrolyte. Furthermore, because extremely strong oxidation and reduction reactions occur in secondary batteries, a binder that does not deteriorate in these reactions or has low reactivity is desired.

[0070] As the binder, it is preferable to use materials such as polystyrene, polymethyl acrylate, polymethyl methacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, nitrocellulose, etc. A combination of two or more of the above binders may also be used.

[0071] Polyimide has excellent thermal, mechanical, and chemical stability. When polyimide is used as a binder, it undergoes dehydration and cyclization (imidization) reactions. These reactions can be carried out, for example, by heat treatment.

[0072] It is particularly preferable to use a fluorine-containing material such as a fluoropolymer, specifically polyvinylidene fluoride (PVDF), etc. PVDF is a resin with a melting point in the range of 134°C to 169°C, and is a material with excellent thermal stability.

[0073] As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Furthermore, as the binder, fluororubber can be used.

[0074] Furthermore, it is preferable to use, for example, a water-soluble polymer as the binder. Examples of the water-soluble polymer that can be used include polysaccharides. Examples of the polysaccharide that can be used include one or more of cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, and starch. It is even more preferable to use these water-soluble polymers in combination with the above-mentioned rubber material.

[0075] Alternatively, the binder may be a combination of a material with particularly excellent viscosity-adjusting properties and another material. For example, rubber materials have excellent adhesive strength and / or elasticity, but may have difficulty adjusting the viscosity when mixed with a solvent. In such cases, it is preferable to mix the binder with a material with particularly excellent viscosity-adjusting properties. Examples of materials with particularly excellent viscosity-adjusting properties include water-soluble polymers. Examples of water-soluble polymers with particularly excellent viscosity-adjusting properties include the aforementioned polysaccharides, such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, and diacetyl cellulose; cellulose derivatives such as regenerated cellulose; and starch.

[0076] In addition, the solubility of cellulose derivatives such as carboxymethyl cellulose can be increased by converting them into salts such as sodium and ammonium salts of carboxymethyl cellulose, making them more effective as viscosity adjusters. Higher solubility can also improve dispersibility with the active material and other components when preparing electrode slurry. In this specification, the cellulose and cellulose derivatives used as electrode binders also include their salts.

[0077] Water-soluble polymers stabilize viscosity by dissolving in water, and can stably disperse active materials and other materials combined as binders, such as styrene-butadiene rubber, in water. Furthermore, because they contain functional groups, they are expected to be easily and stably adsorbed onto the surface of active materials. Furthermore, many cellulose derivatives, such as carboxymethyl cellulose, contain functional groups, such as hydroxyl and carboxyl groups, and because of these functional groups, the polymers are expected to interact with each other and widely cover the surface of the active material.

[0078] [Electrolyte] The secondary battery has an electrolyte containing carrier ions. In this specification and the like, the electrolyte is not limited to an electrolyte containing an organic solvent that is liquid at room temperature, but also includes a solid electrolyte, and also includes an electrolyte containing both an organic solvent that is liquid at room temperature and a solid electrolyte that is solid at room temperature (semi-solid electrolyte). Note that a lithium salt dissolved in an organic solvent that is liquid at room temperature may be referred to as an electrolyte solution.

[0079] <Organic solvent that is liquid at room temperature> An example of an organic solvent that is liquid at room temperature will be described below.

[0080] The organic solvent that is liquid at room temperature is preferably an aprotic organic solvent, and for example, one or more of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate (EP), propyl propionate (PP), methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, sultone, etc. can be used.

[0081] By using one or more flame-retardant and non-volatile ionic liquids (room-temperature molten salts) as an organic solvent that is liquid at room temperature, it is possible to prevent the battery cell from exploding or catching fire even if the internal temperature rises due to an internal short circuit or overcharging of the battery cell. The ionic liquid is composed of a cation and an anion, and includes an organic cation and an anion. Examples of organic cations used in the organic solvent include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, and aromatic cations such as imidazolium cations and pyridinium cations. Examples of anions used in the organic solvent include monovalent amide anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkylsulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.

[0082] The lithium salt dissolved in the organic solvent is, for example, LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiAlCl 4 , LiSCN, LiBr, LiI, Li 2 SO 4 , Li 2 B 10 Cl 10 , Li 2 B 12 Cl 12 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 4 F 9 SO 2 ) (CF3 SO 2 ), and LiN(C 2 F 5 SO 2 ) 2 One or more selected from the above can be used.

[0083] <Additives> The organic solvent may contain an additive. The additive can suppress reactive decomposition of the electrolyte that may occur on the positive electrode surface or the negative electrode surface when the secondary battery is operated at high voltage and / or high temperature. Examples of additives that can be used include vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), and lithium bis(oxalate)borate (LiBOB). LiBOB is particularly preferred because it easily forms a good coating. VC or FEC is preferred because it can form a good coating on the negative electrode during charge and discharge, improving cycle characteristics.

[0084] The compound represented by the following general formula (G1) may be contained as an additive: The compound represented by the following general formula (G1) has two cyano groups and can be called a dinitrile compound.

[0085]

[0086] In the general formula (G1), R represents a hydrocarbon having 1 to 5 carbon atoms. Preferably, in the general formula (G1), R represents a hydrocarbon having 2 to 4 carbon atoms.

[0087] Specific examples of the general formula (G1) include succinonitrile, glutaronitrile, and adiponitrile (ADN).

[0088] The structural formula (H1) of succinonitrile is shown below.

[0089]

[0090] The structural formula (H2) of glutaronitrile is shown below.

[0091]

[0092] The structural formula (H3) of adiponitrile is shown below.

[0093]

[0094] Although not applicable to the above general formula (G1), as an example of a dinitrile compound, the structural formula (H4) of ethylene glycol bis(propionitrile) ether (EGBE) is shown below.

[0095]

[0096] As the additive, one or more dinitrile compounds can be used.

