Atomization core, atomizer and electronic atomization device

By using a combination of porous glass ceramic matrix and metal heating film, the problem of insufficient strength of the electronic cigarette atomization core is solved, the service life is extended, the aroma reduction and taste consistency are improved, and the compressive strength and stability are achieved .

WO2024245033A1PCT designated stage expired Publication Date: 2024-12-05SMOORE INTERNATIONAL HOLDINGS LIMITED +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/094249
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-20
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The porous matrix of the existing electronic cigarette atomized core has poor strength and insufficient thermal shock resistance, resulting in short service life and inconsistent taste.

Method used

The porous glass ceramic matrix is ​​used as the porous matrix of the atomized core. By regulating its composition and porosity, combined with a metal heating film, the strength and stability of the atomized core are improved, and the porous structure is maintained to reduce the generation of smoke scale.

Benefits of technology

It effectively extends the service life of the atomized core, improves the reductivity and taste consistency of the fragrance, enhances the compressive strength, and avoids local breakage and damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024094249_05122024_PF_FP_ABST
    Figure CN2024094249_05122024_PF_FP_ABST
Patent Text Reader

Abstract

An atomization core, an atomizer and an electronic atomization device. The atomization core comprises a porous matrix and a heating body, wherein the porous matrix is a porous glass ceramic matrix, and comprises the following components in atomic percentages: 60-65 at% of oxygen, and 20-35 at% of silicon. By regulating and controlling the components and content of the porous glass ceramic matrix, the strength of the obtained porous matrix can be effectively improved, the stability of the matrix is better, and the service life thereof is effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Atomizing core, atomizer and electronic atomizing device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application filed with the Patent Office of China on June 1, 2023, with application number 202310645706.2 and invention name “A kind of atomizing core, atomizer and electronic atomizing device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the field of electronic atomization technology, and in particular to an atomization core, an atomizer, and an electronic atomization device. Background Art

[0004] As a good substitute for traditional cigarettes, the advantage of electronic cigarettes is that they reduce harmful substances such as tar and CO in the smoke. The atomization method of electronic cigarettes currently on the market is mainly resistive heating atomization, which atomizes the electronic cigarette oil through the heat generated by the atomizer core. The existing atomizer core usually includes a porous matrix and a heating element. The porous matrix usually adopts materials with a porous structure such as cotton core and porous ceramics to achieve the function of guiding the atomization medium to the heating element. However, in the existing technology, ceramic materials are usually prepared by diatomaceous earth, etc. The composition of traditional ceramic materials such as diatomaceous earth is complex, resulting in poor strength of the porous matrix of electronic cigarettes, which in turn makes its thermal shock resistance poor, and is prone to local detachment and breakage, affecting the taste and its service life.

[0005] Summary of the Invention

[0006] The purpose of this application is to overcome the defects of the prior art in that the porous matrix of the atomizer core has poor strength, which affects its taste and service life, and further provide an atomizer core, an atomizer and an electronic atomization device.

[0007] To achieve the above objectives, this application adopts the following technical solutions:

[0008] The present application provides an atomizer core, which includes a porous substrate and a heating element;

[0009] The porous matrix is ​​a porous glass ceramic matrix, and its components include, in atomic percentage, 60-65 at % of oxygen and 20-35 at % of silicon.

[0010] Optionally, the porous glass-ceramic matrix, in atomic percentage,

[0011] The composition also includes at least one of sodium 3-7.5 at %, magnesium 0.09-2 at %, aluminum 0.23-3 at %, and calcium 1-3.5 at %.

[0012] Optionally, the porosity of the porous glass-ceramic matrix is ​​50-90%.

[0013] Optionally, the porous glass-ceramic matrix includes a crystalline phase and an amorphous phase, and the crystallinity is 50-99%.

[0014] Optionally, the crystalline phase includes a quartz phase.

[0015] Optionally, the average pore size of the porous glass-ceramic matrix is ​​15-45 μm.

[0016] Optionally, the compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa.

