Vinyl polymer, and active energy ray-curable composition containing same
The vinyl polymer composition addresses the challenges of breaking strength, water resistance, and adhesion by incorporating specific structural units, resulting in efficient alkali solubility and suitable performance for diverse applications.
Patent Information
- Application Number
- PCT/JP2024/011052
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-03-21
- Publication Date
- 2024-11-28
AI Technical Summary
Existing active energy ray-curable compositions face challenges in achieving excellent breaking strength, water resistance, and adhesion to substrates after alkali development, while also requiring efficient removal of unexposed areas through alkali solubility.
A vinyl polymer with specific structural units, including alkyl acrylate, carboxy, and acryloyl or acrylamide groups, is developed, which has a tailored glass transition temperature, acid value, and acryloyl equivalent, allowing for improved curing properties and alkali solubility.
The vinyl polymer composition achieves excellent breaking strength, water resistance, and adhesion to substrates after alkali development, while enabling efficient removal of unexposed areas, making it suitable for various applications such as interlayer insulating films and pattern formation in display devices.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Vinyl polymer and active energy ray-curable composition containing the same
[0001] The present invention relates to an active energy ray-curable composition which, upon irradiation with active energy rays, gives a cured product which is excellent in breaking strength and water resistance and which has excellent adhesion to a substrate after alkali development, and which has excellent alkali solubility in unexposed areas, and to a vinyl polymer which gives such a composition.
[0002] Conventionally, active energy ray-curable compositions utilizing active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays have properties such as excellent workability in coating and high curing speed, and therefore have been widely used as photoresists, pigment-dispersed resists, spacers for liquid crystal display devices, adhesives, coating agents, sealants, excipients, etc. Acrylic polymers are widely used as the main component of active energy ray-curable compositions for such applications. Active energy ray-curable compositions containing acrylic polymers are described, for example, in the following Patent Documents 1 to 6.
[0003] Patent Document 1 discloses a photosensitive resin composition for use in photosensitive films, supported photosensitive films, printed wiring boards, and semiconductor devices, which contains (A-1) a (meth)acrylic copolymer containing an ethylenically unsaturated group and a carboxyl group and having a main chain glass transition temperature of 150°C or higher, (A-2) a (meth)acrylic copolymer containing an ethylenically unsaturated group and a carboxyl group and having a main chain glass transition temperature of -20°C or lower, (B) an inorganic filler having an average particle size of 0.5 μm or more and 2.5 μm or less, (C) a photopolymerization initiator, and (D) an epoxy resin, wherein the weight-average molecular weights of the components (A-1) and (A-2) are each 30,000 or less, and the content of the component (B) is 60% by mass or more and 85% by mass or less, when the total solid content of the photosensitive resin composition is 100% by mass.
[0004] Patent Document 2 discloses a colorant dispersion liquid for forming a colored pattern on, for example, a color filter substrate for a liquid crystal display device, a sensor substrate for a touch panel, or the like, which contains at least a colorant, an acrylic copolymer, and an organic solvent, wherein the acrylic copolymer has at least a structure having an ethylenically unsaturated group in the side chain, a structure having a tertiary amino group in the side chain and / or a structure having a quaternary ammonium salt in the side chain, a structure having a carboxyl group in the side chain, and a structure having an aromatic ring, and which has a base number of 5 to 70 mmol / 100 g, an acid value of 50 to 120 mg KOH / g, and a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography of 5,000 to 30,000.
[0005] Patent Document 3 discloses, for example, an insulating resin composition used in the manufacture of multilayer printed wiring boards, which comprises: (1) an alkali-soluble acrylic polymer and / or methacrylic polymer having a carboxyl group; (2) a polymerizable compound having one or more C═C unsaturated double bonds; (3) an ultraviolet polymerization initiator for the polymerizable compound (2); (4) a sensitizer for ultraviolet polymerization; (5) a thermal polymerization initiator for the polymerizable compound (2); (6) a crosslinked elastic polymer in the form of fine particles having a particle size of less than 1 μm and containing a carboxyl group; and (7) a fine particle material having a particle size of 1 to 10 μm, wherein a cured product of the composition is insoluble in chemicals, but the fine particle material (7) in the cured product is soluble in the chemicals.
[0006] Patent Document 4 discloses, for example, a resin composition for insulating materials, which is used as an interlayer insulating material for multilayer printed wiring boards, and which contains (1) an alkali-soluble acrylic polymer and / or methacrylic polymer having a carboxyl group, (2) a polymerizable compound having one or more C═C unsaturated double bonds, (3) a particulate crosslinked elastic polymer having an average particle size of 5 μm or less, and (4) a polymerization initiator capable of initiating polymerization of the C═C unsaturated double bonds by heating and / or irradiation with active energy rays.
[0007] Patent Document 5 discloses an active energy ray-curable composition for forming an optical film used as a polarizer protective film or the like, which contains: component (A): a (meth)acrylate polymer having a (meth)acryloyl group on a side chain, which is a reaction product of a (meth)acrylate polymer (a1) having a functional group reactive with a carboxyl group or a hydroxyl group on a side chain [hereinafter referred to as “polymer (a1)]” with a compound (a2) having a carboxyl group or a hydroxyl group and a (meth)acryloyl group and having a number average molecular weight of 180 or more [hereinafter referred to as “compound (a2)]”; and / or component (B): a (meth)acrylate polymer having a (meth)acryloyl group on a side chain, which is a reaction product of a (meth)acrylate polymer (b1) having a carboxyl group or a hydroxyl group on a side chain, obtained by copolymerizing compound (a2) with a monomer copolymerizable therewith, and compound (b2) having a functional group reactive with a carboxyl group or a hydroxyl group and a (meth)acryloyl group.
[0008] Furthermore, Patent Document 6 discloses an active energy ray-curable composition that contains a (meth)acrylate polymer (A) (hereinafter referred to as "component (A)") modified with an unsaturated double bond-containing oligomer (a2) (hereinafter referred to as "unsaturated oligomer (a2)") having a glass transition temperature (Tg) of -30 to -90°C, and is used for, for example, adhesives, coating materials, inks, film molding materials, and the like. The Patent Document 6 discloses that component (A) can be a reaction product of a copolymer (a1) (hereinafter referred to as "copolymer (a1)") that contains a structural unit derived from a (meth)acrylate monomer (a1-1) that does not have a reactive group and a structural unit derived from a (meth)acrylate monomer (a1-2) that has a reactive group such as an epoxy group, a carboxyl group, a hydroxyl group, or an isocyanate group, and an unsaturated oligomer (a2) that has an ethylenically unsaturated group and a group that reacts with the reactive group, via the reactive group.
[0009] Japanese Patent Application Laid-Open No. 2018-165799 International Publication No. 13 / 175978 Japanese Patent Application Laid-Open No. 10-182758 Japanese Patent Application Laid-Open No. 10-147685 Japanese Patent Application Laid-Open No. 2014-115538 Japanese Patent Application Laid-Open No. 2021-105170
[0010] For example, in a touch panel display using a liquid crystal display element or an organic EL element, a light-emitting element and a sealing layer are sequentially stacked on a substrate, and a contact hole is provided in the sealing layer, if necessary, via a wiring base layer. Patterning of the contact hole is usually performed by photolithography, which includes exposure to ultraviolet light or the like and alkaline development. In such photolithography, it is desirable to form a cured resin pattern that has excellent adhesion to the base of the sealing layer or wiring base layer, and excellent breaking strength and film retention.
[0011] An object of the present invention is to provide an active energy ray-curable composition which, upon irradiation with active energy rays such as ultraviolet light, visible light, electron beams, or X-rays, gives a cured product (cured film) which is excellent in breaking strength and water resistance and which has excellent adhesion to a substrate and film retention after alkali development, and which has excellent alkali solubility in unexposed areas, and a vinyl polymer which gives such a composition.
[0012] The present inventors have found that the above-mentioned problems can be solved by using a vinyl polymer containing a predetermined structural unit and having a glass transition temperature, an acid value, and an acryloyl equivalent adjusted to fall within a predetermined range, and a composition containing the vinyl polymer.
