Medical magnesium alloy and preparation method therefor
Through laser integration into additive manufacturing technology and heat treatment in oxygen-rich environments, medical magnesium alloys with excellent mechanical properties and corrosion resistance were prepared, which solved the problem of fast degradation rate of magnesium alloys in physiological environments and met the application of biomedical field need.
Patent Information
- Application Number
- PCT/CN2024/082278
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-03-18
- Publication Date
- 2024-12-05
AI Technical Summary
Magnesium alloys have a fast degradation rate in physiological environments and have poor mechanical properties, which cannot meet the application requirements in the field of biomedical science.
Using laser incorporation of additive manufacturing technology to print magnesium alloy powder, physical polishing and heat treatment in oxygen-rich environments, magnesium alloys containing zinc, manganese, neodymium, yttrium and scandium were prepared to form a dense passivation layer to improve corrosion resistance. and mechanical properties.
Effectively slow down the degradation rate of magnesium alloys, improve their corrosion resistance and mechanical properties, and make their application prospects in the field of biomedical medicine.
Smart Images

Figure CN2024082278_05122024_PF_FP_ABST
Abstract
Description
Medical magnesium alloy and preparation method thereof
[0001] This application claims the benefit of Chinese patent application No. 2023106310852, filed May 31, 2023. This application incorporates the entirety of the aforementioned Chinese patent application. Technical Field
[0002] The present application relates to the technical field of magnesium alloys, and in particular to a medical magnesium alloy and a preparation method thereof. Background Art
[0003] The density of magnesium metal is only 1.8g / cm 3 , and is the lightest metal structural material. Magnesium alloys also boast high specific strength, specific stiffness, shock absorption, recyclability, and excellent thermal and electrical conductivity, making them suitable for industrial processing and forming, earning them the nickname "21st Century Green Engineering Metal." As a high-performance engineering material, magnesium alloys are widely used in military weaponry, transportation, electronic communications, healthcare, and other fields.
[0004] Magnesium alloys are attracting increasing attention in biomedical applications due to their excellent biocompatibility and comprehensive mechanical properties, such as elastic modulus, that are similar to those of human bone. However, their high chemical activity and rapid degradation in physiological environments, coupled with their poor mechanical properties, have severely hindered their development and application in biomedical applications. Therefore, effectively controlling the degradation rate of magnesium alloys and improving their mechanical properties are crucial for expanding their medical applications.
[0005] Summary of the Invention
[0006] The main purpose of this application is to provide a medical magnesium alloy and a preparation method thereof, so as to solve the problem in the prior art that magnesium alloys have a fast degradation rate in physiological environments, poor mechanical properties, and cannot meet the application requirements in the biomedical field.
[0007] In order to achieve the above-mentioned purpose, according to one aspect of the present application, a method for preparing a medical magnesium alloy is provided, which comprises: using laser fusion additive manufacturing technology to print out a formed magnesium alloy sample from magnesium alloy powder; physically polishing the outer surface of the formed magnesium alloy sample; and heat treating the physically polished formed magnesium alloy sample in an oxygen-rich environment to obtain a medical magnesium alloy; wherein, in terms of weight percentage, the magnesium alloy powder comprises 0.15-0.4wt% zinc, 0.01-0.05wt% manganese, 0.5-2.2wt% neodymium, 3.7-4.3wt% yttrium and the remainder magnesium.