[0097] Fluorobenzene may also be added to the organic solvent. The concentration of the additive may be, for example, 0.1 wt% to 5 wt% of the total electrolyte solution. PS or EGBE are preferred because they form a good coating on the positive electrode during charge and discharge, improving cycle characteristics. FB is preferred because it improves the wettability of the organic solvent to the positive and negative electrodes. Dinitrile compounds are preferred because their nitrile groups orient to the positive and negative electrodes, inhibiting oxidative decomposition of the organic solvent and improving voltage resistance. Furthermore, dinitrile compounds are preferred because they can prevent copper dissolution during overdischarge when a copper-containing current collector is used on the negative electrode. Considering the use of secondary batteries at high voltages, adding a nitrile compound is preferred.

[0098] The organic solvent does not need to be liquid at room temperature; a semi-solid material called a polymer gel electrolyte can be used instead. Using a polymer gel electrolyte increases safety against leakage and other issues. It also allows for thinner and lighter battery cells.

[0099] Examples of polymers that can be gelled include silicone gel, acrylic gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, and fluorine-based polymer gel.

[0100] Examples of polymers that can be used include polymers having a polyalkylene oxide structure such as polyethylene oxide (PEO), PVDF, polyacrylonitrile, and copolymers containing these. For example, PVDF-HFP, which is a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The polymer formed may also have a porous shape.

[0101] [Separator] The secondary battery preferably has a separator. Examples of separators that can be used include those made of paper, nonwoven fabric, glass fiber, ceramics, or synthetic fibers such as nylon (polyamide), vinylon (polyvinyl alcohol fiber), polyester, acrylic, polyolefin, and polyurethane. The separator is preferably processed into an envelope shape and disposed so as to encase either the positive electrode or the negative electrode.

[0102] The separator may have a multilayer structure. For example, an organic film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine-based material, a polyamide material, or a mixture of these. Examples of ceramic materials include aluminum oxide particles and silicon oxide particles. Examples of fluorine-based materials include PVDF and polytetrafluoroethylene. Examples of polyamide materials include nylon and aramid (meta-aramid, para-aramid).

[0103] Coating with ceramic materials improves oxidation resistance, suppressing separator degradation during high-voltage charging and discharging and improving the reliability of secondary batteries. Coating with fluorine-based materials also improves adhesion between the separator and electrodes, improving output characteristics. Coating with polyamide-based materials, especially aramid, improves heat resistance, improving the safety of secondary batteries.

[0104] For example, both sides of a polypropylene film may be coated with a mixed material of aluminum oxide and aramid, or the surface of the polypropylene film that contacts the positive electrode may be coated with a mixed material of aluminum oxide and aramid, and the surface that contacts the negative electrode may be coated with a fluorine-based material.

[0105] When a separator with a multilayer structure is used, the safety of the secondary battery can be maintained even if the overall thickness of the separator is thin, and therefore the discharge capacity per volume of the secondary battery can be increased.

[0106] [Negative Electrode] The negative electrode includes a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer may also include a conductive material and a binder.

[0107] [Negative Electrode Active Material] The negative electrode active material may be, for example, lithium metal or an alloy material (alloy with copper, tin, or cobalt). Alternatively, a carbon material or silicon may be used. Examples of the carbon material include graphite, graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon nanotubes, graphene, and carbon black.

[0108] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, spherical graphite having a spherical shape can be used as the artificial graphite. For example, MCMB may have a spherical shape and is preferred. Furthermore, it is relatively easy to reduce the surface area of ​​MCMB and this may be preferred. Examples of natural graphite include flake graphite and spherical natural graphite.

[0109] When lithium ions are inserted into graphite (when a lithium-graphite intercalation compound is formed), graphite exhibits a low potential similar to that of lithium metal (0.05 V to 0.3 V vs. Li / Li + This allows the lithium-ion secondary battery to exhibit a high operating voltage. The conductive material and binder that can be contained in the negative electrode active material layer can be the same materials as the conductive material and binder that can be contained in the positive electrode active material layer.

[0110] [Negative Electrode Current Collector] For the negative electrode current collector, in addition to copper, the same materials as those for the positive electrode current collector can be used.

[0111] [Coin-type secondary battery] An example of a coin-type secondary battery manufactured using the above-described positive electrode, electrolyte, separator, and negative electrode will be described. Fig. 3A is an exploded perspective view of a coin-type (single-layer flat) secondary battery, Fig. 3B is an external view, and Fig. 3C is a cross-sectional view thereof. Coin-type secondary batteries are mainly used in small electronic devices.

[0112] 3A is a schematic diagram that shows the overlapping of components (upper and lower relationships and positional relationships) for ease of understanding, and therefore, FIGS. 3A and 3B are not completely corresponding views.

[0113] In Fig. 3A, a positive electrode 304, a separator 310, a negative electrode 307, a spacer 322, and a washer 312 are stacked. These are sealed with a negative electrode can 302 and a positive electrode can 301 by a gasket. Note that the gasket for sealing is not shown in Fig. 3A. The spacer 322 and the washer 312 are used to protect the inside or to fix the position inside the can when the positive electrode can 301 and the negative electrode can 302 are crimped together. The spacer 322 and the washer 312 are made of stainless steel or an insulating material.

[0114] A positive electrode 304 has a laminated structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 .

[0115] FIG. 3B is a perspective view of the completed coin-type secondary battery.

[0116] In the coin-type secondary battery 300, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, are insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed by a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed by a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. The negative electrode 307 is not limited to a laminated structure, and may be formed of lithium metal foil or a lithium-aluminum alloy foil.

[0117] It is to be noted that the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 each only need to have an active material layer formed on one side.

[0118] The positive electrode can 301 and the negative electrode can 302 can be made of a metal such as nickel, aluminum, or titanium that is corrosion-resistant to the electrolyte, or an alloy of these metals or an alloy of these metals with other metals (e.g., stainless steel). Furthermore, to prevent corrosion by the electrolyte, etc., they are preferably coated with nickel, aluminum, or the like. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.

