Composite conductive agent, and negative electrode composition, negative electrode sheet, battery and electric device comprising same
By adhering the organic film-forming additive to the surface of the conductive substrate, the problems of SEI film instability and precipitation risks in the secondary battery are solved, and higher cycling performance and stability are achieved, and battery life is extended.
Patent Information
- Application Number
- PCT/CN2023/121041
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2023-09-25
- Publication Date
- 2024-12-05
AI Technical Summary
The solid electrolyte interface film (SEI film) on the surface of the negative electrode film layer in existing secondary batteries is unstable, resulting in a degradation of battery capacity and cycling performance. The organic film-forming additives are prone to precipitation during drying, occupying the binder position, resulting in Risk of membrane shedding.
A composite conductive agent is used, in which the organic film-forming additive is attached to the surface of the conductive substrate through chemical bonds and is uniformly dispersed in the negative electrode slurry to form a stable SEI film, reducing the risk of precipitation, and improving the density and uniformity of the SEI film.
It significantly improves the cycle performance and stability of the battery, extends the cycle life of the battery, reduces the risk of negative electrode film falling off, and improves the rate performance and energy density of the battery.
Smart Images

Figure CN2023121041_05122024_PF_FP_ABST
Abstract
Description
Composite conductive agent, negative electrode composition containing the same, negative electrode sheet, battery and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310611703.7 filed on May 26, 2023, entitled “Composite conductive agent, negative electrode composition containing same, negative electrode sheet, battery and electrical device”, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to a composite conductive agent, a negative electrode composition containing the composite conductive agent, a negative electrode sheet, a battery, and an electrical device. Background Art
[0004] Secondary batteries rely on the reciprocal intercalation and deintercalation of active ions between the positive and negative electrodes to charge and discharge. Lithium-ion batteries, for example, offer outstanding characteristics such as high energy density, long cycle life, zero pollution, and no memory effect. Consequently, secondary batteries, as a clean energy source, have gradually spread from electronic products to large-scale devices such as electric vehicles, aligning with sustainable environmental and energy development strategies. Consequently, this has placed higher demands on the cycle performance of secondary batteries.
[0005] Summary of the Invention
[0006] In order to achieve the above-mentioned objectives, the present application provides a composite conductive agent, which can improve the cycle performance of the battery containing the composite conductive agent; the present application also provides a negative electrode composition, a negative electrode sheet, a battery and an electrical device containing the composite conductive agent.
[0007] A first aspect of an embodiment of the present application provides a composite conductive agent, which includes a conductive substrate and an organic film-forming additive. The organic film-forming additive includes halogen atoms, and the organic film-forming additive is attached to the surface of the conductive substrate.
[0008] Without intending to be bound by any theory or explanation, the composite conductive agent of the embodiment of the present application contains an organic film-forming additive, and the organic film-forming additive molecules contain halogen atoms, which can interact with the electrolyte to form a solid electrolyte interface (SEI film) in situ. In the related art, when preparing the negative electrode slurry, the organic film-forming additive is mixed with other ingredients as an independent component, and the resulting negative electrode slurry is coated and dried to form a negative electrode film layer; however, during the drying process of the negative electrode slurry, the organic film-forming additive will migrate to the surface of the formed negative electrode film layer and precipitate, which on the one hand causes the SEI film subsequently formed on the surface of the negative electrode film layer to be unstable, and on the other hand may occupy the position of the binder, resulting in the risk of the negative electrode film layer falling off from the current collector surface. Compared with the related art, in the embodiment of the present application, the organic film-forming additive is attached to the surface of the conductive substrate, which can allow the organic film-forming additive to be uniformly dispersed in the negative electrode slurry along with the conductive substrate, and then uniformly dispersed in the negative electrode slurry coating. This significantly reduces the probability of organic film-forming additives precipitating during the drying process of the negative electrode sheet, thereby reducing the risk of the negative electrode film layer falling off the current collector surface due to precipitation of organic film-forming additives. Furthermore, it ensures that the organic film-forming additives are evenly distributed throughout the negative electrode film layer. A suitable amount of organic film-forming additives uniformly distributed throughout the negative electrode film layer facilitates the in-situ formation of a dense, uniform, and stable SEI film on the negative electrode film surface, effectively suppressing battery capacity decay and improving the stability of the negative electrode environment.
[0009] Therefore, the composite conductive agent of the embodiment of the present application is applied to a secondary battery, which can effectively improve the cycle performance of the battery.
[0010] In any embodiment of the present application, the organic film-forming additive is attached to the surface of the conductive substrate through chemical bonds.
[0011] When the organic film-forming additive is attached to the surface of the conductive substrate through chemical bonds, the organic film-forming additive and the conductive substrate can be more firmly combined, thereby reducing the risk of the organic film-forming additive falling off the conductive substrate surface during the preparation and processing of the negative electrode. This is conducive to further improving the uniformity and stability of the SEI film, and thus improving the cycling performance of the battery.
[0012] In any embodiment of the present application, the conductive substrate includes a carbon material, and the carbon material includes unsaturated carbon-carbon double bonds and / or carbon-carbon triple bonds.
[0013] The organic film-forming additives include fluorine-containing film-forming additives, which contain fluorine-substituted carbon chains and electrophilic groups pendant from the carbon chains.
[0014] The fluorine-containing film-forming additive is attached to the surface of the conductive substrate through a covalent bond formed by the reaction of an electrophilic group with a carbon-carbon double bond and / or a carbon-carbon triple bond.
[0015] When the organic film-forming additive includes a fluorine-containing film-forming additive, it is beneficial to further improve the density of the SEI film, thereby further improving the stability of the negative electrode environment during the charge and discharge cycle, thereby improving the cycle performance of the battery.
[0016] In any embodiment of the present application, the molecular chain of the fluorine-containing film-forming additive comprises a structural unit copolymer segments.
[0017] Here, R1 and R2 each independently represent a hydrogen atom or a C1-C6 alkyl group.
[0018] Therefore, the composite conductive agent of the embodiment of the present application is applied to the negative electrode sheet of a secondary battery, and can form a uniform, dense and stable SEI film on the surface of the negative electrode sheet, thereby improving the cycle performance of the battery.
[0019] In any embodiment of the present application, in the fluorine-containing film-forming additive, and The average molar ratio of is 0.5 to 5. Therefore, the composite conductive agent of the embodiment of the present application has a suitable content of conductive substrate and fluorine-containing film-forming additive, and is applied to the negative electrode sheet to enable the battery to maintain good rate performance and improve the cycle performance of the battery.
[0020] In any embodiment of the present application, the weight average molecular weight Mw of the fluorine-containing film-forming additive is 3000 to 800000. This not only improves the film-forming performance of the composite conductive agent, but also enables the composite conductive agent to be evenly dispersed and entangled with each other in the negative electrode film layer, so that the composite conductive agent has certain bonding properties.
[0021] In any embodiment of the present application, the fluorine-containing film-forming additive includes one or more of the compounds shown in Formula 1.
