Hard mask manufacturing method
By controlling nitrogen and argon gas flow rates and processing pressures, along with bias power, the method achieves microcrystalline tungsten films with small grain sizes and controlled stress, addressing the challenges of shape integrity and etching precision in hard mask manufacturing for semiconductor devices.
Patent Information
- Application Number
- PCT/JP2024/005418
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-02-16
- Publication Date
- 2024-12-05
AI Technical Summary
The existing methods for manufacturing hard masks with tungsten films struggle to produce microcrystalline films with small grain sizes and controlled stress, which is crucial for maintaining shape integrity during semiconductor device processing.
The method involves forming a tungsten nitride film using reactive sputtering with controlled nitrogen and argon gas flow rates and pressures, followed by forming a tungsten film with adjustable stress by managing the total pressure and bias power in the processing chamber, allowing for precise control of grain size and stress within predetermined ranges.
This approach results in a microcrystalline tungsten film with a grain size of 60 nm or less and stress within ±300 MPa, enhancing the precision and reliability of the hard mask in limiting the dry etching process.
Smart Images

Figure JP2024005418_05122024_PF_FP_ABST
Abstract
Description
Hard mask manufacturing method
[0001] The present invention relates to a method for manufacturing a hard mask.
[0002] For example, in the manufacturing process of a semiconductor device, a predetermined thin film (e.g., SiO 2 A dry etching process is performed on a tungsten nitride film (film). At this time, a (metal) hard mask, for example, is provided on the surface of the substrate to be processed to limit the dry etching processing range. One such hard mask is known, for example, from Patent Document 1, which includes a tungsten nitride film as an underlayer and a tungsten film laminated on the tungsten nitride film. In this process, a tungsten target is used as a first step, and a rare gas and nitrogen gas are introduced into a processing chamber under a vacuum atmosphere to form a tungsten nitride film on the surface of the substrate to be processed by a reactive sputtering method. In a second step, a tungsten target is used as a second step, and a tungsten film is formed on the surface of the tungsten nitride film by a sputtering method in a processing chamber under a vacuum atmosphere. Subsequently, desired openings are patterned by, for example, lithography.
[0003] Here, tungsten films formed by sputtering have a higher density than carbon films and have excellent dry etching resistance, but they are known to have large grain sizes (100 nm or more) and may result in poor processing shape during patterning of openings in later processes. Therefore, it is desirable for such tungsten films to be finely crystalline films with as small a grain size as possible, but depending on the application of the tungsten film, it is also desirable for the film stress to be maintained within a predetermined range. For example, when sufficient focusing is required in the lithography process, it is desirable to maintain the film stress within ±300 MPa (more preferably within ±100 MPa).
[0004] Japanese Patent Application Laid-Open No. 2022-27215
[0005] In view of the above, an object of the present invention is to provide a method for manufacturing a hard mask that makes it possible to adjust the film stress according to the film thickness while making the tungsten film a fine crystal film.
[0006] In order to solve the above problems, the method for manufacturing a hard mask of the present invention includes a first step in which a target made of tungsten is used, a rare gas and a nitrogen gas are introduced into a processing chamber having a vacuum atmosphere, and a tungsten nitride film is formed on the surface of a substrate to be processed by a reactive sputtering method; and a second step in which a target made of tungsten is used, and a tungsten film is formed on the surface of the tungsten nitride film by a sputtering method in the processing chamber having a vacuum atmosphere, wherein in the first step, the flow rate ratio of the rare gas to the nitrogen gas is set to 1.5 or less and the pressure in the processing chamber is set to 1 Pa or more, and in the second step, stress corresponding to the thickness of the tungsten film is adjusted by controlling at least one of the total pressure in the processing chamber and the bias power input to the substrate to be processed during film formation.
[0007] As a result of intensive research, the present inventors have discovered the following: Specifically, when forming a tungsten nitride film on the surface of a substrate to be processed by reactive sputtering in the first step, increasing the flow rate ratio of nitrogen gas to rare gas and the pressure in the processing chamber reduces the grain size of the tungsten film formed in the second step, while increasing the stress (absolute value) of the tungsten film. Based on this finding, the present invention employs a configuration in which the flow rate ratio of rare gas to nitrogen gas is set to 1.5 or less and the pressure in the processing chamber is set to 1 Pa or more to form a tungsten nitride film in the first step, and then a tungsten film is formed on the surface of the tungsten nitride film in the second step, thereby enabling the formation of a fine-crystalline tungsten film with a small grain size (e.g., 60 nm or less) over the entire surface of the substrate to be processed. Then, by controlling at least one of the total pressure in the processing chamber and the bias power applied to the substrate to be processed during film formation in the second step, the stress of the tungsten film can be adjusted to a predetermined range (for example, within ±300 MPa, more preferably, within ±100 MPa) according to the film thickness.
