Method for producing polypropylene-dispersed high-density polyethylene composition, and article manufactured thereby
By prepolymerizing propylene on an activated catalyst and polymerizing polypropylene and polyethylene at different sites, the method enhances the heat resistance and strength of HDPE, achieving superior physical properties compared to traditional blends.
Patent Information
- Application Number
- PCT/KR2024/095506
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-03-14
- Publication Date
- 2024-11-28
AI Technical Summary
High-density polyethylene (HDPE) lacks sufficient heat resistance and strength compared to other materials like PET or nylon, and simple blending with polypropylene does not adequately improve its physical properties due to poor kneading properties on a micro scale.
A method involving the prepolymerization of propylene on an activated catalyst to form a polypropylene catalyst seed, followed by polymerizing polypropylene and polyethylene at different catalyst sites, resulting in a high-density polyethylene composition with dispersed polypropylene, which enhances heat resistance and strength.
The method produces a high-density polyethylene composition with improved shear modulus, tensile strength, and elongation, exceeding the physical properties of traditional HDPE and polypropylene/HDPE blends, with a shear modulus of 0.1 to 0.3 MPa and tensile strength of 400 to 800 kgf/cm², and elongation of 750 to 1100%.
Smart Images

Figure KR2024095506_28112024_PF_FP_ABST
Abstract
Description
Method for producing a high-density polyethylene composition in which polypropylene is dispersed and articles produced thereby
[0001] The present disclosure relates to a method for producing a high-density polyethylene composition having polypropylene dispersed therein and an article produced thereby.
[0002] As the importance of a circular economy grows, research is actively being conducted to replace existing composite material packaging films (nylon / PET / polyethylene, etc.) with recyclable single-material polyethylene packaging materials.
[0003] However, polyethylene suffers from inferior physical properties compared to PET or nylon, such as heat resistance and strength. While attempts have been made to improve the mechanical properties of polyethylene by stretching it biaxially or uniaxially, such attempts to improve properties during processing through stretching are limited. Therefore, ongoing research is being conducted to significantly improve the physical properties of polyethylene.
[0004] Against this backdrop, the importance of high-density polyethylene (HDPE), known for its superior physical properties, including strength and heat resistance, is rising. However, even when HDPE is used, it still lacks the required physical properties, such as heat resistance and strength.
[0005] In order to improve the properties of high-density polyethylene, the properties can be partially improved by simply blending high-density polyethylene with polypropylene, which has excellent properties such as heat resistance and strength, at a certain ratio to produce a polypropylene / high-density polyethylene blend resin.
[0006] Although polymer blends of this type are already being commercially produced, they still have insufficient miscibility at the microscale, and therefore, they still have the disadvantage of not securing the desired properties.
[0007] When physically blending polypropylene / high-density polyethylene resins, the properties may vary depending on the type or molecular weight of the resin, but for example, an article manufactured from the physically blended material has a shear modulus of 0.1 MPa or less and a tensile strength of 400 kgf / cm measured at 145°C. 2 Below or with an elongation of 700% or less, it has limitations in securing properties higher than this.
[0008] The difficulty in improving these properties is that when high-density polyethylene and polypropylene are simply blended, the mixing properties on a microscale are poor, and therefore, the properties of the blended material are not sufficiently excellent.
[0009] Therefore, the present invention provides a new high-density polyethylene composition capable of micro-blending, which simultaneously satisfies properties that play opposite and complementary roles, such as strength and elongation, and provides a new method for manufacturing the same. In addition, from the composition, a shear modulus measured at 145°C of 0.1 MPa or more and a tensile strength of 400 kgf / cm or more are obtained. 2 The present invention provides an article manufactured from a high-density polyethylene composition that achieves a remarkable increase in physical properties, such as an elongation of 700% or more.
[0010] The present disclosure provides a high-density polyethylene composition having excellent heat resistance and strength, specifically shear modulus, tensile strength, and elongation, and having excellent mixability, in which polypropylene is dispersed, by prepolymerizing propylene on an activated catalyst to form a polypropylene catalyst seed, polymerizing polypropylene at a certain weight % on the formed polypropylene catalyst seed, and then polymerizing polyethylene.
