Heating thin film, atomization core, and atomization device
By adopting an isometric crystal structure of the iron-based alloy film, the dry burning and wet burning performance problems of the heating film in the electronic atomization assembly are solved, which reduces costs and improves durability, and is suitable for electronic vaping atomization assembly.
Patent Information
- Application Number
- PCT/CN2024/089325
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-04-23
- Publication Date
- 2024-12-05
AI Technical Summary
The metal heating film in existing electronic atomization components is prone to dry-fired failure and electrochemical corrosion during the heating process, making it difficult to meet the performance requirements of dry-fired and wet-fired at the same time, and the cost is high, which limits the mass production and promotion of the heating body.
Using an iron-based alloy film, austenite crystal form with an isometric crystal structure and a face-centered cubic structure is prepared by physical vapor deposition and heat treatment to form a stainless steel film with a thickness of 0.5-3um, including Fe, Cr, Ni, Mo All components have high temperature oxidation resistance and electrochemical corrosion resistance.
It reduces the production cost of heating film, significantly improves the performance of dry and wet burns, extends service life, and reduces the resistance change rate, and is suitable for electronic cigarette atomization components.
Smart Images

Figure CN2024089325_05122024_PF_FP_ABST
Abstract
Description
Heating film, atomizing core and atomizing device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on May 31, 2023, with application number 202310636422.7 and invention name “A heating film, atomization core and atomization device”, the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The application involves a heating film, an electronic cigarette atomization component and an electronic cigarette, belonging to the field of electronic cigarette technology. Background Art
[0004] New electronic atomizer components often use thin-film heating films instead of traditional thick-film ones. The advantages of thin-film heating films include good material consistency, thin film thickness, and the fact that they don't fill the micropores on the heating surface of a porous substrate, thus not affecting the speed of e-liquid transfer and achieving higher atomization efficiency. Commonly used metal-based resistive heating films are primarily low-resistivity metal materials such as Ag, Cu, and Al.
[0005] Electronic atomization components face the following problems during use: On the one hand, if there is insufficient liquid supply during the heating and atomization process, the heating film will dry-burn and the temperature can even reach over 1000°C, which can easily lead to the failure of the heating film due to dry burning; on the other hand, atomization is achieved by heating the heating film with electricity (the potential difference is usually around 3-4V). At the same time, due to the wide variety of e-cigarette liquids, the ingredients in them also contain some corrosive media. Therefore, during the atomization process, the metal heating film is prone to electrochemical corrosion, which leads to corrosion failure of the heating film. Therefore, electronic atomization components have very strict requirements for metal heating films, which need to meet both dry-burning and wet-burning performance requirements. Commonly used metal heating films are difficult to meet the requirements.
[0006] Currently, the heating film system that fully meets the requirements is mainly based on the precious metal platinum, but the cost of this material is extremely high, and there is a great cost barrier to the subsequent mass production and promotion of heating elements. Therefore, it is urgent to develop a low-cost heating film based on base metal materials and meet the performance requirements of the heating film of the electronic atomization component to be resistant to dry burning and wet burning.
[0007] Summary of the Invention
[0008] The technical problem to be solved by this application is to provide a heating film based on an iron-based alloy, reduce the production cost of the heating film, and meet the performance requirements of the heating film of the electronic atomization component for both dry burning and wet burning. This application adopts the following technical solutions:
[0009] A heating film is an iron-based alloy film having an equiaxed crystal structure.
[0010] Optionally, the heating film has a thickness of 0.5-3 μm.
[0011] Optionally, the iron-based alloy film is a stainless steel film.
[0012] Optionally, the iron-based alloy film comprises the following components by mass fraction:
[0013] Fe: 61-72%, Cr: 16-20%, Ni: 10-15%, Mo: 2-4%;
[0014] Optionally, the iron-based alloy film comprises the following components by mass fraction:
[0015] Fe: 67~72%, Cr: 16-18%, Ni: 10-12%, Mo~2-3%;
[0016] Optionally, the iron-based alloy film comprises the following components by mass fraction:
[0017] Fe: 61~67%, Cr~18-20%, Ni~12-15%, Mo~3-4%;
[0018] Optionally, the iron-based alloy film contains other elements in an amount less than 1% by mass.
[0019] Optionally, the iron-based alloy film has an austenite crystal form with a face-centered cubic structure;
[0020] The iron-based alloy film is measured using CuKα radiation and θ-2θ scanning. In the X-ray diffraction pattern of the iron-based alloy film, the X-ray diffraction peak intensity ratio of the crystal (111) plane to the (200) plane is (1-3.5):1.