[0008] In the present invention, when bias power is supplied to the substrate from an AC power supply connected via a matching box, the bias power control preferably includes the time required for impedance matching by the matching box, which allows for effective adjustment of the stress in the tungsten film even when the pressure in the processing chamber for the second step is relatively high.
[0009] 1 is a schematic cross-sectional view showing a hard mask according to an embodiment of the present invention; 2 is a schematic cross-sectional view of a sputtering apparatus capable of implementing the hard mask manufacturing method according to the present embodiment; 3 (a) to (c) are AFM images showing the results of an inventive experiment confirming the effects of the present invention, and 4 (d) to (f) and 5 (g) to (i) are AFM images showing the results of comparative experiments 1 and 2; 6 (a) to (c) are graphs showing changes in stress in a tungsten film when the argon gas flow rate is changed; 7 (b) to (c) are graphs showing changes in stress in a tungsten film when the bias power is changed; and 8 (c) to (i) are graphs showing changes in stress in a tungsten film when the time until impedance matching is achieved after bias power is applied is changed.
[0010] Hereinafter, with reference to the drawings, an embodiment of the hard mask Hm of the present invention and a method for manufacturing the same will be described. The hard mask Hm is formed on the surface of a substrate Sw to limit the etching processing range when a dry etching process is performed on the substrate Sw.
[0011] 1, the hard mask Hm has a tungsten nitride (WN) film Ly1 formed on the surface of a substrate Sw, and a tungsten (W) film Ly2 laminated on the tungsten nitride film Ly1. The substrate Sw may be a substrate such as a silicon wafer or a substrate having a predetermined thin film (e.g., SiO 2A hard mask Hm having an insulating film such as a TEOS film or a metal film such as an Al film formed thereon can be used. The thickness of the tungsten nitride film Ly1 can be set, for example, within a range of 5 to 15 nm. The thickness of the tungsten film Ly2 can be set, for example, within a range of 100 to 500 nm. An opening Op having a predetermined outline is then patterned in the hard mask Hm using known lithography techniques, and the portion of the substrate Sw exposed at the bottom of this opening Op is dry-etched to form the desired etching shape. A method for manufacturing the hard mask Hm of this embodiment will now be described.
[0012] Referring to FIG. 2 , Sm denotes a sputtering apparatus capable of implementing the method for manufacturing the hard mask Hm of this embodiment. The sputtering apparatus Sm includes a vacuum chamber 1 capable of forming a vacuum atmosphere, which defines a processing chamber Pc. An exhaust pipe 11 leading to a vacuum pump unit Pu, such as a turbomolecular pump or a rotary pump, is connected to the bottom wall of the vacuum chamber 1, enabling the vacuum chamber 1 to be evacuated. A conductance valve 12 is installed in the exhaust pipe 11 so as to adjust the effective pumping speed of the vacuum pump unit Pu. A gas pipe 14 equipped with a mass flow controller 13 is connected to the side wall of the vacuum chamber 1, enabling a rare gas (e.g., argon gas) and nitrogen gas to be introduced into the vacuum chamber 1 at predetermined flow rates. Hereinafter, terms indicating directions such as "upper" and "lower" will be described based on the installation position shown in FIG. 2 .
[0013] A stage 2 is disposed at the bottom of the vacuum chamber 1. The stage 2 is made of an insulator I 1The sputtering chamber 1 includes a base 21 made of a thermally conductive metal (e.g., SUS) and mounted on the lower wall of the vacuum chamber 1 via a matching box Mb. The base 21 is connected to an output from a high-frequency power supply (bias power supply Pb) via a matching box Mb, and during sputtering, high-frequency power of a predetermined frequency (e.g., 13.56 MHz) is applied to the base 21, thereby applying a predetermined bias power to the substrate Sw. Since known devices can be used for the chuck plate 22, bias power supply Pb, and matching box Mb, further description thereof will be omitted. Although not specifically shown or described, a heater and a coolant circulation path are mounted on the base 21. The heater can be energized from an external power supply, or a coolant can be circulated through the coolant circulation path from a chiller unit (not shown), thereby controlling the substrate Sw to a predetermined temperature by heat conduction from the base 21.
