Condensed polycyclic aromatic compound, material for photoelectric conversion element, organic thin film, and organic photoelectric conversion element

A novel fused polycyclic aromatic compound with a thiophene ring bonded at the 3-position addresses the limitations of existing BTBT compounds by enhancing EQE, suppressing dark current, and improving response speed in organic photoelectric conversion devices, making them suitable for practical use.

WO2024242042A1PCT designated stage expired Publication Date: 2024-11-28NIPPON KAYAKU CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018283
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-31
Filing Date
2024-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current organic photoelectric conversion devices using BTBT compounds face challenges in simultaneously improving External Quantum Efficiency (EQE) and suppressing dark current, while also lacking sufficient response speed for practical use.

Method used

A novel fused polycyclic aromatic compound with a thiophene ring bonded at the 3-position is developed, which provides a low HOMO energy level, enhancing EQE, reducing dark current, and achieving excellent response speed when used in organic photoelectric conversion devices.

Benefits of technology

The compound achieves high EQE, low dark current values, and fast response speed in organic photoelectric conversion elements, making it suitable for practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018283_28112024_PF_FP_ABST
    Figure JP2024018283_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are: a condensed polycyclic aromatic compound that serves as an organic photoelectric conversion material that has excellent external quantum efficiency (EQE), dark current, and response speed when used in a photoelectric conversion element; and a material for a photoelectric conversion element, an organic thin film, and an organic photoelectric conversion element that use the condensed polycyclic aromatic compound. The condensed polycyclic aromatic compound is represented by formula (1). (In formula (1), X and Y each independently represent a divalent aromatic hydrocarbon group or a single bond, excluding when X and Y are both a divalent linking group formed by removing two hydrogen atoms from benzene, when X and Y are both a single bond, and when one of X and Y is a divalent linking group formed by removing two hydrogen atoms from benzene and the other is a single bond.)
Need to check novelty before this filing date? Find Prior Art

Description

Fused polycyclic aromatic compound, photoelectric conversion element material, organic thin film, and organic photoelectric conversion element

[0001] The present invention relates to a novel fused polycyclic aromatic compound and its use. More specifically, the present invention relates to a fused polycyclic aromatic compound that is a benzothieno[3,2-b][1]benzothiophene (hereinafter abbreviated as "BTBT") derivative, as well as a photoelectric conversion element material, an organic thin film, and an organic photoelectric conversion element using the same.

[0002] Organic electronics devices have been the subject of vigorous research and development in recent years because they can be supplied stably as they do not contain rare metals or other such raw materials, have flexibility not found in inorganic materials, and can be manufactured by wet film formation. For example, organic thin-film devices such as organic electroluminescence (EL) elements, field-effect transistors, and organic photoelectric conversion elements have attracted attention, and various organic electronics materials, such as condensed polycyclic aromatic compounds, which can be used in these thin-film devices, have been researched and developed.

[0003] Among the above devices, organic photoelectric conversion elements are used in optical sensors and the like, and their use in image sensors, for example, is being considered (Patent Document 1). When used as an image sensor, it is important to improve the external quantum efficiency (EQE), which indicates the degree to which irradiated light is efficiently converted into electrical energy, and to suppress the current value (dark current) when no light is irradiated. In addition to these characteristics, image sensors are required to have a high response speed when switching light irradiation on and off in order to clearly capture moving objects (Patent Document 2).

[0004] In order to satisfy such required characteristics, organic photoelectric conversion elements currently use a bulk heterojunction structure formed by a mixed film of a P-type organic semiconductor material (hole transport material) and an N-type organic semiconductor material (electron transport material) as a photoelectric conversion layer, and studies are being conducted to achieve both an improvement in EQE and a suppression of dark current. In such research and development, the use of a BTBT compound, which is known to exhibit high hole transport properties, as a P-type organic semiconductor material has been considered (Patent Document 3).

[0005] WO2022 / 114065 Patent No. 6674547 WO2016 / 185858 WO2018 / 016465

[0006] However, among the photoelectric conversion elements using BTBT compounds reported so far, few have been able to simultaneously improve EQE and suppress dark current, and none have achieved a response speed sufficient for practical use. Patent Document 4 reports a BTBT compound that is excellent in improving EQE and suppressing dark current when used in a photoelectric conversion element, but there is no description about response, and evaluation by the present inventors has revealed that a response speed sufficient for practical use cannot be achieved.

[0007] As mentioned above, many BTBT compounds exhibit high hole transport properties and therefore can satisfy the EQE requirement, but achieving this while also suppressing dark current has been a difficult task. One cause of dark current is believed to be the unintended generation of charge due to thermal excitation from the HOMO (Highest Occupied Molecular Orbital) level of a P-type organic semiconductor material to the LUMO (Lowest Unoccupied Molecular Orbital) level of an N-type organic semiconductor material at the organic semiconductor P-N interface. The generation of dark current due to thermal excitation is more likely to occur the smaller the energy difference between the HOMO level of the P-type semiconductor material and the LUMO level of the N-type semiconductor material. Conversely, the larger the energy difference, the more likely it is that unnecessary charge generation can be prevented, thereby suppressing dark current. Therefore, in order to suppress dark current, a material with a low HOMO energy level of a P-type organic semiconductor material is preferred.