[0017] Optionally, the compressive strength of the porous glass-ceramic matrix is ​​6-18 MPa.

[0018] Optionally, the heating element is a metal heating film;

[0019] Optionally, the metal heating film is selected from at least one of stainless steel and nickel-containing alloy.

[0020] The present application provides an atomizer, which includes the atomizer core described above.

[0021] The present application also provides an atomizing device, which includes the atomizing core described above.

[0022] Beneficial effects of this application:

[0023] The atomizer core provided herein comprises a porous substrate and a heating element. The porous substrate is a porous glass-ceramic substrate, and its composition, in atomic percentage, includes 60-65% oxygen and 20-35% silicon. By using a porous glass-ceramic substrate as the porous substrate for an electronic cigarette, and by regulating the composition and content of the porous glass-ceramic substrate, the ceramic substrate obtained can effectively improve the strength of the porous substrate and the atomizer core, thereby improving the stability of the substrate and the atomizer core and effectively extending their service life, while maintaining flavor consistency and enhancing aroma reproducibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the following is a brief introduction to the drawings required for use in the specific implementation methods or the description of the prior art. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0025] FIG1 is a SEM image of the porous substrate in Example 1 of the present application;

[0026] Figure 2 is a physical picture of the atomizer core heating element in Example 1 of the present application;

[0027] FIG3 is a graph showing the taste test results of the embodiment of the present application using atomized medium a;

[0028] FIG4 is a graph showing the taste test results of the embodiment of the present application using atomized medium b;

[0029] Figure 5 is a schematic diagram of the atomizer of the present application;

[0030] Figure 6 is a schematic diagram of the electronic atomization device of the present application;

[0031] Reference numerals: 1-atomizer, 2-battery assembly. DETAILED DESCRIPTION

[0032] The following examples are provided to further better understand the present application, but are not limited to the best implementation mode described herein, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the scope of protection of the present application.

[0033] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in this field can be used. If the manufacturer of the reagents or instruments is not specified, they are all commercially available conventional reagents.

[0034] In existing technology, ceramic materials such as diatomaceous earth are typically used. The complex composition of traditional ceramic materials like diatomaceous earth results in poor strength of the porous matrix of e-cigarettes, which in turn suffers from poor thermal shock resistance and is prone to localized detachment and breakage, shortening their service life. Furthermore, the complex composition of diatomaceous earth raw materials is often difficult to control, which can easily lead to inconsistent taste and reduced aroma in electronic atomization devices.

[0035] To this end, the present application provides an atomizer core comprising a porous substrate and a heating element. The porous substrate is a porous glass-ceramic substrate, whose composition, in atomic percentage, includes 60-65 at% oxygen and 20-35 at% silicon. The inventors have discovered that by using a porous glass-ceramic substrate as the porous substrate of an electronic cigarette and regulating the composition and content of the porous glass-ceramic substrate to obtain a ceramic substrate, the strength of the porous substrate and the atomizer core containing the ceramic substrate can be effectively improved, the substrate and the atomizer core having the ceramic substrate are more stable, and their service life is effectively extended, while maintaining taste consistency and improving aroma reproduction.

[0036] At the same time, the obtained porous matrix can still have good overall compressive strength under the condition of high porosity, and can be used in atomizer cores to increase service life; maintaining the porous structure inside the matrix can reduce the generation of soot and improve the taste.

[0037] Furthermore, the atomizer core of the present application is highly robust, preventing problems such as breakage and failure caused by insufficient strength during use. The porous matrix is ​​also more stable under the thermal shock of the atomization process, making it less susceptible to localized cracking and damage caused by compositional variations. Consequently, the atomizer core of the present application has a longer service life.

[0038] In an optional embodiment, the composition further includes at least one of 3-7.5 at % sodium, 0.09-2 at % magnesium, 0.23-3 at % aluminum, and 1-3.5 at % calcium, in atomic percentage.

