Resin-coated metal plate for containers, metal container, and method for producing resin-coated metal plate for containers
The resin-coated metal plate with controlled ethylene terephthalate units and specific orientation addresses the challenges of workability and retort whitening resistance, ensuring effective adhesion and resistance to whitening during sterilization.
Patent Information
- Application Number
- PCT/JP2024/018239
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional resin-coated metal plates for containers face challenges in achieving simultaneously good workability, film adhesion, and retort whitening resistance due to insufficient crystallization and orientation of the resin coating layer, leading to issues like whitening during retort sterilization and poor water barrier properties.
A resin-coated metal plate with a polyester resin coating layer where 90 mol% or more of structural units are ethylene terephthalate units, featuring specific crystallinity and orientation controlled through laser Raman spectroscopy and X-ray diffraction, is developed, with a molten resin layer near the metal plate for adhesion and oriented surface for improved resistance and workability.
The solution provides excellent workability, film adhesion, and retort whitening resistance by controlling the crystallinity and orientation of the resin coating layer, suppressing bubble expansion and maintaining hardness, thereby preventing whitening during retort sterilization.
Smart Images

Figure JP2024018239_28112024_PF_FP_ABST
Abstract
Description
Resin-coated metal sheet for containers, metal container, and method for manufacturing resin-coated metal sheet for containers
[0001] The present invention relates to a resin-coated metal sheet for containers having a polyester resin coating layer on at least one surface of a metal sheet, a metal container using the resin-coated metal sheet for containers, and a method for producing the resin-coated metal sheet for containers.
[0002] Conventionally, metal sheets, such as tin-free steel (TFS) and aluminum, used as materials for metal containers have been coated with paint to improve corrosion resistance and weather resistance. However, this coating technique requires a long processing time due to the complex coating and baking processes, and also has the problem of discharging a large amount of solvent. Therefore, resin-coated metal sheets for containers, in which the surface of the metal sheet is coated with a thermoplastic film, have been developed and are currently widely used industrially, mainly as materials for beverage cans.
[0003] Resin-coated metal sheets for metal containers are required to have performance such as processability and coating adhesion, as well as design and color stability. When conventional resin-coated metal sheets using polyester resins are used with the resin coating layer facing the outer surface of the container, a whitening phenomenon occurs in which the resin coating layer turns white during the retort sterilization process. When whitening occurs, the design of the container is significantly impaired, so several studies have been conducted to suppress the whitening phenomenon, i.e., to improve retort whitening resistance.
[0004] In Patent Document 1, "a resin-coated metal sheet having a polyester resin layer mainly composed of polyethylene terephthalate on both sides, in which a cross section of the polyester resin layer in the thickness direction is measured by laser Raman spectroscopy using linearly polarized laser light, and -1 The half-width of the peak due to the nearby C=0 stretching vibration is 16.0 cm -1 ~24.0cm -1 The document describes a resin-coated metal sheet for containers, characterized in that the resin-coated metal sheet has a viscosity in the range of 1000 to 10000 MPa.
[0005] In Patent Document 2, "a non-stretched thermoplastic polyester resin layer is provided, and the thermoplastic polyester resin layer has a thickness of 1730 cm by laser Raman spectroscopy using linearly polarized laser light on the interface side with the metal material." -1 The half-value width of the Raman shift peak of the thermoplastic polyester resin due to the C═O stretching vibration in the vicinity is 20 cm -1 More than 24cm -1 and a first region on the surface side opposite to the metal material, in which the half width of the Raman shift peak is 14 cm or less. -1 More than 18cm -1 The document describes a thermoplastic polyester resin-coated metal sheet having a second region that is:
[0006] JP 2010-105263 A JP 2017-213884 A
[0007] However, with conventional technology, it has been difficult to achieve all of the following: processability, coating adhesion, and retort whitening resistance. In Patent Document 1, heat treatment is performed for 5 to 15 seconds, but because this is a short time, depending on the lamination conditions before the heat treatment, crystallization of the resin coating layer may be insufficient, resulting in insufficient retort whitening resistance. In Patent Document 2, an unstretched resin coating layer is used, so the resin chains constituting the resin coating layer are not aligned in the plane direction of the resin coating layer. As a result, the water barrier properties of the resin coating layer are poor, and sufficient retort whitening resistance is not achieved. Furthermore, a resin coating layer without orientation is brittle, and there is a risk of the resin coating layer cracking during processing.
[0008] In view of the above problems, the present invention aims to provide a resin-coated metal sheet for containers that has excellent processability, coating adhesion, and retort whitening resistance, a method for producing the same, and a metallic container using the metal sheet.
[0009] The present inventors conducted extensive research to solve the above-mentioned problems and have come to the following conclusion. When a resin coating layer has a layer with appropriate crystallinity and orientation near the metal sheet side and a layer with orientation perpendicular to the thickness direction near the surface side, it exhibits excellent processability, coating adhesion, and retort whitening resistance. In this case, the resin coating layer near the metal sheet side is a molten resin layer with low crystallinity to ensure coating adhesion to the metal sheet. By strictly controlling the crystallinity and orientation, both excellent coating adhesion and retort whitening resistance can be achieved. Furthermore, by having orientation perpendicular to the thickness direction near the surface side of the resin coating layer, a resin coating layer with excellent processability can be obtained. The appropriate index of crystallinity and orientation can be expressed as the peak half-width measured by laser Raman spectroscopy.
