Superhigh-temperature cement paste suspension stabilizer as well as preparation method and application thereof
By using ultra-high temperature cement slurry suspension stabilizer prepared by using specific polymer monomers in deep wells, the problem of instability of settlement at ultra-high temperatures in the prior art is solved, and stability is achieved under 240°C. The performance and construction performance are improved, meeting the safety and quality requirements of deep well ultra-deep well cementing.
Patent Information
- Application Number
- CN202310594836.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-24
Smart Images

Figure CN119019603A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oil and gas well cementing admixtures, and specifically relates to an ultra-high temperature cement slurry suspension stabilizer and a preparation method and application thereof. Background Art
[0002] The oil and gas resources in deep and ultra-deep layers have great potential and have become an important strategic area for increasing oil and gas reserves and production. Oil and gas fields have successively discovered deep oil and gas reservoirs of more than 8,000 meters, and are moving towards 9,000-10,000 meters. The bottom hole temperature has jumped from 180°C to more than 200°C and has broken through 240°C. Cementing is a key technology to ensure the quality of well engineering and achieve safe and efficient development. The quality of cementing is directly related to the success or failure of drilling engineering and the life of oil and gas wells. Deep wells and ultra-deep wells are necessary means to open up deep oil and gas resources, but facing complex geological and complex working conditions such as ultra-deep, ultra-high temperature, and high pressure, the difficulty of cementing has increased dramatically, and the risk of construction operations is high. High-performance ultra-high temperature cement slurry system is the core to ensure the safety and quality of cementing operations in complex deep and ultra-deep wells.
[0003] Sedimentation stability is one of the important parameters to ensure the comprehensive performance of high-temperature cement slurry system, and is particularly important in ultra-high temperature cementing of deep and ultra-deep wells. Under high and ultra-high temperature conditions, the sedimentation stability of cement slurry faces severe challenges: ① The viscosity of cement slurry is weakened, the Brownian motion of particles is accelerated, the suspension capacity of liquid phase is deteriorated, and a large number of solid phase particles are aggregated and settled; ② The system contains a large amount of polymer fluid loss reducers, retarders, etc., which have problems such as high-temperature thinning or even high-temperature degradation failure, resulting in reduced viscosity of cement slurry liquid phase and reduced supporting capacity, aggravating the instability of the system; ③ The cementing annulus gap of deep and ultra-deep wells is small and the sealing section is long, which requires extremely high stability of high-temperature cement slurry. If the cement slurry column is seriously unstable, it will affect the safety and quality of cementing operations, and even cause gas channeling or cementing accidents. Therefore, improving the sedimentation stability of high-temperature and ultra-high temperature cementing slurry systems is crucial to ensuring the safety of cementing operations, cementing quality and long-term effective sealing in deep and ultra-deep wells.
[0004] The prior art has disclosed a variety of methods to solve the above problems. CN102086386A discloses a 200°C oil well cement anti-settling agent prepared by a method of aqueous free radical polymerization of 2-acrylamido-2-methylpropanesulfonic acid (AMPS), acrylamide (AM), and N-vinyl pyrrolidone (NVP). The anti-settling agent can effectively improve the high-temperature sedimentation stability of cement slurry and has been successfully tested in the cementing of deep gas wells in Daqing Oilfield. The bottom hole temperature is 145°C, but it is not suitable for cementing conditions with a bottom hole circulation temperature of more than 200°C. CN107629771A discloses an AMPS / DMAA / AA / NVP copolymer suspension stabilizer with a multi-branched structure. It does not thicken at low temperatures and does not dilute at high temperatures, but its temperature resistance is only 150°C, which cannot meet the downhole environment of deep wells and ultra-deep wells. CN109321219A discloses an oil well cement sedimentation stabilizer, which introduces hydrophobic monomers and utilizes their high-temperature hydrophobic association and phase separation to increase the liquid phase viscosity, achieving low-temperature non-thickening and high-temperature thickening, effectively solving the problem of cement slurry sedimentation instability in deep and ultra-deep wells, but the operating temperature is relatively low (200°C). CN 114409845A provides a 240°C resistant cement slurry suspension stabilizer and its preparation method, which utilizes an organic-inorganic nano-intercalation hybrid polymerization process to organically combine high molecular weight polymers with inorganic materials, and the cement slurry sedimentation stability at 240°C can be controlled at 0.03g / cm 3 It can meet the technical requirements of deep and ultra-deep well cementing, but it involves multiphase mixed reactions of organic and inorganic materials, and the preparation process is relatively complicated.
[0005] Although the above-mentioned existing technologies have achieved certain results in improving the temperature resistance of cement slurry systems and the settlement stability of the systems, most of them still cannot meet the technical requirements for large-scale application of cement slurries for cementing at ultra-high temperatures (above 200°C) in complex deep wells and ultra-deep wells. At present, the settlement stability of cement slurry systems at ultra-high temperatures is improved by simply increasing the amount of polymer suspension stabilizers, but this often leads to severe thickening of the slurry and inability to mix, which is not conducive to deep well and ultra-deep well cementing field operations.
[0006] In view of this, there is an urgent need to develop an ultra-high temperature cement slurry suspension stabilizer to meet the requirements of safe cementing operations and cementing quality in deep wells and ultra-deep wells with ultra-high temperature. Summary of the invention
[0007] In order to solve the above technical problems, the purpose of the present invention is to provide an ultra-high temperature cement slurry suspension stabilizer and its preparation method and application. The ultra-high temperature cement slurry suspension stabilizer of the present invention can withstand high temperatures of 240°C and can meet the requirements of deep well ultra-deep well ultra-high temperature cementing safety operation and cementing quality.
[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides an ultra-high temperature cement slurry suspension stabilizer, which comprises a polymer prepared from a 2-acrylamide-2-methylpropanesulfonic acid monomer, a vinyl polycyclic monomer, an unsaturated acrylamide monomer, an unsaturated cationic monomer and an unsaturated surfactant monomer containing a long carbon side chain;
[0009] Among them, the mass ratio of 2-acrylamide-2-methylpropanesulfonic acid monomer, vinyl polycyclic monomer, unsaturated acrylamide monomer, unsaturated cationic monomer and unsaturated surfactant monomer containing long carbon side chain is (18-25): (5-13): (15-25): (1.7-2.5): (0.5-1.5).
[0010] In the above-mentioned ultra-high temperature cement slurry suspension stabilizer, preferably, the vinyl polycyclic monomer includes one or a combination of N-vinyl pyrrolidone, N-vinyl caprolactam and sodium styrene sulfonate, etc. The present invention uses vinyl polycyclic monomers to inhibit the high temperature hydrolysis of the molecular chain of the prepared polymer, increase the rigidity of the molecular chain, and improve the temperature resistance of the polymer molecular structure.
[0011] In the above-mentioned ultra-high temperature cement slurry suspension stabilizer, preferably, the unsaturated acrylamide monomer includes one or a combination of acrylamide, diacetone acrylamide, N,N-dimethyl acrylamide and N,N-diethyl acrylamide, etc. The unsaturated acrylamide monomer used in the present invention can improve the temperature and salt resistance of the prepared polymer.
