Resin pipe

The multilayer resin pipe design addresses the challenges of flexibility and resistance in EV cooling systems by using a high-glass-transition-temperature inner layer and a polyamide outer layer, achieving enhanced bending workability and refrigerant resistance for EV cooling systems.

WO2024242188A1PCT designated stage expired Publication Date: 2024-11-28ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019105
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2024-05-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing resin pipes for EV cooling systems face challenges with flexibility, bending workability, connector press-fitting, and resistance to unbending under environmental conditions, particularly at high temperatures and with refrigerants.

Method used

A multilayer resin pipe design featuring a first resin composition with a glass transition temperature of 100°C or higher as the innermost layer and a polyamide-based second resin composition as the outermost layer, with optional intermediate layers, enhancing flexibility and bending workability while maintaining mechanical strength and resistance to refrigerants.

Benefits of technology

The multilayer resin pipe achieves a well-balanced combination of flexibility, bending workability, and resistance to unbending, even under high-temperature and refrigerant exposure conditions, ensuring reliable performance in EV cooling systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a resin pipe which is excellent in terms of flexibility, low-temperature impact resistance, and bending workability of the pipe in a balanced manner. In order to achieve the above, the present invention provides a multilayer resin pipe which comprises at least (A) a layer that is formed of a first resin composition and (B) a layer that is formed of a second resin composition, the resin pipe being characterized in that: the first resin composition contains a first matrix resin and optionally other components, and the glass transition temperature of the first matrix resin is 100°C or higher; and the second resin composition contains a second matrix resin containing a polyamide, and optionally other components.
Need to check novelty before this filing date? Find Prior Art

Description

Resin pipe

[0001] The present invention relates to a resin pipe.

[0002] Polyamide resins have properties suitable for use as engineering plastics, such as excellent mechanical properties, thermal properties, and chemical resistance, and are therefore widely used in a wide range of applications, including machine parts, automobile parts, and various electrical and electronic parts, primarily for injection molding.

[0003] Meanwhile, electric vehicles (EVs), which are expected to rapidly expand in the future, require long, thin-diameter molded products as cooling pipes through which refrigerants for cooling batteries pass. The mainstream method for producing long, thin-diameter molded products is to bend a straight tubular primary molded body obtained by extrusion molding, press-fit connectors onto both ends of the pipe, and use the resulting product as a single component. In bending, it is preferable to minimize the difference between the angle at which the pipe is bent during processing and the angle at which it is bent in the finished pipe, as this reduces the need for modification of the mold used to bend the pipe. For connector press-fitting, from the perspective of work efficiency, it is required that the connector be press-fit into the pipe at room temperature. Furthermore, in recent years, there has been concern that bent pipes may unbend under actual operating conditions, resulting in stress on the points at which the pipe is fixed, resulting in damage to the pipe.

[0004] It is known that polyamide resins for extrusion molding, which are obtained by adding a crosslinked ethylene-1-butene copolymer to polyamide 6, can provide pipes with excellent flexibility (see, for example, Patent Document 1). It is also known that polyamide resins for extrusion molding, which are obtained by adding a maleic anhydride-grafted ethylene-propylene copolymer or a maleic anhydride-grafted SEBS (styrene-ethylene / 1-butene-styrene block copolymer) to polyamide 12, can be extrusion-molded and have excellent flexibility and chemical resistance (see, for example, Patent Document 2). While polyamides are generally hydrolyzable, multilayer resin pipes having a polypropylene inner layer containing a heat stabilizer and a polyamide outer layer are known to suppress polyamide hydrolysis and to have excellent resistance to refrigerants such as glycol aqueous solutions at 130°C (refrigerant resistance) and interlayer peel strength (see, for example, Patent Document 3). It is also known that resin pipes using syndiotactic polystyrene for the inner and outer layers and a polyamide intermediate layer have excellent resistance to snow-melting salts (see, for example, Patent Document 4).

[0005] Japanese Patent Publication No. 2023-78137 Japanese Patent No. 3850608 Japanese Patent No. 4909267 Japanese Patent No. 4096782

[0006] However, while the technology described in Patent Document 1 allows for extrusion molding and produces pipes with excellent flexibility and impact resistance, it lacks strength at high temperatures, resulting in issues such as liquid leakage at the temperature of an EV's operating environment, as well as issues with recursion at the operating environment. Furthermore, the technology described in Patent Document 2 has the problem that even if a polyamide resin composition is extrusion moldable and has excellent flexibility and chemical resistance, it is difficult to improve the pipe's bending workability, connector press-fitting ability, and recursion resistance under actual operating conditions. Furthermore, the technology described in Patent Document 3 has the problem that even if a resin pipe has even better chemical resistance, it is difficult to improve the pipe's bending workability, connector press-fitting ability, and recursion resistance under actual operating conditions. Furthermore, the technology described in Patent Document 4 has the problem that even if a resin pipe has excellent resistance to snow-melting salts, it is difficult to improve the pipe's bending workability, connector press-fitting ability, recursion resistance under actual operating conditions, and resistance to various oils during the assembly process into an actual vehicle.

[0007] The present invention has been made in view of the above circumstances, and provides a multi-layer resin pipe that is excellent in balance between flexibility and pipe bending workability.

[0008] The present inventors have conducted extensive research into multilayer resin pipes in order to solve the above-mentioned problems, and as a result have found that by adjusting the components of the resin material that makes up each layer and constructing the pipe from a resin composition containing a matrix resin with a glass transition temperature of at least 100°C and a resin composition containing polyamide, it is possible to achieve a good balance between flexibility, pipe bending processability, and other physical properties.

[0009] The present invention has been made based on the above findings, and its gist is as follows: 1. A multilayer resin pipe including at least a layer formed from (A) a first resin composition and a layer formed from (B) a second resin composition, wherein the first resin composition contains a first matrix resin and optionally other components, and the first matrix resin has a glass transition temperature of 100°C or higher, and the second resin composition contains a second matrix resin containing a polyamide and optionally other components. 2. The resin pipe according to item 1, wherein the layer formed from the (A) first resin composition is the innermost layer and the layer formed from the (B) second resin composition is the outermost layer, the innermost layer is in contact with the inside of the outermost layer, and the first matrix resin has a functional group reactive with the polyamide or contains a polyamide. 3. the layer formed from the (A) first resin composition is the innermost layer, and the layer formed from the (B) second resin composition is the outermost layer; the resin pipe further comprises one or more (C) intermediate layers provided between the innermost layer and the outermost layer, the (C) intermediate layer containing a matrix resin and optionally other components, the matrix resin in a resin composition forming one of the (C) intermediate layers that contacts the inner side of the layer formed from the (B) second resin composition has a functional group reactive with the polyamide or contains a polyamide, when the (C) intermediate layer is made up of a plurality of layers, the matrix resins contained in the respective resin compositions contain one or more of the same polymer species, or the matrix resin of one (C) intermediate layer has a functional group reactive with the matrix resin of another (C) intermediate layer, and further satisfies any of the following conditions (1) to (3):(1) The matrix resin contained in the innermost layer of the (C) intermediate layer and the first matrix resin each contain at least one of the same polymer species. (2) The matrix resin contained in the innermost layer of the (C) intermediate layer has a functional group reactive with the first matrix resin. (3) The first matrix resin has a functional group reactive with the matrix resin contained in the innermost layer of the (C) intermediate layer. 4. The resin pipe according to 2 or 3 above, characterized in that the first resin composition has a flexural modulus of 2.0 GPa or less at room temperature. 5. The resin pipe according to 4 above, characterized in that the first resin composition has a flexural modulus of 1.5 GPa or less at room temperature. 6. The resin pipe according to any one of 2 to 5 above, characterized in that the second resin composition has a flexural modulus of 1.5 GPa or less at room temperature. 7. The resin pipe according to 6 above, characterized in that the second resin composition has a flexural modulus of 1.0 GPa or less at room temperature. 8. The resin pipe according to any one of claims 2 to 7, characterized in that the glass transition temperature of the first resin composition is 115°C or higher. 9. The resin pipe according to any one of claims 2 to 8, characterized in that the first resin composition contains a polyphenylene ether resin, and the content of the polyphenylene ether resin in 100 parts by weight of the first resin composition is 10 parts by weight or higher. 10. The resin pipe according to any one of claims 2 to 8, characterized in that the first matrix resin contains a polyphenylene ether resin, and the content of the polyphenylene ether resin in 100 parts by weight of the first matrix resin is 10 parts by weight or higher. 11. The resin pipe according to any one of claims 2 to 10, characterized in that the first matrix resin is amorphous. 12. The resin pipe according to claim 7, characterized in that the glass transition temperature of the first resin composition is 130°C or higher.13. The resin pipe according to any one of items 2 to 12 above, wherein a matrix resin in a resin composition forming a layer in contact with the inner side of the layer formed from the (B) second resin composition has a functional group reactive with the polyamide, and the functional group reactive with the polyamide is at least one selected from a carboxy group, an acid anhydride, an amino group, a glycidyl group, an oxazoline group, and functional groups derived therefrom. 14. The resin pipe according to any one of items 2 to 12 above, wherein a polyamide content relative to 100 mass% of matrix resin in a resin composition forming a layer in contact with the inner side of the layer formed from the (B) second resin composition is 50 mass% or more, and the polyamide content relative to 100 mass% of the first matrix resin is 50 mass% or more. 15. The resin pipe according to any one of items 1 to 14 above, wherein the second resin composition has a flexural modulus of less than 0.8 GPa. 16. The resin pipe according to item 15, characterized in that a layer formed from the (A) first resin composition and a layer formed from the (B) second resin composition are in contact with each other, and the first matrix resin has a functional group reactive with the polyamide or contains a polyamide. 17. The resin pipe according to item 15 or 16, characterized in that the layer formed from the (B) second resin composition is located outside the layer formed from the (A) first resin composition. 18. The resin pipe according to any one of items 15 to 17, characterized in that the water absorption of the first matrix resin is less than 1.0%. 19. The resin pipe according to any one of items 15 to 18, characterized in that the water absorption of the first resin composition is less than 1.0%. 20. The resin pipe according to any one of items 15 to 19, characterized in that the content of the polyamide resin is 50 parts by weight or less when the total amount of resin components of the second resin composition is 100 parts by weight. 21. 21. The resin pipe according to any one of 15 to 20, wherein the second resin composition contains a polyolefin resin, and at least a portion of the polyolefin resin is crosslinked.22. The resin pipe according to any one of the above items 15 to 21, wherein the second resin composition contains polyolefin resins, at least one of which contains monomer units derived from α-olefins, and the mass proportion of the monomer units derived from α-olefins among all monomer units constituting the polyolefin resin is 3% by mass or more and 20% by mass or less. 23. The resin pipe according to any one of the above items 15 to 22, wherein the second resin composition exhibits at least one melting peak of 80°C or more and less than 150°C when heated from 23°C at 20°C / min as measured with a differential scanning calorimeter. 24. The resin pipe according to any one of items 1 to 23, wherein the resin pipe is used in an air or cooling water circuit. 25. The resin pipe according to any one of items 1 to 23, wherein the resin pipe is used in an automobile cooling piping.

