Porous carbon dioxide capture agent and manufacturing method therefor
The method addresses the inefficiencies of existing CO2 capture technologies by synthesizing a porous carbon dioxide collector using a metal-organic framework with a transition metal precursor, an alkali metal precursor, and an organic acid, achieving high CO2 capture efficiency and selectivity while minimizing solvent use and energy consumption, making it suitable for industrial-scale, environmentally friendly production.
Patent Information
- Application Number
- PCT/KR2023/017111
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2023-10-31
- Publication Date
- 2024-11-28
AI Technical Summary
Current carbon capture technologies, particularly chemical absorption methods, face challenges such as toxicity, energy inefficiency, and environmental pollution due to the use of excessive organic solvents in the synthesis of metal-organic frameworks (MOFs) for CO2 capture, which limits their industrial application and increases manufacturing costs.
A method for producing a porous carbon dioxide collector using a metal-organic framework synthesized with a transition metal precursor, an alkali metal precursor, and an organic acid in an aqueous solution, utilizing pure water as a solvent and a cyclic condensation process at controlled temperatures and times to reduce solvent usage and energy consumption, resulting in a material with high specific surface area and CO2/N2 selectivity.
The method enables the production of a porous carbon dioxide collector with a specific surface area of 750-1000 m^2/g, pore volume of 0.6-1.0 cm^3/g, and CO2/N2 selectivity of 110-130, suitable for mass production and environmentally friendly, while reducing manufacturing costs and environmental impact.
Smart Images

Figure KR2023017111_28112024_PF_FP_ABST
Abstract
Description
Porous carbon dioxide capture agent and method for producing the same
[0001] The present invention relates to a porous carbon dioxide capture agent and a method for producing the same, and more particularly, to a porous carbon dioxide capture agent and a method for producing the same using an environmentally friendly synthesis method.
[0002] CO2 contributes to global warming and extreme weather events. Approximately 45% of CO2 in the environment comes from various industries, such as thermal power plants, cement, and steel production. Atmospheric CO2 levels have increased from 280 ppm in the early 1800s to over 400 ppm in 2018, and recent studies predict that CO2 levels could reach at least 550 ppm by 2050 and 950 ppm by 2100. Global efforts are underway to control atmospheric CO2 concentrations by using non-carbon energy sources and reducing fossil fuel use. However, current energy generation technologies based on fossil fuels are still in use. Therefore, carbon capture and storage (CCS) is one promising technology for controlling atmospheric CO2 concentrations.
[0003] In recent years, many CO2 capture technologies have been established, including physical adsorption, chemical absorption, cryogenic distillation, and membrane separation. Among these, chemical absorption is commonly used for CO2 capture, utilizing aqueous amine solutions due to its simple operation. However, this chemical absorption method has several drawbacks, including toxicity, solution loss, equipment corrosion, and the high energy requirement for regeneration. Therefore, the challenge lies in developing a promising adsorbent that possesses high CO2 capacity and selectivity, competitive production costs, and minimal environmental impact.
[0004] To solve the above problems, solid adsorbents such as activated carbon, zeolites, mesoporous silica, covalent organic frameworks (COFs), and metal organic frameworks (MOFs) have been used as CO2 adsorbents.
[0005] Among these, metal-organic frameworks are nanoporous materials that have very well-defined pore sizes, as well as high surface areas, pore volumes, and rigid structures. In addition, the pore size and the chemical environment within the pores can be easily controlled by selecting appropriate organic ligands, i.e., bidentate compounds, and they have the advantages of excellent heat and chemical resistance. Porous metal-organic frameworks are composed of metal oxide aggregates and organic linkers, and the coordination structures formed from these metal ion moieties and organic ligands can form various framework structures, ranging from simple molecular forms through self-assembly to linear primary structures, plate-like secondary structures, and complex three-dimensional structures. A typical synthetic method is solvothermal synthesis, which uses a polar solvent to dissolve the precursors of each component at an appropriate concentration, places them in a sealed container, and heats them to synthesize them under the pressure generated by the self-generation.