[0013] Embodiments of the present invention are as follows. [1] A vinyl-based polymer comprising the following structural units (a1), (a2), and (a3): (a1) a structural unit derived from an alkyl acrylate, wherein the alkyl group has 2 or more carbon atoms; (a2) a structural unit having a carboxy group; and (a3) a structural unit having an acryloyl group and / or an acrylamide group, wherein the vinyl-based polymer has a glass transition temperature (Tg) of -20°C to 60°C, an acid value of 20 to 80 mgKOH / g, and an acryloyl equivalent of 200 to 800 g / eq. [1A] The vinyl-based polymer according to [1], wherein the alkyl group of the structural unit (a1) has 4 to 18 carbon atoms. [1B-1] The vinyl-based polymer according to [1] or [1A], wherein the glass transition temperature (Tg) is -10°C to 50°C. [1B-2] The vinyl polymer according to any one of [1] to [1B-1], wherein the glass transition temperature (Tg) is 0°C to 30°C. [1C-1] The vinyl polymer according to any one of [1] to [1B-2], wherein the acid value is 20 to 50 mgKOH / g. [1C-2] The vinyl polymer according to any one of [1] to [1C-1], wherein the acid value is 25 to 40 mgKOH / g. [1D-1] The vinyl polymer according to any one of [1] to [1C-2], wherein the acryloyl equivalent is 220 to 500 g / eq. [1D-2] The vinyl polymer according to any one of [1] to [1D-1], wherein the acryloyl equivalent is 250 to 400 g / eq. [1E-1] The vinyl polymer according to any one of [1] to [1D-2], wherein the content of the structural unit (a1) is 5 to 40 mass% based on all structural units contained in the vinyl polymer. [1E-2] The vinyl polymer according to any one of [1] to [1E-1], wherein the content of the structural unit (a1) is 10 to 25 mass% based on all structural units contained in the vinyl polymer. [1F-1] The vinyl polymer according to any one of [1] to [1E-2], wherein the content of the structural unit (a2) is 3 to 30 mass% based on all structural units contained in the vinyl polymer.[1F-2] The vinyl polymer according to any one of [1] to [1F-1], wherein the content of the structural unit (a2) is 5 to 20 mass% based on all structural units contained in the vinyl polymer. [1G-1] The vinyl polymer according to any one of [1] to [1F-2], wherein the content of the structural unit (a3) is 20 to 80 mass% based on all structural units contained in the vinyl polymer. [1G-2] The vinyl polymer according to any one of [1] to [1G-1], wherein the content of the structural unit (a3) is 50 to 70 mass% based on all structural units contained in the vinyl polymer. [2] The vinyl polymer according to any one of [1] to [1G-2], wherein the structural unit (a3) contains a structural unit represented by at least one formula selected from the group consisting of the following general formulas (1) and (2): (In the formula, R 1 and R 2 are each independently a hydrogen atom or a methyl group, 1 is hydrogen or a monovalent organic group; Y 1 ~Y 3 each independently represents a divalent alkylene group which may have a ring structure and / or a branched structure, and Q 1 ~Q 4 are each independently —O— or —NH—.) [2-1] Y 1 ~Y 3 The vinyl polymer according to [2], wherein the divalent alkylene group has 1 to 8 carbon atoms. [2-2] Y 1 ~Y 3 The vinyl polymer according to [2] or [2-1], wherein the divalent alkylene group has 2 to 4 carbon atoms. [2-3] Y 1 ~Y 3 The vinyl polymer according to any one of [2] to [2-2], wherein the divalent alkylene group has 2 carbon atoms. [3] The vinyl polymer according to any one of [1] to [2-3], wherein the structural unit (a2) contains a structural unit represented by the following general formula (3): (In the formula, R 3 is a hydrogen atom or a methyl group, and Z 1 is a divalent organic group containing an ester bond, and Q5 is -O- or -NH-.) [3-1] Q 5 And Z 1 [3-2] The vinyl polymer according to [3], wherein the distance between the carbon atom adjacent to Q is 2 to 14 atoms. 5 And Z 1 The vinyl polymer according to [3] or [3-1], wherein the carbon atoms adjacent to Q are spaced apart by a distance of 4 to 12 atoms. [3-3] 5 And Z 1 The vinyl polymer according to any one of [3] to [3-2], wherein the distance between adjacent carbon atoms is 6 to 8 atoms. [4] The vinyl polymer according to any one of [1] to [3-3], wherein the alkyl group of the structural unit (a1) has 8 or more carbon atoms. [4-1] The vinyl polymer according to any one of [1] to [4], wherein the alkyl group of the structural unit (a1) has 8 to 14 carbon atoms. [4-2] The vinyl polymer according to any one of [1] to [4-1], wherein the alkyl group of the structural unit (a1) has 12 to 14 carbon atoms. [5] The vinyl polymer according to any one of [1] to [4-2], further comprising structural units derived from styrene and / or α-methylstyrene. [5-1] The vinyl polymer according to [5], wherein the content of the structural units derived from styrene and / or α-methylstyrene is 5 to 40 mass% based on the total structural units contained in the vinyl polymer. [5-2] The vinyl polymer according to [5] or [5-1], wherein the content of the structural units derived from styrene and / or α-methylstyrene is 10 to 25 mass% based on all structural units contained in the vinyl polymer. [6] The vinyl polymer according to any one of [1] to [5-2], wherein the structural units (a2) and (a3) contain a structural unit represented by the following general formula (4): (In the formula, R 4 is a hydrogen atom or a methyl group, Z 2 is a divalent organic group containing an ester bond.) [6-1] Z 2 [6-2] The vinyl polymer according to [6], wherein the distance between two carbon atoms adjacent to Z is 2 to 8 atoms. 2[6-3] The vinyl polymer according to [6] or [6-1], wherein a distance of 3 to 6 atoms is between two carbon atoms adjacent to Z. 2 [7A-1] The vinyl polymer according to any one of [1] to [7], wherein the weight average molecular weight determined by gel permeation chromatography is 7,000 to 15,000. [7B-1] The vinyl polymer according to any one of [1] to [7A-1], wherein the weight average molecular weight (Mw) / number average molecular weight (Mn) ratio is less than 3.0. [7B-2] The vinyl polymer according to any one of [1] to [7B-1], wherein the weight average molecular weight (Mw) / number average molecular weight (Mn) ratio is 1.8 or less. [8] An active energy ray-curable composition containing the vinyl polymer according to any one of [1] to [7B-2]. [9] The active energy ray-curable composition according to [8], further comprising a photopolymerization initiator. [9A] The active energy ray-curable composition according to [8], which does not contain a photopolymerization initiator.
[0014] In this specification, "(meth)acrylate" means acrylate and / or methacrylate. Furthermore, "(meth)acryloyl" means acryloyl and / or methacryloyl. Furthermore, "(meth)acrylic" means acrylic and / or methacrylic. Furthermore, in this specification, "weight average molecular weight (Mw)" and "number average molecular weight (Mn)" are values calculated using standard polystyrene standards by gel permeation chromatography (GPC).
[0015] When a film (uncured film) formed using an active energy ray-curable composition containing the vinyl polymer of the present invention is irradiated with active energy rays, a cured film having excellent breaking strength and water resistance, and excellent adhesion to a substrate and film retention after alkaline development can be obtained. Furthermore, since the vinyl polymer of the present invention has excellent alkali solubility, the unexposed areas of the film (uncured film) can be efficiently removed by alkaline development. Therefore, pattern formation using active energy rays can be suitably carried out. Taking advantage of these properties, the active energy ray-curable composition of the present invention is suitable for use as a pixel-forming material such as an interlayer insulating film, a planarizing film, a surface protective film, a spacer, a color resist used in the colored layer of a color filter, or a black matrix in a display device such as a liquid crystal or organic electroluminescence (EL) device; a material for forming a patterned cured resin layer having contact holes arranged around electrodes in a touch panel; a material for insulating between wirings in a flexible printed circuit board in a semiconductor; an interlayer insulating film-forming material; a planarizing film; a photoresist; a solder resist; an etching resist; and the like.
[0016] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these and various modifications are possible without departing from the gist of the present invention.
[0017] <Vinyl Polymer> One embodiment of the present invention relates to a vinyl polymer comprising the following structural units (a1), (a2), and (a3): (a1) a structural unit derived from an alkyl acrylate, wherein the alkyl group has 2 or more carbon atoms; (a2) a structural unit having a carboxy group; and (a3) a structural unit having an acryloyl group and / or an acrylamide group; wherein the vinyl polymer has a glass transition temperature (Tg) of −20° C. to 60° C., an acid value of 20 to 80 mg KOH / g, and an acryloyl equivalent of 200 to 800 g / eq.
[0018] [Structural Unit (a1)] The structural unit (a1) is a structural unit derived from an alkyl acrylate, and the alkyl group has 2 or more carbon atoms. The structural unit (a1) contained in the vinyl polymer of the present invention may be of one type or of two or more types.
[0019] The alkyl group of the alkyl acrylate constituting the structural unit (a1) has 2 or more carbon atoms, preferably 4 to 18, more preferably 8 to 14, and even more preferably 12 to 14. When the alkyl group has 2 or more carbon atoms, the water resistance and flexibility of the coating film are improved. On the other hand, when the alkyl group has 18 or fewer carbon atoms, the coating film tends to be uniform.
[0020] Examples of alkyl acrylates constituting the structural unit (a1) include ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-pentyl acrylate, n-hexyl acrylate, n-heptyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, n-nonyl acrylate, isononyl acrylate, decyl acrylate, undecyl acrylate, lauryl acrylate, tridecyl acrylate, tetradecyl acrylate, pentadecyl acrylate, hexadecyl acrylate, heptadecyl acrylate, stearyl acrylate, nonadecyl acrylate, eicosyl acrylate, heneicosyl acrylate, behenyl acrylate, tetracosyl acrylate, hexacosyl acrylate, octacosyl acrylate, triacontyl acrylate, Examples of the acrylate include dotriacontyl acrylate, tetratriacontyl acrylate, hexatriacontyl acrylate, octatriacontyl acrylate, tetracontyl acrylate, isodecyl acrylate, isoundecyl acrylate, isolauryl acrylate, isotridecyl acrylate, isotetradecyl acrylate, isopentadecyl acrylate, isohexadecyl acrylate, isoheptadecyl acrylate, isostearyl acrylate, isononadecyl acrylate, isoeicosyl acrylate, isoheneicosyl acrylate, isobehenyl acrylate, isotetracosyl acrylate, isohexacosyl acrylate, isooctacosyl acrylate, isotriacontyl acrylate, isodotriacontyl acrylate, isotetratriacontyl acrylate, isohexatriacontyl acrylate, isooctatriacontyl acrylate, and isotetracontyl acrylate.