[0039] In an optional embodiment, the porosity of the porous glass-ceramic matrix is ​​50-90%. For example, the porosity of the porous glass-ceramic matrix can be selected to be 50%, 51%, 52%, 53%, 54%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 77%, 79%, 80%, 82%, 83%, 84%, 85%, 86%, 88%, 89%, 90%.

[0040] In an optional embodiment, the porous glass-ceramic matrix includes a crystalline phase and an amorphous phase, and has a crystallinity of 50-99%. For example, the crystallinity of the porous glass-ceramic matrix can be 50%, 51%, 52%, 53%, 54%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 77%, 79%, 80%, 82%, 83%, 84%, 85%, 86%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, or 99%. Optionally, the raw glass bubbles can also have a certain degree of crystallinity, that is, the raw glass bubbles can be glass or glass ceramic. Furthermore, the crystalline phase includes a quartz phase. The melting point of the quartz phase is about 1700°C, which has a higher melting point. This temperature is much higher than the softening point of glass, so the basic form of the matrix can be further maintained from being destroyed during the molding process, avoiding problems such as collapse, further maintaining the porous structure inside the matrix, and improving the strength of the matrix. The composition ratio of the present application is easy to form a high-melting-point crystalline phase (such as a quartz phase). Since the temperature of the high-melting-point crystalline phase is much higher than the softening point of glass, the crystalline phase partially forms a skeleton structure, which keeps the macroscopic morphology of the matrix from changing significantly during the sintering molding process, avoiding problems such as collapse, and maintaining the porous structure inside the matrix.

[0041] In an optional embodiment, the average pore size of the porous glass-ceramic substrate is 15-45 μm. For example, the average pore size of the porous glass-ceramic substrate can be 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 26 μm, 27 μm, 28 μm, 29 μm, 30 μm, 31 μm, 32 μm, 33 μm, 34 μm, 35 μm, 36 μm, 37 μm, 38 μm, 39 μm, 40 μm, 41 μm, 42 μm, 43 μm, 44 μm, or 45 μm. The pore size range is moderate, achieving both liquid-guiding and liquid-locking effects. It should be noted that the pore size of the porous glass-ceramic matrix can also be controlled and adjusted by the selection of raw glass bubbles. By appropriate screening, raw glass bubbles of the required particle size can be obtained. Through suitable raw glass bubbles and preparation process, the pore structure of the porous glass-ceramic matrix can be controlled.

[0042] In an optional embodiment, the compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa; further optionally, the compressive strength of the porous glass-ceramic matrix is ​​6-18 MPa. For example, the compressive strength of the porous glass-ceramic matrix can be 6 MPa, 6.1 MPa, 6.3 MPa, 6.5 MPa, 6.6 MPa, 6.7 MPa, 6.8 MPa, 6.9 MPa, 7 MPa, 7.1 MPa, 7.3 MPa, 7.4 MPa, 7.5 MPa, 7.6 MPa, 7.8 MPa, 7.9 MPa, 8 MPa, 8.4 MPa, 8.8 MPa, 9 MPa, 9.2MPa, 9.7MPa, 10MPa, 10.5MPa, 10.9MPa, 11MPa, 11.6MPa, 11.9MPa, 12MPa, 12.5MPa, 12.8MP a. 13MPa, 13.5MPa, 14MPa, 14.5MPa, 15MPa, 15.5MPa, 16MPa, 16.5MPa, 17MPa, 17.5MPa, 18MPa.

[0043] The present application does not specifically limit the specific shape and material of the heating element. For example, the heating element can be selected from a metal heating film. Furthermore, the metal heating film is selected from at least one of stainless steel and nickel-containing alloy.

[0044] In some optional embodiments, the heating element is provided on at least one surface of the porous glass-ceramic substrate, and the preparation method includes at least one of printing, welding, evaporation, and deposition. For example, it is optional to print the heating element slurry on the substrate and sinter it at a preset temperature. Alternatively, the heating element or heating network is welded to the substrate. Alternatively, the heating element is evaporated / deposited on the substrate by physical vapor deposition (PVD) or chemical vapor deposition (CVD).