[0011] The present disclosure provides a method for producing a high-density polyethylene composition having polypropylene dispersed therein, comprising: a) a catalyst activation step of forming an activated catalyst by introducing a catalyst, a cocatalyst, and a donor; b) a catalyst stabilization step of prepolymerizing propylene on the activated catalyst to form a polypropylene catalyst seed; c) a first polymerization step of introducing propylene and polymerizing polypropylene on the polypropylene catalyst seed; and d) a second polymerization step of subsequently introducing ethylene and polymerizing polyethylene.
[0012] In one embodiment, the method for producing the high-density polyethylene composition in which the polypropylene is dispersed may be to polymerize the polypropylene in an amount of 1 to 30 wt% based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed in step c).
[0013] In one embodiment, the method for producing the high-density polyethylene composition in which the polypropylene is dispersed may be to polymerize polypropylene in an amount of 7 to 20 wt% based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed in step c).
[0014] In one embodiment, the catalyst may comprise a Ziegler-Natta catalyst.
[0015] In one embodiment, the cocatalyst may include at least one selected from the group consisting of TEAL (triethylaluminum), TIBAL (Triisobutylaluminum), and TOA (trioctyl aluminum).
[0016] In one embodiment, the donor may include at least one selected from the group consisting of cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, isobutylisopropyldimethoxysilane, diisobutyldimethoxysilane, dicyclopentyldimethoxysilane, and dicyclohexyldimethoxysilane.
[0017] In one embodiment, the weight of the cocatalyst relative to the weight of the catalyst may be in the range of 4 to 5.
[0018] In one embodiment, the weight of the cocatalyst relative to the donor weight may be in the range of 5 to 9.
[0019] In one embodiment, step b) may be performed in two loop reactors connected in series.
[0020] In one embodiment, the fraction of propylene in the reactor in step c) may be 15 mol% or less.
[0021] In one embodiment, the method for producing a high-density polyethylene composition having polypropylene dispersed therein may further include the step of e) steam cleaning and drying the high-density polyethylene composition having polypropylene dispersed therein obtained in step d).
[0022] In one embodiment, the method for producing a high-density polyethylene composition in which polypropylene is dispersed may further include the step of f) adding an additive to the high-density polyethylene composition in which polypropylene is dispersed after step e) and extruding the same.
[0023] In one embodiment, the method for producing a high-density polyethylene composition in which polypropylene is dispersed may further include adding an antistatic agent in step c).
[0024] In one embodiment, the method for producing a high-density polyethylene composition in which polypropylene is dispersed may further include adding an antistatic agent in step d).
[0025] In one embodiment, the method for producing a high-density polyethylene composition in which polypropylene is dispersed may further include adding ethylene in step c).
[0026] In addition, the present disclosure provides an article made of a high-density polyethylene composition having polypropylene dispersed therein, wherein the high-density polyethylene composition having polypropylene dispersed therein comprises 1 to 30 wt% of polypropylene based on the total weight of the high-density polyethylene composition having polypropylene dispersed therein, and wherein the article has an elongation of 750 to 1100% as measured by the ASTM D638 method.
[0027] In one embodiment, the high-density polyethylene composition having polypropylene dispersed therein may contain 7 to 20 wt% of polypropylene based on the total weight of the high-density polyethylene composition having polypropylene dispersed therein.
[0028] In one embodiment, the shear modulus of the article measured by the ASTM E143 method may be 0.1 to 0.3 MPa.
[0029] In one embodiment, the tensile strength of the above article measured by the ASTM D638 method is 400 to 800 kgf / cm. 2 It could be.
[0030] A method for producing a high-density polyethylene composition in which polypropylene is dispersed according to the present disclosure and a composition produced thereby are provided, wherein propylene is prepolymerized on an activated catalyst to form a polypropylene catalyst seed, then polypropylene is polymerized at a certain weight % on the formed polypropylene catalyst seed, and then polyethylene is polymerized, thereby providing a method for producing a high-density polyethylene composition in which polypropylene is dispersed and has excellent physical properties such as heat resistance and strength, specifically shear modulus, tensile strength, and elongation, and excellent mixability, and a composition.
[0031] The high-density polyethylene composition having dispersed polypropylene according to the present disclosure polymerizes polypropylene and polyethylene on the polypropylene catalyst seed. The introduced ethylene and propylene polymerize into polyethylene and polypropylene at different catalyst sites, respectively, and since the polymerization reaction occurs at different catalyst sites, a copolymer is not formed. Thus, the high-density polyethylene composition having dispersed polypropylene according to the present disclosure has structural characteristics that inevitably exhibit superior miscibility compared to a simple blend because it polymerizes into polyethylene and polypropylene at different sites of a single catalyst. This superior miscibility of the high-density polyethylene composition having dispersed polypropylene according to the present disclosure can be experimentally confirmed from the very uniform appearance of the film surface in the micrograph of Example 1 in FIG. 1.