[0008] In view of the above circumstances, an object of the present invention is to provide a fused polycyclic aromatic compound that provides an organic photoelectric conversion element with a high EQE, a low dark current value, and an excellent response speed, as well as a photoelectric conversion element material, an organic thin film, and an organic photoelectric conversion element using the same.

[0009] As a result of extensive investigations, the present inventors have developed an organic semiconductor material having a low HOMO level energy that is significant when used in a photoelectric conversion element, by using a novel fused polycyclic aromatic compound in which a thiophene ring bonded at the 3-position is located at the molecular end, and have found that this solves the above-mentioned problems, thereby completing the present invention.

[0010] That is, the present invention relates to the following [1] to [7]. [1] A compound represented by the following formula (1): (In formula (1), X and Y each independently represent a divalent aromatic hydrocarbon group and a single bond, excluding the cases where X and Y are both divalent linking groups obtained by removing two hydrogen atoms from benzene, where X and Y are both single bonds, and where one of X and Y is a divalent linking group obtained by removing two hydrogen atoms from benzene and the other is a single bond.)

[0011] [2] The condensed polycyclic aromatic compound according to [1], wherein X and Y are the same. [3] The condensed polycyclic aromatic compound according to [1], wherein X and Y are different from each other. [4] The condensed polycyclic aromatic compound according to any one of [1] to [3], wherein X and Y are each independently a divalent linking group formed by removing two hydrogen atoms from benzene, biphenyl, or naphthalene. [5] A material for photoelectric conversion elements containing the condensed polycyclic aromatic compound according to [1]. [6] An organic thin film comprising the condensed polycyclic aromatic compound according to [1] or the material for photoelectric conversion elements according to [5]. [7] An organic photoelectric conversion element having the organic thin film according to [6].

[0012] According to the present invention, it is possible to provide a fused polycyclic aromatic compound that provides an organic photoelectric conversion element with a high EQE, a low dark current value, and an excellent response speed, as well as a photoelectric conversion element material, an organic thin film, and an organic photoelectric conversion element using the same. In this specification, the fused polycyclic aromatic compound represented by formula (1) may be referred to as the "compound of the present invention."

[0013] FIG. 1 is a schematic cross-sectional view showing one embodiment of an organic photoelectric conversion element.

[0014] [Fused Polycyclic Aromatic Compound] The fused polycyclic aromatic compound of the present invention is represented by the following formula (1).

[0015]

[0016] In formula (1), X and Y each independently represent a divalent aromatic hydrocarbon group and a single bond. The divalent aromatic hydrocarbon group is a divalent linking group obtained by removing two arbitrary hydrogen atoms from the aromatic ring of an aromatic hydrocarbon compound. The aromatic hydrocarbon compound that can serve as the divalent linking group preferably has 6 to 18 carbon atoms, more preferably 6 to 12 carbon atoms. The aromatic hydrocarbon compound that can serve as the divalent linking group is not particularly limited as long as it is a hydrocarbon compound having aromaticity. Examples of divalent aromatic hydrocarbon groups include linking groups obtained by removing two hydrogen atoms from an aromatic organic compound selected from benzene, naphthalene, biphenyl, anthracene, terphenyl, phenanthrene, tetracene, chrysene, pyrene, fluorene, phenylnaphthalene, and diphenylnaphthalene. The divalent aromatic hydrocarbon group is preferably a divalent linking group obtained by removing two hydrogen atoms from benzene, naphthalene, biphenyl, anthracene, terphenyl, or phenylnaphthalene, and more preferably a divalent linking group obtained by removing two hydrogen atoms from benzene, naphthalene, or biphenyl. The divalent aromatic hydrocarbon group may have a substituent, and the substituent that may be present is not particularly limited. Note that when X and Y are single bonds, this means that a thiophene ring is directly bonded to the BTBT ring. However, this does not include cases where X and Y are both divalent linking groups obtained by removing two hydrogen atoms from benzene, where X and Y are both single bonds, or where one of X and Y is a divalent linking group obtained by removing two hydrogen atoms from benzene and the other is a single bond.

[0017] The two thiophene rings at the ends of the molecule in formula (1) may have substituents on the three unbonded carbon atoms, but preferably have no substituents. The two thiophene rings at the ends of the molecule in formula (1) do not have any further fused ring structures.

[0018] Next, a method for synthesizing the fused polycyclic aromatic compound represented by formula (1) will be described. The fused polycyclic aromatic compound represented by formula (1) can be synthesized using dihalogenated BTBT (2,7-dihalogenobenzo[b]benzo[4,5]thieno[2,3-b]thiophene) represented by formula (S) below, synthesized by a known method. When X and Y are the same, the compound can be synthesized by a coupling reaction using two equivalents of a boronic acid derivative represented by formula (T) below (Reaction Formula A). On the other hand, when X and Y are different from each other, the compound can be synthesized by sequentially coupling a boronic acid derivative represented by formula (T) below with a boronic acid derivative represented by formula (U) below (Reaction Formula B).

[0019]

[0020]

[0021] Z in formula (S) 1 and Z 2 each independently represents bromine or iodine, and R in formula (T) and formula (U) 1 , R 2 , R 3 , and R 4 each independently represents hydrogen or an alkyl group. In formula (S), formula (T), and formula (U), X and Y have the same meaning as X and Y in formula (1).