[0012] In the above-mentioned ultra-high temperature cement slurry suspension stabilizer, preferably, the unsaturated cationic monomer includes one or a combination of dimethyldiallylammonium chloride, acryloyloxyethyltrimethylammonium chloride and methacryloyloxyethyltrimethylammonium chloride. The present invention adopts the above-mentioned unsaturated cationic monomers to adjust the molecular weight of the prepared polymer, solve the problem of cement slurry ash-down difficulty, and at the same time, form an ion association structure in the polymer solution to further improve the temperature resistance and suspension ability of the polymer.
[0013] In the above-mentioned ultra-high temperature cement slurry suspension stabilizer, preferably, the unsaturated surfactant monomer containing a long carbon side chain includes one or a combination of hexadecyl dimethyl allyl ammonium chloride, 2-acrylamide hexadecane sulfonic acid and 2-acrylamide dodecane sulfonic acid, etc. The present invention adopts the above-mentioned unsaturated surfactant monomer containing a long carbon side chain and introduces a hydrophobic group, which is beneficial to improve the high temperature viscosity increasing ability of the prepared polymer, reduce the molecular weight of the polymer, and can play a solubilizing role, which is beneficial to the solution polymerization reaction.
[0014] According to a specific embodiment of the present invention, preferably, the ultrahigh temperature cement slurry suspension stabilizer is prepared by the following steps:
[0015] A 2-acrylamide-2-methylpropanesulfonic acid monomer, a vinyl polycyclic monomer, an unsaturated acrylamide monomer, an unsaturated cationic monomer and an unsaturated surfactant monomer containing a long carbon side chain in a mass ratio of (18-25): (5-13): (15-25): (1.7-2.5): (0.5-1.5) are polymerized in the presence of an initiator and a solvent to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer. In some specific embodiments of the present invention, the solvent can be water. In some specific embodiments of the present invention, the polymerization reaction temperature can be 70-85°C and the time can be 4-6h.
[0016] More preferably, the ultrahigh temperature cement slurry suspension stabilizer is prepared by the following steps:
[0017] In parts by mass, 18-25 parts of 2-acrylamide-2-methylpropanesulfonic acid monomer are dissolved in 20-30 parts of water, and the pH value is adjusted to 6-7 to obtain a first mixture; 0.5-1.5 parts of an unsaturated surfactant monomer containing a long carbon side chain are dissolved in 120-180 parts of water, and the pH value is selectively adjusted to 6-7 to obtain a second mixture; the first mixture and the second mixture are mixed, and then 15-25 parts of an unsaturated acrylamide monomer, 1.7-2.5 parts of an unsaturated cationic monomer, and 5-13 parts of a vinyl polycyclic monomer are added, and stirred evenly to obtain a third mixture; then an initiator is added to the third mixture, and after a polymerization reaction, a polymer solution is obtained, which is the ultra-high temperature cement slurry suspension stabilizer.
[0018] In some specific embodiments of the present invention, the pH adjuster used to adjust the pH value to 6-7 can be a conventional pH adjuster such as an acid or base in the art, and the present invention does not specifically limit it.
[0019] In some specific embodiments of the present invention, when the unsaturated surfactant monomer containing a long carbon side chain is hexadecyl dimethyl allyl ammonium chloride, the pH value after it is dissolved in water is generally 6-7, and then there is no need to use a pH adjuster to adjust its pH value; when the unsaturated surfactant monomer containing a long carbon side chain is 2-acrylamidohexadecanesulfonic acid and / or 2-acrylamidododecanesulfonic acid, it is generally necessary to use a pH adjuster to adjust its pH value to 6-7.
[0020] In some specific embodiments of the present invention, preferably, the amount of the initiator is 0.05-0.12% of the total mass of the third mixture. Specifically, the initiator can be added dropwise to the third mixture in the form of a solution. The initiator solution can be prepared by the following steps: dissolving 0.05-0.12% of the initiator, in parts by mass, in an appropriate amount of water to obtain an initiator solution. Preferably, the concentration of the initiator in the initiator solution is 0.09-0.34%.
[0021] In some specific embodiments of the present invention, preferably, the initiator includes one or a combination of ammonium persulfate, potassium persulfate and azobisisobutylimidazoline hydrochloride, etc. In the present invention, adding an initiator is beneficial to the polymerization reaction.
[0022] In some specific embodiments of the present invention, preferably, the dropping speed of the initiator solution is 10-20 mL / min.
[0023] In some specific embodiments of the present invention, preferably, during the process of adding the initiator to the third mixture, the reaction temperature is controlled to be 50-65°C, and when the initiator is added, the reaction temperature is controlled to be 70-85°C and the reaction is carried out for 4-6 hours.
[0024] The present invention can make the polymerization reaction proceed smoothly by controlling the dripping speed of the initiator solution, as well as the temperature and time of the polymerization reaction, thereby preparing the ultra-high temperature cement slurry suspension stabilizer of the present invention.
[0025] According to a specific embodiment of the present invention, preferably, the weight average molecular weight of the polymer in the ultra-high temperature cement slurry suspension stabilizer is 1,000,000-1,400,000, and the molecular weight distribution index is 1.8-2.3.
[0026] The ultra-high temperature cement slurry suspension stabilizer of the present invention is a polymer suspension stabilizer prepared by solution polymerization of the above five monomers. The ultra-high temperature cement slurry suspension stabilizer of the present invention adopts a vinyl polycyclic monomer, which is beneficial to inhibiting the high temperature hydrolysis of the molecular chain of the prepared polymer, increasing the rigidity of the molecular chain, and improving the heat resistance of the polymer molecular structure. The unsaturated acrylamide monomer used in the present invention can improve the heat resistance and salt resistance of the prepared polymer. The present invention adopts unsaturated cationic monomers and unsaturated surfactant monomers containing long carbon side chains, wherein the unsaturated cationic monomers increase the polymerization steric hindrance between monomers in the solution due to the ionic bond between the unsaturated cationic monomers, which can regulate the size, charge distribution and molecular chain conformation of the polymer molecular chain, and at the same time, can form an ionic association structure to improve the heat resistance and suspension ability of the polymer; the unsaturated surfactant monomer used in the present invention contains a long carbon side chain and a hydrophobic group in its structure, which can increase the solubility of the polymerized monomer, improve the heat resistance of the prepared polymer, and form a hydrophobic association structure in the solution, further improving the high temperature suspension ability of the polymer solution.
[0027] The ultra-high temperature cement slurry suspension stabilizer of the present invention improves the ultra-high temperature suspension stability of the polymer by means of molecular structure optimization design, synergistic enhancement of anion-cation-hydrophobic multifunctional groups, effective introduction of temperature-resistant and salt-resistant groups, and molecular weight control. Among them, the anion-cation-hydrophobic multifunctional group can regulate the spatial structure of the polymer in the solution, the anion group and the cationic group can improve the adsorption efficiency of the polymer on the surface of cement particles and the adaptability to the material, and the hydrophobic group can improve the spatial association ability of the polymer at high temperature. The coupling effect of the above-mentioned ionic association, hydrophobic association and other multiple effects can enable the polymer prepared by the present invention to actively adapt to the downhole temperature changes and the application environment of the cementing cement slurry, so as to achieve the effect of not excessive thickening at low temperature and not significant dilution at high temperature. The molecular weight and distribution of the polymer are mainly achieved through the polymerization steric hindrance of unsaturated cationic monomers and unsaturated surfactant monomers containing long carbon side chains, so as to shorten the slurry mixing time and reduce the initial consistency, improve the on-site adaptability of the cement slurry and the safety of deep well and ultra-deep well cementing operations.