[0010] According to the present invention, it is possible to provide a multi-layer resin pipe that is excellent in balance between flexibility and pipe bending workability.

[0011] Hereinafter, a mode for carrying out the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail. The following present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0012] In this specification, "polyamide" refers to a polymer having an amide (-NHCO-) ​​group in the main chain. In addition, in this specification, "matrix resin" refers to a resin component that forms a continuous phase among resin components in a resin composition, and does not include a resin component that forms a dispersed phase.

[0013] <Resin Pipe> The resin pipe of the present embodiment includes at least (A) a layer formed from a first resin composition (hereinafter also referred to as "(A) layer") and (B) a layer formed from a second resin composition (hereinafter also referred to as "(B) layer"), wherein the first resin composition contains a first matrix resin and optionally other components, and the first matrix resin has a glass transition temperature of 100°C or higher, and the second resin composition contains a second matrix resin containing polyamide and optionally other components.

[0014] The multilayer resin pipe of this embodiment has the above-mentioned configuration, so that the layer formed from (A) the first resin composition suppresses deformation due to stress relaxation of the layer formed from (B) the second resin composition, and the first resin composition exhibits excellent mechanical strength in the high temperature range, making it possible to provide a multilayer resin pipe that is excellent in balance between flexibility and pipe bending processability.

[0015] Hereinafter, each of the components of the multilayer resin pipe of this embodiment will be described in detail.

[0016] (A) Layer Formed from First Resin Composition The resin pipe of this embodiment includes at least a layer formed from a first resin composition (A). The matrix resin of the first resin composition used in the layer (A) has a glass transition temperature of 100°C or higher, preferably 115°C or higher, more preferably 130°C or higher, and even more preferably 140°C or higher. By setting the glass transition temperature of the first matrix resin within the above range, deformation due to stress relaxation of the second resin composition after bending can be suppressed, and the resin pipe tends to have excellent resilience under actual use conditions.

[0017] Here, the first matrix resin contained in the first resin composition includes, but is not limited to, acrylonitrile-butadiene-styrene copolymer, polyamide, polycarbonate, polyethersulfone, polyetheretherketone, polyphenylene ether, polytetrafluoroethylene, etc. When air flows inside the pipe, the first matrix resin is preferably polyamide, polycarbonate, polyethersulfone, polyetheretherketone, polyphenylene ether, or polytetrafluoroethylene. When an aqueous medium flows inside the pipe, the first matrix resin is preferably polyamide, polyethersulfone, polyetheretherketone, polyphenylene ether, or polytetrafluoroethylene, and more preferably polyethersulfone, polyetheretherketone, polyphenylene ether, or polytetrafluoroethylene. Polyphenylene ether is particularly preferred as the first matrix resin from the viewpoint of suppressing changes in the conductivity of the aqueous medium. Furthermore, when an oil-based medium flows inside the pipe, polyamide, polyetheretherketone, polyethersulfone, or polytetrafluoroethylene is preferred.

[0018] When the first resin composition contains polyphenylene ether, the content of the polyphenylene ether is preferably 10 parts by weight or more, more preferably 20 parts by weight or more, even more preferably 25 parts by weight or more, even more preferably 35 parts by weight or more, particularly preferably 40 parts by weight or more, and most preferably 45 parts by weight or more, per 100 parts by weight of the first resin composition. When the content of the polyphenylene ether resin is equal to or greater than the lower limit, the glass transition point of the first resin composition tends to be higher, and a resin pipe having better bending resistance and high-temperature pressure resistance tends to be obtained. The upper limit of the amount of polyphenylene ether resin in the first resin composition is not particularly limited, but can be, for example, 80 parts by weight per 100 parts by weight of the first resin composition. When the content of the polyphenylene ether resin is equal to or less than the upper limit, a resin pipe having excellent impact resistance tends to be obtained.

[0019] In addition, the first resin composition preferably contains 50 parts by weight or more of an amorphous resin, preferably 70 parts by weight or more of an amorphous resin, more preferably 90 parts by weight or more of an amorphous resin, and may contain 100 parts by weight of an amorphous resin, per 100 parts by weight of the first resin composition. Here, being amorphous means that no melting peak is detected in a differential scanning calorimeter. By containing 50 parts by weight or more of an amorphous resin in the first resin composition, residual stress during bending of the resin pipe is reduced, and a resin pipe with excellent bending workability and resistance to bending back tends to be obtained.

[0020] The first resin composition preferably has a flexural modulus of 2.5 GPa or less, more preferably 2.0 GPa or less, and particularly preferably 1.5 GPa or less. When the flexural modulus is within this range, the pipe becomes more flexible, and the stress during bending is reduced, resulting in excellent bending processability and a tendency to suppress cracking of the pipe when a connector is press-fitted.

[0021] Furthermore, the first resin composition may further contain any polyolefin, elastomer, plasticizer, etc. to control the flexural modulus within the above range. Polyolefins and elastomers are generally incompatible with the first matrix resin and tend to form a dispersed phase. Furthermore, when a liquid flows through the pipe, the content of the plasticizer in the first resin composition is preferably 10 parts by mass or less per 100 parts by mass of the first matrix resin. This prevents the plasticizer from leaking into the liquid flowing through the pipe, thereby preventing deterioration of the liquid and a decrease in the flexibility of the pipe. From this perspective, the content of the plasticizer is more preferably 5 parts by mass or less, even more preferably 2 parts by mass or less, per 100 parts by mass of the first matrix resin, and may even be 0 parts by mass.

[0022] Furthermore, the first resin composition preferably has a water absorption rate of less than 1.0%, more preferably less than 0.5%. A water absorption rate of less than 1.0% can prevent a significant decrease in the glass transition temperature when LLC is filled, and tends to further prevent bending back at the operating temperature of 80°C when LLC is filled. From the same perspective, the first matrix resin preferably has a water absorption rate of less than 1.0%, more preferably less than 0.5%.

[0023] Furthermore, when the (A) layer is in contact with the (B) layer described later (when the (A) layer is in contact with the inside or outside of the (B) layer), the first matrix resin preferably contains a polyamide contained in the matrix resin of the resin composition used in the (B) layer described later, or the first matrix resin preferably has a functional group reactive with the polyamide or contains a polyamide. This increases the adhesive strength between the (A) layer and the (B) layer, suppresses deformation of the (B) layer due to stress relaxation, and provides a multilayer resin pipe that is excellent in balance with flexibility, low-temperature impact resistance, pipe bending processability, resistance to rebending under actual use conditions, and resistance to liquid leakage.

[0024] Here, when the first matrix resin contains a polyamide, the polyamide content is not particularly limited, but is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, based on 100% by mass of the total amount of the first matrix resin, and may be 100% by mass.

[0025] Furthermore, examples of the functional group reactive with the polyamide include, but are not limited to, a carboxy group, an acid anhydride group, an amino group, a glycidyl group, an oxazoline group, and derivatives thereof.

[0026] Furthermore, when the first matrix resin has a functional group reactive with polyamide, the amount of the functional group is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and particularly preferably 0.15 parts by mass or more, per 100 parts by mass of the first matrix resin. The upper limit is not particularly limited, but may be 50 parts by mass or less, 30 parts by mass or less, or 20 parts by mass or less. The amount of the functional group can be measured by known methods such as neutralization titration or nuclear magnetic resonance analysis.

[0027] Methods for introducing functional groups into the matrix resin include a method of adding a compound having a functional group during polymerization and polymerizing the resulting mixture, and a method of melt-kneading the resin, the compound having a functional group, and, if necessary, a peroxide, using an extruder or kneader.

[0028] The amount of functional groups can be measured by neutralization titration, nuclear magnetic resonance analysis, etc. When the matrix resin contained in the first resin composition has the functional groups, the adhesive strength between Layer (A) and Layer (B) tends to be increased.

[0029] Furthermore, when the (A) layer is in contact with a (C) intermediate layer (described later, the (C) intermediate layer being a layer provided between the (A) layer and the (B) layer), it is preferable that the first matrix resin contains the same type of polymer as the polymer contained in the matrix resin of the resin composition used in the (C) intermediate layer with which it is in contact, or that the first matrix resin has a functional group reactive with the matrix resin of the resin composition used in the (C) intermediate layer with which it is in contact. By containing the same type of polymer or having the functional group, the adhesive strength between the (A) layer and the (C) intermediate layer with which it is in contact on the inside or outside tends to be increased.

[0030] The functional group contained in the first matrix resin can be selected arbitrarily from known knowledge depending on the type of matrix resin in the resin composition used in the intermediate layer (C).

[0031] When the first matrix resin has a functional group reactive with the matrix resin of the resin composition used in the intermediate layer (C), the amount of the functional group is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and particularly preferably 0.15 parts by mass or more, relative to 100 parts by mass of the first matrix resin. The upper limit is not particularly limited, but may be 50 parts by mass or less, 30 parts by mass or less, or 20 parts by mass or less.

[0032] Furthermore, when the first matrix resin contains polyphenylene ether, the content of the polyphenylene ether is preferably 10 parts by weight or more, more preferably 25 parts by weight or more, even more preferably 30 parts by weight or more, even more preferably 40 parts by weight or more, particularly preferably 50 parts by weight or more, even particularly preferably 60 parts by weight or more, most preferably 80 parts by weight or more, and may even be 100 parts by weight. When the content of the polyphenylene ether resin is equal to or more than the above lower limit, the glass transition temperature of the first matrix resin tends to be higher, and a resin pipe that is more excellent in bending resistance and high-temperature pressure resistance tends to be obtained.

[0033] Furthermore, the first matrix resin is preferably amorphous. Here, "amorphous" means that no melting peak is detected in a differential scanning calorimeter. When the first matrix resin is amorphous, residual stress during bending of the resin pipe tends to be small, resulting in a resin pipe with excellent bending workability and resistance to bending back.