[0045] The preparation method of the atomizer core in this application can be a conventional method in the art, or a glass bubble sintering process can be used. The glass bubble is a hollow glass "microsphere" that can be obtained commercially. In the preparation process of this application, the raw glass bubble is sintered to form a glass ceramic bubble with a certain degree of crystallinity and an opening. Optionally, the glass bubble sintering process includes the following steps:

[0046] 1) mixing raw glass bubbles with a binder, a slip agent, and water and extruding the mixture to obtain a green body;

[0047] 2) sintering the green body in step 1) through a first sintering, a second sintering, and a third sintering to obtain a porous glass-ceramic matrix;

[0048] 3) Printing the heating element slurry on the porous glass ceramic substrate in step 2) and sintering it into shape.

[0049] In some optional embodiments, in step 1), the binder may be an organic binder; specifically, the binder is selected from at least one of methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose; the slip agent may be an aliphatic hydrocarbon slip agent, such as paraffin and metal stearate; specifically, the slip agent is sodium stearate.

[0050] In some optional embodiments, the extrusion molding pressure in step 1) is 1-40 bar. Most of the glass bubbles do not break during the extrusion molding process, maintaining the complete spherical shape of the individual glass bubbles. Therefore, the extrusion molding pressure can be appropriately adjusted based on the compressive strength of the selected glass bubbles.

[0051] In some optional embodiments, the first temperature of the first sintering in step 2) is at least 200° C., for example, 300° C. to 400° C., and / or the first dwell time is at least 1 minute, for example, 1 to 10 hours. During the sintering process at this temperature, substances such as solvents and binders in the green body are removed.

[0052] In some optional embodiments, the second sintering temperature is greater than 400°C and less than the softening point of the glass of the glass bubbles; for example, 500°C, 600°C, 700°C, etc., and the second dwell time is at least 1 minute, for example, 1 to 10 hours. The second temperature is greater than 400°C and less than the softening point of the glass of the glass bubbles. This is intended to maintain the original morphology of the green body. At the same time, because the temperature is already above 400°C, the glass components in the glass bubbles begin to undergo a phase transition. The disordered glass phase partially crystallizes into a crystalline phase within this temperature range, transforming the glass bubbles into glass-ceramic bubbles or increasing the proportion of the crystalline phase within the glass bubbles. Simultaneously, due to this transition, some glass bubbles begin to rupture, forming at least one opening. Therefore, the sintering time within this temperature range can be appropriately adjusted to adjust the crystallinity of the porous glass-ceramic. It is understood that the raw glass bubbles may also contain a certain proportion of crystalline phases, which can shorten the sintering time during this process.

[0053] In some optional embodiments, the third temperature of the third sintering is greater than the softening point of the glass. Specifically, the softening point temperature of the glass is less than 900°C. The third residence time can be at least 1 minute, for example, 1 to 10 hours. At this temperature, the glass component has fluidity, so the adjacent glass-ceramic bubbles are directly bonded to each other, and the glass-ceramic bubbles are bonded to form a porous glass-ceramic matrix with an integrated structure; at the same time, because the glass-ceramic bubbles still have crystalline phase components, the crystalline phase components serve as a skeleton so that their morphology does not collapse and still maintains a basically complete morphology. In addition, the glass-ceramic bubbles further crack to form a large number of openings, which are interconnected to form pores, and the pores extend through the porous glass-ceramic matrix and reach the surface of the porous glass-ceramic matrix.

[0054] The third temperature is higher than the softening point of the glass of the glass bubbles. The glass-ceramic bubbles are heated to at least the softening temperature of the amorphous glass, causing most of the glass-ceramic bubbles to open due to expansion of the gas within the bubbles. Simultaneously, the heating causes adjacent glass-ceramic bubbles to sinter together, forming a bond. Overall, the bonded open glass-ceramic bubbles form pores within a porous glass-ceramic matrix, effectively improving atomization efficiency and liquid conduction in atomizers and electronic atomization devices.

[0055] In some optional embodiments, the mass ratio of glass bubbles to binder, slip agent, and water is (70-110): (25-35): (2.5-3): (40-50).