[0008] Furthermore, the magnesium alloy powder further comprises 1.5 to 3.5 wt% of scandium; preferably, the particle size of the magnesium alloy powder is 20 to 80 μm, the D50 particle size is 45 to 50 μm, and the sphericity is greater than 98%; further preferably, the magnesium alloy powder is composed of 0.15 wt% of zinc, 0.01 wt% of manganese, 0.5 wt% of neodymium, 3.7 wt% of yttrium, 1.5 wt% of scandium and the balance of magnesium, in terms of weight percentage; or the magnesium alloy powder is composed of 0.20 wt% of zinc, 0.02 wt% of manganese, 1 wt% of % yttrium, 2.0 wt% scandium and the balance magnesium; or, the magnesium alloy powder consists of 0.25 wt% zinc, 0.03 wt% manganese, 1.5 wt% neodymium, 3.9 wt% yttrium, 2.5 wt% scandium and the balance magnesium; or, the magnesium alloy powder consists of 0.30 wt% zinc, 0.04 wt% manganese, 2.0 wt% neodymium, 4.0 wt% yttrium, 3.0 wt% scandium and the balance magnesium; or, the magnesium alloy powder consists of 0.40 wt% zinc, 0.05 wt% manganese, 1.5 wt% neodymium, 3.9 wt% yttrium, 2.5 wt% scandium and the balance magnesium. The magnesium alloy powder consists of 0.20wt% zinc, 0.03wt% manganese, 2.0wt% neodymium, 3.7wt% yttrium, 3.0wt% scandium and the balance magnesium.
[0009] Furthermore, the heat treatment includes: first heating the formed magnesium alloy sample after physical polishing treatment in an oxygen-rich environment at a temperature of 520-530°C for 6-10 hours; then water-cooling the heated formed magnesium alloy sample in an oxygen-rich environment at a temperature of 20-25°C at a cooling rate of 100-200°C / s to obtain a medical magnesium alloy; preferably, in the oxygen-rich environment, the oxygen volume content is ≥90%, and more preferably ≥99%.
[0010] Furthermore, the oxygen pressure during the heating process is ≤1 bar, preferably 0.3 to 0.6 bar; preferably, the oxygen flow rate during the heating process is 0.5 to 1 L / min.
[0011] Furthermore, the water cooling treatment time is 3 to 5 s; preferably, during the water cooling process, the volume of water used is 30 to 50 times the volume of the heated formed magnesium alloy sample; preferably, the oxygen flow rate during the water cooling process is 0.5 to 1 L / min.
[0012] Furthermore, physical polishing is performed by sandblasting; preferably, compressed air with a pressure of 2 to 6 bar is used as a carrier gas to carry hydroxyapatite powder for sandblasting; further preferably, the particle size of the hydroxyapatite powder is less than 100 μm, preferably 60 to 80 μm.
[0013] Furthermore, printing is carried out in a laser powder bed melting device; preferably, during the printing process, the laser power is 60 to 120 W, the scanning speed is 500 to 1200 mm / s, the powder thickness of each printed layer is 20 to 50 μm, and argon is used as the protective gas.
[0014] Furthermore, before the physical polishing treatment, the preparation method further includes a step of removing free powder particles on the surface of the formed magnesium alloy sample using compressed air.
[0015] Furthermore, after water cooling, the preparation method also includes: taking out the water-cooled material from the water, first drying the water-cooled material with compressed air, then placing the water-cooled material in anhydrous ethanol for ultrasonic cleaning for 10 to 15 minutes, and then drying the water-cooled material to obtain a medical magnesium alloy.
[0016] Furthermore, after physical polishing and before heat treatment, the preparation method further comprises: depositing yttrium ions on the outer surface of the formed magnesium alloy sample by ion implantation; preferably, the implantation dose of yttrium ions is 5×10 16 ~5×10 17 ions / cm 2 .
[0017] In order to achieve the above-mentioned objectives, according to one aspect of the present application, a medical magnesium alloy prepared by the aforementioned method for preparing a medical magnesium alloy is provided.
[0018] Based on the above preparation method, the medical magnesium alloy obtained in this application is not easy to degrade rapidly in a physiological environment, has excellent corrosion resistance, has better development prospects in the biomedical field, and also has very excellent mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings that constitute part of this application are used to provide a further understanding of this application. The illustrative embodiments of this application and their descriptions are used to explain this application and do not constitute an improper limitation on this application. In the drawings:
[0020] FIG1 shows a graph showing the thickness measurement of the film layer of the formed magnesium alloy sample obtained in Example 1.