[0032] In addition, the high-density polyethylene composition of the present disclosure having polypropylene dispersed therein has excellent heat resistance and strength, specifically shear modulus, tensile strength, and elongation, compared to conventional high-density polyethylene or polypropylene / high-density polyethylene blend resins, due to the polypropylene being dispersed therein. This excellent heat resistance and strength, specifically shear modulus, tensile strength, and elongation, appear to be due to the difference in the degree to which polypropylene is dispersed within the resin.
[0033] In the case of polypropylene / high-density polyethylene blend resins, polypropylene is dispersed within a high-density polyethylene matrix and blended, and is dispersed as a polymer unit. In contrast, in the high-density polyethylene composition of the present disclosure, polypropylene is prepolymerized into propylene polymer units, so it is dispersed in much smaller polymer units, and thus the degree of dispersion is even. Due to this difference, the high-density polyethylene composition of the present disclosure appears to exhibit excellent heat resistance and strength, specifically, shear modulus, tensile strength, and elongation.
[0034] Figure 1 is a photograph of the film surface taken with a microscope at a magnification of 50 times, after manufacturing the polymer in the form of a film according to Example 1.
[0035] Figure 2 is a photograph of the film surface taken with a microscope at a magnification of 50 times, manufactured in the form of a film using a blend manufactured according to Comparative Example 1.
[0036] Hereinafter, a method for producing a high-density polyethylene composition in which polypropylene is dispersed and a composition produced thereby will be described in detail.
[0037] Unless otherwise defined, the technical and scientific terms used herein have the meaning commonly understood by a person of ordinary skill in the art to which this invention pertains, and in the following description, descriptions of well-known functions and configurations that may unnecessarily obscure the gist of the present invention are omitted.
[0038] Additionally, the singular forms used herein may be intended to include the plural forms as well, unless the context specifically indicates otherwise.
[0039] In addition, units used in this specification without special mention are based on weight, and for example, units of % or ratio mean weight% or weight ratio, and weight% means the weight% that any one component of the entire mixture occupies in the mixture unless otherwise defined.
[0040] Additionally, the numerical ranges used herein include lower and upper limits and all values within that range, increments logically derived from the shape and width of the defined range, all doubly defined values, and all possible combinations of upper and lower limits of numerical ranges defined in different shapes. Unless otherwise specifically defined in the specification of the present invention, values outside the numerical range that may arise due to experimental error or rounding of values are also included in the defined numerical range.
[0041] The term "includes" in this specification is an open-ended description equivalent to expressions such as "comprises," "contains," "has," or "characterizes," and does not exclude additional elements, materials, or processes not listed.
[0042] Hereinafter, a method for producing a high-density polyethylene composition in which polypropylene is dispersed according to the present disclosure will be described in detail.
[0043] The present disclosure provides a method for producing a high-density polyethylene composition having polypropylene dispersed therein, comprising: a) a catalyst activation step of forming an activated catalyst by introducing a catalyst, a cocatalyst, and a donor; b) a catalyst stabilization step of prepolymerizing propylene on the activated catalyst to form a polypropylene catalyst seed; c) a first polymerization step of introducing propylene and polymerizing polypropylene on the polypropylene catalyst seed; and d) a second polymerization step of subsequently introducing ethylene and polymerizing polyethylene.
[0044] The high-density polyethylene composition having dispersed polypropylene according to the present disclosure polymerizes polypropylene and polyethylene on the polypropylene catalyst seed. The introduced ethylene and propylene polymerize into polyethylene and polypropylene at different catalyst sites, respectively, and since the polymerization reaction occurs at different catalyst sites, a copolymer is not formed. Thus, the high-density polyethylene composition having dispersed polypropylene according to the present disclosure has structural characteristics that inevitably exhibit superior miscibility compared to a simple blend because it polymerizes into polyethylene and polypropylene at different sites of a single catalyst. This superior miscibility of the high-density polyethylene composition having dispersed polypropylene according to the present disclosure can be experimentally confirmed from the very uniform appearance of the film surface in the micrograph of Example 1 in FIG. 1.