[0021] The content of the structural unit (a1) is preferably 5 to 40% by mass, and more preferably 10 to 25% by mass, when the total of all structural units contained in the vinyl polymer of the present invention is taken as 100% by mass. When this range is satisfied, the active energy ray-curable composition has excellent adhesion to substrates, wiring, etc., and further, when the composition is cured, the cured product has excellent breaking strength (particularly flexibility).
[0022] [Structural Unit (a2)] The structural unit (a2) is a structural unit having a carboxy group. The structural unit (a2) may be a structural unit derived from a vinyl compound having a carboxy group, or may be a structural unit obtained by modifying a structural unit derived from a vinyl compound having an active functional group to add a carboxy group to the active functional group. The structural unit (a2) contained in the vinyl polymer of the present invention may be of only one type or of two or more types.
[0023] In the structural unit derived from a vinyl compound having a carboxy group, the carboxy group is preferably located at a position at least four carbon atoms away from the main chain. A vinyl copolymer containing such a structural unit is less likely to leave development residues during alkaline development.
[0024] Examples of vinyl compounds having a carboxy group include (meth)acrylic acid, ethacrylic acid, crotonic acid, cinnamic acid, maleic acid monoester, fumaric acid monoester, itaconic acid monoester, maleic acid, fumaric acid, itaconic acid, phthalic acid monohydroxyethyl acrylate, ω-carboxy-polycaprolactone monoacrylate, (meth)acryloyloxyethyl succinate, (meth)acryloyloxyethyl hexahydrophthalate, (meth)acryloyloxyethyl phthalate, acrylate, (meth)acryloyloxyethyl-2-hydroxyethyl phthalate, β-carboxyethyl acrylate, a phthalic anhydride adduct of pentaerythritol triacrylate, a succinic anhydride adduct of pentaerythritol triacrylate, a succinic anhydride adduct of dipentaerythritol triacrylate, a phthalic anhydride adduct of dipentaerythritol triacrylate, an ε-caprolactone-modified (meth)acrylic acid, and carboxyethyl (meth)acrylate.
[0025] Examples of structural units in which a carboxy group is added to the active functional group of a structural unit derived from a vinyl compound having an active functional group by modification include a structural unit obtained by reacting an acid anhydride with a structural unit derived from a vinyl monomer having a hydroxy group, a structural unit obtained by reacting a compound having an epoxy group with a structural unit derived from a vinyl monomer having a carboxy group, and then reacting the hydroxy group generated by the reaction with an acid anhydride, and a structural unit obtained by reacting a compound having a carboxy group with a structural unit derived from a vinyl monomer having an epoxy group, and then reacting the hydroxy group generated by the reaction with an acid anhydride.
[0026] Among these, the structural unit (a2) preferably contains a structural unit represented by the following general formula (3): A vinyl copolymer containing such a structural unit is less likely to leave development residues during alkaline development and has good alkali solubility. (In the formula, R 3 is a hydrogen atom or a methyl group, Z 1 is a divalent organic group containing an ester bond, and Q 5 is —O— or —NH—.)
[0027] Q 5 And Z 1 The distance between the carbon atom adjacent to "-Q" is preferably 2 to 14 atoms, more preferably 4 to 12 atoms, and even more preferably 6 to 8 atoms. 5 -C 2 H 4 -O-C(=O)-C 2 H 4 When the structure of "—COOH" is included, Q 5 And Z 1 There is a distance of six atoms (5 carbon atoms + 1 oxygen atom) between the adjacent carbon atoms.
[0028] The content of the structural unit (a2) is preferably 3 to 30% by mass, and more preferably 5 to 20% by mass, when the total of all structural units contained in the vinyl polymer of the present invention is taken as 100% by mass. When the content satisfies these ranges, when the active energy ray-curable composition is cured, the cured product has water resistance and alkali resistance, and facilitates pattern formation by photolithography.
[0029] [Structural unit (a3)] The structural unit (a3) is a structural unit having an acryloyl group and / or an acrylamide group. The structural unit (a3) is preferably a structural unit obtained by modifying a structural unit derived from a vinyl compound having an active functional group with an acryloyl group or an acrylamide group added to the active functional group. The structural unit (a3) contained in the vinyl polymer of the present invention may be of only one type or of two or more types.
[0030] Examples of structural units obtained by modifying a structural unit derived from a vinyl compound having an active functional group with an acryloyl group or an acrylamide group added to the active functional group include a structural unit obtained by reacting a structural unit derived from a vinyl monomer having a hydroxy group with an isocyanate group-containing acrylate, a structural unit obtained by reacting a structural unit derived from a vinyl monomer containing a carboxy group with an epoxy group-containing acrylate, a structural unit obtained by reacting a structural unit derived from a vinyl monomer containing an epoxy group with a carboxy group-containing acrylate, and a structural unit obtained by reacting a structural unit derived from a vinyl monomer containing an epoxy group with a carboxy group-containing acrylate, and further reacting an isocyanate group-containing acrylate with the hydroxy group generated by the reaction of the structural unit derived from a vinyl monomer containing an epoxy group.
[0031] Among these, the structural unit (a3) preferably contains a structural unit represented by at least one formula selected from the group consisting of the following general formulas (1) and (2): A vinyl copolymer containing such a structural unit exhibits good substrate adhesion and film retention. (In the formula, R 1 and R 2 are each independently a hydrogen atom or a methyl group, 1 is hydrogen or a monovalent organic group; Y 1 ~Y 3 each independently represents a divalent alkylene group which may have a ring structure and / or a branched structure, and Q 1 ~Q 4 are each independently —O— or —NH—.
[0032] Y 1 ~Y 3 The divalent alkylene group preferably has 1 to 8 carbon atoms, more preferably 2 to 4 carbon atoms, and even more preferably 2 carbon atoms.
[0033] The content of the structural unit (a3) is preferably 20 to 80% by mass, and more preferably 50 to 70% by mass, when the total of all structural units contained in the vinyl polymer of the present invention is taken as 100% by mass. When the content satisfies these ranges, the active energy ray-curable composition has excellent adhesion to substrates, wiring, etc., and excellent curability by active energy rays.
[0034] [Structural unit (a2) and structural unit (a3)] The structural units (a2) and (a3) may be the same structural unit. That is, when one structural unit has a carboxy group and an acryloyl group and / or an acrylamide group, the structural unit is deemed to simultaneously satisfy the structural unit (a2) and the structural unit (a3). Examples of such structural units include a structural unit obtained by reacting a structural unit derived from a vinyl monomer having a carboxy group with an epoxy group-containing acrylate to generate a hydroxyl group, and then reacting the resulting hydroxyl group with an acid anhydride; a structural unit obtained by reacting a structural unit derived from a vinyl monomer having an epoxy group with a carboxy group-containing acrylate to generate a hydroxyl group, and then reacting the resulting hydroxyl group with an acid anhydride;
[0035] Among these, it is preferable to contain a structural unit represented by the following general formula (4): A vinyl copolymer containing such a structural unit can adjust the carboxyl group and the acryloyl group to an appropriate balance, and in addition to being excellent in curability by active energy rays, can also achieve both alkali solubility and film retention. (In the formula, R 4 is a hydrogen atom or a methyl group, Z 2 is a divalent organic group containing an ester bond.
[0036] Z 2 The distance between two adjacent carbon atoms is preferably 2 to 8 atoms, more preferably 3 to 6 atoms, and even more preferably 4 atoms.
[0037] When the structural units (a2) and (a3) are the same structural unit, the content of the structural unit is divided equally between (a2) and (a3).
[0038] [Other structural units] The vinyl copolymer of the present invention preferably further contains structural units derived from styrene and / or α-methylstyrene in addition to the above structural units (a1), (a2), and (a3). From the viewpoint of polymerizability, it is particularly preferable to contain structural units derived from styrene. When these structural units are contained, water resistance and alkali resistance can be obtained in the cured product when the active energy ray-curable composition is cured.
[0039] The content of structural units derived from styrene or α-methylstyrene is preferably 5 to 40% by mass, and more preferably 10 to 25% by mass, when the total of all structural units contained in the vinyl polymer of the present invention is 100% by mass.
[0040] The vinyl polymer of the present invention may contain, in addition to the above-mentioned structural units (a1), (a2), and (a3) and styrene or α-methylstyrene, another structural unit (a4). The structural unit (a4) is not particularly limited, but is preferably a structural unit derived from a vinyl compound. Examples of the monomer that forms the structural unit (a4) include alkyl methacrylates having an ester moiety containing an aliphatic hydrocarbon group, methyl acrylate, alkyl (meth)acrylates having an ester moiety containing an alicyclic hydrocarbon group, aromatic (meth)acrylates having an ester moiety containing an aromatic hydrocarbon group, hydroxy group-containing vinyl compounds, amino group-containing vinyl compounds, cyanide vinyl compounds (acrylonitrile, methacrylonitrile, etc.), unsaturated acid anhydrides, maleimide compounds, alkyl (meth)acrylates having an ester moiety containing an alkoxyalkyl group, halogen-containing vinyl compounds (vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, etc.), vinyl silane compounds (trimethoxyvinylsilane, triethoxyvinylsilane, methyldimethoxyvinylsilane, methyldiethoxyvinylsilane, dimethylmethoxysilane, etc.), vinyl ester compounds (vinyl acetate, vinyl propionate, etc.), and vinyl ether compounds (methyl vinyl ether, ethyl vinyl ether, butyl vinyl ether, cyclohexyl vinyl ether, etc.).