[0022] Among them, R 11 ~R 14 Each independently represents a hydrogen atom or a C1-C6 alkyl group.
[0023] m is selected from integers of 0 to 3000, n is selected from integers of 30 to 3000, p is selected from integers of 0 to 3000, and m+p>0.
[0024] The fluorine-containing film-forming additive is attached to the surface of the conductive substrate through a covalent bond formed by the reaction of an azide group with a carbon-carbon double bond and / or a carbon-carbon triple bond.
[0025] The compound represented by Formula 1 has specific structural units that can enhance the conductivity and film-forming properties of the composite conductive agent. Therefore, when applied to the negative electrode of a secondary battery, the composite conductive agent can improve the density, uniformity, and stability of the SEI film, thereby enhancing the battery's cycling performance.
[0026] In any embodiment of the present application, R 11 ~R 14 Each independently represents a hydrogen atom or a C1-C3 alkyl group.
[0027] In any embodiment of the present application, m is selected from an integer of 300 to 3000, n is selected from an integer of 30 to 3000, and p is selected from an integer of 300 to 3000.
[0028] When R 11 ~R 14 When at least one of m, n, and p satisfies the aforementioned conditions, the composite conductive agent's conductivity and film-forming properties can be further enhanced. Consequently, the composite conductive agent, when applied to the negative electrode of a secondary battery, can further improve the density, uniformity, and stability of the SEI film, thereby enhancing the battery's cycling performance.
[0029] In any embodiment of this application,
[0030] In any embodiment of this application,
[0031] When m, n, and p in Formula 1 meet the above conditions, the fluorine-containing film-forming additive molecular chain can contain an appropriate amount of azide groups, thereby connecting the fluorine-containing film-forming additive molecular chain to an appropriate amount of conductive substrate. Thus, the conductive properties of the composite conductive agent can be improved. In addition, when m, n, and p in Formula 1 meet the above conditions, the fluorine-containing film-forming additive can also have an appropriate fluorine content, thereby improving the density and stability of the SEI film. Therefore, the composite conductive agent of the embodiment of the present application is applied to the negative electrode of a secondary battery, which can further improve the cycle performance of the battery.
[0032] In any embodiment of the present application, 0.5≤m / p≤1.5.
[0033] In any embodiment of the present application, 0.8≤m / p≤1.2.
[0034] When the ratio of m to p in the compound shown in Formula 1 is within the above range, it can be considered that the molecular chain of the fluorine-containing film-forming additive has a high symmetry. In other words, when the ratio of m to p is within the above range, the fluorine atoms can be more evenly distributed in the molecular chain of the fluorine-containing film-forming additive. As a result, the uniformity of the SEI film formed in situ by the composite conductive agent can be further improved. Therefore, the composite conductive agent of the embodiment of the present application is applied to the negative electrode of the secondary battery, which can further improve the cycle performance of the battery.
[0035] In any embodiment of the present application, the conductive substrate includes one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0036] The surface of the conductive substrate selected from the above types may include an appropriate amount of reactive oxygen-containing groups, making it easy to modify to introduce unsaturated carbon-carbon double bonds and / or carbon-carbon triple bonds, thereby allowing the conductive substrate to be firmly bonded to the organic film-forming additive. As a result, the composite conductive agent of the embodiments of the present application can form a more uniform SEI film in situ in the negative electrode film layer, thereby improving the cycling performance of the battery.
[0037] In any embodiment of the present application, the weight percentage of the conductive substrate is 8% to 95% based on the total weight of the composite conductive agent. By adjusting the weight percentage of the conductive substrate in the composite conductive agent, the conductive properties and film-forming properties of the composite conductive agent can be regulated. When the weight percentage of the conductive substrate falls within the given range, the composite conductive agent of the embodiment of the present application, when applied to the negative electrode of a secondary battery, can improve the battery's cycle stability and extend the battery's cycle life.
[0038] A second aspect of an embodiment of the present application provides a negative electrode composition, which includes a negative electrode active material and the composite conductive agent of the first aspect.
[0039] The negative electrode composition of the second aspect of the present invention includes the composite conductive agent of the first aspect. When applied to the negative electrode sheet of a secondary battery, it can form a dense, uniform, and stable SEI film in situ on the surface of the negative electrode film layer, thereby effectively suppressing the battery's capacity decay and improving the stability of the negative electrode environment. As a result, the battery's cycling performance can be effectively improved.
[0040] In any embodiment of the present application, based on the total mass of the negative electrode composition, the mass percentage of the composite conductive agent is 0.2% to 3.0%, and can be optionally 0.5% to 2.0%.
[0041] The mass percentage of the composite conductive agent is within the above-mentioned appropriate range, so that the negative electrode film layer contains an appropriate amount of fluorine-containing film-forming additive, thereby improving the density and uniformity of the SEI film, thereby improving the cycle stability of the battery.
[0042] A third aspect of an embodiment of the present application provides a negative electrode plate, comprising a negative electrode current collector and a negative electrode film layer located on at least one side of the negative electrode current collector, wherein the negative electrode film layer comprises the negative electrode composition of the second aspect.
[0043] The negative electrode sheet of the third aspect of the present invention comprises the negative electrode composition of the second aspect. When applied to the negative electrode sheet of a secondary battery, a dense, uniform, and stable SEI film can be formed in situ on the surface of the negative electrode film layer, thereby effectively suppressing the capacity decay of the battery and improving the stability of the negative electrode environment. Thus, the cycle performance of the battery can be effectively improved.
[0044] In any embodiment of the present application, the infrared absorption spectrum of the negative electrode plate may have a wavelength at 1180 cm -1 ~1185cm -1 The characteristic peaks are characteristic of -CF2-. When the infrared absorption spectrum of the negative electrode sheet exhibits these characteristic peaks, it helps further enhance the density of the SEI film. This, in turn, helps further improve the stability of the negative electrode environment during charge-discharge cycles, thereby enhancing the battery's cycling performance.
[0045] A fourth aspect of an embodiment of the present application provides a battery, comprising the negative electrode plate of the third aspect.
[0046] A fifth aspect of an embodiment of the present application provides an electrical device, comprising the battery of the fourth aspect.
[0047] The electric device according to the embodiment of the present application includes the battery according to the fourth aspect, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] FIG1 is a schematic diagram of an embodiment of a battery cell of the present application.
[0049] FIG. 2 is an exploded view of the embodiment of the battery cell of the present application shown in FIG. 1 .
[0050] FIG3 is a schematic diagram of an embodiment of a battery module of the present application.
[0051] FIG4 is a schematic diagram of an embodiment of a battery pack of the present application.
[0052] FIG5 is an exploded view of the embodiment of the battery pack of the present application shown in FIG4 .
[0053] FIG6 is a schematic diagram of an embodiment of an electric device of the present application. The electric device may include a battery pack or a battery module according to an embodiment of the present application as a power source.