[0028] The second aspect of the present invention provides a method for preparing the above-mentioned ultra-high temperature cement slurry suspension stabilizer, which comprises the following steps:
[0029] A 2-acrylamide-2-methylpropanesulfonic acid monomer, a vinyl polycyclic monomer, an unsaturated acrylamide monomer, an unsaturated cationic monomer and an unsaturated surfactant monomer containing a long carbon side chain in a mass ratio of (18-25):(5-13):(15-25):(1.7-2.5):(0.5-1.5) are polymerized in the presence of an initiator and a solvent to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer.
[0030] In some specific embodiments of the present invention, the solvent may be water.
[0031] In the above preparation method, preferably, the polymerization reaction temperature may be 70-85° C. and the reaction time may be 4-6 h.
[0032] According to a specific embodiment of the present invention, preferably, the preparation method of the ultra-high temperature cement slurry suspension stabilizer comprises the following steps:
[0033] In parts by mass, 18-25 parts of 2-acrylamide-2-methylpropanesulfonic acid monomer are dissolved in 20-30 parts of water, and the pH value is adjusted to 6-7 to obtain a first mixture; 0.5-1.5 parts of an unsaturated surfactant monomer containing a long carbon side chain are dissolved in 120-180 parts of water, and the pH value is selectively adjusted to 6-7 to obtain a second mixture; the first mixture and the second mixture are mixed, and then 15-25 parts of an unsaturated acrylamide monomer, 1.7-2.5 parts of an unsaturated cationic monomer, and 5-13 parts of a vinyl polycyclic monomer are added, and stirred evenly to obtain a third mixture; then an initiator is added to the third mixture, and after a polymerization reaction, a polymer solution is obtained, which is the ultra-high temperature cement slurry suspension stabilizer.
[0034] In the above-mentioned preparation method, the pH adjuster used to adjust the pH value to 6-7 can be a conventional pH adjuster such as an acid or a base in the art, and the present invention does not specifically limit it.
[0035] In the above-mentioned preparation method, preferably, the amount of the initiator is 0.05-0.12% of the total mass of the third mixture. Specifically, the initiator can be added dropwise to the third mixture in the form of a solution. The initiator solution can be prepared by the following steps: dissolving 0.05-0.12% of the initiator, in parts by mass, in an appropriate amount of water to obtain an initiator solution. Preferably, the concentration of the initiator in the initiator solution is 0.09-0.34%.
[0036] In the above preparation method, preferably, the initiator includes one or a combination of ammonium persulfate, potassium persulfate and azobisisobutylimidazoline hydrochloride.
[0037] In the above preparation method, preferably, the dropping speed of the initiator solution is 10-20 mL / min.
[0038] In the above preparation method, preferably, during the process of adding the initiator to the third mixture, the reaction temperature is controlled to be 50-65°C. When the initiator is added, the reaction temperature is controlled to be 70-85°C and the reaction is carried out for 4-6 hours.
[0039] The third aspect of the present invention provides an application of the above-mentioned ultra-high temperature cement slurry suspension stabilizer as an additive to a cement slurry system for cementing high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, ultra-deep wells, and extra-deep wells.
[0040] According to a specific embodiment of the present invention, in the above-mentioned application, the depth of the deep well is generally 4500-6000m, the depth of the ultra-deep well is generally 6000-9000m, and the depth of the ultra-deep well is generally above 9000m.
[0041] In the above application, preferably, based on 100 parts by mass of cement in the cement slurry system, the added amount of the ultra-high temperature cement slurry suspension stabilizer is 3-5 parts.
[0042] According to a specific embodiment of the present invention, the specific formula of the above-mentioned cement slurry system can be routinely adjusted by those skilled in the art according to actual conditions. Generally speaking, the raw material composition of the cement slurry system includes: 100 parts of cement, 3-5 parts of the ultra-high temperature cement slurry suspension stabilizer of the present invention, 15-50 parts of strength stabilizer, 0 part-appropriate amount of density regulator, 0-3 parts of dispersant, 2-9 parts of fluid loss agent, 0.1-9 parts of retarder, 0-0.5 parts of defoamer and appropriate amount of water, etc. Among them, cement can be G-grade oil well cement, and strength stabilizer, density regulator, dispersant, fluid loss agent, retarder, defoamer, etc. can all be conventional cement slurry system additives in the field, and the present invention does not specifically limit them.
[0043] The existing cement slurry suspension stabilizer loses its performance under high temperature or ultra-high temperature conditions, resulting in deterioration of the cement slurry system's sedimentation stability and severe viscosity increase at room temperature, making it difficult to mix on site and increasing the risk of cementing operations. The ultra-high temperature cement slurry suspension stabilizer provided by the present invention can significantly improve the ultra-high temperature sedimentation stability of the cement slurry system, so that the sedimentation stability of the cement slurry system under 240°C can be controlled within 0.03g / cm 3 (upper and lower density difference) and has no adverse effects on its construction performance and mechanical properties, and can meet the cementing technology requirements of deep wells and ultra-deep wells with bottom hole circulation temperature of 240℃ and below.
[0044] The ultra-high temperature cement slurry suspension stabilizer of the present invention produces a certain degree of intramolecular and intermolecular association through hydrophobic groups under room temperature (20°C-30°C), reduces the hydrodynamic radius of the polymer molecular chain, prevents the polymer molecular chain from excessively stretching in water, a large amount of association into a network, and strong adsorption on the surface of cement particles, etc. At the same time, unsaturated cationic monomers and unsaturated surfactant monomers containing long carbon side chains effectively regulate the polymer molecular weight and its distribution, reduce its low-temperature viscosity-increasing characteristics, and effectively solve the problem of cement slurry ash removal difficulties. As the temperature rises (30°C-160°C), the polymer molecular chains of the ultra-high temperature cement slurry suspension stabilizer of the present invention gradually stretch, increase hydrophilicity, and gradually expose hydrophobic side chains, forming a polymer solution with a spatial network structure through the hydrophobic association structure of the hydrophobic micro-region; at the same time, the anionic groups and cationic groups in the polymer structure selectively adsorb on the surfaces of different types of cement minerals and solid phase particles, "locking" the solid phase particles in the slurry, and improving the sedimentation stability of the cement slurry. Under high temperature and ultra-high temperature (>160°C) conditions, the polycyclic impedance groups in the polymer of the ultra-high temperature cement slurry suspension stabilizer of the present invention protect the amide groups to prevent high temperature hydrolysis. Therefore, the main chain, side chain and spatial network structure of the polymer molecule are not completely disintegrated, and still have strong solid phase suspension ability. At the same time, the polymer spatial network structure formed by ionic association and hydrophobic association becomes denser as the temperature rises, which can effectively alleviate the high temperature dilution phenomenon of the cement slurry liquid phase and improve the high temperature suspension supporting capacity of the liquid phase, thereby improving the rheological properties of the slurry and improving the ultra-high temperature stability of the cement slurry system, ensuring the comprehensive performance of the cement slurry system, and ensuring the safety of deep well and ultra-deep well cementing operations and long-term stable sealing capabilities.