[0006] However, these synthetic methods are extremely energy-intensive and inefficient, requiring reaction times exceeding several days to obtain fully crystalline MOF compounds due to the extremely slow nucleation and crystallization processes. Furthermore, the inefficient synthesis methods of porous MOFs, which significantly increase manufacturing costs, have been identified as an obstacle to industrial application. Furthermore, these typical synthetic methods have limitations in surface area and adsorption capacity, and the excessive use of organic solvents can cause environmental pollution. Consequently, these methods pose challenges for industrial application.
[0007] The present invention has been devised to solve the above problems, and aims to provide a porous carbon dioxide capture agent and a method for producing the same, which can be manufactured in an environmentally friendly manner and reduce the burden of manufacturing costs by reducing the use of organic solvents.
[0008] As a means for achieving the above-described object, the present invention provides a method for producing a porous carbon dioxide capture agent, comprising the steps of: preparing a metal-organic framework precursor aqueous solution by adding a transition metal precursor, an alkali metal precursor, and an organic acid to water; circulating and condensing the prepared metal-organic framework precursor aqueous solution; and drying the condensed metal-organic framework precursor aqueous solution.
[0009] Here, the transition metal precursor may include dimethyl zinc, diethyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate, and zinc sulfate.
[0010] Here, the alkali metal precursor may include at least one material selected from the group consisting of potassium hydroxide, sodium hydroxide, lithium oxide, barium oxide, potassium carbonate, sodium carbonate, lithium carbonate, barium carbonate, sodium methoxide, sodium ethoxide, potassium ethoxide, and potassium isopropoxide.
[0011] Here, the organic acid may be at least one substance selected from the group consisting of acetic acid, formic acid, citric acid, oxalic acid, and ascorbic acid.
[0012] Here, the transition metal precursor and the alkali metal precursor may be included in a molar ratio of 1:1 to 1:5.
[0013] Here, the heating temperature in the above-mentioned cyclic condensation step may be 80 to 120°C.
[0014] Here, the heating time in the above-mentioned cyclic condensation step may be 5 to 10 hours.
[0015] Here, the drying step can be performed in a vacuum.
[0016] In addition, as a means for achieving the above-described purpose, the present invention provides a porous carbon dioxide capture agent formed using a composition including a transition metal precursor, an alkali metal precursor, and an organic acid.
[0017] Here, the specific surface area of the porous carbon dioxide capture agent is 750 to 1000 m 2 / g may be.
[0018] Here, the pore volume of the porous carbon dioxide capture agent is 0.6 to 1.0 cm 3 / g may be.
[0019] Here, the CO2 / N2 selectivity of the porous carbon dioxide capture agent may be 110 to 130.
[0020] Here, the XRD spectrum peaks (2θ) of the porous carbon dioxide capture agent formed above can appear at 7.4°, 11.26°, 13.61°, 15.5°, 21.19°, 25.28°, 26.22°, 27.99°, 28.8°, 35.63°, and 37.17°.
[0021] The method for manufacturing the porous carbon dioxide capture agent of the present invention can be environmentally friendly, as it uses only pure water as a solvent for synthesis.
[0022] In addition, the method for manufacturing the porous carbon dioxide capture agent of the present invention can be suitable for mass production through a simple manufacturing method.
[0023] In addition, the porous carbon dioxide capture agent manufactured according to the method of the present invention can exhibit high CO2 / N2 selectivity.
[0024] Figure 1 is a flowchart showing the manufacturing process of the porous carbon dioxide capture agent of the present invention.
[0025] FIG. 2 is a schematic diagram showing the crystal structure of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention.
[0026] FIG. 3 is an SEM image of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention.
[0027] FIG. 4 is an XRD spectrum of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention.
