Fluororubber composition and crosslinked molded object formed therefrom

The fluororubber composition, featuring hollow particles and a reinforcing agent, addresses the challenge of creating lightweight products with reduced compression set by forming a crosslinked structure that enhances mechanical properties and maintains voids, resulting in a lightweight and compression-resistant product.

WO2024242013A1PCT designated stage expired Publication Date: 2024-11-28ZEON CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018101
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-28
Filing Date
2024-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current methods for producing lightweight fluororubber products with reduced compression set are limited, as existing techniques either struggle with controlling pore size in foamed elastomers or fail to achieve both weight reduction and compression resistance simultaneously.

Method used

A fluororubber composition incorporating hollow particles with specific characteristics, such as a shell containing a resin and a hollow part, and a reinforcing agent like carbon black or silica, which are crosslinked with an organic peroxide to form a lightweight and compression-resistant molded product.

Benefits of technology

The fluororubber composition achieves a lightweight crosslinked molded product with reduced compression set and improved mechanical properties, including weight reduction, heat insulation, and enhanced wear resistance, by forming a three-dimensional crosslinked structure that maintains voids and improves adhesion between hollow particles and fluororubber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000002
    Figure JPOXMLDOC01-APPB-M000002
  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided are a fluororubber composition capable of providing a crosslinked molded object having a low weight and a low compression set and a crosslinked molded object obtained by crosslinking and molding the fluororubber composition. The fluororubber composition comprises hollow particles and a fluororubber. The hollow particles each comprise a shell including a resin and have a hollow surrounded by the shell, and have an iodine value, as determined in accordance with JIS K 0070, of 10-100 g / 100 g. The fluororubber is one crosslinkable with a peroxide.
Need to check novelty before this filing date? Find Prior Art

Description

Fluororubber composition and crosslinked molded article thereof

[0001] The present disclosure relates to a fluororubber composition containing hollow particles and a crosslinked molded article thereof.

[0002] Rubber is used in a wide range of fields for various purposes such as shock absorbers, packings, tubes, O-rings, gaskets, seals, etc. For example, there is a demand for lightweight rubber products for automobiles to improve fuel efficiency.

[0003] One known method for reducing the weight of rubber products is to mix a foaming agent into rubber and foam it by heating during the molding process to produce a foamed elastomer molded body (see, for example, Patent Document 1). However, with methods using a foaming agent, it is difficult to control the size of the pores formed by foaming, so there is a limit to the dimensional stability that can be achieved. On the other hand, a method for introducing a large number of fine pores into a molded body to impart properties or functions such as weight reduction, thermal insulation, and opacity is known, which involves the inclusion of hollow particles (see, for example, Patent Documents 2 and 3). In the method of incorporating hollow particles, the cavities of the hollow particles contained in the molding material become the pores, so there is no problem of controlling the size of the pores formed by foaming, as occurs when using a foaming agent.

[0004] Furthermore, among rubbers, fluororubber is superior to other rubbers in heat resistance, chemical resistance, etc., and is therefore used in applications requiring heat resistance in particular, such as automobile engine parts, and applications requiring chemical resistance, such as in the chemical field. Patent Document 4 discloses a fluororubber composition that uses two specific types of processing aids in combination to improve crosslinking rate, mold releasability, hardness, compression set resistance, and other properties required for molding processability.

[0005] Patent No. 6116787 International Publication No. 2020 / 261926 International Publication No. 2021 / 112110 International Publication No. 2019 / 230830

[0006] However, no fluororubber product has been known to date that is both lightweight and has good compression set resistance.

[0007] The present disclosure has been made in consideration of the above problems, and aims to provide a fluororubber composition that can provide a crosslinked molded article that is lightweight and has reduced compression set, and a crosslinked molded article obtained by crosslinking the fluororubber composition.

[0008] The present disclosure provides the following fluororubber composition: [1] A fluororubber composition comprising hollow particles and a fluororubber, wherein the hollow particles have a shell containing a resin and a hollow portion surrounded by the shell, and the iodine value measured in accordance with JIS K 0070 is 10 g / 100 g or more and 100 g / 100 g or less, and the fluororubber is a fluororubber that can be crosslinked with a peroxide.

[0009] [2] The fluororubber composition according to [1], wherein the content of the hollow particles per 100 parts by mass of the fluororubber is 1 part by mass or more and 50 parts by mass or less. [3] The fluororubber composition according to [1] or [2], wherein the fluororubber is a fluororubber containing at least one halogen atom selected from iodine and bromine in the molecular chain. [4] The fluororubber composition according to any one of [1] to [3], wherein the proportion of particles having a circularity of 0.85 or less is less than 15% by mass of the hollow particles. [5] The fluororubber composition according to any one of [1] to [4], wherein the hollow particles have a residual volatile component content of less than 100 ppm. [6] The fluororubber composition according to any one of [1] to [5], wherein the hollow particles contain, as the resin, a polymer containing 50% by mass or more of crosslinkable monomer units. [7] The fluororubber composition according to any one of [1] to [6], wherein the hollow particles have a volume average particle size of 0.1 μm or more and 100 μm or less. [8] The fluororubber composition according to any one of [1] to [7], further comprising a reinforcing agent, the reinforcing agent being at least one selected from carbon black and silica, and the content of the reinforcing agent relative to 100 parts by mass of the fluororubber is 1 part by mass or more and 15 parts by mass or less. [9] The nitrogen adsorption specific surface area of ​​the carbon black is 5 m or less. 2 / g or more 150m 2

[10] The fluororubber composition according to [8], wherein the reinforcing agent is silica treated with a coupling agent.

[0010] The present disclosure also provides the following crosslinked molded article:

[11] A crosslinked molded article obtained by crosslinking the fluororubber composition according to any one of [1] to

[10] with an organic peroxide.

[0011] According to the present disclosure, it is possible to provide a fluororubber composition capable of providing a crosslinked molded article that is lightweight and has reduced compression set, and a crosslinked molded article thereof.

[0012] 1A to 1C are diagrams illustrating an example of a method for producing hollow particles used in the present disclosure.

[0013] The fluororubber composition and crosslinked molded article of the present disclosure are described in detail below. In this disclosure, the term "to" in a numerical range means that the numerical values ​​before and after the term "to" are included as the lower and upper limits. In this disclosure, (meth)acrylate refers to acrylate and methacrylate, (meth)acrylic refers to acrylic and methacrylic, and (meth)acryloyl refers to acryloyl and methacryloyl.

[0014] 1. Fluororubber Composition The fluororubber composition of the present disclosure comprises hollow particles and a fluororubber, wherein the hollow particles have a shell containing a resin and a hollow portion surrounded by the shell, and the iodine value measured in accordance with JIS K 0070 is 10 g / 100 g or more and 100 g / 100 g or less, and the fluororubber is a fluororubber that can be crosslinked with a peroxide. The fluororubber composition of the present disclosure is used as a molding material for producing a crosslinked molded article. The fluororubber composition of the present disclosure can provide a crosslinked molded article that is lightweight and has reduced compression set. The hollow particles, fluororubber, and other components contained in the fluororubber composition of the present disclosure are described in detail below.

[0015] [Hollow Particles] The hollow particles used in the present disclosure are hollow particles having a shell containing a resin and a hollow portion surrounded by the shell, and are characterized in that the iodine value measured in accordance with JIS K 0070 is 10 g / 100 g or more and 100 g / 100 g or less. Note that in the present disclosure, the iodine value measured in accordance with JIS K 0070 may be simply referred to as the iodine value.

[0016] The iodine value of hollow particles can be used as an indicator of the amount of reactive unsaturated bonds present on the outer surface of hollow particles. Here, reactive unsaturated bonds are typically radical-reactive unsaturated bonds that undergo addition reactions in the presence of radicals. The hollow particles used in the present disclosure have an iodine value of 10 g / 100 g or more, and therefore have a specific amount or more of reactive unsaturated bonds on the outer surface. When such hollow particles are added to a fluororubber and the fluororubber is crosslinked using an organic peroxide, the crosslinking reaction of the fluororubber proceeds due to the radicals generated from the organic peroxide, and the crosslinking reaction between the reactive unsaturated bonds of the hollow particles and the fluororubber also proceeds. Therefore, in a crosslinked molded article obtained by crosslinking the fluororubber composition of the present disclosure using an organic peroxide, the outer surface of the hollow particles and the fluororubber are crosslinked, resulting in excellent adhesion at the interface between the hollow particles and the fluororubber, and less peeling at the interface between the hollow particles and the fluororubber. Furthermore, compared to fluororubber, hollow particles have a higher restoring force when an external force is applied and are less susceptible to plastic deformation. The reason for the reduced compression set in crosslinked molded articles of the fluororubber composition of the present disclosure is believed to be that the fluororubber is crosslinked to the hollow particles, allowing the fluororubber to follow the restoration of the hollow particles when an external force is applied. If the outer surfaces of the hollow particles are not crosslinked to the fluororubber, plastic deformation of the fluororubber is not suppressed, resulting in a large compression set. Furthermore, in crosslinked molded articles of the fluororubber composition of the present disclosure, the hollow particles are resistant to crushing and easily maintain voids, resulting in an excellent weight-reducing effect due to the hollow particles. The reason for the resistance of the hollow particles to crushing is believed to be that a three-dimensional crosslinked structure is formed near the hollow particle surface due to crosslinking between the hollow particle surface and the fluororubber. Furthermore, this three-dimensional crosslinked structure is believed to improve the Young's modulus of the crosslinked molded article, thereby reducing compression set and improving abrasion resistance. Thus, the hollow particles have the effect of reducing the weight of crosslinked molded articles of the fluororubber composition of the present disclosure and reducing the compression set of the crosslinked molded articles. Furthermore, hollow particles can impart various properties to the crosslinked molded article, such as heat insulation and the ability to retain functional components such as antibacterial agents, in addition to reducing the weight and compression set of the crosslinked molded article.

[0017] When the iodine value of the hollow particles is 10 g / 100 g or more, a sufficient number of crosslinks are formed between the hollow particles and the fluororubber, resulting in an excellent effect of reducing the compression set of the crosslinked molded article. The iodine value of the hollow particles used in the present disclosure is preferably 12 g / 100 g or more, more preferably 15 g / 100 g or more, even more preferably 20 g / 100 g or more, and even more preferably 30 g / 100 g or more. On the other hand, if there are too many reaction sites on the outer surface of the hollow particles, crosslinks are likely to be formed between the hollow particles, which makes the hollow particles more likely to aggregate, worsening the dispersibility of the hollow particles and making it impossible to sufficiently reduce the compression set of the crosslinked molded article. When the iodine value of the hollow particles used in the present disclosure is 100 g / 100 g or less, a sufficient number of crosslinks are formed between the hollow particles and the fluororubber, resulting in a reduction in the compression set of the crosslinked molded article. The iodine value of the hollow particles used in the present disclosure is preferably 80 g / 100 g or less, more preferably 70 g / 100 g or less, and even more preferably 40 g / 100 g or less, from the viewpoint of reducing the compression set of the crosslinked molded article.

[0018] The hollow particles used in the present disclosure are particles having a resin-containing shell (outer shell) and a hollow portion surrounded by the shell, and have a reactive unsaturated bond on the outer surface of the shell. Examples of the reactive unsaturated bond include reactive unsaturated bonds contained in vinyl groups, (meth)acryloyl groups, allyl groups, butenyl groups, maleimide groups, nadimide groups, propargyl groups, or ethynyl groups. Ethylenically unsaturated bonds are preferred, and ethylenically unsaturated bonds contained in at least one group selected from the group consisting of vinyl groups, (meth)acryloyl groups, and allyl groups are more preferred, and ethylenically unsaturated bonds contained in at least one group selected from vinyl groups and (meth)acryloyl groups are even more preferred. Note that the (meth)acryloyl group refers to both an acryloyl group and a methacryloyl group. In the hollow particles used in the present disclosure, the reactive unsaturated bond on the outer surface of the shell may be a reactive unsaturated bond possessed by a crosslinkable monomer unit or a reactive unsaturated bond possessed by a coupling agent used for surface treatment, but is preferably a reactive unsaturated bond possessed by a crosslinkable monomer unit. In other words, it is preferable that at least one polymerizable functional group possessed by the crosslinkable monomer is present unreacted on the surface of the shell. The crosslinkable monomer, coupling agent, etc. used in the production of hollow particles will be described in detail in the "Production Method of Hollow Particles" section below.

[0019] The resin contained in the shell of the hollow particles used in the present disclosure is typically a polymer of a polymerizable monomer used in the hollow particle manufacturing method described below. The shell of the hollow particles may further contain a surface treatment agent, an additive, or the like, as long as the object of the present disclosure is not impaired. In the hollow particles used in the present disclosure, the content of the resin contained in the shell is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 98% by mass or more, and the shell may be made of resin.

[0020] The shell of the hollow particles used in the present disclosure may be a resin layer containing a polymer of a polymerizable monomer, the outer surface of which may be surface-treated with a coupling agent. Surface-treated shells of the hollow particles used in the present disclosure are preferred in that the crosslinked molded article of the present disclosure has improved mechanical properties such as tensile strength, tear strength, and abrasion resistance.

[0021] The hollow particles used in the present disclosure may have polar groups such as amino groups or acidic groups on the particle surface. Examples of methods for introducing polar groups onto the surfaces of hollow particles include a method of reacting a modifier for introducing polar groups, a method of surface treatment with a coupling agent having a polar group, and a method of using a polymerizable monomer having a polar group.

[0022] In the hollow particles used in the present disclosure, the hollow portion is a hollow space clearly distinguishable from the shell. The shell of the hollow particle may have a porous structure, in which case the hollow portion has a size clearly distinguishable from the numerous minute spaces uniformly dispersed within the porous structure. Furthermore, from the viewpoint of weight reduction, the hollow particles used in the present disclosure preferably have the hollow portion filled with a gas such as air. The hollow particles used in the present disclosure may have one or more hollow portions, but from the viewpoint of maintaining a good balance between high porosity and mechanical strength, those having only one or two hollow portions are preferred, and those having only one hollow portion are preferred. In the hollow particles used in the present disclosure, the proportion of particles having only one hollow portion by number is preferably 90% or more, more preferably 95% or more, and even more preferably more than 95%. Furthermore, the shell of the hollow particles used in the present disclosure, and the partition walls separating adjacent hollow portions when the hollow particles have two or more hollow portions, may be porous, but are preferably solid in order to reduce the compression set of the cross-linked molded product and improve the mechanical strength of the hollow particles. The shape of the hollow particles used in the present disclosure may be, for example, spherical, oval, or irregular, but is preferably spherical in terms of the dispersibility and pressure resistance of the hollow particles. One example of the shape of the hollow particles used in the present disclosure is a bag made of a thin film and inflated with gas, and its cross-section is shown in hollow particle 10 in (5) of Figure 1. In this example, a thin film is provided on the outside, and the interior is filled with gas. The hollow portion of the hollow particle can be confirmed, for example, by observing the cross-section of the particle using an SEM or by observing the particle itself using a TEM. The shape of the hollow particles can be confirmed, for example, by observing the hollow particles with an SEM or TEM.

