Plasticizer, method for producing same, and thermoplastic resin composition

A (meth)acrylic polymer with specific molecular and SP value characteristics is used to enhance the cold resistance and weatherability of thermoplastic resin compositions, addressing the limitations of phthalate esters by ensuring compatibility and preventing volatilization, thus maintaining the integrity of molded articles in low-temperature conditions.

WO2024242177A1PCT designated stage expired Publication Date: 2024-11-28TOAGOSEI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019072
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Thermoplastic resin compositions using phthalate esters as plasticizers face issues with long-term weather resistance and cold resistance, as the phthalate esters are released over time, leading to loss of flexibility and brittleness, especially in low-temperature environments.

Method used

A (meth)acrylic polymer with a weight average molecular weight of 1,650 or less, an SP value of 9.50 or more, and a glass transition temperature of -77°C or less is used as a plasticizer, which is produced by polymerizing monomers in a solvent containing a primary alcohol at temperatures between 180°C and 350°C, enhancing compatibility and cold resistance when blended with thermoplastic resins.

Benefits of technology

The use of this (meth)acrylic polymer as a plasticizer results in a molded article with improved cold resistance and weatherability, maintaining flexibility and strength over time, even in low-temperature environments, while preventing the plasticizer from volatilizing during heat molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This plasticizer contains a (meth)acrylic polymer including a structural unit derived from a (meth)acrylic acid alkyl ester. The (meth)acrylic polymer has a weight average molecular weight of 1,650 or less, an SP value of 9.50 or more, and a glass transition temperature of -77°C or less.
Need to check novelty before this filing date? Find Prior Art

Description

Plasticizer, method for producing same, and thermoplastic resin composition

[0001] [CROSS-REFERENCE TO RELATED APPLICATIONS] This application claims priority to Japanese Patent Application No. 2023-86436, filed on May 25, 2023, the entire contents of which are incorporated herein by reference. The present disclosure relates to a plasticizer and a method for producing the same, and a thermoplastic resin composition.

[0002] Plasticizers are generally used to soften thermoplastic resins such as vinyl chloride resins and ABS resins. Phthalate esters such as dioctyl phthalate and diisononyl phthalate have been widely known as plasticizers. However, when a molded article is produced by blending a phthalate ester with a thermoplastic resin, the phthalate ester in the molded article is released over time, causing the resin to lose flexibility over time, and the molded article may not be able to maintain its weather resistance for a long period of time. In light of this, it has been proposed to use a relatively low-molecular-weight (meth)acrylic polymer as a plasticizer to ensure compatibility with the thermoplastic resin while improving the weather resistance of the molded article obtained by combining the thermoplastic resin with the polymer (see, for example, Patent Documents 1 and 2).

[0003] Patent Document 1 discloses the use of an acrylic polymer obtained by polymerizing monomers at a temperature of 180 to 350° C. for 5 to 60 minutes as a plasticizer. Patent Document 2 discloses the use of a copolymer of an alkoxyalkyl (meth)acrylate and another monomer as a plasticizer.

[0004] International Publication No. WO 2001 / 83619 International Publication No. WO 2002 / 100943

[0005] The present inventors have found through their investigations that molded articles obtained by mixing the (meth)acrylic polymers disclosed in Patent Documents 1 and 2 with thermoplastic resins are brittle in low-temperature environments (for example, at temperatures of −10° C. or −20° C.) and are prone to breakage when subjected to impact in low-temperature environments. Furthermore, such molded articles are required to be resistant to breakage even when exposed to low-temperature environments long after production and to have excellent cold resistance.

[0006] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide a plasticizer that can be used in combination with a thermoplastic resin to obtain a molded article having excellent cold resistance.

[0007] According to the present disclosure, there are provided the following plasticizer, a method for producing the same, and a thermoplastic resin composition.

[0008] [1] A plasticizer containing a (meth)acrylic polymer containing structural units derived from a (meth)acrylic acid alkyl ester, wherein the (meth)acrylic polymer has a weight-average molecular weight of 1,650 or less, an SP value of 9.50 or more, and a glass transition temperature of -77°C or less. [2] The plasticizer according to [1], wherein the (meth)acrylic polymer has a carbon-carbon double bond content of 0.10 meq / g or more and 0.36 meq / g or less. [3] The plasticizer according to [1] or [2], wherein the (meth)acrylic polymer contains structural units derived from a (meth)acrylic acid alkyl ester having an alkyl group having 3 or more carbon atoms in an amount of 40% by mass or more, based on the total structural units of the (meth)acrylic polymer. [4] A method for producing the plasticizer according to any one of [1] to [3], comprising a step of polymerizing a monomer in a solvent containing a primary alcohol to obtain the (meth)acrylic polymer. [5] A method for producing the plasticizer according to [4], wherein the primary alcohol is normal butanol or 2-ethylhexanol. [6] A method for producing the plasticizer according to [4] or [5], wherein the polymerization temperature is within a temperature range of 180° C. or higher and 350° C. or lower. [7] A thermoplastic resin composition containing the plasticizer according to any one of [1] to [3] or the plasticizer obtained by the production method according to any one of [4] to [6], and a thermoplastic resin.

[0009] By mixing the plasticizer of the present disclosure with a thermoplastic resin and molding the mixture, a molded article with excellent cold resistance can be obtained.

[0010] The present disclosure will be described in detail below. In this specification, "(meth)acrylic" means acrylic and / or methacrylic, "(meth)acrylate" means acrylate and / or methacrylate, and "(meth)acrylo" means acrylo and / or methacrylo.

[0011] The plasticizer of the present disclosure contains a (meth)acrylic polymer (hereinafter also referred to as "(meth)acrylic polymer (P)") containing structural units derived from a (meth)acrylic acid alkyl ester. The (meth)acrylic polymer (P) has a weight-average molecular weight of 1,650 or less, an SP value of 9.50 or more, and a glass transition temperature of -77°C or less.

