Liquid crystal polyester resin, liquid crystal polyester resin composition, and molded article formed thereof
The liquid crystal polyester resin composition addresses gas generation and flame retardancy issues by controlling the structural units, resulting in improved performance for thin-walled electronic components.
Patent Information
- Application Number
- PCT/JP2024/015713
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional liquid crystal polyester resins face challenges in controlling gas generation during high-temperature injection molding, leading to issues like drawling and reduced flame retardancy, especially in the production of thin-walled electronic components.
A liquid crystal polyester resin composition is developed with specific structural units derived from aromatic hydroxycarboxylic acids, aromatic diols, and dicarboxylic acids, controlled to generate less than 300 ppm of aromatic carboxylic acid and acetic acid under defined conditions, enhancing flame retardancy and preventing drawling.
The solution effectively suppresses gas generation and improves flame retardancy, making the resin suitable for molding small electronic components with excellent processability and long-term stability.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Liquid crystal polyester resin, liquid crystal polyester resin composition and molded article made thereof
[0001] The present invention relates to a liquid crystal polyester resin, a liquid crystal polyester resin composition, and a molded article made thereof, more particularly to a liquid crystal polyester resin, a liquid crystal polyester resin composition, and a molded article obtained using the same.
[0002] Liquid crystal polyester resins have excellent heat resistance, fluidity, and dimensional stability, making them suitable for electrical and electronic components that require these properties. In recent years, the miniaturization of smartphones and other devices has led to increased demand for higher component integration, thinner walls, and lower profile components. Therefore, liquid crystal polyester resins with enhanced fluidity are required as materials for these components. However, reducing the viscosity of liquid crystal polyester resins to ensure thin-wall fluidity increases gas content during melt processing, leading to the development of low-gas liquid crystal polyester resins. Low-gas liquid crystal polyester resins can prevent gases generated during melt processing from being retained inside molded products. They can also suppress gas generation during heat treatment at relatively low temperatures (up to 280°C) below the melting point, such as reflow processing. Molded products with reduced gas generation offer excellent processability and reduced deterioration during long-term use, so low-gas properties are desirable not only for materials but also for molded products.
[0003] For example, Patent Document 1 discloses that a liquid crystalline resin containing controlled amounts of acetic acid, phenol, and carbon dioxide is achieved by controlling the acetylation rate of the aromatic diol used to be lower than usual. Patent Document 2 discloses that the generation of gases such as phenol can be reduced by using a wholly aromatic polyester resin composed of structural units derived from 6-hydroxy-2-naphthoic acid, 4,4'-dihydroxybiphenyl, hydroquinone, and terephthalic acid, without using p-hydroxybenzoic acid, which causes phenol gas. Patent Document 3 discloses that fogging caused by gases generated from the polymer can be reduced by controlling the type and ratio of terminal substrates of a wholly aromatic liquid crystalline polyester within a specific range. Patent Document 4 proposes a liquid crystalline polyester resin that contains p-hydroxybenzoic acid as the main component and structural units derived from 6-hydroxy-2-naphthoic acid, 4,4'-dihydroxybiphenyl, hydroquinone, and terephthalic acid, thereby reducing blisters caused by generated gases and improving warpage. On the other hand, due to the recent increase in the complexity of part shapes, molded products are increasingly being produced under high temperature and high injection speed (high shear) conditions in injection molding in order to fill thin-walled areas, and it has become difficult to achieve the resin properties currently required with conventional liquid crystal polyester resins.
[0004] JP 2006-89714 A JP 2009-127025 A International Publication No. 2012 / 090407 International Publication No. 2018 / 101214
[0005] When liquid crystal polyester resins are melt-mixed using a twin-screw extruder or processed using an injection molding machine, they are subjected to high temperatures, shear stress, and sometimes reduced pressure, resulting in the generation of various types of gases due to resin decomposition. Depending on the composition of the gases generated, particularly under high temperatures and high injection rates, gas expansion and resin decomposition can occur, leading to drooling (a phenomenon in which the resin leaks and sags from the nozzle tip during molding) and stringing (a phenomenon in which unsolidified resin stretches out like a thread from the top of the spool when the mold is opened). Furthermore, under high-temperature conditions, such as exposure to flames, the flame retardancy of some types of gases can be reduced. While liquid crystal polyester resins have superior flame retardancy compared to other resins, the recent trend toward thinner materials has led to the demand for even greater flame retardancy. Conventional liquid crystal polyester resins have been unable to adequately control gas generation under more severe conditions. For example, Patent Document 1 discloses a liquid crystal polyester resin in which the generation of phenol, acetic acid, and carbon dioxide gas components when the resin is held at a temperature of melting point +10°C for 30 minutes in a helium gas atmosphere is suppressed. However, there is a problem in that gas components that affect moldability and flame retardancy (e.g., aromatic carboxylic acids) and gas components that are generated under reduced pressure conditions that correlate well with moldability and flame retardancy are not controlled. Similarly, Patent Documents 2 to 4 also insufficiently control gas components that may cause drowning.
[0006] An object of the present invention is to provide a liquid crystal polyester resin, a liquid crystal polyester resin composition, and a molded article made thereof, which are excellent in flame retardancy and suppress gas generation that causes drowning during injection molding at high temperatures.
[0007] As a result of extensive research to solve the above problems, the present inventors have found that a liquid crystal polyester resin containing 20 to 80 mol % of the following structural units derived from aromatic hydroxycarboxylic acid, 10 to 40 mol % of structural units derived from aromatic diol, and 10 to 40 mol % of structural units derived from aromatic dicarboxylic acid, relative to 100 mol % of all structural units of the liquid crystal polyester resin, in which the gas components generated under the conditions described below are controlled, has excellent moldability and flame retardancy, and have arrived at the present invention.
[0008] That is, the present invention is as follows: (1) A liquid crystal polyester resin containing 20 to 80 mol % of structural units derived from aromatic hydroxycarboxylic acid, 10 to 40 mol % of structural units derived from aromatic diol, and 10 to 40 mol % of structural units derived from aromatic dicarboxylic acid, relative to 100 mol % of all structural units of the liquid crystal polyester resin, wherein the liquid crystal polyester resin satisfies the following requirement (α): Requirement (α): When the liquid crystal polyester resin is maintained at a temperature of melting point Tm+20°C for 60 minutes under a reduced pressure of 13.3 kPa or less, the total amount of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin is less than 300 ppm; The melting point Tm of the liquid crystal polyester resin is the endothermic peak temperature (Tm) observed in differential calorimetry when the liquid crystal polyester resin is heated from room temperature at a temperature increase condition of 20°C / min. 1 ) after the observation of Tm 1 The endothermic peak temperature is the temperature observed when the resin is held at +20°C for 5 minutes, cooled to room temperature at a temperature decrease rate of 20°C / min, and then heated again at a temperature increase rate of 20°C / min. (2) A liquid crystal polyester resin according to (1), which contains 0.1 to 100 ppm of iron atoms. (3) A liquid crystal polyester resin according to (1) and (2), which contains the following structural unit (I), and satisfies the following formula (a): 2≦[I]≦20 (a), where [I] represents the content (mol %) of each structural unit (I) below relative to 100 mol % of all structural units in the liquid crystal polyester resin.
[0009]
[0010] (4) A liquid crystal polyester resin according to any one of (1) to (3) containing the following structural units (I) and (II), which satisfies the following formulae (b) and (c): 0.01≦[II]≦5 (b) [II] / [I]<1 (c) [I] and [II] represent the content (mol %) of each of the following structural units (I) and (II) relative to 100 mol % of all structural units in the liquid crystal polyester resin.
[0011]
[0012] (5) A liquid crystal polyester resin according to any one of (1) to (4), which contains the following structural units (II) and (III), and satisfies the following formula (d): 0.92<[III] / ([II]+[III])<1 (d) [II] and [III] represent the content (mol %) of each of the following structural units (II) and (III) relative to 100 mol % of all structural units in the liquid crystal polyester resin.