[0010] The gist and configuration of the present invention, which has been completed based on the above findings, is as follows.
[0011] [1] A resin-coated metal sheet for containers having a polyester resin coating layer on at least one side of the metal sheet, the polyester resin coating layer comprising 90 mol % or more of its constituent units being ethylene terephthalate units, wherein the thickness of the polyester resin coating layer is measured by laser Raman spectroscopy in which linearly polarized laser light is incident on the thickness direction cross section of the polyester resin coating layer so that the polarization plane is perpendicular to the thickness direction of the polyester resin coating layer, and the thickness of the polyester resin coating layer is measured by laser Raman spectroscopy in which linearly polarized laser light is incident on the thickness direction cross section of the polyester resin coating layer so that the polarization plane is perpendicular to the thickness direction of the polyester resin coating layer. -1 (I) the half width of the peak due to the C═O stretching vibration in the vicinity of the polyester resin coating layer is 14.0 cm at a position 1.0 μm thick from the interface between the polyester resin coating layer and the metal plate -1 18.5cm or more -1 (II) the thickness of the polyester resin coating layer is 14.0 cm or less at a position 1.0 μm thick from the surface of the polyester resin coating layer -1 18.0cm or more -1 or less, and the thickness of the polyester resin coating layer is 1730 cm or less, which is determined by laser Raman spectroscopy, in which linearly polarized laser light is incident on the cross section in the thickness direction of the polyester resin coating layer so that the polarization plane of the laser light is parallel to the thickness direction of the polyester resin coating layer. -1a value A / B obtained by dividing a half-value width A at a position 1.0 μm thick from the interface between the polyester resin coating layer and the metal sheet by a half-value width B at a position 1 / 2 the thickness of the polyester resin coating layer, of a peak due to C═O stretching vibration in the vicinity of the polyester resin coating layer, is 0.80 or more and 1.10 or less.
[0012] [2] In the polyester resin coating layer, the diffraction peak intensity I of the (100) plane by X-ray diffraction 100 and the diffraction peak intensity of the (110) plane I 110 Relative to I 100 / I 110 The resin-coated metal sheet for containers according to the above [1], wherein the modulus is 2.00 or more and 8.50 or less.
[0013] [3] A metal container formed from the resin-coated metal sheet for containers according to [1] or [2] above, wherein the polyester resin coating layer is located on the outer surface of the container.
[0014] [4] A method for producing a resin-coated metal plate for containers, comprising: a laminating step of thermocompressing an oriented polyester resin coating film, the constituent units of which account for 90 mol % or more of ethylene terephthalate units, onto a metal plate using a laminating roll to obtain a resin-coated metal plate having a polyester resin coating layer formed on at least one side of the metal plate; and a heat treatment step of holding the resin-coated metal plate at 80°C or higher and 165°C or lower for 10 minutes or longer to obtain a resin-coated metal plate for containers.
[0015] [5] The method for producing a resin-coated metal sheet for containers according to the above [4], wherein in the laminating step, the temperature of the metal sheet during thermocompression bonding is 260°C or higher and 279°C or lower.
[0016] According to the present invention, it is possible to provide a resin-coated metal sheet for containers that is excellent in processability, coating adhesion, and retort whitening resistance, a method for producing the same, and a metallic container using the metal sheet.
[0017] 1 is a cross-sectional view showing the configuration of a resin-coated metal sheet for containers according to one embodiment of the present invention. FIG. 2 is a view showing the polarization direction of a laser in laser Raman spectroscopy.
[0018] A resin-coated metal sheet for containers according to one embodiment of the present invention will be described below. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example. Furthermore, hereinafter, "%" indicates "% by mass" unless otherwise specified.
[0019] Fig. 1 shows a cross-sectional view of a resin-coated metal sheet for containers according to one embodiment of the present invention. The resin-coated metal sheet for containers 1 includes a metal sheet 2 and a polyester resin coating layer 3 (hereinafter also referred to as "resin coating layer"). While Fig. 1 shows an example in which the resin-coated metal sheet for containers 1 has the resin coating layer 3 on one side of the metal sheet 2, the resin coating layer 3 may be provided on both sides of the metal sheet 2.
[0020] [Metal Sheet] As the metal sheet of the resin-coated metal sheet, a steel sheet such as tinplate or tin-free steel (TFS) can be used. Tinplate has a plating amount of 0.5 g / m 2 15g / m or more 2 The coating amount of tin-free steel is preferably within the following range: 2 More than 200g / m 2 and a metal Cr layer having a coating amount of 3 mg / m in terms of metal Cr layer. 2 30g / m or more 2 It is preferable that the surface of the substrate has a Cr oxide layer as follows:
[0021] The type of metal sheet is not particularly limited as long as it can be formed into the desired shape, but steel sheets having the following chemical compositions and manufacturing methods are preferred: (1) A steel sheet obtained by recrystallization annealing using low-carbon steel with a C (carbon) content of 0.010% or more and 0.10% or less through continuous annealing. (2) A steel sheet obtained by recrystallization annealing using low-carbon steel with a C content of 0.010% or more and 0.10% or less through continuous annealing and overaging. (3) A steel sheet obtained by recrystallization annealing using box annealing using low-carbon steel with a C content of 0.010% or more and 0.10% or less. (4) A steel sheet obtained by secondary cold rolling (DR (Double Reduced) rolling) using low-carbon steel with a C content of 0.010% or more and 0.10% or less through recrystallization annealing using continuous annealing or box annealing. (5) A steel sheet obtained by using IF (Interstitial Free) steel, which is made by adding elements that fix dissolved C, such as Nb and Ti, to ultra-low carbon steel with a C content of 0.003% or less, and recrystallizing the steel sheet by continuous annealing.
