Laminate

The laminate with an organic thin film peeling layer and electroless plating catalyst layer addresses the challenges of thin copper foil handling and environmental concerns by facilitating easy peeling and forming smooth, fine-patterned copper layers for printed wiring boards, enhancing their quality and reducing costs.

WO2024247656A1PCT designated stage expired Publication Date: 2024-12-05NISSAN CHEM CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017383
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-10
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The manufacturing of printed wiring boards faces challenges with the use of thin copper foils, as conventional etching methods often result in trapezoidal cross-sectional shapes due to side etching, leading to surface defects like wrinkles, which can cause short circuits and disconnections. Additionally, the use of chromium in release layers poses environmental concerns and increases manufacturing costs.

Method used

A laminate is developed with a supporting base material, a peeling layer made of an organic thin film, and an electroless plating catalyst layer, where the peeling layer is formed from a composition containing a fluorine-containing polymer and a thermosetting resin, allowing for the easy peeling of an electroless copper layer without chromium, reducing environmental impact and improving the quality of printed wiring boards.

Benefits of technology

The laminate enables the formation of thin electroless copper layers with improved smoothness, reducing side etching and enabling finer wiring patterns while minimizing environmental impact and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017383_05122024_PF_FP_ABST
    Figure JP2024017383_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a laminate which can form a thin copper layer and allows said copper layer to be easily peeled off while achieving a reduction in environmental load, and in which (A) a support substrate, (B) a release layer composed of an organic thin film, and (C) an electroless plating catalyst layer are sequentially laminated.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate

[0001] The present invention relates to laminates for use in the manufacture of printed wiring boards.

[0002] Conventionally, electrolytic copper foils such as those disclosed in Patent Document 1 and rolled copper foils such as those disclosed in Patent Document 2 have been used to manufacture copper-clad laminates, and printed wiring boards have been manufactured by etching the copper layer formed on the copper-clad laminates.

[0003] The manufacturing method of the copper-clad laminate differs between the manufacturing of rigid copper-clad laminates and the manufacturing of flexible copper-clad laminates. When manufacturing rigid copper-clad laminates, a method is generally used in which a book of copper foil, a resin-impregnated substrate (prepreg) in a B-stage (semi-cured) state, and other spacer end plates are stacked in multiple layers, sandwiched between hot plates, and high pressure is applied in a high-temperature atmosphere to cure the resin in the resin-impregnated substrate and simultaneously press-bond the copper foil (hereinafter, this process may be referred to as "pressing"). When manufacturing flexible copper-clad laminates, a method is generally used in which copper foil and an organic polymer insulating layer-forming material such as polyimide are bonded together by hot pressing or roll lamination, or a method is used in which a polyamic resin component is applied to copper foil by a casting method or the like and heated to form a polyimide resin layer.

[0004] Meanwhile, in recent years, electronic devices such as smartphones have become smaller and thinner, and this has led to demands for smaller and thinner internal circuit boards and semiconductor packages. To address this demand, finer patterns of circuit wiring have been developed to achieve higher density wiring, and thin, smooth copper foil is required to form finely shaped circuits. Furthermore, conventional etching methods have the problem of trapezoidal cross-sectional shapes of fine patterns (the occurrence of side etching).

[0005] To meet this demand, those skilled in the art have attempted to use thinner copper foils. However, the thinner the copper foil, the more difficult it is to handle, leading to the increased likelihood of defects such as wrinkles. If wrinkles are present in the copper foil, cracks will form at the wrinkled areas during press molding, causing the constituent resin of the fluidized prepreg to seep out, contaminating the surface of the copper-clad laminate and impairing its surface flatness. These surface defects in the copper-clad laminate can cause short circuits and disconnections in the wiring circuits formed in the subsequent manufacturing process of the printed wiring board. Furthermore, these defects, such as wrinkles, also occur when manufacturing flexible copper-clad laminates. The wrinkles present in the copper foil remain as irregularities on the surface even after the copper-clad laminate is formed, causing similar problems.

[0006] For these reasons, electrolytic copper foils with carrier foils (supporting substrates) have been used to form the copper layers of copper-clad laminates. Electrolytic copper foils with carrier foils can generally be broadly divided into peelable and etchable types. The peelable type involves physically peeling and removing the carrier foil after forming the copper-clad laminate, while the etchable type involves etching and removing the carrier foil after forming the copper-clad laminate. Recently, peelable electrolytic copper foils with carrier foils have become more popular because they do not require an etching process and are therefore more cost-effective. For example, Patent Documents 3 and 4 disclose peelable electrolytic copper foils with carrier foils.

[0007] This peelable electrolytic copper foil with carrier foil has a layer structure in which a release layer is provided between the carrier foil layer (support substrate) and the copper foil layer. It is also required that the carrier foil can be peeled off with an appropriate peel strength even after being subjected to the heat history of press processing. In the production process of printed wiring boards, when an ultrathin copper foil (copper layer) is laminated (transferred) onto a resin substrate by high-temperature pressing to produce a seed layer for printed wiring boards (a resin substrate and a copper layer laminated together), if the release layer between the carrier foil layer and the copper foil layer has poor heat resistance, appropriate peelability cannot be obtained, and part of the carrier foil may tear off and remain on the surface of the copper foil layer, or the carrier foil layer and the copper foil layer may not be peeled off.

[0008] As a technology relating to a carrier foil-attached copper foil that allows easy peeling of the carrier foil during press working, Patent Document 3 discloses a composite material having a carrier strip, an electrodeposited copper foil layer deposited from a copper-containing alkaline electrolyte, and a release layer disposed between the carrier strip and the copper foil layer to facilitate peeling of the copper foil layer from the carrier strip. Patent Document 4 discloses an ultrathin copper foil with a carrier, which is characterized by having a release layer, a diffusion barrier layer, and an electroplated copper layer laminated in this order on the surface of a carrier foil, and the surface of the electroplated copper layer being roughened.

[0009] However, Patent Documents 3 and 4 state that the release layer preferably contains chromium, chromium oxide, or chromium hydroxide (hereinafter, these may be collectively referred to simply as "chromium"). Patent Document 4 specifically states that the peel strength when peeling the carrier foil is significantly affected by the amount of chromium layer deposited. However, as is well known to those skilled in the art, controlling the amount of chromium deposited is difficult in mass production, which tends to increase manufacturing management costs. Furthermore, chromium is a restricted substance under the European Directive on Environmental Pollutants (WEEE / RoHS), and its active use is not recommended.

[0010] Therefore, in the production of the ultra-thin copper foil with a carrier, it is required to reduce the amount of chromium used from the viewpoint of reducing the environmental load. Furthermore, from the viewpoint of improving the productivity and quality of printed wiring boards, it is required to be able to form a thin copper foil (copper layer) and to be able to easily peel off the copper foil (copper layer) during press processing.

[0011] JP-A No. 10-18075 JP-A No. 8-158027 Special Publication No. 2005-502496 International Publication No. 2002 / 024444

[0012] The present invention has been made in view of the above circumstances, and aims to provide a laminate that can form a thin copper layer while reducing the environmental load and that can easily peel off the copper layer.

[0013] As a result of intensive research to achieve the above object, the present inventors have found that in a laminate having a release layer formed on a supporting substrate, by making the release layer an organic thin film, the release layer does not contain chromium, thereby realizing a reduction in environmental load, and by further laminating an electroless plating catalyst layer thereon, it is possible to form a thin copper layer (electroless copper layer) by applying an electroless plating process to form the copper layer. They have also found that the release layer is easily peeled off at the interface with the electroless plating catalyst layer, and that the electroless copper layer can be transferred to a resin substrate for a printed wiring board without generating wrinkles or the like during press processing, thereby completing the present invention.

[0014] That is, the present invention provides the following laminates: 1. A laminate comprising (A) a support substrate, (B) a release layer made of an organic thin film, and (C) an electroless plating catalyst layer laminated in this order. 2. The laminate of 1, in which (D) an electroless copper layer is further laminated on the (C) electroless plating catalyst layer. 3. The laminate of 2, in which the (A) support substrate is a plastic support substrate. 4. The laminate of 2, in which the (B) release layer made of an organic thin film is a release layer obtained from a composition for forming a release layer containing a fluorine-containing polymer and a thermosetting resin. 5. The laminate of 4, in which the thermosetting resin is made of polyurea and a crosslinking agent. 6. The laminate of 5, in which the polyurea contains a repeating unit represented by the following formula (U1): [In the formula, A u1 , A u2 , A u3 , A u4 , A u5 and A u6 are each independently a hydrogen atom, a methyl group, or an ethyl group; u1 is a group represented by the following formula (U1-1), (U1-2), (U1-3) or (U1-4), (In the formula, R u1 and R u2are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, and the phenyl group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms; and R u1 and R u2 may be bonded to each other to form a ring having 3 to 6 carbon atoms together with the carbon atoms to which they are bonded, and R u3 represents an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, and the phenyl group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms. u1 is a group represented by the following formula (U1-5) or (U1-6). (In the formula, X u2 is a group represented by formula (U1-1), formula (U1-2) or formula (U1-4), and Q u2 represents an alkylene group having 1 to 10 carbon atoms, a phenylene group, a naphthylene group, or an anthrylene group, and the phenylene group, naphthylene group, and anthrylene group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms; u1 and n u2 are each independently 0 or 1. 7. The laminate of 4, wherein the fluorine-containing polymer is a polymer containing a repeating unit represented by the following formula (a1), a repeating unit represented by the following formula (b), and a repeating unit represented by the following formula (c): (In the formula, R A are each independently a hydrogen atom or a methyl group, and R B1 is a branched alkyl group having 3 or 4 carbon atoms in which at least one hydrogen atom is substituted with a fluorine atom, and R Cis an alkyl group having 1 to 10 carbon atoms and a hydroxy group or a polycyclic alkyl group having 6 to 20 carbon atoms and a hydroxy group, and R D is an alkyl group having 1 to 10 carbon atoms which may be substituted with a polycyclic alkyl group having 6 to 20 carbon atoms, a polycyclic alkyl group having 6 to 20 carbon atoms, or an aryl group having 6 to 12 carbon atoms.) 8. The laminate of 2, wherein the electroless plating catalyst layer (C) contains a polymer having an alkoxy group, a hydroxy group, an ammonium group, a carboxy group, or a cyano group, and metal fine particles. 9. The laminate of 8, wherein the metal fine particles are palladium fine particles. 10. The laminate of 8, wherein the polymer is a hyperbranched polymer. 11. The laminate of 10, wherein the hyperbranched polymer is a hyperbranched polymer represented by formula [1] and having a weight average molecular weight of 500 to 5,000,000. [In the formula, R 1 are each independently a hydrogen atom or a methyl group, 2 , R 3 and R 4 are each independently a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, an arylalkyl group having 7 to 20 carbon atoms, or —(CHCHO) m R 5 (In the formula, R 5 represents a hydrogen atom or a methyl group, and m represents an integer of 2 to 100; the alkyl group and arylalkyl group may be substituted with an alkoxy group, a hydroxy group, an ammonium group, a carboxy group, or a cyano group; 2 , R 3 and R 4 two groups together represent a linear, branched or cyclic alkylene group, or R 2 , R 3 and R 4 and may form a ring together with the nitrogen atom to which they are attached, - is an anion, n is an integer from 2 to 100,000, and A 1 is a structure represented by the following formula [2]. (In the formula, A 2represents a linear, branched or cyclic alkylene group having 1 to 30 carbon atoms which may contain an ether bond or an ester bond; Y 1 , Y 2 , Y 3 and Y 4 are each independently a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a nitro group, a hydroxy group, an amino group, a carboxyl group, or a cyano group. 12. A laminate according to claim 10, in which the metal fine particles and the hyperbranched polymer form a composite. 13. A laminate according to claim 10, in which the hyperbranched polymer is a hyperbranched polymer represented by formula [3] and has a weight average molecular weight of 500 to 5,000,000. (In the formula, R 1 , R 2 , R 3 , R 4 and n are the same as above.) 14. A method for producing a laminate as recited in any one of 2 to 13, comprising the steps of: (A) forming a release layer composed of (B) an organic thin film on a supporting substrate; and (C) forming an electroless plating catalyst layer on the release layer composed of (B) the organic thin film. 15. A method for producing a laminate as recited in 14, further comprising the step of forming an electroless copper layer (D) on the electroless plating catalyst layer (C). 16. A method for producing a seed layer for a printed wiring board, comprising: pressing the (D) electroless copper layer of the laminate as recited in any one of 2 to 13 onto a resin substrate, peeling off the (A) supporting substrate, and transferring the (D) electroless copper layer to the resin substrate. 17. A method for producing a seed layer for a printed wiring board, comprising: pressing the (D) electroless copper layer of the laminate as recited in any one of 2 to 13 onto a resin substrate, peeling off the (A) supporting substrate, and transferring the (D) electroless copper layer to the resin substrate, and then removing the (C) electroless plating catalyst layer with a palladium etching solution. 18. 19. A method for producing a seed layer for a printed wiring board according to 16 or 17, wherein when peeling off the (A) supporting substrate, peeling occurs at the interface between the (B) release layer made of an organic thin film and the (C) electroless plating catalyst layer. 19. A method for producing a printed wiring board using the seed layer for a printed wiring board according to 16 or 17.

