Leader tape

The leader tape with enhanced breaking strength and abrasivity, using barium ferrite magnetic powder and a multi-layer structure, addresses the issue of head damage and reliability in magnetic tape loading/unloading, ensuring effective and error-free operation.

WO2024241930A1PCT designated stage expired Publication Date: 2024-11-28SONY GROUP CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017571
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-13
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional leader tapes cause head damage and reduce error rates in magnetic tape loading/unloading due to small scratches, and adjusting process conditions to prevent scratches often renders magnetic tape unusable.

Method used

A leader tape with a breaking strength of 28N or more and abrasivity of 17.5 μm or less, incorporating a magnetic layer with barium ferrite magnetic powder and optimized calendering conditions to adjust strength and abrasivity, and a multi-layer structure including a base and back layer to enhance reliability and prevent head damage.

Benefits of technology

The solution significantly improves the reliability of magnetic tape loading/unloading while preventing head damage by maintaining the required breaking strength and abrasivity levels, ensuring reliable operation without malfunctioning during 20,000 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017571_28112024_PF_FP_ABST
    Figure JP2024017571_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present technology is to provide a leader tape that inhibits head damage caused by small scratches. The present technology provides a leader tape having a breaking strength of 28 N or more and having an abrasivity of 17.5 μm or less with respect to a plate of 81% Ni and 19% Fe over 30 cycles. The leader tape may have an abrasivity of 16.4 μm or less with respect to a plate of 81% Ni and 19% Fe over 30 cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Leader tape

[0001] The present technology relates to leader tapes.

[0002] For example, as a magnetic tape cartridge for data storage used as data backup for computers, etc., a single-reel magnetic tape cartridge has conventionally been used, which comprises a cartridge body formed by joining an upper shell and a lower shell, and a single tape reel rotatably housed within the cartridge body and wound with magnetic tape.

[0003] There are various types of single-reel magnetic tape cartridges. Among them, there is one that has an engaged member that is connected to the feeding end of the magnetic tape for tape withdrawal and engages with the tape withdrawal means on the tape drive side to guide the magnetic tape into the tape drive. This engaged member, for example, has a roughly U-shape and is connected to the feeding end of the magnetic tape via a leader tape (see Patent Document 1 below).

[0004] One end of the leader tape is wound around the shaft of the member to be engaged and turned over, and then the turned over portion is welded or glued to the surface of the tape.

[0005] The opposite end of the leader tape is butt-joined to the leading end (feed-out end) of the magnetic tape by a splicing tape.

[0006] Japanese Patent Application Laid-Open No. 2001-357655

[0007] The objective of this technology is to provide a leader tape that suppresses head damage caused by small scratches.

[0008] The present technology provides a leader tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 round trips against a Ni 81% / Fe 19% plate. The abrasivity of 16.4 μm or less after 30 round trips against a Ni 81% / Fe 19% plate may be. The breaking strength may be 35 N or more. A leader tape according to the present technology may include a magnetic layer and an underlayer, in this order. The magnetic layer may include barium ferrite magnetic powder. The average thickness (average total thickness) may be 16.0 μm or more. The average thickness of the underlayer may be 1.25 μm or more. The surface roughness Rab of the magnetic layer surface may be 5.0 nm or more. The average thickness of the underlayer may be 1.35 μm or more. The abrasivity after 30 double strokes against a Ni81% / Fe19% plate may be 14.5 μm or less. The abrasivity after 30 double strokes against a Ni81% / Fe19% plate may be 12 μm or less. The breaking strength may be 40 N or more. The present technology also provides a magnetic recording medium including a magnetic tape having a leader tape and a data recording write area, which has a breaking strength of 28 N or more and an abrasivity after 30 double strokes against a Ni81% / Fe19% plate of 17.5 μm or less. The present technology also provides a magnetic recording cartridge containing a leader tape and a magnetic tape having a data recording write area joined together, the leader tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 round trips against a Ni81% / Fe19% plate.

[0009] FIG. 1 is a cross-sectional view showing the configuration of a leader tape according to an embodiment of the present technology. FIG. 2 is a schematic diagram showing the relationship between the leader tape LT and a measuring machine 21 to which an abrasicity bar A is attached. FIG. 3 is a schematic diagram showing a Knoop indenter. FIG. 4 is a schematic diagram showing an indentation 22 made on the side surface of the abrasicity bar A that contacts the leader tape LT. FIG. 5 is a diagram showing an example of the shape of magnetic powder particles. FIG. 6 is an example of a TEM photograph of a sample cross section. FIG. 7 is another example of a TEM photograph of a sample cross section. FIG. 8 is an exploded perspective view showing an example of the configuration of a magnetic recording cartridge. FIG. 9 is a diagram showing the relationship between the number of cycles and load / unload time. FIG. 10 is a diagram showing the relationship between the number of cycles and load / unload time.

[0010] Preferred embodiments for carrying out the present technology will be described below. Note that the embodiments described below are representative embodiments of the present technology, and the scope of the present technology is not limited to these embodiments.

[0011] The present technology will be described in the following order: 1. Description of the present technology 2. One embodiment of the present technology (1) Structure of leader tape (2) Description of each layer (3) Physical properties and structure (4) Manufacturing method of leader tape (5) One embodiment of magnetic recording cartridge 3. Examples

[0012] In this specification, unless a measurement environment is specifically stated in connection with the explanation of the measurement method, the measurement is performed in an environment of 25°C ± 2°C and 50% RH ± 5% RH.

[0013] 1. Description of the technology

[0014] Next-generation magnetic recording media uses highly sensitive TMR heads. Even small scratches on these TMR heads can cause head damage, resulting in a lower error rate. With conventional leader tapes, even if the magnetic tape can be loaded and unloaded (retracted and wound), small scratches can cause head damage, resulting in a lower error rate. Furthermore, with conventional leader tapes, changing the process conditions to prevent scratches can make it impossible to load and unload the magnetic tape.

[0015] The inventors have discovered that adjusting the breaking strength of the leader tape can improve the reliability of loading and unloading (pulling out and rewinding) the magnetic tape, and that head damage can be controlled by adjusting the abrasiveness, which is related to the abrasive force of the leader tape. More specifically, the inventors have discovered that using small-particle-size barium ferrite magnetic powder and small-particle-size alumina particles and optimizing process conditions (calendering conditions) can adjust the breaking strength and the abrasiveness, which is related to the abrasive force. It is necessary to appropriately adjust the calendering conditions to prevent a decrease in breaking strength due to thermal load.

[0016] The breaking strength of the leader tape according to the present technology can be 28 N or more, preferably 35 N or more, more preferably 38 N or more, even more preferably 40 N or more, and even more preferably 41 N or more. Furthermore, from the viewpoint of improving the reliability of loading / unloading (unwinding / unwinding) the magnetic tape, there is no particular upper limit to the breaking strength. The method for measuring the breaking strength will be explained in 2.(3) below.

[0017] From the viewpoint of suppressing head damage, the abrasivity of the leader tape according to the present technology after 30 round trips on a Ni81% / Fe19% plate can be 17.5 μm or less, preferably 16.4 μm or less, more preferably 15.4 μm or less, even more preferably 14.5 μm or less, 14.4 μm or less, and even more preferably 13.4 μm or less, 12 μm or less. The method for measuring the abrasivity after 30 round trips on a Ni81% / Fe19% plate will be explained in 2.(3) below.

[0018] The leader tape according to the present technology includes a magnetic layer and an underlayer in this order. Furthermore, the leader tape according to the present technology may include a magnetic layer, an underlayer, a base layer, and a back layer in this order.

[0019] The leader tape according to the present technology may preferably be a long leader tape.

[0020] In the leader tape according to the present technology, from the viewpoint of suppressing an increase in abrasivity due to the roughness of the base layer, the average thickness of the underlayer is preferably 1.25 μm or more, more preferably 1.30 μm or more, even more preferably 1.35 μm or more, and still more preferably 1.40 μm or more, and the average thickness of the underlayer is preferably 1.60 μm or less, more preferably 1.55 μm or less, and even more preferably 1.50 μm or less. A method for measuring the average thickness of the underlayer will be described below in 2.(3).

