Method for producing energy-responsive composition, and energy-responsive composition
The method allows for high-density arrangement of quantum dots using an associative polymer in a low dielectric solvent, addressing stability and steric repulsion issues, enhancing quantum efficiency and light-emitting characteristics.
Patent Information
- Application Number
- PCT/JP2024/017348
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-28
AI Technical Summary
Quantum dots with a perovskite crystal structure have low stability against external stimuli, leading to fusion and loss of unique properties when present at high density, which reduces their light-emitting characteristics due to steric repulsion from polymer ligands used for protection.
A method involving a solvent with a low dielectric constant and an associative polymer with a main chain and polar group, allowing self-association to form unimeric micelles that facilitate high-density arrangement of quantum dots without separation, using a polymer as a ligand.
Enables high-density arrangement of quantum dots while maintaining stability and light-emitting properties, improving quantum efficiency and density without the drawbacks of steric repulsion.
Smart Images

Figure JP2024017348_28112024_PF_FP_ABST
Abstract
Description
Method for producing energy-responsive composition, energy-responsive composition
[0001] The present disclosure relates to a method for producing an energy responsive composition, and to an energy responsive composition.
[0002] Quantum dots with a perovskite crystal structure have a narrow full width at half maximum in their spectral sensitivity characteristics and exhibit high color purity, making them well-known for their application in organic electroluminescence (EL) materials, quantum dot light-emitting materials, and solar cell materials. Furthermore, because the absorption and emission wavelengths can be controlled by the halogen composition, they have the advantage of easily providing materials that respond to light over a wide wavelength range.
[0003] On the other hand, quantum dots with a perovskite crystal structure are known to have low stability against external stimuli such as light, heat, air, and moisture. In particular, when quantum dots exist in a high density in the solid phase, they tend to fuse together. When this occurs, the quantum dots lose their unique properties, such as the quantum size effect, and the desired physical properties are no longer exhibited.
[0004] In JP 2021-91870, stability is improved by using a ligand containing an organic acid salt and a polymer containing an acidic group to protect against external stimuli.
[0005] Patent Publication No. 2021-91870
[0006] Quantum efficiency can be improved by using the technology described in JP 2021-91870 A. However, when using a polymer for protection, as in the technology described in JP 2021-91870 A, the steric repulsion between the polymer chains makes it impossible to bring the quantum dots closer together. This reduces the density of quantum dots per unit volume, resulting in a problem of reduced properties such as light emission.
[0007] The present invention has been made in view of the above-mentioned problems, and aims to provide a method for producing an energy-responsive composition that can arrange quantum dots at a high density even when a polymer is used as a ligand. Another aim of the present invention is to provide an energy-responsive composition that includes a polymer and has quantum dots arranged at a high density.
[0008] A method for producing an energy responsive composition according to an embodiment of the present invention includes the steps of: preparing a polymer-containing liquid containing a solvent exhibiting a relative dielectric constant of a predetermined value or less; and an associative polymer having a main chain containing a plurality of carbons and a polar group more polar than the main chain, and which self-associates in the solvent; bringing energy responsive nanoparticles into contact with the polymer-containing liquid (P) to prepare a mixed liquid; and extracting an energy responsive composition containing a plurality of energy responsive protected particles, each of which comprises nanoparticles and an associative polymer, from the mixed liquid R by reducing the solvent content.
[0009] Moreover, the energy-responsive composition according to an embodiment of the present invention includes a plurality of energy-responsive protected particles, each of which has an energy-responsive nanoparticle and an associative polymer having a main chain containing a plurality of carbons and a polar group more polar than the main chain, and among the plurality of energy-responsive protected particles, a pair of adjacent energy-responsive protected particles are in contact with each other by the associative polymers that they possess being in contact with each other, and the nanoparticles that they possess are spaced apart from each other.
[0010] According to the present invention, it is possible to provide a method for producing an energy-responsive composition that allows quantum dots to be arranged at a high density even when a polymer is used as a ligand, and also to provide an energy-responsive composition that includes a polymer and has quantum dots arranged at a high density.
[0011] FIG. 1 is a process diagram of a method for producing an energy-responsive composition according to a first embodiment; FIG. 2 is a diagram showing a schematic configuration of a polymer-containing liquid according to a first embodiment; FIG. 3 is a diagram showing a schematic configuration of a mixed liquid according to a first embodiment; FIG. 4 is a diagram showing a schematic configuration of an energy-responsive composition according to a first embodiment; FIG. 5 is a diagram showing a form of an energy-responsive composition according to a second embodiment, extracted while supported on a support substrate; FIG. 6 is a diagram showing a form of an energy-responsive composition according to a second embodiment, extracted while supported on a support substrate; FIG. 7 is a diagram showing a form of an energy-responsive composition according to a second embodiment, extracted while supported on a support substrate.
[0012] Preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings. The dimensions, materials, shapes, relative positions, and other details of the components described in these embodiments are not intended to limit the scope of the present invention.
[0013] <First Embodiment> A method for producing an energy-responsive composition according to a first embodiment will be described with reference to Figure 1 and Figures 2A to 2C. Figure 1 is a process diagram showing each step of a method 1000 for producing an energy-responsive composition according to the first embodiment. Figures 2A to 2C are diagrams showing the schematic configurations of a polymer-containing liquid (Figure 2A), a mixed liquid (Figure 2B), and an energy-responsive composition (Figure 2C) according to the first embodiment.
[0014] The energy-responsive composition manufacturing method 1000 executes steps S101 to S19 as shown in FIG.
[0015] (Step S103 of preparing a polymer-containing liquid) Step S103 of preparing a polymer-containing liquid includes a step of preparing a polymer-containing liquid (P) containing a solvent 10 exhibiting a relative dielectric constant of a predetermined value or less, and an associative polymer 40 having a main chain 20 containing a plurality of carbon atoms and a polar group 30 having polarity greater than that of the main chain 20, and which self-associates in the solvent.
[0016] (Step S105 of Preparing a Mixture) The step S105 of preparing a mixture includes a step of bringing the energy-responsive nanoparticles (Q) into contact with the polymer-containing liquid (P) to prepare a mixture (R).
[0017] (Step S107 of extracting energy-responsive composition) Step S107 of extracting the energy-responsive composition includes a step of extracting an energy-responsive composition (S) containing a plurality of energy-responsive protected particles, each of which includes nanoparticles and an associative polymer, from the mixed liquid R by reducing the solvent content.
[0018] (Consideration of Effects) The detailed reasons why the above-described effects are obtained in the manufacturing method 1000 of the energy responsive composition 100 according to this embodiment are not clear, but the present inventors consider the following.