[0034] The first resin composition may further contain other components as needed, as long as the effects of this embodiment are not impaired. Examples of other components include, but are not limited to, thermoplastic resins other than those listed above, ultraviolet absorbers, antioxidants, photodegradation inhibitors, heat-resistant materials, plasticizers, lubricants, release agents, nucleating agents, flame retardants, colorants, dyes, pigments, fillers, and impact-resistant materials. Because the properties of the other components vary significantly, there are various suitable contents for each component that do not substantially impair the effects of this embodiment. A person skilled in the art can easily determine the suitable content of each of the other components.

[0035] (B) Layer Formed from Second Resin Composition The resin pipe of this embodiment includes at least a layer formed from a second resin composition (B). The second resin composition includes a second matrix resin containing polyamide and optionally other resin components (domain resins).

[0036] Furthermore, the mass proportion of the polyamide resin relative to 100 parts by mass of the total mass of the resin components contained in the second resin composition is preferably 20 to 50 parts by mass, more preferably 25 to 45 parts by mass, and even more preferably 30 to 40 parts by mass, when the viscosity of the polyolefin resin is sufficiently high due to crosslinking or the like, as described below. Furthermore, when the viscosity of the polyolefin resin is at a normal level, the mass proportion is preferably 50 parts by mass or more and 100 parts by mass or less, more preferably 50 parts by mass or more and 80% by mass or less, and even more preferably 50 parts by mass or more and 65 parts by mass or less. When the mass proportion of the polyamide resin is equal to or greater than the lower limit, the polyamide resin can be reliably used as a matrix, and a resin pipe with excellent leakage resistance tends to be obtained. When the mass proportion of the polyamide resin is equal to or less than the upper limit, a more flexible resin pipe tends to be obtained.

[0037] Examples of the polyamide resin include, but are not limited to, polyamide resins obtained by condensation polymerization of diamines and dicarboxylic acids, polyamide resins obtained by ring-opening polymerization of lactams, polyamide resins obtained by self-condensation of aminocarboxylic acids, and copolymers obtained by copolymerization of two or more monomers constituting these polyamide resins. These polyamide components may be used alone or in combination of two or more.

[0038] The polymerization monomers that serve as raw materials for the polyamide resin are described in detail below. Diamines Examples of diamines include, but are not limited to, aliphatic diamines, alicyclic diamines, and aromatic diamines.

[0039] The aliphatic diamine may be a linear saturated aliphatic diamine or a branched saturated aliphatic diamine. Examples of the branched saturated aliphatic diamine include diamines having a substituent branched from the main chain.

[0040] The linear saturated aliphatic diamine preferably has 2 to 20 carbon atoms, and examples thereof include ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, and tridecamethylenediamine.

[0041] The branched saturated aliphatic diamine preferably has 3 to 20 carbon atoms, and examples thereof include 2-methylpentamethylenediamine (also referred to as "2-methyl-1,5-diaminopentane"), 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyloctamethylenediamine, and 2,4-dimethyloctamethylenediamine.

[0042] Examples of the alicyclic diamine (also referred to as alicyclic diamine) include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, 1,3-cyclopentanediamine, 4,4'-diaminodicyclohexylmethane, and 4,4'-diaminodicyclohexylpropane.

[0043] Examples of aromatic diamines include, but are not limited to, metaxylylenediamine, paraxylylenediamine, metaphenylenediamine, orthophenylenediamine, and paraphenylenediamine.

[0044] These diamines may be used alone or in combination of two or more.

[0045] Dicarboxylic Acids Examples of dicarboxylic acids include, but are not limited to, aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and aromatic dicarboxylic acids.

[0046] The aliphatic dicarboxylic acid may be a linear saturated aliphatic dicarboxylic acid or a branched saturated aliphatic dicarboxylic acid, and preferably has a carbon number of 3 to 20. Examples of such aliphatic dicarboxylic acids include, but are not limited to, malonic acid, dimethylmalonic acid, succinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, itaconic acid, 2,3-diethylglutaric acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane diacid, and diglycolic acid.

[0047] The number of carbon atoms in the alicyclic structure of the alicyclic dicarboxylic acid (also referred to as alicyclic dicarboxylic acid) is not particularly limited, but is preferably 3 or more and 10 or less, more preferably 5 or more and 10 or less, from the viewpoint of the balance between the water absorbency and the crystallinity of the resulting component.

[0048] The alicyclic dicarboxylic acid may be unsubstituted or may have a substituent. The substituent is preferably an alkyl group having 1 to 4 carbon atoms. Examples of the substituent include, but are not limited to, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group.

[0049] Examples of such alicyclic dicarboxylic acids include, but are not limited to, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,3-cyclopentanedicarboxylic acid.

[0050] Examples of the aromatic dicarboxylic acid include, but are not limited to, unsubstituted or substituted aromatic dicarboxylic acids having from 8 to 20 carbon atoms. Examples of the substituent include, but are not limited to, an alkyl group having from 1 to 6 carbon atoms, an aryl group having from 6 to 12 carbon atoms, an arylalkyl group having from 7 to 20 carbon atoms, a halogen group, an alkylsilyl group having from 3 to 10 carbon atoms, a sulfonic acid group, and a group having a sulfonate salt. Examples of the halogen group include a chloro group and a bromo group. Examples of the salt constituting the group having a sulfonate salt include a sodium salt.

[0051] Examples of such aromatic dicarboxylic acids include, but are not limited to, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, and 5-sodium sulfoisophthalic acid.

[0052] These dicarboxylic acids may be used alone or in combination of two or more.

[0053] Lactams Examples of the lactam include, but are not limited to, butyrolactam, pivalolactam, ε-caprolactam, caprylolactam, enantholactam, undecanelactam, and laurolactam (dodecanelactam). Among these, ε-caprolactam, undecanelactam, and laurolactam (dodecanelactam) are preferred from the viewpoint of polymerization production. These lactams may be used alone or in combination of two or more.

[0054] Aminocarboxylic Acids Examples of aminocarboxylic acids include, but are not limited to, compounds in which the above-mentioned lactams are ring-opened, more specifically, ω-aminocarboxylic acids, α,ω-aminocarboxylic acids, and the like.

[0055] The aminocarboxylic acid may be an aliphatic aminocarboxylic acid or an aromatic aminocarboxylic acid. Examples of the aromatic aminocarboxylic acid include, but are not limited to, para-aminomethylbenzoic acid.

[0056] From the viewpoint of increasing the degree of crystallinity, the aminocarboxylic acid is preferably a linear or branched saturated aliphatic aminocarboxylic acid having from 4 to 14 carbon atoms and substituted with an amino group at the ω position. Specific examples of preferred aminocarboxylic acids include, but are not limited to, 6-aminocaproic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid.

[0057] These aminocarboxylic acids may be used alone or in combination of two or more.

[0058] The polyamide resin is not limited to the following, but examples thereof include polyamide 66 (polyhexamethylene adipamide), polyamide 610 (polyhexamethylene sebacamide), polyamide 612 (polyhexamethylene dodecamide), polyamide 6 (polycaprolactam), polyamide 11 (aminoundecanoic acid copolymer), polyamide 12 (laurolactam copolymer), polyamide 1010 (polydecamethylene secabamide), polyamide 1012 (polydecamethylene dodecamide), and polyamide 116 (polyundecamethylene adipamide). Polyamide MXD6 (polymetaxylylene adipamide), Polyamide 66 / 6I (polyhexamethylene adipamide / polyisophthaladipamide copolymer), Polyamide 6I / 6T (polyisophthaladipamide / polyterephthaladipamide copolymer), Polyamide 6 / 11 (caprolactam / aminoundecanoic acid copolymer), Polyamide 6 / 12 (caprolactam / laurolactam copolymer), Polyamide 6 / 66 / 12 (caprolactam / polyhexamethylene adipamide / laurolactam copolymer), Polyamide TMHT (trimethyl Polyamide 4T (polytetramethylene terephthalamide), Polyamide 4T / Polyamide 6T (polytetramethylene terephthalamide / polyhexamethylene terephthalamide copolymer), Polyamide 6T (polyhexamethylene terephthalamide), Polyamide 2Me-5T (poly 2-methylpentamethylene terephthalamide), Polyamide 9T (polynonamethylene terephthalamide), 2Me-8T (poly 2-methyloctamethylene terephthalamide), Polyamide 6C (polyhexamethylene cyclohexamethylene polyamide 2Me-5C (poly 2-methylpentamethylenecyclohexanedicarboxamide), polyamide 9C (polynonamethylenecyclohexanedicarboxamide), 2Me-8C (poly 2-methyloctamethylenecyclohexanedicarboxamide), polyamide 10T (polydecamethylene terephthalamide), polyamide 11T (polyundecamethylene terephthalamide), polyamide 12T (polydodecamethylene terephthalamide), polyamide 10C (polydecamethylenecyclohexanedicarboxamide),Examples include polyamide 11C (polyundecamethylenecyclohexanedicarboxamide) and polyamide 12C (polydodecamethylenecyclohexanedicarboxamide).

[0059] Among these, examples of the polyamide resins that may be used from the viewpoints of flexibility and chemical resistance include polyamide 610, polyamide 612, polyamide 11, polyamide 12, polyamide 1010, polyamide 1012, polyamide 116, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 12, polyamide 4T (polytetramethylene terephthalamide), and polyamide 4T / polyamide 6T (polytetramethylene terephthalamide / polyhexamethylene terephthalamide copolymer). , polyamide 6T (polyhexamethylene terephthalamide), polyamide 9T, 2Me-8T, polyamide 9C, 2Me-8C, polyamide 10T, polyamide 11T, polyamide 12T, polyamide 10C, polyamide 11C, or polyamide 12C are preferred, and polyamide 610, polyamide 612, polyamide 11, polyamide 12, polyamide 1010, polyamide 1012, polyamide 6 / 11, polyamide 6 / 12, and polyamide 6 / 66 / 12 are particularly preferred.

[0060] The second resin composition preferably has a flexural modulus of 2.0 GPa or less, more preferably 1.5 GPa or less, even more preferably 1.0 GPa or less, particularly preferably less than 0.8 GPa, more preferably 0.6 GPa or less, even particularly preferably 0.5 GPa or less, and even more particularly preferably 0.4 GPa or less. When the flexural modulus is within the above range, the pipe becomes flexible, and the stress during bending is reduced, resulting in excellent bending processability and a tendency to suppress cracking of the pipe when a connector is press-fitted.