[0021] From the viewpoint of adjusting the appropriate abrasiveness by the average thickness of the underlayer, the average thickness (average total thickness) t of the leader tape according to the present technology is T is preferably 17.7 μm or less, more preferably 17.5 μm or less, even more preferably 17.3 μm or less, and still more preferably 17.1 μm or less, and the average thickness (average total thickness) t of the leader tape T The average thickness (average total thickness) t of the leader tape is preferably 16.0 μm or more, more preferably 16.3 μm or more, even more preferably 16.5 μm or more, and still more preferably 16.8 μm or more. T The measurement method will be explained in 2. (3) below.

[0022] In a leader tape according to the present technology, the average thickness of the magnetic layer is preferably 0.060 μm or more, more preferably 0.063 μm or more, even more preferably 0.066 μm or more, and even more preferably 0.069 μm or more, from the viewpoint of suppressing an increase in abrasivity due to the roughness of the base layer. Furthermore, from the viewpoint of preventing an increase in abrasivity and damage to the magnetic head, the average thickness of the magnetic layer is preferably 0.080 μm or less, more preferably 0.077 μm or less, even more preferably 0.074 μm or less, and even more preferably 0.071 μm or less. The method for measuring the average thickness of the magnetic layer will be described below in 2.(3).

[0023] The average thickness of the base layer of the leader tape according to the present technology is preferably 14.0 μm or more, more preferably 14.2 μm or more, even more preferably 14.4 μm or more, still more preferably 14.6 μm or more, and is preferably 16.0 μm or less, more preferably 15.8 μm or less, even more preferably 15.6 μm or less, still more preferably 15.4 μm or less. The method for measuring the average thickness of the base layer will be explained in 2.(3) below.

[0024] The average thickness of the back layer of the leader tape according to the present technology is preferably 0.30 μm or more, more preferably 0.35 μm or more, even more preferably 0.40 μm or more, still more preferably 0.45 μm or more, and is preferably 0.65 μm or less, more preferably 0.60 μm or less, even more preferably 0.55 μm or less, still more preferably 0.50 μm or less. The method for measuring the average thickness of the back layer will be explained in 2.(3) below.

[0025] From the viewpoint of improving the reliability of loading / unloading (pulling out / winding) the magnetic tape, the leader tape according to the present technology has a surface roughness Rab of the magnetic layer surface of preferably 5.0 nm or more, more preferably 5.2 nm or more, even more preferably 5.5 nm or more, and still more preferably 5.7 nm or more, and the surface roughness Rab of the magnetic layer surface is preferably 8.0 nm or less, more preferably 7.5 nm or less, even more preferably 7.0 nm or less, and still more preferably 7.0 nm or less. The method for measuring the surface roughness Rab of the magnetic layer surface will be explained in 2.(3) below.

[0026] The magnetic layer of the leader tape according to the present technology may contain magnetic powder. The magnetic powder may be preferably barium ferrite magnetic powder. The average particle volume of the barium ferrite magnetic powder is preferably 2000 nm. 3 or less, more preferably 1800 nm 3 or less, and more preferably 1600 nm 3 The average particle volume within the above range can provide a smooth surface for the leader tape. The average particle volume of the barium ferrite magnetic powder is preferably 500 nm or less. 3More preferably, 800 nm or more 3 More preferably, 1000 nm or more 3 or more, and even more preferably 1200 nm 3 The method for measuring the average particle volume of the barium ferrite magnetic powder will be explained in 2.(3) below.

[0027] In the leader tape according to the present technology, the range of the electrical resistance value on the surface of the magnetic layer is preferably 1×10 12 The electrical resistance may be less than Ω / sq. The method for measuring the electrical resistance will be explained in 2.(3) below.

[0028] 2. Embodiments of the present technology

[0029] (1) Leader tape structure

[0030] First, the configuration of a leader tape 10 according to an embodiment of the present technology will be described with reference to Fig. 1. As shown in Fig. 1, the leader tape 10 includes a long base layer (also referred to as a substrate) 11, an underlayer 12 provided on one main surface of the base layer 11, a magnetic layer 13 provided on the underlayer 12, and a back layer 14 provided on the other main surface of the base layer 11. Hereinafter, of the two main surfaces of the leader tape 10, the surface on which the magnetic layer 13 is provided will be referred to as the magnetic surface, and the surface opposite to the magnetic surface (the surface on which the back layer 14 is provided) will be referred to as the back surface.

[0031] The leader tape 10 has a long shape and runs in the longitudinal direction during recording and reproduction.

[0032] (2) Explanation of each layer

[0033] (base layer)

[0034] The base layer 11 can function as a support for the leader tape 10 and can be, for example, a flexible, long, non-magnetic substrate, particularly a non-magnetic film. The base layer 11 can contain, for example, at least one of polyester resins, polyolefin resins, cellulose derivatives, vinyl resins, aromatic polyether ketone resins, and other polymer resins. When the base layer 11 contains two or more of the above materials, the two or more materials can be mixed, copolymerized, or laminated.

[0035] The polyester-based resin may be, for example, one or a mixture of two or more of PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PBT (polybutylene terephthalate), PBN (polybutylene naphthalate), PCT (polycyclohexylene dimethylene terephthalate), PEB (polyethylene-p-oxybenzoate), and polyethylene bisphenoxycarboxylate. According to a preferred embodiment of the present technology, the base layer 11 may be formed from PET or PEN.

[0036] The polyolefin resin may be, for example, one or a mixture of two or more of PE (polyethylene) and PP (polypropylene).

[0037] The cellulose derivative may be, for example, one or a mixture of two or more of cellulose diacetate, cellulose triacetate, CAB (cellulose acetate butyrate), and CAP (cellulose acetate propionate).

[0038] The vinyl resin may be, for example, one or a mixture of two or more of PVC (polyvinyl chloride) and PVDC (polyvinylidene chloride).

[0039] The aromatic polyetherketone resin may be, for example, one or a mixture of two or more of PEK (polyetherketone), PEEK (polyetheretherketone), PEKK (polyetherketoneketone), and PEEKK (polyetheretherketoneketone). According to a preferred embodiment of the present technology, the base layer 11 may be formed from PEEK.

[0040] The other polymer resin may be, for example, one or a mixture of two or more of PA (polyamide, nylon), aromatic PA (aromatic polyamide, aramid), PI (polyimide), aromatic PI (aromatic polyimide), PAI (polyamideimide), aromatic PAI (aromatic polyamideimide), PBO (polybenzoxazole, e.g., Zylon (registered trademark), polyether, polyetherester, PES (polyethersulfone), PEI (polyetherimide), PSF (polysulfone), PPS (polyphenylene sulfide), PC (polycarbonate), PAR (polyarylate), and PU (polyurethane).

[0041] (magnetic layer)

[0042] The magnetic layer 13 may contain magnetic powder. The magnetic powder may preferably contain barium ferrite magnetic powder. In addition to the barium ferrite magnetic powder, the magnetic layer 13 may also contain abrasive particles and conductive particles. In addition to the above components, the magnetic layer 13 may further contain a binder and additives.

[0043] (Magnetic powder)

[0044] Examples of magnetic particles constituting the magnetic powder contained in the magnetic layer 13 include, but are not limited to, hexagonal ferrite, barium ferrite (BaFe), Co ferrite, and strontium ferrite. The magnetic powder may be one of these, or a combination of two or more. Particularly preferably, the magnetic powder may include barium ferrite magnetic powder, cobalt ferrite magnetic powder, or strontium ferrite magnetic powder. These magnetic particles may be appropriately selected by those skilled in the art based on factors such as the manufacturing method of the magnetic layer 13.

[0045] The average particle size (average maximum particle size) D of the magnetic powder can be preferably 22 nm or less, more preferably 8 nm or more and 22 nm or less, and even more preferably 10 nm or more and 20 nm or less.