[0019] An associative polymer 40, which has a main chain 20 containing multiple carbon atoms and polar groups 30 that are more polar than the main chain 20 and self-associates in a solvent 10, forms a morphology called a unimer micelle, in which the polar groups 30 associate with each other within a single polymer molecule under certain conditions (Figure 2A). Unimer micelles are small, measuring only a few nanometers in size (average micelle diameter of approximately 2-10 nm), and the polar groups 30 are hidden inside. Therefore, coordination is difficult to proceed even when mixed with energy-responsive nanoparticles 60 (Figure 2B). When the content of solvent 10 in the mixed solution (R) is reduced, the distance between the nanoparticles 60 first decreases with increasing concentration. Next, the association dissolves, and coordination proceeds while maintaining the nanoparticles 60 close to each other. At this time, coordination proceeds in such a way that some of the nanoparticles cross-link each other, further reducing the distance between the nanoparticles 60 (Figure 2C).
[0020] (Self-association) In this embodiment, self-association refers to intramolecular association of at least some of the polar groups 30 with each other due to electrostatic interaction in a solvent 10 exhibiting a relative dielectric constant of a predetermined value or less. The polar groups 30 do not necessarily have to interact directly with each other, and a small amount of polar substance such as water may be present between them. Furthermore, association of different types of polar groups with each other due to electrostatic interaction is also considered to be self-association.
[0021] (Nanoparticles) The energy-responsive nanoparticles Q in this embodiment are preferably nanoparticles containing, as an allotrope, nanocrystals having a perovskite-type crystal structure whose constituent components are an A site (monovalent cation), a B site (divalent cation), and an X site (monovalent anion including a halide anion). The perovskite-type crystal structure is a perovskite-type structure, ABX 3 Type crystal structure, ABX 3 This can be rephrased as a type structure. 2 B 1 B 2 X 6 The perovskite crystal structure also includes a double perovskite crystal structure represented by the following formula: In this specification, the energy-responsive nanoparticle Q may be referred to as a nanoparticle, a luminescent nanoparticle, a luminescent nanocrystal, a photoresponsive nanocrystal, or a quantum dot.
[0022] The average particle size of the nanoparticles is preferably 1 nm or more and 30 nm or less, and more preferably 2 nm or more and 25 nm or less. If the average particle size is less than 1 nm, the stability may be insufficient. If the average particle size is more than 30 nm, the dispersibility in the medium may be insufficient.
[0023] [A Site of Perovskite Structure] A monovalent cation is used at the A site. The monovalent cation used at the A site is an ammonium cation (NH 4 + ), and alkylammonium cations having 6 or less carbon atoms, formamidinium cations (HC(NH 2 ) 2 + ), guanidinium cation (C(NH 2 ) 3 + cations of nitrogen-containing organic compounds such as imidazolium cation, pyridinium cation, and pyrrolidinium cation; and lithium cation (Li + ), sodium cation (Na + ), potassium cation (K + ), rubidium cation (Rb + ), and cesium cation (Cs + ) and other alkali metal cations.
[0024] These monovalent cations employed in the A site have a small ion diameter and are large enough to fit into the crystal lattice, allowing the perovskite compound to form a stable three-dimensional crystal.
[0025] Preferred examples of alkylammonium cations having 6 or less carbon atoms include methylammonium cations (CH 3 NH 3 + ), ethylammonium cation (C 2 H 5 NH 3 + ), propylammonium cation (C 3 H 7 NH 3+ ) etc.
[0026] From the viewpoint of obtaining high luminous efficiency, it is preferable to use at least one of methylammonium cation, formamidinium cation, and cesium cation as the A site, and from the viewpoint of suppressing color change, it is more preferable to use cesium cation as the A site. Two or more of these monovalent cations employed as the A site may be used in combination.
[0027] When the A site is a cesium cation, a raw material for synthesizing nanoparticles can be a cesium salt. Examples of such cesium salts include cesium chloride, cesium bromide, cesium iodide, cesium hydroxide, cesium carbonate, cesium hydrogen carbonate, cesium bicarbonate, cesium formate, cesium acetate, cesium propionate, cesium pivalate, and cesium oxalate. An appropriate cesium salt can be used from these candidate salts depending on the synthesis method.
[0028] When the A site is another alkali metal cation, a salt in which the cesium element of the above-mentioned cesium compound is replaced with another alkali metal cation element can be used as the raw material.
[0029] When the A site is a nitrogen-containing organic compound cation such as a methylammonium cation, a neutral compound other than a salt such as methylamine can be used as the raw material. Two or more of these raw materials may be used in combination.
[0030] [B Site of Perovskite Crystal Structure] Divalent cations including divalent transition metal cations or divalent typical metal cations are employed in the B site of the perovskite crystal structure.
[0031] The divalent transition metal cation is scandium cation (Sc 2+ ), titanium cation (Ti 2 +), vanadium cation (V 2+ ), chromium cation (Cr 2+ ), manganese cations (Mn 2+ ), iron cation (Fe 2+ ), cobalt cation (Co 2+), nickel cation (Ni 2+ ), copper cation (Cu 2+ ), palladium cation (Pd 2+ ), europium cation (Eu 2+ ), ytterbium cation (Yb 2+ ) will be adopted.
[0032] The divalent typical metal cation is the magnesium cation (Mg 2+ ), calcium cation (Ca 2+ ), strontium cation (Sr 2+ ), barium cation (Ba 2+ ), zinc cation (Zn 2+ ), cadmium cation (Cd 2+ ), germanium cation (Ge 2+ ), tin cations (Sn 2+ ), lead cation (Pb 2+ ) may be employed.
[0033] Among these divalent cations, divalent typical metal cations are preferred in terms of growing stable three-dimensional crystals, tin cations or lead cations are more preferred, and lead cations are particularly preferred in terms of obtaining high luminescence intensity. Two or more of these divalent cations may be used in combination, and the perovskite crystal structure may be a so-called double perovskite structure.
[0034] When the B site is a lead cation, examples of raw materials used in nanoparticle synthesis include lead compounds, and appropriate compounds can be used depending on the synthesis method. Examples of lead compounds that can be used include lead chloride, lead bromide, lead iodide, lead oxide, lead hydroxide, lead sulfide, lead carbonate, lead formate, lead acetate, lead 2-ethylhexanoate, lead oleate, lead stearate, lead naphthenate, lead citrate, lead maleate, and lead acetylacetonate. When the B site is another divalent metal cation, salts of the above-mentioned lead compounds in which the lead element is replaced with another divalent metal cation element can be used as raw materials. Two or more of these raw materials may be used in combination.
[0035] [X Site of Perovskite Crystal Structure] A monovalent anion including a halide anion is used as X in the perovskite crystal structure. As the halide anion, a fluoride anion (F - ), chloride anion (Cl - ), bromide anion (Br - ), iodide anion (I - Among these, chloride anions, bromide anions, and iodide anions are preferred because they form stable three-dimensional crystals and emit strong light in the visible light range. The emitted light color is blue when chloride anions are used, green when bromide anions are used, and red when iodide anions are used.
