Adhesive sheet for manufacturing semiconductor package
The adhesive sheet addresses the stability and continuity issues in semiconductor manufacturing by using an acrylic resin-based adhesive with specific properties, ensuring stable seed layer formation and easy separation, thus enhancing the semiconductor package manufacturing process.
Patent Information
- Application Number
- PCT/JP2024/001643
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-01-22
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional adhesive sheets for semiconductor package manufacturing lack the necessary high-temperature stability and dimensional consistency to effectively support electronic components and seed layers during high-temperature processes, leading to issues with seed layer continuity and positional accuracy.
A pressure-sensitive adhesive sheet with a resin layer made of acrylic resin, having a surface roughness of 600 nm or less, a linear expansion coefficient of -50×10^-5 /K to 50×10^-5 /K at 230°C to 240°C, and an elastic modulus of 10 MPa or more after UV irradiation, which includes a base material and optionally a gas generation layer, ensuring stability and releasability.
The adhesive sheet provides a stable and smooth surface for seed layer formation, maintains positional accuracy, and allows for easy separation from the substrate, preventing cracks and delamination during high-temperature processes.
Smart Images

Figure JP2024001643_05122024_PF_FP_ABST
Abstract
Description
Adhesive sheets for semiconductor package manufacturing
[0001] The present invention relates to an adhesive sheet for manufacturing semiconductor packages.
[0002] In recent years, in order to improve the characteristics of semiconductor devices, there has been an accelerating trend, particularly in areas such as semiconductor packaging, to perform high-temperature processes by fixing semiconductor chips and encapsulated resin substrates to a rigid support substrate. Typical examples include processes in which multiple electronic components are arranged at predetermined intervals on an adhesive sheet and then encapsulated with resin, processes in which a rewiring layer is formed, and processes in which copper pillar structures are formed to create three-dimensional semiconductor packages. Adhesive sheets used in such heat-resistant processes require flatness to hold the arranged electronic components on a smooth surface and dimensional stability to maintain the relative positions of the electronic components. Furthermore, when forming wiring or pillar structures in copper plating processes, a thin metal film (seed layer) having a thickness on the order of several nanometers may be formed on the adhesive sheet by sputtering, vacuum deposition, or the like, and an adhesive sheet capable of forming the thin metal film well is required.
[0003] Patent No. 5588950
[0004] The present invention has been made to solve the above-mentioned conventional problems, and an object of the present invention is to provide a pressure-sensitive adhesive sheet for use in semiconductor package production that is suitable for use at high temperatures.
[0005] [1] The adhesive sheet for semiconductor package production according to an embodiment of the present invention is an adhesive sheet for semiconductor package production that is disposed on a substrate and used, and includes a resin layer made of an acrylic resin, and at least one surface of the resin layer has a surface roughness Ra of 600 nm or less. [2] The adhesive sheet for semiconductor package production according to [1] above has a linear expansion coefficient of -50 × 10 at 230 °C to 240 °C. -5 / K~50×10 -5 / K. [3] In the pressure-sensitive adhesive sheet for producing a semiconductor package according to [1] or [2] above, the resin layer may be formed from an active energy ray-curable resin composition containing an acrylic polymer, a pentaerythritol-based polyfunctional acrylate, and a photopolymerization initiator. [4] In the pressure-sensitive adhesive sheet for producing a semiconductor package according to any of [1] to [3] above, the resin layer may have a nanoindenter elastic modulus of 10 MPa or more after ultraviolet irradiation at 25°C. [5] In the pressure-sensitive adhesive sheet for producing a semiconductor package according to any of [1] to [4] above, the thickness of the resin layer after dropping a polar solvent onto the resin layer and leaving it at 25°C for 15 minutes may be 130% or less of the thickness before the dropping. [6] The pressure-sensitive adhesive sheet for producing a semiconductor package according to any of [1] to [5] above may further include a substrate, the resin layer being disposed on one side of the substrate, and the substrate being made of a polyimide-based resin, a polyester-based resin, or a polyether ether ketone-based resin. [7] In the pressure-sensitive adhesive sheet for producing a semiconductor package according to any one of [1] to [6] above, the resin layer of the pressure-sensitive adhesive sheet may be attached to a polyimide plate, and the adhesive strength after standing at 230°C for 2 hours may be 5 N / 20 mm or less. [8] The pressure-sensitive adhesive sheet for producing a semiconductor package according to any one of [1] to [7] above may further comprise a gas-generating layer, the resin layer, the base material, and the gas-generating layer being arranged in this order. [9] A method for using the pressure-sensitive adhesive sheet for producing a semiconductor package according to an embodiment of the present invention includes placing the pressure-sensitive adhesive sheet for producing a semiconductor package according to any one of [1] to [8] above on a support substrate, forming wiring on the resin layer of the pressure-sensitive adhesive sheet for producing a semiconductor package, and then applying an external stimulus to the pressure-sensitive adhesive sheet for producing a semiconductor package to separate the pressure-sensitive adhesive sheet for producing a semiconductor package from the support substrate.
[10] A method of using an adhesive sheet for semiconductor package manufacturing according to an embodiment of the present invention includes placing the adhesive sheet for semiconductor package manufacturing described in any one of [1] to [8] above on a support substrate, forming copper pillars on the resin layer of the adhesive sheet for semiconductor package manufacturing, and then applying an external stimulus to the adhesive sheet for semiconductor package manufacturing to separate the adhesive sheet for semiconductor package manufacturing from the support substrate.
[0006] According to the present invention, it is possible to provide a pressure-sensitive adhesive sheet for use in manufacturing semiconductor packages that is suitable for use at high temperatures.
[0007] 1( a ) to 1 ( d ) are schematic cross-sectional views of an adhesive sheet for producing a semiconductor package according to one embodiment of the present invention.
[0008] A. Overview of the Pressure-Sensitive Adhesive Sheet for Semiconductor Package Production FIG. 1 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet for semiconductor package production according to one embodiment of the present invention. The pressure-sensitive adhesive sheet 100 for semiconductor package production includes a resin layer 10. The resin layer is made of an acrylic resin. The pressure-sensitive adhesive sheet 100 for semiconductor package production may be made of only the resin layer 10 as shown in FIG. 1( a), or may include the resin layer 10 and other layers. For example, the pressure-sensitive adhesive sheet 100 for semiconductor package production may further include a substrate 20 as shown in FIGS. 1( b), 1( c), and 1( d). In this case, the pressure-sensitive adhesive sheet 100 for semiconductor package production may include the substrate 20 and a resin layer 10 disposed on at least one surface of the substrate 20. Furthermore, as shown in FIGS. 1( c) and 1( d), the pressure-sensitive adhesive sheet 100 for semiconductor package production may include a pressure-sensitive adhesive layer 30 or a gas-generating layer 40. In one embodiment, a pressure-sensitive adhesive sheet 100 for semiconductor package production is provided that includes the resin layer 10, the substrate 20, and the pressure-sensitive adhesive layer 30 in this order. In one embodiment, there is provided a pressure-sensitive adhesive sheet 100 for producing a semiconductor package, which comprises, in this order, a resin layer 10, a substrate 20, and a gas generation layer 40. In the embodiments shown in Figures 1(c) and 1(d), the substrate 20 may be omitted. In the following description, the "pressure-sensitive adhesive sheet for producing a semiconductor package" may also be simply referred to as the "pressure-sensitive adhesive sheet."
