Liquid crystal polyester resin, liquid crystal polyester resin composition, and molded article formed thereof
The liquid crystal polyester resin composition addresses metal corrosion and warpage issues by optimizing structural units to reduce phenol gas generation, enhancing its suitability for high-temperature applications in electronic components.
Patent Information
- Application Number
- PCT/JP2024/015710
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-28
AI Technical Summary
Liquid crystal polyester resins used in electronic components face issues with metal corrosion due to phenol gas generation during processing and high-temperature exposure, leading to warpage and corrosion problems, especially in highly integrated and miniaturized devices.
A liquid crystal polyester resin composition with specific structural units, such as aromatic hydroxycarboxylic acids and diols, is developed to reduce phenol gas generation under reduced pressure, incorporating at least 15 to 75 mol% of structural unit (I) and 2 to 20 mol% of structural unit (II), which minimizes metal corrosion and warpage when used in high-temperature environments.
The composition effectively reduces phenol gas generation to 100 ppm or less, significantly minimizing metal corrosion and warpage in molded products, especially when used in high-temperature environments, making it suitable for small electronic parts and components in contact with metal.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Liquid crystal polyester resin, liquid crystal polyester resin composition and molded article made thereof
[0001] The present invention relates to a liquid crystal polyester resin, a liquid crystal polyester resin composition, and a molded article made thereof, more particularly to a liquid crystal polyester resin, a liquid crystal polyester resin composition, and a molded article obtained using the same.
[0002] Liquid crystal polyester resins are used in electrical and electronic components that require these properties due to their excellent heat resistance, fluidity, and dimensional stability. In recent years, the miniaturization of smartphones and other devices has led to increased demand for higher integration, thinner walls, and lower profile components. Therefore, materials for these components must have thin-wall fluidity and low warpage. However, reducing the viscosity of liquid crystal polyester resins to ensure thin-wall fluidity increases the amount of gases, particularly phenol gas, that are generated from the polymer during melt processing. Therefore, when liquid crystal polyester resins are used in contact with metal components such as terminals, exposure to high temperatures during reflow molding processes can release phenol gas, corroding the metal. Furthermore, the recent trend toward higher integration of components means that they are used for long periods of time in high-temperature environments, which can also release phenol gas even under these operating conditions, potentially causing increased corrosion.
[0003] Phenol gas is primarily generated by thermal denaturation of p-hydroxybenzoic acid, which is often the main component of liquid crystal polyester resins, and is generated in large amounts during polymer polymerization and melt processing. Studies to reduce the amount of generated gas have been proposed, including, for example, a liquid crystal polyester resin in which the acetylation rate of the aromatic diol used in polymer polymerization is controlled to be lower than usual, thereby reducing the amount of acetic acid, phenol, and carbon dioxide generated when the resin is maintained at a melting point +10°C for 30 minutes in a helium gas atmosphere (see, for example, Patent Document 1), and a liquid crystal polyester resin in which the amount of generated gas, such as phenol, is reduced by including structural units derived from 6-hydroxy-2-naphthoic acid, 4,4'-dihydroxybiphenyl, hydroquinone, and terephthalic acid, without using p-hydroxybenzoic acid (see, for example, Patent Document 2).
[0004] Furthermore, a liquid crystal polyester resin has been proposed (for example, Patent Document 3) that contains p-hydroxybenzoic acid as a main component and structural units derived from 6-hydroxy-2-naphthoic acid, 4,4′-dihydroxybiphenyl, hydroquinone, and terephthalic acid, thereby reducing blisters caused by generated gas and improving low warpage.
[0005] JP 2006-89714 A JP 2009-127025 A International Publication No. 2018 / 101214
[0006] The technology described in Patent Document 1 defines the amount of gas generated under an inert gas atmosphere, but in recent years, metal corrosivity in use in high-temperature environments has been highly correlated with the amount of gas generated under reduced pressure, which is a more severe condition. The method described in Patent Document 1 insufficiently reduces the amount of gas generated under reduced pressure, so while it is effective in reducing metal corrosivity to a certain extent, its metal corrosivity in use in high-temperature environments is still insufficient. Furthermore, the liquid crystal polyester resin described in Patent Document 1 also has issues with low warpage. The method described in Patent Document 2 reduces the amount of gas generated, but the reduction in the amount of gas generated under reduced pressure is insufficient, so its metal corrosivity in use in high-temperature environments is still insufficient. Furthermore, its low warpage also has issues. Furthermore, the method described in Patent Document 3 is ineffective in reducing metal corrosivity, and its low warpage is still insufficient.
[0007] An object of the present invention is to provide a liquid crystal polyester resin, a liquid crystal polyester resin composition, and a molded article made thereof that are less corrosive to metals when used in a high-temperature environment and have excellent low warpage properties.
[0008] As a result of extensive research to solve the above problems, the present inventors have found that a liquid crystal polyester resin containing at least 15 to 75 mol % of structural unit (I) and 2 to 20 mol % of structural unit (II) as aromatic hydroxycarboxylic acids, relative to 100 mol % of all structural units of the liquid crystal polyester resin, and which generates no more than a certain amount of phenol gas under heating and reduced pressure, has reduced metal corrosiveness when used in a high-temperature environment and excellent low warpage properties, thereby completing the present invention.
[0009] That is, the present invention is as follows: (1) A liquid crystal polyester resin containing, relative to 100 mol % of all structural units of the liquid crystal polyester resin, 20 to 80 mol % of the following structural units derived from an aromatic hydroxycarboxylic acid, 10 to 40 mol % of structural units derived from an aromatic diol, and 10 to 40 mol % of structural units derived from an aromatic dicarboxylic acid, wherein the aromatic hydroxycarboxylic acids contain at least 15 to 75 mol % of structural unit (I) and 2 to 20 mol % of structural unit (II), and the liquid crystal polyester resin generates 100 ppm or less of phenol gas when maintained at a temperature above the melting point by 20° C. for 60 minutes under a reduced pressure of 13.3 kPa or less.
[0010]
[0011] (2) The liquid crystal polyester resin according to (1), wherein the structural unit (I) is 80 to 97 mol % relative to 100 mol % of the total of the structural units (I) and (II). (3) The liquid crystal polyester resin according to (1) or (2), wherein the aromatic diol contains the structural unit (III) in an amount of 2 to 20 mol % relative to 100 mol % of all structural units of the liquid crystal polyester resin.
[0012]
[0013] (4) The aromatic diol contains structural units (III) and (IV), and the structural unit (III) accounts for 45 to 90 mol% relative to 100 mol% of the total of the structural units (III) and (IV). (1) Liquid crystal polyester resin according to any one of (1) to (3).