[0061] Furthermore, the second resin composition may further contain any polyolefin, elastomer, plasticizer, etc. in order to control the flexural modulus within the above range. Polyolefins and elastomers are generally incompatible with the second matrix resin and tend to form a dispersed phase.

[0062] Furthermore, when the second resin composition is heated from 23° C. at 20° C. / min using a differential scanning calorimeter, it preferably exhibits at least one melting peak at 80° C. or higher but lower than 150° C., more preferably in the range of 100° C. or higher but lower than 140° C., and even more preferably in the range of 105° C. or higher but lower than 130° C. By exhibiting a melting peak in this range, it tends to be possible to obtain a resin pipe that is better balanced between flexibility and high-temperature liquid leakage resistance.

[0063] Furthermore, from the viewpoint of improving flexibility, low-temperature impact resistance, and extensibility in a melt, the second resin composition of this embodiment may contain at least one at least partially crosslinked polyolefin resin or ethylene-α-olefin copolymer. The at least partially crosslinked polyolefin resin and the ethylene-α-olefin copolymer may be the same or different. For example, the second resin composition may contain a crosslinked ethylene-α-olefin copolymer.

[0064] The polyolefin resin may have a functional group reactive with a polyamide resin. The polyolefin resin may contain a component having a melting point of 80° C. or higher.

[0065] The polyolefin resin may be composed of two or more (preferably two) types of resins, but is not limited to the following. For example, it may be composed of two types: an ethylene-α-olefin copolymer having a functional group reactive with the terminal amine group of the polyamide resin, and a crystalline olefin resin exhibiting a melting point of 80°C or higher. It may be composed of two types: a crystalline olefin resin having a functional group reactive with the terminal amine group of the polyamide resin and exhibiting a melting point of 80°C or higher, and an ethylene-α-olefin copolymer. When the polyolefin resin contains two or more components, some or all of the components may be crosslinked. From the viewpoint of preventing poor dispersion in the polyamide composition, it is preferable that all of the components be crosslinked.

[0066] The functional group can be introduced into the polyolefin resin by using a known method. Specific examples include a method of copolymerizing a copolymerizable monomer having a functional group during polymerization, a method of introducing a monomer having a functional group as an end-capping agent during polymerization, and a method of grafting by melt-kneading a polyolefin resin, a monomer having a functional group, and a polymerization initiator. These introduction methods can be used alone or in appropriate combination, and grafting can also be performed simultaneously with the crosslinking reaction described below.

[0067] The polyolefin resin may contain a polyolefin containing one or more α-olefin-derived monomer units. The mass proportion of the α-olefin-derived monomer units among all the monomer units constituting the polyolefin resin is the proportion of the total mass of the α-olefin-derived monomer units contained in all the polyolefin resins, expressed in mass% with the total mass of all the polyolefin resins being 100% by mass. From the viewpoint of achieving impact resistance, high-temperature refrigerant resistance, and low water absorption, the mass proportion of the α-olefin-derived monomer units among the monomer units constituting the polyolefin resin is preferably 3% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 17% by mass or less, and particularly preferably 7% by mass or more and 15% by mass or less. The mass proportion of the α-olefin-derived monomer units among the monomer units constituting the polyolefin resin can be measured by nuclear magnetic resonance spectroscopy or the like. Any method can be used to measure the mass proportion of the α-olefin-derived monomer units among the monomer units constituting the polyolefin resin, but specific examples of the method can be measured using the method described in the Examples below.

[0068] The radical initiator used in crosslinking the polyolefin resin is not particularly limited, and known radical initiators can be used. Examples include persulfates such as potassium persulfate and ammonium persulfate, and various organic peroxides exemplified below, such as alkyl hydroperoxide-based peroxides such as t-butyl hydroperoxide and cumene hydroperoxide, diacyl peroxide-based peroxides such as benzoyl peroxide and lauroyl peroxide, dialkyl peroxide-based peroxides such as di-t-butyl peroxide and t-butyl peroxylaurate, and azo compound-based peroxides such as 2,2'-azobisisobutyronitrile and 2,2'-azobis-2,4-dimethylvaleronitrile. Among these, organic peroxides are preferred for dynamic crosslinking of polyethylene resins, as they have the ability to abstract hydrogen from polyethylene resins. Dialkyl peroxide-based peroxides, which efficiently abstract hydrogen, are more preferred, and 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane is particularly preferred from the viewpoint of reaction rate at processing temperatures. The amount of the crosslinking agent used is preferably about 0.1 to 5 parts by weight, more preferably 0.5 to 3.0 parts by weight, per 100 parts by weight of the polyolefin resin.

[0069] To accelerate the crosslinking, a crosslinking coagent can be added. The coagent typically contains multiple unsaturated groups such as allyl or acrylic esters. Examples of the coagent include N,N'-(m-phenylene)dimaleamide, trimethylolpropane trimethyl acrylate, tetraallyloxyethane, triallyl cyanurate, tetramethylene diacrylate, or polyethylene oxide glycol dimethacrylate. From the viewpoints of reactivity and thermal stability, triallyl cyanurate (TAIC) is preferred. The amount of the coagent used is preferably about 0.1 to 5 parts by weight, more preferably 0.5 to 3.0 parts by weight, per 100 parts by weight of the polyolefin resin.

[0070] An antioxidant can be added to achieve an optimal crosslinking amount and to obtain heat aging resistance. Antioxidants are useful for controlling the crosslinking reaction because they can quench radicals, which are active species in the crosslinking reaction, and stop the reaction. Useful antioxidants include, but are not limited to, phosphorus ester antioxidants, hindered phenol antioxidants, amine antioxidants, or mixtures of two or more of these compounds. Because of their high thermal stability improving effect on polyamide resin compositions, the use of N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide]hindered phenol, available from BASF Japan as Irganox 1098, 3-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionic acid-n-octadecyl, available from Irganox 1076, and 2,2-bis[[[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]oxy]methyl]propane-1,3-diol 1,3-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], available from Irganox 1010, is particularly preferred. The proportion of the antioxidant compound in the polyamide resin composition is preferably 0.01 to 5 parts by weight, more preferably about 0.3 to 2.0 parts by weight, and particularly preferably 0.5 to 1.0 part by weight.

[0071] The method for carrying out the crosslinking reaction is not particularly limited as long as it is a production method including a step of maintaining raw material components containing the polyolefin resin and, if necessary, the crosslinking agent and / or the crosslinking aid at a high temperature. For example, there is a method of mixing the raw material components using a Henschel mixer, a tumbler mixer, or the like, as necessary, and then kneading them using a single-screw or twin-screw extruder, a Banbury mixer, a pressure kneader, or an open roll. From the viewpoints of productivity and ease of kneading with the polyamide resin, it is preferable to carry out the crosslinking reaction by melt kneading in a single-screw or twin-screw extruder, and it is particularly preferable to carry out the crosslinking reaction by melt kneading in a twin-screw extruder.

[0072] The second resin composition may further contain other components as necessary, as long as the effects of this embodiment are not impaired. Examples of other components include, but are not limited to, thermoplastic resins other than those listed above, ultraviolet absorbers, antioxidants, photodegradation inhibitors, heat-resistant materials, plasticizers, lubricants, mold release agents, nucleating agents, flame retardants, colorants, dyes, pigments, fillers, and impact-resistant materials. Because the properties of the other components vary significantly, the appropriate content of each component that does not substantially impair the effects of this embodiment varies. A person skilled in the art can easily determine the appropriate content of each of the other components.

[0073] (C) Intermediate Layer The resin pipe of this embodiment may further include a (C) intermediate layer between the (A) layer and the (B) layer, as needed. The number of (C) intermediate layers may be any number. By including the (C) intermediate layer, the resin pipe of this embodiment tends to be able to further improve its barrier properties, adhesiveness, and other functions.

[0074] The matrix resin contained in the resin composition used in the layer of the (C) intermediate layer that contacts the (B) layer preferably contains the polyamide contained in the matrix resin of the second resin composition used in the (B) layer, or the matrix resin preferably has a functional group reactive with polyamide. This increases the adhesive strength between the portion of the (C) intermediate layer that contacts the (B) layer and the (B) layer, suppresses deformation due to stress relaxation of the (B) layer, and provides a resin pipe that is excellent in balance of refrigerant resistance, pipe bending processability, connector press-fitting ability, and re-bending resistance under actual use conditions. When the matrix resin contained in the resin composition constituting the layer of the (C) intermediate layer that contacts the (B) layer contains polyamide, the polyamide content is not particularly limited, but is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, based on the total amount of the matrix resin as 100%. It may even be 100% by mass.

[0075] Furthermore, it is preferable that the layer of the (C) intermediate layer that is in contact with the (A) layer satisfies any one of the following conditions (1) to (3): (1) the matrix resin contained in the innermost layer (the layer located most radially inward of the pipe) of the (C) intermediate layer and the first matrix resin each contain at least one of the same polymer species, (2) the matrix resin contained in the innermost layer of the (C) intermediate layer has a functional group reactive with the first matrix resin, and (3) the first matrix resin has a functional group reactive with the matrix resin contained in the innermost layer of the (C) intermediate layer. Note that the functional group contained in the matrix resin can be arbitrarily selected from known knowledge depending on the type of the first matrix resin.

[0076] Furthermore, when the (C) intermediate layer is in contact with another (C) intermediate layer, it is preferable that the matrix resins contained in the respective resin compositions contain one or more of the same polymer species, or that the matrix resin of one (C) intermediate layer has a functional group reactive with the matrix resin of the other (C) intermediate layer. The functional group reactive with the matrix resin can be arbitrarily selected from known knowledge depending on the type of material used for the (C) intermediate layer.

[0077] Furthermore, when the resin composition used in the intermediate layer (C) has a functional group that reacts with an adjacent layer, the amount of the functional group is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and particularly preferably 0.15 parts by mass or more, relative to 100 parts by mass of the matrix resin material used in the intermediate layer (C). The upper limit is not particularly limited, but can be 50 parts by mass or less, 30 parts by mass or less, or 20 parts by mass or less.