[0028] Figure 5 is a graph showing six adsorption isotherms according to IUPAC (International Union of Pure and Applied Chemistry).
[0029] FIG. 6 is a graph showing an N2 adsorption isotherm of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention.
[0030] FIG. 7 is a graph showing CO2 and N2 adsorption isotherms of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention.
[0031] FIG. 8 is a graph showing the CO2 / N2 selectivity of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention.
[0032] FIG. 9 is a graph showing a CO2 adsorption isotherm of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention.
[0033] The present invention is susceptible to various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, this is not intended to limit the present invention to specific embodiments, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.
[0034] Throughout this specification, whenever a part is said to "include" a component, this means that it may include other components, but not to the exclusion of other components, unless otherwise specifically stated.
[0035] The terms "about," "substantially," and the like, as used herein, are used to mean at or near the numerical value when manufacturing and material tolerances inherent to the meanings stated are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that contain precise or absolute numerical values to aid understanding of the present disclosure. Furthermore, throughout the present disclosure, the terms "step of doing" or "step of" do not mean "step for."
[0036] Those skilled in the art will appreciate that the gist of the present invention can be applied in a variety of ways, and therefore the scope of the present invention is not limited to the following examples. The scope of the present invention extends to any portion that would be readily replaceable or modified by a person skilled in the art using prior art, based on the matters set forth in the claims.
[0037] Hereinafter, the present invention will be described in more detail with reference to the attached drawings when necessary.
[0038]
[0039] <Method for manufacturing a porous carbon dioxide capture agent>
[0040] As a means for achieving the above-described purpose, the present invention provides a method for producing a porous carbon dioxide capture agent.
[0041] Figure 1 is a flow chart showing the manufacturing process of the porous carbon dioxide capture agent of the present invention. Referring to Figure 1, it can be confirmed that the porous carbon dioxide capture agent of the present invention includes the steps of: preparing a metal-organic framework precursor aqueous solution by adding a transition metal precursor, an alkali metal precursor, and an organic acid to water; circulating and condensing the prepared metal-organic framework precursor aqueous solution; and drying the condensed metal-organic framework precursor aqueous solution.
[0042] Metal-organic frameworks (MOFs) are porous materials composed of metal ions or clusters containing metals linked by organic ligands. They are a type of coordination polymer. MOFs form three-dimensional structures, maintaining porosity while maintaining strong bonds, enabling diverse functions such as gas storage, catalysis, drug delivery, and chemical sensors.
[0043] The above circulating condensation is also called reflux condensation, and reflux refers to the operation of condensing the vapor generated by heating into a liquid state and then returning it to its original state. To prevent volatile substances or solvents from becoming vapor and evaporating while heating continues, a cooler is attached to the top of the reaction vessel to condense the vaporized substances into a liquid and return them to the original reaction vessel. The cooler used for this purpose is called a reflux condenser, and this operation can promote the reaction while boiling the solution. The reflux condenser is used to change the physical state of the vapor released from the heated solvent back to a liquid through a linear or spiral circulating cooling method. It has the advantage of being able to heat the mixture for a long time by reducing solvent loss.
[0044] Furthermore, since the porous carbon dioxide capture agent of the present invention uses only pure water as a solvent, it can be manufactured through an environmentally friendly manufacturing method.
[0045] Here, the transition metal precursor may include, but is not limited to, dimethyl zinc, diethyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate, and zinc sulfate.
[0046] Here, the alkali metal precursor may include at least one material selected from the group consisting of potassium hydroxide, sodium hydroxide, lithium oxide, barium oxide, potassium carbonate, sodium carbonate, lithium carbonate, barium carbonate, sodium methoxide, sodium ethoxide, potassium ethoxide, and potassium isopropoxide, but is not limited thereto.
[0047] Here, the organic acid may be at least one substance selected from the group consisting of acetic acid, formic acid, citric acid, oxalic acid, and ascorbic acid, but is not limited thereto.