[0041] In the vinyl polymer of the present invention, the upper limit of the content of the structural unit (a4) is preferably 20% by mass, and more preferably 10% by mass, when the total of all structural units contained in the vinyl polymer of the present invention is 100% by mass.
[0042] [Average Molecular Weight] The weight-average molecular weight (Mw) of the vinyl polymer of the present invention is preferably 5,000 to 20,000, more preferably 7,000 to 15,000, because this facilitates pattern formation by photolithography. When the weight-average molecular weight of the vinyl polymer is 5,000 or more, the linearity of the formed pattern is good. On the other hand, when the weight-average molecular weight of the vinyl polymer is 20,000 or less, development residues are less likely to be generated during alkaline development. Furthermore, the PDI (=weight-average molecular weight (Mw) / number-average molecular weight (Mn)) of the vinyl polymer of the present invention is preferably less than 3.0, more preferably 1.8 or less. When the PDI is less than 3.0, the molecular weight distribution becomes narrow, and a decrease in the residual film rate during alkaline development and the generation of development residues can be suppressed. The weight-average molecular weight (Mw) and number-average molecular weight (Mn) can be measured according to the method described in the Examples below.
[0043] [Acryloyl Equivalent] The acryloyl equivalent of the vinyl polymer of the present invention is 200 to 800 g / eq, preferably 220 to 500 g / eq, and more preferably 250 to 400 g / eq, because flexibility, adhesion to substrates, tensile properties, and film retention of a cured product can be obtained when the active energy ray-curable composition is cured. The acryloyl equivalent can be measured according to the method described in the Examples below.
[0044] [Glass Transition Temperature] The glass transition temperature of the vinyl polymer of the present invention must be −20 to 60° C., preferably −10 to 50° C., and more preferably 0 to 30° C., in order to obtain flexibility and adhesion to a substrate in a cured product when the active energy ray-curable composition is cured. The glass transition temperature can be measured according to the method described later in the Examples.
[0045] [Acid Value] The acid value of the vinyl polymer of the present invention is 20 to 80 mgKOH / g, preferably 20 to 50 mgKOH / g, and more preferably 25 to 40 mgKOH / g, in order to facilitate pattern formation by photolithography. By setting the acid value to 20 mgKOH / g or more, developer permeability tends to be increased and development latitude (tolerance to the pH and temperature of the developer and the development time) tends to be improved, while by setting the acid value to 80 mgKOH / g or less, it becomes possible to obtain a more appropriate pattern with excellent film retention. The acid value can be measured according to the method described in the Examples below.
[0046] <Method for producing vinyl polymer> The method for producing the vinyl polymer of the present invention is not particularly limited, and methods such as suspension polymerization, emulsion polymerization, solution polymerization, or bulk polymerization of a monomer that provides a predetermined structural unit can be applied. Among these, bulk polymerization and solution polymerization are preferred in that they are easy to produce and do not contain impurities such as emulsifiers in the polymer solution.
[0047] As the solvent used in the polymerization of the vinyl polymer of the present invention, a known general-purpose solvent can be used, but solvents containing a hydroxy group, a carboxy group, etc. are not preferred from the viewpoint of production stability. Specifically, ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, propylene glycol monomethyl ether acetate, toluene, acetonitrile, etc. can be preferably used.
[0048] In the polymerization of the vinyl polymer of the present invention, a chain transfer agent can be used to adjust the molecular weight. As the chain transfer agent, a known general-purpose agent such as a thiol type, a secondary alcohol type, a naphthoquinone type, or an α-methylstyrene dimer can be used, but it is preferable to use a thiol type chain transfer agent because it is easy to control the molecular weight.
[0049] Among chain transfer agents, it is particularly preferable to use a reversible addition-fragmentation chain transfer agent (RAFT agent) for the polymerization of the vinyl polymer of the present invention. By carrying out polymerization using a RAFT agent, it is possible to suppress the PDI low and form a copolymer with a narrow molecular weight distribution, which makes it possible to achieve both a high film retention rate during alkaline development and suppression of development residues.
[0050] For the polymerization of the vinyl polymer of the present invention, known general-purpose polymerization initiators such as azo initiators and peroxide initiators can be used. However, it is preferable to use an azo initiator since it does not inhibit the effects of the chain transfer agent and RAFT agent described above.
[0051] In the production of the vinyl polymer of the present invention, the structural units (a2) and (a3) can be obtained not only directly by polymerizing the corresponding monomers, but also by a multi-step reaction in which a mixture of the monomer constituting the structural unit (a1) and a monomer having an active functional group is polymerized to form a copolymer (hereinafter referred to as "precursor polymer PP"), and then this precursor polymer PP is modified with another compound. The polymerization conditions for the precursor polymer PP can be the same as those for the vinyl copolymer.
[0052] As the modification reaction of the precursor polymer PP, the reaction between a hydroxy group and an isocyanate group, the reaction between an epoxy group and a carboxy group, and the reaction between a hydroxy group and an acid anhydride are preferably used because they produce few reaction impurities and the reaction proceeds under relatively mild conditions.
[0053] During polymerization of the precursor polymer PP or during formation of the acryloyl group or acrylamide group contained in the structural unit (a3), vinyl monomers having these functional groups can be used, namely, vinyl monomer compounds having a hydroxy group, vinyl monomers having an isocyanate group, vinyl monomers having an epoxy group, and vinyl monomers having a carboxy group.
[0054] Examples of vinyl monomers having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polybutylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, polyethylene glycol-polypropylene glycol mono(meth)acrylate, poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate, polyethylene glycol-polytetramethylene glycol mono(meth)acrylate, and 2-hydroxyethyl(meth)acrylamide, and these may be used alone or in combination of two or more. Among these, 2-hydroxyethyl acrylate and 2-hydroxyethyl acrylamide are preferred from the viewpoint of efficient introduction of functional groups when forming the acryloyl group or acrylamide group contained in the structural unit (a3).
[0055] Examples of vinyl monomers having an isocyanate group include 2-(meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate, etc. Among these, 2-acryloyloxyethyl isocyanate is preferred from the viewpoint of efficient introduction of a functional group when forming the acryloyl group or acrylamide group contained in the structural unit (a3).
[0056] Examples of vinyl monomers having an epoxy group include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, etc., and these may be used alone or in combination of two or more. Among these, glycidyl methacrylate is preferred from the viewpoints of availability and the ability to efficiently introduce a functional group when forming the acryloyl group or acrylamide group contained in the structural unit (a3).
[0057] Examples of vinyl compounds having a carboxy group include (meth)acrylic acid, ethacrylic acid, crotonic acid, cinnamic acid, maleic acid monoester, fumaric acid monoester, itaconic acid monoester, maleic acid, fumaric acid, itaconic acid, phthalic acid monohydroxyethyl acrylate, ω-carboxy-polycaprolactone monoacrylate, (meth)acryloyloxyethyl succinate, (meth)acryloyloxyethyl hexahydrophthalate, (meth)acryloyloxyethyl phthalate, (meth)acryloyloxy Examples of suitable acrylates include ethyl-2-hydroxyethyl phthalate, β-carboxyethyl acrylate, a phthalic anhydride adduct of pentaerythritol triacrylate, a succinic anhydride adduct of pentaerythritol triacrylate, a succinic anhydride adduct of dipentaerythritol triacrylate, a phthalic anhydride adduct of dipentaerythritol triacrylate, an ε-caprolactone-modified (meth)acrylic acid, and carboxyethyl (meth)acrylate. These may be used alone or in combination of two or more. Among these, acrylic acid is preferred from the viewpoint of efficient introduction of a functional group when forming the acryloyl group or acrylamide group contained in the structural unit (a3).
[0058] Examples of acid anhydrides include succinic anhydride, maleic anhydride, itaconic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, etc., and these may be used alone or in combination of two or more. Among these, polymerizable maleic anhydride can be used during polymerization of the precursor polymer PP, and succinic anhydride is preferred from the viewpoint of efficient introduction of functional groups when forming the acryloyl group or acrylamide group contained in the structural unit (a3).
[0059] The modification reaction of the precursor polymer PP can be carried out in the presence of a catalyst in an organic solvent such as ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, propylene glycol monomethyl ether acetate, toluene, acetonitrile, etc. Solvents containing active functional groups such as hydroxyl groups, carboxyl groups, and epoxy groups are not preferred because they may interfere with the modification reaction.
[0060] Examples of catalysts used in the reaction of an epoxy group with a carboxy group and in the reaction of a hydroxy group with an acid anhydride include tetrabutylammonium bromide, tetrabutylammonium chloride, tetramethylammonium bromide, tetramethylammonium chloride, triphenylphosphine, tributylphosphine, 1,8-diazabicyclo[5,4,0]-7-undecene, 1,4-diazabicyclo[2,2,2]octane, etc. The amount of catalyst used is usually about 0.5 to 5% by mass based on the amount of the copolymer after modification.