[0014]
[0015] (5) A method for producing a liquid crystal polyester resin according to any one of (1) to (4), comprising reacting a hydroxycarboxylic acid and / or a diol with acetic anhydride to acetylate at least a portion of the phenolic hydroxyl groups, followed by deacetylation polymerization with a dicarboxylic acid, wherein the deacetylation polymerization reaction is carried out for 40 to 120 minutes at a temperature of 230 to 245°C. (6) A liquid crystal polyester resin composition comprising 10 to 200 parts by weight of a filler relative to 100 parts by weight of the liquid crystal polyester resin according to any one of (1) to (4). (7) A molded article comprising the liquid crystal polyester resin according to any one of (1) to (4) or the liquid crystal polyester resin composition according to (6). (8) The molded article according to (7), wherein the molded article is any one selected from the group consisting of a connector, a relay, a switch, a coil bobbin, and an actuator part for a camera module. (9) A molded article comprising a liquid crystal polyester resin containing 20 to 80 mol % of structural units derived from an aromatic hydroxycarboxylic acid, 10 to 40 mol % of structural units derived from an aromatic diol, and 10 to 40 mol % of structural units derived from an aromatic dicarboxylic acid, wherein the aromatic hydroxycarboxylic acid contains at least 15 to 75 mol % of structural units (I) and 2 to 20 mol % of structural units (II), wherein the amount of phenol gas generated when the molded article is maintained at 280°C for 60 minutes under a reduced pressure of 13.3 kPa or less is 60 ppm or less.
[0016] The liquid crystal polyester resin of the present invention has reduced metal corrosion resistance when used in a high-temperature environment and has excellent low warpage. The liquid crystal polyester resin of the present invention is particularly suitable for use in molding small electrical and electronic components or in contact with metal components such as terminals.
[0017] 1 is a schematic diagram of a glass ampoule used for measuring the amount of phenol gas generated, and FIG. 2 is a schematic diagram of a glass ampoule sealed under reduced pressure, and FIG. 3 is a perspective view of a molded connector product produced in Examples and a conceptual diagram showing the measurement site of the amount of warpage.
[0018] The present invention will be described in detail below.
[0019] Liquid crystal polyester resin is a polyester that forms an anisotropic molten phase. Examples of such polyester resins include polyesters composed of structural units selected from the below-described oxycarbonyl unit, dioxy unit, dicarbonyl unit, etc. so as to form an anisotropic molten phase.
[0020] The liquid crystal polyester resin of the present invention is a liquid crystal polyester resin containing at least 15 to 75 mol% of the structural unit (I) and 2 to 20 mol% of the structural unit (II) as aromatic hydroxycarboxylic acids described below, and when maintained at a temperature of melting point + 20°C for 60 minutes under a reduced pressure of 13.3 kPa (100 torr) or less, the amount of phenol gas generated is 100 ppm or less. This means that the amount of phenol gas generated during melt processing is small. Hereinafter, the amount of phenol gas generated from the liquid crystal polyester resin when maintained at a temperature of melting point Tm + 20°C for 60 minutes under a reduced pressure of 13.3 kPa or less may be simply referred to as the "amount of phenol gas generated."
[0021] When the structural unit (I) and the structural unit (II) are used in combination as structural units of the liquid crystal polyester resin, the crystallinity of the liquid crystal polyester resin can be controlled and high strength can be achieved, but the monomer constituting the structural unit (I) is likely to remain unreacted, and phenol gas is likely to be generated by thermal denaturation. By setting the structural unit constituting the liquid crystal polyester resin within the preferred range described below, or by setting the manufacturing method for the liquid crystal polyester resin to the preferred embodiment described below, the monomer constituting the structural unit (I) is sufficiently incorporated into the polymer chain, thereby suppressing thermal denaturation and reducing the amount of phenol gas generated. Such a liquid crystal polyester resin that uses the structural unit (I) and the structural unit (II) in combination and generates a low amount of phenol gas can reduce metal corrosivity when used in a high-temperature environment. Furthermore, since the amount of phenol gas generated during melt processing is low, the amount of phenol gas remaining in the molded product is reduced, and the amount of phenol gas released when the molded product is further processed at high temperatures is reduced, thereby reducing metal corrosivity during high-temperature processing of the molded product. In addition to having high strength, the liquid crystal polyester resin of the present invention is less likely to produce minute unfilled portions in the molded product due to the generated gas even when molded under molding conditions that tend to leave residual gas, such as a low injection speed, and therefore has excellent low warpage properties, thereby reducing deformation after heating. Details of the structural units constituting the liquid crystal polyester resin and the manufacturing method thereof will be described in the following structural units constituting the liquid crystal polyester resin and the "Method for manufacturing liquid crystal polyester resin" below.
[0022] If the amount of phenol gas generated is more than 100 ppm, the metal corrosiveness deteriorates when used in a high-temperature environment, and the molded product warps more, which is undesirable. Furthermore, when a molded product is produced, the amount of phenol gas generated increases when the product is kept at 280°C, which deteriorates the metal corrosiveness, which is undesirable. The amount of phenol gas generated is preferably 90 ppm or less, more preferably 80 ppm or less, even more preferably 70 ppm or less, and particularly preferably 60 ppm or less. The lower limit is 0 ppm.
[0023] The melting point is the endothermic peak temperature (Tm 1 ) after the observation of Tm1 This refers to the endothermic peak temperature (Tm) observed when the sample is held at +20°C for 5 minutes, cooled to room temperature at a temperature decreasing rate of 20°C / min, and then heated again at a temperature increasing rate of 20°C / min.
[0024] The method for calculating the amount of phenol gas generated is as follows. First, 5 g of liquid crystal polyester resin pellets are dried at 150°C for 3 hours using a hot air dryer, and then placed in the heated portion (A) of a glass ampoule tube having the shape shown in Figure 1. Using a vacuum pump (ULVAC DTC-22), a vacuum is drawn from the tip of the glass ampoule tube, controlling the pressure in the system to 13.3 kPa (100 torr) or less. Then, the portion (B) 70 mm from the tip is heated and melted with a gas burner to seal the tube, producing an analytical ampoule as shown in Figure 2. Next, the heated portion (A) of the analytical ampoule is maintained at a temperature of 20°C above the melting point of the liquid crystal polyester resin for 60 minutes using a ceramics electric tubular furnace (Asahi Rika Seisakusho ARF-30K (temperature controller AMF-N type)). Gas components generated from the liquid crystal polyester resin pellets by heating are collected in the portion (C). The ampoule was removed from the ceramic electric tubular furnace and cooled to room temperature, after which the (C) portion was cut out from the ampoule with a file. The cut-out (C) portion was weighed, and all of the gas components condensed in the (C) portion were dissolved in deuterated dimethyl sulfoxide (0.8 g). A small amount of 1,4-dioxane was added as an internal standard, and the resulting solution was analyzed using a JNM-ECZ500R (manufactured by JEOL Ltd.). 1 H-NMR measurement is performed. In addition, the (C) portion from which the trapped components have been removed is washed with acetone, dried in a glass dryer at 60°C for 1 hour, and then weighed again, and the total amount of evolved gas is calculated from the difference in weight of the (C) portion before and after removal of the trapped components. 1 The ratio of the integral values of the peak derived from phenol to the peak derived from the internal standard (1,4-dioxane) is determined from the H-NMR spectrum. The amount of phenol gas (ppm) generated from the liquid crystal polyester resin is calculated from this ratio and the total amount of generated gas.
[0025] Here, the degree of vacuum inside the ampoule glass tube is not particularly limited as long as it is 13.3 kPa (100 torr) or less, and may be, for example, a high vacuum state of 133 Pa (1 torr) or less. By creating a vacuum state inside the ampoule glass tube, phenol gas is easily generated from the liquid crystal polyester resin, and the phenol gas can be efficiently collected.