[0015] The laminate of the present invention does not contain chromium in the release layer, and a thin electroless copper layer can be formed by applying an electroless plating process. This allows for the production of an electroless copper layer laminate suitable for forming fine patterns while reducing the environmental impact. Furthermore, since the release layer is easily peeled off at the interface with the electroless plating catalyst layer, the thin electroless copper layer can be transferred to the resin substrate side of the printed wiring board during press processing without causing wrinkles or the like. As a result, a seed layer for printed wiring boards suitable for forming fine patterns can be obtained with good reproducibility. Furthermore, since the resulting seed layer for printed wiring boards has a thin electroless copper layer, the amount of copper used can be reduced. In addition, side etching during flash etching in the wiring formation process of the printed wiring board is reduced, resulting in finer wiring. Furthermore, by using a plastic support substrate, the smoothness of the electroless copper layer is significantly improved compared to when a conventional copper plate is used as the support substrate, allowing for the formation of printed wiring boards with low transmission loss in the high frequency band.

[0016] Fig. 1 is a cross-sectional view showing an example of a laminate according to the present invention. Fig. 2 is a cross-sectional view showing an example of an electroless copper layer laminate according to the present invention. Fig. 3 is a diagram showing a manufacturing process flow for a printed wiring board using the electroless copper layer laminate of the present invention. Fig. 4 is a diagram showing a manufacturing process flow for removing an electroless plating catalyst layer in the manufacturing process flow for a printed wiring board using the electroless copper layer laminate of the present invention. Fig. 5 is a transmission electron microscope image of Pd particles obtained in Synthesis Example 2-3. Fig. 6 is a transmission electron microscope image of Pd particles obtained in Synthesis Example 2-5.

[0017] The present invention will be described in more detail below. Figure 1 shows an example of the cross-sectional structure of the laminate of the present invention. As shown in Figure 1, the laminate 10 of the present invention is obtained by sequentially stacking (A) a supporting substrate 11, (B) a release layer 12 made of an organic thin film, and (C) an electroless plating catalyst layer 13. Furthermore, by using the laminate 10, it is also possible to provide a laminate 1 (hereinafter sometimes referred to as "electroless copper layer laminate 1") in which (A) a supporting substrate 11, (B) a release layer 12 made of an organic thin film, (C) an electroless plating catalyst layer 13, and (D) an electroless copper layer 14 are sequentially stacked (see Figure 2).

[0018] (A) Support substrate 11 The support substrate 11 can be appropriately selected from known materials and is not particularly limited, but specific examples include metal foils such as foils of copper, aluminum, iron, gold, silver, nickel, palladium, molybdenum, or alloys thereof; and plastic support substrates such as polyimide, polyetherimide, polyamideimide, polyethylene terephthalate (PET), polyethylene naphthalate, polycarbonate, polyphenylene ether, polyphenylene sulfide, and polyether ether ketone. In the present invention, a plastic support substrate is preferred because it can be expected to reduce the amount of metal used, reduce weight, and improve flatness, and there is no deterioration over time due to oxidation. Furthermore, in consideration of heat resistance, polyimide or polyethylene terephthalate is more preferred.

[0019] There are no particular restrictions on the thickness of the support substrate 11, but it should be adjusted appropriately to a thickness that is suitable for fulfilling the role of the support substrate, and is generally 5 to 100 μm. From the viewpoint of reducing weight and raw material costs, a small thickness of the plastic support substrate is preferable; if the thickness of the plastic support substrate is too small, the handleability of the carrier-attached ultra-thin copper foil decreases. Therefore, the thickness of the carrier is preferably 5 to 100 μm, more preferably 10 to 50 μm.

[0020] Commercially available products can be used as the support substrate 11. For example, commercially available polyimide products include the "Kapton (registered trademark)" series of polyimide films manufactured by Toray Industries, Inc. Commercially available polyethylene terephthalate products include the "Cosmoshine (registered trademark)" series of polyethylene terephthalate films manufactured by Toyobo Co., Ltd., the "Tetoron (registered trademark)" series (currently "Toyobo Ester (registered trademark) Film" manufactured by Toyobo Co., Ltd.) manufactured by Teijin Limited, and the "Lumirror" series of polyethylene terephthalate films manufactured by Toray Industries, Inc.

[0021] (B) Release Layer 12 Made of Organic Thin Film The release layer 12 made of an organic thin film (hereinafter sometimes simply referred to as "release layer") is a layer that has excellent adhesion to the support substrate 11 and adequate adhesion and release properties to the electroless plating catalyst layer 13, and serves to properly fix the electroless copper layer 14 formed by electroless plating treatment to the support substrate 11, and to release the electroless copper layer 14 together with the electroless plating catalyst layer 13 from the support substrate 11 during press working. Furthermore, the release layer 12 is made of an organic thin film and does not contain chromium, which has conventionally been used to form release layers, and is therefore expected to reduce environmental impact.

[0022] The release layer 12 is preferably obtained from a release layer-forming composition containing a thermosetting resin and a fluorine-containing polymer.

[0023] [Thermosetting Resin] Examples of the thermosetting resin include polyurea resin, polyacrylic resin, polyimide resin, melamine resin, epoxy resin, phenol resin, unsaturated polyester resin, vinyl ester resin, polyurethane resin, and silicone resin, with polyurea resin being preferred.

[0024] The polyurea resin is made from polyurea and a crosslinking agent as raw materials. In the present invention, the polyurea preferably contains a repeating unit represented by the following formula (U1) because it has excellent heat resistance.

[0025]

[0026] In formula (1), Au1 , A u2 , A u3 , A u4 , A u5 and A u6 are each independently a hydrogen atom, a methyl group, or an ethyl group. From the viewpoint of releasability and productivity, A u1 ~A u6 are preferably all hydrogen atoms.

[0027] In formula (1), X u1 is a group represented by the following formula (U1-1), (U1-2), (U1-3) or (U1-4).

[0028] In formulas (U1-1) and (U1-2), R u1 and R u2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, and the phenyl group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms; and R u1 and R u2 may be bonded to each other to form a ring having 3 to 6 carbon atoms together with the carbon atoms to which they are attached.

[0029] In formula (U1-3), R u3 represents an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, and the phenyl group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms.

[0030] Q u1 is a group represented by the following formula (U1-5) or (U1-6).

[0031]

[0032] In formula (U1-5), X u2is a group represented by formula (U1-1), formula (U1-2) or formula (U1-4). u1 and n u2 are each independently 0 or 1.

[0033] In the above formula (U1-5), for example, X u2 is a group represented by formula (U1-2), the structure is represented by formula (U1-5-1).

[0034] (In the formula, R u1 and R u2 is the same as above.)

[0035] In formula (U1-6), Q u2 is an alkylene group having 1 to 10 carbon atoms, a phenylene group, a naphthylene group, or an anthrylene group. The phenylene group, naphthylene group, and anthrylene group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms. u2 is a phenylene group, a naphthylene group, or an anthrylene group, the bonding positions thereof are not particularly limited. That is, for example, the phenylene group may be bonded at the 1st and 2nd positions, or at the 1st and 3rd positions, or at the 1st and 4th positions, the naphthylene group may be bonded at the 1st and 2nd positions, or at the 1st and 4th positions, or at the 1st and 5th positions, or at the 2nd and 3rd positions, and the anthrylene group may be bonded at the 1st and 2nd positions, or at the 1st and 4th positions, or at the 9th and 10th positions, and any of these may be acceptable.

[0036] The alkyl group having 1 to 6 carbon atoms may be linear, branched, or cyclic, and examples thereof include a methyl group, an ethyl group, an isopropyl group, an n-butyl group, a cyclohexyl group, etc. The alkenyl group having 3 to 6 carbon atoms may be linear, branched, or cyclic, and examples thereof include a 2-propenyl group, a 3-butenyl group, etc.

[0037] The alkoxy group having 1 to 6 carbon atoms may be linear, branched, or cyclic, and examples thereof include a methoxy group, an ethoxy group, an isopropoxy group, an n-pentyloxy group, and a cyclohexyloxy group. The alkylthio group having 1 to 6 carbon atoms may be linear, branched, or cyclic, and examples thereof include a methylthio group, an ethylthio group, an isopropylthio group, an n-pentylthio group, and a cyclohexylthio group. The halogen atom may include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. In addition, R u1 and R u2 Examples of the ring having 3 to 6 carbon atoms formed by bonding include a cyclobutane ring, a cyclopentane ring, and a cyclohexane ring.

[0038] The alkylene group having 1 to 10 carbon atoms may be linear, branched, or cyclic, and examples thereof include a methylene group, an ethylene group, a propylene group, a pentamethylene group, a cyclohexylene group, and a 2-methylpropylene group.

[0039] In addition, in formula (U1), X u1 is a group represented by formula (U1-2), the structure is represented by formula (U2) below, u1 When R is a group represented by formula (U1-3), the structure is represented by formula (U3) below. u3 However, it is preferably a 2-propenyl group.

[0040] (In the formula, A u1 ~A u6 , R u1 ~R u3 and Q u1 is the same as above.)

[0041] In formula (U1), Q u1 Preferably, Q contains a cyclic structure from the viewpoint of the heat resistance of the polyurea of ​​the component (A). u1 is a group represented by formula (U1-5) or a group represented by formula (U1-6), and Q u2is preferably a cyclic alkylene group, a phenylene group, a naphthylene group or an anthrylene group, and more preferably a group represented by formula (U1-5).

[0042] The repeating unit represented by formula (U1) is preferably one represented by the following formulae (U4) to (U22): In the following formulae, Me is a methyl group, and Et is an ethyl group.

[0043]

[0044]

[0045]

[0046]

[0047]

[0048] The polyurea can be synthesized, for example, by referring to International Publication No. 2005 / 098542.

[0049] The weight average molecular weight (Mw) of the polyurea is preferably 1,000 to 200,000, more preferably 3,000 to 100,000, even more preferably 4,000 to 30,000, and even more preferably 5,000 to 20,000. The dispersity (Mw / Mn) is preferably 1.3 to 4.0, more preferably 1.4 to 2.5. Mn is the number average molecular weight, and Mw and Mn are values ​​measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0050] The crosslinking agent may be any known crosslinking agent, and is not particularly limited. In the present invention, from the viewpoint of reaction rate, it is preferable to use a crosslinking agent selected from compounds having a nitrogen atom substituted with a hydroxyalkyl group and / or an alkoxymethyl group.

[0051] The crosslinking agent is preferably a compound represented by any one of the following formulas (C-1) to (C-5).

[0052]

[0053] In the formula, R 11 ~R26 are each independently a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, preferably an alkyl group having 1 to 6 carbon atoms. 27 is a hydrogen atom or a methyl group.

[0054] Specific examples of the crosslinking agent include nitrogen-containing compounds such as hexamethylolmelamine, tetramethylolbenzoguanamine, 1,3,4,6-tetramethylolglycoluril, hexamethoxymethylmelamine, tetramethoxymethylbenzoguanamine, 1,3,4,6-tetrakis(methoxymethyl)glycoluril, 1,3,4,6-tetrakis(butoxymethyl)glycoluril, and 1,3,4,6-tetrakis(hydroxymethyl)glycoluril.

[0055] Other examples of commercially available nitrogen-containing compounds include methoxymethyl-type melamine compounds (trade names: Cymel (registered trademark) 300, Cymel 301, Cymel 303, Cymel 350), butoxymethyl-type melamine compounds (trade names: Mycoat (registered trademark) 506, Mycoat 508), glycoluril compounds (trade names: Cymel 1170, Powderlink 1174), methylated urea resins (trade names: UFR65), butylated urea resins (trade names: UFR300, U-VAN10S60, U-VAN10R, U-VAN11HV), and urea / formaldehyde resins (trade names: Beckamine (registered trademark) J-300S, Beckamine P-955, Beckamine N) manufactured by Allnex Corporation.

[0056] Also usable as the crosslinking agent are polymers produced using (meth)acrylamide compounds substituted with hydroxymethyl groups or alkoxymethyl groups, such as N-hydroxymethyl(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-ethoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide. Examples of such polymers include poly(N-butoxymethyl(meth)acrylamide), copolymers of N-butoxymethyl(meth)acrylamide and styrene, copolymers of N-hydroxymethyl(meth)acrylamide and methyl(meth)acrylate, copolymers of N-ethoxymethylmethacrylamide and benzyl methacrylate, and copolymers of N-butoxymethyl(meth)acrylamide, benzyl(meth)acrylate, and 2-hydroxypropyl(meth)acrylate.