[0012] (Molecular Weight Characteristics of Polymer) If the weight average molecular weight (Mw) of the (meth)acrylic polymer used as the plasticizer exceeds 1,650, the molded article obtained by combining it with a thermoplastic resin will have poor cold resistance. From the viewpoint of obtaining a molded article with excellent cold resistance, the Mw of the (meth)acrylic polymer (P) is preferably 1,600 or less, more preferably 1,550 or less, even more preferably 1,500 or less, and even more preferably 1,450 or less. There are no particular restrictions on the lower limit of the Mw of the (meth)acrylic polymer (P), but from the viewpoint of suppressing volatilization of the plasticizer during heat molding of the thermoplastic resin and from the viewpoint of obtaining a molded article with good weather resistance, it is preferably 500 or more, more preferably 600 or more, and even more preferably 1,000 or more.

[0013] The number average molecular weight (Mn) of the (meth)acrylic polymer (P) is preferably 1,500 or less, more preferably 1,450 or less, even more preferably 1,400 or less, and even more preferably 1,300 or less. The lower limit of Mn of the (meth)acrylic polymer (P) is, for example, 500 or more, preferably 600 or more, and more preferably 800 or more. In this specification, the molecular weight of the polymer is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0014] The molecular weight distribution (Mw / Mn) of the (meth)acrylic polymer (P), which is the ratio of Mw to Mn, is preferably 1.60 or less, and more preferably 1.50 or less, from the viewpoint of enhancing the effect of plasticizing the thermoplastic resin. The lower limit of Mw / Mn of the (meth)acrylic polymer (P) is not particularly limited, and can be 1.0 or more.

[0015] (SP Value of Polymer) When the SP value of the (meth)acrylic polymer used as a plasticizer is less than 9.50, the plasticizer has poor compatibility with thermoplastic resins. From the viewpoints of improving the compatibility between the (meth)acrylic polymer (P) and the thermoplastic resin, imparting sufficient flexibility to the thermoplastic resin composition, and obtaining a molded article with excellent cold resistance, the SP value of the (meth)acrylic polymer (P) is preferably 9.51 or more, more preferably 9.52 or more. There are no particular restrictions on the upper limit of the SP value of the (meth)acrylic polymer (P), but from the viewpoint of improving compatibility with the thermoplastic resin, it may be, for example, 11.0 or less, or 10.0 or less. In this specification, the SP value of the polymer is a value calculated by the Fedors method (unit: [cal / cm 3 ] 1/2 )

[0016] (Glass Transition Temperature of Polymer) If the glass transition temperature (Tg) of the (meth)acrylic polymer used as the plasticizer is higher than -77°C, a molded article obtained using a resin composition containing the plasticizer and a thermoplastic resin will have poor cold resistance. From the viewpoint of obtaining a molded article with excellent cold resistance, the Tg of the (meth)acrylic polymer (P) is preferably -78°C or lower. There are no particular restrictions on the lower limit of the Tg of the (meth)acrylic polymer (P), but from the viewpoint of easy availability of raw materials, it is, for example, -90°C or higher. In this specification, the Tg of the polymer is a value obtained using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min in a nitrogen atmosphere. Details of the measurement conditions are as described in the Examples below.

[0017] (Amount of Carbon-Carbon Double Bonds in Polymer) It is preferable that at least a portion of the polymers constituting the (meth)acrylic polymer (P) have a terminal carbon-carbon double bond. When at least a portion of the (meth)acrylic polymer (P) has a terminal carbon-carbon double bond, the compatibility of the (meth)acrylic polymer (P) with thermoplastic resins can be further improved. From the viewpoint of improving the compatibility of the (meth)acrylic polymer (P) with thermoplastic resins, the content of carbon-carbon double bonds in the (meth)acrylic polymer (P) (hereinafter also referred to as "double bond concentration") is preferably 0.10 meq / g or more, more preferably 0.15 meq / g or more. The upper limit of the double bond concentration is preferably 0.36 meq / g or less, more preferably 0.35 meq / g or less, even more preferably 0.32 meq / g or less, and even more preferably 0.30 meq / g or less, from the viewpoint of ensuring weather resistance in a molded article of a thermoplastic resin containing a plasticizer. 1 It is a value calculated from the amount of double bonds in the polymer determined by H-NMR measurement and the composition of the polymer. Details of the measurement method follow the method described in the Examples below.

[0018] (Viscosity of Polymer) From the viewpoint of enhancing the plasticizing effect, the viscosity of the (meth)acrylic polymer (P) is preferably 1,500 mPa s or less, more preferably 800 mPa s or less, and even more preferably 600 mPa s or less. There are no particular restrictions on the lower limit of the viscosity of the (meth)acrylic polymer (P). However, from the viewpoint of suppressing bleed-out of the (meth)acrylic polymer (P) in a molded article produced from a thermoplastic resin composition containing the (meth)acrylic polymer (P), the viscosity is usually preferably 100 mPa s or more, more preferably 120 mPa s or more. In this specification, the viscosity of the polymer is a value measured at 25°C using a B-type viscometer.

[0019] (Structural Unit of Polymer) Next, the structural unit of the (meth)acrylic polymer (P) exhibiting the above-mentioned physical properties will be described. The (meth)acrylic polymer (P) contains a structural unit derived from a (meth)acrylic acid alkyl ester.

[0020] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, and eicosyl (meth)acrylate.

[0021] In the (meth)acrylic polymer (P), the content of structural units derived from a (meth)acrylic acid alkyl ester is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on the total structural units of the (meth)acrylic polymer (P), from the viewpoint of sufficiently enhancing the plasticizing effect of the (meth)acrylic polymer (P) and from the viewpoint of improving the weather resistance of a molded article obtained by combining the (meth)acrylic polymer (P) with a thermoplastic resin. Note that, as the (meth)acrylic acid alkyl ester constituting the (meth)acrylic polymer (P), one type may be used alone, or two or more types may be used in combination.

[0022] From the viewpoint of improving the cold resistance of a molded article obtained by using the (meth)acrylic polymer (P) in combination with a thermoplastic resin, the (meth)acrylic acid alkyl ester constituting the (meth)acrylic polymer (P) preferably contains a (meth)acrylic acid alkyl ester having an alkyl group having 3 or more carbon atoms.

[0023] In the (meth)acrylic polymer (P), from the viewpoint of obtaining a molded product having excellent cold resistance, the content of structural units derived from a (meth)acrylic acid alkyl ester having an alkyl group having 3 or more carbon atoms is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, still more preferably 40% by mass or more, still more preferably 50% by mass or more, even more preferably 60% by mass or more, and still more preferably 70% by mass or more, based on all structural units of the (meth)acrylic polymer (P).