[0061] Examples of catalysts used in the reaction of hydroxy groups and isocyanate groups include organotin compounds such as dibutyltin dichloride; fatty acid salts of organotin compounds such as dibutyltin dilaurate, dibutyltin di(2-ethylhexanoate), dibutyltin diacetate, dihexyltin diacetate, and dioctyltin dilaurate; thioglycolic acid ester salts of organotin compounds such as dimethyltin bis(isooctylthioglycolate) salt, dimethyltin bis(isooctylthioglycolate) salt, and dioctyltin bis(isooctylthioglycolate) salt; tin carboxylates such as tin octoate and tin decanoate; bismuth carboxylate; titanium complexes; and zirconium complexes. The amount of catalyst used is typically about 0.01 to 0.1% by mass relative to the amount of the copolymer after modification.
[0062] When the precursor polymer PP is modified to form the structural unit (a3), or when a copolymer containing the structural unit (a3) is further modified, it is preferable to add a polymerization inhibitor such as methoxyphenol, hydroquinone, dibutylhydroxytoluene, or phenothiazine to the reaction system in order to suppress the reaction of the polymerizable unsaturated bond.
[0063] The vinyl polymer of the present invention can be cured by active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays. As described below, the vinyl polymer of the present invention is suitable for pattern formation for electronic materials, using photolithography, including exposure and alkaline development, on a film formed using an active energy ray-curable composition containing the vinyl polymer together with a photopolymerization initiator, other polyfunctional polymers, and the like, which are used depending on the type of active energy ray. In the present invention, for example, when a portion of a film containing a vinyl polymer and a photopolymerization initiator is irradiated with ultraviolet light, the vinyl polymer in the irradiated portion (exposed portion) becomes a crosslinked resin (cured resin), while the vinyl polymer in the unirradiated portion (unexposed portion) does not denature. Because the vinyl polymer of the present invention has excellent alkaline solubility, alkaline development can be carried out efficiently, for example, when a pattern is formed while leaving the crosslinked resin (cured resin) portion. When a film (uncured film) made of the vinyl polymer of the present invention is contacted with a 2.38% by mass aqueous solution of tetramethylammonium hydroxide at 23°C, the alkaline dissolution rate can be preferably 50 nm / sec or more, more preferably 60 nm / sec or more. By adjusting the alkali dissolution rate to 40 nm / sec or more, the composition can be used without any problems as an active energy ray-curable composition, and a desired pattern can be obtained after alkali development.
[0064] <Active energy ray-curable composition> The active energy ray-curable composition of the present invention is a composition containing the vinyl polymer of the present invention (hereinafter referred to as "vinyl polymer (A)"). The active energy ray-curable composition may also contain a photopolymerization initiator, another multifunctional polymer, a surfactant, a polymerization inhibitor, a light resistance improver, fine particles, or a liquid medium from the viewpoint of coatability onto substrates, wiring, etc.
[0065] The photopolymerization initiator is not particularly limited as long as it is excited by energy such as ultraviolet light, visible light, or near-infrared light to generate radicals and at least promote the radical polymerization of the vinyl polymer of the present invention. Examples of the photopolymerization initiator include benzyl dimethyl ketal, benzil, benzoin, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, oligo[2-hydroxy-2-methyl-1-[4 -1-(methylvinyl)phenyl]propanone, 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl]-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)]phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholinophenyl)butan-1-one aromatic ketone compounds such as N,N'-benzophenone, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 4-(methylphenylthio)phenylphenylmethane, methyl-2-benzophenone, 1-[4-(4-benzoylphenylsulfanyl)phenyl]-2-methyl-2-(4-methylphenylsulfonyl)propan-1-one, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, N,N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone and the like;Acylphosphine oxide compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, ethyl-(2,4,6-trimethylbenzoyl)phenylphosphinate, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide; thioxanthone, 2-chlorothioxanthone, and 2,4-diethylthioxanthone; thioxanthone compounds such as thioxanthone, isopropyl thioxanthone, 1-chloro-4-propyl thioxanthone, 3-[3,4-dimethyl-9-oxo-9H-thioxanthone-2-yl]oxy]-2-hydroxypropyl-N,N,N-trimethylammonium chloride, and fluorothioxanthone; acridone compounds such as acridone and 10-butyl-2-chloroacridone; 1,2-octanedione 1-[4-(phenylthio)-2-(O-phenyl)-2-oxanthone; oxime esters such as ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime); oxime esters such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-phenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-phenylimidazole dimer, 2,4,5-triarylimidazole dimers such as 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-5-phenylimidazole dimer, and 2-(2,4-dimethoxyphenyl)-4,5-diphenylimidazole dimer; and acridine derivatives such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane.
[0066] The content of the photopolymerization initiator is preferably 0.1 to 10 parts by mass, more preferably 1 to 6 parts by mass, based on 100 parts by mass of the content of the vinyl polymer (A).
[0067] Examples of the polyfunctional polymer include polyfunctional (meth)acrylates, aromatic polyvinyl compounds, diallyl compounds, allyl (meth)acrylate, dicyclopentenyl (meth)acrylate, etc. Among these, polyfunctional (meth)acrylates are preferred.
[0068] Examples of polyfunctional (meth)acrylates include polyol poly(meth)acrylates such as glycerin tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri- or tetra(meth)acrylate, ditrimethylolpropane tri- or tetra(meth)acrylate, diglycerin tri- or tetra(meth)acrylate, and dipentaerythritol tri-, tetra-, penta-, or hexa(meth)acrylate; ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, polybutylene (Poly)alkylene glycol di(meth)acrylates such as ethylene glycol di(meth)acrylate and poly(1-methylbutylene glycol) di(meth)acrylate; di(meth)acrylates of aliphatic diols such as 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate; tri(meth)acrylates of glycerin alkylene oxide adducts, tri- or tetra(meth)acrylates of pentaerythritol alkylene oxide adducts, di ... pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adducts, pentaerythritol alkylene oxide adduct Poly(meth)acrylates of polyol alkylene oxide adducts such as tri- or tetra(meth)acrylates of trimethylolpropane alkylene oxide adducts, tri- or tetra(meth)acrylates of diglycerin alkylene oxide adducts, and tri-, tetra-, penta-, or hexa(meth)acrylates of dipentaerythritol alkylene oxide adducts; di(meth)acrylates having a bisphenol skeleton such as ethylene oxide-modified di(meth)acrylate of bisphenol A and di(meth)acrylate of bisphenol A;Examples of the aromatic polyvinyl compounds include di(meth)acrylates having an alicyclic skeleton such as tricyclodecanedimethylol di(meth)acrylate; (meth)acrylates having an isocyanurate skeleton such as ethylene oxide-modified diacrylate of isocyanuric acid and ε-caprolactone-modified tris((meth)acryloxyethyl)isocyanurate; urethane (meth)acrylates having a polyester skeleton; urethane (meth)acrylates having a polycarbonate skeleton; epoxy (meth)acrylates; polyether (meth)acrylates; polybasic acid-modified tri- or tetra(meth)acrylates of pentaerythritol; and polybasic acid-modified tetra-, penta-, or hexa(meth)acrylates of dipentaerythritol. Examples of aromatic polyvinyl compounds include divinylbenzene and 1,3,5-trivinylbenzene.
[0069] When the active energy ray-curable composition of the present invention contains a polyfunctional polymer, the content ratio thereof is preferably 10 to 200 parts by mass, more preferably 50 to 150 parts by mass, relative to 100 parts by mass of the content of the vinyl polymer (A).
[0070] As the surfactant, various surfactants such as fluorine-based surfactants, nonionic surfactants, cationic surfactants, anionic surfactants, and silicone surfactants can be used, and fluorine-based surfactants are preferred because they can further improve coating properties. Examples of fluorine-based surfactants include Megafac F171, F172, F173, F176, F177, F141, F142, F143, F144, R30, R41, R40LM, F437, F475, F479, F482, F554, F-557, F568, and F780 (all manufactured by DIC Corporation), Fluorad FC430, FC431, and FC171 (all manufactured by Sumitomo 3M Limited), Surflon S-382, S-386, S-242, S-243, and S-244. Examples include S-420, S-431, S-611, S-47, S-651, S-656 (all manufactured by AGC Inc.), PF636, PF656, PF6320, PF6520, PF7002, PF-151N (all manufactured by OMNOVA), Unidyne DSN-403N, DS-101, DS-202, DS-401, DS-403, DSN-403N, NS-1602, NS-1603, NS-1605, NS-9013 (all manufactured by Daikin Industries, Ltd.).
[0071] When the active energy ray-curable composition of the present invention contains a surfactant, the content thereof is preferably 0.001 to 0.2 mass%, more preferably 0.0015 to 0.1 mass%, and even more preferably 0.002 to 0.05 mass%, relative to the total solid content of the composition. When the content of the surfactant is within the above range, the coatability of the active energy ray-curable composition is good, and the occurrence of coating unevenness and striae can be more effectively suppressed.
[0072] Examples of the polymerization inhibitor include hydroquinone, p-methoxyphenol, di-t-butyl-p-cresol, pyrogallol, t-butylcatechol, benzoquinone, 4,4'-thiobis(3-methyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), phenothiazine, and 2-mercaptobenzimidazole.