[0022] The mechanical properties of the metal sheet are not particularly limited as long as they can be formed into the desired shape. To maintain workability and sufficient can body strength, it is preferable to use a metal sheet with a yield point (YP) of 220 MPa or more and 580 MPa or less. Furthermore, the Lankford value (r value), which is an index of plastic anisotropy, is preferably 0.8 or more. Furthermore, the absolute value of the in-plane anisotropy Δr of the r value is preferably 0.7 or less.
[0023] The composition of the metal sheet is not particularly limited, but a steel sheet containing, for example, Si, Mn, P, S, Al, and N may be used. The Si content is preferably 0.001% or more and 0.1% or less. The Mn content is preferably 0.01% or more and 0.6% or less. The P content is preferably 0.002% or more and 0.05% or less. The S content is preferably 0.002% or more and 0.05% or less. The Al content is preferably 0.005% or more and 0.100% or less. The N content is preferably 0.0005% or more and 0.020% or less. The composition may further contain Ti, Nb, B, Cu, Ni, Cr, Mo, V, and the like. The total content of these elements is preferably 1.0% or less.
[0024] The thickness of the metal plate is not particularly limited, but may be, for example, 0.01 mm or more and 0.35 mm or less.
[0025] [Resin Coating Layer] The resin coating layer is a polyester resin coating layer in which 90 mol % or more of the polyester structural units are ethylene terephthalate units. It is preferable that 95 mol % or more of the polyester structural units are ethylene terephthalate units. Furthermore, when the proportion of ethylene terephthalate units in the structural units is less than 100 mol %, the remainder may be various dicarboxylic acid units or glycol units as shown below.
[0026] As the dicarboxylic acid unit, units derived from aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, diphenylsulfonedicarboxylic acid, diphenoxyethanedicarboxylic acid, 5-sodiumsulfoisophthalic acid, and phthalic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid; alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; and oxycarboxylic acids such as p-oxybenzoic acid can be used.
[0027] As the glycol unit, units derived from aliphatic glycols such as ethylene glycol, propanediol, butanediol, pentanediol, hexanediol, and neopentyl glycol; alicyclic glycols such as cyclohexanedimethanol; aromatic glycols such as bisphenol A and bisphenol S; and diethylene glycol can be used.
[0028] The above-mentioned dicarboxylic acids and glycols may be used in combination in such a manner that the processability is not impaired.
[0029] The resin material forming the resin coating layer is not limited by its manufacturing method. In addition, in manufacturing the polyester resin coating, additives such as fluorescent whitening agents, antioxidants, heat stabilizers, ultraviolet absorbers, antistatic agents, and lubricants may be added as needed.
[0030] The thickness of the resin coating layer is not particularly limited, but may be, for example, 0.01 mm or more and 0.10 mm or less.
[0031] The inventors have discovered that excellent retort whitening resistance can be achieved by setting the crystallinity and orientation of the resin coating layer within appropriate ranges. The inventors believe that the whitening phenomenon during retort sterilization occurs through the following mechanism: Water vapor that penetrates the resin coating layer at the beginning of the retort sterilization process is cooled by the low-temperature contents near the metal-plate interface in the resin coating layer and condenses within the resin coating layer. As the temperature of the contents rises, the condensed water vaporizes, forming bubbles near the metal-plate interface in the resin coating layer, causing the whitening phenomenon. Therefore, by setting the crystallinity and orientation of the resin coating layer near the metal-plate interface within appropriate ranges, the hardness of the resin coating layer is maintained and the expansion of bubbles is suppressed, thereby suppressing the whitening phenomenon.
[0032] The crystallinity and orientation of the resin coating layer were determined by laser Raman spectroscopy. -1 The half-width of the peak due to the nearby C═O stretching vibration can be used as an index for evaluation. -1It is known that the half-width of the peak due to the C=O stretching vibration in the vicinity of 1730 cm is correlated with the density of the polyester resin (AJ Melverger, "Laser-Raman Study of Crystallinity Changes in Poly(ethylene Terephtalate)", Journal of Polymer Science Part A2 (Polymer Physics) vol. 10, published February 1972, pp. 317-322). It is also known that there is a correlation between the density of the resin and the volume fraction crystallinity ("Solid Structure of Polymers II", edited by the Polymer Experiments Editorial Committee of the Society of Polymer Science, Kyoritsu Shuppan Co., Ltd., published 1984). Therefore, the half-width of the peak due to the C=O stretching vibration in the vicinity of 1730 cm is correlated with the density of the polyester resin (AJ Melverger, "Laser-Raman Study of Crystallinity Changes in Poly(ethylene Terephtalate)", Journal of Polymer Science Part A2 (Polymer Physics) vol. 10, published February 1972, pp. 317-322). It is also known that there is a correlation between the density of the resin and the volume fraction crystallinity ("Solid Structure of Polymers II", edited by the Polymer Experiments Editorial Committee of the Society of Polymer Science, published by Kyoritsu Shuppan Co., Ltd., 1984). -1 By measuring the half-width of the peak due to the nearby C═O stretching vibration, the crystallinity of the polyester resin can be determined through the density of the polyester resin.