[0024] As the (meth)acrylic acid alkyl ester constituting the (meth)acrylic polymer (P), among the above, a (meth)acrylic acid alkyl ester having 3 to 14 carbon atoms can be preferably used, and a (meth)acrylic acid alkyl ester having 4 to 12 carbon atoms can be more preferably used, in that it can give a polymer excellent in cold resistance and weather resistance.

[0025] Moreover, from the viewpoint of being able to sufficiently lower the glass transition temperature of the (meth)acrylic polymer (P), an acrylic acid alkyl ester can be preferably used as a monomer constituting the (meth)acrylic polymer (P). In the (meth)acrylic polymer (P), the content of structural units derived from the acrylic acid alkyl ester is preferably 40 mass% or more, more preferably 50 mass% or more, even more preferably 60 mass% or more, still more preferably 70 mass% or more, even more preferably 80 mass% or more, and still more preferably 90 mass% or more, based on the total structural units of the (meth)acrylic polymer (P).

[0026] In terms of being able to sufficiently lower the glass transition temperature of the (meth)acrylic polymer (P), an alkyl acrylate ester having an alkyl group having 6 to 8 carbon atoms can be preferably used as at least a part of the monomers constituting the (meth)acrylic polymer (P). The amount used can be appropriately set depending on the desired glass transition temperature of the polymer. Specifically, in the (meth)acrylic polymer (P), the content of structural units derived from an alkyl acrylate ester having an alkyl group having 6 to 8 carbon atoms is, for example, 5% by mass or more, and preferably 10% by mass or more, based on the total structural units of the (meth)acrylic polymer (P).

[0027] The (meth)acrylic polymer (P) may be composed solely of structural units derived from a (meth)acrylic acid alkyl ester. Alternatively, the (meth)acrylic polymer (P) may further have structural units derived from a monomer other than a (meth)acrylic acid alkyl ester (hereinafter also referred to as "other monomers"), for the purpose of adjusting the glass transition temperature of the polymer, within a range that does not impair the effects of the present disclosure.

[0028] The other monomer is not particularly limited as long as it is a monomer copolymerizable with the (meth)acrylic acid alkyl ester. Examples of the other monomer include unsaturated carboxylic acids, unsaturated acid anhydrides, aliphatic cyclic (meth)acrylic acid esters, aromatic (meth)acrylic acid esters, (meth)acrylic acid alkoxyalkyl esters, (meth)acrylic acid hydroxyalkyl esters, polyalkylene glycol mono(meth)acrylates, halogen-containing vinyl compounds, vinyl ester compounds, vinyl ether compounds, heterocyclic ring-containing vinyl compounds, amino group-containing vinyl compounds, amide group-containing vinyl compounds, nitrile group-containing vinyl compounds, aromatic vinyl compounds, maleimide compounds, etc. The other monomer may be used alone or in combination of two or more.

[0029] Specific examples of these include unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, citraconic acid, cinnamic acid, succinic acid monohydroxyethyl (meth)acrylate, ω-carboxy-caprolactone mono(meth)acrylate, β-carboxyethyl (meth)acrylate, 4-carboxystyrene, etc., and unsaturated acid anhydrides such as maleic anhydride, itaconic anhydride, citraconic anhydride, etc.

[0030] Examples of aliphatic cyclic esters of (meth)acrylic acid include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, etc. Specific examples of aromatic esters of (meth)acrylic acid include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxymethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 3-phenoxypropyl (meth)acrylate, etc.

[0031] Examples of the alkoxyalkyl (meth)acrylate include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, n-propoxyethyl (meth)acrylate, n-butoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, n-propoxypropyl (meth)acrylate, n-butoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxybutyl (meth)acrylate, n-propoxybutyl (meth)acrylate, and n-butoxybutyl (meth)acrylate.

[0032] Examples of the hydroxyalkyl (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Examples of the polyalkylene glycol mono(meth)acrylate include polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and polyethylene glycol-polypropylene glycol mono(meth)acrylate.

[0033] Examples of halogen-containing vinyl compounds include vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride. Examples of heterocycle-containing vinyl compounds include glycidyl (meth)acrylate, (3,4-epoxycyclohexyl)methyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate. Examples of vinyl ester compounds include vinyl acetate and vinyl propionate. Examples of vinyl ether compounds include methyl vinyl ether, ethyl vinyl ether, and butyl vinyl ether.

[0034] Examples of the amino group-containing vinyl compound include dimethylaminomethyl (meth)acrylate, diethylaminomethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-diethylaminoethyl (meth)acrylate, 2-(di-n-propylamino)ethyl (meth)acrylate, 2-dimethylaminopropyl (meth)acrylate, 2-diethylaminopropyl (meth)acrylate, 2-(di-n-propylamino)propyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, 3-diethylaminopropyl (meth)acrylate, and 3-(di-n-propylamino)propyl (meth)acrylate.

[0035] Examples of the amide group-containing vinyl compound include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and N-methylol(meth)acrylamide.

[0036] Examples of the nitrile group-containing vinyl compound include cyanomethyl (meth)acrylate, 1-cyanoethyl (meth)acrylate, 2-cyanoethyl (meth)acrylate, 1-cyanopropyl (meth)acrylate, 2-cyanopropyl (meth)acrylate, 3-cyanopropyl (meth)acrylate, 4-cyanobutyl (meth)acrylate, 6-cyanohexyl (meth)acrylate, 2-ethyl-6-cyanohexyl (meth)acrylate, 8-cyanooctyl (meth)acrylate, (meth)acrylonitrile, α-ethylacrylonitrile, α-isopropylacrylonitrile, α-chloroacrylonitrile, and α-fluoroacrylonitrile.

[0037] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, β-methylstyrene, vinylxylene, methylstyrene, ethylstyrene, butylstyrene, methoxystyrene, hydroxystyrene, isopropenylphenol, vinylbenzoic acid, and vinylnaphthalene.

[0038] Examples of the maleimide compound include maleimide and N-substituted maleimide compounds. Examples of the N-substituted maleimide compound include N-alkyl-substituted maleimides such as N-methylmaleimide, N-ethylmaleimide, N-n-propylmaleimide, N-isopropylmaleimide, N-n-butylmaleimide, N-isobutylmaleimide, and N-tert-butylmaleimide; N-cycloalkyl-substituted maleimides such as N-cyclopentylmaleimide and N-cyclohexylmaleimide; N-aralkyl-substituted maleimides such as N-benzylmaleimide; and N-aryl-substituted maleimides such as N-phenylmaleimide, N-(4-hydroxyphenyl)maleimide, N-(4-acetylphenyl)maleimide, and N-(4-methoxyphenyl)maleimide.