[0073] The light resistance improver may be an ultraviolet absorber or a light stabilizer. Examples of ultraviolet absorbers include benzotriazole compounds such as 2-(2'-hydroxy-5-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole, and 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)benzotriazole; triazine compounds such as 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-iso-octyloxyphenyl)-s-triazine; 2,4-dihydroxybenzophenone; Benzophenone compounds such as 2-hydroxy-4-methoxy-benzophenone, 2-hydroxy-4-methoxy-4'-methylbenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,4,4'-trihydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,3,4,4'-tetrahydroxybenzophenone, 2,3',4,4'-tetrahydroxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone are mentioned. Examples of light stabilizers include low molecular weight hindered amine compounds such as N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)-N,N'-diformylhexamethylenediamine, bis(1,2,6,6-pentamethyl-4-piperidyl)-2-(3,5-ditertiarybutyl-4-hydroxybenzyl)-2-n-butylmalonate, and bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate; and high molecular weight hindered amine compounds such as N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)-N,N'-diformylhexamethylenediamine and bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate.
[0074] The fine particles may be made of metal, inorganic compound, rubber, or resin and have a particle size of about 1 to 100 μm. Examples of inorganic compounds include oxides of silicon, aluminum, zirconium, titanium, zinc, lead, germanium, indium, tin, antimony, cerium, lithium, etc., or composite oxides thereof, calcium carbonate, bentonite, etc. The rubber or resin may be made of a crosslinked polymer.
[0075] The liquid medium is usually an organic solvent, for example, a hydrocarbon such as n-hexane, benzene, toluene, xylene, ethylbenzene, or cyclohexane; an alcohol solvent such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutyl alcohol, 2-methoxyethanol, 2-ethoxyethanol, 2-(methoxymethoxy)ethanol, 2-isopropoxyethanol, 2-butoxyethanol, 2-isopentyloxyethanol, 2-hexyloxyethanol, 2-phenoxyethanol, 2-benzyloxyethanol, furfuryl alcohol, tetrahydrofurfuryl alcohol, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, or propylene glycol monomethyl ether; or tetrahydrofuran. ether solvents such as dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, bis(2-methoxyethyl)ether, bis(2-ethoxyethyl)ether, and bis(2-butoxyethyl)ether; ketone solvents such as acetone, methyl ethyl ketone, methyl-n-propyl ketone, diethyl ketone, butyl methyl ketone, methyl isobutyl ketone, methyl pentyl ketone, di-n-propyl ketone, diisobutyl ketone, phoron, isophorone, cyclopentanone, cyclohexanone, and methylcyclohexanone; ester solvents such as ethyl acetate, butyl acetate, isobutyl acetate, methyl glycol acetate, propylene glycol monomethyl ether acetate, and cellosolve acetate; and aprotic polar solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, and γ-butyrolactone. These organic solvents can be used alone or in combination of two or more.By selecting an appropriate liquid medium when dissolving the active energy ray-curable composition, it is possible to effectively suppress the occurrence of coating unevenness and striations when the active energy ray-curable composition is applied, and the precipitation of specific components in the active energy ray-curable composition due to changes over time.
[0076] When the active energy ray-curable composition of the present invention contains a liquid medium, the content ratio thereof is appropriately selected depending on the application and is not particularly limited. When the active energy ray-curable composition of the present invention is used for forming a pattern for an electronic material, the content ratio is preferably 20 to 400 parts by mass, more preferably 40 to 200 parts by mass, based on 100 parts by mass of the vinyl polymer (A) or 100 parts by mass of the total amount of the vinyl polymer (A) and the polyfunctional polymer.
[0077] The active energy ray-curable composition of the present invention can be produced by mixing raw material components such as the vinyl polymer (A) using various mixers and dispersers.
[0078] In the present invention, when a film (uncured film) containing a vinyl polymer formed using the active energy ray-curable composition is irradiated with active energy rays, a cured film can be obtained that has excellent breaking strength and water resistance and excellent adhesion to a substrate (substrate made of an inorganic material, a resin, etc.) after alkaline development. Utilizing these properties, the active energy ray-curable composition of the present invention is particularly suitable for producing electronic components having a patterned cured resin layer on a substrate, wiring, etc. Examples of substrates for electronic components include plate-like substrates made of soda glass, alkali-free glass, Pyrex (registered trademark) glass, quartz glass, etc. used in liquid crystal display devices, etc., substrates having a (transparent) conductive film disposed on the surface of these substrates, photoelectric conversion element substrates (silicon substrates, etc.) used in solid-state imaging devices, etc., and color filter substrates, etc.
[0079] When preparing a patterned cured resin layer, a method can be applied which sequentially includes a step of forming a film (uncured film) on the surface of a substrate using an active energy ray-curable composition (hereinafter referred to as the "film-forming step"), a step of irradiating the film with active energy rays through a mask or by scanning exposure without using a mask (hereinafter referred to as the "exposure step"), and a step of developing the exposed film using an alkaline aqueous solution (hereinafter also referred to as the "developer") (hereinafter referred to as the "developing step"). When electron beams or X-rays are used in the exposure step, an active energy ray-curable composition not containing a photopolymerization initiator can be used in the film-forming step. When ultraviolet rays or visible light are used in the exposure step, an active energy ray-curable composition containing a photopolymerization initiator can be used in the film-forming step.
[0080] In the above-mentioned film-forming step, a liquid active energy ray-curable composition is applied by a conventionally known application method using a bar coater, an applicator, a doctor blade, a knife coater, a comma coater, a reverse roll coater, a die coater, a lip coater, a gravure coater, a microgravure coater, or the like to form a coating film, and then, if necessary, the organic solvent in the composition is removed by drying under reduced pressure or heating to form a coating (uncured film). The film thickness is appropriately selected depending on the application.
[0081] In the exposure step, a predetermined portion of the coating is exposed, and the exposed portion is made of a cured resin, while the unexposed portion remains as an uncured resin. The cured resin is a crosslinked resin formed based on the acryloyl group or acrylamide group possessed by the structural unit (a3) of the vinyl polymer (A) contained in the active energy ray-curable composition. The active energy ray used in the exposure step is ultraviolet light, visible light, electron beam, or X-ray. Ultraviolet light can be irradiated using an irradiation device using a high-pressure mercury lamp, a metal halide lamp, an ultraviolet (UV) electrodeless lamp, a light-emitting diode (LED), an ultraviolet laser, or the like as a light source. Electron beams can be irradiated using an electrocurtain type, a broad beam type linear filament type, or a scanning type electron beam accelerator. Ultraviolet light is preferred as the active energy ray because it can form a cured resin in a short time and with low energy irradiation. The dose, irradiation amount, irradiation intensity, etc. of the ultraviolet light are appropriately selected depending on the application.
[0082] In the development step, when a developer (an alkaline aqueous solution) is brought into contact with the exposed film, the unexposed areas are dissolved and removed, leaving behind the exposed areas (cured resin areas that are insoluble in the alkaline aqueous solution). Examples of the developer include aqueous solutions of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium bicarbonate, sodium silicate, sodium metasilicate, aqueous ammonia, ethylamine, diethylamine, monoethanolamine, diethanolamine, triethanolamine, dimethylethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, choline, pyrrole, piperidine, 1,8-diazabicyclo-[5.4.0]-7-undecene, and 1,5-diazabicyclo-[4.3.0]-5-nonene. The developer may contain, for example, a water-soluble organic solvent such as methanol or ethanol, an antifoaming agent, a surfactant, and the like. The development conditions are not particularly limited. In the developing step, shower developing, spray developing, dip (immersion) developing, puddle (liquid puddle) developing, etc. can be used.
[0083] After the above-mentioned development step, washing with water, drying, etc. are usually carried out, and if necessary, a heat treatment can be carried out.
[0084] In the present invention, a coating film of the active energy ray-curable composition formed on the surface of a substrate is dried, and then the resulting film (uncured film, average film thickness: 4.0 μm) is irradiated with active energy rays to form a cured film. When this cured film is sprayed with a 2.38% aqueous solution of tetramethylammonium hydroxide (23° C.) at 0.15 MPa under the conditions described in the Examples below, the film thickness retention can be preferably 85% or more, more preferably 91% or more, and even more preferably 94% or more.
[0085] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are by mass unless otherwise specified.
[0086] Various values in the examples may be used as preferred lower or upper limits in the embodiments of the present invention. Two values of the same type in the examples may be appropriately combined to form a preferred range of values.
[0087] 1. Abbreviations BA: n-butyl acrylate HA: 2-ethylhexyl acrylate LA: lauryl acrylate AA: acrylic acid GMA: glycidyl methacrylate HEA: 2-hydroxyethyl acrylate St: styrene MA: methyl acrylate MMA: methyl methacrylate OTG: 2-ethylhexyl thioglycolate DBTTC: S,S-dibenzyl trithiocarbonate ABN-E: 2,2'-azobis(2-methylbutyronitrile) MAA: methacrylic acid HEAA: 2-hydroxyesylacrylamide AOI: 2-isocyanatoethyl acrylate 4HBAGE: 4-hydroxybutyl acrylate glycidyl ether TPP: triphenylphosphine DBTDL: dibutyltin dilaurate BHT: butylhydroxytoluene
[0088] 2. Methods for Measuring Physical Properties of Polymers The methods for measuring the molecular weight (Mw and Mn) of a vinyl polymer, the acid value of a vinyl polymer, the equivalent weight of the (meth)acryloyl group contained therein, and the glass transition temperature of a vinyl polymer are shown below.