[0045] The technical solution of the present invention has at least the following beneficial effects:
[0046] (1) The ultra-high temperature cement slurry suspension stabilizer of the present invention improves the ultra-high temperature resistance and suspension stability of the polymer suspension stabilizer by means of the effective introduction of temperature-resistant and salt-resistant groups, rigid ring structure suspension support, synergistic enhancement of anion-cation-hydrophobic multifunctional groups and self-regulation of molecular weight, and improves the construction performance of the cement slurry system, thereby enhancing the ability of the cement slurry system to adapt to complex environments in complex wells such as deep wells and ultra-deep wells.
[0047] (2) The ultra-high temperature cement slurry suspension stabilizer of the present invention has a temperature resistance of up to 240°C, and the sedimentation stability of the cement slurry system is controlled at 0.03 g / cm at 240°C. 3 It has good compatibility with other cement slurry system admixtures and has no adverse effects on the construction performance and mechanical properties of the cement slurry system.
[0048] (3) The preparation method of the ultra-high temperature cement slurry suspension stabilizer of the present invention is simple, green, safe and environmentally friendly, the raw materials are easily available and the production cost is low, and it can realize industrial production and large-scale promotion and application.
[0049] (4) The ultra-high temperature cement slurry suspension stabilizer of the present invention has strong adaptability and can meet the cementing technical requirements of special wells such as high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, ultra-deep wells, and extra-deep wells.
[0050] In summary, the present invention provides an ultra-high temperature cement slurry suspension stabilizer and its preparation method and application, in particular, a 240°C high temperature resistant cement slurry polymer suspension stabilizer suitable for deep well and ultra-deep well cementing and its preparation method and application. The ultra-high temperature cement slurry suspension stabilizer provided by the present invention has a wide applicable temperature range and can control the sedimentation stability of the cement slurry system at 240°C to 0.03g / cm 3 The raw materials of the ultra-high temperature cement slurry suspension stabilizer of the present invention are cheap and easily available, and have good compatibility with other additives of cementing cement slurry systems, which significantly improves the comprehensive performance of the cement slurry system and meets the requirements of ultra-high temperature cementing safety operations and cementing quality in deep wells and ultra-deep wells. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is the infrared spectrum of the polymer in the ultra-high temperature cement slurry suspension stabilizer provided in Example 1.
[0052] Figure 2a , Figure 2b , Figure 2c and Figure 2d ESEM images of the polymer solutions prepared in Example 3 and Comparative Example 1 after being treated at 25° C. and 240° C. for 2 h, respectively.
[0053] Figure 3 The thickening curve of the cement slurry system mixed with the ultra-high temperature cement slurry suspension stabilizer provided in Example 1 under the conditions of 240°C×100MPa.
[0054] Figure 4 It is a thickening curve diagram of the cement slurry system mixed with the high-temperature cement slurry suspension stabilizer provided in Comparative Example 1 under the conditions of 240°C×100MPa. DETAILED DESCRIPTION
[0055] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0056] According to a specific embodiment of the present invention, preferably, the ultrahigh temperature cement slurry suspension stabilizer provided by the present invention is prepared by at least the following steps:
[0057] Dissolve 18-25 parts by mass of 2-acrylamide-2-methylpropanesulfonic acid monomer in 20-30 parts of deionized water, and adjust the pH value to 6-7 to obtain a first mixture;
[0058] Dissolving 0.5-1.5 parts of an unsaturated surfactant monomer containing a long carbon side chain in 120-180 parts of deionized water, and selectively adjusting the pH value to 6-7 to obtain a second mixture;
[0059] The first mixture and the second mixture are fully mixed, and then 15-25 parts of unsaturated acrylamide monomers, 1.7-2.5 parts of unsaturated cationic monomers, and 5-13 parts of vinyl polycyclic monomers are added in sequence, and stirred evenly to obtain a third mixture;
[0060] dissolving 0.05-0.12% of the initiator, which accounts for 0.05-0.12% of the total mass of the third mixture, in 100 parts of deionized water to obtain an initiator solution (the concentration of the initiator in the initiator solution is 0.09-0.34%);
[0061] The initiator solution is added to the third mixture at a dropping speed of 10-20 mL / min, and in the process of adding the initiator solution to the third mixture, the reaction temperature is controlled to be 50-65°C. After the initiator solution is added, the reaction temperature is controlled to be 70-85°C and the reaction is carried out for 4-6 hours to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer.
[0062] Example 1
[0063] This embodiment provides an ultra-high temperature cement slurry suspension stabilizer, which is prepared by at least the following steps:
[0064] Dissolve 25 g of 2-acrylamido-2-methylpropanesulfonic acid in 30 g of deionized water, and slowly add 4.5 g of sodium hydroxide to adjust the pH value to 7 to obtain a first mixture;
[0065] Dissolving 1.5 g of hexadecyldimethylallyl ammonium chloride in 170 g of deionized water to obtain a second mixture;
[0066] The first mixture and the second mixture are fully mixed, and then 25 g of N,N-dimethylacrylamide, 2.5 g of acryloyloxyethyl trimethylammonium chloride, and 12 g of N-vinyl pyrrolidone are added in sequence, and stirred evenly to obtain a third mixture;
[0067] Dissolve 0.318 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0068] The initiator solution is added to the third mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 65°C. After the dropping is completed, the temperature is raised to 85°C for reaction. The reaction time is 4 hours to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer.
[0069] Example 2
[0070] This embodiment provides an ultra-high temperature cement slurry suspension stabilizer, which is prepared by at least the following steps:
[0071] Dissolve 18 g of 2-acrylamido-2-methylpropanesulfonic acid in 25 g of deionized water, and slowly add 3.2 g of sodium hydroxide to adjust the pH value to 6 to obtain a first mixture;
[0072] Dissolving 0.5 g of hexadecyldimethylallyl ammonium chloride in 125 g of deionized water to obtain a second mixture;
[0073] The first mixture and the second mixture are fully mixed, and then 15 g of N,N-dimethylacrylamide, 1.7 g of acryloyloxyethyl trimethylammonium chloride, and 8 g of N-vinyl pyrrolidone are added in sequence, and stirred evenly to obtain a third mixture;
[0074] Dissolve 0.147 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0075] The initiator solution is added to the third mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 65°C. After the dropping is completed, the temperature is raised to 85°C for reaction. The reaction time is 4 hours to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer.
[0076] Example 3
[0077] This embodiment provides an ultra-high temperature cement slurry suspension stabilizer, which is prepared by at least the following steps:
[0078] Dissolve 21 g of 2-acrylamido-2-methylpropanesulfonic acid in 25 g of deionized water, and slowly add 4.2 g of sodium hydroxide to adjust the pH value to 6 to obtain a first mixture;
[0079] Dissolve 1 g of hexadecyldimethylallyl ammonium chloride in 155 g of deionized water to obtain a second mixture;
[0080] The first mixture and the second mixture are fully mixed, and then 20 g of N,N-dimethylacrylamide, 2.3 g of acryloyloxyethyl trimethylammonium chloride, and 10 g of N-vinyl pyrrolidone are added in sequence, and stirred evenly to obtain a third mixture;
[0081] Dissolve 0.225 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0082] The initiator solution is added to the third mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 60°C. After the dropping is completed, the temperature is raised to 75°C for reaction. The reaction time is 5 hours to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer.