[0048] Here, the transition metal precursor and the alkali metal precursor may be included in a molar ratio of 1:1 to 1:5. If the molar ratio of the transition metal precursor and the alkali metal precursor is outside the above-described range (for example, if the molar ratio of the transition metal precursor: alkali metal precursor is 1:0.5 or 1:7), a problem may arise in that it is difficult to form the crystal structure of the target metal-organic framework. Furthermore, since an additional process of filtering or removing the excess transition metal precursor and alkali metal precursor is required, a problem in that the process becomes complicated may arise. Therefore, in the present invention, it is preferable that the transition metal precursor and the alkali metal precursor be included in a molar ratio of 1:1 to 1:5.
[0049] Here, the heating temperature in the above-mentioned cyclic condensation step may be 80 to 120°C. If the heating temperature is lower than 80°C, a problem may arise in which the crystal structure of the metal-organic framework is not sufficiently formed. On the other hand, if the heating temperature exceeds 120°C, it is not economical because it does not exhibit improved effects compared to when the heating temperature is 80 to 120°C. Accordingly, in the present invention, the heating temperature is preferably 80 to 120°C.
[0050] Here, the heating time in the above-mentioned cyclic condensation step may be 5 to 10 hours. If the heating time is less than 5 hours, a problem may arise in that the crystal structure of the metal-organic framework is not sufficiently formed. On the other hand, if the heating time exceeds 10 hours, a change in the crystal structure of the metal-organic framework may occur, and thus a problem in that the CO2 adsorption capacity and CO2 / N2 selectivity may decrease. Accordingly, the heating time is preferably 5 to 10 hours.
[0051] Here, the drying step may be performed in a vacuum, but is not limited thereto.
[0052]
[0053] Porous carbon dioxide capture agent
[0054] In addition, as a means for achieving the above-described purpose, the present invention provides a porous carbon dioxide capture agent formed using a composition including a transition metal precursor, an alkali metal precursor, and an organic acid.
[0055] The types of the transition metal precursor, the alkali metal precursor, and the organic acid are the same as described above.
[0056] Figure 2 is a schematic diagram showing the crystal structure of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention. Referring to Figure 2, it can be seen that alkali metal cations appear as cream-colored spheres, transition metal cations appear as purple spheres, and in the case of organic acids, hydrogen appears as white wires, carbon as black wires, and oxygen as red wires, respectively. Furthermore, it can be seen that pores are distributed as the porous carbon dioxide capture agent of the present invention is formed by the above-mentioned framework.
[0057] The porous carbon dioxide capture agent of the present invention has a porous crystal structure by forming a metal-organic framework using a composition including the transition metal precursor, the alkali metal precursor, and an organic acid, and thus can be characterized by a large specific surface area and pore volume.
[0058] More specifically, the specific surface area of the porous carbon dioxide capture agent is 750 to 1000 m 2 / g may be.
[0059] In addition, the pore volume of the porous carbon dioxide capture agent is 0.6 to 1.0 cm 3 / g may be.
[0060] The specific surface area and pore volume of the porous carbon dioxide capture agent of the present invention will be described in more detail in the {Examples and Evaluation} section below.
[0061] In addition, in order for a carbon dioxide capture agent to be evaluated as having excellent carbon dioxide adsorption capacity, it is desirable to exhibit high CO2 / N2 selectivity, that is, excellent adsorption capacity for CO2 while simultaneously exhibiting low adsorption capacity for N2. Here, the CO2 / N2 selectivity of the porous carbon dioxide capture agent may be 110 to 130. Specific details regarding the CO2 / N2 selectivity of the carbon dioxide adsorption composite of the present invention will also be described in more detail in the {Examples and Evaluation} paragraph below.
[0062] In addition, the porous carbon dioxide capture agent of the present invention may exhibit XRD spectrum peaks having specific crystallinity by including the metal organic framework described above. Specific XRD spectrum peaks (2θ) of the porous carbon dioxide capture agent may appear at 7.4°, 11.26°, 13.61°, 15.5°, 21.19°, 25.28°, 26.22°, 27.99°, 28.8°, 35.63°, and 37.17°.