[0119] These negative electrode 307, positive electrode 304, and separator 310 are immersed in an electrolyte solution, and as shown in FIG. 3C , the positive electrode 304, separator 310, negative electrode 307, and negative electrode can 302 are stacked in this order with the positive electrode can 301 facing downwards, and the positive electrode can 301 and the negative electrode can 302 are crimped together via a gasket 303, thereby producing a coin-type secondary battery 300.

[0120] By having the above-described configuration, the coin-type secondary battery 300 can have a high discharge capacity and excellent cycle characteristics.

[0121] Embodiment 2 Although an example of a coin-type secondary battery has been shown in Embodiment 1, in this embodiment, examples of manufacturing a cylindrical secondary battery and a laminated secondary battery will be described below.

[0122] [Cylindrical Secondary Battery] An example of a cylindrical secondary battery manufactured using the positive electrode, electrolyte, separator, and negative electrode described in Embodiment 1 will be described with reference to Fig. 4A . As shown in Fig. 4A , a cylindrical secondary battery 616 has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap 601 and the battery can (external can) 602 are insulated from each other by a gasket (insulating packing) 610.

[0123] 4B is a schematic diagram showing a cross section of a cylindrical secondary battery. The cylindrical secondary battery shown in FIG. 4B has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and battery can (external can) 602 are insulated by a gasket (insulating packing) 610.

[0124] A battery element is provided inside a hollow cylindrical battery can 602, in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with a separator 605 sandwiched between them. Although not shown, the battery element is wound around a central axis. One end of the battery can 602 is closed and the other end is open. The battery can 602 can be made of a metal, such as nickel, aluminum, or titanium, or an alloy of these metals or an alloy of these metals with other metals (e.g., stainless steel), which is corrosion-resistant to the electrolyte. Furthermore, it is preferable to coat the battery can 602 with nickel, aluminum, or the like to prevent corrosion by the electrolyte. Inside the battery can 602, the wound battery element, in which the positive electrode, negative electrode, and separator are wound, is sandwiched between a pair of opposing insulating plates 608 and 609. A nonaqueous electrolyte (not shown) is injected inside the battery can 602, in which the battery element is provided. The nonaqueous electrolyte may be the same as that used in coin-type secondary batteries.

[0125] Since the positive and negative electrodes used in a cylindrical storage battery are wound, it is preferable to form active materials on both sides of the current collector.

[0126] By using the positive electrode active material 200A of one embodiment of the present invention for the positive electrode 604, a high-capacity and lightweight cylindrical secondary battery 616 can be provided.

[0127] A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. Both the positive electrode terminal 603 and the negative electrode terminal 607 can be made of a metal material such as aluminum. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 613, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 613 is electrically connected to the positive electrode cap 601 via a PTC (Positive Temperature Coefficient) element 611. The safety valve mechanism 613 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the increase in internal pressure of the battery exceeds a predetermined threshold. The PTC element 611 is a thermosensitive resistor whose resistance increases as the temperature increases, and the increased resistance limits the amount of current to prevent abnormal heat generation. The PTC element 611 is made of barium titanate (BaTiO 3 )-based semiconductor ceramics, etc. can be used.

[0128] 4C shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616. The positive electrodes of each secondary battery are in contact with and electrically connected to conductors 624 separated by insulators 625. The conductors 624 are electrically connected to a control circuit 620 via wiring 623. The negative electrodes of each secondary battery are electrically connected to the control circuit 620 via wiring 626. The control circuit 620 may be a charge / discharge control circuit that performs charging and discharging, or a protection circuit that prevents overcharging and / or overdischarging.

[0129] 4D shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616, which are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of secondary batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 by wiring 627. The plurality of secondary batteries 616 may be connected in parallel, in series, or in parallel and then further connected in series. By configuring the power storage system 615 to have a plurality of secondary batteries 616, it is possible to extract a large amount of power.

[0130] A plurality of secondary batteries 616 may be connected in parallel and then further connected in series.

[0131] Furthermore, a temperature control device may be provided between the multiple secondary batteries 616. When the secondary batteries 616 are overheated, they can be cooled by the temperature control device, and when the secondary batteries 616 are too cold, they can be heated by the temperature control device. This makes it difficult for the performance of the power storage system 615 to be affected by the outside air temperature.

[0132] 4D , the power storage system 615 is electrically connected to a control circuit 620 via wiring 621 and wiring 622. The wiring 621 is electrically connected to the positive electrodes of the plurality of secondary batteries 616 via a conductive plate 628, and the wiring 622 is electrically connected to the negative electrodes of the plurality of secondary batteries 616 via a conductive plate 614.

[0133] <Laminated Lithium-ion Battery> An example of a laminated lithium-ion battery 500 is shown in FIGS. 5A and 5B . FIGS. 5A and 5B are external views, and the lithium-ion battery 500 includes the electrolyte and separator (not shown in FIG. 12 ) described in the above embodiment, a negative electrode 506, and a positive electrode 507. In the lithium-ion battery 500, the negative electrode 506 preferably has a larger area than the positive electrode 507. The lithium-ion battery 500 further includes a negative electrode lead electrode 510 electrically connected to the negative electrode 506 and a positive electrode lead electrode 511 electrically connected to the positive electrode 507. The electrolyte layer, the negative electrode 506, and the positive electrode 507 are housed in an outer casing 509, and a portion of the negative electrode lead electrode 510 and a portion of the positive electrode lead electrode 511 protrude from the outer casing 509. The outer casing 509 has an adhesive region 508 on a portion of its outer periphery. Fig. 5A shows an example in which the negative electrode lead electrode 510 and the positive electrode lead electrode 511 protrude from the same side of the exterior body 509, and the adhesive region 508 is located at least on the side from which each lead electrode protrudes and two sides adjacent to that side. Fig. 5B shows an example in which the side from which the negative electrode lead electrode 510 protrudes from the exterior body 509 and the side from which the positive electrode lead electrode 511 protrudes from the exterior body 509 face each other, and the adhesive region 508 is located at least on the two sides from which each lead electrode protrudes and one side sandwiched between those two sides. In Figs. 5A and 5B, the sides on which the adhesive region 508 is not located may correspond to the sides on which the exterior body 509 is folded.