[0045] In the above step a), the catalyst, cocatalyst, and donor come into contact to activate the reaction centers of the catalyst. The above step b) is necessary to prevent fouling during the polymerization process. If the catalyst particles are directly introduced into a reactor performing a polymerization reaction such as step c) or step d), most of the catalyst particles are pulverized due to the sudden temperature increase and violent reaction, forming catalyst fine particles, resulting in a large amount of fouling. The method for producing a high-density polyethylene composition having dispersed polypropylene of the present disclosure forms a polypropylene catalyst seed in the above step b) to exhibit an excellent effect of preventing fouling during the polymerization reaction.
[0046] In one embodiment, in step c), polypropylene may be polymerized in an amount of 30 wt% or less, 20 wt% or less, or 15 wt% or less, based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed. In addition, in step c), polypropylene may be polymerized in an amount of 0.1 wt% or more, 1 wt% or more, 2 wt% or more, 3 wt% or more, 4 wt% or more, 5 wt% or more, 7 wt% or more, 10 wt% or more, or 12 wt% or more, based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed. In step c), polypropylene may be polymerized in an amount of 1 to 30 wt% or 7 to 20 wt%, based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed. In the step c), when polypropylene is polymerized in an amount of 1 to 30 wt% based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed, the high-density polyethylene composition in which the polypropylene is dispersed has excellent physical properties such as heat resistance and strength, specifically shear modulus, tensile strength, and elongation.
[0047] In one embodiment, the catalyst may include, but is not limited to, at least one selected from the group consisting of a Ziegler-Natta catalyst and a metallocene. Specifically, the catalyst may include a Ziegler-Natta catalyst.
[0048] In one embodiment, the cocatalyst may include, but is not limited to, at least one selected from the group consisting of TEAL (triethylaluminum), TIBAL (Triisobutylaluminum), and TOA (trioctyl aluminum). Specifically, the cocatalyst may include TEAL (triethylaluminum).
[0049] In one embodiment, the donor may include at least one selected from the group consisting of cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, isobutylisopropyldimethoxysilane, diisobutyldimethoxysilane, dicyclopentyldimethoxysilane, and dicyclohexyldimethoxysilane, but is not limited thereto. Specifically, the donor may include cyclohexylmethyldimethoxysilane.
[0050] In one embodiment, the weight of the cocatalyst relative to the weight of the catalyst may be 1 or more, 2 or more, 3 or more, or 4 or more. Additionally, the weight of the cocatalyst relative to the weight of the catalyst may be 8 or less, 7 or less, 6 or less, or 5 or less. The weight of the cocatalyst relative to the weight of the catalyst may be in the range of 4 to 5.
[0051] In one embodiment, the weight of the cocatalyst relative to the donor weight may be 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, or 6 or more. Additionally, the weight of the cocatalyst relative to the donor weight may be 10 or less, 9 or less, 8 or less, or 7 or less. The weight of the cocatalyst relative to the donor weight may be in the range of 5 to 9.
[0052] In one embodiment, step b) may be performed in two loop reactors connected in series. By operating two prepolymerization loop reactors connected in series in this manner, the morphology of the high-density polyethylene composition in which polypropylene is dispersed can be optimally maintained.
[0053] In one embodiment, the fraction of propylene in the reactor in step c) may be 15 mol% or less. In this way, by setting an upper limit of the fraction of propylene in the reactor in step c), there is an effect of maintaining stable process operation and preventing overreaction of propylene.
[0054] In one embodiment, the method for producing a high-density polyethylene composition having dispersed polypropylene may further include the step of e) steam-cleaning and drying the high-density polyethylene composition having dispersed polypropylene obtained in step d). Through this step, the catalyst, cocatalyst, and hydrocarbon components contained in the high-density polyethylene composition having dispersed polypropylene can be removed, and the monomers can be recovered.
[0055] In one embodiment, the method for producing a high-density polyethylene composition having polypropylene dispersed therein may further include the step of f) adding an additive to the high-density polyethylene composition having polypropylene dispersed therein after step e) and extruding the same. Through this step, the additive and the high-density polyethylene composition having polypropylene dispersed therein can be uniformly mixed.
[0056] In one embodiment, an antistatic agent may be further added in step c). In another embodiment, an antistatic agent may be further added in step d). Since the polymer is non-conductive, static electricity accumulated on the surface may cause plugging during the process. The antistatic agent has hydrophilic and hydrophobic radicals in one molecule, so that the hydrophobic radicals are attached to the polymer surface, and the hydrophilic radicals are directed toward the air and attract moisture in the air. At this time, the static electricity accumulated on the polymer surface is dissipated by the conductivity of the water absorbed by the antistatic agent, and also the accumulation of frictional static electricity can be reduced.