[0039] From the viewpoint of fully exerting the plasticizing effect, it is preferable that the (meth)acrylic polymer (P) is substantially free of structural units having a carboxyl group. Specifically, the content of structural units having a carboxyl group in the (meth)acrylic polymer (P) is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1.5% by mass or less, still more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, based on the total structural units of the (meth)acrylic polymer (P).

[0040] The plasticizer of the present disclosure may be composed of a (meth)acrylic polymer (P), or may further contain a component different from the (meth)acrylic polymer (P) (hereinafter also referred to as "other component"). The content of the (meth)acrylic polymer (P) in the plasticizer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, still more preferably 98% by mass or more, and even more preferably 99% by mass or more, based on the total amount of the plasticizer. The (meth)acrylic polymer (P) blended in the plasticizer may be one type or two or more types.

[0041] Examples of other components to be blended in the plasticizer include an oligomer of a (meth)acrylic polymer different from the (meth)acrylic polymer (P) that exhibits a plasticizing effect; a known ester-based or ether-based plasticizer; etc. Only one type of other component may be used, or two or more types may be used.

[0042] <<Method for Producing Plasticizer>> The method for producing the plasticizer of the present disclosure is not particularly limited. The plasticizer of the present disclosure can be produced, for example, by a method including a step of obtaining a (meth)acrylic polymer (P) by polymerizing a monomer (hereinafter also referred to as a “polymerization step”).

[0043] (Polymerization step) The polymerization method for producing the (meth)acrylic polymer (P) is not particularly limited. The (meth)acrylic polymer (P) can be obtained by polymerizing monomers using a known radical polymerization method such as solution polymerization, suspension polymerization, emulsion polymerization, or bulk polymerization. Among these, the solution polymerization method is preferred because it is easy to control the molecular weight and structure of the polymer.

[0044] In the case of solution polymerization, for example, a polymerization solvent and monomers are charged into a reactor, and a polymerization initiator is added to polymerize to obtain a target polymer. When carrying out polymerization, the method of charging each raw material including the monomer may be a batch-type initial lump-sum charging in which all raw materials are charged at once, a semi-continuous charging in which at least a portion of the raw materials are continuously fed into the reactor, or a continuous polymerization method in which all raw materials are continuously fed and at the same time the produced resin is continuously withdrawn from the reactor.

[0045] An example of a preferred polymerization method for obtaining the (meth)acrylic polymer (P) is a high-temperature continuous polymerization method in which raw materials containing monomers, a polymerization solvent, and a polymerization initiator are supplied to a pressurized reactor at a constant supply rate, the raw materials are heated to a high temperature, and polymerization is carried out, and an amount of polymer solution corresponding to the amount of raw materials supplied is withdrawn from the reactor. This polymerization method makes it possible to obtain a (meth)acrylic polymer with a low molecular weight and low viscosity. It is also possible to easily obtain a (meth)acrylic polymer having a terminal carbon-carbon double bond. Furthermore, when producing a (meth)acrylic polymer using the high-temperature continuous polymerization method, molecular weight control can be suitably performed even when the amount of polymerization initiator or chain transfer agent used is reduced, and the amount of impurities in the plasticizer can be reduced. Therefore, when a mixture of the plasticizer of the present disclosure and a thermoplastic resin is molded, a molded product with excellent weather resistance and cold resistance and high strength can be obtained.

[0046] As the polymerization solvent, an organic solvent can be preferably used. Examples of the organic solvent include cyclic ethers such as tetrahydrofuran and dioxane; chain ethers such as methyl orthoformate and trimethyl orthoacetate; aromatic hydrocarbons such as benzene, toluene, and xylene; esters such as ethyl acetate and butyl acetate; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; and alcohols such as methanol, ethanol, normal propyl alcohol, isopropyl alcohol, normal butanol, secondary butyl alcohol, isobutyl alcohol, tertiary butyl alcohol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 1-hexanol, 2-hexanol, 3-methyl-3-pentanol, 1-heptanol, 1-octanol, 2-ethylhexanol, and 3-ethyl-3-hexanol.

[0047] The polymerization solvent preferably contains a primary alcohol. In the polymerization step for obtaining the (meth)acrylic polymer (P), by polymerizing a monomer in a solvent containing a primary alcohol, it is possible to obtain a (meth)acrylic polymer (P) that can be used to obtain a molded article having excellent cold resistance when the (meth)acrylic polymer (P) obtained by the polymerization is mixed with a thermoplastic resin and molded. From the viewpoint of enhancing the effect of improving the cold resistance of a molded article obtained using the (meth)acrylic polymer (P), the primary alcohol used in the polymerization solvent preferably has 4 to 8 carbon atoms, and from the viewpoint of easy availability of the raw material, normal butanol or 2-ethylhexanol is particularly preferred.

[0048] When polymerization is carried out using a primary alcohol as a polymerization solvent, the polymerization solvent may be a solvent consisting solely of a primary alcohol, or may be a mixed solvent of a primary alcohol and a polymerization solvent other than the primary alcohol (hereinafter also referred to as "other solvent"). Examples of other solvents include the organic solvents exemplified above. The amount of primary alcohol used is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 50% by mass or more, based on the total amount of the polymerization solvent.

[0049] The amount of the polymerization solvent used is preferably 5 to 180 parts by mass, more preferably 10 to 150 parts by mass, per 100 parts by mass of the total amount of the monomers. The polymerization solvent may be used alone or in combination of two or more.

[0050] The polymerization initiator is not particularly limited, and known radical polymerization initiators such as organic peroxides, inorganic peroxides, and azo compounds can be used.

[0051] Specific examples of the polymerization initiator include organic peroxides such as di-tert-butyl peroxide, cyclohexanone peroxide, dibenzoyl peroxide, 3,3,5-trimethylcyclohexanone peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, etc. Specific examples of inorganic peroxides include potassium persulfate, sodium persulfate, etc.