[0089] (1) Molecular Weight Four columns "TSKgel SuperMultipore HZ-M" (product name) manufactured by Tosoh Corporation were connected together and placed in a gel permeation chromatograph "HLC-8320" (model name) manufactured by Tosoh Corporation, and the polystyrene-equivalent number average molecular weight (Mn), weight average molecular weight (Mw), and PDI (= Mw / Mn) were measured under the following measurement conditions: Column temperature: 40°C, Eluent: Tetrahydrofuran, Detector: RI
[0090] (2) Acid Value: The acid value was measured in accordance with JIS K 0070 (acid value measurement) using an automatic titrator "COM1600ST" (model name) manufactured by Hiranuma Sangyo Co., Ltd. That is, a vinyl polymer was weighed out so that the titration amount was about 10 mL, and diluted with about 50 mL of tetrahydrofuran, and then titrated with a 0.1 N KOH / ethanol solution.
[0091] (3) (Meth)acryloyl equivalent (g / eq) Calculated using the amount of monomer and modifier used in the production of the vinyl polymer, the acid value of the vinyl polymer, or the reaction rate calculated from infrared absorption spectrum. The type of polymerizable functional group is indicated according to the type of modifier used.
[0092] (4) Glass Transition Temperature (Tg) Tg was measured using a differential scanning calorimeter "Q-100" (model name) manufactured by TA Instrument under the following conditions: Temperature increase rate: 10°C / min Atmosphere: nitrogen gas
[0093] 3. Synthesis of Vinyl Copolymer <Production Example 1> A 500 mL flask equipped with a stirrer and thermometer was charged with 20 g of lauryl acrylate, 60 g of glycidyl methacrylate, and 20 g of styrene as monomers, and 50 g of butyl acetate as a polymerization solvent. The mixture was degassed with nitrogen bubbling while stirring, and then heated to 80°C. 0.5 g of 2,2'-azobis(2-methylbutyronitrile) ("ABN-E" manufactured by Nippon Finechem) was added as an initiator to initiate polymerization. Simultaneously, 3 g of 2-ethylhexyl thioglycolate was added dropwise over 2 hours as a chain transfer agent. After the reaction was continued for 5 hours from the start of polymerization, the temperature was raised to 90°C and the reaction was continued for an additional 2 hours. Analysis of residual monomers by gas chromatography revealed that the overall monomer conversion was 98% or higher. The temperature was then raised to 90°C, and 5% ON (a mixed gas of 5% oxygen and 95% nitrogen) was blown in, while 0.07 g of BHT as a polymerization inhibitor, 30.4 g of acrylic acid (1.0 equivalent relative to glycidyl methacrylate) as a modifier, 1.3 g of triphenylphosphine as a modification catalyst, and 20.7 g of butyl acetate as a solvent were added to initiate modification reaction 1, and the reaction was continued for 16 hours. Analysis of residual acrylic acid by gas chromatography showed that the reaction rate was 98% or higher. The temperature was then raised to 90°C, and 5% ON (a mixed gas of 5% oxygen and 95% nitrogen) was blown in, while 8.4 g of succinic anhydride (0.2 equivalent relative to the reactant of glycidyl methacrylate and acrylic acid) as a modifier and 4.5 g of butyl acetate as a solvent were added to initiate modification reaction 2, and the reaction was continued for 3 hours. Analysis of succinic anhydride by gas chromatography showed that the reaction rate was 98% or higher. Through the above operations, a 65% solution of vinyl copolymer PA1 was obtained. Analysis of PA1 revealed Mn = 7,500, Mw = 23,300, PDI = 3.11, acid value 33 (mg KOH / g), and glass transition temperature 20°C. Furthermore, based on the chemicals used, the (meth)acryloyl equivalent was 337 (g / eq), and the type of polymerizable functional group was acryloyl. Furthermore, the structural units (a1), (a2), and (a3), structural units derived from styrene or α-methylstyrene, other monomers, and structural units derived from components other than monomers such as initiators and chain transfer agents were 14%, 9%, 60%, 14%, 0%, and 2%, respectively.
[0094] <Production Examples 2 to 15, Comparative Production Examples 1 to 9> Vinyl copolymers PA2 to 15 and PB1 to 9 were obtained in the same manner as in Production Example 1, except that the production raw materials were changed as shown in Table 1-1 or Table 1-2. The results of measuring the physical properties of the polymers and the content ratio of each structural unit are shown in Table 1-1 or Table 1-2.
[0095] Preparation Example 16: A 500 mL flask equipped with a stirrer and thermometer was charged with 20 g of butyl acrylate, 20 g of lauryl acrylate, 30 g of 2-hydroxyethyl acrylate, 20 g of styrene, and 10 g of methyl methacrylate as monomers, and 50 g of butyl acetate as a polymerization solvent. The mixture was degassed with nitrogen bubbling while stirring, and then heated to 80°C. 0.5 g of 2,2'-azobis(2-methylbutyronitrile) ("ABN-E" manufactured by Nippon Finechem) was added as an initiator to initiate polymerization. Simultaneously, 6.0 g of 2-ethylhexyl thioglycolate was added dropwise over 2 hours as a chain transfer agent. After the reaction was continued for 5 hours from the start of polymerization, the temperature was raised to 90°C and the reaction was continued for an additional 2 hours. Analysis of residual monomers by gas chromatography revealed that the overall monomer conversion was greater than 98%. The temperature was then raised to 90°C, and while blowing in 5% ON (a mixed gas of 5% oxygen and 95% nitrogen), 0.07 g of BHT as a polymerization inhibitor, 25.5 g (0.7 equivalents relative to 2-hydroxyethyl acrylate) of 2-isocyanatoethyl acrylate ("Karenz AOI" manufactured by Resonac) as a modifying agent, 0.03 g of dibutyltin dilaurate as a modifying catalyst, and 21.0 g of butyl acetate as a solvent were added to initiate modification reaction 1, and the reaction was continued for 5 hours. IR analysis of the solution was performed to confirm the change in the peak of the isocyanate group from the initial stage to the end of the reaction, and it was estimated that the reaction rate of 2-isocyanatoethyl acrylate was 98% or higher. The temperature was then raised to 90°C, and 5% ON (a mixed gas of 5% oxygen and 95% nitrogen) was blown in. 7.8 g of succinic anhydride (1.0 equivalent relative to the amount of 2-hydroxyethyl acrylate remaining unreacted with 2-isocyanatoethyl acrylate) as a modifier and 4.2 g of butyl acetate as a solvent were added to initiate modification reaction 2, and the reaction was continued for 3 hours. Analysis of the succinic anhydride by gas chromatography indicated a reaction rate of 98% or greater. This procedure yielded a 65% solution of vinyl copolymer PA16. Analysis of PA16 revealed Mn = 4,400, Mw = 10,600, PDI = 2.41, acid value 31 (mg KOH / g), and glass transition temperature 10°C. Furthermore, based on the reagents used, the (meth)acryloyl equivalent was 773 (g / eq), and the type of polymerizable functional group was acryloyl.The structural units (a1), (a2), and (a3), structural units derived from styrene or α-methylstyrene, other monomers, and structural units derived from components other than monomers such as initiators and chain transfer agents accounted for 29%, 12%, 33%, 14%, 7%, and 5%, respectively.
[0096] Preparation Example 17: A 500 mL flask equipped with a stirrer and thermometer was charged with 30 g of lauryl acrylate as monomers, 16 g of maleic anhydride, 40 g of styrene, and 14 g of methyl acrylate, and 50 g of butyl acetate as a polymerization solvent. The mixture was degassed with nitrogen bubbling while stirring, and then heated to 80°C. 0.5 g of 2,2'-azobis(2-methylbutyronitrile) ("ABN-E" manufactured by Nippon Finechem Co., Ltd.) was added as an initiator to initiate polymerization. Simultaneously, 6.0 g of 2-ethylhexyl thioglycolate was added dropwise over 2 hours as a chain transfer agent. After the reaction was continued for 5 hours from the start of polymerization, the temperature was raised to 90°C and the reaction was continued for an additional 2 hours. Analysis of residual monomers by gas chromatography revealed that the overall monomer conversion was 98% or higher. The temperature was then raised to 90°C, and 5% ON (a mixture of 5% oxygen and 95% nitrogen) was blown in. 0.06 g of BHT as a polymerization inhibitor, 18.9 g of 2-hydroxyethyl acrylate (1.0 equivalent relative to maleic anhydride) as a modifier, 1.3 g of triphenylphosphine as a modification catalyst, and 16.2 g of butyl acetate as a solvent were added to initiate modification reaction 1, and the reaction was continued for 5 hours. Analysis of residual 2-hydroxyethyl acrylate by gas chromatography indicated a reaction rate of 98% or greater. This procedure yielded a 65% solution of vinyl copolymer PA17. Analysis of PA17 revealed Mn = 4,000, Mw = 9,300, PDI = 2.33, acid value 73 (mg KOH / g), and glass transition temperature 50°C. Furthermore, based on the chemicals used, the (meth)acryloyl equivalent was 769 (g / eq), and the type of polymerizable functional group was acryloyl. The structural units (a1), (a2), and (a3), structural units derived from styrene or α-methylstyrene, other monomers, and structural units derived from components other than monomers such as initiators and chain transfer agents accounted for 24%, 14%, 14%, 32%, 11%, and 5%, respectively.