[0057] In one embodiment, ethylene may be further added in step c). In this way, if ethylene is further added in step c), the polypropylene content of the high-density polyethylene composition in which polypropylene is dispersed can be adjusted as desired.
[0058] Also described is an article manufactured from a high-density polyethylene composition containing dispersed polypropylene of the present disclosure. Any details that overlap with those described above in the method for manufacturing a high-density polyethylene composition containing dispersed polypropylene are omitted.
[0059] The present disclosure provides an article made of a high-density polyethylene composition having polypropylene dispersed therein, wherein the high-density polyethylene composition having polypropylene dispersed therein comprises 1 to 30 wt% of polypropylene based on the total weight of the high-density polyethylene composition having polypropylene dispersed therein, and wherein the article has an elongation of 750 to 1100% as measured by the ASTM D638 method.
[0060] The present disclosure provides a high-density polyethylene composition in which polypropylene is dispersed, wherein polypropylene and polyethylene are polymerized in a polypropylene catalyst seed, and the polypropylene catalyst seed is formed by prepolymerizing a catalyst and propylene.
[0061] The high-density polyethylene composition having dispersed polypropylene according to the present disclosure polymerizes polypropylene and polyethylene on the polypropylene catalyst seed. The introduced ethylene and propylene polymerize into polyethylene and polypropylene at different catalyst sites, respectively, and since the polymerization reaction occurs at different catalyst sites, a copolymer is not formed. Thus, the high-density polyethylene composition having dispersed polypropylene according to the present disclosure has structural characteristics that inevitably exhibit superior miscibility compared to a simple blend because it polymerizes into polyethylene and polypropylene at different sites of a single catalyst. This superior miscibility of the high-density polyethylene composition having dispersed polypropylene according to the present disclosure can be experimentally confirmed from the very uniform appearance of the film surface in the micrograph of Example 1 in FIG. 1.
[0062] In the case of polypropylene / high-density polyethylene blend resins, polypropylene is dispersed within a high-density polyethylene matrix and blended as polymer units. In contrast, the high-density polyethylene composition of the present disclosure disperses polypropylene in much smaller polymer units because the polypropylene is prepolymerized into propylene polymer units, thereby achieving a more even dispersion. Due to this difference, articles manufactured from the high-density polyethylene composition of the present disclosure exhibit superior heat resistance and strength, specifically, shear modulus, tensile strength, and elongation.
[0063] In one embodiment, the high-density polyethylene composition having polypropylene dispersed therein may comprise polypropylene in an amount of 30 wt% or less, 20 wt% or less, or 15 wt% or less, based on the total weight of the high-density polyethylene composition having polypropylene dispersed therein. In addition, the high-density polyethylene composition having polypropylene dispersed therein may comprise polypropylene in an amount of 0.1 wt% or more, 1 wt% or more, 2 wt% or more, 3 wt% or more, 4 wt% or more, 5 wt% or more, 7 wt% or more, 10 wt% or more, or 12 wt% or more, based on the total weight of the high-density polyethylene composition having polypropylene dispersed therein. The high-density polyethylene composition having polypropylene dispersed therein may comprise polypropylene in an amount of 1 to 30 wt% or 7 to 20 wt%, based on the total weight of the high-density polyethylene composition having polypropylene dispersed therein.
[0064] When the high-density polyethylene composition in which the polypropylene is dispersed contains 1 to 30 wt% of polypropylene based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed, the article manufactured from the high-density polyethylene composition in which the polypropylene is dispersed has excellent physical properties such as heat resistance and strength, specifically shear modulus, tensile strength, and elongation. In one embodiment, the shear modulus of the article measured at 145°C by the ASTM E143 method may be 0.1 MPa or more, 0.11 MPa or more, 0.12 MPa or more, 0.13 MPa or more, 0.14 MPa or more, or 0.15 MPa or more. Additionally, the shear modulus of the above article measured at 145°C by the ASTM E143 method may be 0.3 MPa or less, 0.25 MPa or less, 0.2 MPa or less, 0.18 MPa or less, or 0.16 MPa or less. The shear modulus of the above article measured at 145°C by the ASTM E143 method may be 0.1 to 0.3 MPa.