[0023] The hollow particles used in the present disclosure may contain a small amount of low-circularity particles, such as cracked or deformed particles, as impurities. However, from the viewpoint of weight reduction and reducing the compression set of the crosslinked molded article, the proportion of particles with a circularity of 0.85 or less is preferably less than 15% by mass, more preferably less than 10% by mass, and even more preferably less than 8% by mass of 100% by mass of hollow particles. Particles with a circularity of 0.85 or less are typically particles that have deformations such as dents or cracks, and are sometimes referred to as "irregularly shaped particles" in the present disclosure. Such irregularly shaped particles have a lower porosity than spherical hollow particles, resulting in a poorer weight reduction effect. Therefore, reducing the proportion of irregularly shaped particles contained in the hollow particles can improve the weight reduction effect of the hollow particles. Furthermore, irregularly shaped particles tend to aggregate more easily when dispersed in fluororubber than spherical particles, resulting in poorer dispersibility. Therefore, reducing the proportion of irregularly shaped particles contained in the hollow particles can improve the dispersibility of the hollow particles, thereby further reducing the compression set of the crosslinked molded article. Furthermore, irregularly shaped particles have the problem of being inferior in pressure resistance compared to spherical particles because they are more susceptible to localized external pressure. When irregularly shaped particles are dispersed in fluororubber, agglomerates are likely to form, and the agglomerates are more susceptible to external pressure, further reducing the pressure resistance. Therefore, the pressure resistance of hollow particles can be improved by reducing the proportion of irregularly shaped particles contained in the hollow particles.

[0024] Circularity is defined as the diameter of a circle having the same area as the projected image of a particle (equivalent circle area diameter) divided by the diameter of a circle having the same perimeter as the projected image of the particle (equivalent circumferential diameter). When a particle is a perfect sphere, the circularity is 1, and the more complex the particle's surface shape, the smaller the circularity value. The hollow particles used in the present disclosure may have an average circularity of 0.950 to 0.995. In the present disclosure, circularity is measured using a flow-type particle image analyzer with an image resolution of 0.185 μm / pixel. A preferred example of a flow-type particle image analyzer is the "IF-3200" manufactured by Jasco International Co., Ltd. A measurement sample is prepared, for example, by dispersing 0.10 to 0.12 g of hollow particles in an aqueous solution of linear alkylbenzenesulfonate (0.3% concentration) for 5 minutes in an ultrasonic cleaner. The average circularity is the average value of the circularity of 1,000 to 3,000 arbitrarily selected particles.

[0025] The porosity of the hollow particles used in the present disclosure is not particularly limited, but from the viewpoint of weight reduction, it is preferably 60% or more, more preferably 65% ​​or more, and even more preferably 70% or more. The upper limit of the porosity of the hollow particles is not particularly limited, but from the viewpoint of suppressing a decrease in the strength of the hollow particles and making them less likely to be crushed, it is preferably 90% or less, more preferably 85% or less, and even more preferably 80% or less.

[0026] The porosity of the hollow particles is the apparent density D 1 and true density D 0 The apparent density of the hollow particles D 1 The measurement method is as follows: First, a volume of 100 cm 3 About 30 cm 3 The volumetric flask is filled with hollow particles, and the mass of the filled hollow particles is accurately weighed. Next, the volumetric flask filled with the hollow particles is accurately filled with isopropanol up to the marked line, taking care not to introduce air bubbles. The mass of isopropanol added to the volumetric flask is accurately weighed, and the apparent density D of the hollow particles is calculated based on the following formula (I): 1 (g / cm 3 ) is calculated by the formula (I) Apparent density D1 Apparent density D = [Mass of hollow particles] / (100 - [Mass of isopropanol] / [Specific gravity of isopropanol at measurement temperature]) 1 corresponds to the specific gravity of the entire hollow particle when the hollow portion is considered to be a part of the hollow particle.

[0027] True density D of hollow particles 0 The measurement method is as follows: After crushing the hollow particles in advance, 3 Approximately 10 g of crushed pieces of hollow particles are filled into a measuring flask, and the mass of the crushed pieces is accurately weighed. Then, in the same manner as in the measurement of the apparent density, isopropanol is added to the measuring flask, and the mass of the isopropanol is accurately weighed. The true density D of the hollow particles is calculated based on the following formula (II): 0 (g / cm 3 ) is calculated using the formula (II) 0 = [mass of crushed pieces of hollow particles] / (100 - [mass of isopropanol] / [specific gravity of isopropanol at measurement temperature]) True density D 0 As is clear from the above measurement method, the true density D 0 In calculating the particle diameter, the hollow portion is not considered to be part of the hollow particle.

[0028] The porosity (%) of the hollow particles is calculated by multiplying the apparent density D 1 and true density D 0 The porosity (%) is calculated by the following formula (III): 1 / True density D 0 ) x 100

[0029] The volume average particle size of the hollow particles used in the present disclosure is not particularly limited, but the lower limit is preferably 0.1 μm or more, more preferably 1 μm or more, and the upper limit is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less. When the volume average particle size of the hollow particles used in the present disclosure is equal to or greater than the above lower limit, aggregation of the hollow particles is suppressed and dispersibility is improved, thereby improving the effect of reducing the compression set of the crosslinked molded article. When the volume average particle size of the hollow particles used in the present disclosure is equal to or less than the above upper limit, reduction in the specific surface area of ​​the hollow particles is suppressed, and as a result, reduction in the interface between the hollow particles and the fluororubber is suppressed, thereby increasing the amount of crosslinking bonds formed between the hollow particles and the fluororubber, and improving the effect of reducing the compression set of the crosslinked molded article.

[0030] The particle size distribution of the hollow particles (volume average particle size (Dv) / number average particle size (Dp)) is not particularly limited, but is preferably 1.05 or more and 1.30 or less, and more preferably 1.10 or more and 1.30 or less. A particle size distribution of 1.30 or less tends to be excellent in reducing the compression set of the crosslinked molded article, and particles with less variation in performance between particles can be obtained. Furthermore, a particle size distribution of 1.30 or less can improve the thickness uniformity, for example, when the crosslinked molded article of the present disclosure is formed into a sheet. The volume average particle size (Dv) and number average particle size (Dp) of the hollow particles can be determined, for example, by measuring the particle size of the hollow particles using a particle size distribution measuring device using the Coulter Counter method, calculating the number average and volume average, respectively, and using the obtained values ​​as the number average particle size (Dp) and volume average particle size (Dv) of the particles. The particle size distribution is the value obtained by dividing the volume average particle size by the number average particle size. The Coulter counter method is a method for measuring particle diameter using an electrical resistance method known as the Coulter principle.

[0031] The hollow particles used in the present disclosure are not particularly limited, but preferably have a residual volatile component content of less than 100 ppm. If the residual volatile component content of the hollow particles is high, the residual volatile component will be present on the outer surface of the hollow particles. The residual volatile component present on the outer surface of the hollow particles inhibits the crosslinking reaction between the reactive unsaturated bonds on the outer surface of the hollow particles and the fluororubber. Therefore, if the residual volatile component content of the hollow particles is high, the adhesion between the hollow particles contained in the crosslinked molded article and the fluororubber will deteriorate, resulting in an increase in the compression set of the crosslinked molded article. In contrast, if the residual volatile component content of the hollow particles is less than 100 ppm, the increase in the compression set of the crosslinked molded article can be sufficiently suppressed. From the viewpoint of reducing the compression set of the crosslinked molded article, the residual volatile component content of the hollow particles used in the present disclosure is more preferably less than 50 ppm, even more preferably less than 30 ppm. The residual volatile components are typically organic compounds with a molecular weight of 500 or less, including, for example, residual polymerizable monomers, residual hydrophobic solvents, and decomposition products of polymerization initiators. The residual volatile component content is the ratio of the mass of the residual volatile components contained in the hollow particles to the mass of the hollow particles. The lower limit of the residual volatile component content of the hollow particles used in the present disclosure is not particularly limited, but from the perspective of ease of production, it may be, for example, 1 ppm or more, 2 ppm or more, or 3 ppm or more. The residual volatile component content of the hollow particles can be measured by purge and trap / gas chromatography (P&T / GC). Specifically, the measurement method described in the Examples below can be used.

[0032] The hollow particles used in the present disclosure preferably have a total content of surfactants and water-soluble polymer stabilizers (hereinafter simply referred to as "surfactants, etc.") present on the outer surface of the particles of 500 ppm or less, more preferably 200 ppm or less, even more preferably 100 ppm or less, and even more preferably 50 ppm or less. The water-soluble polymer stabilizer may be either organic or inorganic. When the content of surfactants, etc. present on the outer surface of hollow particles is below the above upper limit, the reactivity between the hollow particles and the fluororubber is suppressed from decreasing, thereby improving the effect of reducing the compression set of the crosslinked molded product. By using only an inorganic dispersion stabilizer as a dispersion stabilizer in the hollow particle manufacturing process described below, the content of surfactants, etc. present on the hollow particle surface can be reduced to below the measurement limit. In the present disclosure, the content of surfactants, etc. present on the outer surface of hollow particles refers to the ratio of the mass of surfactants, etc. present on the outer surface of hollow particles to the mass of the hollow particles. The surfactants, etc. present on the outer surface of hollow particles can be extracted, for example, by ultrasonicating the hollow particles in water. The type and mass of the surfactants, etc. extracted in water can be determined by 1 It can be identified from the peak position and peak intensity of the H-NMR spectrum. In this method, the measurement limit of the amount of surfactant or the like present on the hollow particle surface is usually 0.05 ppm.

[0033] The thermal decomposition initiation temperature of the hollow particles used in the present disclosure is not particularly limited, but from the viewpoint of heat resistance, it is preferably 345°C or higher, more preferably 350°C or higher. The upper limit of the thermal decomposition initiation temperature of the hollow particles is not particularly limited, but may be, for example, 400°C or lower. In the present disclosure, the thermal decomposition initiation temperature of the hollow particles is the temperature at which a 5% weight loss occurs, and can be measured using a TG-DTA device under conditions of a nitrogen atmosphere, a nitrogen flow rate of 230 mL / min, and a heating rate of 10°C / min.

[0034] In the fluororubber composition of the present disclosure, the content of hollow particles is not particularly limited. On a mass basis, the lower limit is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and even more preferably 10 parts by mass or more, per 100 parts by mass of the fluororubber. The upper limit is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less. In the fluororubber composition of the present disclosure, the content of hollow particles on a volume basis is also not particularly limited. On a volume basis, the lower limit is preferably 15% by volume or more, more preferably 20% by volume or more, even more preferably 30% by volume or more, and the upper limit is preferably 70% by volume or less, more preferably 60% by volume or less, and even more preferably 50% by volume or less. When the content of hollow particles is equal to or greater than the lower limit, the hollow particles have excellent effects of reducing weight and compression set. When the content of hollow particles is equal to or less than the upper limit, the fluororubber composition is easily kneaded. Furthermore, since the deterioration of the dispersibility of the hollow particles is suppressed, the hollow particles are excellent in the effect of reducing compression set. Moreover, since a sufficient amount of fluororubber can be contained, the inherent properties of the fluororubber can be sufficiently maintained in the fluororubber composition.

[0035] [Method for Producing Hollow Particles] The hollow particles used in the present disclosure are produced, for example, by a production method based on suspension polymerization, as described below. One embodiment of the method for producing hollow particles used in the present disclosure includes the steps of: preparing a mixture containing a polymerizable monomer, a hydrophobic solvent, a polymerization initiator, a dispersion stabilizer, and an aqueous medium; suspending the mixture to prepare a suspension in which droplets of a monomer composition containing the polymerizable monomer, the hydrophobic solvent, and the polymerization initiator are dispersed in the aqueous medium; subjecting the suspension to a polymerization reaction to prepare a precursor composition in which precursor particles having a hollow portion surrounded by a resin-containing shell and filled with the hydrophobic solvent are dispersed in the aqueous medium; and removing the hydrophobic solvent from the precursor particles. In the present disclosure, hollow particles whose hollow portions are filled with the hydrophobic solvent are sometimes referred to as "precursor particles," as they are considered to be intermediates to hollow particles whose hollow portions are filled with gas. In this disclosure, "precursor composition" means a composition that includes precursor particles.

[0036] In the above-described manufacturing method, a mixture containing a polymerizable monomer, a hydrophobic solvent, a polymerization initiator, a dispersion stabilizer, and an aqueous medium is suspended, whereby the polymerizable monomer and the hydrophobic solvent undergo phase separation, resulting in the preparation of a suspension in which droplets of a monomer composition are dispersed in the aqueous medium, with the distribution structure being such that the polymerizable monomer is unevenly distributed on the surface and the hydrophobic solvent is unevenly distributed in the center. When this suspension is subjected to a polymerization reaction, a polymer begins to precipitate on the surface of the droplets of the monomer composition. As the polymerization reaction progresses, the droplet surfaces harden, forming shells, resulting in hollow particles with hollow spaces filled with the hydrophobic solvent. By adding a crosslinkable monomer to the mixture, reactive unsaturated bonds can be introduced into the outer surface of the shell.

[0037] The above-mentioned production method includes a step of preparing a mixed solution, a step of preparing a suspension, a step of subjecting the suspension to a polymerization reaction, and a step of removing the hydrophobic solvent, and may further include other steps. Furthermore, as far as technically possible, two or more of the above steps and other additional steps may be performed simultaneously as a single step, or the order may be reversed. For example, the preparation of the mixed solution and the suspension may be performed simultaneously in a single step, such as by simultaneously adding the materials for preparing the mixed solution and suspending them.

[0038] A preferred example of the method for producing hollow particles includes the following steps: (1) mixed solution preparation step: preparing a mixed solution containing a polymerizable monomer, a hydrophobic solvent, a polymerization initiator, a dispersion stabilizer, and an aqueous medium; (2) suspending step: suspending the mixed solution to prepare a suspension in which droplets of a monomer composition containing a polymerizable monomer, a hydrophobic solvent, and a polymerization initiator are dispersed in an aqueous medium; (3) polymerizing step: subjecting the suspension to a polymerization reaction to prepare a precursor composition in which precursor particles having a hollow portion surrounded by a shell containing a resin and filled with the hydrophobic solvent are dispersed in the aqueous medium; (4) solid-liquid separation step: obtaining a solid content containing precursor particles or hollow particles by solid-liquid separation; and (5) solvent removal step: removing the hydrophobic solvent from the precursor particles to obtain hollow particles.

[0039] FIG. 1 is a schematic diagram illustrating an example of the manufacturing method of the present disclosure. (1) to (5) in FIG. 1 correspond to the above-described steps (1) to (5). In the method illustrated in FIG. 1, the solvent removal step is performed after the solid-liquid separation step. However, the solid-liquid separation step may also be performed after the solvent removal step. In FIG. 1, the white arrows between the diagrams indicate the order of the steps. Note that FIG. 1 is merely a schematic diagram for explanatory purposes, and the manufacturing method of the present disclosure is not limited to that shown in the diagram. Furthermore, the structure, dimensions, and shape of the materials used in the manufacturing method of the present disclosure are not limited to those of the various materials illustrated in these diagrams. (1) in FIG. 1 is a cross-sectional schematic diagram illustrating one embodiment of a mixed solution used in the mixed solution preparation step. As shown in this diagram, the mixed solution contains an aqueous medium 1 and a low-polarity material 2 dispersed in the aqueous medium 1. Here, the low-polarity material 2 refers to a material that has low polarity and is difficult to mix with the aqueous medium 1. In the present disclosure, the low-polarity material 2 contains a polymerizable monomer, a hydrophobic solvent, and a polymerization initiator. FIG. 1 (2) is a cross-sectional schematic diagram showing one embodiment of a suspension in the suspension step. The suspension includes an aqueous medium 1 and droplets 8 of a monomer composition dispersed in the aqueous medium 1. The droplets 8 of the monomer composition contain a polymerizable monomer, a hydrophobic solvent, and a polymerization initiator, but the distribution within the droplets is non-uniform. The droplets 8 of the monomer composition are phase-separated into a hydrophobic solvent 4a and a material other than the hydrophobic solvent, including the polymerizable monomer, a material 4b, with the hydrophobic solvent 4a concentrated in the center and the material other than the hydrophobic solvent 4b concentrated on the surface, and a dispersion stabilizer (not shown) attached to the surface. FIG. 1 (3) is a cross-sectional schematic diagram showing one embodiment of a precursor composition obtained by the polymerization step, including precursor particles encapsulating a hydrophobic solvent in their hollow portions. The precursor composition includes an aqueous medium 1 and precursor particles 9 encapsulating a hydrophobic solvent 4a in their hollow portions, dispersed in the aqueous medium 1. The shell 6 forming the outer surface of the precursor particle 9 is formed by polymerization of the polymerizable monomer in the droplet 8 of the monomer composition, and contains a polymer of the polymerizable monomer as a resin. Figure 1 (4) is a cross-sectional schematic diagram showing one embodiment of the precursor particle after the solid-liquid separation step. This Figure 1 (4) shows the state in which the aqueous medium 1 has been removed from the state of Figure 1 (3). Figure 1 (5) is a cross-sectional schematic diagram showing one embodiment of the hollow particle after the solvent removal step.1 (5) shows the state after removing the hydrophobic solvent 4a from the state shown in FIG. 1 (4). By removing the hydrophobic solvent from the precursor particles, hollow particles 10 having gas-filled hollow portions 7 inside the shells 6 are obtained. The above five steps and other steps will be described below in order.