[0046] The average particle size D of the magnetic powder is determined as follows. First, the magnetic recording medium 10 to be measured is processed by a focused ion beam (FIB) method or the like to prepare a thin section, and the cross section of the thin section is observed by a TEM. Next, 500 ε-iron oxide particles are randomly selected from the TEM photograph, and the maximum particle size d of each particle is measured. max The maximum particle size d of the magnetic powder is measured. max The particle size distribution of the maximum particle size d max " means the so-called maximum Feret diameter, specifically the maximum distance between two parallel lines drawn from any angle so as to be tangent to the contour of the ε-iron oxide particle. Then, the calculated maximum particle size d max From the particle size distribution, the maximum particle size d max The median diameter (50% diameter, D50) is determined and used as the average particle size (average maximum particle size) D of the magnetic powder.

[0047] The shape of the magnetic powder is preferably at least one of plate-like and rectangular. The shape of the magnetic powder depends on the crystal structure of the magnetic particles. Examples of plate-like magnetic powder include BaFe and strontium ferrite, which have a hexagonal plate-like shape. Examples of rectangular-shaped magnetic powder include cobalt ferrite, which has a cubic shape.

[0048] According to another preferred embodiment of the present technology, the magnetic powder may include barium ferrite (BaFe) magnetic powder. The barium ferrite magnetic powder includes magnetic particles of iron oxide having barium ferrite as a main phase (hereinafter referred to as "barium ferrite particles"). The barium ferrite magnetic powder can achieve a smooth surface for the leader tape. From this perspective, barium ferrite magnetic powder is preferred as the magnetic powder.

[0049] The average particle size of the barium ferrite magnetic powder can be preferably 50 nm or less, more preferably 10 nm or more and 40 nm or less, and even more preferably 12 nm or more and 25 nm or less.

[0050] According to yet another preferred embodiment of the present technology, the magnetic powder may be cobalt ferrite magnetic powder. The cobalt ferrite magnetic powder includes magnetic particles of iron oxide having cobalt ferrite as a main phase (hereinafter referred to as "cobalt ferrite magnetic particles"). The cobalt ferrite magnetic particles preferably have uniaxial anisotropy. The cobalt ferrite magnetic particles have, for example, a cubic or approximately cubic shape. The cobalt ferrite is cobalt ferrite containing Co. The cobalt ferrite may further include one or more elements selected from the group consisting of Ni, Mn, Al, Cu, and Zn in addition to Co.

[0051] Cobalt ferrite has, for example, an average composition represented by the following formula (1): Co x M y Fe 2 O z ... (1) (In formula (1), M is, for example, one or more metals selected from the group consisting of Ni, Mn, Al, Cu, and Zn. x is a value within the range of 0.4≦x≦1.0. y is a value within the range of 0≦y≦0.3. However, x and y satisfy the relationship (x+y)≦1.0. z is a value within the range of 3≦z≦4. A part of Fe may be substituted with another metal element.)

[0052] The average particle size of the cobalt ferrite magnetic powder may be preferably 25 nm or less, more preferably 23 nm or less.

[0053] According to yet another preferred embodiment of the present technology, the magnetic powder may include a powder of nanoparticles containing hexagonal ferrite (hereinafter referred to as "hexagonal ferrite particles"). The hexagonal ferrite particles have, for example, a hexagonal plate shape or an approximately hexagonal plate shape. The hexagonal ferrite may preferably contain at least one of Ba, Sr, Pb, and Ca, more preferably at least one of Ba and Sr. Specifically, the hexagonal ferrite may be, for example, barium ferrite or strontium ferrite. Barium ferrite may further contain at least one of Sr, Pb, and Ca in addition to Ba. Strontium ferrite may further contain at least one of Ba, Pb, and Ca in addition to Sr. More specifically, the hexagonal ferrite may be represented by the general formula MFe 12 O 19 The magnetic powder may have an average composition represented by the formula: where M is, for example, at least one metal selected from Ba, Sr, Pb, and Ca, preferably at least one metal selected from Ba and Sr. M may be a combination of Ba and one or more metals selected from the group consisting of Sr, Pb, and Ca. Alternatively, M may be a combination of Sr and one or more metals selected from the group consisting of Ba, Pb, and Ca. In the above general formula, part of Fe may be substituted with another metal element. When the magnetic powder contains a powder of hexagonal ferrite particles, the average particle size of the magnetic powder may be preferably 50 nm or less, more preferably 10 nm to 40 nm, and even more preferably 15 nm to 30 nm.

[0054] (abrasive particles)

[0055] The abrasive particles may preferably be inorganic particles. Examples of such abrasive particles include α-alumina with an α-conversion rate of 90% or more, β-alumina, γ-alumina, silicon carbide, chromium oxide, cerium oxide, α-iron oxide, corundum, silicon nitride, titanium carbide, titanium oxide, silicon dioxide, tin oxide, magnesium oxide, tungsten oxide, zirconium oxide, boron nitride, zinc oxide, calcium carbonate, calcium sulfate, barium sulfate, molybdenum disulfide, acicular α-iron oxide obtained by dehydrating and annealing magnetic iron oxide raw materials, optionally surface-treated with aluminum and / or silica, and diamond powder. Alumina particles such as α-alumina, β-alumina, and γ-alumina, and silicon carbide are preferably used as abrasive particles. These abrasive particles may be acicular, spherical, cubic, or other shapes, but those with angular shapes are preferred because they have high abrasiveness. The average particle size of the abrasive particles may be preferably 20 nm to 80 nm, more preferably 25 nm to 75 nm, even more preferably 30 nm to 70 nm, and even more preferably 35 nm to 65 nm. When the abrasive particles are alumina particles, the average particle size of the alumina particles may be preferably 20 nm to 80 nm, more preferably 25 nm to 75 nm, even more preferably 30 nm to 70 nm, and even more preferably 35 nm to 65 nm.

[0056] (Conductive particles)

[0057] The conductive particles may be fine particles primarily composed of carbon, preferably carbon particles, such as carbon black. Examples of carbon black include Asahi #15 and #15HS from Asahi Carbon Co., Ltd. Hybrid carbon, in which carbon is attached to the surface of silica particles, may also be used. The conductive particles may have an average particle size of preferably 30 to 90 nm, more preferably 35 to 85 nm, even more preferably 40 to 80 nm, and even more preferably 45 to 75 nm.

[0058] (Binder)

[0059] The binder is preferably a resin having a structure in which a crosslinking reaction has been imparted to a polyurethane resin or a vinyl chloride resin, etc. However, the binder is not limited to these, and other resins may be appropriately blended depending on the physical properties required of the leader tape 10. There is no particular limitation on the resin to be blended, so long as it is a resin that is generally used in coating-type leader tapes 10.

[0060] Examples of the binder include polyvinyl chloride, polyvinyl acetate, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, acrylic acid ester-acrylonitrile copolymer, acrylic acid ester-vinyl chloride-vinylidene chloride copolymer, acrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinyl chloride copolymer, methacrylic acid ester-ethylene copolymer, polyvinyl fluoride, vinylidene chloride-acrylonitrile copolymer, acrylonitrile-butadiene copolymer, polyamide resin, polyvinyl butyral, cellulose derivatives (cellulose acetate butyrate, cellulose diacetate, cellulose triacetate, cellulose propionate, nitrocellulose), styrene-butadiene copolymer, polyester resin, amino resin, and synthetic rubber.

[0061] Furthermore, a thermosetting resin or a reactive resin may be used as the binder, and examples of such a resin include a phenolic resin, an epoxy resin, a urea resin, a melamine resin, an alkyd resin, a silicone resin, a polyamine resin, and a urea-formaldehyde resin.

[0062] In addition, in order to improve the dispersibility of the magnetic powder, each of the above-mentioned binders contains -SO 3 M, -OSO 3 M, -COOM, P=O(OM) 2 In the formula, M is a hydrogen atom or an alkali metal such as lithium, potassium, or sodium.