[0052] Examples of azo compounds include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2-(tert-butylazo)-2-cyanopropane, 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(2-methylpropane), and dimethyl 2,2'-azobis(2-methylpropionate).

[0053] Furthermore, as the polymerization initiator, a redox type polymerization initiator comprising a known oxidizing agent and a known reducing agent may be used. Examples of redox type polymerization initiators include those using sodium sulfite, sodium thiosulfate, sodium formaldehyde sulfoxylate, ascorbic acid, ferrous sulfate, or the like as a reducing agent, and potassium peroxodisulfate, hydrogen peroxide, tert-butyl hydroperoxide, or the like as an oxidizing agent. Furthermore, a known chain transfer agent can also be used in combination with the polymerization initiator. When producing the (meth)acrylic polymer (P), among the above, organic peroxides can be preferably used as the polymerization initiator because they allow for easy control of the molecular weight within the desired range.

[0054] In producing the (meth)acrylic polymer (P), the amount of the polymerization initiator used is, for example, 0.01 to 20 parts by mass, and preferably 0.05 to 15 parts by mass, per 100 parts by mass of the total amount of the monomers used in the polymerization.

[0055] From the viewpoints of controlling the molecular weight of the (meth)acrylic polymer (P) within the above range and suppressing coloration of the reaction solution due to the progress of the decomposition reaction, it is preferable to carry out the polymerization at a high temperature. Specifically, the polymerization temperature is preferably within a temperature range of 180°C or higher and 350°C or lower. From the above viewpoints, the polymerization temperature is more preferably 200°C or higher, even more preferably 210°C or higher, and even more preferably 220°C or higher. The upper limit of the polymerization temperature is more preferably 330°C or lower, even more preferably 310°C or lower, and even more preferably 290°C or lower.

[0056] When polymerization is carried out by the high-temperature continuous polymerization method, the residence time of the raw materials is, for example, 2 to 60 minutes. The pressure during polymerization may be any pressure that can maintain the polymerization temperature.

[0057] If the polymer obtained by the polymerization contains sulfur atoms derived from compounds having sulfur atoms, such as mercaptans, this can cause a decrease in the weather resistance and tensile properties of the polymer. Therefore, it is preferable that the sulfur atom content in the (meth)acrylic polymer (P) is as low as possible. Specifically, the sulfur atom content in the (meth)acrylic polymer (P) is preferably 0 ppm or more and less than 1000 ppm, more preferably 0 ppm or more and less than 100 ppm, even more preferably 0 ppm or more and less than 10 ppm, and even more preferably 0 ppm or more and less than 1 ppm. In this specification, the "sulfur atom content" refers to the total amount of sulfur atoms contained in the polymer, and can be quantified by ICP atomic emission spectroscopy.

[0058] Phosphorus atoms derived from phosphorus compounds and the like also cause a decrease in the weather resistance and tensile properties of the polymer. Therefore, it is preferable that the phosphorus atom content in the (meth)acrylic polymer (P) is as small as possible. Specifically, the phosphorus atom content in the (meth)acrylic polymer (P) is preferably 0 ppm or more and less than 1000 ppm, more preferably 0 ppm or more and less than 100 ppm, even more preferably 0 ppm or more and less than 10 ppm, and even more preferably 0 ppm or more and less than 1 ppm. In this specification, the "phosphorus atom content" refers to the total amount of phosphorus atoms contained in the polymer, and can be quantified by ICP atomic emission spectroscopy.

[0059] Metal atoms derived from metal complex compounds, etc., can also cause a decrease in the weather resistance and tensile properties of the polymer, and can also cause discoloration. Therefore, it is preferable that the metal atom content in the (meth)acrylic polymer (P) be as low as possible. Specifically, the metal atom content in the (meth)acrylic polymer (P) is preferably 0 ppm or more and less than 1000 ppm, more preferably 0 ppm or more and less than 100 ppm, even more preferably 0 ppm or more and less than 10 ppm, and even more preferably 0 ppm or more and less than 1 ppm. In this specification, the "metal atom content" refers to the total amount of metal atoms contained in the polymer, and can be quantified by ICP atomic emission spectroscopy. Note that metal complex compounds include metal complex compounds used as chain transfer agents, as well as metals present in the monomers, polymerization initiators, and polymerization solvents used in the production of the polymer, and metals mixed in from the outside during production. Generally, commercially available monomers, polymerization initiators, and polymerization solvents are purified by distillation, recrystallization, or the like, and therefore the metal atom content of these raw materials is less than 2 ppm. However, using unpurified raw materials is not preferred because the metal atom content in the raw materials becomes high.

[0060] Residual volatile components remaining in the (meth)acrylic polymer (P), such as solvents, unreacted monomers, and decomposition products derived from the polymerization initiator, can also cause a decrease in the weather resistance and tensile properties of the polymer. These residual volatile components initially function as plasticizers, but gradually volatilize from the polymer over time, which can cause the polymer to lose its initial tensile properties or emit an odor. Therefore, it is preferable that the amount of residual volatile components in the (meth)acrylic polymer (P) be as small as possible. Specifically, the amount of residual volatile components in the (meth)acrylic polymer (P) is preferably 0.0% or more and less than 2.0%, more preferably 0.0% or more and less than 1.5%, even more preferably 0.0% or more and less than 1.0%, even more preferably 0.0% or more and less than 0.8%, and even more preferably 0.0% or more and less than 0.5%. In this specification, the "amount of residual volatile components" refers to the total amount of residual volatile components contained in the polymer, which can be quantified by gas chromatography.

[0061] The polymer obtained by the above polymerization may be subjected to isolation and / or purification treatment in order to remove low-molecular-weight compounds contained in the polymer. When the polymer is isolated and / or purified, these treatments can be carried out by adopting known methods. For example, the polymer can be isolated by thin-film distillation, reprecipitation, or the like. The obtained polymer may be used as a plasticizer as it is, or may be used as a plasticizer after blending with other components as necessary.

[0062] <<Thermoplastic Resin Composition>> Next, the thermoplastic resin composition of the present disclosure will be described. The thermoplastic resin composition contains the above-described plasticizer of the present disclosure and a thermoplastic resin.