[0022] The method for purifying the fused polycyclic aromatic compound represented by formula (1) is not particularly limited, and known methods such as recrystallization, column chromatography, and vacuum sublimation purification can be used. These methods can also be combined as necessary.

[0023] Specific examples of the fused polycyclic aromatic compound represented by formula (1) are shown below, but the compound is not limited to these examples.

[0024]

[0025] [Photoelectric conversion element material] The photoelectric conversion element material contains a fused polycyclic aromatic compound represented by formula (1). The photoelectric conversion element material may contain components other than the compound represented by formula (1) as long as the effects of the present invention are not impaired. However, the content of the compound represented by formula (1) in the photoelectric conversion element material is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, particularly preferably 98% by mass or more, and most preferably 99% by mass or more. The photoelectric conversion element material may also contain only the compound represented by formula (1). Note that the photoelectric conversion element material may contain one or more fused polycyclic aromatic compounds represented by formula (1) alone or in combination. The photoelectric conversion element material containing the fused polycyclic aromatic compound represented by formula (1) can be used as a hole transport material in a photoelectric conversion element to realize a photoelectric conversion element with excellent response speed.

[0026] [Organic Thin Film] The organic thin film is characterized by containing the above-mentioned photoelectric conversion element material. The film thickness of the organic thin film may be selected depending on the application, but is usually 1 nm to 1 μm, preferably 5 nm to 500 nm, and more preferably 10 nm to 500 nm. Methods for forming the organic thin film include dry processes (methods using the photoelectric conversion element material as is) such as a vapor deposition method in which a fused polycyclic aromatic compound represented by formula (1) is vapor-deposited onto a substrate on which the organic thin film is to be formed, and solution processes (methods using a solution in which the photoelectric conversion element material is dissolved and / or dispersed in an organic solvent, etc.) in which a fused polycyclic aromatic compound represented by formula (1) is mixed with an organic solvent, etc. to prepare a solution for the organic thin film, and the organic thin film solution is applied to a substrate to form the organic thin film. Examples of solution processes include spin coating, drop casting, dip coating, spraying, relief printing such as flexographic printing and resin relief printing, lithographic printing such as offset printing, dry offset printing and pad printing, intaglio printing such as gravure printing, stencil printing such as screen printing, mimeograph printing and ring graph printing, inkjet printing, microcontact printing, etc., and methods combining a plurality of these techniques. When forming a film by a solution process, it is preferable to evaporate the solvent after the above-mentioned coating or printing to form a thin film.

[0027] [Organic Photoelectric Conversion Element] An organic photoelectric conversion element is an element composed of an organic semiconductor material, electrodes, etc., and converts light into electricity. FIG. 1 shows an example of an organic photoelectric conversion element. An organic photoelectric conversion element 7 includes, in this order, a substrate 1, a first electrode 2, an electron blocking layer 3, a photoelectric conversion layer 4, a hole blocking layer 5, and a second electrode 6. The organic photoelectric conversion element 7 is characterized in that the photoelectric conversion layer 4 has an organic thin film containing the above-mentioned photoelectric conversion element material as a hole transport material. The organic photoelectric conversion element of the present invention is not limited to the structure shown in FIG. 1, and layers can be added or omitted as necessary.

[0028] - Substrate 1 - The substrate 1 is a member that supports the organic photoelectric conversion element 7. There are no particular limitations on the material of the substrate 1, and for example, a substrate made of glass, transparent plastic, quartz, or the like can be used. Note that, when light is incident from the second electrode 6 side in FIG. 1, the substrate 1 does not necessarily have to be transparent. Here, "having transparency" means having excellent transmittance for light of a specific wavelength to be converted into current. Furthermore, a further substrate may be disposed outside the second electrode 6, but at least one of the substrate 1 and the substrate outside the second electrode 6 must be transparent.

[0029] - First electrode 2, second electrode 6 - The first electrode 2 and the second electrode 6 have the function of collecting holes and electrons generated in the photoelectric conversion layer 4. Since they also need the function of allowing light to enter the photoelectric conversion layer 4, at least one of the first electrode 2 and the second electrode 6 needs to be transparent. There are no particular limitations on the material of the first electrode 2 and the second electrode 6 as long as it is conductive, but examples thereof include ITO, IZO, SnO 2 , ATO (antimony-doped tin oxide), ZnO, AZO (Al-doped zinc oxide), GZO (gallium-doped zinc oxide), TiO 2 Examples of the conductive material include transparent conductive materials such as FTO, metals such as gold, silver, platinum, chromium, aluminum, iron, cobalt, nickel, and tungsten, inorganic conductive materials such as copper iodide and copper sulfide, and conductive polymers such as polythiophene, polypyrrole, and polyaniline. The first electrode 2 and the second electrode 6 may be composed of a mixture of two or more of these materials as needed, or may be composed of two or more layers stacked together.

[0030] - Electron Blocking Layer 3 - The electron blocking layer 3 is provided to suppress dark current that occurs when electrons are injected from one electrode into the photoelectric conversion layer 4 when a bias voltage is applied between the two electrodes. The electron blocking layer 3 also functions as a hole transport layer that transports holes generated by charge separation in the photoelectric conversion layer 4 to the electrode. The electron blocking layer 3 can be arranged as a single layer or multiple layers as needed.