[0033] Figure 2 shows the direction 4 perpendicular to the thickness direction of the resin coating layer 3 and the direction 5 parallel to it. Conventionally, values obtained by laser Raman spectroscopy by irradiating a linearly polarized laser beam onto a thickness-wise cross section of the resin coating layer with the polarization plane set to direction 5 have been used. However, such average values in the thickness direction of the resin coating layer 3 alone cannot accurately evaluate the crystallinity near the metal plate side or the orientation state near the surface side. Therefore, in the present invention, the half-width of the peak obtained by irradiating a linearly polarized laser beam onto a thickness-wise cross section of the resin coating layer 3 with the polarization plane set to direction 4 (i.e., a direction parallel to the surface of the metal plate 2) is also used. This allows the degree of crystallinity of the resin coating layer 3 near the metal plate and near the surface, respectively.
[0034] A linearly polarized laser beam is incident on a cross section of the polyester resin coating layer in the thickness direction so that the polarization plane is perpendicular to the thickness direction of the polyester resin coating layer. This is determined by laser Raman spectroscopy. -1 The half width of the peak due to the C═O stretching vibration in the vicinity of the polyester resin coating layer was 14.0 cm at a position 1.0 μm thick from the interface between the polyester resin coating layer and the metal plate. -1 18.5cm or more -1 The peak half width is 14.0 cm or less.-1 If the peak half width is less than 18.5 cm, the crystallinity of the resin coating layer near the metal sheet interface is too high, resulting in poor coating adhesion. -1 If it exceeds 15.0 cm, the crystallinity of the resin coating layer is too low, the resin coating layer is not sufficiently cured, the expansion of bubbles cannot be suppressed, and the retort whitening resistance is poor. -1 The peak half width is preferably 16.5 cm or more. -1 The peak half width is preferably 15.0 cm or less. -1 16.5cm or more -1 More preferably, it is:
[0035] A linearly polarized laser beam is incident on a cross section of the polyester resin coating layer in the thickness direction so that the polarization plane is perpendicular to the thickness direction of the polyester resin coating layer. This is determined by laser Raman spectroscopy. -1 The half-width of the peak due to the C═O stretching vibration in the vicinity of the surface of the polyester resin coating layer was 14.0 cm at a depth of 1.0 μm from the surface of the polyester resin coating layer. -1 18.0cm or more -1 The peak half width is 14.0 cm or less. -1 If the peak half width is less than 18.0 cm, the crystallization will proceed excessively, resulting in embrittlement and poor processability. -1 If the peak half width is more than 15.0 cm, the amount of crystals is small and the blocking resistance described below is poor. -1 The peak half width is preferably 17.0 cm or more. -1 The peak half width is preferably 15.0 cm or less. -1 17.0cm or more -1 More preferably, it is:
[0036] A linearly polarized laser beam is incident on a cross section of the polyester resin coating layer in the thickness direction so that the polarization plane is parallel to the thickness direction of the polyester resin coating layer, and the wavelength of the linearly polarized laser beam is measured by laser Raman spectroscopy. -1The value A / B, obtained by dividing the half-width A of the peak due to the C=O stretching vibration at a position 1.0 μm thick from the interface between the polyester resin coating layer and the metal sheet by the half-width B at a position 1 / 2 the thickness of the polyester resin coating layer, is 0.80 or more and 1.10 or less. If A / B exceeds 1.10, the adhesion between the metal sheet and the resin coating layer is impaired, and processability is not obtained. On the other hand, if A / B is less than 0.80, although the coating adhesion is excellent, retort whitening resistance is not obtained. A / B is preferably 1.05 or less, and more preferably 1.03 or less. Furthermore, A / B is preferably 0.85 or more, and more preferably 0.90 or more. Furthermore, A / B is more preferably 0.85 or more and 1.05 or less, and most preferably 0.90 or more and 1.03 or less. Furthermore, from the viewpoint of suppressing bubble expansion, the half-width value A is 20.5 cm -1 It is preferable that:
[0037] The half-width of the peak and the A / B ratio can be measured as follows: Laser Raman spectroscopy is performed by irradiating a linearly polarized laser beam onto the thickness direction cross section of the resin coating layer to be measured so that the polarization plane is perpendicular to the thickness direction cross section of the resin coating layer. -1 The half-width of the peak due to the C=O stretching vibration in the vicinity of the resin coating layer is obtained. The measurement positions are a position 1.0 μm thick from the interface between the resin coating layer and the metal plate, and a position 1.0 μm thick from the surface of the resin coating layer. Similarly, laser Raman spectroscopy is performed on the thickness-direction cross section of the manufactured resin-coated metal plate for containers by irradiating linearly polarized laser light so that the polarization plane is parallel to the thickness-direction cross section of the resin coating layer. As a result, the peak at 1730 cm -1 The half-width of the peak due to the C=O stretching vibration in the vicinity of the metal plate is obtained. The half-width measured at a position 1.0 μm thick from the interface of the resin coating layer with the metal plate is defined as A, and the half-width measured at a position 1 / 2 the thickness of the resin coating layer is defined as B, and the half-width ratio A / B is calculated. Note that a Raman force manufactured by Nanophoton Inc. can be used for the laser Raman spectroscopy analysis. The laser wavelength is 532 nm, and a 100x objective lens is used, with an aperture diameter of 25 μm and a diffraction grating of 600 gr / mm.
