Etching liquid and method for manufacturing semiconductor device
The etching solution, featuring a quinone compound and hydroquinone in a controlled solvent and pH environment, addresses the challenge of balancing etching speed and surface roughness for molybdenum-containing materials, ensuring effective semiconductor device manufacturing.
Patent Information
- Application Number
- PCT/JP2024/016882
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-02
- Publication Date
- 2024-11-28
AI Technical Summary
Current etching solutions for molybdenum-containing materials fail to achieve a balance between high etching speed and surface roughness suppression, particularly in semiconductor device manufacturing.
An etching solution comprising a quinone compound with a quinone structure, a solvent that includes water or a water-soluble organic solvent, and a hydroquinone compound, with specific concentrations and pH control, is used to enhance etching rate and reduce surface roughness.
The solution provides an excellent etching rate while effectively suppressing surface roughness of molybdenum-containing materials, making it suitable for semiconductor device manufacturing.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Etching solution, semiconductor device manufacturing method
[0001] The present invention relates to an etching solution and a method for manufacturing a semiconductor device.
[0002] As electronic devices become increasingly miniaturized, there is an increasing demand for efficient and highly accurate etching processes for removing unwanted metal inclusions from substrates in the electronic device manufacturing process.
[0003] For example, Patent Document 1 discloses an etching solution for etching a two-layer film of copper and molybdenum, which contains hydrogen peroxide, an acidic substance, an amine compound, a hydrogen peroxide decomposition inhibitor, and molybdenum erosion-promoting ions.
[0004] Japanese Patent Application Laid-Open No. 2022-052909
[0005] The present inventors have investigated the etching of a molybdenum-containing material using the etching solution disclosed in the above document, and have found that it is not possible to achieve both a high etching rate and suppression of surface roughness of the molybdenum-containing material after etching treatment, and that there is room for further improvement.
[0006] Therefore, an object of the present invention is to provide an etching solution that has an excellent etching rate and can suppress roughness of the surface of a molybdenum-containing material after etching. Another object of the present invention is to provide a method for manufacturing a semiconductor device using the etching solution.
[0007] As a result of extensive research into solving the above problems, the present inventors have found that the problems can be solved by the following configuration.
[0008] [1] An etching solution for use with a molybdenum-containing material, comprising a quinone compound having a quinone structure and a solvent. [2] The etching solution according to [1], wherein the solvent comprises at least one selected from the group consisting of water and water-soluble organic solvents. [3] The etching solution according to [1] or [2], wherein the content of the quinone compound is 0.0001 to 10.0 mass% relative to the total mass of the etching solution. [4] The etching solution according to any one of [1] to [3], wherein the quinone compound is a compound represented by formula (1) described below. [5] The etching solution according to any one of [1] to [3], wherein the quinone compound is a compound represented by formula (1) 1 and R 2 do not bond to each other to form a benzene ring, and R 3 and R 4The etching solution according to [4], wherein the quinone compound is a compound represented by formula (1) above, in which the quinone compounds are not bonded to each other to form a benzene ring. [6] The etching solution according to any one of [1] to [5], wherein the quinone compound includes at least one selected from the group consisting of p-benzoquinone, p-chloranil, fluoranil, 2,3-dichloro-5,6-dicyano-p-benzoquinone, chloranilic acid, and tetrahydroxy-1,4-benzoquinone. [7] The etching solution according to any one of [1] to [6], further including a hydroquinone compound having a p-hydroquinone structure, wherein the content of the hydroquinone compound is 1 ppt by mass to 1 ppm by mass relative to the total mass of the etching solution. [8] The etching solution according to any one of [1] to [7], wherein the amount of dissolved oxygen is 3 to 50 mg / L. [9] The etching solution according to any one of [1] to [8], wherein the relative dielectric constant at 20°C of the solvent is 7 to 75.
[10] The etching solution according to any one of [1] to [9], wherein the solvent contains water and a water-soluble organic solvent, and the content of the water is 20 to 95 mass% based on the total mass of the solvent.
[11] The etching solution according to any one of [1] to
[10] , wherein the solvent contains at least one selected from the group consisting of water, methanol, ethanol, 1-propanol, 2-propanol, dimethyl sulfoxide, sulfolane, N,N-dimethylformamide, N-methylpyrrolidone, pyridine, acetonitrile, acetone, tetrahydrofuran, and glycerin.
[12] The etching solution according to any one of [1] to
[11] , wherein the solvent contains at least one selected from the group consisting of water, alcohol solvents, sulfoxide solvents, nitrile solvents, and sulfone solvents.
[13] The etching solution according to any one of [1] to
[12] , further containing a surfactant.
[14] The etching solution according to any one of [1] to
[13] , wherein the content of Cr atoms is 1 ppt by mass to 1 ppb by mass relative to the total mass of the etching solution.
[15] The etching solution according to any one of [1] to
[14] , wherein the pH is 3 to 10.
[16] A method for manufacturing a semiconductor device, comprising the step of etching the molybdenum-containing material using the etching solution according to any one of [1] to
[15] .
[0009] According to the present invention, there is provided an etching solution which has an excellent etching rate and can suppress roughening of the surface of a molybdenum-containing material after etching. The present invention also provides a method for manufacturing a semiconductor device using the etching solution.
[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.
[0011] In this specification, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the upper and lower limits. In this specification, in numerical ranges described in stages, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. In this specification, a combination of two or more preferred embodiments is a more preferred embodiment. Furthermore, in this specification, when two or more types of a certain component are present, the "content" of that component means the total content of those two or more components.
[0012] In this specification, when there are a plurality of substituents, linking groups, etc. (hereinafter referred to as "substituents, etc.") represented by a specific symbol, or when a plurality of substituents, etc. are simultaneously specified, it means that the respective substituents, etc. may be the same or different from each other. This also applies to the specification of the number of substituents, etc.
[0013] As used herein, "ppm" means "parts-per-million (10 -6 ) and "ppb" stands for "parts-per-billion (10 -9 ) and "ppt" stands for "parts-per-trillion (10-12 )." In this specification, "Å" corresponds to 0.1 nm.
[0014] [Etching Solution] The etching solution of the present invention (hereinafter also simply referred to as "etching solution") will be described in detail below. The etching solution of the present invention is used for a molybdenum-containing material and contains a quinone compound having a quinone structure and a solvent.
[0015] Although the reason why the etching solution having the above-described configuration can solve the problems of the present invention is not entirely clear, the inventors speculate as follows. The following speculation does not limit the mechanism by which the effect is obtained. In other words, mechanisms other than those described below are also within the scope of the present invention. When etching a molybdenum-containing material, depending on the oxidizing agent, the etching solution may penetrate into the grain boundaries of the molybdenum-containing material, removing the grains individually, which can cause surface roughness after etching. The etching solution of the present invention uses a quinone compound as an oxidizing agent for the molybdenum-containing material. Because the quinone compound has a quinone structure that can coordinate to the surface of the molybdenum-containing material, it can quickly oxidize the surface of the molybdenum-containing material and achieve an excellent etching rate. Furthermore, the coordination of the quinone compound to the surface of the molybdenum-containing material temporarily protects the oxide layer, preventing the etching solution from penetrating into the grain boundaries, allowing a uniform oxide film to be formed, and reducing surface roughness of the molybdenum-containing material after etching. As a result, the etching solution of the present invention is thought to be able to achieve both a high etching rate and reduced surface roughness of the molybdenum-containing material after etching. The property of being able to suppress roughness of the surface of a molybdenum-containing material after etching is also referred to simply as "suppression of surface roughness," and superiority in at least one of the etching rate and the suppression of surface roughness is also referred to as "superior effect of the present invention."
[0016] [Quinone Compound] The etching solution contains a quinone compound, which is a compound having a quinone structure. The quinone compound is not particularly limited as long as it has a quinone structure as the entire structure or a partial structure of the compound. Examples of the quinone structure include a structure in which two carbon atoms in an aromatic ring are substituted with carbonyl carbons (C═O), and may also be a non-benzene-based quinone structure (for example, a quinone structure composed of a 7-membered ring, a 10-membered ring, a 5-membered ring, or a 12-membered ring). The aromatic ring may be either an aromatic hydrocarbon ring or an aromatic heterocyclic ring, with an aromatic hydrocarbon ring being preferred. The aromatic ring may be either a monocyclic or polycyclic ring, with a monocyclic ring being preferred. The number of carbon atoms in the aromatic ring is preferably 5 to 20, more preferably 6 to 12. The quinone structure is preferably a benzene-based quinone structure, more preferably a benzoquinone structure, a naphthoquinone structure, or an anthraquinone structure, and even more preferably a benzoquinone structure. The positions of the two carbonyl groups in the quinone structure are not particularly limited, and for example, when the quinone compound has a benzoquinone structure, the benzoquinone structure may be either a 1,2-benzoquinone structure (orthobenzoquinone structure) or a 1,4-benzoquinone structure (parabenzoquinone structure). When the quinone compound has a benzoquinone structure, it is particularly preferred that it has a parabenzoquinone structure. The molecular weight of the quinone compound is not particularly limited, but is preferably 50 to 500, and more preferably 100 to 300.