[0134] <Method for Manufacturing Laminated Secondary Battery> An example of a method for manufacturing a laminated secondary battery 500, the external views of which are shown in FIGS. 5A and 5B , which is manufactured using the above-described positive electrode, electrolyte, separator, and negative electrode, will be described with reference to FIGS. 6A to 6C .

[0135] First, a positive electrode 503 and a negative electrode 506 are prepared as shown in FIG. 6A . Next, as shown in FIG. 6B , the negative electrode 506, a separator 507, and a positive electrode 503 are laminated together. Here, an example is shown in which five pairs of negative electrodes 506 and four pairs of positive electrodes 503 are used. This can also be called a laminate consisting of the negative electrode 506, the separator 507, and the positive electrode 503. Next, the tab regions of the positive electrodes 503 are bonded together, and a positive electrode lead electrode 510 is bonded to the tab region of the outermost positive electrode 503. For example, ultrasonic welding or the like may be used for bonding. Similarly, the tab regions of the negative electrodes 506 are bonded together, and a negative electrode lead electrode 511 is bonded to the tab region of the outermost negative electrode 506.

[0136] Next, as shown in FIG. 6C, the above-described laminate is placed on an exterior body 509.

[0137] Next, as shown in Fig. 6C, the exterior body 509 is folded at the portion indicated by the dashed line. Thereafter, the outer periphery of the exterior body 509 is joined. For example, thermocompression bonding or the like may be used for joining. At this time, an area (hereinafter referred to as an inlet) that is not joined is provided in a part (or one side) of the exterior body 509 so that an electrolyte can be introduced later.

[0138] Next, the electrolyte solution is introduced into the inside of the exterior body 509 through an inlet provided in the exterior body 509. The introduction of the electrolyte solution is preferably carried out under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is joined. In this manner, the laminated secondary battery 500 can be produced.

[0139] By using the powdered positive electrode active material 200A of one embodiment of the present invention for the positive electrode 503, the secondary battery 500 can have a high capacity and a light weight.

[0140] This embodiment mode can be implemented in appropriate combination with other embodiment modes or examples.

[0141] Embodiment 3 In this embodiment, an example in which a secondary battery which is one embodiment of the present invention is mounted on an electronic device will be described with reference to FIGS. 7A to 8C. FIG.

[0142] 7A shows an example of a wearable device. Wearable devices use high-capacity, lightweight secondary batteries as a power source. Furthermore, in order to enhance splash-proof, water-resistant, or dust-proof performance when used at home or outdoors, there is a demand for wearable devices that can be charged wirelessly as well as via wired charging, with an exposed connector.

[0143] For example, the secondary battery of one embodiment of the present invention can be mounted on an eyeglasses-type device 4000 as shown in FIG. 7A . The eyeglasses-type device 4000 includes a frame 4000 a and a display unit 4000 b. Mounting the secondary battery on the temples of the curved frame 4000 a makes it possible to provide the eyeglasses-type device 4000 with a lightweight design, a good weight balance, and a long continuous use time. The inclusion of the secondary battery of one embodiment of the present invention allows for a configuration that can accommodate space savings associated with a smaller housing.

[0144] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on the headset device 4001. The headset device 4001 includes at least a microphone unit 4001a, a flexible pipe 4001b, and an earphone unit 4001c. A high-capacity, lightweight secondary battery can be provided in the flexible pipe 4001b and / or the earphone unit 4001c. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving due to a smaller housing can be realized.

[0145] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on a device 4002 that can be directly attached to the body. A high-capacity and lightweight secondary battery 4002b can be provided in a thin housing 4002a of the device 4002. By providing the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving due to miniaturization of the housing can be realized.

[0146] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on a device 4003 that can be attached to clothing. A high-capacity and lightweight secondary battery 4003b can be provided in a thin housing 4003a of the device 4003. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving due to miniaturization of the housing can be realized.

[0147] Furthermore, the secondary battery of one embodiment of the present invention can be mounted on the belt-type device 4006. The belt-type device 4006 includes a belt portion 4006a and a wireless power receiving portion 4006b, and a high-capacity, lightweight secondary battery can be mounted inside the belt portion 4006a. By including the secondary battery of one embodiment of the present invention, a configuration that can accommodate space saving due to miniaturization of the housing can be realized.

[0148] Furthermore, the secondary battery of one embodiment of the present invention can be mounted on the wristwatch device 4005. The wristwatch device 4005 has a display portion 4005a and a belt portion 4005b, and a high-capacity, lightweight secondary battery can be provided on the display portion 4005a or the belt portion 4005b. By providing the secondary battery of one embodiment of the present invention, a configuration that can accommodate space saving due to miniaturization of the housing can be realized.

[0149] The display unit 4005a can display not only the time but also various other information such as incoming emails and phone calls.

[0150] Furthermore, since the wristwatch device 4005 is a wearable device that is worn directly on the arm, it may be equipped with sensors that measure the user's pulse, blood pressure, etc. Data on the user's exercise volume and health can be accumulated to manage the user's health.

[0151] FIG. 7B shows a perspective view of the wristwatch-type device 4005 removed from the wrist.

[0152] 7C shows a side view of the device 4005. Fig. 7C shows that the device 4005 includes a secondary battery 913. The secondary battery 913 is provided at a position overlapping the display portion 4005a, and is small and lightweight.

[0153] 7D shows an example of a wireless earphone. Here, the wireless earphone is shown as having a pair of main bodies 4100a and 4100b, but this does not necessarily have to be a pair.

[0154] The main bodies 4100a and 4100b each have a driver unit 4101, an antenna 4102, and a secondary battery 4103. They may also have a display unit 4104. They also preferably have a substrate on which a circuit such as a wireless IC is mounted, a charging terminal, and the like. They may also have a microphone.