[0021] FIG2 shows a graph showing the ultimate tensile strength test of the formed magnesium alloy samples obtained in Example 1 and Comparative Example 1.
[0022] FIG3 shows a compressive strength test diagram of the formed magnesium alloy samples obtained in Example 1 and Comparative Example 1.
[0023] FIG4 shows a test diagram of elastic coefficients of formed magnesium alloy samples obtained in Example 1 and Comparative Example 1.
[0024] FIG5 shows the elemental analysis diagram of the surface layer of the formed magnesium alloy sample obtained in Example 1.
[0025] FIG6 shows the degradation process of the medical magnesium alloy sample obtained in Example 1 in a simulated body fluid (Hanks).
[0026] FIG7 shows a scanning electron microscope image of the medical magnesium alloy sample obtained in Comparative Example 1.
[0027] FIG8 shows a scanning electron microscope image of the medical magnesium alloy sample obtained in Example 1.
[0028] FIG9 shows a test graph of hydrogen evolution in simulated body fluid (Hanks) of the medical magnesium alloy samples obtained in Example 1, Example 2 and Comparative Example 1. DETAILED DESCRIPTION
[0029] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments in this application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0030] As described in the background section of this application, the prior art has the problem of a fast degradation rate and poor mechanical properties of magnesium alloys. To address this problem, this application provides a method for preparing a medical magnesium alloy, the method comprising: using laser fusion additive manufacturing technology to print a molded magnesium alloy sample from magnesium alloy powder; physically polishing the outer surface of the molded magnesium alloy sample; and heat treating the physically polished molded magnesium alloy sample in an oxygen-rich environment to obtain a medical magnesium alloy; wherein, in terms of weight percentage, the magnesium alloy powder comprises 0.15-0.4wt% zinc, 0.01-0.05wt% manganese, 0.5-2.2wt% neodymium, 3.7-4.3wt% yttrium, and the remainder magnesium.
[0031] First, the magnesium alloy powder includes 0.15-0.4wt% zinc, 0.01-0.05wt% manganese, 0.5-2.2wt% neodymium, 3.7-4.3wt% yttrium, and the balance magnesium. First, zinc has a low melting point (419.58°C), the same crystal structure (hcp) as magnesium, and a similar atomic radius to magnesium. It can form a continuous solid solution with magnesium and has a high solid solubility in magnesium (approximately 6.2%). On the one hand, zinc can combine with neodymium and yttrium to form a high-strength precipitation-strengthened magnesium alloy, thereby improving the strength of the product; on the other hand, zinc can also refine the grain size and reduce stress corrosion sensitivity, thereby improving the corrosion resistance of the product. Second, compared to other metal elements (such as iron), the addition of manganese to magnesium alloys can not only give the product excellent strength and corrosion resistance, but also better weldability. This has positive significance for improving the melting quality in additive manufacturing micro-casting technology and has a better prospect for industrial application. Third, the addition of neodymium and yttrium not only improves the strength of magnesium alloys, but also improves their corrosion resistance. Specifically, after heat treatment, neodymium and yttrium can form a dense passivation layer (oxide film) on the surface of magnesium alloy products. The formation of this passivation layer can significantly reduce the degradation rate of magnesium alloys. At the same time, a large amount of yttrium-zinc phase and magnesium-yttrium phase will be generated in the product, reducing the probability of generating MgZn and MgZn2 phases and their growth. In this way, the precipitated phase of the yttrium-containing alloy can become more numerous, more dispersed, and finer, thereby refining the product alloy structure and improving the product's tensile strength and corrosion resistance.
[0032] Secondly, the inventors found that the fluidity of magnesium alloy powder including 0.15-0.4wt% zinc, 0.01-0.05wt% manganese, 0.5-2.2wt% neodymium, 3.7-4.3wt% yttrium and the remainder magnesium is not very good. Such magnesium alloy powder with specific composition, combined with micro-casting laser and additive manufacturing technology, can be further printed to obtain molded magnesium alloy samples with excellent performance, and has better application prospects.