[0063] Furthermore, the polar functional group is -NR1R2, -NR1R2R3 + X - A side chain type having a terminal group of >NR1R2 + X - In the formula, R1, R2, and R3 are hydrogen atoms or hydrocarbon groups, and X - is a halogen ion such as fluorine, chlorine, bromine, or iodine, or an inorganic or organic ion. Examples of the polar functional group include —OH, —SH, —CN, and an epoxy group.

[0064] (Additives)

[0065] The magnetic layer 13 may further contain non-magnetic reinforcing particles such as aluminum oxide (α, β, or γ alumina), chromium oxide, silicon oxide, diamond, garnet, emery, boron nitride, titanium carbide, silicon carbide, titanium carbide, titanium oxide (rutile or anatase titanium oxide), etc.

[0066] (base layer)

[0067] The underlayer 12 is a non-magnetic layer containing non-magnetic powder and a binder as its main components. The above description of the binder contained in the magnetic layer 13 also applies to the binder contained in the underlayer 12. The underlayer 12 may further contain at least one additive selected from the group consisting of conductive particles, lubricants, hardeners, and rust inhibitors, as needed.

[0068] (Non-magnetic powder)

[0069] The non-magnetic powder contained in the underlayer 12 may include, for example, at least one type selected from inorganic particles and organic particles. One type of non-magnetic powder may be used alone, or two or more types of non-magnetic powder may be used in combination. The inorganic particles may include, for example, one or a combination of two or more types selected from metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, and metal sulfides. More specifically, the inorganic particles may be, for example, one or more types selected from iron oxyhydroxide, hematite, titanium oxide, and carbon black. The shape of the non-magnetic powder may be, for example, acicular, spherical, cubic, plate-like, or other shapes, but is not particularly limited to these.

[0070] (Back layer)

[0071] The back layer 14 may contain a binder and a non-magnetic powder. The back layer 14 may also contain various additives such as a lubricant, a curing agent, and an antistatic agent, as necessary. The above description of the binder and non-magnetic powder contained in the underlayer 12 also applies to the binder and non-magnetic powder contained in the back layer 14.

[0072] The average particle size of the inorganic particles contained in the back layer 14 is preferably 10 nm or more and 150 nm or less, and more preferably 15 nm or more and 110 nm or less. The average particle size of the inorganic particles can be determined in the same manner as the average particle size D of the magnetic powder described above.

[0073] (3) Physical properties and structure

[0074] (Breaking strength)

[0075] A 1 / 2 inch wide, 300 mm long sample piece is prepared and attached to the tensile tester, and a 150 mm long portion is pulled under the following conditions to measure the load at break.

[0076] <Tension conditions>

[0077] Tensile tester: AUTOGRAPH AG100D, manufactured by Shimadzu Corporation Tensile speed: 15 mm / min

[0078] (Abrasivity)

[0079] Abbreviations refer to an index that indicates the degree of wear on the magnetic head caused by the leader tape as it contacts and runs against the magnetic head. To measure abravisivity, a plate-shaped abravisivity bar A made of a metal material (81% Ni / 19% Fe, purity: 99.95) is first prepared. A sample piece of leader tape approximately 400 m long is also prepared. Measurements are performed at 23°C and 45% RH. Figure 2 is a schematic diagram showing the relationship between the leader tape LT and a measuring instrument 21 to which the abravisivity bar A is attached. As shown in Figure 2, the abravisivity bar A has a length of 100 μm on the surface that contacts the leader tape LT in a direction parallel to the running direction d1 of the leader tape LT and a length of 18 mm in a direction perpendicular to the running direction of the leader tape LT (also referred to as the tape width direction) d2. Before attaching the abrasivitity bar A to the measuring machine 21 shown in FIG. 2, seven indentations 22 with an indentation size (long axis length of the indentation) of 130 μm are made in the width direction of the leader tape on the side surface that contacts the leader tape LT using a Knoop indenter shown in FIG. 3. FIG. 3(a) is a top view of the Knoop indenter. FIG. 3(b) is a right side view of the Knoop indenter. FIG. 3(c) is a front view of the Knoop indenter. FIG. 4 is a schematic diagram showing the indentations 22 made on the side surface of the abrasivitity bar A that contacts the leader tape LT. The indentation sizes (long axis length of the indentation) of the seven indentations 22 are measured, and the arithmetic average value is taken as the indentation size (long axis length of the indentation) before running.

[0080] Next, an abrasivitity bar A is attached to the measuring machine 21 shown in Figure 2. The leader tape LT is run in contact with the abrasivitity bar A under the following running conditions.

[0081] <Driving conditions>

[0082] Wrap angle: 12° Tension: 1N Travel speed: 3 m / s Measurement length: 290 m Number of runs: 30 round trips

[0083] After the run, the indentation size (long axis length of the indentation) of the seven indentations 22 made on the side of the abrasivitivity bar A is measured, and the arithmetic mean value is taken as the indentation size (long axis length of the indentation) after the run.

[0084] The amount of indentation scraping off is calculated from the indentation size (long axis length of the indentation) before and after running using the following formula, and the amount of indentation scraping off due to running is taken as abrasiveness: Abrasivity (μm) (amount of indentation scraping off) = indentation size before running (long axis length of the indentation) - indentation size after running (long axis length of the indentation)

[0085] (Surface roughness Rab)

[0086] The surface roughness Rab is a value measured on the surface 13S of the magnetic layer 13 of the leader tape 10 shown in Figure 1. The surface roughness Rab is determined as follows. First, the leader tape LT housed in the cartridge 10A shown in Figure 5 is unwound, and a length of about 10 cm of the leader tape LT is cut out from the end of the drawn-out leader tape LT at a position 30 to 40 m longitudinally toward the connection between the leader tape LT and the magnetic tape T, and attached to a glass slide (i.e., with the back layer surface attached to the glass slide) to obtain a sample piece. Next, the surface roughness of the magnetic layer surface 13S of the sample piece is measured using a non-contact roughness meter using optical interference described below.

[0087] <Surface roughness measurement conditions>

[0088] Equipment: Non-contact roughness meter using optical interference (non-contact surface and layer cross-sectional shape measurement system VertScan R5500GL-M100-AC manufactured by Ryoka Systems Co., Ltd.) Objective lens: 20x (approximately 236 μm x 177 μm field of view) Resolution: 640 points x 480 points Measurement mode: phase Wavelength filter: 520 nm Surface correction: Corrected using a quadratic polynomial approximation surface

[0089] As described above, the surface roughness is measured at at least five positions in the longitudinal direction, and then the average value of the arithmetic mean roughnesses Sa (nm) automatically calculated from the surface profiles obtained at each position is defined as the surface roughness Rab (nm).

[0090] (Average thickness of leader tape (average total thickness) t T )

[0091] Average thickness t of leader tape LT Tis obtained as follows. First, the leader tape LT housed in the cartridge 10A is unwound, and a sample is prepared by cutting the leader tape LT to a length of 250 mm at a position 30 m longitudinally from the end of the drawn-out leader tape LT toward the joint between the leader tape LT and the magnetic tape T. Next, the thickness of the sample is measured at five positions using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, and the measured values ​​are simply averaged (arithmetic mean) to obtain the average thickness t T The five measurement positions are selected at random from the sample so that they are different positions in the longitudinal direction of the leader tape LT.

[0092] (Average thickness of base layer)

[0093] The average thickness of the underlayer 12 is determined as follows. First, the leader tape LT housed in the cartridge 10A is unwound, and the leader tape LT is cut into 250 mm lengths at three locations, 10 m, 30 m, and 50 m from the end of the drawn-out leader tape LT toward the connection between the leader tape LT and the magnetic tape T, to prepare three samples. Next, each sample is thinned using an FIB method or the like. When using the FIB method, a carbon layer and a tungsten layer are formed as protective films as a pretreatment for observing the cross-sectional TEM images described below. The carbon layer is formed by vapor deposition on the surface of the leader tape LT facing the magnetic layer 13 and the surface facing the back layer 14, and the tungsten layer is further formed by vapor deposition or sputtering on the surface facing the magnetic layer 13. The thinning is performed along the longitudinal direction of the leader tape LT. That is, the thinning results in a cross section parallel to both the longitudinal direction and the thickness direction of the leader tape LT.