[0063] Fig. 3 is a SEM image of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention. Referring to Fig. 3, it can be confirmed that the porous carbon dioxide capture agent of the present invention is composed of polygonal particles.
[0064] Hereinafter, the claims of the present specification will be described in more detail with reference to the attached drawings and embodiments. However, since the drawings and embodiments presented in this specification may be modified in various ways by those skilled in the art and may have various forms, the disclosure of the present invention should not be considered to limit the present invention to a specific disclosed form, but to include all equivalents and substitutes included in the spirit and technical scope of the present invention. In addition, the attached drawings are presented to help those skilled in the art understand the present invention more accurately, and may be depicted in an exaggerated or reduced form compared to reality.
[0065]
[0066] {Examples and Evaluation}
[0067] <Example>
[0068] 1. Comparison by heating time
[0069] Example 1-1
[0070] Zn(CH3COO)2·2H2O (4.6 g) and C6H8O7·H2O (4.4 g) were dissolved in 100 mL of water, and then KOH (3.51 g) was added to the same solution. The solution was stirred for 5 minutes and then transferred to a 250 mL round-bottom flask. The water temperature of the condenser was 5–10°C. The water condenser was set to maintain the temperature at 5–10°C. The cyclic condensation was performed at 100°C and 70 rpm for 7 hours. Upon completion of the reaction, the reaction mixture was cooled to room temperature, and the formation of a white precipitate was confirmed. The precipitate was washed with ethyl ether (twice) and methanol (three times). The methanol solvent was exchanged three times a day for 3 days to remove impurities. The final product was dried under vacuum without heating for 2 hours, and then heated at 100°C under vacuum for 6 hours to obtain the desired product.
[0071]
[0072] Example 1-2
[0073] A porous carbon dioxide capture agent was manufactured in the same manner as in Example 1-1, except that the above cyclic condensation was performed at 100 °C and 70 rpm for 8 hours (hereinafter referred to as “Example 1-2”).
[0074]
[0075] Example 1-3
[0076] A porous carbon dioxide capture agent was manufactured in the same manner as in Example 1-1, except that the above cyclic condensation was performed at 100 °C and 70 rpm for 9 hours (hereinafter referred to as “Example 1-3”).
[0077]
[0078] Comparative Example 1-1
[0079] A porous carbon dioxide capture agent was manufactured in the same manner as in Example 1-1, except that the above cyclic condensation was performed at 100 °C and 70 rpm for 3 hours (hereinafter referred to as “Comparative Example 1-1”).
[0080]
[0081] Comparative Example 1-2
[0082] A porous carbon dioxide capture agent was manufactured in the same manner as in Example 1-1, except that the above cyclic condensation was performed at 100 °C and 70 rpm for 5 hours (hereinafter referred to as “Comparative Example 1-2”).
[0083]
[0084] 2. Comparison by heating temperature
[0085] Example 2-1
[0086] A porous carbon dioxide capture agent was manufactured in the same manner as in Example 1-1, except that the above cyclic condensation was performed at 100 °C and 70 rpm for 8 hours (hereinafter referred to as “Example 2-1”).
[0087]
[0088] Example 2-2
[0089] A porous carbon dioxide capture agent was manufactured in the same manner as in Example 1-1, except that the above cyclic condensation was performed at 120 °C and 70 rpm for 8 hours (hereinafter referred to as “Example 2-2”).
[0090]
[0091] Comparative Example 2-1
[0092] A porous carbon dioxide capture agent was manufactured in the same manner as in Example 1-1, except that the above cyclic condensation was performed at 60 °C and 70 rpm for 8 hours (hereinafter referred to as “Comparative Example 2-1”).
[0093]
[0094] The contents of the above-described examples and comparative examples are shown in Table 1 below.