[0083] Example 4
[0084] This embodiment provides an ultra-high temperature cement slurry suspension stabilizer, which is prepared by at least the following steps:
[0085] Dissolve 25 g of 2-acrylamido-2-methylpropanesulfonic acid in 30 g of deionized water, and slowly add 4.5 g of sodium hydroxide to adjust the pH value to 6 to obtain a first mixture;
[0086] Dissolve 1.5 g of 2-acrylamidohexadecanesulfonic acid in 170 g of deionized water, and slowly add 0.2 g of sodium hydroxide to adjust the pH value to 6 to obtain a second mixture;
[0087] The first mixture and the second mixture are fully mixed, and then 25 g of N,N-dimethylacrylamide, 2 g of methacryloyloxyethyl trimethylammonium chloride, and 5 g of N-vinyl caprolactam are added in sequence, and stirred evenly to obtain a third mixture;
[0088] Dissolve 0.318 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0089] The initiator solution is added to the third mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 65°C. After the dropping is completed, the temperature is raised to 85°C for reaction. The reaction time is 4 hours to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer.
[0090] Example 5
[0091] This embodiment provides an ultra-high temperature cement slurry suspension stabilizer, which is prepared by at least the following steps:
[0092] Dissolve 25 g of 2-acrylamido-2-methylpropanesulfonic acid in 30 g of deionized water, and slowly add sodium hydroxide to adjust the pH value to 7 to obtain a first mixture;
[0093] Dissolving 1.5 g of hexadecyldimethylallyl ammonium chloride in 170 g of deionized water to obtain a second mixture;
[0094] The first mixture and the second mixture are fully mixed, and then 25 g of N,N-dimethylacrylamide, 2.5 g of acryloyloxyethyl trimethylammonium chloride, and 12 g of N-vinyl pyrrolidone are added in sequence, and stirred evenly to obtain a third mixture;
[0095] Dissolve 0.318 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0096] The initiator solution is added to the third mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 50°C. After the dropping is completed, the temperature is raised to 70°C for reaction. The reaction time is 6 hours to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer.
[0097] Comparative Example 1
[0098] This comparative example provides a high-temperature cement slurry suspension stabilizer, which differs from Example 1 in that no unsaturated cationic monomer is added. Specifically, the high-temperature cement slurry suspension stabilizer of this comparative example is prepared by at least the following steps:
[0099] Dissolve 25 g of 2-acrylamido-2-methylpropanesulfonic acid in 30 g of deionized water, and slowly add 4.5 g of sodium hydroxide to adjust the pH value to 7 to obtain a first mixture;
[0100] Dissolving 1.5 g of hexadecyldimethylallyl ammonium chloride in 170 g of deionized water to obtain a second mixture;
[0101] The first mixture and the second mixture are fully mixed, and then 25 g of N,N-dimethylacrylamide and 12 g of N-vinyl pyrrolidone are added in sequence, and stirred evenly to obtain a third mixture;
[0102] Dissolve 0.318 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0103] The initiator solution is added to the third mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 65°C. After the dropping is completed, the temperature is raised to 85°C for reaction. The reaction time is 4 hours to obtain a polymer solution, which is the high-temperature cement slurry suspension stabilizer.
[0104] Comparative Example 2
[0105] This comparative example provides a high-temperature cement slurry suspension stabilizer, which differs from Example 1 in that no unsaturated surfactant monomer containing a long carbon side chain is added. Specifically, the high-temperature cement slurry suspension stabilizer of this comparative example is prepared by at least the following steps:
[0106] 25 g of 2-acrylamido-2-methylpropanesulfonic acid was dissolved in 30 g of deionized water, 4.5 g of sodium hydroxide was slowly added to adjust the pH value to 7, and then 170 g of deionized water was added, and then 25 g of N,N-dimethylacrylamide, 2.5 g of acryloyloxyethyltrimethylammonium chloride, and 12 g of N-vinylpyrrolidone were added in sequence, and stirred evenly to obtain a mixture;
[0107] Dissolve 0.318 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0108] The initiator solution is added to the mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 65° C. After the dropping is completed, the temperature is raised to 85° C. for reaction. The reaction time is 4 hours to obtain a polymer solution, which is the high-temperature cement slurry suspension stabilizer.
[0109] Comparative Example 3
[0110] This comparative example provides a high-temperature cement slurry suspension stabilizer, which is different from Example 1 in that the amount of the unsaturated surfactant monomer containing a long carbon side chain is 2 g. Specifically, the high-temperature cement slurry suspension stabilizer of this comparative example is prepared by at least the following steps:
[0111] Dissolve 25 g of 2-acrylamido-2-methylpropanesulfonic acid in 30 g of deionized water, and slowly add 4.5 g of sodium hydroxide to adjust the pH value to 7 to obtain a first mixture;
[0112] Dissolve 2 g of hexadecyldimethylallyl ammonium chloride in 170 g of deionized water to obtain a second mixture;
[0113] The first mixture and the second mixture are fully mixed, and then 25 g of N,N-dimethylacrylamide, 2.5 g of acryloyloxyethyl trimethylammonium chloride, and 12 g of N-vinyl pyrrolidone are added in sequence, and stirred evenly to obtain a third mixture;
[0114] Dissolve 0.318 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0115] The initiator solution is added to the third mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 65°C. After the dropping is completed, the temperature is raised to 85°C for reaction. The reaction time is 4 hours to obtain a polymer solution, which is the high-temperature cement slurry suspension stabilizer.
[0116] Comparative Example 4
[0117] This comparative example provides a high-temperature cement slurry suspension stabilizer, which is different from Example 1 in that the amount of the unsaturated cationic monomer added is 3 g. Specifically, the high-temperature cement slurry suspension stabilizer of this comparative example is prepared by at least the following steps:
[0118] Dissolve 25 g of 2-acrylamido-2-methylpropanesulfonic acid in 30 g of deionized water, and slowly add 4.5 g of sodium hydroxide to adjust the pH value to 7 to obtain a first mixture;
[0119] Dissolving 1.5 g of hexadecyldimethylallyl ammonium chloride in 170 g of deionized water to obtain a second mixture;
[0120] The first mixture and the second mixture are fully mixed, and then 25 g of N,N-dimethylacrylamide, 3 g of acryloyloxyethyl trimethylammonium chloride, and 12 g of N-vinyl pyrrolidone are added in sequence, and stirred evenly to obtain a third mixture;
[0121] Dissolve 0.318 g of potassium persulfate in 100 g of deionized water to obtain an initiator solution;
[0122] The initiator solution is added to the third mixture at a dropping speed of 10 mL / min. During the dropping of the initiator solution, the water bath heating temperature is controlled to be 65°C. After the dropping is completed, the temperature is raised to 85°C for reaction. The reaction time is 4 hours to obtain a polymer solution, which is the high-temperature cement slurry suspension stabilizer.
[0123] Test Example 1
[0124] In this test example, the cement slurry suspension stabilizers prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were tested and analyzed by gel permeation chromatography. The results are shown in Table 1.