[0054] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 battery cell; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION
[0055] Hereinafter, the embodiments of the composite conductive agent, the negative electrode composition containing the composite conductive agent, the negative electrode sheet, the battery and the electric device of the present application will be described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0056] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0057] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0058] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0059] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0060] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0061] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0062] As used herein, the term "alkyl" refers to a saturated hydrocarbon group, including both straight-chain and branched structures. Examples of alkyl groups include, but are not limited to, methyl, ethyl, propyl (e.g., n-propyl, isopropyl), butyl (e.g., n-butyl, isobutyl, sec-butyl, tert-butyl), and pentyl (e.g., n-pentyl, isopentyl, neopentyl). In various embodiments, a C1-C6 alkyl group, i.e., an alkyl group, may contain 1 to 6 carbon atoms.
[0063] Throughout this specification, substituents of compounds are disclosed in groups or ranges. It is expressly intended that such descriptions include every individual subcombination of the members of these groups and ranges. For example, the term "C1-C6 alkyl" is expressly intended to disclose individually C1, C2, C3, C4, C5, C6, C1-C6, C1-C5, C1-C4, C1-C3, C1-C2, C2-C6, C2-C5, C2-C4, C2-C3, C3-C6, C3-C5, C3-C4, C4-C6, C4-C5, and C5-C6 alkyl.
[0064] With the application and promotion of secondary batteries in various electronic products and new energy vehicles and other industries, higher requirements are placed on the cycle performance of secondary batteries.
[0065] During the first charging process of a secondary battery, a solid electrolyte interface (SEI) film is formed on the surface of the negative electrode active material. The SEI film is insoluble in organic solvents and can exist stably in organic electrolyte solutions. The SEI film allows active lithium ions to pass through, but does not allow solvent molecules to pass through, thereby effectively inhibiting the co-embedding of solvent molecules and reducing the damage to the negative electrode active material caused by the co-embedding of solvent molecules. However, during the charge and discharge cycle, the SEI film may rupture due to reasons such as the expansion of the negative electrode active material, and active lithium ions need to be continuously consumed to form a new SEI film. The SEI film is unstable, which not only aggravates the capacity decay of the battery, but is also not conducive to maintaining the stability of the negative electrode environment, thereby worsening the cycle performance of the battery. Since the formation mechanism and composition of the SEI film are not very clear at present, how to generate a stable SEI film remains a very challenging technical task.
[0066] In view of this, an embodiment of the present application provides a composite conductive agent, which can improve the cycle performance of a battery containing the composite conductive agent; the present application also provides a negative electrode composition, a negative electrode sheet, a battery and an electrical device containing the composite conductive agent.
[0067] Composite conductive agent
[0068] In a first aspect of an embodiment of the present application, a composite conductive agent is proposed, which includes a conductive substrate and an organic film-forming additive. The organic film-forming additive includes halogen atoms, and the organic film-forming additive is attached to the surface of the conductive substrate.
[0069] In this application, "the organic film-forming additive is attached to the surface of the conductive substrate" means that the organic film-forming additive molecules are anchored to the surface of the conductive substrate through interaction with the surface of the conductive substrate. For example, the organic film-forming additive may be attached to the surface of the conductive substrate through chemical bonds or strong hydrogen bonds. As an example, those skilled in the art may modify the organic film-forming additive and / or the conductive substrate to allow the organic film-forming additive to interact with the conductive substrate (e.g., to form chemical bonds or hydrogen bonds), thereby allowing the organic film-forming additive to adhere to the surface of the conductive substrate.
[0070] Without intending to be bound by any theory or explanation, the composite conductive agent of the embodiment of the present application contains an organic film-forming additive, and the organic film-forming additive molecules contain halogen atoms, which can interact with the electrolyte to form an SEI film in situ. In the related art, when preparing the negative electrode slurry, the organic film-forming additive is mixed with other ingredients as an independent component, and the resulting negative electrode slurry is coated and dried to form a negative electrode film layer; however, during the drying process of the negative electrode slurry, the organic film-forming additive will migrate to the surface of the formed negative electrode film layer and precipitate, which on the one hand causes the SEI film subsequently formed on the surface of the negative electrode film layer to be unstable, and on the other hand may occupy the position of the binder, resulting in the risk of the negative electrode film layer falling off from the current collector surface. Compared with the related art, in the embodiment of the present application, the organic film-forming additive is attached to the surface of the conductive substrate, which can allow the organic film-forming additive to be uniformly dispersed in the negative electrode slurry along with the conductive substrate, and then uniformly dispersed in the negative electrode slurry coating. This significantly reduces the probability of organic film-forming additives precipitating during the drying process of the negative electrode sheet, thereby reducing the risk of the negative electrode film layer falling off the current collector surface due to precipitation of organic film-forming additives. Furthermore, it ensures that the organic film-forming additives are evenly distributed throughout the negative electrode film layer. A suitable amount of organic film-forming additives uniformly distributed throughout the negative electrode film layer facilitates the in-situ formation of a dense, uniform, and stable SEI film on the negative electrode film surface, effectively suppressing battery capacity decay and improving the stability of the negative electrode environment.
[0071] Therefore, the composite conductive agent of the embodiment of the present application is applied to a secondary battery, which can effectively improve the cycle performance of the battery.
[0072] Examples of conductive substrates may include one or more conductive materials known in the art. Examples of organic film-forming additives may include fluorine-containing film-forming additives and / or chlorine-containing film-forming additives known in the art. Those skilled in the art may select suitable conductive substrates and organic film-forming additives based on actual application needs, provided that the organic film-forming additive adheres to the surface of the conductive substrate. This is not a limitation herein.
[0073] In some embodiments, the organic film-forming additive is attached to the surface of the conductive substrate via chemical bonds.
[0074] Without intending to be bound by any theory or explanation, when the organic film-forming additive is attached to the surface of the conductive substrate through chemical bonds, the organic film-forming additive and the conductive substrate can be more firmly combined, thereby reducing the risk of the organic film-forming additive falling off the conductive substrate surface during the preparation and processing of the negative electrode plate. This helps to further improve the uniformity of the organic film-forming additive in the negative electrode film layer, thereby improving the uniformity and stability of the SEI film, and further improving the cycling performance of the battery.
[0075] In some embodiments, the conductive substrate comprises a carbon material, which may include unsaturated carbon-carbon double bonds and / or carbon-carbon triple bonds. The organic film-forming additive may include a fluorine-containing film-forming additive, which may include a fluorine-substituted carbon chain and an electrophilic group pendant from the carbon chain. The fluorine-containing film-forming additive is attached to the surface of the conductive substrate via a covalent bond formed by the reaction of the electrophilic group with the carbon-carbon double bond and / or carbon-carbon triple bond.
[0076] Without intending to be bound by any theory or explanation, when the organic film-forming additive includes a fluorine-containing film-forming additive, it is beneficial to further enhance the density of the SEI film, thereby further enhancing the stability of the negative electrode environment during charge and discharge cycles, thereby improving the cycle performance of the battery.
[0077] In some embodiments, the molecular chain of the fluorine-containing film-forming additive comprises a structural unit of wherein R1 and R2 may each independently represent a hydrogen atom or a C1 to C6 alkyl group.