[0036] Two or more halide anions may be used in combination. In particular, when chloride anions, bromide anions, and iodide anions are used in combination, the emission wavelength of the nanoparticles can be set to a desired wavelength depending on the content ratio of the anion species. That is, in particular, when chloride anions, bromide anions, and iodide anions are used in combination, an emission spectrum that covers almost the entire range of visible light from blue to red can be obtained while maintaining a narrow full width at half maximum depending on the content ratio of the anion species, which is preferable.
[0037] The X site may contain a monovalent anion other than a halide anion. Such a monovalent anion other than a halide anion may be a cyanide anion (CN - ), thiocyanate anion (SCN - ), isothiocyanate anion (CNS - As raw materials for synthesizing nanoparticles, an appropriate one can be selected depending on the synthesis method from salts with counter cations at the A site and B site, such as cesium chloride and lead bromide, and salts with other cations.
[0038] The nanoparticles Q in this embodiment can be produced by the following processes: For example, a hot injection method is used in which raw material solutions are mixed at high temperatures, and then rapidly cooled after the formation of fine particles to obtain a stable product, and a ligand-assisted reprecipitation method is used in which fine particles are obtained by reprecipitation utilizing the difference in miscibility of the product with the solvent.
[0039] Another manufacturing method that can be used is a room-temperature synthesis method in which a mixture of non-halogenated A-site and B-site raw materials, which do not contain any X-site components, is mixed with a separately prepared X-site raw material solution under mild conditions at about room temperature to obtain fine particles.Furthermore, this manufacturing method can be used in a mechanochemical method in which solid raw materials are reacted by mechanical mixing such as milling or ultrasonic treatment to obtain product fine particles, and in a in situ synthesis method in which a raw material solution is applied to a substrate and then crystals are grown directly to obtain a reaction product.
[0040] By allowing the ligand described below to coexist during the production of nanoparticles Q, it is possible to coordinate the ligand to the surface of nanoparticles Q and stabilize the dispersion. If necessary, excess ligand may be removed by centrifugation or the like.
[0041] (Solvent) As the solvent, a solvent exhibiting a relative dielectric constant of a predetermined value or less can be used. The predetermined value is preferably 6.0 or less, and more preferably 4.5 or less.
[0042] Specific examples include aromatic hydrocarbons such as xylene (dielectric constant 2.3) and toluene (dielectric constant 2.4); hydrocarbons such as hexane (dielectric constant 1.9); alicyclic hydrocarbons such as cyclohexane (dielectric constant 2.0); esters such as ethyl acetate (dielectric constant 6.0) and butyl acetate (dielectric constant 5.0); alkyl halides such as chloroform (dielectric constant 4.9); and ethers such as diethyl ether (dielectric constant 4.3). If necessary, these solvents can be mixed and used. In this case, the weighted average of the dielectric constants of the individual solvents is used. Furthermore, the polymerizable compounds described below can also be used as solvents.
[0043] (Ligand) In this embodiment, the ligand 30 is preferably selected from at least one compound or ion selected from the group consisting of weak acids such as carboxylic acids, weak bases such as amines, and salts or ions thereof.
[0044] Examples of the acid include branched or straight-chain fatty acids having 1 to 30 carbon atoms. The alkyl chain may be saturated or unsaturated. Among these, from the viewpoints of solubility in solvents and stability, straight-chain fatty acids are preferred, and oleic acid is more preferred.
[0045] Examples of the base include branched or linear organic bases having 1 to 30 carbon atoms. The alkyl chain may be saturated or unsaturated. Among these, from the viewpoints of solubility in solvents and stability, linear organic bases are preferred, and oleylamine is more preferred.
[0046] The ligands may be used alone or in combination of two or more.
[0047] (Amount of Ligands Relative to Nanoparticles Q) When nanoparticles Q is taken as 100, the amount of ligands is preferably 10 to 500, more preferably 20 to 400, and even more preferably 30 to 300. If the amount of ligands is less than 10 or more than 300, the dispersion stability of nanoparticles Q may be insufficient.
[0048] (Associative Polymer) In this embodiment, the associative polymer 40 includes an associative polymer that has a main chain 20 containing a plurality of carbon atoms and a polar group 30 that is more polar than the main chain 20, and that self-associates in the solvent 10.
[0049] The main chain 20 is the longest series of covalently bonded atoms and may have side chains. The side chains may be linear, branched, or cyclic alkyl groups, linear, branched, or cyclic heteroalkyl groups, aryl groups, heteroaryl groups, aralkyl groups, or heteroaralkyl groups. Some of these groups may further have substituents.
[0050] The polar group 30 is at least one selected from the group consisting of strong acids such as sulfonic acid and phosphonic acid, strong bases such as quaternary ammonium cations, zwitterionic groups such as sulfobetaine, phosphobetaine, and carboxybetaine, and salts or ions thereof.
[0051] As the associative polymer, a copolymer (described later) obtained by polymerizing at least two types of monomers can be used.
[0052] (Amount of associative polymer relative to nanoparticle Q) When nanoparticle Q is taken as 100, the amount of associative polymer is preferably 1 or more and 1,000 or less, more preferably 10 or more and 800 or less, and even more preferably 30 or more and 600 or less. If the amount of associative polymer is less than 10, the fusion effect may not be sufficiently obtained. If the amount of associative polymer is more than 600, unimer micelles may not be successfully formed in the solvent.
[0053] (Number of mmoles of polar groups per 1 g of nanoparticles Q) The number of mmoles of polar groups per 1 g of nanoparticles Q is preferably 0.01 to 10, more preferably 0.03 to 8, and more preferably 0.1 to 6. When the number of mmoles of polar groups per 1 g of nanoparticles Q is within the above range, the effect of preventing fusion is easily obtained. When it is less than 0.01, fusion may not be effectively prevented. When it is more than 10, unimer micelles may not be successfully formed in a low-polarity medium. The number of mmoles corresponds to the content of polar groups contained in 1 g of nanoparticles Q, and is multiplied by 10 -3 This is a unit corresponding to mol.
[0054] <Method for Producing Energy-Responsive Composition> Hereinafter, the method for producing nanoparticles of the present invention will be described in detail.
[0055] The manufacturing method of the present invention includes the following steps: a step of preparing a polymer-containing liquid (P) containing a solvent 10 exhibiting a relative dielectric constant of a predetermined value or less and an associative polymer 40 having a main chain containing multiple carbon atoms and polar groups 30 more polar than the main chain, and which self-associates in the solvent 10; a step of contacting energy-responsive nanoparticles (Q) with the polymer-containing liquid (P) to prepare a mixture (C); and a step of extracting an energy-responsive composition (S) containing a plurality of energy-responsive protected particles, each comprising nanoparticles Q and associative polymer 40, from the mixture C by reducing the content of solvent 10.