[0125] Table 1
[0126] Number average molecular weight Weight average molecular weight Distribution Index Example 1 560415 1058652 1.88905 Example 2 677219 1295621 1.91315 Example 3 677969 1302683 1.92145 Example 4 603983 1353682 2.24126 Example 5 510608 1152401 2.25692 Comparative Example 1 851710 2265156 2.65954 Comparative Example 2 278460 502654 1.80512 Comparative Example 3 278460 1401458 2.64056 Comparative Example 4 278503 656892 2.35865
[0127] As shown in Table 1, the weight average molecular weight of the polymers prepared in Examples 1 to 5 is between 1 million and 1.4 million, and the molecular weight distribution index is between 1.8 and 2.3. In the comparative examples, comparative example 1 does not add unsaturated cationic monomers, so the molecular weight and molecular weight distribution of the polymer cannot be effectively regulated, resulting in the molecular weight and distribution index of the polymer being far greater than the recommended range, which will lead to excessive polymer viscosity enhancement, which may affect cement ash removal; comparative example 2 does not add unsaturated surfactant monomers containing long carbon side chains. Although the polymer has a suitable molecular weight distribution index, the molecular weight is too small. This is because the polymer of the unsaturated surfactant monomer without the introduction of long carbon side chains has few long chain alkyl groups distributed on the side chains, resulting in a decrease in molecular weight, and too low molecular weight and few alkane groups in the side chains will lead to poor suspension ability of the polymer; comparative example 3 adds an excessive amount of unsaturated surfactant monomers, resulting in a large molecular weight distribution index. This is because the unsaturated surfactant monomer itself contains multiple functional groups, and the excessive introduction makes the polymerization process more complicated and the product more inhomogeneous; comparative example 4 adds an excessive amount of unsaturated cationic monomers, and the steric hindrance of the cationic monomers affects the polymerization reaction, so the molecular weight of the polymer is reduced.
[0128] Test Example 2
[0129] In this test example, the ultra-high temperature cement slurry suspension stabilizer prepared in Example 1 was subjected to infrared spectroscopy analysis. The obtained infrared spectrum is shown in the figure below. Figure 1 shown.
[0130] The polymer prepared in Example 1 after purification was scanned by infrared spectrum using KBr tablet method with Fourier transform infrared spectrometer in the wave number range of 4000-400 cm -1 The step of purifying the polymer solution prepared in Example 1 includes: precipitating the polymer solution with an appropriate amount of ethanol solution, washing and drying, repeating the process three times, and then crushing to obtain a purified polymer.
[0131] Depend on Figure 1 It can be seen that 3439.8cm -1 、1543.3cm -1 is the NH stretching vibration peak of the amide group, 1640.9 cm -1 is the stretching vibration peak of C=O in the amide group, 1700 cm -1 The absorption near is the stretching vibration of -C=O on the pyrrole ring, 2920.1cm -1 、2065.6cm -1、1443.8cm -1 、1404.1cm -1 The CH characteristic peak of methyl (-CH3), 1188.7cm -1 、1043.9cm -1 and 977.2cm -1 It is the characteristic peak of S=O in the sulfonic acid group, 651.8cm -1 It is the characteristic peak of SO in sulfonic acid group, 1291cm -1 -CN- stretching vibration peak, 720.2cm -1 It is the characteristic peak of -CH2- of long carbon side chain alkane and is at 1650cm -1 No characteristic peak of C=C double bond appears nearby; this indicates that all monomers in Example 1 participate in the copolymerization reaction, and the product is the target product, i.e., a five-membered copolymer of 2-acrylamido-2-methylpropanesulfonic acid, hexadecyldimethylallylammonium chloride, N,N-dimethylacrylamide, acryloyloxyethyltrimethylammonium chloride, and N-vinylpyrrolidone.
[0132] Test Example 3
[0133] In this test example, the microstructure of the polymers obtained after the polymer solutions prepared in Example 3 and Comparative Example 1 were treated at 25° C. and 240° C. for 2 hours were analyzed by environmental scanning electron microscopy (ESEM).
[0134] Figure 2a and Figure 2b The microstructure of the polymer solution prepared in Comparative Example 1 after being treated at 25°C and 240°C. Figure 2a and Figure 2b It can be seen that at room temperature, the polymer prepared in Comparative Example 1 is basically a linear structure, and the molecular chains are hydrophobically associated by the reactive surfactant to form a network structure as a whole. However, as the temperature rises, the hydrophobic association structure between molecules is gradually destroyed, and the molecular chains undergo partial chain scission and conformational transformation. The microstructure of the polymer treated at 240°C is spherical, resulting in the polymer suspension stabilizer having basically no suspension support capacity at ultra-high temperature and failing in performance. Therefore, the cement slurry system mixed with the high-temperature cement slurry suspension stabilizer prepared in Comparative Example 1 is severely precipitated after being cured at 240°C.
[0135] Figure 2c and Figure 2d The microstructure of the polymer solution prepared in Example 3 after being treated at 25°C and 240°C. Figure 2c and Figure 2dIt can be seen that at room temperature, the polymer prepared in Example 3 presents a stacked, porous mucosal conformation in water. The reason is that the polymer has a spatial network structure through ionic association and hydrophobic association between and within the polymer molecules, which can significantly increase the viscosity and supporting capacity of the polymer solution and prevent solid phase particles such as cement from sinking; the polymer treated at 240°C still presents a spatial network structure, and the interaction between molecular segments is strong, indicating that the microstructure of the polymer prepared in Example 3 after ultra-high temperature treatment changes little or only part of the segments are destroyed without affecting its overall performance. Therefore, the ultra-high temperature cement slurry suspension stabilizer provided in Example 3 has strong temperature resistance and ultra-high temperature suspension stability.
[0136] Test Example 4
[0137] According to the relevant provisions of the petroleum and natural gas industry standard GB / T 19139-2012 "Test Methods for Oil Well Cement", the performance of the suspension stabilizers prepared in Examples 1 to 5 and Comparative Examples 1 to 4 was evaluated, and the results are shown in Table 2. The investigation of the sedimentation stability of the cement slurry system includes: the cement slurry system is cured at the experimental temperature and pressure for 30 minutes through a high-temperature and high-pressure thickener, then cooled to 90°C, removed, and the surface floating oil is removed, and the density difference d of the upper and lower parts of the cement slurry is tested. m1 After stirring evenly, place it at 90℃ for 2 hours and test the density difference d of the upper and lower cement slurry m2 , and the free fluid was examined at the same time.
[0138] In order to simulate the change in the sedimentation stability performance of the cement slurry system when pumping is stopped midway due to an unexpected situation during the ultra-high temperature cementing operation of deep wells and ultra-deep wells, the cement slurry system mixed with the suspension stabilizer of the embodiment of the present invention and the comparative example was investigated at the experimental temperature and pressure. The viscosity change value at the moment of startup after stopping for 30 minutes was studied to study its sedimentation stability performance; if the instantaneous viscosity recoil value at startup is greater than 40Bc, the fluid pumping pressure will be greatly increased, and there is a risk of leaking the formation; if it is less than 40Bc, the sedimentation stability of the cement slurry system is considered to be good.