[0038] X-ray diffraction peak intensity of the (100) plane I 100 and the diffraction peak intensity of the (110) plane I 110 Relative to I 100 / I 110 is preferably 2.00 or more and 8.50 or less. When a resin-coated metal sheet heated at or above the glass transition point of the resin coating layer is compressed under high load, such as in a coil, there is a risk of the resin surface fusing and sticking (blocking). Preventing blocking makes it easier to unwind the coil and improves the surface performance of the product. The inventors have clarified that the crystallinity of the entire resin coating layer, not just the outermost layer where resins contact each other, affects blocking resistance. Furthermore, the intensity ratio I of the diffraction peaks of the (100) plane and the (110) plane obtained by X-ray diffraction of the resin coating layer is 100 / I 110 It has been found that when the intensity ratio I is in the range of 2.00 or more and 8.50 or less, the blocking resistance is particularly excellent. 100 / I 110 If the strength ratio is 2.00 or more, the crystallinity of the entire resin coating layer is sufficiently high, and it is possible to suitably prevent the resin coating layer from melting and fusing when pressed during heating. Regarding blocking resistance, the higher the crystallinity of the resin coating layer, the better, but for a general resin-coated metal sheet, the substantial upper limit of the strength ratio is 8.50. 100 / I 110 is more preferably 3.50 or more. 100 / I 110 It is more preferable that the intensity ratio I is 8.00 or less. 100 / I 110 It is more preferable that the value is 3.50 or more and 8.00 or less.
[0039] The diffraction peak intensity of each orientation can be measured as follows. X-ray diffraction is performed on the resin-coated metal sheet for containers to be measured using a Smart Lab manufactured by Rigaku Corporation. The X-ray tube is CuKα, the measurement angle range is 2θ = 10° to 30°, and the scan speed can be set to 80 seconds / degree. The peaks present at measurement angles of 24° to 29° are considered to be peaks of the (100) plane, and the intensity I100 The peaks present at measurement angles of 22° to 24° are taken as the peaks of the (110) plane, and the intensity I 110 From the obtained intensities, the peak intensity ratio I 100 / I 110 Ask for.
[0040] By using the resin-coated metal sheet for containers described above, it is possible to provide a metal container that is excellent in processability, coating adhesion, and retort whitening resistance. In one example, the metal container includes a member formed from the resin-coated metal sheet for containers, and the member has a polyester resin coating layer on the outer surface of the container. The metal container and the member can be manufactured by conventional methods.
[0041] [Manufacturing method] Next, a method for manufacturing a resin-coated metal sheet for containers will be described. A resin coating layer having the above-mentioned properties can be achieved by a two-step process: (1) thermocompression bonding of an oriented polyester resin coating to a metal sheet by controlling the thermal history (laminating process), and then (2) heating and aging the metal sheet (heat treatment process).
[0042] First, a non-stretched polyester resin coating is produced using a polyester resin in which 90 mol % or more of the constituent units are ethylene terephthalate units. As described above in the description of the resin coating layer, a polyester resin in which 90 mol % or more of the constituent units are ethylene terephthalate units can be used as the polyester resin constituting the polyester resin coating. Additives and the like are also as described above in the description of the resin coating layer.
[0043] The method for producing a polyester resin coating is not particularly limited, but in one example, it can be produced as follows. First, a polyester resin is charged into an extruder, if necessary, after being dried under heat and vacuum, and the polyester resin is heated and melted in the extruder. The heated and melted polyester resin is extruded through a filter or the like. At this time, foreign matter and denatured resin can be removed by the filter. The extruded polyester resin is formed into a sheet using a T-die, discharged, and extruded onto a cooling body such as a casting drum. The extruded sheet is cooled and solidified to obtain an unstretched polyester resin coating.
[0044] Next, the unstretched polyester resin coating is stretched to form a stretched polyester resin coating. As a method for obtaining a stretched polyester resin coating, a sequential biaxial stretching method in which the polyester resin is stretched in one of the longitudinal direction and the width direction and then in the other direction, or a simultaneous biaxial stretching method in which the polyester resin is stretched in the longitudinal direction and the width direction simultaneously, or the like is preferably used. The stretched polyester resin coating is preferably a biaxially stretched polyester resin coating.