[0021] Optionally, the iron-based alloy film has no grain boundaries along the thickness direction.
[0022] This application also proposes a method for preparing the above-mentioned heating film, which includes the following steps:
[0023] Step 1) preparing an iron-based alloy film by physical vapor deposition;
[0024] Step 2) heat-treating the iron-based alloy film described in step 1) to form an equiaxed crystal structure, thereby obtaining the heating film.
[0025] Optionally, in step 1), the iron-based alloy film is prepared by physical vapor deposition co-sputtering of a single metal target or physical vapor deposition sputtering of an alloy target.
[0026] Optionally, the heat treatment method in step 2) is to heat the -2 Pa vacuum degree, keep warm at 600-800℃ for 30min, and cool after the insulation.
[0027] Optionally, after the insulation in step 2) is completed, the furnace is cooled.
[0028] Optionally, in step 2), in 3*10 -4 Pa~5*10 -2 Pa vacuum degree and keep warm at 700-800℃ for 30-120min.
[0029] The present application also proposes an electronic cigarette atomization core, which includes the above-mentioned heating film.
[0030] Optionally, the atomizer core includes a heating substrate, the heating substrate is provided with the heating film, and the heating film is provided with a protective film.
[0031] The present application also proposes an atomizing device, which includes the above-mentioned heating film and / or the above-mentioned atomizing core.
[0032] Compared with the existing technology, this application has the following technical effects:
[0033] The present application proposes a heating film, which is an iron-based alloy film, and the iron-based alloy film has an equiaxed crystal structure. Iron-based alloys such as stainless steel have certain corrosion resistance and oxidation resistance and can be used to make heating materials. However, since iron-based alloys such as stainless steel blocks usually have a columnar crystal structure when prepared into films, they grow along a specific crystal direction and have a large defect content. When used as a heating film for dry and wet burning tests, it is easy for oxidation or corrosion to occur along the columnar crystal boundaries, resulting in excessive increase in resistance and a short lifespan. The iron-based alloy heating film in the present application has an equiaxed crystal structure, the grain growth is isotropic, and the grains do not have obvious orientation, which overcomes the disadvantage of the short service life of the heating film with a columnar crystal structure, can meet the performance requirements of the heating film resistant to dry burning and wet burning during the use of the atomization core, and the cost is significantly reduced compared to the platinum heating film. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] FIG1 is a cross-sectional morphology diagram of the heating film of Example 1;
[0035] FIG2 is a cross-sectional morphology diagram of the heating film of Example 2;
[0036] FIG3 is a cross-sectional morphology of the heating film of Comparative Example 1;
[0037] FIG4 is a cross-sectional morphology of the heating film of Comparative Example 2;
[0038] FIG5 is an X-ray diffraction pattern of the heating film of each embodiment and comparative example. DETAILED DESCRIPTION
[0039] Iron-based alloys such as stainless steel have certain corrosion resistance and oxidation resistance and can be used to make heating materials. However, since stainless steel blocks usually have a columnar crystal structure when prepared into films, they grow along a specific crystal direction and have a large defect content. When used as heating films for dry and wet burning tests, they are prone to oxidation or corrosion along the columnar crystal boundaries, resulting in excessive increase in resistance and a short lifespan. The present application proposes a heating film, which is an iron-based alloy film, and the iron-based alloy film has an equiaxed crystal structure. In this equiaxed crystal structure film, the grains grow isotropically, and there is no obvious orientation of the grains, which overcomes the disadvantage of the low lifespan of the columnar crystal structure heating film. And compared with platinum heating films, the cost is significantly reduced. In a specific embodiment, the iron-based alloy film has an equiaxed crystal structure.
[0040] In an optional embodiment, the heating film has a thickness of 0.5-3 μm, for example, the film thickness is 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, or 5 μm.
[0041] In an optional embodiment, the iron-based alloy film is a stainless steel film. In an optional embodiment, the iron-based alloy film comprises the following components by mass: Fe: 61-72%, Cr: 16-20%, Ni: 10-15%, Mo: 2-4%. Alternatively, the iron-based alloy film comprises by mass: Fe: 67-72%, Cr: 16-18%, Ni: 10-12%, Mo ~2-3%. Alternatively, the iron-based alloy film comprises by mass: Fe: 61-67%, Cr ~18-20%, Ni ~12-15%, Mo ~3-4%.