[0065] In one embodiment, the tensile strength of the above product measured by the ASTM D638 method is 400 kgf / cm. 2 Above, 450 kgf / cm 2 or more than 500 kgf / cm 2 It may be more than 800 kgf / cm. In addition, the tensile strength of the above product measured by the ASTM D638 method is 800 kgf / cm. 2 Below 750 kgf / cm 2 Below 700 kgf / cm 2 Below 650 kgf / cm 2 Less than or equal to 600 kgf / cm 2 The tensile strength of the above product measured by the ASTM D638 method may be 400 to 800 kgf / cm. 2 It could be.
[0066] In one embodiment, the elongation of the above article measured by the ASTM D638 method is 700% or more, 750% or more. Above, 800% The elongation of the article may be 850% or more, or 900% or more. In addition, the elongation of the article as measured by the ASTM D638 method may be 1200% or less, 1100% or less, 1050% or less, 1000% or less, or 950% or less. The elongation of the article as measured by the ASTM D638 method may be 750 to 1100%.
[0067] That is, an article manufactured from a high-density polyethylene composition in which polypropylene is dispersed according to the present disclosure exhibits excellent physical properties such as shear modulus, tensile strength, and elongation compared to a simple blend resin of polypropylene and high-density polyethylene.
[0068] In one embodiment, an article manufactured from the high-density polyethylene composition in which the polypropylene is dispersed may have a shear modulus measured at 145°C of 0.1 to 0.3 MPa, or a tensile strength of 400 to 800 kgf / cm. 2 It may be, or the elongation may be 750 to 1100%, or it may satisfy at least two of the above property ranges among the above shear modulus, the above tensile strength and the above elongation, or it may satisfy all three property ranges simultaneously.
[0069] In one embodiment, the article may be, but is not limited to, a film, a sheet, a foam, a fiber, an envelope, or a packaging material.
[0070] The high-density polyethylene composition having polypropylene dispersed therein according to the present disclosure can then be molded into a suitable shape from the viewpoint of further deformation and end use.
[0071]
[0072] The present invention will be described in more detail below based on the following examples and comparative examples. However, the following examples and comparative examples are merely illustrative examples for further illustrating the present invention, and the present invention is not limited by the following examples and comparative examples. Unless otherwise specified, all temperatures herein are expressed in degrees Celsius, and unless otherwise specified, the amount of composition used is expressed in weight percent.
[0073] [Shear modulus measurement]
[0074] A 2 mm thick sheet was manufactured using a press from the pellets, and the shear modulus was measured using a rheometer (MCR 702, Anton Paar) in Temperature / Torsion mode while increasing the temperature from 120°C to 150°C according to the ASTM E143 method.
[0075] [Tensile strength and elongation measurement]
[0076] A film with a thickness of 30 μm was manufactured from pellets using a 40 mm blown film extruder (40 mmΦ Screw, 75 mmΦ Die, 2 mm Die Gap), and the extrusion conditions were fixed as C1 / C2 / C3 / A / D1 / D2=160 / 165 / 170 / 175 / 180 / 180℃, Screw Speed= 60 rpm, Blow-up Ratio (BUR)=2.
[0077] The tensile strength and elongation of the film were measured using a tensile tester (Instron 5500R) at a speed of 500 mm / min according to the ASTM D638 method.
[0078] [Example 1]
[0079] 1. Catalytic activation step (R-101)
[0080] Ziegler-Natta catalyst Z-213 (magnesium chloride titanium tetrachloride complex, Lyondellbasell) 1.75 kg / hr, donor (cyclohexylmethyldimethoxysilane) 1.1 kg / hr, and TEAL (triethylaluminum) 7.7 kg / hr are introduced into R-101 (pre-contact drum) operated at approximately 15°C and brought into contact, whereby the reaction centers of the catalyst are activated before coming into contact with the monomer.
[0081] 2. Catalyst stabilization (prepolymerization) stage (R-200A / B)
[0082] The prepolymerization reaction takes place in two loop reactors (R-200A / B), each filled with liquid propane. Propylene is the only monomer fed. The activated catalyst, activated by R-101, is fed into the first prepolymerization reactor, R-200A (operating at 20°C and 17 Kg), where it reacts with propylene. Propylene is fed at a rate of 140 kg / hr, and morphology begins to form in the catalyst.