[0013]
[0014] (6) A method for producing a liquid-crystalline polyester resin according to any one of (1) to (5), comprising reacting a hydroxycarboxylic acid and / or a diol with acetic anhydride to acetylate at least a portion of the phenolic hydroxyl groups, followed by deacetylation polymerization with a dicarboxylic acid, wherein the feed ratio of raw material monomers satisfies the following formula (e): 1<[aromatic diol] / [aromatic dicarboxylic acid]<1.5 (e), where [aromatic diol] and [aromatic dicarboxylic acid] represent the amounts (molar) of the aromatic diol and aromatic dicarboxylic acid charged during the production of the liquid-crystalline polyester resin. (7) A liquid-crystalline polyester resin composition comprising 10 to 200 parts by weight of a filler per 100 parts by weight of the liquid-crystalline polyester resin according to any one of (1) to (5). (8) A molded article comprising the liquid-crystalline polyester resin according to any one of (1) to (5) or the liquid-crystalline polyester resin composition according to (7). (9) The molded article according to (8), wherein the molded article is any one selected from the group consisting of a connector, a relay, a switch, a coil bobbin, and an actuator part for a camera module. (10) A molded article comprising a liquid crystal polyester resin containing 20 to 80 mol% of structural units derived from aromatic hydroxycarboxylic acid, 10 to 40 mol% of structural units derived from aromatic diol, and 10 to 40 mol% of structural units derived from aromatic dicarboxylic acid, relative to 100 mol% of all structural units of the liquid crystal polyester resin, wherein the total amount of aromatic carboxylic acid and acetic acid generated when the molded article is maintained at 280°C under a reduced pressure of 13.3 kPa or less for 60 minutes is less than 100 ppm.
[0015] The liquid crystal polyester resin of the present invention suppresses drowning during injection molding and has excellent flame retardancy. The liquid crystal polyester resin of the present invention is particularly suitable for use in molding small electrical and electronic parts.
[0016] 1 is a schematic diagram of a glass ampoule used for measuring the amount of phenol gas generated. FIG 2 is a schematic diagram of a glass ampoule in which liquid crystal polyester resin pellets are sealed under reduced pressure.
[0017] The present invention will be described in detail below.
[0018] Liquid crystal polyester resin is a polyester that forms an anisotropic molten phase. Examples of such polyester resins include polyesters composed of structural units selected from the below-described oxycarbonyl unit, dioxy unit, dicarbonyl unit, etc. so as to form an anisotropic molten phase.
[0019] The liquid crystal polyester resin of the present invention is characterized in that the gas components and amounts generated during melting are controlled. That is, the liquid crystal polyester resin of the present invention satisfies the following requirement (α): (α): When the liquid crystal polyester resin is maintained at a temperature of the melting point (Tm) + 20°C under a reduced pressure of 13.3 kPa or less for 60 minutes, the total amount of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin is less than 300 ppm.
[0020] The melting point Tm of the liquid crystal polyester resin is the endothermic peak temperature (Tm 1 ) after the observation of Tm 1 This is the endothermic peak temperature observed when the sample is held at +20°C for 5 minutes, cooled to room temperature at a temperature decreasing rate of 20°C / min, and then heated again at a temperature increasing rate of 20°C / min.
[0021] The aromatic carboxylic acids referred to above refer to terephthalic acid, isophthalic acid, and benzoic acid. Terephthalic acid and isophthalic acid are used as raw material monomers for liquid crystal polyester resins, but they may exist unreacted in the liquid crystal polyester resin. Furthermore, if structural units derived from terephthalic acid or isophthalic acid are unevenly distributed near the terminals of the liquid crystal polyester resin, terephthalic acid and isophthalic acid are released by sublimation and decomposition when the liquid crystal polyester resin is heated and retained above its melting point (Tm). Benzoic acid is produced during the decomposition process of aromatic dicarboxylic acids such as terephthalic acid and isophthalic acid, and aromatic hydroxycarboxylic acids such as hydroxybenzoic acid, during polymerization or during heating and retention. Isophthalic acid, in particular, has a bent structure with carboxylic acid moieties close together, making it bulky and prone to decomposition. Regarding acetic acid, when a liquid crystal polyester resin is produced by deacetic acid polymerization using acetic anhydride, as described below, trace amounts of acetic acid may remain in the liquid crystal polyester resin. Furthermore, in the case of a liquid crystal polyester resin with a large number of acetyl terminals, when the liquid crystal polyester resin is heated and retained at a temperature equal to or higher than the melting point Tm, acetic acid is released by decomposition.
[0022] In the present invention, it has been discovered that by controlling the total amount of aromatic carboxylic acid and acetic acid generated when a liquid crystal polyester resin is heated and retained under reduced pressure under the above-mentioned conditions to less than 300 ppm, drooling during injection molding is suppressed and flame retardancy is improved. When these components are released at 300 ppm or more from a liquid crystal polyester resin, large amounts of the acid components, aromatic carboxylic acid and acetic acid, are released during heating and retention, such as during melt-kneading under reduced pressure or injection molding. This accelerates decomposition of the liquid crystal polyester resin, making drooling more likely to occur during injection molding and reducing the flame retardancy of the molded product. The total amount of aromatic carboxylic acid and acetic acid is preferably 200 ppm or less, more preferably 150 ppm or less, and most preferably 100 ppm or less. Hereinafter, the term "the total amount of aromatic carboxylic acid and acetic acid generated from a liquid crystal polyester resin when held at a temperature of the melting point (Tm) + 20°C for 60 minutes under a reduced pressure of 13.3 kPa or less" may be abbreviated as "gas generation amount."
[0023] The liquid crystal polyester resin of the present invention has a gas generation amount controlled to less than 300 ppm. While the detailed breakdown is not limited, from the viewpoint of further suppressing drool during injection molding and further improving flame retardancy, the terephthalic acid content is preferably less than 150 ppm, more preferably 100 ppm or less, and even more preferably 50 ppm or less. The isophthalic acid content is preferably 75 ppm or less, more preferably 50 ppm or less, and even more preferably 25 ppm or less. The benzoic acid content is preferably 50 ppm or less, and even more preferably 25 ppm or less. The acetic acid content is preferably 100 ppm or less, more preferably 75 ppm or less, and even more preferably 50 ppm or less.
[0024] The method for controlling the amount of gas generated to a preferred range includes, for example, setting the structural units constituting the liquid crystal polyester resin to a preferred range and / or setting the method for producing the liquid crystal polyester resin to a preferred method. Details will be described in the following structural units constituting the liquid crystal polyester resin and in the "Method for producing a liquid crystal polyester resin" below.
[0025] The method for calculating the amounts of aromatic carboxylic acid and acetic acid generated is described below. First, 5 g of liquid crystal polyester resin pellets are dried at 150°C for 3 hours using a hot air dryer, and then placed in the heated portion (A) of a glass ampoule tube having the shape shown in Figure 1. A vacuum pump (ULVAC DTC-22) is used to evacuate the tip of the glass ampoule tube, controlling the pressure inside the system to 13.3 kPa or less. Then, the portion (B) 70 mm from the tip is heated and melted with a gas burner to seal the tube, producing an analytical ampoule as shown in Figure 2. Next, the heated portion (A) of the analytical ampoule is maintained at a temperature of 20°C above the melting point of the liquid crystal polyester resin for 60 minutes using a ceramics electric tubular furnace (Asahi Rika Seisakusho ARF-30K (temperature controller AMF-N type)). Gas components generated from the liquid crystal polyester resin pellets by heating are collected in the portion (C). The ampoule was removed from the ceramic electric tubular furnace and cooled to room temperature, after which the (C) portion was cut out from the ampoule with a file. The cut-out (C) portion was weighed, and all of the gas components condensed in the (C) portion were dissolved in deuterated dimethyl sulfoxide (0.8 g). A small amount of 1,4-dioxane was added as an internal standard, and the resulting solution was analyzed using a JNM-ECZ500R manufactured by JEOL Ltd. 1 H-NMR measurement is performed. In addition, the (C) portion from which the trapped components have been removed is washed with acetone, dried in a glass dryer at 60°C for 1 hour, and then weighed again, and the total amount of evolved gas is calculated from the difference in weight of the (C) portion before and after removal of the trapped components. 1 From the H-NMR spectrum, the integral ratio of the peaks derived from aromatic carboxylic acids (terephthalic acid, isophthalic acid, benzoic acid), the peak derived from acetic acid, and the peak of the internal standard (1,4-dioxane) is calculated. From this and the total amount of the evolved gas, the amount (ppm) of aromatic carboxylic acid and acetic acid gas evolved from the liquid crystal polyester resin is calculated.
[0026] Here, the degree of vacuum inside the ampoule glass tube is not particularly limited as long as it is 13.3 kPa or less, and may be, for example, a high vacuum state of 0.133 kPa or less.
[0027] Next, the structural units constituting the liquid crystal polyester resin will be described.
[0028] The liquid crystal polyester resin of the present invention contains 20 to 80 mol% of structural units derived from aromatic hydroxycarboxylic acids as oxycarbonyl units, relative to 100 mol% of all structural units in the liquid crystal polyester resin. If the content of these structural units is less than 20 mol%, liquid crystallinity is impaired, resulting in reduced flame retardancy. The content of these structural units is preferably 25 mol% or more, more preferably 30 mol% or more. On the other hand, if the content of these structural units is greater than 80 mol%, it becomes difficult to control the amount of gas generated to less than 300 ppm, drowning is likely to occur, and the flame retardancy of the molded article is also reduced. The content of these structural units is preferably 75 mol% or less, more preferably 70 mol% or less, and even more preferably 55 mol% or less.