[0155] The case 4110 has a secondary battery 4111. It is preferable that the case 4110 also has a board on which circuits such as a wireless IC and a charge control IC are mounted, and a charging terminal. It may also have a display unit, buttons, and the like.

[0156] The main units 4100a and 4100b can wirelessly communicate with other electronic devices such as smartphones. This allows sound data and the like sent from other electronic devices to be played back on the main units 4100a and 4100b. If the main units 4100a and 4100b have microphones, the sound picked up by the microphones can be sent to the other electronic device, and the sound data after processing by the electronic device can be sent back to the main units 4100a and 4100b for playback. This allows the devices to be used as, for example, translation devices.

[0157] The secondary battery 4103 included in the main body 4100a can be charged from the secondary battery 4111 included in the case 4110. A coin-type secondary battery, a cylindrical secondary battery, or the like can be used as the secondary battery 4111 and the secondary battery 4103. The secondary battery obtained in Embodiment 1 is lightweight and has a high energy density. Using the secondary battery 4103 and the secondary battery 4111 can contribute to space saving and weight reduction associated with miniaturization of the wireless earphone.

[0158] 8A shows an example of a cleaning robot. The cleaning robot 6300 includes a display unit 6302 arranged on the top surface of a housing 6301, a plurality of cameras 6303 arranged on the side surfaces, a brush 6304, operation buttons 6305, a secondary battery 6306, various sensors, and the like. Although not shown, the cleaning robot 6300 is provided with tires, a suction port, and the like. The cleaning robot 6300 can move by itself, detect dust 6310, and suck up the dust from a suction port arranged on the bottom surface.

[0159] For example, the cleaning robot 6300 can analyze an image captured by the camera 6303 to determine whether or not there is an obstacle such as a wall, furniture, or a step. Furthermore, when an object that may become entangled in the brush 6304, such as a wire, is detected through image analysis, the rotation of the brush 6304 can be stopped. The cleaning robot 6300 includes a secondary battery 6306 according to one embodiment of the present invention and a semiconductor device or an electronic component therein. By using the secondary battery 6306 according to one embodiment of the present invention in the cleaning robot 6300, the weight of the cleaning robot 6300 can be reduced, and therefore the cleaning robot 6300 can be an electronic device with a long operating time.

[0160] Fig. 8B shows an example of a robot. The robot 6400 shown in Fig. 8B includes a secondary battery 6409, an illuminance sensor 6401, a microphone 6402, an upper camera 6403, a speaker 6404, a display unit 6405, a lower camera 6406, an obstacle sensor 6407, a movement mechanism 6408, a computing device, etc.

[0161] The microphone 6402 has a function of detecting the user's speaking voice, environmental sounds, etc. The speaker 6404 has a function of emitting sound. The robot 6400 can communicate with the user using the microphone 6402 and the speaker 6404.

[0162] The display unit 6405 has a function of displaying various information. The robot 6400 can display information desired by the user on the display unit 6405. The display unit 6405 may be equipped with a touch panel. The display unit 6405 may also be a detachable information terminal, which can be installed in a fixed position on the robot 6400 to enable charging and data transfer.

[0163] The upper camera 6403 and the lower camera 6406 have the function of capturing images of the surroundings of the robot 6400. Furthermore, the obstacle sensor 6407 can detect the presence or absence of obstacles in the direction of travel when the robot 6400 moves forward using the movement mechanism 6408. The robot 6400 can recognize the surrounding environment and move safely using the upper camera 6403, the lower camera 6406, and the obstacle sensor 6407.

[0164] The robot 6400 includes a secondary battery 6409 according to one embodiment of the present invention and a semiconductor device or an electronic component inside the robot 6400. By using the secondary battery according to one embodiment of the present invention in the robot 6400, the weight of the entire robot 6400 can be reduced, and the robot 6400 can be an electronic device with a long operating time.

[0165] 8C shows an example of an air vehicle (also called a drone). The air vehicle 6500 shown in FIG. 8C has a propeller 6501, a camera 6502, a secondary battery 6503, and the like, and has the function of flying autonomously.

[0166] For example, image data captured by the camera 6502 is stored in the electronic component 6504. The electronic component 6504 can analyze the image data and detect the presence or absence of obstacles during movement. Furthermore, the electronic component 6504 can estimate the remaining battery charge from a change in the storage capacity of the secondary battery 6503. The flying object 6500 includes the secondary battery 6503 according to one embodiment of the present invention therein. By using the secondary battery according to one embodiment of the present invention in the flying object 6500, the secondary battery is lightweight and has a high capacity, and therefore the flying object 6500 can be made lighter overall and have a longer operating time.

[0167] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0168] Embodiment 4 In this embodiment, an example in which a secondary battery of one embodiment of the present invention is mounted on a vehicle will be described.

[0169] By installing a secondary battery in a vehicle, next-generation clean energy vehicles such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs) can be realized.

[0170] FIG. 9 illustrates an example of a vehicle using a secondary battery according to one embodiment of the present invention. An automobile 8400 shown in FIG. 9A is an electric automobile using an electric motor as a power source for traveling. Alternatively, it is a hybrid automobile that can appropriately select and use an electric motor or an engine as a power source for traveling. By using one embodiment of the present invention, a vehicle with a long cruising distance can be realized. Furthermore, the automobile 8400 includes a secondary battery 8402. For example, modules of the secondary battery 8402 can be arranged on the floor of the interior of the vehicle. The secondary battery 8402 not only drives the electric motor 8406 but also supplies power to light-emitting devices such as a headlight 8401 and a room light (not shown).

[0171] The secondary battery can also supply power to display devices such as a speedometer and a tachometer included in the automobile 8400. The secondary battery can also supply power to semiconductor devices such as a navigation system included in the automobile 8400.