[0031] The electron blocking layer 3 may contain a P-type organic semiconductor material, which is a hole-transporting material. The P-type organic semiconductor material may be a material for a photoelectric conversion element containing the fused polycyclic aromatic compound represented by the above formula (1), or may be another P-type organic semiconductor material.

[0032] Other p-type organic semiconductor materials that can be used include, for example, compounds having a condensed polycyclic aromatic group such as naphthalene, anthracene, phenanthrene, pyrene, chrysene, naphthacene, triphenylene, perylene, fluoranthene, fluorene, and indene; compounds having a π-electron-rich aromatic group such as cyclopentadiene derivatives, furan derivatives, thiophene derivatives, pyrrole derivatives, benzofuran derivatives, benzothiophene derivatives, dinaphthothienothiophene derivatives, indole derivatives, pyrazoline derivatives, dibenzofuran derivatives, dibenzothiophene derivatives, carbazole derivatives, and indolocarbazole derivatives; and aromatic amine derivatives, styrylamine derivatives, benzidine derivatives, porphyrin derivatives, phthalocyanine derivatives, and quinacridone derivatives.

[0033] Photoelectric Conversion Layer 4 The photoelectric conversion layer 4 is a layer in which holes and electrons are generated by charge separation of excitons generated by incident light. The photoelectric conversion layer 4 may be formed solely of a photoelectric conversion material, or may be formed in combination with a P-type organic semiconductor material, which is a hole-transporting material, or an N-type organic semiconductor material, which is an electron-transporting material. Two or more P-type organic semiconductor materials may be used, or two or more N-type organic semiconductor materials may be used. It is desirable that one or more of the photoelectric conversion material, P-type organic semiconductor material, and N-type organic semiconductor material contained in the photoelectric conversion layer 4 contain a dye material that has the function of absorbing light of a desired wavelength in the visible region. In a preferred embodiment, a material for a photoelectric conversion element containing a fused polycyclic aromatic compound represented by formula (1) is used as the P-type organic semiconductor material, which is a hole-transporting material.

[0034] The photoelectric conversion material may be any material that generates excitons in response to incident light, and examples of the photoelectric conversion material that can be used include compounds having a condensed polycyclic aromatic group such as naphthalene, anthracene, phenanthrene, pyrene, chrysene, naphthacene, triphenylene, perylene, fluoranthene, fluorene, and indene; compounds having a π-electron-rich aromatic group such as cyclopentadiene derivatives, furan derivatives, thiophene derivatives, pyrrole derivatives, benzofuran derivatives, benzothiophene derivatives, dinaphthothienothiophene derivatives, indole derivatives, pyrazoline derivatives, dibenzofuran derivatives, dibenzothiophene derivatives, carbazole derivatives, and indolocarbazole derivatives; aromatic amine derivatives, styrylamine derivatives, benzidine derivatives, porphyrin derivatives, phthalocyanine derivatives, and quinacridone derivatives. From the viewpoint of the utilization efficiency of incident light, a material with a high absorption coefficient is preferred, and for example, pyrromethene derivatives, porphyrin derivatives, subporphyrin derivatives, phthalocyanine derivatives, subphthalocyanine derivatives, quinacridone derivatives, pyrrolopyrrole derivatives, coumarin derivatives, perylene derivatives, and aromatic amine derivatives can be used.

[0035] When the above-mentioned photoelectric conversion element material is used as a P-type organic semiconductor material, it may be used in combination with other P-type organic semiconductor materials, or two or more of the above-mentioned photoelectric conversion element materials may be used. Examples of other P-type organic semiconductor materials include compounds having a condensed polycyclic aromatic group such as naphthalene, anthracene, phenanthrene, pyrene, chrysene, naphthacene, triphenylene, perylene, fluoranthene, fluorene, and indene, cyclopentadiene derivatives, furan derivatives, thiophene derivatives, pyrrole derivatives, benzofuran derivatives, benzothiophene derivatives, dinaphthothienothiophene derivatives, indole derivatives, pyrazoline derivatives, dibenzofuran derivatives, dibenzothiophene derivatives, carbazole derivatives, and compounds having a π-electron-rich aromatic group such as indolocarbazole derivatives, aromatic amine derivatives, styrylamine derivatives, benzidine derivatives, porphyrin derivatives, phthalocyanine derivatives, and quinacridone derivatives. Examples of polymeric P-type organic semiconductor materials include polyphenylene vinylene derivatives, polyparaphenylene derivatives, polyfluorene derivatives, polyvinyl carbazole derivatives, and polythiophene derivatives. The polymeric P-type organic semiconductor material may be mixed with the photoelectric conversion element material of the present invention or a non-polymeric P-type organic semiconductor material, or two or more polymeric P-type organic semiconductor materials may be mixed and used.

[0036] The N-type organic semiconductor material may be any material having electron transport properties, and examples thereof include naphthalene tetracarboxylic acid diimide, perylene tetracarboxylic acid diimide, fullerenes, and azole derivatives such as imidazole, thiazole, thiadiazole, oxazole, oxadiazole, and triazole. One or more selected from these N-type organic semiconductor materials may be used alone or in combination.