[0017] The quinone compound is also preferably a compound represented by formula (1).
[0018]
[0019] In formula (1), R 1 ~R 4each independently represents a hydrogen atom or a substituent. Examples of the substituent include an alkyl group, an alkenyl group, an aryl group, a hydroxy group, a carbonyl group, a cyano group, a halogen atom, an alkoxy group, an aryloxy group, an alkyloxycarbonyl group, a nitro group, a fluoroalkyl group, and an amino group. The alkyl group and alkoxy group preferably have 1 to 20 carbon atoms, more preferably 1 to 12, and even more preferably 1 to 6. The aryl group and aryloxy group preferably have 5 to 20 carbon atoms, more preferably 6 to 12. The alkyloxycarbonyl group preferably has 2 to 21 carbon atoms, more preferably 2 to 13, and even more preferably 2 to 7. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, with a fluorine atom or a chlorine atom being preferred. The fluoroalkyl group is an alkyl group substituted with at least one fluorine atom, and may be a perfluoroalkyl group. R 1 ~R 4 Among these, a hydrogen atom, an alkyl group, a hydroxy group, a cyano group, or a halogen atom is preferable.
[0020] R 1 and R 2 may be bonded to each other to form a benzene ring which may have a substituent, R 3 and R 4 may be bonded to each other to form a benzene ring which may have a substituent. 1 and R 2 do not bond to each other to form a benzene ring, and R 3 and R 4 It is also preferable that they do not bond to each other to form a benzene ring. The substituents that the benzene ring may have include the above-mentioned R 1 ~R 4 Examples of the group represented by the formula (I) include the substituents exemplified above.
[0021] Examples of quinone compounds represented by formula (1) include p-benzoquinone, p-chloranil, p-fluoranil (fluoranil), p-bromanil (bromanil), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone (DDQ), chloranilic acid, tetrahydroxy-1,4-benzoquinone (tetrahydroxybenzoquinone), ubiquinone, toluquinone, 2,6-dimethyl-1,4-benzoquinone, 2,5-dimethyl-1,4-benzoquinone, 1,4-naphthoquinone, and anthraquinone. Examples of quinone compounds other than those mentioned above include 1,2-benzoquinone, 3,5-di-tert-butyl-1,2-benzoquinone, o-chloranil, o-fluoranil, o-bromanil, 1,2-naphthoquinone, o-pleiadienequinone, and acenaphthenequinone. Of these, the quinone compound is preferably p-benzoquinone, p-chloranil, fluoranil, DDQ, chloranilic acid, tetrahydroxybenzoquinone, o-chloranil, 3,5-di-tert-butyl-1,2-benzoquinone, 1,4-naphthoquinone, or anthraquinone, more preferably p-benzoquinone, p-chloranil, fluoranil, DDQ, chloranilic acid, tetrahydroxybenzoquinone, o-chloranil, 1,4-naphthoquinone, or anthraquinone, still more preferably p-benzoquinone, p-chloranil, fluoranil, DDQ, chloranilic acid, or tetrahydroxybenzoquinone, and particularly preferably p-benzoquinone, p-chloranil, fluoranil, chloranilic acid, or tetrahydroxybenzoquinone.
[0022] The quinone compound may be used alone or in combination of two or more. In order to obtain a more excellent effect of the present invention, the content of the quinone compound is preferably 0.000005 to 20.0 mass%, more preferably 0.0001 to 10.0 mass%, still more preferably 0.001 to 10.0 mass%, and particularly preferably 0.01 to 1.0 mass%, relative to the total mass of the etching solution.
[0023] [Solvent] The etching solution contains a solvent. The solvent is not particularly limited as long as it can dissolve the quinone compound, and examples thereof include water, organic solvents, and mixtures thereof. Preferably, the etching solution contains at least one solvent selected from the group consisting of water and water-soluble organic solvents. The water-soluble organic solvent refers to an organic solvent having a solubility in water at 25°C of 50 g / L or more. The water-soluble organic solvent is preferably miscible with water at any ratio.
[0024] The relative dielectric constant of the solvent is preferably 5 to 90, more preferably 7 to 75, even more preferably 20 to 75, particularly preferably 24 to 75, and most preferably 50 to 75, in terms of achieving superior effects of the present invention. The relative dielectric constant is preferably within the above range at 15 to 30°C, and more preferably within the above range at 20°C. Known literature values can be used as the relative dielectric constant. The literature values can be values found in "Chemistry Handbook, Basics II, Revised 5th Edition" (Maruzen Co., Ltd., 2004). If no literature value is found, the CRC Handbook of Chemistry and Physics can be referenced. If no known literature value is found, a value measured by a known method can be used. Examples of methods for measuring the dielectric constant include a method in which 50 mL of solvent is prepared as a measurement sample adjusted to a predetermined temperature, and an AC voltage of 1 MHz is applied using a Keycom E4980A precision LCR meter and a Keycom DPT-013-050 electrode, and a method in which the dielectric constant is measured using a Mitsuwa Frontech Model 871. When a mixed solvent containing two or more solvents is used, the above-mentioned literature value can be used as the dielectric constant. If no literature value is available, the value measured for the mixed solvent using the above-mentioned method can be used.
[0025] Examples of the solvent include water, alcohol solvents, sulfoxide solvents, sulfone solvents, nitrile solvents, amide solvents, amine solvents, ketone solvents, ester solvents, ether solvents, carboxylic acid solvents, hydrocarbon solvents, and halogen-based solvents. The solvent preferably contains at least one selected from the group consisting of water, alcohol solvents, sulfoxide solvents, sulfone solvents, nitrile solvents, amide solvents, amine solvents, ketone solvents, ether solvents, ester solvents, and halogen-based solvents, more preferably contains at least one selected from the group consisting of water, alcohol solvents, sulfoxide solvents, sulfone solvents, amide solvents, nitrile solvents, and ketone solvents, still more preferably contains at least one selected from the group consisting of water, alcohol solvents, sulfoxide solvents, sulfone solvents, and nitrile solvents, and particularly preferably contains at least one selected from the group consisting of water and alcohol solvents. Furthermore, when the relative dielectric constant of the solvent is 24 or more, the organic solvent is preferably an alcohol solvent, a sulfoxide solvent, a sulfone solvent, a ketone solvent, an ether solvent, an ester solvent, a nitrile solvent, or a halogen-based solvent, and more preferably an alcohol solvent, a sulfoxide solvent, a sulfone solvent, a ketone solvent, an ether solvent, or an ester solvent.
[0026] The alcohol solvent may be either a monool solvent having one hydroxy group or a polyol solvent having two or more hydroxy groups, but a monool solvent is preferred. The number of carbon atoms in the alcohol solvent is preferably 1 to 12, more preferably 1 to 6, and even more preferably 1 or 2. Examples of monool solvents include methanol, ethanol, 1-propanol, 2-propanol, t-butyl alcohol, 1-butanol, 2-butanol, isobutyl alcohol, 2-pentanol, t-pentyl alcohol, hexanol, 3-methoxy-3-methyl-1-butanol (MMB), 3-methoxy-1-butanol, 1-methoxy-2-butanol, allyl alcohol, propargyl alcohol, 2-butenyl alcohol, 3-butenyl alcohol, 4-penten-2-ol, tetrahydrofurfuryl alcohol, furfuryl alcohol, and benzyl alcohol. Methanol, ethanol, 1-propanol, 2-propanol, t-butyl alcohol, 1-butanol, 2-butanol, or isobutyl alcohol is preferred, and methanol or ethanol is more preferred. Examples of polyol solvents include glycerin, ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, 2-methyl-1,3-propanediol, 1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 2,3-butanediol, hexylene glycol, pinacol, and 1,3-cyclopentanediol.
[0027] Sulfoxide solvents include, for example, dimethyl sulfoxide (DMSO).
[0028] Examples of sulfone solvents include sulfolane, 3-methylsulfolane, and 2,4-dimethylsulfolane.
[0029] An example of the nitrile solvent is acetonitrile.
[0030] Examples of amide solvents include N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), 1-methyl-2-pyrrolidone, 2-pyrrolidinone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, formamide, N-methylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropanamide, and hexamethylphosphoric triamide.
[0031] Examples of the amine solvent include pyridine, triethylamine, and diethylamine.
[0032] Examples of ketone solvents include acetone, dimethyl ketone (propanone), cyclobutanone, cyclopentanone, cyclohexanone, methyl ethyl ketone (2-butanone), 5-hexanedione, methyl isobutyl ketone, 1,4-cyclohexanedione, 1,3-cyclohexanedione, and cyclohexanone.