[0063] Examples of thermoplastic resins include polyolefins (e.g., polyethylene, polypropylene, etc.), vinyl chloride resins (polyvinyl chloride, ethylene-vinyl chloride copolymer, polyvinylidene chloride, etc.), polyvinyl acetate resins, polyurethane resins, polystyrene resins, AS resins (acrylonitrile-styrene copolymers), ABS resins (acrylonitrile-butadiene-styrene copolymers), AXS resins (styrene copolymers of rubber components other than acrylonitrile-butadiene), acrylic resins, polymethyl methacrylate resins, polycarbonate resins, polyester resins (e.g., polyethylene terephthalate, polybutylene terephthalate, etc.), polyamide resins, polyethers (e.g., polyacetal, polyphenylene ether, etc.), polyetherimides, polyamideimides, etc. Among these, vinyl chloride resins are preferred. The thermoplastic resin may be used alone or in combination of two or more types.

[0064] The content of the plasticizer in the thermoplastic resin composition can be appropriately set depending on the type of thermoplastic resin, the application of the thermoplastic resin composition, etc. From the viewpoint of easily adjusting the hardness of a molded body formed from the thermoplastic resin composition and obtaining a molded body in which plasticizer bleeding is suppressed, the content of the plasticizer is preferably 20 parts by mass or more and 150 parts by mass or less per 100 parts by mass of the thermoplastic resin. From the above viewpoint, the content of the plasticizer is more preferably 30 parts by mass or more, even more preferably 40 parts by mass or more, and even more preferably 50 parts by mass or more per 100 parts by mass of the thermoplastic resin. Furthermore, the content of the plasticizer is more preferably 120 parts by mass or less, even more preferably 100 parts by mass or less, and even more preferably 90 parts by mass or less per 100 parts by mass of the thermoplastic resin.

[0065] The thermoplastic resin composition may further contain, in addition to the plasticizer and the thermoplastic resin, a component different from the plasticizer and the thermoplastic resin. Examples of such components include various additives such as reinforcing agents (calcium carbonate, silica, zinc oxide, titanium oxide, etc.), antioxidants, UV absorbers, antiaging agents, processing aids, hydrochloric acid scavengers, flame retardants, antistatic agents, antifogging agents, antibacterial agents, preservatives, and colorants. The blending ratios of these components can be appropriately set depending on each component, as long as the effects of the present disclosure are not impaired.

[0066] The thermoplastic resin composition is kneaded preferably at a temperature at which the thermoplastic resin in the thermoplastic resin composition melts, and then molded by a known molding method to obtain a molded article (molded resin product). The molded article thus obtained is plasticized using the (meth)acrylic polymer (P), so the plasticizer is less likely to volatilize during the molded article production process, and bleeding of the plasticizer in the obtained molded article can be suppressed. Furthermore, the molded article obtained from the thermoplastic resin composition of the present disclosure has good cold resistance both in the early stages after production and long periods after production, and also has high strength.

[0067] The present disclosure will be specifically described below based on examples. However, the present disclosure is not limited to these examples. In the following, "parts" and "%" mean "parts by mass" and "% by mass", respectively, unless otherwise specified.

[0068] Details of the measurement methods used to evaluate the polymer are as follows. <Measurement of the amount of residual volatile components in the polymer> Gas chromatograph: GC390 (manufactured by GL Sciences) Column: CP-WAX52CB (manufactured by Agilent Technologies) Carrier gas: Nitrogen gas (1.9 mL / min) Injection temperature: 220°C Detector temperature: 230°C Oven temperature: 40°C x 5 minutes hold, heated at 7°C / min, 230°C x 5 minutes hold Preparation of calibration curve 0.1 g each of the component to be measured (standard) and isobutyl acrylate (internal standard) were precisely weighed and dissolved in tetrahydrofuran (10 mL). This mixture was measured by gas chromatography, and the detection sensitivity for each component relative to the internal standard was determined. Measurement 1 g of polymer and 0.02 g of isobutyl acrylate were precisely weighed and dissolved in tetrahydrofuran (10 mL). This mixture was measured by gas chromatography, and the composition of the volatile components was determined. <Molecular Weight Measurement> Using a gel permeation chromatograph (model "HLC-8320", manufactured by Tosoh Corporation), the weight average molecular weight (Mw) and number average molecular weight (Mn) in terms of polystyrene were obtained under the following conditions: Measurement conditions Column: TSKgel SuperMultiporeHZ-M x 4, manufactured by Tosoh Corporation Column temperature: 40°C Eluent: Tetrahydrofuran Detector: RI

[0069] <Viscosity Measurement> Using a TVE-20H viscometer (salt water / plate method, manufactured by Toki Sangyo Co., Ltd.), the viscosity of the polymer was measured with an E-type viscometer under the following conditions: Measurement conditions: Cone shape: angle 1°34', radius 24 mm Temperature: 25°C ± 0.5°C

[0070] <Measurement of Glass Transition Temperature (Tg)> The Tg of the polymer was measured using a differential scanning calorimeter (DSC) under the following conditions: DSC: DSC 214 Polymer manufactured by NETZSCH Co., Ltd. Heating temperature: 10°C / min Measurement atmosphere: nitrogen

[0071] <Quantitative Determination of Double Bond Amount>1 The amount of double bonds per unit mass of the polymer (i.e., double bond concentration) was calculated from the ratio of the integral value of the signal at around 5.5 ppm derived from hydrogen bonded to the double bond to the integral value of the signal at 3.0 to 4.5 ppm derived from hydrogen bonded to the carbon adjacent to the ester group, as measured by H-NMR, and the composition of the polymer.