[0037] -Hole Blocking Layer 5- The hole blocking layer 5 is provided to suppress dark current generated when holes are injected from one electrode into the photoelectric conversion layer 4 when a bias voltage is applied between the two electrodes. The hole blocking layer 5 also functions as an electron transport layer that transports electrons generated by charge separation in the photoelectric conversion layer 4 to the electrode. The hole blocking layer 5 may have a single layer or multiple layers as necessary. The hole blocking layer 5 can be made of an N-type organic semiconductor material having electron transport properties. The N-type organic semiconductor material may be any material having electron transport properties, and examples thereof include polycyclic aromatic polycarboxylic anhydrides such as naphthalene tetracarboxylic diimide and perylene tetracarboxylic diimide, and imidized products thereof; fullerenes such as C60 and C70; azole derivatives such as imidazole, thiazole, thiadiazole, oxazole, oxadiazole, and triazole; tris(8-quinolinolato)aluminum(III) derivatives; phosphine oxide derivatives; nitro-substituted fluorene derivatives; diphenylquinone derivatives; thiopyran dioxide derivatives; carbodiimide; fluorenylidenemethane derivatives; anthraquinodimethane and anthrone derivatives; bipyridine derivatives; quinoline derivatives; and indolocarbazole derivatives. One or more of these N-type organic semiconductor materials may be used alone or in combination.

[0038] The organic photoelectric conversion element 7 can be used in solar cells, optical sensors, image sensors, photocounters, LIDAR, and the like.

[0039] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" means parts by mass, "M" means molar concentration, and "%" means mass %. The structures of the compounds described in the synthesis examples were determined by mass spectrometry (FAB-MS) and nuclear magnetic resonance spectrometry (NMR) as necessary. 1 H-NMR spectra were measured using Avance 400 or Avance 500 (Bruker), FAB-MS spectra were measured using JMS-700 (JEOL), and absorption spectra were measured using UV-3600 (SHIMADZU).

[0040] Example 1 Synthesis of Compound (1-1) (Step 1-1) Synthesis of an intermediate compound represented by the following formula (M1-1) Under a nitrogen atmosphere, 4-bromo-4'-iodobiphenyl (30.0 parts, 83.8 mmol), 3-thiopheneboronic acid (11.8 parts, 92.2 mmol), and potassium carbonate (57.8 parts, 419 mmol) were added to a mixture of toluene (215 mL), tetrahydrofuran (215 mL), and water (107 mL) and stirred. Tetrakistriphenylphosphine palladium (3.40 parts, 2.94 mmol) was added thereto, and the reaction solution was heated and stirred under reflux. After 6 hours, the reaction solution was cooled to room temperature, and the precipitated solid was collected by suction filtration. The solid was washed with water and ethanol and dried in a dryer to obtain the compound represented by formula (M1-1) (yield 23.0 parts, 86%) as a white solid. The mass spectrometry measurement results for the compound represented by formula (M1-1) were as follows: FAB-MS: m / z=315 [M+H] +

[0041] (Step 1-2) Synthesis of an intermediate compound represented by the following formula (M1-2) Under a nitrogen atmosphere, the compound represented by formula (M1-1) obtained in step 1-1 (22.0 parts, 70.0 mmol), bis(pinacolato)diboron (21.4 parts, 84.0 mmol), and potassium acetate (16.5 parts, 168 mmol) were added to a 1,4-dioxane (350 mL) solution and stirred. [1,1'-bis(diphenylphosphino)ferrocene]dichloropalladium(II) (2.86 parts, 3.50 mmol) was added thereto, and the reaction solution was heated to 100°C. After 8 hours, the reaction solution was cooled to room temperature, water and toluene were added, the mixture was separated, and extracted with toluene. The resulting organic layer was dried over anhydrous magnesium sulfate and filtered, and the organic solvent was then distilled off by concentration under reduced pressure. The resulting residue was purified by silica gel column chromatography (solvent: toluene) to obtain the compound represented by formula (M1-2) (yield: 18.5 parts, 73%) as a white solid. The mass spectrometry measurement results for the compound represented by formula (M1-2) were as follows: FAB-MS: m / z=363 [M+H] +

[0042] (Step 1-3) Synthesis of Compound (1-1) Under a nitrogen atmosphere, diiodoBTBT (1.80 parts, 3.68 mmol) synthesized by the method described in Japanese Patent No. 4945757, the compound represented by formula (M1-2) obtained in step 1-2 (3.20 parts, 8.84 mmol), and tripotassium phosphate (2.73 parts, 12.9 mmol) were added to DMF (200 parts) and stirred. Tetrakis(triphenylphosphine)palladium (0.213 parts, 0.184 mmol) was added thereto, and the reaction solution was heated to 90°C and stirred for 3 hours. After completion of the reaction, the reaction solution was cooled to room temperature, water was added, and the precipitated solid was collected by suction filtration. The obtained solid was washed with water and acetone and dried in a dryer. The obtained solid was further purified by vacuum sublimation to obtain compound (1-1) of the present invention (1.56 parts, yield 60%) as a yellow crystalline solid.