[0026] Next, the structural units constituting the liquid crystal polyester resin will be described.
[0027] The liquid crystal polyester resin of the present invention contains 20 to 80 mol% of structural units derived from aromatic hydroxycarboxylic acid as oxycarbonyl units, relative to 100 mol% of all structural units in the liquid crystal polyester resin. If the content of these structural units is less than 20 mol%, liquid crystallinity is impaired, resulting in poor warpage. The content of these structural units is preferably 25 mol% or more, more preferably 30 mol% or more. On the other hand, if the content of these structural units is greater than 80 mol%, it becomes difficult to control the phenol gas concentration to 100 ppm or less, resulting in poor metal corrosiveness and poor warpage when used in a high-temperature environment. The content of these structural units is preferably 75 mol% or less, more preferably 70 mol% or less.
[0028] The liquid crystal polyester resin of the present invention contains 15 to 75 mol% of structural unit (I) as a structural unit derived from an aromatic hydroxycarboxylic acid. If the content of this structural unit is less than 15 mol%, liquid crystallinity is impaired, resulting in poor warpage. From the viewpoint of reducing metal corrosivity and achieving excellent low warpage in high-temperature environments, the content of this structural unit is preferably 25 mol% or more, and even more preferably 35 mol% or more. On the other hand, if the content of this structural unit is more than 75 mol%, it becomes difficult to control the phenol gas concentration to 100 ppm or less, resulting in poor metal corrosivity and warpage in high-temperature environments. From the viewpoint of reducing metal corrosivity and achieving excellent low warpage in high-temperature environments, the content of this structural unit is preferably 65 mol% or less, and more preferably 55 mol% or less.
[0029]
[0030] The liquid crystal polyester resin of the present invention contains 2 to 20 mol% of structural unit (II) as a structural unit derived from an aromatic hydroxycarboxylic acid. The structural unit (II) is a structural unit derived from 6-hydroxy-2-naphthoic acid. If the content of this structural unit is less than 2 mol%, it becomes difficult to control the crystallinity of the liquid crystal polyester resin, resulting in poor warpage. Furthermore, when using a production method in which the deacetic acid polymerization reaction at a temperature of 230 to 245°C (described below) is controlled to control the amount of phenol gas generated within a suitable range, the reaction of structural unit (I) is promoted, resulting in the formation of a highly crystalline structure, which affects the reactions of other structural units. Therefore, even if the amount of phenol gas generated is controlled to 100 ppm, warpage and metal corrosivity during use in a high-temperature environment are also poor. From the viewpoint of reducing metal corrosivity during use in a high-temperature environment and achieving excellent low warpage, the content of this structural unit is preferably 2.5 mol% or more, more preferably 3 mol% or more. On the other hand, if the content of the structural unit is more than 20 mol%, it becomes difficult to control the amount of phenol gas generated to 100 ppm or less, and metal corrosiveness and warpage in use in a high-temperature environment deteriorate. From the viewpoint of reducing metal corrosiveness in use in a high-temperature environment and achieving excellent low warpage, the content of the structural unit is preferably 15 mol% or less, and more preferably 10 mol% or less.
[0031]
[0032] In the liquid crystal polyester resin of the present invention, when the amount of phenol gas generated is controlled to 100 ppm or less, it can reduce the metal corrosiveness in use under high temperature environment, and from the viewpoint of excellent low warpage, the content of structural unit (I) is preferably 80 mol% or more, more preferably 85 mol% or more, and even more preferably 90 mol% or more, based on the total 100 mol% of structural unit (I) and structural unit (II).On the other hand, when the amount of phenol gas generated is controlled to 100 ppm or less, it can reduce the metal corrosiveness in use under high temperature environment, and from the viewpoint of excellent low warpage, the content of structural unit (I) is preferably 97 mol% or less, more preferably 96 mol% or less, and even more preferably 95 mol% or less.
[0033] The liquid crystal polyester resin of the present invention may contain, as an oxycarbonyl unit, a structural unit other than the structural units (I) and (II). Specific examples of other oxycarbonyl units include structural units derived from m-hydroxybenzoic acid, etc.
[0034] The liquid crystal polyester resin of the present invention contains, as dioxy units, 10 to 40 mol% of structural units derived from aromatic diols, relative to 100 mol% of all structural units in the liquid crystal polyester resin. If the content of these structural units is less than 10 mol%, it becomes difficult to control the amount of phenol gas generated to 100 ppm or less, and metal corrosiveness and warpage deteriorate when used in high-temperature environments. The content of these structural units is preferably 15 mol% or more, more preferably 20 mol% or more. On the other hand, if the content of these structural units is more than 40 mol%, liquid crystallinity is impaired, resulting in worsening warpage. The content of these structural units is preferably 35 mol% or less, more preferably 30 mol% or less. Examples of structural units derived from aromatic diols include structural units derived from 4,4'-dihydroxybiphenyl, hydroquinone, resorcinol, t-butylhydroquinone, phenylhydroquinone, chlorohydroquinone, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 3,4'-dihydroxybiphenyl, 2,2-bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfide, and 4,4'-dihydroxybenzophenone.
[0035] The liquid crystal polyester resin of the present invention is easy to control the amount of phenol gas generated to 100 ppm or less, can reduce metal corrosiveness in use under high temperature environments, and has excellent low warpage properties. In view of this, the liquid crystal polyester resin preferably contains 2 mol% or more of structural unit (III) as a structural unit derived from aromatic diol, based on 100 mol% of all structural units of the liquid crystal polyester resin, preferably contains 5 mol% or more, and more preferably contains 8 mol% or more. The structural unit (III) is a structural unit derived from hydroquinone. On the other hand, the amount of phenol gas generated is easy to control to 100 ppm or less, can reduce metal corrosiveness in use under high temperature environments, and has excellent low warpage properties. In view of this, the liquid crystal polyester resin preferably contains 20 mol% or less of structural unit (III), more preferably contains 18 mol% or less, and even more preferably contains 16 mol% or less.
[0036]
[0037] The liquid crystal polyester resin of the present invention is capable of easily controlling the amount of phenol gas generated to 100 ppm or less, reducing metal corrosiveness in use in high-temperature environments, and exhibiting excellent low warpage. From this viewpoint, the liquid crystal polyester resin preferably contains 2 mol% or more, more preferably 4 mol% or more, and even more preferably 6 mol% or more of structural units (IV) derived from aromatic diols, relative to 100 mol% of all structural units in the liquid crystal polyester resin. The structural unit (IV) is a structural unit derived from 4,4'-dihydroxybiphenyl. On the other hand, from the viewpoint of easily controlling the amount of phenol gas generated to 100 ppm or less, reducing metal corrosiveness in use in high-temperature environments, and exhibiting excellent low warpage, the liquid crystal polyester resin preferably contains 20 mol% or less, more preferably 17 mol% or less, and even more preferably 14 mol% or less of structural units (III).