[0033] Furthermore, the outer surface finish of the formed magnesium alloy sample printed out by the laser-infused additive manufacturing technology is poor. It is difficult for such a sample to form a passivation layer (oxide film) with good density and continuity on the surface during the subsequent heat treatment. Therefore, the present application performs physical polishing on the outer surface of the formed magnesium alloy sample before heat treatment. It is further explained here that in the art, chemical methods (such as acid treatment) are often used when treating the surface finish of magnesium alloy samples. However, these chemical methods not only cannot effectively improve the surface finish of the sample, but also fail to form an oxide film with good density and continuity during the subsequent heat treatment. At the same time, when using reagents (such as acid) for treatment, it is inevitable that chemical reactions will occur with the active metal (such as Mg) in the magnesium alloy sample or the yttrium on the surface, thereby directly affecting the formation and content of the oxide film, resulting in poor passivation quality of the magnesium alloy, insufficient corrosion resistance, and decreased product application performance. Moreover, in actual production, large-scale pickling operations will have operational safety issues and environmental pollution problems, and the pickling time is not easy to control. The physical polishing mode adopted in this application can not only make the outer surface of the formed magnesium alloy sample smoother, but also facilitate the formation of a passivation layer (oxide film) with better density and continuity in subsequent heat treatment. The product can also have excellent strength and corrosion resistance, and the operation is simpler, faster and safer.
[0034] In particular, the applicant has discovered that high-temperature heat treatment in a conventional air environment can cause magnesium to react with certain substances (e.g., CO2) to form impurities (e.g., MgCO3). This can affect the passivation effect of magnesium, thereby reducing the density and continuity of the product's passivation layer. Consequently, the degradation rate of the magnesium alloy still cannot effectively meet the requirements of biomedical applications. The present application avoids the above problems by heat-treating the formed magnesium alloy samples after physical polishing in an oxygen-rich environment, significantly slowing the degradation rate of the magnesium alloy and improving its strength.
[0035] In summary, based on the above preparation method, the medical magnesium alloy obtained in this application is not easily degraded rapidly in a physiological environment, has excellent corrosion resistance, has better development prospects in the biomedical field, and also has very excellent high-strength performance.
[0036] To further slow the degradation rate of the product, the magnesium alloy powder preferably also includes 1.5-3.5 wt% scandium. The addition of scandium can improve the strength and ductility of magnesium alloys. Scandium has a higher limit solubility in magnesium than other rare earth elements, and can improve the strength and ductility of magnesium alloys through age hardening and texture weakening.
[0037] In some preferred embodiments, the magnesium alloy powder is composed of 0.15wt% zinc, 0.01wt% manganese, 0.5wt% neodymium, 3.7wt% yttrium, 1.5wt% scandium and the balance magnesium, by weight percentage; or, the magnesium alloy powder is composed of 0.20wt% zinc, 0.02wt% manganese, 1wt% neodymium, 3.8wt% yttrium, 2.0wt% scandium and the balance magnesium; or, the magnesium alloy powder is composed of 0.25wt% zinc, 0.03wt% manganese, 1.5wt% neodymium, 3.9wt% yttrium, 2.5wt% scandium and the balance magnesium. and the balance magnesium; or, the magnesium alloy powder consists of 0.30wt% zinc, 0.04wt% manganese, 2.0wt% neodymium, 4.0wt% yttrium, 3.0wt% scandium and the balance magnesium; or, the magnesium alloy powder consists of 0.40wt% zinc, 0.05wt% manganese, 2.2wt% neodymium, 4.3wt% yttrium, 3.5wt% scandium and the balance magnesium; or, the magnesium alloy powder consists of 0.20wt% zinc, 0.03wt% manganese, 2.0wt% neodymium, 3.7wt% yttrium, 3.0wt% scandium and the balance magnesium.