[0094] The cross section of each of the obtained thinned samples is observed using a transmission electron microscope (TEM) under the following conditions: Apparatus: TEM (H9000NAR manufactured by Hitachi, Ltd.) Acceleration voltage: 300 kV Magnification: 100,000 times

[0095] Next, using the obtained TEM image, the thickness of the underlayer 12 is measured at at least 10 positions in the longitudinal direction of the leader tape LT, and then the measured values ​​are simply averaged (arithmetic averaged) to obtain the average thickness (μm) of the underlayer 12.

[0096] (average thickness of base layer)

[0097] The average thickness of the base layer 11 is determined as follows. First, the leader tape LT housed in the magnetic recording cartridge 10A is unwound, and a sample is prepared by cutting the leader tape LT to a length of 250 mm at a position 30 m in the longitudinal direction from the end of the drawn-out leader tape LT toward the joint between the leader tape LT and the magnetic tape T. In this specification, the "longitudinal direction" in the "longitudinal direction from the joint between the leader tape LT and the magnetic tape T" refers to the direction from one end of the leader tape LT toward the other end on the opposite side.

[0098] Next, all layers of the sample other than the base layer 11 (i.e., the underlayer 12, magnetic layer 13, and backing layer 14) are removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, the thickness of the sample (base layer 11) is measured at five positions, and the measured values ​​are simply averaged (arithmetic mean) to calculate the average thickness of the base layer 11. The five measurement positions are randomly selected from the sample so that they are each a different position in the longitudinal direction of the leader tape LT.

[0099] (Average thickness of the back layer t b )

[0100] Average thickness t of the back layer 14 b is calculated as follows: First, the average thickness (average total thickness) t of the leader tape LT T Measure the average thickness t TThe method for measuring the average total thickness (average total thickness) is as described above in "Average Thickness of Leader Tape." Next, the leader tape LT housed in the cartridge 10A is unwound, and a sample is prepared by cutting the leader tape LT to a length of 250 mm at a position 30 m longitudinally from the end of the drawn-out leader tape LT toward the joint between the leader tape LT and the magnetic tape T. Next, the back layer 14 of the sample is removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, the thickness of the sample is measured at five positions using a Mitutoyo Laser Hologram Gauge (LGH-110C), and the measured values ​​are simply averaged (arithmetic average) to obtain the average thickness t B Then, the average thickness t of the back layer 14 is calculated using the following formula: b The five measurement positions are selected at random from the sample so that they are different positions in the longitudinal direction of the leader tape LT. b [μm] = t T [μm]-t B [μm]

[0101] (Average thickness of the magnetic layer t m )

[0102] Average thickness t of the magnetic layer 13 mis determined as follows. First, the leader tape LT housed in the cartridge 10A is unwound, and three samples of 250 mm length are cut from the leader tape LT at three positions, 10 m, 30 m, and 50 m from the end of the drawn-out leader tape LT toward the connection between the leader tape LT and the magnetic tape T. Next, each sample is thinned by processing using an FIB method or the like. When using the FIB method, a carbon layer and a tungsten layer are formed as protective films as a pretreatment for observing the cross-sectional TEM image described below. The carbon layer is formed by vapor deposition on the surface of the leader tape LT facing the magnetic layer 13 and the surface facing the back layer 14, and the tungsten layer is further formed by vapor deposition or sputtering on the surface facing the magnetic layer 13. The thinning is performed along the longitudinal direction of the leader tape LT. In other words, the thinning results in a cross section parallel to both the longitudinal direction and the thickness direction of the leader tape LT.

[0103] The cross section of each obtained thinned sample is observed using a transmission electron microscope (TEM) under the following conditions to obtain a TEM image of each thinned sample. Note that the magnification and acceleration voltage may be adjusted appropriately depending on the type of device.

[0104] Apparatus: TEM (Hitachi H9000NAR) Acceleration voltage: 300 kV Magnification: 100,000 times

[0105] Next, using the TEM image of each obtained thinned sample, the thickness of the magnetic layer 13 was measured at 10 positions on each thinned sample. The 10 measurement positions on each thinned sample were randomly selected from the sample so that they were different positions in the longitudinal direction of the leader tape LT. The measured values ​​of each obtained thinned sample (thickness of the magnetic layer 13 at 30 points in total) were simply averaged (arithmetic average) to obtain an average value, which was the average thickness t of the magnetic layer 13. m Let [nm].

[0106] (average particle size of magnetic powder)

[0107] When the magnetic powder contains hexagonal ferrite particles, the average particle size and average aspect ratio of the magnetic powder can be determined as follows. First, the leader tape LT housed in the cartridge 10A is unwound, and the leader tape LT is cut out at a position 30 m longitudinally from the end of the drawn-out leader tape LT toward the connection between the leader tape LT and the magnetic tape T. Next, the leader tape LT to be measured is processed and thinned using a FIB method or the like. When using the FIB method, a carbon layer and a tungsten layer are formed as protective films as a pretreatment for observing the cross-sectional TEM image described below. The carbon layer is formed by vapor deposition on the surface of the leader tape LT facing the magnetic layer 13 and the surface facing the back layer 14, and the tungsten layer is further formed by vapor deposition or sputtering on the surface facing the magnetic layer 13. The thinning is performed along the length (longitudinal direction) of the leader tape LT. In other words, the thinning results in a cross section parallel to both the longitudinal and thickness directions of the leader tape LT.

[0108] The cross section of the obtained thin sample is observed using a transmission electron microscope (H-9500 manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 200 kV and a total magnification of 500,000 times, so as to include the entire magnetic layer 13 in the thickness direction of the magnetic layer 13, and a TEM photograph is taken. The number of TEM photographs prepared is such that 50 particles can be extracted that can measure the plate diameter DB and plate thickness DA (see Figure 5) shown below.

[0109] In this specification, the size of a hexagonal ferrite particle (hereinafter referred to as "particle size") is defined as the plate diameter DB, which is the major axis of the plate surface or bottom surface, when the particle shape observed in the TEM photograph is plate-like or columnar (however, the thickness or height is smaller than the major axis of the plate surface or bottom surface) as shown in FIG. 5. The thickness or height of the particle observed in the TEM photograph is defined as the plate thickness DA. When the plate surface or bottom surface of the particle observed in the TEM photograph is hexagonal, the major axis means the longest diagonal distance. When the thickness or height of a particle is not constant within a single particle, the thickness or height of the largest particle is defined as the plate thickness DA.

[0110] Next, 50 particles are selected from the TEM photograph based on the following criteria: Particles with parts outside the field of view of the TEM photograph are not measured, and only particles with a clear outline and that exist independently are measured. When particles overlap, particles with a clear boundary between them and whose overall shape can be determined are measured as individual particles, but particles with an unclear boundary and whose overall shape cannot be determined are not measured, as their shape cannot be determined.

[0111] Examples of TEM photographs are shown in Figures 6 and 7. In Figures 6 and 7, for example, particles indicated by arrows a and d are selected because their plate thickness (thickness or height) DA can be clearly confirmed. The plate thickness DA of each of the selected 50 particles is measured. The plate thicknesses DA thus obtained are simply averaged (arithmetic mean) to obtain the average plate thickness DA. ave Calculate the average plate thickness DA ave is the average particle plate thickness. Next, the plate diameter DB of each magnetic powder is measured. In order to measure the plate diameter DB of the particles, 50 particles whose plate diameter DB can be clearly confirmed are selected from the TEM photograph. For example, in Figures 6 and 7, the particles indicated by arrows b and c are selected because their plate diameter DB can be clearly confirmed. The plate diameter DB of each of the selected 50 particles is measured. The plate diameter DBs thus determined are simply averaged (arithmetic averaged) to obtain the average plate diameter DB. ave Average plate diameter DB ave is the average grain size. And the average plate thickness DA ave and average plate diameter DB ave The average aspect ratio of the particles (DB ave / DA ave ) is required.