[0014] A cathode unit Cu is attached to the ceiling of the vacuum chamber 1. The cathode unit Cu has a tungsten target 3 arranged to face the substrate Sw, and a magnet unit 4 arranged above the target 3. The target 3 has a shape (circular in plan view) that corresponds to the contour of the substrate Sw, and an insulator I 2 The target 3 is attached to the underside of a backing plate 31 attached to the vacuum chamber 1 via a magnet unit 4. The target 3 is connected to the output of a sputtering power supply E, such as a DC power supply, so that a predetermined power can be supplied to the target 3 during film formation. The magnet unit 4 can have a known structure that generates a magnetic field in the space below the sputtering surface 3a of the target 3, captures electrons ionized below the sputtering surface 3a during sputtering, and efficiently ionizes sputtered particles scattered from the target 3, so a detailed description will be omitted here.
[0015] Although not shown, the sputtering apparatus Sm has a known control means including a microcomputer, a sequencer, or the like, which controls the operation of the sputtering power supply E and the bias power supply Pb, the aperture of the conductance valve 12, the operation of the mass flow controller 13, the operation of the vacuum pump unit Pu, the operation of the magnet unit 4, etc. A method for manufacturing the hard mask Hm of this embodiment using the sputtering apparatus Sm will now be described in detail.
[0016] A substrate Sw is placed on the upper surface of a stage 2 placed in a vacuum chamber 1, the vacuum chamber 1 is evacuated to a predetermined pressure, and once the predetermined pressure is reached, argon gas is introduced into the vacuum chamber 1 at a flow rate of 150 to 300 sccm and nitrogen gas is introduced at a flow rate of 100 sccm or more (at this time, the flow rate ratio of argon gas to nitrogen gas is set to 1.5 or less and the pressure inside the vacuum chamber 1 is set to 1 Pa or more), and DC power (e.g., 2 kW to 6 kW) with a negative potential is applied to the target 3 from a sputtering power supply E. This forms a plasma atmosphere inside the vacuum chamber 1, and the tungsten target 3 is reactively sputtered to form a tungsten nitride film Ly1 on the surface of the substrate Sw (first step). When the flow rates of argon gas and nitrogen gas are set so that the flow rate ratio of argon gas to nitrogen gas is 1.5 or less and the pressure inside the vacuum chamber 1 does not reach 1 Pa, the effective pumping speed of the vacuum pump unit Pu can be adjusted by adjusting the aperture of the conductance valve 12 to maintain the pressure inside the vacuum chamber 1 at 1 Pa or higher. However, if the pressure inside the vacuum chamber 1 exceeds, for example, 30 Pa, it becomes difficult to adjust the stress of the tungsten film in the second step described below. In the first step, bias power (e.g., 50 W to 300 W) may be applied to the substrate Sw from the bias power supply Pb during film formation.
[0017] Once the tungsten nitride film Ly1 has been formed on the surface of the substrate Sw to a predetermined thickness (after completion of the first step), the introduction of only the nitrogen gas is stopped, and only argon gas is introduced into the vacuum chamber 1 at a flow rate of 150 to 300 sccm (at this time, the pressure inside the vacuum chamber 1 is 0.1 Pa to 30 Pa). The power supplied from the sputtering power supply E to the target 3 is then changed to, for example, a range of 4 kW to 12 kW. This causes the tungsten target 3 to be sputtered, and a tungsten film Ly2 is formed (laminate) on the surface of the tungsten nitride film Ly1 to a predetermined thickness (second step). In the second step, as in the first step, bias power (for example, 50 W to 300 W) may be supplied to the substrate Sw from the bias power supply Pb. After the tungsten film Ly2 has been formed, openings Op are patterned in the tungsten film Ly2 and the tungsten nitride film Ly1 using known lithography techniques or the like. If the pressure inside the vacuum chamber 1 exceeds 30 Pa in the second step, it becomes difficult to adjust the stress of the tungsten film.
[0018] As described above, in the first step, the flow rate ratio of the rare gas to the nitrogen gas is set to 1.5 or less and the pressure in the vacuum chamber 1 is set to 1 Pa or more, and then in the second step, a tungsten film Ly2 is formed on the surface of the tungsten nitride film Ly1, thereby making it possible to form a fine-crystalline tungsten film Ly2 with a small grain size (for example, 60 nm or less) over the entire surface of the substrate Sw.