[0038] In a preferred embodiment, the magnesium alloy powder has a particle size of 20 to 80 μm, a D50 particle size of 45 to 50 μm, and a sphericity greater than 98%. This is based on the considerations that: a magnesium alloy powder with a particle size below 20 μm and a D50 particle size below 45 μm, on the one hand, increases safety risks and is prone to explosions, posing a high safety hazard to equipment operation; on the other hand, it can cause the product to degrade faster. A magnesium alloy powder with a particle size above 80 μm and a D50 particle size above 50 μm can lead to poor melting quality of the magnesium alloy, easily causing internal defects, low density, poor product surface quality, and, in particular, accelerated degradation. Therefore, based on the above considerations, the magnesium alloy powder of this application has a particle size of 20 to 80 μm, a D50 particle size of 45 to 50 μm, and a sphericity greater than 98%. This improves safety and improves product performance in all aspects.
[0039] In order to further improve the strength of the product and slow down the degradation rate of the product, the heat treatment includes: first heating the formed magnesium alloy sample after physical polishing in an oxygen-rich environment at a temperature of 520-530°C for 6-10 hours; then water-cooling the heated formed magnesium alloy sample in an oxygen-rich environment at a temperature of 20-25°C at a cooling rate of 100-200°C / s (for example, 100°C / s, 150°C / s or 200°C / s) to obtain a medical magnesium alloy. In order to further improve the corrosion resistance of the product, in a preferred embodiment, the oxygen volume content in the oxygen-rich environment is ≥90%, for example, 90%, 92%, 94%, 96%, 98% or 100%; more preferably ≥99%.
[0040] In order to make the heat treatment process more stable and the product performance more uniform. In a preferred embodiment, the oxygen pressure during the heating process is ≤1 bar, preferably 0.3~0.6 bar. The oxygen flow rate during the heating process is 0.5~1L / min. The water cooling treatment time is 3~5s. During the water cooling process, the volume of water used is 30~50 times the volume of the heated formed magnesium alloy sample (for example, it can be 30 times, 35 times, 40 times, 45 times or 50 times). The oxygen flow rate during the water cooling process is 0.5~1L / min. Based on this, the density and continuity of the magnesium passivation layer are better, so that the degradation rate and strength of the magnesium alloy can better meet the application requirements in the biomedical field.
[0041] In order to further improve the efficiency of sandblasting, physical polishing is performed by sandblasting. In a preferred embodiment, compressed air with a pressure of 2 to 6 bar is used as a carrier gas to carry hydroxyapatite powder for sandblasting. Hydroxyapatite powder has a hard material, moderate particle size, good biocompatibility, and is harmless to the human body. Using compressed air with a pressure of 2 to 6 bar as a carrier gas to carry hydroxyapatite powder for sandblasting is more conducive to the formation of a passivation layer (oxide film) with better density and continuity in subsequent heat treatment. The product can have excellent strength and corrosion resistance at the same time, and the operation is simpler, faster, and safer. Preferably, the particle size of the hydroxyapatite powder is <100 μm, more preferably 60 to 80 μm, for example, it can be 60 μm, 70 μm or 80 μm. In a preferred embodiment, compressed air with a pressure of 2 to 6 bar is used as a carrier gas to carry hydroxyapatite powder for sandblasting until the surface is smooth (bright silver appears).
[0042] In a preferred embodiment, printing is performed in a laser powder bed fusion device. During printing, the laser power is 60 to 120 W, for example, 60 W, 80 W, 100 W, or 120 W; the scanning speed is 500 to 1200 mm / s, for example, 500 mm / s, 600 mm / s, 700 mm / s, 800 mm / s, 900 mm / s, 1000 mm / s, 1100 mm / s, or 1200 mm / s; the thickness of each powder layer is controlled to be 20 to 50 μm, for example, 20 μm, 30 μm, 40 μm, or 50 μm; and argon is used as the shielding gas during printing, with the oxygen content in the system being no greater than 0.001% by volume.