[0078] In the above embodiment, the fluorine-containing film-forming additive can be used to form a structural unit Monomers and structural units The monomers are formed by alternating copolymerization, random copolymerization or block copolymerization, which is not limited here.
[0079] Without intending to be bound by any theory or explanation, the structural units It has a high content of F atoms, which can interact with the electrolyte to form a dense and stable SEI film in situ; the structural unit The fluorine-containing film-forming additive can be grafted onto the surface of the conductive substrate through the reaction of the azide group with the carbon-carbon double bond and / or carbon-carbon triple bond contained in the conductive substrate, so that the fluorine-containing film-forming additive is attached to the surface of the conductive substrate through the covalent bond formed by the reaction of the azide group with the carbon-carbon double bond and / or carbon-carbon triple bond. As a result, the composite conductive agent of the embodiment of the present application can be used in the negative electrode of a secondary battery to form a uniform, dense, and stable SEI film on the surface of the negative electrode, thereby improving the cycle performance of the battery.
[0080] In some embodiments, the fluorine-containing film-forming additive comprises: and The average molar ratio can be 0.5-5, for example, 0.5, 0.7, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, 4.2, 4.5, 4.8, 5, or a range consisting of any two of the above values.
[0081] Without intending to be bound by any theory or explanation, when the fluorine-containing film-forming additive, the structural unit and When the average molar ratio of satisfies the above range, the composite conductive agent can have both good conductivity and good film-forming properties, thereby enabling the secondary battery to have both good rate performance and cycle performance. and The average molar ratio of is within the above-mentioned suitable range, which allows the fluorine-containing film-forming additive to combine with an appropriate amount of conductive substrate to obtain a composite conductive agent. The composite conductive agent has a suitable conductive substrate content and is applied to the negative electrode pole piece to form a conductive network inside the negative electrode film layer, thereby reducing polarization and allowing the battery to maintain good rate performance. The composite conductive agent also has a suitable fluorine-containing film-forming additive content and is applied to the negative electrode pole piece to form a dense and stable SEI film on the surface of the negative electrode pole piece, thereby improving the cycle performance of the battery.
[0082] In some embodiments, the weight average molecular weight Mw of the fluorine-containing film-forming additive may be 3,000-800,000, for example, 3,000, 5,000, 8,000, 10,000, 50,000, 100,000, 300,000, 500,000, 800,000, or a range consisting of any two of the above values.
[0083] Without intending to be bound by any theory or explanation, when the weight-average molecular weight (Mw) of the fluorine-containing film-forming additive falls within the given range, the fluorine-containing film-forming additive can have an appropriate molecular chain length and fluorine atom content. Having an appropriate molecular chain length and fluorine atom content not only improves the film-forming performance of the composite conductive agent, but also allows the composite conductive agent to be evenly dispersed and entangled with each other in the negative electrode film layer, thus imparting a certain degree of bonding performance to the composite conductive agent. This allows the negative electrode film layer to have a lower binder content, thereby allowing the battery to have a higher energy density.
[0084] The weight-average molecular weight has a meaning well known in the art and can represent the sum of the weight fractions of molecules of different molecular weights in a polymer multiplied by their corresponding molecular weights. The weight-average molecular weight can be measured using equipment and methods known in the art. For example, it can be measured using high-temperature GPC (differential refractive index detector).
[0085] In some embodiments, the fluorine-containing film-forming additive may include one or more of the compounds shown in Formula 1.
[0086] In formula 1, R 11 ~R 14 Each independently represents a hydrogen atom or a C1-C6 alkyl group.
[0087] m is selected from an integer of 0 to 3000, n is selected from an integer of 30 to 3000, p is selected from an integer of 0 to 3000, and m+p>0. Optionally, m+p≥300.
[0088] The fluorine-containing film-forming additive is attached to the surface of the conductive substrate through a covalent bond formed by the reaction of an azide group with a carbon-carbon double bond and / or a carbon-carbon triple bond.
[0089] The compound represented by Formula 1 has specific structural units that can enhance the conductivity and film-forming properties of the composite conductive agent. Therefore, when applied to the negative electrode of a secondary battery, the composite conductive agent can improve the density, uniformity, and stability of the SEI film, thereby enhancing the battery's cycling performance.
[0090] In the compound shown in Formula 1, the respective values of m, n, and p can be measured by equipment and methods known in the art. For example, the nuclear magnetic resonance hydrogen spectrum of the fluorine-containing film-forming additive can be measured by a nuclear magnetic resonance instrument, and the respective values of m, n, and p can be measured using the nuclear magnetic resonance hydrogen spectrum.
[0091] In some embodiments, R 11 ~R 14 Each independently may represent a hydrogen atom or a C1-C3 alkyl group.
[0092] Alternatively, in some embodiments, R 11 ~R 14 At least one of represents a hydrogen atom. As an example, R 11 ~R 14 They may all represent hydrogen atoms.
[0093] In some embodiments, m is selected from an integer ranging from 300 to 3000, n is selected from an integer ranging from 30 to 3000, and p is selected from an integer ranging from 300 to 3000.
[0094] Alternatively, in some embodiments, m is selected from an integer of 1000 to 2000, n is selected from an integer of 100 to 2000, and p is selected from an integer of 1000 to 2000.
[0095] Without intending to be bound by any theory or explanation, when R 11 ~R 14 When at least one of m, n, and p satisfies the aforementioned conditions, the composite conductive agent's conductivity and film-forming properties can be further enhanced. Consequently, the composite conductive agent, when applied to the negative electrode of a secondary battery, can further improve the density, uniformity, and stability of the SEI film, thereby enhancing the battery's cycling performance.
[0096] In some embodiments, Equation 1 may satisfy: For example, It can be 0.05, 0.10, 0.12, 0.15, 0.19, 0.21, 0.23, 0.27, 0.30, 0.32, 0.35, or a range formed by any two of the above values.
[0097] In some embodiments, Formula 1 may also satisfy: etc.
[0098] It is not intended to be limited to any theory or explanation. When m, n, and p in Formula 1 meet the above conditions, the fluorine-containing film-forming additive molecular chain can contain an appropriate amount of azide groups, thereby connecting the fluorine-containing film-forming additive molecular chain to an appropriate amount of conductive substrate. Thus, the conductivity of the composite conductive agent can be improved. In addition, when m, n, and p in Formula 1 meet the above conditions, the fluorine-containing film-forming additive can also have a suitable fluorine content, thereby improving the density and stability of the SEI film. Therefore, the composite conductive agent of the embodiment of the present application is applied to the negative electrode of the secondary battery, which can further improve the cycle performance of the battery.
[0099] In some embodiments, Formula 1 may satisfy: 0.5≤m / p≤1.5. For example, m / p may be 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, or a range consisting of any two of the above values.
[0100] In some embodiments, Formula 1 may further satisfy: 0.8≤m / p≤1.2. For example, m / p may be 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, or a range consisting of any two of the above values.