[0045] Next, the stretched polyester resin film is subjected to a lamination process in which the stretched polyester resin film is thermocompression bonded to a metal plate. The stretched polyester resin film is heated to a temperature equal to or higher than its melting point and thermocompression bonded to the metal plate using a lamination roll (thermocompression film lamination method). In order to control the properties of the resin coating layer, it is preferable that the resin coating layer after thermocompression bonding be molten near the interface with the metal plate and oriented near the surface on the opposite side.
[0046] In addition, the temperature of the metal plate during thermocompression bonding is preferably 279°C or less in order to control the X-ray diffraction intensity ratio. If the temperature of the metal plate during thermocompression bonding is 279°C or less, the diffraction peak intensity I of the (100) plane by X-ray diffraction is 100 and the diffraction peak intensity of the (110) plane I 110 Relative to I 100 / I 110 can be 2.00 or more. The temperature of the metal plate during thermocompression bonding is preferably 260°C or more, more preferably 265°C or more. When the temperature of the metal plate during thermocompression bonding is 260°C or more, the wettability of the stretched polyester resin coating and the metal plate can be suitably obtained. The temperature of the metal plate during thermocompression bonding is more preferably 260°C or more and 279°C or less, and most preferably 265°C or more and 279°C or less.
[0047] In order to control the surface vicinity of the resin coating layer to an appropriate orientation, it is preferable to maintain the orientation formed during the production of the stretched polyester resin coating without melting the surface vicinity of the stretched polyester resin coating. To this end, it is preferable to set the temperature of the laminating roll that presses the stretched polyester resin coating onto the metal plate during thermocompression bonding to (the melting point of the resin coating layer - 100) ° C or less. This effectively prevents the surface of the stretched polyester resin coating from being heated above its melting point during thermocompression bonding, making it possible to maintain the orientation of the stretched polyester resin coating. The temperature of the laminating roll is more preferably (the melting point of the resin coating layer - 120 ° C) or less, and even more preferably (the melting point of the resin coating layer - 140 ° C) or less. Furthermore, the temperature of the laminating roll is preferably (the melting point of the resin coating layer - 200 ° C) or more. The temperature of the laminating roll is preferably (melting point of the resin coating layer - 200°C) or higher (melting point of the resin coating layer - 100)°C or lower, more preferably (melting point of the resin coating layer - 200°C) or higher (melting point of the resin coating layer - 120)°C or lower, and even more preferably (melting point of the resin coating layer - 200°C) or higher (melting point of the resin coating layer - 140)°C or lower.
[0048] The time during which the stretched polyester resin coating is thermocompressed to the metal plate by the laminating roll (hereinafter referred to as the thermocompression bonding time) is preferably short so as to maintain the oriented state. The thermocompression bonding time is preferably 5 msec or more, and more preferably 40 msec or less. By setting the thermocompression bonding time to 5 msec or more, sufficient time for the stretched polyester resin coating to thermally flow is ensured, which improves wetting to the metal plate and further improves coating adhesion. Furthermore, by setting the thermocompression bonding time to 40 msec or less, it is more preferable that the oriented state remains. The thermocompression bonding time is more preferably 5 msec or more and 40 msec or less.
[0049] Next, the metal sheet after the lamination step is subjected to a heat treatment (heat treatment step). In the heat treatment step, the metal sheet side of the resin coating layer is moderately crystallized, and the crystallinity of the resin coating layer is adjusted to within the range specified in the present invention. The heat treatment method is not particularly limited, and for example, a method of heating the resin coating layer from the surface side by heating the atmosphere at a high temperature using a hot air oven may be used. Alternatively, a method of heating using an induction heater or near-infrared rays may be used.
[0050] The heat treatment temperature is 80°C or higher and 165°C or lower. This temperature range is the temperature range from the glass transition temperature to the cold crystallization peak of a polyester resin in which 90 mol% or more of the constituent units are ethylene terephthalate units. The heat treatment temperature is preferably 90°C or higher. The heat treatment temperature is preferably 120°C or lower. The heat treatment temperature is more preferably 90°C or higher and 120°C or lower. By setting the heat treatment temperature to 90°C or higher and 120°C or lower, it is possible to preferably obtain retort whitening resistance while suppressing a decrease in coating adhesion due to excessive crystallization. After reaching the predetermined temperature, the temperature is controlled so as to be maintained within this temperature range. The heat treatment temperature is based on the temperature of the metal plate.
[0051] The heat treatment time is 10 minutes or more. If the treatment time is less than 10 minutes, crystallization of the resin coating layer near the metal plate becomes insufficient, making it difficult to obtain retort whitening resistance. Furthermore, the heat treatment time is preferably 48 hours or less. If the treatment time is 48 hours or less, crystallization of the resin coating layer near the metal plate is favorable, and adhesion between the metal plate and the resin coating layer is favorably obtained. The heat treatment time is preferably 1 hour or more, and more preferably 5 hours or more. Furthermore, the heat treatment time is preferably 24 hours or less. The heat treatment time is preferably 1 hour or more and 48 hours or less, and more preferably 5 hours or more and 24 hours or less.
[0052] The manufacturing conditions other than those mentioned above can be the same as those in the ordinary method.