[0019] In order to confirm the above-mentioned effect, the following experiment was carried out using the sputtering apparatus Sm. In the invention experiment, SiO 2A 100 nm TEOS (tetraethoxysilane) film was deposited on the substrate Sw. Argon gas was introduced into the vacuum chamber 1 at a flow rate of 300 sccm, and nitrogen gas was introduced at a flow rate of 200 sccm (the flow rate ratio of argon gas to nitrogen gas was 1.5). The aperture of the conductance valve 12 was adjusted to maintain the pressure in the vacuum chamber 1 at 1 Pa. Then, 3 kW of DC power was applied to the tungsten target 3, and 300 W of bias power was applied to the substrate Sw, depositing a 5 nm tungsten nitride film Ly1 (Step 1). Subsequently, argon gas was introduced into the vacuum chamber 1 at a flow rate of 150 sccm, and 6 kW of DC power was applied to the tungsten target 3, depositing a 195 nm tungsten film Ly2 (Step 2). 3(a) to 3(c) show the results (AFM images) of atomic force microscopy (AFM) observations of the surface of the tungsten film Ly2 in the central portion (FIG. 3(a)), peripheral portion (FIG. 3(b)), and intermediate region (FIG. 3(c)) of the substrate Sw on which the tungsten film Ly2 was formed. These images confirmed that the tungsten film Ly2 was composed of fine crystals with a small grain size over the entire in-plane surface of the substrate Sw, as compared with those in Comparative Experiment 1 (FIGS. 3(d) to 3(f)) and Comparative Experiment 2 (FIGS. 3(g) to 3(i)), which will be described later. Furthermore, when the surface of this tungsten film Ly2 was observed with a scanning transmission electron microscope (STEM), the grain size was found to be 60 nm or less.
[0020] As a comparative experiment 1 to the above-mentioned inventive experiment, a substrate Sw on which a tungsten film Ly2 was formed was obtained in the same manner as the above-mentioned inventive experiment, except that in the first step, the flow rate of argon gas introduced into the vacuum chamber 1 was 150 sccm, the flow rate of nitrogen gas was 70 sccm (the flow rate ratio of argon gas to nitrogen gas was 2.1), and the pressure in the vacuum chamber 1 was maintained at less than 1 Pa. Furthermore, as in the above-mentioned inventive experiment, the surface of the tungsten film Ly2 was observed by AFM in the central portion ( FIG. 3( d )), peripheral portion ( FIG. 3( e )), and intermediate region ( FIG. 3( f )) of the substrate Sw on which the tungsten film Ly2 was formed. As a result, it was confirmed that the tungsten film Ly2 was a crystalline film with a large grain size throughout the entire surface of the substrate Sw, compared to that of the above-mentioned inventive experiment. Furthermore, when the surface of this tungsten film Ly2 was observed by STEM, the grain size was 100 nm or more.
[0021] Furthermore, in Comparative Experiment 2, a substrate Sw on which a tungsten film Ly2 was formed was obtained in the same manner as in the above-described inventive experiment, except that the flow rates of argon gas and nitrogen gas introduced into the vacuum chamber 1 in the first step were set to 132 sccm and 88 sccm (the flow rate ratio of argon gas to nitrogen gas was 1.5), respectively, and the pressure inside the vacuum chamber 1 was maintained at less than 1 Pa. Furthermore, similar to the above-described inventive experiment, the surface of the tungsten film Ly2 in the central portion ( FIG. 3( g) ), peripheral portion ( FIG. 3( h) ), and intermediate region therebetween ( FIG. 3( i) ) of the substrate Sw on which the tungsten film Ly2 was formed was observed by AFM. As a result, it was confirmed that the central portion and intermediate region were made of fine crystals with small grain sizes, while the peripheral region was a crystalline film with large grain sizes.
[0022] Next, an experiment was conducted to form a tungsten film Ly2 on the surface of the tungsten nitride film Ly1 using a substrate Sw on which a tungsten nitride film Ly1 had been formed under the conditions of the first step of the above-mentioned invention experiment (i.e., a flow rate ratio of argon gas to nitrogen gas of 1.5 and a pressure in the vacuum chamber 1 of 1 Pa). In this experiment, the power (DC power) input to the tungsten target 3 was set to 6 kW. Then, in the second step, the flow rate of argon gas introduced into the vacuum chamber 1 was changed within a range of 150 to 300 sccm, and a tungsten film Ly2 was formed to a thickness of 195 nm (at this time, the pressure in the vacuum chamber 1 was in a range of 0.1 Pa to 30 Pa). The stress (MPa) of the tungsten film Ly2 formed by changing the argon gas flow rate was measured using a thin film stress measurement device, and the results are shown in Figure 4. This confirmed that as the flow rate of argon gas introduced into the vacuum chamber 1 in the second step, i.e., the pressure (total pressure) within the vacuum chamber 1, increased, the stress of the tungsten film Ly2 changed from the compressive direction to the tensile direction via the zero point, and then further increased in the tensile direction. It was also confirmed that the tungsten film Ly2 formed by changing the argon gas flow rate was also made up of fine crystals with small grain sizes over the entire in-plane surface of the substrate Sw.