[0040] (1) Mixed Liquid Preparation Step This step is a step of preparing a mixed liquid containing a polymerizable monomer, a hydrophobic solvent, a polymerization initiator, a dispersion stabilizer, and an aqueous medium. The mixed liquid may further contain other materials as long as the purpose of the present disclosure is not impaired. The materials of the mixed liquid will be described in the following order: (A) polymerizable monomer, (B) hydrophobic solvent, (C) polymerization initiator, (D) dispersion stabilizer, and (E) aqueous medium.

[0041] (A) Polymerizable Monomer In the present disclosure, a polymerizable monomer is a compound having a functional group capable of addition polymerization (sometimes simply referred to as a polymerizable functional group in the present disclosure). In the present disclosure, a compound having an ethylenically unsaturated bond as a functional group capable of addition polymerization is generally used as the polymerizable monomer. As the polymerizable functional group, a radically polymerizable group is preferred. In terms of excellent reactivity, at least one selected from the group consisting of a (meth)acryloyl group, a vinyl group, and an allyl group is preferred, and at least one selected from a (meth)acryloyl group and a vinyl group is more preferred. In the present disclosure, a polymerizable monomer having only one polymerizable functional group is referred to as a non-crosslinkable monomer, and a polymerizable monomer having two or more polymerizable functional groups is referred to as a crosslinkable monomer. The crosslinkable monomer can form a crosslinked bond in a polymer by a polymerization reaction. The crosslinkable monomer becomes a crosslinkable monomer unit in the shell, and the non-crosslinkable monomer becomes a non-crosslinkable monomer unit in the shell. In the present disclosure, a polymerizable monomer consisting of carbon and hydrogen is referred to as a hydrocarbon monomer, a crosslinkable monomer consisting of carbon and hydrogen is referred to as a crosslinkable hydrocarbon monomer, and a non-crosslinkable monomer consisting of carbon and hydrogen is referred to as a non-crosslinkable hydrocarbon monomer. Furthermore, a polymerizable monomer having a (meth)acryloyl group as a polymerizable functional group is referred to as an acrylic monomer, a crosslinkable monomer having a (meth)acryloyl group as a polymerizable functional group is referred to as a crosslinkable acrylic monomer, and a non-crosslinkable monomer having a (meth)acryloyl group as a polymerizable functional group is referred to as a non-crosslinkable acrylic monomer. In a crosslinkable acrylic monomer, at least one polymerizable functional group may be a (meth)acryloyl group, but it is preferred that all polymerizable functional groups are (meth)acryloyl groups.

[0042] The polymerizable monomer may be any known polymerizable monomer conventionally used in the preparation of hollow particles. While not particularly limited, it is preferable to include at least a crosslinkable monomer in order to achieve an iodine value of the hollow particles within the above range. The iodine value of the hollow particles can be achieved within the above range by allowing a portion of the reactive unsaturated bonds of the crosslinkable monomer to remain unreacted on the outer surface of the shell. Furthermore, when the crosslinkable monomer is included as the polymerizable monomer, the crosslink density of the polymer precipitated on the droplet surface increases when the suspension is subjected to a polymerization reaction. Furthermore, the precipitates are crosslinked to each other, thereby increasing the crosslink density of the shell. This facilitates the formation of a shell with excellent strength, and the hollow particles are more likely to become spherical, resulting in the formation of hollow portions clearly distinguishable from the shell within the particles. The stronger the shell, the less likely the hollow particles are to undergo plastic deformation. Therefore, improving the shell strength can improve the effect of reducing the compression set of the crosslinked molded product.

[0043] Examples of the crosslinkable monomer include crosslinkable hydrocarbon monomers such as aromatic divinyl monomers such as divinylbenzene, divinylbiphenyl, and divinylnaphthalene; straight-chain or branched diolefins such as butadiene, isoprene, 2,3-dimethylbutadiene, pentadiene, and hexadiene; and diene monomers such as alicyclic diolefins such as dicyclopentadiene, cyclopentadiene, and ethylidenetetracyclododecene; allyl (meth)acrylate, vinyl (meth)acrylate, ethylene glycol diolefins, and the like. (meth)acrylate, diethylene glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 3-(meth)acryloyloxy-2-hydroxypropyl (meth)acrylate, 1,3-bis(methacryloyloxy)-2-hydroxypropane, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol Difunctional crosslinkable acrylic monomers such as ricol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, bisphenol A di(meth)acrylate, and their ethoxylated derivatives, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, crosslinkable acrylic monomers having three or more functionalities such as acrylate, dipentaerythritol poly(meth)acrylate, and their ethoxylated derivatives; crosslinkable allylic monomers such as diallyl phthalate; crosslinkable macromers such as polybutadiene, polyisoprene, styrene-butadiene block copolymer (SBS), styrene-isoprene block copolymer (SIS), polyphenylene ether vinyl-modified at both ends, and polyphenylene ether (meth)acrylic-modified at both ends. These crosslinkable monomers can be used alone or in combination of two or more.

[0044] In the present disclosure, in order to set the iodine value of the hollow particles within the above range and to improve the strength of the shell and reduce the compression set of the crosslinked molded article, the crosslinkable monomer preferably contains at least one selected from a crosslinkable acrylic monomer and a crosslinkable hydrocarbon monomer, and more preferably contains a combination of a crosslinkable acrylic monomer and a crosslinkable hydrocarbon monomer. Among crosslinkable monomers, crosslinkable acrylic monomers are preferred from the viewpoint of improving the shell strength, while crosslinkable hydrocarbon monomers are preferred from the viewpoint of easily introducing reactive unsaturated bonds into the outer surface of the shell. Among crosslinkable hydrocarbon monomers, aromatic divinyl monomers are preferred, and divinylbenzene is particularly preferred. As the crosslinkable acrylic monomer, both the bifunctional crosslinkable acrylic monomers and trifunctional or higher crosslinkable acrylic monomers described above are preferred. From the viewpoint of improving the shell strength and reducing the compression set of the crosslinked molded article, it is preferable to contain at least a bifunctional crosslinkable acrylic monomer, and it is more preferable to contain a combination of a bifunctional crosslinkable acrylic monomer and a trifunctional or higher functional crosslinkable acrylic monomer. Among the bifunctional crosslinkable acrylic monomers, at least one selected from the group consisting of ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, and pentaerythritol di(meth)acrylate is preferred. Among the trifunctional or higher functional crosslinkable acrylic monomers, at least one selected from the group consisting of trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate is preferred.

[0045] In the present disclosure, in order to set the iodine value of the hollow particles within the above range and to improve the shell strength and reduce the compression set of the crosslinked molded article, the content of the crosslinkable monomer in 100% by mass of polymerizable monomers is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more. In the present disclosure, the polymerizable monomer may consist of a crosslinkable monomer, but may also contain a non-crosslinkable monomer, which will be described later as a polymerizable monomer. Therefore, the content of the crosslinkable monomer in 100% by mass of polymerizable monomers may be, for example, 99% by mass or less, 98% by mass or less, or 97% by mass or less. The content of each monomer in 100% by mass of polymerizable monomers corresponds to the content of each monomer unit in 100% by mass of all monomer units constituting the polymer contained in the shell.

[0046] In order to set the iodine value of the hollow particles within the above range and to improve the shell strength and reduce the compression set of the crosslinked molded article, the content of the crosslinkable hydrocarbon monomer in 100% by mass of the polymerizable monomer is preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more as a lower limit, and is not particularly limited to an upper limit, and may be 100% by mass, but is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 70% by mass or less, and even more preferably 60% by mass or less. From the same viewpoint, the content of the crosslinkable acrylic monomer in 100% by mass of the polymerizable monomer is not particularly limited to a lower limit, and may be 0% by mass, but is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and even more preferably 40% by mass or more as an upper limit, and is preferably 90% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less as an upper limit. Furthermore, when a bifunctional crosslinkable acrylic monomer and a tri- or higher functional crosslinkable acrylic monomer are contained in combination, from the viewpoint of setting the iodine value of the hollow particles within the above range and improving the shell strength to reduce the compression set of the crosslinked molded article, the content of the bifunctional crosslinkable acrylic monomer relative to the total 100 mass% of the bifunctional crosslinkable acrylic monomer and the tri- or higher functional crosslinkable acrylic monomer is preferably 20 mass% or more, more preferably 30 mass% or more, and even more preferably 40 mass% or more, and the upper limit is preferably 70 mass% or less, more preferably 60 mass% or less, and even more preferably 50 mass% or less.

[0047] In order to set the iodine value of the hollow particles within the above range and to improve the shell strength and reduce the compression set of the crosslinked molded article, when the crosslinkable monomer contains a crosslinkable acrylic monomer and a crosslinkable hydrocarbon monomer, the content of the crosslinkable acrylic monomer relative to 100 parts by mass of the total of the crosslinkable acrylic monomer and the crosslinkable hydrocarbon monomer is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, and still more preferably 40 parts by mass or more, and the upper limit is preferably 90 parts by mass or less, preferably 70 parts by mass or less, and more preferably 60 parts by mass or less.

[0048] In the present disclosure, in order to set the iodine value of the hollow particles within the above range and to improve the shell strength and reduce the compression set of the crosslinked molded product, the total content of the crosslinkable acrylic monomer and the crosslinkable hydrocarbon monomer per 100 parts by mass of the crosslinkable monomer is preferably 80 parts by mass or more, more preferably 90 parts by mass or more, even more preferably 95 parts by mass or more, and still more preferably 99 parts by mass or more.

[0049] In the present disclosure, the polymerizable monomer may further include a non-crosslinkable monomer. Examples of the non-crosslinkable monomer include aromatic monovinyl monomers such as styrene, vinyltoluene, α-methylstyrene, p-methylstyrene, ethylvinylbenzene, ethylvinylbiphenyl, and ethylvinylnaphthalene, linear or branched monoolefins such as ethylene, propylene, and butylene, and alicyclic monoolefins such as vinylcyclohexane, norbornene, tricyclododecene, and 1,4-methano-1,4,4a,9a-tetrahydrofluorene, and other non-crosslinkable hydrocarbon monomers; methyl(meth)acrylate; acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, t-butylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-aminoethyl (meth)acrylate, (meth)acrylic acid, (meth)acrylamide, N-methylol (meth)acrylamide, N-butoxymethyl (meth)acrylamide, methoxypolyethylene glycol (meth)acrylate, ethoxypolyethylene glycol non-crosslinkable acrylic monomers such as polyethylene glycol (meth)acrylate, propoxy polyethylene glycol (meth)acrylate, butoxy polyethylene glycol (meth)acrylate, hexaoxy polyethylene glycol (meth)acrylate, octoxy polyethylene glycol polypropylene glycol (meth)acrylate, lauroxy polyethylene glycol (meth)acrylate, stearoxy polyethylene glycol (meth)acrylate, phenoxy polyethylene glycol polypropylene glycol (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol propylene glycol mono(meth)acrylate, polyethylene glycol tetramethylene glycol (meth)acrylate, propylene glycol polybutylene glycol mono(meth)acrylate, and monoethylene glycol mono(meth)acrylate; carboxylic acid vinyl ester monomers such as vinyl acetate; halogenated aromatic vinyl monomers such as halogenated styrene;Examples of suitable non-crosslinkable monomers include vinyl halide monomers such as vinyl chloride, vinylidene halide monomers such as vinylidene chloride, vinylpyridine, and non-crosslinkable macromers such as polystyrene (one end of which is (meth)acrylic-modified) and polymethyl methacrylate (one end of which is (meth)acrylic-modified). These non-crosslinkable monomers can be used alone or in combination of two or more.

[0050] The content of the non-crosslinkable monomer in 100% by mass of the polymerizable monomer is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 10% by mass or less, and more preferably 5% by mass or less, from the viewpoint of setting the iodine value of the hollow particles within the above range and of suppressing a decrease in shell strength. The lower limit of the content of the non-crosslinkable monomer in 100% by mass of the polymerizable monomer is not particularly limited, and may be, for example, 1% by mass or more, 2% by mass or more, or 3% by mass or more.

[0051] The content of the polymerizable monomer in the mixed solution is not particularly limited, but from the viewpoint of the balance between the porosity, particle size, and mechanical strength of the hollow particles, it is preferably 15 to 50% by mass, more preferably 20 to 40% by mass, relative to 100% by mass of the total mass of the components in the mixed solution excluding the aqueous medium. Furthermore, in order to prevent a decrease in the strength of the resulting hollow particles, the content of the polymerizable monomer in the mixed solution is preferably 96% by mass or more, more preferably 97% by mass or more, relative to 100% by mass of the total mass of the solids, excluding the hydrophobic solvent, of the materials that form the oil phase. In the present disclosure, the solids refer to all components excluding the solvent, and liquid polymerizable monomers and the like are considered to be included in the solids.

[0052] (B) Hydrophobic Solvent The hydrophobic solvent used in the manufacturing method of the present disclosure is a non-polymerizable, poorly water-soluble organic solvent. The hydrophobic solvent acts as a spacer material that forms hollow spaces inside the particles. In the suspension process described below, a suspension is obtained in which droplets of a monomer composition containing a hydrophobic solvent are dispersed in an aqueous medium. In the suspension process, phase separation occurs within the droplets of the monomer composition, and the hydrophobic solvent, which has low polarity, tends to collect inside the droplets. Ultimately, the droplets of the monomer composition contain the hydrophobic solvent inside, and other materials other than the hydrophobic solvent are distributed around the periphery according to their respective polarities. Then, in the polymerization process described below, an aqueous dispersion containing precursor particles encapsulating the hydrophobic solvent is obtained. In other words, as the hydrophobic solvent collects inside the particles, hollow spaces filled with the hydrophobic solvent are formed inside the resulting precursor particles.

[0053] The hydrophobic solvent can be appropriately selected from known hydrophobic solvents and is not particularly limited. Examples include esters such as ethyl acetate and butyl acetate; ether esters such as propylene glycol monomethyl ether acetate and propylene glycol monoethyl ether acetate; and hydrocarbon solvents. Among these, hydrocarbon solvents are preferred, and hydrocarbon solvents having 5 to 8 carbon atoms are more preferred. Examples of hydrocarbon solvents include aliphatic hydrocarbons including chain hydrocarbon solvents such as pentane, hexane, heptane, octane, 2-methylbutane, 2-methylpentane, and paraffin solvents, and cyclic hydrocarbon solvents such as cyclohexane, methylcyclohexane, and cycloheptane; and aromatic hydrocarbons such as benzene, toluene, and xylene. These hydrophobic solvents can be used alone or in combination of two or more.