[0172] The automobile 8500 shown in FIG. 9B can charge its secondary battery by receiving power from an external charging facility using a plug-in system and / or a wireless power supply system. FIG. 9B shows a state in which a ground-mounted charging device 8021 charges a secondary battery 8024 mounted on the automobile 8500 via a cable 8022. The charging method and connector specifications may be determined as appropriate using a predetermined system, such as CHAdeMO (registered trademark) or Combo. The charging device 8021 may be a charging station installed in a commercial facility or a household power source. For example, plug-in technology can be used to charge the secondary battery 8024 mounted on the automobile 8500 using external power supply. Charging can be performed by converting AC power to DC power using a conversion device, such as an AC-DC converter.

[0173] Although not shown, a power receiving device can be mounted on a vehicle and power can be supplied contactlessly from a ground-based power transmitting device to charge the vehicle. In the case of this contactless power supply method, by incorporating a power transmitting device into the road and / or exterior wall, charging can be performed not only while the vehicle is stopped but also while the vehicle is moving. This contactless power supply method can also be used to transmit and receive power between vehicles. Furthermore, a solar cell can be installed on the exterior of the vehicle to charge the secondary battery while the vehicle is stopped and / or moving. For such contactless power supply, an electromagnetic induction method and / or a magnetic field resonance method can be used.

[0174] 9C shows an example of a two-wheeled vehicle using the secondary battery of one embodiment of the present invention. A scooter 8600 shown in FIG. 9C includes a secondary battery 8602, a side mirror 8601, and a turn signal light 8603. The secondary battery 8602 can supply electricity to the turn signal light 8603.

[0175] 9C , the secondary battery 8602 can be stored in the under-seat storage 8604. Even if the under-seat storage 8604 is small, the secondary battery 8602 can be stored in the under-seat storage 8604. The secondary battery 8602 is removable, and when charging, the secondary battery 8602 can be carried indoors, charged, and stored before riding.

[0176] According to one aspect of the present invention, the secondary battery can be made lighter and the discharge capacity of the secondary battery can be increased. Therefore, the capacity per unit weight can be increased, allowing the secondary battery itself to be made smaller and lighter. Reducing the size and weight of the secondary battery itself contributes to reducing the weight of the vehicle, thereby improving the cruising range. Furthermore, the secondary battery mounted on the vehicle can also be used as a power supply source for purposes other than the vehicle. In this case, for example, it is possible to avoid using a commercial power source during peak power demand periods. Avoiding the use of a commercial power source during peak power demand periods can contribute to energy conservation and the reduction of carbon dioxide emissions.

[0177] 10A is an example of an electric bicycle using the secondary battery of one embodiment of the present invention. The secondary battery of one embodiment of the present invention can be applied to an electric bicycle 8700 shown in FIG. 10A. The power storage device of one embodiment of the present invention includes, for example, a plurality of secondary batteries and a charge / discharge control unit.

[0178] The electric bicycle 8700 includes a power storage device 8702. The power storage device 8702 can supply electricity to a motor (electric unit) that assists the rider. The power storage device 8702 is portable and is shown removed from the bicycle in FIG. 10B, where it corresponds to a secondary battery unit. The power storage device 8702 also includes a plurality of built-in batteries 8701, and a display unit 8703 can display the remaining battery charge. The remaining charge is also displayed on the display unit 8703. The power storage device 8702 also includes a charge / discharge control unit 8704 that can control charging or detect abnormalities of the secondary battery. The charge / discharge control unit 8704 is electrically connected to the positive and negative electrodes of the battery 8701. The electric vehicle main unit of the electric bicycle 8700 also includes an operation unit 8712 provided in the handle portion. The operation unit 8712 includes a display unit 8713, a power switch 8714, and a power storage device 8711.

[0179] Since the secondary battery of one embodiment of the present invention is made of inexpensive materials, the cost of the electric bicycle 8700 can be significantly reduced.

[0180] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0181] In this example, a battery cell was fabricated and a charge / discharge test was carried out, and the results are shown. Note that the present invention is not limited to the following example.

[0182] The procedure for fabricating a battery cell using the powdered positive electrode active material 200A obtained in the first embodiment will be described below. The procedure will be explained with reference to FIGS. 1 and 2.

[0183] (Preparation of Graphene Oxide Dispersion 901) First, a graphene oxide aqueous dispersion (NiSiNa material, product name Rap GO (TQ-11)) was prepared. The concentration of the graphene oxide aqueous dispersion was approximately 4 wt %. 3.75 g of the graphene oxide aqueous dispersion was diluted with pure water to prepare 500 mL of a dispersion. The pH of the dispersion after stirring was 3.05.

[0184] Graphene oxide is sometimes sold as a powder. In such cases, an aqueous dispersion of graphene oxide can be prepared by adding water to the powder and stirring thoroughly. The composition of graphene oxide can be estimated by weighing it using simultaneous thermogravimetric differential thermal analysis / mass spectrometry (TG-DTA / MS).

[0185] Graphene oxide is a polar substance containing functional groups such as epoxy, carbonyl, carboxyl, and hydroxyl groups, and the oxygen in these functional groups is negatively charged in polar solvents. Therefore, different graphene oxides are less likely to aggregate with each other, but they interact strongly with polar solvents such as N-methyl-2-pyrrolidone (NMP). Therefore, the interaction between the functional groups, such as epoxy groups, contained in graphene oxide and the polar solvent is thought to inhibit aggregation of graphene oxides, resulting in uniform dispersion of graphene oxide in the polar solvent.

[0186] Next, 1.52 g of anhydrous sodium thiosulfate (Na 2 S 2 O 3 ) was added. The mixture was stirred in an ice bath for 10 minutes. The pH at this time was 3.24.

[0187] Next, 0.179 L of 0.024 M hydrochloric acid was added at a rate of 5 mL / min. Stirring was continued for 10 hours or more in an ice bath. The pH after stirring was 2.29. The reaction resulting from the addition of hydrochloric acid can be represented by the following reaction formula:

[0188]

[0189] Next, the mixture was suction-filtered using a Merck Omnipore membrane filter with a mesh size of 0.1 μm to obtain a precipitate. The mixture was washed with pure water, filtered again, and then purified water was added to adjust the volume to 100 ml. Then, ultrasonic waves at a frequency of 40 kHz were applied for 15 minutes.