[0009] In one embodiment, the pressure-sensitive adhesive sheet for semiconductor package production is used by being placed on a substrate. The substrate may be a support substrate during semiconductor package production. The pressure-sensitive adhesive sheet for semiconductor package production may be used by temporarily fixing the sheet on the substrate and then carrying out the semiconductor package production process on the resin layer. In one embodiment, a semiconductor chip is placed on the resin layer, and then resin sealing of the semiconductor chip, rewiring process, etc. are carried out. In another embodiment, a seed layer for plating is directly formed on the surface of the resin layer to provide wiring or pillars.
[0010] In one embodiment, the pressure-sensitive adhesive sheet is configured to be removably removable. For example, as shown in Figures 1(c) and 1(d), a pressure-sensitive adhesive layer 30 or a gas-generating layer 40 is provided, and removability is imparted to the layer. The removably removable pressure-sensitive adhesive sheet can be used as a temporary fixing material on a substrate (e.g., a support substrate) in a predetermined step during semiconductor package manufacturing. After the predetermined step, the removability of the pressure-sensitive adhesive sheet functions favorably when separating the semiconductor package product or intermediate semiconductor package product from the substrate.
[0011] The surface roughness Ra of one side of the resin layer is 600 nm or less. The resin layer surface having a surface roughness Ra of 600 nm or less can be the surface of the resin layer opposite the substrate. In an embodiment of the present invention, by having a surface with a low surface roughness Ra as described above, a pressure-sensitive adhesive sheet can be provided on which a seed layer for plating can be preferably formed. On such a pressure-sensitive adhesive sheet, the seed layer can be formed as a high-quality continuous film. The use of the pressure-sensitive adhesive sheet is particularly effective in that continuity can be maintained even when the seed layer is formed as a thin film. Forming the seed layer as a thin film reduces the difference in dimensional change between the seed layer and the resin layer even at high temperatures, thereby preventing cracks from occurring in the seed layer. The surface roughness Ra of one side of the resin layer is preferably 400 nm or less, more preferably 300 nm or less, even more preferably 200 nm or less, and particularly preferably 100 nm or less. The lower limit of the surface roughness Ra of one side of the resin layer is, for example, 50 nm (preferably 20 nm).
[0012] In one embodiment, the adhesive strength at 23°C when the resin layer of the pressure-sensitive adhesive sheet is attached to a stainless steel plate (SUS304) is preferably 0.1 N / 20 mm to 10 N / 20 mm, more preferably 0.15 N / 20 mm to 8 N / 20 mm. Within these ranges, a pressure-sensitive adhesive sheet capable of favorably holding electronic components can be obtained. The adhesive strength is measured in accordance with JIS Z 0237:2000. Specifically, the pressure-sensitive adhesive sheet is attached to an adherend (e.g., a stainless steel plate (arithmetic mean surface roughness Ra: 50±25 nm), a polyimide film) using a 2 kg roller in one reciprocating motion, and then left at 23°C for 30 minutes. After this, the pressure-sensitive adhesive sheet is peeled off at a peel angle of 180° and a pulling speed of 300 mm / min to measure the adhesive strength.
[0013] In another embodiment, the adhesive strength at 23°C when the resin layer of the pressure-sensitive adhesive sheet is attached to a stainless steel plate (SUS304) is preferably 0 N / 20 mm to 1.0 N / 20 mm, more preferably 0.01 N / 20 mm to 0.5 N / 20 mm.
[0014] The adhesive strength a after the resin layer of the pressure-sensitive adhesive sheet is attached to a polyimide film and left at 200°C for 2 hours is preferably 5 N / 20 mm or less, more preferably 2 N / 20 mm or less, and even more preferably 1 N / 20 mm or less. Within this range, when the adherend is separated after the heating step, the resin layer adhering to the adherend as a residue can be easily peeled off and removed. Such a resin layer can be a resin layer that is difficult to decompose at high temperatures, and can be formed, for example, by using an active energy ray-curable resin composition containing a photoreactive monomer or oligomer as described below, or by using an epoxy-based crosslinking agent as a crosslinking agent. The lower limit of the adhesive strength a is, for example, 0.005 N / 20 mm.
[0015] The adhesive strength b after adhering the resin layer of the pressure-sensitive adhesive sheet to a polyimide plate and heating at 230°C for 2 hours is preferably 5 N / 20 mm or less, more preferably 2 N / 20 mm or less, and even more preferably 1 N / 20 mm or less. Within this range, when the adherend is separated after the heating step, the resin layer adhering to the adherend as a residue can be easily peeled off and removed. Such a resin layer can be a resin layer that is difficult to decompose at high temperatures, and can be formed, for example, by using an active energy ray-curable resin composition containing a photoreactive monomer or oligomer, as described below, or by using an epoxy-based crosslinking agent as a crosslinking agent. The lower limit of the adhesive strength b is, for example, 0.01 N / 20 mm.
[0016] The pressure-sensitive adhesive sheet preferably has a linear expansion coefficient of −500×10 at 230° C. to 240° C. -5 / K~100×10 -5 / K, more preferably −50×10 -5 / K~50×10 -5 / K, and more preferably −30×10 -5 / K~30×10 -5 / K, and particularly preferably −15×10 -5 / K~15 x 10 -5 / K. If the temperature is in this range, it is possible to provide an adhesive sheet that allows for the stable formation of a thin seed layer. Furthermore, when a semiconductor chip is placed on the adhesive sheet, it is possible to place it with good positional accuracy. In particular, the linear expansion coefficient at 230°C to 240°C is -50 × 10 -5 / K~50×10 -5 The linear expansion coefficient can be determined by TMA measurement in accordance with JIS K 7197.
[0017] In one embodiment, the pressure-sensitive adhesive sheet has a linear expansion coefficient of 20×10 at 230° C. to 240° C. -5 / K~50×10 -5 / K is said to be.
[0018] The pressure-sensitive adhesive sheet preferably has a linear expansion coefficient of −100×10 at 200° C. to 210° C. -5 / K~100×10 -5 / K, more preferably −50×10 -5 / K~50×10 -5 / K, more preferably −30×10 -5 / K~30×10 -5 / K, and more preferably −15×10 -5 / K~15 x 10 -5 / K. If the temperature is in this range, it is possible to provide an adhesive sheet that allows for the stable formation of a thin seed layer. Furthermore, when a semiconductor chip is placed on the adhesive sheet, it is possible to place it with good positional accuracy. In particular, the linear expansion coefficient at 200°C to 210°C is -50 × 10 -5 / K~50×10 -5 If the ratio is 1 / K, the above effect becomes significant.
[0019] The thickness of the pressure-sensitive adhesive sheet is preferably 1 μm to 300 μm, and more preferably 3 μm to 200 μm.
[0020] B. Resin Layer The nanoindenter elastic modulus of the resin layer after ultraviolet irradiation at 25°C is preferably 10 MPa or more, more preferably 100 MPa or more, even more preferably 1000 MPa or more, and even more preferably 5000 MPa or more. Within this range, a resin layer that is less likely to swell in polar solvents can be formed, and the effects of the present invention are remarkable. The upper limit of the nanoindenter elastic modulus of the resin layer after ultraviolet irradiation at 25°C is, for example, 20,000 MPa. A method for measuring the nanoindenter elastic modulus after ultraviolet irradiation will be described later.
[0021] The tensile modulus of the resin layer at 25 ° C is preferably 10 MPa or more, more preferably 100 MPa or more, even more preferably 300 MPa or more, and particularly preferably 600 MPa or more. Within this range, a resin layer that is less likely to swell in polar solvents can be formed. If such a resin layer is present, delamination of the adhesive sheet caused by swelling of the resin layer can be prevented when subjected to a resist process for wiring formation. The upper limit of the tensile modulus of the resin layer at 25 ° C is, for example, 2 GPa. The method for measuring tensile elasticity will be described later.