[0023] Furthermore, a substrate Sw on which a tungsten nitride film Ly1 was formed under the conditions of the first step of the above-described invention experiment was used, and in the second step, the input power (DC power) to the tungsten target 3 was set to 6 kW, and the flow rate of argon gas introduced into the vacuum chamber 1 was set to 300 sccm. The bias power input to the substrate Sw from the bias power supply Pb was varied in the range of 0 to 300 W, and a tungsten film Ly2 was formed to a thickness of 195 nm. The stress (MPa) of the tungsten film Ly2 formed by varying the bias power was measured using a thin film stress measurement device, and the results are shown in Figure 5. It was confirmed that as the input bias power increased, the stress of the tungsten film Ly2 changed from the tensile direction to the compressive direction via the zero point, and then further increased in the compressive direction. It was also confirmed that the tungsten film Ly2 formed by varying the bias power was composed of fine crystals with small grain sizes across the entire surface of the substrate Sw.
[0024] Furthermore, a substrate Sw on which a tungsten nitride film Ly1 was formed under the conditions of the first step of the above-mentioned invention experiment was used, and in the second step, the power (DC power) input to the tungsten target 3 was set to 6 kW, the flow rate of argon gas introduced into the vacuum chamber 1 was set to 150 sccm, the pressure inside the vacuum chamber 1 was set to 10 Pa or more, and the bias power input to the substrate Sw from the bias power supply Pb was set to 800 W. The time until impedance matching using the matching box Mb was then varied within a range of 0.5 to 2.0 seconds, and a tungsten film Ly2 was formed to a thickness of 195 nm. The stress (MPa) of the tungsten film Ly2 formed by varying the time until impedance matching was measured using a thin film stress measurement device, and the results are shown in Figure 6. It was confirmed that the stress of the tungsten film Ly2 decreased in the compressive direction when the time until impedance matching was increased. It was also confirmed that the tungsten film Ly2 formed by changing the time until impedance matching was also composed of fine crystals with small grain sizes over the entire surface of the substrate Sw.
[0025] Based on the above findings, by controlling at least one of the total pressure in the vacuum chamber 1 and the bias power supplied to the substrate Sw during film formation in the second step, the stress of the tungsten film Ly2 can be adjusted within a predetermined range (for example, within ±300 MPa, more preferably, within ±100 MPa) depending on its film thickness. Furthermore, when bias power to the substrate Sw is supplied from a bias power supply Pb connected via a matching box Mb, by controlling the time until impedance matching by the matching box Mb, the stress of the tungsten film Ly2 can also be adjusted within a predetermined range depending on its film thickness even when the pressure in the vacuum chamber 1 in the second step is relatively high (for example, 10 Pa or higher).
[0026] Although the embodiments of the present invention have been described above, various modifications are possible without departing from the scope of the technical concept of the present invention. In the above embodiments, the stress of the tungsten film Ly2 is adjusted by individually changing the total pressure in the vacuum chamber 1, the bias power applied to the substrate Sw during film formation, and the time until impedance matching, but the stress of the tungsten film Ly2 can also be adjusted by simultaneously changing two or more of these conditions.
[0027] Mb...matching box, Ly1...tungsten nitride film, Ly2...tungsten film, Pb...bias power supply (AC power supply), Pc...processing chamber, Sw...substrate (substrate to be processed), 3...target.
Claims
1. A method for manufacturing a hard mask comprising: a first step of forming a tungsten nitride film on the surface of a substrate to be processed by reactive sputtering using a tungsten target and introducing a rare gas and nitrogen gas into a processing chamber having a vacuum atmosphere; and a second step of forming a tungsten film on the surface of the tungsten nitride film by sputtering in the processing chamber having a vacuum atmosphere, wherein in the first step, the flow rate ratio of the rare gas to the nitrogen gas is set to 1.5 or less and the pressure in the processing chamber is set to 1 Pa or more; and in the second step, stress according to the thickness of the tungsten film is adjusted by controlling at least one of the total pressure in the processing chamber and the bias power input to the substrate to be processed during film formation.
2. A method for manufacturing a hard mask according to claim 1, in which bias power to the substrate to be processed is supplied from an AC power source connected via a matching box, and the control of the bias power includes the time required for impedance matching by the matching box.
Citation Information
Patent Citations
Method for forming tungsten or tungsten-containing thin film
JP2004270035A
Thin film device and method of manufacturing thin film device
JP2014204214A
Method for fabricating semiconductor device using tungsten as sacrificial hard mask
US20060079093A1