[0043] In order to further improve the efficiency of subsequent physical polishing, the preparation method further includes a step of removing free powder particles on the surface of the formed magnesium alloy sample using compressed air before physical polishing.
[0044] In order to further remove scum on the surface of the product, preferably after water cooling, the preparation method also includes: taking the water-cooled material out of the water, first blowing the water-cooled material dry with compressed air, then placing the water-cooled material in anhydrous ethanol for ultrasonic cleaning for 10 to 15 minutes, and then placing the water-cooled material in a drying oven for drying to obtain a medical magnesium alloy.
[0045] In order to further improve the corrosion resistance of the product, in a preferred embodiment, after physical polishing and before heat treatment, the preparation method further includes: depositing yttrium ions on the outer surface of the formed magnesium alloy sample by ion implantation. The ion implantation method is to accelerate the ions to be implanted in the product in a vacuum at low temperature, so that the ions with high kinetic energy can directly enter the product. Preferably, the implantation dose of yttrium ions is 5×10 16 ~5×10 17 ions / cm 2 .
[0046] The present application also provides a medical magnesium alloy prepared by the aforementioned preparation method of medical magnesium alloy. Based on the above reasons, the medical magnesium alloy of the present application can not only meet the degradation rate requirements of the physiological environment, but also has excellent strength properties.
[0047] The present application is further described in detail below with reference to specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in this application.
[0048] Example 1
[0049] The magnesium alloy powder used in this example is a customized magnesium alloy powder produced by Tangshan Weihao Magnesium Powder Co., Ltd. Its composition and particle size meet the requirements for raw material powders specified in this article. The magnesium alloy powder comprises 0.2 wt% zinc, 0.03 wt% manganese, 2.0 wt% neodymium, 3.7 wt% yttrium, 3.0 wt% scandium, and the balance magnesium. The magnesium alloy powder has a D50 particle size of 47 μm and a sphericity of 99%.
[0050] The above magnesium alloy powder was printed into molded magnesium alloy samples using the S-210 laser powder bed melting equipment produced by Xi'an Polylite Additive Technology Co., Ltd.
[0051] A porous model was created and sliced using dedicated slicing software. The resulting file was then imported into the 3D printer for printing. Argon was used as the shielding gas during printing, with a laser power of 100W, a scan speed of 1000mm / s, a preheat temperature of 200°C, and a powder layer thickness of 40μm. After printing, the sample was removed from the substrate, avoiding contact with water, grease, and other materials during removal.
[0052] Compressed air with a pressure of 3 bar was used to remove free powder particles on the surface of the formed magnesium alloy samples.
[0053] Compressed air with a pressure of 3 bar was used as a carrier gas to carry hydroxyapatite powder (particle size of 80 μm), and the outer surface of the formed magnesium alloy sample was sandblasted until the surface of the magnesium alloy appeared bright silver. Then the sample was taken out and placed in anhydrous ethanol for ultrasonication for 10 minutes. After ultrasonication, the magnesium alloy sample was taken out and placed in an air drying oven for drying (temperature 50°C).
[0054] The cleaned and dried magnesium alloy samples are placed in a tubular furnace (which has a heating tube, and the tail of the heating tube is connected to a sealed water tank, the sealed water tank is connected to a temperature sensor to measure the temperature inside the tank, and the sealed water tank is filled with deionized water) for heat treatment. Before starting the heating, oxygen-rich gas (oxygen purity greater than 99.99%) is introduced into the heating tube of the tubular furnace for 10 minutes, the heating tube is cleaned, and the heating tube is sealed and heated. The heating rate is 10°C / min, the temperature is raised to 525°C, and the temperature is kept warm for 8 hours. The heating process is carried out in an oxygen-rich environment with an oxygen pressure of 0.5 bar and an oxygen flow rate of 0.75L / min.