[0029] The liquid crystal polyester resin of the present invention preferably contains 2 to 20 mol% of structural unit (I) as a structural unit derived from an aromatic hydroxycarboxylic acid. The structural unit (I) is a structural unit derived from 6-hydroxy-2-naphthoic acid. The structural unit (I) has a naphthalene structure, is bulky, and inhibits molecular motion, thereby suppressing decomposition of molecular chains near the structural unit (I) during heating and retention. Furthermore, the structural unit (I) reacts well with the structural unit (IV) described below, further suppressing the generation of benzoic acid gas associated with the decomposition of the structural unit (IV). These effects make it easy to control the amount of gas generated to less than 300 ppm. Furthermore, the structural unit (I) is highly aromatic, promoting char formation when exposed to flame, and therefore, the inclusion of the structural unit (I) can also enhance flame retardancy. The content of the structural unit (I) is preferably 2.5 mol% or more, more preferably 3 mol% or more. From the viewpoint of flame retardancy and suppression of drowning, the content is preferably 15 mol % or less, and more preferably 10 mol % or less.
[0030]
[0031] From the viewpoint of improving liquid crystallinity and excellent flame retardancy, the liquid crystal polyester resin of the present invention preferably contains 15 to 75 mol% of structural unit (IV) as a structural unit derived from an aromatic hydroxycarboxylic acid. The content of structural unit (IV) is more preferably 25 mol% or more, and even more preferably 35 mol% or more. Furthermore, from the viewpoint of easily controlling the amount of gas generation to less than 300 ppm, the content is preferably 65 mol% or less, and more preferably 55 mol% or less.
[0032]
[0033] The liquid crystal polyester resin of the present invention may contain, as an oxycarbonyl unit, a structural unit other than the structural units (I) and (IV). Specific examples of other oxycarbonyl units include structural units derived from m-hydroxybenzoic acid.
[0034] The liquid crystal polyester resin of the present invention contains, as dicarbonyl units, 10 to 40 mol% of structural units derived from aromatic dicarboxylic acids, relative to 100 mol% of all structural units in the liquid crystal polyester resin. If the content of these structural units is less than 10 mol%, liquid crystallinity is impaired, resulting in reduced flame retardancy. The content of these structural units is preferably 15 mol% or more, more preferably 20 mol% or more. On the other hand, if the content of these structural units is greater than 40 mol%, it becomes difficult to control the amount of gas generated to less than 300 ppm, drowning is more likely to occur, and the flame retardancy of the molded article is also reduced. The content of these structural units is preferably 35 mol% or less, more preferably 30 mol% or less. Examples of structural units derived from aromatic dicarboxylic acids include structural units derived from terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, 1,2-bis(2-chlorophenoxy)ethane-4,4'-dicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, etc. From the viewpoints of excellent availability and an excellent moldable temperature range, it is preferable to use a structural unit selected from structural units derived from terephthalic acid and structural units derived from isophthalic acid.
[0035] The liquid crystal polyester resin of the present invention preferably contains 0.01 mol% or more of the structural unit (II) as a structural unit derived from an aromatic dicarboxylic acid, relative to 100 mol% of all structural units of the liquid crystal polyester resin, from the viewpoint of easily controlling the amount of gas generation to less than 300 ppm, having excellent flame retardancy, and being able to suppress drowning. The structural unit (II) is a structural unit derived from isophthalic acid. On the other hand, from the viewpoint of more easily controlling the amount of gas generation to less than 300 ppm, the structural unit (II) is preferably contained in an amount of 5 mol% or less, more preferably 3 mol% or less, and even more preferably 1.5 mol% or less. Since the structural unit (II) has a bent structure, decomposition and deterioration are likely to occur from the site where the structural unit is introduced due to heating retention. Therefore, the effects of the present invention can be enhanced by setting the amount in the above preferred range.
[0036]
[0037] The liquid crystal polyester resin of the present invention is easy to control the amount of gas generated to less than 300 ppm, has excellent flame retardancy, and can suppress drowning. From the viewpoint of this, it preferably contains 5 mol% or more, preferably 10 mol% or more, and more preferably 15 mol% or more of structural unit (III) as a structural unit derived from an aromatic dicarboxylic acid relative to 100 mol% of all structural units of the liquid crystal polyester resin. The structural unit (III) is a structural unit derived from terephthalic acid. On the other hand, from the viewpoint of further facilitating the control of the amount of gas generated to less than 300 ppm, it is preferable to contain 35 mol% or less of structural unit (III), more preferably 30 mol% or less, and even more preferably 25 mol% or less.
[0038]
[0039] The liquid crystal polyester resin of the present invention may contain, as a dicarbonyl unit, a structural unit other than the structural units (II) and (III). As other dicarbonyl units, structural units derived from aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, and hexahydroterephthalic acid; and structural units derived from alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 1,3-cyclohexanedicarboxylic acid can be used within a range that does not impair the effects of the present invention.
[0040] In the liquid crystal polyester resin of the present invention, the amount of gas generated can be easily controlled to less than 300 ppm, flame retardancy is excellent, and drowning can be suppressed. From the viewpoint of this, the ratio of the content of the structural unit (I) to the structural unit (II) relative to 100 mol% of all structural units of the liquid crystal polyester resin ([II] / [I]) is preferably less than 1. By setting it in this range, the structural unit (II) is sufficiently incorporated into the polymer chain, and the amount of gas generated can be further controlled. [II] / [I] is more preferably 0.9 or less. On the other hand, the lower limit of [II] / [I] is not particularly limited, and it may be 0.005 or more. From the viewpoint of this, the amount of gas generated can be easily controlled to less than 300 ppm, flame retardancy is excellent, and drowning can be suppressed. [II] / [I] is preferably 0.01 or more, more preferably 0.05 or more.
[0041] [I] and [II] respectively represent the contents (mol %) of the structural units (I) and (II) relative to 100 mol % of all structural units in the liquid crystal polyester resin.
[0042] From the viewpoints of easily controlling the amount of gas generated to less than 300 ppm, being excellent in flame retardancy, and being able to suppress drowning, the liquid crystal polyester resin of the present invention preferably has a relationship in which the contents of structural units (II) and (III) relative to 100 mol% of all structural units in the liquid crystal polyester resin satisfy the following formula (d): 0.92<[III] / ([II]+[III])<1 (d) [II] and [III] respectively represent the contents (mol%) of structural units (II) and (III) relative to 100 mol% of all structural units in the liquid crystal polyester resin.
[0043] Since the structural unit (II) is gasified and released at a higher rate during heating and retention than other structural units, by controlling it within the above range, it becomes easy to control the amount of gas generated to less than 300 ppm, thereby achieving excellent flame retardancy and suppressing drowning. [III] / ([II]+[III]) is more preferably 0.94 or more.
[0044] The liquid crystal polyester resin of the present invention contains, as dioxy units, 10 to 40 mol% of structural units derived from aromatic diols, relative to 100 mol% of all structural units in the liquid crystal polyester resin. If the content of these structural units is less than 10 mol%, it becomes difficult to control the amount of gas generated to less than 300 ppm, drowning becomes more likely, and the flame retardancy of the molded product also decreases. The content of these structural units is preferably 15 mol% or more, more preferably 20 mol% or more. On the other hand, if the content of these structural units is more than 40 mol%, liquid crystallinity is impaired, resulting in decreased flame retardancy. The content of these structural units is preferably 35 mol% or less, more preferably 30 mol% or less. Examples of structural units derived from aromatic diols include structural units derived from 4,4'-dihydroxybiphenyl, hydroquinone, resorcinol, t-butylhydroquinone, phenylhydroquinone, chlorohydroquinone, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 3,4'-dihydroxybiphenyl, 2,2-bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfide, and 4,4'-dihydroxybenzophenone.
[0045] The liquid crystal polyester resin of the present invention is easy to control the amount of gas generated to less than 300 ppm, has excellent flame retardancy, and can suppress drowning. From the viewpoint of this, it is preferable that the liquid crystal polyester resin contains 2 mol% or more of the structural unit (V) as a structural unit derived from an aromatic diol, relative to 100 mol% of all structural units of the liquid crystal polyester resin, preferably 5 mol% or more, and more preferably 8 mol% or more. The structural unit (V) is a structural unit derived from hydroquinone. On the other hand, from the viewpoint of further facilitating the control of the amount of gas generated to less than 300 ppm, it is preferable that the structural unit (V) contains 20 mol% or less, more preferably 18 mol% or less, and even more preferably 16 mol% or less.