[0033] Examples of ester solvents include chain esters such as ethyl acetate, butyl acetate, ethyl lactate, methyl 3-methoxypropanoate, propylene glycol monomethyl ether acetate, ethylene glycol monoacetate, diethylene glycol monoacetate, ethylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol diacetate, and propylene glycol diacetate, and cyclic esters such as propylene carbonate, ethylene carbonate, and diethyl carbonate.
[0034] Examples of the ether solvent include dialkyl ethers such as diethyl ether, diisopropyl ether, dibutyl ether, t-butyl methyl ether, and cyclohexyl methyl ether; glycol ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, tetraethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, triethylene glycol diethyl ether, tetraethylene glycol diethyl ether, ethylene glycol dimethyl ether, triethylene glycol dimethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol propyl ether, diethylene glycol monobutyl ether, diethylene glycol monoethyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, and triethylene glycol monobutyl ether; and cyclic ethers such as tetrahydrofuran and 1,4-dioxane.
[0035] Carboxylic acid solvents include, for example, formic acid, acetic acid, and propionic acid.
[0036] Examples of hydrocarbon solvents include aliphatic hydrocarbon solvents such as hexane, heptane, pentane, octane, cyclohexane, methylcyclohexane, cyclopentane, and methylcyclopentane, and aromatic hydrocarbon solvents such as toluene, xylene, and ethylbenzene.
[0037] Examples of halogen-based solvents include chloroform, dichloromethane, tetrachloroethylene, and 1-bromopropane.
[0038] Among these, the solvent preferably contains at least one selected from the group consisting of water, methanol, ethanol, 1-propanol, 2-propanol, DMSO, sulfolane, DMF, NMP, pyridine, acetonitrile, acetone, glycerin, and THF, more preferably contains at least one selected from the group consisting of water, methanol, ethanol, 1-propanol, 2-propanol, DMSO, sulfolane, DMF, NMP, acetonitrile, acetone, THF, and glycerin, still more preferably contains at least one selected from the group consisting of water, methanol, ethanol, DMSO, sulfolane, acetonitrile, and glycerin, and particularly preferably contains at least one selected from the group consisting of water, methanol, and ethanol.
[0039] The solvent may be used alone or in combination of two or more. When two or more solvents are used in combination, water and a water-soluble organic solvent may be used in combination, or two or more organic solvents may be used in combination. In order to achieve better effects of the present invention, the content of the solvent is preferably 60.0 mass% or more, more preferably 80.0 mass% or more, even more preferably 90.0 mass% or more, and particularly preferably 99.0 mass% or more, relative to the total mass of the etching solution. The upper limit is less than 100 mass%, preferably 99.999 mass% or less, more preferably 99.99 mass% or less, and even more preferably 99.97 mass% or less. When the solvent contains water and a water-soluble organic solvent, in order to achieve better effects of the present invention, the content of water is preferably 10 to 99 mass%, more preferably 20 to 95 mass%, and even more preferably 40 to 90 mass%, relative to the total mass of the solvent.
[0040] [Surfactant] In order to obtain a more excellent effect of the present invention, it is preferable that the etching solution contains a surfactant. The surfactant is not particularly limited as long as it is a compound having a hydrophilic group and a hydrophobic group (lipophilic group) in one molecule, and examples thereof include nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants, with nonionic surfactants being preferred.
[0041] Surfactants often have at least one hydrophobic group selected from the group consisting of an aliphatic hydrocarbon group, an aromatic hydrocarbon group, and a combination thereof. When the hydrophobic group contains an aromatic hydrocarbon group, the number of carbon atoms in the hydrophobic group of the surfactant is preferably 6 or more, more preferably 10 or more. There is no particular upper limit, but it is often 20 or less. When the hydrophobic group consists solely of an aliphatic hydrocarbon group, the number of carbon atoms in the hydrophobic group of the surfactant is preferably 9 or more, more preferably 13 or more, and even more preferably 16 or more. There is no particular upper limit, but it is often 30 or less. The total number of carbon atoms in the surfactant is preferably 10 to 100.
[0042] Examples of nonionic surfactants include ester-type nonionic surfactants such as sorbitan fatty acid esters and glycerin fatty acid esters, ether-type nonionic surfactants such as polyoxyalkylene alkyl ethers, polyoxyalkylene alkenyl ethers, and polyoxyethylene alkylphenyl ethers, ester-ether-type nonionic surfactants such as polyoxyalkylene monoalkylates, polyoxyalkylene dialkylates, and polyoxyethylene sorbitan fatty acid esters, alkanolamine-type nonionic surfactants, alkylamine ether-type surfactants such as polyoxyethylene alkylamines, alkylamide ether-type surfactants such as bispolyoxyalkylene alkylamides, polyoxyalkylene glycol-type surfactants, oxyethylene oxypropylene block copolymers, and acetylene glycol-type nonionic surfactants. Polyoxyalkylene alkyl ethers, polyoxyalkylene monoalkylates, polyoxyalkylene dialkylates, polyoxyalkylene glycol-type surfactants, and acetylene glycol-type nonionic surfactants are preferred, and acetylene glycol-type nonionic surfactants are more preferred.
[0043] As the nonionic surfactant, for example, a nonionic surfactant represented by formula (S-1) is preferred.
[0044]
[0045] Rs1 and R s2 R each independently represents a hydrogen atom, an alkyl group which may have a substituent, or a phenyl group which may have a substituent. The alkyl group may be linear, branched, or cyclic, and is preferably linear. The alkyl group preferably has 1 to 6 carbon atoms, more preferably 1 to 4 carbon atoms. Examples of substituents that the alkyl group and phenyl group may have include an alkyl group (preferably having 1 to 3 carbon atoms), an alkoxy group (preferably having 1 to 3 carbon atoms), and a halogen atom. s1 and R s2 is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom.
[0046] R s3 and R s4 R each independently represents an alkylene group having 1 to 6 carbon atoms. The alkylene group having 1 to 6 carbon atoms may be linear, branched, or cyclic, and is preferably linear. The alkylene group preferably has 1 to 4 carbon atoms, more preferably 2 to 3 carbon atoms. s3 and R s4 If there are multiple R s3 and R s4 may be the same or different.
[0047] R s5 ~R s8 each independently represents an alkyl group having 1 to 18 carbon atoms which may have a substituent. The alkyl group may be linear, branched, or cyclic, but is preferably linear or branched. The alkyl group preferably has 1 to 12 carbon atoms, more preferably 1 to 6 carbon atoms. Examples of the substituent that the alkyl group may have include an alkyl group (preferably having 1 to 3 carbon atoms), an alkoxy group (preferably having 1 to 3 carbon atoms), a phenyl group, and a halogen atom. Examples of the alkyl group include a methyl group, an ethyl group, an n-butyl group, a 2-methylpropyl group, a 2-methylbutyl group, and a 2,4-dimethylpentyl group. R s5 ~R s8Among these, a linear alkyl group having 1 to 4 carbon atoms or a branched alkyl group having 3 to 6 carbon atoms is preferred.
[0048] m1 and m2 each independently represent an integer of 0 to 30, preferably an integer of 0 to 10, and more preferably an integer of 0 to 5. m1+m2 represents an integer of 0 to 60, preferably an integer of 0 to 40, and more preferably an integer of 0 to 10.
[0049] It is also preferable that the nonionic surfactant represented by formula (S-1) has a bilaterally symmetric structure. s1 and R s2 are the same, and R s3 and R s4 are the same, and R s5 and R s6 are the same, and R s7 and R s8 In this case, m1 and m2 may be the same or different, but are preferably the same.
[0050] The specific gravity of the nonionic surfactant is 0.80 to 1.20 g / cm 3 is preferably 0.95 to 1.10 g / cm 3 is more preferable. The HLB (Hydrophile-Lipophile Balance) value of the nonionic surfactant is preferably 1 to 18, more preferably 2 to 10. The HLB value is defined as a value calculated using the Griffin equation (20 x Mw / M; Mw = molecular weight of the hydrophilic moiety, M = molecular weight of the nonionic surfactant), and catalog values or values calculated by other methods may also be used. The closer the HLB value is to 20, the more hydrophilic the surfactant is, and the closer it is to 0, the more lipophilic the surfactant is. The static surface tension of a 0.1% by mass aqueous solution of the nonionic surfactant at 23°C is preferably 10 to 55 mN / m, more preferably 25 to 40 mN / m. The static surface tension can be measured using a known method.