[0101] Without intending to be bound by any theory or explanation, when the ratio of m to p in the compound shown in Formula 1 is within the above range, it can be considered that the molecular chain of the fluorine-containing film-forming additive has a high symmetry. In other words, when the ratio of m to p is within the above range, the fluorine atoms can be more evenly distributed in the molecular chain of the fluorine-containing film-forming additive. As a result, the uniformity of the SEI film formed in situ by the composite conductive agent can be further improved. Therefore, the composite conductive agent of the embodiment of the present application is applied to the negative electrode of the secondary battery to further improve the cycle performance of the battery.
[0102] In some embodiments, the conductive substrate may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0103] The surface of the conductive substrate selected from the above types may include an appropriate amount of reactive oxygen-containing groups, making it easy to modify to introduce unsaturated carbon-carbon double bonds and / or carbon-carbon triple bonds, thereby allowing the conductive substrate to be firmly bonded to the organic film-forming additive. As a result, the composite conductive agent of the embodiments of the present application can form a more uniform SEI film in situ in the negative electrode film layer, thereby improving the cycling performance of the battery.
[0104] In some embodiments, based on the total mass of the composite conductive agent, the mass percentage of the conductive substrate can be 8% to 95%, for example, 8%, 12%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or a range consisting of any two of the above values.
[0105] Without intending to be bound by any theory or explanation, adjusting the mass percentage of the conductive substrate in the composite conductive agent can regulate the conductive properties and film-forming properties of the composite conductive agent. When the mass percentage of the conductive substrate meets the given range, the composite conductive agent of the embodiment of the present application is applied to the negative electrode of the secondary battery, which can not only improve the conductive properties of the negative electrode and suppress the internal resistance growth of the battery during the cycle, but also form a dense SEI film in situ on the surface of the negative electrode, thereby enhancing the stabilizer of the negative electrode environment and suppressing the capacity decay of the battery. As a result, the cycle stability of the battery can be improved and the cycle life of the battery can be extended.
[0106] The composite conductive agent of the embodiment of the present application can be obtained in various ways. As an example, the composite conductive agent can be obtained through the following steps S10 to S30.
[0107] S10, providing a conductive material modified with carbon-carbon double bonds and / or carbon-carbon triple bonds.
[0108] Step S10 can be achieved by methods known in the art. In some embodiments, the conductive material may include a conductive carbon material, for example, conductive carbon black Super P. Providing a conductive material modified with a carbon-carbon double bond and / or a carbon-carbon triple bond can specifically include: mixing conductive carbon black and propargyl alcohol, a catalytic amount of N,N'-dicyclohexylcarboximide (DCC) and 4-dimethylaminopyridine (DMAP) evenly, so that groups such as carboxyl groups on the surface of the conductive carbon black react with propargyl alcohol under the catalysis of DCC and DMAP, thereby obtaining a conductive carbon black modified with a carbon-carbon double bond. The molar ratio of conductive carbon black to propargyl alcohol can be (1:0.8) to (1:1.2).
[0109] S20, providing an organic film-forming additive containing an electrophilic group, wherein the organic film-forming additive includes a halogen atom.
[0110] Step S20 can be achieved by methods known in the art. The organic film-forming additive containing halogen atoms can be modified, or an organic film-forming additive containing both electrophilic groups and halogen atoms can be directly synthesized, which is not limited here.
[0111] S30, uniformly mixing the conductive material modified with carbon-carbon double bonds and / or carbon-carbon triple bonds and the organic film-forming additive containing electrophilic groups in an appropriate amount of solvent, evacuating the mixture (to avoid oxidation of free radicals), and then adding a catalytic amount of CuCl under an inert atmosphere to allow the conductive material modified with carbon-carbon double bonds and / or carbon-carbon triple bonds to react with the organic film-forming additive containing electrophilic groups in an appropriate amount of solvent at a reaction temperature. The resulting crude product is poured into ice ether at 0°C for sedimentation to obtain a composite conductive agent.
[0112] In step S30, the inert atmosphere may include a nitrogen atmosphere and / or a rare gas atmosphere. The reaction temperature may be 23°C to 27°C, for example, room temperature (25°C).
[0113] In some embodiments, providing an organic film-forming additive containing an electrophilic group may include the following steps S21 to S24 .
[0114] S21, acryloyl chloride, ethyl azido and a catalytic amount of triethylamine are mixed evenly in an appropriate amount of tetrahydrofuran (THF) solvent to allow acryloyl chloride and ethyl azido to react to obtain an intermediate product A.
[0115] In step S21, the inert atmosphere may include a nitrogen atmosphere and / or a rare gas atmosphere. The reaction temperature may be -5°C to 5°C, for example, 0°C.
[0116] S22, dissolving vinylidene fluoride in an appropriate amount of THF solvent, evacuating the mixture (to avoid oxidation of free radicals), adding an initiator under an inert atmosphere to allow the vinylidene fluoride to polymerize at the reaction temperature, and pouring the crude product into 0°C ice ether for precipitation to separate and obtain the intermediate product B.
[0117] In step S22, the inert atmosphere may include a nitrogen atmosphere and / or a noble gas atmosphere. The initiator may include, but is not limited to, one or more of a peroxide initiator, an azo initiator, and a redox initiator, such as azobisisobutyronitrile (AIBN). The reaction temperature may be 65°C to 75°C, for example, 70°C.
[0118] S23, dissolving intermediate product A and intermediate product B in an appropriate amount of THF solvent, evacuating the mixture (to avoid oxidation of free radicals), adding an initiator under an inert atmosphere, causing intermediate product A and intermediate product B to undergo polymerization reaction at the reaction temperature, pouring the crude product into 0°C ice ether for precipitation, and separating to obtain intermediate product C.
[0119] In step S23, the inert atmosphere may include a nitrogen atmosphere and / or a noble gas atmosphere. The initiator may include, but is not limited to, one or more of a peroxide initiator, an azo initiator, and a redox initiator, such as azobisisobutyronitrile (AIBN). The reaction temperature may be 65°C to 75°C, for example, 70°C.
[0120] S24, dissolving the intermediate product C and vinylidene fluoride in an appropriate amount of THF solvent, evacuating the mixture (to prevent free radical oxidation), and then adding an initiator under an inert atmosphere to allow the intermediate product C and vinylidene fluoride to undergo a polymerization reaction at the reaction temperature. The crude product is poured into 0°C ice ether for sedimentation, and an organic film-forming additive containing an electrophilic group is separated.
[0121] In step S24, the inert atmosphere may include a nitrogen atmosphere and / or a noble gas atmosphere. The initiator may include, but is not limited to, one or more of a peroxide initiator, an azo initiator, and a redox initiator, such as azobisisobutyronitrile (AIBN). The reaction temperature may be 65°C to 75°C, for example, 70°C.
[0122] Negative electrode composition
[0123] A second aspect of an embodiment of the present application provides a negative electrode composition, which includes a negative electrode active material and the composite conductive agent of the first aspect.