[0190] Then, 20 ml of a 1 M aqueous solution of lithium ascorbate was added. The 1 M aqueous solution of lithium ascorbate was prepared in advance by adding lithium hydroxide to a 1 M aqueous solution of ascorbic acid to neutralize it.

[0191] The ascorbic acid used was L-ascorbic acid with a purity of 99.6% manufactured by Wako Pure Chemical Industries, Ltd. The oxidation-reduction reaction of ascorbic acid can be represented by reaction formula (A-1).

[0192]

[0193] Next, in order to reduce the graphene oxide, the mixture was refluxed at 95° C. for 90 minutes. After the reflux was completed, the mixture was allowed to cool naturally.

[0194] The mixture was then filtered using a Merck Omnipore membrane filter with a mesh size of 0.1 μm. After filtration, the filter was washed with pure water. The residue remaining on the filter paper was dried under vacuum. The residue was then collected by sieving it through a 53 μm mesh sieve in a dry room. The collected amount was 0.066 g.

[0195] By repeating the above process, a sufficient amount of powdered positive electrode active material 200A was obtained.

[0196] Then, a positive electrode is produced as follows, an example of which flow is shown in FIG.

[0197] First, each material was weighed in a dry room. The powdered positive electrode active material 200A, the conductive additive 906, and the binder 907 were weighed so that the weight ratio of each was 80 wt %, 10 wt %, and 10 wt %. In this example, acetylene black was used as the conductive additive 906, and an NMP solution of PVDF (solvent 908) was used as the binder 907.

[0198] Acetylene black was added to the powdered positive electrode active material 200A, and an NMP solution was added as the solvent 908 to perform hard kneading, and then an NMP solution of PVDF was added and further kneaded. Then, the NMP solution was added as the viscosity adjusting solvent 909, and the mixture was kneaded to prepare a slurry.

[0199] The slurry prepared by the above method was applied to a current collector (aluminum foil) and dried at 50°C for 12 hours or more under a reduced pressure atmosphere to volatilize the NMP solution. Further, a heat treatment was performed under a reduced pressure atmosphere at 100°C to 130°C for 30 minutes to less than 2 hours to prepare an electrode (cathode 201) in which a positive electrode active material layer was formed on the current collector. The ultimate vacuum pressure during heating was approximately 1000 Pa. The temperature range under the reduced pressure atmosphere was 20°C to 120°C, and the time required to raise the temperature from 20°C to 120°C was approximately 15 minutes. In this embodiment, the heat treatment under a reduced pressure atmosphere at 120°C for 1 hour crystallizes the PVDF contained in the positive electrode active material layer, improving the adhesion of the electrode.

[0200] The positive electrode 201 was punched into a disk shape with a diameter of 12 mm. This was used as the positive electrode to make a 2032-type coin battery, which was used as a battery cell. The battery cell used polypropylene (PP) as a separator, lithium metal as a negative electrode, and lithium hexafluorophosphate (LiPF ) in a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7 as an electrolyte. 6 The battery cell was assembled in a glove box filled with inert gas.

[0201] A cross-sectional schematic diagram of this battery cell is shown in Figure 11. As shown in Figure 11, the battery cell has a laminated structure with a separator between a positive electrode 201 and a negative electrode 202. The positive electrode 201 has a positive electrode active material layer containing sulfur on a positive electrode current collector. The positive electrode active material layer contains sulfur on the surface of flake-shaped graphene (reduced graphene oxide). An electrolyte is also present between the positive electrode 201 and the negative electrode 202, and in the holes in the separator.

[0202] (Characteristics of Storage Battery) The results of constant current charge / discharge characteristics obtained by measuring the battery characteristics of the battery cell at a constant current are shown in FIG.

[0203] The charging mode was CC (Constant Current) mode, and the discharging mode was also CC (Constant Current). The discharge rate and charge rate were 10 mA / g (the weight used in the calculation is the weight of the positive electrode active material layer). The cutoff voltage had a lower limit of 1.4 V and an upper limit of 2.8 V. The charge / discharge test was performed at room temperature (approximately 25°C).

[0204] The discharge rate and charge rate are values ​​calculated by considering the weight of reduced graphene oxide, i.e., the powder positive electrode active material 200A (weight including reduced graphene), as the active material. In this specification, sulfur or a sulfur compound functions as the active material, and reduced graphene is a conductive material for imparting conductivity, but is considered to be included in the category of positive electrode active material. Furthermore, the positive electrode active material may consist solely of elemental sulfur or a sulfur compound. In such cases, the total weight of the elemental sulfur or sulfur compound may be measured, and the capacity per weight may be calculated. The positive electrode active material has fine particles of sulfurized active material attached to at least a portion of the reduced graphene, which is a conductive material. The fine particles of the active material are elemental sulfur, lithium disulfide, or lithium polysulfide.

[0205] That is, it was confirmed that a secondary battery using the powdered positive electrode active material A as the positive electrode active material can be charged and discharged, and has a large capacity per weight.

[0206] A cycle test was also performed. Cells made from electrodes that were not heated to 120°C were also prepared.

[0207] Before the cycle test, the battery cells were discharged at room temperature (25°C) at a constant current of 10 mA / g to 1.4 V (CC mode), and then charged at a constant current of 10 mA / g to 2.8 V (CC mode). After a 10-minute rest period, the cells were discharged at a constant current of 10 mA / g to 1.4 V (also called the cutoff voltage), and then charged at a constant current of 10 mA / g to 2.8 V. The 10-minute rest period was followed.

[0208] Thereafter, as the first discharge of the cycle test, the battery was discharged at a constant current of 10 mA / g at room temperature (25°C) to 1.4 V, and then, as the first charge, it was charged at a constant current of 2.8 V at a charge rate. This cycle was repeated 50 times. A 10-minute rest period was provided between each cycle.