[0051] Examples of acetylene glycol-based nonionic surfactants include the "Surfynol 104 series" such as Surfynol 104E (2,4,7,9-tetramethyl-5-decyne-4,7-diol, specific gravity 1.00, HLB value 4), 104H, 104A, 104PA, and 104PG-50; Surfynol 420 and 440 (ethoxylated 2,4,7,9-tetramethyl-5-decyne-4,7-diol (addition mole number of ethylene oxide 3.5), specific gravity 0.98); , HLB value 8), "Surfynol 400 series" such as 465 and 485, Surfynol 61, 82, 504, CT-111, CT-121, CT-131, CT-136, CT-141, CT-151, CT-171, CT-324, DF-37, DF-58, DF-75, DF-110D, DF-210, GA, OP-340, PSA-204, PSA-216, PSA-336, SE, SE-F, and Dynol 604 (manufactured by Nissin Chemical Industry Co., Ltd. and Air Products Inc.). In addition to the above, Olfine A, B, AK-02, CT-151W, E1004, E1010, P, SPC, STG, Y, 32W, PD-001, PD-002W, PD-003, PD-004, EXP. 4001, EXP. 4036, EXP. 4051, AF-103, AF-104, SK-14, AE-3 (all manufactured by Nissin Chemical Industry Co., Ltd.), Acetylenol E00, E13T, E40, E60, E81, E100, E200 (all manufactured by Kawaken Fine Chemicals Co., Ltd.), and EMALEX 100, 500, 600, 700, BHA, DAPE, CS, PS, 1600, 1800, OD, 2400 (manufactured by Nippon Emulsion Co., Ltd.). In addition, the nonionic surfactants described in paragraphs
[0074] to
[0078] of JP 2017-151432 A can also be used, and the contents of these surfactants are incorporated herein by reference.
[0052] Examples of anionic surfactants include phosphate ester surfactants having a phosphate ester group, sulfonic acid surfactants having a sulfo group, phosphonic acid surfactants having a phosphonic acid group, carboxylic acid surfactants having a carboxy group, and sulfate ester surfactants having a sulfate ester group, with sulfonic acid surfactants or sulfate ester surfactants being preferred.
[0053] Examples of phosphate ester surfactants include alkyl phosphate esters and polyoxyalkylene alkyl ether phosphate esters, as well as salts thereof. Examples of sulfonic acid surfactants include alkyl sulfonic acids, alkyl benzene sulfonic acids, alkyl naphthalene sulfonic acids, alkyl diphenyl ether disulfonic acids, alkyl methyl taurines, sulfosuccinic acid diesters, polyoxyalkylene alkyl ether sulfonic acids, and salts thereof, with alkyl sulfonic acids or their salts being preferred. Examples of phosphonic acid surfactants include alkyl phosphonic acids, polyvinyl phosphonic acids, and aminomethyl phosphonic acids. Examples of carboxylic acid surfactants include alkyl carboxylic acids, alkenyl carboxylic acids, alkyl benzene carboxylic acids, and polyoxyalkylene alkyl ether carboxylic acids, as well as anhydrides and salts thereof. The alkyl group contained in the anionic surfactant is not particularly limited, but is preferably an alkyl group having 7 to 25 carbon atoms, and more preferably an alkyl group having 8 to 17 carbon atoms.
[0054] Specific examples of carboxylic acid surfactants include decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, polyoxyethylene lauryl ether acetic acid, and polyoxyethylene tridecyl ether acetic acid.
[0055] Examples of anionic surfactants that can be used include Takesurf A-24, A-21-P, A-2806-S, A-2821-S, A-2832-S, A-32-B, A-40-S, A-41-BN, A-41-C, A-41-B, A-41-S, A-43-S, A-43-NQ, A-4433, A-44-TW, A-4441, A-4442-P, A-45-K, A-51-B, A-51-G, and A-51-P (manufactured by Takemoto Oil Co., Ltd.). In addition to the above, the compounds described in paragraphs
[0068] to
[0087] of JP-A-2023-024267 and paragraphs
[0116] to
[0123] of WO 2022 / 044893 can also be used, and the contents of these compounds are incorporated herein.
[0056] Examples of cationic surfactants include aliphatic amine salts, aliphatic quaternary ammonium salts, alkylpyridinium surfactants, alkylamine acetate surfactants, and modified aliphatic polyamines (e.g., polyethylene polyamines).
[0057] Examples of amphoteric surfactants include carboxybetaine, sulfobetaine, imidazolinium betaine, and alkylamine oxide.
[0058] Examples of surfactants include the compounds described in paragraphs
[0092] to
[0096] of JP-A-2015-158662, paragraphs
[0045] to
[0046] of JP-A-2012-151273, and paragraphs
[0014] to
[0020] of JP-A-2009-147389, the contents of which are incorporated herein by reference.
[0059] In order to obtain superior effects of the present invention, the content of the surfactant is preferably 0.00001 to 5.0 mass%, more preferably 0.00005 to 3.0 mass%, and even more preferably 0.0005 to 0.5 mass%, relative to the total mass of the etching solution. The mass ratio of the content of the surfactant to the content of the quinone compound is preferably 0.0001 to 1500, more preferably 0.001 to 50, and even more preferably 0.01 to 1.
[0060] [Hydroquinone Compound] In order to obtain superior effects of the present invention, the etching solution preferably contains a hydroquinone compound having a p-hydroquinone structure. The hydroquinone compound is not particularly limited as long as it has the p-hydroquinone structure as the entire structure or a partial structure of the compound, and examples thereof include p-hydroquinone and compounds in which the hydrogen atoms of p-hydroquinone are substituted with substituents. Examples of the substituents include alkyl groups, alkenyl groups, aryl groups, hydroxy groups, carbonyl groups, cyano groups, halogen atoms, alkoxy groups, aryloxy groups, alkyloxycarbonyl groups, and amino groups. The benzene ring contained in the p-hydroquinone structure of the hydroquinone compound may be part of a fused ring. For example, the hydroquinone compound may be 1,4-naphthalenediol.
[0061] The hydroquinone compound is preferably a compound represented by the following formula (2):
[0062]
[0063] In formula (2), R 5 ~R 8 each independently represents a hydrogen atom or a substituent. Examples of the substituent include an alkyl group, an alkenyl group, an aryl group, a hydroxy group, a carbonyl group, a cyano group, a halogen atom, an alkoxy group, an aryloxy group, an alkyloxycarbonyl group, and an amino group, with an alkyl group, a hydroxy group, a cyano group, or a halogen atom being preferred. The alkyl group and alkoxy group preferably have 1 to 20 carbon atoms, more preferably 1 to 12, and even more preferably 1 to 6. The aryl group and aryloxy group preferably have 5 to 20 carbon atoms, and more preferably 6 to 12. The alkyloxycarbonyl group preferably has 2 to 21 carbon atoms, more preferably 2 to 13, and even more preferably 2 to 7.
[0064] R 5 and R 6 may be bonded to each other to form a benzene ring which may have a substituent, R 7 and R 8may be bonded to each other to form a benzene ring which may have a substituent. 5 and R 6 do not bond to each other to form a benzene ring, and R 7 and R 8 It is also preferable that they do not bond to each other to form a benzene ring. The substituents that the benzene ring may have include the above-mentioned R 5 ~R 8 Examples of the group represented by the formula (I) include the substituents exemplified above.
[0065] Examples of hydroquinone compounds include p-hydroquinone, p-toluhydroquinone (methylhydroquinone), 2,6-dimethylhydroquinone, 2,3-dimethylhydroquinone, methoxyhydroquinone, chlorohydroquinone, tetrachlorohydroquinone, bromohydroquinone, tetrabromohydroquinone, tetrafluorohydroquinone, 2,3-dicyanohydroquinone, hexahydroxybenzene, 1,4-naphthalenediol, and 9,10-anthracenediol, with p-hydroquinone or methylhydroquinone being preferred.
[0066] The hydroquinone compound may be used alone or in combination of two or more. In order to obtain a more excellent effect of the present invention, the content of the hydroquinone compound is preferably 0.1 ppt by mass to 5 ppm by mass, more preferably 1 ppt by mass to 1 ppm by mass, and still more preferably 0.1 to 100 ppb by mass, relative to the total mass of the etching solution.
[0067] [pH Adjuster] The etching solution may contain a pH adjuster to adjust and maintain the pH of the etching solution. The pH adjuster is a basic compound or an acidic compound that is different from the compounds (e.g., quinone compounds, surfactants, and hydroquinone compounds) that may be contained in the etching solution. However, it is permissible to adjust the pH of the etching solution by adjusting the amount of each of the above components added.
[0068] A basic compound is a compound that exhibits basicity (a pH greater than 7.0) in an aqueous solution, and examples thereof include basic organic compounds and basic inorganic compounds. Examples of basic organic compounds include organic amine compounds and quaternary ammonium salt compounds, with quaternary ammonium salt compounds being preferred. Examples of quaternary ammonium salt compounds include tetraalkylammonium compounds such as tetramethylammonium hydroxide (TMAH), trimethylethylammonium hydroxide (TMEAH), dimethyldiethylammonium hydroxide (DMDEAH), methyltriethylammonium hydroxide (MTEAH), tetraethylammonium hydroxide (TEAH), tetrapropylammonium hydroxide (TPAH), and tetrabutylammonium hydroxide (TBAH); choline compounds such as 2-hydroxyethyltrimethylammonium hydroxide; and benzyltrimethylammonium hydroxide (BTMAH). Examples of basic inorganic compounds include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, as well as alkaline earth metal hydroxides.