[0054] In the suspension step, since phase separation between the polymerizable monomer and the hydrophobic solvent is likely to occur in droplets of the monomer composition, it is preferable to select an organic solvent that has a lower solubility in water than the crosslinkable monomer contained in the polymerizable monomer as the hydrophobic solvent. Furthermore, when the polymerizable monomer contains a hydrocarbon monomer, the hydrophobic solvent is preferably a hydrocarbon-based solvent, more preferably a chain hydrocarbon-based solvent, even more preferably a chain hydrocarbon-based solvent having 5 to 8 carbon atoms, and even more preferably at least one selected from the group consisting of pentane, hexane, heptane, and octane.

[0055] Furthermore, although not particularly limited, the boiling point of the hydrophobic solvent is preferably 130° C. or lower, more preferably 100° C. or lower, from the viewpoint of ease of removal in the solvent removal step described below, and is preferably 50° C. or higher, more preferably 60° C. or higher, from the viewpoint of ease of inclusion in the precursor particles. When the hydrophobic solvent is a mixed solvent containing multiple types of hydrophobic solvents and has multiple boiling points, it is preferable that the boiling point of the solvent with the highest boiling point among the solvents contained in the mixed solvent is not higher than the above-mentioned upper limit, and it is preferable that the boiling point of the solvent with the lowest boiling point among the solvents contained in the mixed solvent is not lower than the above-mentioned lower limit.

[0056] Furthermore, the hydrophobic solvent preferably has a dielectric constant of 2.5 or less at 20°C. The dielectric constant is one of the indicators of the polarity of a compound. When the dielectric constant of the hydrophobic solvent is sufficiently small, such as 2.5 or less, phase separation proceeds rapidly in the droplets of the monomer composition, and hollow spaces are likely to be formed. Examples of hydrophobic solvents having a dielectric constant of 2.5 or less at 20°C are as follows. The values ​​in parentheses are the dielectric constant values: pentane (1.8), hexane (1.9), heptane (1.9), octane (1.9), and cyclohexane (2.0). Regarding the dielectric constant at 20°C, reference can be made to values ​​described in known literature (e.g., "Chemical Handbook: Basics," 4th Revised Edition, edited by the Chemical Society of Japan, Maruzen Co., Ltd., published September 30, 1993, pages II-498 to II-503) and other technical information. The method for measuring the relative dielectric constant at 20°C includes, for example, a relative dielectric constant test carried out in accordance with JIS C 2101:1999, 23, at a measurement temperature of 20°C.

[0057] The porosity of the hollow particles can be adjusted by changing the amount of hydrophobic solvent in the mixed solution. In the suspension process described below, the polymerization reaction proceeds with the hydrophobic solvent encapsulated in oil droplets containing the polymerizable monomer, etc., and therefore the higher the hydrophobic solvent content, the higher the porosity of the resulting hollow particles tends to be. In the present disclosure, the content of the hydrophobic solvent in the mixed solution is preferably 100 to 650 parts by mass per 100 parts by mass of the polymerizable monomer, as this facilitates control of the particle size of the hollow particles, increases the porosity while maintaining the strength of the hollow particles, and reduces the amount of residual hydrophobic solvent within the particles. The content of the hydrophobic solvent in the mixed solution is more preferably 120 to 500 parts by mass, and even more preferably 140 to 300 parts by mass per 100 parts by mass of the polymerizable monomer.

[0058] (C) Polymerization Initiator In the production method of the present disclosure, the mixed liquid preferably contains an oil-soluble polymerization initiator as the polymerization initiator. The oil-soluble polymerization initiator is not particularly limited as long as it is an oil-philic initiator having a solubility in water of 0.2 mass% or less, and examples thereof include organic peroxides such as benzoyl peroxide, lauroyl peroxide, t-butylperoxy-2-ethylhexanoate, t-butylperoxydiethyl acetate, and t-butylperoxypivalate; and azo compounds such as 2,2'-azobis(2,4-dimethylvaleronitrile), azobisisobutyronitrile, and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile).

[0059] The content of the polymerization initiator is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the polymerizable monomer in the mixed solution. When the content of the polymerization initiator is equal to or greater than the above-mentioned lower limit, the polymerization reaction can proceed sufficiently, while when the content is equal to or less than the above-mentioned upper limit, there is little risk of the polymerization initiator remaining after completion of the polymerization reaction, and there is also little risk of an unexpected side reaction proceeding.

[0060] (D) Dispersion Stabilizer The dispersion stabilizer is an agent that disperses droplets of the monomer composition in an aqueous medium during the suspension process. Examples of dispersion stabilizers include inorganic dispersion stabilizers, organic or inorganic water-soluble polymer stabilizers, and surfactants. In the present disclosure, inorganic dispersion stabilizers are preferably used as the dispersion stabilizer because they facilitate control of the particle size of the droplets in the suspension, facilitate removal of the dispersion stabilizer during the washing process, and prevent the shell from becoming too thin, thereby suppressing a decrease in the strength of the hollow particles. Examples of inorganic dispersion stabilizers include sulfates such as barium sulfate and calcium sulfate; carbonates such as barium carbonate, calcium carbonate, and magnesium carbonate; phosphates such as calcium phosphate; metal oxides such as aluminum oxide and titanium oxide; metal hydroxides such as aluminum hydroxide, magnesium hydroxide, calcium hydroxide, barium hydroxide, and ferric hydroxide; and inorganic compounds such as silicon dioxide. These inorganic dispersion stabilizers can be used alone or in combination. Among these inorganic dispersion stabilizers, poorly water-soluble inorganic dispersion stabilizers are preferred. Here, poor water solubility preferably means a solubility of less than 1 g / L in water at 25° C. Among these, poorly water-soluble inorganic dispersion stabilizers are preferably metal hydroxides, and more preferably magnesium hydroxide.

[0061] In the present disclosure, it is particularly preferable to use a poorly water-soluble inorganic dispersion stabilizer dispersed in an aqueous medium in the form of colloidal particles, i.e., in the form of a colloidal dispersion containing poorly water-soluble inorganic dispersion stabilizer colloidal particles. This allows the inorganic dispersion stabilizer to be easily removed by the washing step described below. A colloidal dispersion containing poorly water-soluble inorganic dispersion stabilizer colloidal particles can be prepared, for example, by reacting at least one selected from alkali metal hydroxides and alkaline earth metal hydroxides with a water-soluble polyvalent metal salt (excluding alkaline earth metal hydroxides) in an aqueous medium. Examples of alkali metal hydroxides include lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of alkaline earth metal hydroxides include barium hydroxide and calcium hydroxide. The water-soluble polyvalent metal salt may be any water-soluble polyvalent metal salt other than the above-mentioned alkaline earth metal hydroxides. Examples include magnesium metal salts such as magnesium chloride, magnesium phosphate, and magnesium sulfate; calcium metal salts such as calcium chloride, calcium nitrate, calcium acetate, and calcium sulfate; aluminum metal salts such as aluminum chloride and aluminum sulfate; barium salts such as barium chloride, barium nitrate, and barium acetate; and zinc salts such as zinc chloride, zinc nitrate, and zinc acetate. Among these, magnesium metal salts, calcium metal salts, and aluminum metal salts are preferred, magnesium metal salts are more preferred, and magnesium chloride is particularly preferred. The method for reacting at least one selected from the above-mentioned alkali metal hydroxides and alkaline earth metal hydroxides with the above-mentioned water-soluble polyvalent metal salt in an aqueous medium is not particularly limited. For example, an aqueous solution of at least one selected from the above-mentioned alkali metal hydroxides and alkaline earth metal hydroxides may be mixed with an aqueous solution of the water-soluble polyvalent metal salt. Furthermore, colloidal silica may be used as a colloidal dispersion containing poorly water-soluble inorganic dispersion stabilizer colloidal particles.

[0062] Examples of organic water-soluble polymer stabilizers include polyvinyl alcohol, polycarboxylic acids (such as polyacrylic acid), celluloses (such as hydroxyethyl cellulose, carboxymethyl cellulose, methyl cellulose, and ethyl cellulose), polyvinylpyrrolidone, polyacrylimide, polyethylene oxide, and poly(hydroxystearic acid-g-methyl methacrylate-co-methacrylic acid) copolymers. Examples of inorganic water-soluble polymer stabilizers include sodium tripolyphosphate. Surfactants are compounds that have both hydrophilic and hydrophobic groups in one molecule, and include known ionic surfactants such as anionic surfactants, cationic surfactants, and amphoteric surfactants, as well as nonionic surfactants. Water-soluble polymer stabilizers and surfactants typically have a solubility of 1 g / L or more in water at 25°C.

[0063] The content of the dispersion stabilizer is not particularly limited, but is preferably 0.5 to 15 parts by mass, more preferably 1 to 10 parts by mass, per 100 parts by mass of the combined weight of the polymerizable monomer and the hydrophobic solvent. By ensuring that the content of the dispersion stabilizer is at or above the lower limit, droplets of the monomer composition can be sufficiently dispersed so as not to coalesce in the suspension. On the other hand, by ensuring that the content of the dispersion stabilizer is at or below the upper limit, an increase in the viscosity of the suspension during granulation can be prevented, thereby avoiding problems such as clogging of the suspension in the granulator. Furthermore, the content of the dispersion stabilizer is preferably 0.5 to 15 parts by mass, more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the aqueous medium.

[0064] In the present disclosure, in order to prevent a decrease in the reactivity between the hollow particles and the fluororubber, the smaller the residual amount of dispersion stabilizer, the more preferable, and it is most preferable that the dispersion stabilizer is not contained, and it is particularly preferable that the dispersion stabilizer is not contained. By using only an inorganic dispersion stabilizer as the dispersion stabilizer, hollow particles can be obtained in which both the water-soluble polymer stabilizer and the surfactant are below the detection limit.

[0065] (E) Aqueous Medium In the present disclosure, the term "aqueous medium" refers to a medium selected from the group consisting of water, a hydrophilic solvent, and a mixture of water and a hydrophilic solvent. When using a mixture of water and a hydrophilic solvent, it is important that the polarity of the entire mixture is not too low in order to form droplets of the monomer composition. In this case, for example, the mass ratio of water to hydrophilic solvent (water:hydrophilic solvent) may be 99:1 to 50:50. The hydrophilic solvent in the present disclosure is not particularly limited as long as it is sufficiently miscible with water and does not cause phase separation. Examples of hydrophilic solvents include alcohols such as methanol and ethanol; tetrahydrofuran (THF); dimethyl sulfoxide (DMSO); and the like.

[0066] The content of the aqueous medium is not particularly limited, but from the viewpoint of setting the particle size and porosity of the hollow particles within the preferred ranges described below, the lower limit is preferably 200 parts by mass or more, more preferably 400 parts by mass or more, and even more preferably 600 parts by mass or more, relative to 100 parts by mass of the polymerizable monomer contained in the mixed liquid, and the upper limit is preferably 1,000 parts by mass or less, and more preferably 800 parts by mass or less.

[0067] The mixed liquid may further contain other materials different from the above-described materials (A) to (E) as long as the object of the present disclosure is not impaired.

[0068] A mixed liquid is obtained by mixing the above-mentioned materials and other materials as needed, and stirring appropriately. In this mixed liquid, an oil phase containing lipophilic materials such as (A) the polymerizable monomer, (B) the hydrophobic solvent, and (C) the polymerization initiator is dispersed in an aqueous phase containing (D) the dispersion stabilizer and (E) the aqueous medium, with particles of about several mm in size. The dispersion state of these materials in the mixed liquid can be observed with the naked eye, depending on the type of material. In the mixed liquid preparation step, the mixed liquid may be obtained by simply mixing the above-mentioned materials and other materials as needed, and stirring appropriately. However, in terms of making the shell more uniform, it is preferable to prepare a mixed liquid by separately preparing an oil phase containing the polymerizable monomer, the hydrophobic solvent, and the polymerization initiator, and an aqueous phase containing the dispersion stabilizer and the aqueous medium, and then mixing them. In the present disclosure, a colloidal dispersion in which a poorly water-soluble inorganic dispersion stabilizer is dispersed in the form of colloidal particles in an aqueous medium is preferably used as the aqueous phase. By preparing the oil phase and the water phase separately in advance and then mixing them, hollow particles having a uniform shell composition can be produced, and the particle size of the hollow particles can be easily controlled.

[0069] (2) Suspension Step The suspension step is a step of preparing a suspension in which droplets of a monomer composition containing a hydrophobic solvent are dispersed in an aqueous medium by suspending the mixed liquid described above. The suspension method for forming droplets of the monomer composition is not particularly limited, and any known suspension method can be used. Examples of dispersers that can be used in preparing the suspension include horizontal or vertical in-line dispersers such as Milder manufactured by Pacific Machinery Works, Ltd., Cavitron manufactured by Eurotec Co., Ltd., and in-line dispersers manufactured by IKA (e.g., DISPAX-REACTOR (registered trademark) DRS); and emulsifying dispersers such as the Homomixer MARK II series manufactured by Primix Corporation. In the dispersion for preparing the suspension, the rotation speed of the disperser is preferably 100 rpm or more, more preferably 200 rpm or more, and even more preferably 300 rpm or more, from the viewpoint of forming hollow portions and setting the volume average particle size of the hollow particles within the above-mentioned preferred range, while from the viewpoint of reducing the proportion of irregularly shaped particles, it is preferably 30,000 rpm or less, more preferably 10,000 rpm or less, and even more preferably 5,000 rpm or less.

[0070] In the suspension prepared in the suspending step, droplets of the monomer composition containing the lipophilic material and having a particle size of approximately 0.1 to 100 μm are uniformly dispersed in the aqueous medium. Such droplets of the monomer composition are difficult to observe with the naked eye and can be observed using known observation equipment such as an optical microscope. During the suspending step, phase separation occurs in the droplets of the monomer composition, which makes it easier for the hydrophobic solvent, which has low polarity, to collect inside the droplets. As a result, the resulting droplets contain the hydrophobic solvent in their interiors and materials other than the hydrophobic solvent distributed around their peripheries.

[0071] The droplets of the monomer composition dispersed in an aqueous medium are formed by surrounding the oil-soluble monomer composition with a dispersion stabilizer. The droplets of the monomer composition contain an oil-soluble polymerization initiator, a polymerizable monomer, and a hydrophobic solvent. The droplets of the monomer composition are small oil droplets, and the oil-soluble polymerization initiator generates polymerization-initiating radicals inside the small oil droplets. Therefore, precursor particles of the desired particle size can be produced without excessive growth of the small oil droplets. In suspension polymerization methods using such oil-soluble polymerization initiators, there is no opportunity for the polymerization initiator to come into contact with the polymerizable monomer dispersed in the aqueous medium. Therefore, the use of an oil-soluble polymerization initiator can suppress the by-production of excess resin particles, such as dense solid particles with a relatively small particle size, in addition to the desired hollow particles.

[0072] (3) Polymerization Step This step is a step of subjecting the suspension obtained in the above-mentioned suspension step to a polymerization reaction to prepare a precursor composition in which precursor particles having a hollow portion surrounded by a shell containing a resin and filled with a hydrophobic solvent are dispersed in an aqueous medium. The precursor particles are formed by polymerization of a polymerizable monomer contained in droplets of the monomer composition, and the shell of the precursor particles contains a polymer of the polymerizable monomer as a resin.