[0056] In some optional embodiments, in step 3), the raw material of the heating element can be at least one of an electronic paste (metal paste), a heating wire, or a heating mesh. The electronic paste can be directly applied to the surface of the porous glass-ceramic substrate by screen printing according to a preset shape and sintered at a preset temperature. The sintering temperature can be adaptively adjusted according to the type of binder phase and metal component in the electronic paste, and the sintering temperature is usually 400-800°C.

[0057] In some optional embodiments, the glass component in the glass bubbles can be soda-lime silicate glass and / or borosilicate glass.

[0058] In some optional embodiments, step 1) further includes adding a pore-forming agent. Optionally, the pore-forming agent is selected from at least one of starch, polymethyl methacrylate (PMMA), polystyrene (PS), and graphite. Optionally, the particle size of the pore-forming agent can range from 1 to 150 μm. It is understood that the addition of the pore-forming agent can further increase the porosity of the porous glass-ceramic matrix while maintaining the strength of the raw glass bubble.

[0059] In some optional embodiments, step 1) further includes a second inorganic material. The second inorganic material can be at least one of clay, talc, silica, and alumina. The melting point or softening point of the above material is higher than the softening point of the glass in the glass bubble.

[0060] In some optional embodiments, the mass ratio of glass bubbles to binder, slip agent, water, pore former, and second inorganic material is (70-110): (25-35): (2.5-3): (40-50): (0-40): (0-4).

[0061] As shown in FIG5 , the present application further provides an atomizer including the aforementioned atomizer core. The atomizer includes a housing, within which a liquid storage tank and an atomization chamber are formed. The liquid storage tank is used to store liquid atomization medium, and the atomization chamber is used to accommodate the aforementioned atomization core. The atomization core can atomize the liquid atomization medium.

[0062] As shown in FIG6 , the present application further provides an electronic atomization device, comprising the aforementioned atomizer 1 and a battery assembly 2. The battery assembly and the atomizer may be integral or detachable. The battery assembly is used to power the atomizer in a preset mode, causing the atomizer to atomize a liquid atomizing medium in accordance with the preset mode.

[0063] The present application is further described in detail below with reference to specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in this application.

[0064] Example 1

[0065] This embodiment provides an atomizer core, which includes a porous substrate and a heating element. The porous substrate is a porous glass-ceramic substrate, and its components, in atomic percentage, include: 62.42 at % oxygen, 31.88 at % silicon, 3.05 at % sodium, 0.12 at % magnesium, 0.24 at % aluminum, and 2.29 at % calcium.

[0066] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0067] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, 2.06 g of clay, and 45.21 g of water, and extruded to form a green body at a molding pressure of 18 bar. The particle size parameters of the glass bubbles were: D10 of 17.16 μm, D50 of 37.74 μm, and D90 of 74.35 μm. The porosity of the glass bubble was 81.6%.

[0068] 2) Sintering the green body in step 1) to obtain a porous glass-ceramic substrate, wherein the first sintering temperature is 290° C., the first sintering time is 3.8 h, the second sintering temperature is 450° C., the second sintering time is 4 h, and the third sintering temperature is 1050° C., and the third sintering time is 4 h;

[0069] 3) Printing the stainless steel slurry on the porous glass ceramic substrate in step 2), sintering the substrate at a temperature of 800° C. for 3.5 hours to obtain the atomizing core.

[0070] Example 2

[0071] This embodiment provides an atomizer core, which includes a porous substrate and a heating element. The porous substrate is a porous glass-ceramic substrate, and its components, in atomic percentage, include: 60.82 at % oxygen, 32.73 at % silicon, 3.76 at % sodium, 0.13 at % magnesium, 0.33 at % aluminum, and 2.23 at % calcium.