[0046]
[0047] The liquid crystal polyester resin of the present invention preferably contains 2 mol% or more, more preferably 4 mol% or more, and even more preferably 6 mol% or more of structural units (VI) derived from aromatic diols, relative to 100 mol% of all structural units of the liquid crystal polyester resin, from the viewpoints of easily controlling the amount of gas generated to less than 300 ppm, excellent flame retardancy, and suppressing drowning. The structural units (VI) are structural units derived from 4,4'-dihydroxybiphenyl. On the other hand, from the viewpoint of even easier control of the amount of gas generated to less than 300 ppm, the structural units (VI) are preferably contained in an amount of 20 mol% or less, more preferably 17 mol% or less, and even more preferably 14 mol% or less.
[0048]
[0049] The liquid crystal polyester resin of the present invention may contain, as a dioxy unit, a structural unit other than the structural units (V) and (VI). As other dioxy units, structural units derived from aliphatic diols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, and neopentyl glycol; and structural units derived from alicyclic diols such as 1,4-cyclohexanediol and 1,4-cyclohexanedimethanol can be used within a range that does not impair the effects of the present invention.
[0050] In addition to the structural units (I) to (VI), the liquid crystal polyester resin may contain structural units derived from p-aminobenzoic acid, p-aminophenol, etc., within the range that does not impair the effects of the present invention.
[0051] When the liquid crystal polyester resin of the present invention contains all of the structural units (I) to (VI) in the above-mentioned ranges, the structural units (II) and (II) are sufficiently incorporated into the polymer chain, making it easy to control the amount of gas generated to less than 300 ppm, and it is preferable that the resin has excellent flame retardancy and suppresses drowning. Also, from the viewpoint of not impairing the effects of the present invention, the total amount of the structural units (I) to (VI) is preferably 99 mol% or more, more preferably 99.5 mol% or more, and even more preferably 100 mol%.
[0052] In addition to the structural units (I) to (VI), the liquid crystal polyester resin may contain structural units derived from p-aminobenzoic acid, p-aminophenol, etc., within the range that does not impair the effects of the present invention.
[0053] The monomers used as raw materials for forming the structural units are not particularly limited as long as they have a structure capable of forming the structural units. In addition, derivatives of such monomers, such as acylated hydroxyl groups, esterified carboxyl groups, acid halides, and acid anhydrides, may also be used.
[0054] The method for calculating the content of each structural unit in a liquid crystal polyester resin is as follows. First, the liquid crystal polyester resin is pulverized, and then tetramethylammonium hydroxide is added. Then, the content of each structural unit can be determined by performing pyrolysis GC / MS measurement using a Shimadzu GCMS-QP5050A. The content of structural units that are not detected or are below the detection limit is calculated as 0 mol %.
[0055] The liquid crystal polyester resin of the present invention preferably contains 0.1 to 100 ppm of iron atoms. Because iron atoms can form complexes with carboxylic acid moieties such as acetic acid, the inclusion of iron atoms in the liquid crystal polyester resin can further reduce the amount of gas generation, provide excellent flame retardancy, and suppress drowning. Furthermore, by adding iron atoms during polymerization of the liquid crystal polyester resin, the iron atoms act as a catalyst, favorably controlling the reactivity of the monomers that provide the structural units (I) to (VI) and reducing the proportion of unreacted materials, making it easy to control the amount of gas generation to less than 300 ppm. The content referred to here is calculated as the weight of iron atoms in the liquid crystal polyester resin. The iron atom content is more preferably 50 ppm or less, even more preferably 30 ppm or less, and most preferably 10 ppm or less.
[0056] The method for incorporating iron atoms into a liquid crystal polyester resin is not particularly limited, and examples thereof include the following: 1. A liquid crystal polyester resin is produced using a monomer raw material containing a trace amount of iron atoms by the method described below in <Method for producing liquid crystal polyester resin>. 2. A trace amount of a compound containing iron atoms is added during production by the method described below in <Method for producing liquid crystal polyester resin>. The compound containing iron atoms is not particularly limited, and examples include iron powder, iron oxide, iron hydroxide, iron chloride, iron sulfide, iron sulfate, and iron acetate. 3. A polymerization apparatus made of stainless steel (SUS), whose main component is iron, is used.
[0057] In the above method, the iron atoms are well dispersed in the liquid crystal polyester resin, and therefore the method 1 is preferred from the viewpoint of effectively exerting the effects of the iron atoms.
[0058] In the present invention, the content of iron atoms contained in the liquid crystal polyester resin is the total amount of iron atoms contained in compounds containing iron atoms contained as impurities (metallic iron, iron oxide, etc.) and iron atoms contained in the polymer skeleton or coordinated to the terminals, etc. The content of iron atoms is a value measured by adding sulfuric acid dropwise to the liquid crystal polyester resin, incinerating at 500°C, dissolving the obtained ash in a 0.1 N nitric acid aqueous solution, and subjecting the resultant ash to atomic absorption spectrometry using an emission spectrometer.
[0059] From the viewpoint of heat resistance, the melting point (Tm) of the liquid crystal polyester resin is preferably 280° C. or higher, more preferably 300° C. or higher, and even more preferably 320° C. or higher. On the other hand, from the viewpoint of processability, the melting point (Tm) of the liquid crystal polyester resin is preferably 370° C. or lower, more preferably 360° C. or lower, and even more preferably 350° C. or lower.
[0060] From the viewpoint of heat resistance, the melt viscosity of the liquid crystal polyester resin is preferably 3 Pa s or more, more preferably 5 Pa s or more, and even more preferably 7 Pa s or more. On the other hand, from the viewpoint of fluidity, the melt viscosity of the liquid crystal polyester resin is preferably 50 Pa s or less, preferably 30 Pa s or less, and even more preferably 20 Pa s or less.
[0061] The melt viscosity is a value measured by a Koka type flow tester at a temperature of the melting point (Tm) of the liquid crystal polyester resin + 20° C. under the condition of a shear rate of 1000 / sec.
[0062] <Method for producing liquid crystal polyester resin> The liquid crystal polyester resin of the present invention can be produced by copolymerizing monomers that provide the structural units (I) to (VI) in a content within the above-mentioned range, or by blending two or more liquid crystal polyester resins obtained by copolymerizing the structural units (I) to (VI) in a content outside the above-mentioned range, so that the structural units (I) to (VI) fall within the above-mentioned range. From the viewpoints of easily controlling the amount of gas generated to less than 300 ppm without inheriting the properties of the liquid crystal polyester resin before blending, excellent flame retardancy, and suppressing drowning, the method of copolymerizing monomers that provide the structural units (I) to (VI) in a content within the above-mentioned range is preferred.
[0063] The method for producing the liquid crystal polyester resin of the present invention is not particularly limited, and can be produced in accordance with known polyester polycondensation methods. From the viewpoint of being able to control the amount of gas generated within a suitable range, a preferred method for producing the liquid crystal polyester resin is to react p-hydroxybenzoic acid-derived structural units, 6-hydroxy-2-naphthoic acid-derived structural units, 4,4'-dihydroxybiphenyl-derived structural units, hydroquinone-derived structural units, and terephthalic acid-derived structural units with isophthalic acid, by reacting p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4,4'-dihydroxybiphenyl, hydroquinone, terephthalic acid, and isophthalic acid with acetic anhydride to acetylate the phenolic hydroxyl groups, followed by deacetylation polymerization.
[0064] Furthermore, in the above-mentioned production method using deacetic acid polymerization, the amount of gas generated can be controlled within a more suitable range by satisfying any one of the following requirements 1 to 3. 1. A method for producing a liquid-crystalline polyester resin by reacting a hydroxycarboxylic acid and / or a diol with acetic anhydride to acetylate at least a portion of the phenolic hydroxyl groups, followed by deacetic acid polymerization with a dicarboxylic acid, wherein the charging ratio of raw material monomers satisfies the following formula (e): 1<[aromatic diol] / [aromatic dicarboxylic acid]<1.5 (e) (where [aromatic diol] and [aromatic dicarboxylic acid] represent the amounts (moles) of the aromatic diol and aromatic dicarboxylic acid charged during the production of the liquid-crystalline polyester resin.) 2. A method for producing a liquid-crystalline polyester by using an aromatic hydroxycarboxylic acid, an aromatic diol, and an aromatic dicarboxylic acid as raw material monomers, acetylating the hydroxyl groups of the aromatic diol with acetic anhydride, followed by deacetic acid polymerization, wherein the average heating rate from the polymerization temperature of 230°C to 250°C is controlled to be 0.4°C / min or less. 3. The method for producing a liquid crystal polyester is carried out by using an aromatic hydroxycarboxylic acid, an aromatic diol, and an aromatic dicarboxylic acid as raw material monomers, acetylating the hydroxyl group of the aromatic diol with acetic anhydride, and then polymerizing the hydroxyl group with acetic anhydride by deacetylation, and controlling the reaction time at or above the melting point Tm of the liquid crystal polyester resin to 120 to 170 minutes.