[0038]
[0039] In the liquid crystal polyester resin of the present invention, the amount of phenol gas generated can be easily controlled to 100 ppm or less, and can reduce metal corrosiveness in use under high temperature environment, and from the viewpoint of excellent low warpage, the content of structural unit (III) is preferably 45 mol% or more, more preferably 47 mol% or more, and even more preferably 50 mol% or more, based on the total 100 mol% of structural unit (III) and structural unit (IV).On the other hand, the amount of phenol gas generated can be easily controlled to 100 ppm or less, and can reduce metal corrosiveness in use under high temperature environment, and from the viewpoint of excellent low warpage, the content of structural unit (III) is preferably 90 mol% or less, more preferably 80 mol% or less, and even more preferably 70 mol% or less.
[0040] The liquid crystal polyester resin of the present invention may contain, as a dioxy unit, a structural unit other than the structural units (III) and (IV). As other dioxy units, structural units derived from aliphatic diols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, and neopentyl glycol; and structural units derived from alicyclic diols such as 1,4-cyclohexanediol and 1,4-cyclohexanedimethanol can be used within a range that does not impair the effects of the present invention.
[0041] The liquid crystal polyester resin of the present invention contains, as dicarbonyl units, 10 to 40 mol% of structural units derived from aromatic dicarboxylic acids, relative to 100 mol% of all structural units in the liquid crystal polyester resin. If the content of these structural units is less than 10 mol%, it becomes difficult to control the amount of phenol gas generated to 100 ppm or less, and metal corrosivity and warpage deteriorate when used in high-temperature environments. The content of these structural units is preferably 15 mol% or more, more preferably 20 mol% or more. On the other hand, if the content of these structural units is more than 40 mol%, liquid crystallinity is impaired, resulting in worsening warpage. The content of these structural units is preferably 35 mol% or less, more preferably 30 mol% or less. Examples of structural units derived from aromatic dicarboxylic acids include structural units derived from terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, 1,2-bis(2-chlorophenoxy)ethane-4,4'-dicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid.
[0042] The liquid crystal polyester resin of the present invention is easy to control the amount of phenol gas generated to 100 ppm or less, can reduce metal corrosiveness in use in a high-temperature environment, and has excellent low warpage properties. From this viewpoint, it is preferable that the liquid crystal polyester resin contains 5 mol% or more of the structural unit (V) as a structural unit derived from an aromatic dicarboxylic acid, relative to 100 mol% of all structural units of the liquid crystal polyester resin, preferably 10 mol% or more, and more preferably 15 mol% or more. The structural unit (V) is a structural unit derived from terephthalic acid. On the other hand, it is easy to control the amount of phenol gas generated to 100 ppm or less, can reduce metal corrosiveness in use in a high-temperature environment, and has excellent low warpage properties. From this viewpoint, it is preferable that the structural unit (V) contains 35 mol% or less, more preferably 30 mol% or less, and even more preferably 25 mol% or less.
[0043]
[0044] The liquid crystal polyester resin of the present invention is easy to control the amount of phenol gas generated to 100 ppm or less, can reduce metal corrosiveness in use under high temperature environments, and has excellent low warpage properties. In view of this, it is preferable that the structural unit (VI) is contained in an amount of 0.01 mol% or more, preferably 0.05 mol% or more, and more preferably 0.1 mol% or more, as a structural unit derived from an aromatic diol, relative to 100 mol% of all structural units of the liquid crystal polyester resin. The structural unit (VI) is a structural unit derived from isophthalic acid. On the other hand, it is easy to control the amount of phenol gas generated to 100 ppm or less, can reduce metal corrosiveness in use under high temperature environments, and has excellent low warpage properties. In view of this, it is preferable that the structural unit (VI) is contained in an amount of 5 mol% or less, more preferably 4 mol% or less, and even more preferably 3 mol% or less.
[0045]
[0046] The liquid crystal polyester resin of the present invention may contain, as a dicarbonyl unit, a structural unit other than the structural units (V) and (VI). As other dicarbonyl units, structural units derived from aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, and hexahydroterephthalic acid; and structural units derived from alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 1,3-cyclohexanedicarboxylic acid can be used within a range that does not impair the effects of the present invention.
[0047] In addition to the structural units (I) to (VI), the liquid crystal polyester resin may contain structural units derived from p-aminobenzoic acid, p-aminophenol, etc., within the range that does not impair the effects of the present invention.
[0048] The liquid crystal polyester resin of the present invention contains the structural units (III) to (VI) in the above-mentioned ranges, so that the structural unit (I) is sufficiently incorporated into the polymer chain, and thermal denaturation can be suppressed, making it easier to control the amount of phenol gas generated to 100 ppm or less.
[0049] In addition, from the viewpoint of not impairing the effects of the present invention, the total amount of the structural units (I) to (VI) is preferably 99 mol% or more, more preferably 99.5 mol% or more, and even more preferably 100 mol%, relative to 100 mol% of all structural units of the liquid crystal polyester resin.
[0050] In addition, the ratio of the total amount of the structural units (III) and (IV) to the total amount of the structural units (V) and (VI) (([III] + [IV]) / ([V] + [VI])) is preferably 0.9 or more and 1.1 or less from the viewpoint of controlling polymerization property.
[0051] The monomers used as raw materials for forming the structural units are not particularly limited as long as they have a structure capable of forming the structural units. In addition, derivatives of such monomers, such as acylated hydroxyl groups, esterified carboxyl groups, acid halides, and acid anhydrides, may also be used.
[0052] The method for calculating the content of each structural unit in a liquid crystal polyester resin is as follows. First, the liquid crystal polyester resin is pulverized, and then tetramethylammonium hydroxide is added. Then, the content of each structural unit can be determined by performing pyrolysis GC / MS measurement using a Shimadzu GCMS-QP5050A. The content of structural units that are not detected or are below the detection limit is calculated as 0 mol %.
[0053] From the viewpoint of heat resistance, the melting point (Tm) of the liquid crystal polyester resin is preferably 280° C. or higher, more preferably 300° C. or higher, and even more preferably 320° C. or higher. On the other hand, from the viewpoint of processability and reducing the amount of phenol gas generated and thereby reducing metal corrosiveness in use in a high-temperature environment, the melting point (Tm) of the liquid crystal polyester resin is preferably 370° C. or lower, more preferably 360° C. or lower, and even more preferably 350° C. or lower.
[0054] The melt viscosity of the liquid crystal polyester resin is preferably 1 Pa s or more, more preferably 3 Pa s or more, and even more preferably 5 Pa s or more from the viewpoint of heat resistance, and from the viewpoint of reducing the amount of phenol gas generated, thereby reducing metal corrosiveness in use under high-temperature environments, and achieving excellent low warpage. On the other hand, from the viewpoint of fluidity, the melt viscosity of the liquid crystal polyester resin is preferably 50 Pa s or less, preferably 20 Pa s or less, more preferably 15 Pa s or less, and particularly preferably 10 Pa s or less.
[0055] The melt viscosity is a value measured by a Koka type flow tester at a temperature of the melting point (Tm) of the liquid crystal polyester resin + 20° C. under the condition of a shear rate of 1000 / sec.
[0056] <Method for producing liquid crystal polyester resin> The method for producing the liquid crystal polyester resin of the present invention includes a method of copolymerizing monomers that provide the structural units (I) to (VI) in a content within the above-mentioned range, or a method of blending two or more liquid crystal polyester resins obtained by copolymerizing the structural units (I) to (VI) in a content outside the above-mentioned range, so that the structural units (I) to (VI) fall within the above-mentioned range. From the viewpoint of not inheriting the properties of the liquid crystal polyester resin before blending, the method of copolymerizing monomers that provide the structural units (I) to (VI) in a content within the above-mentioned range is preferred.