[0072] The preparation method thereof comprises the following steps:

[0073] 1) 90 g of glass bubbles were mixed with 26 g of hydroxyethyl cellulose, 2.6 g of sodium stearate, 4 g of clay, 50 g of water, and 10 g of polymethyl methacrylate (PMMA) and extruded to form a green body at a molding pressure of 22 bar. The particle size parameters of the glass bubbles were: D10 of 17.16 μm, D50 of 37.74 μm, and D90 of 74.35 μm; and the porosity of the glass bubble alone was 81.6%.

[0074] 2) Sintering the green body in step 1) to obtain a porous glass-ceramic substrate, wherein the first sintering temperature is 260° C., the first sintering time is 1 hour, the second sintering temperature is 800° C., the second sintering time is 3 hours, and the third sintering temperature is 1100° C., and the third sintering time is 6 hours;

[0075] 3) Printing the stainless steel slurry on the porous glass ceramic substrate in step 2), sintering the substrate at a temperature of 800° C. and a sintering time of 1.5 h to obtain the atomizing core.

[0076] Example 3

[0077] This embodiment provides an atomizer core, which includes a porous substrate and a heating element. The porous substrate is a porous glass-ceramic substrate, and its components, in atomic percentage, include: 64.71 at % oxygen, 29.83 at % silicon, 1.56 at % sodium, 0.23 at % magnesium, 0.53 at % aluminum, and 3.24 at % calcium.

[0078] The preparation method thereof comprises the following steps:

[0079] 1) 80 g of glass bubbles were mixed with 26 g of hydroxyethyl cellulose, 2.6 g of sodium stearate, 4 g of clay, 50 g of water, and 25 g of polymethyl methacrylate (PMMA) and extruded to form a green body at a molding pressure of 25 bar. The particle size parameters of the glass bubbles were: D10 of 17.16 μm, D50 of 37.74 μm, and D90 of 74.35 μm. The porosity of the glass bubble was 81.6%.

[0080] 2) Sintering the green body in step 1) to obtain a porous glass-ceramic substrate, wherein the first sintering temperature is 260° C., the first sintering time is 1 hour, the second sintering temperature is 800° C., the second sintering time is 3 hours, and the third sintering temperature is 1080° C., and the third sintering time is 6 hours;

[0081] 3) Printing the stainless steel slurry on the porous glass ceramic substrate in step 2), sintering the substrate at a temperature of 800° C. and a sintering time of 1.5 h to obtain the atomizing core.

[0082] Comparative Example 1

[0083] This comparative example provides an atomizer core, which differs from Example 3 in that the porous matrix is ​​made of cotton core material.

[0084] Comparative Example 2

[0085] This comparative example provides an atomizer core, which differs from Example 1 in that the porous substrate is a porous ceramic substrate, the main component of which is diatomaceous earth.

[0086] Test Example 1

[0087] The porous ceramic matrix of the atomizer core of the embodiment of the present application is characterized by parameters such as porosity, compressive strength, and pore size.

[0088] The porosity and pore size were tested using a mercury intrusion method (using a mercury intrusion porosimeter). The compressive strength was tested using five parallel samples from the same embodiment, according to GB / T 4740-1999, Test Method for Compressive Strength of Ceramic Materials.

[0089] The atomizer cores of the examples were puffed for a preset number of puffs (the preset number of puffs in this application is 500). Failures were tested during this process and statistically recorded. Failure scenarios primarily include: 1. Significant changes in the atomizer core resistance (e.g., a significant increase in resistance due to a breakage or detachment of the heating element); 2. The atomizer output was less than half of the initial atomizer output. The atomizer cores in Examples 1-3 all met the preset service life of 500 puffs, with no failures observed.

[0090] The smoke production was also tested, including bare-die smoke production at a power of 7.5W and smoke production when assembled into an atomizer at a power of 6.5W. These tests were conducted using fruit (watermelon) flavored e-liquid (atomizing medium a).

[0091] The above test results are shown in Table 1.

[0092] Table 1 Test data of Examples 1-3

[0093] Test Example 2

[0094] The atomizer cores of the embodiment and comparative example were assembled into an atomizer, and five testers were asked to puff on each of the vapes and score them according to the preset dimensions. The scores were statistically averaged to obtain the puff taste score of the sample.