[0022] The tensile modulus of the resin layer at 200°C is preferably 3 MPa or more, more preferably 10 MPa or more, even more preferably 100 MPa or more, and particularly preferably 500 MPa or more. Within this range, a resin layer with small dimensional change can be formed. This is particularly advantageous in that a resin layer that is resistant to dimensional change even at high temperatures can be formed. Having such a resin layer can prevent cracking of a seed layer for plating when the seed layer is formed. This effect is significant, combined with the ability to form a thin-film seed layer, as described above. The upper limit of the tensile modulus of the resin layer at 200°C is, for example, 2 GPa. The method for measuring tensile modulus will be described later.
[0023] The tensile modulus of the resin layer at 230°C is preferably 3 MPa or more, more preferably 10 MPa or more, even more preferably 100 MPa or more, and particularly preferably 500 MPa or more. Within this range, a resin layer with small dimensional change can be formed. This is particularly advantageous in that a resin layer that is resistant to dimensional change even at high temperatures can be formed. Having such a resin layer can prevent cracking of a seed layer for plating when the seed layer is formed. This effect is significant, coupled with the ability to form a thin-film seed layer, as described above. The upper limit of the tensile modulus of the resin layer at 230°C is, for example, 2 GPa.
[0024] The linear expansion coefficient of the resin layer at 230°C to 240°C is preferably -50 x 10 -5 / K~50×10 -5 / K, more preferably −30×10 -5 / K~30×10 -5 / K, and more preferably −15×10 -5 / K~15 x 10 -5 / K.
[0025] In one embodiment, the linear expansion coefficient of the resin layer at 230°C to 240°C is 20 x 10 -5 / K~50×10 -5 Within this range, a resin layer having favorable adhesive properties is formed, and a pressure-sensitive adhesive sheet suitable for applications such as arranging a chip on the resin layer can be obtained.
[0026] The linear expansion coefficient of the resin layer at 200°C to 210°C is preferably 10 x 10 -5 / K~150 x 10 -5 / K, more preferably 15×10 -5 / K~100×10 -5 / K, and more preferably 20×10 -5 / K~50×10 -5 / K.
[0027] The thickness of the resin layer is preferably 1 μm to 50 μm, more preferably 2 μm to 25 μm, and even more preferably 3 μm to 20 μm.
[0028] When a polar solvent is dropped onto the resin layer and allowed to stand at 25°C for 15 minutes, the thickness of the resin layer is preferably 130% or less, more preferably 120% or less, and even more preferably 110% or less, of the thickness before the drop. Within this range, a pressure-sensitive adhesive sheet with excellent chemical resistance can be obtained. For example, when used in a resist process, a pressure-sensitive adhesive sheet with excellent durability against resist removal solutions can be obtained. In one embodiment, a pressure-sensitive adhesive sheet with excellent chemical resistance as described above can be obtained by forming a resin layer so as to have a high elastic modulus. Furthermore, the thickness of the resin layer after the polar solvent is dropped onto the resin layer is preferably 100% or more of the thickness before the drop. The polar solvent is, for example, N-methyl-2-pyrrolidone. It may also be propylene glycol monomethyl ether acetate or dimethyl sulfoxide. A resin layer with a small change in thickness as described above is a resin layer that is less likely to swell due to a polar solvent. For example, by configuring the elastic modulus or linear expansion coefficient to be within the above range, a resin layer that is less likely to swell can be obtained.
[0029] (Active Energy Ray-Curable Resin Composition) In one embodiment, the resin layer is formed from an active energy ray-curable resin composition.
[0030] The active energy ray-curable resin composition contains an acrylic polymer as a base polymer. The term "base polymer" refers to the main component of the polymer contained in the active energy ray-curable resin composition. In this specification, the term "main component" refers to a component that accounts for more than 50% by weight, unless otherwise specified.
[0031] The acrylic polymer is preferably, for example, a polymer of a monomer raw material containing an alkyl(meth)acrylate as a main monomer and a secondary monomer copolymerizable with the main monomer. Here, the main monomer refers to a component that accounts for more than 50% by weight of the monomer composition in the monomer raw material. The content of the main monomer is preferably 60 to 100 parts by weight, more preferably 70 to 99.5 parts by weight, per 100 parts by weight of the total amount of monomers in the monomer raw material.
[0032] As the alkyl(meth)acrylate, for example, a compound represented by the following formula (1) can be suitably used: CH 2 = C(R 1 ) COOR 2 (1) Here, R in the above formula (1) 1 is a hydrogen atom or a methyl group. 2 is a branched or linear alkyl group having 1 to 20 carbon atoms (hereinafter, this range of carbon atoms may be referred to as "C1-20"). 2 is preferably a branched or straight-chain C1-14 alkyl group, more preferably a branched or straight-chain C6-14 alkyl group, and even more preferably a branched or straight-chain C8-12 alkyl group.
[0033] Specific examples of the alkyl(meth)acrylate include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, n-butyl(meth)acrylate, isobutyl(meth)acrylate, s-butyl(meth)acrylate, pentyl(meth)acrylate, isopentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, and isooctyl(meth)acrylate. ) acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and the like. These alkyl (meth)acrylates can be used alone or in combination of two or more. Among them, 2-ethylhexyl acrylate (2EHA) and lauryl (meth)acrylate (LA, LMA) are particularly preferred.
[0034] The secondary monomer copolymerizable with the alkyl(meth)acrylate main monomer can be useful for introducing crosslinking points into the acrylic polymer and for increasing the cohesive strength of the acrylic polymer. As the secondary monomer, for example, the following functional group-containing monomer components can be used alone or in combination of two or more: Carboxy group-containing monomers: for example, ethylenically unsaturated monocarboxylic acids such as acrylic acid (AA), methacrylic acid (MAA), crotonic acid, etc.; ethylenically unsaturated dicarboxylic acids such as maleic acid, itaconic acid, citraconic acid, etc., and anhydrides thereof (maleic anhydride, itaconic anhydride, etc.); hydroxyl group-containing monomers: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, etc.; unsaturated alcohols such as vinyl alcohol, allyl alcohol, etc.; ether compounds such as 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, etc.; amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate; epoxy group-containing monomers: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, allyl glycidyl ether; Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile; keto group-containing monomers: for example, diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, vinyl acetoacetate; monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, N-(meth)acryloylmorpholine;Alkoxysilyl group-containing monomers: for example, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane; Isocyanate group-containing monomers: (meth)acryloyl isocyanate, 2-(meth)acryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate;
[0035] The content of the structural unit derived from the secondary monomer is preferably 1 to 20 parts by weight, and more preferably 2 to 15 parts by weight, relative to 100 parts by weight of the base polymer. Within this range, a favorably crosslinked resin layer can be obtained, and the effects of the present invention become more pronounced.
[0036] Copolymerization components other than the above-mentioned secondary monomers can also be used. Examples of such copolymerization components include vinyl ester-based monomers such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene, substituted styrenes (such as α-methylstyrene) and vinyltoluene; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, cyclopentyl di(meth)acrylate and isobornyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as aryl (meth)acrylates (such as phenyl (meth)acrylate), aryloxyalkyl (meth)acrylates (such as phenoxyethyl (meth)acrylate) and arylalkyl (meth)acrylates (such as benzyl (meth)acrylate); olefin-based monomers such as ethylene, propylene, isoprene, butadiene and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; vinyl ether-based monomers such as methyl vinyl ether and ethyl vinyl ether; and the like. The copolymerization components other than these secondary monomers may be used alone or in combination of two or more thereof. The amount of such copolymerization components is, for example, 0.5 to 20 parts by weight per 100 parts by weight of the total amount of monomers in the monomer raw material.