[0057] More preferred examples of the crosslinking agent include hexamethoxymethylmelamine, tetramethoxymethylbenzoguanamine, 1,3,4,6-tetrakis(methoxymethyl)glycoluril (POWDERLINK 1174), 1,3,4,6-tetrakis(butoxymethyl)glycoluril, and 1,3,4,6-tetrakis(hydroxymethyl)glycoluril.

[0058] These crosslinking agents can undergo a crosslinking reaction by self-condensation, and can also undergo a crosslinking reaction with the hydroxyl groups in the polyurea. This crosslinking reaction makes the resulting release layer 12 strong and less soluble in organic solvents.

[0059] The content of the crosslinking agent is preferably 10 to 100 parts by mass, more preferably 20 to 50 parts by mass, per 100 parts by mass of the polyurea. When the content of the crosslinking agent is within the above range, a composition can be obtained that can provide a release layer 12 that has appropriate releasability and excellent stability after film formation. The crosslinking agents may be used alone or in combination of two or more.

[0060] [Fluorine-containing polymer] As the fluorine-containing polymer, known ones can be used, and are not particularly limited.Specific examples include the fluorine polymers described in WO 2020 / 158521 and WO 2021 / 132383, but in the present invention, a polymer containing a repeating unit represented by the following formula (a1), a repeating unit represented by the following formula (b) and a repeating unit represented by the following formula (c) is preferred.

[0061]

[0062] In the formula, R A are each independently a hydrogen atom or a methyl group. B1 R is a branched alkyl group having 3 or 4 carbon atoms in which at least one hydrogen atom is substituted with a fluorine atom. C is an alkyl group having 1 to 10 carbon atoms and a hydroxy group, or a polycyclic alkyl group having 6 to 20 carbon atoms and a hydroxy group. D represents an alkyl group having 1 to 10 carbon atoms which may be substituted with a polycyclic alkyl group having 6 to 20 carbon atoms, a polycyclic alkyl group having 6 to 20 carbon atoms, or an aryl group having 6 to 12 carbon atoms.

[0063] Examples of the branched alkyl group having 3 or 4 carbon atoms include an isopropyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. B1 As the branched alkyl group, those in which at least one hydrogen atom has been substituted with a fluorine atom are preferred, and specific examples include a 1,1,1-trifluoroisopropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group, and a nonafluorotert-butyl group.

[0064] Examples of the alkyl group having 1 to 10 carbon atoms and having a hydroxy group include a hydroxymethyl group, a 2-hydroxyethyl group, a 3-hydroxypropyl group, a 4-hydroxybutyl group, a 5-hydroxypentyl group, a 6-hydroxyhexyl group, a 7-hydroxyheptyl group, an 8-hydroxyoctyl group, a 9-hydroxynonyl group, a 10-hydroxydecyl group, a 2-hydroxy-1-methylethyl group, a 2-hydroxy-1,1-dimethylethyl group, a 3-hydroxy-1-methylpropyl group, a 3-hydroxy-2-methylpropyl group, a 3-hydroxy-1,1-dimethylpropyl group, a 3-hydroxy-1,2-dimethylpropyl group, a 3-hydroxy-2,2-dimethylpropyl group, a 4-hydroxy-1-methylbutyl group, a 4-hydroxy hydroxyalkyl groups having 2 to 10 carbon atoms, such as 1-hydroxyethyl group, 1-hydroxypropyl group, 2-hydroxypropyl group, 1-hydroxybutyl group, 2-hydroxybutyl group, 1-hydroxyhexyl group, 2-hydroxyhexyl group, 1-hydroxyoctyl group, 2-hydroxyoctyl group, 1-hydroxydecyl group, 2-hydroxydecyl group, 1-hydroxy-1-methylethyl group, and 2-hydroxy-2-methylpropyl group, wherein the carbon atom to which the hydroxy group is bonded is a secondary or tertiary carbon atom.

[0065] Examples of the polycyclic alkyl group having 6 to 20 carbon atoms include a 1-adamantyl group, a 2-adamantyl group, an isobornyl group, a norbornyl group, etc. Examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-biphenyl group, a 2-biphenyl group, etc.

[0066] Examples of the polycyclic alkyl group having 6 to 20 carbon atoms and having a hydroxy group include a 3-hydroxy-1-adamantyl group, a 4-hydroxy-1-adamantyl group, a 5-hydroxy-1-adamantyl group, a 3-hydroxy-2-adamantyl group, a 4-hydroxy-2-adamantyl group, a 5-hydroxy-2-adamantyl group, and a hydroxynorbornyl group. Examples of the aryl group having 6 to 12 carbon atoms and having a hydroxy group include a 4-hydroxyphenyl group and a 3-hydroxyphenyl group.

[0067] The fluorine-containing polymer may also contain a repeating unit represented by the following formula (a2), a repeating unit represented by the following formula (b), a repeating unit represented by the following formula (c), and a repeating unit represented by the following formula (d):

[0068]

[0069] In the formula, R A , R C and R D is the same as above. B2 is a branched alkyl group having 3 or 4 carbon atoms in which at least one hydrogen atom has been substituted with a fluorine atom (excluding 2-methyl-1,1,1,3,3,3-hexafluoroisopropyl group). Examples of the branched alkyl group having 3 or 4 carbon atoms include the same as those mentioned above. R E is a single bond, a polycyclic alkylene group having 6 to 20 carbon atoms, or an arylene group having 6 to 12 carbon atoms. F is a single bond or an alkylene group having 1 to 10 carbon atoms. G is a methyl group, an ethyl group, or a hydroxy group.

[0070] Examples of the polycyclic alkylene group having 6 to 20 carbon atoms include groups in which one hydrogen atom has been removed from the specific examples of the polycyclic alkyl group having 6 to 20 carbon atoms described above, such as an adamantylene group, an isobornylene group, and a norbornylene group.

[0071] Examples of the arylene group having 6 to 12 carbon atoms include groups in which one hydrogen atom has been removed from the specific examples of the aryl group having 6 to 12 carbon atoms described above, such as a phenylene group, a naphthylene group, and a biphenylylene group.

[0072] The alkylene group having 1 to 10 carbon atoms includes the above-mentioned Q u2 In the present invention, alkylene groups having 1 to 5 carbon atoms are preferred, methylene groups and ethylene groups are more preferred, and methylene groups are even more preferred.

[0073] Examples of the repeating unit represented by formula (a1) or (a2) include, but are not limited to, those represented by the following formulae (a-1) to (a-3). A is the same as above.

[0074]

[0075] Examples of the repeating unit represented by formula (b) include, but are not limited to, those represented by the following formulas (b-1) to (b-17). A is the same as above.

[0076]

[0077] Examples of the repeating unit represented by formula (c) include, but are not limited to, those represented by the following formulae (c-1) to (c-15). A is the same as above.

[0078]

[0079] Examples of the repeating unit represented by formula (d) include, but are not limited to, those represented by the following formulae (d-1) to (d-8). A is the same as above.

[0080]

[0081] When the fluorine-containing polymer contains a repeating unit represented by formula (a1), a repeating unit represented by formula (b), and a repeating unit represented by formula (c), and the carbon atom to which the hydroxy group in the hydroxyalkyl group in the repeating unit represented by formula (b) is bonded is a secondary or tertiary carbon atom (hereinafter, such a fluorine-containing polymer will be referred to as fluorine-containing polymer D1), the content of the repeating unit represented by formula (a1) is preferably 30 to 60 mol%, more preferably 35 to 50 mol%, of all repeating units. The content of the repeating unit represented by formula (b) is preferably 10 to 35 mol%, more preferably 15 to 30 mol%, of all repeating units. The content of the repeating unit represented by formula (c) is preferably 5 to 60 mol%, more preferably 20 to 50 mol%, of all repeating units.

[0082] The fluorine-containing polymer contains a repeating unit represented by formula (a1), a repeating unit represented by formula (b), and a repeating unit represented by formula (c), and when the carbon atom to which the hydroxy group in the hydroxyalkyl group in the repeating unit represented by formula (b) is bonded is a primary carbon atom (hereinafter, such a fluorine-containing polymer will be referred to as fluorine-containing polymer D2), the content of the repeating unit represented by formula (a1) is preferably 15 to 60 mol%, more preferably 25 to 60 mol%, even more preferably 30 to 60 mol%, and still more preferably 35 to 50 mol% of all repeating units. The content of the repeating unit represented by formula (b) is preferably 8 to 38 mol%, preferably 10 to 38 mol%, more preferably 10 to 35 mol%, and still more preferably 15 to 30 mol% of all repeating units. The content of the repeating unit represented by formula (c) is preferably 2 to 77 mol%, more preferably 2 to 65 mol%, even more preferably 5 to 60 mol%, and still more preferably 20 to 50 mol% of all repeating units.

[0083] When the fluorine-containing polymer contains a repeating unit represented by formula (a2), a repeating unit represented by formula (b), a repeating unit represented by formula (c), and a repeating unit represented by formula (d) (hereinafter, such a fluorine-containing polymer will be referred to as fluorine-containing polymer D3), the content of the repeating unit represented by formula (a2) is preferably 2 to 45 mol%, more preferably 5 to 35 mol%, of all repeating units. The content of the repeating unit represented by formula (b) is preferably 20 to 35 mol%, more preferably 25 to 35 mol%, of all repeating units. The content of the repeating unit represented by formula (c) is preferably 30 to 45 mol%, more preferably 35 to 45 mol%, of all repeating units. The content of the repeating unit represented by formula (d) is preferably 5 to 18 mol%, more preferably 5 to 15 mol%, of all repeating units.

[0084] The Mw of the fluorine-containing polymer is preferably from 2,000 to 10,000, more preferably from 3,000 to 6,000, and the Mw / Mn is preferably from 1.0 to 2.1, more preferably from 1.0 to 1.9.

[0085] The content of the fluorine-containing polymer is 5 to 100 parts by mass relative to 100 parts by mass of the polyurea. By setting the content of the fluorine-containing polymer within this range, good coating properties and appropriate releasability can be obtained.

[0086] When the fluorine-containing polymer is fluorine-containing polymer D1, the content thereof is preferably 10 to 100 parts by mass, more preferably 20 to 100 parts by mass, and even more preferably 30 to 100 parts by mass, relative to 100 parts by mass of the polyurea. When the fluorine-containing polymer is a polymer other than fluorine-containing polymer D1, the content thereof is preferably 5 to 80 parts by mass, more preferably 5 to 50 parts by mass, relative to 100 parts by mass of the polyurea.

[0087] The fluorine-containing polymers may be used alone or in combination of two or more.

[0088] [Acid Compound or Salt thereof] The release layer-forming composition of the present invention may contain an acid compound or a salt thereof. Examples of the acid compound include sulfonic acid compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate, salicylic acid, camphorsulfonic acid, sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, dodecylbenzenesulfonic acid, 1-naphthalenesulfonic acid, and pyridinium 1-naphthalenesulfonic acid, and carboxylic acid compounds such as salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, and hydroxybenzoic acid. Examples of salts of the acid compounds include pyridinium salts, isopropanolamine salts, and N-methylmorpholine salts of the above acids. Specific examples include pyridinium p-toluenesulfonate, pyridinium 1-naphthalenesulfonate, isopropanolamine p-toluenesulfonate, and N-methylmorpholine p-toluenesulfonate.

[0089] When the release layer-forming composition contains an acid compound or a salt thereof, the content thereof is preferably 0.01 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the polyurea. When the content of the acid compound or a salt thereof is within the above range, a composition can be obtained that can provide a release layer 12 that has high heat resistance and appropriate release properties and is excellent in stability after film formation. The acid compound or a salt thereof may be used alone or in combination of two or more types.

[0090] [Solvent] The release layer-forming composition may contain a solvent. The solvent is not particularly limited in type, structure, etc., as long as it can dissolve the above-mentioned components and other additives described later, but in the present invention, glycol ether-based solvents having 3 to 20 carbon atoms, ester-based solvents having 3 to 20 carbon atoms, ketone-based solvents having 3 to 20 carbon atoms, or cyclic compound-based solvents having 3 to 20 carbon atoms are preferred.

[0091] Examples of the glycol ether solvents include propylene glycol monomethyl ether (PGME), propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether, propylene glycol monobutyl ether, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol monomethyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether (Diglyme), diethylene glycol diethyl ether, and diethylene glycol monomethyl ether. monohexyl ether, diethylene glycol butyl methyl ether, triethylene glycol monomethyl ether, triethylene glycol dimethyl ether (Triglyme), diethylene glycol monobutyl ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, diethylene glycol dibutyl ether, dimethoxytetraethylene glycol, dipropylene glycol methyl ether, dipropylene glycol dimethyl ether, dipropylene glycol monomethyl ether, diethylene glycol monoethyl ether acetate (DEGEEA), methoxymethyl butanol, tripropylene glycol dimethyl ether, triethylene glycol butyl methyl ether, and the like.