[0042] In an optional embodiment, the iron-based alloy film has an austenite crystal form with a face-centered cubic structure; the iron-based alloy film is measured using CuKα radiation and θ-2θ scanning, and in the X-ray diffraction pattern exhibited by the iron-based alloy film, the X-ray diffraction peak intensity ratio of the crystal (111) plane to the (200) plane is (1-3.5):1. In an optional embodiment, the iron-based alloy film has no grain boundaries along the thickness direction. It has strong resistance to high-temperature oxidation and electrochemical corrosion.
[0043] This application also proposes a method for preparing the above-mentioned heating film, which includes the following steps:
[0044] Step 1) preparing an iron-based alloy film by physical vapor deposition;
[0045] Step 2) Heat-treating the iron-based alloy film described in step 1) to form an equiaxed crystal structure, thereby obtaining the heating film. This preparation method utilizes physical vapor deposition to prepare a film having a thickness of 0.5-3 μm, which is then heat-treated to obtain the heating film. The resulting heating film has a uniform and dense thickness, is highly resistant to high-temperature oxidation and electrochemical corrosion, and has a low manufacturing cost.
[0046] In an optional embodiment, in step 1), the iron-based alloy film is prepared by physical vapor deposition co-sputtering of a single metal target or physical vapor deposition sputtering of an alloy target.
[0047] In an optional embodiment, the heat treatment method in step 2) is to heat the -3 Pa vacuum, 700-800 ° C temperature for 30 minutes, and then cool after the end of the heat preservation. In an optional embodiment, the heat treatment is completed and cooled with the furnace. In an optional embodiment, the heat treatment is carried out at 3*10 -4 Pa~5*10 -2 Pa vacuum degree and keep warm at 700-800℃ for 30-120min.
[0048] The present application also proposes an electronic cigarette atomizer core, wherein the electronic cigarette atomizer component includes the above-mentioned heating film. In an optional embodiment, the atomizer core includes a heating substrate, the heating substrate is provided with the heating film, and the heating film is provided with a protective film.
[0049] The present application also proposes an atomization device, which includes at least one of the above-mentioned heating film and the above-mentioned electronic cigarette atomization core.
[0050] The atomizer core and atomizer device using the above-mentioned heating film can resist high-temperature oxidation to a certain extent in the dry-burning test of the heating film, and ensure that the resistance value increases by less than 20% in the 8.5W dry-burning test; in the wet-burning test of the heating film, it can also improve the film's resistance to electrochemical corrosion, ensuring that the resistance value remains stable under long-term power-on and smoke oil environment.
[0051] The following examples are provided only for the purpose of illustrating the present application in more detail. Therefore, according to the purpose of the present application, it will be apparent to those skilled in the art that the examples should not be construed as limiting the scope of the present application. The materials involved in the examples are all commercially available products.
[0052] The test method for resistance change in each embodiment and comparative example is as follows: Dry-burning test resistance change method: first test the initial resistance R0 of the heating film, the heating film is powered on for 3s and then off for 8s at a constant power of 7.5W, and dry-burned in the air for 10 cycles. The resistance R10 of the heating film after 10 cycles of dry-burning can be calculated. The resistance change rate ΔR before and after dry-burning can be calculated as (R10-R0) / R0, and the resistance change rate ΔR is required to be <20%.
[0053] Wet burning test resistance change method: load the heating element with e-liquid, test the initial resistance R0 after loading, select a 7.5W constant power battery, power on for 3s and then stop for 15s, test the resistance Rx of the heating film of the cartridge after 150 puffs, calculate the resistance change rate before and after wet burning ΔR = (Rx-R0) / R0, and the resistance change rate ΔR is required to be less than 20%.
[0054] The cross-sectional morphology of the heating film in each embodiment and comparative example was obtained by breaking the sample to obtain a natural cross-section, sputtering a conductive layer of Pt for 20 seconds, and observing with a FEI Apreo C Lovac field emission scanning electron microscope.
[0055] X-ray diffraction patterns in various embodiments and comparative examples: Phase analysis was performed using a Rigaku Miniflex X-ray diffractometer (XRD) with a scanning range of 30° to 90°.
[0056] The strawberry-watermelon ice fruit-flavored e-liquid in each embodiment is: strawberry-watermelon flavored e-liquid (40 mg) produced by Shenzhen Yupeng Technology Co., Ltd.