[0124] The negative electrode composition of the second aspect of the present invention includes the composite conductive agent of the first aspect. When applied to the negative electrode sheet of a secondary battery, it can form a dense, uniform, and stable SEI film in situ on the surface of the negative electrode film layer, thereby effectively suppressing the battery's capacity decay and improving the stability of the negative electrode environment. As a result, the battery's cycling performance can be effectively improved.
[0125] In some embodiments, based on the total mass of the negative electrode composition, the mass percentage of the composite conductive agent may be 0.2% to 3.0%, and optionally 0.5% to 2.0%.
[0126] Without intending to be limited by any theory or explanation, the mass percentage of the composite conductive agent is within the above-mentioned appropriate range, so that the negative electrode film layer contains an appropriate amount of fluorine-containing film-forming additives, thereby improving the density and uniformity of the SEI film, thereby improving the cycle stability of the battery.
[0127] In the negative electrode composition of the embodiment of the present application, the negative electrode active material may adopt the negative electrode active material for secondary batteries known in the art. As an example, the negative electrode active material may include one or more of graphite, soft carbon, hard carbon, mesophase carbon microbeads, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials. The embodiments of the present application are not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials for secondary batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0128] In some embodiments, the negative electrode active material may include a silicon-based material. The negative electrode composition of the present invention includes a composite conductive agent, which can improve the density and uniformity of the SEI film, thereby improving the stability and capacity of the silicon-based material during cycling, thereby allowing the battery to have a high energy density.
[0129] In some embodiments, the negative electrode composition may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0130] In some embodiments, the negative electrode composition may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0131] Negative electrode
[0132] A third aspect of an embodiment of the present application provides a negative electrode plate, which includes a negative electrode current collector and a negative electrode film layer located on at least one side of the negative electrode current collector, and the negative electrode film layer includes the negative electrode composition of the second aspect.
[0133] The negative electrode sheet of the third aspect of the present invention comprises the negative electrode composition of the second aspect. When applied to the negative electrode sheet of a secondary battery, a dense, uniform, and stable SEI film can be formed in situ on the surface of the negative electrode film layer, thereby effectively suppressing the capacity decay of the battery and improving the stability of the negative electrode environment. Thus, the cycle performance of the battery can be effectively improved.
[0134] In some embodiments, the infrared absorption spectrum of the negative electrode sheet may have a wavelength at 1180 cm -1 ~1185cm -1 characteristic peaks.
[0135] The above characteristic peaks are characteristic of -CF2-. When the infrared absorption spectrum of the negative electrode exhibits these characteristic peaks, it helps further enhance the density of the SEI film. This, in turn, helps further improve the stability of the negative electrode environment during charge and discharge cycles, thereby enhancing the battery's cycling performance.
[0136] The infrared absorption spectrum of the negative electrode sheet can be measured using equipment and methods known in the art. For example, the negative electrode film layer can be scraped to obtain a negative electrode film powder, which is then mixed with a solvent (e.g., N-methylpyrrolidone) and fully dissolved before filtration. The filter residue is then subjected to infrared spectroscopy to obtain the infrared absorption spectrum of the negative electrode sheet.
[0137] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector may have two opposing surfaces in its thickness direction, and the negative electrode film layer may be disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0138] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil or aluminum foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0139] In some embodiments, the negative electrode sheet can be prepared by the following method: dispersing the above-mentioned negative electrode composition, such as the negative electrode active material, the composite conductive agent, the binder and any other components in a solvent (such as deionized water) to form a negative electrode slurry; coating the negative electrode slurry on one or both surfaces of the negative electrode collector; after drying, cold pressing and other processes, the negative electrode sheet of the present application can be obtained.
[0140] In addition, the negative electrode plates of the embodiments of the present application do not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plates of the embodiments of the present application may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) disposed between the negative electrode current collector and the negative electrode film layer. In other embodiments, the negative electrode plates of the embodiments of the present application may further include a protective layer covering the surface of the negative electrode film layer.
[0141] Battery
[0142] A fourth aspect of the present application provides a battery. The battery described in the present application may include one or more battery cells to provide a single physical module with higher voltage and capacity. When there are multiple battery cells, the multiple battery cells are connected in series, parallel, or hybrid via a busbar.
[0143] The battery cell may be a secondary battery, also known as a rechargeable battery or storage battery. This refers to a battery cell that can be recharged to activate the active material after discharge and continue to be used. The present application does not specifically limit the type of secondary battery. For example, the secondary battery may be a lithium-ion battery, a lithium metal battery, etc. In particular, the secondary battery may be a lithium-ion battery.
[0144] Typically, a battery cell includes an electrode assembly and an electrolyte, and the electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator.
[0145] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0146] [Positive electrode]
[0147] The positive electrode sheet included in the battery of the embodiment of the present application includes a positive electrode current collector and a positive electrode film layer located on at least one side of the positive electrode current collector, and the positive electrode film layer includes a positive electrode active material.
[0148] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0149] In the positive electrode sheet of the embodiment of the present application, the positive electrode active material may adopt the positive electrode active material for secondary batteries well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides and their respective modified compounds. However, the embodiment of the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for lithium-ion batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include but are not limited to lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0150] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0151] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0152] In some embodiments, the positive electrode film layer may further include a conductive agent and an optional dispersant. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0153] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0154] [Negative electrode]
[0155] The negative electrode sheet included in the battery of the embodiment of the present application includes the negative electrode sheet of the third aspect of the embodiment of the present application. The embodiment of the negative electrode sheet has been described and illustrated in detail above and will not be repeated here. It is understood that the battery of the embodiment of the present application can achieve the beneficial effects of any of the above-mentioned embodiments of the negative electrode sheet of the embodiment of the present application.
[0156] [Isolation film]
[0157] The separator is disposed between the positive electrode and the negative electrode to serve as an isolation film. The present invention has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0158] In some embodiments, the material of the separator can be selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0159] [Electrolytes]
[0160] The electrolyte conducts ions between the positive and negative electrodes. The present invention does not specifically limit the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be in liquid or gel form.
[0161] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0162] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0163] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0164] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0165] In some embodiments, the battery cell further includes a housing for housing the electrode assembly and electrolyte. The housing of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the housing of the battery cell may be a soft shell, such as a pouch-type soft shell. The soft shell may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0166] The embodiment of the present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square, or any other shape. For example, FIG1 shows a battery cell 5 with a square structure as an example.
[0167] In some embodiments, referring to Figure 2, the housing may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0168] The preparation method of the battery cell of the embodiment of the present application is well known. In some embodiments, the electrode assembly can be placed in a housing, dried, injected with electrolyte, and then vacuum packaged, allowed to stand, formed, and shaped to obtain a battery cell.
[0169] In some embodiments, the battery referred to in the embodiments of this application refers to a single physical module comprising one or more battery cells to provide higher voltage and capacity. For example, the battery referred to in the embodiments of this application may be a battery module or a battery pack. Batteries generally include a housing for enclosing one or more battery cells. The housing prevents liquids or other foreign matter from affecting the charging or discharging of the battery cells.