[0056] (Step of Preparing Mixture (C)) The nanoparticles Q produced by the above-mentioned method are brought into contact with a polymer-containing liquid P in which the associative polymer 40 produced by the method described below is dispersed in a solvent 10. A known technique is applied as the contact method. Examples of the contact method include a method of mixing the liquid in which the nanoparticles Q are dispersed with the polymer-containing liquid P in liquid phase, and a method of adding the polymer-containing liquid P to the solid-phase nanoparticles Q and re-dispersing them to mix them. Another contact method that can be used is a method of applying the polymer-containing liquid P while rotating the nanoparticles Q present as a solid phase on a support (spin coating). When dispersing the nanoparticles Q in a liquid, the dispersion solvent may be the same as or different from the solvent of the polymer-containing liquid P. The dispersion solvent of the nanoparticles Q preferably has a relative dielectric constant of a predetermined value or less. The predetermined value is preferably 6.0 or less, and more preferably 4.5 or less.
[0057] The temperature during preparation of mixture C is preferably −80° C. or higher and 50° C. or lower, and more preferably −30° C. or higher and 40° C. or lower. If the temperature is lower than −80° C., the nanoparticles may not be brought into contact with the associative polymer-containing liquid well. If the temperature is higher than 50° C., the association of the associative polymer may be dissolved, and coordination may proceed.
[0058] (Step of Extracting Energy-Responsive Composition (S)) By reducing the solvent content, an energy-responsive composition (S) containing a plurality of energy-responsive protected particles, each containing nanoparticles Q and an associative polymer 40, is extracted from the mixture C. Preferred methods for reducing the solvent content include volatilizing the solvent under atmospheric pressure and volatilizing the solvent under reduced pressure. In this case, it is preferable to apply the mixture C onto a support.
[0059] The temperature at which the solvent is evaporated is preferably −80° C. or higher and 50° C. or lower, and more preferably −30° C. or higher and 40° C. or lower. If the temperature is lower than −80° C., the solvent may not evaporate efficiently. If the temperature is higher than 50° C., the association of the associative polymer may be dissolved, and coordination may proceed.
[0060] In the step of extracting the energy-responsive composition, it is preferable that adjacent pairs of the energy-responsive protected particles among the plurality of energy-responsive protected particles are in contact with each other by contacting the associative polymers 40 that they possess, and that the nanoparticles that they possess are spaced apart.
[0061] The step of extracting the energy responsive composition preferably includes removing the solvent 10 .
[0062] After the step of extracting the energy-responsive composition, a step of promoting coordination of the associative polymer with the nanoparticles by heating may be included, if necessary.
[0063] (Method for Producing Associative Polymer) A detailed description is given below of a method for producing a polymer compound that can be used as associative polymer 40. The method for producing the polymer compound is not particularly limited as long as it can produce the polymer with the above structure, but it can be produced, for example, by the following method (i) or (ii).
[0064] That is, the method (i) for producing a polymer compound includes a method of producing a monomer having a structural unit containing a polar group and then polymerizing the monomer, and the method (ii) for producing a polymer compound includes a method of synthesizing a polymer main chain and then bonding a polar group to the polymer main chain.
[0065] From the viewpoints of easy availability of monomers and control of the amount of functional groups, the method shown in (i) is preferred. Hereinafter, a method for synthesizing a polymer compound containing a zwitterionic group as a polar group using the method shown in (i) will be described in detail.
[0066] As a monomer for introducing a polar group into a polymer compound, a vinyl ether derivative, an acrylate derivative, a methacrylate derivative, an α-olefin derivative, an aromatic vinyl derivative, etc. From the viewpoint of ease of production of the monomer, it is preferable to use an acrylate derivative or a methacrylate derivative as such a monomer.
[0067] The corresponding acrylate derivatives or methacrylate derivatives can be produced by the method described in the following literature: K. Ishihara and two others, "Polymer Journal", (Japan), Society of Polymer Science, 1990, Vol. 22, pp. 355-360
[0068] The method for polymerizing the above monomers includes radical polymerization and ionic polymerization, and living polymerization can also be used for the purpose of controlling the molecular weight distribution and structure. From an industrial perspective, radical polymerization is preferably used.
[0069] Radical polymerization can be carried out by using a radical polymerization initiator, by irradiating with light such as radiation or laser light, by using a photopolymerization initiator in combination with light irradiation, by heating, etc. The radical polymerization initiator may be any one that can generate radicals and initiate a polymerization reaction, and is selected from compounds that generate radicals by the action of heat, light, radiation, an oxidation-reduction reaction, etc.
[0070] For example, azo compounds, organic peroxides, inorganic peroxides, organometallic compounds, photopolymerization initiators, etc. may be mentioned.
[0071] More specific examples include azo compounds such as 2,2'-azobisisobutyronitrile (AIBN) and 2,2'-azobis(2,4-dimethylvaleronitrile); organic peroxides such as benzoyl peroxide (BPO), tert-butyl peroxypivalate, and tert-butylperoxyisopropyl carbonate; inorganic peroxides such as potassium persulfate and ammonium persulfate; and redox initiators such as hydrogen peroxide-iron(II) salt systems, BPO-dimethylaniline systems, and cerium(IV) salt-alcohol systems. Examples of photopolymerization initiators include acetophenone systems, benzoin ether systems, and ketal systems. Two or more of these radical polymerization initiators may be used in combination.
[0072] The preferred temperature range for the polymerization temperature of the vinyl monomer varies depending on the type of polymerization initiator used and is not particularly limited, but polymerization is generally carried out at a temperature of −30° C. to 150° C., and a more preferred temperature range is 40° C. to 120° C.
[0073] The amount of the polymerization initiator used in this case is preferably 0.1 to 20 parts by mass per 100 parts by mass of the monomer, and the amount used is preferably adjusted so as to obtain a polymer compound having the target molecular weight distribution.
[0074] The polymerization method is not particularly limited and may be any of solution polymerization, suspension polymerization, emulsion polymerization, dispersion polymerization, precipitation polymerization, bulk polymerization, and the like.
[0075] The resulting polymer compound may be purified as needed. There are no particular limitations on the production method, and methods such as reprecipitation, dialysis, and column chromatography may be used.
[0076] The structure of the produced polymer compound can be identified by various instrumental analyses, such as nuclear magnetic resonance (NMR), gel permeation chromatography (GPC), and inductively coupled plasma atomic emission spectrometry (ICP-AES).
[0077] (Polymerizable Compound) Polymerization of the polymerizable compound is promoted by receiving energy such as light or heat, and the polymerizable compound becomes a component that imparts viscosity to the photoresponsive composition and hardens it. The polymerizable compound can be a radically polymerizable compound or a cationically polymerizable compound. These may be used alone or in combination of two or more. Furthermore, either a photopolymerizable compound or a thermally polymerizable compound can be used. In the present specification, the form in which a polymerizable compound is polymerized and the viscosity is increased may be referred to as a polymer.