[0073] The polymerization method is not particularly limited, and for example, a batch system, a semi-continuous system, or a continuous system can be used. The polymerization temperature is preferably 40 to 90°C, and more preferably 50 to 80°C. The polymerization reaction time is preferably 1 to 48 hours, and more preferably 1 to 36 hours. In the polymerization step, the shell portion of the droplets of the monomer composition containing the hydrophobic solvent therein is polymerized, and therefore, as described above, hollow portions filled with the hydrophobic solvent are formed inside the obtained precursor particles.

[0074] (4) Solid-Liquid Separation Step This step is a step of obtaining a solid content containing precursor particles or hollow particles by solid-liquid separation of a slurry containing precursor particles or hollow particles. The solid-liquid separation step may be performed on a precursor composition containing precursor particles obtained by the above-mentioned polymerization step, or on an aqueous dispersion of hollow particles obtained after the solvent removal step described below. The method of solid-liquid separation is not particularly limited, and known methods can be used. Examples of solid-liquid separation methods include centrifugation, filtration, and static separation. Among these, filtration is preferred because of its simple operation and high efficiency of removing the dispersion stabilizer. When the solvent removal step is performed after the solid-liquid separation step, an optional step such as a pre-drying step may be performed after the solid-liquid separation step and before the solvent removal step. When the solid-liquid separation step is performed after the solvent removal step, an optional step such as a drying step to remove the remaining aqueous medium may be performed after the solid-liquid separation step. The drying method in the above-mentioned preliminary drying step or drying step is not particularly limited, and examples thereof include a method in which the solid content obtained in the solid-liquid separation step is dried using a drying device such as a dryer or a drying appliance such as a hand dryer.

[0075] (5) Solvent Removal Step This step is a step of removing the hydrophobic solvent contained in the precursor particles. For example, after the above-mentioned solid-liquid separation step, the hydrophobic solvent contained in the precursor particles is removed in air, whereby the hydrophobic solvent inside the precursor particles is replaced with air, and hollow particles filled with gas are obtained.

[0076] In this process, "in the air" strictly refers to an environment in which no liquid is present outside the precursor particles, or an environment in which only a trace amount of liquid is present outside the precursor particles, so that the removal of the hydrophobic solvent is not affected. "In the air" can also be referred to as a state in which the precursor particles are not present in a slurry, or a state in which the precursor particles are present in a dry powder. In other words, in a method for removing the hydrophobic solvent from the precursor particles in the air, it is important to remove the hydrophobic solvent in an environment in which the precursor particles are in direct contact with the external gas.

[0077] The method for removing the hydrophobic solvent from the precursor particles in air is not particularly limited, and known methods can be used. Examples of such methods include vacuum drying, heat drying, flash drying, or a combination of these methods. In particular, when using heat drying, the heating temperature must be equal to or higher than the boiling point of the hydrophobic solvent and equal to or lower than the maximum temperature at which the shell structure of the precursor particles does not collapse. Therefore, depending on the shell composition and the type of hydrophobic solvent in the precursor particles, the heating temperature may be, for example, 50 to 200°C, 70 to 200°C, or 100 to 200°C. The drying operation in air replaces the hydrophobic solvent inside the precursor particles with the external gas, resulting in hollow particles whose hollow portions are filled with gas.

[0078] The drying atmosphere is not particularly limited and can be appropriately selected depending on the application of the hollow particles. Examples of the drying atmosphere include air, oxygen, nitrogen, argon, etc. Hollow particles with a temporary vacuum inside can also be obtained by filling the inside of the hollow particles with a gas and then drying under reduced pressure.

[0079] Alternatively, the hydrophobic solvent encapsulated in the precursor particles may be removed from the slurry containing the precursor particles and an aqueous medium without solid-liquid separation of the slurry-like precursor composition obtained in the polymerization step. In this method, the hydrophobic solvent encapsulated in the precursor particles can be removed, for example, by bubbling an inert gas through the precursor composition at a temperature equal to or higher than the boiling point of the hydrophobic solvent minus 35°C. When the hydrophobic solvent is a mixed solvent containing multiple hydrophobic solvents and has multiple boiling points, the boiling point of the hydrophobic solvent in the solvent removal step is the boiling point of the solvent with the highest boiling point among the solvents contained in the mixed solvent, i.e., the highest boiling point among the multiple boiling points. The temperature at which the inert gas is bubbled through the precursor composition is preferably equal to or higher than the boiling point of the hydrophobic solvent minus 30°C, more preferably equal to or higher than the boiling point of the hydrophobic solvent, in order to reduce the amount of hydrophobic solvent remaining in the hollow particles. The bubbling temperature is typically equal to or higher than the polymerization temperature in the polymerization step. Although not particularly limited, the temperature during bubbling may be 50°C or higher and 100°C or lower. The inert gas to be bubbling is not particularly limited, but examples thereof include nitrogen, argon, etc. The bubbling conditions are appropriately adjusted depending on the type and amount of hydrophobic solvent so as to remove the hydrophobic solvent encapsulated in the precursor particles. Although not particularly limited, for example, the inert gas may be bubbled at a rate of 1 to 3 L / min for 1 to 10 hours. This method produces a slurry of hollow particles encapsulating an inert gas. The hollow particles obtained by solid-liquid separation of this slurry are dried, and the aqueous medium remaining in the hollow particles is removed, thereby producing hollow particles whose hollow portions are filled with gas.

[0080] Comparing a method of obtaining hollow particles having hollow spaces filled with gas by performing solid-liquid separation on a slurry-like precursor composition and then removing the hydrophobic solvent in the precursor particles in an atmosphere of air, with a method of obtaining hollow particles having hollow spaces filled with gas by removing the hydrophobic solvent encapsulated in precursor particles in a slurry containing the precursor particles and an aqueous medium, performing solid-liquid separation, and then removing the aqueous medium remaining in the hollow particles in an atmosphere of air, the former method has the advantage that the hollow particles are less likely to be crushed in the step of removing the hydrophobic solvent, while the latter method has the advantage that the amount of remaining hydrophobic solvent is reduced by performing bubbling with an inert gas. Other methods for removing the hydrophobic solvent contained in the precursor particles without subjecting the slurry-like precursor composition obtained in the polymerization step to solid-liquid separation include, for example, a method in which the hydrophobic solvent contained in the precursor particles is evaporated and distilled off from the precursor composition under a predetermined pressure (high pressure, normal pressure, or reduced pressure); or a method in which an inert gas such as nitrogen, argon, or helium, or water vapor is introduced into the precursor composition under a predetermined pressure (high pressure, normal pressure, or reduced pressure), and the hydrophobic solvent is evaporated and distilled off.

[0081] (6) Others As steps other than the above steps (1) to (5), for example, the following steps (6-a) surface treatment step, (6-b) sieving step, (6-c) washing step, and (6-d) particle interior substitution step may be added.

[0082] (6-a) Surface Treatment Step The method for producing hollow particles used in the present disclosure may include a surface treatment step of treating the outer surface of the shell with a coupling agent after the polymerization step described above. The coupling agent has a functional group capable of bonding with an organic substance and a functional group capable of bonding with an inorganic substance in one molecule, and can increase the affinity between the organic material and the inorganic material. Examples of coupling agents include silane coupling agents, titanium coupling agents, and aluminum coupling agents, with silane coupling agents being preferred. Examples of the silane coupling agent include alkoxysilanes having a vinyl group, such as vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltris(β-methoxyethoxy)silane; alkoxysilanes having a methacryloyl group or an acryloyl group, such as γ-acryloxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane; and alkoxysilanes having an epoxy group, such as γ-glycidoxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and γ-glycidoxypropylmethyldiethoxysilane. alkoxysilanes having an amino group such as γ-aminopropyltriethoxysilane, N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and N-β-(aminoethyl)γ-aminopropylmethyldimethoxysilane; alkoxysilanes having a mercapto group such as γ-mercaptopropyltrimethoxysilane; alkoxysilanes having a halogen group such as γ-chloropropyltrimethoxysilane; silanes having a vinyl group and a halogen group such as vinyltrichlorosilane; methyltriacetoxysilane; and the like.Examples of titanium coupling agents include isopropyl triisostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate), Examples of suitable coupling agents include bis(dioctylpyrophosphate)ethylene titanate, isopropyl trioctanoyl titanate, isopropyl dimethacrylisostearoyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctylphosphate) titanate, isopropyl tri(N-amidoethylaminoethyl) titanate, dicumylphenyloxyacetate titanate, and diisostearoyl ethylene titanate. Examples of suitable aluminum coupling agents include acetoalkoxyaluminum diisopropylate. The coupling agent used in the present disclosure is preferably one in which the functional group in its molecular structure is capable of crosslinking with fluororubber. Examples of suitable functional groups capable of crosslinking with fluororubber include vinyl groups and (meth)acryloyl groups. The coupling agent may be used as is or dissolved in a solvent.

[0083] (6-b) Sieving Step (Foreign Matter Removal Step) The method for producing hollow particles used in the present disclosure preferably includes a sieving step after the solvent removal step described above. By performing the sieving step, coarse powder and aggregates can be removed, and foreign matter can be easily removed. Any known sieving method can be used, and is not particularly limited. For example, sieving may be performed using a metal mesh such as a stainless steel mesh or a resin mesh such as a nylon mesh. More specifically, the mesh carrying the hollow particles is vibrated to obtain hollow particles that have passed through the mesh, thereby obtaining sieved hollow particles. The mesh opening used in the sieving step is appropriately selected depending on the size of the hollow particles. It is preferable that the mesh opening be such that the proportion of particles with a circularity of 0.85 or less in the obtained hollow particles is less than 15% by mass.

[0084] (6-c) Washing Step The washing step is a step in which an acid or alkali is added to remove the dispersion stabilizer remaining on the precursor particles or hollow particles. When the dispersion stabilizer used is an acid-soluble inorganic dispersion stabilizer, it is preferable to add an acid to the slurry containing the precursor particles or hollow particles to perform washing. On the other hand, when the dispersion stabilizer used is an alkali-soluble inorganic dispersion stabilizer, it is preferable to add an alkali to the slurry containing the precursor particles or hollow particles to perform washing. Furthermore, when an acid-soluble inorganic dispersion stabilizer is used as the dispersion stabilizer, it is preferable to add an acid to the slurry containing the precursor particles or hollow particles to adjust the pH of the slurry to preferably 6.5 or less, more preferably 6 or less. As the acid to be added, inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as formic acid and acetic acid can be used. However, sulfuric acid is particularly preferred because of its high dispersion stabilizer removal efficiency and its small burden on the production equipment.

[0085] (6-d) Particle Interior Substitution Process The particle interior substitution process is a process in which the gas or liquid inside the hollow particles is replaced with another gas or liquid. This substitution can change the environment inside the hollow particles, selectively confine molecules inside the hollow particles, or modify the chemical structure inside the hollow particles to suit the application.

[0086] [Fluororubber] The fluororubber used in the present disclosure is a fluororubber that can be crosslinked with a peroxide. Examples of the fluororubber that can be crosslinked with a peroxide include fluororubbers containing a halogen atom with an atomic weight of 35 or more in the molecular chain. Among these, fluororubbers containing at least one halogen atom selected from iodine and bromine in the molecular chain are preferred, and fluororubbers containing bromine in the molecular chain are particularly preferred. When a halogen atom with an atomic weight of 35 or more is present in the molecular chain, the halogen atom is easily released from the molecular chain by radicals generated from the organic peroxide during crosslinking, generating highly active radicals from the fluororubber, which can then add to a crosslinking aid such as triallyl isocyanurate (TAIC) to efficiently form crosslinks. In the fluororubber composition of the present disclosure, the hollow particles have reactive unsaturated bonds on their outer surfaces, which function similarly to a crosslinking aid. Therefore, when the fluororubber is crosslinked with an organic peroxide, the fluororubber also forms crosslinks with the reactive unsaturated bonds on the surface of the hollow particles.

[0087] A preferred example of the fluororubber crosslinkable with a peroxide is a fluororubber obtained by introducing a halogen atom having an atomic weight of 35 or more into a copolymer of a fluoropolymerizable monomer. Examples of the fluoropolymerizable monomer include vinylidene fluoride (vinylidene fluoride), hexafluoropropylene (hexafluoropropylene), tetrafluoroethylene (tetrafluoroethylene), pentafluoropropylene, trifluoroethylene, trifluorochloroethylene, vinyl fluoride, perfluoromethyl vinyl ether, perfluoroethyl vinyl ether, perfluoropropyl vinyl ether, perfluoroacrylic acid ester, and perfluoroalkyl acrylate.

[0088] The fluororubber used in the present disclosure may be one in which a non-fluorine polymerizable monomer is copolymerized. Examples of the non-fluorine polymerizable monomer copolymerizable with the fluorine-containing polymerizable monomer include ethylene, propylene, butylene, alkyl carboxylic acid vinyl ester, alkyl vinyl ether, vinyl chloride, vinylidene chloride, acrylic acid, and methacrylic acid. When the fluororubber used in the present disclosure is copolymerized with a non-fluorine polymerizable monomer, the copolymerization ratio of the fluorine-containing polymerizable monomer in the fluororubber used in the present disclosure is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more.

[0089] Examples of fluororubbers used in the present disclosure include fluororubbers in which halogen atoms with an atomic weight of 35 or more have been introduced into fluororubbers such as tetrafluoroethylene propylene rubber (FEPM), vinylidene fluoride rubber (FKM), tetrafluoroethylene-perfluoromethyl vinyl ether rubber (FFKM), and tetrafluoroethylene rubber (TFE). Among these, fluororubbers in which halogen atoms with an atomic weight of 35 or more have been introduced into vinylidene fluoride rubber (FKM) are preferred. As vinylidene fluoride rubber (FKM), particularly preferred are a binary copolymer of vinylidene fluoride and hexafluoropropylene (VdF-HFP copolymer), a terpolymer of vinylidene fluoride, hexafluoropropylene, and tetrafluoroethylene (VdF-HFP-TFE copolymer), and a terpolymer of vinylidene fluoride, hexafluoropropylene, and perfluoroalkyl vinyl ether.

[0090] As described above, the fluororubber used in the present disclosure is preferably a copolymer of fluorine-containing polymerizable monomers into which halogen atoms with an atomic weight of 35 or more have been introduced as crosslinking reaction active sites, more preferably at least one halogen atom selected from iodine and bromine has been introduced, and even more preferably bromine has been introduced. The method for introducing the halogen atoms into the copolymer of fluorine-containing polymerizable monomers is not particularly limited. For example, by carrying out a polymerization reaction in the presence of a terminally halogenated fluoroalkyl or alkylene compound, the halogen atoms can be introduced into the main chain terminal of the copolymer of fluorine-containing polymerizable monomers. Examples of terminally halogenated fluoroalkyl or alkylene compounds include 1-bromoperfluoroethane, 1-bromoperfluoropropane, 1-bromoperfluorobutane, 1-bromoperfluoropentane, 1-bromoperfluorohexane, 1-iodoperfluoroethane, 1-iodoperfluoropropane, 1-iodoperfluorobutane, 1-iodoperfluoropentane, and 1-iodoperfluorohexane. Further examples of the terminally halogenated fluoroalkyl or alkylene compound include 1-bromo-2-iodotetrafluoroethane, 1-bromo-3-iodoperfluoropropane, 1-bromo-4-iodoperfluorobutane, 2-bromo-3-iodoperfluorobutane, monobromomonoiodoperfluoropentane, monobromomonoiodoperfluoro-n-hexane, 1,2-dibromoperfluoroethane, 1,3-dibromoperfluoropropane, 1,4-diiodooctafluorobutane, 1,4-dibromoperfluorobutane, 1,5-dibromoperfluoropentane, 1,6-dibromoperfluorohexane, 1,2-diiodoperfluoroethane, 1,3-diiodoperfluoropropane, 1,4-diiodoperfluorobutane, 1,5-diiodoperfluoropentane, 1,6-dibromoperfluorohexane, etc. These compounds can also be used as chain transfer agents. Alternatively, if the polymerization reaction is carried out in the presence of a halogenated olefin, the halogen atom can be introduced into the main chain, terminal or side chain of the copolymer of the fluorine-containing polymerizable monomer.Examples of halogenated olefins include 1-iodotrifluoroethylene, 1,1-difluoro-2-iodoethylene, 1,1-difluoro-2-bromoethylene, bromotrifluoroethylene, dibromotetrafluoropropylene, dibromodifluoroethylene, tribromotrifluoropropylene, hexabromopropylene, hexaiodopropylene, diiodotetrafluoropropylene, iodotetrafluorobutene, perfluoro(2-bromoethyl vinyl ether), perfluoro(2-iodoethyl vinyl ether), etc. The fluororubber used in the present disclosure preferably has the above-mentioned halogen atoms at the molecular chain terminals in order to improve reactivity.