[0057] The method for producing the liquid crystal polyester resin of the present invention is not particularly limited, and can be produced in accordance with known polyester polycondensation methods. From the viewpoint of reducing the amount of phenol gas generated, thereby reducing metal corrosiveness in use in high-temperature environments and achieving excellent low warpage, a preferred method for producing a liquid crystal polyester resin is to react p-hydroxybenzoic acid-derived structural units, 6-hydroxy-2-naphthoic acid-derived structural units, 4,4'-dihydroxybiphenyl-derived structural units, hydroquinone-derived structural units, and terephthalic acid-derived structural units with acetic anhydride to acetylate at least a portion of the phenolic hydroxyl groups, followed by deacetylation polymerization.
[0058] Furthermore, in the above-described production method, the amount of phenol gas generated can be controlled within a suitable range by satisfying the following requirements. It is preferable to satisfy the following requirement 1, and it is more preferable to satisfy requirements 1 and 2. 1. The deacetic acid polymerization reaction is carried out at a temperature of 230 to 245°C for 40 to 120 minutes. 2. When increasing the degree of polymerization of the liquid crystal polyester resin, the reaction is carried out under reduced pressure, and the reaction is completed at a reduced pressure of 4.0 kPa (30 torr) or less.
[0059] Regarding requirement 1 above, a temperature of 230 to 245°C is a temperature range in which the deacetylation polymerization of p-hydroxybenzoic acid, which constitutes structural unit (I), and 6-hydroxy-2-naphthoic acid, which constitutes structural unit (II), is promoted. By carrying out the deacetylation polymerization reaction sufficiently within this temperature range, p-hydroxybenzoic acid is sufficiently incorporated into the polymer chain before it sublimes and becomes unreactive, thereby preventing unreacted p-hydroxybenzoic acid from being thermally denatured and generating phenol gas. Furthermore, using p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid in combination promotes only the reaction of p-hydroxybenzoic acid, thereby preventing the formation of a highly crystalline structure. The deacetylation polymerization reaction time at a temperature of 230 to 245°C is preferably 50 minutes or more, more preferably 60 minutes or more. On the other hand, 110 minutes or less is more preferable, and 100 minutes or less is even more preferable.
[0060] Regarding requirement 2 above, if unreacted p-hydroxybenzoic acid remains, generation of phenol gas can be suppressed by removing it from the polymer system by reducing the pressure during the polymerization reaction. The degree of reduced pressure is preferably 2.7 kPa (20 torr) or less, more preferably 1.3 kPa (10 torr) or less.
[0061] <Filler> The liquid crystal polyester resin of the present invention may be a liquid crystal polyester resin composition containing a filler to impart mechanical strength and other properties to the liquid crystal polyester resin. The filler used in the present invention is not particularly limited, and examples thereof include fibrous, whisker-like, plate-like, powdery, and granular fillers. Specific examples of fibrous or whisker-like fillers include glass fibers, PAN-based and pitch-based carbon fibers, metal fibers such as stainless steel fibers, aluminum fibers, and brass fibers, organic fibers such as aromatic polyamide fibers and liquid crystal polyester fibers, gypsum fibers, ceramic fibers, asbestos fibers, zirconia fibers, alumina fibers, silica fibers, titanium oxide fibers, silicon carbide fibers, rock wool, potassium titanate whiskers, barium titanate whiskers, aluminum borate whiskers, silicon nitride whiskers, and acicular titanium oxide. Examples of plate-like fillers include mica, talc, kaolin, glass flakes, clay, molybdenum disulfide, and wollastonite. Examples of powdery or granular fillers include silica, glass beads, titanium oxide, zinc oxide, calcium polyphosphate, and graphite. The surfaces of the fillers used in the present invention may be treated with a known coupling agent (e.g., a silane-based coupling agent, a titanate-based coupling agent, etc.) or other surface treatment agents. Two or more of the fillers used in the present invention may be used in combination.
[0062] Among the above fillers, glass fiber is preferred because of its excellent mechanical strength, particularly tensile strength and bending strength, heat resistance, and dimensional stability. The type of glass fiber is not particularly limited as long as it is one generally used to reinforce resins, and examples include long fiber type and short fiber type chopped strands and milled fiber. Furthermore, plate-like fillers are preferred because of their excellent thin-wall flowability and low warpage, and mica is particularly preferred.
[0063] The surface of the filler may be treated with a known coupling agent (e.g., a silane coupling agent, a titanate coupling agent, etc.) or other surface treatment agent. The glass fibers may be coated or bundled with a thermoplastic resin such as an ethylene / vinyl acetate copolymer or a thermosetting resin such as an epoxy resin.
[0064] The liquid crystal polyester resin composition of the present invention may further contain conventional additives selected from antioxidants, heat stabilizers (e.g., hindered phenols, hydroquinone, phosphites, thioethers, and their substitution products), ultraviolet absorbers (e.g., resorcinol, salicylate), color inhibitors such as phosphites and hypophosphites, lubricants and mold release agents (montanic acid and its metal salts, its esters, its half esters, stearyl alcohol, stearamide, polyethylene wax, etc.), colorants including dyes or pigments, conductive agents or colorants such as carbon black, crystal nucleating agents, plasticizers, flame retardants (bromine-based flame retardants, phosphorus-based flame retardants, red phosphorus, silicone-based flame retardants, etc.), flame retardant assistants, and antistatic agents, within the range that does not impair the effects of the present invention.
[0065] In the liquid crystal polyester resin composition of the present invention, the content of the filler is preferably 10 to 200 parts by weight per 100 parts by weight of the liquid crystal polyester resin. If the content of the filler is 10 parts by weight or more, the mechanical strength of the molded article can be improved. The content of the filler is more preferably 15 parts by weight or more, and even more preferably 20 parts by weight or more. On the other hand, if the content of the filler is 200 parts by weight or less, a liquid crystal polyester resin composition having excellent moldability and thin-wall flowability and capable of easily injection-molding small, thin-walled molded articles can be obtained, which is preferable. The content of the filler is more preferably 150 parts by weight or less, and even more preferably 100 parts by weight or less.
[0066] Examples of methods for blending the filler and additives include a dry blending method in which a filler and other solid additives are blended with a liquid crystal polyester resin, a solution blending method in which a filler and other liquid additives are blended with a liquid crystal polyester resin, a method in which the filler and other additives are added during polymerization of the liquid crystal polyester resin, and a method in which the liquid crystal polyester resin and the filler and other additives are melt-kneaded. Among these, the melt-kneading method is preferred.
[0067] Known methods can be used for melt-kneading. Examples include a Banbury mixer, a rubber roll mill, a kneader, and a single-screw or twin-screw extruder. Twin-screw extruders are preferred. The melt-kneading temperature is preferably equal to or higher than the melting point of the liquid crystal polyester resin and equal to or lower than the melting point + 50°C.