[0092] Examples of the ester solvent include ethyl acetate, propyl acetate, butyl acetate, isobutyl acetate, ethyl lactate, γ-butyrolactone, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, methyl methoxypropionate, and ethyl ethoxypropionate.

[0093] Examples of the ketone solvent include methyl ethyl ketone, cyclohexanone, cyclopentanone, and benzophenone.

[0094] Examples of the cyclic compound solvent include N-methylpyrrolidone and γ-butyrolactone.

[0095] When the release layer-forming composition contains a solvent, the content thereof is preferably an amount such that the solids concentration in the release layer-forming composition of the present invention is 0.1 to 40% by mass, more preferably 0.5 to 20% by mass, and even more preferably 0.5 to 10% by mass. The solids are a collective term for all components of the release layer-forming composition other than the solvent. The solvents may be used alone or in combination of two or more.

[0096] [Other Additives] The release layer-forming composition may contain a surfactant as needed. By adding a surfactant, the coatability of the release layer-forming composition on the substrate can be improved. As the surfactant, known surfactants such as nonionic surfactants, fluorine-based surfactants, and silicone-based surfactants can be used.

[0097] Specific examples of the nonionic surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether; polyoxyethylene-polyoxypropylene block copolymers; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; and polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate.

[0098] Examples of the fluorine-based surfactants and the like include EFTOP (registered trademark) EF301, EF303, EF352 (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), MEGAFAC (registered trademark) F171, F173, F554, F559, F563, R-30, R-40, R-40-LM, DS-21 (manufactured by DIC Corporation), FLUORAD (registered trademark) FC430, FC431 (manufactured by 3M), ASAHIGUARD (registered trademark) AG710, SURFLOON (registered trademark) S-382, SC101, SC102, SC103, SC104, SC105, SC106 (manufactured by AGC Inc.), and the like.

[0099] Furthermore, examples of silicone surfactants include organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0100] When the release layer-forming composition contains a surfactant, the content thereof is preferably 0.0001 to 1 part by mass, and more preferably 0.001 to 0.5 parts by mass, relative to 100 parts by mass of the polyurea. The surfactant may be used alone or in combination of two or more.

[0101] In addition, the above-mentioned release layer forming composition may contain other additives such as silane coupling agents, rheology adjusters, pigments, dyes, storage stabilizers, antifoaming agents, antioxidants, etc., as long as the effects of the present invention are not impaired.

[0102] <Preparation of Release Layer-Forming Composition> The method for preparing the release layer-forming composition is not particularly limited. Examples of the preparation method include a method of mixing a crosslinking agent, a fluorine-containing polymer, an acid compound or its salt, and a solvent in a predetermined ratio with a solution of polyurea dissolved in a solvent to prepare a homogeneous solution, and a method of further adding and mixing other additives as necessary at an appropriate stage of the preparation method.

[0103] In preparing the above-mentioned release layer forming composition, the solution of specific copolymer (polymer) obtained by polymerization reaction in solvent can be used as it is.In this case, for example, in the solution of polyurea, similarly as above, acid compound or its salt, further crosslinking agent, fluorine-containing polymer, solvent etc. are added to make a uniform solution.At this time, for the purpose of concentration adjustment, can also add solvent.At this time, the solvent used in the process of generating polyurea and the solvent used for adjusting the concentration of release layer forming composition can be the same or different.

[0104] The prepared solution of the composition for forming the release layer is preferably used after being filtered using a filter having a pore size of about 0.2 μm.

[0105] The viscosity of the composition for forming the release layer is set appropriately taking into consideration the thickness of the release layer 12 to be produced, etc., but when the aim is to reproducibly obtain a film having a thickness of about 0.01 to 5 μm, the viscosity is usually about 1 to 5,000 mPa·s at 25°C, and preferably about 1 to 2,000 mPa·s.

[0106] Here, the viscosity can be measured using a commercially available viscometer for measuring the viscosity of liquids, for example, by referring to the procedure described in JIS K7117-2, at a composition temperature of 25°C. Preferably, a cone-plate type rotational viscometer is used as the viscometer, and preferably the same type of viscometer is used with a 1°34' x R24 standard cone rotor, and the viscosity can be measured at a composition temperature of 25°C. An example of such a rotational viscometer is the TVE-25L manufactured by Toki Sangyo Co., Ltd.

[0107] <Formation of release layer 12 consisting of organic thin film> A baking method including a step of applying the above-mentioned release layer-forming composition onto a support substrate 11 and then baking at 180 to 250°C can obtain a release layer 12 that has excellent adhesion to the support substrate 11 and moderate adhesion and releasability to the electroless plating catalyst layer 13.

[0108] The heating time cannot be generally specified because it varies depending on the heating temperature, but is usually 1 minute to 5 hours. As long as the maximum temperature during the baking is within the above range, the baking process may include a baking step at a temperature lower than the maximum temperature.

[0109] A preferred example of the heating mode in the present invention is to heat at 50 to 150°C for 1 minute to 1 hour, and then increase the heating temperature to 180 to 250°C for 5 minutes to 4 hours. A particularly preferred example of the heating mode is to heat at 50 to 150°C for 1 minute to 1 hour, and then heat at 200 to 250°C for 5 minutes to 2 hours. Another more preferred example of the heating mode is to heat at 50 to 150°C for 1 to 30 minutes, and then heat at 200 to 250°C for 5 minutes to 1 hour.

[0110] The coating method is not particularly limited, but examples thereof include cast coating, spin coating, blade coating, dip coating, roll coating, bar coating, die coating, inkjet printing, and printing methods (relief printing, intaglio printing, lithography, screen printing, etc.).

[0111] Examples of heating equipment include a hot plate, an oven, etc. The heating atmosphere may be air or an inert gas, and may be atmospheric pressure or reduced pressure.

[0112] The thickness of the release layer 12 is usually about 0.01 to 50 μm, and from the viewpoint of productivity, it is preferably about 0.01 to 30 μm, more preferably about 0.01 to 20 μm, and the desired thickness is achieved by adjusting the thickness of the coating film before heating.

[0113] The release layer 12 has excellent adhesion to the support substrate 11, particularly to a plastic support substrate, and also has adequate adhesion to and adequate releasability with the electroless plating catalyst layer 13. Therefore, the release layer 12 can be transferred onto the resin substrate during press working without damaging the electroless copper layer 14. Furthermore, since it does not contain chromium, it has a low environmental impact.

[0114] (C) Electroless plating catalyst layer 13 The electroless plating catalyst layer 13 is a base layer for forming the electroless copper layer 14 described below on the release layer 12 made of an organic thin film, and is a layer formed from a base agent containing a polymer having an alkoxy group, a hydroxy group, an ammonium group, a carboxy group, or a cyano group, and metal fine particles.

[0115] The polymer is preferably a hyperbranched polymer, which is a highly branched polymer having an irregular branched structure obtained by polymerizing, for example, an ABx type multifunctional monomer (where A and B are functional groups that react with each other, and the number X of Bs is 2 or more).

[0116] Furthermore, the hyperbranched polymer is preferably a hyperbranched polymer represented by the following formula [1], which has a weight average molecular weight of 500 to 5,000,000.

[0117]

[0118] In the formula, R 1 R each independently represents a hydrogen atom or a methyl group. 2 , R 3 and R 4 are each independently a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, an arylalkyl group having 7 to 20 carbon atoms, or —(CHCHO) m R 5 (In the formula, R 5 represents a hydrogen atom or a methyl group, and m represents an integer of 2 to 100. The alkyl group and arylalkyl group may be substituted with an alkoxy group, a hydroxy group, an ammonium group, a carboxyl group, or a cyano group. 2 , R 3 and R 4 two groups together represent a linear, branched or cyclic alkylene group, or R 2 , R 3 and R 4 and the nitrogen atom to which they are attached may be joined together to form a ring. -represents an anion, and n is the number of repeating structural units and is an integer of 2 to 100,000.

[0119] The above R 2 , R 3 and R 4 Examples of the linear alkyl group having 1 to 20 carbon atoms in (D) include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, an n-hexadecyl group, an n-heptadecyl group, an n-octadecyl group, an n-nonadecyl group, and an n-eicosyl group. In terms of preventing the primer from eluting in the electroless plating solution used to form the electroless copper layer (D), preferred are groups having 8 or more carbon atoms, and an n-octyl group is particularly preferred. Examples of the branched alkyl group include an isopropyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. Examples of the cyclic alkyl group include groups having a cyclopentyl ring or cyclohexyl ring structure.

[0120] The above R 2 , R 3 and R 4 Examples of the arylalkyl group having 7 to 20 carbon atoms include a benzyl group and a phenethyl group.

[0121] The above R 2 , R 3 and R 4 Examples of linear alkylene groups formed by combining two of the above groups include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, and an n-hexylene group. Examples of branched alkylene groups include an isopropylene group, an isobutylene group, and a 2-methylpropylene group. Examples of cyclic alkylene groups include alicyclic aliphatic groups having a monocyclic, polycyclic, or bridged ring structure with 3 to 30 carbon atoms. Specific examples include groups having a monocyclo, bicyclo, tricyclo, tetracyclo, or pentacyclo structure with 4 or more carbon atoms. These alkylene groups may contain a nitrogen atom, a sulfur atom, or an oxygen atom within the group.

[0122] In the structure represented by the above formula [1], R 2 , R 3 and R 4 The ring formed by combining these with the nitrogen atom bonded thereto may contain a nitrogen atom, a sulfur atom or an oxygen atom in the ring, and examples thereof include a pyridine ring, a pyrimidine ring, a pyrazine ring, a quinoline ring and a bipyridyl ring.

[0123] Above X - The anion of the formula (I) is preferably a halogen atom, PF6 - , BF4 - or perfluoroalkanesulfonates.

[0124] In the above formula [1], A 1 represents a structure represented by the following formula [2].

[0125]

[0126] In the formula, A 2 represents a linear, branched or cyclic alkylene group having 1 to 30 carbon atoms which may contain an ether bond or an ester bond. 1 , Y 2 , Y 3 and Y 4 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a nitro group, a hydroxy group, an amino group, a carboxyl group, or a cyano group.

[0127] Above A 2 Specific examples of the alkylene group include linear alkylene groups such as methylene, ethylene, n-propylene, n-butylene, and n-hexylene, and branched alkylene groups such as isopropylene, isobutylene, and 2-methylpropylene. Examples of the cyclic alkylene group include alicyclic aliphatic groups having a monocyclic, polycyclic, or bridged ring structure with 3 to 30 carbon atoms. Specific examples include groups having a monocyclo, bicyclo, tricyclo, tetracyclo, or pentacyclo structure with 4 or more carbon atoms. Examples of the structure of the alicyclic moiety of the alicyclic aliphatic group include, but are not limited to, structures represented by the following formulas (a) to (s).

[0128]

[0129] In addition, Y in the above formula [2] 1 , Y 2 , Y 3 and Y 4 Examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, an isopropyl group, a cyclohexyl group, and an n-pentyl group. Examples of the alkoxy group having 1 to 20 carbon atoms include a methoxy group, an ethoxy group, an isopropoxy group, a cyclohexyloxy group, and an n-pentyloxy group. 1 , Y 2 , Y 3 and Y 4 are each independently preferably a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.

[0130] In addition, the above A 1 is preferably a structure represented by the following formula [4]:

[0131]

[0132] A preferred embodiment of the hyperbranched polymer represented by the above formula [1] is a hyperbranched polymer represented by the following formula [3], but is not limited thereto.

[0133] (In the formula, R 1 , R 2 , R 3 , R 4 and n is the same as above.)

[0134] The weight-average molecular weight Mw of the hyperbranched polymer is preferably 500 to 5,000,000, more preferably 1,000 to 1,000,000, even more preferably 2,000 to 500,000, and even more preferably 3,000 to 200,000. The dispersity: Mw (weight-average molecular weight) / Mn (number-average molecular weight) is preferably 1.0 to 7.0, more preferably 1.1 to 6.0, and even more preferably 1.2 to 5.0. The weight-average molecular weight Mw is a polystyrene-equivalent value measured by gel permeation chromatography.

[0135] The hyperbranched polymer represented by the formula [1] can be synthesized by known methods. For example, the method described in International Publication No. 2012 / 141215 can be referenced, and the hyperbranched polymer can be obtained by reacting an amine compound with a hyperbranched polymer having halogen atoms at the molecular end. The hyperbranched polymer having halogen atoms at the molecular end can be produced from a hyperbranched polymer having dithiocarbamate groups at the molecular end, as described in International Publication No. 2008 / 029688. The hyperbranched polymer having dithiocarbamate groups at the molecular end can be a commercially available product, and Hypertech (registered trademark) HPS-200 manufactured by Nissan Chemical Industries, Ltd. is a suitable example.