[0055] After heating, the magnesium alloy sample was not removed. The quartz tube was rotated so that the sample fell into a sealed water tank connected to the tail for cooling. The sealed water tank was filled with deionized water. The volume of the deionized water was 40 times the volume of the heated formed magnesium alloy sample. The temperature of the deionized water was 20°C. The oxygen flow rate during the water cooling process was 0.75L / min.
[0056] After 5 seconds, the magnesium alloy sample was taken out of the water and dried with compressed air.
[0057] Example 2
[0058] The only difference from Example 1 is that after the sandblasting treatment and before the heat treatment, the preparation method further includes the following steps: using an ion implanter with a double Penning type multi-charge heavy ion source to implant yttrium oxide as a sputtering material to deposit yttrium ions on the outer surface of the formed magnesium alloy sample; the implantation dose of the yttrium ions is 1×10 17 ions / cm 2 , the injection depth reaches 1μm.
[0059] Comparative Example 1:
[0060] The only difference from Example 1 is that the magnesium alloy powder includes 0.03 wt % manganese, 2.0 wt % neodymium, 3.7 wt % yttrium, 3.0 wt % scandium and the balance magnesium.
[0061] Comparative Example 2
[0062] The only difference from Example 1 is that the heat treatment is performed under atmospheric environment.
[0063] Performance characterization:
[0064] FIG1 shows a graph showing the film thickness measurement of the formed magnesium alloy sample in Example 1. It can be seen from FIG1 that the oxide film thickness is relatively stable and uniform, about 1 micron.
[0065] Figures 2, 3, and 4 show mechanical property test graphs of the formed magnesium alloy samples obtained in Example 1 and Comparative Example 1. Figure 2 shows the ultimate tensile strength test graph of the formed magnesium alloy samples obtained in Example 1 and Comparative Example 1; Figure 3 shows the compressive strength test graph of the formed magnesium alloy samples obtained in Example 1 and Comparative Example 1; and Figure 4 shows the elastic modulus test graph of the formed magnesium alloy samples obtained in Example 1 and Comparative Example 1. Figures 2, 3, and 4 show that the addition of zinc and limiting the zinc content to a range of 0.15-0.4 wt% have a significant impact on the mechanical properties of the product, with the compressive strength and ultimate tensile strength having a more pronounced impact.
[0066] Figure 5 shows the elemental analysis of the surface layer of the formed magnesium alloy sample obtained in Example 1. From Figure 5 , it can be seen that the yttrium and oxygen contents in the surface layer are significantly increased, achieving the effect of surface oxidation.
[0067] FIG6 shows the medical magnesium alloy sample obtained in Example 1 (sample size: 10×10 mm, height 20 mm, porosity 60%, average pore diameter 0.45 μm, surface area of about 3275 mm 2 As shown in Figure 6, the modified magnesium alloy gradually corroded in the simulated body fluid, with its weight reduced by only 50% after 10 days, significantly slowing down the degradation rate of the magnesium alloy in a physiological environment.
[0068] Figure 7 shows a scanning electron micrograph of the medical magnesium alloy sample obtained in Comparative Example 1. Figure 8 shows a scanning electron micrograph of the medical magnesium alloy sample obtained in Example 1. Figures 7 and 8 show that the film produced by heat treatment in an atmospheric environment is loose and not dense. Heat treatment in an oxygen-rich environment produces a dense film with uniform thickness.
[0069] Figure 9 shows a graph showing hydrogen evolution in a simulated body fluid (Hanks) for the medical magnesium alloy samples obtained in Example 1, Example 2, and Comparative Example 1. As can be seen from Figure 9 , the medical magnesium alloy sample of Example 2 exhibits superior corrosion resistance to that of the medical magnesium alloy sample of Example 1, and the medical magnesium alloy sample of Example 1 exhibits superior corrosion resistance to that of the medical magnesium alloy sample of Comparative Example 1.
[0070] The above are merely preferred embodiments of the present application and are not intended to limit the present application. Those skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present application shall be included within the scope of protection of the present application.