[0095] Taste tests were conducted using atomization medium a (fruit flavor) at an atomization power of 6.5W. Comparative Example 1 uses a cotton wick as the porous matrix. The results, as shown in Figure 3, show that Examples 1-3 outperform Comparative Example 1 in terms of vapor volume and aroma reproduction, but are slightly weaker in sweetness. All other dimensions are essentially equivalent to Comparative Example 1.

[0096] Taste tests were conducted using atomization medium b (tobacco flavor) at an atomization power of 6.5W. Comparative Example 2 employed an atomizer core with a porous ceramic matrix. As shown in Figure 4, Examples 1-3 outperformed Comparative Example 2 in terms of sweetness and aroma restoration, while remaining essentially equivalent to Comparative Example 2 in all other dimensions.

[0097] The inventors have analyzed and determined that the chemical composition of the porous glass-ceramic matrix in the embodiments of this application primarily includes silicon, oxygen, and other key components. These key components are chemically stable and are unlikely to dissolve in the atomizing medium or react with it to produce odorous substances. Other trace components, such as calcium, sodium, and magnesium, do not and are unlikely to dissolve in the atomizing medium or react with it to produce odorous substances. Therefore, the atomizing medium exhibits excellent aroma reduction and a pleasant taste in all formulations.

[0098] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will appreciate that other variations or modifications can be made based on the above description. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications derived therefrom remain within the scope of protection of this application.

Claims

1. An atomizer core, characterized in that: The atomizing core comprises a porous matrix and a heating element; The porous matrix is ​​a porous glass ceramic matrix, and its components include, in atomic percentage, 60-65 at % oxygen and 20-35 at % silicon.

2. The atomizer core according to claim 1, characterized in that: The porous glass ceramic matrix, in terms of atomic percentage, also includes at least one of 3-7.5 at% sodium, 0.09-2 at% magnesium, 0.23-3 at% aluminum, and 1-3.5 at% calcium.

3. The atomizer core according to claim 1 or 2, characterized in that: The porosity of the porous glass-ceramic matrix is ​​50-90%; Preferably, the porosity of the porous glass-ceramic matrix is ​​60-80%; Particularly preferably, the porosity of the porous glass-ceramic matrix is ​​62-77%.

4. The atomizer core according to any one of claims 1 to 3, characterized in that: The porous glass ceramic matrix comprises a crystalline phase and an amorphous phase, and the crystallinity is 50-99%.

5. The atomizer core according to claim 4, characterized in that: The crystalline phase includes a quartz phase.

6. The atomizer core according to any one of claims 1 to 5, characterized in that: The average pore size of the porous glass-ceramic matrix is ​​15-45 μm; Preferably, the average pore size of the porous glass-ceramic matrix is ​​20 to 35 μm; Particularly preferably, the average pore size of the porous glass-ceramic matrix is ​​20-22 μm.

7. The atomizer core according to any one of claims 1 to 6, characterized in that: The compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa.

8. The atomizer core according to any one of claims 1 to 7, characterized in that: The compressive strength of the porous glass-ceramic matrix is ​​6-18MPa.

9. The atomizer core according to any one of claims 1 to 8, characterized in that: The heating element is a metal heating film; Optionally, the metal heating film is selected from at least one of stainless steel and nickel-containing alloy.

10. An atomizer (1), characterized in that: The atomizer (1) comprises the atomizer core according to any one of claims 1 to 9.

11. An electronic atomization device, characterized in that: The electronic atomization device comprises the atomizer (1) according to claim 10.

Citation Information

Patent Citations

  • Electronic cigarette smoker and electronic cigarette

    CN110250590A

  • Porous ceramic material for atomizing core, porous ceramic body, ceramic atomizing core, preparation method and electronic cigarette

    CN114634372A

  • Heating assembly, atomizer and electronic atomization device

    CN114794574A

  • Atomization core, preparation method thereof and electronic atomization device

    CN115028366A

  • Atomizer and aerosol generating device

    CN215347023U