[0139] Therefore, this test example combines the above-mentioned multiple methods to investigate the improvement effect of the suspension stabilizer on the sedimentation stability of the ultra-high temperature cement slurry system.
[0140] Table 2
[0141]
[0142] Note: # represents the mass percentage of cement; d m1 The cement slurry system is cured at the experimental temperature and pressure for 30 minutes, then cooled to 90°C, removed, and the surface oil removed, and the upper and lower density difference is directly tested; d m2It is the difference in density between the upper and lower density after the cement slurry system is stirred evenly after high-temperature curing and then placed in a 90℃ water bath for curing for 2 hours.
[0143] The formula of the cement slurry system used in this test at an experimental temperature above 160°C is: by mass, 100 parts of Jiahua G-grade oil well cement (HSR) + 50 parts of quartz sand (200 mesh) + 1.2 parts of the first dispersant + 1.2 parts of the second dispersant + 4 parts of fluid loss additive + 5 parts of retarder + x parts (i.e. % bwoc in Table 2) of suspension stabilizer + (56-x) parts of water; the density of the cement slurry system is 1.90 g / cm 3 .
[0144] The formula of the cement slurry system used in this test at an experimental temperature of 120-160°C is: by mass, 100 parts of Jiahua G-grade oil well cement (HSR) + 35 parts of quartz sand (200 mesh) + 3 parts of microsilica + 0.8 parts of the first dispersant + 4 parts of fluid loss additive + 2 parts of retarder + x parts (i.e. %bwoc in Table 2) of suspension stabilizer + (53-x) parts of water; the density of the cement slurry system is 1.90 g / cm 3 .
[0145] Among them, the first dispersant, the second dispersant, the retarder and the fluid loss reducer are respectively the aldehyde-ketone condensation polymer dispersant DRS-1S, the polycarboxylic acid dispersant DRS-2S, the acrylamide retarder DRH-3L and the acrylamide fluid loss reducer DRF-3L, all of which are products produced by China National Petroleum Corporation Engineering and Technology Research Institute Co., Ltd.
[0146] As shown in Table 2, under the experimental condition of 240°C, the cement slurry system containing the ultra-high temperature cement slurry suspension stabilizer provided by Examples 1-5 of the present invention has a ash-lowering time of less than 35s, good fluidity, and a sedimentation stability controlled at 0.03 g / cm 3 Below this value, there is no free liquid and the ultra-high temperature thickening experiment is normal.
[0147] However, the cement slurry system containing the high temperature cement slurry suspension stabilizer provided in Comparative Example 1 and Comparative Example 2 was difficult to ash (>60s), the slurry thickened severely, and the sedimentation stability was poor (>0.1g / cm 3 ), there is a lot of free liquid (>1.4%) and the viscosity rebounds high when the machine is restarted after stopping for 30 minutes.
[0148] Although the cement slurry systems added with the high-temperature cement slurry suspension stabilizers provided in Comparative Examples 3 and 4 are easy to ash and have good fluidity, the system stability, free liquid and stoppage tests cannot meet the requirements of cementing operations.
[0149] The reasons for the above differences are preliminarily analyzed as follows: the molecular structure of the suspension stabilizer prepared in Comparative Example 1 does not contain groups provided by unsaturated cationic monomers, the polymer has a high molecular weight and cannot form an ion association structure at high temperature, so it has the characteristics of room temperature viscosity increase and high temperature dilution, thereby affecting the mixing and sedimentation stability of the high temperature cement slurry system. The suspension stabilizer prepared in Comparative Example 2 does not use unsaturated surfactant monomers containing long carbon side chains, the polymer molecular weight is large and there is no hydrophobic association structure, therefore, the room temperature viscosity increase of the cement slurry system is serious, the high temperature sedimentation stability is poor, and the serious sedimentation leads to the problem of thickening suspension, which poses a great challenge to the safety of ultra-deep well and ultra-high temperature cementing operations. The suspension stabilizers prepared in Comparative Examples 3 and 4 respectively introduce excessive unsaturated cationic monomers and excessive unsaturated surfactant monomers containing long carbon side chains, the monomer polymerization steric hindrance is large, affecting the polymer reaction process, the molecular weight of the obtained polymer suspension stabilizer is low, and the excessive cationic groups act on the surface of cement particles to change their surface charge distribution, thereby causing the cement slurry system to become unstable under ultra-high temperature conditions. The comparison between the above-mentioned embodiments and comparative examples also verifies the superiority of the molecular structure of the ultra-high temperature cement slurry suspension stabilizer prepared in the embodiments of the present invention, which ultimately determines its excellent performance.
[0150] Figure 3 The thickening curve of the cement slurry system mixed with the ultra-high temperature cement slurry suspension stabilizer provided in Example 1 under the conditions of 240°C×100MPa. Figure 3 It can be seen that the consistency curve of the cement slurry system mixed with the ultra-high temperature cement slurry suspension stabilizer prepared in Example 1 is stable, the initial consistency is about 18Bc, and as the temperature increases, the consistency decreases slightly, and there is no adverse phenomenon such as abnormal gelation during the thickening process.
[0151] Figure 4 This is a thickening curve of the cement slurry system mixed with the high-temperature cement slurry suspension stabilizer provided in Comparative Example 1 under the conditions of 240°C×100MPa. Figure 4 It can be seen that the installed consistency of the cement slurry system is 35Bc, which cannot meet the on-site mixing requirements, and the consistency decreases significantly with increasing temperature. This phenomenon shows that the high-temperature cement slurry suspension stabilizer prepared in Comparative Example 1 has obvious room temperature viscosity-increasing properties, making the cement slurry system difficult to mix on-site. In addition, the polymer solution in the cement slurry liquid phase is severely diluted at high temperature, and the sedimentation stability of the system gradually deteriorates, thereby affecting the comprehensive performance of the cement slurry system and increasing the risk of cementing operations.
[0152] Therefore, the ultra-high temperature cement slurry suspension stabilizer provided by the embodiment of the present invention has a temperature resistance of more than 240°C, which can significantly improve the sedimentation stability of the ultra-high temperature cement slurry system, and its comprehensive performance is better than that of the suspension stabilizer provided by the comparative example. At the same time, the ultra-high temperature cement slurry suspension stabilizer prepared by the embodiment of the present invention has a wide applicable temperature range. In the experimental temperature range of 120-240°C, by adjusting the amount of ultra-high temperature cement slurry suspension stabilizer, the construction performance of the cement slurry system can be significantly improved to ensure the safety of deep well and ultra-deep well cementing operations.
[0153] In summary, the ultra-high temperature cement slurry suspension stabilizer of the present invention has a wide applicable temperature range and stable performance, and can ensure the comprehensive performance of the cementing cement slurry system with a bottom hole circulation temperature of 240°C and below and the safety of ultra-high temperature cementing operations. It has good application prospects in cementing of deep wells, ultra-deep wells, extra-deep wells, high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, etc.
[0154] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. An ultra-high temperature cement slurry suspension stabilizer, the suspension stabilizer comprising a polymer prepared from 2-acrylamide-2-methylpropanesulfonic acid monomer, vinyl polycyclic monomer, unsaturated acrylamide monomer, unsaturated cationic monomer and unsaturated surfactant monomer containing a long carbon side chain; in, The mass ratio of 2-acrylamide-2-methylpropanesulfonic acid monomer, vinyl polycyclic monomer, unsaturated acrylamide monomer, unsaturated cationic monomer and unsaturated surfactant monomer containing long carbon side chain is (18-25): (5-13): (15-25): (1.7-2.5): (0.5-1.5).