[0057] Example 1
[0058] Preparation of heating film:
[0059] Step 1) Using a magnetron sputtering device, an iron-based alloy film is prepared on a heating substrate by direct current (DC) sputtering of an alloy target. The iron-based alloy film comprises, by mass, 70% Fe, 16.5% Cr, 10.5% Ni, and 2.5% Mo. The alloy contains unavoidable impurities such as C, Si, and P, with the total impurity content being less than 1% by mass. The heating substrate has an array pore structure with a porosity of 20%.
[0060] Step 2) The iron-based alloy film prepared above is heat-treated at 800°C for 30 minutes under a vacuum degree of 3*10-3Pa, and then cooled in the furnace to obtain a heating substrate covered with a heating film.
[0061] A 100nm Al2O3 protective film is deposited on the surface of the heating film, and then assembled into a heating component. The effective heating area of the heating film is 3.5mm 2(This value does not take into account porosity.) The assembled electronic cigarette was further assembled into an electronic cigarette. The assembled electronic cigarette was subjected to dry burning and wet burning tests, and the test results were:
[0062] The dry-burning capacity of the heating film: 8.5W dry-burning 10 puffs has a resistance change of 18% (8.5W constant power on for 3s and rest for 8s in air dry-burning); the wet-burning capacity of the heating film: 7.5W puffing of strawberry watermelon ice fruit flavored e-liquid for 800 puffs has a resistance change of 14.5% (7.5W puffing for 3s and resting for 15s, capacity 55mL).
[0063] The cross-sectional morphology of the heating film is shown in Figure 1: the film thickness is 1600nm. The film is dense, with block-like equiaxed crystals, no obvious grain boundaries, and few defects. The film was subjected to XRD testing, and the X-ray diffraction pattern of the heating film was analyzed to be an austenite crystal with a face-centered cubic structure. As shown in Figure 5, the test results show that the film does not have an obvious grain growth orientation. Using CuKα radiation and θ-2θ scanning for measurement, in the X-ray diffraction pattern of the iron-based alloy film, the X-ray diffraction peak intensity ratio of the crystal (111) plane to the (200) plane is 1.87.
[0064] Example 2
[0065] Preparation of heating film:
[0066] Step 1) Using a magnetron sputtering device, an iron-based alloy film is prepared on a heating substrate by direct current (DC) sputtering of an alloy target. The iron-based alloy film comprises, by mass, 63.5% Fe, 19% Cr, 13.5% Ni, and 3.5% Mo. The alloy contains unavoidable impurities such as C, Si, and P, with the total impurity content being less than 1% by mass. The heating substrate has an array pore structure with a porosity of 20%.
[0067] Step 2) The iron-based alloy film prepared above is heat-treated at 800°C for 30 minutes under a vacuum of 3*10-3 Pa, and then cooled in the furnace to obtain a heating substrate covered with the heating film.
[0068] A 100nm Al2O3 protective film is deposited on the surface of the heating film, and then assembled into a heating component. The effective heating area of the heating film is 3.5mm 2 (This value does not take into account porosity.) The assembled electronic cigarette was further assembled into an electronic cigarette. The assembled electronic cigarette was subjected to dry burning and wet burning tests, and the test results were:
[0069] The dry-burning capacity of this heating element: 8.5W dry-burning 10 puffs resistance change = 18% (8.5W constant power on 3s and rest 8s dry-burning in air); wet-burning capacity: 7.5W strawberry watermelon ice fruit flavor e-liquid 800 puffs resistance change = 10% (7.5W puff 3s and rest 15s, capacity 55mL).
[0070] The cross-sectional morphology of the heating film is shown in Figure 2: the film thickness is 1700nm. The film is dense, with block-like equiaxed crystals, no obvious grain boundaries, and few defects. XRD testing of the film, as shown in Figure 5, shows that the X-ray diffraction pattern of the heating film is an austenitic crystal with a face-centered cubic structure and no obvious grain growth orientation. Using CuKα radiation and θ-2θ scanning for measurement, in the X-ray diffraction pattern of the iron-based alloy film, the X-ray diffraction peak intensity ratio of the crystal (111) plane to the (200) plane is 2.63.