[0069] An acidic compound is a compound that exhibits acidity (pH less than 7.0) in an aqueous solution. Examples of the acidic compound include acidic inorganic compounds. Examples of the acidic inorganic compound include hydrochloric acid (hydrogen chloride), sulfuric acid, nitric acid, nitrous acid, sulfurous acid, phosphoric acid, boric acid, and hexafluorophosphoric acid. The acidic compound used as the pH adjuster may be a salt of an acidic compound, as long as it becomes an acid or an acid ion (anion) in an aqueous solution.
[0070] The pH adjuster may be used alone or in combination of two or more. The content of the pH adjuster can be selected depending on the types and amounts of other components and the target pH of the etching solution. For example, the content of the pH adjuster is preferably 0.0001 to 5 mass %, more preferably 0.001 to 1 mass %, based on the total mass of the etching solution.
[0071] [Other Components] The etching solution may contain other components in addition to those described above, such as an anticorrosive agent, a dispersant, and an antifoaming agent.
[0072] The corrosion inhibitor is a compound that suppresses over-etching of a molybdenum-containing material. The corrosion inhibitor is not particularly limited, but examples include azole compounds, pyrazine compounds, pyrimidine compounds, indole compounds, indolizine compounds, indazole compounds, quinoline compounds, pyrrole compounds, and oxazole compounds, with azole compounds being preferred. The azole compound is a compound containing at least one nitrogen atom and having a heterocyclic 5-membered ring with aromaticity. Examples of azole compounds include imidazole compounds, pyrazole compounds, thiazole compounds, triazole compounds, and tetrazole compounds. Examples of azole compounds include the compounds described in paragraphs
[0046] to
[0050] of WO 2021 / 166571, the contents of which are incorporated herein by reference.
[0073] [Properties of Etching Solution] The properties of the etching solution will be described in detail below.
[0074] <pH> The etching solution may be either acidic or basic. In terms of achieving superior effects of the present invention, the pH of the etching solution is preferably 1 to 14, more preferably 2 to 11, and even more preferably 3 to 10. The pH of the etching solution can be controlled, for example, using the pH adjuster described above. The pH of the etching solution can be measured using a known pH meter by a method in accordance with JIS Z8802-1984. The pH is measured at 25°C.
[0075] <Dissolved Oxygen Amount> In order to obtain a more excellent effect of the present invention, the dissolved oxygen amount in the etching solution is preferably 0.1 to 100 mg / L, and more preferably 3 to 50 mg / L. The dissolved oxygen amount in the etching solution can be measured by a fluorescence method (for example, a fluorescence dissolved oxygen measurement sensor manufactured by Hamilton).
[0076] The method for adjusting the amount of dissolved oxygen in the etching solution is not particularly limited, and examples include a method for reducing the amount of dissolved oxygen in the raw materials and / or etching solution used to prepare the etching solution, a method for increasing the amount of dissolved oxygen, and a combination thereof. Alternatively, the amount of dissolved oxygen in the etching solution may be adjusted by preparing the etching solution using a combination of raw materials (e.g., solvents) with appropriate dissolved oxygen amounts. Examples of methods for reducing the amount of dissolved oxygen include a bubbling method in which an inert gas (e.g., nitrogen gas) is blown into the raw materials and / or etching solution used to prepare the etching solution, and a degassing method under vacuum or reduced pressure. Examples of methods for increasing the amount of dissolved oxygen include a bubbling method in which oxygen gas is blown into the raw materials and / or etching solution used to prepare the etching solution. The amount of dissolved oxygen is preferably adjusted using a bubbling method for the etching solution, since it is easy to adjust the content of each component and the amount of dissolved oxygen.
[0077] <Cr Atoms> The etching solution may contain Cr atoms. In order to achieve the effects of the present invention more effectively, the content of Cr atoms is preferably 0.1 mass ppt to 5 mass ppb, and more preferably 1 mass ppt to 1 mass ppb, relative to the total mass of the etching solution. The content of Cr atoms is measured by ICP-MS (inductively coupled plasma mass spectrometry). As an ICP-MS device, for example, Agilent 8900 triple quadrupole ICP-MS (inductively coupled plasma mass spectrometry, for semiconductor analysis, option #200) manufactured by Agilent Technologies, NexION350S manufactured by PerkinElmer, and Agilent 8800 manufactured by Agilent Technologies can be used.
[0078] The Cr atoms may be intentionally added, unavoidably contained in the raw materials of the etching solution, or unavoidably contained during the production, storage, and / or transportation of the etching solution. The form of the Cr atoms in the etching solution is not particularly limited, and they may be contained as Cr-containing particles or Cr ions. The Cr-containing particles may be in the form of simple Cr, a Cr alloy, or Cr associated with an organic substance, and the Cr ions may form a salt or a complex.
[0079] The method for adjusting the content of Cr atoms is not particularly limited, and examples thereof include a method for removing Cr atoms from the etching solution and / or raw materials used to prepare the etching solution, a method for adding a component containing Cr atoms, and a combination thereof. As a method for removing Cr atoms, a known method may be appropriately selected depending on the form of the Cr atoms, and examples include purification treatments such as filtration and ion exchange, which will be described later. When the Cr atoms are in the form of metal particles, filtration is preferred, and when the Cr atoms are in the form of ions, ion exchange is preferred. Among these, a method for subjecting a solvent used to prepare the etching solution to a purification treatment is preferred, and a method for subjecting the solvent to ion exchange is more preferred.
[0080] <Coarse Particles> The etching solution may contain coarse particles, but the content thereof is preferably low. Coarse particles refer to particles having a diameter (particle size) of 0.1 μm or more when the particle shape is considered as a sphere. The coarse particles contained in the etching solution include particles such as dust, dirt, organic solids, and inorganic solids contained as impurities in the raw materials, as well as particles such as dust, dirt, organic solids, and inorganic solids brought in as contaminants during the preparation of the etching solution, and these particles ultimately exist as insoluble particles in the etching solution without dissolving.
[0081] It is more preferable that the etching solution is substantially free of coarse particles. Substantially free of coarse particles means that the content of particles having a particle size of 0.1 μm or more is 10,000 or less per mL of the etching solution, preferably 5,000 or less. The lower limit is preferably 0 or more per mL of the first etching solution, more preferably 0.01 or more. The content of coarse particles present in the etching solution can be measured in the liquid phase using a commercially available measuring device that uses a laser as a light source for light scattering liquid particle measurement. Examples of methods for removing coarse particles include purification processes such as filtering, which will be described later.
[0082] [Production Method] The etching solution can be produced by a known method. For example, a method for preparing the etching solution includes sequentially adding a quinone compound, a solvent, and, if necessary, optional components, followed by stirring to mix them, and, if necessary, adding a pH adjuster to adjust the pH of the mixed solution. When adding each component to a container, they may be added all at once or may be added in multiple divided portions.
[0083] The etching solution may be prepared using a known agitator or disperser as the agitator and a stirring method. Examples of the agitator include an industrial mixer, a portable agitator, a mechanical stirrer, and a magnetic stirrer. Examples of the disperser include an industrial disperser, a homogenizer, an ultrasonic disperser, and a bead mill.
[0084] The mixing of the components in the etching solution preparation step, the purification treatment described below, and the storage of the produced etching solution are preferably carried out at 40° C. or lower, more preferably at 30° C. or lower. The lower limit is preferably 5° C. or higher, more preferably 10° C. or higher. By preparing, treating, and / or storing the etching solution within the above temperature range, the performance can be stably maintained for a long period of time.
[0085] It is preferable to perform a purification treatment in advance on one or more of the raw materials used to prepare the etching solution. Examples of the purification treatment include known methods such as distillation, ion exchange, reprecipitation, and filtration. The degree of purification is preferably such that the raw materials have a purity of 99% by mass or more, and more preferably such that the raw solution has a purity of 99.9% by mass or more. The upper limit is preferably 99.9999% by mass or less.
[0086] The ion exchange method is not particularly limited, and any known method can be used. Examples include a method in which the product to be purified is brought into contact with an ion exchange resin such as an anion exchange resin or a cation exchange resin, and a method in which the product is passed through an RO membrane (reverse osmosis membrane) or the like.