2. The ultra-high temperature cement slurry suspension stabilizer according to claim 1, wherein: The vinyl polycyclic monomer includes one or a combination of N-vinyl pyrrolidone, N-vinyl caprolactam and sodium styrene sulfonate.
3. The ultra-high temperature cement slurry suspension stabilizer according to claim 1, wherein: The unsaturated acrylamide monomers include one or a combination of acrylamide, diacetone acrylamide, N,N-dimethyl acrylamide and N,N-diethyl acrylamide.
4. The ultra-high temperature cement slurry suspension stabilizer according to claim 1, wherein: The unsaturated cationic monomer includes one or a combination of dimethyldiallylammonium chloride, acryloyloxyethyltrimethylammonium chloride and methacryloyloxyethyltrimethylammonium chloride.
5. The ultra-high temperature cement slurry suspension stabilizer according to claim 1, wherein: The unsaturated surfactant monomer containing a long carbon side chain includes one or a combination of hexadecyldimethylallylammonium chloride, 2-acrylamidohexadecanesulfonic acid and 2-acrylamidododecanesulfonic acid.
6. The ultra-high temperature cement slurry suspension stabilizer according to any one of claims 1 to 5, wherein: The ultra-high temperature cement slurry suspension stabilizer is prepared by the following steps: A 2-acrylamide-2-methylpropanesulfonic acid monomer, a vinyl polycyclic monomer, an unsaturated acrylamide monomer, an unsaturated cationic monomer and an unsaturated surfactant monomer containing a long carbon side chain in a mass ratio of (18-25): (5-13): (15-25): (1.7-2.5): (0.5-1.5) are polymerized in the presence of an initiator and a solvent to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer; Preferably, the ultrahigh temperature cement slurry suspension stabilizer is prepared by the following steps: In parts by mass, 18-25 parts of 2-acrylamide-2-methylpropanesulfonic acid monomer are dissolved in 20-30 parts of water, and the pH value is adjusted to 6-7 to obtain a first mixture; 0.5-1.5 parts of an unsaturated surfactant monomer containing a long carbon side chain are dissolved in 120-180 parts of water, and the pH value is selectively adjusted to 6-7 to obtain a second mixture; the first mixture and the second mixture are mixed, and then 15-25 parts of an unsaturated acrylamide monomer, 1.7-2.5 parts of an unsaturated cationic monomer, and 5-13 parts of a vinyl polycyclic monomer are added, and stirred evenly to obtain a third mixture; then an initiator is added to the third mixture, and after a polymerization reaction, a polymer solution is obtained, which is the ultra-high temperature cement slurry suspension stabilizer.
7. The ultra-high temperature cement slurry suspension stabilizer according to claim 6, wherein: The amount of the initiator used is 0.05-0.12% of the total mass of the third mixture.
8. The ultra-high temperature cement slurry suspension stabilizer according to claim 6, wherein: The initiator includes one or a combination of ammonium persulfate, potassium persulfate and azobisisobutylimidazoline hydrochloride.
9. The ultra-high temperature cement slurry suspension stabilizer according to claim 6, wherein: The initiator is added dropwise to the third mixture in the form of a solution; the concentration of the initiator in the initiator solution is 0.09-0.34%; and the dropping speed of the initiator solution is 10-20 mL / min.
10. The ultra-high temperature cement slurry suspension stabilizer according to claim 6, wherein: In the process of adding the initiator to the third mixture, the reaction temperature is controlled to be 50-65° C., and when the initiator is added, the reaction temperature is controlled to be 70-85° C. and the reaction is carried out for 4-6 hours.
11. A method for preparing the ultra-high temperature cement slurry suspension stabilizer according to any one of claims 1 to 10, comprising the following steps: A 2-acrylamide-2-methylpropanesulfonic acid monomer, a vinyl polycyclic monomer, an unsaturated acrylamide monomer, an unsaturated cationic monomer and an unsaturated surfactant monomer containing a long carbon side chain in a mass ratio of (18-25): (5-13): (15-25): (1.7-2.5): (0.5-1.5) are polymerized in the presence of an initiator and a solvent to obtain a polymer solution, which is the ultra-high temperature cement slurry suspension stabilizer; Preferably, the ultrahigh temperature cement slurry suspension stabilizer is prepared by the following steps: In parts by mass, 18-25 parts of 2-acrylamide-2-methylpropanesulfonic acid monomer are dissolved in 20-30 parts of water, and the pH value is adjusted to 6-7 to obtain a first mixture; 0.5-1.5 parts of an unsaturated surfactant monomer containing a long carbon side chain are dissolved in 120-180 parts of water, and the pH value is selectively adjusted to 6-7 to obtain a second mixture; the first mixture and the second mixture are mixed, and then 15-25 parts of an unsaturated acrylamide monomer, 1.7-2.5 parts of an unsaturated cationic monomer, and 5-13 parts of a vinyl polycyclic monomer are added, and stirred evenly to obtain a third mixture; then an initiator is added to the third mixture, and after a polymerization reaction, a polymer solution is obtained, which is the ultra-high temperature cement slurry suspension stabilizer.
12. The preparation method according to claim 11, wherein The amount of the initiator used is 0.05-0.12% of the total mass of the third mixture.
13. The preparation method according to claim 11, wherein: The initiator includes one or a combination of ammonium persulfate, potassium persulfate and azobisisobutylimidazoline hydrochloride.
14. The preparation method according to claim 11, wherein: The initiator is added dropwise to the third mixture in the form of a solution; the concentration of the initiator in the initiator solution is 0.09-0.34%; and the dropping speed of the initiator solution is 10-20 mL / min.
15. The preparation method according to claim 11, wherein In the process of adding the initiator to the third mixture, the reaction temperature is controlled to be 50-65° C., and when the initiator is added, the reaction temperature is controlled to be 70-85° C. and the reaction is carried out for 4-6 hours.
16. Use of the ultra-high temperature cement slurry suspension stabilizer according to any one of claims 1 to 10 as an additive for cement slurry systems for cementing high temperature and high pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, ultra-deep wells, and extra-deep wells.
17. The use according to claim 16, wherein: Based on 100 parts by mass of cement in the cement slurry system, the added amount of the ultra-high temperature cement slurry suspension stabilizer is 3-5 parts.
Citation Information
Patent Citations
Thermal tackifying copolymer cement paste high-temperature stabilizer and preparation method thereof
CN111808231A
High-temperature-resistant polymerization suspension stabilizer cement paste for oil well cement and preparation method thereof
CN113736016A
High-temperature well cementation suspension stabilizer emulsion polymer as well as preparation method and application thereof
CN115975108A
Suspension stabilizer for high-temperature and high-density well cementation cement slurry as well as preparation method and application of suspension stabilizer
CN115975133A
High-temperature retarder suitable for oil and gas well cementation, preparation method thereof and cementing slurry
US20200239760A1
Cited By
High-temperature-resistant suspending stabilizer for water-based high-fluid-loss leak-stopping slurry, preparation method and application thereof