[0170] In some embodiments, a battery may contain multiple battery cells, which may be connected in series, in parallel, or in a hybrid configuration. A hybrid configuration refers to a combination of series and parallel connections. Multiple battery cells may be directly connected in series, in parallel, or in a hybrid configuration, and then the entire battery cell structure is housed within a housing. Alternatively, multiple battery cells may be first connected in series, in parallel, or in a hybrid configuration to form a battery module, which is then further connected in series, in parallel, or in a hybrid configuration to form a single unit and housed within a housing.
[0171] FIG3 is a schematic diagram of an example battery module 4. As shown in FIG3 , there are multiple battery cells 5, which are first connected in series, in parallel, or in a mixed series to form a battery module 4. The multiple battery cells 5 in the battery module 4 can be electrically connected via a busbar component to achieve the series, parallel, or mixed series connection of the multiple battery cells 5 in the battery module 4. In the battery module 4, the multiple battery cells 5 can be arranged sequentially along the length of the battery module 4. Of course, they can also be arranged in any other manner. The multiple battery cells 5 can further be fixed by fasteners.
[0172] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0173] Figures 4 and 5 are schematic diagrams of an example battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a housing and multiple battery modules 4 disposed within the housing. The multiple battery modules 4 within the battery pack 1 may be electrically connected via a busbar assembly to enable series, parallel, or mixed connection of the multiple battery modules 4 within the battery pack 1. The housing includes an upper housing 2 and a lower housing 3. The upper housing 2 is used to cover the lower housing 3 and form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery box.
[0174] Electrical devices
[0175] The embodiments of the present application also provide an electric device, which includes a battery cell provided in the embodiments of the present application, and the battery cell is used to provide electrical energy. The battery cell can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0176] As the electrical device, a battery cell, a battery module including a plurality of battery cells, or a battery pack can be selected according to its usage requirements.
[0177] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module can be used.
[0178] As another example, an electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and may use a battery cell as a power source.
[0179] Example
[0180] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0181] Example 1
[0182] Preparation of composite conductive agent
[0183] Step (1): At 25° C., 1.1 mol of propargyl alcohol and 1 mol of conductive carbon black are reacted under the catalysis of 0.1 mol of N,N'-dicyclohexylcarboximide (DCC) and 0.1 mol of 4-dimethylaminopyridine (DMAP) for 8 hours to obtain modified conductive carbon black containing a carbon-carbon triple bond.
[0184] Step (2): At 0°C, 1.1 mol of acryloyl chloride and 1 mol of ethyl azide were added under the catalysis of 1 mL of triethylamine and reacted for 4 h to obtain intermediate product A.
[0185] Step (3): Weigh 1 mol of vinylidene fluoride, dissolve it in 200 mL of tetrahydrofuran, evacuate the flask (to avoid oxidation of free radicals), continuously introduce N2 into the three-necked flask, add 0.05 g of azobisisobutyronitrile initiator, heat to 70°C, stir and react for 12 hours, and then pour the obtained crude product into 0°C ice ether for precipitation to obtain intermediate product B.
[0186] Step (4): Weigh 0.1 mol of intermediate product B, add 1 mol of intermediate product A, dissolve in 200 mL of tetrahydrofuran (THF), evacuate (to avoid oxidation of free radicals), continuously introduce N2 into a three-necked flask, add 0.01 g of azobisisobutyronitrile initiator, heat to 70°C, stir the reaction for 12 hours, and then pour the obtained crude product into 0°C ice ether to precipitate to obtain intermediate product C.
[0187] Step (5): Weigh 0.1 mol of intermediate product C, add 1 mol of vinylidene fluoride, dissolve in 200 mL of tetrahydrofuran, evacuate (to avoid oxidation of free radicals), continuously introduce N2 into a three-necked flask, add 0.05 g of azobisisobutyronitrile initiator, heat to 70°C, stir and react for 12 hours, and then pour the obtained crude product into 0°C ice ether for precipitation to obtain intermediate product D.
[0188] Step (6): Weigh 1 mol of the intermediate product D, dissolve it in 200 mL of tetrahydrofuran, then add 1 mol of modified conductive carbon black, evacuate the flask (to avoid oxidation of free radicals), continuously introduce N2 into the three-necked flask, add 0.1 mol of CuCl, stir and react at room temperature for 12 hours, pour the obtained crude product into 0°C ice ether for precipitation, and obtain a composite conductive agent after separation and drying.
[0189] Preparation of positive electrode
[0190] The positive electrode active material lithium iron phosphate, the positive electrode binder polyvinylidene fluoride (PVDF), and the conductive agent acetylene black are mixed in a mass ratio of 96:2.5:1.5, N-methylpyrrolidone (NMP) is added as a solvent, the solid content is adjusted to 70%-80%, and the mixture is stirred evenly to obtain a positive electrode slurry; the positive electrode slurry is coated on aluminum foil, and then dried, cold pressed, and cut to obtain a positive electrode sheet.
[0191] Preparation of negative electrode sheet
[0192] The negative electrode active material artificial graphite, composite conductive agent, binder SBR, and sodium carboxymethyl cellulose (CMC-Na) are mixed in a mass ratio of 96:1.5:1.5:1, dispersed in deionized water, and stirred evenly to obtain a negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil, dried, and then dried, cold pressed, and cut to obtain a negative electrode sheet.
[0193] Isolation film
[0194] Polypropylene film is used as the isolation film.
[0195] Preparation of electrolyte
[0196] LiPF6 was dissolved in a solvent prepared by ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate in a volume ratio of 1:1:1 to obtain an electrolyte with a LiPF6 concentration of 1 mol / L.
[0197] Preparation of secondary batteries
[0198] The positive electrode sheet, separator, and negative electrode sheet are stacked in order to obtain an electrode assembly; the electrode assembly is placed in a packaging shell, and after drying, liquid injection, vacuum packaging, standing, forming, shaping and other processes, a secondary battery is obtained.
[0199] Examples 2 to 11
[0200] Based on the preparation process of the composite conductive agent in Example 1, the amounts of the intermediate product D and the modified conductive carbon in step (6), and the amounts of azobisisobutyronitrile m1 to m3 in steps (3) to (5) were adjusted as shown in Table 1 to prepare the composite conductive agents of Examples 2 to 11. The preparation of the positive electrode sheets, negative electrode sheets, separators, electrolytes, and secondary batteries of Examples 2 to 11 was the same as that of Example 1.
[0201] Comparative Example 1
[0202] Based on the preparation process of the positive electrode sheet, negative electrode sheet, separator, electrolyte and secondary battery of Example 1, the composite conductive agent was replaced with conductive carbon black of equal mass to prepare the secondary battery of Comparative Example 1.
[0203] Comparative Example 2
[0204] Based on the preparation process of the composite conductive agent in Example 1, an intermediate product D was prepared; 1 mol of the intermediate product D was weighed and uniformly mixed with 1 mol of unmodified conductive carbon black to obtain a mixed conductive agent.