[0078] The resin composition used in the intermediate layer (C) may further contain other components as necessary, as long as the effects of this embodiment are not impaired. Examples of other components include, but are not limited to, thermoplastic resins other than those listed above, ultraviolet absorbers, antioxidants, photodegradation inhibitors, heat-resistant materials, plasticizers, lubricants, release agents, nucleating agents, flame retardants, colorants, dyes, pigments, fillers, and impact-resistant materials. Because the properties of the other components vary significantly, the appropriate content of each component that does not substantially impair the effects of this embodiment varies. Those skilled in the art can easily determine the appropriate content of each of the other components.

[0079] (Positional Relationship between Layer (A) and Layer (B)) Either the layer formed from the (A) first resin composition or the layer formed from the (B) second resin composition may be located on the outside, but it is more preferable that the layer formed from the (B) second resin composition be located on the outside (radially outward of the pipe), and it is particularly preferable that the layer formed from the (B) second resin composition be the outermost layer (the radially outermost layer of the pipe). By having the layer formed from the (B) second resin composition located on the outside, a resin pipe that is excellent in low-temperature impact resistance, refrigerant resistance, and oil resistance tends to be obtained.

[0080] (Other Conditions of the Resin Pipe) The total thickness of the resin pipe of this embodiment is preferably 0.5 to 3.0 mm, more preferably 0.8 to 2.5 mm, even more preferably 0.9 to 2.0 mm, and most preferably 1.0 to 1.5 mm. In this case, the thickness of Layer (A) is preferably 0.2 mm to 1.0 mm, preferably 0.3 mm to 0.8 mm, and particularly preferably 0.3 to 0.5 mm. The thickness of Layer (B) is preferably 0.5 mm to 2.5 mm, preferably 0.7 mm to 2.0 mm, and particularly preferably 0.8 to 1.5 mm. Note that all of the above thicknesses are average thicknesses.

[0081] The outer diameter of the resin pipe of this embodiment is preferably 8 to 60 mm, more preferably 10 to 40 mm, and most preferably 12 to 30 mm. When the outer diameter is in this range, the pipe tends to have excellent bending workability.

[0082] Furthermore, the outer shape of the resin pipe of this embodiment may be straight or corrugated, or may be straight with only some sections corrugated. A straight shape allows for an increased production speed and is therefore more productive, while a corrugated shape tends to increase the flexibility of the pipe.

[0083] The resin pipe of this embodiment can be obtained by extrusion molding using a known device with the above-described configuration.

[0084] The multilayer resin pipe of this embodiment can withstand short-term peak loads up to 150°C that occur in automotive applications, depending on the type of first resin composition used in the (A) layer and the type of second resin composition used in the (B) layer, and has high resistance to thermal degradation, good burst pressure strength, and excellent bending processability and re-bending properties. The multilayer resin pipe according to the claimed invention is resistant to high temperatures up to about 135°C for ethylene glycol-water mixtures used as refrigerants.

[0085] As described above, the resin pipe of this embodiment has a good balance of flexibility, low-temperature impact resistance, pipe bending workability, resistance to bending back under actual use conditions, and resistance to liquid leakage, and therefore can be used in a variety of applications. For example, it is preferably used as a cooling pipe used in an air or cooling water circuit or as a cooling piping for an automobile.

[0086] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.

[0087] (Constituent Components of Resin Pipe) The constituent components of the resin composition used in each layer of the multilayer pipe sample will be described below. PPE-1: Polyphenylene ether (manufactured by Asahi Kasei Corporation, model number: ZYLON S201A, glass transition temperature 215°C, hydroxy group ratio 0.023%) PPE-2: Maleic anhydride modified polyphenylene ether (manufactured by Asahi Kasei Corporation, model number: ZYLON R4919, glass transition temperature: 215°C, maleic acid modification ratio 0.3%) PS: Polystyrene (manufactured by PS Japan, model number: 685, glass transition temperature 100°C) PA-1: Polyamide 612 (PA612) (manufactured by Asahi Kasei Corporation, model number: Leona 4102, melting point 215°C, glass transition temperature 50°C, amino terminal group ratio 0.06%, carboxy terminal group ratio 0.23%) PA-2: Polyamide 612 (PA612) (manufactured by Asahi Kasei Corporation, model number: Leona 4400, melting point 215°C, glass transition temperature 50°C, amino end group ratio 0.02%, carboxy end group ratio 0.14%) PA-3: Polyamide 12 (PA12) (melting point 175°C, relative viscosity in sulfuric acid 1.9, glass transition temperature 50°C, amino end group ratio 0.06%, carboxy end group ratio 0.18%) *PA-3 was synthesized using a known method to achieve the above physical properties. PA-4: Polyamide 9T (PA9T) (melting point 310°C, relative viscosity in sulfuric acid 2.2, glass transition temperature 120°C, amino end group ratio 0.06%, carboxy end group ratio 0.20%) *PA-4 was synthesized using a known method to achieve the above physical properties.SEBS-1: styrene-ethylene butylene-styrene block copolymer (manufactured by Asahi Kasei Corporation, model number: Tuftec N504) SEBS-2: maleic acid-modified styrene-ethylene butylene-styrene block copolymer (manufactured by Asahi Kasei Corporation, model number: Tuftec M1913, maleic acid modification rate 1.0%) EBR-1: maleic acid-modified ethylene-butene copolymer (manufactured by Mitsui Chemicals, Inc., model number: Tafmer MA8510, maleic acid modification rate 0.5%) p-16: polypropylene (manufactured by Novatec, model number: EA9FTD, glass transition temperature 0°C) p-17: maleic acid-modified polypropylene (manufactured by Mitsui Chemicals, Inc., model number: QB510, glass transition temperature 0°C, maleic acid modification rate 0.04%) p-18: ethylene glycidyl methacrylate copolymer (manufactured by Sumitomo Chemical Co., Ltd., model number: BF2B, glass transition temperature -30°C, glycidyl group ratio 6.0%); antioxidant-1: phenolic antioxidant (manufactured by BASF, model number: Irganox 1098); antioxidant-2: phenolic antioxidant (manufactured by BASF, model number: Irganox 1010).

[0088] The melting point and glass transition temperature of each polyamide resin were measured using a Diamond DSC manufactured by Perkin-Elmer in accordance with ISO 11357. The relative viscosity of each polyamide resin in 96% sulfuric acid was measured in accordance with ISO 307.

[0089] Furthermore, the amino terminal group ratio of each polyamide resin was measured by neutralization titration as follows. First, 3.0 g of the obtained polyamide was dissolved in 100 mL of a 90% by mass aqueous phenol solution. Next, the obtained solution was titrated with 0.025 N hydrochloric acid to determine the amino terminal group ratio (%). The endpoint was determined from the indicated value of the pH meter.

[0090] The maleic anhydride modification rate of each resin was calculated from the ratio of the peak area derived from maleic anhydride to the peak area derived from the matrix resin by proton NMR.

[0091] (Production of Resin Compositions Used in Each Layer) The resin compositions used in each layer of the multi-layer pipe were prepared using a twin-screw extruder TEM26SX manufactured by Shibaura Machine Co., Ltd. A pre-blended resin and antioxidant was fed from the top feed port. The molten mixture extruded from the die head was cooled into strands and pelletized to obtain the resin compositions used in each layer. The cylinder temperature was 280 to 320°C. The matrix resins of each resin composition were as shown in Table 1.

[0092] (Production of Multipurpose Test Pieces) Pellets of the resin composition used in each layer of the multilayer pipe were dried in a nitrogen stream to reduce the moisture content in the resin composition to 500 ppm or less. Next, pellets of the resin composition with the adjusted moisture content were molded into multipurpose test pieces (A-type, dumbbell-shaped tensile test pieces) in accordance with ISO 3167 using an injection molding machine (NEX-50IV, manufactured by Nissei Plastics Co., Ltd.). The dimensions of the multipurpose test piece were: total length ≧ 170 mm, distance between tabs 109.3 ± 3.2 mm, parallel portion length 80 ± 2 mm, shoulder radius 24 ± 1 mm, end width 20 ± 0.2 mm, central parallel portion width 10 ± 0.2 mm, thickness 4 ± 0.2 mm. Specific injection molding conditions were injection and dwell time: 25 seconds, cooling time: 15 seconds. When the resin compositions were p-1 to p-10 and p-13 to p-15, the mold temperature was 80°C and the cylinder temperature was 280°C, when the resin compositions were p-11 and p-12, the mold temperature was 100°C and the cylinder temperature was 330°C, and when the resin compositions were p-16 to p-18, the mold temperature was 20°C and the cylinder temperature was 200°C.

[0093] Example 1 (1) Production of Resin Compositions Used in Each Layer (1-1) Production of Resin Composition p-1 A twin-screw extruder TEM26SX manufactured by Shibaura Machine Co., Ltd. was used to produce the resin compositions used in each layer of the multilayer pipe. A pre-blended resin and antioxidant was fed from the top feed port. The molten mixture extruded from the die head was cooled into strands and pelletized to obtain pellets of resin composition p-1 used in each layer. The cylinder temperature was 240 to 320°C. The type and content of each component are shown in Table 1. (1-2) Production of Resin Compositions p-2 to p-15 Pellets of polyamide resin compositions p-2 to p-15 were obtained using the same method as for resin composition p-1, except that the type and content of each component were as shown in Table 1.

[0094] (2) Production of multilayer pipe Resin compositions p-1 and p-8 were dried at 80°C for 4 hours under reduced pressure to reduce the moisture content in the resin composition to 500 ppm or less. Next, pellets of the resin composition with the adjusted moisture content were placed in two extrusion molding machines (BELLAFORM, BH45-25D). The cylinder temperature was set to 250°C. A resin pipe Pa-1 with an outer diameter of 19 mm and an inner diameter of 16 mm was obtained by passing through a two-layer die.

[0095] [Examples 2 to 9, Examples 14 to 15, Comparative Examples 1 and 4] Resin pipes Pa-2 to Pa-9, Pa-14 to Pa-15, and Pb-1 and Pb-4 were obtained under the same conditions as in Example 1, except that the resin compositions of each layer were as shown in Table 1.

[0096] [Example 10, Example 11] The resin compositions of each layer were as shown in Table 1, and the cylinder temperature of the extruder using p-11 and p-12 was 320 ° C. Except for this, resin pipes Pa-10 and Pa-11 were obtained under the same conditions as in Example 1.

[0097] [Example 12] Resin compositions p-13, p-5, and p-8 were dried at 80°C for 4 hours under a reduced pressure atmosphere to reduce the moisture content in the resin composition to 500 ppm or less. Next, pellets of the resin composition with the adjusted moisture content were charged into three extrusion molding machines (BELLAFORM, BH45-25D). The cylinder temperature was set to 250°C. A resin pipe Pa-12 with an outer diameter of 19 mm and an inner diameter of 16 mm was obtained by passing through a three-layer die.