[0083] The prepolymer from R-200A is then fed into the second prepolymerization reactor R-200B (operating temperature 30°C and operating pressure 17 K / G) and reacted with propylene. Propylene is fed at a rate of 230 kg / hr, which fully activates the catalyst and prevents R-201 from fouling.
[0084] 3. First polymerization stage (R-201)
[0085] Polypropylene and activated catalyst formed in R-200A / B are fed into the front end of the compressor (C-201), mixed with propane and propylene gas circulated by the compressor (C-201), and reacted by forming a fluidized bed in R-201 (first gas phase reactor). At this time, 2100 kg of propylene is fed and polymerized. Propane does not participate in the reaction and is used to control the pressure inside the reactor. The fraction of propylene inside the reactor is maintained at 15 mol% or less for operational stability. In addition, 3 kg / hr of antistatic agent (Atmer 163, CRODA) is fed. The reactor R-201 is operated under an operating pressure of 15 to 17 K / G and an operating temperature of 58 to 61°C.
[0086] 4. Second polymerization stage (R-202)
[0087] The polymer that has undergone the primary reaction in R-201 passes through F-201 (Recycle Gas Filter) into R-202 (second gas phase reactor) and undergoes a fluidization reaction by propane, ethylene, and hydrogen circulated by a compressor (C-202). 14,500 kg / hr of ethylene and 3 kg / hr of hydrogen are fed into R-202. Additionally, 3.2 kg / hr of an antistatic agent (Atmer 163, CRODA) is fed. Propylene is polymerized up to 15 wt% based on the total weight of the high-density polyethylene composition in which polypropylene is dispersed in R-201, and the remaining 85 wt% is polymerized by the ethylene input in R-202. Gas fluidization within the reactor is accomplished by a centrifugal compressor (C-202). Reactor R-202 is operated at an operating pressure of 20 to 23 K / G and an operating temperature of 78 to 81°C.
[0088] The reacted polymer was degassed, steam-cleaned, and dried to obtain a powdered polymer. The obtained powdered polymer was pelletized using an extruder to obtain pellets.
[0089] The pellets obtained above were processed according to the measurement method described above, and the shear modulus, tensile strength, and elongation were measured, and are shown in Table 1.
[0090] [Example 2]
[0091] The same procedure as Example 1 was followed, except that propylene was polymerized up to 10 wt% in the first polymerization stage (R-201) reactor and the remaining 90% was polymerized by introducing ethylene in the second polymerization stage (R-202) reactor.
[0092] Shear modulus, tensile strength, and elongation were measured and are shown in Table 1.
[0093] [Example 3]
[0094] The same procedure as Example 1 was followed, except that propylene was polymerized up to 5 wt% in the first polymerization stage (R-201) reactor and the remaining 95% was polymerized by introducing ethylene in the second polymerization stage (R-202) reactor.
[0095] Shear modulus, tensile strength, and elongation were measured and are shown in Table 1.
[0096] [Comparative Example 1]
[0097] A blend of 15 wt% polypropylene (GJ-183, Lotte Chemical) and 85 wt% HDPE product (MF5000, Lotte Chemical) was manufactured in pellet form.
[0098] Shear modulus, tensile strength, and elongation were measured and are shown in Table 1.
[0099] [Comparative Example 2]
[0100] A blend of 10 wt% polypropylene (GJ-183, Lotte Chemical) and 90 wt% HDPE product (MF5000, Lotte Chemical) was manufactured in pellet form.
[0101] Shear modulus, tensile strength, and elongation were measured and are shown in Table 1.
[0102] [Comparative Example 3]
[0103] A blend of 5 wt% polypropylene (GJ-183, Lotte Chemical) and 95 wt% HDPE product (MF5000, Lotte Chemical) was manufactured in pellet form.
[0104] Shear modulus, tensile strength, and elongation were measured and are shown in Table 1.
[0105] [Comparative Example 4]
[0106] A 100% HDPE product (MF5000, Lotte Chemical) without polypropylene blending was manufactured in pellet form.
[0107] Shear modulus, tensile strength, and elongation were measured and are shown in Table 1.