[0068] Examples of the kneading method include: 1) a method in which the liquid crystal polyester resin, filler, and other additives are added all at once from a base-loading feeder and kneaded (lump-loading kneading method); 2) a method in which the liquid crystal polyester resin and other additives are added from a base-loading feeder and kneaded, and then the filler and other additives are added from a side feeder and kneaded (side feed method); and 3) a method in which a liquid crystal polyester composition (master pellets) containing a high concentration of the liquid crystal polyester resin and other additives is prepared, and then the master pellets are kneaded with the liquid crystal polyester resin and filler to a specified concentration (master pellet method).
[0069] <Molded Articles> The liquid crystal polyester resin and liquid crystal polyester resin composition of the present invention can be processed into molded articles having excellent surface appearance (color tone), mechanical properties, and heat resistance by conventional molding methods such as injection molding, extrusion molding, press molding, solution casting, and spinning. Examples of molded articles include injection molded articles, extrusion molded articles, press molded articles, sheets, pipes, various films such as unstretched films, uniaxially stretched films, and biaxially stretched films, and various fibers such as unstretched yarns and ultrastretched yarns. In particular, injection molded articles are preferred from the viewpoint of processability. When melt molding, it is preferable to melt mold at 370 ° C or less, more preferably 360 ° C or less, in order to suppress deterioration of the liquid crystal polyester resin and liquid crystal polyester resin composition, suppress the generation of phenol gas when a molded article described below is maintained at 280 ° C, suppress metal corrosiveness, and improve mechanical strength.
[0070] The molded article of the present invention comprises a liquid crystal polyester resin containing 20 to 80 mol% of structural units derived from an aromatic hydroxycarboxylic acid, 10 to 40 mol% of structural units derived from an aromatic diol, and 10 to 40 mol% of structural units derived from an aromatic dicarboxylic acid, wherein the aromatic hydroxycarboxylic acid comprises at least 15 to 75 mol% of structural units (I) and 2 to 20 mol% of structural units (II), and the amount of phenol gas generated when maintained at 280°C for 60 minutes under a reduced pressure of 13.3 kPa or less is 60 ppm or less. 280°C is a temperature close to the temperature at which molded articles are subjected to secondary processing such as reflow treatment, and this temperature reduces the release of phenol gas during secondary processing of the molded article, demonstrating excellent processability.
[0071] By using a liquid crystal polyester resin with a phenol gas generation amount of 100 ppm or less, as described above in the liquid crystal polyester resin section, the amount of phenol gas generated during melt processing such as melt kneading or injection molding is reduced, and the amount of phenol gas remaining in the molded product is reduced, making it possible to reduce the amount of phenol gas generated when maintained at 280° C. to 60 ppm or less. Such molded products can reduce metal corrosiveness when processed at high temperatures.
[0072] On the other hand, when a liquid crystal polyester resin that generates more than 100 ppm of phenol gas is used, the amount of phenol gas generated during melt processing increases, and the amount of phenol gas remaining in the molded product also increases, so that the amount of phenol gas generated when maintained at 280° C. exceeds 60 ppm. Such molded products have poor metal corrosiveness when processed at high temperatures.
[0073] The amount of phenol gas generated when the molded article is maintained at 280° C. is preferably 50 ppm or less, more preferably 40 ppm or less, from the viewpoint of reducing metal corrosiveness when used in a high-temperature environment.
[0074] The amount of phenol gas generated from the molded article is measured in the same manner as described in the liquid crystal polyester resin section, except that the temperature of the ceramic electric tubular furnace is set to 280° C. In the case of a liquid crystal polyester resin composition containing a filler, the amount of gas generated is calculated by converting it into the amount of gas generated from the liquid crystal polyester resin excluding the filler.
[0075] Molded articles obtained by molding the liquid crystal polyester resin and liquid crystal polyester resin composition of the present invention can be preferably used as electrical and electronic parts. Examples of electrical and electronic parts include flexible printed circuit boards, laminate circuit boards, printed wiring boards, and three-dimensional circuit boards used in antennas for mobile communication and electronic devices such as personal computers, GPS-equipped devices, mobile phones, and millimeter-wave and quasi-millimeter-wave radars such as collision prevention radars, tablets, and smartphones; lamp reflectors and lamp sockets for LEDs, small cells and microcell components for communication base stations of mobile communication terminals, antenna covers, housings, sensors, actuator parts for camera modules, connectors, relay cases and bases, switches, coil bobbins, and capacitors. In particular, from the viewpoint of reduced metal corrosion in high-temperature environments and excellent low warpage, they are useful for connectors, relays, switches, coil bobbins, and actuator parts for camera modules that are used in contact with metal parts and have thin-walled complex shapes.
[0076] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. In the examples, the composition and properties of the liquid crystal polyester resin were measured by the following methods.
[0077] (1) Composition Analysis of Liquid Crystalline Polyester Resin 2 μL of a 25% methanol solution of tetramethylammonium hydroxide was added to 0.1 mg of crushed liquid crystal polyester resin pellets, and pyrolysis GC / MS measurement was performed using a Shimadzu GCMS-QP5050A to determine the content ratio of each structural unit in the liquid crystal polyester resin.
[0078] (2) Measurement of the melting point (Tm) of the liquid crystal polyester resin The endothermic peak temperature (Tm) observed when the liquid crystal polyester resin is heated from room temperature at a temperature increase rate of 20°C / min using a differential scanning calorimeter DSC-7 (manufactured by PerkinElmer) was measured. 1 ) after the observation of Tm 1 After holding at +20°C for 5 minutes, the sample was cooled to room temperature at a temperature decreasing rate of 20°C / min, and then heated again at a temperature increasing rate of 20°C / min. The endothermic peak temperature observed when the sample was heated was taken as the melting point (Tm).
[0079] (3) Melt Viscosity of Liquid Crystalline Polyester Resin Using a high-speed flow tester CFT-500D (orifice 0.5φ×10 mm) (manufactured by Shimadzu Corporation), the melt viscosity of the liquid crystal polyester resin was measured at Tm+20° C. and a shear rate of 1000 / s.
[0080] (4) Amount of Phenol Gas Generated Five grams of liquid crystal polyester resin pellets were dried at 150°C for 3 hours using a hot air dryer and then placed in the heated portion (A) of a glass ampoule tube with the shape shown in Figure 1. Using a vacuum pump (ULVAC DTC-22), a vacuum was applied from the tip of the glass ampoule tube, maintaining the system at a reduced pressure of 133 Pa (1 torr). The portion (B) 70 mm from the tip was heated and melted with a gas burner, sealing the tube, and preparing an analytical ampoule as shown in Figure 2. Next, the heated portion (A) of the analytical ampoule was held at a temperature of 20°C above the melting point of the liquid crystal polyester resin for 60 minutes using a ceramic electric tubular furnace (Asahi Rika Seisakusho ARF-30K (temperature controller AMF-N type)), and the generated gas was collected in the portion (C). The ampoule was removed from the ceramic electric tubular furnace and cooled to room temperature. The portion (C) was then cut out of the ampoule with a file. After weighing the cut-out (C) portion, all of the gas components aggregated in the (C) portion were dissolved in deuterated dimethyl sulfoxide (0.8 g), and a small amount of 1,4-dioxane was added as an internal standard. The resulting solution was analyzed using a JNM-ECZ500R manufactured by JEOL Ltd. 1 H-NMR measurement was performed. In addition, the (C) portion from which the trapped components had been removed was washed with acetone, dried in a glass dryer at 60°C for 1 hour, and then reweighed. The total amount of evolved gas was calculated from the difference in weight of the (C) portion before and after removal of the trapped components. 1 The integrated value ratio of the peak derived from phenol and the peak derived from the internal standard (1,4-dioxane) was determined from the H-NMR spectrum. From this and the total amount of the generated gas, the amount of phenol gas (ppm) generated from the liquid crystal polyester resin was calculated.