[0091] In the fluororubber used in the present disclosure, the content of halogen atoms having an atomic weight of 35 or more is not particularly limited, but from the viewpoint of reactivity, it is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, and from the viewpoint of suppressing deterioration of the properties of the fluororubber, it is preferably 5% by mass or less, more preferably 3% by mass or less.

[0092] The fluorine content of the fluororubber used in the present disclosure is not particularly limited, but is preferably 60 to 75% by mass, and more preferably 64 to 70% by mass.

[0093] In the present disclosure, commercially available products may be used as the peroxide-crosslinkable fluororubber. Examples of commercially available peroxide-crosslinkable fluororubber products include the GAL series, GBL series, GF series, GLT series, GFLT series, and ETP series of Viton (registered trademark) from Chemours Inc.; and the G-800 series, G-900 series, and LT series of Dai-El (registered trademark) from Daikin Industries, Ltd. These commercially available products contain halogen atoms with an atomic weight of 35 or more as crosslinking reaction active sites in the molecular chain of the fluororubber.

[0094] The Mooney viscosity of the fluororubber used in the present disclosure is not particularly limited, but from the viewpoint of ease of kneading, the Mooney viscosity (ML(1+10)) at 121°C is preferably 10 to 150, more preferably 15 to 100, and even more preferably 20 to 70.

[0095] In the fluororubber composition of the present disclosure, the content of the fluororubber is not particularly limited, but the lower limit is preferably 70% by mass or more, more preferably 80% by mass or more, and the upper limit is preferably 99% by mass or less, more preferably 96% by mass or less, and even more preferably 90% by mass or less, relative to 100% by mass of the fluororubber composition. When the content of the fluororubber is equal to or greater than the above lower limit, the fluororubber composition can be easily kneaded, and the original properties of the fluororubber can be sufficiently maintained in the fluororubber composition. When the content of the fluororubber is equal to or less than the above upper limit, hollow particles can be sufficiently contained, thereby achieving excellent weight reduction effects and compression set reduction effects due to the hollow particles. In the present disclosure, the fluororubber may be used alone or in combination of two or more types.

[0096] [Organic Peroxide] In the present disclosure, an organic peroxide is used as a cross-linking agent for the fluororubber. The fluororubber composition of the present disclosure may or may not contain an organic peroxide. When the fluororubber composition of the present disclosure does not contain an organic peroxide, an organic peroxide may be added to the fluororubber composition of the present disclosure during cross-linking molding. The organic peroxide may be any organic peroxide commonly used in the rubber industry as a peroxide for crosslinking fluororubber. Examples of the organic peroxide include, but are not limited to, dialkyl peroxides such as 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, 1,3-bis(t-butylperoxyisopropyl)benzene, and 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane; diacyl peroxides such as benzoyl peroxide and isobutyryl peroxide; peroxy esters such as 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane and t-butylperoxyisopropyl carbonate; and 1-isopropyl-2-(t-butylperoxy)benzene. Among these, dialkyl peroxides are preferred. These organic peroxides may be used alone or in combination of two or more.

[0097] The content of the organic peroxide is not particularly limited, but the lower limit is preferably 0.1 part by mass or more, more preferably 0.2 part by mass or more, and even more preferably 0.5 part by mass or more, relative to 100 parts by mass of the fluororubber, and the upper limit is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less. When the content of the organic peroxide is equal to or more than the lower limit, sufficient crosslinking can be achieved, and when it is equal to or less than the upper limit, deterioration of the physical properties such as rubber elasticity of the crosslinked product is suppressed.

[0098] [Crosslinking Aid] In the present disclosure, a crosslinking aid is typically used to crosslink the fluororubber. Like the organic peroxide described above, the crosslinking aid may or may not be included in the fluororubber composition of the present disclosure. When the fluororubber composition of the present disclosure does not contain a crosslinking aid, a crosslinking aid may be added to the fluororubber composition of the present disclosure during crosslinking molding. Examples of the crosslinking aid include polyfunctional unsaturated compounds such as triallyl isocyanurate, trimethallyl isocyanurate, triallyl cyanurate, triallyl trimellitate, N,N-m-phenylene bismaleimide, diallyl phthalate, tris(diallylamine)-s-triazine, triallyl phosphite, 1,2-polybutadiene, ethylene glycol diacrylate, and diethylene glycol diacrylate. Among these, triallyl isocyanurate and trimethallyl isocyanurate are particularly preferred. These crosslinking aids may be used alone or in combination of two or more.

[0099] The content of the cross-linking aid is not particularly limited, but the lower limit is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the fluororubber. This allows for sufficient cross-linking. The upper limit of the content of the cross-linking aid is not particularly limited, but from the viewpoint of cost and from the viewpoint of suppressing deterioration of physical properties such as rubber elasticity of the cross-linked product, it is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less.

[0100] [Other Components] The fluororubber composition of the present disclosure may contain additives such as plasticizers (softeners), reinforcing agents, fillers, processing aids, lubricants, antioxidants, UV absorbers, foaming agents, foaming aids, pigments, colorants, dispersants, and flame retardants, as necessary, within the scope of the present disclosure. Furthermore, the reinforcing agents and fillers contained in the fluororubber composition of the present disclosure may be surface-treated with the above-mentioned coupling agents that can be used for the hollow particles used in the present disclosure. Surface-treating at least one selected from the reinforcing agents and fillers contained in the fluororubber composition of the present disclosure with the above-mentioned coupling agents is preferred in terms of improving the mechanical properties of the crosslinked molded article, such as tensile strength, tensile stress, tear strength, and abrasion resistance. It is more preferred that the hollow particles used in the present disclosure and at least one selected from the reinforcing agents and fillers are surface-treated with the above-mentioned coupling agents.

[0101] As the plasticizer (softener), those generally used as plasticizers or softeners in rubber products, or those that impart flexibility, can be used. For example, petroleum-based softeners such as process oil, lubricating oil, paraffin, liquid paraffin, petroleum asphalt, and Vaseline; coal tar-based softeners such as coal tar and coal tar pitch; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, and coconut oil; tall oil; waxes such as beeswax, carnauba wax, and lanolin; fatty acids and fatty acid salts such as ricinoleic acid, palmitic acid, barium stearate, calcium stearate, and zinc laurate; synthetic polymers such as petroleum resin, atactic polypropylene, and coumarone-indene resin; ester-based plasticizers such as dioctyl phthalate, dioctyl adipate, and dioctyl sebacate; carbonate-based plasticizers such as diisododecyl carbonate; and other plasticizers such as microcrystalline wax, sub(factice), liquid polybutadiene, modified liquid polybutadiene, liquid thiokol, and hydrocarbon-based synthetic lubricating oils. These plasticizers can be used alone or in combination of two or more. The content of the plasticizer (softener) in the fluororubber composition is not particularly limited, and is usually 10 to 200 parts by mass, preferably 35 to 100 parts by mass, and more preferably 45 to 90 parts by mass, per 100 parts by mass of the fluororubber.

[0102] Reinforcing agents have the effect of enhancing the mechanical properties of crosslinked molded articles, such as tensile strength, tensile stress, tear strength, and abrasion resistance. It is believed that in crosslinked molded articles containing reinforcing agents, these mechanical properties are enhanced by the formation of bound rubber at the interface of the reinforcing agent. Specific examples of such reinforcing agents include carbon black such as SRF, GPF, FEF, FF, HAF, HAF-LS, HAF-HS, ISAF, ISAF-LS, ISAF-HS, SAF, FT, and MT, and silica. Examples of silica include natural silica such as quartz powder and silica stone powder; and synthetic silica such as silicic anhydride (silica gel, Aerosil, etc.), hydrous silicic acid, hydrous silicate salts, and finely powdered silicic acid. These reinforcing agents can be used alone or in combination of two or more. The amount of reinforcing agent is not particularly limited, and is typically less than 230 parts by mass per 100 parts by mass of fluororubber. The content of the reinforcing agent per 100 parts by mass of the fluororubber is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, from the viewpoint of improving the mechanical properties of the crosslinked molded product, while it is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less, from the viewpoint of facilitating kneading of the fluororubber composition.

[0103] Carbon black has a nitrogen adsorption specific surface area of ​​5 m 2 / g or more 150m 2 Carbon black having a nitrogen adsorption specific surface area of ​​5 m / g or less is preferably used, and among them, carbon black having a nitrogen adsorption specific surface area of ​​5 m / g or less is preferably used because of its excellent compatibility with fluororubber. 2 / g or more 25m 2 From the viewpoint of compatibility with fluororubber, the nitrogen adsorption specific surface area of ​​the carbon black is more preferably 5 m / g or less. 2 / g or more 20m 2 / g or less, and even more preferably 5m 2 / g or more 15m 2 / g or less, particularly preferably 5m 2 / g or more 10m 2 The specific examples of carbon black mentioned above all have a nitrogen adsorption specific surface area of ​​5 m 2 / g or more 150m2 Among them, FT carbon (nitrogen adsorption specific surface area: 13 m 2 / g) and MT carbon (nitrogen adsorption specific surface area: 7 m 2 / g) is a nitrogen adsorption specific surface area of ​​5 m 2 / g or more 25m 2 The nitrogen adsorption specific surface area of ​​carbon black is measured in accordance with JIS K6217-2.

[0104] As the reinforcing agent, at least one selected from carbon black and silica can be preferably used because of its excellent effect of enhancing the mechanical properties of the crosslinked molded article. Carbon black is particularly effective in enhancing the mechanical properties of the crosslinked molded article and is also preferred because it also has the effect of reducing the compression set of the crosslinked molded article. On the other hand, the crosslinked molded article will turn black when it contains carbon black. Therefore, carbon black is preferably used as a reinforcing agent in applications where blackening is acceptable, while silica is preferably used as a reinforcing agent in applications where blackening is not acceptable. In this way, the type of reinforcing agent can be appropriately selected depending on the application of the crosslinked molded article. Furthermore, as described above, the reinforcing agent may be surface-treated with the above-mentioned coupling agent that can be used for hollow particles. In applications where blackening is not acceptable, silica treated with a coupling agent is particularly preferably used as a reinforcing agent.

[0105] Examples of fillers include inorganic fillers such as calcium carbonate, light calcium carbonate, heavy calcium carbonate, magnesium carbonate, talc, clay, glass beads, and glass balloons; and organic fillers such as high styrene resin, coumarone-indene resin, phenolic resin, lignin, modified melamine resin, and petroleum resin, with inorganic fillers being particularly preferred. These fillers can be used alone or in combination of two or more. The amount of filler to be added is not particularly limited, and is typically 30 to 200 parts by mass per 100 parts by mass of the fluororubber.

[0106] Examples of processing aids include higher fatty acids such as ricinoleic acid, stearic acid, palmitic acid, and lauric acid; salts of higher fatty acids such as barium stearate, zinc stearate, and calcium stearate; and esters of higher fatty acids such as ricinoleic acid, stearic acid, palmitic acid, and lauric acid. Examples of antioxidants include amine-based, hindered phenol-based, and sulfur-based antioxidants.

[0107] Examples of lubricants include hydrocarbon compounds or mixtures such as liquid paraffin, fatty acid compounds such as stearic acid, fatty acid amide compounds such as stearic acid amide, ester compounds such as butyl stearate, and alcohol compounds such as stearyl alcohol, as well as metal soaps. Examples of pigments include inorganic pigments such as titanium dioxide, zinc oxide, ultramarine, red iron oxide, lithopone, lead, cadmium, iron, cobalt, aluminum, hydrochloride salts, and nitrates, and organic pigments such as azo pigments, phthalocyanine pigments, quinacridone pigments, quinacridonequinone pigments, dioxazine pigments, anthrapyrimidine pigments, anthanthrone pigments, indanthrone pigments, flavanthrone pigments, perylene pigments, perinone pigments, diketopyrrolopyrrole pigments, quinonaphthalone pigments, anthraquinone pigments, thioindigo pigments, benzimidazolone pigments, isoindoline pigments, and carbon black.

[0108] [Uses of Fluororubber Composition] The fluororubber composition of the present disclosure is used as a molding material for producing a crosslinked molded article. A crosslinked molded article obtained by melt molding or the like using the fluororubber composition of the present disclosure as a molding material may be, for example, a fluororubber component, an elastomer component integrally molded with a component made of another material, a coating, or a filler chip material. The crosslinked molded article obtained by crosslinking the fluororubber composition of the present disclosure is a rubber product having excellent heat resistance, chemical resistance, and oil resistance due to the fluororubber being the main component, and further, due to the inclusion of hollow particles, is lightweight and has reduced compression set. Examples of uses of the crosslinked molded article produced using the fluororubber composition of the present disclosure include various rubber components used in various fields such as automobiles, electricity, electronics, construction, aviation, and space. More specifically, examples of the crosslinked molded articles include automotive parts such as hoses, packings, tubes, O-rings, gaskets, sealing materials, vibration-proof rubber, and weatherstrips; construction materials such as waterproof sheets and sealing materials; electrical rubber parts such as high-voltage cables and connectors; industrial products such as heat-resistant conveyor belts, chemical-resistant rolls, and heat-resistant hoses; and sealing materials for semiconductor manufacturing equipment, chemical plants, and residential use. Sealing materials are particularly required to have low compression set because their sealing properties deteriorate upon plastic deformation. The crosslinked molded articles containing the hollow particles used in the present disclosure have reduced compression set, making them particularly suitable for use in applications requiring low compression set, such as sealing materials. Furthermore, applications of the crosslinked molded articles of the present disclosure include overcoat or undercoat materials that require thermal insulation and shock-absorbing properties (cushioning), cushioning materials for footwear such as sports shoes and sandals, home appliance parts, stationery, and tools.

[0109] [Method for Producing Fluororubber Composition] The method for producing the fluororubber composition of the present disclosure can be a conventional method and is not particularly limited. For example, a method can be used in which, while kneading the fluororubber, hollow particles, organic peroxide, crosslinking aid, and other components added as needed are added to the fluororubber, and then the mixture is further kneaded. Alternatively, a method can be used in which a raw material mixture containing the fluororubber, hollow particles, organic peroxide, crosslinking aid, and other components added as needed is prepared, and then the raw material mixture is kneaded. The fluororubber or raw material mixture is kneaded at a temperature at which the fluororubber softens. Furthermore, kneading machines used for the kneading include, for example, known kneaders such as single-screw kneaders, twin-screw kneaders, kneaders, Banbury mixers, pressure kneaders, and roll kneaders. Among these, kneading that applies high shear force, such as roll kneading, is preferred. A kneader used for roll kneading can be, for example, a twin-roll mixer, and more specifically, a DY6-15 mixing roll (manufactured by Daihan Co., Ltd.) can be used. Furthermore, in the production of the fluororubber composition of the present disclosure, the compounding components may be homogenized by pre-kneading at a temperature at which the fluororubber softens, and then finish-kneading may be performed by applying a high shear force such as roll kneading. This makes it possible to obtain a fluororubber composition in which the compounding components are further homogenized and finely divided. Furthermore, when the fluororubber composition is crosslinked and molded, the fluororubber composition before crosslinking recovered from the molding device can be reused as a raw material mixture.