[0065] Regarding the above requirement 1, by adding an aromatic diol monomer in excess of the aromatic dicarboxylic acid monomer, the reaction rate of the aromatic dicarboxylic acid monomer, which has low reactivity, is improved, and in the liquid crystal polyester resin, structural units derived from the aromatic dicarboxylic acid monomer can be unevenly distributed in the chain rather than at the polymer terminal. This prevents gas derived from the aromatic dicarboxylic acid from being released from the terminal during heat melting, making it easier to control the generated gas components. Furthermore, aromatic diols are highly sublimable and may sublimate and be released outside the system during polymerization depending on the polymerization equipment and conditions. Therefore, adding an excess of aromatic diol compensates for the released amount, preventing the structural units derived from the aromatic dicarboxylic acid monomer from being unevenly distributed at the terminal of the liquid crystal polyester resin, making it easier to control the generated gas components. The value of [aromatic diol] / [aromatic dicarboxylic acid] is more preferably 1.01 or more, and even more preferably 1.03 or more. Furthermore, from the viewpoint of polymerizability, it is more preferably 1.30 or less, and even more preferably 1.20 or less. Furthermore, when an aromatic diol is added in excess within the above-mentioned preferred range, the excess is released outside the system as the reaction proceeds, but the above-mentioned 2. When the reaction is carried out by the method described in 3. and 4., the aromatic diol is released from the system more efficiently, so that almost no unreacted aromatic diol remains in the liquid crystal polyester resin. When a plurality of monomers, such as hydroquinone and 4,4'-dihydroxybiphenyl, are used in combination as the aromatic diol, it is optional to select which monomer is charged in excess, but it is preferable to charge all of the aromatic diols in excess from the viewpoint of easy control of the amount of gas generated.
[0066] Regarding the above requirement 2, at a polymerization temperature of 230°C to 250°C, the reactivity of the acetylated aromatic diol monomer increases, while the rate of release of the acetylated aromatic diol monomer outside the system due to sublimation also increases. By setting the average temperature rise rate from 230°C to 250°C to 0.4°C / min or less, the acetylated aromatic diol monomer can be sufficiently reacted while suppressing release outside the system due to sublimation. This prevents the structural units derived from aromatic dicarboxylic acid monomers from being unevenly distributed at the terminals of the liquid crystal polyester resin, making it easier to control the gas components generated. The average temperature rise rate from 230°C to 250°C is more preferably 0.3°C / min or less, and even more preferably 0.2°C / min or less.
[0067] Regarding the above requirement 3, by controlling the reaction time above the melting point to 120 to 170 minutes, it is possible to remove unnecessary acetic acid from the polymerization system and promote the elimination of acetic acid from the acetyl terminal of the liquid crystal polyester resin, thereby reducing the acetic acid component in the liquid crystal polyester resin obtained after polymerization and making it easier to control the gas components generated. Furthermore, since the thermal decomposition of the liquid crystal polyester resin during polymerization can be suppressed, the increase in terminals and the increase in gas components associated with the inclusion of decomposition products can also be suppressed. The reaction time above the melting point is more preferably 130 minutes or more. Also, 160 minutes or less is preferred.
[0068] By satisfying two or more of the above requirements 1 to 3, it becomes easier to control the amount of gas generated to less than 300 ppm.
[0069] <Filler> The liquid crystal polyester resin of the present invention may be a liquid crystal polyester resin composition containing a filler to impart mechanical strength and other properties to the liquid crystal polyester resin. The filler used in the present invention is not particularly limited, and examples thereof include fibrous, whisker-like, plate-like, powdery, and granular fillers. Specific examples of fibrous or whisker-like fillers include glass fibers; PAN-based and pitch-based carbon fibers; metal fibers such as stainless steel fibers, aluminum fibers, and brass fibers; organic fibers such as aromatic polyamide fibers and liquid crystal polyester fibers; gypsum fibers, ceramic fibers, asbestos fibers, zirconia fibers, alumina fibers, silica fibers, titanium oxide fibers, silicon carbide fibers, rock wool, potassium titanate whiskers, barium titanate whiskers, aluminum borate whiskers, silicon nitride whiskers, and acicular titanium oxide. Examples of plate-like fillers include mica, talc, kaolin, glass flakes, clay, molybdenum disulfide, and wollastonite. Examples of powdery or granular fillers include silica, glass beads, titanium oxide, zinc oxide, calcium polyphosphate, and graphite. The surfaces of the fillers used in the present invention may be treated with a known coupling agent (e.g., a silane-based coupling agent, a titanate-based coupling agent, etc.) or other surface treatment agents. Two or more of the fillers used in the present invention may be used in combination.
[0070] Among the above fillers, glass fiber is preferably used because of its excellent mechanical strength, particularly tensile strength and bending strength, heat resistance, and dimensional stability. The type of glass fiber is not particularly limited as long as it is generally used to reinforce resins, and examples include long fiber type and short fiber type chopped strands and milled fiber. Furthermore, plate-shaped fillers are preferably used because of their excellent thin-wall flowability.
[0071] The surface of the filler may be treated with a known coupling agent (e.g., a silane coupling agent, a titanate coupling agent, etc.) or other surface treatment agent. The glass fibers may be coated or bundled with a thermoplastic resin such as an ethylene / vinyl acetate copolymer or a thermosetting resin such as an epoxy resin.
[0072] The liquid crystal polyester resin composition of the present invention may further contain conventional additives selected from antioxidants, heat stabilizers (e.g., hindered phenols, hydroquinone, phosphites, thioethers, and their substitution products), ultraviolet absorbers (e.g., resorcinol, salicylate), color inhibitors such as phosphites and hypophosphites, lubricants and mold release agents (montanic acid and its metal salts, its esters, its half esters, stearyl alcohol, stearamide, polyethylene wax, etc.), colorants including dyes or pigments, conductive agents or colorants such as carbon black, crystal nucleating agents, plasticizers, flame retardants (bromine-based flame retardants, phosphorus-based flame retardants, red phosphorus, silicone-based flame retardants, etc.), flame retardant assistants, and antistatic agents, within the range that does not impair the effects of the present invention.
[0073] In the liquid crystal polyester resin composition of the present invention, the content of the filler is preferably 10 to 200 parts by weight per 100 parts by weight of the liquid crystal polyester resin. If the content of the filler is 10 parts by weight or more, the mechanical strength of the molded article can be improved. The content of the filler is more preferably 15 parts by weight or more, and even more preferably 20 parts by weight or more. On the other hand, if the content of the filler is 200 parts by weight or less, a liquid crystal polyester resin composition having excellent moldability and thin-wall flowability and capable of easily injection-molding small, thin-walled molded articles can be obtained, which is preferable. The content of the filler is more preferably 150 parts by weight or less, and even more preferably 100 parts by weight or less.
[0074] Examples of methods for blending the filler and additives include a dry blending method in which a filler and other solid additives are blended with a liquid crystal polyester resin, a solution blending method in which a filler and other liquid additives are blended with a liquid crystal polyester resin, a method in which the filler and other additives are added during polymerization of the liquid crystal polyester resin, and a method in which the liquid crystal polyester resin and the filler and other additives are melt-kneaded. Among these, the melt-kneading method is preferred.
[0075] Known methods can be used for melt-kneading. Examples include a Banbury mixer, a rubber roll mill, a kneader, and a single-screw or twin-screw extruder. Twin-screw extruders are preferred. The melt-kneading temperature is preferably equal to or higher than the melting point of the liquid crystal polyester resin and equal to or lower than the melting point + 50°C.
[0076] Examples of the kneading method include: 1) a method in which the liquid crystal polyester resin, filler, and other additives are added all at once from a base-loading feeder and kneaded (lump-loading kneading method); 2) a method in which the liquid crystal polyester resin and other additives are added from a base-loading feeder and kneaded, and then the filler and other additives are added from a side feeder and kneaded (side feed method); and 3) a method in which a liquid crystal polyester composition (master pellets) containing a high concentration of the liquid crystal polyester resin and other additives is prepared, and then the master pellets are kneaded with the liquid crystal polyester resin and filler to a specified concentration (master pellet method).
[0077] <Molded Articles> The liquid crystal polyester resin and liquid crystal polyester resin composition of the present invention can be processed into molded articles having excellent surface appearance (color tone), mechanical properties, and heat resistance by conventional molding methods such as injection molding, extrusion molding, press molding, solution casting, and spinning. Examples of molded articles include injection molded articles, extrusion molded articles, press molded articles, sheets, pipes, various films such as unstretched films, uniaxially stretched films, and biaxially stretched films, and various fibers such as unstretched yarns and ultrastretched yarns. In particular, injection molded articles are preferred from the viewpoint of processability. When melt molding, melt molding is preferably performed at 370 ° C or less, more preferably 360 ° C or less, from the viewpoints of suppressing deterioration of the liquid crystal polyester resin and liquid crystal polyester resin composition, suppressing the generation of aromatic carboxylic acids and acetic acids generated when a molded article described below is maintained at 280 ° C, thereby improving flame retardancy, and improving mechanical strength.