[0098] [Example 13 and Example 16] Resin pipes Pa-13 and Pa-16 were obtained under the same conditions as in Example 12, except that the resin compositions of each layer were as shown in Table 1 and the cylinder temperature of the intermediate layer was 200 ° C.

[0099] Comparative Example 2 A resin pipe Pb-2 was obtained under the same conditions as in Example 12, except that the resin compositions of each layer were as shown in Table 1 and the cylinder temperatures of the inner and intermediate layers were 200°C.

[0100] Comparative Example 3 A multilayer pipe Pb-3 was obtained in the same manner as in Example 12, except that the resin compositions of each layer were as shown in Table 1, the cylinder temperatures of the inner and intermediate layers were 200°C, and the cylinder temperature of the outer layer was 320°C.

[0101] <Evaluation method>

[0102] (1) Flexural Modulus Using the prepared multipurpose test piece (Type A), a tensile test was performed in accordance with ISO 527 to measure the flexural modulus (GPa). The bending speed was 2 mm / min. When the flexural modulus was 2.0 GPa or less, it was evaluated as having excellent flexibility, bending workability, bending recovery property, and connector press-fitting ability.

[0103] (2) Connector press-fitting test A hose nipple with an outer diameter of 20 mm was press-fitted into the resin pipes obtained in the examples and comparative examples at room temperature. Pipes that could be press-fitted without being damaged were evaluated as having excellent connector press-fitting properties.

[0104] (Evaluation criteria) ○: No damage to the pipe △: Whitening is observed on the pipe ×: Damage to the pipe

[0105] (3) LLC Resistance (Refrigerant Resistance) A connector was press-fitted into the resin pipes obtained in the Examples and Comparative Examples, and a 50% aqueous ethylene glycol solution was poured into the pipe, sealing the ethylene glycol solution inside the pipe. The pipe was placed in an oven at 130°C and heated for 500 hours, after which the ethylene glycol inside was drained and the pipe was washed with pure water. A tensile test was performed using the treated pipe to measure its tensile strength. The tensile strength retention rate of the treated pipe was calculated from the tensile strength of the treated pipe relative to the tensile strength of the treated pipe before treatment. A tensile strength retention rate of 80% or more was considered to be excellent in LLC resistance.

[0106] (4) Bending Angle (Bending Workability of Pipe) The resin pipes obtained in the examples and comparative examples were heated in an oven for 10 minutes, bent to 90°C with an R19 pipe bender, and cooled at room temperature for 5 minutes. The heating temperature was set to the melting point of the resin composition constituting the inner layer and outer layer of the multilayer pipe with the lower melting point -20°C. The bending angle of the pipe after cooling was measured and evaluated according to the following criteria. The closer the bending angle was to 90°C, the better the bending workability was. ◎: 90°≦bending angle≦91° ○: 91°>bending angle≦95° △: 95°>bending angle≦100° ×:bending angle>100°

[0107] (5) Bending Resistance (Bending Resistance in Actual Use Environment) The pipes bent in the evaluation in (4) above were heated in ovens at 80°C, 100°C, and 130°C for one week. The bending angle of the pipes after cooling was measured and evaluated according to the following criteria. The closer the bending angle to 90°C without peeling, the better the bending workability was. ◎: 90°≦bending angle≦95° ○: 95°>bending angle≦100° △: 100°>bending angle≦110° ×:bending angle>110° Peeling: Peeling of each layer was observed during heating in the oven.

[0108] (6) Oil Resistance The resin pipes obtained in the Examples and Comparative Examples were immersed in working oil for 24 hours and evaluated according to the following criteria: ○: No change in the appearance of the pipe ×: Swelling and surface roughness of the pipe

[0109]

[0110]

[0111] From the results in Tables 1 and 2, resin pipes Pa-1 to Pa-16 were superior in flexibility and bending accuracy, while Pa-1 to Pa-13 were even superior in connector press-fitting ability and LLC resistance, as well as in bending angle, bending back resistance, and oil resistance. Furthermore, in a comparison of Pa-10, Pa-11, and Pb-3, which have different flexural moduli of the resin compositions constituting the pipes, the lower the flexural modulus, the better the connector press-fitting ability. Furthermore, in a comparison of Pa-1 to Pa-5, which have different Tg of the inner layer, the higher the Tg of the inner layer, the better the bending back resistance. Furthermore, in a comparison of Pa-1 to Pa-13, which have a polyamide outer layer, with Pb-4, which has a polyphenylene ether outer layer, the polyamide outer layer tended to provide better oil resistance.

[0112] On the other hand, multilayer resin pipes Pa-14 to Pa-16 and Pb-1 to Pb-4 (Examples 14 to 16, Comparative Examples 1 to 4) did not achieve excellent results in connector pressability, LLC resistance, bend angle, rebend resistance, and oil resistance. While Pa-14 and Pa-15 showed good results in connector pressability, LLC resistance, and bend angle, the resin matrix of the inner layer did not contain functional groups reactive with the polyamide of the outer layer, resulting in insufficient adhesion and peeling. Furthermore, Pa-16 showed good results in connector pressability, LLC resistance, and bend angle, but because it contained polyphenylene ether and had a high glass transition temperature as a composition, the glass transition temperature of the polyamide forming the matrix was low, and therefore it was unable to demonstrate good rebend resistance. Furthermore, Pb-4 had a polyphenylene ether layer instead of polyamide in the outer layer, but because the amorphous resin served as the matrix, its oil resistance was insufficient.

[0113] Examples of other embodiments of the present invention will be described below, but the present invention is not limited to the following examples.

[0114] (Constituent Components of Resin Pipe) Hereinafter, each constituent component of the resin composition used in each layer of the multilayer pipe sample will be described. PPE-2-1: Polyphenylene ether (manufactured by Asahi Kasei Corporation, model number: ZYLON S201A, glass transition temperature 215°C, hydroxy group ratio 0.023%) PPE-2-2: Maleic anhydride modified polyphenylene ether (manufactured by Asahi Kasei Corporation, model number: ZYLON R4919, glass transition temperature: 215°C, maleic acid modification ratio 0.3%) PS: Polystyrene (manufactured by PS Japan, model number: 685, glass transition temperature 100°C) PA-2-1: Polyamide 612 (PA612) (manufactured by Asahi Kasei Corporation, model number: Leona 4102, melting point 215°C, glass transition temperature 50°C, amino group terminal ratio 0.06%, carboxy group terminal ratio 0.23%) PA-2-2: Polyamide 9T (PA9T) (melting point 310°C, relative viscosity in sulfuric acid 2.2, glass transition temperature 120°C, amino terminal group ratio 0.06%, carboxy terminal group ratio 0.20%) *PA-2-2 was synthesized by a known method so as to have the above physical properties.SEBS-2-1: styrene-ethylene butylene-styrene block copolymer (manufactured by Asahi Kasei Corporation, model number: Tuftec N504) EBR-2-1: maleic acid grafted ethylene-butene copolymer (manufactured by Mitsui Chemicals, Inc., melting point: 70°C, model number: Tafmer MA8510, MFR: 2.4 g / 10 min, acid modification rate: 0.50 mass%, weight average molecular weight: 51,500) EBR-2-2: maleic acid grafted ethylene-butene copolymer (manufactured by Mitsui Chemicals, Inc., melting point: 80°C, model number: Tafmer MA9015, MFR: 11 g / 10 min, acid modification rate: 0.75 mass%, weight average molecular weight: 29,800) p2-3: polypropylene (manufactured by Novatec, model number: EA9FTD, glass transition temperature 0°C) p2-4: maleic acid modified polypropylene (manufactured by Mitsui Chemicals, Inc., model number: QB510, glass transition temperature 0°C, maleic acid modification rate 0.04%) Antioxidant-2-1: phenolic antioxidant (manufactured by BASF, model number: Irganox 1098) Antioxidant-2-2: phenolic antioxidant (manufactured by BASF, model number: Irganox 1010) Crosslinker-2-1: 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane (model number: Perhexa 25B-40, CAS number: 78-63-7, manufactured by NOF Corporation, diluted with silica, purity 40% by weight) Crosslinking aid-2-1: triallyl isocyanate (model number: Taiku M-60, CAS number 1025-15-6, manufactured by Mitsubishi Chemical Corporation, diluted with calcium silicate and having a purity of 60% by weight).

[0115] The melting point and glass transition temperature of each matrix resin were measured in accordance with ISO 11357 using a Diamond DSC manufactured by Perkin-Elmer, and are shown in Table 3. The relative viscosity in 96% sulfuric acid of each of the polyamide resins was measured in accordance with ISO 307.

[0116] The melting peak of the second resin composition polyamide resin composition was measured in accordance with JIS-K7121 using a Diamond DSC manufactured by Perkin-Elmer, and the results are shown in Table 3. At this time, the temperature at the top of the peak observed in the range of 100°C or higher and lower than 150°C was taken as the melting peak (°C) of 100°C or higher and lower than 150°C. When multiple melting peaks of 100°C or higher and lower than 150°C were observed, the peak with the largest melting enthalpy was taken as the melting peak of 100°C or higher and lower than 150°C.

[0117] Furthermore, the amino terminal group ratio of each of the polyamide resins was measured by neutralization titration as follows. First, 3.0 g of the obtained polyamide was dissolved in 100 mL of a 90% by mass aqueous phenol solution. Next, the obtained solution was titrated with 0.025 N hydrochloric acid to determine the amino terminal group ratio (%). The endpoint was determined from the indicated value of the pH meter.

[0118] The maleic anhydride modification rate of each of the resins was calculated from the ratio of the peak area derived from maleic anhydride to the peak area derived from the matrix resin by proton NMR.