[0071] Example 3
[0072] A heating film is prepared according to the method in Example 1, wherein the iron-based alloy film contains, by mass fraction, the following: Fe~61%, Cr~19.5%, Ni~15%, Mo~4%, and the rest are unavoidable impurities such as C, Si, P, and the total mass percentage of impurities is less than 1%. The other steps are the same as in Example 1. Dry burning and wet burning tests are carried out, and the test results are as follows: Dry burning capacity: 8.5W dry burning 10 puffs resistance change = 19% (8.5W constant power on 3s and stop 8s dry burning in air); Wet burning capacity: Strawberry Watermelon Ice Fruit Flavored E-liquid 7.5W puffs resistance change = 9% (7.5W puff 3s and stop 15s, capacity 55mL).
[0073] Example 4
[0074] A heating film is prepared according to the method in Example 1, wherein the iron-based alloy film contains, by mass fraction, the following: Fe~71%, Cr~16.5%, Ni~10%, Mo~2%, and the rest are inevitable impurities such as C, Si, P, and the total mass percentage of impurities is less than 1%. The other steps are the same as in Example 1. Dry burning and wet burning tests are carried out, and the test results are as follows: Dry burning capacity: 8.5W dry burning 10 puffs resistance change = 9% (8.5W constant power on for 3s and stop for 8s dry burning in air); Wet burning capacity: Strawberry Watermelon Ice Fruit Flavored E-liquid 7.5W puffs resistance change = 19% (7.5W puffs for 3s and stop for 15s, capacity 55mL).
[0075] Comparative Example 1
[0076] Preparation of heating film:
[0077] An iron-based alloy film is deposited on a heating substrate using a magnetron sputtering device using a DC sputtering method. The iron-based alloy film comprises, by mass, approximately 70% Fe, 16.5% Cr, 10.5% Ni, and 2.5% Mo. The alloy contains unavoidable impurities such as C, Si, and P, with the total impurity content being less than 1% by mass. The heating substrate has an array of pores with a porosity of approximately 20%.
[0078] A 100nm Al2O3 protective film is deposited on the surface of the heating film, and then assembled into a heating component. The effective heating area of the heating film is 3.5mm 2 (This value does not take into account porosity.) The assembled electronic cigarette was further assembled into an electronic cigarette. The assembled electronic cigarette was subjected to dry burning and wet burning tests, and the test results were:
[0079] The dry-burning capacity of the heating film: 7.5W dry-burning 10 puffs resistance change = 90%, 6.5W dry-burning 10 puffs resistance change = 19% (7.5w / 6.5W constant power power on 3s and rest 8s dry-burning in air); wet-burning capacity: 7.5W strawberry watermelon ice fruit flavored e-liquid 600 puffs resistance change = 15%, 800 puffs resistance change = 35% (7.5W puff 3s and rest 15s, capacity 55mL).
[0080] The cross-sectional morphology of the heating film is shown in Figure 3: the film thickness is 1700nm. The film is dense, with obvious columnar crystal features in some areas and obvious grain boundaries. The film was subjected to XRD testing, as shown in Figure 5. The X-ray diffraction pattern analysis of the heating film includes a face-centered cubic austenite crystal form and a body-centered cubic ferrite crystal form. The measurement was performed using CuKα radiation and θ-2θ scanning. In the X-ray diffraction pattern of the iron-based alloy film, the peak intensity ratio of the (111) plane to the (200) plane in the face-centered cubic austenite crystal form is 4.
[0081] Comparative Example 2
[0082] Preparation of heating film:
[0083] An iron-based alloy film is prepared on a heating substrate using a magnetron sputtering device using a DC sputtering method. The iron-based alloy film comprises, by mass, 63.5% Fe, 19% Cr, 13.5% Ni, and 3.5% Mo. The alloy contains unavoidable impurities such as C, Si, and P, with the total impurity content being less than 1% by mass. The heating substrate has an array of pores with a porosity of approximately 20%.
[0084] A 100nm Al2O3 protective film is deposited on the surface of the heating film, and then assembled into a heating component. The effective heating area of the heating film is 3.5mm 2 (This value does not take into account porosity.) The assembled electronic cigarette was further assembled into an electronic cigarette. The assembled electronic cigarette was subjected to dry burning and wet burning tests, and the test results were:
[0085] The dry-burning capacity of this heating element: 6.5W dry-burning 10 puffs resistance change = 83%, 5.5W dry-burning 10 puffs resistance change = 18% (6.5w / 5.5W constant power power on 3s and rest 8s dry-burning in air); wet-burning capacity: 7.5W strawberry watermelon ice fruit flavor e-liquid 300 puffs resistance change = 17%, 400 puffs resistance change = 38% (7.5W puff 3s and rest 15s, capacity 55mL).