[0078] The molded article of the present invention is a molded article comprising a liquid crystal polyester resin containing 20 to 80 mol% of structural units derived from aromatic hydroxycarboxylic acid, 10 to 40 mol% of structural units derived from aromatic diol, and 10 to 40 mol% of structural units derived from aromatic dicarboxylic acid, relative to 100 mol% of all structural units of the liquid crystal polyester resin. When the molded article is held at 280°C for 60 minutes under a reduced pressure of 13.3 kPa or less, the total amount of aromatic carboxylic acid and acetic acid generated is less than 100 ppm. The temperature of 280°C is close to the temperature during secondary processing, such as reflow treatment, and the temperature in the usage environment of the molded article. The low amount of gas generated at 280°C indicates that acid component gases are unlikely to be released during secondary processing or use, and indicates that the material has excellent processability and is suitable for long-term use.
[0079] As described above in the liquid crystal polyester resin section, by using a liquid crystal polyester resin in which the amount of gas generated, i.e., the amount of aromatic carboxylic acid and acetic acid generated when held at the melting point +20°C for 60 minutes under a reduced pressure of 13.3 kPa or less, is 300 ppm or less, gas generated during melt processing such as melt kneading and injection molding is reduced, and the gas components remaining in the molded product are reduced, making it possible to reduce the amount of aromatic carboxylic acid and acetic acid gas generated when held at 280°C to 100 ppm or less. Such molded products have excellent processability such as reflow and are suitable for long-term use, and also have excellent flame retardancy.
[0080] On the other hand, when a liquid crystal polyester resin with a gas generation rate of 300 ppm or more is used, a large amount of gas is generated during melt processing such as melt kneading and injection molding, and the amount of gas components remaining in the molded product increases.When the molded product is maintained at 280°C, the amount of aromatic carboxylic acid and acetic acid gas generated exceeds 100 ppm, which reduces processability such as reflow and deteriorates flame retardancy.
[0081] The amount of aromatic carboxylic acid and acetic acid generated when the molded article is maintained at 280° C. is more preferably 80 ppm or less, and most preferably 50 ppm or less, from the viewpoint of excellent flame retardancy.
[0082] The amount of aromatic carboxylic acid and acetic acid generated from the molded article is measured in the same manner as described in the liquid crystal polyester resin section, except that the temperature of the ceramic electric tubular furnace is set to 280° C. In the case of a liquid crystal polyester resin composition containing a filler, the amount of gas generated is calculated by converting it into the amount of gas generated from the liquid crystal polyester resin excluding the filler.
[0083] Molded articles obtained by molding the liquid crystal polyester resin and liquid crystal polyester resin composition of the present invention can be preferably used as electrical and electronic parts. Examples of electrical and electronic parts include flexible printed circuit boards, laminated circuit boards, printed wiring boards, and three-dimensional circuit boards used in antennas for mobile communication and electronic devices such as personal computers, GPS-equipped devices, mobile phones, and millimeter-wave and quasi-millimeter-wave radars such as collision prevention radars, tablets, and smartphones; lamp reflectors and lamp sockets for LEDs, small cells and microcell components for communication base stations of mobile communication terminals, antenna covers, housings, sensors, actuator parts for camera modules, connectors, relay cases and bases, switches, coil bobbins, and capacitors. In particular, because they can be molded over a wide range of molding temperatures and have little thickness dependency in flowability, they are useful for connectors with thin-walled complex shapes, relays, switches, coil bobbins, and actuator parts for camera modules.
[0084] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. In the examples, the composition and properties of the liquid crystal polyester resin were measured by the following methods.
[0085] (1) Composition analysis of liquid crystal polyester resin 2 μL of a 25% methanol solution of tetramethylammonium hydroxide was added to 0.1 mg of the pulverized liquid crystal polyester resin, and pyrolysis GC / MS measurement was performed using a Shimadzu GCMS-QP5050A to determine the content ratio of each structural unit in the liquid crystal polyester resin.
[0086] (2) Measurement of the melting point (Tm) of the liquid crystal polyester resin The endothermic peak temperature (Tm) observed when the liquid crystal polyester resin is heated from room temperature at a temperature increase rate of 20°C / min using a differential scanning calorimeter DSC-7 (manufactured by PerkinElmer) was measured. 1 ) after the observation of Tm 1 After holding at +20°C for 5 minutes, the sample was cooled to room temperature at a temperature decreasing rate of 20°C / min, and then heated again at a temperature increasing rate of 20°C / min. The endothermic peak temperature observed when the sample was heated was taken as the melting point (Tm).
[0087] (3) Melt Viscosity of Liquid Crystalline Polyester Resin Using a high-speed flow tester CFT-500D (orifice 0.5φ×10 mm) (manufactured by Shimadzu Corporation), the melt viscosity of the liquid crystal polyester resin was measured at Tm+20° C. and a shear rate of 1000 / s.
[0088] (4) Total Amount of Aromatic Carboxylic Acid and Acetic Acid Generated from Liquid Crystalline Polyester Resin Five grams of liquid crystal polyester resin was placed in the heated portion (A) of a glass ampoule tube shaped as shown in Figure 1 . A vacuum pump (ULVAC DTC-22) was used to evacuate the tip of the glass ampoule tube, maintaining the system at a reduced pressure of 13.3 kPa or less. The portion (B) 70 mm from the tip was heated and melted with a gas burner, sealing the tube, and preparing an ampule for analysis ( Figure 2 ). The heated portion (A) of the ampoule for analysis was maintained at a temperature of 20°C above the melting point of the liquid crystal polyester resin for 60 minutes using a ceramics electric tubular furnace (Asahi Rika Seisakusho ARF-30K (temperature controller AMF-N type)). The evolved gas was collected in the portion (C). The ampoule was removed from the ceramics electric tubular furnace and cooled to room temperature. The portion (C) was then cut out of the ampoule with a file. After weighing the cut-out (C) portion, all of the gas components condensed at the (C) portion were dissolved in deuterated dimethyl sulfoxide (0.8 g), and a small amount of 1,4-dioxane was added as an internal standard. The resulting solution was analyzed using a JNM-ECZ500R (manufactured by JEOL Ltd.). 1 H-NMR measurement was performed. In addition, the (C) portion from which the trapped components had been removed was washed with acetone, dried in a glass dryer at 60°C for 1 hour, and then reweighed. The total amount of evolved gas was calculated from the difference in weight of the (C) portion before and after removal of the trapped components. 1 From the H-NMR spectrum, the integral ratio of the peaks derived from aromatic carboxylic acids (terephthalic acid, isophthalic acid, benzoic acid), the peak derived from acetic acid, and the peak of the internal standard (1,4-dioxane) was determined. From this and the total amount of evolved gas, the total amount (ppm) of aromatic carboxylic acid and acetic acid evolved from the liquid crystal polyester resin was calculated. This total amount is shown in Table 2 as "amount of evolved gas."
[0089] (5) Amount of Fe Atoms 15 g of liquid crystal polyester resin was placed in a platinum crucible, sulfuric acid was added dropwise, and the resin was incinerated in an electric furnace at 500 °C. The resulting ash was dissolved in a 0.1 N nitric acid aqueous solution to obtain a dilute nitric acid acidic solution. The sample was measured by atomic absorption spectroscopy using an SPS4000 emission spectrometer (manufactured by SII NanoTechnology). The iron atom content was calculated from the peak intensity of the peak (238.204 nm) derived from iron atoms. In Table 2, the iron content contained in the liquid crystal polyester resin is referred to as "iron content (ppm)." The iron content contained in the raw material monomer described below was also measured using the same method. If the iron content was less than 0.1 ppm, it was marked as "not contained."
[0090] (6) Evaluation of drawing properties The liquid crystal polyester resin or liquid crystal polyester resin composition was dried at 150 ° C. for 3 hours using a hot air dryer, and then subjected to a TR30EHA injection molding machine (manufactured by Sodick) with a nozzle tip diameter of 1.4 mm. Under high temperature and high speed injection conditions, that is, the cylinder temperature was set to the melting point of the liquid crystal polyester resin + 30 ° C. (in the case of a liquid crystal polyester resin composition containing a filler, the melting point + 40 ° C.), the mold temperature was set to 90 ° C., and a mold capable of molding a molded product of width 5.0 mm x length 80 mm x thickness 0.2 mm was used, and the molding pressure was adjusted to a length of 80 mm. 50 shots were continuously molded under molding conditions of 45 MPa for 0.5 seconds, an injection speed of 200 mm / s, and a molding cycle of 13 seconds. When continuously molded under high temperature and high injection conditions such as these, gas generated accumulates in the cylinder. The cycle was then stopped, the nozzle was retracted, and the time (seconds) until the resin began to leak out from the nozzle tip was measured. The amount (g) of liquid crystal polyester resin leaking out from the nozzle tip in 10 seconds was then measured. In Table 2, the time (seconds) until the resin began to leak out is recorded as "drooling start time (s)," and the amount (g) of liquid crystal polyester resin leaking out from the nozzle tip in 10 seconds is recorded as "drooling amount (g)." The longer the dragging start time, the better, with 10 seconds or more being preferred. The smaller the dragging amount, the better, with less than 1 g being preferred.