[0087] The filter used for filtering is not particularly limited as long as it is one that has been conventionally used for filtering purposes. Examples include filters made of fluororesins such as polytetrafluoroethylene (PTFE) and tetrafluoroethylene perfluoroalkyl vinyl ether copolymer (PFA), polyamide resins such as nylon, polyallylsulfone (PAS), and polyolefin resins (including high-density or ultra-high molecular weight) such as polyethylene and polypropylene (PP). Among these materials, materials selected from the group consisting of polyethylene, polypropylene (including high-density polypropylene), fluororesins (including PTFE and PFA), and polyamide resins (including nylon) are preferred, and fluororesin filters are more preferred. Filtering raw materials using filters made of these materials can effectively remove highly polar foreign matter that is likely to cause defects.
[0088] The purification process may be a combination of two or more of the above purification methods. For example, the raw material may be subjected to a primary purification process by passing it through an RO membrane, followed by a secondary purification process by passing it through a purification device made of a cation exchange resin, an anion exchange resin, or a mixed-bed ion exchange resin. The purification process may also be performed multiple times.
[0089] One or more of the raw materials for preparing the etching solution and the etching solution may be subjected to a treatment for adjusting the dissolved oxygen content. Specific methods for adjusting the dissolved oxygen content are as described above.
[0090] The etching solution can be filled into any container for storage, transportation, and use, as long as corrosiveness and other issues are not a problem. For semiconductor applications, a container with a high level of cleanliness within the container and suppressing the elution of impurities from the inner wall of the container's storage section into each solution is preferred. Examples of such containers include various containers commercially available as containers for semiconductor etching solutions, such as the "Clean Bottle" series manufactured by Aicello Chemical Co., Ltd. and the "Pure Bottle" manufactured by Kodama Resin Industry Co., Ltd., but are not limited to these. Furthermore, the containers exemplified in paragraphs
[0121] to
[0124] of International Publication No. 2022 / 004217 can also be used, and the contents of these containers are incorporated herein.
[0091] The interior of these containers is preferably cleaned before filling them with the etching solution. The liquid used for cleaning is preferably one in which the amount of metal impurities (e.g., Cr atoms) in the liquid is reduced. After production, the etching solution may be bottled in a container such as a gallon bottle or a coated bottle, and then transported and stored.
[0092] To prevent changes in the components of the etching solution during storage, the container may be filled with an inert gas (such as nitrogen or argon) with a purity of 99.99995% by volume or higher. A gas with a low water content is particularly preferred. During transportation and storage, the etching solution may be kept at room temperature, or the temperature may be controlled to a range of -20°C to 20°C to prevent deterioration.
[0093] It is preferable that all of the manufacturing of the etching solution, handling including opening and cleaning of the container, filling of the etching solution, processing analysis, and measurement be performed in a clean room. The clean room preferably meets the 14644-1 clean room standard. It is preferable that the clean room meets any of ISO (International Organization for Standardization) Class 1, ISO Class 2, ISO Class 3, and ISO Class 4, more preferably ISO Class 1 or ISO Class 2, and even more preferably ISO Class 1.
[0094] [Uses] The etching solution is an etching solution used for molybdenum-containing materials, and is preferably used for etching molybdenum-containing materials in materials to be treated during the manufacture of semiconductor devices.
[0095] The substrate to be treated with the etching solution is not particularly limited as long as it contains a molybdenum-containing material, and examples thereof include a substrate containing a molybdenum-containing material. When the substrate contains a molybdenum-containing material, the molybdenum-containing material may be present on the front, back, side, or groove of the substrate, for example. When the substrate contains a molybdenum-containing material, this includes not only a case where the molybdenum-containing material is present directly on the surface of the substrate, but also a case where the molybdenum-containing material is present on the substrate via another layer. The molybdenum-containing material may be located on only one major surface of the substrate, or on both major surfaces of the substrate. The molybdenum-containing material may be located on the entire major surface of the substrate, or on a portion of the major surface of the substrate.
[0096] The molybdenum-containing material is not particularly limited as long as it contains 30 mass% or more of molybdenum (molybdenum atoms) relative to the total mass of the molybdenum-containing material, but preferably contains 50 mass% or more, and more preferably contains 75 mass% or more of molybdenum. The upper limit is not particularly limited, and may be 100 mass%. Examples of the form of the molybdenum-containing material include molybdenum itself, alloys of molybdenum with other metals (molybdenum alloys), and oxides, nitrides, oxynitrides, silicides, and sulfides thereof. Examples of other metals that form alloys with molybdenum include copper (Cu), cobalt (Co), ruthenium (Ru), aluminum (Al), titanium (Ti), tantalum (Ta), Rh (rhodium), Cr (chromium), Hf (hafnium), Os (osmium), Pt (platinum), Ni (nickel), Mn (manganese), Zr (zirconium), La (lanthanum), Ir (iridium), and tungsten (W). The molybdenum content in the molybdenum alloy is 30 mass% or more, preferably 50 mass% or more, and more preferably 75 mass% or more, based on the total mass of the molybdenum alloy. The upper limit is not particularly limited, and may be less than 100 mass%. Examples of molybdenum-containing substances include molybdenum itself, molybdenum alloys, and molybdenum silicides (e.g., MoSi 2 ), or molybdenum sulfide (e.g., MoS 2 ) is preferred, and molybdenum alone, a molybdenum alloy containing 50 mass % or more of molybdenum based on the total mass, MoSi 2 , or MoS 2 is more preferred, and molybdenum alone is even more preferred.
[0097] The form of the molybdenum-containing material in the workpiece is not particularly limited, and examples thereof include a film-like form (molybdenum-containing film) and a wiring-like form (molybdenum-containing wiring). When the molybdenum-containing material is in the form of a film or wiring, its thickness is not particularly limited and may be appropriately selected depending on the application. The thickness of the film-like or wiring-like molybdenum-containing material is preferably 500 nm or less, more preferably 20 nm or less, and even more preferably 50 nm or less. There is no particular lower limit, but a thickness of 1 nm or more is preferred.
[0098] The type of substrate to be processed is not particularly limited, and examples thereof include various substrates such as semiconductor wafers, glass substrates for photomasks, glass substrates for liquid crystal displays, glass substrates for plasma displays, substrates for FEDs (Field Emission Displays), substrates for optical disks, substrates for magnetic disks, and substrates for magneto-optical disks. Materials constituting the semiconductor substrate include, for example, silicon, silicon germanium, and III-V group compounds such as GaAs, or any combination thereof. The size, thickness, shape, and layer structure of the substrate are not particularly limited and can be appropriately selected as desired.
[0099] When the workpiece is a semiconductor substrate, the semiconductor substrate may have an insulating film. The insulating film in the workpiece is not particularly limited, and examples thereof include an insulating film containing one or more materials selected from the group consisting of silicon nitride (SiN), silicon oxide, silicon carbide (SiC), silicon carbonitride, silicon oxide carbide (SiOC), silicon oxynitride, and TEOS (tetraethoxysilane). Among these, SiN, TEOS, SiC, or SiOC are preferred as the material. The insulating film may also be composed of multiple films.
[0100] The workpiece may have various layers and / or structures other than those described above, as desired. For example, when the workpiece is a substrate, the workpiece may have members such as a barrier layer, metal wiring, a gate electrode, a source electrode, a drain electrode, an insulating layer, a ferromagnetic layer, an integrated circuit structure, and / or a non-magnetic layer.
[0101] The method for manufacturing the workpiece is not particularly limited. The method for forming the insulating film and the molybdenum-containing material on the substrate is not particularly limited as long as it is a method commonly used in this field. For example, the method for forming the insulating film includes a method in which a wafer constituting a semiconductor substrate is heat-treated in the presence of oxygen gas to form a silicon oxide film, and then silane and ammonia gases are introduced to form a silicon nitride film by chemical vapor deposition (CVD). Examples of methods for forming a molybdenum-containing material (e.g., a molybdenum-containing film) on an insulating film include sputtering, physical vapor deposition (PVD), atomic layer deposition (ALD), chemical vapor deposition, and molecular beam epitaxy (MBE). Furthermore, the above methods may be performed through a predetermined mask to form a patterned molybdenum-containing material on a substrate.
[0102] [Etching Method] The etching solution of the present invention is preferably used in an etching treatment step for etching molybdenum-containing materials in a workpiece during the manufacture of a semiconductor device. The workpiece to be etched is as described above.
[0103] The specific method for etching a molybdenum-containing material using an etching solution is not particularly limited, and known methods can be used, such as contacting the molybdenum-containing material with the etching solution. The contact method is not particularly limited, and examples include immersing the workpiece in the etching solution contained in a tank, spraying the etching solution on the workpiece, flowing the etching solution on the workpiece, and any combination thereof. Immersing the workpiece in the etching solution is preferred. Furthermore, mechanical stirring may be used to further enhance the etching ability of the etching solution. Examples of mechanical stirring methods include circulating the etching solution over the workpiece, flowing or spraying the etching solution over the workpiece, and stirring the etching solution using ultrasonic waves or megasonics.