[0086] The cross-sectional morphology of the heating film is shown in Figure 4. The film thickness is 1750nm. The cross-sectional morphology of the heating film shows obvious columnar crystal features, and the columnar crystal boundaries run through the height direction of the film layer. As shown in Figure 5, the X-ray diffraction pattern of the heating film shows a body-centered cubic ferrite crystal type, growing along the (110) crystal direction.
[0087] Comparative Example 3
[0088] A heating film was prepared according to the method in Example 1, wherein the material composition was consistent with that in Example 1, except that a heat treatment temperature of 500°C was selected and the temperature was kept for 60 minutes, and the other steps were the same as those in the example. Upon inspection, the cross section still had columnar crystal characteristics, and the columnar crystal boundaries ran through the height direction of the film layer. Dry burning and wet burning tests were carried out, and the test results were as follows: Dry burning capacity: 7.5W dry burning 10 puffs resistance change = 33% (7.5W constant power on for 3s and stop for 8s in the air); Wet burning capacity: Strawberry Watermelon Ice Fruit Flavored E-liquid 7.5W puffs resistance change = 23% (7.5W puffs for 3s and stop for 15s, capacity 55mL).
[0089] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will readily appreciate that other variations or modifications based on the above descriptions are possible. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications arising therefrom remain within the scope of protection of this application.
Claims
1. A heating film, characterized in that: The heating film is an iron-based alloy film, and the iron-based alloy film has an equiaxed crystal structure.
2. The heating film according to claim 1, characterized in that: The heating film has a thickness of 0.5-3um.
3. The heating film according to claim 1, characterized in that: The iron-based alloy film is a stainless steel film.
4. The heating film according to claim 1, characterized in that: The iron-based alloy film comprises the following components by mass fraction: Fe: 61-72%, Cr: 16-20%, Ni: 10-15%, Mo: 2-4%.
5. The heating film according to claim 4, characterized in that: The iron-based alloy film comprises the following components by mass fraction: Fe: 67-72%, Cr: 16-18%, Ni: 10-12%, Mo~2-3%.
6. The heating film according to claim 4, characterized in that: The iron-based alloy film comprises the following components by mass fraction: Fe: 61-67%, Cr-18-20%, Ni-12-15%, Mo-3-4%.
7. The heating film according to claim 1, characterized in that: The iron-based alloy film has an austenite crystal form with a face-centered cubic structure; The iron-based alloy film is measured by CuKα radiation and θ-2θ scanning. In the X-ray diffraction spectrum of the iron-based alloy film, the X-ray diffraction peak intensity ratio of the crystal (111) plane to the (200) plane is (1-3.5):
1.
8. The heating film according to claim 7, characterized in that: The iron-based alloy film has no grain boundaries along the thickness direction.
9. The method for preparing a heat-generating film according to any one of claims 1 to 8, characterized in that: The steps include: Step 1) preparing an iron-based alloy film by physical vapor deposition; Step 2) heat-treating the iron-based alloy film described in step 1) to form an equiaxed crystal structure, thereby obtaining the heat-generating film.
10. The method for preparing a heating film according to claim 9, characterized in that: In the step 1), the iron-based alloy film is prepared by physical vapor deposition co-sputtering of a single metal target or physical vapor deposition sputtering of an alloy target.
11. The method for preparing a heating film according to claim 9, characterized in that: The heat treatment method in step 2) is to heat the -2 The mixture is kept at a vacuum degree of 0.04 Pa and a temperature of 600-800°C for 30-120 min, and then cooled.
12. An atomizer core, characterized in that: The atomizer core includes the heating film according to any one of claims 1 to 8.
13. The atomizer core according to claim 12, characterized in that: The atomizing core comprises a heating substrate, the heating substrate is provided with the heating film, and the heating film is provided with a protective film.
14. An atomizing device, characterized in that: The atomizing device comprises the heating film according to any one of claims 1 to 8 and / or the atomizing core according to claim 12 or 13.
Citation Information
Patent Citations
Heating body, preparation method thereof and electronic smoking set
CN112167727A
Heating element and electronic atomization device
CN115363270A
Atomizing core preparation method
CN115836753A
Plane shape heat generator and manufacturing method thereof, plane shape heat generator panel using the same
CN1482836A
Galvanized pot