[0108] Shear modulus (measured at 145℃, MPa) Tensile strength (kgf / cm) 2 ) Elongation (%) Example 10.154510900 Example 20.139470885 Example 30.128445830 Comparative Example 10.091200400 Comparative Example 20.084350600 Comparative Example 30.072390690 Comparative Example 40.061395698
[0109] Compared to the case of simply blending or not blending polypropylene as in Comparative Examples 1 to 4, Examples 1 to 3, in which propylene was prepolymerized on a catalyst seed to form a polypropylene catalyst seed, polypropylene was polymerized on the formed polypropylene catalyst seed, and polyethylene was polymerized on the polymerized polypropylene catalyst seed, exhibited excellent shear modulus, tensile strength, and elongation, indicating that the physical properties were significantly improved. In contrast, the simple blends of polypropylene described in Comparative Examples 1 to 4 were measured to have low values for shear modulus, tensile strength, and elongation, indicating that the physical properties were insufficient. Although the preferred embodiments of the present invention have been described above, it is clear that the present invention can use various changes and equivalent ranges, and that the above examples can be appropriately modified and applied in the same manner. Therefore, the above description does not limit the scope of the present invention defined by the following claims.
Claims
1. a) A catalyst activation step of forming an activated catalyst by introducing a catalyst, a cocatalyst, and a donor; b) a catalyst stabilization step of prepolymerizing propylene on the activated catalyst to form a polypropylene catalyst seed; c) a first polymerization step of polymerizing polypropylene onto the polypropylene catalyst seed by introducing propylene; and d) A method for producing a high-density polyethylene composition in which polypropylene is dispersed, comprising a second polymerization step of polymerizing polyethylene by introducing ethylene.
2. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein in step c), polypropylene is polymerized in an amount of 1 to 30 wt% based on the total weight of the high-density polyethylene composition in which polypropylene is dispersed.
3. In paragraph 2, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein in step c), polypropylene is polymerized in an amount of 7 to 20 wt% based on the total weight of the high-density polyethylene composition in which polypropylene is dispersed.
4. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein the catalyst comprises a Ziegler-Natta catalyst.
5. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein the cocatalyst comprises at least one selected from the group consisting of TEAL (triethylaluminum), TIBAL (Triisobutylaluminum), and TOA (trioctyl aluminum).
6. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein the donor comprises at least one selected from the group consisting of cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, isobutylisopropyldimethoxysilane, diisobutyldimethoxysilane, dicyclopentyldimethoxysilane, and dicyclohexyldimethoxysilane.
7. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein the weight of the cocatalyst is in the range of 4 to 5 based on the weight of the catalyst.
8. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein the weight of the cocatalyst is in the range of 5 to 9 with respect to the weight of the donor.
9. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein step b) is performed in two loop reactors connected in series.
10. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein the fraction of propylene in the reactor in step c) is 15 mol% or less.
11. In paragraph 1, e) A method for producing a high-density polyethylene composition in which polypropylene is dispersed, further comprising a step of steam cleaning and drying the high-density polyethylene composition in which polypropylene is dispersed obtained in step d).
12. In paragraph 11, f) A method for producing a high-density polyethylene composition in which polypropylene is dispersed, further comprising the step of adding an additive to the high-density polyethylene composition in which polypropylene is dispersed and extruding the composition after going through the step e).
13. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein an antistatic agent is further added in step c).
14. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein an antistatic agent is further added in step d).
15. In paragraph 1, A method for producing a high-density polyethylene composition in which polypropylene is dispersed, wherein ethylene is further added in step c).
16. An article manufactured from a high-density polyethylene composition in which polypropylene is dispersed, The high-density polyethylene composition in which the polypropylene is dispersed contains 1 to 30 wt% of polypropylene based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed, An article having an elongation of 750 to 1100% as measured by the ASTM D638 method.
17. In paragraph 16, An article wherein the high-density polyethylene composition in which the polypropylene is dispersed comprises 7 to 20 wt% of polypropylene based on the total weight of the high-density polyethylene composition in which the polypropylene is dispersed.
18. In paragraph 16, An article having a shear modulus of 0.1 to 0.3 MPa measured at 145°C according to the ASTM E143 method of the above article.
19. In paragraph 16, The tensile strength of the above product measured by the ASTM D638 method is 400 to 800 kgf / cm. 2 People, goods.
Citation Information
Patent Citations
An improved Ziegler-Natta catalyst for olefin polymerization.
KR1019980070873A
Hybrid supported metallocene catalyst and preparation of polyethylene copolymer using the same
KR1020060091528A
Brake system, brake control device, system, control method and vehicle
KR1020210008894A
Method and unmanned parking control system for providing parking service to customer
KR102607779B1
Polypropylene-polyethylene composition with improved flowability
US20180215846A1