[0081] (5) Metal Corrosion Resistance 30 g of liquid crystal polyester resin pellets were dried at 150 ° C for 3 hours using a hot air dryer, then placed in an aluminum cup, and a 20 mm × 10 mm × 1 mm thick copper plate was placed on the pellets and covered with a glass petri dish. Next, using a hot air dryer, heat treatment was performed at 150 ° C for 200 hours or at 200 ° C for 6 hours, and the presence or absence of metallic luster on the copper plate and discoloration to dark brown or blackish brown were visually confirmed, and the metal corrosion resistance was determined to be excellent in the following order: A, B, C, D. The better the metal corrosion resistance after 6 hours of heat treatment at 200 ° C, the more metal corrosion resistance can be reduced when used in a high-temperature environment.
[0082] A: Metallic luster, no discoloration B: No metallic luster, no discoloration C: No metallic luster, dark brown, no black-brown D: No metallic luster, dark brown, black-brown (6) Warpage The liquid crystal polyester resin was dried at 150 ° C for 3 hours using a hot air dryer, and then subjected to a Fanuc α30C injection molding machine (manufactured by Fanuc) to obtain a connector molded product with a terminal pitch 6 of 0.4 mm, a minimum thickness 7 (partition wall) of 0.2 mm, and external dimensions of 3 mm wide x 2 mm high x 30 mm long, as shown in Figure 3a. The cylinder temperature was set to the melting point of the liquid crystal polyester resin + 10 ° C, the mold temperature was set to 90 ° C, the injection pressure was set to the minimum filling pressure, and the injection speed was set to 50 or 100 mm / s. The liquid crystal polyester resin was filled through a pin gate G1 (gate diameter 0.3 mm) installed on one short side 2 of the connector molded product shown in Figure 3a. The resulting molded connector was left in an oven heated to 260°C for 3 minutes, and the amount of warpage of the molded connector after heat treatment was measured. Figure 3b is a conceptual diagram showing the measurement points for the amount of warpage in the molded connector. The plane A-B, which connects both ends of the long surface 1 of the molded connector with a straight line, was used as reference plane a, and the distance between the reference plane a and the maximum deformation plane b was measured and recorded as the amount of warpage 8. The smaller the amount of warpage, the better the low warpage.
[0083] (7) Amount of phenol gas in molded product Five grams of the connector molded product molded in (6) was weighed, and the amount of phenol gas (ppm) generated from the molded product was calculated in the same manner as in (4), except that the heat treatment temperature in the ceramic electric tubular furnace was set to 280°C.
[0084] (8) Metal Corrosion of Molded Articles 30 g of the connector molded article molded in (6) was weighed, and the metal corrosivity of the molded article was evaluated in the same manner as in (5), except that the heat treatment was performed at 280°C for 1 hour.
[0085] [Example 1] A 5L reaction vessel equipped with a stirring blade and a distillation tube was charged with 808 parts by weight of p-hydroxybenzoic acid (HBA), 88 parts by weight of 6-hydroxy-2-naphthoic acid (HNA), 229 parts by weight of 4,4'-dihydroxybiphenyl (DHB), 161 parts by weight of hydroquinone (HQ), 428 parts by weight of terephthalic acid (TPA), 19 parts by weight of isophthalic acid (IPA), and 1278 parts by weight of acetic anhydride (1.07 equivalents of phenolic hydroxyl groups total), and the mixture was stirred under a nitrogen gas atmosphere at 145 ° C. for 120 minutes, and then heated from 145 ° C. to 360 ° C. over 320 minutes. At this time, the temperature increase was controlled so that the reaction time from 230 ° C. to 245 ° C. was 95 minutes. Thereafter, the polymerization temperature was maintained at 360 ° C., and the pressure was reduced to 1.0 torr (133 Pa) over 1.0 hour. The reaction was continued until a predetermined stirring torque was reached, at which point the polymerization was completed. The polymer was then extruded into strands through a die having one circular outlet with a diameter of 6 mm, and pelletized with a cutter to obtain a liquid crystal polyester resin (A-1).
[0086] [Example 2] A liquid crystal polyester resin (A-2) was obtained in the same manner as in Example 1, except that the temperature increase time from 145°C to 360°C was 295 minutes and the reaction time from 230°C to 245°C was 70 minutes.
[0087] [Example 3] Polymerization was carried out in the same manner as in Example 1, except that the amount of acetic anhydride charged was 1,314 parts by weight (1.10 equivalents of the total of phenolic hydroxyl groups). When the polymerization reached a predetermined stirring torque at a reduced pressure of 3.0 kPa (23 torr), the polymerization was completed, and a liquid crystal polyester resin (A-3) was obtained.
[0088] [Example 4] A liquid crystal polyester resin (A-4) was obtained in the same manner as in Example 1, except that the temperature increase time from 145°C to 360°C was 270 minutes and the reaction time from 230°C to 245°C was 45 minutes.
[0089] [Example 5] A liquid crystal polyester resin (A-5) was obtained in the same manner as in Example 1, except that the temperature increase time from 145°C to 360°C was 340 minutes and the reaction time from 230°C to 245°C was 115 minutes.
[0090] [Example 6] A liquid crystal polyester resin (A-6) was obtained in the same manner as in Example 1, except that the amount of the monomers charged was changed to HBA 905 parts by weight, HNA 88 parts by weight, DHB 109 parts by weight, HQ 193 parts by weight, TPA 321 parts by weight, and IPA 68 parts by weight.
[0091] [Example 7] A liquid crystal polyester resin (A-7) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to HBA 970 parts by weight, HNA 88 parts by weight, DHB 196 parts by weight, HQ 116 parts by weight, and TPA 350 parts by weight.
[0092] [Example 8] A liquid crystal polyester resin (A-8) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to HBA 1018 parts by weight, HNA 264 parts by weight, DHB 44 parts by weight, HQ 135 parts by weight, TPA 214 parts by weight, and IPA 29 parts by weight.
[0093] [Example 9] A liquid crystal polyester resin (A-9) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to 469 parts by weight of HBA, 242 parts by weight of HNA, 131 parts by weight of DHB, 309 parts by weight of HQ, 564 parts by weight of TPA, and 19 parts by weight of IPA.
[0094] [Example 10] A liquid crystal polyester resin (A-10) was obtained in the same manner as in Example 1, except that the amount of monomers charged was changed to 808 parts by weight of HBA, 88 parts by weight of HNA, 501 parts by weight of DHB, 408 parts by weight of TPA, and 39 parts by weight of IPA.