[0078] Examples of the radical polymerizable compound that can be used include monofunctional (meth)acrylate compounds, bifunctional (meth)acrylate compounds, trifunctional or higher functional (meth)acrylate compounds, hydroxyl group-containing (meth)acrylate compounds, carboxy group-containing (meth)acrylate compounds, and vinyl compounds.
[0079] Examples of monofunctional (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, and 3,3,5-trimethylcyclohexyl acrylate. , tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, isobornyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, and cyclic trimethylolpropane formal (meth)acrylate can be used.
[0080] Examples of bifunctional (meth)acrylate compounds include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol 200 di(meth)acrylate, polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, and polyethylene glycol 600 Di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol 400 di(meth)acrylate, polypropylene glycol 700 di(meth)acrylate, neopentyl glycol di(meth)acrylate, neopentyl glycol PO-modified di(meth)acrylate, EO-modified bisphenol A di(meth)acrylate, PO-modified bisphenol A di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate can be used.
[0081] Examples of trifunctional or higher functional (meth)acrylate compounds that can be used include trimethylolpropane tri(meth)acrylate, trimethylolpropane EO-modified tri(meth)acrylate, trimethylolpropane PO-modified tri(meth)acrylate, glycerin propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and EO-modified pentaerythritol tetraacrylate.
[0082] Examples of vinyl compounds that can be used include vinyl acetate, vinyl benzoate, vinyl pivalate, vinyl butyrate, vinyl methacrylate, and N-vinylpyrrolidone.
[0083] The cationically polymerizable compound may be either a photopolymerizable compound or a thermally polymerizable compound. These may be used alone or in combination of two or more. Typical examples of the cationically polymerizable compound include epoxy compounds, oxacene compounds, and vinyl ether compounds.
[0084] The amount of the polymerizable compound including the radical polymerizable compound and the cationically polymerizable compound used is preferably 1 to 99 parts by mass, more preferably 3 to 90 parts by mass, and even more preferably 5 to 80 parts by mass, relative to the total parts by mass of the photoresponsive composition.
[0085] (Polymerization initiator) In a polymerization reaction, a polymerization initiator and a polymerizable compound are generally used in combination. The polymerization initiator is a compound that generates active species that initiate a polymerization reaction when irradiated with active energy rays or heat, and known polymerization initiators can be used. Examples of the main active species that initiate a polymerization reaction include radical polymerization initiators that generate radicals and cationic polymerization initiators that generate acids, and these may be used in combination. Examples of photoradical polymerization initiators that generate radicals when exposed to active energy rays include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl methyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butane, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl) acetophenones such as 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl]propanone, 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl]-2-methylpropan-1-one; benzoins such as benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; phosphines such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; and other phenyl glyoxylic methyl esters.
[0086] Among the photoradical polymerization initiators, acetophenones such as aminoketones, phosphines, and oxime ester compounds are preferred. These can be used alone or in combination depending on the properties desired for the cured product. When a radical polymerization initiator is used, the amount used is preferably 0.01 to 100 parts by mass, and more preferably 0.1 to 50 parts by mass, per 100 parts by mass of the total solid content in the composition.
[0087] (Other Additives) In this embodiment, the energy responsive composition may be mixed with an oxygen remover, an antioxidant, a scattering agent such as titanium oxide, a surfactant, an anti-mold agent, a light stabilizer, or other additives that impart various properties, a diluting solvent, etc., as needed.
[0088] Second Embodiment Energy responsive composition 100 according to a second embodiment will be described with reference to FIGS. 3A to 3C.
[0089] 3A to 3C show the form of energy-responsive composition 200 according to this embodiment extracted while supported on substrate 90 having support surface 90S. Figures 3B and 3C are two-sided views showing the supported form of energy-responsive composition 200 viewed macroscopically. Figure 3A is a microscopic enlarged partial view of Figure 3B.
[0090] The energy-responsive composition 100 includes a plurality of energy-responsive protected particles 150. Each of the energy-responsive protected particles 150 includes an energy-responsive nanoparticle 110 and an associative polymer 140 that has a main chain 120 including a plurality of carbons and a polar group 130 that is more polar than the main chain 120 and that is coordinated to the nanoparticle 110.
[0091] Among the multiple energy-responsive protected particles, a pair of adjacent energy-responsive protected particles (150, 150') are in contact with each other by the associative polymers (140, 140') that they possess being in contact with each other, and the nanoparticles (110, 110') that they possess are spaced apart from each other.
[0092] (Nanoparticles) The nanoparticles 110 in this embodiment are preferably nanoparticles containing nanocrystals having a perovskite crystal structure as allotropes, with the A site (monovalent cations), the B site (divalent cations), and the X site (monovalent anions including halide anions) as constituent components. Each constituent component may be the same as that of the nanoparticle Q shown in the first embodiment.
[0093] (Associative Polymer) In this embodiment, the associative polymer 140 has a main chain 120 containing multiple carbon atoms and polar groups 130 that are more polar than the main chain. Preferably, at least a portion of the associative polymer 140 is coordinated to the nanoparticles 110 so that the nanoparticles Q are protected on a particle-by-particle basis.
[0094] The main chain 120 is the longest series of covalently bonded atoms and may have side chains. The side chains may be linear, branched, or cyclic alkyl groups, linear, branched, or cyclic heteroalkyl groups, aryl groups, heteroaryl groups, aralkyl groups, or heteroaralkyl groups. Some of these groups may further have substituents.
[0095] The polar group 130 is at least one selected from the group consisting of strong acids such as sulfonic acid and phosphonic acid, strong bases such as quaternary ammonium cations, zwitterionic groups such as sulfobetaine, phosphobetaine, and carboxybetaine, and salts or ions thereof.
[0096] A copolymer obtained by polymerizing at least two types of monomers can be used as the associative polymer 140. The associative polymer 140 can be the same as the associative polymer 40 shown in the first embodiment.
[0097] Third Embodiment The energy responsive composition of the present invention can be applied to a quantum dot-containing wavelength conversion sheet (QD sheet), a quantum dot-containing wavelength conversion layer (QD-CC), and a quantum dot-containing electroluminescence (QD-EL) device.
[0098] Here, a QD-EL device to which the energy responsive composition according to the present invention is applied will be described.
[0099] The QD-EL device of the present invention comprises, for example, electrodes (cathode and anode), an electron injection / transport layer, an emitting layer, and a hole injection / transport layer. A surface treatment layer may be provided on any surface of the emitting layer.
[0100] (Electrode) The material of the electrode is not particularly limited, and for example, a material used in an organic electroluminescence (EL) element or the like can be suitably used. Examples include transparent conductive oxides such as indium tin oxide (ITO), metals such as Al, alloys of Ag, Pd, and Cu (APC electrode), alloys of Mg and Ag, and laminates (laminate electrodes) in which a metal layer and a transparent conductive oxide layer such as ITO are laminated. Of the anode and cathode, the electrode on the side from which light emitted from the light-emitting layer is extracted is preferably transparent.