[0043]

[0044] Example 2: Synthesis of Compound (1-2) (Step 2-1) Synthesis of an intermediate compound represented by the following formula (M2-1) Under a nitrogen atmosphere, 6-bromo-2-naphthol (10.0 parts, 44.8 mmol), 3-thiopheneboronic acid (6.90 parts, 53.8 mmol), and sodium carbonate (14.2 parts, 134 mmol) were added to a mixture of toluene (120 mL), ethanol (80 mL), and water (40 mL) and stirred. Tetrakistriphenylphosphine palladium (3.40 parts, 2.94 mmol) was added thereto, and the reaction solution was heated and stirred under reflux. After 6 hours, the reaction solution was cooled to room temperature and acidified (pH = 2) by adding dilute hydrochloric acid, and the precipitated solid was collected by suction filtration. The solid was washed with water and ethanol and dried in a dryer to obtain the compound represented by formula (M2-1) (yield 7.53 parts, 74%) as a white solid. The mass spectrometry measurement results for the compound represented by formula (M2-1) were as follows: FAB-MS: m / z=227 [M+H] +

[0045] (Step 2-2) Synthesis of an intermediate compound represented by the following formula (M2-2) Under a nitrogen atmosphere, the compound represented by formula (M2-1) obtained in step 2-1 (3.84 parts, 17.0 mmol) and pyridine (2.74 mL, 34.0 mmol) were added to a dichloromethane (200 mL) solution, cooled to 0°C in an ice bath, and stirred. Trifluoromethanesulfonic anhydride (5.75 parts, 20.4 mmol) was slowly added dropwise thereto, and the reaction solution was warmed to room temperature. After 3 hours, the reaction solution was treated with a saturated aqueous ammonium chloride solution and extracted with dichloromethane. The resulting organic layer was dried over anhydrous magnesium sulfate and filtered, and the organic solvent was then distilled off by concentration under reduced pressure. The resulting residue was purified by silica gel column chromatography (solvent: toluene / hexane) to obtain the compound represented by formula (M2-2) (yield 5.40 parts, 89%) as a white solid. The mass spectrometry measurement results for the compound represented by formula (M2-2) were as follows. FAB-MS: m / z=359 [M+H] +

[0046] (Step 2-3) Synthesis of intermediate compound represented by the following formula (M2-3) The synthesis of the intermediate compound represented by formula (M2-3) was carried out in accordance with step 1-2, except that the compound represented by formula (M2-2) obtained in step 2-2 (5.40 parts, 15.1 mmol) was used instead of the intermediate compound represented by formula (M1-1), and the same operation was carried out to obtain the intermediate compound represented by formula (M2-3) (yield 3.40 parts, 67%) as a white solid. The mass spectrometry measurement results of the compound represented by formula (M2-3) were as follows. FAB-MS: m / z = 493 [M+H] +

[0047] (Step 2-4) Synthesis of Compound (1-2) Compound (1-2) was synthesized in accordance with Step 1-3, except that the compound represented by formula (M2-3) (2.30 parts, 6.84 mmol) obtained in Step 2-3 was used instead of the intermediate compound represented by formula (M1-2). The compound (1-2) of the present invention (yield 1.25 parts, 64%) was synthesized as a yellow solid.

[0048]

[0049] Example 3: Synthesis of Compound (1-4) (Step 3-1) Synthesis of an intermediate compound represented by the following formula (M3-1) Under a nitrogen atmosphere, 1-bromo-4-iodobenzene (20.0 parts, 70.9 mmol) and 3-thiopheneboronic acid (9.50 parts, 74.5 mmol) were added to a mixture of toluene (150 mL), ethanol (25 mL), and 2 M potassium carbonate (71 mL) and stirred. Tetrakistriphenylphosphine palladium (2.05 parts, 1.77 mmol) was added thereto, and the reaction solution was heated and stirred under reflux. After 6 hours, the reaction solution was cooled to room temperature and diluted with 100 mL of water. The organic layer was extracted with toluene, and the resulting organic layer was dried over anhydrous magnesium sulfate, and the solid was removed by suction filtration. The organic solution was concentrated under reduced pressure, and the resulting solid was washed with water and methanol and dried in a dryer to obtain the compound represented by formula (M3-1) (yield 15.2 parts, 89%) as a white solid. The mass spectrometry measurement results for the compound represented by formula (M3-1) were as follows: FAB-MS: m / z=241 [M+H] +

[0050] (Step 3-2) Synthesis of intermediate compound represented by the following formula (M3-2) The synthesis of the intermediate compound represented by formula (M3-2) was carried out in accordance with step 1-2, except that the compound represented by formula (M3-1) obtained in step 3-1 (13.0 parts, 54.2 mmol) was used instead of the intermediate compound represented by formula (M1-1), and the same operation was carried out to obtain the intermediate compound represented by formula (M3-2) (yield 12.7 parts, 82%) as a white solid. The mass spectrometry measurement results of the compound represented by formula (M3-2) were as follows. FAB-MS: m / z = 287 [M+H] +

[0051] (Step 3-3) Synthesis of an intermediate compound represented by the following formula (M3-3) Under a nitrogen atmosphere, diiodoBTBT (1.22 parts, 2.48 mmol), the compound represented by formula (M3-2) obtained in step 3-2 (0.851 parts, 2.98 mmol), and tripotassium phosphate (1.05 parts, 4.96 mmol) were added to DMF (200 parts) and stirred. Tetrakis(triphenylphosphine)palladium (0.143 parts, 0.124 mmol) was added thereto, and the reaction solution was heated to 90 °C and stirred for 3 hours. After completion of the reaction, the reaction solution was cooled to room temperature, water was added, and the precipitated solid was collected by suction filtration. The obtained solid was washed with water and acetone and dried in a dryer. The obtained crude intermediate compound represented by formula (M3-3) (1.17 parts) was used in the next reaction without further purification.