Claims
1. A method for preparing a medical magnesium alloy, characterized in that: include: Use laser fusion additive manufacturing technology to print magnesium alloy powder into molded magnesium alloy samples; Physically polishing the outer surface of the formed magnesium alloy sample; In an oxygen-rich environment, heat-treating the molded magnesium alloy sample after the physical polishing to obtain the medical magnesium alloy; Wherein, in terms of weight percentage, the magnesium alloy powder includes 0.15-0.4wt% zinc, 0.01-0.05wt% manganese, 0.5-2.2wt% neodymium, 3.7-4.3wt% yttrium and the balance magnesium.
2. The method for preparing a medical magnesium alloy according to claim 1, characterized in that: The magnesium alloy powder further includes 1.5 to 3.5 wt % of scandium; The magnesium alloy powder has a particle size of 20 to 80 μm, a D50 particle size of 45 to 50 μm, and a sphericity greater than 98%.
3. The method for preparing a medical magnesium alloy according to claim 2, characterized in that: The heat treatment comprises: firstly heating the molded magnesium alloy sample after the physical polishing treatment in an oxygen-rich environment at a temperature of 520-530° C. for 6-10 hours; then water cooling the heated molded magnesium alloy sample in an oxygen-rich environment at a temperature of 20-25° C. at a cooling rate of 100-200° C. / s to obtain the medical magnesium alloy; In the oxygen-rich environment, the volume content of oxygen is ≥90%.
4. The method for preparing a medical magnesium alloy according to claim 3, characterized in that: The oxygen pressure during the heating process is ≤1 bar; The oxygen flow rate during the heating process is 0.5-1 L / min.
5. The method for preparing a medical magnesium alloy according to claim 3, characterized in that: The water cooling treatment time is 3 to 5 seconds; During the water cooling process, the volume of water used is 30 to 50 times the volume of the heated formed magnesium alloy sample; The oxygen flow rate during the water cooling process is 0.5 to 1 L / min; After the water cooling, the preparation method further includes: taking the water-cooled material out of the water, first drying the water-cooled material with compressed air, then placing the water-cooled material in anhydrous ethanol for ultrasonic cleaning for 10 to 15 minutes, and then drying the water-cooled material to obtain the medical magnesium alloy.
6. The method for preparing a medical magnesium alloy according to any one of claims 1 to 5, characterized in that: The physical polishing is performed by sandblasting; Using compressed air with a pressure of 2 to 6 bar as a carrier gas to carry the hydroxyapatite powder to perform the sandblasting treatment; The particle size of the hydroxyapatite powder is less than 100 μm.
7. The method for preparing a medical magnesium alloy according to claim 1, characterized in that: The printing is performed in a laser powder bed fusion device; During the printing process, the power of the laser is 60-120 W, the scanning speed is 500-1200 mm / s, the powder thickness of each printing layer is 20-50 μm, and argon is used as the protective gas.
8. The method for preparing a medical magnesium alloy according to claim 1, characterized in that: Before the physical polishing treatment, the preparation method further comprises the step of removing free powder particles on the surface of the formed magnesium alloy sample by using compressed air.
9. The method for preparing a medical magnesium alloy according to claim 1, characterized in that: After the physical polishing and before the heat treatment, the preparation method further comprises: depositing yttrium ions on the outer surface of the molded magnesium alloy sample by ion implantation; The implantation dose of yttrium ions is 5×10 16 ~5×10 17 ions / cm 2 .
10. A medical magnesium alloy prepared by the method for preparing a medical magnesium alloy according to any one of claims 1 to 9.
Citation Information
Patent Citations
Medical magnesium alloys and their preparation methods
CN116356171B
High-ductility rare earth wrought magnesium alloy
CN104313438A
High-strength high-ductility Mg-Ga-Li-series magnesium alloy capable of quickly realizing ageing strengthening and preparation method thereof
CN110983135A
Medical magnesium alloy and preparation method thereof
CN116356171A
Magnesium material production method
JP2008291310A