[0101] The thickness of the anode is not particularly limited and may be, for example, 10 nm or more, 30 nm or more, or 50 nm or more, and may be 1000 nm or less, 500 nm or less, or 200 nm or less. The thickness of the cathode is not particularly limited and may be, for example, 10 nm or more, 30 nm or more, or 50 nm or more, and may be 1000 nm or less, 500 nm or less, or 200 nm or less.
[0102] (Hole Injection / Transport Layer) Materials used in organic electroluminescence (EL) can be suitably used for the hole injection / transport layer. Examples of organic materials include polyvinylcarbazole (PVK), poly(9,9-dioctylfluorene-co-N-(4-butylphenyl)-diphenylamine) (TFB), poly(bis(4-phenyl)(2,4,6-trimethylphenyl)amine) (PTAA), poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine] (poly-TPD), and poly(3,4-ethylenedioxythiophene):poly(styrenesulfonate) (PEDOT:PSS). Examples of inorganic materials include NiO, TiO2, and MoOx. These materials may be used alone or in combination of two or more.
[0103] The hole injection / transport layer may have a single layer structure or a laminated structure. In the case of a laminated structure, it may include a hole injection layer disposed on the anode side and a hole transport layer disposed on the light emitting layer side.
[0104] In the case of a single-layer structure, the thickness of the hole injection / transport layer is appropriately adjusted in consideration of the effects on hole injection, transport, and optical properties. For example, the lower limits of the thickness of the hole injection layer and the hole transport layer may be 10 nm and 20 nm, respectively, and the upper limits of the thickness of the hole injection layer and the hole transport layer may be 1000 nm and 500 nm, respectively.
[0105] (Light-emitting layer) The energy-responsive composition according to the present invention can be used as a light-emitting layer.
[0106] The thickness of the light-emitting layer is not particularly limited and may be, for example, 10 nm or more, 50 nm or more, or 75 nm or more, and may be 1000 nm or less, 500 nm or less, or 250 nm or less.
[0107] (Electron Injection / Transport Layer) Materials used in organic electroluminescence (EL) devices can be suitably used for the electron injection / transport layer. Examples of organic materials include LiF, 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene (TPBi), N,N'-di-1-naphthyl-N,N'-diphenylbenzidine (NPD), 4,4'-bis(N-carbazolyl)-1,1'-biphenyl (CBP), and 4,6-bis(3,5-di(pyridin-3-yl)phenyl)-2-methylpyrimidine (B3PyMPM). Examples of inorganic materials include a-ZSO (amorphous zinc silicate; Zn—Si—O), ZnO, and SnO. These materials may be used alone or in combination.
[0108] The electron injection / transport layer may have a single layer structure or a laminated structure. In the case of a laminated structure, it may include an electron injection layer disposed on the cathode side and an electron transport layer disposed on the light-emitting layer side.
[0109] In the case of a single-layer structure, the thickness of the electron injection / transport layer is not particularly limited and is appropriately adjusted in consideration of the influence on the electron injection property, transport property, and optical properties. For example, the lower limit of the thickness of the electron injection layer and the electron transport layer is 1 nm and 10 nm, respectively. The upper limit of the thickness of the electron injection layer and the electron transport layer is 1000 nm or less and 500 nm or less.
[0110] In the above description, the light-emitting element is mainly a bottom-emission type in which light is extracted from the anode side (substrate side), but is not limited to this. For example, the light-emitting element may be a top-emission type in which light is extracted from the cathode side (opposite substrate side).
[0111] ((Measurement Method)) Various physical properties can be measured as follows.
[0112] ((Disposition Density)) The placement density of the energy-responsive composition can be measured using a transmission electron microscope (TEM) or a scanning electron microscope (SEM) when observation from a perpendicular direction is possible. When observation from a perpendicular direction to the energy-responsive composition is not possible, measurement can be performed using a cross-sectional SEM. The placement density can be evaluated using, for example, the average inter-surface distance of particles, the particle occupancy rate per unit area in an image, etc. The average inter-surface distance of particles can be determined by selecting, for example, 100 particles using image processing software, measuring the shortest distance between each particle, and averaging the measured values.
[0113] The relative arrangement density can also be calculated from the amount of light absorbed or emitted per unit volume of the film. Since the amount of light emitted varies depending on the luminescence quantum yield (PLQY), it is preferable to calculate it from the amount of absorption.
[0114] ((Stability Evaluation)) The stability of the energy responsive composition can be evaluated by, for example, PLQY evaluation and evaluation of the fusion rate between nanoparticles by TEM observation.
[0115] ((Molecular Weight Distribution Measurement)) The molecular weight distribution of the associative polymer can be calculated by gel permeation chromatography (GPC) in terms of monodisperse polymethyl methacrylate. Measurement of the molecular weight by GPC can be performed, for example, as follows.
[0116] The sample is added to the eluent below so that the sample concentration becomes 1% by mass, and the solution is left to stand at room temperature for 24 hours to dissolve. The solution is then filtered through a solvent-resistant membrane filter with a pore size of 0.45 μm to obtain the sample solution, which is measured under the following conditions: Apparatus: Agilent 1260 infinity system (Agilent Technologies) Column: PFG analytical linear M columns (PSS) Eluent: 2,2,2-trifluoroethanol Flow rate: 0.2 ml / min Oven temperature: 40°C Sample injection volume: 20 μL
[0117] The molecular weight distribution of the sample is calculated using a molecular weight calibration curve prepared using a standard polymethyl methacrylate resin (EasiVial PM Polymer Standard Kit, manufactured by Agilent Technologies).
[0118] (Structural Analysis of Associative Polymers) The structural analysis of associative polymers can be carried out using nuclear magnetic resonance (NMR). For example, using an ECA-600 (600 MHz) manufactured by JEOL Ltd., 1 H-NMR, and 13 C-NMR spectrum measurement is performed in a deuterated solvent containing tetramethylsilane as an internal standard at 25°C. The chemical shift value is read as a ppm shift value (δ value) with the internal standard tetramethylsilane set as 0.
[0119] (Method for Confirming Coordination of Associative Polymer to Nanoparticles) Whether or not the associative polymer 40 is coordinated to the nanoparticles Q can be confirmed by nuclear magnetic resonance (NMR). For example, using an ECA-600 (600 MHz) manufactured by JEOL Ltd., 1 H-NMR measurement is carried out. 1 Coordination can be confirmed by the fact that the δ value of the H signal shifts from the δ value in the case of the associative polymer alone and the half-value width changes.
[0120] ((Analysis of the Association State of Associative Polymer)) The association state of the associative polymer can be analyzed using NMR or dynamic light scattering (DLS). When using NMR, for example, an ECA-600 (600 MHz) manufactured by JEOL Ltd. is used. 1 H-NMR is measured. When there is association, the chemical shift value of the polar group signal changes from the value in the non-associated state. Furthermore, when there is association, the molecular movement is restricted, so the spectrum is observed to be broadened overall. If necessary, relaxation time measurement can be performed to analyze the association state in more detail. When DLS is used, the association state can be analyzed from the particle size. When the associative polymer is intramolecularly associated, a particle size of about several nm is observed.