[0072] 1. Polymer Synthesis [Production Example 1] Production of (meth)acrylic polymer P-1 The temperature of a 1000 mL pressurized stirred tank reactor equipped with an oil jacket was maintained at 250°C. Next, while maintaining a constant pressure in the reactor, a monomer mixture containing 70 parts of n-butyl acrylate (hereinafter referred to as "BA"), 30 parts of 2-ethylhexyl acrylate (hereinafter referred to as "HA"), 35 parts of normal butanol (hereinafter referred to as "n-BuOH"), 30 parts of methyl ethyl ketone (hereinafter referred to as "MEK"), and 2 parts of di-t-butyl peroxide (manufactured by NOF Corporation, trade name "Perbutyl D", hereinafter referred to as "DTBP") as a polymerization initiator was continuously fed from a raw material tank to the reactor at a constant feed rate (48 g / min), and the polymerization reaction was allowed to proceed with a residence time of 12 minutes (see Table 1). Then, a reaction liquid equivalent to the amount of the monomer mixture fed was continuously withdrawn from the outlet of the reactor and recovered. Although the reaction temperature dropped once immediately after the start of the reaction, a temperature rise due to the heat of polymerization was observed. Therefore, the reaction temperature was maintained at 257°C to 259°C (Table 1 lists the median value of 258°C) by controlling the temperature of the oil jacket. The point at which the liquid temperature in the reactor stabilized after the start of the monomer mixture supply was designated the start point for collecting the reaction liquid, and the reaction was carried out for 25 minutes from the start point. In this production example, the amount of the monomer mixture supplied was 1.2 kg, and the amount of the reaction liquid recovered was 1.2 kg. The mixed liquid of the polymer, solvent, and unreacted monomer discharged from the reactor was continuously introduced into a thin-film evaporator to separate volatile components such as unreacted monomer, yielding 0.66 kg of polymer P-1. Polymer P-1 had an Mw of 1,410, an Mn of 980, a viscosity of 203 mPa·s, and an SP value of 9.60 [cal / cm 3 ] 1/2 The polymer P-1 had a Tg of -78°C and a double bond concentration of 0.25 meq / g. The amount of residual volatile components such as unreacted monomers contained in the polymer P-1 was 0.5%.

[0073] [Production Examples 2 to 9, Comparative Production Examples 1 to 5] Polymers P-2 to P-14, which are (meth)acrylic polymers, were obtained in the same manner as in Production Example 1, except that the types and amounts of raw materials used were changed as shown in Table 1. The amount of residual volatile components such as unreacted monomers contained in polymers P-2 to P-14 was less than 0.8%. In Table 1, "C1" represents methoxyethyl acrylate, "2-EhOH" represents 2-ethylhexanol, and "IPA" represents isopropyl alcohol. The monomer composition ratios of polymers P-1 to P-14 are the same as the monomer charging ratios.

[0074]

[0075] 2. Production and Evaluation of Thermoplastic Resin Compositions (I) (1) Production of Thermoplastic Resin Compositions The following thermoplastic resin compositions were produced using the (meth)acrylic polymers P-1 to P-14 obtained in the above Production Examples and Comparative Production Examples as plasticizers and flexible vinyl chloride resin as the thermoplastic resin. [Example 1] 100 parts of flexible vinyl chloride resin (manufactured by Shin-Dai-Ichi Vinyl Corporation, trade name "ZEST 1300Z"), 80 parts of polymer P-1, 30 parts of calcium carbonate (manufactured by Maruo Calcium Co., Ltd., trade name "Super SSS"), 10 parts of titanium oxide (manufactured by Ishihara Sangyo Kaisha, Ltd., trade name "Tipake R820"), 1.2 parts of calcium stearate, 0.3 parts of zinc stearate, and 2 parts of an antioxidant (manufactured by BASF, trade name "Tinuvin B75") were mixed and kneaded at 160°C using a Labo Plastomill to obtain thermoplastic resin composition R-1 (see Table 2).

[0076] [Examples 2 to 10, Comparative Examples 1 to 6] Thermoplastic resin compositions R-2 to R-16 were obtained in the same manner as in Example 1, except that the types and amounts of plasticizers used were changed as shown in Table 2. In Table 2, "DINP" stands for diisononyl phthalate.

[0077] (2) Evaluation The following evaluations were carried out using the thermoplastic resin compositions obtained in each of the Examples and Comparative Examples. The evaluation results are shown in Table 2. <Compatibility> During the production of the thermoplastic resin composition, the state of the resin after kneading (degree of cohesion) was observed. In Table 2, "○" indicates good compatibility (resin is cohesive), and "×" indicates poor compatibility (resin is not cohesive and falls apart).

[0078] <Tensile Test> The thermoplastic resin composition was press-molded at 190°C to obtain a No. 3 dumbbell test piece (thickness: 1 mm). The test piece was conditioned at 23°C and 50% RH for 24 hours, and then the breaking stress (MPa) and breaking elongation (%) were measured at a tension speed of 200 mm / min using a tensile tester (Autograph AGS-J, manufactured by Shimadzu Corporation).

[0079] <Cold Resistance> (Evaluation of cold resistance of molded articles early after production (before weather resistance test)) The thermoplastic resin composition was press molded at 190°C to obtain test pieces with a length of 38 mm, a width of 6 mm, and a thickness of 2 mm. These test pieces were conditioned at 23°C and 50% RH for 24 hours. Thereafter, the presence or absence of fracture occurring in the test pieces at -20°C was confirmed using a brittle temperature tester (S-type, manufactured by Toyo Seiki Seisaku-sho, Ltd.). In Table 2, "○" indicates "no fracture" and "×" indicates "fracture."

[0080] (Evaluation of cold resistance of molded body after weather resistance test) A test piece of the same shape and size as the test piece used in the cold resistance evaluation of the molded body immediately after production was placed in a metaling weather meter "DAIPLA METAL WEATHER KU-R5NCI-A" (product name) manufactured by Daipla Wintes Co., Ltd., and an accelerated weather resistance test was carried out. The accelerated conditions were a metal halide lamp illuminance of 80 mW / cm 2 The test environment was a temperature of 63°C, humidity of 70% RH, and a two-minute shower every two hours. This procedure was repeated for 1,200 hours, and then the cold resistance was evaluated using the same evaluation method as above.

[0081]

[0082] As is clear from the results in Table 2, (meth)acrylic polymers P-1 to P-9, which had an Mw of 1,650 or less, an SP value of 9.50 or more, and a glass transition temperature of -77°C or less, had good compatibility with flexible vinyl chloride resin. Furthermore, the thermoplastic resin compositions of Examples 1 to 10, which contained (meth)acrylic polymers P-1 to P-9 and flexible vinyl chloride resin, were able to give molded articles with high strength and excellent cold resistance.

[0083] In contrast, Comparative Examples 1, 3, and 5, which used a (meth)acrylic polymer having a glass transition temperature higher than −77° C. as a plasticizer, and Comparative Example 2, which used a (meth)acrylic polymer having a glass transition temperature higher than −77° C. and an Mw greater than 1,650 as a plasticizer, exhibited poor cold resistance both before and after the weather resistance test. Furthermore, Comparative Example 4, which used a (meth)acrylic polymer having a low SP value as a plasticizer, failed to produce a molded article because the plasticizer was incompatible with the soft vinyl chloride resin. The molded article of Comparative Example 4 could not be evaluated for stress at break, elongation at break, and cold resistance, and therefore is marked “evaluation not possible” in Table 2. Comparative Example 6, which used diisononyl phthalate as a plasticizer, exhibited poor cold resistance after the weather resistance test.