[0110] The conditions for kneading the fluororubber or raw material mixture are not particularly limited. However, when an organic peroxide is contained, the kneading temperature is preferably less than the 10-hour half-life temperature of the organic peroxide. The kneading temperature here refers to the set temperature of the kneading device. The kneading time is preferably within one hour. By using such kneading conditions, the crosslinking reaction of the fluororubber during kneading can be prevented, scorching can be prevented, and the compounding components can be uniformly mixed. As an example, kneading can be performed using the following method: Using a roll kneader, the kneading temperature is set to 70 to 90°C. After the kneader temperature has stabilized, the fluororubber is added. Next, while the kneader rotor is rotating at a speed of 10 to 35 rpm, components such as hollow particles and organic peroxide are added in any order. After all materials have been added, the mixture is kneaded for 10 to 30 minutes. This produces the fluororubber composition of the present disclosure.

[0111] 2. Crosslinked Molded Article The crosslinked molded article of the present disclosure is a molded article obtained by crosslinking the above-described fluororubber composition of the present disclosure with an organic peroxide. By crosslinking the fluororubber composition of the present disclosure with an organic peroxide, the crosslinking reaction of the fluororubber proceeds, and the crosslinking reaction between the reactive unsaturated bonds of the hollow particles and the fluororubber proceeds, thereby obtaining the crosslinked molded article of the present disclosure. The method for crosslinking the fluororubber composition can be appropriately selected from known methods depending on the shape of the desired molded article, and is not particularly limited. Examples include melt molding methods such as extrusion molding, compression molding, extrusion lamination, injection molding, press molding, and blow molding. The temperature when crosslinking the fluororubber composition is not particularly limited, but is preferably equal to or higher than the 10-hour half-life temperature of the organic peroxide from the viewpoint of sufficiently proceeding the crosslinking reaction of the fluororubber and the crosslinking reaction between the hollow particles and the fluororubber. The upper limit of the temperature when crosslinking the fluororubber composition of the present disclosure is not particularly limited, but is preferably equal to or lower than the 1-minute half-life temperature of the organic peroxide. Alternatively, primary vulcanization may be performed by heating and pressurizing at a temperature of 100 to 250°C, followed by post-curing at a temperature higher than the primary vulcanization temperature but not higher than 300°C to perform secondary vulcanization. The primary vulcanization time may be, for example, 1 to 180 minutes, and the secondary vulcanization time may be, for example, 1 to 30 hours. The pressure during heating and pressurizing to crosslink and mold the fluororubber composition is not particularly limited, but may be, for example, 1 MPa to 20 MPa.

[0112] The form of the crosslinked molded article of the present disclosure is not particularly limited, and for example, the fluororubber composition in a molten state may be molded into a long sheet, a block, a filler, or the like, or the long sheet may be wound up into a roll, or the long sheet may be cut to a predetermined length and subjected to secondary processing into a strip, or the like.

[0113] The crosslinked molded article of the present disclosure preferably has a compression set of less than 60%, more preferably less than 40%, and even more preferably less than 25%, as measured in accordance with the room temperature test of JIS K 6262:2013. The lower limit of the compression set of the crosslinked molded article of the present disclosure is not particularly limited, but is usually 10% or more. The fluororubber composition of the present disclosure used as a molding material for the crosslinked molded article of the present disclosure usually has a compression set of 60% or more before crosslinking molding.

[0114] The crosslinked molded article of the present disclosure preferably has a tensile stress at 100% elongation of 2 MPa or more, more preferably 4 MPa or more, and even more preferably 6 MPa or more, as measured in accordance with JIS K 6251: 2017. The upper limit of the tensile stress at 100% elongation of the crosslinked molded article of the present disclosure is not particularly limited, but is usually 30 MPa or less.

[0115] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to these examples. Note that parts and percentages are by mass unless otherwise specified.

[0116] <Production of Hollow Particles> [Production Example 1 (Hollow Particles A)] (1) Mixture Preparation Step First, the following materials were mixed to form an oil phase: Crosslinkable acrylic monomer: ethylene glycol dimethacrylate 25 parts Crosslinkable acrylic monomer: trimethylolpropane trimethacrylate 30 parts Crosslinkable hydrocarbon monomer: divinylbenzene 45 parts Oil-soluble polymerization initiator: 2,2'-azobis(2,4-dimethylvaleronitrile) 3 parts Hydrophobic solvent: hexane 160 parts Separately, in a stirring tank at room temperature, an aqueous solution of 12.1 parts of sodium hydroxide (alkali metal hydroxide) in 121 parts of ion-exchanged water was gradually added with stirring to an aqueous solution of 17.1 parts of magnesium chloride (a water-soluble polyvalent metal salt) in 494 parts of ion-exchanged water to prepare a magnesium hydroxide colloid (poorly water-soluble metal hydroxide colloid) dispersion (4 parts magnesium hydroxide), which served as an aqueous phase. The resulting aqueous phase and oil phase were mixed to prepare a mixed liquid.

[0117] (2) Suspension step The mixture obtained in the mixture preparation step was stirred and suspended for 1 minute using a disperser (manufactured by Primix Corporation, product name: Homomixer) at a rotation speed of 4,000 rpm, to prepare a suspension in which droplets of the monomer composition encapsulating the hydrophobic solvent were dispersed in water.

[0118] (3) Polymerization step: The suspension obtained in the suspension step was stirred for 1 hour and 30 minutes under a nitrogen atmosphere at a temperature of 65°C to carry out a polymerization reaction, thereby obtaining a precursor composition containing precursor particles encapsulating a hydrophobic solvent.

[0119] (4) Washing step and solid-liquid separation step The precursor composition was washed with dilute sulfuric acid (25°C, 10 minutes) to adjust the pH to 5.5 or less. Next, after separating the water by filtration, 200 parts of ion-exchanged water was added to re-slurry the mixture. The water washing treatment (washing, filtration, dehydration) was repeated several times at room temperature (25°C), and the mixture was filtered to obtain a solid fraction. The obtained solid fraction was dried in a dryer at a temperature of 40°C to obtain precursor particles encapsulating the hydrophobic solvent.

[0120] (5) Solvent Removal Step The precursor particles obtained in the solid-liquid separation step were heat-treated in a vacuum dryer at 200°C in a nitrogen atmosphere for 12 hours to remove the hydrophobic solvent contained in the particles, thereby obtaining hollow particles.

[0121] (6) Sieving Step The hollow particles obtained in the solvent removal step were sieved using a nylon mesh with an opening of 100 μm, and the hollow particles that passed through the mesh and fell to the bottom were collected to remove coarse particles, thereby obtaining hollow particles A.

[0122] [Production Example 2 (Hollow Particles B)] Hollow particles of Production Example 2 (hollow particles B) were obtained in the same manner as in Production Example 1, except that the amount of polymerizable monomer added to the oil phase in the above "(1) Mixture preparation step" was changed according to Table 1.

[0123] [Production Example 3 (Hollow Particles C)] Hollow particles of Production Example 3 (hollow particles C) were obtained in the same procedure as in Production Example 1, except that the rotation speed of the disperser in the above "(2) suspension step" was changed to 400 rpm.

[0124] [Production Example 4 (Hollow Particles D)] Hollow particles of Production Example 4 (hollow particles D) were obtained in the same procedure as in Production Example 1, except that the amount of polymerizable monomer added to the oil phase in the above "(1) Mixture preparation step" was changed according to Table 1.

[0125] [Production Example 5 (Hollow Particles E)] Hollow particles of Production Example 5 (hollow particles E) were obtained in the same manner as in Production Example 1, except that in the above-mentioned "(1) mixed solution preparation step", the polymerizable monomer added to the oil phase was changed to 100 parts of divinylbenzene alone.

[0126] [Comparative Production Example 1 (Dense Solid Particles A)] Dense solid particles (dense solid particles A) of Comparative Production Example 1 were obtained in the same procedure as Production Example 1, except that in the above "(2) Suspension Step", the rotation speed of the disperser was changed to 10 rpm.

[0127] [Evaluation of Particle Properties] The following physical property evaluations were carried out for the hollow particles obtained in Production Examples 1 to 5 and the solid particles obtained in Comparative Production Example 1. The results of the particle property evaluations are shown in Table 1.

[0128] 1. Iodine Value Measurement The iodine value of the particles was measured in accordance with JIS K 0070. The specific measurement method is as follows: 0.7 to 2 g of particles (sample) and 10 mL of chloroform were added to a 300 mL iodine flask, and 25 mL of Wiess's solution was added as a reaction solution. The flask was gently stirred and sealed, and then allowed to stand in the dark at 25°C for 30 minutes. Next, 20 mL of 100 g / L potassium iodide solution and 100 mL of purified water were added and stirred. Using a burette, titration was performed with a titrant (0.1 mol / L sodium thiosulfate solution). When the solution turned pale yellow, an indicator (1% starch solution) was added. The titration was continued, and the point at which the blue color disappeared was the endpoint. Separately from this main test, a blank test was performed using a solution without added particles, and the iodine value of the particles was calculated using the following formula. The iodine value is the amount of halogen bonded to 100 g of a sample when the halogen is reacted with the sample, converted into grams of iodine. Iodine value (g / 100 g) = {(V 0 -V 1 ) × f × 1.269} / S, S: sample mass (g), V 1 V: Volume of titrant in this test (mL)0 : Volume of titrant in blank test (mL) f: Factor of titrant

[0129] 2. Percentage of particles with one hollow part Particles fixed on carbon tape were intentionally broken by rubbing them with a cotton swab. The interiors of 100 broken particles were observed using an SEM to identify the number of hollow parts per particle, and the percentage of particles with only one hollow part was calculated.

[0130] 3. Percentage of Irregularly Shaped Particles Measurement samples were prepared by dispersing 0.10 to 0.12 g of particles in an aqueous solution of linear alkylbenzenesulfonate (0.3% concentration) in an ultrasonic cleaner for 5 minutes. Using a flow-type particle image analyzer (manufactured by Jasco International Co., Ltd., product name: IF-3200), the circularity of each particle contained in the measurement sample was measured under the following measurement conditions. The mass ratio of particles with a circularity of 0.85 or less was calculated and used as the percentage of irregularly shaped particles. The number of particles contained in the measurement sample increased with decreasing particle size, but was within the range of 1,000 to 3,000 particles in all manufacturing examples. (Measurement Conditions) Flow cell spacer thickness: 50 μm Telecentric zoom lens magnification: 4.5x Total magnification: 9.0x Measurement volume: 0.5 mL Image resolution: 0.185 μm / pixel Detection algorithm: Ghost detection Threshold: 15%

[0131] 4. Residual Volatile Component Content The residual volatile component content of the particles was determined by the purge and trap / gas chromatography (P&T / GC) method shown below. 0.1 g of particles was placed in a purge vessel, and while helium gas was flowing as a carrier gas at 50 ml / min, the purge vessel was heated from room temperature at a rate of 10°C / min and held at a temperature of 200°C for 30 minutes, and the generated volatile components were collected in a trap tube at -130°C. The collected residual volatile components were quantified to determine the residual volatile component content of the particles. The measurement equipment was an Agilent Gas Chromatograph 6890 (FID method), the analytical measuring instrument was a Shimadzu Corporation C-R7A Chromatopack, the purge & trap sampler was an Agilent TDS, and the column was a J&W DB-5 (L = 30 m, ID = 0.32 mm, Film = 0.25 μm), and the measurement was performed under the following conditions: Column temperature: 50°C (hold for 2 minutes) to 270°C (heating increased at 10°C / min) Sample inlet temperature: 280°C Detection temperature: 280°C Carrier gas: helium gas, flow rate: 1 ml / min

[0132] 5. Particle size and particle size distribution Particle size was measured using a particle size distribution analyzer (product name: Multisizer 4e, manufactured by Beckman Coulter, Inc.) using the Coulter counter method, and the number average and volume average were calculated to determine the number average particle size (Dp) and volume average particle size (Dv). The particle size distribution (Dv / Dp) was calculated by dividing the volume average particle size by the number average particle size. The measurement conditions were aperture diameter: 50 μm, dispersion medium: Isoton II (product name), concentration: 10%, and number of particles measured: 100,000. Specifically, 0.2 g of particle sample was placed in a beaker, and a surfactant aqueous solution (product name: Drywell, manufactured by Fujifilm Corporation) was added as a dispersant. 2 ml of dispersion medium was added to the beaker to wet the particles, and then 10 ml of dispersion medium was added. The mixture was dispersed in an ultrasonic disperser for 1 minute, and then measured using the particle size distribution analyzer.

[0133] 6. Porosity 6-1. Measurement of apparent density of hollow particles First, a volume of 100 cm 3 About 30 cm 3The volumetric flask was filled with hollow particles, and the mass of the filled hollow particles was accurately weighed. Next, the volumetric flask filled with the hollow particles was accurately filled with isopropanol up to the marked line, taking care not to introduce air bubbles. The mass of the isopropanol added to the volumetric flask was accurately weighed, and the apparent density D of the hollow particles was calculated based on the following formula (I): 1 (g / cm 3 The apparent density D was calculated using the formula (I). 1 = [Mass of hollow particles] / (100 - [Mass of isopropanol] / [Specific gravity of isopropanol at measurement temperature])

[0134] 6-2. Measurement of true density of hollow particles After crushing the hollow particles in advance, 3 Approximately 10 g of crushed pieces of hollow particles was filled into a measuring flask, and the mass of the crushed pieces was accurately weighed. Then, in the same manner as in the measurement of the apparent density, isopropanol was added to the measuring flask, and the mass of the isopropanol was accurately weighed. The true density D of the hollow particles was calculated based on the following formula (II): 0 (g / cm 3 ) was calculated. 0 = [Mass of crushed hollow particle fragments] / (100 - [Mass of isopropanol] / [Specific gravity of isopropanol at measurement temperature])

[0135] 6-3. Calculation of porosity Apparent density D of hollow particles 1 and true density D 0 The porosity of the hollow particles was calculated based on the following formula (III): Formula (III) Porosity (%) = 100 - (apparent density D 1 / True density D 0 ) x 100

[0136]

[0137] <Production of Fluororubber Composition and Crosslinked Molded Article> [Example 1] As a peroxide-crosslinkable fluororubber, 100 parts of a fluororubber in which bromine has been introduced into the molecular chain by further copolymerizing a brominated olefin with a terpolymer of vinylidene fluoride, hexafluoropropylene, and tetrafluoroethylene (product name: Viton (registered trademark) GBL-200S, manufactured by Chemours Inc., fluorine content: 67 mass%, Mooney viscosity at 121°C (ML(1+10)): 25, specific gravity: 1.84) was charged into a twin mixing roll kneader (model name: DY6-15, roll diameter: 6 inches, roll clearance: 0.5 mm, manufactured by Daihan Co., Ltd.) kept at a temperature of 80°C. The rotation speed of the kneader rotor was set to 10 to 35 rpm, and the fluororubber was wound around the roll. Then, 17.5 parts of the hollow particles A obtained in Production Example 1 were added to the kneader, followed by 2 parts of Perhexa (registered trademark) 25B-40 (manufactured by NOF Corporation, compound name: 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 10-hour half-life temperature: 117.9°C, 1-minute half-life temperature: 179.8°C) as a crosslinking agent and 4 parts of triallyl isocyanurate (TAIC) as a crosslinking aid, to obtain a mixture. The obtained mixture was kneaded for 15 minutes, to obtain the fluororubber composition of Example 1.