[0053] The metal plate was a 0.22 mm thick TFS (metal Cr layer: 120 mg / m 2 Cr oxide layer: 10 mg / m in terms of metal Cr2 The polyester resin (ethylene terephthalate unit ratio: 100 mol%) shown in Table 1 was charged into an extruder, heated and melted, then extruded through a filter and cooled to solidify, yielding a polyester resin coating. The polyester resin coating was stretched in the longitudinal direction and then in the width direction to yield a biaxially stretched polyester resin coating. The thickness of the polyester resin coating was 12 μm. Note that No. 25 was subjected to the next step without stretching.
[0054]
[0055] A biaxially oriented polyester resin coating (unstretched polyester resin coating in the case of No. 25) was coated on a metal plate using a film lamination method (film thermocompression bonding method). The metal plate was heated to the temperature shown in Table 1, and a biaxially oriented polyester resin coating (unstretched polyester resin coating in the case of No. 25) was thermocompression bonded to both sides of the metal plate using a laminating roll. The melting point of the resin coating layer (PET) was approximately 260°C. The laminating roll temperature was 160°C or less, and the thermocompression bonding time was within the range of 5 msec to 40 msec. A resin-coated metal plate in which both sides of the metal plate were coated with a resin coating layer was produced by water cooling 1 second after thermocompression bonding. The resin-coated metal plate was then subjected to a heat treatment under the conditions shown in Table 1 to obtain a resin-coated metal plate for containers.
[0056] Laser Raman spectroscopy and X-ray diffraction were performed using the methods described above. The results of each measurement are shown in Table 1. In Table 1, the direction of the polarization plane is described as "horizontally polarized" when it is perpendicular to the cross section of the resin coating layer in the thickness direction, relative to the direction of the metal plate surface, and as "vertically polarized" when it is parallel to the cross section of the resin coating layer in the thickness direction.
[0057] The resin-coated metal sheets of the invention and comparative examples were evaluated for retort whitening resistance, coating adhesion, processability, and blocking resistance by the methods described below. Table 1 shows the evaluation results.
[0058] (1) Evaluation of retort whitening resistance Using a resin-coated metal sheet for containers, cans were made so that the resin coating layer to be evaluated was on the outer surface of the can. Distilled water was filled into the can, and then a lid was sealed. The can was then placed in a retort apparatus with the bottom facing downwards, and subjected to retort sterilization at 125°C for 90 minutes. Water at 20°C was then filled into the retort apparatus, and the can was quenched. The bottom of the can after quenching was observed and evaluated according to the following criteria: Rating "4": No whitening. Rating "3": Light whitening was observed in an area of 3% or less by area percentage. No practical problems. Rating "2": Whitening was observed in an area of more than 3% but not more than 50% by area percentage. No practical problems. Rating "1": Whitening was observed in an area of more than 50% by area percentage. There were practical problems.
[0059] (2) Evaluation of Coating Adhesion Paraffin wax was applied to a resin-coated metal sheet for containers. Then, a disk with a diameter of 200 mm was punched out. The disk was drawn into a cup with a drawing ratio of 2.00 using a cupping press, so that the resin coating layer to be evaluated was on the outer surface of the can. The obtained cup was then subjected to a two-stage redrawing process to drawing ratios of 2.20 and 2.50. The can flange was trimmed to obtain a redrawn can. The obtained can body was subjected to a retort sterilization treatment at 125°C for 90 minutes in a retort apparatus. The trim portion of the can body after the retort sterilization treatment was observed over the entire circumference and evaluated according to the following criteria: Rating "4": No peeling. Rating "3": Peeling of up to 1 mm or less was observed. No practical problems. Rating "2": Peeling of more than 1 mm but not more than 3 mm was observed. No practical problems. Rating "1": Peeling of more than 3 mm was observed. There were practical problems.
[0060] (3) Evaluation of processability Paraffin wax was applied to a resin-coated metal sheet for containers. Then, a disk with a diameter of 200 mm was punched out. The disk was drawn into a cup with a drawing ratio of 2.00 using a cupping press, so that the resin coating layer to be evaluated faced the outer surface of the can. The obtained cup was then subjected to a two-stage re-drawing process to drawing ratios of 2.20 and 2.50. A panel was processed at the bottom of the can. The processed can bottom panel of the obtained can body was observed and evaluated according to the following criteria: Rating "4": No damage to the polyester resin coating layer after molding. Rating "3": Minor damage was observed in some parts of the polyester resin coating layer after molding. No practical problems. Rating "2": Partial damage was observed in the polyester resin coating layer after molding. No practical problems. Rating "1": Minor damage was observed all around the polyester resin coating layer after molding. Problems in practical use.
[0061] (4) Evaluation of Blocking Resistance The resin-coated metal sheet before heat treatment was cut into several pieces of 20 mm square, and the resin-coated metal sheets were stacked. 2 Heat treatment was performed at the respective heat treatment temperatures and heat treatment times shown in the table under a pressure of 1000 kJ / cm2. The overlapping resin-coated metal sheets were peeled off with tweezers, and it was evaluated whether the resin-coated metal sheets peeled off without resistance. In addition, the surfaces of the resin-coated metal sheets after peeling were observed using a scanning electron microscope to check for surface damage, and the evaluation was performed according to the following criteria. Rating "4": There was no resistance at all during peeling, and no damage to the resin coating layer. Rating "3": There was slight resistance during peeling, but no damage to the resin coating layer. Rating "2": There was relatively strong resistance during peeling, but no damage to the resin coating layer. Rating "1": There was strong resistance during peeling. The resin coating layer was fused, and damage was observed on the surface.