[0095] ClassificationHeating temperature (℃)Heating time (hours)Example 1-11007Example 1-21008Example 1-31009Comparative Example 1-11003Comparative Example 1-21005Example 2-11008Example 2-21208Comparative Example 2-1608
[0096] In addition, a conventional metal-organic framework was manufactured according to a known technique.
[0097]
[0098] Comparative Example 3 (Zeolite 13X)
[0099] A metal-organic framework was manufactured based on the manufacturing method described in [S. Cavenati, CA Grande, AE Rodrigues, Adsorption equilibrium of methane, carbon dioxide, and nitrogen on zeolite 13X at high pressures, Journal of Chemical & Engineering Data 49(4) (2004) 1095-1101] (hereinafter referred to as “Comparative Example 3”).
[0100]
[0101] Comparative Example 4 (Activated Carbon)
[0102] The activated carbon described in [RP Ribeiro, TP Sauer, FV Lopes, RF Moreira, CA Grande, AE Rodrigues, Adsorption of CO2, CH4, and N2 in activated carbon honeycomb monolith, Journal of Chemical & Engineering Data 53(10) (2008) 2311-2317] was used (hereinafter referred to as “Comparative Example 4”).
[0103]
[0104] Comparative Example 5 (MOF-177)
[0105] A metal-organic framework was manufactured based on the manufacturing method described in [D. Saha, Z. Bao, F. Jia, S. Deng, Adsorption of CO2, CH4, N2O, and N2 on MOF-5, MOF-177, and zeolite 5A, Environmental science & technology 44(5) (2010) 1820-1826] (hereinafter referred to as “Comparative Example 5”).
[0106]
[0107] Comparative Example 6 (MIL-96(Al)-Ca4)
[0108] A metal-organic framework was prepared based on the preparation method described in [HR Abid, ZH Rada, Y. Li, HA Mohammed, Y. Wang, S. Wang, H. Arandiyan, X. Tan, S. Liu, Boosting CO 2 adsorption and selectivity in metal-organic frameworks of MIL-96 (Al) via second metal Ca coordination, RSC Advances 10(14) (2020) 8130-8139] (hereinafter referred to as “Comparative Example 6”).
[0109]
[0110] Evaluation
[0111] Fig. 4 is an XRD spectrum of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention. The main peaks and the intensities of each peak shown in Fig. 4 are shown in Table 2 below.
[0112] Angle(2θ)Intensity7.420306413.616558927.992627128.82110511.262045121.191935835.631528026.221508915.51490637.171190625.2811828
[0113] Referring to Fig. 4 and Table 2, it can be seen that the XRD diffraction pattern shows major peaks at 7.4°, 13.61°, 27.99°, 28.8°, 11.26°, 21.19°, and 35.63°.
[0114] Figure 5 is a graph showing six types of adsorption isotherms according to the International Union of Pure and Applied Chemistry (IUPAC). Referring to Figure 5, it can be confirmed that Type Ⅰ represents an adsorption isotherm when there are mainly micropores, Type Ⅱ represents when there are almost no micropores, Type Ⅲ represents when the adsorbate is weak, Type Ⅳ represents when there are mainly mesopores and capillary condensation appears, Type Ⅴ represents when the adsorbate is weak and capillary condensation appears, and Type Ⅵ represents an adsorption isotherm when gas is layered again on the adsorbed gas surface.
[0115] Fig. 6 is a graph showing the N2 adsorption isotherm of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention. Referring to Fig. 6, it can be confirmed that the N2 adsorption isotherm of the porous carbon dioxide capture agent of the present invention synthesized for various reaction times shows a Type I isotherm according to the IUPAC classification. This is a result suggesting that the porous carbon dioxide capture agent of the present invention has a microporous structure. Furthermore, it can be confirmed that Example 1-1 shows the highest N2 adsorption capacity, and from this result, it can be inferred that Example 1-1 has the highest pore volume.