[0136] The metal microparticles may be any known metal microparticles, and are not particularly limited. Examples of metal species include iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), tin (Sn), platinum (Pt), and gold (Au). In the present invention, one of these metals may be used, or an alloy of two or more of these metals may be used. Among these, palladium microparticles are preferred. Note that oxides of the above metals may also be used as the metal microparticles.

[0137] The metal fine particles can be obtained by reducing metal ions, for example, by irradiating an aqueous solution of a metal salt with light from a high-pressure mercury lamp, or by adding a compound having a reducing action (a so-called reducing agent) to the aqueous solution. For example, a base agent containing a hyperbranched polymer and metal fine particles can be prepared by reducing the metal ions by adding an aqueous solution of a metal salt to a solution in which the hyperbranched polymer has been dissolved and irradiating the solution with ultraviolet light, or by adding an aqueous solution of a metal salt and a reducing agent to the solution, while forming a composite of the hyperbranched polymer and metal fine particles.

[0138] Examples of the metal salt include chloroauric acid, silver nitrate, copper sulfate, copper nitrate, copper acetate, tin chloride, platinous chloride, chloroplatinic acid, Pt(dba)2 [dba = dibenzylideneacetone], Pt(cod)2 [cod = 1,5-cyclooctadiene], Pt(CH3)2(cod), palladium chloride, palladium acetate (Pd(OC(=O)CH3)2), palladium nitrate, Pd2(dba)3.CHCl3, Pd(dba)2, and Ni(cod)2.

[0139] The reducing agent is not particularly limited, and various reducing agents can be used, and it is preferable to select the reducing agent depending on the metal species contained in the obtained primer. Examples of the reducing agent that can be used include metal borohydrides such as sodium borohydride and potassium borohydride; aluminum hydride salts such as lithium aluminum hydride, potassium aluminum hydride, cesium aluminum hydride, beryllium aluminum hydride, magnesium aluminum hydride, and calcium aluminum hydride; hydrazine compounds; citric acid and its salts; succinic acid and its salts; ascorbic acid and its salts; primary or secondary alcohols such as methanol, ethanol, isopropanol, and polyols; trimethylamine, triethylamine, diisopropylethylamine, diethylmethylamine, methyl ... tertiary amines such as amine, tetramethylethylenediamine [TMEDA], and ethylenediaminetetraacetic acid [EDTA]; hydroxylamine; and phosphines such as tri-n-propylphosphine, tri-n-butylphosphine, tricyclohexylphosphine, tribenzylphosphine, triphenylphosphine, triethoxyphosphine, 1,2-bis(diphenylphosphino)ethane [DPPE], 1,3-bis(diphenylphosphino)propane [DPPP], 1,1′-bis(diphenylphosphino)ferrocene [DPPF], and 2,2′-bis(diphenylphosphino)-1,1′-binaphthyl [BINAP].

[0140] The average particle size of the metal fine particles is preferably 1 to 100 nm. This is because if the average particle size of the metal fine particles exceeds 100 nm, the surface area decreases and the catalytic activity decreases. The average particle size is more preferably 75 nm or less, and particularly preferably 1 to 30 nm.

[0141] The content of the hyperbranched polymer in the primer is preferably 50 to 2,000 parts by mass relative to 100 parts by mass of the metal fine particles. If it is less than 50 parts by mass, the dispersibility of the metal fine particles is insufficient, and if it exceeds 2,000 parts by mass, the organic substance content increases, making it more likely to cause problems with physical properties, etc. A more preferred content is 100 to 1,000 parts by mass.

[0142] <Base Agent Comprising Hyperbranched Polymer and Metal Particles> The base agent comprises the hyperbranched polymer having the above-described ammonium groups at its molecular terminals and metal particles, and preferably the hyperbranched polymer and the metal particles form a composite. Here, the composite refers to a particulate form in which the hyperbranched polymer and the metal particles coexist in contact with or in proximity to the metal particles due to the action of the ammonium groups at the terminals of the hyperbranched polymer. In other words, the composite is expressed as a composite having a structure in which the ammonium groups of the hyperbranched polymer are attached to or coordinated with the metal particles. Therefore, the "composite" in the present invention may include not only a composite in which the metal particles and the hyperbranched polymer are bonded to form a single composite, as described above, but also a composite in which the metal particles and the hyperbranched polymer exist independently without forming a bond.

[0143] The formation of the composite of the hyperbranched polymer and metal particles is carried out simultaneously with the preparation of a primer containing the hyperbranched polymer and metal particles, and methods for this include synthesizing metal particles stabilized to some extent by lower ammonium ligands and then exchanging the ligands with the hyperbranched polymer, or forming the composite by directly reducing metal ions in a solution of the hyperbranched polymer having ammonium groups. Furthermore, as described above, the composite can also be formed by reducing the metal ions by adding an aqueous solution of a metal salt to a solution in which the hyperbranched polymer is dissolved and irradiating the solution with ultraviolet light, or by adding an aqueous solution of a metal salt and a reducing agent to the solution.

[0144] In the ligand exchange method, metal microparticles stabilized to a certain extent by lower ammonium ligands as raw materials can be synthesized by a method described in Journal of Organometallic Chemistry 1996, 520, 143-162, etc. A hyperbranched polymer having ammonium groups is dissolved in the resulting reaction mixture solution of metal microparticles, and the mixture is stirred at room temperature (approximately 25°C) or with heating to obtain the desired metal microparticle composite.

[0145] The solvent to be used is not particularly limited as long as it can dissolve the hyperbranched polymer and metal fine particles at the required concentration or higher, but specific examples include alcohols such as ethanol, propanol, isopropanol, etc.; halogenated hydrocarbons such as methylene chloride and chloroform, cyclic ethers such as tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, etc.; nitriles such as acetonitrile and butyronitrile, etc., and mixtures of these solvents. Among these, tetrahydrofuran is preferred in the present invention.

[0146] The temperature at which the reaction mixture of metal microparticles and the hyperbranched polymer having ammonium groups are mixed can usually be in the range of 0°C to the boiling point of the solvent used, and is preferably in the range of room temperature (approximately 25°C) to 60°C.

[0147] In the ligand exchange method, the metal particles can also be stabilized to some extent in advance by using a phosphine-based dispersant (phosphine ligand) in addition to the amine-based dispersant (lower ammonium ligand).

[0148] In the direct reduction method, a hyperbranched polymer having metal ions and ammonium groups is dissolved in a solvent and reacted under a hydrogen gas atmosphere to obtain the desired metal microparticle composite. Examples of metal ion sources that can be used include the metal salts mentioned above and metal carbonyl complexes such as hexacarbonyl chromium [Cr(CO)6], pentacarbonyl iron [Fe(Co)5], octacarbonyl dicobalt [Co2(CO)8], and tetracarbonyl nickel [Ni(CO)4]. Zero-valent metal complexes such as metal olefin complexes, metal phosphine complexes, and metal nitrogen complexes can also be used.

[0149] The solvent used is not particularly limited as long as it can dissolve the hyperbranched polymer having metal ions and ammonium groups in the required concentration or more, but specific examples include alcohols such as ethanol and propanol; halogenated hydrocarbons such as methylene chloride and chloroform; cyclic ethers such as tetrahydrofuran, 2-methyltetrahydrofuran, and tetrahydropyran; nitriles such as acetonitrile and butyronitrile; and mixtures of these solvents. Among these, tetrahydrofuran is preferred in the present invention. The temperature at which the hyperbranched polymer having metal ions and ammonium groups is mixed can usually be in the range of 0°C to the boiling point of the solvent used.

[0150] In addition, as a direct reduction method, the target metal fine particle composite can be obtained by dissolving a hyperbranched polymer having metal ions and ammonium groups in a solvent and subjecting it to a thermal decomposition reaction.

[0151] The metal ion source used here may be the above-mentioned metal salts, metal carbonyl complexes, other zero-valent metal complexes, or metal oxides such as silver oxide.

[0152] The solvent to be used is not particularly limited as long as it can dissolve the hyperbranched polymer having metal ions and ammonium groups in the required concentration or more, but specific examples include alcohols such as methanol, ethanol, n-propanol, isopropanol, and ethylene glycol; halogenated hydrocarbons such as methylene chloride and chloroform; cyclic ethers such as tetrahydrofuran, 2-methyltetrahydrofuran, and tetrahydropyran; nitriles such as acetonitrile and butyronitrile; aromatic hydrocarbons such as benzene and toluene; and mixtures of these solvents. Of these, toluene is preferred in the present invention.

[0153] The temperature at which the hyperbranched polymer having metal ions and ammonium groups is mixed can usually be in the range of 0°C to the boiling point of the solvent used, and is preferably near the boiling point of the solvent, for example, 110°C (heated reflux) in the case of toluene.

[0154] The composite of the hyperbranched polymer having ammonium groups and the metal fine particles thus obtained can be made into a solid form such as powder through a purification process such as reprecipitation.

[0155] The primer contains the hyperbranched polymer having the ammonium group and metal fine particles (preferably a composite of these), and may be in the form of a varnish used when forming the electroless plating catalyst layer 13 described below.

[0156] <Formation of Electroless Plating Catalyst Layer 13> (C) The electroless plating catalyst layer 13 can be formed by applying the above-mentioned primer onto the (B) release layer 12 made of the organic thin film. Specifically, first, the hyperbranched polymer having ammonium groups and metal fine particles (preferably a composite thereof) are dissolved or dispersed in an appropriate solvent to form a varnish, and the varnish is applied onto the (B) release layer 12 made of the organic thin film, and then the solvent is evaporated and dried to form a thin layer.

[0157] The method for applying the primer can be a known method, and is not particularly limited, and examples thereof include spin coating; blade coating; dip coating; roll coating; bar coating; die coating; spray coating; inkjet printing; pen lithography such as fountain pen nanolithography (FPN) and dip pen nanolithography (DPN); relief printing methods such as letterpress printing, flexographic printing, resin relief printing, contact printing, microcontact printing (μCP), nanoimprinting lithography (NIL), and nanotransfer printing (nTP); intaglio printing methods such as gravure printing and engraving; lithographic printing; stencil printing methods such as screen printing and mimeograph printing; offset printing; and the like.

[0158] In the present invention, among these coating methods, spin coating, spray coating, inkjet printing, pen lithography, contact printing, μCP, NIL, and nTP are preferred. Spin coating has the advantage of being able to apply a highly volatile solution in a short time, and can also be applied with high uniformity. Spray coating can be applied with a very small amount of varnish, making it industrially very advantageous.

[0159] The solvent used here is not particularly limited as long as it dissolves or disperses the complex, but examples include water; aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, chlorobenzene, and dichlorobenzene; alcohols such as methanol, ethanol, and isopropanol; ethers such as tetrahydrofuran, methyltetrahydrofuran, 1,4-dioxane, diethyl ether, diethylene glycol dimethyl ether, and propylene glycol methyl ether; esters such as ethyl acetate; ketones such as acetone, ethyl methyl ketone, isobutyl methyl ketone, cyclopentanone, and cyclohexanone; aliphatic hydrocarbons such as n-heptane, n-hexane, and cyclohexane; halogenated aliphatic hydrocarbons such as 1,2-dichloroethane and chloroform; amides such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide; and dimethyl sulfoxide. These solvents may be used alone or in combination. Furthermore, glycols such as ethylene glycol, propylene glycol, and butylene glycol may be added to adjust the viscosity of the varnish.

[0160] The concentration of the complex dissolved or dispersed in the solvent is not limited, but the concentration of the complex in the varnish is preferably 0.05 to 90% by mass, more preferably 0.1 to 80% by mass.

[0161] The method for drying the solvent is not particularly limited, and for example, the solvent may be evaporated using a hot plate or oven in an appropriate atmosphere, i.e., in air, an inert gas such as nitrogen, or in a vacuum. This makes it possible to obtain an electroless plating catalyst layer 13 having a uniform film surface. The baking temperature is not particularly limited as long as it can evaporate the solvent, but it is preferably 40 to 250°C.

[0162] The thickness of the electroless plating catalyst layer 13 is usually about 0.01 to 50 μm, and from the viewpoint of productivity, it is preferably about 0.01 to 20 μm, more preferably about 0.01 to 10 μm, and the desired thickness is achieved by adjusting the thickness of the coating film before heating.