[0138] The obtained fluororubber composition was press-molded at 10 MPa for 10 minutes using a hot press at 160°C to form a cylindrical shape with a diameter of 29±0.5 mm and a height of 12.5±0.5 mm, followed by secondary vulcanization (180°C, 4 hours) to obtain a cylindrical crosslinked molded article of Example 1. The cylindrical crosslinked molded article thus obtained was used as a test piece for compression set measurement (JIS K 6262) described below. The obtained fluororubber composition was also press-molded at 10 MPa for 10 minutes using a hot press at 160°C to form a dumbbell-shaped No. 3 according to JIS K 6251, followed by secondary vulcanization (180°C, 4 hours) to obtain a dumbbell-shaped crosslinked molded article of Example 1. The dumbbell-shaped crosslinked molded article thus obtained was used as a test piece for tensile stress at 100% elongation (JIS K 6251) described below.

[0139] [Examples 2 to 3] Fluororubber compositions and crosslinked molded articles of Examples 2 to 3 were obtained in the same manner as in Example 1, except that the amount of hollow particles A obtained in Production Example 1 was changed according to Table 2.

[0140] [Examples 4 to 7] Fluororubber compositions and crosslinked molded articles of Examples 4 to 7 were obtained in the same manner as in Example 1, except that hollow particles B obtained in Production Example 2, hollow particles C obtained in Production Example 3, hollow particles D obtained in Production Example 4, or hollow particles E obtained in Production Example 5 were used in accordance with Table 2 instead of hollow particles A obtained in Production Example 1 in Example 1.

[0141] [Comparative Example 1] A fluororubber composition and a crosslinked molded article of Comparative Example 1 were obtained in the same manner as in Example 1, except that the dense solid particles A obtained in Comparative Production Example 1 were used instead of the hollow particles A obtained in Production Example 1, and the amount of dense solid particles A added was set as shown in Table 2.

[0142] Comparative Example 2 A fluororubber composition and a crosslinked molded article of Comparative Example 2 were obtained in the same manner as in Example 1, except that in Example 1, Viton (registered trademark) A-200 (manufactured by Chemours Inc., specific gravity: 1.82) was used as the fluororubber instead of Viton (registered trademark) GBL-200S, VC No. 30 (manufactured by Chemours Inc., compound name: bisphenol AF) was used as the crosslinking agent instead of Perhexa (registered trademark) 25B-40, and TAIC was not used as the crosslinking aid.

[0143] Comparative Example 3 A fluororubber composition and a crosslinked molded article of Comparative Example 3 were obtained in the same manner as in Example 1, except that in Example 1, Viton (registered trademark) B-202 (manufactured by Chemours Inc., specific gravity: 1.84) was used as the fluororubber instead of Viton (registered trademark) GBL-200S, Diak No. 1 (manufactured by DuPont, compound name: hexamethylenediamine carbamate) was used as the crosslinking agent instead of Perhexa (registered trademark) 25B-40, and TAIC was not used as the crosslinking aid.

[0144] Reference Example 1 A fluororubber composition and a crosslinked molded article of Reference Example 1 were obtained in the same manner as in Example 1, except that the hollow particles A obtained in Production Example 1 were not added.

[0145] [Examples 8 to 9] In Example 1, the amount of hollow particles A added was changed according to Table 3, and MT carbon (nitrogen adsorption specific surface area: 7 m) was also used as a reinforcing agent when hollow particles A were added. 2 Fluororubber compositions and crosslinked molded articles of Examples 8 and 9 were obtained in the same manner as in Example 1, except that fluororubber compositions (1 / g) were added in the amounts shown in Table 3.

[0146] [Example 10] A fluororubber composition and a crosslinked molded article of Example 10 were obtained in the same manner as in Example 1, except that hollow particles B obtained in Production Example 2 were added in the amount shown in Table 3 instead of hollow particles A obtained in Production Example 1 in Example 1, and MT carbon was also added as a reinforcing agent in the amount shown in Table 3 when hollow particles B were added.

[0147] Examples 11 and 12 In Example 1, fluororubber compositions and crosslinked molded articles of Examples 11 and 12 were obtained in the same manner as in Example 1, except that Viton (registered trademark) GBL-600S (manufactured by Chemours Inc., fluorine content: 67% by mass, Mooney viscosity at 121°C (ML(1+10)): 65, specific gravity: 1.84, VdF-HFP-TFE terpolymer system) was used instead of Viton (registered trademark) GBL-200S, the amount of hollow particles A added was changed according to Table 3, and MT carbon was also added as a reinforcing agent in the amount shown in Table 3 when hollow particles A was added.

[0148] Examples 13 to 14 In Example 1, fluororubber compositions and crosslinked molded articles of Examples 13 to 14 were obtained in the same manner as in Example 1, except that Viton (registered trademark) GF-200S (manufactured by Chemours Inc., fluorine content: 70% by mass, Mooney viscosity at 121°C (ML(1+10)): 25, specific gravity: 1.90, VdF-HFP-TFE terpolymer system) was used instead of Viton (registered trademark) GBL-200S, the amount of hollow particles A added was changed according to Table 3, and MT carbon was also added as a reinforcing agent in the amount shown in Table 3 when hollow particles A was added.

[0149] [Example 15] A fluororubber composition and a crosslinked molded article of Example 15 were obtained in the same manner as in Example 1, except that the amount of hollow particles A added in Example 1 was changed according to Table 3, and that coupling agent-treated silica was also added as a reinforcing agent in the amount shown in Table 3 when hollow particles A was added. Note that silica surface-treated with a silane coupling agent (vinyltrimethoxysilane, product name: KBM-1003, manufactured by Shin-Etsu Chemical Co., Ltd.) was used as the coupling agent-treated silica.

[0150] [Evaluation of Physical Properties of Crosslinked Molded Article] 1. Weight Reduction Rate Using a sample cut into a 1 cm square and 2 mm thick piece from the crosslinked molded article, the specific gravity of the crosslinked molded article was measured by the underwater displacement method in accordance with JIS K 7112:1999. From the specific gravity of the crosslinked molded article measured above and the specific gravity of the fluororubber used in the crosslinked molded article, the weight reduction rate (%) was calculated according to the following formula (1): Formula (1): Weight Reduction Rate (%) = {(Specific gravity of fluororubber - Specific gravity of crosslinked molded article) / Specific gravity of fluororubber} x 100

[0151] 2. Compression Set In accordance with the room temperature test of JIS K 6262:2013, a cylindrical cross-linked molded body having a diameter of 29±0.5 mm and a height of 12.5±0.5 mm was used as a test piece, and the compression set (%) of the cross-linked molded body was measured under the conditions of a standard temperature of 23±2°C, a test temperature of 30°C, a test time of 168 hours, and a compression ratio of the test piece of 25%, and evaluated based on the following evaluation criteria. (Compression Set Evaluation Criteria) S: Compression set less than 25% A: Compression set 25% or more but less than 40% B: Compression set 40% or more but less than 60% C: Compression set 60% or more

[0152] More specifically, the compression set was measured by the following procedure. First, the thickness of the central part of the test piece was measured at standard temperature. The test piece was placed on a compression plate (a smooth stainless steel plate), and a spacer (9.3 mm thick) was sandwiched between the outside of the test piece. The compression plate was then compressed until it was in close contact with the spacer. The device compressing the test piece was kept in a thermostatic chamber at the test temperature for the test time. After the test time had elapsed, the device was removed, and the test piece was immediately released from the compressed state. After leaving it at standard temperature for 30 minutes, the thickness of the central part of the test piece was measured. The compression set (%) was calculated from the thickness of the test piece before and after compression and the thickness of the spacer using the following formula (2):

[0153] CS: Compression set (%) t 0 t: original thickness of test piece (mm) 1 t: Spacer thickness (mm) 2 : Thickness (mm) of test piece after 30 minutes after removal from compression device

[0154] 3. Tensile stress at 100% elongation In accordance with JIS K 6251:2017, a dumbbell-shaped No. 3 crosslinked molded article was used as a test piece, and the tensile stress at 100% elongation was determined at a test temperature of 25°C using a fully automatic tensile tester for rubber (product name: No. 211 Strograph AE Elastomer, manufactured by Toyo Seiki Seisaku-sho, Ltd.), and evaluated based on the following evaluation criteria. The tensile stress at 100% elongation was taken as the average value of the values ​​determined for three test pieces. (Evaluation criteria for tensile stress) S: Tensile stress at 100% elongation is 6 MPa or more A: Tensile stress at 100% elongation is 4 MPa or more but less than 6 MPa B: Tensile stress at 100% elongation is 2 MPa or more but less than 4 MPa C: Tensile stress at 100% elongation is less than 2 MPa

[0155]

[0156]

[0157] [Discussion] The crosslinked molded articles obtained in Examples 1 to 7 were obtained by crosslinking a fluororubber composition containing hollow particles having an iodine value of 10 g / 100 g or more and 100 g / 100 g or less and a fluororubber that can be crosslinked with a peroxide using an organic peroxide. Compared to the crosslinked molded article of Reference Example 1, which is a crosslinked molded article of a fluororubber that does not contain hollow particles, the crosslinked molded articles obtained in Examples 1 to 7 were lighter in weight and had smaller compression set. Furthermore, a comparison of Examples 1 to 3 showed that the greater the amount of hollow particles contained in the crosslinked molded article, the higher the weight reduction rate and the smaller the compression set tended to be. The compression set of Example 1 was smaller than that of Example 4. This is presumably because the iodine value of the hollow particles was appropriately low in Example 1, which suppressed aggregation of the hollow particles and resulted in uniform dispersion, and because the residual volatile component content of the hollow particles in Example 1 was low, the reactivity between the hollow particles and the fluororubber was good, resulting in the hollow particles uniformly suppressing plastic deformation of the crosslinked molded product. The compression set of Example 1 was smaller than that of Example 5. This is presumably because the particle size of the hollow particles in Example 1 was appropriately small, which increased the number of interfaces between the hollow particles and the fluororubber and resulted in the formation of more crosslinks between the hollow particles and the fluororubber. The compression set of Example 1 was smaller than that of Example 6. This is presumably because the iodine value of the hollow particles in Example 1 was higher, resulting in the formation of more crosslinks between the hollow particles and the fluororubber. The compression set in Example 1 was smaller than that in Example 7. This is presumably because the iodine value of the hollow particles in Example 1 was appropriately low, which prevented the hollow particles from agglomerating and resulted in uniform dispersion, allowing the hollow particles to uniformly suppress plastic deformation of the crosslinked molded body.

[0158] On the other hand, the crosslinked molded article obtained in Comparative Example 1 contained dense solid particles instead of hollow particles. Because the dense solid particles A used in Comparative Example 1 had a lower specific gravity than the fluororubber, the crosslinked molded article obtained in Comparative Example 1 was lighter than the crosslinked molded article of Reference Example 1. However, compared with the crosslinked molded article of Example 2, which contained the same mass of hollow particles A as Comparative Example 1, and the crosslinked molded article of Example 3, which contained the same volume of hollow particles A as Comparative Example 1, the weight reduction rate was lower, and the weight reduction effect was inferior. The reduction in compression set in the crosslinked molded article obtained in Comparative Example 1 is presumably due to the formation of crosslinked bonds between the dense solid particles and the fluororubber, as the iodine value of the dense solid particles A was in the range of 10 g / 100 g to 100 g / 100 g. The crosslinked molded articles obtained in Comparative Examples 2 and 3 were crosslinked using a polyol- or polyamine-based crosslinking agent rather than an organic peroxide. The crosslinked molded articles obtained in Comparative Examples 2 and 3 were lighter in weight than the crosslinked molded article of Reference Example 1 due to the inclusion of hollow particles, but the compression set was not reduced. This is presumably because crosslinking was not formed between the hollow particles and the fluororubber in the crosslinked molded articles obtained in Comparative Examples 2 and 3.

[0159] The crosslinked molded articles obtained in Examples 8 to 15 were obtained by crosslinking a fluororubber composition containing hollow particles having an iodine value of 10 g / 100 g or more and 100 g / 100 g or less, a peroxide-crosslinkable fluororubber, and a reinforcing agent, using an organic peroxide. The crosslinked molded articles obtained in Examples 8 to 15 were lighter in weight and had smaller compression set than the crosslinked molded article of Reference Example 1, which is a crosslinked molded article of a fluororubber that does not contain hollow particles. Furthermore, the crosslinked molded articles obtained in Examples 8 to 15, which contained a reinforcing agent, had improved tensile stress at 100% elongation compared to the crosslinked molded articles obtained in Examples 1 to 7, which did not contain a reinforcing agent. The crosslinked molded articles obtained in Examples 8 to 14, which used carbon black as a reinforcing agent, also had an improved reduction in compression set compared to the crosslinked molded articles obtained in Examples 1 to 7, which did not contain a reinforcing agent.

[0160] REFERENCE SIGNS LIST 1 aqueous medium 2 low-polarity material 4a hydrophobic solvent 4b material other than hydrophobic solvent 6 shell 7 hollow portion 8 droplet 9 precursor particle 10 hollow particle with hollow portion filled with gas

Claims

1. A fluororubber composition comprising hollow particles and a fluororubber, wherein the hollow particles have a shell containing a resin and a hollow portion surrounded by the shell, and the iodine value measured in accordance with JIS K 0070 is 10 g / 100 g or more and 100 g / 100 g or less, and the fluororubber is a fluororubber that can be crosslinked with a peroxide.

2. The fluororubber composition according to claim 1, wherein the content of the hollow particles per 100 parts by mass of the fluororubber is 1 part by mass or more and 50 parts by mass or less.

3. The fluororubber composition according to claim 1 or 2, wherein the fluororubber is a fluororubber containing at least one halogen atom selected from iodine and bromine in the molecular chain.

4. The fluororubber composition according to claim 1 or 2, wherein the proportion of hollow particles having a circularity of 0.85 or less is less than 15 mass %.

5. The fluororubber composition according to claim 1 or 2, wherein the hollow particles have a residual volatile content of less than 100 ppm.

6. The fluororubber composition according to claim 1 or 2, wherein the hollow particles contain, as the resin, a polymer containing 50 mass % or more of crosslinkable monomer units.

7. The fluororubber composition according to claim 1 or 2, wherein the volume average particle size of the hollow particles is from 0.1 μm to 100 μm.

8. The fluororubber composition according to claim 1 or 2, further comprising a reinforcing agent, the reinforcing agent being at least one selected from carbon black and silica, and the content of the reinforcing agent per 100 parts by mass of the fluororubber is 1 part by mass or more and 15 parts by mass or less.

9. The nitrogen adsorption specific surface area of ​​the carbon black is 5 m 2 / g or more 150m 2 The fluororubber composition according to claim 8, wherein the modulus of elasticity is 1 / g or less.

10. The fluororubber composition according to claim 8, wherein the reinforcing agent is silica treated with a coupling agent.

11. A crosslinked molded article obtained by crosslinking the fluororubber composition according to claim 1 or 2 with an organic peroxide.

Citation Information

Patent Citations

  • Rubber composition for vulcanization molding, production method and use thereof

    JP6116787B1

  • Tetrafluoroethylene-propylene vulcanized rubber and preparation method thereof

    CN109721898A

  • Rubber composition, and rubber member and conveying roller which are produced by using the composition

    JP2012126809A

  • Fluorine rubber composition for open crosslinking and method for crosslinking fluorine rubber composition

    JP2020183490A

  • Intermediate elastomer compositions

    US20070135577A1