[0104] The contact time between the workpiece and the etching solution can be adjusted as appropriate, but is preferably 10 seconds to 20 minutes, more preferably 1 minute to 15 minutes, and even more preferably 3 minutes to 15 minutes. The temperature of the etching solution during treatment is preferably 20 to 75°C, more preferably 20 to 60°C.
[0105] After the etching process, a process of contacting the etched workpiece with a rinse liquid (hereinafter also referred to as a "rinsing process") may be performed. By performing the rinsing process, etching residues and / or the etching liquid on the workpiece can be efficiently removed. The rinsing process is preferably performed continuously after the etching process, and is a process of rinsing the semiconductor substrate with a rinse liquid. The rinsing process may be performed using the mechanical stirring method described above.
[0106] Examples of the rinse solution include water (preferably deionized water), methanol, ethanol, isopropyl alcohol (IPA), N-methylpyrrolidinone, γ-butyrolactone, dimethyl sulfoxide, ethyl lactate, and propylene glycol monomethyl ether acetate. Alternatively, an aqueous rinse solution having a pH greater than 8.0 (such as diluted aqueous ammonium hydroxide) may be used, or the solvent used in the etching solution of the present invention may be used.
[0107] The method of contacting the rinsing liquid with the workpiece can be the same as the method of contacting the rinsing liquid with the workpiece. The contact time between the workpiece and the rinsing liquid can be appropriately changed depending on the type and content of components contained in the etching liquid and the composition of the workpiece, but in practice it is preferably 10 to 120 seconds, more preferably 20 to 90 seconds, and even more preferably 30 to 60 seconds.
[0108] The rinsing step may be followed by a drying step for drying the workpiece, such as a spin drying method, a method of passing a dry gas over the semiconductor substrate, a method of heating the workpiece with a heating means such as a hot plate or an infrared lamp, a Marangoni drying method, a Rotagoni drying method, an IPA (isopropyl alcohol) drying method, or any combination thereof.
[0109] [Method for manufacturing a semiconductor device] The etching process can be suitably applied to a method for manufacturing a semiconductor device. The etching process can be performed before or after other processes performed on a substrate. The etching process can be incorporated into other processes while the other processes are being performed, or the etching process can be incorporated into other processes.
[0110] Examples of other processes include processes for forming structures such as metal wiring, gate structures, source structures, drain structures, insulating films, ferromagnetic layers, and non-magnetic layers (e.g., layer formation, etching, chemical mechanical polishing, and modification), resist formation processes, exposure processes, removal processes, heat treatment processes, cleaning processes, and inspection processes. Examples of other processes include the coating film formation process described in paragraph
[0021] and the laser irradiation process described in paragraph
[0022] of JP 2019-061978 A, the contents of which are incorporated herein by reference.
[0111] The etching process is preferably used for recess etching of metal wiring or a liner disposed on a substrate, thereby removing a portion of the metal wiring to form a recess.
[0112] The etching process may be applied to, for example, NAND, DRAM (Dynamic Random Access Memory), SRAM (Static Random Access Memory), ReRAM (Resistive Random Access Memory), FRAM (registered trademark) (Ferroelectric Random Access Memory), MRAM (Magnetoresistive Random Access Memory), or PRAM (Phase change Random Access Memory), or may be a logic circuit or a processor.
[0113] The present invention will be described in more detail below with reference to the following examples. The materials, amounts used, ratios, treatment details, and treatment procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the following examples.
[0114] In the following examples, the pH of the compositions was measured at 25°C using a pH meter (manufactured by Horiba, Ltd., model "F-74") in accordance with JIS Z8802-1984. In addition, in producing the compositions of the examples and comparative examples, handling of containers, preparation of compositions, filling, storage, and analytical measurements were all carried out in a clean room meeting ISO class 2 or lower. Unless otherwise specified, each raw material used in each etching solution shown below was of high purity grade, and was further purified in advance by distillation, ion exchange, filtration, or a combination of these.
[0115] [Preparation of Etching Solution] The solvent shown in the table below was added to a 250 mL beaker, and each component was added so as to obtain the composition shown in the table below. The mixture was thoroughly stirred using a 1-inch Teflon (registered trademark) coated stirrer to prepare the etching solutions of the Examples and Comparative Examples. The quinone compound, as well as the hydrogen peroxide and nitric acid used in the Comparative Examples, were added immediately before the evaluations described below were performed. The solvent content is the remainder of each component other than the solvent shown in the table.
[0116] Before mixing, an ion exchange resin (Amberlite IR-124, manufactured by Organo Corporation) was added to each solvent, followed by stirring and filtration to remove the ion exchange resin. The Cr content of each etching solution was adjusted by changing the stirring time after the addition of the ion exchange resin as described above and by adding a chromium standard solution (Cr 1000) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a Cr atom source. The Cr content (content of Cr atoms) of each etching solution was quantified using ICP-MS (manufactured by Agilent Technologies, Inc.).
[0117] For the etching solutions of Examples 46 to 49, after mixing the components, oxygen was bubbled through the solution at 0.2 L / min for 2 minutes while stirring at 700 rpm using the stirrer, and then nitrogen was bubbled through the solution for the specified time shown below to adjust the amount of dissolved oxygen. The amount of dissolved oxygen in each etching solution was measured using a fluorescent dissolved oxygen sensor (manufactured by Hamilton). Example 46: 1 minute Example 47: 1 minute 30 seconds Example 48: 5 minutes Example 49: 10 minutes
[0118] The components used in the etching solution are shown below.
[0119] [Quinone compounds] p-Benzoquinone (compound represented by formula (1)) p-Chloranil (compound represented by formula (1)) Fluoranil (compound represented by formula (1)) DDQ (2,3-dichloro-5,6-dicyano-1,4-benzoquinone, compound represented by formula (1)) Chloranilic acid (compound represented by formula (1)) Tetrahydroxybenzoquinone (compound represented by formula (1)) o-Chloranil 3,5-di-tert-butyl-1,2-benzoquinone 1,4-naphthoquinone (compound represented by formula (1)) Anthraquinone (compound represented by formula (1))
[0120] [Solvents] Water, Methanol, Ethanol, 1-Propanol, 2-Propanol, DMSO (Dimethyl Sulfoxide), Sulfolane, DMF (N,N-Dimethylformamide), NMP (N-Methyl-2-pyrrolidone), Pyridine, Acetonitrile, Acetone, Glycerin, THF (Tetrahydrofuran), Toluene
[0121] [Surfactants] Surfynol 440 (nonionic surfactant, manufactured by Nissin Chemical Industry Co., Ltd.) Surfynol 104E (nonionic surfactant, manufactured by Nissin Chemical Industry Co., Ltd.) Decanoic acid (anionic surfactant)
[0122] [Quinone compounds] Hydroquinone 1,4-naphthalenediol Methylhydroquinone
[0123] [Other additives] Hydrogen chloride (pH adjuster) TMAH (tetramethylammonium hydroxide, pH adjuster) Hydrogen peroxide (oxidizer) Nitric acid (oxidizer)
[0124] [Evaluation] A molybdenum-containing metallic molybdenum layer was formed on one surface of a 12-inch silicon wafer by PVD, and the wafer was cut into a 2 × 2 cm square to prepare a substrate for evaluation. The thickness of the metallic molybdenum layer was 25 nm. Using the etching solutions of each Example and Comparative Example prepared by the above method and the test substrate, the etching rate and surface roughness were evaluated by the following method.
[0125] [Etching Rate] The evaluation substrate was immersed for 10 minutes in the etching solution of each Example or Comparative Example adjusted to 25°C. Thereafter, the substrate was washed with running water at 500 mL / min for 30 seconds and dried using a nitrogen gun to obtain an etched substrate. The thickness of the metal molybdenum layer before and after etching was measured using an X-ray fluorescence analyzer for thin film evaluation (XRF; X-ray Fluorescence, manufactured by Rigaku Corporation, AZX-400). The etching amount was calculated from the difference in thickness before and after etching, and the etching rate (Å / min) was calculated by dividing this by the treatment time. The etching rate was evaluated according to the following evaluation criteria. An etching rate rating of 2 or higher is preferred.
[0126] 5: 100 Å / min or more 4: 50 Å / min or more but less than 100 Å / min 3: 30 Å / min or more but less than 50 Å / min 2: 10 Å / min or more but less than 30 Å / min 1: Less than 10 Å / min
[0127] [Surface Roughness] The surface of the molybdenum layer of the substrate after the etching treatment obtained in the etching rate evaluation described above was observed using an atomic force microscope (AFM; Atomic Force Microscope, AFM Dimension Icon, manufactured by Bruker Corporation) to determine the surface roughness Ra. The suppression of surface roughness was evaluated from the obtained surface roughness Ra. The surface roughness rating is preferably 2 or higher.