[0037] The weight average molecular weight Mw of the acrylic polymer is preferably 10×10 4 ~500 x 10 4 and more preferably 20×10 4 ~200 x 10 4 and more preferably 30×10 4 ~100 x 10 4 Within this range, a resin layer with little adhesive residue and excellent adhesion can be formed. In this specification, Mw refers to a value calculated in terms of standard polystyrene obtained by GPC.
[0038] The acrylic polymer can be obtained by any suitable polymerization method, such as solution polymerization, emulsion polymerization, bulk polymerization, or suspension polymerization.
[0039] The active energy ray-curable resin composition may further contain a photoreactive monomer or oligomer having multiple functional groups with carbon-carbon multiple bonds. Addition of the photoreactive monomer or oligomer can produce a resin layer with excellent properties at high temperatures, for example, a resin layer with a high elastic modulus and low dimensional change rate at 200°C to 240°C. Examples of functional groups with carbon-carbon multiple bonds include acryloyl groups, methacryloyl groups, vinyl groups, allyl groups, and acetylene groups. Among these, compounds with ethylenically unsaturated functional groups are preferred, and (meth)acrylic compounds with ethylenically unsaturated functional groups are more preferred. Compounds with ethylenically unsaturated functional groups readily generate radicals when exposed to ultraviolet light, and the use of such compounds allows for the formation of a resin layer that can be cured in a short time. Furthermore, the use of (meth)acrylic compounds with ethylenically unsaturated functional groups allows for the formation of a resin layer with appropriate hardness after curing. Specific examples of photoreactive monomers or oligomers include (meth)acryloyl group-containing compounds such as trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and urethane (meth)acrylate compounds; dimers to pentamers of the (meth)acryloyl group-containing compounds; and the like. These compounds may be used alone or in combination of two or more.
[0040] In one embodiment, a pentaerythritol-based polyfunctional acrylate is used as the photoreactive monomer or oligomer. The use of a pentaerythritol-based polyfunctional acrylate allows for the formation of a resin layer that has excellent dimensional stability even at high temperatures and is suitable for forming a seed layer. Examples of pentaerythritol-based polyfunctional acrylates include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0041] The content of the photoreactive monomer or oligomer is preferably 20 parts by weight or more, more preferably 50 parts by weight or more, even more preferably 100 parts by weight or more, and particularly preferably 200 parts by weight or more, per 100 parts by weight of the base polymer. The upper limit of the content of the photoreactive monomer or oligomer is preferably 400 parts by weight, more preferably 300 parts by weight, per 100 parts by weight of the base polymer. The content of the photoreactive monomer or oligomer can adjust the elastic modulus (particularly the elastic modulus at 200°C to 240°C) and linear expansion coefficient (particularly the linear expansion coefficient at 200°C to 240°C) of the resin layer. Furthermore, by adjusting the content of the photoreactive monomer or oligomer, the effects of the present invention become more pronounced.
[0042] Preferably, the active energy ray-curable resin composition contains a crosslinking agent. Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, and amine-based crosslinking agents. These crosslinking agents can be used alone or in combination of two or more.
[0043] The content of the crosslinking agent is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 8 parts by weight, relative to 100 parts by weight of the base polymer of the active energy ray-curable resin composition. Within this range, a resin layer with little dimensional change can be formed, and the effects of the present invention become remarkable.
[0044] In one embodiment, an epoxy-based crosslinking agent is preferably used. The epoxy-based crosslinking agent is a compound having an epoxy group, and specific examples thereof include N,N,N',N'-tetraglycidyl-m-xylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500N"), and the like. P"), ethylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 40E"), propylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 70P"), polyethylene glycol diglycidyl ether (manufactured by NOF Corporation, trade name "Epiol E-400"), polypropylene glycol diglycidyl ether (manufactured by NOF Corporation, trade name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol" EX-611), glycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. When the resin layer contains an epoxy-based crosslinking agent, the content of the epoxy-based crosslinking agent can be set to any appropriate amount depending on the desired properties, and is typically 0.01 to 10 parts by weight, and more preferably 0.03 to 5 parts by weight, relative to 100 parts by weight of the base polymer.
[0045] In one embodiment, an isocyanate-based crosslinking agent is preferably used, as it can react with a variety of functional groups. Specific examples of the isocyanate-based crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate HX"). Preferably, a crosslinking agent having three or more isocyanate groups is used.
[0046] Preferably, the active energy ray-curable resin composition contains a photopolymerization initiator, for example, α-ketol compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and 1-hydroxycyclohexylphenyl ketone; acetophenone compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; and ketal compounds such as benzyl dimethyl ketal. aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone compounds such as benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates.
[0047] The content of the photopolymerization initiator is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 12 parts by weight, and even more preferably 1 to 12 parts by weight, relative to 100 parts by weight of the base polymer.
[0048] The active energy ray-curable resin composition may further contain any appropriate additives as needed, such as a tackifier, a plasticizer (e.g., a trimellitic ester-based plasticizer or a pyromellitic ester-based plasticizer), a pigment, a dye, a filler, an antioxidant, a conductive material, an ultraviolet absorber, a light stabilizer, a release adjuster, a softener, a surfactant, a flame retardant, an antioxidant, and a solvent.
[0049] C. Substrate The substrate may be made of any suitable resin. Examples of the resin include polyolefin resins such as polyethylene resins, polypropylene resins, polybutene resins, and polymethylpentene resins, polyurethane resins, polyester resins, polyimide resins, polyether ketone resins, polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, fluorine resins, silicone resins, cellulose resins, and ionomer resins.
[0050] In one embodiment, a substrate made of a polyester resin is used as the substrate. A substrate made of a polyester resin preferably has rigidity, and the use of such a substrate can prevent displacement when fixing an electronic component.
[0051] In one embodiment, the substrate is made of a polyimide-based resin, a polyester-based resin, or a polyether ether ketone-based resin.
[0052] The thickness of the substrate is preferably 2 μm to 300 μm, more preferably 5 μm to 200 μm, and even more preferably 10 μm to 200 μm.
[0053] D. Pressure-sensitive adhesive layer / gas-generating layer The pressure-sensitive adhesive layer may be composed of any appropriate pressure-sensitive adhesive. The pressure-sensitive adhesive may be a curable pressure-sensitive adhesive or a pressure-sensitive adhesive. The pressure-sensitive adhesive layer may include, for example, an acrylic pressure-sensitive adhesive, a rubber pressure-sensitive adhesive, a silicone pressure-sensitive adhesive, or the like. For example, the active energy ray-curable resin composition may be used as the pressure-sensitive adhesive.
[0054] The thickness of the pressure-sensitive adhesive layer is, for example, 1 μm to 100 μm.
[0055] In one embodiment, the gas-generating layer can generate gas in response to an external stimulus. The gas-generating layer exhibits peelability due to the generated gas. For example, the gas-generating layer can be generated by decomposing components thereof with infrared or ultraviolet light, or by incorporating heat-expandable microspheres that expand at a predetermined temperature and then expanding by heating.
[0056] In one embodiment, the gas generating layer contains an infrared absorbing agent, an ultraviolet absorbing agent, or heat-expandable microspheres as the gas generating component.
[0057] In one embodiment, the gas-generating layer includes any appropriate adhesive and a gas-generating component. That is, the gas-generating layer may be configured by incorporating the gas-generating component into the adhesive layer. Alternatively, the gas-generating layer may be formed by combining the gas-generating layer with another layer (e.g., an adhesive layer), and the adhesive strength of the other layer may be reduced by a change in shape (such as distortion) of the gas-generating layer.