[0095] [Example 11] Polymerization was carried out in the same manner as in Example 1, except that the amount of acetic anhydride charged was 1,338 parts by weight (1.12 equivalents of the total of phenolic hydroxyl groups). When the polymerization reached a predetermined stirring torque at a reduced pressure of 45 torr, the polymerization was completed, and a liquid crystal polyester resin (A-11) was obtained.
[0096] The liquid crystal polyester resins obtained in Examples 1 to 11 and Comparative Examples 1 to 3 were evaluated in the above items (1) to (6), and the results are shown in Tables 1 and 2.
[0097] Comparative Example 1 A liquid crystal polyester resin (A'-12) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to 870 parts by weight of HBA, 352 parts by weight of DHB, 89 parts by weight of HQ, 292 parts by weight of TPA, and 157 parts by weight of IPA, the temperature rise time from 145°C to 360°C was changed to 240 minutes, and the reaction time from 230°C to 245°C was changed to 15 minutes.
[0098] Comparative Example 2 Liquid crystal polyester resin (A'-13) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to 870 parts by weight of HBA, 352 parts by weight of DHB, 89 parts by weight of HQ, 292 parts by weight of TPA, and 157 parts by weight of IPA.
[0099] [Comparative Example 3] A liquid crystal polyester resin (A'-14) was obtained in the same manner as in Example 1, except that the temperature increase time from 145°C to 360°C was 250 minutes and the reaction time from 230°C to 245°C was 25 minutes.
[0100]
[0101]
[0102] Liquid crystal polyester resin compositions were prepared by further adding a filler to the liquid crystal polyester resins obtained in Example 1 and Comparative Example 3. The fillers used in each of the Examples and Comparative Examples are shown below.
[0103] Filler (B) (B-1) Milled fiber (40M-10A) manufactured by Nippon Electric Glass Co., Ltd. [Example 12, Comparative Example 4] Using a Toshiba Machine TEM35B twin-screw extruder equipped with a side feeder, the liquid crystal polyester resins (A-1, A'-14) obtained in each production example were added from the hopper in the amounts shown in Table 2, and filler (B-1) was added from the side feeder in the amount shown in Table 2. The cylinder temperature was set to the melting point of the liquid crystal polyester resin + 10°C, and the mixture was melt-kneaded to obtain pellets. The resulting pellets of the liquid crystal polyester resin composition were dried with hot air and evaluated in the same manner as in (5) to (8). The results are shown in Table 2. In the evaluation of (7), the amount of gas generated from the liquid crystal polyester resin excluding the filler was calculated in terms of the amount of gas generated.
[0104]
[0105] From the results in Tables 1 to 3, by using a liquid crystal polyester resin containing 15 to 75 mol% of the structural unit (I) and 2 to 20 mol% of the structural unit (II) and having a phenol gas content of 100 ppm or less, or a liquid crystal polyester resin composition using such a resin, it is possible to reduce metal corrosivity when used in a high-temperature environment and obtain a molded article with excellent low warpage. Furthermore, when the obtained molded article was maintained at 280°C, the phenol gas content was 70 ppm or less, thereby reducing metal corrosivity when processed at high temperatures.
[0106] The liquid crystal polyester resin and liquid crystal polyester resin composition of the present invention can reduce metal corrosiveness when used in a high-temperature environment and have excellent low warpage properties, and are therefore suitable for use in electrical and electronic components and mechanical components such as connectors, relays, switches, coil bobbins, and actuator components for camera modules.
[0107] (A) Pellet sealing and heating area (B) Sealed tube area (C) Evolved gas collection area (D) Liquid crystal polyester resin pellet 1 Long side 2 Short side 3 Length 4 Height 5 Width 6 Terminal pitch 7 Minimum thickness part 8 Warpage G1 Pin gate a Reference surface b Maximum deformation surface
Claims
1. A liquid crystal polyester resin containing 20 to 80 mol % of structural units derived from aromatic hydroxycarboxylic acid, 10 to 40 mol % of structural units derived from aromatic diol, and 10 to 40 mol % of structural units derived from aromatic dicarboxylic acid, relative to 100 mol % of all structural units of the liquid crystal polyester resin, and containing at least 15 to 75 mol % of structural unit (I) and 2 to 20 mol % of structural unit (II) as the aromatic hydroxycarboxylic acid, wherein the amount of phenol gas generated when the liquid crystal polyester resin is kept at a melting point + 20°C for 60 minutes under a reduced pressure of 13.3 kPa or less is 100 ppm or less; The melting point of the liquid crystal polyester resin is the endothermic peak temperature (Tm) observed when the liquid crystal polyester resin is heated from room temperature at a temperature increase of 20°C / min in differential calorimetry. 1 ) after the observation of Tm 1 This is the endothermic peak temperature observed when the sample is held at +20° C. for 5 minutes, cooled to room temperature at a temperature drop rate of 20° C. / min, and then heated again at a temperature rise rate of 20° C. / min.
2. The liquid crystal polyester resin according to claim 1, wherein the content of the structural unit (I) is 80 to 97 mol % relative to 100 mol % in total of the structural units (I) and (II).
3. The liquid crystal polyester resin according to claim 1, which contains 2 to 20 mol % of the structural unit (III) as the aromatic diol relative to 100 mol % of all structural units of the liquid crystal polyester resin.
4. The liquid crystal polyester resin according to claim 1, which contains structural units (III) and (IV) as the aromatic diol, and the content of structural unit (III) is 45 to 90 mol % relative to 100 mol % in total of structural units (III) and (IV).
5. A method for producing a liquid crystal polyester resin according to any one of claims 1 to 4, comprising reacting a hydroxycarboxylic acid and / or a diol with acetic anhydride to acetylate at least a portion of the phenolic hydroxyl groups, and then polymerizing the resulting mixture with a dicarboxylic acid to produce a liquid crystal polyester resin, the method comprising carrying out the deacetylation polymerization reaction at a temperature of 230 to 245°C for 40 to 120 minutes.
6. A liquid crystal polyester resin composition comprising 10 to 200 parts by weight of a filler based on 100 parts by weight of the liquid crystal polyester resin according to any one of claims 1 to 4.
7. A molded article comprising the liquid crystal polyester resin according to any one of claims 1 to 4, or the liquid crystal polyester resin composition according to claim 6.
8. The molded article according to claim 7, which is any one selected from the group consisting of a connector, a relay, a switch, a coil bobbin, and an actuator part of a camera module.
9. A molded article comprising a liquid crystal polyester resin containing 20-80 mol % of structural units derived from aromatic hydroxycarboxylic acid, 10-40 mol % of structural units derived from aromatic diol, and 10-40 mol % of structural units derived from aromatic dicarboxylic acid, and containing at least 15-75 mol % of structural unit (I) and 2-20 mol % of structural unit (II) as the aromatic hydroxycarboxylic acid, wherein the amount of phenol gas generated when the molded article is held at 280°C for 60 minutes under a reduced pressure of 13.3 kPa or less is 60 ppm or less.
Citation Information
Patent Citations
Liquid crystal resin composition and molded product
JP1997221582A
Wholly aromatic liquid crystalline polyester resin, and composition containing the same
JP2012126842A
Liquid crystal polyester and method for producing the same
JP2014172953A
Liquid crystal polymer composition
JP2020186334A
Liquid crystal polyester resin composition and molded article composed of the same
JP2024042190A