[0112] (Average particle volume of magnetic powder)

[0113] The average particle volume of the magnetic powder can be calculated as follows. First, as described above in relation to the method for calculating the average particle size of the magnetic powder, the average plate thickness DA ave and average plate diameter DB ave Next, the average particle volume V of the magnetic powder is calculated using the following formula:

[0114]

[0115] (electrical resistance value)

[0116] Using electrodes with an interelectrode distance of 12.65 mm, a test piece (tape length 300 mm, tape width 12.65 mm) was placed on the electrode with the magnetic layer surface facing down, a load of 1.62 N was applied to both ends, and an applied voltage was applied. After 1 minute of application, the electrical resistance value was measured using an electrical resistance measuring device (ULTRA HIGH RESISTANCE METER R8340A, manufactured by ADVATEST). The applied voltage refers to the voltage actually applied to the test piece during measurement. The applied voltage during measurement is set as follows depending on the resistance value R:

[0117] Resistance value R>5×10 4 When Ω / sq: Applied voltage: 100±10V 5×10 4 Ω / sq > resistance value R > 5 x 10 3 When Ω / sq: Applied voltage: 10±1V Resistance value R<5×10 3 When Ω / sq: Applied voltage: Maximum voltage at which the leader tape does not deform

[0118] (4) Leader tape manufacturing method

[0119] Next, a method for manufacturing the leader tape 10 having the above-described configuration will be described. First, a base layer forming paint is prepared by kneading and / or dispersing non-magnetic powder, a binder, etc. in a solvent. Next, a magnetic layer forming paint is prepared by kneading and / or dispersing magnetic powder, a binder, etc. in a solvent. The following solvents, dispersing devices, and kneading devices can be used, for example, to prepare the magnetic layer forming paint and the base layer forming paint.

[0120] Examples of solvents that can be used in preparing the coating material include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohol-based solvents such as methanol, ethanol, and propanol; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, propyl acetate, ethyl lactate, and ethylene glycol acetate; ether-based solvents such as diethylene glycol dimethyl ether, 2-ethoxyethanol, tetrahydrofuran, and dioxane; aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene; and halogenated hydrocarbon-based solvents such as methylene chloride, ethylene chloride, carbon tetrachloride, chloroform, and chlorobenzene. One of these may be used, or a mixture of two or more of them may be used.

[0121] Examples of the kneading device used in preparing the above-mentioned coating material include, but are not limited to, a continuous twin-screw kneader, a continuous twin-screw kneader capable of multi-stage dilution, a kneader, a pressure kneader, and a roll kneader. Examples of the dispersing device used in preparing the above-mentioned coating material include, but are not limited to, a roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, a spike mill, a pin mill, a tower mill, a pearl mill (such as the "DCP Mill" manufactured by Eirich), a homogenizer, and an ultrasonic disperser.

[0122] Next, a paint for forming an underlayer is applied to one main surface of the base layer 11 and dried to form the underlayer 12. Subsequently, a paint for forming a magnetic layer is applied to the underlayer 12 and dried to form the magnetic layer 13 on the underlayer 12.

[0123] The resulting leader tape 10 is then rewound around a large-diameter core and cured. Finally, the leader tape 10 is calendered and then cut to a predetermined width (e.g., 1 / 2 inch width). To prevent thermal stress from causing deformation and reducing the tape's breaking strength, the calendering temperature is preferably 95°C or lower, more preferably 90°C or lower, and even more preferably 85°C or lower. To prevent excessive abrasive force, the calendering temperature is preferably 65°C or higher, more preferably 70°C or higher, and even more preferably 75°C or higher. The above steps result in the desired long, slender leader tape 10.

[0124] (5) One embodiment of a magnetic recording cartridge

[0125] [Cartridge configuration]

[0126] The leader tape according to the present technology may be included in a magnetic recording medium including a magnetic tape having a data recording and writing area. More specifically, this may be a magnetic recording medium including a leader tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 round trips against a Ni81% / Fe19% plate, and a magnetic tape having a data recording and writing area. The leader tape according to the present technology may also be spliced ​​with a magnetic tape and housed in a magnetic recording cartridge for use. Within the magnetic recording cartridge, the leader tape may be wound around a reel, for example. This may be a magnetic recording cartridge housing a leader tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 round trips against a Ni81% / Fe19% plate, spliced ​​with a magnetic tape having a data recording and writing area.

[0127] An example of the configuration of a magnetic recording cartridge 10A equipped with a leader tape LT having the above-described configuration will be described with reference to FIG.

[0128] 8 is an exploded perspective view showing an example of the configuration of a magnetic recording cartridge 10A. The magnetic recording cartridge 10A is a magnetic recording cartridge that conforms to the LTO (Linear Tape-Open) standard, and includes a cartridge case 10B made up of a lower shell 212A and an upper shell 212B, a reel 10C around which a magnetic tape T is wound, a reel lock 214 and a reel spring 215 for locking the rotation of the reel 10C, a spider 216 for unlocking the locked state of the reel 10C, a slide door 217 that straddles the lower shell 212A and the upper shell 212B and opens and closes a tape pull-out opening 212C provided in the cartridge case 10B, a door spring 218 that biases the slide door 217 to a closed position of the tape pull-out opening 212C, a write protect 219 for preventing accidental erasure, and a cartridge memory 211. The reel 10C is generally disk-shaped with an opening in the center, and is composed of a reel hub 213A and a flange 213B made of a hard material such as plastic. A leader tape LT is connected to one end of the magnetic tape T. A leader pin 220 is provided at the tip of the leader tape LT.

[0129] The present technology can also employ the following configurations. [1] A leader tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 double strokes against a Ni 81% / Fe 19% plate. [2] The leader tape according to [1], having an abrasivity of 16.4 μm or less after 30 double strokes against a Ni 81% / Fe 19% plate. [3] The leader tape according to [1] or [2], having a breaking strength of 35 N or more. [4] The leader tape according to any one of [1] to [3], comprising a magnetic layer and an underlayer, in this order. [5] The leader tape according to [4], wherein the magnetic layer comprises barium ferrite magnetic powder. [6] The leader tape according to any one of [1] to [5], having an average thickness (average total thickness) of 16.0 μm or more. [7] The leader tape according to any one of [4] to [6], wherein the underlayer has an average thickness of 1.25 μm or more. [8] The leader tape according to any one of [4] to [7], wherein the surface roughness Rab of the magnetic layer surface is 5.0 nm or more. [9] The leader tape according to any one of [4] to [8], wherein the underlayer has an average thickness of 1.35 μm or more.

[10] The leader tape according to any one of [1] to [9], wherein the abrasivity after 30 round trips on a Ni81% / Fe19% plate is 14.5 μm or less.

[11] The leader tape according to any one of [1] to

[10] , wherein the abrasivity after 30 round trips on a Ni81% / Fe19% plate is 12 μm or less.

[12] The leader tape according to any one of [1] to

[11] , wherein the breaking strength is 40 N or more.

[13] A magnetic recording medium comprising a leader tape and a magnetic tape having a data recording and writing area, the leader tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 round trips against a Ni81% / Fe19% plate.

[14] A magnetic recording cartridge containing a joined leader tape and a magnetic tape having a data recording and writing area, the leader tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 round trips against a Ni81% / Fe19% plate.

[0130] 3. Working Example

[0131] Hereinafter, the present technology will be specifically explained using examples, but the present technology is not limited to these examples.

[0132] In this example, the breaking strength, abrasivity, surface roughness of the magnetic layer surface, and average thickness (average total thickness) of the leader tape t T , the average thickness of the magnetic layer t m The average thickness of the underlayer, the average thickness of the base layer, the average thickness of the back layer, and the electrical resistance value were determined by the measurement method described in the above embodiment.

[0133] The load / unload test and head damage evaluation were carried out as follows.