[0163] (D) Electroless Copper Layer 14 By subjecting the electroless plating catalyst layer 13 formed as described above to an electroless plating treatment using a predetermined plating solution, an electroless copper layer 14 is formed on the electroless plating catalyst layer 13. The electroless plating treatment (step) is not particularly limited, and any commonly known electroless plating treatment can be performed, for example, a method in which a conventionally known electroless plating solution is used and the electroless plating base layer formed on the substrate is immersed in the plating solution (bath).

[0164] The electroless plating solution may contain primarily metal ions (metal salts), a complexing agent, and a reducing agent, and may also contain other additives such as a pH adjuster, a pH buffer, a reaction accelerator (second complexing agent), a stabilizer, and a surfactant (for improving the wettability of the surface to be treated, etc.) as appropriate depending on the application.

[0165] In the present invention, the metal used in the metal plating film formed by electroless plating is copper, which may contain at least one metal selected from the group consisting of iron, cobalt, nickel, palladium, silver, tin, platinum, and gold, provided that the effects of the present invention are not impaired.

[0166] The complexing agent and reducing agent may also be appropriately selected depending on the metal ion. Furthermore, a commercially available plating solution may be used as the electroless plating solution for forming the electroless copper layer. Specific examples of commercially available products include electroless plating solution (Printoganth (registered trademark) PVG2) manufactured by Atotech, electroless copper plating chemicals (Melplate CU series) manufactured by Meltex Co., Ltd., electroless nickel plating solution (ICP Nicoron series) manufactured by Okuno Chemical Industries, Ltd., and electroless copper plating solution (OPC-700 Electroless Copper M-K, ATS Addcopper IW).

[0167] Specific examples of plating solutions containing metals other than copper include electroless nickel plating chemicals (Melplate NI series), electroless tin plating solution (Substar SN-5), electroless gold plating solution (Flash Gold 330, Self Gold OTK-IT) manufactured by Meltex Inc., electroless palladium plating solution (Palette II), electroless gold plating solution (Dip G series, NC Gold series) manufactured by Kojima Chemical Co., Ltd., electroless silver plating solution (S-Dia AG-40) manufactured by Sasaki Chemical Co., Ltd., electroless nickel plating solution (Shumar (registered trademark) series, Shumar (registered trademark) Kaniblack (registered trademark) series) and electroless palladium plating solution (S-KPD) manufactured by Nippon Kanigen Co., Ltd.

[0168] In the electroless plating process, the formation rate and thickness of the metal coating can be controlled by adjusting the temperature, pH, immersion time, metal ion concentration of the plating bath, whether or not stirring is performed and the stirring rate, whether or not air or oxygen is supplied and the supply rate, etc.

[0169] The thickness of the electroless copper layer 14 is preferably 2 μm or less, more preferably 1.0 μm or less, even more preferably 0.5 μm or less, and even more preferably 0.2 μm or less, from the viewpoint of reducing side etching during flash etching. The lower limit is not particularly limited, but is usually 0.05 μm or more.

[0170] In the present invention, the use of electroless plating allows for a thinner electroless copper layer 14. By forming the electroless copper layer 14 thinly, the amount of copper used can be reduced, and side etching during flash etching in the wiring formation process of the printed wiring board is also reduced, resulting in finer wiring.

[0171] [Laminate] The laminate 10 of the present invention can be obtained by laminating, in order by the method and under the conditions described above, a release layer 12 made of an organic thin film and an electroless plating catalyst layer 13 on a supporting substrate 11. Furthermore, by laminating, by the method and under the conditions described above, an electroless copper layer 14 on the electroless plating catalyst layer 13 of the laminate 10, the laminate 1 of the present invention (electroless copper layer laminate 1) can be obtained.

[0172] [Method of manufacturing a printed wiring board] An example of a manufacturing process flow for a printed wiring board using the laminate 1 of the present invention (electroless copper layer laminate 1) is shown in Figure 3. An example of a method of manufacturing a printed wiring board using the laminate 1 of the present invention will be described below.

[0173] First, the electroless copper layer 14 of the laminate 1 of the present invention is placed face-to-face with a resin substrate 2 and pressure-bonded to obtain a composite of the laminate 1 and the resin substrate 2 (FIGS. 1(1) and 1(2)). An adhesive layer made of a thermoplastic resin or a thermosetting resin may be used to improve adhesion between the electroless copper layer 14 and the resin substrate 2. The release layer 12 and the electroless plating catalyst layer 13 are peeled at their interface, and the electroless copper layer 14 is transferred to the resin substrate 2, resulting in a printed wiring board seed layer S in which the electroless copper layer 14 and the electroless plating catalyst layer 13 are laminated on the resin substrate 2 (FIG. 1(3)). A photosensitive resist is applied (not shown) to the entire surface of the electroless plating catalyst layer 13 on the printed wiring board seed layer S, and after exposure and development, a photoresist layer 3 with openings in the areas requiring plating is formed (FIG. 1(4)). A wiring pattern 4 is formed in these openings by electroplating (FIG. 1(5)). After the photoresist layer 3 is removed with a resist remover, the electroless plating catalyst layer 13 and the electroless copper layer 14 remaining between the wiring patterns 4 are removed by flash etching, thereby obtaining a printed wiring board P on which the desired wiring pattern 4 is formed (FIG. 6(6)).

[0174] In the above manufacturing method, a method of forming a wiring pattern 4 on an electroless plating catalyst layer 13 of a seed layer S for a printed wiring board has been shown, but if necessary, the electroless plating catalyst layer 13 may be removed using a treatment liquid such as a palladium etching solution before applying a photosensitive resist as shown in Fig. 4 (Fig. 4 (4). In this case, the seed layer S for a printed wiring board has an electroless copper layer 14 laminated on a resin substrate 2.) This results in the wiring pattern 4 being formed directly on the electroless copper layer 14, which is expected to result in suppression of noise in electrical signals.

[0175] Furthermore, the obtained printed wiring board P may be sealed with a moisture scavenger or the like according to a standard method, if necessary, to prevent deterioration of the characteristics.

[0176] In the electroless copper layer laminate 1 of the present invention, the peel force when peeling at the interface between the release layer 12 and the electroless plating catalyst layer 13 is preferably 0.020 N / mm or less, more preferably less than 0.010 N / mm, and even more preferably 0.005 N / mm or less, from the viewpoint of easily peeling without damaging the electroless copper layer 14. On the other hand, the lower limit of the peel force is not particularly limited, but is preferably 0.001 N / mm or more, more preferably 0.0015 N / mm or more, from the viewpoint of stably fixing the electroless copper layer 14 on the supporting substrate 11.

[0177] EXAMPLES The present invention will be specifically described below with reference to examples of the present invention, but the present invention should not be construed as being limited to these examples.

[0178] The abbreviations for compounds used in the following examples are as follows: PGME: Propylene glycol monomethyl ether PGMEA: Propylene glycol monomethyl ether acetate PL-LI: 1,3,4,6-tetrakis(methoxyethyl)glycoluril (manufactured by Allnex Corporation, trade name: POWDERLINK 1174) PPTS: Pyridinium p-toluenesulfonate HPMA: 2-hydroxypropyl methacrylate ADMA: 2-adamantyl methacrylate HFiPMA: 1,1,1,3,3,3-hexafluoroisopropyl methacrylate HADM: 3-hydroxy-1-adamantyl methacrylate DCP: Dicyclopentanyl methacrylate BuMA: Butyl methacrylate AIBN: Azobisisobutyronitrile DDT: Dodecanethiol IPA: Isopropyl alcohol IPE: Diisopropyl ether DEGMEE: Diethylene glycol monoethyl ether

[0179]

[0180] In the following examples, the physical properties of samples were measured under the following conditions using the following apparatus. (1) GPC (Gel Permeation Chromatography) [Synthesis Examples 1-1 to 1-6] Apparatus: GPC apparatus manufactured by JASCO Corporation (Synthesis Examples) Column: Shodex (registered trademark) KD801 + KD805 manufactured by Showa Denko K.K. Column temperature: 40°C Solvent: dimethylformamide / LiBr.HO (29.6 mM) / HPO (29.6 mM) / tetrahydrofuran (0.1 mass%) Detector: UV (254 nm), RI [Synthesis Examples 2-1, 2-2, 2-4] Apparatus: HLC-8220GPC manufactured by Tosoh Corporation Column: Shodex (registered trademark) KF-804L + KF-803L manufactured by Showa Denko K.K. Column temperature: 40°C Solvent: tetrahydrofuran Detector: UV (254 nm), RI (2) 1 H-NMR spectrum Apparatus: JNM-L400 manufactured by JEOL Ltd. Solvent: CDCl3 Internal standard: tetramethylsilane (0.00 ppm) (3) 13 C-NMR spectrum Apparatus: JNM-ECA700 manufactured by JEOL Ltd. Solvent: CDCl3 Relaxation reagent: trisacetylacetonate chromium (Cr(acac)3) Reference: CDCl3 (77.0 ppm) (4) TEM (Transmission Electron Microscope) [Synthesis Example 2-3] Apparatus: HT-7700 manufactured by Hitachi, Ltd. Acceleration voltage: 100 kV [Synthesis Example 2-5] Apparatus: H-8000 manufactured by Hitachi, Ltd. Acceleration voltage: 200 kV (5) ICP Atomic Emission Spectroscopy (Inductively Coupled Plasma Atomic Emission Spectroscopy) [Synthesis Example 2-3] Apparatus: 5110 manufactured by Agilent Technologies [Synthesis Example 2-5] Apparatus: ICPM-8500 manufactured by Shimadzu Corporation (6) Fluorescent X-ray Film Thickness Measurement Apparatus: HT-7700 manufactured by Hitachi, Ltd. Acceleration voltage: 100 kV [Synthesis Example 2-6] Apparatus: H-8000 manufactured by Hitachi, Ltd. Acceleration voltage: 200 kV (7) ICP Atomic Emission Spectroscopy (Inductively Coupled Plasma Atomic Emission Spectroscopy) [Synthesis Example 2-6] Apparatus: 5110 manufactured by Agilent Technologies [Synthesis Example 2-6] Apparatus: ICPM-8500 manufactured by Shimadzu Corporation Fluorescent X-ray film thickness meter EX-731 Energy range: 67 to 96 Collimator: 0.5 mmφ X-ray output: 11 (7) Peel force measurement Apparatus: Autograph AGS-X500N manufactured by Shimadzu Corporation Peel angle: 180° Peel speed: 300 mm / min

[0181] [1] Polymer Synthesis [Synthesis Example 1-1] Polyurea Synthesis 100 g of monoallyl diglycidyl isocyanurate (manufactured by Shikoku Chemical Industry Co., Ltd.), 66.4 g of 5,5-diethylbarbituric acid, and 4.1 g of benzyltriethylammonium chloride were dissolved in 682 g of PGME, and the mixture was allowed to react at 130° C. for 24 hours to obtain a solution containing polyurea (solids concentration: 20% by mass). GPC analysis showed that the resulting polyurea had an Mw of 8,000 and an Mw / Mn of 1.5.

[0182] [Synthesis Example 1-2] Synthesis of fluorine-containing polymer (S1) 8.04 g of HFiPMA, 4.91 g of HPMA, 10.00 g of ADMA, and 0.93 g of AIBN, 1.15 g of DDT were dissolved in 100.10 g of PGME, and the mixture was reacted at 70 ° C. for 20 hours to obtain an acrylic polymer (S1) solution (solid concentration 20% by mass). The composition ratio of each unit was HFiPMA: HPMA: ADMA = 30: 30: 40 (molar ratio). As a result of GPC analysis, the Mw of the obtained acrylic polymer (S1) was 5,310, and Mw / Mn was 1.8.

[0183] [Synthesis Example 1-3] Synthesis of fluorine-containing polymer (S2) 53.6 g of HFiPMA, 16.4 g of HPMA, 50.0 g of ADMA, 4.66 g of AIBN, and 5.74 g of DDT were dissolved in 521.4 g of PGME and reacted at 70 ° C. for 20 hours to obtain an acrylic polymer (S2) solution (solid content concentration 20% by mass). The composition ratio (molar ratio) of each unit was HFiPMA: HPMA: ADMA = 40: 20: 40. As a result of GPC analysis, the Mw of the obtained acrylic polymer (S2) was 5,370, and Mw / Mn was 1.8.

[0184] [Synthesis Example 1-4] Synthesis of fluorine-containing polymer (S3) 6.43 g of HFiPMA, 3.22 g of HADM, 6.00 g of ADMA, 0.56 g of AIBN, and 0.69 g of DDT were dissolved in 67.6 g of PGME and reacted at 70 ° C. for 20 hours to obtain an acrylic polymer (S3) solution (solid content concentration 20% by mass). The composition ratio (molar ratio) of each unit was HFiPMA: HADM: ADMA = 40: 20: 40. As a result of GPC analysis, the Mw of the obtained acrylic polymer (S3) was 5,520, and Mw / Mn was 1.8.