[0116] Fig. 7 is a graph showing CO2 and N2 adsorption isotherms of a porous carbon dioxide capture agent manufactured according to an embodiment of the present invention. To investigate the effect of reaction time on CO2 capture performance, CO2 and N2 adsorption capacities were measured separately using a volumetric method in a pressure range of 0 to 1 bar at 288 K. More specifically, Fig. 7a is a graph showing a CO2 adsorption isotherm of a porous carbon dioxide capture agent manufactured according to an embodiment of the present invention, and Fig. 7b is a graph showing a N2 adsorption isotherm of a porous carbon dioxide capture agent manufactured according to an embodiment of the present invention.
[0117] From the results shown in the above Figure 7, the specific surface area and pore volume of each example and comparative example were calculated and shown in Table 3 below.
[0118] Specific surface area (m) 2 / g) pore volume (cm) 3 / g)Embodiment 1-18340.76Embodiment 1-29500.86Embodiment 1-38950.81Comparative Example 1-17530.68Comparative Example 1-27920.72
[0119] Referring to FIG. 7 and Table 3, it can be confirmed that Comparative Example 1-1 shows the lowest CO2 capacity due to the low crystal structure. This can be confirmed to be consistent with the low surface area of Comparative Example 1-1 described in Table 3 above. It can be confirmed that the CO2 capacity (3.44 mmol / g) of Comparative Example 1-1 shows a result that is much lower than that of Example 1-2 (5.1 mmol / g), which indicates that optimizing the heating time is important for carbon dioxide capture performance. In addition, the maximum CO2 capacity can be confirmed in Example 1-2 (heating time 8 hours), which corresponds to the largest surface area and pore volume provided by the complete crystal structure of the metal-organic framework. However, it can be confirmed that when the heating time exceeds 8 hours, the CO2 capacity decreases by 10% compared to Example 1-2 (Example 1-3). In addition, it can be confirmed that the N2 adsorption does not show an increasing trend as the reaction time increases. Based on the above results, it can be inferred that in the method for manufacturing a porous carbon dioxide capture agent of the present invention, the CO2 / N2 adsorption selectivity can be improved as the heating time increases up to a maximum of 8 hours.
[0120] Fig. 8 is a graph showing the CO2 / N2 selectivity of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention. Referring to Fig. 8, it can be seen that the CO2 / N2 selectivity gradually increases in the order of Comparative Example 1-1, Comparative Example 1-2, Example 1-1, and Example 1-2, but shows a slightly decreased value in Example 1-3. In addition, it can be seen that Example 1-2, which has a heating time of 8 hours, shows the highest CO2 / N2 selectivity of 129.
[0121] Fig. 9 is a graph showing the CO2 adsorption isotherm of a porous carbon dioxide capture agent manufactured according to one embodiment of the present invention. Referring to Fig. 9, it can be seen that Example 2-1 exhibits a CO2 adsorption capacity of 4 mmol / g, and Example 2-2 exhibits a slightly higher capacity of 4.1 mmol / g. However, Example 2-2 may be less economical than Example 2-1 because the heating temperature is 120°C, i.e., more energy is required to synthesize the porous carbon dioxide capture agent.
[0122]
[0123] The CO2 / N2 selectivity of the above-mentioned manufactured examples 1-2 and comparative examples 3 to 6 is shown in Table 4 below.
[0124] Classification CO2 / N2 Selectivity Example 1-2129 Comparative Example 37 Comparative Example 46.5 Comparative Example 517 Comparative Example 660.3
[0125] Referring to Table 4, it can be confirmed that the porous carbon dioxide capture agent of the present invention exhibits superior CO2 / N2 selectivity compared to known metal-organic frameworks, despite being manufactured through a simple manufacturing method that is environmentally friendly and can be mass-produced using water.
[0126] The method for manufacturing the porous carbon dioxide capture agent of the present invention can be environmentally friendly, as it uses only pure water as a solvent for synthesis.