[0134] (Load / Unload Test)

[0135] <Sample preparation>

[0136] The evaluation samples for the load / unload test were prepared as follows: The leader tape of each example and comparative example was attached to the end of a commercially available LTO9 magnetic tape using adhesive tape, and the attached tape was housed in a magnetic recording cartridge shown in Figure 8 to prepare an evaluation cartridge.

[0137] <Load / Unload Test Procedure>

[0138] The equipment used was one LTO9 FH drive and one HH drive, with the head TMR element resistance values ​​confirmed for all channels. The head TMR element resistance values ​​were measured after removing the flexible cable. A load / unload test was performed on the above evaluation samples using the following procedure. The test was conducted in an environment with a temperature of 25°C ± 2°C and a humidity of 45% RH ± 5%. (i) Insert the evaluation cartridge into the LTO9 drive. (ii) Pull out the tape from the evaluation cartridge (tape path). (iii) Rewind the tape into the evaluation cartridge (tape path return). (iv) Remove the evaluation cartridge from the LTO9 drive.

[0139] The above operations (i) to (ii) are called loading, and the operations (iii) to (iv) are called unloading. The operations (i) to (iv) constitute one cycle, and the operations (i) to (iv) are performed up to 20,000 cycles.

[0140] During the load / unload test, the LTO9 drive is judged to have no malfunction (drive hard error) and to have no stoppage up to 20,000 cycles. If a malfunction (drive hard error) occurs before 20,000 cycles, the test is deemed unmeasurable. A long load / unload time (referring to the cycle time when one cycle consists of a load operation and an unload operation) is considered a malfunction. Specifically, a cycle time exceeding 120 seconds is considered a malfunction. For example, FIG. 9 shows the relationship between the number of cycles and the load / unload time when no malfunction occurs in a load / unload test using an LTO9HH drive. In FIG. 9, the load / unload time is within approximately 80 seconds by 20,000 cycles, and it is determined that no malfunction has occurred. Meanwhile, FIG. 10 shows the relationship between the number of cycles and the load / unload time when a malfunction occurs in a load / unload test using an LTO9HH drive. In FIG. 10, the load / unload time exceeds about 120 seconds by the time of 10,000 cycles, and it is determined that a malfunction has occurred.

[0141] (head damage)

[0142] <Head damage test procedure>

[0143] The evaluation sample was subjected to a head damage test using the following procedure. (i) As with the load / unload test, the TMR element resistance of the head was measured before the test. (ii) The load / unload test was performed. (iii) The TMR element resistance of the LTO9 drive after the 20,000 cycle test was measured, and the TMR element resistance of the LTO9 drive before the load / unload test, measured in operation (i), was set as the initial value. If the TMR element resistance value decreased by 80% or more from the initial value, it was determined that head damage had occurred because sufficient reproduction capability could not be ensured. If the TMR element resistance value decreased by less than 80% from the initial value, it was determined that no head damage had occurred.

[0144] [Example 1]

[0145] (Preparation process of paint for forming magnetic layer)

[0146] The magnetic layer-forming paint was prepared as follows. First, a first composition having the following formulation was kneaded using an extruder. Next, the kneaded first composition and a second composition having the following formulation were added to a stirring tank equipped with a disperser and premixed. Subsequently, further sand mill mixing was performed and filtering was performed to prepare the magnetic layer-forming paint.

[0147] (First composition)

[0148] Magnetic powder (hexagonal ferrite with M-type structure, composition: Ba-Ferrite, shape: plate-like hexagonal particles, average particle volume: 1600 nm 3 Vinyl chloride resin (cyclohexanone solution 30% by mass): 46 parts by mass (degree of polymerization 300, Mn = 10,000, contains polar groups OSOK = 0.07 mmol / g and secondary OH = 0.3 mmol / g)

[0149] (Second composition)

[0150] Vinyl chloride resin: 1.6 parts by mass (as a 30% by mass resin in cyclohexanone solution) n-butyl stearate: 2 parts by mass Methyl ethyl ketone: 121.3 parts by mass Toluene: 121.3 parts by mass Cyclohexanone: 60.7 parts by mass Aluminum oxide powder: 7.5 parts by mass (α-Al2O3, average particle size 50 nm, manufactured by Sumitomo Chemical Co., Ltd., trade name: HIT100, Mohs hardness: 9) Carbon black: 2.0 parts by mass (average particle size 70 nm, manufactured by Tokai Carbon Co., Ltd., trade name: Seest TA)

[0151] Finally, 2 parts by weight of polyisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Co., Ltd.) and 2 parts by weight of myristic acid were added as curing agents to the magnetic layer-forming coating material prepared as described above.

[0152] (Preparation process of paint for forming base layer)

[0153] The paint for forming the primer layer was prepared as follows. First, the third composition having the following composition was kneaded using an extruder. Next, the kneaded third composition and the fourth composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Subsequently, further mixing was performed using a sand mill and filtering was performed to prepare the paint for forming the primer layer.

[0154] (Third composition)

[0155] Acicular iron oxide powder: 100 parts by mass (α-Fe2O3, average major axis length 0.15 μm) Aluminum oxide powder: 5 parts by mass (α-Al 2 O 3 , average particle size 80 nm, manufactured by Sumitomo Chemical Co., Ltd., trade name: HIT82, Mohs hardness: 9) Vinyl chloride resin: 55.6 parts by mass (resin solution: resin content 30% by mass, cyclohexanone 70% by mass)

[0156] (Fourth composition)

[0157] Polyurethane resin UR8200 (manufactured by Toyobo Co., Ltd.): 18.5 parts by mass, n-butyl stearate: 2 parts by mass, methyl ethyl ketone: 108.2 parts by mass, toluene: 108.2 parts by mass, cyclohexanone: 18.5 parts by mass, carbon black: 10 parts by mass (average particle size 20 nm)

[0158] Finally, 2 parts by mass of polyisocyanate (trade name: Coronate L, manufactured by Tosoh Corporation) and 2 parts by mass of myristic acid were added as a curing agent to the base layer forming paint prepared as described above.

[0159] (Step of preparing paint for forming back layer)

[0160] A paint for forming a back layer was prepared as follows. The following raw materials were mixed in a stirring tank equipped with a disperser and filtered to prepare a paint for forming a back layer. Carbon black (manufactured by Asahi Carbon Co., Ltd., product name: #80): 100 parts by mass Polyester polyurethane: 150 parts by mass (resin solution: polyurethane resin blend amount 30% by mass, cyclohexanone blend amount 70% by mass) (manufactured by Nippon Polyurethane Co., Ltd., product name: N-2304) Methyl ethyl ketone: 500 parts by mass Toluene: 400 parts by mass Cyclohexanone: 100 parts by mass Polyisocyanate (product name: Coronate L, manufactured by Tosoh Corporation): 9 parts by mass

[0161] (Film forming process)

[0162] Using the coating material prepared as described above, leader tapes were prepared as follows.

[0163] First, a long PEN film (base film) with an average thickness of 14.97 μm was prepared as a support for the base layer of the leader tape. Next, a primer layer-forming paint was applied to one main surface of the PEN film and dried to form a primer layer on one main surface of the PEN film, with an average thickness of 1.50 μm in the final product. Next, a magnetic layer-forming paint was applied to the primer layer and dried to form a magnetic layer on the primer layer, with an average thickness of 0.07 μm in the final product.

[0164] Next, a back layer-forming coating material was applied to the other main surface of the PEN film on which the underlayer and magnetic layer had been formed, and then dried to form a back layer with an average thickness of 0.46 μm in the final product. The PEN film on which the underlayer, magnetic layer, and back layer had been formed was then subjected to a curing treatment. The surface of the magnetic layer was then smoothed by calendering at a calender temperature of 80° C.

[0165] (Cutting process)

[0166] The leader tape obtained as described above was cut into a width of 1 / 2 inch (12.65 mm), thereby obtaining a long leader tape.