[0185] [Synthesis Example 1-5] Synthesis of fluorine-containing polymer (S4) 9.16 g of HFiPMA, 2.80 g of HPMA, 8.00 g of DCP, 0.80 g of AIBN, and 0.98 g of DDT were dissolved in 86.9 g of PGME and reacted at 70 ° C. for 20 hours to obtain an acrylic polymer (S4) solution (solid content concentration 20% by mass). The composition ratio (molar ratio) of each unit was HFiPMA:HPMA:DCP = 40:20:40. As a result of GPC analysis, the Mw of the obtained acrylic polymer (S4) was 5,970 and Mw / Mn was 1.9.

[0186] [Synthesis Example 1-6] Synthesis of fluorine-containing polymer (S5) 6.97 g of HFiPMA, 2.84 g of HPMA, 7.00 g of BuMA, 0.81 g of AIBN, and 1.00 g of DDT were dissolved in 74.4 g of PGME and reacted at 70 ° C. for 20 hours to obtain an acrylic polymer (S5) solution (solid content concentration 20% by mass). The composition ratio (molar ratio) of each unit was HFiPMA:HPMA:BuMA = 30:20:50. As a result of GPC analysis, the Mw of the obtained acrylic polymer (S5) was 4,840, and Mw / Mn was 2.0.

[0187] [2] Synthesis of Pd particle composite [Synthesis Example 2-1] Synthesis of HPS-Cl

[0188] HPS-Cl was synthesized according to the method described in WO 2012 / 141215, as follows. A 500 mL reaction flask was charged with 27 g of sulfuryl chloride (Kishida Chemical Co., Ltd.) and 50 g of chloroform, and the mixture was stirred to dissolve uniformly. This solution was cooled to 0°C under a nitrogen stream. A separate 300 mL reaction flask was charged with 15 g of hyperbranched polymer HPS having dithiocarbamate groups at the molecular end and 150 g of chloroform, and the mixture was stirred under a nitrogen stream until uniform. The solution was added from the 300 mL reaction flask containing the HPS / chloroform solution to the sulfuryl chloride / chloroform solution cooled to 0°C over 60 minutes using a liquid transfer pump under a nitrogen stream, so that the temperature of the reaction solution was kept between -5 and 5°C. After the addition was complete, the reaction solution was stirred for 6 hours while maintaining the temperature between -5 and 5°C. A solution of 16 g of cyclohexene (Tokyo Chemical Industry Co., Ltd.) dissolved in 50 g of chloroform was then added to the reaction solution so that the temperature of the reaction solution was -5 to 5°C. After the addition was complete, the reaction solution was added to 1,200 g of IPA to precipitate a polymer. The precipitate was collected by filtration, and the resulting white powder was dissolved in 100 g of chloroform. This was then added to 500 g of IPA to reprecipitate the polymer. The precipitate was filtered and vacuum dried to obtain 8.5 g of a hyperbranched polymer (HPS-Cl) having chlorine atoms at the molecular terminals as a white powder (yield: 99%). The weight-average molecular weight (Mw) of the resulting HPS-Cl measured in terms of polystyrene by GPC was 14,000, and the polydispersity (Mw / Mn) was 2.9.

[0189] [Synthesis Example 2-2] Synthesis of HPS-N(Me)OctCl (In the formula, Me represents a methyl group, and Oct represents an octyl group.)

[0190] HPS-N(Me)OctCl was synthesized according to the method described in WO 2014 / 042215, as follows. A 100 mL reaction flask equipped with a reflux tower was charged with 4.6 g (30 mmol) of HPS-Cl produced in Synthesis Example 2-1 and 15 g of chloroform, and the mixture was stirred until homogeneous. To this solution, a solution of 5.0 g (31.5 mmol) of dimethyloctylamine [Kao Corporation, Farmin® DM0898] dissolved in 7.5 g of chloroform was added, followed by the addition of 7.5 g of IPA. This mixture was stirred at 65°C under a nitrogen atmosphere for 40 hours. After cooling to a liquid temperature of 30°C, the solvent was distilled off. The resulting residue was dissolved in 60 g of chloroform, and this solution was added to 290 g of IPE for reprecipitation purification. The precipitated polymer was filtered under reduced pressure and dried in vacuo at 50°C to obtain 9.3 g of a hyperbranched polymer (HPS-N(Me)2OctCl) having dimethyloctylammonium groups at the molecular terminals as a white powder. The weight-average molecular weight (Mw) of the resulting HPS-Cl, calculated from its Mw (14,000) and the ammonium group introduction rate (100%), was 28,000.

[0191] Synthesis Example 2-3: Synthesis of Pd[HPS-N(Me)OctCl] 4.6 g of palladium acetate (Kawaken Fine Chemicals Co., Ltd.) and 100 g of chloroform were charged into a 500 mL reaction flask equipped with a condenser and stirred until homogeneous. A solution of 5.0 g of HPS-N(Me)OctCl prepared in Synthesis Example 2-2 dissolved in 100 g of chloroform was added to this solution using a dropping funnel. The inside of the dropping funnel was washed into the reaction flask using 100 g of chloroform and 100 g of ethanol. This mixture was stirred at 60°C under a nitrogen atmosphere for 14 hours. After cooling to a liquid temperature of 30°C, the solvent was distilled off. The resulting residue was dissolved in a mixture of 38 g of chloroform and 38 g of ethanol, and this solution was added to 750 g of IPE for reprecipitation purification. The precipitated polymer was filtered under reduced pressure and dried in vacuo at 50°C to obtain 7.0 g of a composite of hyperbranched polymer with ammonium groups at the molecular end and Pd particles (Pd[HPS-N(Me)2OctCl]) as a black powder. ICP emission spectrometry revealed that the Pd content of the resulting Pd[HPS-N(Me)2OctCl] was 31% by mass. Figure 5 shows a TEM image of the resulting Pd particles. TEM observation revealed that the Pd particle diameter was approximately 2 to 4 nm.

[0192] Synthesis Example 2-4: Synthesis of HPS-NOct3Cl

[0193] HPS-NOct3Cl was synthesized according to the method described in WO 2012 / 141215, as follows. A 100 mL reaction flask equipped with a reflux tower was charged with 4.6 g (30 mmol) of HPS-Cl produced in Synthesis Example 2-1, 10.6 g (30 mmol) of trioctylamine (manufactured by Junsei Chemical Co., Ltd.), and 45 g of chloroform, and the atmosphere was replaced with nitrogen. This mixture was heated to reflux with stirring for 48 hours. After cooling to a liquid temperature of 30°C, the solvent was distilled off. The resulting residue was dissolved in 150 g of chloroform and cooled to 0°C. This solution was added to 3,000 g of IPE at 0°C for reprecipitation and purification. The precipitated polymer was filtered under reduced pressure and dried in vacuo at 40°C, yielding 9.6 g of a hyperbranched polymer (HPS-NOct3Cl) having trioctylammonium groups at its molecular terminals as a pale yellow powder. The weight average molecular weight Mw of HPS-NOct3Cl calculated from the Mw (14,000) of the obtained HPS-Cl and the ammonium group introduction rate (71%) was 37,000.

[0194] [Synthesis Example 2-5] Synthesis of Pd[HPS-NOct3Cl] 4.3 g of palladium acetate [Kawaken Fine Chemicals Co., Ltd.] and 200 g of chloroform were charged into a 1 L two-neck flask and stirred until homogenous. A solution of 18.0 g of HPS-NOct3Cl prepared according to Synthesis Example 2-4 dissolved in 200 g of chloroform was added to this solution using a dropping funnel. 100 g of ethanol was used to wash the inside of the dropping funnel into the reaction flask. This mixture was stirred at 60°C for 17 hours. After cooling to a liquid temperature of 30°C, the solvent was distilled off. The resulting residue was dissolved in 300 g of THF and cooled to 0°C. This solution was added to 6,000 g of IPE at 0°C and purified by reprecipitation. The precipitated polymer was filtered under reduced pressure and dried in vacuo at 60°C to obtain 19.9 g of a composite of hyperbranched polymer with ammonium groups at the molecular end and Pd particles (Pd[HPS-NOct3Cl]) as a black powder. ICP emission spectrometry revealed that the Pd content of the resulting Pd[HPS-NOct3Cl] was 11% by mass. Figure 6 shows a TEM image of the resulting Pd particles. TEM observation revealed that the Pd particle diameter was approximately 2-4 nm.

[0195] [3] Preparation of release layer-forming composition [Preparation Example 1-1] Preparation of release layer-forming composition 1 100 parts by weight of the polyurea obtained in Synthesis Example 1-1, 32 parts by weight of PL-LI, 3 parts by weight of PPTS, 16.8 parts by weight of fluorine-containing polymer (S1), 0.5 parts by weight of "Megafac F-554" manufactured by DIC, and PGMEA were added, and the mixture was diluted with PGME to a solids concentration of 2% by weight and a PGMEA concentration of 30% by weight to prepare release layer-forming composition 1.

[0196] Preparation Example 1-2 Preparation of Release Layer-Forming Composition 2 A release layer-forming composition 2 was obtained in the same manner as in Preparation Example 1-1, except that the fluorine-containing polymer (S2) was used instead of the fluorine-containing polymer (S1).

[0197] Preparation Example 1-3 Preparation of Release Layer-Forming Composition 3 A release layer-forming composition 3 was obtained in the same manner as in Preparation Example 1-1, except that the fluorine-containing polymer (S3) was used instead of the fluorine-containing polymer (S1).

[0198] Preparation Example 1-4 Preparation of Release Layer-Forming Composition 4 A release layer-forming composition 4 was obtained in the same manner as in Preparation Example 1-1, except that the fluorine-containing polymer (S4) was used instead of the fluorine-containing polymer (S1).

[0199] Preparation Example 1-5 Preparation of Release Layer-Forming Composition 5 A release layer-forming composition 5 was obtained in the same manner as in Preparation Example 1-1, except that the fluorine-containing polymer (S5) was used instead of the fluorine-containing polymer (S1).

[0200] [3] Preparation of Plating Primer [Preparation Example 2-1] Preparation of Electroless Plating Primer 1 75 mg of Pd[HPS-N(Me)OctCl] produced in Synthesis Example 2-3 and 2.5 mg of a leveling agent "Polyflow No. 56 (manufactured by Kyoeisha Chemical Co., Ltd.)" were dissolved in 2.46 g of DEGMEE and 2.46 g of IPA to prepare electroless plating primer 1 with a solids concentration of 1.5 mass %.

[0201] Preparation Example 2-2 Preparation of Electroless Plating Primer 2 75 mg of Pd[HPS-NOct3Cl] produced in Synthesis Example 2-5 was dissolved in 4.93 g of normal propanol to prepare electroless plating primer 2 with a solids concentration of 1.5 mass %.

[0202] [4] Preparation of Electroless Plating Solution [Preparation Example 3] Preparation of Electroless Copper Plating Solution An electroless copper plating solution was prepared as follows using commercially available Printganth (registered trademark) PVG2 [manufactured by Atotech Japan Co., Ltd.]: To a 200 mL flask were added 150 mL of pure water, 28 mL of Basic Printganth PVG2, 17 mL of Copper Printganth PVG2, 0.76 mL of Moderator Printganth PVG2, 0.08 mL of Stabilizer Printganth PVG2, 3 mL of Reducer Cu, and 1 mL of 10 mass % NaOH aq, followed by stirring and heating to 34°C to prepare an electroless copper plating solution.

[0203] [5] Preparation of Laminate (Support Substrate / Release Layer / Electroless Plating Catalyst Layer) [Example 1-1] A release layer-forming composition 1 was bar-coated to a thickness of 12 μm on a PET film (Tetron (registered trademark) manufactured by Teijin Limited (currently Toyobo Ester (registered trademark) Film) HB3 manufactured by Toyobo Co., Ltd.), and a coating film was obtained by heating at 100°C for 5 minutes using an oven. This coating film was further cured by heating at 150°C for 10 minutes using an oven, and a PET film with a release layer was obtained. Thereafter, electroless plating primer 1 was bar-coated to a thickness of 6 μm on the release layer on the PET film, and a laminate A was obtained by heating at 150°C for 5 minutes using an oven.

[0204] [Example 1-2] Release layer-forming composition 1 was bar-coated onto a polyimide film (Toray Industries, Inc., "Kapton" 300H, thickness 75 μm) to a thickness of 12 μm, and heated in an oven at 100°C for 5 minutes to obtain a coating film. This coating film was further cured by heating in an oven at 150°C for 10 minutes to obtain a polyimide film with a release layer. Thereafter, electroless plating primer 1 was bar-coated onto the release layer on the polyimide film to a thickness of 6 μm, and heated in an oven at 150°C for 5 minutes to obtain a coating film. This coating film was further heated in an oven at 170°C for 30 minutes to obtain a laminate B.