[0209] The resulting cycle characteristics are shown in Figure 13. The sample heat-treated at 120°C for 1 hour under reduced pressure exhibited a higher capacity value than the sample not heat-treated at 120°C for 1 hour. The increase in capacity is thought to be due to the progress of crystallization of the material forming the positive electrode active material layer, specifically PVDF, which strengthened the bonding strength inside the positive electrode and at the interface between the positive electrode active material layer and the current collector, thereby reducing the electrode contact resistance. It is known that the crystallization temperature of the PVDF used in this example is between 135°C and 140°C. Heating a sulfur-containing positive electrode active material layer at a relatively high temperature, such as 135°C to 140°C, may result in the complete evaporation of sulfur within the positive electrode. Therefore, by limiting the heat treatment to a temperature between 100°C and 130°C under reduced pressure for 30 minutes to less than 2 hours, the amount of sulfur evaporation can be reduced and the contact resistance of the positive electrode can be reduced.

[0210] 200A: positive electrode active material, 201: positive electrode, 202: negative electrode, 300: secondary battery, 301: positive electrode can, 302: negative electrode can, 303: gasket, 304: positive electrode, 305: positive electrode current collector, 306: positive electrode active material layer, 307: negative electrode, 308: negative electrode current collector, 309: negative electrode active material layer, 310: separator, 312: washer, 322: spacer, 500: secondary battery, 503: positive electrode, 506: negative electrode, 507: separator, 509: outer casing, 510: positive electrode lead electrode, 511: negative electrode lead electrode, 601: positive electrode cap, 602: battery can, 603: positive electrode terminal, 604: positive electrode, 60 5: separator, 606: negative electrode, 607: negative electrode terminal, 608: insulating plate, 609: insulating plate, 611: PTC element, 613: safety valve mechanism, 614: conductive plate, 615: power storage system, 616: secondary battery, 620: control circuit, 621: wiring, 622: wiring, 623: wiring, 624: conductor, 625: insulator, 626: wiring, 627: wiring, 628: conductive plate, 890: carbon material, 893: pure water, 894: hydrochloric acid, 895: pure water, 896: mixed liquid, 901: dispersion liquid, 902: material, 903: first mixed liquid, 904: second mixed liquid, 907: binder, 908: solvent, 9 09: solvent, 913: secondary battery, 4000a: frame, 4000b: display unit, 4000: eyeglasses-type device, 4001a: microphone unit, 4001b: flexible pipe, 4001c: earphone unit, 4001: headset-type device, 4002a: housing, 4002b: secondary battery, 4002: device, 4003a: housing, 4003b: secondary battery, 4003: device, 4005a: display unit, 4005b: belt unit, 4005: wristwatch-type device, 4006a: belt unit, 4006b: wireless power supply receiving unit, 4006: belt-type device, 4100a : Main body, 4100b: Main body, 4101: Driver unit, 4102: Antenna, 4103: Secondary battery, 4104: Display unit, 4110: Case, 4111: Secondary battery, 6300: Cleaning robot, 6301: Housing, 6302: Display unit, 6303: Camera, 6304: Brush, 6305: Operation button, 6306: Secondary battery, 6310: Dust, 6400: Robot, 6401: Illuminance sensor, 6402: Microphone, 6403: Upper camera, 6404: Speaker, 6405: Display unit, 6406: Lower camera, 6407: Obstacle sensor, 6408: Moving mechanism,6409: Secondary battery, 6500: Aircraft, 6501: Propeller, 6502: Camera, 6503: Secondary battery, 6504: Electronic component, 8021: Charging device, 8022: Cable, 8024: Secondary battery, 8400: Automobile, 8401: Headlight, 8402: Secondary battery, 8406: Electric motor, 8500: Automobile, 8600: Scooter, 8601: Side mirror, 8602: Secondary battery, 8603: Turn signal light, 8604: Under-seat storage,

Claims

A method for producing a secondary battery including a positive electrode, a separator, an electrolyte, and a negative electrode, comprising the steps of: The water in which the graphene oxide is dispersed is mixed with thiosulfate, Hydrochloric acid is further added, mixed, and then filtered. The residue is dried to form a powder containing elemental sulfur; The powder is added to pure water and stirred, and then a mixed aqueous solution of ascorbic acid and lithium hydroxide is added. The mixed liquid is heated to reduce the graphene oxide, and then moisture is removed to obtain a powdered positive electrode active material. A conductive assistant, a solvent, and a binder having fluorine are added to the powdered positive electrode active material to form a slurry. The slurry is applied onto a positive electrode current collector and dried. A method for producing a secondary battery, comprising: heating under reduced pressure to crystallize the fluorine-containing binder; and forming the material containing elemental sulfur as a positive electrode active material layer to serve as the positive electrode.

2. The method for producing a secondary battery according to claim 1, wherein the separator and the electrolyte are disposed between the positive electrode and the negative electrode.

2. The method for producing a secondary battery according to claim 1, wherein the heating under reduced pressure after the application and drying of the slurry is performed at 100° C. or higher and 130° C. or lower for 30 minutes or longer and shorter than 2 hours. a positive electrode active material layer on a positive electrode current collector; a separator on the positive electrode active material layer; A negative electrode on the separator, the positive electrode active material layer has a plurality of graphenes, at least a portion of which is formed by subjecting graphene oxide to a reduction treatment, and has elemental sulfur on a surface of the graphene; The positive electrode active material layer at least partially comprises a crystallized binder.

5. The secondary battery according to claim 4, wherein the negative electrode is lithium metal.

5. The secondary battery according to claim 4, wherein the binder contains fluorine.

Citation Information

Patent Citations

  • Carbon-sulfur complex, electrochemical element using the same, and lithium ion battery

    JP2013214503A

  • Manufacturing method of electrode, electrode, storage battery, and electronic apparatus

    JP2016006767A

  • Binder composition for secondary battery electrode, secondary battery electrode mixture, secondary battery electrode and secondary battery

    JP2017117754A

  • Conformable alkali metal-sulfur batteries with deformable, conductive, quasi-solid electrodes

    JP2020525984A

  • Positive electrode for lithium secondary battery and lithium secondary battery including the same

    JP2022553033A