[0167] The 1 / 2 inch wide leader tape was connected to a commercially available LTO9 magnetic tape via an adhesive tape, and the tape was wound around a reel provided in the cartridge case to obtain a magnetic recording cartridge.

[0168] The resulting leader tape had a breaking strength of 41.2 N, an abrasivity after 30 round trips of 12.0 μm, a surface roughness Rab of the magnetic surface of 5.7 nm, an electrical resistance of 8.08E+05 Ω / cm, and an average thickness (average total thickness) t T The average thickness of the underlayer was 17.0 μm, and the average thickness of the underlayer was 1.50 μm.

[0169] [Example 2]

[0170] Example 1 refers to the average thickness (average total thickness) of the leader tape t T A leader tape was obtained in the same manner as in Example 1, except that the surface roughness Rab of the magnetic surface was 5.5 nm and the electrical resistance was 2.07E+06 Ω / cm.

[0171] [Example 3]

[0172] Example 1 refers to the average thickness (average total thickness) of the leader tape t TA leader tape was obtained in the same manner as in Example 1, except that the average surface roughness Rab of the magnetic surface was 6.1 nm, the average thickness of the underlayer was 1.30 μm, the breaking strength was 40.7 N, and the abrasivity after 30 strokes was 16.4 μm. The resulting leader tape had an electrical resistance of 1.12E+06 Ω / cm.

[0173] [Comparative Example 1]

[0174] Example 1 refers to the average thickness (average total thickness) of the leader tape t T A leader tape was obtained in the same manner as in Example 1, except that the surface roughness Rab of the magnetic surface was 5.6 nm, the average thickness of the underlayer was 16.8 μm, the average thickness of the underlayer was 1.30 μm, the calendering temperature was 60° C., the breaking strength was 41.8 N, and the abrasivity after 30 strokes was 18.7 μm. The resulting leader tape had a surface roughness Rab of 5.6 nm and an electrical resistance of 3.85E+06 Ω / cm.

[0175] [Comparative Example 2]

[0176] Example 1 refers to the average thickness (average total thickness) of the leader tape t T A leader tape was obtained in the same manner as in Example 1, except that the surface roughness Rab of the magnetic surface was 5.5 nm, the average thickness of the underlayer was 16.6 μm, the average thickness of the underlayer was 1.15 μm, the calendering temperature was 60° C., the breaking strength was 42.0 N, and the abrasivity after 30 strokes was 19.8 μm. The resulting leader tape had a surface roughness Rab of 5.5 nm and an electrical resistance of 3.35E+06 Ω / cm.

[0177] [Comparative Example 3]

[0178] Example 1 refers to the average thickness (average total thickness) of the leader tape t TA leader tape was obtained in the same manner as in Example 1, except that the surface roughness Rab of the magnetic surface was 5.3 nm, the average thickness of the underlayer was 16.6 μm, the average thickness of the underlayer was 1.15 μm, the calendering temperature was 100° C., the breaking strength was 27.5 N, and the abrasivity after 30 strokes was 7.9 μm. The resulting leader tape had a surface roughness Rab of 5.3 nm on the magnetic surface and an electrical resistance of 1.00E+06 Ω / cm.

[0179] [Comparative Example 4]

[0180] Example 1 refers to the average thickness (average total thickness) of the leader tape t T A leader tape was obtained in the same manner as in Example 1, except that the surface roughness Rab of the magnetic surface was 5.4 nm, the average thickness of the underlayer was 0.90 μm, the calendering temperature was 100° C., the breaking strength was 26.0 N, and the abrasivity after 30 strokes was 18 μm. The resulting leader tape had a surface roughness Rab of 5.4 nm and an electrical resistance of 8.90E+05 Ω / cm.

[0181] [Comparative Example 5]

[0182] This example differs from Example 1 in that a metal magnetic powder (Fe—Co acicular magnetic powder, average major axis length 0.1 μm) was used instead of barium ferrite magnetic powder, and the average thickness (average total thickness) of the leader tape was t T A leader tape was obtained in the same manner as in Example 1, except that the surface roughness Rab of the magnetic surface was 6.5 nm, the average thickness of the underlayer was 16.6 μm, the average thickness of the underlayer was 1.15 μm, the calendering temperature was 115° C., the breaking strength was 40.5 N, and the abrasivity after 30 strokes was 38.1 μm. The resulting leader tape had a surface roughness Rab of 6.5 nm and an electrical resistance of 1.63E+06 Ω / cm.

[0183] Table 1 shows the configurations and evaluation results of the leader tapes of Examples 1 to 3 and Comparative Examples 1 to 5.

[0184]

[0185] The results shown in Table 1 reveal the following.

[0186] All of the leader tapes of Examples 1 to 3 had a breaking strength of 28 N or more, and an abrasivity of 17.5 μm or less after 30 round trips against a Ni81% / Fe19% plate. No malfunctions or head damage occurred in the load / unload test.

[0187] On the other hand, the leader tapes of Comparative Examples 3 and 4, which had a breaking strength of less than 28 N, malfunctioned in the load / unload test, and the electrical resistance value for head damage evaluation could not be measured. Furthermore, Comparative Examples 1, 2, and 5, which had an abrasivity of more than 17.5 μm after 30 round trips on a Ni 81% / Fe 19% plate, suffered head damage.

[0188] Although the embodiments and examples of the present technology have been specifically described above, the present technology is not limited to the above-described embodiments and examples, and various modifications based on the technical ideas of the present technology are possible.

[0189] For example, the configurations, methods, steps, shapes, materials, and numerical values, etc., given in the above-described embodiments and examples are merely examples, and different configurations, methods, steps, shapes, materials, and numerical values, etc., may be used as necessary. Furthermore, the chemical formulas of compounds, etc., are representative, and are not limited to the valences, etc., given as long as they are general names of the same compounds.

[0190] Furthermore, the configurations, methods, processes, shapes, materials, numerical values, and the like of the above-described embodiments and examples can be combined with each other without departing from the spirit of the present technology.

[0191] Furthermore, in this specification, a numerical range indicated using "to" indicates a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range in a certain stage may be replaced with the upper limit or lower limit of a numerical range in another stage. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more types.

[0192] 10 Leader tape 11 Base layer 12 Underlayer 13 Magnetic layer 14 Back layer

Claims

1. A leader tape having a breaking strength of 28N or more and an abrasivity of 17.5μm or less after 30 round trips against a Ni81% / Fe19% plate.

2. The leader tape of claim 1, having an abrasivity of 16.4 μm or less after 30 round trips against a Ni 81% / Fe 19% plate.

3. The leader tape according to claim 1, having a breaking strength of 35N or more.

4. The leader tape of claim 1, comprising, in order, a magnetic layer and an underlayer.

5. The leader tape of claim 4, wherein said magnetic layer comprises barium ferrite magnetic powder.

6. The leader tape according to claim 1, having an average thickness (average total thickness) of 16.0 μm or more.

7. The leader tape according to claim 4, wherein the average thickness of said underlayer is 1.25 μm or more.

8. The leader tape according to claim 4, wherein the surface roughness Rab of the magnetic layer surface is 5.0 nm or more.

9. The leader tape according to claim 4, wherein the average thickness of said underlayer is 1.35 μm or more.

10. The leader tape of claim 1, having an abrasivity of 14.5 μm or less after 30 round trips against a Ni 81% / Fe 19% plate.

11. The leader tape of claim 1, having an abrasivity of 12 μm or less after 30 round trips against a Ni 81% / Fe 19% plate.

12. The leader tape according to claim 1, having a breaking strength of 40 N or more.

13. A magnetic recording medium comprising a magnetic tape having a leader tape and a data recording write area, the magnetic tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 round trips against a Ni81% / Fe19% plate.

14. A magnetic recording cartridge containing a leader tape and a magnetic tape having a data recording write area joined together, the leader tape having a breaking strength of 28 N or more and an abrasivity of 17.5 μm or less after 30 round trips against a Ni81% / Fe19% plate.

Citation Information

Patent Citations

  • Leader tape

    JP2007164906A

  • Magnetic recording medium

    WO2022209316A1