[0128] 5: Surface roughness Ra is 0.5 nm or less 4: Surface roughness Ra is more than 0.5 nm and less than 1.0 nm 3: Surface roughness Ra is more than 1.0 nm and less than 1.5 nm 2: Surface roughness Ra is more than 1.5 nm and less than 2.0 nm 1: Surface roughness Ra is more than 2.0 nm
[0129] [Results] The table below shows the composition and evaluation results of each etching solution. In the table, the content of the solvent is the remainder of the components shown in the table below. In the table, when two or more components are used, the mixing ratio of each component shown in the table is the mass ratio. For example, when "water / ethanol (8 / 2)" is written in the solvent column, it means that a mixed solvent of water / ethanol = 8 / 2 (mass ratio) was used as the solvent. In the table, the relative dielectric constant of the solvent is the value at 20°C. In the table, "ppb" in the content indicates mass ppb. Table 2 is a continuation of Table 1, and Table 4 is a continuation of Table 3.
[0130]
[0131]
[0132]
[0133]
[0134] From the results shown in the above table, it was confirmed that the etching solution of the present invention has an excellent etching rate and can suppress surface roughness.
[0135] Comparison of Examples 1 to 6, 14 to 15, 17 to 19, and 36 confirmed that the effects of the present invention are more excellent when the quinone compound contains at least one selected from the group consisting of p-benzoquinone, p-chloranil, fluoranil, 2,3-dichloro-5,6-dicyano-p-benzoquinone, chloranilic acid, and tetrahydroxy-1,4-benzoquinone, and that the effects of the present invention are even more excellent when the quinone compound contains at least one selected from the group consisting of p-benzoquinone, p-chloranil, fluoranil, chloranilic acid, and tetrahydroxy-1,4-benzoquinone. Comparison of Examples 1 to 6, 14 to 15, 17 to 19, and 36 confirmed that the effects of the present invention are more excellent when the quinone compound is a compound represented by formula (1), and that the effects of the present invention are even more excellent when the quinone compound contains at least one selected from the group consisting of p-benzoquinone, p-chloranil, fluoranil, chloranilic acid, and tetrahydroxy-1,4-benzoquinone. 1 and R 2 do not bond to each other to form a benzene ring, and R 3 and R 4It was confirmed that the effects of the present invention are even better when the quinone compound is a compound represented by formula (1) in which the quinone compounds are not bonded to each other to form a benzene ring. Comparisons between Examples 1 and 7 to 9, and between Examples 10 to 13 and 36, confirmed that when the quinone compound content is 0.0001% by mass or more, relative to the total mass of the etching solution, the etching rate is better; when it is 0.001% by mass or more, the etching rate is even better; when it is 0.01% by mass or more, the etching rate is particularly good; and when it is 10.0% by mass or less, surface roughness can be further suppressed. Comparisons between Examples 20 to 38 and 63 confirmed that the effects of the present invention are better when the solvent contains at least one selected from the group consisting of water and water-soluble organic solvents, and that the effects of the present invention are even better when it contains at least one selected from the group consisting of water, alcohol solvents, sulfoxide solvents, nitrile solvents, and sulfone solvents. A comparison of Examples 20 to 38 and Example 63 confirmed that the effects of the present invention were better when the solvent contained at least one selected from the group consisting of water, methanol, ethanol, 1-propanol, 2-propanol, dimethyl sulfoxide, sulfolane, N,N-dimethylformamide, N-methylpyrrolidone, pyridine, acetonitrile, acetone, tetrahydrofuran, and glycerin, and that surface roughness could be further suppressed when the solvent contained at least one selected from the group consisting of water, methanol, ethanol, dimethyl sulfoxide, sulfolane, and acetonitrile. A comparison of Examples 20 to 38 and Example 63 confirmed that the effects of the present invention were better when the solvent had a dielectric constant at 20 ° C. of 7 or more, even better when the solvent had a dielectric constant of 20 or more, and particularly better when the solvent had a dielectric constant of 50 or more. It was also confirmed that surface roughness could be further suppressed when the solvent had a dielectric constant at 20 ° C. of 75 or less. From a comparison between Example 1 and Examples 20 to 25, it was confirmed that when the solvent contains water and a water-soluble organic solvent, the effect of the present invention is better when the content of water is 20 to 95 mass% with respect to the total mass of the solvent.A comparison of Example 1 and Examples 39 to 42 confirmed that the effects of the present invention were better when the surfactant content was 0.0005 to 0.5 mass% relative to the total mass of the etching solution. A comparison of Example 1 and Examples 43 to 45 confirmed that when the etching solution contained a surfactant, surface roughness could be more effectively suppressed, and when the surfactant was a nonionic surfactant, the effects of the present invention were better. A comparison of Example 27 and Examples 46 to 49 confirmed that when the dissolved oxygen content was 3 mg / L or more, the etching rate was better, and when the dissolved oxygen content was 50 mg / L or less, surface roughness could be more effectively suppressed. A comparison of Example 1 and Examples 50 to 41 confirmed that the effects of the present invention were better when the Cr atom content was 1 mass ppt to 1 mass ppb relative to the total mass of the etching solution. A comparison of Example 1 and Examples 52 to 55 confirmed that the effects of the present invention were better when the pH was 3 to 10. A comparison of Example 1 and Examples 56 to 58 confirmed that the effects of the present invention were better when the etching solution contained a hydroquinone compound. Comparison of Example 1 and Examples 59 to 61 confirmed that the effects of the present invention are more excellent when the content of the hydroquinone compound is 1 ppt by mass to 1 ppm by mass relative to the total mass of the etching solution.
Claims
1. An etching solution for use with molybdenum-containing materials, comprising a quinone compound having a quinone structure and a solvent.
2. The etching solution according to claim 1, wherein the solvent comprises at least one selected from the group consisting of water and water-soluble organic solvents.
3. The etching solution according to claim 1 or 2, wherein the content of the quinone compound is 0.0001 to 10.0 mass % based on the total mass of the etching solution.
4. The etching solution according to claim 1 or 2, wherein the quinone compound is a compound represented by formula (1). In formula (1), R 1 ~R 4 R each independently represents a hydrogen atom or a substituent. 1 and R 2 may be bonded to each other to form a benzene ring which may have a substituent, R 3 and R 4 may be bonded to each other to form a benzene ring which may have a substituent.
5. The quinone compound is R 1 and R 2 do not bond to each other to form a benzene ring, R 3 and R 4 The etching solution according to claim 4 , which is a compound represented by formula (1) in which are not bonded to each other to form a benzene ring.
6. The etching solution according to claim 1 or 2, wherein the quinone compound comprises at least one selected from the group consisting of p-benzoquinone, p-chloranil, fluoranil, 2,3-dichloro-5,6-dicyano-p-benzoquinone, chloranilic acid, and tetrahydroxy-1,4-benzoquinone.
7. The etching solution according to claim 1 or 2, further comprising a hydroquinone compound having a p-hydroquinone structure, the content of said hydroquinone compound being 1 ppt by mass to 1 ppm by mass relative to the total mass of said etching solution.
8. The etching solution according to claim 1 or 2, wherein the amount of dissolved oxygen is 3 to 50 mg / L.
9. The etching solution according to claim 1 or 2, wherein the solvent has a relative dielectric constant of 7 to 75 at 20° C.
10. The etching solution according to claim 1 or 2, wherein the solvent contains water and a water-soluble organic solvent, and the content of the water is 20 to 95 mass % based on the total mass of the solvent.
11. The etching solution according to claim 1 or 2, wherein the solvent contains at least one selected from the group consisting of water, methanol, ethanol, 1-propanol, 2-propanol, dimethyl sulfoxide, sulfolane, N,N-dimethylformamide, N-methylpyrrolidone, pyridine, acetonitrile, acetone, tetrahydrofuran, and glycerin.
12. The etching solution according to claim 1 or 2, wherein the solvent comprises at least one selected from the group consisting of water, alcohol solvents, sulfoxide solvents, nitrile solvents, and sulfone solvents.
13. The etching solution according to claim 1 or 2, further comprising a surfactant.
14. The etching solution according to claim 1 or 2, wherein the content of Cr atoms is 1 ppt by mass to 1 ppb by mass with respect to the total mass of the etching solution.
15. The etching solution according to claim 1 or 2, having a pH of 3 to 10.
16. A method for manufacturing a semiconductor device, comprising the step of etching the molybdenum-containing material with the etching solution according to claim 1 or 2.
Citation Information
Patent Citations
Chemical etching composition and application method thereof
CN116356325A
Etching solution for selectively removing silicon-germanium alloy from silicon-germanium / germanium stack during manufacture of semiconductor device
JP2019165218A
Etching compositions and methods for EUV mask protection structures
JP2022553203A
Method and composition for etching molybdenum
US20210324525A1