[0058] The gas generating layer containing the infrared absorber is a layer that can be gasified by irradiating the gas generating layer with infrared laser light. Examples of the infrared absorber include cesium tungsten oxide, lanthanum hexaboride, tin-doped indium oxide, antimony-doped tin oxide, cyanine compounds, phthalocyanine compounds, dithiol metal complexes, naphthoquinone compounds, diimmonium compounds, and azo compounds.
[0059] The content of the infrared absorber is preferably 1 to 100 parts by weight, more preferably 1 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, relative to 100 parts by weight of the gas generating layer. Within such a range, a pressure-sensitive adhesive sheet capable of forming a better deformed portion upon irradiation with laser light can be obtained.
[0060] The gas generating layer containing the ultraviolet absorber is a layer that can be gasified by irradiating the gas generating layer with ultraviolet laser light. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, triazine-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers. Details of the gas generating layer containing the ultraviolet absorber are described in, for example, Japanese Patent No. 6890216, and the description in this publication is incorporated herein by reference.
[0061] The content of the ultraviolet absorber is preferably 1 to 100 parts by weight, more preferably 1 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, relative to 100 parts by weight of the gas generating layer. Within such a range, a pressure-sensitive adhesive sheet capable of forming a better deformed portion upon laser light irradiation can be obtained.
[0062] The heat-expandable microspheres can expand at a predetermined temperature. When the heat-expandable microspheres in the gas-generating layer expand upon heating, the heat-expandable microspheres cause unevenness on the adhesive surface (i.e., the surface of the pressure-sensitive adhesive layer), resulting in a decrease or loss of adhesive strength.
[0063] The heat-expandable microspheres can be any suitable type as long as they are capable of expanding or foaming upon heating. For example, microspheres having an elastic shell encapsulating a substance that expands easily upon heating can be used. Such heat-expandable microspheres can be produced by any suitable method, such as coacervation or interfacial polymerization.
[0064] Examples of substances that expand easily when heated include low-boiling liquids such as propane, propylene, butene, normal butane, isobutane, isopentane, neopentane, normal pentane, normal hexane, isohexane, heptane, octane, petroleum ether, methane halides, and tetraalkylsilanes; and azodicarbonamide, which gasifies by thermal decomposition.
[0065] Examples of materials constituting the shell include polymers composed of nitrile monomers such as acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-ethoxyacrylonitrile, and fumaronitrile; carboxylic acid monomers such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, and citraconic acid; vinylidene chloride; vinyl acetate; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, and β-carboxyethyl acrylate; styrene monomers such as styrene, α-methylstyrene, and chlorostyrene; and amide monomers such as acrylamide, substituted acrylamide, methacrylamide, and substituted methacrylamide. Polymers composed of these monomers may be homopolymers or copolymers. Examples of such copolymers include vinylidene chloride-methyl methacrylate-acrylonitrile copolymer, methyl methacrylate-acrylonitrile-methacrylonitrile copolymer, methyl methacrylate-acrylonitrile copolymer, and acrylonitrile-methacrylonitrile-itaconic acid copolymer.
[0066] The heat-expandable microspheres may be formed using inorganic or organic blowing agents, such as ammonium carbonate, ammonium bicarbonate, sodium bicarbonate, ammonium nitrite, sodium boron hydroxide, and various azides. Examples of organic blowing agents include fluorinated alkane compounds such as trichloromonofluoromethane and dichloromonofluoromethane; azo compounds such as azobisisobutyronitrile, azodicarbonamide and barium azodicarboxylate; hydrazine compounds such as paratoluenesulfonylhydrazide, diphenylsulfone-3,3'-disulfonylhydrazide, 4,4'-oxybis(benzenesulfonylhydrazide) and allylbis(sulfonylhydrazide); semicarbazide compounds such as p-toluylenesulfonylsemicarbazide and 4,4'-oxybis(benzenesulfonylsemicarbazide); triazole compounds such as 5-morpholyl-1,2,3,4-thiatriazole; and N-nitroso compounds such as N,N'-dinitrosopentamethylenetetramine and N,N'-dimethyl-N,N'-dinitrosoterephthalamide.
[0067] The particle size of the heat-expandable microspheres before heating is preferably 0.5 to 80 μm, more preferably 5 to 45 μm, even more preferably 10 to 20 μm, and particularly preferably 10 to 15 μm. Therefore, the average particle size of the heat-expandable microspheres before heating is preferably 6 to 45 μm, more preferably 15 to 35 μm. The particle size and average particle size are values determined by particle size distribution measurement using a laser scattering method.
[0068] The heat-expandable microspheres preferably have an appropriate strength so that they do not burst until their volumetric expansion rate reaches at least 5 times, more preferably at least 7 times, and even more preferably at least 10 times. When such heat-expandable microspheres are used, their adhesive strength can be efficiently reduced by heat treatment.
[0069] The expansion initiation temperature of the heat-expandable microspheres is preferably 80°C to 250°C, more preferably 80°C to 230°C, even more preferably 80°C to 200°C, even more preferably 80°C to 150°C, particularly preferably 80°C to 120°C, and most preferably 80°C to 100°C. In this specification, the expansion initiation temperature of heat-expandable microspheres refers to the lowest temperature at which the thickness of the gas-generating layer increases by 5% or more from the thickness at room temperature. For example, the expansion initiation temperature may correspond to the temperature at which the adhesive strength of the gas-generating layer side of the pressure-sensitive adhesive tape decreases to 1.0 N / 20 mm or less and 50% or less of the initial adhesive strength.
[0070] The content of the heat-expandable microspheres in the gas-generating layer can be appropriately set depending on the desired adhesive strength reduction, etc. The content of the heat-expandable microspheres is, for example, 1 to 150 parts by weight, preferably 10 to 130 parts by weight, and more preferably 25 to 100 parts by weight, per 100 parts by weight of the adhesive layer.
[0071] E. Method for Producing Pressure-Sensitive Adhesive Sheet The pressure-sensitive adhesive sheet can be produced by any appropriate method. For example, the pressure-sensitive adhesive sheet can be obtained by coating the active energy ray-curable resin composition on a substrate for coating. As the coating method, various methods can be used, such as bar coater coating, air knife coating, gravure coating, gravure reverse coating, reverse roll coating, lip coating, die coating, dip coating, offset printing, flexographic printing, and screen printing. The substrate for coating may be used as the substrate for the pressure-sensitive adhesive sheet as is, or the resin layer may be peeled off from the substrate for coating to form the pressure-sensitive adhesive sheet.
[0072] Preferably, a coating layer of an active energy ray-curable resin composition is cured with active energy rays to form a resin layer. As the active energy rays, ultraviolet rays are preferably used. The coating layer can be cured, for example, with an integrated light dose of 50 J / cm. 2 ~1000 J / cm 2 It is formed by irradiating ultraviolet light of 1000 kJ / cm.
[0073] Alternatively, a method may be employed in which a resin layer is separately formed on a release liner and then laminated to a coating substrate. The surface roughness Ra of the resin layer surface can be controlled by the surface roughness Ra of the release liner. By forming a resin layer on a release liner with a small surface roughness Ra, the smoothness of the resin layer surface in contact with the release liner can be increased. The surface roughness Ra of the release liner is preferably 100 nm or less, more preferably 80 nm or less, and even more preferably 50 nm or less. The lower limit of the surface roughness Ra of the release liner is, for example, 20 nm.
[0074] F. Method of Using the Adhesive Sheet As described above, the adhesive sheet can be used when manufacturing a semiconductor package, specifically when temporarily fixing predetermined elements when manufacturing a semiconductor package.
[0075] In one embodiment, the pressure-sensitive adhesive sheet is used as a temporary fixing material in a so-called FOWLP (Fan Out Wafer Level Package) process.