[0205] [Example 1-3] Release layer-forming composition 2 was bar-coated onto a polyimide film (Toray Industries, Inc., "Kapton" 300H, thickness 75 μm) to a thickness of 12 μm, and heated in an oven at 100°C for 5 minutes to obtain a coating film. This coating film was further cured by heating in an oven at 230°C for 10 minutes to obtain a polyimide film with a release layer. Thereafter, electroless plating primer 2 was bar-coated onto the release layer on the polyimide film to a thickness of 6 μm, and heated in an oven at 150°C for 5 minutes to obtain a coating film. This coating film was further heated in an oven at 250°C for 30 minutes to obtain a laminate C.

[0206] Example 1-4 A laminate D was obtained in the same manner as in Example 1-3, except that the release layer-forming composition 3 was used instead of the release layer-forming composition 2.

[0207] Example 1-5 A laminate E was obtained in the same manner as in Example 1-3, except that the release layer-forming composition 4 was used instead of the release layer-forming composition 2.

[0208] Example 1-6 A laminate F was obtained in the same manner as in Example 1-3, except that the release layer-forming composition 5 was used instead of the release layer-forming composition 2.

[0209] Comparative Example 1-1 An electroless plating primer 1 was bar-coated to a film thickness of 6 μm on a PET film (Tetoron (registered trademark) manufactured by Teijin Limited (currently Toyobo Ester (registered trademark) Film manufactured by Toyobo Co., Ltd.) HB3), and heated in an oven at 150° C. for 5 minutes to obtain a plastic film a with a plating catalyst layer.

[0210] Comparative Example 1-2 Electroless plating primer 1 was bar-coated onto a polyimide film (Kapton 300H, manufactured by Toray Industries, Inc., thickness 75 μm) to a film thickness of 6 μm, and heated in an oven at 150° C. for 5 minutes to obtain a coating film. This coating film was further heated in an oven at 170° C. for 30 minutes to obtain a plastic film b with a plating catalyst layer.

[0211] Comparative Example 1-3 Electroless plating primer 2 was bar-coated onto a polyimide film (Kapton 300H, manufactured by Toray Industries, Inc., thickness 75 μm) to a film thickness of 6 μm, and heated in an oven at 150° C. for 5 minutes to obtain a coating film. This coating film was further heated in an oven at 250° C. for 30 minutes to obtain a plastic film c with a plating catalyst layer.

[0212] [6] Preparation of electroless copper layer laminate (support substrate / release layer / electroless plating catalyst layer / electroless copper layer) [Example 2-1] Laminate 1 prepared in Example 1-1 was immersed for 10 minutes in the electroless copper plating solution prepared in Preparation Example 3. The substrate was taken out, washed with water, and dried on a hot plate at 120°C for 10 minutes to obtain electroless copper layer laminate A.

[0213] Example 2-2 An electroless copper layer laminate B was obtained in the same manner as in Example 2-1, except that the laminate B was used instead of the laminate A.

[0214] Example 2-3 An electroless copper layer laminate C was obtained in the same manner as in Example 2-1, except that the laminate C was used instead of the laminate A.

[0215] Example 2-4 An electroless copper layer laminate D was obtained in the same manner as in Example 2-1, except that the laminate D was used instead of the laminate A.

[0216] Example 2-5 An electroless copper layer laminate E was obtained in the same manner as in Example 2-1, except that the laminate E was used instead of the laminate A.

[0217] Example 2-6 An electroless copper layer laminate F was obtained in the same manner as in Example 2-1, except that the laminate F was used instead of the laminate A.

[0218] Comparative Example 2-1 An electroless copper layer laminate a was obtained in the same manner as in Example 2-1, except that the laminate A was replaced with a plastic film a with a plating catalyst layer.

[0219] Comparative Example 2-2 An electroless copper layer laminate b was obtained in the same manner as in Example 2-1, except that the laminate A was replaced with the plastic film b with a plating catalyst layer.

[0220] Comparative Example 2-3 An electroless copper layer laminate c was obtained in the same manner as in Example 2-1, except that the laminate A was replaced with the plastic film c with a plating catalyst layer.

[0221] [6] Evaluation of peel strength of electroless copper layer Cellotape (registered trademark) (CT-24, manufactured by Nichiban Co., Ltd.) was attached to the electroless copper layer laminates A to F and a to c, and the peel strength was measured by peeling it off using the above-mentioned device. Those that could not be peeled were marked as not peelable. The results are shown in Table 1.

[0222]

[0223] Furthermore, when the electroless copper layer laminate C obtained in Example 2-3 was heated on a hot plate at 240°C for 30 minutes under nitrogen flow and then evaluated for peel strength, the peel strength was 0.0017 N / mm, indicating that the peel strength of the electroless copper layer was maintained even when a high-temperature baking process was added.

[0224] Observation of the peeled surface of the electroless copper layer of the Examples shown in Table 1 revealed the adhesion of black palladium particles to the electroless copper layer side, but no such adhesion was observed on the supporting substrate side. From this result, it is inferred that the peeled interface is the interface between the peel layer made of an organic thin film and the electroless plating catalyst layer.

[0225] The above results demonstrated that the release layers of the examples exhibited excellent adhesion to the support substrate and excellent releasability from the electroless plating catalyst layer. On the other hand, the electroless copper layer could not be peeled from the support substrate in the comparative electroless copper layer laminates a to c, which did not have a release layer. After peeling the support substrate from the electroless copper layer of the examples shown in Table 1, the resulting peeled surface on the side of the seed layer for printed wiring boards was degreased using OPC Paraclean (manufactured by Okuno Pharmaceutical Co., Ltd.). The seed layer was then immersed in OPC Paladelet, a palladium etching solution (manufactured by Okuno Pharmaceutical Co., Ltd.), and the peeled surface changed from the black color of palladium to a glossy copper color. This suggests that the electroless plating catalyst layer was removed, exposing the electroless copper layer. Based on the above, the product can be used in the next step with the electroless plating catalyst layer remaining, or it can be used after removing the electroless plating catalyst layer.

[0226] REFERENCE SIGNS LIST 1 Laminate (electroless copper layer laminate) 10 Laminate 11 Support substrate 12 Release layer made of organic thin film 13 Electroless plating catalyst layer 14 Electroless copper layer 2 Resin substrate 3 Photoresist layer 4 Wiring pattern S Seed layer for printed wiring board P Printed wiring board

Claims

1. A laminate in which (A) a supporting substrate, (B) a release layer made of an organic thin film, and (C) an electroless plating catalyst layer are laminated in this order.

2. The laminate according to claim 1, further comprising (D) an electroless copper layer laminated on said (C) electroless plating catalyst layer.

3. The laminate according to claim 2, wherein said supporting substrate (A) is a plastic supporting substrate.

4. The laminate according to claim 2, wherein the release layer (B) made of an organic thin film is obtained from a composition for forming a release layer which contains a fluorine-containing polymer and a thermosetting resin.

5. The laminate according to claim 4, wherein said thermosetting resin comprises polyurea and a crosslinking agent.

6. The laminate according to claim 5, wherein the polyurea contains a repeating unit represented by the following formula (U1): [In the formula, A u1 , A u2 , A u3 , A u4 , A u5 and A u6 are each independently a hydrogen atom, a methyl group, or an ethyl group; u1 is a group represented by the following formula (U1-1), (U1-2), (U1-3) or (U1-4), (In the formula, R u1 and R u2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, the phenyl group being optionally substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms; u1 and R u2 may be bonded to each other to form a ring having 3 to 6 carbon atoms together with the carbon atom to which they are bonded, R u3is an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, and the phenyl group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms. u1 is a group represented by the following formula (U1-5) or (U1-6). (In the formula, X u2 is a group represented by formula (U1-1), formula (U1-2) or formula (U1-4), and Q u2 represents an alkylene group having 1 to 10 carbon atoms, a phenylene group, a naphthylene group, or an anthrylene group, the phenylene group, the naphthylene group, and the anthrylene group being optionally substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, a hydroxy group, and an alkylthio group having 1 to 6 carbon atoms; u1 and n u2 are each independently 0 or 1.

7. The laminate according to claim 4, wherein the fluorine-containing polymer is a polymer containing a repeating unit represented by the following formula (a1), a repeating unit represented by the following formula (b) and a repeating unit represented by the following formula (c). (In the formula, R A are each independently a hydrogen atom or a methyl group; R B1 is a branched alkyl group having 3 or 4 carbon atoms in which at least one hydrogen atom is substituted with a fluorine atom, R C is an alkyl group having 1 to 10 carbon atoms and a hydroxyl group or a polycyclic alkyl group having 6 to 20 carbon atoms and a hydroxyl group, R D represents an alkyl group having 1 to 10 carbon atoms which may be substituted with a polycyclic alkyl group having 6 to 20 carbon atoms, a polycyclic alkyl group having 6 to 20 carbon atoms, or an aryl group having 6 to 12 carbon atoms.

8. The laminate according to claim 2, wherein the electroless plating catalyst layer (C) contains a polymer having an alkoxy group, a hydroxy group, an ammonium group, a carboxy group or a cyano group, and fine metal particles.

9. The laminate according to claim 8, wherein said metal particles are palladium particles.

10. The laminate according to claim 8, wherein said polymer is a hyperbranched polymer.

11. The laminate according to claim 10, wherein the hyperbranched polymer is a hyperbranched polymer represented by formula [1] having a weight average molecular weight of 500 to 5,000,000. [In the formula, R 1 are each independently a hydrogen atom or a methyl group; R 2 , R 3 and R 4 are each independently a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, an arylalkyl group having 7 to 20 carbon atoms, or -(CHCHO) m R 5 (In the formula, R 5 represents a hydrogen atom or a methyl group, and m represents an integer of 2 to 100. The alkyl group and the arylalkyl group may be substituted with an alkoxy group, a hydroxy group, an ammonium group, a carboxy group, or a cyano group. 2 , R 3 and R 4 two of the groups taken together represent a linear, branched or cyclic alkylene group, or R 2 , R 3 and R 4 and may form a ring together with the nitrogen atom to which they are attached, - is an anion, n is an integer from 2 to 100,000, 1 is a structure represented by the following formula [2]. (In the formula, A 2 represents a linear, branched or cyclic alkylene group having 1 to 30 carbon atoms which may contain an ether bond or an ester bond; Y 1 , Y 2 , Y 3 and Y4 are each independently a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a nitro group, a hydroxyl group, an amino group, a carboxyl group, or a cyano group.

12. The laminate according to claim 10, wherein the metal particles and the hyperbranched polymer form a composite.

13. The laminate according to claim 10, wherein the hyperbranched polymer is a hyperbranched polymer represented by formula [3] having a weight average molecular weight of 500 to 5,000,000. (In the formula, R 1 , R 2 , R 3 , R 4 and n is the same as above.) 14. A method for producing a laminate according to any one of claims 2 to 13, comprising the steps of: (A) forming a release layer made of an organic thin film (B) on a supporting substrate; and (C) forming an electroless plating catalyst layer on the release layer made of an organic thin film (B).

15. The method for producing a laminate according to claim 14, further comprising the step of forming an electroless copper layer (D) on the electroless plating catalyst layer (C).

16. A method for producing a seed layer for a printed wiring board, comprising: pressing the electroless copper layer (D) of the laminate according to any one of claims 2 to 13 onto a resin substrate; peeling off the supporting substrate (A); and transferring the electroless copper layer (D) to the resin substrate.

17. A method for producing a seed layer for printed wiring boards, comprising: pressing the (D) electroless copper layer of the laminate of any one of claims 2 to 13 onto a resin substrate; peeling off the (A) supporting base material; transferring the (D) electroless copper layer to the resin substrate; and removing the (C) electroless plating catalyst layer with a palladium etching solution.

18. The method for producing a seed layer for a printed wiring board according to claim 16, wherein when the supporting substrate (A) is peeled off, the peeling occurs at the interface between the release layer (B) made of an organic thin film and the electroless plating catalyst layer (C).

19. A method for producing a printed wiring board, which uses the seed layer for a printed wiring board according to claim 16.

20. The method for producing a seed layer for a printed wiring board according to claim 17, wherein when the supporting substrate (A) is peeled off, the peeling occurs at the interface between the release layer (B) made of an organic thin film and the electroless plating catalyst layer (C).

21. A method for producing a printed wiring board, using the seed layer for a printed wiring board according to claim 17.

Citation Information

Patent Citations

  • Electromagnetic wave shielding sheet and method for manufacturing the same

    JP2003198183A

  • Metal-coated article, metal wiring board, and their manufacturing method

    JP2006240222A

  • Manufacturing method of element substrate

    JP2008177490A

  • Perforated metallic foil with carrier and method for producing the same

    JP2013227637A

  • Catalyst composition for transfer film for electroless plating, and transfer film for electroless plating