[0119] Furthermore, the proportion of α-olefin-derived components (α-olefin ratio) among the monomer components constituting the polyolefin resin was quantified by extracting the polyolefin component from the composition or molded article and analyzing the components by nuclear magnetic resonance spectroscopy, and the results are shown in Table 3. 5 mL of hexafluoroisopropanol (HFIP) and 5 mL of chloroform were added to 1 g of pellets, and the mixture was allowed to stand for 18 hours. The remaining suspended matter was separated, and 5 mL of HFIP and 5 mL of chloroform were added again, followed by centrifugation at 3000 rpm for 1 hour to separate the suspended matter. Centrifugation and collection of the suspended matter were repeated three times, and the resulting suspended matter was vacuum-dried to recover a black solid. Next, 5 mL of hexafluoroisopropanol (HFIP) and 15 mL of chloroform were added to 100 mg of the resulting solid, and the suspended matter was collected and vacuum-dried to obtain a solid. 4 mg of this solid was dissolved in deuterated orthodichlorobenzene and heated at 140 °C. 1H-NMR measurement was performed. The α-olefin ratio (mass %) was determined from the integral ratio of the peaks in the range of 1 to 2 ppm and the molecular weights of the constituent monomers.

[0120] (Production of Resin Compositions Used in Each Layer) The resin compositions used in each layer of the multi-layer pipe were prepared using a twin-screw extruder TEM26SX manufactured by Shibaura Machine Co., Ltd. A pre-blended resin and antioxidant was fed from the top feed port. The molten mixture extruded from the die head was cooled into strands and pelletized to obtain the resin compositions used in each layer. The cylinder temperature was 280 to 320°C. The matrix resins of each resin composition were as shown in Table 3.

[0121] (Production of Multipurpose Test Pieces) Pellets of the resin composition used in each layer of the multilayer pipe were dried in a nitrogen stream to reduce the moisture content in the resin composition to 500 ppm or less. Next, pellets of the resin composition with the adjusted moisture content were molded into multipurpose test pieces (A-type, dumbbell-shaped tensile test pieces) in accordance with ISO 3167 using an injection molding machine (NEX-50IV, manufactured by Nissei Plastics Co., Ltd.). The dimensions of the multipurpose test piece were: total length ≧ 170 mm, distance between tabs 109.3 ± 3.2 mm, parallel portion length 80 ± 2 mm, shoulder radius 24 ± 1 mm, end width 20 ± 0.2 mm, central parallel portion width 10 ± 0.2 mm, thickness 4 ± 0.2 mm. Specific injection molding conditions were injection and dwell time: 25 seconds, cooling time: 15 seconds. When the resin compositions were p2-1, p2-5 to p2-19, the mold temperature was 80°C and the cylinder temperature was 280°C; when the resin composition was p2-2, the mold temperature was 100°C and the cylinder temperature was 330°C; and when the resin compositions were p2-3 to p2-4, the mold temperature was 20°C and the cylinder temperature was 200°C.

[0122] Flexural Modulus of Multipurpose Test Pieces Using the multipurpose test pieces (Type A) prepared as described above, a tensile test was performed in accordance with ISO 527 to measure the flexural modulus (GPa), which is shown in Table 3. The bending speed was 2 mm / min. A flexural modulus of 2.0 GPa or less was evaluated as being excellent in flexibility, bending workability, bending recovery property, and connector press-fitting ability.

[0123] - Confirmation of Matrix Components The matrix components in each resin composition were confirmed as follows. Pellets of the polyamide resin composition prepared using the method described below were cut parallel to the flow direction. After trimming the sample, the cut surface was smoothed using a diamond knife on a cryomicrotome (Leica UC6). Subsequently, the cut surface was stained using a 5 wt% aqueous solution of phosphotungstic acid. After staining, a 100 nm depth was cut off from the surface of the cut surface using a diamond knife on a cryomicrotome (Leica UC6) to remove deposits derived from the dye. The sample was fixed to a sample stage using carbon paste and used as an observation sample. The observation sample was irradiated with an electron beam using a scanning electron microscope (Hitachi High-Tech SU8220) under the conditions of lens mode High, acceleration voltage 1 kV, and working distance 5 mm, and observation was performed. An Upper LA100 detector was used (backscattered electron image). The field of view angle was adjusted so that the left and right directions of the image were parallel to the flow direction. The component observed with bright luminance was regarded as the polyamide resin, and the component observed with dark luminance as the polyolefin component, and the dispersibility was evaluated. The components forming the matrix phase were judged according to the following criteria.

[0124] Example 2-1 (1) Preparation of Resin Compositions Used in Each Layer (1-1) Preparation of Resin Composition p2-1 A twin-screw extruder TEM26SX manufactured by Shibaura Machine Co., Ltd. was used to prepare the resin compositions used in each layer of the multilayer pipe. A pre-blended resin and antioxidant were fed through the top feed port. The molten mixture extruded from the die head was cooled into strands and pelletized to obtain pellets of resin composition p2-1 used in each layer. The cylinder temperature was 240 to 320°C. The type and content of each component are shown in Table 3. (1-2) Preparation of Resin Compositions p2-2, 13, and 19 Pellets of polyamide resin compositions p2-2, 13, and 19 were obtained using the same method as for resin composition p2-1, except that the type and content of each component were as shown in Table 3. (1-3) Preparation of Resin Composition p2-5 A twin-screw extruder TEM26SX manufactured by Shibaura Machine Co., Ltd. was used. A pre-blended mixture of (B) polyolefin resin, (C) crosslinking agent, and (D) crosslinking aid was fed through the top feed port. Furthermore, a pre-blended mixture of (A) polyamide resin and antioxidant was fed through the side feed port located on the fifth barrel. The molten mixture extruded from the die head was cooled into strands and pelletized to obtain pellets of polyamide resin composition E1. The type and content of each component were as shown in Table 3. (1-4) Production of Resin Compositions p2-6 to p2-12 and p2-14 to 18. Pellets of polyamide resin compositions p2-6 to p2-12 and p2-14 to 18 were obtained using the same method as for resin composition p2-5, except that the type and content of each component were as shown in Table 3.

[0125] (2) Production of Multilayer Pipe Resin compositions p2-1 and p2-5 were dried at 80°C for 4 hours under reduced pressure to reduce the moisture content in the resin composition to 500 ppm or less. Next, pellets of the resin composition with the adjusted moisture content were placed into two extrusion molding machines (BELLAFORM, BH45-25D). The cylinder temperature for the outer layer was 300°C, and the cylinder temperature for the inner layer was 280°C. A resin pipe E-1 was obtained through a two-layer die, with an outer diameter of 19 mm, an inner diameter of 16 mm, an inner layer thickness of 0.3 mm, and an outer layer thickness of 1.2 mm. The type, adhesive mode, type of matrix resin, type, amount, and Tg of functional groups, and flexural modulus of elasticity of the resin composition used in each layer are shown in Table 4.

[0126] [Examples 2-2 to 2-8, Examples 2-11 to 2-13, Comparative Examples 2-1 to 2-4, Comparative Examples 2-6, and 2-7] Resin pipes E2-2 to E2-8, E2-11 to E-2-13, and C2-1 to C2-4, 6, and 7 were obtained under the same conditions as in Example 2-1, except that the resin compositions of each layer were as shown in Table 4.

[0127] [Example 2-9] A resin pipe P2-9 was obtained under the same conditions as in Example 2-1, except that the resin compositions of each layer were as shown in Table 4 and the cylinder temperature of the extruder using p2-2 was 320°C.

[0128] [Example 2-10] Resin compositions p2-5 and p2-1 were dried at 80°C under reduced pressure for 4 hours to reduce the moisture content in the resin compositions to 500 ppm or less. Next, pellets of the resin compositions with adjusted moisture content were loaded into two extrusion molding machines (BELLAFORM, BH45-25D). The cylinder temperature for the outer layer was 300°C, and the cylinder temperature for the inner layer was 280°C. The extrusion was passed through a two-layer die to obtain a resin pipe E2-10 with an outer diameter of 19 mm and an inner diameter of 16 mm. The thicknesses of the inner and outer layers were reversed compared to E2-1. The type, adhesive mode, type of matrix resin, type, amount, and Tg of functional groups, and flexural modulus of the resin compositions used in each layer are shown in Table 4.

[0129] [Comparative Example 2-5] Resin compositions p2-3, p2-4, and p2-5 were dried under reduced pressure at 80°C for 4 hours to reduce the moisture content in the resin composition to 500 ppm or less. Next, pellets of the resin composition with the adjusted moisture content were placed into three extrusion molding machines (BELLAFORM, BH45-25D). The cylinder temperature of the outer layer was 250°C, and the cylinder temperatures of the inner and intermediate layers were 200°C. A resin pipe C2-5 was obtained through a three-layer die, with an outer diameter of 19 mm, an inner diameter of 16 mm, an inner layer thickness of 0.375 mm, an intermediate layer thickness of 0.225 mm, and an outer layer thickness of 0.9 mm. The type, adhesive mode, type of matrix resin, type, amount, and Tg of functional groups, and flexural modulus of elasticity of the resin composition used in each layer are shown in Table 4.

[0130] [Example 2-14] Resin compositions p2-1 and p2-13 were dried at 80°C for 4 hours under reduced pressure to reduce the moisture content in the resin composition to 500 ppm or less. Next, pellets of the resin composition with the adjusted moisture content were placed into three extrusion molding machines (BELLAFORM, BH45-25D). The cylinder temperatures of the outer and inner layers were 300°C, and the cylinder temperature of the intermediate layer was 280°C. The resin pipe C-11 was obtained through a three-layer die, with an outer diameter of 19 mm, an inner diameter of 16 mm, an inner layer thickness of 0.2 mm, an intermediate layer thickness of 0.1 mm, and an outer layer thickness of 1.2 mm. The type, adhesive mode, type of matrix resin, type, amount, and Tg of functional groups, and flexural modulus of elasticity of the resin composition used in each layer are shown in Table 4.

[0131] <Evaluation> Each of the obtained resin pipe samples was evaluated as follows. The evaluation results are shown in Table 4.

[0132] (1) Tensile Modulus of Elasticity The resin pipes obtained in the Examples and Comparative Examples were subjected to a tensile test using an Instron universal testing machine (capacity: 100 kN, model: 5582) and a pipe shape fixture to measure the tensile modulus of elasticity (GPa). The tensile speed was 50 mm / min. A pipe having a tensile modulus of elasticity of 1.0 GPa or less was evaluated as having excellent flexibility.