[0084] 3. Production and Evaluation of Thermoplastic Resin Compositions (II) (1) Production of Thermoplastic Resin Compositions The (meth)acrylic polymers P-1, P-8, P-10, P-11, and P-13 obtained in the above Production Examples and Comparative Production Examples were used as plasticizers, and rigid vinyl chloride resin was used as the thermoplastic resin to produce the following thermoplastic resin compositions. [Example 11] 100 parts of rigid vinyl chloride resin (manufactured by Taiyo Vinyl Chloride Co., Ltd., trade name "TH-700"), 40 parts of polymer P-1, 2.5 parts of calcium carbonate (manufactured by Maruo Calcium Co., Ltd., trade name "Super SSS"), 0.15 parts of barium stearate, 2.85 parts of zinc stearate, and 2 parts of epoxidized soybean oil (manufactured by New Japan Chemical Co., Ltd., trade name "Sansocizer E-2000H") were mixed and kneaded in a Laboplastomill at 165 ° C. to obtain a thermoplastic resin composition R-17 (see Table 3).

[0085] Example 12, Comparative Examples 7 to 9 Thermoplastic resin compositions R-18 to R-21 were obtained in the same manner as in Example 11, except that the types of plasticizers used were as shown in Table 3.

[0086] (2) Evaluation The following evaluations were performed using the thermoplastic resin compositions obtained in each Example and Comparative Example. The evaluation results are shown in Table 3. <Compatibility> During the production of the thermoplastic resin compositions, the state of the resin (degree of cohesion) after kneading was observed using the same methods and criteria as in Examples 1 to 10 and Comparative Examples 1 to 6. <Tensile Test> (Room Temperature Tensile Test) The thermoplastic resin compositions were press-molded at 190°C to obtain No. 3 dumbbell test pieces (1 mm thick). These test pieces were conditioned at 23°C and 50% RH for 24 hours, and then the breaking stress (MPa) and breaking elongation (%) were measured at a tension rate of 200 mm / min using a tensile tester (Autograph AGS-J, manufactured by Shimadzu Corporation). (Low Temperature Tensile Test) The thermoplastic resin compositions were press-molded at 190°C to obtain No. 3 dumbbell test pieces (1 mm thick). These test pieces were conditioned at 23°C and 50% RH for 24 hours. Thereafter, the specimen was cured in an environment of −5° C. for 1 hour, and then the breaking stress (MPa) and breaking elongation (%) were measured under the conditions of a tensile speed of 200 mm / min and a temperature of −5° C. using a tensile testing machine (INSTRON 5566A, manufactured by Instron Corporation) attached to a high and low temperature thermostatic chamber (G00159-1, manufactured by Mita Sangyo Co., Ltd.).

[0087]

[0088] As is clear from the results in Table 3, the thermoplastic resin compositions of Examples 11 and 12, which comprised (meth)acrylic polymers P-1 and P-8 having an Mw of 1,650 or less, an SP value of 9.50 or more, and a glass transition temperature of -77 ° C. or less, and a rigid vinyl chloride resin, were able to obtain molded articles with excellent elongation even at -5 ° C. In contrast, Comparative Example 7, in which a (meth)acrylic polymer having a glass transition temperature higher than -77 ° C. was used as a plasticizer, and Comparative Example 8, in which a (meth)acrylic polymer having a glass transition temperature higher than -77 ° C. and an Mw of more than 1,650 was used as a plasticizer, did not provide sufficient elongation of the molded article at -5 ° C. Furthermore, in Comparative Example 9, in which a (meth)acrylic polymer having an SP value lower than 9.50 was used as a plasticizer, the plasticizer was not compatible with the rigid vinyl chloride resin, and a molded article could not be obtained.

[0089] From the above results, it was revealed that a plasticizer containing a (meth)acrylic polymer that contains structural units derived from a (meth)acrylic acid alkyl ester, has a weight-average molecular weight of 1,650 or less, an SP value of 9.50 or more, and a glass transition temperature of −77° C. or less, can provide a molded article with excellent cold resistance when used in combination with a thermoplastic resin.

[0090] The present invention is not limited to the above-described embodiments, and encompasses various modifications and equivalent modifications within the scope of the spirit of the present invention. Therefore, in light of the above teachings, various combinations and forms, as well as other combinations and forms including only one element, more than one element, or less than one element, are to be understood as falling within the scope and spirit of the present invention.

Claims

1. A plasticizer comprising a (meth)acrylic polymer containing a structural unit derived from an alkyl (meth)acrylate ester, wherein the (meth)acrylic polymer has a weight average molecular weight of 1,650 or less, an SP value of 9.50 or more, and a glass transition temperature of -77°C or less.

2. The plasticizer according to claim 1, wherein the (meth)acrylic polymer has a carbon-carbon double bond content of 0.10 meq / g or more and 0.36 meq / g or less.

3. The plasticizer according to claim 1, wherein the (meth)acrylic polymer contains structural units derived from an alkyl (meth)acrylate ester having an alkyl group having 3 or more carbon atoms in an amount of 40 mass% or more based on the total structural units of the (meth)acrylic polymer.

4. A method for producing the plasticizer according to any one of claims 1 to 3, comprising the step of obtaining the (meth)acrylic polymer by polymerizing a monomer in a solvent containing a primary alcohol.

5. The method for producing a plasticizer according to claim 4, wherein the primary alcohol is normal butanol or 2-ethylhexanol.

6. The method for producing the plasticizer according to claim 4, wherein the polymerization temperature is within the range of 180°C or higher and 350°C or lower.

7. A thermoplastic resin composition comprising the plasticizer according to any one of claims 1 to 3 and a thermoplastic resin.

Citation Information

Patent Citations

  • Curable composition

    JP2006022169A

  • Pressure sensitive adhesive composition and adhesive tape

    JP2007084638A

  • Optical film and plasticizer for forming sheet

    JP2014091752A

  • Thermoplastic elastomer composition

    JP2018184544A