[0091] (7) Evaluation of Flame Retardancy The liquid crystal polyester resin or liquid crystal polyester resin composition was dried at 150°C for 3 hours using a hot air dryer, and then subjected to a NEX1000 injection molding machine (manufactured by Nissei Plastics Industrial Co., Ltd.). The cylinder temperature was set to the melting point of the liquid crystal polyester resin + 10°C, the mold temperature was set to 90°C, and the injection speed was set to 100 mm / s. Five rectangular combustion test specimens measuring 13 mm wide, 125 mm long, and 0.38 mm thick were obtained. The five obtained combustion test specimens were used to evaluate flame retardancy according to the evaluation criteria specified in the UL94 vertical test. For each test specimen, the time from the first flame contact to the second flame contact until the fire extinguished was measured, and the total combustion time for the five test specimens was calculated as the combustion time. In Table 2, this is indicated as "combustion time (s)." The shorter the total combustion time ("combustion time (s)") of the five specimens, the better the flame retardancy, and a value of 50 seconds or less is preferable.
[0092] (8) Total amount of aromatic carboxylic acid and acetic acid generated from molded article 5 g of the molded article obtained by the method described in (7) was weighed, and the amount of aromatic carboxylic acid and acetic acid generated from the molded article (ppm) was calculated in the same manner as in (4) except that the heat treatment was changed to 280°C for 1 hour. In Tables 2 and 3, this is referred to as "amount of gas generated from molded article."
[0093] Example 1 A 5-L stainless steel reactor equipped with a stirring blade and a distillation tube was charged with 808 parts by weight of p-hydroxybenzoic acid (HBA), 88 parts by weight of 6-hydroxy-2-naphthoic acid (HNA), 229 parts by weight of 4,4'-dihydroxybiphenyl (DHB), 166 parts by weight of hydroquinone (HQ), 428 parts by weight of terephthalic acid (TPA), 19 parts by weight of isophthalic acid (IPA), and 1,288 parts by weight of acetic anhydride (1.07 equivalents of phenolic hydroxyl groups in total), and the mixture was reacted at 145°C for 120 minutes with stirring under a nitrogen gas atmosphere. The mixture was then heated from 145°C to 360°C over 320 minutes. The average heating rate from 230°C to 250°C was controlled to be 0.16°C / min. Thereafter, the polymerization temperature was maintained at 360°C, and the pressure was reduced to 1.0 torr (133 Pa) over 1.0 hour. The reaction was continued, and polymerization was completed when a predetermined stirring torque was reached. At this time, the reaction time at or above the melting point Tm of the liquid crystal polyester resin was 135 minutes. Next, the polymer was extruded into strands through a die having one circular discharge port with a diameter of 6 mm, and pelletized with a cutter to obtain liquid crystal polyester resin (A-1). Polymerization was carried out using raw materials in which the iron atoms contained in the monomers HBA, HNA, DHB, HQ, TPA, and IPA were 1, 1, 1, 0.1, 0.1, and 0.1 ppm, respectively. Furthermore, the value of the aforementioned [aromatic diol] / [aromatic dicarboxylic acid], which is the raw material charging ratio, is listed in Table 1 as "[diol] / [dicarboxylic acid]" (the same applies to Examples 2 to 10 and Comparative Examples 1 to 4).
[0094] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated using the method described in (4) above. The amounts of TPA, IPA, benzoic acid, and acetic acid generated were 44, 9, 15, and 11 ppm, respectively. In Table 2, these total amounts are shown as "gas generation amount" (the same applies to Examples 2 to 10 and Comparative Examples 1 to 4).
[0095] [Example 2] A liquid crystal polyester resin (A-2) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to 236 parts by weight of DHB and 169 parts by weight of HQ. The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated using the method described in (4) above. The amounts of TPA, IPA, benzoic acid, and acetic acid generated were 34, 9, 10, and 15 ppm, respectively.
[0096] [Example 3] A liquid crystal polyester resin (A-3) was obtained in the same manner as in Example 1, except that the temperature increase was controlled so that the average temperature increase rate from 230°C to 250°C was 0.50°C / min. The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated using the method described in (4) above. The amounts of TPA, IPA, benzoic acid, and acetic acid generated were 76, 13, 20, and 5 ppm, respectively.
[0097] [Example 4] A liquid crystal polyester resin (A-4) was obtained in the same manner as in Example 1, except that the amount of monomer charged was changed to 161 parts by weight of HQ. The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated using the method described in (4) above. As a result, the amounts of TPA, IPA, benzoic acid, and acetic acid generated were 83, 19, 22, and 25 ppm, respectively.
[0098] [Example 5] A liquid crystal polyester resin (A-5) was obtained in the same manner as in Example 1, except that 0.13 parts by weight of iron powder was further added when the monomers were charged. The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated using the method described in (4) above. As a result, the amounts of TPA, IPA, benzoic acid, and acetic acid generated were 110, 38, 38, and 23 ppm, respectively.
[0099] [Example 6] A liquid crystal polyester resin (A-6) was obtained in the same manner as in Example 1, except that a 5 L reaction vessel made of Hastelloy was used and polymerization was carried out using raw materials in which the iron atoms contained in the monomers HBA, HNA, DHB, HQ, TPA, and IPA were all less than 0.1 ppm. The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated using the method described in (4) above, and the amounts of TPA, IPA, benzoic acid, and acetic acid generated were 101, 31, 22, and 31 ppm, respectively.
[0100] Example 7 A liquid crystal polyester resin (A-7) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to 873 parts by weight of HBA and no HNA (0 parts by weight).
[0101] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated by the method described in (4) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 116, 48, 50 and 50 ppm, respectively.
[0102] The amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 40, 17, 17 and 17 ppm, respectively.
[0103] Example 8 A liquid crystal polyester resin (A-8) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to 369 parts by weight of TPA and 78 parts by weight of IPA.
[0104] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated by the method described in (4) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 34, 49, 33 and 25 ppm, respectively.
[0105] The amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above, and the amounts of TPA, IPA, benzoic acid, and acetic acid generated were 12, 17, 11, and 9 ppm, respectively.
[0106] Example 9 A liquid crystal polyester resin (A-9) was obtained in the same manner as in Example 1, except that the amounts of the monomers charged were changed to 447 parts by weight of TPA and no IPA (0 part by weight).
[0107] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated by the method described in (4) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 121, 0, 22 and 25 ppm, respectively.
[0108] The amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 44, 0, 8 and 9 ppm, respectively.
[0109] [Example 10] A liquid crystal polyester resin (A-10) was obtained in the same manner as in Example 1, except that the amount of monomers charged was changed to HBA 970 parts by weight, no HNA added (0 parts by weight), DHB 314 parts by weight, HQ 81 parts by weight, TPA 358 parts by weight, and IPA 31 parts by weight.
[0110] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated by the method described in (4) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 130, 50, 35 and 62 ppm, respectively.
[0111] The amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 42, 16, 11 and 20 ppm, respectively.
[0112] [Comparative Example 1] A 5L stainless steel reactor equipped with a stirring blade and a distillation tube was charged with 932 parts by weight of HBA, 293 parts by weight of DHB, 74 parts by weight of HQ, 344 parts by weight of TPA, 30 parts by weight of IPA, and 1228 parts by weight of acetic anhydride (1.07 equivalents of phenolic hydroxyl groups in total). The mixture was stirred under a nitrogen gas atmosphere at 145 ° C. for 150 minutes, and then heated from 145 ° C. to 360 ° C. over 240 minutes. At this time, the average heating rate from 230 ° C. to 250 ° C. was controlled to be 0.90 ° C. / min. Thereafter, the polymerization temperature was maintained at 360 ° C. and the pressure was reduced to 1.0 torr (133 Pa) over 1.0 hour. The reaction was further continued, and the polymerization was completed when the predetermined stirring torque was reached. At this time, the reaction time at or above the melting point Tm of the liquid crystal polyester resin was 135 minutes. The polymer was then extruded in the form of strands through a die having one circular outlet with a diameter of 6 mm and pelletized with a cutter to obtain a liquid crystal polyester resin (A'-11). The other conditions were the same as in Example 1.