[0097] <Production Example 18> A vinyl copolymer PA18 was obtained in the same manner as in Production Example 17, except that the production raw materials were changed as shown in Table 1-1. The results of measuring the physical properties of the polymer and the content ratio of each structural unit are shown in Table 1-1.
[0098]
[0099] 4. Production and Evaluation of Active Energy Ray-Curable Compositions Active energy ray-curable compositions were prepared using solutions containing vinyl polymers (PA1 to 18 or PB1 to 9) obtained in Production Examples 1 to 18 or Comparative Production Examples 1 to 9 (butyl acetate solutions with copolymer concentrations of 65%) and the following raw materials, and various evaluations were performed. (i) Polyfunctional acrylate: Aronix M-420 (trade name), a pentaerythritol penta- and hexaacrylate manufactured by Toagosei Co., Ltd., was used. (ii) Photopolymerization initiator: Omnirad 184 (trade name), a 1-hydroxycyclohexyl phenyl ketone manufactured by Sanyo Trading Co., Ltd., was used. (iii) Solvent: Butyl acetate was used.
[0100] Example 1 An active energy ray-curable composition was prepared by mixing 76.9 parts of the solution of vinyl polymer PA1 obtained in Production Example 1 (comprising 50 parts of vinyl polymer and 26.9 parts of butyl acetate), 50 parts of a polyfunctional acrylate, 5 parts of a photopolymerization initiator, and 23.1 parts of butyl acetate. This active energy ray-curable composition was then used to produce a cured product, which was then evaluated for tensile properties, water resistance, substrate adhesion, film retention, and alkali solubility (uncured film). The results are shown in Table 2-1.
[0101] (1) Tensile Properties A PET film "Lumirror T-60" (product name, film thickness: 100 μm) manufactured by Toray Industries, Inc. was prepared as a base film, and an active energy ray-curable composition was applied to its surface using a bar coater #0 so that the film thickness after drying would be 30 to 40 μm. Next, the coating film was dried (90°C, 10 minutes) using a forced air dryer to obtain a laminated film having a coating (uncured film). Thereafter, using a high-pressure mercury lamp manufactured by Eye Graphics Co., Ltd., in a concentrated type under atmospheric conditions, the active energy ray-curable composition was applied to the surface of the base film at a UVA irradiance of 500 mW / cm. 2, and the irradiation dose per time is 200 mJ / cm 2 The laminated film was passed twice on a conveyor under this light irradiation, and the coating was irradiated with ultraviolet light to form a cured film. Next, the film with the cured film was cut into 1 cm wide strips, and the cured film was peeled off from the base film. Then, the breaking elongation and breaking strength were measured at a tensile speed of 5 mm / min using a tensile tester "Autograph AGS-J" (trade name) manufactured by Shimadzu Corporation.
[0102] (2) Water Resistance The film having the cured film prepared in (1) above was cut into a piece of 3 x 3 cm, immersed in warm water at 50°C, and left for 7 days. The appearance of the cured film was then visually evaluated based on the following criteria: ○: No change in appearance from the initial state △: Very slight whitening occurred ×: Obvious whitening occurred
[0103] (3) Adhesion to Substrate The active energy ray-curable composition was applied to the surface of a copper plate "C1020" (product name) manufactured by Engineering Test Services Co., Ltd. using a spin coater so that the film thickness after drying would be 4.0 μm. The coating film was then dried (90°C, 10 minutes) using a ventilation dryer to obtain a laminate having a coating (uncured film). Thereafter, using a high-pressure mercury lamp manufactured by Eye Graphics Co., Ltd., the composition was irradiated with UVA light at a UVA irradiance of 500 mW / cm in a concentrated manner under atmospheric conditions. 2 , and the irradiation dose per time is 800 mJ / cm 2 The laminate was adjusted to be 100% by weight, and the laminate was passed twice on a conveyor under this light irradiation to irradiate the coating with ultraviolet light, forming a cured film. Next, the copper plate with the cured film was immersed in a 2.38% tetramethylammonium hydroxide aqueous solution (23 ° C) for 5 minutes, then washed with running ultrapure water for 1 minute, and dried with nitrogen blowing. The cured film after this alkali treatment was subjected to a cross-cut peel test according to JIS K 5600-5-6 to evaluate the substrate adhesion. When all 100 cross-cuts were in adhesion, it was scored as 100 / 100.
[0104] (4) Film Retention A 2.38% aqueous solution of tetramethylammonium hydroxide (23°C) was sprayed onto the cured film of the copper plate with the cured film prepared in (3) above at 0.15 MPa for 1 minute, and then washed with running ultrapure water for 1 minute and dried by nitrogen blowing. Before and after this spraying, the film thickness was measured using a laser microscope "VK-9700" (model name) manufactured by Keyence Corporation, and the film thickness retention was calculated using the following formula: Film Thickness Retention (%) = (film thickness after spraying / film thickness before spraying) × 100
[0105] (5) Alkali Solubility (Uncured Film) An active energy ray-curable composition was applied to the surface of a copper plate "C1020" (product name) manufactured by Engineering Test Services Co., Ltd. using a spin coater so that the film thickness after drying was 4.0 μm. The coating was then dried (90°C, 10 minutes) using a forced air dryer to obtain a laminate having a film (uncured film). Thereafter, a 2.38% aqueous tetramethylammonium hydroxide solution (23°C) was sprayed onto the coating of this laminate at 0.15 MPa, and the time (seconds) until the coating completely dissolved was measured to calculate the alkali dissolution rate (nm / second).
[0106] Examples 2 to 18 and Comparative Examples 1 to 9 Preparation of active energy ray-curable compositions, production of cured products, and evaluation of the cured products were carried out in the same manner as in Example 1, except that the vinyl polymers (polymer solutions containing the vinyl polymers) used were as shown in Table 2-1 or Table 2-2.
[0107]
[0108] The following is clear from Tables 2-1 and 2-2. Examples 1 to 18 exhibited excellent breaking strength in terms of tensile properties, whereas Comparative Example 4 exhibited insufficient flexibility, and sample cracking occurred in the tensile test, making measurement impossible. Similarly, Comparative Example 4 also exhibited poor adhesion. Examples 1 to 18 exhibited excellent water resistance, whereas Comparative Examples 1, 7, 8, and 9 exhibited poor results. Examples 1 to 18 exhibited good film retention, whereas Comparative Examples 2, 3, 5, 7, and 8 exhibited poor results. Furthermore, Examples 1 to 18 exhibited good alkali solubility, whereas Comparative Example 6 exhibited poor results.
[0109] The vinyl polymer of the present invention is suitable as a raw material component of an active energy ray-curable composition useful as a pixel-forming material such as an interlayer insulating film, a planarizing film, a surface protective film, a spacer, a color resist used in the colored layer of a color filter, a black matrix, etc. in display devices such as liquid crystal and organic EL, a material for forming a patterned cured resin layer having contact holes arranged around electrodes in a touch panel, a material for insulating between wirings of a flexible printed circuit board in a semiconductor, a material for forming an interlayer insulating film, a planarizing film, a photoresist, a solder resist, an etching resist, etc. The active energy ray-curable composition of the present invention can also be used as a coating agent, etc.
Claims
1. A vinyl polymer comprising the following structural units (a1), (a2), and (a3): (a1) a structural unit derived from an alkyl acrylate, the alkyl group having 2 or more carbon atoms; (a2) a structural unit having a carboxy group; and (a3) a structural unit having an acryloyl group and / or an acrylamide group; said vinyl polymer having a glass transition temperature (Tg) of -20°C to 60°C, an acid value of 20 to 80 mgKOH / g, and an acryloyl equivalent of 200 to 800 g / eq.
2. The vinyl polymer according to claim 1, wherein the structural unit (a3) comprises at least one structural unit represented by the formula (1) or (2) below: (In the formula, R 1 and R 2 are each independently a hydrogen atom or a methyl group; 1 is hydrogen or a monovalent organic group; Y 1 ~Y 3 each independently represents a divalent alkylene group which may have a ring structure and / or a branched structure, 1 ~Q 4 are each independently -O- or -NH-.
3. The vinyl polymer according to claim 1, wherein the structural unit (a2) comprises a structural unit represented by the following general formula (3): (In the formula, R 3 is a hydrogen atom or a methyl group; Z 1 is a divalent organic group containing an ester bond, Q 5 is -O- or -NH-.) 4. The vinyl polymer according to claim 2 or 3, wherein the alkyl group in the structural unit (a1) has 8 or more carbon atoms.
5. The vinyl polymer according to claim 2 or 3, further comprising structural units derived from styrene and / or α-methylstyrene.
6. The vinyl polymer according to claim 1, wherein the structural units (a2) and (a3) contain a structural unit represented by the following general formula (4): (In the formula, R 4 is a hydrogen atom or a methyl group; Z 2 is a divalent organic group containing an ester bond.
7. The vinyl polymer according to claim 2, 3 or 6, which has a weight average molecular weight of 5,000 to 20,000 as determined by gel permeation chromatography.
8. An active energy ray-curable composition comprising the vinyl polymer according to claim 7.
9. The active energy ray-curable composition according to claim 8, further comprising a photopolymerization initiator.
Citation Information
Patent Citations
Photopolymerizable composition
JP1997251207A
Polymerizable composition
JP2004300315A
Thermosetting composition
JP2009079189A
Thermosetting resin composition containing (METH)acrylate resin, and cured product using the same
JP2012012580A
Photosensitive resin composition for color filter
JP2012193219A