[0052] (Step 3-4) Synthesis of Compound (1-4) Under a nitrogen atmosphere, the compound represented by formula (M3-3) obtained in step 3-3 (1.17 parts), the compound represented by formula (M1-2) obtained in step 1-2 (1.08 parts, 2.98 mmol), and tripotassium phosphate (1.05 parts, 4.96 mmol) were added to DMF (200 parts) and stirred. Tetrakis(triphenylphosphine)palladium (0.143 parts, 0.124 mmol) was added thereto, and the reaction solution was heated to 90°C and stirred for 3 hours. After completion of the reaction, the reaction solution was cooled to room temperature, water was added, and the precipitated solid was collected by suction filtration. The obtained solid was washed with water and acetone and dried in a dryer. The obtained solid was further purified by vacuum sublimation to obtain compound (1-4) of the present invention (0.628 parts, two-stage yield 40%) as a yellow crystalline solid.

[0053]

[0054] [Example 4: Synthesis of compound (1-22)]

[0055] (Step 4-1) Synthesis of an intermediate compound represented by the following formula (M4-1) Under a nitrogen atmosphere, diiodoBTBT (1.02 parts, 2.07 mmol), 3-thiopheneboronic acid (0.344 parts, 2.69 mmol), and tripotassium phosphate (1.31 parts, 6.21 mmol) were added to DMF (180 parts) and stirred. Tetrakis(triphenylphosphine)palladium (0.109 parts, 0.104 mmol) was added thereto, and the reaction solution was heated to 90°C and stirred for 1 hour. After completion of the reaction, the reaction solution was cooled to room temperature, water was added, and the precipitated solid was collected by suction filtration. The obtained solid was washed with water and acetone and dried in a dryer. The obtained crude intermediate compound represented by formula (M4-1) (0.902 parts) was used in the next reaction without further purification.

[0056] (Step 4-2) Synthesis of Compound (1-22) Under a nitrogen atmosphere, the compound represented by formula (M4-1) obtained in step 4-1 (0.902 parts), the compound represented by formula (M1-2) obtained in step 1-2 (0.976 parts, 2.69 mmol), and tripotassium phosphate (1.31 parts, 6.21 mmol) were added to DMF (parts) and stirred. Tetrakis(triphenylphosphine)palladium (0.109 parts, 0.104 mmol) was added thereto, and the reaction solution was heated to 90°C and stirred for 3 hours. After completion of the reaction, the reaction solution was cooled to room temperature, water was added, and the precipitated solid was collected by suction filtration. The obtained solid was washed with water and acetone and dried in a dryer. The obtained solid was further purified by vacuum sublimation to obtain compound (1-22) of the present invention (0.369 parts, two-stage yield 32%) as a yellow crystalline solid.

[0057]

[0058] Comparative Examples 1 to 5: Synthesis of Comparative Compounds (2-1) to (2-5) The following comparative compounds (2-1) to (2-5) were synthesized using known methods.

[0059]

[0060] (Measurement of HOMO Level Energy of Organic Thin Film) Each of the organic compounds obtained in Examples 1 to 4 and Comparative Examples 1 to 5 was subjected to resistance heating vacuum deposition on a pre-cleaned glass substrate to prepare an organic thin film (film thickness: 100 nm) of each compound. The HOMO level energy of each obtained organic thin film was determined by photoelectron spectroscopy (AC-3, Riken Keiki Co., Ltd.). The HOMO level energy of the organic thin film of each compound is shown in Table 1.

[0061]

[0062] From these results, it can be said that the organic thin film prepared using the compound of the present invention has a lower HOMO level energy than the organic thin films prepared using each of the comparative compounds except for the comparative compound (2-5), and is highly likely to be effective in suppressing dark current when used in a photoelectric conversion element. While the comparative compound (2-5) has a low HOMO level energy, it has low crystallinity due to its twisted structure, and the intermolecular interactions in the thin film are reduced, so a decrease in EQE is expected. Below, photoelectric conversion elements were actually prepared and examined.

[0063] Example 5: Preparation of photoelectric conversion element A On a glass substrate on which an electrode made of ITO with a film thickness of 70 nm was formed, an electron blocking layer was formed by depositing a photoelectric conversion element A at a substrate temperature of room temperature and a vacuum degree of 4.0×10 -5 A film of CzBDF (manufactured by Tokyo Chemical Industry Co., Ltd.) was formed to a thickness of 10 nm under the conditions of 0.05 Pa. Next, as a photoelectric conversion layer, the compound (1-1) obtained in Example 1, Cl 6 -SubPc-OPh (manufactured by Lumitec) and fullerene (C60, manufactured by Tokyo Chemical Industry Co., Ltd.) were co-deposited at a deposition rate ratio of 4:4:2 to form an organic thin film with a thickness of 230 nm. Subsequently, a commonly available dpy-NDI (manufactured by Tokyo Chemical Industry Co., Ltd.) was deposited to a thickness of 10 nm to form a hole-blocking layer. Finally, an aluminum film was deposited to a thickness of 100 nm as an electrode to prepare photoelectric conversion element A.