[0113] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated by the method described in (4) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 160, 50, 50 and 96 ppm, respectively.
[0114] The amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 57, 18, 18 and 34 ppm, respectively.
[0115] Comparative Example 2 A liquid crystal polyester resin (A'-12) was obtained in the same manner as in Comparative Example 1, except that the reaction time at or above the melting point Tm of the liquid crystal polyester resin was changed to 175 minutes.
[0116] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated by the method described in (4) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 210, 65, 51 and 85 ppm, respectively.
[0117] The amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 73, 22, 17 and 29 ppm, respectively.
[0118] [Comparative Example 3] Liquid crystal polyester resin (A'-13) was obtained in the same manner as in Comparative Example 1, except that the amounts of the monomers charged were changed to 932 parts by weight of HBA, 251 parts by weight of DHB, 99 parts by weight of HQ, 284 parts by weight of TPA, and 90 parts by weight of IPA, and the reaction time at or above the melting point Tm of the liquid crystal polyester resin was changed to 175 minutes.
[0119] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated by the method described in (4) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 225, 100, 62 and 90 ppm, respectively.
[0120] The amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 80, 36, 22 and 32 ppm, respectively.
[0121] [Comparative Example 4] A liquid crystal polyester resin (A'-14) was obtained in the same manner as in Example 1, except that the amount of the monomer charged was 161 parts by weight of hydroquinone (HQ) and the temperature increase rate from 230°C to 250°C was controlled to be 0.50°C / min.
[0122] The amounts of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin were calculated by the method described in (4) above, and the amounts of TPA, IPA, benzoic acid and acetic acid generated were 189, 11, 58 and 79 ppm, respectively.
[0123] The amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above, and the amounts of TPA, IPA, benzoic acid, and acetic acid generated were 61, 4, 19, and 26 ppm, respectively.
[0124] The liquid crystal polyester resins obtained in Examples 1 to 10 and Comparative Examples 1 to 4 were evaluated in the above items (1) to (8), and the results are shown in Tables 1 and 2.
[0125]
[0126]
[0127] Liquid crystal polyester resin compositions were prepared by further adding a filler to the liquid crystal polyester resin obtained in Example 1 and Comparative Example 1. The fillers used in each of the Examples and Comparative Examples are shown below.
[0128] Filler (B) (B-1) Milled fiber (40M-10A) manufactured by Nippon Electric Glass Co., Ltd. [Example 11, Comparative Example 5] In a Toshiba Machine TEM35B type twin-screw extruder equipped with a side feeder, the liquid crystal polyester resins (A-1, A'-11) obtained in each production example were charged from the hopper in the amounts shown in Table 3, and the filler (B-1) was charged from the side feeder in the amounts shown in Table 3, and the cylinder temperature was set to the melting point of the liquid crystal polyester resin + 10 ° C., and melt-kneaded to obtain pellets. The resulting pellets of the liquid crystal polyester resin composition were dried with hot air and evaluated in the same manner as in (6) and (7), and the results are shown in Table 3.
[0129] For Example 11, the amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated by the method described in (8) above. As a result, the amounts of TPA, IPA, benzoic acid, and acetic acid generated were 16, 4, 5, and 7 ppm, respectively.
[0130] For Comparative Example 5, the amounts of aromatic carboxylic acid and acetic acid generated from the molded article were calculated using the method described in (8) above. As a result, the amounts of TPA, IPA, benzoic acid, and acetic acid generated were 60, 23, 25, and 45 ppm, respectively.
[0131]
[0132] From the results in Tables 1 to 3, it can be seen that by using a liquid crystal polyester resin having a total amount of aromatic carboxylic acid and acetic acid of 300 ppm or less, or a liquid crystal polyester resin composition using such a resin, the total amount of aromatic carboxylic acid and acetic acid generated from a molded article at 280°C is 100 ppm or less, drowning is suppressed, and a liquid crystal polyester resin, resin composition, and molded article having excellent flame retardancy can be obtained.
[0133] The liquid crystal polyester resin and liquid crystal polyester resin composition of the present invention have excellent flame retardancy and suppressed drooling during injection molding, and therefore can be suitably used for connectors, relays, switches, coil bobbins, and actuator parts for camera modules, and are particularly suitable for connectors, which have become increasingly thin-walled and fine-pitch in recent years.
[0134] (A) Pellets sealing and heating area (B) Sealed tube area (C) Evolved gas collection area (D) Liquid crystal polyester resin pellets
Claims
1. A liquid crystal polyester resin containing 20 to 80 mol % of structural units derived from aromatic hydroxycarboxylic acid, 10 to 40 mol % of structural units derived from aromatic diol, and 10 to 40 mol % of structural units derived from aromatic dicarboxylic acid, based on 100 mol % of all structural units of the liquid crystal polyester resin, and satisfying the following requirement (α): Requirement (α): When held for 60 minutes at a temperature of melting point Tm + 20°C under a reduced pressure of 13.3 kPa or less, the total amount of aromatic carboxylic acid and acetic acid generated from the liquid crystal polyester resin is less than 300 ppm; The melting point Tm of the liquid crystal polyester resin is the endothermic peak temperature (Tm) observed when the liquid crystal polyester resin is heated from room temperature at a temperature increase of 20°C / min in differential calorimetry. 1 ) after the observation of Tm 1 This is the endothermic peak temperature observed when the sample is held at +20° C. for 5 minutes, cooled to room temperature at a temperature drop rate of 20° C. / min, and then heated again at a temperature rise rate of 20° C. / min.
2. The liquid crystal polyester resin according to claim 1, which contains 0.1 to 100 ppm of iron atoms.
3. A liquid crystal polyester resin according to claims 1 and 2, which contains the following structural unit (I) and satisfies the following formula (a): 2≦[I]≦20 ... (a) [I] indicates the content (mol %) of each of the following structural units (I) relative to 100 mol % of all structural units in the liquid crystal polyester resin.
4. A liquid crystal polyester resin according to claims 1 to 3, which contains the following structural units (I) and (II), and satisfies the following formulas (b) and (c): 0.01≦[II]≦5...(b) [II] / [I]<1...(c) [I] and [II] indicate the content (mol %) of each of the following structural units (I) and (II) relative to 100 mol % of all structural units in the liquid crystal polyester resin.
5. A liquid crystal polyester resin according to any one of claims 1 to 4, which comprises the following structural units (II) and (III) and satisfies the following formula (d): 0.92<[III] / ([II]+[III])<1 ... (d) [II] and [III] represent the content (mol %) of each of the following structural units (II) and (III) relative to 100 mol % of all structural units in the liquid crystal polyester resin.
6. A method for producing a liquid crystal polyester resin according to any one of claims 1 to 5, comprising reacting a hydroxycarboxylic acid and / or a diol with acetic anhydride to acetylate at least a portion of the phenolic hydroxyl groups, followed by deacetylation polymerization with a dicarboxylic acid, wherein the ratio of raw material monomers charged satisfies the following formula (e): 1<[aromatic diol] / [aromatic dicarboxylic acid]<1.5 ... (e) [Aromatic diol] and [aromatic dicarboxylic acid] represent the amounts (moles) of the aromatic diol and aromatic dicarboxylic acid charged during the production of the liquid crystal polyester resin.
7. A liquid crystal polyester resin composition comprising 10 to 200 parts by weight of a filler based on 100 parts by weight of the liquid crystal polyester resin according to any one of claims 1 to 5.
8. A molded article comprising the liquid crystal polyester resin according to any one of claims 1 to 5, or the liquid crystal polyester resin composition according to claim 7.
9. The molded article according to claim 8, which is any one selected from the group consisting of a connector, a relay, a switch, a coil bobbin, and an actuator part of a camera module.
10. A molded article containing a liquid crystal polyester resin that contains 20 to 80 mol % of structural units derived from aromatic hydroxycarboxylic acid, 10 to 40 mol % of structural units derived from aromatic diol, and 10 to 40 mol % of structural units derived from aromatic dicarboxylic acid, relative to 100 mol % of all structural units of the liquid crystal polyester resin, and the total amount of aromatic carboxylic acid and acetic acid generated when the molded article is held at 280°C for 60 minutes under a reduced pressure of 13.3 kPa or less is less than 100 ppm.
Citation Information
Patent Citations
Liquid crystalline resin, method for producing the same, liquid crystalline resin composition and molded product
JP2006089714A
Wholly aromatic polyester and polyester resin composition
JP2009127025A
Wholly aromatic liquid crystal polyester and method for manufacturing same
WO2012090407A1
Wholly aromatic liquid-crystal polyester resin
WO2018101214A1
Method for preparing full-aromatic polyester
CN101210068A