[0133] (2) Low-temperature impact resistance test After the resin pipes obtained in the examples and comparative examples were allowed to stand at -40°C for 2 hours or more, the pipes were fixed to the sample setting section of a Charpy impact tester (model: DG CB) manufactured by Toyo Seiki Seisakusho, and an impact was applied with a 7.5 J hammer. The state of the pipes was then observed and evaluated according to the following criteria. (Evaluation criteria) ○: No damage to the pipe △: The surface of the pipe was damaged, but no leakage occurred when liquid was passed through it ×: The pipe was damaged, and liquid leaked when liquid was passed through it

[0134] (3) Bending Angle (Bending Workability of Pipe) The resin pipes obtained in the Examples and Comparative Examples were heated in an oven for 10 minutes, bent to 90° using an R19 pipe bender, and cooled at room temperature for 5 minutes. The heating temperature was set to the melting point of the resin composition constituting the inner layer and outer layer of the multilayer pipe with the lower melting point -20°C. The bending angle of the pipe after cooling was measured and evaluated according to the following criteria. The closer the bending angle was to 90°, the better the bending workability was evaluated. ◎: 90°≦bending angle≦91° ○: 91°>bending angle≦95° △: 95°>bending angle≦100° ×:bending angle>100°

[0135] (4) Bending Resistance (Bending Resistance Under Various Temperature Environments) The pipes bent in the evaluation of (4) above were heated in ovens at 80°C, 100°C, and 130°C for one week. Regarding 80°C LLC-sealed bending resistance, a connector was press-fitted into the resin pipes obtained in the Examples and Comparative Examples, a 50% by volume aqueous solution of ethylene glycol was poured into the pipe, and the ethylene glycol aqueous solution was sealed inside the pipe. The pipes were then placed in an oven at 80°C and heated for one week. The bending angle of the pipes after cooling was measured and evaluated according to the following criteria. The closer the bending angle to 90° was to the absence of peeling and the bending processability, the better the bending workability. ⊚: 90°≦bending angle≦95°; ◯: 95°>bending angle≦100°; △: 100°>bending angle≦110°; ×: bending angle>110°

[0136] (5) Presence or absence of liquid leakage at 100°C A connector was press-fitted into the resin pipes obtained in the examples and comparative examples, and a 50% by volume aqueous solution of ethylene glycol was poured into the pipe, sealing the ethylene glycol aqueous solution inside the pipe. This pipe was placed in an oven at 100°C and heated for 1000 hours, after which the presence or absence of liquid leakage from the connector of the treated pipe was confirmed. The evaluation was performed according to the following criteria: ◎ (Excellent): 60% or more of the solution remains, and there is no sign of liquid leakage at the connector. ○ (Excellent): 60% or more of the solution remains, but there is a sign of liquid leakage at the connector. △ (Good): The remaining amount of solution is less than 60%, and there is a sign of liquid leakage at the connector. × (Poor): The connector is loose / the pipe does not maintain its shape.

[0137]

[0138]

[0139] The results in Tables 3 and 2 show that the resin pipe samples E2-1 to E2-14 were excellent in flexibility, pipe bending workability, re-bending resistance under actual use environments, and liquid leakage resistance, while the resin pipe samples E2-1 to E2-10 were excellent in all of flexibility, low-temperature impact resistance, pipe bending workability, re-bending resistance under actual use environments, and liquid leakage resistance. Furthermore, in a comparison of E2-1 and E2-9, which have different matrix resins in the resin compositions constituting the inner layer, it was found that the use of PPE / PS resin as the matrix resin reduced re-bending, and in particular suppressed the tendency for re-bending to increase upon contact with 80°C LLC.

[0140] On the other hand, the multilayer resin pipes E2-10 to E2-14 and C2-1 to C2-7 (Examples 2-10 to 2-14, Comparative Examples 2-1 to 2-11) did not achieve excellent results in all aspects: flexibility, low-temperature impact resistance, pipe bending workability, re-bending resistance under actual use environments, and leakage resistance. Although the resin pipes E2-11 to E2-13 showed good results in pipe bending workability, re-bending resistance under actual use environments, and leakage resistance, the low-temperature impact resistance was insufficient, and there was room for improvement in flexibility, bending workability, and re-bending resistance. Furthermore, the resin pipes C2-1 to C2-4 had insufficient leakage resistance at 100 ° C. The resin pipes C2-5 to C2-7 had insufficient re-bending resistance and leakage resistance at 100 ° C, and there was also room for improvement in bending workability. Furthermore, although the resin pipe E2-14 showed good results in terms of pipe bending workability, resistance to bending back under actual use conditions, and resistance to liquid leakage, its low-temperature impact resistance was insufficient, and there was room for improvement in resistance to bending back.

[0141] According to the present invention, a multi-layer resin pipe having excellent flexibility and bending workability in a well-balanced manner can be provided. The resin pipe of the present invention can be used as a material for various parts for automobiles, the machinery industry, industrial materials, industrial materials, daily necessities, household goods, etc.

Claims

1. A multi-layered resin pipe having at least (A) a layer formed from a first resin composition and (B) a layer formed from a second resin composition, wherein the first resin composition contains a first matrix resin and optionally other components, and the glass transition temperature of the first matrix resin is 100°C or higher, and the second resin composition contains a second matrix resin containing polyamide and optionally other components.

2. The resin pipe according to claim 1, characterized in that the layer formed from the (A) first resin composition is an innermost layer, the layer formed from the (B) second resin composition is an outermost layer, the innermost layer is in contact with the inside of the outermost layer, and the first matrix resin has a functional group reactive with the polyamide or contains a polyamide.

3. The resin pipe according to claim 1, characterized in that: a layer formed from said (A) first resin composition is an innermost layer; a layer formed from said (B) second resin composition is an outermost layer; and the resin pipe further comprises one or more (C) intermediate layers provided between said innermost layer and said outermost layer; said (C) intermediate layer contains a matrix resin and optionally other components; a matrix resin in a resin composition forming one of said (C) intermediate layers that contacts the inside of said layer formed from said (B) second resin composition has a functional group reactive with said polyamide or contains polyamide; when said (C) intermediate layer is composed of a plurality of layers, the matrix resins contained in the respective resin compositions contain one or more of the same polymer species, or the matrix resin of any of said (C) intermediate layers has a functional group reactive with the matrix resin of the other (C) intermediate layer; and further satisfies any of the following conditions (1) to (3): (1) The matrix resin contained in the innermost layer of the (C) intermediate layer and the first matrix resin each contain at least one of the same polymer species. (2) The matrix resin contained in the innermost layer of the (C) intermediate layer has a functional group reactive with the first matrix resin. (3) The first matrix resin has a functional group reactive with the matrix resin contained in the innermost layer of the (C) intermediate layer.

4. A resin pipe as described in claim 2 or 3, characterized in that the first resin composition has a flexural modulus at room temperature of 2.0 GPa or less.

5. The resin pipe according to claim 4, wherein the first resin composition has a flexural modulus of elasticity of 1.5 GPa or less at room temperature.

6. A resin pipe as described in claim 2 or 3, characterized in that the second resin composition has a flexural modulus at room temperature of 1.5 GPa or less.

7. The resin pipe according to claim 6, wherein the second resin composition has a flexural modulus at room temperature of 1.0 GPa or less.

8. The resin pipe according to claim 2 or 3, wherein the glass transition temperature of the first resin composition is 115°C or higher.

9. A resin pipe as described in claim 2 or 3, characterized in that the first resin composition contains a polyphenylene ether resin, and the content of the polyphenylene ether resin in 100 parts by weight of the first resin composition is 10 parts by weight or more.

10. A resin pipe as described in claim 2 or 3, characterized in that the first matrix resin contains a polyphenylene ether resin, and the content of the polyphenylene ether resin in 100 parts by weight of the first matrix resin is 10 parts by weight or more.

11. The resin pipe according to claim 2 or 3, wherein the first matrix resin is amorphous.

12. The resin pipe according to claim 7, wherein the glass transition temperature of the first resin composition is 130° C. or higher.

13. A resin pipe as described in claim 2 or 3, characterized in that a matrix resin in the resin composition forming a layer that contacts the inner side of the layer formed from the (B) second resin composition has a functional group reactive with the polyamide, and the functional group reactive with the polyamide is at least one selected from a carboxy group, an acid anhydride, an amino group, a glycidyl group, an oxazoline group and functional groups derived therefrom.

14. A resin pipe as described in claim 2 or 3, characterized in that the polyamide content relative to 100 mass% of matrix resin in the resin composition forming a layer that contacts the inner side of the layer formed from the second resin composition (B) is 50 mass% or more, and the polyamide content relative to 100 mass% of the first matrix resin is 50 mass% or more.

15. The resin pipe according to claim 1, wherein the second resin composition has a flexural modulus of elasticity of less than 0.8 GPa.

16. The resin pipe described in claim 15, characterized in that the layer formed from the (A) first resin composition and the layer formed from the (B) second resin composition are in contact with each other, and the first matrix resin has a functional group reactive with the polyamide or contains a polyamide.

17. A resin pipe as described in claim 15 or 16, characterized in that the layer formed from the second resin composition (B) is located outside the layer formed from the first resin composition (A).

18. A resin pipe as described in claim 15 or 16, characterized in that the water absorption rate of the first matrix resin is less than 1.0%.

19. A resin pipe as described in claim 15 or 16, characterized in that the water absorption rate of the first resin composition is less than 1.0%.

20. A resin pipe as described in claim 15 or 16, characterized in that when the total amount of the resin components of the second resin composition is 100 parts by weight, the content of the polyamide resin is 50 parts by weight or less.

21. The resin pipe according to claim 15 or 16, wherein the second resin composition contains a polyolefin resin, and at least a portion of the polyolefin resin is crosslinked.

22. A resin pipe as described in claim 15 or 16, characterized in that the second resin composition contains polyolefin resins, at least one of the polyolefin resins contains monomer units derived from α-olefins, and the mass proportion of monomer units derived from α-olefins among all monomer units constituting the polyolefin resin is 3 mass% or more and 20 mass% or less.

23. A resin pipe as described in claim 15 or 16, characterized in that the second resin composition exhibits at least one melting peak of 80°C or higher and less than 150°C when heated from 23°C at 20°C / min using a differential scanning calorimeter.

24. A resin pipe as claimed in any one of claims 1 to 3, 15 and 16, which is used in an air or cooling water circuit.

25. A resin pipe according to any one of claims 1 to 3, 15 and 16, which is used as a cooling piping for an automobile.

Citation Information

Patent Citations

  • Piping member

    JP2008291183A

  • Multilayer co-extruded tubes

    JP2012529396A

  • Molded article for piping

    JP2017075264A

  • Multilayer structures containing continuous fibers for heat transfer fluids - Patent Application 20070122997

    JP2019501797A

  • Polyamide compositions and articles made therefrom

    JP2022553748A