[0076] In one embodiment, the pressure-sensitive adhesive sheet can be used as a temporary fixing material when providing wiring on the pressure-sensitive adhesive sheet. In one embodiment, there is provided a method of using the pressure-sensitive adhesive sheet, the method comprising: placing the pressure-sensitive adhesive sheet on a support substrate; forming wiring on a resin layer of the pressure-sensitive adhesive sheet; and then applying an external stimulus to the pressure-sensitive adhesive sheet to separate the pressure-sensitive adhesive sheet from the support substrate.
[0077] In one embodiment, in the method of using the pressure-sensitive adhesive sheet, before forming wiring, a semiconductor chip is placed and the semiconductor chip is sealed with resin. The semiconductor package manufacturing process including these steps is a process known to those skilled in the art as a so-called chip-first process, and therefore a detailed description thereof will be omitted.
[0078] In another embodiment, in the method of using the pressure-sensitive adhesive sheet, a seed layer is formed before forming wiring. The seed layer is a layer that serves as a conductor when forming metal layers such as wiring and copper pillars by plating. Examples of metals that constitute the seed layer include copper and / or titanium. The seed layer can be formed by any appropriate method (e.g., sputtering, vacuum deposition). The semiconductor package manufacturing process including these steps is known to those skilled in the art as a so-called RDL (redistribution line) first process, and therefore a detailed description thereof will be omitted.
[0079] In one embodiment, the pressure-sensitive adhesive sheet can be used as a temporary fixing material when providing copper pillars on the pressure-sensitive adhesive sheet. In one embodiment, a method for using the pressure-sensitive adhesive sheet is provided, comprising: placing the pressure-sensitive adhesive sheet on a support substrate; forming copper pillars on a resin layer of the pressure-sensitive adhesive sheet; and then applying an external stimulus to the pressure-sensitive adhesive sheet to separate the pressure-sensitive adhesive sheet from the support substrate. Any appropriate method can be used to form the copper pillars. Preferably, a seed layer is formed before forming the copper pillars.
[0080] Examples of external stimuli that can be applied when separating the pressure-sensitive adhesive sheet include heating, infrared radiation, ultraviolet radiation, etc. Preferably, a pressure-sensitive adhesive sheet having a gas-generating layer is used, and separability is achieved by applying an external stimulus to the gas-generating layer.
[0081] Any appropriate laser light is used for infrared irradiation and ultraviolet irradiation depending on the configuration of the pressure-sensitive adhesive sheet. The conditions for laser light irradiation can also be any appropriate conditions depending on the configuration of the pressure-sensitive adhesive sheet. In one embodiment, IR laser light is used as the laser light. The wavelength of the IR laser light is preferably 800 nm or more, more preferably 800 nm to 10,600 nm, and even more preferably 900 nm to 1,200 nm. The output of the IR laser light is, for example, 0.01 W to 20 W. In another embodiment, UV laser light is used as the laser light. The wavelength of the UV laser light is preferably 380 nm or less, more preferably 150 nm to 380 nm, and even more preferably 240 nm to 360 nm. The output of the UV laser light is, for example, 0.1 W to 4.0 W.
[0082] In one embodiment, after separating the pressure-sensitive adhesive sheet from the support substrate, the resin layer remaining on the object disposed on the resin layer (e.g., a semiconductor chip, a seed layer, a metal layer (wiring, copper pillar) obtained through seed layer formation, etc.) is removed. In one embodiment, the resin layer is removed by peeling. For example, when a pressure-sensitive adhesive sheet including a substrate is used, the resin layer can be removed by peeling. In another embodiment, the resin layer is removed by polishing. The resin layer may also be removed using a surface treatment technique such as plasma treatment.
[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Test and evaluation methods in the examples are as follows. Unless otherwise specified, "parts" and "%" are by weight.
[0084] (1) Surface Roughness Ra The arithmetic surface roughness Ra of the resin layer surface of the PSA sheet was measured in accordance with JIS B 0601. The measuring instrument used was an optical surface roughness meter (manufactured by Veeco Metrology Group, trade name "Wyko NT9100").
[0085] (2) Tensile Modulus of Resin Layer and Pressure-Sensitive Adhesive Sheet Using a dynamic viscoelasticity measuring device (manufactured by TA Instrument, product name "RSA-3"), the tensile modulus was measured at 25°C, 200°C, and 230°C under the following conditions: Measurement frequency: 1 Hz, Strain: 0.05%, Chuck distance: 20 mm, Sample width: 10 mm, Heating rate from 0°C to 250°C at 5°C / min.
[0086] (3) Linear expansion coefficient of resin layer and adhesive sheet Using a TMA Q400 (manufactured by TA-instrument), the linear expansion coefficient (CTE) of the resin layer and adhesive sheet at 200-210 ° C and 230-240 ° C was measured under the conditions of a nitrogen gas flow rate of 50.0 ml / min and an applied load of 0.0196 N in tension mode. Specifically, the adhesive sheets and resin layers obtained in the examples and comparative examples were prepared, punched out to a size of 4 mm x 30 mm using a jig, and set on the TMA Q400 probe at 8 mm intervals. The temperature was once increased from 20 ° C to 110 ° C at a heating rate of 10 ° C / min, and then decreased from 110 ° C to 20 ° C at a cooling rate of 10 ° C / min to remove the influence of contained moisture, and then again increased from 20 ° C to 300 ° C at a heating rate of 10 ° C / min. The dimensional change of the pressure-sensitive adhesive sheet was measured while the temperature was increased at a rate of 100-210°C. From the obtained data, the slope of the dimensional change at 200-210°C and 230-240°C was calculated, and the CTE value was extracted.
[0087] (4) Nanoindenter elastic modulus of resin layer: 500 mJ / cm 2 The resin layer irradiated with ultraviolet light was subjected to measurement of the elastic modulus of the resin layer surface using a nanoindenter (manufactured by Hysitron Inc., product name "Triboindenter TI-950") by a single indentation method at a predetermined temperature (25°C) under the measurement conditions of an indentation speed of about 500 nm / sec, an extraction speed of about 500 nm / sec, and an indentation depth of about 3000 nm.
[0088] (5) Change in Resin Layer Thickness Due to Dropping of Polar Solvents With the resin layer of the pressure-sensitive adhesive sheet exposed, 0.1 mL of each of three polar solvents, N-methyl-2-pyrrolidone (Kishida Chemicals), propylene glycol monomethyl ether acetate (Tokyo Chemical Industry Co., Ltd.), and dimethyl sulfoxide (Tokyo Chemical Industry Co., Ltd.), was dropped onto the sheet, and the sheet was then left to stand at 25°C for 15 minutes. After that, the various polar solvents were wiped off, and the thickness of the resin layer before and after the dropping was measured to calculate the rate of change.
[0089] (6) Adhesive Strength The resin layer of the adhesive sheet was attached to a polyimide film (manufactured by Toray Industries, Inc., trade name "Kapton 100H", thickness: 25 μm) and left at 200 ° C for 2 hours. The gas-generating layer side of the adhesive sheet was then attached and fixed to a stainless steel plate, and the adhesive strength of the adhesive sheet to the polyimide film was measured according to JIS Z 0237:2000 (lamination conditions: 1 round trip with a 2 kg roller, tensile speed: 300 mm / min, peel angle 180 °, measurement temperature: 23 ° C). The adhesive strength after 2 hours at 230 ° C after attachment was also measured in the same manner. The polyimide film used as the adherend was one that had been freed from the effects of moisture. Specifically, a polyimide film was used that had been previously dried by heating at 200 ° C for 30 minutes.