[0121] (Crystalline Structure (Crystalline Phase) Analysis of Nanoparticles) Analysis of the crystalline structure (crystalline phase) and composition of nanoparticles can be performed using X-ray diffraction (XRD). For example, the crystalline structure and composition can be analyzed by measuring an X-ray diffraction pattern using a RINT 2100 (manufactured by Rigaku) and comparing it with diffraction patterns in a database. Depending on the shape and size of the specimen to be analyzed, electron diffraction (ED) attached to a cross-sectional TEM may be employed.
[0122] ((Nanoparticle Composition Analysis)) The composition of nanoparticles can also be analyzed using XPS and ICP optical emission spectroscopy. The molar ratio of A and B can be measured from the signal intensity of XPS, and the concentration of X can be measured from the emission intensity of ICP optical emission spectroscopy (for example, CIROS CCD (manufactured by SPECTRO)).
[0123] ((Amount of Ligand and Associative Polymer Relative to Nanoparticles)) The amount of ligand and associative polymer relative to the amount of nanoparticles can be determined by TG-DTA measurement and NMR measurement. For example, the amount of nanoparticles in the energy-responsive composition is measured by TG-DTA measurement. Next, the amount of ligand and the amount of associative polymer in the energy-responsive composition are determined by NMR measurement, thereby making it possible to determine the amount of ligand and associative polymer relative to nanoparticles.
[0124] ((Amount of Polar Groups in Associative Polymer)) The amount of polar groups in the associative polymer can be determined by NMR measurement. For example, 1H-NMR is measured using an ECA-600 (600 MHz) manufactured by JEOL Ltd. The amount of polar groups in the associative polymer is calculated by comparing the signal intensity derived from the polar groups with the signal intensity derived from other parts.
[0125] ((Number of mmoles of polar groups per 1 g of nanoparticles)) The number of mmoles of polar groups per 1 g of nanoparticles can be calculated from the amount of nanoparticles determined by the above method, the amount of associative polymer, and the amount of polar groups in the associative polymer.
[0126] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.
[0127] [Production of Associative Polymer A] A reaction vessel equipped with a condenser, stirrer, thermometer, and nitrogen inlet tube was prepared. 5.9 parts of 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonic acid, 48.0 parts of hexyl methacrylate, 3.9 parts of azobisisobutyronitrile, and 900 parts of 2,2,2-trifluoroethanol were charged into the reaction vessel. Nitrogen bubbling was then performed on the reaction vessel for 30 minutes. The resulting reaction mixture was heated at 65°C for 8 hours under a nitrogen atmosphere to complete the polymerization reaction. After cooling the reaction solution to room temperature, 300 parts of water was added to precipitate the product. After centrifugation, the supernatant was removed. The solvent was removed by distillation under reduced pressure, followed by drying under reduced pressure at 50°C and 0.1 kPa or less to obtain Associative Polymer A. NMR analysis confirmed that the structural unit having a polar group accounted for 7 mol% of all monomer units. Furthermore, GPC analysis revealed that the weight average molecular weight (Mw) was 13,200.
[0128] [Production of Associative Polymer b] Associative polymer b was produced in the same manner as associative polymer a, except that the amount of 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonic acid was changed from 5.9 parts to 15.2 parts and the amount of hexyl methacrylate was changed from 48.0 parts to 42.3 parts.
[0129] The structures, compositions and molecular weights of the produced associative polymers a to b are shown in Table 1.
[0130]
[0131] [Preparation of associative polymer-containing liquid] (Association liquid a of associative polymer a in toluene) 0.8 parts of associative polymer a and 99.2 parts of toluene were charged into a reaction vessel equipped with a stirrer, thermometer, and reflux condenser, and the temperature was raised to 80°C and heated for 5 minutes. After confirming that the associative polymer a was completely dissolved, the mixture was rapidly cooled to room temperature to obtain an association liquid a of associative polymer a in toluene. DLS measurement confirmed that unimer micelles with a particle size of 5 nm had been formed.
[0132] (Association Solution b-1 of Associative Polymer b in Toluene) Association Solution b-1 of Associative Polymer b in Toluene was prepared in the same manner as for Associative Polymer a in Toluene, except that Associative Polymer b was used instead of Associative Polymer a. DLS measurement confirmed that unimer micelles with a particle size of 4 nm were formed.
[0133] (Association Solution b-2 of Associative Polymer b in Chloroform) 0.8 parts of associative polymer b and 99.2 parts of chloroform were placed in a reaction vessel equipped with a stirrer, a thermometer, and a reflux condenser, and the mixture was heated to 60°C and heated for 5 minutes. After rapid cooling to room temperature, an association solution b-2 of associative polymer b in chloroform was obtained.
[0134] [Production of Nanoparticles Q-1] 10 parts of cesium carbonate, 27 parts of oleic acid, and 385 parts of 1-octadecene were placed in a flask, heated to 120°C, and degassed for 30 minutes using a vacuum pump. The mixture was further heated to 150°C under a dry nitrogen stream and maintained for 30 minutes to obtain a cation raw material solution.
[0135] Separately, 10 parts of lead(II) bromide and 494 parts of 1-octadecene were placed in a flask, heated to a liquid temperature of 120°C, and degassed for 1 hour using a vacuum pump. 89 parts of oleic acid and 31 parts of oleylamine were added, and the mixture was further degassed for 30 minutes using a vacuum pump. Thereafter, the nitrogen flow was replaced and the liquid temperature was raised to 185°C.
[0136] 40 parts of the cation source liquid was added, and after 5 seconds, the mixture was cooled on ice. 2000 parts of ethyl acetate was added, and the mixture was centrifuged to remove the supernatant. The resulting residue was dispersed in toluene to adjust the solid concentration to 1% by weight, and CsPbBr 3 A dispersion of nanoparticles Q-1 having a perovskite crystal structure was obtained. The ratio of nanoparticles Q in the solid content measured by TG-DTA was 53 wt %.
[0137] [Production of Nanoparticles Q-2] CsPb(Br / I) was prepared in the same manner as in the luminescent nanocrystal dispersion a, except that 3.2 parts of lead(II) bromide and 9.3 parts of lead(II) iodide were used instead of 10 parts of lead(II) bromide. 3 A dispersion of nanoparticles Q-2 having a perovskite crystal structure was obtained. The ratio of nanoparticles Q to the solid content measured by TG-DTA was 52 wt %.
[0138] Example 1 100 parts of dispersion a of nanoparticles Q-1 were placed in a container, and the solvent was distilled off under reduced pressure. 100 parts of association solution a of associative polymer a in toluene were added and re-dispersed. 3 The mixture was spin-coated on a cleaned 2 cm x 2 cm glass substrate at 1000 rpm for 20 seconds to obtain Energy Responsive Composition 100-1.