[0064]

[0065] [Examples 6 to 8: Preparation of photoelectric conversion elements B to D] Photoelectric conversion elements B to D were prepared by the same procedure as in Example 5, except that compound (1-2) obtained in Example 2, compound (1-4) obtained in Example 3, and compound (1-22) obtained in Example 4 were used instead of compound (1-1).

[0066] Comparative Examples 6 to 10: Preparation of Photoelectric Conversion Elements P to T Comparative photoelectric conversion elements P to T were prepared by the same procedure as in Example 5, except that comparative compound (2-1), comparative compound (2-2), comparative compound (2-3), comparative compound (2-4), and comparative compound (2-5) were used instead of the compound represented by compound (1-1).

[0067] (Evaluation of Organic Photoelectric Conversion Elements) Photoelectric conversion elements were evaluated based on the examples of WO2018-105269. Specifically, for each of photoelectric conversion elements A to D and P to T, 2.0 × 10 5 A voltage was applied to achieve an intensity of 1000 V / cm, and the EQE and dark current of the photoelectric conversion at 550 nm were measured. The results are shown in Table 2. Evaluation criteria: EQE: 85% or more: "○", 80% or more but less than 85%: "△", less than 80%: "X", Dark current: 5.0×10 -11 A / cm 2 If less than 5.0 x 10: "○" -11 Above 1.0 x 10 -10 A / cm 2 If less than 1.0 x 10: "△" -10 A / cm 2 In the above cases: "X" In practice, the larger the EQE, the more efficiently the irradiated light can be converted into electrical energy, so "O" means superior and "X" means inferior. The smaller the dark current, the more the current value when light irradiation is turned off can be suppressed, so "O" means superior and "X" means inferior.

[0068]

[0069] (Evaluation of response speed) The response was evaluated based on the example of WO2018 / 105269. Specifically, each of the obtained photoelectric conversion elements was subjected to 2.0 × 10 5 A voltage was applied to the device so that the intensity was 100 V / cm. Then, the LED (light-emitting diode) was momentarily turned on, and light was irradiated from the lower electrode on the transparent conductive film (ITO) side. The photocurrent at that time was measured with an oscilloscope, and the rise time from 0 to 97% signal intensity was measured. The rise time of the device in Comparative Example 6 was then determined relative to that of Comparative Example 6, which was defined as 1. The results are shown in Table 3. Evaluation criteria: Relative rise time compared to Comparative Example 6: Less than 0.1: "AA" 0.1 or more but less than 0.2: "A" 0.2 or more but less than 0.4: "B" 0.4 or more but less than 0.6: "C" 0.6 or more: "D" In practice, it is desirable for the photoelectric conversion device to have a fast photoresponse speed, i.e., for the photocurrent value to approach 100% in a short time after exposure to light. Therefore, "AA" indicates the best, and "D" indicates the worst.

[0070]

[0071] The results in Tables 2 and 3 show that the photoelectric conversion elements of Examples 5 to 8 not only exhibited good EQE and dark current values, but also had excellent response speeds. In particular, the dark current and response speeds were generally good results compared to the comparative examples. On the other hand, the photoelectric conversion elements of Comparative Examples 6 to 10 were inferior in at least one of the EQE, dark current values, and response speeds.

[0072] By using the fused polycyclic aromatic compound represented by formula (1), it is possible to provide an organic semiconductor device (photoelectric conversion element, optical sensor) that has a high EQE, suppresses dark current, and is excellent in response speed.

[0073] REFERENCE SIGNS LIST 1 Substrate 2 First electrode 3 Electron blocking layer 4 Photoelectric conversion layer 5 Hole blocking layer 6 Second electrode 7 Organic photoelectric conversion element

Claims

1. The following formula (1) (In formula (1), X and Y each independently represent a divalent aromatic hydrocarbon group or a single bond, excluding the cases where X and Y are both divalent linking groups obtained by removing two hydrogen atoms from benzene, where X and Y are both single bonds, and where one of X and Y is a divalent linking group obtained by removing two hydrogen atoms from benzene and the other is a single bond).

2. The condensed polycyclic aromatic compound according to claim 1, wherein X and Y are the same.

3. The condensed polycyclic aromatic compound according to claim 1, wherein X and Y are different from each other.

4. The condensed polycyclic aromatic compound according to any one of claims 1 to 3, wherein X and Y are each independently a divalent linking group formed by removing two hydrogen atoms from benzene, biphenyl, or naphthalene.

5. A material for photoelectric conversion devices containing the condensed polycyclic aromatic compound according to claim 1.

6. An organic thin film comprising the condensed polycyclic aromatic compound according to claim 1 or the material for a photoelectric conversion device according to claim 5.

7. An organic photoelectric conversion element having the organic thin film according to claim 6.

Citation Information

Patent Citations

  • OLED electronic transport layer material and preparation method and application thereof

    CN107936038A

  • Photoelectric conversion element material for imaging device and photoelectric conversion element containing the same

    JP2018078270A

  • Photoelectric conversion element for imaging element

    JP2019050398A

  • P active materials for organic photoelectric conversion layers in organic photodiodes

    JP2021500757A