[0090] (7) Surface Roughness Ra of Seed Layer Using a batch sputtering device, Ti and Cu were deposited on the resin layer by DC discharge under an Ar atmosphere while the resin layer of the adhesive sheet was exposed, forming a seed layer with a Ti / Cu = 150 nm / 300 nm. The arithmetic surface roughness Ra of the obtained seed layer surface was measured in accordance with JIS B0601. An optical surface roughness meter (manufactured by Veeco Metrology Group, trade name "Wyko NT9100") was used as the measuring instrument. (8) Seed Layer Moldability The seed layer formed on the resin layer was visually observed. In the table, a mirror-like surface of the metal thin film was obtained and the Ra was 200 nm or less, a mirror-like surface of the metal thin film was obtained but the Ra was greater than 200 nm, and a failure (×) was indicated. (9) Cracks in the seed layer The seed layer formed on the resin layer was visually observed. In the table, cases where no cracks were visible were marked as pass (◯), and cases where cracks were visible were marked as fail (×).
[0091] [Production Example 1] Preparation of Acrylic Polymer A 30 parts by weight of 2-ethylhexyl acrylate, 70 parts by weight of methyl acrylate, 10 parts by weight of acrylic acid, and 0.2 parts by weight of benzoyl peroxide as a polymerization initiator were added to ethyl acetate, and the mixture was heated to 70°C to obtain an ethyl acetate solution of an acrylic copolymer (Polymer A).
[0092] [Production Example 2] Preparation of Acrylic Polymer B To toluene were added 50 parts by weight of butyl acrylate, 50 parts by weight of ethyl acrylate, 5 parts by weight of acrylic acid, 0.1 parts by weight of 2-hydroxyethyl acrylate, 0.3 parts by weight of trimethylolpropane triacrylate, and 0.1 parts by weight of benzoyl peroxide as a polymerization initiator, and the mixture was heated to 70°C to obtain a toluene solution of an acrylic copolymer (Polymer B).
[0093] [Production Example 3] Resin layer-forming composition A A resin layer-forming composition A was prepared by mixing an ethyl acetate solution of polymer A (polymer A: 100 parts by weight), 0.3 parts by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "TETRAD-C"), 100 parts by weight of a UV oligomer (manufactured by Mitsubishi Chemical Corporation, trade name "Shikou UV-1700B"), and 1.5 parts by weight of a photopolymerization initiator (manufactured by BASF SE, trade name "Omnirad 127D").
[0094] [Production Example 4] Gas Generating Layer-Forming Composition A An ethyl acetate solution of polymer A (polymer A: 100 parts by weight), 0.3 parts by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "TETRAD-C"), 50 parts by weight of a UV oligomer (manufactured by Mitsubishi Chemical Corporation, trade name "Shikou UV-1700B"), 1.5 parts by weight of a photopolymerization initiator (manufactured by BASF SE, trade name "Omnirad 127D"), an ultraviolet absorber (a reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hydroxyphenyl and [(C10-C16 (mainly C12-C13) alkyloxy)methyl]oxirane, trade name "TINUVIN" 20 parts by weight of "400" manufactured by BASF and 30 parts by weight of an infrared absorbing carbon black pigment (trade name "SZ7740" manufactured by Dainichiseika Color & Chemicals Co., Ltd.) were mixed together to prepare a gas generating layer forming composition A.
[0095] [Example 1] The resin layer-forming composition A obtained in Production Example 1 was applied to a polyethylene terephthalate film (manufactured by Toray Industries, Inc., trade name "Cerapeel", thickness: 38 μm, surface roughness Ra: 77.97 nm) with a silicone release agent-treated surface so that the thickness after solvent evaporation (drying) would be 10 μm, and then dried to form a resin precursor layer on the polyethylene terephthalate film. The gas-generating layer-forming composition A obtained in Production Example 2 was applied to a polyethylene terephthalate film (thickness: 75 μm) with a silicone release agent-treated surface so that the thickness after solvent evaporation (drying) would be 10 μm, and then dried to form a gas-generating precursor layer on the polyethylene terephthalate film. Next, the resin precursor layer and the gas-generating precursor layer were laminated together between rolls, and 500 mJ / cm was applied from the resin precursor layer side. 2The adhesive sheet was subjected to the above-described evaluations. The results are shown in Table 1.
[0096] [Example 2] A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that acrylic polymer B was used instead of acrylic polymer A and the content of the epoxy-based crosslinking agent was 1 part by weight. The obtained pressure-sensitive adhesive sheet was subjected to the above-mentioned evaluations. The results are shown in Table 1.
[0097]
[0098] [Production Example 5] Resin layer-forming composition B A resin layer-forming composition B was prepared by mixing a toluene solution of polymer B (polymer B: 100 parts by weight), 1.0 part by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "TETRAD-C"), 20 parts by weight of a UV oligomer (manufactured by Mitsubishi Chemical Corporation, trade name "Shikou UV-1700B"), and 1.5 parts by weight of a photopolymerization initiator (manufactured by BASF SE, trade name "Omnirad 127D").
[0099] [Production Example 6] Gas generating layer-forming composition B A gas generating layer-forming composition B was prepared by mixing an ethyl acetate solution of polymer A (polymer A: 100 parts by weight), 0.3 parts by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "TETRAD-C"), 50 parts by weight of a UV oligomer (manufactured by Mitsubishi Chemical Corporation, trade name "Shikou UV-1700B"), 1.5 parts by weight of a photopolymerization initiator (manufactured by BASF Corporation, trade name "Omnirad 127D"), and 30 parts by weight of an infrared absorber carbon black pigment (trade name "SZ7740", manufactured by Dainichiseika Color & Chemicals Co., Ltd.).
[0100] [Example 3] The resin layer-forming composition B obtained in Production Example 5 was applied to one side of a polyimide film (manufactured by DuPont Toray Co., Ltd., trade name "Kapton 100H", thickness: 25 μm, surface roughness Ra: 77.97 nm) so that the thickness after solvent evaporation (drying) would be 5 μm, and then dried to form a resin precursor layer on the polyimide film, and a polyethylene terephthalate film with a silicone release agent-treated surface (manufactured by Toray Co., Ltd., trade name "Cerapeel", thickness: 38 μm) was laminated between rolls to bond it. Next, the gas-generating layer-forming composition B obtained in Production Example 6 was applied to a polyethylene terephthalate film with a silicone release agent-treated surface (thickness: 75 μm) so that the thickness after solvent evaporation (drying) would be 10 μm, and then dried, and the polyimide film was laminated between rolls to bond it to the opposite side of the resin layer, and 500 mJ / cm 2 The adhesive sheet was then subjected to UV irradiation under the conditions of . In this manner, a pressure-sensitive adhesive sheet (resin layer / polyimide film / gas-generating layer) sandwiched between polyethylene terephthalate films with silicone release agent-treated surfaces was obtained. The resulting pressure-sensitive adhesive sheet was subjected to the above-mentioned evaluations. The results are shown in Table 2.
[0101] [Examples 4 to 6] Pressure-sensitive adhesive sheets were obtained in the same manner as in Example 3, except that the blending amount of the UV oligomer in the resin layer-forming composition was as shown in Table 2. The obtained pressure-sensitive adhesive sheets were subjected to the above-mentioned evaluations. The results are shown in Table 2.
[0102]
[0103] Production Example 7 Gas-Generating Layer-Forming Composition C A gas-generating layer-forming composition C was prepared by mixing a toluene solution of polymer B (polymer B: 100 parts by weight), 1.0 part by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "TETRAD-C"), 20 parts by weight of a UV oligomer (manufactured by Mitsubishi Chemical Corporation, trade name "Shikou UV-1700B"), 1.5 parts by weight of a photopolymerization initiator (manufactured by BASF Corporation, trade name "Omnirad 127D"), and heat-expandable microspheres (manufactured by Sekisui Chemical Co., Ltd., trade name "Advancell EMS-024").