[0062] In the resin-coated metal sheets for containers of the invention, the retort whitening resistance, coating adhesion, and processability were all good (evaluated as "2" or higher). On the other hand, in the comparative examples, the evaluation results for any of the retort whitening resistance, coating adhesion, and processability were insufficient (evaluated as "1"). No. 1 had a large half-width of the C=O peak at 1.0 μm from the metal sheet surface and a large half-width of the C=O peak at 1.0 μm from the resin coating layer surface, and the amount of crystals was small, so it had poor retort whitening resistance. In addition, no crystal peaks were observed in X-ray diffraction, so it had poor blocking resistance. No. 2 also had a large half-width of the C=O peak at 1.0 μm from the metal sheet surface and a small amount of crystals, so it had poor retort whitening resistance. In No. 23 and No. 24, the heat treatment temperature was high, causing excessive crystallization, resulting in an excessively large half-value width ratio A / B, and poor coating adhesion, processability, and blocking resistance. In No. 25, a non-stretched polyester resin coating was used, resulting in a small amount of crystallization and poor retort whitening resistance, processability, and blocking resistance. From the above, the effects of the present invention are clear.
[0063] Among the invention examples, the X-ray diffraction peak intensity ratio I 100 / I 110 Those having a value of 2.00 or more and 8.50 or less had good retort whitening resistance, coating adhesion, and processability, as well as good blocking resistance (rating of 2 or more). This demonstrates that by setting the X-ray diffraction peak intensity ratio within the preferred range of the present invention, a resin-coated metal sheet for containers having excellent blocking resistance can be obtained.
[0064] According to the present invention, it is possible to provide a resin-coated metal sheet for containers that is excellent in processability, coating adhesion, and retort whitening resistance, a method for producing the same, and a metallic container using the metal sheet.
[0065] 1 Resin-coated metal sheet for container 2 Metal sheet 3 Resin coating layer 4 Direction perpendicular to the thickness direction of the resin coating layer 5 Direction parallel to the thickness direction of the resin coating layer
Claims
1. A resin-coated metal plate for containers having a polyester resin coating layer on at least one side of the metal plate, the polyester resin coating layer being composed of 90 mol % or more of ethylene terephthalate units, and a linear polarized laser beam having a polarization plane perpendicular to the thickness direction of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer, the ... is incident on the thickness direction cross section of the polyester resin coating layer, the linear polarized laser beam having a polarization plane perpendicular to the thickness direction of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating layer is incident on the thickness direction cross section of the polyester resin coating -1 (I) the half-value width of the peak due to the C═O stretching vibration in the vicinity of the metal plate is 14.0 cm at a position 1.0 μm thick from the interface of the polyester resin coating layer with the metal plate -1 18.5cm or more -1 (II) The thickness of the polyester resin coating layer is 14.0 cm or less at a position 1.0 μm thick from the surface of the polyester resin coating layer. -1 18.0cm or more -1 or less, which is determined by laser Raman spectroscopy, in which linearly polarized laser light is incident on a cross section in the thickness direction of the polyester resin coating layer such that the polarization plane is parallel to the thickness direction of the polyester resin coating layer, and -1 A resin-coated metal sheet for containers, wherein a value A / B obtained by dividing a half-value width A at a position 1.0 μm thick from the interface between the polyester resin coating layer and the metal sheet, and a half-value width B at a position 1 / 2 the thickness of the polyester resin coating layer, is 0.80 or more and 1.10 or less, for a peak due to C═O stretching vibration in the vicinity of the interface.
2. In the polyester resin coating layer, the diffraction peak intensity I of the (100) plane by X-ray diffraction 100 and the diffraction peak intensity of the (110) plane I 110 Comparison with I 100 / I 110 The resin-coated metal sheet for containers according to claim 1, wherein the modulus of elasticity is 2.00 or more and 8.50 or less.
3. A metal container formed from the resin-coated metal sheet for containers according to claim 1 or 2, in which the polyester resin coating layer is located on the outer surface side of the container.
4. A method for producing a resin-coated metal plate for containers, comprising: a lamination step of thermocompressing an oriented polyester resin coating, the constituent units of which are 90 mol % or more ethylene terephthalate units, onto a metal plate using a lamination roll to obtain a resin-coated metal plate having a polyester resin coating layer formed on at least one side of the metal plate; and a heat treatment step of holding the resin-coated metal plate at 80°C or higher and 165°C or lower for 10 minutes or more to obtain a resin-coated metal plate for containers.
5. The method for producing a resin-coated metal sheet for containers according to claim 4, wherein the temperature of the metal sheet during thermocompression bonding in the laminating step is 260°C or higher and 279°C or lower.
Citation Information
Patent Citations
Laminated metal sheet for can excellent in processability after heat treatment
JP2004345232A
Resin-coated metal sheet for container
JP2010105263A
Thermoplastic polyester resin coated metal sheet, can made of thermoplastic polyester resin coated metal sheet and manufacturing method of thermoplastic polyester resin coated metal sheet
JP2017213884A
Resin-coated metal plate for container
WO2021020549A1