[0205] Based on the preparation process of the positive electrode sheet, negative electrode sheet, separator, electrolyte and secondary battery of Example 1, the composite conductive agent was replaced with a mixed conductive agent of equal mass to prepare the secondary battery of Comparative Example 2.
[0206] The following tests were performed on Examples 1 to 11 and Comparative Examples 1 to 2. The test results are shown in Table 2.
[0207] (1) Battery DC resistance (DCR) test
[0208] At 25°C, the secondary battery was allowed to stand for 30 minutes, and then charged at a constant current of 0.33C to 3.65V; then charged at a constant voltage of 3.65V to a cutoff current of 0.05C; after standing for 5 minutes, the battery was discharged at a constant current of 0.33C for 90 minutes to a cutoff current of 0.5C, and the voltage at this time was recorded as U0; after standing for 1 hour, the battery was discharged at a rate of 2C for 30 seconds, the discharge current was recorded as I, and the voltage at the 10th second of discharge was recorded as U1; after standing for 5 minutes, the test was terminated.
[0209] The DCR of the battery = (U1-U0) / I.
[0210] (2) Normal temperature cycle performance test
[0211] At 25°C, let the secondary battery rest for 30 minutes, then discharge it at 0.33C to 2.5V. After resting for 30 minutes, charge it at 0.33C constant current to 3.65V, then charge it at 3.65V constant voltage to a cutoff current of 0.05C; let it rest for 30 minutes; discharge it at 0.33C to 2.5V; let it rest for 30 minutes. Repeat the above steps for the same battery, and record the discharge capacity C1 of the first cycle and the discharge capacity C of the 1000th cycle. 1000 .
[0212] Cycle capacity retention rate P of secondary battery 1000 =(C 1000 / C1)*100%.
[0213] Table 1
[0214] Table 2
[0215] As can be seen from Table 1 and Table 2, the composite conductive agent provided in the embodiments of the present application is applied to the negative electrode of a secondary battery, which can effectively reduce the internal resistance of the battery and improve the cycle performance of the battery.
[0216] Based on the test results of Examples 1-5, it can be seen that adjusting the relative contents of the conductive base material and the film-forming additive in the composite conductive agent can adjust the conductivity and film-forming properties of the composite conductive agent, thereby adjusting the internal resistance and cycle performance of the battery. Based on the test results of Examples 1, 6-11, it can be seen that adjusting the content of the electrophilic group in the film-forming additive can adjust the content of the conductive base material in the composite conductive agent, thereby adjusting the conductivity and film-forming properties of the composite conductive agent, thereby adjusting the internal resistance and cycle performance of the battery.
[0217] In contrast, the conventional conductive agent used in Comparative Example 1 resulted in unsatisfactory battery internal resistance and cycle performance. In the mixed conductive agent of Comparative Example 2, the film-forming additive did not adhere to the surface of the conductive substrate, which not only failed to improve the battery's cycle performance but also worsened its internal resistance and cycle performance.
[0218] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A composite conductive agent, comprising: Conductive substrate; as well as The organic film-forming additive comprises halogen atoms and is attached to the surface of the conductive substrate.
2. The composite conductive agent according to claim 1, wherein The organic film-forming additive is attached to the surface of the conductive substrate through chemical bonds.
3. The composite conductive agent according to claim 1 or 2, wherein: The conductive substrate comprises a carbon material, wherein the carbon material comprises an unsaturated carbon-carbon double bond and / or a carbon-carbon triple bond; The organic film-forming additive comprises a fluorine-containing film-forming additive, wherein the fluorine-containing film-forming additive comprises a fluorine-substituted carbon chain and an electrophilic group suspended from the carbon chain. The fluorine-containing film-forming additive is attached to the surface of the conductive substrate through a covalent bond formed by the reaction of the electrophilic group with the carbon-carbon double bond and / or carbon-carbon triple bond.
4. The composite conductive agent according to claim 3, wherein: The molecular chain of the fluorine-containing film-forming additive comprises structural units: The copolymer chain segment Here, R1 and R2 each independently represent a hydrogen atom or a C1-C6 alkyl group.
5. The composite conductive agent according to claim 3 or 4, wherein: In the fluorine-containing film-forming additive, and The average molar ratio is 0.5-5.
6. The composite conductive agent according to any one of claims 3 to 5, wherein The weight average molecular weight Mw of the fluorine-containing film-forming additive is 3,000 to 800,000.
7. The composite conductive agent according to any one of claims 3 to 6, wherein The fluorine-containing film-forming additive includes one or more of the compounds shown in Formula 1, Among them, R 11 ~R 14 Each independently represents a hydrogen atom or a C1-C6 alkyl group; m is selected from an integer of 0 to 3000, n is selected from an integer of 30 to 3000, p is selected from an integer of 0 to 3000, and m+p>0; The fluorine-containing film-forming additive is attached to the surface of the conductive substrate via a covalent bond formed by the reaction of an azide group with the carbon-carbon double bond and / or carbon-carbon triple bond.
8. The composite conductive agent according to claim 7, wherein: R 11 ~R 14 Each independently represents a hydrogen atom, a C1-C3 alkyl group; and / or m is selected from integers ranging from 300 to 3000, n is selected from integers ranging from 300 to 3000, and p is selected from integers ranging from 300 to 3000; and / or 9. The composite conductive agent according to claim 7 or 8, wherein:
10. The composite conductive agent according to claim 7 or 8, wherein: 0.5≤m / p≤1.
5.
11. The composite conductive agent according to claim 7 or 8, wherein: 0.8≤m / p≤1.
2.
12. The composite conductive agent according to any one of claims 1 to 11, wherein The conductive substrate includes one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
13. The composite conductive agent according to any one of claims 1 to 12, wherein Based on the total mass of the composite conductive agent, the mass percentage of the conductive substrate is 8% to 95%. 14 . A negative electrode composition comprising a negative electrode active material and the composite conductive agent according to claim 1 .
15. The negative electrode composition according to claim 14, wherein: Based on the total mass of the negative electrode composition, the mass percentage of the composite conductive agent is 0.2%~3.0%。 16 . A negative electrode sheet, comprising a negative electrode current collector and a negative electrode film layer located on at least one side of the negative electrode current collector, wherein the negative electrode film layer comprises the negative electrode composition according to claim 14 .
17. The negative electrode sheet according to claim 16, wherein: The infrared absorption spectrum of the negative electrode has a peak at 1180 cm -1 ~1185cm -1 characteristic peaks.
18. A battery comprising the negative electrode sheet according to claim 16 or 17.
19. An electrical device comprising the battery as claimed in claim 18.
Citation Information
Patent Citations
Water system battery and positive pole piece thereof
CN107785579A
Polymer, preparation method and application thereof, secondary battery, battery module, battery pack and electric device
CN115819690A
Electrolyte solution, electrochemical device, and electronic apparatus
CN116053588A
Composite conductive agent, negative electrode composition containing composite conductive agent, negative electrode pole piece, battery and electric device
CN116344826A
Nonaqueous electrolyte solution and electrochemical element using same
US20120171581A1