[0127] In addition, the method for manufacturing the porous carbon dioxide capture agent of the present invention can be suitable for mass production through a simple manufacturing method.
[0128] In addition, the porous carbon dioxide capture agent manufactured according to the method of the present invention can exhibit high CO2 / N2 selectivity.
[0129] The above description is merely an example of the technical idea of the present invention, and those skilled in the art will appreciate that various modifications and variations can be made without departing from the essential characteristics of the present invention.
[0130] Accordingly, the embodiments disclosed in the present invention are intended to illustrate, rather than limit, the technical concept of the present invention, and the scope of the technical concept of the present invention is not limited by these embodiments. The scope of protection of the present invention should be interpreted by the following claims, and all technical concepts within the scope equivalent thereto should be construed as being included within the scope of the present invention.
Claims
1. A step of preparing a metal-organic framework precursor aqueous solution by adding a transition metal precursor, an alkali metal precursor, and an organic acid to water; A step of circulating and condensing the above-mentioned metal-organic framework precursor aqueous solution; and A method for producing a porous carbon dioxide capture agent, comprising: a step of drying the above-described condensed metal-organic framework precursor aqueous solution.
2. In paragraph 1, A method for producing a porous carbon dioxide capture agent, wherein the transition metal precursor comprises dimethyl zinc, diethyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate, and zinc sulfate.
3. In paragraph 1, A method for producing a porous carbon dioxide capture agent, wherein the alkali metal precursor comprises at least one material selected from the group consisting of potassium hydroxide, sodium hydroxide, lithium oxide, barium oxide, potassium carbonate, sodium carbonate, lithium carbonate, barium carbonate, sodium methoxide, sodium ethoxide, potassium ethoxide, and potassium isopropoxide.
4. In paragraph 1, A method for producing a porous carbon dioxide capture agent, wherein the organic acid is at least one substance selected from the group consisting of acetic acid, formic acid, citric acid, oxalic acid, and ascorbic acid.
5. In paragraph 1, A method for producing a porous carbon dioxide capture agent, wherein the transition metal precursor and the alkali metal precursor are included in a molar ratio of 1:1 to 1:
5.
6. In paragraph 1, A method for manufacturing a porous carbon dioxide capture agent, wherein the heating temperature in the above-mentioned circulating condensation step is 80 to 120°C.
7. In paragraph 1, A method for manufacturing a porous carbon dioxide capture agent, wherein the heating time in the above-mentioned circulating condensation step is 5 to 10 hours.
8. In paragraph 1, A method for manufacturing a porous carbon dioxide capture agent, wherein the drying step is performed in a vacuum.
9. A porous carbon dioxide capture agent formed using a composition comprising a transition metal precursor, an alkali metal precursor, and an organic acid.
10. In paragraph 9, Specific surface area of 750 to 1000 m 2 / g, porous carbon dioxide capture agent.
11. In paragraph 9, Pore volume of 0.6 to 1.0 cm 3 / g, porous carbon dioxide capture agent.
12. In paragraph 9, A porous carbon dioxide capture agent having a CO2 / N2 selectivity of 110 to 130.
13. In paragraph 9, A porous carbon dioxide capture agent, characterized in that the XRD spectrum peaks (2θ) of the porous carbon dioxide capture agent formed above appear at 7.4°, 11.26°, 13.61°, 15.5°, 21.19°, 25.28°, 26.22°, 27.99°, 28.8°, 35.63°, and 37.17°.
Citation Information
Patent Citations
Metal-organic framework for adsorbents of an adsorption chiller and preparation method thereof
KR1020180043536A
Intra prediction method and apparatus
KR1020210000636A
Method and device for processing video, and storage medium
KR1020220014278A
Magnetic component and display device having the same
KR1020220113653A
Method of tunneling device fabrication using a natural oxide film to form intermediate layer
KR1020220122046A