[0139] Examples 2 to 4, Comparative Example 2 Energy responsive compositions 100-2 to 100-4 and 100-6 were obtained in the same manner as in Example 1, except that the types of nanoparticles Q, associative polymer and associative liquid were changed as shown in Table 2.
[0140] Comparative Example 1 100 parts of dispersion a of nanoparticles Q-1 were placed in a container, and the solvent was distilled off under reduced pressure. 100 parts of association solution a of associative polymer a in toluene were added and re-dispersed, and the mixture was heated at 50°C for 20 minutes to complete the coordination. 3 The mixture was spin-coated on a cleaned 2 cm x 2 cm glass substrate at 1000 rpm for 20 seconds to obtain Energy Responsive Composition 100-5.
[0141]
[0142] [Evaluation] [Nanoparticle Density Evaluation 1] The density of the nanoparticles was evaluated based on the amount of light absorbed by the energy responsive compositions 100-1 to 100-6.
[0143] The measurement conditions and evaluation criteria are shown below.
[0144] <Measurement conditions> Measurement device: Absolute PL quantum yield measurement device C9920-03 (manufactured by Hamamatsu Photonics) Excitation light wavelength: 460 nm Excitation light integration range: Excitation light wavelength ±10 nm
[0145] <Evaluation criteria> A: Absorbance is 6×10 6 B: Absorbance is 4 x 10 6 That's it, 6 x 10 6 C: Absorbance is less than 4 x 10 6 less than
[0146] The evaluation results are shown in Table 3.
[0147] [Stability Evaluation 1] Each sample was allowed to stand in air for 7 days, and then PLQY was measured to evaluate stability.
[0148] The measurement conditions and evaluation criteria are shown below.
[0149] <Measurement conditions> Measurement device: Absolute PL quantum yield measurement device C9920-03 (manufactured by Hamamatsu Photonics) Excitation light wavelength: 460 nm Excitation light integration range: Excitation light wavelength ±10 nm Emission light integration range: (Excitation light wavelength + 20) nm to 770 nm
[0150] <Evaluation criteria> A: PLQY is 70% or more B: PLQY is 50% or more but less than 70% C: PLQY is 50% or less
[0151] The evaluation results are shown in Table 3.
[0152] [Nanoparticle Density Evaluation 2] Each of the energy responsive compositions 100-1 to 100-6 was diluted 20 times and 3 μL was applied to a support film (Hi-Res Carbon HRC-C10). The solvent was evaporated at room temperature and TEM observation was performed using a Technai F30 (manufactured by FEI). The average inter-surface distance for 100 particles was calculated from the TEM image, and the density of the nanoparticles was evaluated according to the following criteria: A: Average inter-surface distance is 5 nm or less B: Average inter-surface distance is more than 5 nm and less than 15 nm C: Average inter-surface distance is more than 15 nm
[0153] The evaluation results are shown in Table 3.
[0154] [Stability Evaluation 2] 100 particles were selected from the TEM image, and the stability of the nanoparticles was evaluated according to the following criteria: A: 5 or less particles showing fusion B: 5 to 10 particles showing fusion C: 10 or more particles showing fusion
[0155] The evaluation results are shown in Table 3.
[0156]
[0157] According to Table 3, energy-responsive compositions 100-1 to 100-4 according to Examples 1 to 4 have high nanoparticle density and high stability. On the other hand, energy-responsive composition 100-5 according to Comparative Example 1 has high stability but low nanoparticle density. Furthermore, energy-responsive composition 100-6 according to Comparative Example 2 has high nanoparticle density but low stability.
[0158] These results indicate that the associative polymer forms unimeric micelles in low-polarity solvents, and coordination does not occur in the dispersion state, but rather coordination proceeds after the nanoparticles are densely arranged during film formation.
[0159] The present invention is not limited to the above-described embodiments, and various modifications and variations can be made without departing from the spirit and scope of the present invention. Therefore, the following claims are appended to apprise the public of the scope of the present invention.
[0160] This application claims priority based on Japanese Patent Application No. 2023-083371, filed on May 19, 2023, the entire contents of which are incorporated herein by reference.
[0161] 100, S Energy responsive composition 1000 Manufacturing method of energy responsive composition 10 Solvent 20 Main chain 30 Polar group 40 Associative polymer 50, P Polymer-containing liquid 60, Q Nanoparticles 70, R Mixed liquid 80 Energy responsive protected particles
Claims
1. A method for producing an energy responsive composition, comprising the steps of: preparing a polymer-containing liquid containing a solvent exhibiting a relative dielectric constant of a predetermined value or less, and an associative polymer having a main chain containing multiple carbons and a polar group that is more polar than the main chain, and which self-associates in the solvent; contacting energy responsive nanoparticles with the polymer-containing liquid to prepare a mixed liquid; and extracting an energy responsive composition containing a plurality of energy responsive protected particles, each of which includes nanoparticles and an associative polymer, from the mixed liquid by reducing the content of the solvent.
2. A method for producing an energy responsive composition as described in claim 1, wherein the step of extracting the energy responsive composition is such that adjacent pairs of energy responsive protected particles among a plurality of energy responsive protected particles are in contact with each other by contacting the associative polymers they possess, and the nanoparticles they possess are spaced apart.
3. A method for producing an energy responsive composition according to claim 1 or 2, wherein the step of extracting the energy responsive composition includes a step of removing the solvent.
4. A method for producing an energy responsive composition according to claim 1 or 2, wherein the nanoparticles comprise a perovskite crystal structure.
5. An energy-responsive composition comprising a plurality of energy-responsive protected particles each having an energy-responsive nanoparticle and an associative polymer having a main chain containing a plurality of carbons and a polar group more polar than the main chain and coordinated to the nanoparticle, wherein adjacent pairs of the plurality of energy-responsive protected particles are in contact with each other by contacting the associative polymers possessed by each of the energy-responsive protected particles, and the nanoparticles possessed by each of the energy-responsive protected particles are spaced apart.
6. The energy responsive composition of claim 5, wherein the nanoparticles comprise a perovskite crystal structure.
7. An energy-responsive composition according to claim 5 or 6, wherein the ligand is coordinated to the nanoparticles so that the nanoparticles are protected on a particle-by-particle basis.
8. The energy responsive composition of claim 5 or 6, wherein the plurality of energy responsive protected particles are supported on a substrate having a support surface.
Citation Information
Patent Citations
Molecular complex containing photo-chromic compound
JP1995026253A
Coated metal oxide nanoparticles and method of making same
JP2008544936A
Perovskite / Polymer Composite Light-Emitting Materials, Manufacturing Methods and Applications
JP2018522959A
Luminescent material, luminescent material composition, luminescence conversion member, backlight unit, and liquid crystal display device
JP2021091870A
Composition and optical functional film including same
WO2016151933A1