[0104] [Example 7] A pressure-sensitive adhesive sheet (resin layer / polyimide film / gas-generating layer) sandwiched between polyethylene terephthalate films with silicone release agent-treated surfaces was obtained in the same manner as in Example 3, except that gas-generating layer-forming composition C was used instead of gas-generating layer-forming composition B. The obtained pressure-sensitive adhesive sheet was subjected to the above-mentioned evaluations. The results are shown in Table 3.
[0105] [Example 8] A pressure-sensitive adhesive sheet (resin layer / polyethylene terephthalate film / gas-generating layer) sandwiched between polyethylene terephthalate films with silicone release agent-treated surfaces was obtained in the same manner as in Example 3, except that a polyethylene terephthalate film (manufactured by Toray DuPont Co., Ltd., product name "Kapton 100H", thickness: 25 μm) was used instead of the polyimide film (manufactured by Toray DuPont Co., Ltd., product name "Lumirror S10", thickness: 38 μm). The obtained pressure-sensitive adhesive sheet was subjected to the above-mentioned evaluations. The results are shown in Table 3.
[0106] [Examples 9 to 11] Pressure-sensitive adhesive sheets were obtained in the same manner as in Example 8, except that the blending amount of the UV oligomer in the resin layer-forming composition was as shown in Tables 3 and 4. The obtained pressure-sensitive adhesive sheets were subjected to the above-mentioned evaluations. The results are shown in Tables 3 and 4.
[0107]
[0108]
[0109] Example 12 A pressure-sensitive adhesive sheet (resin layer / polyethylene naphthalate film / gas-generating layer) sandwiched between polyethylene terephthalate films with silicone release agent-treated surfaces was obtained in the same manner as in Example 3, except that a polyethylene naphthalate film (Teonex (registered trademark) film Q51C-50, manufactured by Teijin Film Solutions Co., Ltd., thickness: 50 μm) was used instead of a polyimide film (manufactured by DuPont-Toray Co., Ltd., trade name "Kapton 100H", thickness: 25 μm). The obtained pressure-sensitive adhesive sheet was subjected to the above-mentioned evaluations. The results are shown in Table 3.
[0110] [Production Example 8] Resin layer-forming composition C A resin layer-forming composition C was prepared by mixing an ethyl acetate solution of polymer A (polymer A: 100 parts by weight) and 5.0 parts by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "TETRAD-C").
[0111] [Example 13] The resin layer-forming composition C obtained in Production Example 8 was applied to one side of a polyimide film (manufactured by DuPont Toray, product name "Kapton 100H", thickness: 25 μm) so that the thickness after solvent evaporation (drying) was 5 μm, and then dried to form a resin layer on the polyimide film, and a polyethylene terephthalate film with a silicone release agent-treated surface (manufactured by Toray, product name "Cerapeel", thickness: 38 μm) was laminated between rolls to bond it. Next, the gas-generating layer-forming composition B obtained in Production Example 6 was applied to a polyethylene terephthalate film (thickness: 75 μm) with a silicone release agent-treated surface so that the thickness after solvent evaporation (drying) was 10 μm, and then dried, and the polyimide film was laminated between rolls to bond it to the side opposite the resin layer. In this way, a pressure-sensitive adhesive sheet (resin layer / polyimide film / gas-generating layer) sandwiched between polyethylene terephthalate films with silicone release agent-treated surfaces was obtained. The resulting pressure-sensitive adhesive sheet was subjected to the above evaluations, and the results are shown in Table 3.
[0112] [Example 14] A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 13, except that the amount of crosslinking agent was 1.0 part by weight. The pressure-sensitive adhesive sheet obtained was subjected to the above-mentioned evaluations. The results are shown in Table 3.
[0113] Comparative Example 1 A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 3, except that a polyethylene terephthalate film with a surface treated with a silicone release agent (manufactured by Toray Industries, Inc., trade name "Cerapeel", thickness: 38 μm) was used instead of a polyethylene terephthalate film with a surface treated with a silicone release agent (manufactured by Kimoto Co., Ltd., trade name "Release MAG01", thickness: 75 μm). The pressure-sensitive adhesive sheet obtained was subjected to the above-mentioned evaluations. The results are shown in Table 4.
[0114] [Comparative Example 2] A pressure-sensitive adhesive sheet was obtained in the same manner as in Comparative Example 1, except that the blending amount of the UV oligomer was set as shown in Table 1. The obtained pressure-sensitive adhesive sheet was subjected to the above-mentioned evaluations. The results are shown in Table 5.
[0115]
[0116] 10 Resin layer 20 Substrate 100 Pressure-sensitive adhesive sheet
Claims
1. An adhesive sheet for manufacturing a semiconductor package that is placed on a substrate and used, the adhesive sheet having a resin layer made of an acrylic resin, and at least one surface of the resin layer having a surface roughness Ra of 600 nm or less.
2. The adhesive sheet for manufacturing a semiconductor package has a linear expansion coefficient of -50×10 at 230° C. to 240° C. -5 / K~50x10 -5 2. The adhesive sheet for producing a semiconductor package according to claim 1, wherein the viscosity is 100 MPa or less.
3. The adhesive sheet for manufacturing a semiconductor package according to claim 1, wherein the resin layer is formed from an active energy ray-curable resin composition containing an acrylic polymer, a pentaerythritol-based multifunctional acrylate, and a photopolymerization initiator.
4. The adhesive sheet for manufacturing a semiconductor package according to claim 1, wherein the resin layer has a nanoindenter elastic modulus of 10 MPa or more after irradiation with ultraviolet light at 25°C.
5. The adhesive sheet for manufacturing a semiconductor package as described in claim 1, wherein the thickness of the resin layer after dropping a polar solvent onto the resin layer and leaving it at 25°C for 15 minutes is 130% or less of the thickness before the dropping.
6. The adhesive sheet for producing a semiconductor package according to claim 1, further comprising a substrate, the resin layer being disposed on one side of the substrate, and the substrate being made of a polyimide resin, a polyester resin or a polyether ether ketone resin.
7. An adhesive sheet for manufacturing a semiconductor package as described in claim 1 or 6, wherein the adhesive strength after the resin layer of the adhesive sheet is attached to a polyimide plate and left at 230°C for 2 hours is 5 N / 20 mm or less.
8. The adhesive sheet for producing a semiconductor package according to claim 6, further comprising a gas generation layer, the resin layer, the substrate and the gas generation layer being arranged in this order.
9. A method for using an adhesive sheet for manufacturing semiconductor packages, comprising: placing the adhesive sheet for manufacturing semiconductor packages according to claim 1 on a support substrate; forming wiring on a resin layer of the adhesive sheet for manufacturing semiconductor packages; and thereafter applying an external stimulus to the adhesive sheet for manufacturing semiconductor packages, thereby separating the adhesive sheet for manufacturing semiconductor packages from the support substrate.
10. A method for using an adhesive sheet for manufacturing semiconductor packages, comprising: placing the adhesive sheet for manufacturing semiconductor packages according to claim 1 on a support substrate; forming copper pillars on a resin layer of the adhesive sheet for manufacturing semiconductor packages; and then applying an external stimulus to the adhesive sheet for manufacturing semiconductor packages to separate the adhesive sheet for manufacturing semiconductor packages from the support substrate.
Citation Information
Patent Citations
Dicing tape, dicing tape integrated adhesive sheet, semiconductor device, and method of manufacturing semiconductor device
JP2011009732A
Pressure sensitive adhesive sheet
JP2015168711A
Mold processing film for semiconductor package
KR1020110076388A